Composite film having functional layer and display device including same
A composite film with an acrylate binder and acrylamide monomer in the functional layer addresses adhesion issues in flexible display devices, ensuring antistatic, antifouling, and chemical resistance while maintaining substrate adhesion.
Patent Information
- Application Number
- JP2022201628
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-02-25
- Filing Date
- 2022-12-16
- Publication Date
- 2024-09-26
- Estimated Expiration
- 2042-12-16
AI Technical Summary
Flexible display devices require cover windows with antistatic, antifouling, and chemical resistance properties, but existing polyimide films face issues with adhesion loss when multiple functional layers are added, or decreased adhesion when multiple functions are integrated into a single layer.
A composite film with a base film and a functional layer containing an acrylate binder and an acrylamide monomer, which maintains adhesion while providing antistatic, antifouling, and chemical resistance properties.
The composite film achieves high adhesion to the substrate, maintains functional properties, and supports flexible display devices with improved scratch resistance and surface quality.
Smart Images

Figure 0007556929000025 
Figure 0007556929000022 
Figure 0007556929000021
Abstract
Description
[Technical field]
[0001] Realization examples relate to composite films having functional layers for antistatic, antifouling and chemical resistance and display devices containing same. [Background technology]
[0002] Display technology continues to develop in response to the demands of the development of IT devices, and technologies such as curved displays and bent displays have already been commercialized. In recent years, flexible display devices that can be flexibly bent or folded in response to external forces have become popular in the field of mobile devices, where large screens and portability are both required. In particular, a major advantage of foldable display devices is that they can be folded up to be small when not in use, making them more portable, and can be unfolded to provide a large screen when in use.
[0003] Polymer films are preferred as cover windows for these flexible display devices. For example, polyimide-based films such as polyamide-imide (PAI) are widely used because they are transparent, flexible, and have excellent mechanical properties.
[0004] However, such polyimide films are vulnerable to scratches from the outside, and further improvement is required in terms of other properties required for cover windows, such as anti-fingerprint properties and anti-static properties.
[0005] For example, Patent Document 1 discloses a cover window film in which a hard coat layer and an anti-fingerprint layer are formed on a substrate layer made of polyamide-imide (PAI) resin, and a configuration in which the film is applied to a flexible display. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Korean Patent No. 20147367 Summary of the Invention [Problem to be solved by the invention]
[0007] In the case of flexible display devices where the front of the display is exposed to the outside, such as in the outfolding type, the cover window is required to have various functions (antistatic, antifouling, chemical resistance) while having flexibility. However, forming multiple functional layers for this purpose can lead to problems such as complicated processes, or achieving various functions in a single layer can lead to problems such as reduced adhesion to the substrate.
[0008] Therefore, as a result of the inventors' research, by introducing an acrylate-based binder and an acrylamide-based monomer into a single functional layer, they have been able to realize a film whose adhesion to the substrate is not reduced even if the functional layer further contains additives such as an antistatic agent and an antifouling agent.
[0009] Therefore, the following embodiments provide a composite film having functional layers for antistatic, antifouling, and chemical resistance, and a display device including the same. [Means for solving the problem]
[0010] According to one embodiment, a composite film is provided, comprising a substrate film and a functional layer formed on the substrate film, the functional layer comprising an acrylate-based binder and an acrylamide-based monomer.
[0011] According to another embodiment, a display device is provided that includes a display panel and a cover window disposed on a front surface of the display panel, the cover window including a substrate film and a functional layer formed on the substrate film, the functional layer including an acrylate-based binder and an acrylamide-based monomer. Effect of the Invention
[0012] According to the above-mentioned embodiment, by using an acrylate-based binder and an acrylamide-based monomer, a film can be realized in which the adhesion to the substrate is not reduced even when additives such as antistatic agents and antifouling agents are introduced into a single functional layer.
[0013] Therefore, the composite film according to the above embodiment can be manufactured using a simple process, and also has various functions such as antistatic properties, antifouling properties, and chemical resistance, while exhibiting flexible properties, and therefore can be usefully applied as a cover window for a flexible display device. [Brief description of the drawings]
[0014] [Figure 1] FIG. 1 is an exploded perspective view of a display device according to one implementation. [Diagram 2] FIG. 2 is a cross-sectional view of a composite film (cover window) according to one implementation. [Diagram 3] FIG. 3 shows the cross-cut test evaluation criteria according to ASTM D3359 Method B. [Figure 4] FIG. 4 shows a method for measuring the contact angle on the surface of a composite film. [Diagram 5] FIG. 5 shows the abrasion resistance test method for evaluating chemical resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] Various implementations and embodiments will now be described in detail with reference to the drawings. In the following description of the implementation examples, if it is determined that a detailed description of related known configurations or functions may make the gist of the implementation examples unclear, the detailed description will be omitted. In addition, the size of each component in the drawings may be exaggerated or omitted for the purpose of explanation, and may differ from the size actually applied.
[0016] In this specification, a description that a certain component is formed above / below another component, or is connected or joined to each other includes the case where these components are formed, connected or joined directly between the components or indirectly via other components. It should be understood that the reference regarding the above / below of each component may change depending on the direction in which the object is observed.
[0017] In this specification, the terms referring to each component are used to distinguish it from other components and are not intended to limit the implementation examples. Furthermore, in this specification, the singular expression includes the plural expression unless the context clearly indicates a different meaning.
[0018] As used herein, the term "comprising" is intended to embody certain features, regions, steps, steps, elements and / or components and does not exclude the presence or addition of other features, regions, steps, steps, elements and / or components, unless specifically stated to the contrary.
[0019] In this specification, the terms "first", "second", etc. are used to describe various components, and the components should not be limited by the terms. The terms are used for the purpose of distinguishing one component from another.
[0020] Molecular weights of compounds or polymers described herein, e.g., number average molecular weight or weight average molecular weight, are given as relative masses based on carbon-12, as is well known, without units, but which may be understood to be molar masses (g / mol) of the same numerical value, if desired.
[0021] As used herein, unless otherwise specified, the term "substituted" refers to deuterium, -F, -Cl, -Br, -I, a hydroxy group, a cyano group, a nitro group, an amino group, an amide group, a hydrazine group, a hydrazone group, an ester group, a ketone group, a carboxyl group, a substituted or unsubstituted C 1 -C 30 Alkyl groups, substituted or unsubstituted C 2 -C 30Alkenyl groups, substituted or unsubstituted C 2 -C 30 Alkynyl groups, substituted or unsubstituted C 1 -C 30 Alkoxy groups, substituted or unsubstituted C 6 -C 30 Alicyclic organic groups, substituted or unsubstituted C 4 -C 30 Heterocyclic groups, substituted or unsubstituted C 6 -C 30 Aryl groups, and substituted or unsubstituted C 4 -C 30 It refers to a group substituted with one or more substituents selected from the group consisting of heteroaryl groups, and two adjacent substituents may be linked to form a ring.
[0022] FIG. 1 is an exploded perspective view of a display device according to one implementation. 1, a display device 1 according to one embodiment includes a display panel 20 and a cover window 10 disposed on a front (viewing surface) of the display panel 20. Specifically, the display device 1 includes the cover window 10, the display panel 20, a substrate 30, and a frame 40 that protects them. In addition, an adhesive layer may be formed between the cover window 10 and the display panel 20. For example, the adhesive layer may include an optically transparent adhesive.
[0023] The display device according to the above implementations may be flexible, for example, the display device may be a flexible display device or a foldable display device.
[0024] The display panel 20 may be a liquid crystal display (LCD) panel. Alternatively, the display panel 20 may be an organic light emitting display (OLED) panel. The organic light emitting display device may include a front polarizer and an organic light emitting display panel. The front polarizer may be disposed on a front surface of the organic light emitting display panel. More specifically, the front polarizer may be attached to a surface of the organic light emitting display panel on which an image is displayed. The organic light emitting display panel displays an image by self-emission in pixel units. The organic light emitting display panel includes an organic light emitting substrate and a driving substrate. The organic light emitting substrate includes a plurality of organic light emitting units each corresponding to a pixel. The organic light emitting units each include a cathode, an electron transport layer, a light emitting layer, a hole transport layer, and an anode. The driving substrate is drivingly coupled to the organic light emitting substrate. That is, the driving substrate may be coupled to the organic light emitting substrate so as to apply a driving signal such as a driving current to the organic light emitting substrate. More specifically, the driving substrate may apply a current to each of the organic light emitting units to drive the organic light emitting substrate.
[0025] The display device 1 is applied with a composite film as a cover window 10 according to one embodiment.
[0026] FIG. 2 is a cross-sectional view of a composite film (cover window) according to one implementation. Referring to FIG. 2, a composite film 10 according to one embodiment includes a base film 100 and a functional layer 200 formed on the base film 100, and the functional layer 200 includes an acrylate-based binder and an acrylamide-based monomer.
[0027] [Composite film characteristics] The composite film has properties that allow it to be used as a cover window.
[0028] The composite film according to the embodiment has a light transmittance, for example, an average visible light transmittance, of a certain level or more, which is advantageous for application to a cover window of a display device. For example, the light transmittance of the film can be 70% or more, 75% or more, 80% or more, 82% or more, 83% or more, 85% or more, or 90% or more. Meanwhile, the upper limit of the light transmittance range of the film is not particularly limited, and can be, for example, 100% or less, 98% or less, 95% or less, or 90% or less. Such a transmittance can be measured, for example, based on the ASTM D1003 standard.
[0029] In addition, the composite film according to the embodiment has a haze of less than a certain level, which is advantageous for application to a cover window of a display device. For example, the haze of the film can be 5% or less, 4% or less, 3.5% or less, 3% or less, 2% or less, or 1.5% or less. Meanwhile, the lower limit of the haze range of the film is not particularly limited, and can be, for example, 0% or more, 0.5% or more, or 1% or more. Such haze can be measured, for example, based on the ASTM D1003 standard.
[0030] As a specific example, the composite film may have a light transmittance of 90% or more and a haze of 1.5% or less.
[0031] Furthermore, the composite film according to the embodiment may have a surface hardness that can be used as a cover window. For example, the surface hardness of the functional layer of the composite film may be HB or more. Specifically, the surface hardness of the functional layer of the composite film may be H or more or 2H or more, but is not limited thereto. Furthermore, the composite film may have a Vickers hardness (HV) of 30 N / mm or more on the surface of the functional layer measured by a nanoindentation test based on the ISO 14577-1:2002(E) standard. 2 More specifically, 35N / mm 2 More than 40N / mm 2 or more than 45N / mm 2 It could be more than that.
[0032] In particular, the composite film according to the embodiment has excellent adhesion between the functional layer and the base film, for example, the surface of the functional layer may have a cross-cut test result of 3B or more, specifically 4B or more, or more specifically 5B, according to ASTM D3359 standard.
[0033] The cross-cut test involves cutting the surface of a sample into a grid at regular intervals, attaching adhesive tape to the surface, and then peeling it off to measure the number of grid units that do not generate flakes. According to the ASTM D3359 standard (Method B), the number of grid units that do not generate flakes is evaluated as a percentage of the total number of grid units, and is divided into five grades (0B to 5B), with the higher the grade number, the better the interlayer adhesion (see Figure 3).
[0034] In addition, the composite film according to the embodiment can have excellent antistatic properties. For example, the surface resistance of the functional layer is 1×10 13 Ω / sq or less. This allows the composite film to prevent static electricity that may be generated during processing or use and maintain surface quality. Specifically, the surface resistance of the functional layer may be 1×10 12 Ω / sq or less, or 1×10 11 More specifically, the surface resistance of the functional layer may be less than 1×10 6 Ω / sq~1×10 13 Ω / sq, 1×10 6 Ω / sq~1×10 11 Ω / sq, 1×10 8 Ω / sq~1×10 11 Ω / sq, or 1×10 10 Ω / sq~1×10 11 It can be Ω / sq.
[0035] In addition, the composite film according to the embodiment may have excellent antifouling properties. Specifically, the water contact angle (initial contact angle, see FIG. 4) measured on the surface of the functional layer may be 100° or more, more specifically, 105° or more, 110° or more, 100° to 150°, or 100° to 130°.
[0036] In particular, the composite film according to the embodiment may have a highly durable antifouling property. For example, after an abrasion test is performed with an organic solvent such as ethanol 4 applied to the surface of the functional layer (see FIG. 5), the measured water contact angle may be 80° or more, 85° or more, or 90° or more. As a specific example, after applying 10 μL of ethanol with a purity of 99.5% or more to the surface of the functional layer and rubbing 3000 times with a load of 1 kg using an eraser 5 for abrasion resistance test, the water contact angle may be 95° or more, more specifically, 100° or more, 95° to 140°, 95° to 120°, or 95° to 110°, but is not limited thereto.
[0037] [Functional Layer] The functional layer is formed on a substrate film. The functional layer may improve and complement the physical properties of the substrate film, thereby improving the mechanical and / or optical properties of the composite film.
[0038] For example, the functional layer may function as a hard coat layer that improves the surface hardness of the composite film, or as a hard coat layer, an antistatic layer, an antifouling layer, a chemical-resistant layer, a light-resistant layer, or a composite functional layer thereof.
[0039] The functional layer may include one or more of an organic component, an inorganic component, and an organic-inorganic hybrid component.
[0040] For example, the functional layer may include an organic resin. The organic resin may include a curable resin, specifically, a thermosetting resin or a UV curable resin. Thus, the functional layer may be a curable coating layer. The organic resin may act as a binder.
[0041] According to one implementation, the functional layer comprises an acrylate-based binder. The content of the acrylate-based binder may be 30 wt % to 95 wt % based on the weight of the functional layer, specifically, the content of the acrylate-based binder may be 40 wt % to 90 wt % or 50 wt % to 80 wt % based on the weight of the functional layer, but is not limited thereto.
[0042] The acrylate-based binder may include at least one selected from a urethane acrylate-based compound and an epoxy acrylate-based compound.
[0043] As a specific example, the acrylate-based binder may include a urethane acrylate-based oligomer and an acrylate-based monomer. More specifically, the acrylate-based binder may include a urethane acrylate-based oligomer having 9 to 18 functional groups and an acrylate-based monomer having 1 to 15 functional groups.
[0044] The urethane acrylate compound may include a urethane bond as a repeating unit and have a plurality of functional groups.
[0045] The urethane acrylate compound may be a urethane compound formed by reacting a diisocyanate compound with a polyol, the end of which is substituted with an acrylate group. For example, the diisocyanate compound may include at least one of a linear, branched or cyclic aliphatic diisocyanate compound having 4 to 12 carbon atoms and an aromatic diisocyanate compound having 6 to 20 carbon atoms. The polyol may include 2 to 4 hydroxyl groups (-OH) and may be a linear, branched or cyclic aliphatic polyol compound having 4 to 12 carbon atoms or an aromatic polyol compound having 6 to 20 carbon atoms. The terminal substitution with the acrylate group may be performed by an acrylate compound having a functional group capable of reacting with an isocyanate group (-NCO). For example, an acrylate compound having a hydroxyl group, an amine group, or the like may be used, and a hydroxyalkyl acrylate or an aminoalkyl acrylate having 2 to 10 carbon atoms may be used.
[0046] The urethane acrylate compound may contain 1 to 18 functional groups, specifically, 2 to 18, 5 to 18, or 9 to 18 functional groups.
[0047] Examples of the urethane acrylate compound include, but are not limited to, a bifunctional urethane acrylate oligomer having a weight average molecular weight of 1400 to 25000, a trifunctional urethane acrylate oligomer having a weight average molecular weight of 1700 to 16000, a tetrafunctional urethane acrylate oligomer having a weight average molecular weight of 500 to 2000, a hexafunctional urethane acrylate oligomer having a weight average molecular weight of 818 to 2600, a nonafunctional urethane acrylate oligomer having a weight average molecular weight of 2500 to 5500, a 10-functional urethane acrylate oligomer having a weight average molecular weight of 3200 to 3900, and a 15-functional urethane acrylate oligomer having a weight average molecular weight of 2300 to 20000.
[0048] The glass transition temperature (Tg) of the urethane acrylate compound may be -80°C to 100°C, -80°C to 90°C, -80°C to 80°C, -80°C to 70°C, -80°C to 60°C, -70°C to 100°C, -70°C to 90°C, -70°C to 80°C, -70°C to 70°C, -70°C to 60°C, -60°C to 100°C, -60°C to 90°C, -60°C to 80°C, -60°C to 70°C, -60°C to 60°C, -50°C to 100°C, -50°C to 90°C, -50°C to 80°C, -50°C to 70°C, or -50°C to 60°C.
[0049] The epoxy acrylate compound may contain 1 to 10 functional groups. Examples of the epoxy acrylate compound include, but are not limited to, a monofunctional epoxy acrylate oligomer having a weight average molecular weight of 100 to 300, a bifunctional epoxy acrylate oligomer having a weight average molecular weight of 250 to 2000, and a tetrafunctional epoxy acrylate oligomer having a weight average molecular weight of 1000 to 3000. The epoxy equivalent of the epoxy acrylate compound may be 50g / eq to 300g / eq, 50g / eq to 200g / eq, or 50g / eq to 150g / eq.
[0050] According to one implementation, the functional layer comprises an acrylamide-based monomer. The acrylamide monomer may play a role in preventing a decrease in adhesion to a substrate, which may occur when various functional additives such as an antistatic agent are incorporated into a single functional layer.
[0051] As an example, the acrylamide monomer may be represented by the chemical formula (I): JPEG0007556929000001.jpg2760, where R 1 and R 2 each independently represents hydrogen or a substituted or unsubstituted monovalent C 6 ~C 30 Alicyclic radicals, substituted or unsubstituted monovalent C 4 ~C 30 Heteroalicyclic groups, substituted or unsubstituted monovalent C 6 ~C 30 Aromatic ring groups, substituted or unsubstituted monovalent C 4 ~C 30 Aromatic heterocyclic groups, substituted or unsubstituted C 1 ~C 30 Alkyl groups, substituted or unsubstituted C 2 ~C 30 Alkenyl group or substituted or unsubstituted C 2 ~C 30 It may be an alkynyl group.
[0052] As a specific example, the acrylamide monomer may be at least one selected from the group consisting of N,N-dimethylacrylamide, N-hydroxyethylacrylamide, diacetone acrylamide, N,N-dimethylaminopropylacrylamide, N,N-diethylacrylamide, and N-isopropylacrylamide.
[0053] The acrylamide monomer may be included in an amount of more than 0 part by weight and not more than 40 parts by weight based on 100 parts by weight of the acrylate binder.
[0054] For example, the content of the acrylamide monomer may be more than 0 parts by weight, 1 part by weight or more, 5 parts by weight or more, 10 parts by weight or more, 15 parts by weight or more, or 20 parts by weight or more based on 100 parts by weight of the acrylate binder. In addition, the content of the acrylamide monomer may be 40 parts by weight or less, 30 parts by weight or less, or 25 parts by weight or less based on 100 parts by weight of the acrylate binder. Specifically, the content of the acrylamide monomer may be 5 parts by weight to 25 parts by weight, 10 parts by weight to 20 parts by weight, 10 parts by weight to 15 parts by weight, or 15 parts by weight to 20 parts by weight based on 100 parts by weight of the acrylate binder, but is not limited thereto.
[0055] For example, the functional layer may further include an antistatic agent, which may include at least one selected from an ionic surfactant and a conductive polymer.
[0056] The ionic surfactant may specifically include an ammonium salt or a quaternary alkyl ammonium salt, etc. More specifically, the ammonium salt and the quaternary alkyl ammonium salt may include a halide such as a chloride or a bromide.
[0057] The conductive polymer may include polythiophene, polypyrrole, polyaniline, polyethylenedioxythiophene (PEDOT), or a mixture thereof. Specifically, the antistatic agent may include polyethylenedioxythiophene (PEDOT). More specifically, the antistatic agent may include, but is not limited to, polyethylenedioxythiophene:polystyrenesulfonate (PEDOT:PSS).
[0058] The content of the antistatic agent may be more than 0 parts by weight, 0.1 parts by weight or more, 0.5 parts by weight or more, 1 part by weight or more, or 3 parts by weight or more, and may be 15 parts by weight or less, 10 parts by weight or less, 7 parts by weight or less, 5 parts by weight or less, 3 parts by weight or less, or 1 part by weight or less, based on 100 parts by weight of the acrylate binder.
[0059] Specifically, when the antistatic agent includes an ionic surfactant, the content of the antistatic agent may be 1 to 10 parts by weight, or 3 to 7 parts by weight, based on 100 parts by weight of the acrylate binder. When the antistatic agent includes a conductive polymer, the content of the antistatic agent may be 0.1 to 3 parts by weight, or 0.3 to 1 part by weight, based on 100 parts by weight of the acrylate binder.
[0060] As another example, the functional layer may further include one or more selected from the group consisting of an anti-fouling agent, a UV absorber, and a photoinitiator.
[0061] The antifouling agent may include, for example, a fluoro-based compound. Specifically, the fluoro-based compound is an acrylate-based compound having a perfluoro-based alkyl group, and a specific example thereof is perfluorohexyl ethyl acrylate, but is not limited thereto. The content of the antifouling agent may be 0.1 parts by weight or more, or 0.2 parts by weight or more, and 3 parts by weight or less, 1 part by weight or less, or 0.5 parts by weight or less, based on 100 parts by weight of the acrylate-based binder, and may be 0.1 to 3 parts by weight, or 0.1 to 1 part by weight.
[0062] The UV absorbent may be a benzophenone-based compound, a benzotriazole-based compound, a triazine-based compound, etc. The content of the UV absorbent may be 1 part by weight or more, 3 parts by weight or more, or 5 parts by weight or more, and 15 parts by weight or less, 12 parts by weight or less, or 10 parts by weight or less, specifically, 1 to 15 parts by weight, or 3 to 12 parts by weight, based on 100 parts by weight of the acrylate-based binder.
[0063] Examples of the photoinitiator include, but are not limited to, 1-hydroxy-cyclohexyl-phenyl ketone, 2-hydroxy-2-methyl-1-phenyl-1-propanone, 2-hydroxy-1-[4-(2-hydroxyethoxy)phenyl]-2-methyl-1-propanone, methylbenzoyl formate, α,α-dimethoxy-α-phenylacetophenone, 2-benzoyl-2-(dimethylamino)-1-[4-(4-morpholinyl)phenyl]-1-butanone, 2-methyl-1-[4-(methylthio)phenyl]-2-(4-morpholinyl)-1-propanone, diphenyl(2,4,6-trimethylbenzoyl)-phosphine oxide, and bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide. In addition, commercially available photoinitiators include Irgacure (registered trademark) 184, Irgacure 500, Irgacure 651, Irgacure 369, Irgacure 907, Darocur (registered trademark) 1173, Darocur MBF, Irgacure 819, Darocur TPO, Irgacure 907, Esacure (registered trademark) KIP 100F, etc. The photoinitiators may be used alone or in combination of two or more different types. The content of the photoinitiator is 1 part by weight or more or 3 parts by weight or more, and 12 parts by weight or less, 10 parts by weight or less, or 7 parts by weight or less, based on 100 parts by weight of the acrylate-based binder, and may be specifically 1 to 12 parts by weight or 3 to 7 parts by weight.
[0064] In addition, the functional layer may further include additives such as a surfactant, a light stabilizer, a yellowing inhibitor, a leveling agent, or a dye for improving color value. For example, the surfactant may be a mono- or di-functional fluorine-based acrylate, a fluorine-based surfactant, or a silicone-based surfactant. The surfactant may be included in the functional layer in a dispersed or crosslinked form. The content of these additives may be variously adjusted within a range that does not deteriorate the physical properties of the functional layer. For example, the content of the additives may be 0.01 wt % to 10 wt % based on the total weight of the functional layer, but is not limited thereto.
[0065] The functional layer may further include a filler. The filler may be, for example, an inorganic particle. Examples of the filler include silica, barium sulfate, zinc oxide, and alumina. The particle size of the filler may be 1 nm to 100 nm. Specifically, the particle size of the filler may be 5 nm to 50 nm, or 10 nm to 30 nm. The filler may include inorganic fillers having different particle size distributions. For example, the filler may include a first inorganic filler having a D50 of 20 nm to 35 nm and a second inorganic filler having a D50 of 40 nm to 130 nm. The content of the filler may be 25 wt% or more, 30 wt% or more, or 35 wt% or more based on the total weight of the functional layer. The content of the filler may be 50 wt% or less, 45 wt% or less, or 40 wt% or less based on the total weight of the functional layer. Alternatively, the functional layer may not include an inorganic filler such as silica.
[0066] The thickness of the functional layer may be 2 μm or more, 3 μm or more, 5 μm or more, or 10 μm or more, and may be 50 μm or less, 30 μm or less, 20 μm or less, or 10 μm or less. For example, the thickness of the functional layer may be 2 μm to 20 μm. Specifically, the thickness of the functional layer may be 5 μm to 20 μm.
[0067] The functional layer may be formed directly on the surface of the base film. Specifically, there may be no other layer between the functional layer and the base film. Alternatively, one of the two surfaces of the functional layer may be provided as an interface between the functional layer and the base film. In particular, the functional layer has excellent adhesion to the base film, and therefore may improve and complement the insufficient physical properties of the base film while maintaining stable film properties.
[0068] The functional layer can be formed by applying a functional layer composition onto the substrate film, followed by drying and curing.
[0069] The functional layer composition may include additives such as antistatic agents, antifouling agents, photoinitiators, UV absorbers, etc., as well as the above-mentioned acrylate-based binder and acrylamide-based compound, and a solvent.
[0070] Examples of the solvent include alcohol-based solvents such as methanol, ethanol, isopropyl alcohol, and butanol; alkoxy alcohol-based solvents such as 2-methoxyethanol, 2-ethoxyethanol, and 1-methoxy-2-propanol; ketone-based solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, methyl propyl ketone, and cyclohexanone; ether-based solvents such as propylene glycol monopropyl ether, propylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monopropyl ether, ethylene glycol monobutyl ether, diethylene glycol monomethyl ether, diethyl glycol monoethyl ether, diethyl glycol monopropyl ether, diethyl glycol monobutyl ether, and diethylene glycol-2-ethylhexyl ether; and aromatic solvents such as benzene, toluene, and xylene, which may be used alone or in combination.
[0071] The content of the solvent is not particularly limited since it can be adjusted in various ways within a range that does not deteriorate the physical properties of the coating composition, but may be included such that the weight ratio of solids:solvent relative to the solids of the components contained in the functional layer composition is 20:80 to 99:1. Specifically, the content of the solvent may be included such that the weight ratio of solids:solvent relative to the solids of the components contained in the functional layer composition is 20:80 to 70:30, 20:80 to 60:40, 20:80 to 50:50, or 25:75 to 40:60, but is not limited thereto. When the solvent is within the above range, the coating composition may have appropriate fluidity and coatability.
[0072] The functional layer composition can be applied by bar coating, knife coating, roll coating, blade coating, die coating, microgravure coating, comma coating, slot die coating, lip coating, solution casting, and the like.
[0073] Thereafter, the solvent contained in the functional layer composition can be removed by a drying step, which can be performed at a temperature of 40° C. to 100° C., preferably 40° C. to 80° C., 50° C. to 100° C., or 50° C. to 80° C., for about 1 to 20 minutes, preferably 1 to 10 minutes or 1 to 5 minutes.
[0074] The functional layer may then be cured by light and / or heat. As an example, the functional layer may be cured by 500 mJ / cm2 UV light in a nitrogen atmosphere. 2 ~1000mJ / cm 2 can be irradiated and cured in an amount of
[0075] [Base film] The substrate film acts as a base layer for the functional layers while providing mechanical properties to the composite film.
[0076] The substrate film may be a polymer film or a glass substrate, specifically a tempered glass substrate having a thickness of less than about 100 μm. For example, the substrate film may include at least one selected from the group consisting of a polymer film or ultra-thin glass (UTG).
[0077] Specifically, the base film may be a polymer film, that is, the base film may include a polymer resin.
[0078] According to one embodiment, the base film includes a polyimide-based resin or a polyamide-based resin, and may be a transparent polyimide-based or polyamide-based film.
[0079] The polyimide-based resin may be formed by simultaneously or sequentially reacting reactants including a diamine compound and a dianhydride compound. Specifically, the polyimide-based resin may include a polyimide-based polymer formed by polymerizing a diamine compound and a dianhydride compound. The polyimide-based resin may include an imide repeat unit derived from the polymerization of the diamine compound and the dianhydride compound. In addition, the polyimide-based resin may be polymerized by further including a dicarbonyl compound, and thus may include a polyamide-imide-based polymer further including an amide repeat unit derived from the polymerization of the diamine compound and the dicarbonyl compound.
[0080] The diamine compound is not particularly limited, and may be, for example, an aromatic diamine compound having an aromatic structure. For example, the diamine compound may be a compound represented by the following Formula 1:
[0081] [C1] JPEG0007556929000002.jpg641 In the above chemical formula 1, E is a substituted or unsubstituted divalent C 6 -C 30 Alicyclic radicals, substituted or unsubstituted divalent C 4 -C 30 Heteroalicyclic groups, substituted or unsubstituted divalent C 6 -C 30 Aromatic ring group, substituted or unsubstituted divalent C 4 -C 30 Aromatic heterocyclic groups, substituted or unsubstituted C 1 -C 30 Alkylene group, substituted or unsubstituted C 2 -C 30 Alkenylene groups, substituted or unsubstituted C 2 -C 30 Alkynylene groups, -O-, -S-, -C(=O)-, -CH(OH)-, -S(=O) 2 -, -Si(CH 3 ) 2 -, -C(CH 3 ) 2 - and -C(CF 3 ) 2-, and e is selected from integers of 1 to 5, and when e is 2 or more, E may be the same or different.
[0082] (E) of Chemical Formula 1 e can be selected from groups represented by the following chemical formulas 1-1a to 1-14a, but is not limited thereto. JPEG0007556929000003.jpg89141
[0083] Specifically, (E) of the above Chemical Formula 1 e can be selected from groups represented by the following chemical formulas 1-1b to 1-13b, but is not limited thereto. JPEG0007556929000004.jpg88131
[0084] More specifically, (E) of the above Chemical Formula 1 e may be a group represented by the above formula 1-6b.
[0085] In one embodiment, the diamine compound may include a compound having a fluorine-containing substituent, or may be a compound having a fluorine-containing substituent, where the fluorine-containing substituent is a fluorinated hydrocarbon group, specifically, but not limited to, a trifluoromethyl group.
[0086] In one embodiment, the diamine compound may be one type of diamine compound, i.e., the diamine compound may consist of a single component.
[0087] For example, the diamine compound may include, but is not limited to, 2,2'-bis(trifluoromethyl)-4,4'-diaminodiphenyl (TFDB) having the following structure: JPEG0007556929000005.jpg4778
[0088] The dianhydride compound has a low birefringence value, and therefore may contribute to improving optical properties such as transmittance of a film including the polyimide resin.
[0089] The dianhydride compound is not particularly limited, and may be an aromatic dianhydride compound having an aromatic structure. For example, the aromatic dianhydride compound may be a compound represented by the following formula 2: [C2] JPEG0007556929000006.jpg3654
[0090] In the above formula 2, G is a substituted or unsubstituted tetravalent C 6 -C 30 Alicyclic radicals, substituted or unsubstituted tetravalent C 4 -C 30 Heteroalicyclic groups, substituted or unsubstituted tetravalent C 6 -C 30 Aromatic ring groups, substituted or unsubstituted tetravalent C 4 -C 30 an aromatic heterocyclic group, wherein the alicyclic group, the heteroalicyclic group, the aromatic ring group, or the aromatic heterocyclic group is present alone or is bonded to each other to form a condensed ring, or is a substituted or unsubstituted C 1 -C 30 Alkylene group, substituted or unsubstituted C 2 -C 30 Alkenylene groups, substituted or unsubstituted C 2 -C 30 Alkynylene groups, -O-, -S-, -C(=O)-, -CH(OH)-, -S(=O) 2 -, -Si(CH 3 ) 2 -, -C(CH 3 ) 2 - and -C(CF 3 ) 2 - is linked by a linking group selected from the following:
[0091] G in the above Chemical Formula 2 may be selected from groups represented by the following Chemical Formulas 2-1a to 2-9a, but is not limited thereto. JPEG0007556929000007.jpg84143
[0092] For example, G in the above Chemical Formula 2 can be a group represented by the above Chemical Formula 2-8a.
[0093] In one embodiment, the dianhydride compound may include a compound having a fluorine-containing substituent, or may be composed of a compound having a fluorine-containing substituent, which may be a fluorinated hydrocarbon group, specifically, but not limited to, a trifluoromethyl group.
[0094] In other implementations, the dianhydride compound may consist of one single component or two mixed components.
[0095] For example, the dianhydride compound may include, but is not limited to, 2,2'-bis-(3,4-dicarboxyphenyl)hexafluoropropane dianhydride (6FDA) having the following structure: JPEG0007556929000008.jpg4076
[0096] The diamine compound and the dianhydride compound can be polymerized to produce a polyamic acid.
[0097] The polyamic acid may then be converted to a polyimide by a dehydration reaction. The polyimide may include a repeating unit represented by the following formula A: [Chemical A] JPEG0007556929000009.jpg4074 In the above chemical formula A, the explanations for E, G, and e are as described above.
[0098] For example, the polyimide may include a repeating unit represented by the following formula A-1, but is not limited thereto. [Chemical A-1] JPEG0007556929000010.jpg37128 In the above chemical formula A-1, n may be an integer of 1 to 400.
[0099] The dicarbonyl compound is not particularly limited, and may be, for example, a compound represented by the following formula 3: [C3] JPEG0007556929000011.jpg1736
[0100] In the above formula 3, J is a substituted or unsubstituted divalent C 6 -C 30 Alicyclic radicals, substituted or unsubstituted divalent C 4 -C 30 Heteroalicyclic groups, substituted or unsubstituted divalent C 6 -C 30 Aromatic ring group, substituted or unsubstituted divalent C 4 -C 30 Aromatic heterocyclic groups, substituted or unsubstituted C 1 -C 30 Alkylene group, substituted or unsubstituted C 2 -C 30 Alkenylene groups, substituted or unsubstituted C 2 -C 30 Alkynylene groups, -O-, -S-, -C(=O)-, -CH(OH)-, -S(=O) 2 -, -Si(CH 3 ) 2 -, -C(CH 3 ) 2 - and -C(CF 3 ) 2 -, j is selected from integers of 1 to 5, and when j is 2 or more, J are the same or different, and X is a halogen atom. Specifically, X can be F, Cl, Br, I, etc. More specifically, X can be Cl, but is not limited thereto.
[0101] (J) of the above Chemical Formula 3 j can be selected from groups represented by the following chemical formulas 3-1a to 3-14a, but is not limited thereto. JPEG0007556929000012.jpg96144
[0102] Specifically, (J) of the above Chemical Formula 3 j can be selected from groups represented by the following chemical formulas 3-1b to 3-8b, but is not limited thereto. JPEG0007556929000013.jpg74150
[0103] More specifically, (J) of the above Chemical Formula 3 j can be a group represented by the above chemical formula 3-1b, a group represented by the above chemical formula 3-2b, or a group represented by the above chemical formula 3-3b.
[0104] In one embodiment, the dicarbonyl compound may be a mixture of at least two different dicarbonyl compounds. When two or more dicarbonyl compounds are used, the dicarbonyl compound may be (J) in Formula 3. j may be used two or more selected from the groups represented by the chemical formulas 3-1b to 3-8b.
[0105] In another implementation, the dicarbonyl compound can be an aromatic dicarbonyl compound that includes an aromatic structure.
[0106] For example, the dicarbonyl compound can include a first dicarbonyl compound and / or a second dicarbonyl compound that is different from the first dicarbonyl compound.
[0107] The first dicarbonyl compound and the second dicarbonyl compound can each be an aromatic dicarbonyl compound.
[0108] The first dicarbonyl compound and the second dicarbonyl compound may be, but are not limited to, different aromatic dicarbonyl compounds.
[0109] When the first dicarbonyl compound and the second dicarbonyl compound are each an aromatic dicarbonyl compound, each of them contains a benzene ring, and therefore can contribute to improving the mechanical properties, such as the surface hardness and tensile strength, of the film containing the produced polyamide-imide resin.
[0110] The dicarbonyl compound may include, but is not limited to, terephthaloyl chloride (TPC), isophthaloyl chloride (IPC), 1,1'-biphenyl-4,4'-dicarbonyl dichloride (BPDC), or a combination thereof, having the following structure: JPEG0007556929000014.jpg31151
[0111] For example, the first dicarbonyl compound may include BPDC and the second dicarbonyl compound may include TPC, but is not limited thereto.
[0112] Specifically, when BPDC is used as the first dicarbonyl compound and TPC is used as the second dicarbonyl compound in appropriate combination, the film containing the produced polyamide-imide resin can have high oxidation resistance.
[0113] Alternatively, the first dicarbonyl compound may include IPC and the second dicarbonyl compound may include TPC, but is not limited thereto.
[0114] Specifically, by using an appropriate combination of IPC as the first dicarbonyl compound and TPC as the second dicarbonyl compound, the produced film containing a polyamide-imide resin can have high oxidation resistance and the production cost can be reduced.
[0115] The diamine compound and the dicarbonyl compound can be polymerized to form a repeating unit represented by the following chemical formula B. [Case B] JPEG0007556929000015.jpg2861 In the above chemical formula B, the explanations for E, J, e, and j are as described above.
[0116] For example, the diamine compound and the dicarbonyl compound can be polymerized to form amide repeat units represented by chemical formulas B-1 and B-2.
[0117] [Case B-1] JPEG0007556929000016.jpg38128 In the chemical formula B-1, x is an integer of 1 to 400.
[0118] [Case B-2] JPEG0007556929000017.jpg37128 In the chemical formula B-2, y is an integer of 1 to 400.
[0119] According to another embodiment, the base film includes a polyester-based resin, and specifically, the base film may be a transparent polyester-based film.
[0120] The polyester resin may be a homopolymer resin or a copolymer resin obtained by polycondensation of a dicarboxylic acid and a diol, or a blend resin obtained by mixing the homopolymer resins or the copolymer resins.
[0121] Examples of the dicarboxylic acid include terephthalic acid, isophthalic acid, orthophthalic acid, 2,5-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, 1,4-naphthalenedicarboxylic acid, 1,5-naphthalenedicarboxylic acid, diphenylcarboxylic acid, diphenoxyethanedicarboxylic acid, diphenylsulfonecarboxylic acid, anthracenedicarboxylic acid, 1,3-cyclopentanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, 1,4-cyclohexanedicarboxylic acid, hexahydroterephthalic acid, hexahydroisophthalic acid, malonic acid, dimethylmalonic acid, succinic acid, 3,3-diethylsuccinic acid, glutaric acid, 2,2-dimethylglutaric acid, adipic acid, 2-methyladipic acid, trimethyladipic acid, pimelic acid, azelaic acid, sebacic acid, suberic acid, and dodecanedicarboxylic acid.
[0122] Examples of the diol include ethylene glycol, propylene glycol, hexamethylene glycol, neopentyl glycol, 1,2-cyclohexanedimethanol, 1,4-cyclohexanedimethanol, decamethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 2,2-bis(4-hydroxyphenyl)propane, and bis(4-hydroxyphenyl)sulfone.
[0123] Preferably, the polyester resin may be an aromatic polyester resin having excellent crystallinity, and may be, for example, composed mainly of polyethylene terephthalate (PET) resin.
[0124] When the base film is a polyester-based film, the polyester-based film may contain a polyester-based resin, specifically a PET resin, at about 85% by weight or more, more specifically, at 90% by weight or more, 95% by weight or more, or 99% by weight or more. As another example, the polyester-based film may further contain another polyester-based resin in addition to the PET resin. Specifically, the polyester-based film may further contain about 15% by weight or less of a polyethylene naphthalate (PEN) resin. More specifically, the polyester-based film may further contain about 0.1% by weight to 10% by weight, or about 0.1% by weight to 5% by weight of a PEN resin.
[0125] Due to this composition, the crystallinity of the polyester film may increase during the manufacturing process, such as heating and stretching, and mechanical properties such as tensile strength may be improved.
[0126] The substrate film may further include a filler in addition to the polymer resin. The filler may be one or more selected from the group consisting of barium sulfate, silica, and calcium carbonate. By including the filler, the base film can improve roughness and winding properties, and can improve running properties and scratch prevention effects during film production.
[0127] The particle size of the filler may be 0.01 μm or more and less than 1.0 μm. For example, the particle size of the filler may be 0.05 μm to 0.9 μm or 0.1 μm to 0.8 μm, but is not limited thereto.
[0128] The filler may be included in an amount of 0.01 wt % to 3 wt % based on the total weight of the base film, for example, but not limited to, 0.05 wt % to 2.5 wt %, 0.1 wt % to 2 wt %, or 0.2 wt % to 1.7 wt % based on the total weight of the base film.
[0129] The thickness of the base film may be 20 μm or more, 30 μm or more, 40 μm or more, 50 μm or more, or 100 μm or more, and 500 μm or less, 400 μm or less, 300 μm or less, or 200 μm or less.Specifically, the thickness of the base film may be 20 μm to 500 μm, more specifically, 40 μm to 200 μm or 50 μm to 200 μm.
[0130] The substrate film may have certain levels of optical and mechanical properties.
[0131] The haze of the base film may be 3% or less. For example, the haze of the base film may be 2% or less, 1.5% or less, or 1% or less, but is not limited thereto.
[0132] The yellowness index (YI) of the base film may be 5 or less. For example, the yellowness index of the base film may be, but is not limited to, 4 or less, 3.8 or less, 2.8 or less, 2.5 or less, 2.3 or less, or 2.1 or less.
[0133] The modulus of the base film may be 5 GPa or more. For example, the modulus of the base film may be 5.2 GPa or more, 5.5 GPa or more, 6.0 GPa or more, 10 GPa or less, 5 GPa to 10 GPa, or 7 GPa to 10 GPa, but is not limited thereto.
[0134] The light transmittance of the base film may be 80% or more. For example, the light transmittance of the base film may be 85% or more, 88% or more, 89% or more, 80% to 99%, or 85% to 99%, but is not limited thereto.
[0135] The compressive strength of the base film may be 0.4 kgf / μm or more. Specifically, the compressive strength of the base film may be 0.45 kgf / μm or more or 0.46 kgf / μm or more, but is not limited thereto.
[0136] The surface hardness of the base film may be HB or more. Specifically, the surface hardness of the base film may be H or more or 2H or more, but is not limited thereto.
[0137] The base film has a tensile strength of 15 kgf / mm 2 Specifically, the tensile strength of the base film may be 18 kgf / mm 2 Above 20kgf / mm 2 Above, 21kgf / mm 2 or more than 22kgf / mm 2 It may be more than this, but is not limited to this.
[0138] The base film may have an elongation percentage of 15% or more. Specifically, the elongation percentage of the base film may be, but is not limited to, 16% or more, 17% or more, or 17.5% or more.
[0139] (Example) The embodiments described below are merely for ease of understanding and are not intended to limit the scope of the invention.
[0140] [Preparation of Functional Layer Composition A] The components in Table 1 below were mixed in a solvent to obtain functional layer composition A. A mixed solvent of methyl isobutyl ketone (MIBK), propylene glycol monomethyl ether (PM), methyl ethyl ketone (MEK) and ethanol was used as the solvent, and the mixed solvent was blended so that the solid content concentration was 25% by weight to 40% by weight based on the total weight of functional layer composition A.
[0141] [Table 1]
[0142] [Preparation of Functional Layer Composition B] The components in Table 2 below were mixed in a solvent to obtain a functional layer composition B. The type and amount of the solvent were the same as those in the composition A.
[0143] [Table 2]
[0144] Example 1: Preparation of composite film The functional layer composition A was prepared and coated on one side of a 50 μm-thick transparent polyimide film (TPI, SKC Corporation) using a Mayer Bar. The solvent in the coating composition was then dried by heat treatment at 60° C. for 2 minutes, and the composition was then coated with 500 mJ / cm 2 under a nitrogen atmosphere. 2 ~1000mJ / cm 2 As a result, a composite film was obtained in which a functional layer with a thickness of about 5 μm was formed on the polyimide film.
[0145] Example 2: Preparation of composite film The same procedure as in Example 1 was repeated, but the content of acrylamide was adjusted to 20 parts by weight (based on the solid content weight) per 100 parts by weight of binder to prepare a composite film.
[0146] Example 3: Preparation of composite film A composite film was produced by repeating the same procedure as in Example 1, except that 0.5 parts by weight of an organic solvent-based conductive polymer (PEDOT-based) was added to the functional layer composition instead of the quaternary ammonium-based antistatic agent.
[0147] Example 4: Preparation of composite film A composite film was produced by repeating the same procedure as in Example 2, except that 0.5 parts by weight of an organic solvent-based conductive polymer (PEDOT-based) was added to the functional layer composition instead of the quaternary ammonium-based antistatic agent.
[0148] (Comparative Example 1: Production of Composite Film) A composite film was prepared by repeating the same procedure as in Example 1, except that acrylamide and the antistatic agent were omitted from the functional layer composition.
[0149] (Comparative Example 2: Production of Composite Film) A composite film was prepared by repeating the same procedure as in Example 1 above, except that acrylamide was omitted from the functional layer composition.
[0150] (Comparative Example 3: Production of Composite Film) A composite film was produced in the same manner as in Example 1 except that the functional layer composition B was used.
[0151] (Comparative Example 4: Production of Composite Film) The same procedure as in Comparative Example 3 was repeated, but the content of the acrylic monomer was adjusted to 20 parts by weight (based on the solid content weight) per 100 parts by weight of the binder to produce a composite film.
[0152] (Comparative Example 5: Production of Composite Film) A composite film was prepared by repeating the same procedure as in Example 3 above, except that acrylamide was omitted from the functional layer composition.
[0153] (Comparative Example 6: Production of Composite Film) A composite film was produced by repeating the same procedure as in Comparative Example 3, except that 0.5 parts by weight of an organic solvent-based conductive polymer (PEDOT-based) was added to the functional layer composition instead of the quaternary ammonium-based antistatic agent.
[0154] (Comparative Example 7: Production of Composite Film) A composite film was produced by repeating the same procedure as in Comparative Example 4, except that 0.5 parts by weight of an organic solvent-based conductive polymer (PEDOT-based) was added to the functional layer composition instead of the quaternary ammonium-based antistatic agent.
[0155] (Test Example 1: Adhesion (Cross-cut test)) The adhesion between the functional layer and the base film of the composite film sample was evaluated by a cross-cut test. The surface of the functional layer was cut into a grid at regular intervals according to the ASTM D 3359 (Method B) standard, and tape (3M Scotch (registered trademark) Magic Tape) was applied on the cut and then peeled off to check the degree of lattice-unit flakes on the surface. The results were graded from 0B to 5B according to the following criteria, with 5B being the most excellent (see Figure 3).
[0156] -5B: The cut surface is clean and the lattice squares are not separated (0% of the lattice area). -4B: Small pieces of coating are separated at the intersections (less than 5% of the grid area) -3B: Small pieces of coating are separated along corners and at the intersections of cuts (>5% but <15% of the grid area) -2B: The edges of the cut surface of the coating and part of the rectangle are separated (more than 15% but less than 35% of the lattice area) -1B: The coating is largely removed along the edges of the cut surface, resulting in the separation of the squares (35% to 65% of the lattice area). -0B: Coating peeling and severe tetragon separation (>65% of lattice area)
[0157] (Test Example 2: Surface Resistance) A voltage of 100 V was applied to the surface of the functional layer of the composite film sample using a surface resistance tester (ST-4, manufactured by SIMCO ion) to measure the resistance.
[0158] (Test Example 3: Antifouling property (initial contact angle)) The water contact angle of the functional layer surface of the composite film sample was measured using a 3.0 μL water droplet with a contact angle measuring instrument (KYOWA DM-CE1). An initial contact angle of 100° or more can be judged to be good (see Figure 4).
[0159] (Test Example 4: Chemical resistance (contact angle after chemical resistance test)) 10 μL of ethanol with a purity of 99.5% or higher was applied to the surface of the functional layer of the composite film sample, and the functional layer surface to which the ethanol had been applied was rubbed 3000 times with a load of 1 kg using an abrasion resistance tester (DEASUNG PRECISION, Korea) and an eraser for abrasion resistance testing (MINOAN, Korea), and then the water contact angle was measured in the same manner as in Test Example 3. If the contact angle after the abrasion resistance test was 95° or more, it could be judged to be good (see FIG. 5). The configurations of the above-mentioned Examples and Comparative Examples and the test results thereof are summarized in the table below.
[0160] [Table 3]
[0161] As shown in the above table, the composite films of Examples 1 to 4 had high adhesion between the functional layer and the base film, and were excellent in performance in terms of antistatic properties, antifouling properties, and chemical resistance.
[0162] On the other hand, the composite film of Comparative Example 1 had very poor antistatic properties despite high adhesion between the functional layer and the base film, and the composite films of Comparative Examples 2 to 7 had good antistatic and antifouling properties but lacked chemical resistance, and in particular had very poor adhesion between the functional layer and the base film. [Explanation of symbols]
[0163] 1: Display device 2: Test equipment 3:Water 4: Ethanol 5: Eraser θ: contact angle 10a: Composite film sample 10: Composite film (cover window) 20: Display panel 30: Substrate 40: Frame 100: Base film 200: Functional layer
Claims
1. A base film; A functional layer formed on the base film, The functional layer is An acrylate binder; and an acrylamide monomer, The acrylamide monomer is contained in an amount of more than 0 parts by weight and 20 parts by weight or less, based on 100 parts by weight of the acrylate binder.
2. The surface resistance of the functional layer is 1×10 13 Ω / sq or less, 2. The composite film for a display device according to claim 1, wherein the surface of the functional layer is subjected to a cross-cut test based on ASTM D3359 standard and has a result of 3B or higher.
3. 2. The composite film for a display device as described in claim 1, wherein the water contact angle measured after applying 10 μL of ethanol with a purity of 99.5% or higher to the surface of the functional layer and rubbing it 3,000 times with a load of 1 kg using an eraser for abrasion resistance testing is 95° or more.
4. 2. The composite film for a display device according to claim 1, wherein the acrylate-based binder comprises a urethane acrylate-based oligomer and an acrylate-based monomer.
5. 10. The composite film for a display device according to claim 1, wherein the functional layer further comprises an antistatic agent.
6. 6. The composite film for a display device according to claim 5, wherein the functional layer further comprises one or more selected from the group consisting of an antifouling agent, a UV absorber, and a photoinitiator.
7. The composite film for a display device according to claim 1 , wherein the functional layer is formed directly on the surface of the base film.
8. The composite film for a display device according to claim 1 , wherein the substrate film comprises at least one selected from the group consisting of a polymer film and ultra-thin glass (UTG).
9. A display panel; a cover window disposed on a front surface of the display panel; The cover window is A base film; A functional layer formed on the base film, The functional layer is An acrylate binder; and an acrylamide-based monomer.
Citation Information
Patent Citations
Material for electrophotographic equipment and conductive roll for electrophotographic equipment
JP2009244461A
Laminate and conductive roller
JP2017001330A
Anti-fogging coated glass
JP2021527022A
KR20147367
Photocurable resin composition
WO2018038056A1