Method for producing transparent conductive film

The transparent conductive film with controlled residual stresses and krypton incorporation addresses the issue of resistance fluctuations and dimensional changes, achieving stable and low-resistance performance.

JP7556912B2Active Publication Date: 2024-09-26NITTO DENKO CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2022074251
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-12-02
Filing Date
2022-04-28
Publication Date
2024-09-26
Estimated Expiration
2041-03-18

AI Technical Summary

Technical Problem

The manufacturing process of transparent conductive films faces challenges where high heating temperatures for crystallization lead to dimensional changes in the resin base film, causing cracks and undesirable fluctuations in the resistance value of the light-transmitting conductive layer.

Method used

A transparent conductive film structure with a transparent resin base material and a light-transmitting conductive layer, where the conductive layer has a specific ratio of compressive residual stresses in different in-plane directions, and incorporates krypton to stabilize the resistance value.

Benefits of technology

The film structure effectively suppresses fluctuations in resistance value and ensures stability by maintaining low resistance through controlled residual stress and crystal growth, reducing warping and enhancing durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007556912000008
    Figure 0007556912000008
  • Figure 0007556912000007
    Figure 0007556912000007
  • Figure 0007556912000005
    Figure 0007556912000005
Patent Text Reader

Abstract

A method for producing a transparent conductive film suitable for suppressing subsequent resistance fluctuations in a light-transmitting conductive layer is provided. [Solution] A transparent conductive film X produced by the present invention comprises a resin film 11 and a light-transmitting conductive layer 20, in this order in the thickness direction. The light-transmitting conductive layer 20 contains a conductive oxide containing In and Sn. The light-transmitting conductive layer 20 has a first compressive residual stress in a first in-plane direction perpendicular to the thickness direction D, and a second compressive residual stress smaller than the first compressive residual stress in a second in-plane direction perpendicular to both the thickness direction D and the first in-plane direction. The ratio of the second compressive residual stress to the first compressive residual stress is 0.82 or less. In the production method of the present invention, the light-transmitting conductive layer 20 of such a transparent conductive film X is formed by sputtering at a film formation pressure of 1 Pa or less.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a transparent conductive film. [Background technology]

[0002] Conventionally, a transparent conductive film having a transparent base film and a transparent conductive layer (light-transmitting conductive layer) in order in the thickness direction has been known. The light-transmitting conductive layer is used as a conductive film for patterning transparent electrodes in various devices such as liquid crystal displays, touch panels, and optical sensors. The light-transmitting conductive layer may also be used as an antistatic layer provided in a device. The light-transmitting conductive layer is formed, for example, by forming a film of a conductive oxide on a resin base film by a sputtering method. In the sputtering method, an inert gas such as argon is conventionally used as a sputtering gas for colliding with a target (a film-forming material supply material) to eject atoms on the target surface. The technology related to such a transparent conductive film is described, for example, in Patent Document 1 below. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Japanese Patent Application Publication No. 5-334924 Summary of the Invention [Problem to be solved by the invention]

[0004] In the manufacturing process of a transparent conductive film, a method may be used in which an amorphous light-transmitting conductive layer is formed on a substrate film, and then the light-transmitting conductive layer is heated to convert it to a crystalline state. In this case, the higher the heating temperature in the crystallization process, the lower the resistance value of the crystalline light-transmitting conductive layer that is formed.

[0005] On the other hand, since the transparent conductive film includes a resin substrate film, if the heating temperature in the crystallization process is excessively high, various problems occur due to dimensional changes in the resin substrate film, etc. (e.g., cracks in the light-transmitting conductive layer). If the heating temperature in the crystallization process is suppressed to avoid such problems, the resistance value of the crystalline light-transmitting conductive layer formed may not be sufficiently small. When a transparent conductive film having such a light-transmitting conductive layer undergoes a heating process in the manufacturing process of an apparatus, etc., including the film, the resistance value of the light-transmitting conductive layer of the transparent conductive film may vary (e.g., decrease). The variation in the resistance value of the light-transmitting conductive layer in the transparent conductive film after manufacturing is undesirable.

[0006] The present invention provides a transparent conductive film suitable for suppressing subsequent resistance fluctuation in a light-transmitting conductive layer. [Means for solving the problem]

[0007] The present invention [1] includes a transparent conductive film comprising a transparent resin substrate and a light-transmitting conductive layer in this order in the thickness direction, the light-transmitting conductive layer having a first compressive residual stress in a first in-plane direction perpendicular to the thickness direction, and a second compressive residual stress smaller than the first compressive residual stress in a second in-plane direction perpendicular to both the thickness direction and the first in-plane direction, and a ratio of the second compressive residual stress to the first compressive residual stress is 0.82 or less.

[0008] The present invention [2] includes the transparent conductive film according to the above [1], in which the light-transmitting conductive layer contains krypton.

[0009] The present invention [3] includes the transparent conductive film according to the above [1] or [2], in which the transparent resin substrate is not adjacent to a glass substrate.

[0010] The present invention [4] is characterized in that the light-transmitting conductive layer has a thickness of 2.2×10 -4 The transparent conductive film according to any one of the above [1] to [3] has a resistivity of less than Ω·cm.

[0011] The present invention [5] includes the transparent conductive film according to any one of the above [1] to [4], wherein the light-transmitting conductive layer has a thickness of 100 nm or more. Effect of the Invention

[0012] In the transparent conductive film of the present invention, the light-transmitting conductive layer has a first compressive residual stress in a first in-plane direction, a second compressive residual stress in a second in-plane direction perpendicular to the first in-plane direction that is smaller than the first compressive residual stress, and the ratio of the second compressive residual stress to the first compressive residual stress is 0.82 or less. Therefore, the transparent conductive film of the present invention is suitable for suppressing subsequent resistance value fluctuations in the light-transmitting conductive layer. [Brief description of the drawings]

[0013] [Figure 1] 1 is a schematic cross-sectional view of one embodiment of a transparent conductive film of the present invention. [Diagram 2] 2A and 2B are schematic cross-sectional views of modified transparent conductive films of the present invention, in which the light-transmitting conductive layer includes a first region and a second region in this order from the transparent resin substrate side, and in which the light-transmitting conductive layer includes a second region and a first region in this order from the transparent resin substrate side. [Diagram 3] 3 shows a method for producing the transparent conductive film shown in Fig. 1. Fig. 3A shows a step of preparing a resin film, Fig. 3B shows a step of forming a functional layer on the resin film, Fig. 3C shows a step of forming a light-transmitting conductive layer on the functional layer, and Fig. 3D shows a step of crystallizing the light-transmitting conductive layer. [Figure 4] This illustrates a case where the light-transmitting conductive layer in the transparent conductive film shown in FIG. 1 is patterned. [Diagram 5] 1 is a graph showing the relationship between the amount of oxygen introduced when forming a light-transmitting conductive layer by a sputtering method and the resistivity of the formed light-transmitting conductive layer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] 1 is a schematic cross-sectional view of a transparent conductive film X, which is one embodiment of the transparent conductive film of the present invention. The transparent conductive film X includes a transparent resin substrate 10 and a light-transmitting conductive layer 20, in this order, toward one side in a thickness direction D. The transparent conductive film X has a shape that spreads in a direction (plane direction) perpendicular to the thickness direction D. The transparent conductive film X is an element included in a touch sensor device, a light control element, a photoelectric conversion element, a heat ray control member, an antenna member, an electromagnetic wave shielding member, a heater member, a lighting device, an image display device, and the like.

[0015] In this embodiment, the transparent resin substrate 10 includes a resin film 11 and a functional layer 12 in this order toward one side in the thickness direction D. The transparent resin substrate 10 has a shape that spreads in a direction (plane direction) perpendicular to the thickness direction D. Specifically, the transparent resin substrate 10 extends in a first in-plane direction perpendicular to the thickness direction D, and extends in a second in-plane direction perpendicular to both the thickness direction D and the first in-plane direction. In this embodiment, the transparent resin substrate 10 has an elongated shape that is long in the first in-plane direction. In this embodiment, the first in-plane direction is a resin flow direction (MD direction) during the manufacturing process of the resin film 11 included in the transparent resin substrate 10, and the second in-plane direction is a width direction (TD direction) perpendicular to both the resin flow direction and the thickness direction D. In this embodiment, the first in-plane direction is the direction in which the thermal dimensional change rate (maximum thermal shrinkage rate) of the transparent resin substrate 10 is maximum, and the second in-plane direction is the direction perpendicular to each of the first in-plane direction and the thickness direction D. The direction in which the thermal dimensional change rate of the transparent resin substrate 10 is maximum can be obtained by measuring the dimensional change rate before and after heating in axial directions at 15° intervals from an axis extending in any direction in the transparent resin substrate 10 as a reference axis (0°). As the heating temperature for obtaining the thermal dimensional change rate, a suitable temperature can be set according to the heat resistance temperature of the resin film 11. When the resin film 11 is polyethylene terephthalate (PET), for example, a heating temperature of 150° C. can be adopted, and when the resin film 11 is a cycloolefin polymer, for example, a heating temperature of 110° C. can be adopted. The heating time is, for example, one hour.

[0016] The resin film 11 is a flexible, transparent resin film. The resin film 11 has a shape that extends in a direction (plane direction) perpendicular to the thickness direction D. Specifically, the resin film 11 extends in a first in-plane direction perpendicular to the thickness direction D, and extends in a second in-plane direction perpendicular to both the thickness direction D and the first in-plane direction. In this embodiment, the resin film 11 has an elongated shape that is long in the first in-plane direction. In this embodiment, the first in-plane direction is the above-mentioned MD direction, and the second in-plane direction is the above-mentioned TD direction.

[0017] Examples of the material of the resin film 11 include polyester resin, polyolefin resin, acrylic resin, polycarbonate resin, polyethersulfone resin, polyarylate resin, melamine resin, polyamide resin, polyimide resin, cellulose resin, and polystyrene resin. Examples of the polyester resin include polyethylene terephthalate (PET), polybutylene terephthalate, and polyethylene naphthalate. Examples of the polyolefin resin include polyethylene, polypropylene, and cycloolefin polymer. Examples of the acrylic resin include polymethacrylate. As the material of the resin film 11, for example, from the viewpoint of transparency and strength, polyester resin is preferably used, and PET is more preferably used.

[0018] The surface of the resin film 11 facing the functional layer 12 may be subjected to a surface modification treatment. Examples of the surface modification treatment include corona treatment, plasma treatment, ozone treatment, primer treatment, glow treatment, and coupling agent treatment.

[0019] The thickness of the resin film 11 is preferably 1 μm or more, more preferably 10 μm or more, and even more preferably 30 μm or more. The thickness of the resin film 11 is preferably 300 μm or less, more preferably 200 μm or less, even more preferably 100 μm or less, and particularly preferably 75 μm or less. These configurations regarding the thickness of the resin film 11 are suitable for ensuring the handleability of the transparent conductive film X.

[0020] The total light transmittance (JIS K 7375-2008) of the resin film 11 is preferably 60% or more, more preferably 80% or more, and even more preferably 85% or more. Such a configuration is suitable for ensuring the transparency required of the transparent conductive film X when the transparent conductive film X is provided in a touch sensor device, a light control element, a photoelectric conversion element, a heat ray control member, an antenna member, an electromagnetic wave shielding member, a heater member, a lighting device, an image display device, and the like. The total light transmittance of the resin film 11 is, for example, 100% or less.

[0021] In this embodiment, the functional layer 12 is located on one surface of the resin film 11 in the thickness direction D. In this embodiment, the functional layer 12 is a hard coat layer that makes it difficult for scratches to form on the exposed surface (the upper surface in FIG. 1 ) of the light-transmitting conductive layer 20.

[0022] The hard coat layer is a cured product of a curable resin composition. Examples of the resin contained in the curable resin composition include polyester resin, acrylic resin, urethane resin, amide resin, silicone resin, epoxy resin, and melamine resin. Examples of the curable resin composition include an ultraviolet-curable resin composition and a thermosetting resin composition. Since the curable resin composition can be cured without high-temperature heating, and therefore is useful for improving the production efficiency of the transparent conductive film X, an ultraviolet-curable resin composition is preferably used as the curable resin composition. Specific examples of the ultraviolet-curable resin composition include the hard coat layer-forming composition described in JP 2016-179686 A.

[0023] The surface of the functional layer 12 facing the light-transmitting conductive layer 20 may be subjected to a surface modification treatment. Examples of the surface modification treatment include corona treatment, plasma treatment, ozone treatment, primer treatment, glow treatment, and coupling agent treatment.

[0024] The thickness of the functional layer 12 as a hard coat layer is preferably 0.1 μm or more, more preferably 0.5 μm or more, and even more preferably 1 μm or more. Such a configuration is suitable for achieving sufficient scratch resistance in the light-transmitting conductive layer 20. From the viewpoint of ensuring the transparency of the functional layer 12, the thickness of the functional layer 12 as a hard coat layer is preferably 10 μm or less, more preferably 5 μm or less, and even more preferably 3 μm or less.

[0025] The thickness of the transparent resin substrate 10 is preferably 1 μm or more, more preferably 10 μm or more, even more preferably 15 μm or more, and particularly preferably 30 μm or more. The thickness of the transparent resin substrate 10 is preferably 310 μm or less, more preferably 210 μm or less, even more preferably 110 μm or less, and particularly preferably 80 μm or less. These configurations regarding the thickness of the transparent resin substrate 10 are suitable for ensuring the handleability of the transparent conductive film X.

[0026] The total light transmittance (JIS K 7375-2008) of the transparent resin substrate 10 is preferably 60% or more, more preferably 80% or more, and even more preferably 85% or more. Such a configuration is suitable for ensuring the transparency required of the transparent conductive film X when the transparent conductive film X is provided in a touch sensor device, a light control element, a photoelectric conversion element, a heat ray control member, an antenna member, an electromagnetic wave shielding member, a heater member, a lighting device, an image display device, and the like. The total light transmittance of the transparent resin substrate 10 is, for example, 100% or less.

[0027] In this embodiment, the transparent conductive film X does not include a glass substrate. The transparent resin substrate 10 is not adjacent to a glass substrate. This configuration is suitable for ensuring the flexibility of the transparent conductive film X.

[0028] In this embodiment, the light-transmitting conductive layer 20 is located on one surface of the resin film 11 in the thickness direction D. The light-transmitting conductive layer 20 is a crystalline film that has both light transparency and conductivity.

[0029] The light-transmitting conductive layer 20 is a layer formed from a light-transmitting conductive material. The light-transmitting conductive material contains, for example, a conductive oxide as a main component.

[0030] Examples of the conductive oxide include metal oxides containing at least one metal or metalloid selected from the group consisting of In, Sn, Zn, Ga, Sb, Ti, Si, Zr, Mg, Al, Au, Ag, Cu, Pd, and W. Specifically, examples of the conductive oxide include indium-containing conductive oxides and antimony-containing conductive oxides. Examples of the indium-containing conductive oxide include indium tin composite oxide (ITO), indium zinc composite oxide (IZO), indium gallium composite oxide (IGO), and indium gallium zinc composite oxide (IGZO). Examples of the antimony-containing conductive oxide include antimony tin composite oxide (ATO). From the viewpoint of achieving high transparency and good electrical conductivity, the conductive oxide is preferably an indium-containing conductive oxide, and more preferably ITO. This ITO may contain a metal or metalloid other than In and Sn in an amount less than the respective contents of In and Sn.

[0031] When ITO is used as the conductive oxide, the indium oxide (In 2 O 3 ) and tin oxide (SnO 2 The ratio of the content of tin oxide to the total content of indium atoms in the ITO used (number of tin atoms / number of indium atoms) is preferably 0.001 or more, more preferably 0.03 or more, even more preferably 0.05 or more, and particularly preferably 0.07 or more. Such a configuration is suitable for ensuring the durability of the light-transmitting conductive layer 20. In addition, the ratio of the number of tin atoms to the number of indium atoms in the ITO used (number of tin atoms / number of indium atoms) is preferably 0.001 or more, more preferably 0.03 or more, even more preferably 0.05 or more, and particularly preferably 0.07 or more. Such a configuration is suitable for ensuring the durability of the light-transmitting conductive layer 20. In addition, the ratio of the number of indium oxide (In 2 O 3 ) and tin oxide (SnO 2The ratio of the content of tin oxide to the total content of indium atoms (SnO 2 ) is preferably 15% by mass or less, more preferably 13% by mass or less, and even more preferably 12% by mass or less. The ratio of the number of tin atoms to the number of indium atoms (SnO 2 ) in the ITO used is preferably 0.16 or less, more preferably 0.14 or less, and even more preferably 0.13 or less. These configurations are suitable for obtaining a light-transmitting conductive layer 20 that is easily crystallized by heating. The ratio of the number of tin atoms to the number of indium atoms in ITO is determined, for example, by specifying the abundance ratio of indium atoms and tin atoms for the measurement object by X-ray photoelectron spectroscopy. The above-mentioned content ratio of tin oxide in ITO is determined, for example, from the abundance ratio of indium atoms and tin atoms thus specified. The above-mentioned content ratio of tin oxide in ITO is determined, for example, from the abundance ratio of indium atoms and tin atoms thus specified. The above-mentioned content ratio of tin oxide in ITO is determined, for example, from the abundance ratio of tin atoms (SnO 2 ) in the ITO target used in sputtering film formation. 2 ) content ratio.

[0032] The light-transmitting conductive layer 20 may contain rare gas atoms. Examples of rare gas atoms include argon (Ar), krypton (Kr), and xenon (Xe). In this embodiment, the rare gas atoms in the light-transmitting conductive layer 20 are derived from rare gas atoms used as a sputtering gas in a sputtering method described later for forming the light-transmitting conductive layer 20. In this embodiment, the light-transmitting conductive layer 20 is a film (sputtered film) formed by a sputtering method.

[0033] The content ratio of rare gas atoms in the light-transmitting conductive layer 20 (for example, the ratio of the total content of Kr and Ar) is preferably 1.2 atomic % or less, more preferably 1.1 atomic % or less, even more preferably 1.0 atomic % or less, even more preferably 0.8 atomic % or less, even more preferably 0.5 atomic % or less, especially preferably 0.4 atomic % or less, very preferably 0.3 atomic % or less, and particularly preferably 0.2 atomic % or less, in the entire region in the thickness direction D. Such a configuration is suitable for forming large crystal grains that realize good crystal growth when the amorphous light-transmitting conductive layer (light-transmitting conductive layer 20' described later) is crystallized by heating to form the light-transmitting conductive layer 20 in the manufacturing process of the transparent conductive film X, and is therefore suitable for obtaining a light-transmitting conductive layer 20 with low resistance (the larger the crystal grains in the light-transmitting conductive layer 20, the lower the resistance of the light-transmitting conductive layer 20). Furthermore, the light-transmitting conductive layer 20 includes a region in which the rare gas atom content is, for example, 0.0001 atomic % or more in at least a portion in the thickness direction D. The rare gas atom content in the light-transmitting conductive layer 20 is preferably, for example, 0.0001 atomic % or more throughout the entire region in the thickness direction D.

[0034] The presence or absence and content of rare gas atoms such as Kr in the light-transmitting conductive layer 20 is identified, for example, by Rutherford backscattering spectrometry, which will be described later in the Examples. The presence or absence of rare gas atoms such as Kr in the light-transmitting conductive layer 20 is identified, for example, by X-ray fluorescence analysis, which will be described later in the Examples. When the content of rare gas atoms in the light-transmitting conductive layer to be analyzed cannot be quantified because it is not equal to or greater than the detection limit (lower limit) by Rutherford backscattering analysis, and the presence of rare gas atoms is identified by X-ray fluorescence analysis, the light-transmitting conductive layer is determined to include a region in which the content of rare gas atoms such as Kr is 0.0001 atomic % or more.

[0035] From the viewpoint of reducing the manufacturing cost of the transparent conductive film X, the light-transmitting conductive layer 20 preferably does not contain Xe.

[0036] From the viewpoint of achieving favorable crystal growth and forming large crystal grains when forming the light-transmitting conductive layer 20 in the manufacturing process of the transparent conductive film X, the light-transmitting conductive layer 20 preferably contains Kr, and more preferably contains only Kr, as a rare gas atom. The configuration suitable for forming large crystal grains in the light-transmitting conductive layer 20 is suitable for achieving low resistance of the light-transmitting conductive layer 20. In addition, the configuration suitable for forming large crystal grains in the light-transmitting conductive layer 20 is suitable for reducing the net compressive residual stress in the light-transmitting conductive layer 20 to be formed.

[0037] The light-transmitting conductive layer 20 includes a region in a part of the thickness direction D in which the Kr content is preferably 1.0 atomic % or less, more preferably 0.7 atomic % or less, even more preferably 0.5 atomic % or less, particularly preferably 0.3 atomic % or less, very preferably 0.2 atomic % or less, and particularly preferably less than 0.1 atomic %. The Kr content in the region is, for example, 0.0001 atomic % or more. Preferably, the light-transmitting conductive layer 20 satisfies such a Kr content in the entire region in the thickness direction D. Specifically, the Kr content in the light-transmitting conductive layer 20 is preferably 1.0 atomic % or less, more preferably 0.7 atomic % or less, even more preferably 0.5 atomic % or less, particularly preferably 0.3 atomic % or less, very preferably 0.2 atomic % or less, and particularly preferably less than 0.1 atomic % in the entire region in the thickness direction D. These configurations are suitable for achieving good crystal growth and forming large crystal grains when an amorphous light-transmitting conductive layer (light-transmitting conductive layer 20′ described below) is crystallized by heating to form the light-transmitting conductive layer 20 during the manufacturing process of the transparent conductive film X, and are therefore suitable for obtaining a light-transmitting conductive layer 20 with low resistance (the larger the crystal grains in the light-transmitting conductive layer 20, the lower the resistance of the light-transmitting conductive layer 20).

[0038] The Kr content in the light-transmitting conductive layer 20 may be non-uniform in the thickness direction D. For example, in the thickness direction D, the Kr content may gradually increase or decrease as it moves away from the transparent resin substrate 10. Alternatively, in the thickness direction D, a partial region in which the Kr content gradually increases as it moves away from the transparent resin substrate 10 may be located on the transparent resin substrate 10 side, and a partial region in which the Kr content gradually decreases as it moves away from the transparent resin substrate 10 may be located on the opposite side to the transparent resin substrate 10. Alternatively, in the thickness direction D, a partial region in which the Kr content gradually decreases as it moves away from the transparent resin substrate 10 may be located on the transparent resin substrate 10 side, and a partial region in which the Kr content gradually increases as it moves away from the transparent resin substrate 10 may be located on the opposite side to the transparent resin substrate 10.

[0039] The light-transmitting conductive layer 20 may contain Kr in a part of the region in the thickness direction D, as exemplified in FIG. 2. FIG. 2A shows a case where the light-transmitting conductive layer 20 includes a first region 21 and a second region 22 in this order from the transparent resin substrate 10 side. The first region 21 contains Kr. The second region 22 does not contain Kr, and contains, for example, a rare gas atom other than Kr. FIG. 2B shows a case where the light-transmitting conductive layer 20 includes the second region 22 and the first region 21 in this order from the transparent resin substrate 10 side. In FIG. 2, the boundary between the first region 21 and the second region 22 is depicted by a virtual line, but in cases where the first region 21 and the second region 22 are not significantly different in composition other than the rare gas atom whose content is small, the boundary between the first region 21 and the second region 22 may not be clearly distinguished.

[0040] From the viewpoint of reducing the resistivity while reducing the compressive residual stress in the light-transmitting conductive layer 20, the light-transmitting conductive layer 20 includes a first region 21 (Kr-containing region) and a second region 22 (Kr-free region) in this order from the transparent resin substrate 10 side.

[0041] When the light-transmitting conductive layer 20 includes the first region 21 and the second region 22, the ratio of the thickness of the first region 21 to the total thickness of the first region 21 and the second region 22 is preferably 1% or more, more preferably 20% or more, even more preferably 30% or more, even more preferably 40% or more, and particularly preferably 50% or more. This ratio is less than 100%. Moreover, the ratio of the thickness of the second region 22 to the total thickness of the first region 21 and the second region 22 is preferably 99% or less, more preferably 80% or less, even more preferably 70% or less, even more preferably 60% or less, and particularly preferably 50% or less. When the light-transmitting conductive layer 20 includes the first region 21 and the second region 22, the configuration regarding the ratio of the thickness of each of the first region 21 and the second region 22 is preferable from the viewpoint of simultaneously achieving a reduction in compressive residual stress and a reduction in resistivity in the light-transmitting conductive layer 20.

[0042] The content of Kr in the first region 21 is preferably 1.0 atomic % or less, more preferably 0.7 atomic % or less, even more preferably 0.5 atomic % or less, even more preferably 0.3 atomic % or less, still more preferably 0.2 atomic %, and particularly preferably less than 0.1 atomic % in the entire area of ​​the first region 21 in the thickness direction D. Such a configuration is suitable for achieving the above-mentioned low resistance and reduction of compressive residual stress in the light transmissible conductive layer 20. The content of Kr in the first region 21 is, for example, 0.0001 atomic % or more in the entire area of ​​the first region 21 in the thickness direction D.

[0043] The Kr content in the first region 21 may be non-uniform in the thickness direction D of the first region 21. For example, in the thickness direction D of the first region 21, the Kr content may gradually increase or decrease as it moves away from the transparent resin substrate 10. Alternatively, in the thickness direction D of the first region 21, a partial region in which the Kr content gradually increases as it moves away from the transparent resin substrate 10 may be located on the transparent resin substrate 10 side, and a partial region in which the Kr content gradually decreases as it moves away from the transparent resin substrate 10 may be located on the opposite side to the transparent resin substrate 10. Alternatively, in the thickness direction D of the first region 21, a partial region in which the Kr content gradually decreases as it moves away from the transparent resin substrate 10 may be located on the transparent resin substrate 10 side, and a partial region in which the Kr content gradually increases as it moves away from the transparent resin substrate 10 may be located on the opposite side to the transparent resin substrate 10.

[0044] The thickness of the light-transmitting conductive layer 20 is, for example, 10 nm or more. The thickness of the light-transmitting conductive layer 20 is preferably more than 40 nm, more preferably 100 nm or more, even more preferably 110 nm or more, and even more preferably 120 nm or more. Such a configuration is suitable for reducing the resistance of the light-transmitting conductive layer 20. In addition, the thickness of the light-transmitting conductive layer 20 is, for example, 1000 nm or less, preferably less than 300 nm, more preferably 250 nm or less, even more preferably 200 nm or less, even more preferably 160 nm or less, particularly preferably less than 150 nm, and most preferably 148 nm or less. Such a configuration is suitable for suppressing warping of the transparent conductive film X.

[0045] The surface resistance of the light-transmitting conductive layer 20 is, for example, 200Ω / □ or less, preferably 100Ω / □ or less, more preferably 50Ω / □ or less, even more preferably 15Ω / □ or less, even more preferably 15Ω / □ or less, and particularly preferably 13Ω / □ or less. The surface resistance of the light-transmitting conductive layer 20 is, for example, 1Ω / □ or more. These configurations regarding the surface resistance are suitable for ensuring the low resistance required of the light-transmitting conductive layer 20 when the transparent conductive film X is provided in a touch sensor device, a light control element, a photoelectric conversion element, a heat ray control member, an antenna member, an electromagnetic wave shielding member, a heater member, a lighting device, and an image display device. The surface resistance can be measured by a four-terminal method in accordance with JIS K7194.

[0046] The resistivity of the light-transmitting conductive layer 20 is, for example, 2.5×10 -4 Ω cm or less, preferably 2.2×10 -4 Less than Ω cm, preferably less than 2×10 -4 Ω cm or less, more preferably 1.9×10 -4 Ω cm or less, particularly preferably 1.8×10 -4 The resistivity of the light-transmitting conductive layer 20 is preferably 0.1×10 -4 Ω·cm or more, preferably 0.5×10 -4 Ω cm or more, more preferably 1.0×10 -4 Ω·cm or more. These configurations regarding the resistivity are suitable for ensuring the low resistance required for the light-transmitting conductive layer 20 when the transparent conductive film X is provided in a touch sensor device, a light control element, a photoelectric conversion element, a heat ray control member, an antenna member, an electromagnetic wave shielding member, a heater member, a lighting device, an image display device, and the like. The resistivity is calculated by multiplying the surface resistance by the thickness. The resistivity can be controlled, for example, by adjusting the rare gas atom content ratio in the light-transmitting conductive layer 20 and adjusting various conditions when the light-transmitting conductive layer 20 is formed by sputtering. The conditions include, for example, the temperature of the base (the transparent resin substrate 10 in this embodiment) on which the light-transmitting conductive layer 20 is formed, the amount of oxygen introduced into the film formation chamber, the air pressure in the film formation chamber, and the horizontal magnetic field strength above the target.

[0047] The total light transmittance (JIS K 7375-2008) of the light-transmitting conductive layer 20 is preferably 60% or more, more preferably 80% or more, and even more preferably 85% or more. Such a configuration is suitable for ensuring the transparency of the light-transmitting conductive layer 20. The total light transmittance of the light-transmitting conductive layer 20 is, for example, 100% or less.

[0048] The light-transmitting conductive layer can be determined to be crystalline, for example, as follows. First, the light-transmitting conductive layer (light-transmitting conductive layer 20 on transparent resin substrate 10 in transparent conductive film X) is immersed in hydrochloric acid with a concentration of 5% by mass at 20° C. for 15 minutes. Next, the light-transmitting conductive layer is washed with water and then dried. Next, the resistance between a pair of terminals separated by a distance of 15 mm (terminal resistance) is measured on the exposed plane of the light-transmitting conductive layer (the surface of light-transmitting conductive layer 20 on the opposite side to transparent resin substrate 10 in transparent conductive film X). In this measurement, if the terminal resistance is 10 kΩ or less, the light-transmitting conductive layer is crystalline. In addition, the light-transmitting conductive layer can be determined to be crystalline by observing the presence of crystal grains in the light-transmitting conductive layer in a planar view using a transmission electron microscope.

[0049] The light-transmitting conductive layer 20 has a first compressive residual stress in a first in-plane direction, and a second compressive residual stress in a second in-plane direction that is smaller than the first compressive residual stress. That is, in the light-transmitting conductive layer 20, the compressive residual stress in the second in-plane direction perpendicular to the first in-plane direction is smaller than the compressive residual stress in at least one direction (first in-plane direction) in the plane of the layer 20. In this embodiment, the first in-plane direction is the above-mentioned MD direction, and the second in-plane direction is the above-mentioned TD direction (the first in-plane direction is perpendicular to the thickness direction D, and the second in-plane direction is perpendicular to both the thickness direction D and the first in-plane direction).

[0050] The first compressive residual stress is preferably 620 MPa or less, more preferably 600 MPa or less, and even more preferably 550 MPa or less. The first compressive residual stress is, for example, 1 MPa or more. The second compressive residual stress is, as long as it is smaller than the first compressive residual stress, preferably 530 MPa or less, more preferably 500 MPa or less, and even more preferably 450 MPa or less. The second compressive residual stress is, for example, 1 MPa or more, as long as it is smaller than the first compressive residual stress. These configurations are suitable for reducing the net internal stress in the light-transmitting conductive layer 20. Being suitable for reducing the compressive residual stress of the light-transmitting conductive layer 20 is suitable for suppressing warpage in the transparent conductive film X to be manufactured.

[0051] The ratio of the second compressive residual stress to the first compressive residual stress is 0.82 or less, and preferably 0.8 or less. The ratio is, for example, 0.1 or more, preferably 0.3 or more, and more preferably 0.4 or more. A configuration in which the second compressive residual stress in the in-plane second direction (TD direction in this embodiment) is smaller than the first compressive residual stress in the in-plane first direction (MD direction in this embodiment) to this extent helps to achieve high crystal stability.

[0052] The transparent conductive film X is produced, for example, as follows.

[0053] First, as shown in FIG. 3A, a resin film 11 is prepared.

[0054] 3B, a functional layer 12 is formed on one surface of the resin film 11 in the thickness direction D. By forming the functional layer 12 on the resin film 11, a transparent resin substrate 10 is produced.

[0055] The functional layer 12 as a hard coat layer can be formed by applying a curable resin composition onto the resin film 11 to form a coating film, and then curing the coating film. When the curable resin composition contains an ultraviolet-curable resin, the coating film is cured by ultraviolet irradiation. When the curable resin composition contains a thermosetting resin, the coating film is cured by heating.

[0056] The exposed surface of the functional layer 12 formed on the resin film 11 is subjected to a surface modification treatment as necessary. When a plasma treatment is used as the surface modification treatment, for example, argon gas is used as an inert gas. The discharge power in the plasma treatment is, for example, 10 W or more and, for example, 5000 W or less.

[0057] Next, as shown in Fig. 3C, an amorphous light-transmitting conductive layer 20' is formed on the transparent resin substrate 10 (film formation process). Specifically, a material is formed on the functional layer 12 of the transparent resin substrate 10 by a sputtering method to form an amorphous light-transmitting conductive layer 20'. The light-transmitting conductive layer 20' is an amorphous film that has both light transparency and conductivity (the light-transmitting conductive layer 20' is converted into a crystalline light-transmitting conductive layer 20 by heating in a crystallization process described later).

[0058] In the sputtering method, it is preferable to use a sputtering deposition apparatus capable of performing a film formation process by a roll-to-roll method. When using a sputtering deposition apparatus of the roll-to-roll method in the manufacture of the transparent conductive film X, a material is deposited on the transparent resin substrate 10 while the long transparent resin substrate 10 is running from a pay-out roll to a take-up roll provided in the apparatus, to form the light-transmitting conductive layer 20'. In addition, in the sputtering method, a sputtering deposition apparatus having one deposition chamber may be used, or a sputtering deposition apparatus having multiple deposition chambers arranged in order along the running path of the transparent resin substrate 10 may be used (when forming the light-transmitting conductive layer 20' including the above-mentioned first region 21 and second region 22, a sputtering deposition apparatus having two or more deposition chambers is used).

[0059] Specifically, in the sputtering method, a sputtering gas (inert gas) is introduced under vacuum conditions into a deposition chamber of a sputter deposition apparatus, while a negative voltage is applied to a target placed on a cathode in the deposition chamber. This generates a glow discharge to ionize gas atoms, and the gas ions collide with the target surface at high speed to eject target material from the target surface, and the ejected target material is deposited on the functional layer 12 of the transparent resin substrate 10.

[0060] The material of the target placed on the cathode in the film formation chamber is the conductive oxide described above for the light-transmitting conductive layer 20, preferably an indium-containing conductive oxide, and more preferably ITO. When ITO is used, the ratio of the tin oxide content to the total content of tin oxide and indium oxide in the ITO is preferably 0.1 mass% or more, more preferably 1 mass% or more, even more preferably 3 mass% or more, still more preferably 5 mass% or more, particularly preferably 7 mass% or more, and is preferably 15 mass% or less, more preferably 13 mass% or less, and even more preferably 12 mass% or less.

[0061] The sputtering method is preferably a reactive sputtering method, in which a reactive gas is introduced into the deposition chamber in addition to the sputtering gas.

[0062] In the case of forming a light-transmitting conductive layer 20' containing rare gas atoms over the entire area in the thickness direction D (first case), the gas introduced into one or more deposition chambers of the sputtering deposition apparatus contains a sputtering gas and oxygen as a reactive gas. In this embodiment, rare gas atoms are used as the sputtering gas. Examples of rare gas atoms include Ar, Kr, and Xe, and Kr is preferably used. When the sputtering gas contains an inert gas other than Kr, the content is preferably 80% by volume or less, more preferably 50% by volume or less.

[0063] When forming the light-transmitting conductive layer 20' including the above-mentioned first region 21 and second region 22 (second case), the gas introduced into the film formation chamber for forming the first region 21 contains Kr as a sputtering gas and oxygen as a reactive gas. The sputtering gas may contain an inert gas other than Kr. The content ratio of the inert gas other than Kr in the sputtering gas is the same as the content ratio described above in the first case.

[0064] In the second case, the gas introduced into the deposition chamber for forming the second region 22 contains an inert gas other than Kr as a sputtering gas and oxygen as a reactive gas. Examples of the inert gas other than Kr include Ar and Xe, and preferably Ar is used.

[0065] In the reactive sputtering method, the ratio of the amount of oxygen introduced to the total amount of sputtering gas and oxygen introduced into the film formation chamber is, for example, 0.01 flow % or more and, for example, 15 flow % or less.

[0066] The air pressure in the film formation chamber during film formation by sputtering (sputter film formation) is, for example, 0.02 Pa or more and, for example, 1 Pa or less.

[0067] The temperature of the transparent resin substrate 10 during sputtering deposition is, for example, 100° C. or lower. In order to suppress outgassing from the transparent resin substrate 10 and thermal expansion of the transparent resin substrate 10 during sputtering deposition, it is preferable to cool the transparent resin substrate 10. The suppression of outgassing and thermal expansion helps to achieve high crystal stability in the light-transmitting conductive layer 20. From this perspective, the temperature of the transparent resin substrate 10 during sputtering deposition is preferably 20° C. or lower, more preferably 10° C. or lower, even more preferably 5° C. or lower, particularly preferably 0° C. or lower, and is, for example, −50° C. or higher, preferably −20° C. or higher, more preferably −10° C. or higher, and even more preferably −7° C. or higher.

[0068] Examples of the power source for applying voltage to the target include a DC power source, an AC power source, an MF power source, and an RF power source. The power source may be a combination of a DC power source and an RF power source. The absolute value of the discharge voltage during sputtering is, for example, 50V or more and, for example, 500V or less.

[0069] In the present manufacturing method, next, as shown in FIG. 3D, the light-transmitting conductive layer 20 is converted (crystallized) from amorphous to crystalline by heating (crystallization step). Examples of heating means include an infrared heater and an oven (heat medium heating oven, hot air heating oven). The environment during heating may be either a vacuum environment or an air environment. Preferably, heating is performed in the presence of oxygen. From the viewpoint of ensuring a high crystallization rate, the heating temperature is, for example, 100° C. or higher, preferably 120° C. or higher. From the viewpoint of suppressing the influence of heating on the transparent resin substrate 10, the heating temperature is, for example, less than 200° C., preferably 180° C. or lower, more preferably 170° C. or lower, and even more preferably 165° C. or lower. The heating time is, for example, 10 hours or shorter, preferably 200 minutes or shorter, more preferably 90 minutes or shorter, and even more preferably 60 minutes or shorter, and also, for example, 1 minute or longer, preferably 5 minutes or longer.

[0070] After the temperature is returned to room temperature after the heating in this step, the transparent resin substrate 10 shrinks. The light-transmitting conductive layer 20 containing Kr is suitable for appropriately shrinking the light-transmitting conductive layer 20 on the transparent resin substrate 10 that shrinks in the state after the temperature is returned to room temperature (the preferred Kr content in the light-transmitting conductive layer 20 is as described above). The shrinkage of the light-transmitting conductive layer 20 after the temperature is returned to room temperature helps to reduce the compressive residual stress in the light-transmitting conductive layer 20.

[0071] In this manner, the transparent conductive film X is produced.

[0072] The light-transmitting conductive layer 20 in the transparent conductive film X may be patterned as shown in FIG. 4. The light-transmitting conductive layer 20 can be patterned by etching the light-transmitting conductive layer 20 through a predetermined etching mask. The patterning of the light-transmitting conductive layer 20 may be performed before or after the above-mentioned crystallization step. The patterned light-transmitting conductive layer 20 functions as, for example, a wiring pattern.

[0073] As described above, the transparent conductive film X has a light-transmitting conductive layer 20 on a transparent resin substrate 10, which has a first compressive residual stress in a first in-plane direction, a second compressive residual stress in a second in-plane direction (orthogonal to the first in-plane direction) that is smaller than the first compressive residual stress, and the ratio of the second compressive residual stress to the first compressive residual stress is 0.82 or less, preferably 0.8 or less. Such a configuration is suitable for realizing high crystal stability in the light-transmitting conductive layer 20. That is, in the transparent conductive film X, a configuration in which the second compressive residual stress in the second in-plane direction is smaller than the first compressive residual stress in the first in-plane direction is suitable for suppressing subsequent resistance value fluctuations of the light-transmitting conductive layer 20 even in the transparent conductive film X in which the crystalline light-transmitting conductive layer 20 is formed through a crystallization process at a relatively low temperature as described above. Specifically, this is as shown in the examples and comparative examples described below.

[0074] In the transparent conductive film X, the functional layer 12 may be an adhesion improving layer for realizing high adhesion of the light-transmitting conductive layer 20 to the transparent resin substrate 10. The configuration in which the functional layer 12 is an adhesion improving layer is suitable for ensuring adhesion between the transparent resin substrate 10 and the light-transmitting conductive layer 20.

[0075] The functional layer 12 may be an index-matching layer for adjusting the reflectance of the surface (one surface in the thickness direction D) of the transparent resin substrate 10. The configuration in which the functional layer 12 is an index-matching layer is suitable for making the pattern shape of the light-transmitting conductive layer 20 on the transparent resin substrate 10 less visible when the light-transmitting conductive layer 20 on the transparent resin substrate 10 is patterned.

[0076] The functional layer 12 may be a peelable functional layer for making it practically possible to peel the light-transmitting conductive layer 20 from the transparent resin substrate 10. The configuration in which the functional layer 12 is a peelable functional layer is suitable for peeling the light-transmitting conductive layer 20 from the transparent resin substrate 10 and transferring the light-transmitting conductive layer 20 to another member.

[0077] The functional layer 12 may be a composite layer in which a plurality of layers are arranged in the thickness direction D. The composite layer preferably includes two or more layers selected from the group consisting of a hard coat layer, an adhesion improving layer, a refractive index adjustment layer, and a release functional layer. Such a configuration is suitable for the functional layer 12 to exhibit the above-mentioned functions of each selected layer in a composite manner. In a preferred embodiment, the functional layer 12 includes an adhesion improving layer, a hard coat layer, and a refractive index adjustment layer on the resin film 11, in this order toward one side of the thickness direction D. In another preferred embodiment, the functional layer 12 includes a release functional layer, a hard coat layer, and a refractive index adjustment layer on the resin film 11, in this order toward one side of the thickness direction D.

[0078] The transparent conductive film X is used in a state where it is fixed to an article and the light-transmitting conductive layer 20 is patterned as necessary. The transparent conductive film X is attached to the article, for example, via an adhesive functional layer. In one embodiment of the present invention, the transparent resin substrate 10 of the transparent conductive film X is not adjacent to the glass substrate, but an adhesive functional layer such as a pressure sensitive adhesive or adhesive may be interposed between the transparent resin substrate 10 and the glass substrate.

[0079] Examples of the article include an element, a member, and a device. That is, examples of the article with a transparent conductive film include an element with a transparent conductive film, a member with a transparent conductive film, and a device with a transparent conductive film.

[0080] Examples of the element include a light control element and a photoelectric conversion element. Examples of the light control element include a current-driven light control element and an electric field-driven light control element. Examples of the current-driven light control element include an electrochromic (EC) light control element. Examples of the electric field-driven light control element include a PDLC (polymer dispersed liquid crystal) light control element, a PNLC (polymer network liquid crystal) light control element, and a SPD (suspended particle device) light control element. Examples of the photoelectric conversion element include a solar cell. Examples of the solar cell include an organic thin-film solar cell and a dye-sensitized solar cell. Examples of the member include an electromagnetic wave shielding member, a heat ray control member, a heater member, and an antenna member. Examples of the device include a touch sensor device, a lighting device, and an image display device.

[0081] The article with a transparent conductive film is suitable for achieving high crystal stability in the light-transmitting conductive layer 20 of the transparent conductive film X that each of them has, and is therefore suitable for causing the light-transmitting conductive layer 20 to exhibit stable characteristics.

[0082] Examples of the above-mentioned fixing functional layer include an adhesive layer and a bonding layer. The material of the fixing functional layer is not particularly limited as long as it has transparency and exhibits a fixing function. The fixing functional layer is preferably formed from a resin. Examples of the resin include acrylic resin, silicone resin, polyester resin, polyurethane resin, polyamide resin, polyvinyl ether resin, vinyl acetate / vinyl chloride copolymer, modified polyolefin resin, epoxy resin, fluororesin, natural rubber, and synthetic rubber. The resin is preferably an acrylic resin because it exhibits adhesive properties such as cohesiveness, adhesiveness, and moderate wettability, is excellent in transparency, and is excellent in weather resistance and heat resistance.

[0083] The adhesion functional layer (resin forming the adhesion functional layer) may contain a corrosion inhibitor to inhibit corrosion of the light-transmitting conductive layer 20. The adhesion functional layer (resin forming the adhesion functional layer) may contain a migration inhibitor (e.g., a material disclosed in JP 2015-022397 A) to inhibit migration of the light-transmitting conductive layer 20. The adhesion functional layer (resin forming the adhesion functional layer) may contain an ultraviolet absorbing agent to inhibit deterioration during outdoor use of the article. Examples of ultraviolet absorbing agents include benzophenone compounds, benzotriazole compounds, salicylic acid compounds, oxalic acid anilide compounds, cyanoacrylate compounds, and triazine compounds.

[0084] In addition, when the transparent substrate 10 of the transparent conductive film X is fixed to an article via an adhesive functional layer, the light-transmitting conductive layer 20 (including the light-transmitting conductive layer 20 after patterning) is exposed in the transparent conductive film X. In such a case, a cover layer may be disposed on the exposed surface of the light-transmitting conductive layer 20. The cover layer is a layer that covers the light-transmitting conductive layer 20, and can improve the reliability of the light-transmitting conductive layer 20 and suppress the deterioration of the function of the light-transmitting conductive layer 20 due to damage. Such a cover layer is preferably formed from a dielectric material, and more preferably from a composite material of a resin and an inorganic material. Examples of the resin include the resins described above with respect to the adhesive functional layer. Examples of the inorganic material include inorganic oxides and fluorides. Examples of the inorganic oxide include silicon oxide, titanium oxide, niobium oxide, aluminum oxide, zirconium dioxide, and calcium oxide. Examples of the fluoride include magnesium fluoride. The cover layer (a mixture of resin and inorganic material) may further contain the above-mentioned corrosion inhibitor, migration inhibitor, and ultraviolet absorbing agent. EXAMPLES

[0085] The present invention will be specifically described below with reference to examples. The present invention is not limited to the examples. In addition, the specific numerical values ​​of the blending amounts (contents), physical property values, parameters, etc. described below can be replaced with the upper limit (a numerical value defined as "equal to or less than") or lower limit (a numerical value defined as "equal to or more than") of the blending amounts (contents), physical property values, parameters, etc. corresponding thereto described in the above-mentioned "Form for carrying out the invention".

[0086] Example 1 A UV-curable resin containing an acrylic resin was applied to one side of a long PET film (50 μm thick, manufactured by Toray Industries, Inc.) as a resin film to form a coating film. The coating film was then cured by UV irradiation to form a hard coat layer (2 μm thick). In this way, a transparent resin substrate including a resin film and a hard coat layer as a functional layer was produced (after the transparent substrate was subjected to a heat treatment at 165° C. for 1 hour, the thermal shrinkage rate of the transparent substrate in the direction in which it shrinks the most (maximum thermal shrinkage rate, in this embodiment, the thermal shrinkage rate in the MD direction) was 0.63%).

[0087] Next, a 130 nm thick amorphous light-transmitting conductive layer was formed on the hard coat layer of the transparent resin substrate by reactive sputtering (film formation process). In the reactive sputtering, a sputtering film formation device (DC magnetron sputtering device) capable of performing a film formation process by roll-to-roll method was used. The sputtering film formation conditions in this embodiment are as follows.

[0088] The target used was a sintered body of indium oxide and tin oxide (tin oxide concentration: 10% by mass). A DC power supply was used as the power source for applying voltage to the target. The horizontal magnetic field strength above the target was 90 mT. The film formation temperature (the temperature of the transparent resin substrate on which the light-transmitting conductive layer is laminated) was -5°C. The ultimate vacuum in the film formation chamber of the device was 0.8×10 -4After evacuating the film formation chamber until the pressure reached 0.2 Pa, Kr as a sputtering gas and oxygen as a reactive gas were introduced into the film formation chamber, and the pressure in the film formation chamber was set to 0.2 Pa. The ratio of the amount of oxygen introduced to the total amount of Kr and oxygen introduced into the film formation chamber was about 2.5 flow %, and the amount of oxygen introduced was within region R of the resistivity-oxygen introduction amount curve as shown in FIG. 5, and the resistivity value of the formed film was 6.5×10 -4 The resistivity vs. oxygen introduction amount curve shown in Figure 5 was created by investigating in advance the dependence of the resistivity of the optically transparent conductive layer on the amount of oxygen introduced, when the optically transparent conductive layer was formed by reactive sputtering under the same conditions as above, except for the amount of oxygen introduced.

[0089] Next, the light-transmitting conductive layer on the transparent resin substrate was crystallized by heating in a hot air oven (crystallization step). In this step, the heating temperature was 165° C. and the heating time was 1 hour.

[0090] In this manner, a transparent conductive film was produced in Example 1. The light-transmitting conductive layer (thickness: 130 nm, crystalline) of the transparent conductive film in Example 1 was composed of a single Kr-containing ITO layer.

[0091] Example 2 Except for changing some of the film formation conditions in the film formation process and changing the heating conditions in the crystallization process, the transparent conductive film of Example 2 was produced in the same manner as the transparent conductive film of Example 1. In the film formation process of this example, the air pressure in the film formation chamber was set to 0.4 Pa, and the thickness of the light-transmitting conductive layer formed was set to 160 nm. In the crystallization process of this example, the heating temperature was set to 155° C., and the heating time was set to 2 hours.

[0092] The light-transmitting conductive layer (thickness: 160 nm, crystalline) of the transparent conductive film of Example 2 was composed of a single Kr-containing ITO layer.

[0093] Example 3 The transparent conductive film of Example 3 was produced in the same manner as the transparent conductive film of Example 1, except that in the film formation process, a first sputtering film formation was carried out in order to form a first region (thickness 50 nm) of the light-transmitting conductive layer on the transparent resin substrate, and a second sputtering film formation was carried out in order to form a second region (thickness 80 nm) of the light-transmitting conductive layer on the first region.

[0094] The conditions for the first sputtering film formation in this example were as follows. A sintered body of indium oxide and tin oxide (tin oxide concentration: 10 mass %) was used as the target. A DC power supply was used as the power supply for applying a voltage to the target. The horizontal magnetic field strength above the target was 90 mT. The film formation temperature was -5°C. The ultimate vacuum in the first film formation chamber of the device was 0.8 x 10 -4 After evacuating the first film formation chamber until the pressure reached 0.2 Pa, Kr as a sputtering gas and oxygen as a reactive gas were introduced into the first film formation chamber, and the pressure in the film formation chamber was set to 0.2 Pa. The amount of oxygen introduced into the film formation chamber was adjusted so that the resistivity of the film formed would be 6.5×10 -4 The resistivity was adjusted to Ω·cm.

[0095] The conditions for the second sputtering deposition in this embodiment are as follows: the ultimate vacuum in the second deposition chamber of the device is 0.8×10 -4 After the second film formation chamber was evacuated to a vacuum until the pressure reached 0.4 Pa, Ar as a sputtering gas and oxygen as a reactive gas were introduced into the second film formation chamber, and the pressure in the film formation chamber was set to 0.4 Pa. In this embodiment, the other conditions in the second sputter formation were the same as those in the first sputter formation.

[0096] In this manner, a transparent conductive film of Example 3 was produced. The light-transmitting conductive layer (thickness 130 nm, crystalline) of the transparent conductive film of Example 3 had a first region (thickness 50 nm) made of a Kr-containing ITO layer and a second region (thickness 80 nm) made of an Ar-containing ITO layer, in this order from the transparent resin substrate side.

[0097] [Examples 4 to 6] The transparent conductive films of Examples 4 to 6 were produced in the same manner as the transparent conductive film of Example 3, except that the thickness of the first region of the light-transmitting conductive layer formed in the film formation process was set to 50 nm to 66 nm (Example 4), 85 nm (Example 5), or 87 nm (Example 6), and the thickness of the second region was set to 80 nm to 64 nm (Example 4), 45 nm (Example 5), or 38 nm (Example 6).

[0098] The light-transmitting conductive layer (thickness 130 nm, crystalline) of the transparent conductive film of Example 4 has a first region (thickness 66 nm) made of a Kr-containing ITO layer and a second region (thickness 64 nm) made of an Ar-containing ITO layer, in that order from the transparent resin substrate side. The light-transmitting conductive layer (thickness 130 nm) of the transparent conductive film of Example 5 has a first region (thickness 85 nm) made of a Kr-containing ITO layer and a second region (thickness 45 nm) made of an Ar-containing ITO layer, in that order from the transparent resin substrate side. The light-transmitting conductive layer (thickness 125 nm) of the transparent conductive film of Example 6 has a first region (thickness 87 nm) made of a Kr-containing ITO layer and a second region (thickness 38 nm) made of an Ar-containing ITO layer, in that order from the transparent resin substrate side.

[0099] Example 7 The transparent conductive film of Example 7 was produced in the same manner as the transparent conductive film of Example 1, except for the following in the sputtering film formation: A mixed gas of krypton and argon (Kr 90 volume %, Ar 10 volume %) was used as the sputtering gas. The pressure in the film formation chamber was 0.2 Pa. The ratio of the amount of oxygen introduced to the total amount of the mixed gas and oxygen introduced into the film formation chamber was about 2.7 flow %, and the amount of oxygen introduced was such that the resistivity of the formed film was 5.7×10 -4 The resistivity was adjusted to Ω·cm.

[0100] The light-transmitting conductive film (thickness: 130 nm, crystalline) of the transparent conductive film of Example 7 is composed of a single ITO layer containing Kr and Ar.

[0101] Comparative Example 1 The transparent conductive film of Comparative Example 1 was produced in the same manner as the transparent conductive film of Example 1, except that in the film formation process, Ar was used instead of Kr as the sputtering gas, and the film formation pressure was changed from 0.2 Pa to 0.4 Pa. The light-transmitting conductive layer (thickness 130 nm, crystalline) of the transparent conductive film of Comparative Example 1 was composed of a single Ar-containing ITO layer.

[0102] Comparative Example 2 The transparent conductive film of Comparative Example 2 was produced in the same manner as the transparent conductive film of Example 2, except that in the film formation step, Ar was used instead of Kr as the sputtering gas, the film formation pressure was changed from 0.2 Pa to 0.4 Pa, and in the crystallization step, instead of the heat treatment at 165° C. for 1 hour, a first heat treatment at 170° C. for 5 minutes and then a second heat treatment at 165° C. for 1 hour were carried out. The light-transmitting conductive layer (thickness 160 nm, crystalline) of the transparent conductive film of Comparative Example 2 was composed of a single Ar-containing ITO layer.

[0103] <Thickness of Light-Transmitting Conductive Layer> The thickness of the light-transmitting conductive layer of each transparent conductive film in Examples 1 to 7 and Comparative Examples 1 and 2 was measured by FE-TEM observation. Specifically, first, a cross-sectional observation sample of each light-transmitting conductive layer in Examples 1 to 7 and Comparative Examples 1 and 2 was prepared by FIB microsampling. In the FIB microsampling method, a FIB device (product name "FB2200", manufactured by Hitachi) was used, and the acceleration voltage was set to 10 kV. Next, the thickness of the light-transmitting conductive layer in the cross-sectional observation sample was measured by FE-TEM observation. In the FE-TEM observation, a FE-TEM device (product name "JEM-2800", manufactured by JEOL) was used, and the acceleration voltage was set to 200 kV.

[0104] The thickness of the first region of each light-transmitting conductive layer in Examples 3 to 6 was measured by preparing a cross-sectional observation sample from an intermediate product before forming the second region on the first region, and observing the sample by FE-TEM. The thickness of the second region of each light-transmitting conductive layer in Examples 3 to 6 was determined by subtracting the thickness of the first region from the total thickness of each light-transmitting conductive layer in Examples 3 to 6. The proportion of the first region in the thickness direction of the light-transmitting conductive layer was 38.5% in Example 3, 50.8% in Example 4, 65.4% in Example 5, and 69.6% in Example 6.

[0105] <Specific resistance> The resistivity of the light-transmitting conductive layer was examined for each of the transparent conductive films of Examples 1 to 7 and Comparative Examples 1 and 2. Specifically, the surface resistance of the light-transmitting conductive layer was measured by a four-terminal method in accordance with JIS K 7194 (1994), and then the resistivity (Ω·cm) was calculated by multiplying the surface resistance value by the thickness of the light-transmitting conductive layer. The results are shown in Table 1.

[0106] Quantitative analysis of rare gas atoms in a light-transmitting conductive layer The contents of Kr and Ar atoms contained in the light-transmitting conductive layer of each of the transparent conductive films of Examples 1 to 7 and Comparative Examples 1 and 2 were analyzed by Rutherford backscattering spectroscopy (RBS). The abundance (atomic %) of Kr atoms and Ar atoms in the light-transmitting conductive layer was obtained by determining the element ratio for the five elements, In+Sn (since it is difficult to measure In and Sn separately in Rutherford backscattering spectroscopy, the two elements were evaluated as a sum), O, Ar, and Kr, which are the detection elements. The apparatus used and the measurement conditions are as follows. As the analysis results, the Kr content (atomic %), Ar content (atomic %), and rare gas atom content (atomic %) are shown in Table 1. Regarding the analysis of the Kr content, in Examples 1 to 7, a reliable measurement value equal to or higher than the detection limit (lower limit) was not obtained (the detection limit may vary depending on the thickness of the light-transmitting conductive layer subjected to the measurement). Therefore, in Table 1, the Kr content in the light-transmitting conductive layer is expressed as "<specific detection limit value at the thickness of the light-transmitting conductive layer subjected to measurement" to indicate that the Kr content is below the detection limit value at the thickness of the same layer (the same applies to the expression of the rare gas atom content).

[0107] <Equipment used> Pelletron 3SDH (manufactured by National Electrostatics Corporation) <Measurement conditions> Incident ions: 4 He ++ Incident energy: 2300keV Incident angle: 0deg Scattering angle: 160deg Specimen current: 6nA Beam diameter: 2mmφ In-plane rotation: None Irradiation dose: 75μC

[0108] <Confirmation of Kr atoms in the light-transmitting conductive layer> It was confirmed that each of the light-transmitting conductive layers in Examples 1 to 7 contained Kr atoms as follows. First, using a scanning X-ray fluorescence analyzer (product name "ZSX PrimusIV", manufactured by Rigaku Corporation), fluorescent X-ray analysis was repeated five times under the following measurement conditions, and the average value of each scanning angle was calculated to create an X-ray spectrum. Then, it was confirmed that a peak appeared near a scanning angle of 28.2° in the created X-ray spectrum, thereby confirming that Kr atoms were contained in the light-transmitting conductive layer.

[0109] <Measurement conditions> Spectrum;Kr-KA Measurement diameter: 30mm Atmosphere: Vacuum Target: Rh Tube voltage: 50kV Tube current: 60mA Primary filter: Ni40 Scanning angle (deg): 27.0~29.5 Step(deg):0.020 Speed ​​(deg / min): 0.75 Attenuator: 1 / 1 Slit: S2 Spectroscopic crystal: LiF(200) Detector: SC PHA: 100~300

[0110] <Compressive Residual Stress in Light-Transmitting Conductive Layer> The compressive residual stress of the light-transmitting conductive layer (crystalline ITO film) of each of the transparent conductive films in Examples 1 to 7 and Comparative Examples 1 and 2 was indirectly determined from the crystal lattice distortion of the light-transmitting conductive layer. Specifically, the procedure is as follows.

[0111] First, a rectangular measurement sample (50 mm x 50 mm) was cut out from the transparent conductive film. Next, the diffraction intensity of the measurement sample was measured at 0.02° intervals in the range of measurement scattering angle 2θ = 60 to 61.6° using a powder X-ray diffractometer (product name "SmartLab", manufactured by Rigaku Corporation) (0.15° / min). Next, based on the peak angle 2θ of the obtained diffraction image (peak of the (622) plane of ITO) and the wavelength λ of the X-ray source, the crystal lattice spacing d of the light-transmitting conductive layer in the measurement sample was calculated, and the lattice distortion ε was calculated based on d. The following formula (1) was used to calculate d, and the following formula (2) was used to calculate ε.

[0112]

number

[0113] In equations (1) and (2), λ is the wavelength (=0.15418 nm) of the X-ray source (Cu Kα radiation), and d 0 is the lattice spacing of ITO in a stress-free state (=0.1518967 nm). The above X-ray diffraction measurement was performed for angles Ψ between the film plane normal and the ITO crystal plane normal of 65°, 70°, 75°, and 85°, and the lattice strain ε at each Ψ was calculated. The angle Ψ between the film plane normal and the ITO crystal plane normal was adjusted by rotating the sample (part of a transparent conductive film) around the TD direction (direction perpendicular to the MD direction in the plane) of the transparent resin substrate in the measurement sample (adjustment of the angle Ψ). The residual stress σ in the in-plane direction of the ITO film was calculated as Sin 2 The relationship between Ψ and lattice strain ε was plotted and the slope of the line was calculated using the following formula (3). The calculated residual stress σ was used as the first compressive residual stress S in the MD direction. 1 The values ​​are shown in Table 1 as (MPa).

[0114]

number

[0115] In equation (3), E is the Young's modulus of ITO (=115 GPa), and ν is the Poisson's ratio of ITO (=0.35).

[0116] In addition, the adjustment of the angle Ψ in the X-ray diffraction measurement was realized by rotating the sample around the MD direction (direction perpendicular to the TD direction in the plane) instead of the TD direction of the transparent resin substrate in the measurement sample. 1 Similarly, the second compressive residual stress S 2 The values ​​are shown in Table 1. Table 1 also shows the second compressive residual stress S 2 The first compressive residual stress S 1 The ratio (S 1 / S 2 ) are also listed.

[0117] <Crystal stability> The crystal stability of the light-transmitting conductive layer was examined for each of the transparent conductive films of Examples 1 to 7 and Comparative Examples 1 and 2. Specifically, first, the first surface resistance R 1 (surface resistance before heat treatment) was measured. Next, the transparent conductive film was heat-treated. In the heat treatment, the heating temperature was 175° C. and the heating time was 1 hour. Next, the second surface resistance R 2 The first surface resistance R 1 Second surface resistance R 2 Ratio (R 2 / R 1 The values ​​are shown in Table 1. 2 / R 1 The closer the value is to 1, the smaller the change in resistance of the light-transmitting conductive layer due to heat treatment, and therefore the higher the crystal stability of the layer.

[0118] [Table 1] [Industrial Applicability]

[0119] The transparent conductive film of the present invention can be used as a conductive film supply material for patterning transparent electrodes in various devices such as liquid crystal displays, touch panels, and optical sensors. [Explanation of symbols]

[0120] X Transparent conductive film D Thickness direction 10 Transparent resin base material 11 Resin film 12 Functional Layer 20 Light-transparent conductive layer 21 First area 22 Second area

Claims

[Claim 1] A transparent resin substrate and a light-transmitting conductive layer containing a conductive oxide containing In and Sn are provided in this order in a thickness direction. the light-transmitting conductive layer has a first compressive residual stress in a first in-plane direction perpendicular to the thickness direction, and has a second compressive residual stress smaller than the first compressive residual stress in a second in-plane direction perpendicular to both the thickness direction and the first in-plane direction; A method for producing a transparent conductive film, comprising the steps of: The method for producing a transparent conductive film comprises forming the light-transmitting conductive layer by a sputtering method at a film formation pressure of 1 Pa or less.

Citation Information

Patent Citations

  • Low antimony lead base alloy and casting method

    JP1984076846A

  • Manufacture of transparent conductive film

    JP1993334924A

  • Transparent conductive film and method for manufacturing the same

    JP2016191156A

  • Organic light-emitting device

    WO2016088378A1