Heat dissipation sheet
A silicone resin and hexagonal boron nitride-based heat dissipation sheet with glass cloth reinforcement addresses the need for resistance to gasoline and engine oil, maintaining thermal efficiency and insulation in harsh environments.
Patent Information
- Application Number
- JP2021548953
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-09-26
- Filing Date
- 2020-09-24
- Publication Date
- 2024-09-26
- Estimated Expiration
- 2040-09-24
AI Technical Summary
Heat-generating electronic components in environments exposed to gasoline or engine oil require a heat dissipation sheet with high resistance to these substances while maintaining efficient heat dissipation.
A heat dissipation sheet composed of a silicone resin binder, hexagonal boron nitride filler, and optionally a glass cloth reinforcement, with specific manufacturing processes to minimize thermal resistance decrease and ensure high withstand voltage.
The sheet maintains thermal resistance and withstand voltage, preventing deterioration when exposed to gasoline or engine oil, ensuring effective heat dissipation and electrical insulation.
Smart Images

Figure 0007556871000003 
Figure 0007556871000002 
Figure 0007556871000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a heat dissipation sheet. [Background technology]
[0002] Heat-generating electronic components such as power devices, transistors, thyristors, and CPUs generate a large amount of heat during use, so they need to be cooled. However, if a large amount of power is consumed to cool the heat-generating electronic components, the power consumption of electronic devices equipped with the heat-generating electronic components increases. For this reason, how to efficiently cool the heat-generating electronic components has become an important issue.
[0003] For heat-generating electronic components, one important issue is how to efficiently dissipate heat generated during use. Conventionally, a common heat dissipation measure has been to conduct heat generated from the heat-generating electronic components to a heat dissipation component such as a heat sink to dissipate the heat. In order to efficiently conduct the heat generated from the heat-generating electronic components to the heat dissipation component, it is desirable to fill the air gap at the contact interface between the heat-generating electronic components and the heat dissipation component with a heat dissipation material. Heat dissipation sheets have been used as such heat dissipation materials because they are easy to handle (see, for example, Patent Document 1). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2012-39060 A Summary of the Invention [Problem to be solved by the invention]
[0005] Some electronic products are used in environments where they are exposed to gasoline and engine oil. It would be useful if a heat dissipation sheet could be used to dissipate heat generated by electronic components in such environments. For this reason, a heat dissipation sheet with high resistance to gasoline and engine oil is required.
[0006] Therefore, an object of the present invention is to provide a heat dissipation sheet that has high resistance to gasoline and engine oil. [Means for solving the problem]
[0007] The inventors have conducted intensive research to achieve the above-mentioned objective and have discovered that the above-mentioned objective can be achieved by using a heat dissipation sheet that has a small rate of decrease in thermal resistance when immersed in an antifreeze solution at a temperature of 25°C containing 98% by mass or more of ethylene glycol for 500 hours. The present invention is based on the above findings and has the following gist. [1] A heat dissipation sheet in which the rate of decrease (%) ((R1-R2) / R1×100) of the thermal resistance (R2) (°C / W) of the heat dissipation sheet measured when fastened with screws at a torque of 6 kgf cm after immersion in an antifreeze solution containing 98% or more by mass of ethylene glycol at a temperature of 25°C for 500 hours is 30% or less compared to the thermal resistance (R1) (°C / W) of the heat dissipation sheet measured when fastened with screws at a torque of 6 kgf cm. [2] The heat dissipation sheet according to [1] above, in which the withstand voltage of the heat dissipation sheet is 6.0 kV or more when the heat dissipation sheet is placed between a TO-3P transistor and an aluminum plate, the TO-3P transistor is fixed to the aluminum plate with a tightening torque of 12 kgf cm using screws, and an AC voltage of 60 Hz is applied between the drain of the TO-3P transistor and the aluminum plate. [3] The heat dissipation sheet according to the above [1] or [2], which contains a resin binder and an inorganic filler. [4] The heat dissipation sheet according to the above [3], wherein the resin binder is a silicone resin. [5] The heat dissipation sheet according to the above [3] or [4], wherein the inorganic filler is an agglomerated particle of hexagonal boron nitride. [6] The heat dissipation sheet according to any one of the above [3] to [5], which contains a glass cloth. [7] The heat dissipation sheet according to any one of the above [1] to [6], which comprises a base resin layer containing a resin having a glass transition point of 200° C. or higher. Effect of the Invention
[0008] According to the present invention, a heat dissipation sheet having high resistance to gasoline and engine oil can be provided. [Brief description of the drawings]
[0009] [Figure 1] 1(a) to 1(c) are diagrams illustrating a method for measuring the thermal resistance of a heat dissipation sheet. [Diagram 2] 2(a) to 2(c) are diagrams for explaining a method for measuring the withstand voltage of a heat dissipation sheet. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The heat dissipation sheet of the present invention will be described below. [Reduction rate of thermal resistance of heat dissipation sheet] The thermal dissipation sheet of the present invention has a thermal resistance (R2) (°C / W) of the thermal dissipation sheet measured by fastening the thermal dissipation sheet with a fastening torque of 6 kgf·cm using a screw after immersing the thermal dissipation sheet in an antifreeze solution containing 98% by mass or more of ethylene glycol at a temperature of 25°C, relative to the thermal resistance (R1) (°C / W) of the thermal dissipation sheet measured by fastening the thermal dissipation sheet with a fastening torque of 6 kgf·cm using a screw before the thermal dissipation sheet is impregnated with the antifreeze solution for 500 hours. If the thermal resistance reduction rate is greater than 30%, the thermal dissipation sheet may deteriorate significantly when exposed to gasoline or engine oil. From this viewpoint, the thermal resistance reduction rate of the thermal dissipation sheet of the present invention is preferably 25% or less, more preferably 20% or less, and even more preferably 17% or less. The lower limit of the range of the thermal resistance reduction rate is not particularly limited, but is, for example, 0%. The lower limit may be 5% or more, or 10% or more.
[0011] The thermal resistance of the heat dissipation sheet of the present invention can be measured, for example, by the method described in the Examples below. In addition, the antifreeze may contain additives such as antioxidants and rust inhibitors (silicates, phosphates, amines, oxidizers, etc.) in addition to ethylene glycol. However, since the amount of these additives is small compared to ethylene glycol, the effect of these additives on the rate of decrease in the thermal resistance of the heat dissipation sheet and the voltage resistance of the heat dissipation sheet described below is small. In addition, it is usually preferable that the thermal resistance of the heat dissipation sheet is low. In this sense, a person skilled in the art would normally think that the larger the rate of decrease in the thermal resistance, the better. Therefore, a person skilled in the art would not easily come up with a heat dissipation sheet of the present invention in which the rate of decrease in the thermal resistance is 30% or less. In the present invention, as described below, the rate of decrease in the thermal resistance is considered to represent the change in the heat dissipation sheet when the heat dissipation sheet is exposed to the antifreeze.
[0012] The reason why the thermal resistance reduction rate of the heat dissipation sheet of the present invention is 30% or less is believed to be as follows, however, the following reasons do not limit the present invention. The heat dissipation sheet of the present invention can be produced, for example, by forming a composition for heat dissipation sheets containing a resin and a filler to produce a molded body, and then heating and pressing the molded body at a predetermined curing temperature to cure it. Furthermore, the heat dissipation sheet of the present invention is heated and pressed at a temperature lower than the curing temperature before heating and pressing the molded body at the curing temperature to cure it. At this stage, the molded body is not cured, so the voids in the molded body are crushed by pressure. This suppresses the penetration of antifreeze into the voids in the heat dissipation sheet, and as a result, it is thought that the swelling of the resin due to the antifreeze is suppressed. And, it is thought that the reduction rate of the thermal resistance of the heat dissipation sheet is 30% or less. It is considered that gasoline and engine oil are less likely to penetrate the voids in the heat dissipation sheet than antifreeze, so if the reduction rate of the thermal resistance of the heat dissipation sheet due to the antifreeze is 30% or less, the resistance to gasoline and engine oil will be stable for a long time. As described above, the present invention is a heat-dissipating sheet that has stable resistance to gasoline and engine oil over the long term, obtained by adjusting the properties of the heat-dissipating sheet by utilizing the changes in the heat-dissipating sheet (changes in thermal resistance) caused by antifreeze.
[0013] [Voltage resistance of heat dissipation sheet] When a heat dissipation sheet is interposed between a TO-3P type transistor and an aluminum plate, the TO-3P type transistor is fixed to the aluminum plate with a tightening torque of 12 kgf·cm using a screw, and an AC voltage of 60 Hz is applied between the drain of the TO-3P type transistor and the aluminum plate, the withstand voltage of the heat dissipation sheet of the present invention is preferably 6.0 kV or more. If the withstand voltage of the heat dissipation sheet of the present invention is 6.0 kV or more, the resistance to gasoline and engine oil is further improved. From this viewpoint, the withstand voltage of the heat dissipation sheet of the present invention is more preferably 9.0 kV or more, and even more preferably 10.0 kV or more. The upper limit of the withstand voltage of the heat dissipation sheet of the present invention is not particularly limited, but is, for example, 30.0 kV. The withstand voltage can be measured, for example, by the method described in the Examples below.
[0014] [Thickness of heat dissipation sheet] The thickness of the heat dissipation sheet of the present invention is preferably 100 to 1000 μm. When the thickness of the heat dissipation sheet of the present invention is 100 μm or more, the heat dissipation sheet can better conform to the unevenness of the mounting surface of the heat-generating electronic component. On the other hand, when the thickness of the heat dissipation sheet of the present invention is 1000 μm or less, the thermal resistance of the heat dissipation sheet can be reduced. From this viewpoint, the thickness of the heat dissipation sheet of the present invention is more preferably 150 to 650 μm.
[0015] [Ingredients of heat dissipation sheet] The heat-dissipating sheet of the present invention preferably contains a resin binder and a filler, which makes it easy to produce a heat-dissipating sheet having a thermal resistance reduction rate of 30% or less.
[0016] (Resin binder) The resin binder used in the heat dissipation sheet of the present invention is not particularly limited as long as it is a resin binder that is usually used in heat dissipation sheets. Examples of the resin binder used in the heat dissipation sheet of the present invention include epoxy resin, silicone resin, acrylic resin, phenolic resin, melamine resin, polyurethane resin, urea resin, unsaturated polyester, fluororesin, polyamide (e.g., polyimide, polyamideimide, polyetherimide, etc.), polyester (e.g., polybutylene terephthalate, polyethylene terephthalate, etc.), polyphenylene ether, polyphenylene sulfide, wholly aromatic polyester, polysulfone, liquid crystal polymer, polyethersulfone, polycarbonate, maleimide-modified resin, ABS resin, AAS (acrylonitrile-acrylic rubber-styrene) resin, AES (acrylonitrile-ethylene-propylene-diene rubber-styrene) resin, etc. These can be used alone or in combination of two or more. From the viewpoint of facilitating the handling of the heat dissipation sheet and from the viewpoint of further increasing the adhesion of the heat dissipation sheet by the flexibility of the heat dissipation sheet, it is preferable that the resin binder is rubber or elastomer. Among these resins, silicone resins are preferred from the viewpoints of heat resistance, weather resistance, electrical insulation and chemical stability.
[0017] From the viewpoint of not containing ionic impurities that cause metal corrosion and not generating by-products after reaction, the silicone resin used in the heat dissipation sheet of the present invention is preferably an addition reaction type silicone resin. The addition reaction type silicone resin is cured by a hydrosilylation reaction between an alkenyl group and a hydrogen atom bonded to a silicon atom using a platinum compound as a catalyst. An example of the addition reaction type silicone resin is silicone under the trade name "LR3303A / B" manufactured by Asahi Kasei Wacker Silicone Co., Ltd.
[0018] (filling material) The filler used in the heat dissipation sheet of the present invention is not particularly limited as long as it is a filler that is usually used in heat dissipation sheets. Examples of the filler used in the heat dissipation sheet of the present invention include inorganic fillers and metal fillers. Examples of inorganic fillers include zinc oxide, alumina, boron nitride, aluminum nitride, silicon carbide, and silicon nitride. Examples of metal fillers include aluminum, silver, and copper. These can be used alone or in combination of two or more. Among these, inorganic fillers are preferred from the viewpoint of electrical insulation, and inorganic fillers aggregated in a lump are more preferred. In aggregated inorganic fillers, voids are also generated within the aggregated filler, resulting in two types of voids, broadly divided into voids within the aggregated particles and voids between the aggregated particles. Even if two types of voids are generated in this way, the properties of the heat dissipation sheet can be appropriately adjusted by antifreeze. Among these inorganic fillers, boron nitride is more preferred from the viewpoint of thermal conductivity and chemical stability. In addition, since boron nitride has anisotropy in thermal conductivity, aggregated boron nitride particles in which the anisotropy in thermal conductivity is suppressed are more preferable. The aggregated boron nitride particles are particles in which scale-like particles of hexagonal boron nitride are aggregated into aggregates.
[0019] <Average particle size of filler> The average particle diameter of the filler is preferably 5 to 90 μm. When the average particle diameter of the filler is 5 μm or more, the content of the filler can be increased. On the other hand, when the average particle diameter of the filler is 90 μm or less, the heat dissipation sheet can be made thin. From this viewpoint, the average particle diameter of the filler is more preferably 10 to 70 μm, further preferably 15 to 50 μm, and particularly preferably 15 to 45 μm. The average particle diameter of the filler can be measured, for example, using a laser diffraction scattering particle size distribution measuring device (LS-13 320) manufactured by Beckman Coulter. The average particle diameter of the filler can be measured without applying a homogenizer before the measurement process. Therefore, when the filler is an agglomerated particle, the average particle diameter of the filler is the average particle diameter of the agglomerated particle. The obtained average particle diameter is, for example, an average particle diameter based on volume statistics.
[0020] <Filler content> The content of the filler relative to 100% by volume of the resin binder and the filler is preferably 30 to 85% by volume. When the content of the filler is 30% by volume or more, the thermal conductivity of the heat dissipation sheet is improved, and sufficient heat dissipation performance is easily obtained. When the content of the filler is 85% by volume or less, the tendency for voids to be generated during molding of the heat dissipation sheet can be suppressed, and the insulation property and mechanical strength of the heat dissipation sheet can be improved. From this viewpoint, the content of the filler relative to 100% by volume of the resin binder and the filler is more preferably 40 to 80% by volume, and even more preferably 45 to 70% by volume.
[0021] (Reinforcing layer) The heat dissipation sheet of the present invention may have a reinforcing layer. The reinforcing layer serves to further improve the mechanical strength of the heat dissipation sheet, and also suppresses the stretching of the heat dissipation sheet in the planar direction when the heat dissipation sheet is compressed in the thickness direction, thereby ensuring insulation. Examples of the reinforcing layer include glass cloth, resin films such as polyester, polyamide, polyimide, polycarbonate, and acrylic resin, cloth fiber mesh cloth such as cotton, hemp, aramid fiber, cellulose fiber, nylon fiber, and polyolefin fiber, nonwoven fabric such as aramid fiber, cellulose fiber, nylon fiber, and polyolefin fiber, metal fiber mesh cloth such as stainless steel, copper, and aluminum, and metal foil such as copper, nickel, and aluminum. These can be used alone or in combination of two or more. Among these, glass cloth is preferred from the viewpoint of thermal conductivity and insulation.
[0022] When glass cloth is used as the reinforcing layer, a commercially available glass cloth having an opening can be used. The thickness of the glass cloth is preferably 10 μm to 150 μm. When the thickness of the glass cloth is 10 μm or more, the glass cloth can be prevented from breaking during handling. On the other hand, when the thickness of the glass cloth is 150 μm or less, the decrease in thermal conductivity of the heat dissipation sheet due to the glass cloth can be prevented. From this viewpoint, the thickness of the glass cloth is more preferably 20 to 90 μm, and further preferably 30 to 60 μm. Some commercially available glass cloths have a fiber diameter of 4 to 9 μm, and these can be used for the heat dissipation sheet. The tensile strength of the glass cloth is, for example, 100 to 1000 N / 25 mm. The length of one side of the opening of the glass cloth is preferably 0.1 to 1.0 mm from the viewpoint of balancing thermal conductivity and strength. An example of a glass cloth that can be used for the heat dissipation sheet is a product name "H25 F104" manufactured by Unitika Ltd.
[0023] The heat dissipation sheet may contain other components in addition to the resin binder, the filler, and the reinforcing layer. The other components are, for example, additives, impurities, etc. The content of the other components in 100% by volume of the heat dissipation sheet may be, for example, 5% by volume or less, preferably 3% by volume or less, and more preferably 1% by volume or less.
[0024] Examples of the additives include reinforcing agents, extenders, heat resistance improvers, flame retardants, adhesion aids, conductive agents, surface treatment agents, and pigments.
[0025] <Base resin layer> The heat dissipation sheet of the present invention may include a base resin layer. The base resin layer serves to further improve the heat resistance and insulation of the heat dissipation sheet. In this case, the heat dissipation sheet of the present invention includes a resin composition layer containing the above-mentioned resin binder and inorganic filler, and a base resin layer adjacent to this resin composition layer. The resin composition layer may include the above-mentioned reinforcing layer.
[0026] The substrate resin layer preferably contains a resin having a glass transition point of 200° C. or higher. If the glass transition point is 200° C. or higher, sufficient heat resistance can be obtained, and the insulating property and thermal conductivity of the laminate can be well maintained. The substrate resin layer may be a layer formed from a coating film or a layer formed from a film.
[0027] Examples of resins constituting the base resin layer include polyimide, polyamideimide, polyamide (particularly aromatic polyamide), polyethersulfone, polyetherimide, polyethylene naphthalate, polytetrafluoroethylene (PTFE), tetrafluoroethylene-perfluoroalkylvinylether copolymer (PFA), etc., and among these, polyimide is preferred. These resins may be used alone or in combination.
[0028] The resin content in the base resin layer is not particularly limited, but the lower limit is preferably 78% by volume or more, more preferably 80% by volume or more, and even more preferably 82% by volume or more, and the upper limit is preferably 92% by volume or less, more preferably 90% by volume or less, and even more preferably 88% by volume or less.
[0029] The substrate resin layer preferably contains an inorganic filler. By containing an inorganic filler in the substrate resin layer, the insulation, thermal conductivity, peel strength, etc. can be improved. In particular, it is presumed that the peel strength is increased because the inorganic filler forms irregularities at the interface between the substrate resin layer and the resin composition layer, resulting in an anchor effect. As the inorganic filler, the same inorganic filler as described above can be used.
[0030] The content of the inorganic filler in the base resin layer is not particularly limited, but the lower limit is preferably 8 volume % or more, more preferably 10 volume % or more, and even more preferably 12 volume % or more, and the upper limit is preferably 22 volume % or less, more preferably 20 volume % or less, and even more preferably 18 volume % or less.
[0031] The substrate resin layer may contain a small amount of the above-mentioned additives or impurities. The total content of the above-mentioned resin and inorganic filler in the substrate resin layer is preferably 90% by volume or more, more preferably 95% by volume or more, and even more preferably 97% by volume or more.
[0032] The thickness of the base resin layer is preferably in the following ranges from the viewpoints of insulation, thermal conductivity, and processability. The lower limit is preferably 0.010 mm or more. By setting the thickness to 0.010 mm or more, the insulation can be further improved and the processability can also be improved. The thickness is more preferably 0.012 mm or more, and even more preferably 0.015 mm or more. The upper limit is preferably 0.100 mm or less. The thickness is more preferably 0.070 mm or less, and even more preferably 0.050 mm or less.
[0033] The film to be the base resin layer can be produced according to a known film production method, or a commercially available product may be used.
[0034] (Heat dissipation sheet type) In the present invention, the form of the heat dissipation sheet is not particularly limited, and it may be a sheet product or a roll product.
[0035] (Method of manufacturing heat dissipation sheet) When silicone resin is used as the resin binder, chunky boron nitride particles are used as the filler, and glass cloth is used as the reinforcing layer, the heat dissipation sheet of the present invention can be produced, for example, by a production method including the following steps 1 to 4. (Process 1) In step 1, a composition for a heat dissipation sheet is prepared by mixing an uncured silicone resin and lump boron nitride particles.
[0036] (Process 2) In step 2, a glass cloth is placed on a film having releasability, and then the composition for a heat-dissipating sheet is applied onto the film having releasability from above the glass cloth, and dried at 60 to 80°C for 4 to 7 minutes to form a sheet. The application method is not particularly limited, and known application methods that can apply the composition uniformly, such as the doctor blade method, the comma coater method, the screen printing method, and the roll coater method, can be adopted. However, the doctor blade method and the comma coater method are preferred from the viewpoint of being able to control the thickness of the applied composition for a heat-dissipating sheet with high precision. In addition, the film having releasability is, for example, a PET film. The composition for a heat-dissipating sheet may be applied onto one side of the glass cloth, or the composition for a heat-dissipating sheet may be applied onto both sides of the glass cloth. When the composition for a heat-dissipating sheet is applied onto both sides of the glass cloth, the composition for a heat-dissipating sheet may be applied onto one side of the glass cloth, and then the composition for a heat-dissipating sheet may be applied onto the other side of the glass cloth. The composition for a heat-dissipating sheet may be applied onto both sides of the glass cloth at the same time.
[0037] In the case of a heat dissipation sheet having a base resin layer, the resin composition is applied onto the base sheet which becomes the base resin layer. As a method for applying the composition to the base sheet, a conventionally known method such as a coater method, a doctor blade method, an extrusion molding method, an injection molding method, a press molding method, etc. can be used. In the case of a heat dissipation sheet having a base resin layer, the composition for heat dissipation sheets may be applied to both sides of the base resin layer and dried so that the base resin layer is disposed in the center of the thickness direction of the heat dissipation sheet.
[0038] (Step 3) In step 3, the mixture is heated in an air atmosphere at a pressure of 100 to 200 kgf / cm using a heat press. 2 The composition for heat-dissipating sheets is preformed by heating and pressurizing the composition for heat-dissipating sheets applied to a film having releasability under conditions of a pressure of 1000 g, a heating temperature of 50 to 80°C, and a pressing time of 30 to 40 minutes. This allows the aggregates of the chunky boron nitride particles to be appropriately loosened. By setting the heating temperature to 50°C or higher, it is possible to prevent the aggregates of the chunky boron nitride particles from being excessively broken down, which causes the scaly particles of boron nitride to be oriented, thereby preventing a decrease in the thermal conductivity of the heat-dissipating sheet. By setting the heating temperature to 80°C or lower, it is possible to remove air bubbles in the composition for heat-dissipating sheets, increase the density of the heat-dissipating sheet, and improve the insulating properties of the heat-dissipating sheet.
[0039] (Step 4) In step 4, the mixture is heated and pressed at 100 to 200 kgf / cm in air, nitrogen, argon, hydrogen, or vacuum using a heat press. 2 The composition for heat-dissipating sheets that has been provisionally molded is further heated and pressurized under conditions of a pressure of 100 kgf / cm, a heating temperature of 80 to 170°C, and a pressing time of 10 to 60 minutes, to thereby form the composition for heat-dissipating sheets into a final shape. 2 By setting the pressure to 200 kgf / cm or more, the heating temperature to 80° C. or more, and the pressing time to 10 minutes or more, it is possible to improve the bonding strength between the composition for a heat-dissipating sheet and the glass cloth. 2By setting the heating temperature at 170° C. or less and the pressing time at 60 minutes or less, the productivity of the heat dissipation sheet can be improved and the manufacturing cost can be reduced. Also, as described above, in the present invention, the heating and pressing are performed gradually to reduce the amount of voids, so the pressing force here is greater than that in step 3.
[0040] The heat dissipation sheet of the present invention may be produced by a production method further comprising the following step 5 after the above step 4. (Step 5) In step 5, the formed composition for heat dissipation sheets is heated at a temperature of 130 to 250°C for a heating time of 2 to 30 hours to further cure the composition for heat dissipation sheets. This makes it possible to remove low molecular weight siloxanes in the resin. If the concentration of low molecular weight siloxanes in the resin is high, siloxane gas is generated, and an insulating coating of silicon oxide is formed on the electrical contacts due to energy from the sliding of electrical contacts or sparks, which may cause contact failure. EXAMPLES
[0041] The present invention will be described in detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples.
[0042] The heat dissipation sheets of the examples and comparative examples were evaluated as follows. (Thickness of heat dissipation sheet) The thickness of the heat dissipating sheet was measured at five random locations using a micrometer, and the average value was taken as the thickness of the heat dissipating sheet of the example or comparative example.
[0043] (Reduction rate of thermal resistance of heat dissipation sheet) Three sheets of heat dissipation sheets that were not soaked in antifreeze were prepared. The thermal resistance (R1) of the heat dissipation sheets before soaking in antifreeze was measured as follows. As shown in Figure 1, a heat dissipation sheet 1 was placed between a TO-3P transistor 2 (manufactured by Mitsubishi Electric Corporation, model number: 2SC3152) and an aluminum heat sink 3 equipped with heat dissipation fins (manufactured by Ryosan Corporation, model number: 40CH104-L76-K). The heat dissipation sheet 1 was then fastened using screws 4 with a nominal diameter of M3 mm with a tightening torque of 6 kgf cm. The contact area between the TO-3P transistor 2 and the heat dissipation sheet 1 was approximately 2.8 cm2. 2 After that, as shown in FIG. 1(c), a transistor temperature measuring thermocouple 5 for measuring the temperature of the TO-3P transistor 2 was attached to the TO-3P transistor 2, and a heat sink temperature measuring thermocouple 6 for measuring the temperature of the heat sink 3 was attached to the heat sink 3. Then, 5 W of power was applied between the collector and emitter of the TO-3P transistor 2, and after the temperature of the TO-3P transistor 2 became almost constant, the temperatures of the TO-3P transistor 2 and the heat sink 3 were measured. Based on the measurement results, the thermal resistance was calculated from the following formula (1): Thermal resistance (℃ / W) = (Transistor temperature (℃) - Heat sink temperature (℃)) ÷ Power applied to the transistor (W) (1) The average value of the thermal resistances of the three heat dissipation sheets was taken as the thermal resistance (R1) of the heat dissipation sheet before it was impregnated with the antifreeze solution in the example or comparative example.
[0044] Next, a heat dissipation sheet was prepared by soaking for 500 hours in an antifreeze solution (Antifreeze Super, manufactured by General Sekiyu Co., Ltd.) containing 98% or more by mass of ethylene glycol at a temperature of 25°C. The thermal resistance of the heat dissipation sheet soaked in antifreeze solution for 500 hours was calculated in the same manner as for the heat dissipation sheet not soaked in antifreeze solution described above. The average value of the thermal resistance of the three heat dissipation sheets was taken as the thermal resistance (R2) of the heat dissipation sheet soaked in antifreeze solution for 500 hours in the examples or comparative examples.
[0045] The rate of decrease in thermal resistance was calculated using the following formula (2). Thermal resistance reduction rate (%) = (R1 (℃ / W) - R2 (℃ / W)) ÷ R1 (℃ / W) × 100 (2)
[0046] Similar evaluations were also performed on heat-dissipating sheets that had been impregnated with the above-mentioned antifreeze for 250 hours and 1000 hours, heat-dissipating sheets that had been impregnated with gasoline (regular gasoline, manufactured by General Sekiyu Co., Ltd.) at a temperature of 25°C for 1000 hours, and heat-dissipating sheets that had been impregnated with engine oil (G Urban SDCC (viscosity 20W30), manufactured by General Sekiyu Co., Ltd.) at a temperature of 25°C for 1000 hours.
[0047] (Voltage resistance of heat dissipation sheet) As shown in FIG. 2, a heat dissipation sheet 1 was placed between a TO-3P type transistor 2 (manufactured by Mitsubishi Electric Corporation, model number: 2SC3152) and an aluminum plate 7. The heat dissipation sheet 1 was then fastened using screws 4 with a nominal diameter of M3 mm with a tightening torque of 12 kgf cm. The contact area between one TO-3P type transistor 2 and the heat dissipation sheet 1 was approximately 2.8 cm2. 2 2(c), an AC voltage of 60 Hz was applied between the emitter of the TO-3P transistor 2 and the aluminum plate 7 using a withstand voltage tester 8 (manufactured by Kikusui Electronics Co., Ltd., model number: TOS 5101), and the voltage was increased from 0 V at a rate of 500 V / s. The voltage at which dielectric breakdown occurred was taken as the withstand voltage of the heat dissipation sheet. It was determined that dielectric breakdown occurred when the leakage current between the emitter of the TO-3P transistor 2 and the aluminum plate 7 exceeded 10 mA. The average value of the withstand voltages of the three heat dissipation sheets was taken as the withstand voltage of the heat dissipation sheet in the example or comparative example.
[0048] The heat dissipation sheets of the examples and comparative examples were prepared as follows. [Example 1] (Preparation of hexagonal boron nitride) Boric acid, melamine, and calcium carbonate (all special grade reagents) were mixed in a mass ratio of 70:50:5, and in a nitrogen gas atmosphere, the temperature was raised from room temperature to 1400°C over one hour, held at 1400°C for three hours, then raised to 1900°C over four hours, held at 1900°C for two hours, and then cooled to room temperature to produce hexagonal boron nitride. This was then crushed, pulverized, and sieved to produce aggregated boron nitride particles. The average particle size of the aggregated boron nitride particles produced was 20 μm.
[0049] (Preparation of composition for heat dissipation sheet) 22 g of silicone resin (manufactured by Wacker Asahi Kasei Silicones, model number: LR3303-20A), 22 g of silicone resin (manufactured by Wacker Asahi Kasei Silicones, model number: LR3303-20B), and 137 g of the prepared aggregate boron nitride particles were added, after which toluene was added as a viscosity modifier so that the solids concentration was 60 wt%. The mixture was then mixed for 15 hours with a turbine-type stirring blade in a stirrer (manufactured by HEIDON, product name: Three-One Motor) to prepare a composition for heat dissipation sheets.
[0050] (Making heat dissipation sheets) After placing a glass cloth (manufactured by Unitika Ltd., product name: H25 F104) on a Teflon (registered trademark) sheet, the above silicone composition was applied to the glass cloth to a thickness of 0.2 mm using a comma coater and dried at 75°C for 5 minutes. Next, the dried silicone composition was turned over so that the glass cloth was on the top, and applied to the glass cloth to a thickness of 0.2 mm using a comma coater and dried at 75°C for 5 minutes to produce a silicone composition sheet in which the silicone composition was applied to both sides of the glass cloth. Thereafter, using a flat plate press machine (manufactured by Yanase Manufacturing Co., Ltd.), the silicone composition was applied to the glass cloth at a temperature of 70°C and a pressure of 120 kgf / cm. 2 The mixture was pressed for 35 minutes under the conditions of 150 kgf / cm2 for preliminary molding. 2 While pressing, the temperature was increased to 150°C at a rate of 10°C / min. Then, the temperature was 150°C and the pressure was 150kgf / cm. 2The sheet was pressed for 45 minutes under the above conditions to perform the main molding. Then, secondary heating was performed for 4 hours at normal pressure and at a temperature of 150°C to produce a 0.30 mm thick heat dissipation sheet of Example 1. The content of the inorganic filler in the heat dissipation sheet was 60% by volume relative to 100% by volume of the total of the resin binder and the inorganic filler.
[0051] [Comparative Example 1] A heat dissipation sheet of Comparative Example 1 having a thickness of 0.30 mm was produced in the same manner as in Example 1, except that pre-molding was not performed.
[0052] [Example 2] A heat-dissipating sheet composition prepared using the same raw materials as in Example 1 was applied onto a glass cloth with a comma coater to a thickness changed from 0.2 mm to 0.15 mm, and then the dried heat-dissipating sheet composition was turned over so that the glass cloth was on top, and the composition was applied onto the glass cloth with a comma coater to a thickness of 0.15 mm instead of 0.2 mm. A heat-dissipating sheet with a thickness of 0.20 mm was prepared in the same manner as in Example 1, except for the following changes.
[0053] [Example 3] A heat dissipation sheet with a thickness of 0.20 mm was produced in the same manner as in Example 1, except that the glass cloth (manufactured by Unitika Ltd., product name: H25 F104) was changed to a polyimide film (manufactured by Toray DuPont Co., Ltd., product name: Kapton 100H, thickness 0.026 mm), and the composition for the heat dissipation sheet was applied to only one side to a thickness of 0.3 mm and then dried.
[0054] [Comparative Example 2] A heat-dissipating sheet composition prepared using the same raw materials as in Comparative Example 1 was applied onto a glass cloth with a comma coater to a thickness changed from 0.2 mm to 0.15 mm, and then the dried heat-dissipating sheet composition was turned over so that the glass cloth was on top, and the composition was applied onto the glass cloth with a comma coater to a thickness of 0.15 mm instead of 0.2 mm. A heat-dissipating sheet with a thickness of 0.20 mm was prepared in the same manner as in Comparative Example 1, except for the following changes.
[0055] The evaluation results are shown in Table 1.
[0056] [Table 1]
[0057] From the above evaluation results, it was found that a heat dissipation sheet that has a thermal resistance drop of 30% or less when soaked in antifreeze for 500 hours has high resistance to gasoline and engine oil. Specifically, it does not deteriorate even when soaked in gasoline and engine oil for more than 1000 hours. In addition, a comparison of 500 hours of immersion in antifreeze with 1000 hours of immersion showed that evaluation was possible with a 500 hour immersion. In addition, when the dielectric breakdown voltages of Examples 1 and 3 were evaluated by a short-time breakdown test (room temperature: 23° C.) according to the method described in JIS C2110, the dielectric breakdown voltage of Example 3 was about 3 kV higher. [Explanation of symbols]
[0058] 1 Heat dissipation sheet 2 TO-3P type transistor 3. Heat sink 4 screws 5 Thermocouples for measuring transistor temperature 6 Thermocouples for heat sink temperature measurement 7 Aluminum plate 8. Withstand voltage tester
Claims
1. A heat dissipation sheet in which the rate of decrease (%) ((R1-R2) / R1 x 100) of the thermal resistance (R2) (°C / W) of the heat dissipation sheet measured by tightening screws with a tightening torque of 6 kgf-cm after immersion in an antifreeze solution at 25°C containing 98% or more by mass of ethylene glycol for 500 hours is 30% or less compared to the thermal resistance (R1) (°C / W) of the heat dissipation sheet measured by tightening screws with a tightening torque of 6 kgf-cm.
2. The heat dissipation sheet according to claim 1, wherein when the heat dissipation sheet is interposed between a TO-3P type transistor and an aluminum plate, the TO-3P type transistor is fixed to the aluminum plate using a screw having a nominal diameter of M3 mm with a tightening torque of 12 kgf cm, and an AC voltage of 60 Hz is applied between the drain of the TO-3P type transistor and the aluminum plate, the withstand voltage of the heat dissipation sheet is 6.0 kV or more.
3. 3. The heat dissipation sheet according to claim 1, further comprising a resin binder and an inorganic filler.
4. The heat dissipation sheet according to claim 3 , wherein the resin binder is a silicone resin.
5. 5. The heat dissipation sheet according to claim 3, wherein the inorganic filler is an agglomerated particle of hexagonal boron nitride.
6. The heat dissipation sheet according to any one of claims 3 to 5, which contains glass cloth.
7. The heat dissipation sheet according to any one of claims 1 to 6, comprising a substrate resin layer containing a resin having a glass transition point of 200°C or higher.
Citation Information
Patent Citations
Heat dissipation structure of electronic component
JP2005005671A
Heat radiating structure and its manufacturing method
JP2005251921A
Method for manufacturing semiconductor module unit
JP2012004468A
Heat-conductive sheet
JP2012039060A
Method of manufacturing thermally conductive sheet and thermally conductive sheet
JP2012212727A