Pigment composition containing plate-like aluminum with excellent explosion stability and its manufacturing method

By coating aluminum flakes with multiple metal oxide layers and TiO2, the pigment composition achieves stability against thermite reactions and maintains color properties, addressing the instability and non-uniformity issues in existing pearlescent pigments.

JP7556612B2Active Publication Date: 2024-09-26CQV
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2023532359
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-12-03
Filing Date
2021-10-25
Publication Date
2024-09-26
Estimated Expiration
2041-10-25

AI Technical Summary

Technical Problem

Existing pearlescent pigments containing aluminum flakes face instability due to thermite reactions, which are exothermic and pose explosion risks, and existing coating methods result in non-uniform coloration.

Method used

Aluminum flakes are coated with multiple metal oxide layers, specifically a first oxide layer with a refractive index of 1.8 or less and a second oxide layer with a refractive index of 1.8 or more, and TiO2 is coated with a metal oxide layer to form a pigment composition with improved explosion stability and chroma.

Benefits of technology

The pigment composition maintains color saturation and hiding power while ensuring stability against thermite reactions, achieving lower apparent specific gravity and enhanced explosion resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007556612000005
    Figure 0007556612000005
  • Figure 0007556612000002
    Figure 0007556612000002
  • Figure 0007556612000001
    Figure 0007556612000001
Patent Text Reader

Abstract

The present invention relates to a pigment composition containing plate-like aluminum and having excellent explosion stability, and a method for producing the same, and more particularly to a pigment composition containing aluminum flakes coated with a plurality of metal oxide layers and TiO2 coated with a metal oxide layer, which ensures explosion stability, and a method for producing the same.The pigment composition of the present invention is blended with TiO2 coated with a metal oxide layer, which has a lower apparent specific gravity than other plate-like inorganic particles, and can prevent a decrease in saturation and hiding power while ensuring stability against the thermite reaction between aluminum and metal oxides.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a pigment composition containing plate-like aluminum with excellent explosion stability, and a manufacturing method and use thereof, and more particularly to a pigment composition containing aluminum flakes coated with a plurality of metal oxide layers and TiO2 coated with a metal oxide layer, and having explosion stability, and a manufacturing method and use thereof. This application claims priority based on Korean Patent Application No. 10-2020-0167192 filed on December 3, 2020, and all contents shown in the specification and drawings of the corresponding application are incorporated herein by reference. [Background technology]

[0002] Pearlescent pigments are a type of special luster pigment that emits pearlescent, iridescent, or metallic light to produce special colors and luster effects using the properties of light and the refraction of materials. Ordinary pigments are designed to produce only a certain color, but pearlescent pigments have the characteristic of changing color depending on the viewing angle, making them applicable to various industrial fields and a field that is continuously being researched and developed. Depending on the difference in refractive index of the medium, they can produce iridescent colors like natural pearls or metallic luster, and various metal oxides such as titanium dioxide, iron oxide, and silicon dioxide are mixed to realize various colors and luster.

[0003] However, when the metal substrate in the pigment contains aluminum, the thermite reaction, an exothermic chemical reaction between aluminum and other metal oxides, can be an issue that requires suppression.

[0004] Patent Document 1: Korean Patent No. 2107608 introduces a process of mixing non-metallic fine particles in the aqueous coating stage and coating with metal oxide, but there is a problem in that it is difficult to coat with a uniform color due to differences in specific gravity and specific surface area between the non-metallic fine particles and metal flakes. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Korean Patent No. 10-2107608 Summary of the Invention [Problem to be solved by the invention]

[0006] Therefore, the inventors have conducted research and efforts to produce a pigment composition that is stable against explosions caused by the thermite reaction of aluminum and metal oxides. As a result, they have discovered that a pigment composition that maintains saturation and hiding power while improving explosion stability can be obtained by mixing aluminum flakes coated with multiple metal oxide layers and TiO2 coated with a metal oxide layer, and have thus completed the present invention. [Means for solving the problem]

[0007] The present invention relates to Aluminum flakes coated with multiple metal oxide layers; and A pigment composition having improved explosion stability is provided that includes TiO2 coated with a metal oxide layer. Said TiO2 can exhibit an average diameter of 1 μm to 150 μm and a thickness of 10 nm to 500 nm.

[0008] The TiO2 may include a hollow space therein.

[0009] The aluminum flakes may be coated in sequence with a first oxide layer comprising a metal oxide having a refractive index of 1.8 or less and a second oxide layer comprising a metal oxide having a refractive index of 1.8 or more.

[0010] The metal oxide may be one or a mixture of two or more selected from Fe2O3, SnO2, ZrO2, SiO2, MgO·2, MgO·2O3, K2O·2, MnO, and Mg2SiO4.

[0011] The metal oxide layer coating the TiO2 can include Fe2O3.

[0012] The aluminum flakes and TiO2 may be mixed in a weight ratio of 1:9 to 7:3.

[0013] The pigment composition may be used in industrial coatings, varnishes, automotive coatings, powder coatings, printing inks or cosmetic applications.

[0014] On the other hand, the present invention is coating the aluminum flakes with a first oxide layer and a second oxide layer in sequence to obtain coated aluminum flakes; Coating the plate-like flakes with TiO2; a step of subjecting the TiO2-coated plate-like flakes to an acid treatment and a base treatment to obtain TiO2 plate-like particles from which the plate-like flakes have been removed; Coating the surface of the TiO2 platelet particles with a metal oxide to obtain coated TiO2 platelet particles; and mixing the coated aluminum flakes with the coated TiO2 platelet particles.

[0015] The surfaces of the TiO2 platelet particles can be coated with a metal oxide containing Fe2O3 to obtain coated TiO2 platelet particles.

[0016] The coated aluminum flakes and the coated TiO2 platelet particles can be dry mixed. Effect of the Invention

[0017] The pigment composition of the present invention is mixed with TiO2 coated with a metal oxide layer, which has a lower apparent specific gravity than other plate-like inorganic particles, and can prevent a decrease in saturation and hiding power while ensuring stability against the thermite reaction between aluminum and metal oxide. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] The present invention will be described in detail below. Prior to this, the terms and words used in the present specification and claims should not be interpreted as being limited to their ordinary or dictionary meanings, but should be interpreted according to the meaning and concept that corresponds to the technical idea of ​​the present invention, based on the principle that the inventor can appropriately define the concept of the term to best describe his / her invention. Therefore, the configurations described in the embodiments of the present specification are merely the most preferred embodiments of the present invention, and do not fully represent the technical idea of ​​the present invention, and therefore there may be various equivalents and modifications that replace them at the time of filing this application.

[0019] The pigment composition of the present invention is characterized by comprising aluminum flakes coated with a plurality of metal oxide layers, and TiO2 coated with a metal oxide layer.

[0020] The TiO2 may be plate-shaped and may include a hollow penetrating the center, but is not limited thereto. When the TiO2 includes a hollow, it is light in weight and has a lower apparent specific gravity than other plate-shaped inorganic pigments, so that the same explosion stability can be ensured even at a lower mixing ratio than other pigments.

[0021] The TiO2 may have an average diameter of 1 μm to 150 μm and a thickness of 10 nm to 500 nm, and when a hollow penetrating the center is included, the thickness of the substrate itself excluding the hollow.

[0022] In addition, the TiO2 may exhibit a different interference color depending on its thickness; specifically, when the TiO2 has a thickness of 30 nm to 70 nm, it exhibits a white interference color; when the TiO2 has a thickness of 70 nm to 100 nm, it exhibits a gold interference color; when the TiO2 has a thickness of 100 nm to 120 nm, it exhibits a red interference color; when the TiO2 has a thickness of 120 nm to 140 nm, it exhibits a violet interference color; when the TiO2 has a thickness of 140 nm to 160 nm, it exhibits a blue interference color; and when the TiO2 has a thickness of 170 nm to 190 nm, it exhibits a green interference color.

[0023] The surface of the TiO2 is coated with a metal oxide layer, which may include one or a mixture of two or more selected from Fe2O3, SnO2, ZrO2, SiO2, MgO·2, MgO·2O3, K2O·2, MnO, and Mg2SiO4, and preferably includes Fe2O3.

[0024] The metal oxide may be contained in an amount of 10 parts by weight to 100 parts by weight, preferably 20 parts by weight to 80 parts by weight, more preferably 25 parts by weight to 50 parts by weight, and most preferably 25 parts by weight to 35 parts by weight, relative to 100 parts by weight of TiO2.

[0025] The aluminum flakes are coated on their surfaces with a plurality of metal oxide layers, and may have an average diameter of 1 μm to 150 μm and a thickness of 10 nm to 500 nm.

[0026] The aluminum flakes may be sequentially coated with a first oxide layer containing a metal oxide having a refractive index of 1.8 or less and a second oxide layer containing a metal oxide having a refractive index of 1.8 or more. Preferably, the metal oxide contained in the first oxide layer may be SiO2, and the metal oxide contained in the second oxide layer may be Fe2O3, but is not limited thereto.

[0027] The pigment composition of the present invention may be a mixture of the aluminum flakes coated with a plurality of metal oxide layers and TiO2 coated with a metal oxide layer in a weight ratio of 1:9 to 7:3, preferably in a weight ratio of 3:7 to 6:4, and most preferably in a weight ratio of 4:6 to 5:5.

[0028] The pigment compositions of the present invention may be used in industrial coatings, varnishes, automotive coatings, powder coatings, printing inks or cosmetic applications.

[0029] The present invention also provides a method for producing a semiconductor device comprising the steps of: coating the aluminum flakes with a first oxide layer and a second oxide layer in sequence to obtain coated aluminum flakes; Coating the plate-like flakes with TiO2; a step of subjecting the TiO2-coated plate-like flakes to an acid treatment and a base treatment to obtain TiO2 plate-like particles from which the plate-like flakes have been removed; Coating the surface of the TiO2 platelet particles with a metal oxide to obtain coated TiO2 platelet particles; and mixing the coated aluminum flakes with the coated TiO2 platelet particles.

[0030] First, aluminum flakes are coated sequentially with a first oxide layer and a second oxide layer.

[0031] Preferably, the metal oxide contained in the first oxide layer may be SiO2, and the metal oxide contained in the second oxide layer may be Fe2O3.

[0032] Specifically, the aluminum flakes are placed in a solvent, a Si precursor compound is added and stirred, and then a basic solution is added and further stirred to form a first passivation layer containing SiO2.

[0033] The Si precursor compound may be tetraethyl orthosilicate (TEOS), tetramethyl orthosilicate (TMOS), or the like.

[0034] Next, the aluminum flakes formed on the first passive layer are put into deionized water, an Fe precursor compound is added, and the mixture is stirred and then heat-treated to form a second passive layer containing Fe2O3. At this time, it is preferable to adjust the pH to a range of 1 to 5 using a pH adjuster, and more preferably, the pH is adjusted to a range of 2 to 4.

[0035] The Fe precursor compound may be FeCl3, Fe(NO3)3, FeSO4, or the like.

[0036] The aluminum flakes on which the second passivation layer has been formed are dehydrated, washed with water, and dried, and then heat-treated at 200°C to 400°C to obtain coated aluminum flakes, which are the first component in the pigment composition.

[0037] Next, separate plate-like flakes are prepared, and the surfaces of the flakes are coated with TiO2.

[0038] Specifically, the plate-like flakes are suspended in deionized water, and a Ti precursor compound and a basic solution are added while maintaining an acidic condition of pH 1 to 5, preferably pH 1.5 to 2.5, and then the mixture is stirred and fired to form a TiO2 coating layer.

[0039] The Ti precursor compound may be TiCl4, TiOCl2, Ti(SO4)2, Ti(NO3)4, or the like.

[0040] The plate-like flakes may include at least one selected from mica, plate-like silica, and glass flakes, among which mica is preferred. As the plate-like flakes, powder that has been crushed and classified, or powder that has been crushed and classified after preparation, may be used.

[0041] The plate-like flakes preferably have an average diameter of 1 μm to 150 μm. If the average diameter of the plate-like flakes is less than the above range, the plate-like flake substrate gradually changes into a spherical shape as the coating thickness increases while the surface of the plate-like flake substrate is coated with a substance, and the squareness ratio decreases. If the squareness ratio decreases, diffuse reflection occurs, resulting in light scattering, and it is not possible to consistently show the same color with the same refractive index. On the other hand, if the average diameter of the plate-like flakes exceeds the above range, the surface area to be coated increases, making it difficult to form a coating layer to realize a color.

[0042] The surface of the plate-like flakes is coated with TiO2, and the TiO2 coating layer can have a thickness of 10 nm to 1,000 nm, preferably 50 nm to 500 nm, and more preferably 100 nm to 300 nm.

[0043] Next, the TiO2 coated plate-like flakes are treated with an acid and a base to obtain TiO2 plate-like particles from which the plate-like flakes have been removed.

[0044] First, TiO2-coated plate-like flakes are mixed and suspended in deionized water, and an acidic solution is added to the mixture, which is then subjected to a primary acid treatment, followed by reflux, washing with water, and filtration.

[0045] In this case, in the acid treatment, it is more preferable to apply ultrasonic waves under the conditions of 15 kHz to 40 kHz and output power of 70 W to 110 W while stirring at a speed of 300 rpm to 500 rpm.

[0046] Agitation may be insufficient when the agitation speed is less than 300 rpm or the ultrasonic output power is less than 70 W. On the other hand, when the agitation speed exceeds 500 rpm or the ultrasonic output power exceeds 110 W, the particles are severely cracked and many unnecessary small particles are generated, making it difficult to control the size to a desired size or to proceed with subsequent processes.

[0047] In this case, the acid solution may be any one selected from sulfuric acid, phosphoric acid, nitric acid, etc.

[0048] Alternatively, a mixed solution of at least two of these may be used. As such an acidic solution, it is preferable to use one diluted to a concentration of 40% to 60% by weight. If the concentration of the acidic solution is below the above range, the plate-like flakes are not dissolved well during the first acid treatment, so that it may be difficult to ensure a hollow structure. On the other hand, if the concentration of the acidic solution exceeds the above range, the excessive concentration may cause a problem that the TiO2 coating layer coated on the plate-like flakes is dissolved together with the plate-like flakes.

[0049] In this step, reflux is preferably carried out at 80°C to 120°C for 4 to 6 hours. If the reflux temperature is less than 80°C or the reflux time is less than 4 hours, a sufficient dissolution rate cannot be ensured, and non-uniform hollow spheres may be generated, which may induce surface cracks due to insoluble plate-like flakes. On the other hand, if the reflux temperature exceeds 120°C or the reflux time exceeds 6 hours, it is not preferable because the hollow sphere coating layer may crack due to stirring or the TiO2 coating layer may separate.

[0050] After the acid treatment, the resultant product is dehydrated and washed with water, and deionized water is mixed therewith to form a suspension, which is then added to a basic solution for secondary base treatment, which is then refluxed and filtered.

[0051] As the basic solution, it is preferable to use a strong base with a concentration of 40% by weight to 55% by weight, and specifically, one or more selected from sodium hydroxide and potassium hydroxide can be used.

[0052] If the concentration of the basic solution is less than 40 wt%, the TiO2-coated plate-like flakes that have been primarily acid-treated may not be completely dissolved, and thus the hollow morphology may not be formed.On the other hand, if the concentration of the basic solution is more than 55 wt%, not only the plate-like flake substrate but also the coated TiO2 layer may be dissolved due to the excessive concentration, which is undesirable.

[0053] In this case, the reflux is preferably carried out at 50° C. to 70° C. for 1 hour to 3 hours.

[0054] Through the above process, the plate-like flakes on which the TiO2 coating layer is formed are first treated with an acid to remove more than half of the plate-like flakes, and then a second alkali treatment is performed, so that it is possible to completely remove the plate-like flakes and form a hollow structure.

[0055] The result of the base treatment is dried to obtain TiO2 plate-like particles having a hollow structure from which the plate-like flakes have been removed.

[0056] In this case, drying is preferably carried out at 100° C. to 150° C. for 10 minutes to 120 minutes. If the drying temperature is less than 100° C., the drying time will be long, and economic efficiency and productivity may decrease. On the other hand, if the drying temperature exceeds 150° C., a phenomenon of increased aggregation between powder particles may occur, which is not preferable.

[0057] Next, the surfaces of the TiO2 platelet particles are coated with a metal oxide to obtain coated TiO2 platelet particles.

[0058] The metal oxide may include Fe2O3, and specifically, the second passive layer including Fe2O3 can be formed by putting the mixture into deionized water, adding an Fe precursor compound, stirring, and then heat treating the mixture. At this time, it is preferable to adjust the pH to a range of 1 to 5 using a pH adjuster, and more preferably, the pH is adjusted to a range of 2 to 4.

[0059] The Fe precursor compound may be FeCl3, Fe(NO3)3, FeSO4, or the like.

[0060] After coating with the metal oxide containing Fe2O3, the product is dehydrated, washed with water, dried, and then heat-treated at 500°C to 1,000°C to obtain coated TiO2 platelet particles, which are the second component in the pigment composition.

[0061] The coated aluminum flakes and the coated TiO2 platelet particles are then mixed to obtain the final pigment composition.

[0062] The coated aluminum flakes and the coated TiO2 platelet particles may be mixed in a weight ratio of 1:9 to 7:3, preferably in a weight ratio of 3:7 to 6:4, and most preferably in a weight ratio of 4:6 to 5:5. In addition, the coated aluminum flakes and the coated TiO2 platelet particles are preferably mixed in a dry state in a state separated from an aqueous solvent or the like.

[0063] Hereinafter, the present invention will be described in detail with reference to examples and experimental examples. However, each embodiment of the present invention can be modified into many other forms, and the scope of the present invention should not be construed as being limited to each embodiment described below. Each embodiment of the present invention is provided to more completely explain the present invention to those having average knowledge in the art.

[0064] Production Example 1: Production of coated aluminum flakes

[0065] A first slurry was prepared by adding 100 g of aluminum flakes having a diameter of 15 μm to 490 g of isopropyl alcohol (IPA). Then, 50 g of tetraethyl orthosilicate (TEOS) was added to the first slurry, and the mixture was stirred at 400 rpm using a 7.5 cm impeller. Next, the first slurry was heated to 50° C., and then 140 g of H2O and 5 g of 25% ammonia water were added. Then, the mixture was stirred for about 20 hours while maintaining the temperature at 50° C., and a first passivation layer made of silicon oxide was formed. Then, the mixture was dehydrated / washed with IPA and dried.

[0066] The second slurry was prepared by adding 30 g of the aluminum flakes coated with the first passivation layer to 300 g of purified water, and the mixture was stirred at 400 rpm using a 7.5 cm impeller. The mixture was then heated to 75°C, adjusted to pH 3.0, and refluxed for 30 minutes. Next, FeCl3 aqueous solution was added while maintaining the pH at 3.0. Caustic soda was used to maintain the pH. The FeCl3 aqueous solution showed a copper color at the beginning of the addition, and after confirming that the color changed from copper to gold as the amount of the FeCl3 aqueous solution added increased, the addition of the FeCl3 aqueous solution was stopped. The powder obtained by dehydrating, washing, and drying with purified water was heat-treated at 300°C for 1 hour to obtain coated aluminum flakes.

[0067] Production Example 2: Production of hollow coated TiO2 plate-like particles

[0068] First, 100g of mica particles were suspended in 2L of deionized water, and then 40% by weight of TiOCl2 and sodium hydroxide solution were added simultaneously while maintaining the pH at 1.5 at 80℃. Through this, a TiO(OH)2 coating layer was formed on the surface of the mica particles. When the desired interference color was obtained, the addition of TiOCl2 and sodium hydroxide solution was stopped, and the mixture was stirred for more than 10 minutes, washed and dried, and then fired at 850℃ to form a TiO2 coating layer on the surface of the synthetic mica particles.

[0069] Next, acid treatment and alkali treatment were performed to produce plate-shaped TiO2 particles. First, a condenser was installed in the reactor, and 400 ml of sulfuric acid was added and stirred at 400 rpm. Next, the mixture was refluxed for 6 hours while maintaining the temperature at 100 ° C, cooled, and then refluxed again while adding 800 ml of water. Then, it was filtered using filter paper and washed four times with 1000 ml of water. Next, the acid-treated powder was placed in a 3 L flask, 800 ml of deionized water was added, and the mixture was stirred at a speed of 400 rpm to suspend it, and then 400 ml of a 50 wt% sodium hydroxide aqueous solution was added and refluxed for 4 hours while maintaining the temperature at 60 ° C. Then, the mixture was filtered using filter paper, washed four times with 800 ml of water, and dried at 120 ° C to produce hollow TiO2 plate-shaped particles.

[0070] 30 g of the hollow TiO2 plate-like particles were added to 500 g of purified water to form a slurry, which was then stirred at 400 rpm using a 7.5 cm impeller. The temperature was then raised to 75°C, and the pH was adjusted to 3.0, followed by refluxing for 30 minutes. Next, FeCl3 aqueous solution was added while maintaining the pH at 3.0. At this time, caustic soda was used to maintain the pH. As the amount of FeCl3 aqueous solution added increased, the color changed to gold, after which the addition of FeCl3 aqueous solution was stopped. The powder obtained by dehydrating, washing and drying with purified water was then heat-treated at 800°C for 1 hour to obtain hollow coated TiO2 plate-like particles.

[0071] Example 1: Preparation of a pigment composition

[0072] The coated aluminum flakes produced in the above Production Example 1 and the coated TiO2 plate-like particles produced in the above Production Example 2 were mixed to produce a pigment composition.

[0073] Experimental example 1: Confirmation of explosion stability

[0074] In the pigment composition of Example 1, the coated aluminum flakes and the coated TiO2 hollow plate-like particles were mixed at different dry mixing ratios, and the explosive power was measured. The results are shown in Table 1 below.

[0075] The following explosive power is shown by comparing the degree of explosion after directly contacting 3g of powder with flame to cause a thermite reaction. The degree of explosion is a value compared relative to the explosive power of the coated aluminum flakes alone (100%), which is set at 10.

[0076] [Table 1]

[0077] As shown in Table 1, it was confirmed that the explosive power remained low up to a weight ratio of 5:5 between the coated aluminum flakes and the coated TiO2 platelet particles, but the explosive power increased as the weight ratio of the coated TiO2 platelet particles increased.

[0078] Meanwhile, the coated aluminum flakes were mixed with synthetic mica or general TiO2 particles coated with metal oxide, and the explosive power was confirmed in the same manner as above. The results are shown in Tables 2 to 4 below.

[0079] For comparison, synthetic mica used was a plate-like synthetic mica having a D50 of about 20 μm and a thickness of about 500 nm.

[0080] In addition, the TiO2-coated synthetic mica was prepared by diluting the synthetic mica with purified water to 10% by weight, and then maintaining the pH at 1.8 at 70°C using TiOCl2 and sodium hydroxide until a gold tone was achieved, followed by dehydration, washing with water, and heat treatment.

[0081] In addition, the Fe2O3-coated synthetic mica was prepared by diluting the synthetic mica with purified water to 10% by weight, and then maintaining the pH at 3.0 at 70°C using FeCl3 and sodium hydroxide until a bronze tone was achieved, followed by dehydration, washing with water, and heat treatment.

[0082] [Table 2]

[0083] [Table 3]

[0084] [Table 4]

[0085] As shown in Tables 2 to 4, it was confirmed that the explosive force was maintained at a high level when aluminum flakes were mixed with general inorganic particles, and therefore it was confirmed that the pigment composition of the present invention had relatively high explosive stability.

[0086] Experimental Example 2: Confirmation of chroma and hiding power of pigment composition

[0087] Through the above experiments, it was confirmed that the pigment composition of the present invention has explosion stability when coated aluminum flakes and coated TiO2 platelet particles are mixed in a weight ratio of 5:5. Therefore, the chroma and hiding power of the pigment composition were measured and compared with those of a pigment composition in which coated aluminum flakes and other inorganic particles were mixed in a weight ratio of 5:5, and the results are shown in Table 5 below.

[0088] In Table 5, the example shows a composition in which the coated aluminum flakes of Preparation Example 1 and the coated TiO2 platelet particles of Preparation Example 2 are mixed in a weight ratio of 5:5.

[0089] Meanwhile, in Table 5 below, Comparative Example 1 shows a composition in which the coated aluminum flakes of Production Example 1 and synthetic mica particles are mixed in a weight ratio of 5:5, Comparative Example 2 shows a composition in which the coated aluminum flakes of Production Example 1 and synthetic mica particles coated with TiO2 are mixed in a weight ratio of 5:5, and Comparative Example 3 shows a composition in which the coated aluminum flakes of Production Example 1 and synthetic mica particles coated with Fe2O3 are mixed in a weight ratio of 5:5.

[0090] [Table 5]

[0091] In Table 5, C * means saturation, dC * means the difference in saturation from the coated aluminum flakes of Production Example 1.

[0092] As shown in Table 5, it was confirmed that the pigment compositions of the Examples exhibited superior chroma and hiding power compared to the other pigment compositions.

Claims

1. Aluminum flakes coated with a plurality of metal oxide layers; and Metal oxide layer coated TiO 2 Including, the aluminum flakes include a first oxide layer containing SiO 2 and a second oxide layer containing a metal oxide having a refractive index of 1.8 or more; The metal oxide layer covering the TiO 2 contains Fe 2 O 3 A pigment composition having improved explosion stability, characterized in that

2. The TiO 2 indicates an average diameter between 1 μm and 150 μm and a thickness between 10 nm and 500 nm The pigment composition according to claim 1.

3. The TiO 2 Contains a hollow space inside The pigment composition according to claim 1.

4. The aluminum flakes and TiO 2 are mixed in a weight ratio of 1:9 to 7:

3. The pigment composition according to claim 1.

5. Used in industrial coatings, varnishes, automotive coatings, powder coatings, printing inks or cosmetic applications The pigment composition according to claim 1.

6. coating aluminum flakes with a first oxide layer comprising SiO2 and a second oxide layer comprising a metal oxide having a refractive index of 1.8 or more, in order to obtain coated aluminum flakes; TiO on plate-shaped flakes 2 coating the The TiO 2 The plate-like flakes coated with TiO were treated with acid and base to obtain TiO2 with the plate-like flakes removed. 2 Obtaining platelet-shaped particles; The TiO 2The surface of the plate-like particle is coated with a metal oxide containing Fe 2 O 3 , and the coated TiO 2 Obtaining platelet-shaped particles; and The coated aluminum flakes and the coated TiO 2 mixing the platelet-shaped particles; A method for producing a pigment composition comprising the steps of:

7. The coated aluminum flakes and the coated TiO 2 Dry mixing with plate-like particles A method for producing the pigment composition according to claim 6.

Citation Information

Patent Citations

  • Iron oxide-coated inorganic sphere

    JP1987146962A

  • Iron-containing titanium dioxide and production thereof

    JP1995069636A

  • Pigment mixture

    JP2000198944A

  • Method for manufacturing aluminum effect pigments coated with metal oxides

    JP2015518910A

  • Metallic glossy pigment based on substrate thin piece with thickness of 1 nm to 50 nm