Aluminum alloy strip for the manufacture of brazed heat exchangers

The aluminum alloy strip with a tailored composition and manufacturing process addresses the challenge of enhancing corrosion resistance and mechanical strength in brazed heat exchangers, achieving improved performance and cost-effectiveness.

JP7556874B2Active Publication Date: 2024-09-26CONSTELLIUM NEUF BRISACH SAS
View PDF 16 Cites 0 Cited by

Patent Information

Application Number
JP2021552542
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-03-05
Filing Date
2020-02-27
Publication Date
2024-09-26
Estimated Expiration
2040-02-27

AI Technical Summary

Technical Problem

Existing aluminum alloys for brazed heat exchangers face challenges in achieving improved corrosion resistance without compromising mechanical strength or brazability, leading to increased manufacturing costs and surface degradation.

Method used

A specific compositional region for the aluminum alloy strip is defined, with Si: 0.10~0.30%, Fe<0.20%, Cu: 0.75~1.05%, Mn: 1.2~1.7%, Mg<0.03%, Ti<0.15%, and the balance aluminum, along with a manufacturing process involving casting, cladding, preheating, hot rolling, and annealing, to enhance corrosion resistance without affecting mechanical strength or brazability.

Benefits of technology

The alloy strip achieves improved corrosion resistance and maintains mechanical strength, reducing product thickness and manufacturing costs while ensuring effective brazing performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007556874000004
    Figure 0007556874000004
  • Figure 0007556874000005
    Figure 0007556874000005
  • Figure 0007556874000006
    Figure 0007556874000006
Patent Text Reader

Abstract

1. Strip intended for the manufacture of brazed heat exchangers, having an aluminium alloy core with the following composition, in mass %, of: Si: 0.10-0.30%, preferably 0.15-0.25%; Fe<0.20%; Cu: 0.75-1.05%, preferably 0.75-1.02%, more preferably 0.75-1.0%; Mn: 1.2-1.7%, preferably 1.2-1.55%, more preferably 1.25-1.4%; Mg<0.03%, preferably <0.025%, more preferably <0.015%; Zn<0.1%; Ti<0.15%; other elements: each <0.05% and total <0.15%; and the remainder being aluminium.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The invention relates to thin strips (typically 0.05 to 3 mm thick, preferably 0.15 to 2.5 mm thick) made of aluminum-manganese core alloys (3000 series according to the Aluminum Association nomenclature) possibly clad on one or both sides with cladding alloys, most often aluminum-silicon brazing alloys (4000 series according to the Aluminum Association nomenclature), and / or with interlayer alloys made of aluminum-manganese alloys (3000 series according to the Aluminum Association nomenclature), arranged between the core and any brazing alloy. These strips are intended in particular for the manufacture of elements such as tubes, collectors and plates of heat exchangers assembled by brazing. These exchangers are found in particular in the cooling systems of motor vehicle engines and in the air conditioning systems of the passenger compartment. Brazing techniques for aluminum alloys are described, for example, in the article "Excellent brazing of aluminum and its alloys" by JC Cucza, A. Uhry and JC Goussain, published in Soudage et Techniques Connexes, November-December 1991, pages 18-29. The strip according to the invention can in particular be used in non-corrosive flux brazing techniques of the NOCOLOK® or CAB (controlled atmosphere brazing) type, and also, according to one variant, in fluxless brazing techniques. [Background technology]

[0002] The properties required for the aluminium alloy strip used for the manufacture of brazed exchangers are, inter alia, good brazeability, high mechanical strength after brazing to allow the use of the thinnest possible thicknesses, sufficient formability to facilitate the formation of tubes, fins, collectors and plates before brazing, and good corrosion resistance. Naturally, it is important that the alloy selected is easy to cast and roll, and that the manufacturing costs of the strip are compatible with the requirements of the automotive industry.

[0003] The alloy used is 3003 with the following composition (% by weight according to EN573-3 standard): Si<0.6%, Fe<0.7%, Cu: 0.05-0.20%, Mn: 1.0-1.5%, Zn<0.10%, other elements each <0.05% and total <0.15%, balance Aluminium.

[0004] A number of alloys have been proposed with the objective of improving any of the above-mentioned utilization properties, more particularly corrosion resistance, and are therefore sometimes given the designation in the industry as "long life" alloys.

[0005] U.S. Pat. No. 5,125,452 (Sumitomo Light Metal Industries Ltd. and Nippon Denso Co. Ltd.) describes a clad strip in which the base alloy has the following composition: Si<0.1, Fe<0.3, Cu:0.05~0.35, Mn:0.3~1.5, Mg0.05~0.5, Ti:0.05~0.35, where Cu-0.2 <Mg<Cu+0.2。

[0006] EP 0326337 (Alcan International) describes a clad strip in which the base alloy has the following composition: Si<0.15, Fe<0.4, Cu:0.1~0.6, Mn:0.7~1.5, Mg<0.8.

[0007] A low Si content, preferably less than 0.05%, allows the formation of a dense layer of Mn precipitates that can act as a barrier to the diffusion of silicon from the coating alloy, increasing the corrosion resistance. WO 94 / 22633 is a variant of the above, differing only in the higher Cu content (0.6-0.9%).

[0008] U.S. Pat. No. 5,350,436 (Kobe Alcoa Transportation Equipment Co., Ltd. and Nippon Denso Co., Ltd.) describes a base alloy of the following composition: Si: 0.3~1.3, Cu<0.2, Mn: 0.3~1.5, Mg<0.2, Ti: 0.02~0.3, Fe not specified.

[0009] Without being bound by theory, it seems that the high Si content (0.8% in the examples) makes it possible to compensate for the absence of Cu and Mg in terms of mechanical strength, the presence of Ti contributes to good corrosion resistance and the absence of Mg favors good brazeability.

[0010] European patent specification No. 0718072 (Hoogovens Aluminium Walzprodukte) describes a base alloy of the following composition: Si>0.15, Fe<0.8, Cu: 0.2-2, Mn: 0.7-1.5, Mg: 0.1-0.6, where Cu+Mg<0.7 and possible additions of Ti, Cr, Zr or V. The examples show a Si content of 0.5%.

[0011] JP 2000-167688 A (Sumitomo Light Metal Industries, Ltd.) discloses an aluminum core alloy containing, by mass percentage, 0.5-2.0% Mn, 0.1-1.0% Cu, 0.1% or less Si, 0.3% or less Fe, 0.06-0.35% Ti, 0.04% or less Mg, and unavoidable impurities, with the remainder being aluminum.

[0012] If we were to summarise here the teaching of the state of the art for this type of alloy, it would be seen that the alloys of the first category have a very low content of Si (<0.15, preferably <0.05%), with or without a low content of Fe, although the requirements are in all cases not as high as for Si. These very low Si contents (<0.05%) can only be obtained from pure base materials, which increases the production costs. The alloys of the second category, by revisiting the need for a very low Si content to obtain good corrosion resistance, have, on the contrary, a rather high Si content (0.5-0.8%) in order to compensate for the loss of mechanical strength, which in some cases is associated with a low content of the hardening elements Mg and Cu. In fact, it is known that for brazing with flux, the Mg content should be reduced to limit the migration of Mg to the cladding layer surface, which leads to the formation of a thick layer of the oxide MgO. The presence of this oxide forces an increase in the amount of flux on the surface to be brazed, which increases the assembly costs and deteriorates the appearance of the surface. Other references still aim for intermediate Si contents (see for example EP 1075935, EP 1413427, EP 2969308 and also US 9546829).

[0013] As for the element Cu, its effect on corrosion resistance appears to be controversial, with some references urging against using excessively high amounts of Cu (see, in particular, U.S. Patent No. 6,019,939 to Alcan International Limited). [Prior art documents] [Patent documents]

[0014] [Patent Document 1] U.S. Patent No. 5,125,452 [Patent Document 2] European Patent No. 0326337 [Patent Document 3] WO 94 / 22633 [Patent Document 4] U.S. Pat. No. 5,350,436 [Patent Document 5] European Patent No. 0718072 [Patent Document 6] JP 2000-167688 A [Patent Document 7] European Patent No. 1075935 [Patent Document 8] European Patent No. 1413427 [Patent Document 9] European Patent No. 2969308 [Patent Document 10] U.S. Pat. No. 9,546,829 [Patent Document 11] U.S. Patent No. 6,019,939 [Non-patent literature]

[0015] [Non-Patent Document 1] "Superior Brazing of Aluminum and Its Alloys" by JC Cucza, A. Uhry and JC Goussain, published in Soudage et Techniques Connexes, November-December 1991, p18-29 Summary of the Invention [Problem to be solved by the invention]

[0016] In the face of increasing market demand, there continues to be a need for new core alloys that have improved corrosion resistance compared to existing alloys without compromising mechanical strength or brazeability, which would allow meeting the ever-present demand for reduced product thickness. [Means for solving the problem]

[0017] Surprisingly, applicants have determined a compositional region in which corrosion resistance can be improved without degrading mechanical strength or brazeability.

[0018] The invention therefore relates to a strip intended for the manufacture of brazed heat exchangers, which strip comprises, in mass %, Si: 0.10 to 0.30%, preferably 0.15 to 0.25%, Fe<0.20%, Cu: 0.75 to 1.05%, preferably 0.75 to 1.02%, more preferably 0.75 to 1.0%, Mn: 1.2 to 1.7%, preferably 1.2 to 1.55%, more preferably 1.25 to 1.4%, Mg<0.03%, preferably <0.025%, more preferably <0.015%; Zn<0.1%, Ti<0.15%, Other elements: <0.05% each and <0.15% in total The rest is aluminum, The present invention relates to a strip having an aluminum alloy core having the following composition:

[0019] The present invention also provides - casting a core alloy plate; - optionally cladding with at least one brazing aluminium alloy and optionally with at least one interlayer aluminium alloy, - pre-heating to a temperature of 450-520°C with a holding step at the maximum temperature preferably for less than 12 hours, more preferably less than 3 hours; - hot rolling the plate without prior homogenization at a temperature of 450-520°C to a thickness of 2-6 mm; - cold rolling to the desired thickness, the thickness of the strip after cold rolling being preferably between 0.15 and 3 mm; - an annealing step at a temperature between 240 and 450 °C, preferably between 240 and 380 °C, with a maintenance step at the maximum temperature for a period between 10 minutes and 15 hours, preferably between 20 minutes and 3 hours; The present invention also relates to a method for producing a strip, the method comprising the successive steps of:

[0020] According to one variant, the invention also provides a method for producing a device comprising: - casting a core alloy plate; - homogenizing the plate at 580-630°C for 1-24 hours; - optionally cladding with at least one brazing aluminium alloy and optionally with at least one interlayer aluminium alloy, - pre-heating to a temperature of 450-520°C with a holding step at the maximum temperature preferably for less than 12 hours, more preferably less than 3 hours; - hot rolling the homogenized and optionally clad plate at a temperature of 450-520°C to a thickness of 2-6 mm; - cold rolling to the desired thickness, the thickness of the strip after cold rolling being preferably between 0.15 and 3 mm; and - an annealing step at a temperature between 240 and 450°C, preferably between 240 and 380°C, with a hold at the maximum temperature for a period between 10 minutes and 15 hours, preferably between 20 minutes and 3 hours; The present invention also relates to a method for producing a strip according to the invention, comprising the successive steps of:

[0021] The invention also relates to a heat exchanger, at least in part, made from the strip according to the invention.

[0022] The invention also relates to the use of a strip according to the invention for the manufacture of a heat exchanger, said strip having improved corrosion resistance without deterioration of the mechanical strength or brazeability. [Brief description of the drawings]

[0023] [Figure 1] 1 represents cross-sectional micrographs of strips after SWAAT test (ASTM G85A3) for samples of Example 1 after 4 weeks of exposure. The deepest corrosion sites are represented. Index A corresponds to the sample with core alloy A (prior art). Index B corresponds to the sample with core alloy B (in accordance with the present invention). Index C corresponds to the sample with core alloy C (in accordance with the present invention). [Diagram 2] 1 represents cross-sectional micrographs of strips after SWAAT testing for samples of Example 2 after two weeks of exposure, where index E corresponds to the sample having core alloy E (in accordance with the present invention) and index F corresponds to the sample having core alloy F (in accordance with the prior art). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0024] In the specification and claims, unless otherwise indicated: - The designation of aluminum alloys shall conform to the nomenclature of the Aluminum Association; - The contents of chemical elements are given as mass percentages.

[0025] The strip according to the invention comprises, in mass %, Si: 0.10 to 0.30%, preferably 0.15 to 0.25%, Fe<0.20%, Cu: 0.75 to 1.05%, preferably 0.75 to 1.02%, more preferably 0.75 to 1.0%, Mn: 1.2 to 1.7%, preferably 1.2 to 1.55%, more preferably 1.25 to 1.4%, Mg<0.03%, preferably <0.025%, more preferably <0.015%; Zn<0.1%, Ti<0.15%, Other elements: <0.05% each and <0.15% in total The rest is aluminum, The aluminum alloy core has the following composition:

[0026] The justification for the compositional limits of the core alloy can be justified as follows: the minimum silicon content of 0.10% allows to avoid the use of costly pure base metals. Moreover, in magnesium-containing alloys, silicon contributes to the mechanical strength by forming precipitates Mg2Si. Above 0.30%, silicon can have a detrimental effect on the corrosion resistance due to the formation of manganese dispersoids AlMnSi and AlMnFeSi.

[0027] An iron content limited to less than 0.25% is likewise advantageous for corrosion resistance and formability, but it is not necessary to reduce it to a very low content of less than 0.15%, which would entail high costs.

[0028] Copper is a hardening element that contributes to mechanical strength, but above 1.1% coarse intermetallic compounds form in the casting which impair the homogeneity of the metal and constitute corrosion initiation sites.

[0029] Manganese is within limits close to those of alloy 3003. It contributes to mechanical strength and corrosion resistance.

[0030] Limited zinc additions may have a beneficial effect on corrosion resistance by modifying the electrochemical mechanisms, especially for alloys with the highest copper loadings, but this addition should be kept below 0.2% to avoid an excessively high probability of general corrosion.

[0031] Preferably, the core alloy contains less than 0.1% Ti. Preferably, the core alloy contains at least 0.05%, more preferably at least 0.06% Ti.

[0032] [Aluminum alloys for brazing] The strip according to the invention generally has a thickness of 0.05 to 3 mm, preferably 0.15 to 2.5 mm, depending on the type of part to be manufactured, and may be clad with a coating alloy, which may be a brazing alloy or an alloy that acts as a sacrificial anode to protect the part against corrosion, such as a zinc alloy like alloy AA7072.

[0033] According to one variant of the invention, the brazing aluminum alloy does not contain any intentional addition of Zn, the latter being preferably present in an amount corresponding to an impurity, ie less than 0.05% by weight.

[0034] The brazing alloys are those in the 4xxx family of alloys that have a liquidus temperature sufficiently low compared to the solidus of the core alloy to provide sufficient temperature interval for brazing, acceptable mechanical strength and good wettability. These alloys may contain additive elements, such as strontium.

[0035] Preferably, the strip of the invention is clad on one or both sides with a brazing aluminium alloy, preferably a 4xxx alloy containing 4-13% by weight, preferably 6-11% by weight, Si and max 0.5% by weight, preferably max 0.3% by weight, Fe.

[0036] Preferably, the brazing aluminum alloy comprises, in mass %, Si: 5-13%, Fe: max. 1%, Cu: max 0.4%, preferably max 0.1%, Mn: max 0.2%, preferably max 0.1%, Mg: max 0.3%, preferably max 0.1%, Zn: max 0.2%, preferably max 0.1%, Ti: max 0.30%, preferably max 0.1%, Other elements: less than 0.05% each and less than 0.15% in total The rest is aluminum, Includes.

[0037] As an example, the composition AA4045 is an aluminium alloy that may be suitable as a brazing alloy according to the present invention, with the composition, in weight percent, being: 9-11% Si, max 0.8% Fe, max 0.30% Cu, max 0.05% Mn, max 0.05% Mg, max 0.10% Zn, max 0.20% Ti, less than 0.05% each and less than 0.15% total of other elements, the balance being aluminium.

[0038] As an example, the above composition preferably contains up to 0.6% Fe.

[0039] As an example, the above composition preferably contains maximum 0.1% Cu.

[0040] As an example, composition AA4343 is an aluminum alloy that may be suitable as a brazing alloy according to the present invention, with the composition, in weight percent, being: 6.8-8.2% Si, max 0.8% Fe, max 0.25% Cu, max 0.10% Mn, max 0.05% Mg, less than 0.05% each and less than 0.15% total of other elements, the balance being aluminum.

[0041] As an example, the above composition preferably contains up to 0.3% Fe.

[0042] As an example, the above composition preferably contains maximum 0.1% Cu.

[0043] Preferably, the brazing alloy according to the present invention is Mg-free.

[0044] Similarly, aluminium alloys with sacrificial anode effect, particularly alloys containing zinc such as the AA7072 alloy, may be used as a cladding on one side.

[0045] [Interlaminar aluminum alloy] Preferably, the strip according to the invention comprises, in mass %, Si: max 0.5%, more preferably max 0.2%, Fe: max 0.7%, more preferably max 0.3%, even more preferably max 0.2%; Mn: 0.3 to 1.4%, more preferably 0.6 to 0.8%, and according to one variant 1 to 1.3%; Cu: max 0.3%, preferably max 0.1%, even more preferably max 0.05%, Other elements: <0.05% each and <0.15% in total The rest is aluminum, and is clad on one or both sides with a so-called interlayer aluminium alloy disposed between the core and any brazing alloy.

[0046] Preferably, the interlayer aluminium alloy of the strip according to the invention contains, in mass %, Si<0.15%; Fe<0.2%; Cu<0.1%; Mn 0.6%-0.8%; Mg<0.02%; other elements <0.05% and total <0.15%; balance aluminium.

[0047] Preferably, the intercalated aluminium alloy is an alloy of the AA3xxx series.

[0048] [strip] The strip according to the invention is a strip known as a brazing strip, which can serve for the manufacture of various parts of heat exchangers, such as tubes, plates, collectors, etc.

[0049] [method] The present invention also provides - casting a core alloy plate; - optionally cladding with at least one brazing aluminium alloy and optionally with at least one interlayer aluminium alloy, - pre-heating to a temperature of 450-520°C, preferably with a holding step at the maximum temperature for less than 12 hours, more preferably less than 3 hours; - hot rolling at a temperature of 450-520°C without prior homogenization to a thickness of 2-6 mm; - cold rolling to the desired thickness, the thickness of the strip after cold rolling being preferably between 0.15 and 3 mm; and - an annealing step at a temperature between 240 and 450 °C, preferably between 240 and 380 °C, with a maintenance step at the maximum temperature for a period between 10 minutes and 15 hours, preferably between 20 minutes and 3 hours; The present invention is also directed to a method for producing the strip, comprising the successive steps of:

[0050] According to one variant, the invention also provides a method for producing a device comprising: - casting a core alloy plate; - homogenizing the plate at a temperature of 580-630°C for 1-24 hours; - optionally cladding with at least one brazing aluminium alloy and optionally with at least one interlayer aluminium alloy, - pre-heating to a temperature of 450-520°C, preferably with a holding step at the maximum temperature for less than 12 hours, more preferably less than 3 hours; - hot rolling the homogenized and optionally clad plate at a temperature of 450-520°C to a thickness of 2-6 mm; - cold rolling to the desired thickness, the thickness of the strip after cold rolling being preferably between 0.15 and 3 mm; and - an annealing step at a temperature between 240 and 450 °C, preferably between 240 and 380 °C, with a maintenance step at the maximum temperature for a period between 10 minutes and 15 hours, preferably between 20 minutes and 3 hours; The present invention also relates to a method for producing the strip according to the invention, comprising the successive steps of:

[0051] Preferably, in the method according to the invention there is no intermediate anneal.

[0052] The strip can be used annealed (temper O) by a final anneal at temperatures between 320 and 380 °C in a continuous or batch furnace if it is intended for parts with significant forming. This anneal leads to a recrystallization of the alloy and improves its formability. In other cases the strip is used in the work-hardened condition leading to better mechanical strength, such as tempers H14 or H24 (according to NF EN515 standard), which are tempers obtained by a recovery anneal at 250-300 °C that avoids recrystallization.

[0053] Prior to the application of the cladding material, homogenization of the core alloy plate can be carried out at temperatures between 580 and 630 °C. This homogenization favors the ductility of the rolled strip and is recommended if the strip is to be used in temper O. This homogenization favors the coalescence of Mn dispersoids.

[0054] [use] The invention is also directed to a heat exchanger, at least in part, made from the strip according to the invention.

[0055] The invention also relates to the use of the strip according to the invention for the manufacture of heat exchangers, said strip having improved corrosion resistance without deterioration of the mechanical strength or brazeability.

[0056] The strip according to the invention can be used in particular in the manufacture of automotive radiators, such as engine cooling radiators, oil radiators, heating radiators and intercoolers, and air conditioning systems. EXAMPLES

[0057] [Example 1] Four alloys were cast, the compositions of which, in mass percentage, are given in Table 1 below: Alloy A is a prior art core alloy; Alloys B and C are core alloys according to the present invention; Alloy D is brazing alloy AA4343.

[0058] [Table 1]

[0059] The alloys listed in Table 1 above were used to form a three-layer sandwich structure with a total thickness of 220 μm according to the following configuration: Brazing alloy (Alloy D - 10% of total thickness) Core alloy (Alloy A, B or C - 80% of total thickness) Brazing alloy (Alloy D - 10% of total thickness).

[0060] After casting and assembly of the layers, the sandwich structure was preheated at 500°C and hot rolled at this temperature to a total thickness of 3.5 mm. The sandwich structure was then cold rolled without intermediate annealing to a total thickness of 220 μm. Finally, the resulting strip was subjected to a recovery anneal at 240°C for 2 hours to obtain the metallurgical temper H24.

[0061] Brazing was then carried out in a Camlaw furnace at 600° C. for 2 minutes.

[0062] On the sandwich structures thus obtained, the pit depth was determined using the SWAAT test (sea water acetic acid test) according to ASTM G85A3, followed by photomicrographic observations using an optical microscope (magnification x100) after 4 weeks of exposure. The results are presented in Figure 1.

[0063] FIG. 1 shows that the core alloy according to the present invention can improve corrosion resistance compared to the prior art core alloy.

[0064] Meanwhile, the mechanical strength after brazing of alloys A, B and C listed in the above Table 1 was measured according to the ISO 6892-1 standard, and the obtained results are presented in Table 2 below.

[0065] [Table 2]

[0066] According to Table 2 above, the core alloy according to the present invention has comparable and even improved mechanical strength compared to the prior art core alloys.

[0067] [Example 2] Three alloys were cast, the compositions of which, in mass percentage, are given in Table 3 below: Alloy E is the core alloy according to the present invention; Alloy F is the core alloy according to the prior art; Alloy D is the brazing alloy AA4343.

[0068] [Table 3]

[0069] The alloys listed in Table 3 above were used to form a three-layer sandwich structure with a total thickness of 400 μm according to the following configuration: Brazing alloy (Alloy D - 7.5% of total thickness) Core alloy (Alloy E or F - 85% of total thickness) Brazing alloy (Alloy D - 7.5% of total thickness).

[0070] After casting, homogenization and assembly of the layers, the sandwich structure was preheated at 500°C and hot rolled at this temperature to a total thickness of 3.5 mm. The sandwich structure was then cold rolled without intermediate annealing to a total thickness of 400 μm. Finally, the obtained strip was subjected to annealing at 360°C for 1 hour to obtain the metallurgical quality O.

[0071] Brazing was then carried out in a Camlaw furnace at 600° C. for 2 minutes.

[0072] On the sandwich structures thus obtained, the pit depth was determined using the SWAAT test (sea water acetic acid test) according to ASTM G85A3, followed by photomicrographic observations using an optical microscope (magnification x 100) after 2 weeks of exposure, the results of which are presented in Figure 2.

[0073] FIG. 2 shows that the core alloy according to the present invention (especially containing 0.75-1.05% Cu) can improve the corrosion resistance compared to the core alloy according to the prior art.

Claims

1. - casting a core alloy plate; - optionally cladding with at least one brazing aluminium alloy and optionally at least one interlayer aluminium alloy, Preheating to a temperature of −450 to 520° C.; - hot rolling this plate, without prior homogenization, at a temperature between 450 and 520°C to a thickness of between 2 and 6 mm; - cold rolling to the desired thickness, the thickness of the strip after cold rolling being between 0.15 and 3 mm; and - an annealing step at a temperature between 240 and 450°C, with a hold at the maximum temperature for between 10 minutes and 15 hours; 1. A method for producing a strip intended for the manufacture of a brazed heat exchanger, having an aluminium alloy core with the following composition, in mass%, 0.10 to 0.30% Si, less than 0.20% Fe, 0.75 to 1.05% Cu, 1.2 to 1.7% Mn, less than 0.03% Mg, less than 0.1% Zn, less than 0.15% Ti, other elements each less than 0.05% and less than 0.15% in total, and the remainder being aluminium, comprising the successive steps of:

2. - casting a core alloy plate; - homogenizing the plate for 1 to 24 hours at a temperature between 580 and 630°C; - optionally cladding with at least one brazing aluminium alloy and optionally with at least one interlayer aluminium alloy, Preheating to a temperature of −450 to 520° C.; - hot rolling the homogenized and optionally clad plate at a temperature between 450 and 520°C to a thickness of between 2 and 6 mm; - cold rolling to the desired thickness, the thickness of the strip after cold rolling being between 0.15 and 3 mm; and - an annealing step at a temperature between 240 and 450°C, with a hold at the maximum temperature for between 10 minutes and 15 hours; 1. A method for producing a strip intended for the manufacture of a brazed heat exchanger, having an aluminium alloy core with the following composition, in mass%, 0.10 to 0.30% Si, less than 0.20% Fe, 0.75 to 1.05% Cu, 1.2 to 1.7% Mn, less than 0.03% Mg, less than 0.1% Zn, less than 0.15% Ti, other elements each less than 0.05% and less than 0.15% in total, and the remainder being aluminium, comprising the successive steps of:

3. 3. A method for producing a strip according to claim 1 or 2, characterized in that it is clad on one or both sides with an aluminium brazing alloy.

4. The brazing aluminum alloy comprises, in mass %, 5 to 13% Si; Maximum 1% Fe: Maximum 0.4% Cu, Mn up to 0.2% Maximum 0.3% Mg, Zn up to 0.2% Ti up to 0.30% Other elements, each less than 0.05% and total less than 0.15%; The rest is aluminum, The method for producing the strip according to claim 3, comprising:

5. A method for manufacturing a strip as claimed in any one of claims 1 to 4, characterized in that it is clad on one or both sides with an interlayer aluminium alloy disposed between the core and any brazing alloy.

6. The interlayer aluminum alloy comprises, in mass %, max 0.5% Si, max 0.7% Fe, 0.3 to 1.4% Mn, Maximum 0.3% Cu, Other elements, each less than 0.05% and total less than 0.15%; The rest is aluminum, The method for producing the strip according to claim 5, comprising:

7. 6. A method for producing strip according to claim 5, characterized in that the interlayer aluminium alloy consists, in mass %, of less than 0.15% Si, less than 0.2% Fe, less than 0.1% Cu, 0.6% to 0.8% Mn, less than 0.02% Mg, less than 0.05% other elements and less than 0.15% in total, the balance being aluminium.

Citation Information

Patent Citations

  • Process for improving the corrosion resistance of brazing sheet

    EP0326337A1

  • Brazing sheet

    EP0718072A1

  • Strip or tube for the fabrication of brazed heat exchangers

    EP1075935A1

  • Strip or tube for the fabrication of brazed heat exchangers

    EP1413427A2

  • Brazing sheet core alloy for heat exchanger

    EP2969308A2