Compositions containing titania-coated silver

The titania-coated silver composition addresses the limitations of existing antibacterial agents by providing transparency, adhesion, durability, and long-term effectiveness through a unique particle structure and formulation.

JP7574486B1Active Publication Date: 2024-10-28OSAKA GAS CO LTD

Patent Information

Application Number
JP2024056417
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2024-03-29
Publication Date
2024-10-28
Estimated Expiration
2044-03-29

AI Technical Summary

Technical Problem

Existing antibacterial agents face challenges in achieving transparency, adhesion to substrates, durability, and long-term stability, with organic agents providing short-term effects and inorganic agents being colored and less transparent.

Method used

A composition comprising titania-coated silver particles, where a portion of the silver particle surface is coated with titania, combined with a Si compound and a solvent, enhances adhesion and stability while maintaining transparency and antibacterial properties.

Benefits of technology

The composition achieves high transparency, strong adhesion to substrates, durability, and long-term antibacterial and antiviral properties by minimizing silver aggregation and improving dispersibility.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007574486000001
    Figure 0007574486000001
  • Figure 0007574486000002
    Figure 0007574486000002
  • Figure 0007574486000003
    Figure 0007574486000003
Patent Text Reader

Abstract

An object of the present invention is to provide a titania-coated silver-containing composition that combines transparency, adhesion to a substrate, durability, antibacterial and antiviral properties, and long-term stability. A composition containing titania-coated silver.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to compositions containing titania-coated silver. [Background technology]

[0002] Patent Document 1 discloses an antibacterial liquid containing antibacterial microparticles, a binder and a solvent, in which the antibacterial microparticles contain silver-supported inorganic oxide, the binder contains at least one compound having a siloxane bond, the solvent contains alcohol and water, the solids concentration relative to the total mass of the antibacterial liquid is less than 5 mass%, and the content of the compound having a siloxane bond relative to the total solids content of the antibacterial liquid is 60 mass% or more. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent Publication No. 2017-043599 Summary of the Invention [Problem to be solved by the invention]

[0004] An object of the present invention is to provide a titania-coated silver-containing composition that combines transparency, adhesion to a substrate, durability, antibacterial and antiviral properties, long-term stability, and the like. [Means for solving the problem]

[0005] The present invention encompasses the following titania-coated silver-containing compositions:

[0006] Section 1. 1. A titania-coated silver composition comprising: (A) titania-coated silver; (B) a Si compound; (C) a solvent; The titania-coated silver (A) is a silver (Ag) fine particle having a part of its surface coated with titania, The (B) Si compound is a hydrolysis product of an alkoxysilane. Titania-coated silver compositions.

[0007] Section 2. 2. The titania-coated silver composition according to claim 1, wherein 1% to 99% of the surface of the silver fine particles in the titania-coated silver (A) is coated with titania.

[0008] Section 3. Item 2. The oxide composite according to item 1, wherein the (B) inorganic oxide fine particles covering the (A) silver fine particles have a random ratio of 50% or more.

[0009] Section 4. 2. The titania-coated silver composition according to claim 1, wherein the titanium (Ti) compound contained in the titania-coated silver (A) exhibits a mass loss of 1% by mass or more at 200°C or higher when the Ti compound is heated to 600°C using a simultaneous differential thermogravimetry and thermomechanical analyzer.

[0010] Section 5. 2. The titania-coated silver composition according to item 1, wherein the Ti compound contained in the titania-coated silver (A) has an average primary particle size of 1 nm to 20 nm.

[0011] Section 6. 2. The titania-coated silver composition according to item 1, wherein the Ag compound contained in the titania-coated silver (A) has an average primary particle size of 1 nm to 2,000 nm.

[0012] Section 7. The ratio of the average primary particle size of the Ag compound to the average primary particle size of the Ti compound contained in the titania-coated silver (A) (Average primary particle size of Ag compound / Average primary particle size of Ti compound) 2 to 100.

[0013] Section 8. In the titania-coated silver composition, 2. The titania-coated silver composition according to item 1, wherein the Ti compound contained in the titania-coated silver (A) is 0.01% by mass to 5% by mass.

[0014] Section 9. In the titania-coated silver composition, 2. The titania-coated silver composition according to item 1, wherein the (B) Si compound is contained in an amount of 0.01% by mass to 20% by mass.

[0015] Section 10. 2. The titania-coated silver composition according to claim 1, wherein the (C) solvent comprises water and an alcohol.

[0016] Section 11. 2. The titania-coated silver composition according to Item 1, wherein the (B) Si compound is a hydrolysis product of tetraethyl orthosilicate (TEOS, tetraethoxysilane).

[0017] Section 12. 12. An antibacterial and antiviral coating solution comprising the titania-coated silver composition according to any one of items 1 to 11.

[0018] Section 13. 1. A method for producing a titania-coated silver composition, comprising: (1) A step of synthesizing a Ti compound in a solvent and providing an organic chain to the Ti compound (2) after step (1), a step of preparing titania-coated silver; and (3) After the step (2), a step of mixing the titania-coated silver having an organic chain bonded thereto with a silicon compound in a solvent to hydrolyze the silicon compound. A method for producing a titania-coated silver composition comprising:

[0019] The method for producing the titania-coated silver composition of the present invention preferably comprises the steps of: (4) After the step (3), a high-pressure dispersion treatment is carried out to disperse the dispersion containing the titania-coated silver.

[0020] Titania-coated silver is silver (Ag) fine particles whose surfaces are partially coated with titania.

[0021] The titania-coated silver-containing composition of the present invention can improve adhesion to a substrate by mixing the titania-coated silver with a binder. The titania-coated silver-containing composition of the present invention is a material that combines transparency, adhesion to a substrate, durability, antibacterial and antiviral properties (antibacterial agent), long-term stability, etc., by hydrolyzing alkoxysilane in the presence of titania-coated silver. Effect of the Invention

[0022] The present invention makes it possible to provide a titania-coated silver-containing composition that combines transparency, adhesion to a substrate, durability, antibacterial and antiviral properties, and long-term stability. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0023] The present invention will be described in detail below.

[0024] The embodiments of the present invention are intended to provide a better understanding of the gist of the invention, and unless otherwise specified, do not limit the content of the invention.

[0025] In this specification, the terms "comprise" and "containing" are concepts which encompass all of "comprise," "consist essentially of," and "consist only of."

[0026] In this specification, when a numerical range is indicated as "A to B," it means "A or more and B or less."

[0027] In this specification, the designations parts, % etc. are generally used.

[0028] In this specification, unless otherwise specified, all parts by mass or % by mass (wt%) are used.

[0029] [1] Titania-coated silver-containing composition Conventionally, organic antibacterial agents have been highly effective immediately, but their effectiveness does not last for a long time. Inorganic antibacterial agents have been effective for a long time, but they are colored, have low transparency, and have low performance. Further study is needed.

[0030] Conventionally, silver nanoparticles have been shown to have high antibacterial and antiviral properties, but they have also been found to have low stability and tend to aggregate or caking easily, and further study is needed.

[0031] Prior art (Patent Document 1) discloses a technique for preventing caking of antibacterial liquid by supporting silver on an inorganic oxide and further compounding it with a binder having a siloxane bond. The method of supporting silver on an inorganic oxide requires that the silver be supported on a support (inorganic oxide) that is larger in size than the silver, and stabilized. Conventionally, when the particle size of the support is large, the transparency of the antibacterial liquid decreases. Thus, there is a trade-off between stably supporting silver on a support in the antibacterial liquid and the transparency of the antibacterial liquid, and a material that can achieve both is needed.

[0032] The inventors changed their approach from the conventional method of supporting silver on a support and succeeded in minimizing the aggregation of silver in a composition (such as an antibacterial solution) by partially covering the silver with titania particles that are sufficiently smaller than silver.

[0033] The present invention relates to a structure in which titania is supported around silver particles, that is, a structure in which titania coats the periphery of silver particles. The titania-coated silver-containing composition of the present invention contains a composite of fine titania-coated silver particles, and is a material that has high transparency, has little silver aggregation, and can stably exhibit antiviral properties.

[0034] The titania-coated silver-containing composition of the present invention can improve adhesion to a substrate by mixing the titania-coated silver with a binder. The titania-coated silver-containing composition of the present invention is a material that combines transparency, adhesion to a substrate, durability, antibacterial and antiviral properties (antibacterial agent), long-term stability, etc., by hydrolyzing alkoxysilane in the presence of titania-coated silver.

[0035] The present invention is a water-repellent coating material that is excellent in transparency, adhesion to substrates, solvent stability, etc., by using titanium oxide having organic chains on the surface and undergoing a sol-gel reaction with a silicon binder. By using the water-repellent coating material of the present invention as a coating material, it is possible to satisfactorily fix photocatalytic titanium oxide to a substrate, and form a coating layer on an article.

[0036] The titania-coated silver-containing composition of the present invention comprises: (A) titania-coated silver; (B) a Si compound; (C) a solvent; The titania-coated silver (A) is a silver (Ag) fine particle having a part of its surface coated with titania, The (B) Si compound is a hydrolysis product of an alkoxysilane.

[0037] (1-1)(A) Titania-coated silver The titania-coated silver composition of the present invention contains (A) titania-coated silver, (B) a Si compound, and (C) a solvent, and in (A) titania-coated silver, a part of the surface of silver (Ag) fine particles is coated with titania. (A) titania-coated silver has a structure in which a titania compound is supported around silver fine particles (carrier), or a structure in which titania coats around silver fine particles (carrier). Water, inorganic acids, free organic acids, etc. generally evaporate at temperatures below 200°C.

[0038] (A) Titania compound (titania nanoparticles) of titania-coated silver has acetyl groups (CH3-C(=O)-, Ac), acetoxy groups (acetyloxy group, CH3-C(=O)-O-, AcO) and the like bonded to at least some of the titanium atoms present on the surface, which are gradually eliminated in the range of 200°C to 600°C. For example, in the case of acetoxy groups, they are gradually eliminated in the range of 200°C to 600°C, reaching a peak at about 260°C.

[0039] Titania compounds can improve the dispersibility of titania particles by adding an organic substance to the fine titania surface.

[0040] The titania compound preferably has an organic chain such as an acetyl group or an acetoxy group bonded to at least some of the titanium atoms present on the surface, and can suppress aggregation of titania nanoparticles during drying or firing, so that cracks, peeling, etc. do not easily occur, and the coating property and transparency are particularly excellent. The titania compound can suppress cracks, peeling, etc., and can easily support metals firmly, so that it also has excellent visible light catalytic activity.

[0041] The titania compound is particularly effective in preventing cracks, peeling, etc., since it can prevent the titania nanoparticles from agglomerating together during drying or firing.

[0042] In titania compounds, when at least some of the titanium atoms present on the surface have organic chains such as acetyl groups or acetoxy groups, these are gradually released in the range of 200°C to 600°C. Therefore, when the temperature is increased using a thermogravimetric and differential thermal analyzer (TG-DTA), the mass loss is large at temperatures above 200°C.

[0043] When titania compounds are heated using a thermogravimetry-differential thermal analyzer (TG-DTA), the mass loss at temperatures above 200°C indicates the number of organic chains, such as acetyl groups and acetoxy groups, that are bonded to titanium atoms on the surface.

[0044] In the titania-coated silver composition of the present invention, the titanium (Ti) compound contained in the titania-coated silver (A) preferably has a mass loss of 1% by mass or more at 200°C or higher when the Ti compound is heated to 600°C using a thermogravimetry-differential thermal analyzer. The mass loss of the Ti compound at 200°C or higher when the Ti compound is heated to 600°C using a thermogravimetry-differential thermal analyzer (TG-DTA) is 0.1% by mass or more, preferably 1% by mass or more, and more preferably 5% by mass or more. The upper limit of the mass loss of the Ti compound is preferably 20% by mass.

[0045] The detailed conditions for the thermogravimetry-differential thermal analyzer (TG-DTA) were as follows: atmosphere: air, heating rate: 3° C. / min.

[0046] The organic chain (acetyl group, acetoxy group, etc.) present on the surface of the Ti compound is preferably an acetyl group (CH3-C(=O)-), an acetoxy group (CH3-C(=O)-O-), etc., from the viewpoints of water solubility, odor, volatility, harmfulness, decomposability, etc.

[0047] The organic chain may be at least one type of organic chain selected from the group consisting of the above organic chains, and one type of organic chain may be bonded alone, or two or more types of organic chains may be bonded depending on the purpose.

[0048] In the titania-coated silver composition of the present invention, the Ti compound contained in the titania-coated silver (A) preferably has an average primary particle diameter of 1 nm to 20 nm. The average primary particle diameter of the Ti compound is preferably 1 nm to 50 nm, more preferably 1 nm to 20 nm, and even more preferably 1 nm to 10 nm. By adjusting the average particle diameter of the Ti compound to this range, it becomes possible to partially coat the periphery of silver with Ti. The titania nanoparticles can form a film having higher visible light catalytic activity and higher transparency. The Ti compound has excellent coating properties.

[0049] The average particle size of the Ti compound (titania nanoparticles) is measured by observation with a transmission electron microscope (TEM).

[0050] The specific surface area of ​​the Ti compound is preferably 150 m 2 / g~500m 2 / g, more preferably 200m 2 / g~400m 2 / g. By adjusting the specific surface area of ​​the Ti compound to this range, it is possible to partially coat the Ti compound with metal (silver and copper) and Ti around the silver to an appropriate extent. The Ti compound has high visible light catalytic activity.

[0051] The specific surface area of ​​the Ti compound is measured by the BET method.

[0052] The Ti compound can have the N, Cl, and S element concentrations of 0 to 5,000 ppm, and more preferably 0 to 1,000 ppm. By adjusting the N, Cl, and S element concentrations of the Ti compound to within this range, corrosion of the substrate can be suppressed. The N, Cl, and S element concentrations of the Ti compound mean that there is no impurity derived from the acidic Ti compound precursor such as TiCl4 or TiOSO4, or there are only a very small amount of impurities.

[0053] The concentrations of N, Cl, and S elements in the Ti compound are measured by WDX (fluorescent X-ray).

[0054] The crystalline form of the Ti compound is preferably anatase type, and the titania nanoparticles are preferably 100% anatase type, not including any crystalline form other than anatase type. By adopting anatase type Ti compound, the visible light catalytic activity of the Ti compound is improved.

[0055] In the titania-coated silver composition of the present invention, the Ag compound contained in the titania-coated silver (A) preferably has an average primary particle size of 1 nm to 2,000 nm.

[0056] Definition of partial cover The titania-coated silver is imaged using an electron microscope (scanning electron microscope (SEM) or transmission electron microscope (TEM)), and the locations of the Ag and Ti particles are clarified by elemental analysis (energy dispersive X-ray analysis (EDS), electron probe microanalyzer (EPMA), electron energy loss spectroscopy (EELS), etc.). After that, 10 Ag particles are randomly selected and arranged in order of particle size. The 5th and 6th smallest Ag nanoparticles are then focused on and binarized using image processing software such as the image analysis software WinROOF (Mitani Shoji Co., Ltd.).

[0057] (A) Particle size ratio α(Ag) / β(Ti) The particle diameter of the Ag particles is α (nm) and the particle diameter of the Ti particles is β (nm). Based on this, α / β is calculated. α / β is preferably 1 / 2 or more.

[0058] By adjusting α(Ag particles) / β(Ti particles) to 1 / 2 or more (silver nanoparticles are relatively large), the transparency of the dispersion containing titania-coated silver can be well maintained. α(Ag) / β(Ti) is more preferably adjusted to 1 to 1,000, and even more preferably adjusted to 1 to 100.

[0059] (B) Coverage of Ag particles As a result of this binarization process, the area of ​​the Ag particle domain is defined as A, and the area of ​​the Ti particle domain that overlaps with the Ag nanoparticle is defined as B. Based on this result, the coverage rate is defined as B (Ti particle) / A (Ag particle) x 100 (%).

[0060] When the Ag particles are completely covered by the Ti particles, the coverage rate is 100%.

[0061] When an Ag particle exists alone, the coverage rate is 0%, and the Ag particle is not covered by the Ti particle.

[0062] In the titania-coated silver composition of the present invention, the titania-coated silver (A) is preferably such that 1% to 99% of the surface of the silver fine particles is coated with titania. The titania-coated silver has a coating rate of preferably 1% to 99%, more preferably 10% to 80%, and even more preferably 20% to 70%. By adjusting the coating rate of titania within the above range, the titania-coated silver exhibits good antibacterial and antiviral activity, and a dispersion containing the titania-coated silver has good dispersion stability.

[0063] When the coverage value of titania-coated silver exceeds 99%, the exposure rate of Ag particles decreases, and antiviral performance may decrease. When the coverage value of titania-coated silver is less than 1%, the stability of Ag particles in titania-coated silver or in dispersion may decrease. By adjusting the coverage rate (B (Ti particles) / A (Ag particles)×100(%)) to 1 surface% to 99 surface%, titania-coated silver can partially coat the surface of Ag particles, improving antiviral performance and providing good stability of dispersion containing titania-coated silver.

[0064] (C) Random ratio of Ag particles The random ratio of Ag particles is defined as follows:

[0065] As a result of binarization processing using image processing software (WinROOF), the coordinate positions of Ag particles are defined as follows: AgXmax (maximum value of the X coordinate of Ag particles) AgXmin (minimum value of the X coordinate of an Ag particle) AgYmax (maximum Y coordinate of Ag particles) AgYmin (minimum value of Y coordinate of Ag particle)

[0066] Next, N inorganic oxide particles are extracted from the inorganic oxide particles by measuring the shape characteristics of the inorganic oxide particles using WinROOF. The n-th inorganic oxide particle is defined as On when the inorganic oxide particles are arbitrarily assigned numbers 1, 2, 3, and so on. For On, the coordinate position is defined as follows: Onx (X coordinate of the center of gravity of the nth inorganic oxide particle) Ony (Y coordinate of the center of gravity of the nth inorganic oxide particle)

[0067] Next, the region of the Ag particle is divided as follows: AgX1=AgXmin (first X coordinate) AgXm+1=AgXm+(AgXmax-AgXmin) / N (m+1th X coordinate) AgY1=AgYmin (first Y coordinate) AgYm+1=AgYm+(AgYmax-AgYmin) / N (m+1th Y coordinate)

[0068] The number of inorganic oxide particles in each of the divided regions and the maximum value thereof are defined as follows. The number of Onx contained within the coordinates of AgXm and AgXm+1 is defined as NOmx. Furthermore, the maximum value of NOmx is defined as NOxmax. The number of Ony contained within the coordinates of AgYm and AgYm+1 is defined as NOmy. Furthermore, the maximum value of NOmx is defined as NOymax.

[0069] The random rate in the X-axis direction (Ranx) and the random rate in the Y-axis direction (Rany) are as follows: Ranx = (1-NOxmax / N) x 100 Rany = (1-NOymax / N) x 100

[0070] This allows the measurement of the randomness (Ranx, Rany). Each of the randomness Ranx and Rany is preferably 50% or more, more preferably 70% or more, and even more preferably 90% or more. In the titania-coated silver composition of the present invention, a high randomness means that the number of Ti particles coated on the Ag particles is large and that they are well-dispersed.

[0071] By adjusting the random ratios Ranx and Rany, the titania-coated silver composition of the present invention makes it possible to efficiently expose Ag particles while increasing the dispersibility of the Ag particles, thereby improving the dispersion stability and antiviral activity of the Ag particles and preventing the elution of Ag from inorganic oxide microparticles.

[0072] (1-2)(B)Si compound (Si binder) The titania-coated silver composition of the present invention contains (A) titania-coated silver, (B) a Si compound, and (C) a solvent, and (B) the Si compound is a hydrolysis product of an alkoxysilane.

[0073] The titania-coated silver composition of the present invention contains a Ti compound (titania particles), and by applying an organic substance to the fine titania surface, the dispersibility of the titania particles can be improved.

[0074] By mixing Ti compounds (titania particles) with alkoxysilanes (Si compounds), which are the raw materials for the binder, and allowing the two to coexist while maintaining high dispersibility, a titania particle composite binder can be produced.

[0075] The titania-coated silver composition of the present invention can improve the cohesion of titania, and can greatly improve the solvent stability and adhesion.

[0076] (B) The Si compound is a hydrolysis product of an alkoxysilane (alkylsilane).

[0077] As the alkoxysilane (alkylsilane), preferably, monoalkoxysilane, dialkoxysilane, trialkoxysilane, tetraethoxysilane, or the like is used.

[0078] As the monoalkoxysilane, trimethylmethoxysilane, trimethylethoxysilane, or the like is preferably used.

[0079] As the dialkoxysilane, preferably dimethyldimethoxysilane, dimethyldiethoxysilane, dimethyldiethoxysilane, diethyldiethoxysilane, diisobutyldimethoxysilane, dimethoxymethyl-n-octylsilane, or the like is used, and more preferably dimethyldimethoxysilane, dimethyldiethoxysilane, or the like is used.

[0080] The trialkoxysilane is preferably methyltrimethoxysilane, methyltriethoxysilane, methyltrippropoxysilane, methyltriisopropoxysilane, ethyltrimethoxysilane, ethyltriethoxysilane, ethyltrippropoxysilane, ethyltriisopropoxysilane, n-propyltrimethoxysilane, n-propyltriethoxysilane, n-propyltrippropoxysilane, n-propyltriisopropoxysilane, isopropyltrimethoxysilane, isopropyltrimethoxysilane, isopropyltrimethoxysilane, isopropyl Tripropoxysilane, n-butyltriethoxysilane, isobutyltrimethoxysilane, isobutyltriethoxysilane, n-hexyltrimethoxysilane, n-hexyltriethoxysilane, n-octyltriethoxysilane, allyltrimethoxysilane, allyltriethoxysilane, etc. are used, and more preferably methyltrimethoxysilane, methyltriethoxysilane, n-propyltrimethoxysilane, n-propyltriethoxysilane, n-hexyltrimethoxysilane, n-hexyltriethoxysilane, etc. are used.

[0081] The tetraalkoxysilane is preferably tetramethoxysilane, tetraethoxysilane, tetrapropoxysilane, or the like, and more preferably tetraethoxysilane (tetraethyl orthosilicate, Si(OC2H5)4, TEOS), tetramethoxysilane, or the like.

[0082] The alkylsilane may be at least one compound selected from the group consisting of the above alkylsilanes. These alkylsilanes may be used alone or in combination (blended) in two or more types depending on the purpose.

[0083] In the titania-coated silver composition of the present invention, the Si compound is particularly preferably a hydrolysis product of TEOS (tetraethyl orthosilicate, tetraethoxysilane).

[0084] (1-3)(C) Solvent The titania-coated silver composition of the present invention contains (A) titania-coated silver, (B) a Si compound, and (C) a solvent.

[0085] In the titania-coated silver composition of the present invention, the (C) solvent preferably contains water and an alcohol.

[0086] The alcohol is preferably an aliphatic alcohol having 1 to 6 carbon atoms, such as methanol, ethanol, propanol, or isopropanol; a non-aliphatic alcohol, such as α-terpineol; a glycol solvent, such as butyl carbitol (diethylene glycol monobutyl ether), hexylene glycol (2-methyl-2,4-pentanediol), ethylene glycol-2-ethylhexyl ether, ethylene glycol monomethyl ether, or propylene glycol monomethyl ether; or a diol, such as 1,4-butanediol, 1,5-pentanediol, or 1,6-hexanediol.

[0087] The alcohol may be at least one compound selected from the group consisting of the above alcohols. These alcohols may be used alone or in combination (blend) of two or more depending on the purpose.

[0088] In the titania-coated silver-containing composition of the present invention, the solvent can be changed. The titania-coated silver-containing composition may be centrifuged, filtered, or the like to remove water from the reaction solution and replace it with an organic solvent.

[0089] (1-4) Titania-coated silver composition In the titania-coated silver composition of the present invention, the ratio of the average primary particle size of the Ag compound to the average primary particle size of the Ti compound contained in the titania-coated silver (A) (average primary particle size of Ag compound / average primary particle size of Ti compound) is preferably 2 to 100.

[0090] In the titania-coated silver composition, the content of the Ti compound contained in the titania-coated silver (A) is preferably 0.01% by mass to 5% by mass.

[0091] In the titania-coated silver composition, the content of the (B) Si compound is preferably 0.01% by mass to 20% by mass.

[0092] (1-5) Antibacterial and antiviral coating liquids (dispersions), paints, and coating films In the titania-coated silver composition of the present invention, the Ti compound (titania particles) can improve the dispersibility of the titania particles by adding an organic substance to the fine titania surface. The Ti compound (titania particles) and alkoxysilane (Si compound), which is the raw material of the binder, are mixed, and the coexistence of both is performed to carry out a hydrolysis reaction while maintaining high dispersibility, thereby producing a titania particle composite binder.

[0093] The titania-coated silver composition of the present invention can improve titania aggregation, and can greatly improve the solvent stability of paint and the adhesion of the coating film. The titania-coated silver composition of the present invention has good dispersibility, and therefore has excellent crack resistance of the coating. The titania-coated silver composition of the present invention can also coat dense titania, and has excellent coatability and transparency, as well as excellent visible light catalytic activity.

[0094] In the titania-coated silver composition of the present invention, the content of the Ti compound is preferably 0.01% by mass to 5% by mass in the composition from the viewpoints of ease of coating, film properties of the coating, and the like.

[0095] In the titania-coated silver composition of the present invention, the content of the Si compound is preferably 0.01% by mass to 20% by mass in the composition from the viewpoints of ease of coating, film properties of the coating, and the like.

[0096] In the titania-coated silver composition of the present invention, from the viewpoints of ease of coating, film properties of the coating, and the like, the content ratio of the Ti compound to the Si compound is preferably 0.02 to 20 (0.02 parts by mass to 20 parts by mass) by mass, and more preferably 0.1 to 1 (0.1 parts by mass to 1 part by mass) by mass.

[0097] The pH of the titania-coated silver composition (dispersion) of the present invention varies depending on the type of metal added and the amount of the metal added, and is preferably 1 to 5, more preferably 2 to 4, from the viewpoint of coatability.

[0098] The present invention encompasses an antibacterial and antiviral coating solution containing the titania-coated silver composition of the present invention, and a paint containing the antibacterial and antiviral coating solution of the present invention.

[0099] The dispersion liquid of the titania-coated silver composition of the present invention is preferably adjusted in viscosity according to the application to prepare a coating material. When the coating material is applied by spin coating, dip coating, spraying, etc., the viscosity is preferably adjusted to be low. When the coating material is applied by brush coating, squeegee method, etc., the viscosity is preferably adjusted to be higher. When the coating material is applied by screen printing, the viscosity is preferably adjusted to be even higher to suppress flowability.

[0100] The coating film formed by the paint containing the antibacterial and antiviral coating liquid of the present invention enables a dense coating.

[0101] The present invention includes an antibacterial and antiviral coating film (coating film) formed by a paint containing the antibacterial and antiviral coating liquid of the present invention.

[0102] The coated product having a coating film is not particularly limited, and examples thereof include building materials, building exteriors, building interiors, window frames, window glass, various lenses, structural members, building facilities such as housing, cooking utensils, textile products, furniture, displays, display protective films, plumbing members, vehicle lighting covers and window glass, mechanical equipment or exteriors of articles, dustproof covers and coatings, display devices, their covers, traffic signs, various display devices, display objects such as billboards, sound insulation walls for roads and railways, exteriors and coatings of bridges and guardrails, interiors and coatings of tunnels, insulators, solar cell covers, solar hot water heater heat collector covers, and other exterior parts of electronic and electrical devices used outside, particularly transparent members, exteriors of vinyl greenhouses, greenhouses, and the like.

[0103] [2] Method for producing titania-coated silver composition The method for producing the titania-coated silver composition of the present invention comprises the steps of: (1) synthesizing a Ti compound in a solvent and providing an organic chain to the Ti compound; (2) after step (1), a step of preparing titania-coated silver; and (3) After the step (2), the method includes a step of mixing the titania-coated silver having an organic chain bonded thereto with a Si compound in a solvent to hydrolyze the Si compound.

[0104] The method for producing the titania-coated silver composition of the present invention preferably comprises the steps of: (4) After the step (3), a high-pressure dispersion treatment is carried out to disperse the dispersion containing the titania-coated silver.

[0105] Titania-coated silver is silver (Ag) fine particles whose surfaces are partially coated with titania.

[0106] (2-1)(1) A step of synthesizing a Ti compound in a solvent and providing an organic chain to the Ti compound In the production method of the present invention, first, an organic substance is applied to the surface of fine titania particles to improve the dispersibility of the titania particles.

[0107] In step (1), an organic chain is bonded to the surface of a Ti compound in a solvent.

[0108] The Ti compound (substance containing titanium) is preferably a substance that becomes titanium oxide when heated. The substance containing titanium is preferably titanium oxide and / or a titanium oxide precursor, and more preferably titanium oxide; titanium hydroxide; titanium alkoxide; titanium halide such as titanium trichloride or titanium tetrachloride (particularly, those neutralized with a base); metallic titanium, etc. are used.

[0109] From the viewpoints of dispersibility, coatability, and visible light catalysis of the resulting titania, the titanium-containing substance is preferably titanium alkoxide, titanium hydroxide, or titanium halide (particularly, one neutralized with a base). From the viewpoints of purity, dispersibility, coatability, transparency, and visible light catalysis, the titanium-containing substance is more preferably titanium alkoxide.

[0110] The titanium alkoxide is preferably titanium tetraisopropoxide, titanium tetra n-butoxide, titanium tetra n-propoxide, titanium tetraethoxide, etc. From the viewpoints of cost, water solubility of by-products, coatability, and visible light catalytic property, the titanium alkoxide is more preferably titanium tetraisopropoxide.

[0111] The Ti compound may be at least one compound selected from the group consisting of the Ti compounds described above. These Ti compounds may be used alone or in combination (blend) of two or more types depending on the purpose.

[0112] The average particle size of the Ti compound is preferably 100 nm or less, more preferably 50 nm or less. The lower limit of the average particle size of the titanium-containing substance is not particularly set, and is preferably about 1 nm. When the particle size is large, it is preferable to use a planetary ball mill, a paint shaker, or the like, after grinding in a dry or wet manner.

[0113] The average particle size of Ti compounds (solids such as titanium oxide and metallic titanium) is measured by observation with a transmission electron microscope (TEM).

[0114] The concentration of the Ti compound in the dispersion is preferably 0.01 mol / L to 5 mol / L, and more preferably 0.05 mol / L to 3 mol / L, from the viewpoints of productivity, viscosity of the reaction liquid, coatability, transparency, and visible light catalytic properties.

[0115] The acid used in the reaction is an organic acid, and since it is preferable that it is a volatile acid, it is preferably an acid represented by the chemical formula C n H 2n+1 Monocarboxylic acids represented by COOH (n=0 to 3) (monocarboxylic acids having 1 to 4 carbon atoms), hydroxycarboxylic acids having 2 to 3 carbon atoms, etc. are used.

[0116] The monocarboxylic acid is preferably formic acid (n=0) or acetic acid (n=1) from the viewpoints of volatility, toxicity and decomposability.

[0117] The hydroxycarboxylic acid is preferably glycolic acid, lactic acid, etc., and from the viewpoints of water solubility and odor, more preferably acetic acid, glycolic acid, lactic acid, etc.

[0118] The organic acid may be at least one compound selected from the group consisting of the above organic acids. These organic acids may be used alone or in combination (blend) of two or more depending on the purpose.

[0119] The amount of organic acid used is adjusted so that the number of moles of acyloxy groups is preferably 1.5 moles or more, particularly preferably 2 moles or more, per mole of titanium in the Ti compound, from the viewpoints of dispersibility, coatability, transparency, visible light catalysis, and cost. The amount of organic acid used can improve stability over time, coatability, transparency, etc., as the organic acid is used in larger amounts. The upper limit of the amount of organic acid used is not particularly limited, and is preferably adjusted so that the number of moles of acyloxy groups is 10 moles or less per mole of titanium in the Ti compound.

[0120] The concentration of the organic acid in the dispersion is preferably 0.02 mol / L to 10 mol / L, and more preferably 0.1 mol / L to 7 mol / L, from the viewpoints of dispersibility, coatability, transparency, visible light catalytic properties, and cost.

[0121] The reaction solvent is preferably an aqueous solvent such as water, the main component being preferably 50% by mass or more. The reaction solvent may contain an alcohol or an ester during the reaction.

[0122] When titanium tetraisopropoxide is used as a raw material, the reaction solvent generates isopropyl alcohol by reaction with an organic acid. Heating may generate an isopropyl ester of the organic acid. The alcohol or ester may be added to the dispersion liquid, or may be generated in the system. The alcohol or ester may be removed by heating in an open system below 100°C, may be removed by reducing pressure, or may remain in the reaction liquid.

[0123] When alcohol is contained in the dispersion liquid, the average particle size of the obtained Ti compound (titania nanoparticles) tends to become small, and therefore alcohol may be intentionally added in order to control the average particle size.

[0124] The pH of the dispersion is preferably 2 or more and less than 6, and more preferably 2.1 to 5, from the viewpoints of corrosion of the apparatus, safety in handling, dispersibility, and the like.

[0125] The method for preparing the dispersion is not particularly limited, and the Ti compound, organic acid, and water (solvent) may be mixed simultaneously or sequentially. In mass production scale, from the viewpoint of preventing aggregation and forming large lumps and facilitating continued stirring, it is preferable to mix the organic acid and water (solvent) and then add the titanium-containing substance while stirring. In laboratory scale, it is preferable to mix the titanium-containing substance and organic acid and then add water while stirring.

[0126] (2-2)(2) After step (1), a step of preparing titania-coated silver Titania-coated silver can be produced by irradiating a composite of a titanium compound and a silver compound with ultraviolet light.

[0127] High pressure dispersion method (pressure treatment) It is desirable to carry out the dispersion treatment of Ti compounds (titania compounds) using a dispersion device that generates high pressure by collision between particles, for example, a jet mill, etc., which can highly disperse titania particles in a liquid, making it possible to partially coat titania.

[0128] A dispersion liquid containing a Ti compound (preferably titania fine particles) is subjected to a pressure treatment of 30 MPa or more (high pressure dispersion method).

[0129] The pressure treatment causes the Ti compound to become finer.

[0130] The pressure level when carrying out the pressure treatment is not particularly limited as long as it can sufficiently atomize the Ti compound. The pressure level is preferably adjusted to 30 MPa or more, more preferably adjusted to 50 MPa to 400 MPa, and further preferably adjusted to 100 MPa to 300 MPa. The pressure treatment is preferably carried out using a high-pressure dispersion device. The high-pressure dispersion device can disperse the Ti compound by applying a mechanical pressure.

[0131] Depending on the pressure, for example, (i) Colliding two or more dispersions of Ti compounds with each other; (ii) Collision of a material dispersion of a Ti compound with a metal or ceramic material (a material having high hardness such as silicon carbide or alumina); (iii) Disperse the Ti compound in a cross-sectional area of ​​1 cm 2 Passing through the following spaces The following processing is performed:

[0132] By applying pressure, it is possible to make the pressure conditions stronger, which makes it possible to more efficiently atomize the Ti compound and further reduce the processing time.

[0133] The pressurization operation is preferably carried out once or more, and more preferably, ten or more times.

[0134] The pressurizing temperature is not particularly limited. The pressurizing temperature is adjusted to a temperature at which the carbonaceous material having a layered structure can be sufficiently exfoliated. The pressurizing temperatures of (i) and (ii) are preferably adjusted to 0°C to 100°C, more preferably 20°C to 95°C. The pressurizing temperature of (iii) is preferably adjusted to 0°C to 100°C when pressure is applied mechanically. The pressurizing temperature of (iii) is preferably adjusted to 373°C to 700°C, more preferably 380°C to 450°C when pressure is generated by the supercritical state of water.

[0135] When the pressure treatment is carried out, it is preferable to carry out ultrasonic dispersion treatment on the dispersion liquid containing the Ti compound as a preliminary treatment (pretreatment) to atomize the Ti compound, which can have the effect of preventing clogging in a high-pressure dispersion device, a supercritical water production device, etc.

[0136] The output of the ultrasonic dispersion treatment is not particularly limited. From the viewpoint of atomization of the Ti compound, the output of the ultrasonic dispersion treatment is preferably adjusted to be stronger than that of the normally performed ultrasonic dispersion treatment (about 40W to 50W). The output of the ultrasonic dispersion treatment is preferably adjusted to 100W or more, more preferably adjusted to 300W to 20,000W, and even more preferably adjusted to 400W to 18,000W.

[0137] The ultrasonic dispersion temperature is not particularly limited. The ultrasonic dispersion temperature is preferably adjusted to a temperature at which the Ti compound can be sufficiently atomized. The ultrasonic dispersion temperature is preferably adjusted to 0°C to 80°C, more preferably 10°C to 70°C.

[0138] The ultrasonic dispersion time is not particularly limited. The ultrasonic dispersion time is preferably adjusted to a time that can sufficiently atomize the Ti compound. The ultrasonic dispersion time is preferably adjusted to 1 to 600 minutes, more preferably 3 to 120 minutes.

[0139] As a pre-treatment or post-treatment of these treatments, dispersion treatments using other dispersion devices such as ordinary mechanical stirring, dispersion treatments using an emulsifying device, and dispersion treatments using a bead mill may be used in combination.

[0140] UV light irradiation The ultraviolet light irradiation is preferably performed at a temperature lower than room temperature (20°C), more preferably at 15°C or lower, from the viewpoints of ease of supporting silver on Ti compound (titania nanoparticles), visible light catalytic activity, reaction rate, productivity, controllability of aspect ratio, discoloration resistance when irradiated with low-intensity ultraviolet light, visibility when irradiated with high-intensity ultraviolet light, and re-transparency in an ultraviolet light-stopped environment. The lower limit of the temperature of the ultraviolet light irradiation is not particularly limited, and is preferably 0°C when reacting at normal pressure. During ultraviolet light irradiation, the dispersion is preferably stirred from the viewpoint of sufficiently reacting the silver salt. The stirring method is not particularly limited, and can be performed according to a conventional method.

[0141] The reaction time of the ultraviolet light irradiation is preferably 1.5 hours or more, and more preferably in the range of 1.5 hours to 36 hours. By adjusting the reaction time to 1.5 hours or more, inorganic oxide fine particles are favorably supported around the silver nanoparticles, and gelation of the silver nanoparticles does not occur. By adjusting the reaction time to 36 hours or less, the particle size of the silver nanoparticles is adjusted, and precipitation of the silver nanoparticles does not occur.

[0142] From the viewpoints of ease of support, reaction rate, reaction controllability and productivity, an ultraviolet irradiation device is preferably used that includes a wavelength of 280 nm to 500 nm. By adjusting the wavelength of the ultraviolet light to a wavelength range of 280 nm or more, the dispersion stability of the titania-coated silver is good. By adjusting the wavelength of the ultraviolet light to a wavelength range of 500 nm or less, silver is reduced well and silver nanoparticles are generated well.

[0143] The composition of the present invention preferably further contains at least one metal selected from the group consisting of silver, copper, and platinum.

[0144] When a silver salt is used as the silver compound, the silver salt is preferably a silver salt whose aqueous solution is acidic or neutral. The silver salt is preferably silver chloride (I), silver nitrate (I), organic acid silver (silver lactate (I), silver acetate (I), silver citrate (I), silver myristate (I), etc.), silver sulfide (I), silver oxide (I), silver phosphate (I), silver carbonate (I), silver bromide (I), silver iodide (I), etc. The silver salt may be at least one compound selected from the group consisting of the above silver salts, and these silver salts may be used alone or in a mixture (blend) of two or more types depending on the purpose.

[0145] The amount of the silver salt used is preferably 50% by mass or less, more preferably 0.01% by mass to 40% by mass, and even more preferably 0.01% by mass to 25% by mass, calculated as the mass of silver element in the silver salt, based on the titanium oxide in the Ti compound (titania nanoparticles) from the viewpoints of dispersibility, transparency, antimicrobial activity (antibacterial activity and antiviral activity), stability of the Ti compound (titania nanoparticles), etc. By adjusting the amount of the silver salt used within this range, it is easy to maintain the coatability and transparency, and antibacterial activity, antiviral activity in a dark place, and photocatalytic activity can be particularly improved.

[0146] Titania-coated silver can be recovered by conventional methods such as precipitating and centrifuging the titania-coated silver. The organic chains are bonded to titanium atoms present on the surface, and (A) titania-coated silver has a structure in which a titania compound is supported around silver particles (carrier), or a structure in which titania coats the periphery of silver particles (carrier).

[0147] (2-3)(3) After step (2), a step of mixing titania-coated silver having an organic chain bonded thereto with a Si compound in a solvent to hydrolyze the Si compound. In step (3), the titania-coated silver having organic chains bonded thereto is mixed with a Si compound in a solvent to hydrolyze the Si compound (preparation of a coating liquid).

[0148] In the manufacturing method of the present invention, next, the titania particles are mixed with alkoxysilane, which is a raw material for the binder, and a hydrolysis reaction is carried out in the coexistence of the two while maintaining high dispersibility, to produce a titania particle composite binder.

[0149] The hydrolysis is preferably carried out by keeping the dispersion at about 65° C. for about 15 hours with a lid on to prevent the solvent from volatilizing.

[0150] The hydrolysis is preferably carried out under normal pressure or under pressure in a closed vessel.

[0151] The pH of the dispersion is preferably 2 or more and less than 6, and more preferably 2.1 to 5, from the viewpoints of corrosion of the apparatus, safety in handling, dispersibility, and the like.

[0152] The organic matter (acetyl groups, acetoxy groups, etc.) bonded to the surface of the Ti compound (titania) in the titania-coated silver reacts with the Si compound (alkylsilane such as TEOS), and the hydrolysis of the Si compound progresses (hydrolyzate of alkylsilane), resulting in a transparent coating liquid.

[0153] (2-4)(4) After step (3), a step of performing a high-pressure dispersion treatment to disperse the dispersion liquid containing the titania-coated silver. The coating liquid is preferably subjected to a high-pressure dispersion treatment (high-pressure dispersion method) to obtain a transparent dispersion liquid.

[0154] The manufacturing method of the present invention uses a new process to prepare a composition containing titania particles, which can improve the aggregation of titania, which has been a problem in the past, and can greatly improve solvent stability and adhesion. EXAMPLES

[0155] The present invention will be specifically described below with reference to examples.

[0156] The present invention is not limited to the following specific examples.

[0157] [1] Preparation of a composition containing titania-coated silver [Example 1] (Step 1) Preparation method of photocatalytic titanium oxide 30g of acetic acid was added to 70g of titanium tetraisopropoxide and stirred, then water was added to make the total amount 400g, and then stirred for 90 minutes. After that, it was heated to 95°C and stirred for 9 hours with a hot stirrer, and a uniform titania sol was obtained. The obtained sol was subjected to ultrasonic dispersion for 30 minutes to obtain a transparent titania sol.

[0158] The TG-DTA of the obtained titania sol was measured by heating it up to 600°C at a temperature increase rate of 3°C / min under an air atmosphere, and the mass loss rate at 200°C or higher was 10% by mass. This mass loss rate at 200°C or higher is due to organic matter derived from acetic acid bonded to the titania surface. In order to adjust the concentration of the obtained titania sol, the titania sol was diluted with water to obtain a titania sol with a TiO2 concentration of 2% by mass (wt%).

[0159] (Step 2) Dispersion treatment (high pressure dispersion method (pressure treatment)) The obtained titania sol was dispersed using a dispersing device that generates high pressure by collision between particles. For example, the dispersion treatment can be performed using a jet mill or the like. By performing the dispersion treatment, a well-dispersed titania sol was obtained.

[0160] (Step 3) Complexation with metal ions Silver nitrate was added to the titania sol with a TiO2 concentration of 2% by mass so that the weight ratio of Ag / TiO2 was 0.01, and the mixture was thoroughly stirred until it became homogeneous. Next, the titania sol was irradiated with an ultraviolet lamp for 24 hours to reduce the silver nitrate, and a silver composite titania sol was obtained.

[0161] (Step 4) Preparation of coating liquid 6 g of tetraethyl orthosilicate (TEOS) and 669 g of 1-propanol were added to 75 g of the 2 mass% silver composite titania sol prepared above. After that, the reactor was covered so that the solvent of the reaction solution would not evaporate, and the reaction solution was kept at 60°C for 12 hours. The organic matter bonded to the titania surface reacted with tetraethyl orthosilicate, and hydrolysis of tetraethyl orthosilicate proceeded, resulting in a transparent coating solution.

[0162] The resulting liquid was subjected to a high-pressure dispersion treatment (high-pressure dispersion method) to obtain a transparent dispersion liquid.

[0163] [Example 2] In Example 2, a coating liquid was prepared in the same process as in Example 1, except that in step 1 of Example 1, the heating time of the hot stirrer was changed to 16 hours.

[0164] [Example 3] In Example 3, a coating liquid was prepared in the same process as in Example 1, except that in step 1 of Example 1, the heating time of the hot stirrer was changed to 24 hours.

[0165] [Example 4] In Example 4, a coating liquid was prepared in the same manner as in Example 1, except that in step 1 of Example 1, the heating time of the hot stirrer was changed to 24 hours, and then the titania sol was irradiated with an ultraviolet lamp for 48 hours.

[0166] [Example 5] In Example 5, a coating liquid was prepared in the same manner as in Example 1, except that in step 1 of Example 1, the titania sol was irradiated with an ultraviolet lamp for 60 hours.

[0167] [Example 6] In Example 6, a coating liquid was prepared in the same manner as in Example 1, except that in step 1 of Example 1, the heating time of the hot stirrer was changed to 24 hours, and then the titania sol was irradiated with an ultraviolet lamp for 120 hours.

[0168] [Example 7] In Example 7, a coating liquid was prepared in the same process as in Example 1, except that in step 4 of Example 1, trimethoxysilane was used as the Si compound.

[0169] [Example 8] In Example 8, a coating liquid was prepared in the same manner as in Example 1, except that in step 3 of Example 1, silver nitrate was added to titania sol having a TiO2 concentration of 2 mass% so that the weight ratio of Ag / TiO2 was 0.005, and the mixture was thoroughly stirred until the entire mixture became homogeneous.

[0170] [Example 9] In Example 9, a coating liquid was prepared in the same manner as in Example 1, except that in step 3 of Example 1, silver nitrate was added to titania sol having a TiO2 concentration of 2 mass% so that the weight ratio of Ag / TiO2 was 0.001, and the mixture was thoroughly stirred until the entire mixture became homogeneous.

[0171] [Example 10] In Example 10, a coating liquid was prepared in the same manner as in Example 1, except that in step 3 of Example 1, silver nitrate was added to titania sol having a TiO2 concentration of 2 mass% so that the weight ratio of Ag / TiO2 was 0.1, and the mixture was thoroughly stirred until the entire mixture became homogeneous.

[0172] [Example 11] In Example 11, a coating liquid was prepared in the same manner as in Example 1, except that in step 3 of Example 1, silver nitrate was added to titania sol having a TiO2 concentration of 2 mass% so that the weight ratio of Ag / TiO2 was 0.0001, and the mixture was thoroughly stirred until the entire mixture became homogeneous.

[0173] [Example 12] In Example 12, a coating liquid was prepared in the same manner as in Example 1, except that in step 4 of Example 1, 3.75 g of 2 mass% silver composite titania sol, 6 g of tetraethyl orthosilicate, and 740.25 g of 1-propanol were added.

[0174] [Example 13] In Example 13, a coating liquid was prepared in the same manner as in Example 1, except that in step 4 of Example 1, 562.5 g of 2 mass% silver composite titania sol was added with 6 g of tetraethyl orthosilicate and 181.5 g of 1-propanol.

[0175] [Example 14] In Example 14, a coating liquid was prepared in the same manner as in Example 1, except that in step 4 of Example 1, 75.0 g of 2 mass% silver composite titania sol, 0.075 g of tetraethyl orthosilicate, and 674.93 g of 1-propanol were added.

[0176] [Example 15] In Example 15, a coating liquid was prepared in the same manner as in Example 1, except that in step 4 of Example 1, 75 g of 2 mass% silver composite titania sol was added with 150 g of tetraethyl orthosilicate and 525 g of 1-propanol.

[0177] [Comparative Example 1] In Comparative Example 1, the antibacterial agent Bactekilar powder manufactured by Fuji Chemical Co., Ltd. was adjusted to 2.0 mass% with distilled water to obtain a silver-loaded oxide slurry, and then 6 g of tetraethyl orthosilicate and 669 g of 1-propanol were added to 75 g of the 2 mass% silver-loaded oxide slurry prepared above, except that a coating liquid was prepared in the same process as in Example 1.

[0178] [Comparative Example 2] In Comparative Example 2, 51 g of ethanol, 30 g of pure water, 1.1 g of MKC Silicate MS51 manufactured by Mitsubishi Chemical Corporation, 45 g of Aluminum Chelate D (diluted with ethanol: solids concentration 1 wt%), 18 g of Emalex 715 manufactured by Nippon Emulsion Co., Ltd., and 3 g of sodium di(2-ethylhexyl)sulfosuccinate were added to a container and mixed.

[0179] Thereafter, 0.66 g of Fuji Chemical's silver-loaded glass bagtelite (solid content concentration 50 wt%) with an average particle size controlled to 1,000 nm was added and stirred for 60 minutes to obtain an antibacterial solution.

[0180] [Comparative Example 3] In Comparative Example 3, 51 g of ethanol, 30 g of pure water, 1.1 g of MKC Silicate MS51 manufactured by Mitsubishi Chemical Corporation, 4.5 g of Aluminum Chelate D (diluted with ethanol: solid content concentration 1 wt%), 18 g of Emalex 715 manufactured by Nippon Emulsion Co., Ltd., and 3 g of sodium di(2-ethylhexyl)sulfosuccinate were added to a container and mixed.

[0181] Thereafter, 1.3 g of Fuji Chemical's silver-loaded glass bagtelite (solid content concentration 50 wt%) with an average particle size controlled to 50 nm was added and stirred for 60 minutes to obtain an antibacterial liquid.

[0182] [2] Evaluation of compositions containing titania-coated silver The obtained coating compositions of the Examples and Comparative Examples were evaluated as follows.

[0183] (1) Transparency of the dispersion The transparency of the coating composition (dispersion liquid) was measured by measuring the transmittance using an ultraviolet-visible spectrophotometer (Shimadzu UV3400). The highest transmittance value in the wavelength range of 400 nm to 800 nm was defined as the transmittance of the composition.

[0184] The criteria for judging the dispersion are as follows: ⊚: The dispersion has the highest transmittance of 80% or more. ◯: The dispersion has the highest transmittance of 50% or more. △: The dispersion has the highest transmittance of 20% or more. ×: The dispersion has a highest transmittance of less than 20%.

[0185] (2) Dispersibility (stability) of the dispersion liquid The coating composition (dispersion) was allowed to stand for 480 hours at 60° C. After standing, the dispersion was visually inspected to evaluate the dispersion stability.

[0186] The criteria for judging the dispersion are as follows: ⊚: No precipitation, gelation, etc. was observed in the dispersion. ◯: Separation is observed in the dispersion liquid, but it can be easily dispersed by stirring by hand. △: Separation is observed in the dispersion liquid, but it can be redispersed by applying an external force such as ultrasonic waves. ×: Precipitation and gelation occurred in the dispersion liquid, and it was not redispersed.

[0187] (3) Adhesion of coating film (dispersion liquid) A coating film was prepared on a substrate by spin coating using the coating composition (dispersion). The spin coating was performed at 2,000 rpm for 60 seconds. After that, the adhesion was confirmed by touching with a finger, and the adhesion of the coating film was evaluated according to the JIS K 5600_5_6 cross-cut test method.

[0188] The criteria for judging the coating are as follows: ⊚: Peeling of the coating film from the substrate is 5% or less. ◯: The coating film peeled off from the substrate by 20% or less. △: Peeling of the coating film from the substrate is 50% or less. ×: The coating film peeled off from the substrate by more than 50%, or peeled off when touched with a finger.

[0189] (4) Antiviral test After drying, the coating composition (dispersion) was subjected to an antiviral test in a dark place in accordance with ISO 21702 using Qβ phage (non-enveloped virus).

[0190] The criteria for judging the antiviral properties of a dispersion are as follows: ◎: The dispersion has an antiviral activity value of 2 or more. ×: The dispersion has an antiviral activity value of less than 2.

[0191] The results of the examples and comparative examples are shown in the table below.

[0192] [Table 1]

[0193] [Table 2]

[0194] [Table 3]

[0195] In Examples 1 to 15, coating compositions (water-repellent coating materials) excellent in the transparency of the dispersion, the dispersion stability of the dispersion, the adhesion of the coating film, the photocatalytic activity of the dispersion, the antiviral property of the dispersion, etc. were obtained.

[0196] In Comparative Example 1, precipitation occurred in the coating composition (dispersion), and after standing, the color changed to reddish brown and gelled.

[0197] [Industrial Applicability] The present invention relates to a structure in which titania is supported around silver particles, that is, a structure in which titania coats the periphery of silver particles. The titania-coated silver-containing composition of the present invention contains a composite of fine titania-coated silver particles, and is a material that has high transparency, has little silver aggregation, and can stably exhibit antiviral properties.

[0198] The titania-coated silver-containing composition of the present invention can improve adhesion to a substrate by mixing the titania-coated silver with a binder. The titania-coated silver-containing composition of the present invention is a material that combines transparency, adhesion to a substrate, durability, antibacterial and antiviral properties (antibacterial agent), long-term stability, etc., by hydrolyzing alkoxysilane in the presence of titania-coated silver.

Claims

1. 1. A titania-coated silver composition comprising: (A) titania-coated silver; (B) a Si compound; (C) Solvent and Contains The silver contained in the titania-coated silver composition is 0.01% by mass to 25% by mass relative to the titanium oxide in the titania compound, a ratio of an average primary particle size of silver (Ag) fine particles to an average primary particle size of the titania compound contained in the titania-coated silver (A) (average primary particle size of silver (Ag) fine particles / average primary particle size of the titania compound) is 2 to 100; The titania-coated silver (A) has 1% to 99% of the surface of a silver (Ag) particle covered with a titania compound, The (B) Si compound is a hydrolysis product of an alkoxysilane. Titania-coated silver compositions.

2. 2. The titania-coated silver composition according to claim 1, wherein the titania compound has at least one organic group selected from the group consisting of an acetyl group and an acetoxy group bonded to at least some of the titanium atoms present on the surface.

3. 2. The titania-coated silver composition according to claim 1, wherein the titania compound contained in the titania-coated silver (A) exhibits a mass loss of 1% by mass or more at 200°C or higher when the titania compound is heated to 600°C using a simultaneous differential thermogravimetry and thermomechanical analysis apparatus.

4. 2. The titania-coated silver composition according to claim 1, wherein the titania compound contained in the titania-coated silver (A) has an average primary particle size of 1 nm to 20 nm.

5. 2. The titania-coated silver composition according to claim 1, wherein the silver (Ag) fine particles contained in the titania-coated silver (A) have an average primary particle size of 1 nm to 2,000 nm.

6. 2. The titania-coated silver composition according to claim 1, wherein the titania compound contained in the titania-coated silver (A) is in a content of 0.01% by mass to 5% by mass.

7. 2. The titania-coated silver composition according to claim 1, wherein the content of the (B) Si compound in the titania-coated silver composition is 0.01% by mass to 20% by mass.

8. 2. The titania-coated silver composition of claim 1, wherein the (C) solvent comprises water and an alcohol.

9. 2. The titania-coated silver composition of claim 1, wherein the (B) Si compound is a hydrolysis product of tetraethyl orthosilicate (TEOS).

10. An antibacterial and antiviral coating solution comprising the titania-coated silver composition according to any one of claims 1 to 9.

11. 1. A method for producing a titania-coated silver composition, comprising: (1) bonding an organic chain to the surface of a titania compound in a solvent; (2) after the step (1), a step of compounding the titania compound with the silver compound to prepare titania-coated silver in which the titania compound coats the silver (Ag) fine particles; and (3) After the step (2), a step of mixing the titania-coated silver having the organic chain bonded thereto with a Si compound in a solvent to react the organic matter bonded to the surface of the titania compound with the Si compound, thereby hydrolyzing the Si compound. Including, In the step (1), the organic chain is at least one organic chain selected from the group consisting of an acetyl group and an acetoxy group; In the step (2), a silver salt is used as the silver compound, and the amount of the silver salt used is 0.01% by mass to 25% by mass, calculated as the mass of silver element in the silver salt, based on the titanium oxide in the titania compound; In the step (3), the Si compound is an alkoxysilane, a ratio of an average primary particle size of silver (Ag) fine particles to an average primary particle size of the titania compound contained in the titania-coated silver (average primary particle size of silver (Ag) fine particles / average primary particle size of the titania compound) is 2 to 100; The titania-coated silver has 1% to 99% of the surface of the silver (Ag) fine particles covered with a titania compound. Method for making titania-coated silver composition.

12. Furthermore, 12. The method for producing the titania-coated silver composition according to claim 11, further comprising the step of: (4) performing a high-pressure dispersion treatment after the step (3) to disperse the dispersion liquid containing the titania-coated silver.

Citation Information

Patent Citations

  • Method for removing solid pollutant with hydrophilic group adhering to surface of composite material and fatty acid-based oil

    JP1998286537A

  • Antibacterial solution, antibacterial film, spray and cloth

    JP2017043599A

  • Metal-carrying titania nanoparticle, and production method thereof

    JP2022155211A

  • Antibacterial coating composition

    JP2022539320A

  • Coating liquid

    JP2023150249A

Cited By

  • Water-repellent paint

    JP2026166138A