Aluminum alloy multi-layer brazing sheet material for flux-free brazing
A multilayer brazing sheet with a 3xxx alloy core and specific Si-containing cladding layers addresses flux-related issues in brazing, achieving efficient and environmentally friendly joint formation in an inert gas atmosphere.
Patent Information
- Application Number
- JP2022546140
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-03-02
- Filing Date
- 2021-01-26
- Publication Date
- 2024-09-26
- Estimated Expiration
- 2041-01-26
AI Technical Summary
Conventional brazing processes for aluminum alloys require the use of flux, which can lead to environmental pollution and affect the quality of the brazed joints, while flux-free brazing in an inert gas atmosphere faces challenges in achieving effective joint formation and preventing oxidation of the molten brazing material.
A multilayer brazing sheet comprising a 3xxx alloy core layer with a covering cladding layer containing 2-5 wt% Si and an Al-Si brazing cladding layer with 7-13 wt% Si, where the covering cladding layer has a thickness twice that of the Al-Si brazing layer, facilitates flux-free brazing by preventing oxidation and ensuring proper joint formation through controlled Mg content and inert gas atmosphere.
The solution enables high-quality brazed joints without flux, reducing environmental impact and improving the brazing process efficiency by minimizing oxidation and ensuring effective joint formation in an inert gas atmosphere.
Smart Images

Figure 0007556969000002 
Figure 0007556969000001
Abstract
Description
[Technical field]
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims the benefit of and priority to European Patent Application No. 20154258.6, filed January 29, 2020, and entitled "Aluminium alloy multi-layered brazing sheet material for fluxfree brazing", and European Patent Application No. 20160495.6, filed March 2, 2020, and entitled "Aluminium alloy multi-layered brazing sheet material for fluxfree brazing", the contents of which are incorporated herein by reference in their entireties.
[0002] Described herein is an aluminum alloy multi-layer brazing sheet product or material for fluxless inert gas atmosphere brazing ("CAB"), comprising a 3xxx series aluminum alloy core layer with a cladding layer containing 2-5 wt% Si on one or both sides of the core layer, and an Al-Si brazing cladding layer containing 6-13 wt% Si located between the core layer and the cladding layer. Also described herein is a brazing assembly produced in a brazing operation, the brazing assembly including various components, at least one component being made from the aluminum alloy multi-layer brazing sheet material described herein. [Background technology]
[0003] Aluminum or aluminum alloy base metals in the form of sheets or extruded profiles are used to make shaped or formed articles. In some of these processes, (formed) aluminum parts containing the base metal are interconnected. Sometimes one end of the base metal is interconnected with the other end, and sometimes one base metal is combined with one or more other base metals. This is generally done by brazing. In a brazing process, at least a portion of the base metal to be brazed is coated with a brazing filler metal or brazing alloy, or a composition that produces a brazing alloy when heated. After the base metal parts are assembled, they are heated until the brazing filler metal or brazing alloy melts. The melting point of the brazing filler metal is lower than the melting point of the aluminum base metal or aluminum core sheet.
[0004] Brazing sheet products have found wide application in heat exchangers and other similar equipment. Conventional brazing sheet products have a core of rolled sheet, usually, but not limited to, 3xxx series aluminum alloy, and an aluminum brazing clad layer (also known as aluminum cladding layer) on at least one surface of the core sheet. The aluminum brazing clad layer is made of a 4xxx series alloy containing silicon as the main alloy component in an amount ranging from 4 to 20 wt%. The aluminum brazing clad layer can be bonded or joined to the aluminum core alloy by various methods known in the art, such as roll bonding, cladding spray forming, or semi-continuous or continuous casting processes.
[0005] These aluminum brazing cladding layers typically have liquidus temperatures in the range of about 540°C to 620°C, below the solidus temperature of the aluminum core alloy. Most brazing is carried out at temperatures between 560°C and 615°C. Summary of the Invention
[0006] The embodiments of the invention encompassed are defined by the claims, not this Summary. This Summary is a high-level overview of various aspects of the invention and introduces some concepts that are further described in the Detailed Description section below. This Summary is not intended to identify key or essential features of the claimed subject matter, nor is it intended to be used alone to determine the scope of the claimed subject matter. The subject matter should be understood by reference to the entire specification, some or all of the drawings, and appropriate portions of the claims.
[0007] The present invention describes an aluminum alloy multilayer brazing sheet product for brazing in an inert gas atmosphere without the use of flux, comprising a core layer made of a 3xxx alloy containing 0.20-0.75 wt% Mg, the core layer having a coating clad layer containing 2-5 wt% Si on one or both sides of the 3xxx alloy core layer, and an Al-Si brazing clad layer containing 7-13 wt% Si located between the 3xxx alloy core layer and the coating clad layer, wherein the coating clad layer has a thickness of X1 and the Al-Si brazing clad layer has a thickness of X2, where X2≧2X1. Optionally, the 3xxx alloy core layer contains 0.20%-0.60% Mg, 0.20%-0.30% Mg, or 0.40%-0.55% Mg.
[0008] In some cases, the coated cladding layer is Bi-free and Li-free. Optionally, the coated cladding layer is Mg-free, Bi-free and Li-free, and comprises the following (wt%): Si (2%-5%); Fe (max. 0.5%); Mn (max. 0.2%); Cu (max. 0.1%); Zn (max. 0.4%); Ti (max. 0.1%); Including incidental impurities (<0.05% each, <0.15% in total) and aluminum.
[0009] Optionally, the Si content of the coated cladding layer is 2.5% to 4.0%.
[0010] In some cases, the 3xxx alloy core layer contains (wt%) Mn (0.5%-1.8%); Mg (0.20%-0.75%); Cu (up to 1.1%); Si (up to 0.2%); Fe (up to 0.7%); Cr (up to 0.3%); Sc (up to 0.3%); Zr and / or V (up to 0.3%); Ti (up to 0.25%); Zn (up to 1.2%); unavoidable impurities (up to 0.05% each, up to 0.2% total), and Aluminum. In some cases, the 3xxx alloy core layer contains (wt%) Mn (0.5%-1.8%); Mg (0.20%-0.75%); Cu (up to 1.1%); Si (up to 0.4%); Fe (up to 0.7%); Cr (up to 0.3%); Sc (up to 0.3%); Zr and / or V (up to 0.3%); Ti (up to 0.25%); Zn (up to 1.2%); unavoidable impurities (up to 0.05% each, up to 0.2% total), and Aluminum.
[0011] Optionally, the 3xxx alloy core layer has a Si content of less than 0.10%. Optionally, the 3xxx alloy core layer has a Si content of less than 0.40% or less than 0.30%. Optionally, the 3xxx alloy core layer has a Cu content of up to 0.15% or in the range of 0.15% to 1.1%.
[0012] In some cases, the Al-Si brazing cladding layer contains (in wt%): Si (7%-13%); Mg (max. 0.5%); Fe (max. 0.7%); Cu (max. 0.3%); Mn (max. 0.8%); Zn (max. 2%); Bi (max 0.3%); Ti (max. 0.25%); Including unavoidable impurities (<0.05% each, <0.2% in total), and aluminum.
[0013] Optionally, the Al-Si brazing cladding layer contains 10% to 13% Si. Optionally, the Al-Si brazing cladding layer contains 0.02% to 0.5% Mg.
[0014] In some cases, the aluminum alloy multi-layer brazing sheet product is surface-treated with an alkaline or acidic etching solution before the brazing process. Optionally, the coating clad layer has a thickness of X1 and the Al-Si brazing clad layer has a thickness of X2, where X2≧2.5X1 or X2≧3X1.
[0015] Also described herein is a process for manufacturing a brazed heat exchanger, comprising the steps of providing at least one aluminum alloy multi-layer brazing sheet product as described herein and brazing by flux-free controlled atmosphere brazing (or controlled atmosphere brazing (CAB)). Optionally, the aluminum alloy multi-layer brazing sheet is surface treated with an alkaline or acidic etchant prior to the brazing step.
[0016] Further described herein is the use of the aluminum alloy multi-layer brazing sheet products described herein for manufacturing heat exchange devices in flux-free controlled atmosphere brazing (CAB) operations.
[0017] Other objects and advantages of the present invention will become apparent from the following detailed description of non-limiting embodiments and the drawings. [Brief description of the drawings]
[0018] [Figure 1] A and B illustrate the arrangement of the aluminum alloy multi-layer brazing sheet product described herein. [Diagram 2] FIG. 2 is an isometric view of a portion of a brazed heat exchanger assembly. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] As understood hereinafter, unless otherwise indicated, aluminum alloy designations and temper designations refer to the Aluminum Association designations in the Aluminum Standards and Data and Registry published by the Aluminum Association in 2019, which are frequently updated, and are well known to those skilled in the art. Temper designations are specified in European standard EN515.
[0020] With respect to any description of alloy compositions or preferred alloy compositions, all references to percentages are in weight percent unless otherwise indicated.
[0021] As used herein, the terms "up to" or "up to about" expressly include, but are not limited to, the possibility of zero weight percent of the particular alloying element to which it refers. For example, up to about 0.20% Cr may include an aluminum alloy having no Cr.
[0022] As used herein, the meanings of "a," "an," or "the" include singular and plural references unless the context clearly dictates otherwise.
[0023] As used herein, a plate generally has a thickness of greater than about 15 mm. For example, a plate can refer to an aluminum product having a thickness of greater than about 15 mm, greater than about 20 mm, greater than about 25 mm, greater than about 30 mm, greater than about 35 mm, greater than about 40 mm, greater than about 45 mm, greater than about 50 mm, or greater than about 100 mm.
[0024] As used herein, a shate, also referred to as a sheet plate, typically has a thickness of about 4 mm to about 15 mm. For example, the shate may have a thickness of about 4 mm, about 5 mm, about 6 mm, about 7 mm, about 8 mm, about 9 mm, about 10 mm, about 11 mm, about 12 mm, about 13 mm, about 14 mm, or about 15 mm.
[0025] As used herein, sheet generally refers to an aluminum product having a thickness of less than about 4 mm. For example, the sheet may have a thickness of less than about 4 mm, less than about 3 mm, less than about 2 mm, less than about 1 mm, less than about 0.5 mm, less than about 0.3 mm, or less than about 0.1 mm.
[0026] All ranges disclosed herein should be understood to encompass any and all subranges subsumed therein. For example, a stated range of "1 to 10" should be considered to encompass any and all subranges between the minimum value of 1 and the maximum value of 10, inclusive, i.e., all subranges beginning with a minimum value of 1 or greater (e.g., 1 to 6.1) and ending with a maximum value of 10 or less (e.g., 5.5 to 10).
[0027] As used herein, the meaning of "ambient temperature" can include a temperature of about 15°C to about 30°C, such as about 15°C, about 16°C, about 17°C, about 18°C, about 19°C, about 20°C, about 21°C, about 22°C, about 23°C, about 24°C, about 25°C, about 26°C, about 27°C, about 28°C, about 29°C, or about 30°C.
[0028] Provided herein is an improved brazing sheet product for brazing in an inert gas atmosphere without the use of a flux. Also provided herein is a multi-layer brazing sheet product for brazing in an inert gas atmosphere.
[0029] Specifically, the present specification provides an aluminum alloy multi-layer brazing sheet product for brazing in an inert gas atmosphere without using a flux, the aluminum alloy multi-layer brazing sheet product comprising: a core layer made of a 3xxx alloy containing 0.20-0.75 wt% Mg, the core layer having a coating clad layer containing 2-5 wt% Si on one or both sides of the 3xxx alloy core layer; and an Al-Si brazing clad layer containing 7-13 wt% Si located between the 3xxx alloy core layer and the coating clad layer, wherein the coating clad layer has a thickness of X1, the Al-Si brazing clad layer has a thickness of X2, and X2≧2X1.
[0030] The 3xxx series aluminum alloy core layer comprises 0.20%-0.75% Mg, preferably 0.20-0.60% Mg. Optionally, the 3xxx series aluminum alloy core layer comprises 0.25%-0.75% Mg, 0.30%-0.75% Mg, or 0.35%-0.75% Mg. In one embodiment, the 3xxx series aluminum alloy core layer comprises 0.20%-0.30% Mg. In another embodiment, the 3xxx series aluminum alloy core layer comprises 0.40%-0.55% Mg.
[0031] In some cases, the coated clad layer (also referred to herein as the thin coated layer) has a liquidus temperature substantially higher than that of the Al-Si brazing clad layer. Therefore, during the subsequent brazing, which is performed above the liquidus temperature of the Al-Si alloy brazing clad layer and below the liquidus temperature of the thin coated clad layer, the molten brazing material melts the Al-Si alloy brazing clad layer while the thin coated clad layer is kept partially solid to prevent or at least limit oxidation of the molten brazing material, and further, the Al-Si alloy brazing material oozes out of the segregated parts of the thin coated clad layer and spreads on the surface of the thin coated clad layer due to volume expansion, forming a new surface that becomes the brazed joint. Finally, the coated clad layer dissolves in the molten filler metal. The presence of Mg in the Al-Si brazing clad layer facilitates the decomposition of the oxide film on the surface of the brazing sheet product prior to brazing as the Mg evaporates from the surface. However, too much Mg content in the Al-Si brazing clad layer creates an undesirable Mg-oxide film prior to brazing, which adversely affects the flow of the molten material during brazing. The Al-Si brazing clad layer may contain limited amounts of Mg, and by retaining a controlled and targeted amount of Mg in the 3xxx series aluminum alloy core layer, some of the Mg will diffuse into the Al-Si brazing clad layer over time during the heating cycle of the brazing operation, slowing down the evaporation of Mg. This avoids the formation of excess Mg-oxides in the early stages of the brazing operation and improves brazing in inert gas atmospheres without fluxes.
[0032] In one embodiment, the aluminum alloy core layer comprises (in wt%): Mn (0.5% to 1.8%, preferably 0.6% to 1.5%, more preferably 0.8% to 1.3%); Mg (0.20% to 0.75%, preferably 0.20% to 0.60%); Cu (maximum 1.1%, preferably maximum 0.15%, or in the range of 0.15% to 1.1%, preferably 0.20% to 0.9%, more preferably 0.20% to 0.60%); Si (max 0.4%, e.g. max 0.2%, preferably <0.10%); Fe (max 0.7%, preferably max 0.5%, more preferably in the range of 0.05% to 0.35%); Cr (max 0.3%, preferably max 0.20%, more preferably max 0.09%, most preferably max 0.04%); Sc (max 0.3%, preferably max 0.25%); Zr and / or V (max 0.3%, preferably max 0.09%, more preferably max 0.04%); Ti (max 0.25%, preferably 0.01%-0.20%, more preferably 0.01%-0.12%); Zn (max 1.2%, preferably max 0.5%, most preferably max 0.2%); It is made from a 3xxx series aluminum alloy consisting of aluminum and impurities, typically with a maximum of 0.05% each and a maximum of about 0.2% in total, and preferably not exceeding a total of about 0.15%.
[0033] The Mn content in the aluminum alloy core layer can be about 0.5%-1.8% Mn, (e.g., 0.6%-1.5%, 0.7%-1.4%, 0.8%-1.3%, or 0.9%-1.2%). Optionally, the Mn content can be about 0.5%, about 0.55%, about 0.6%, about 0.65%, about 0.7%, about 0.75%, about 0.8%, about 0.85%, about 0.9%, about 0.95%, about 1%, about 1.05%, about 1.1%, about 1.15%, about 1.2%, about 1.25%, about 1.3%, about 1.35%, about 1.4%, about 1.45%, about 1.5%, about 1.55%, about 1.6%, about 1.65%, about 1.7%, about 1.75%, or about 1.8%.
[0034] The Mg content in the aluminum alloy core layer can be about 0.2%-0.75% Mg (e.g., 0.20%-0.60%, 0.25%-0.55%, 0.30-0.50%, or 0.35%-0.45%). Optionally, the Mg content can be about 0.2%, about 0.25%, about 0.3%, about 0.35%, about 0.4%, about 0.45%, about 0.5%, about 0.55%, about 0.6%, about 0.65%, about 0.7%, or about 0.75%.
[0035] The Cu content in the aluminum alloy core layer can be up to 1.1% Cu (e.g., up to 0.15%, 0.15%-1.1%, 0.20%-0.9%, or 0.20%-0.60%). Optionally, the Cu content can be about 0.05%, about 0.1%, about 0.15%, about 0.2%, about 0.25%, about 0.3%, about 0.35%, about 0.4%, about 0.45%, about 0.5%, about 0.55%, about 0.6%, about 0.65%, about 0.7%, about 0.75%, about 0.8%, about 0.85%, about 0.9%, about 0.95%, about 1%, about 1.05%, or greater than about 1.1%.
[0036] The Si content in the aluminum alloy core layer can be up to 0.4% Si, up to 0.3% Si, or up to 0.2% Si (e.g., less than 0.10%, 0.01%-0.2%, 0.05%-0.4%, 0.05%-0.3%, 0.1%-0.4%, 0.05%-0.2%, or 0.05%-0.10%). Optionally, the Si content can be about 0.05%, about 0.06%, about 0.07%, about 0.08%, about 0.09%, about 0.1%, about 0.11%, about 0.12%, about 0.13%, about 0.14%, about 0.15%, about 0.16%, about 0.17%, about 0.18%, about 0.19%, about 0.2%, about 0.21%, about 0.2 It may be about 2%, about 0.23%, about 0.24%, about 0.25%, about 0.26%, about 0.27%, about 0.28%, about 0.29%, about 0.3%, about 0.31%, about 0.32%, about 0.33%, about 0.34%, about 0.35%, about 0.36%, about 0.37%, about 0.38%, about 0.39% or about 0.4%.
[0037] The Fe content in the aluminum alloy core layer can be up to 0.7% Fe (e.g., up to 0.5%, 0.05%-0.35%, 0.06%-0.35%, 0.1%-0.3%, or 0.15%-0.25%). Optionally, the Fe content can be about 0.01%, about 0.05%, about 0.1%, about 0.15%, about 0.2%, about 0.25%, about 0.3%, about 0.35%, about 0.4%, about 0.45%, about 0.5%, about 0.55%, about 0.6%, about 0.65%, or about 0.7%.
[0038] The Cr content in the aluminum alloy core layer can be up to 0.3% Cr (e.g., up to 0.20%, up to 0.09%, up to 0.04%, 0.05%-0.3%, 0.1%-0.25%, or 0.15%-0.2%). Optionally, the Cr content can be about 0.01%, about 0.05%, about 0.1%, about 0.15%, about 0.2%, about 0.25%, or about 0.3%.
[0039] The Sc content in the aluminum alloy core layer can be up to 0.3% Sc (e.g., up to 0.25%, up to 0.20%, up to 0.09%, up to 0.04%, 0.05%-0.3%, 0.1%-0.25%, or 0.15%-0.2%). Optionally, the Sc content can be about 0.01%, about 0.05%, about 0.1%, about 0.15%, about 0.2%, about 0.25%, or about 0.3%.
[0040] The Zr and / or V content in the aluminum alloy core layer can be up to 0.3% Zr and / or V (e.g., up to 0.25%, up to 0.20%, up to 0.09%, up to 0.04%, 0.05%-0.3%, 0.1%-0.25%, or 0.15%-0.2%). Optionally, the Zr and / or V content can be about 0.01%, about 0.05%, about 0.1%, about 0.15%, about 0.2%, about 0.25%, or about 0.3%.
[0041] The Ti content in the aluminum alloy core layer can be up to 0.25% Ti (e.g., 0.01%-0.20% or 0.01%-0.12%). Optionally, the Ti content can be about 0.01%, about 0.05%, about 0.1%, about 0.15%, about 0.2%, or about 0.25%.
[0042] The Zn content in the aluminum alloy core layer can be up to 1.2% Zn (e.g., up to 0.5%, up to 0.2%, 0.05%-1.2%, 0.06%-1.2%, 0.1%-1.0%, or 0.25%-0.8%). Optionally, the Zn content can be about 0.05%, about 0.1%, about 0.15%, about 0.2%, about 0.25%, about 0.3%, about 0.35%, about 0.4%, about 0.45%, about 0.5%, about 0.55%, about 0.6%, about 0.65%, about 0.7%, about 0.75%, about 0.8%, about 0.85%, about 0.9%, about 0.95%, about 1%, about 1.05%, about 1.1%, about 1.15%, or about 1.2%.
[0043] The aluminum alloy core layer also contains aluminum and impurities, as described above.
[0044] Optionally, the aluminum alloy core layer may be one of the following aluminum alloy designations: AA3002, AA3102, AA3003, AA3103, AA3103A, AA3103B, AA3203, AA3403, AA3004, AA3004A, AA3104, AA3204, AA3304, AA3005, AA3005A, AA3105, AA3105A, AA3105B, AA3007, AA3107, AA3 AA3025, AA3026, AA3030, AA3130, and AA3065.
[0045] In one embodiment, the coating cladding layer does not contain any wetting element or any element that modifies the surface tension of the molten Al-Si alloy, selected from the group of Ag, Be, Bi, Ca, Ce, La, Li, Na, Pb, Se, Sb, Sr, Th, and Y. By "free," we mean that Ag, Be, Bi, Ca, Ce, La, Li, Na, Pb, Se, Sb, Sr, Th, or Y are not intentionally added to the chemical composition, but trace amounts of the elements may still find their way into the coating layer through impurities and / or leakage from contact with manufacturing equipment. In practice, this means that each of these specified elements, if present, is present in an amount up to about 0.005%, typically less than about 0.001%. For example, one example of a trace amount is less than 10 ppm Sr, preferably less than 5 ppm Sr. Another example of an even trace amount is less than 10 ppm Na, preferably less than 3 ppm Na.
[0046] The coating cladding layer is preferably Mg-free, meaning that its level is below about 0.05%, such as below about 0.03% or below 0.01%. By "free" we mean that Mg is not intentionally added to the chemical composition, but trace amounts of the element may still find their way into the coating layer through impurities and / or leakage from contact with manufacturing equipment.
[0047] In one embodiment, the coated cladding layer comprises (in wt%): Si (2% to 5%, preferably 2.5% to 4.0%, more preferably 3.0% to 3.9%); Fe (max 0.5%, preferably max 0.3%); Mn (max 0.2%, preferably max 0.10%); Cu (max 0.1%, preferably max 0.05%); Zn (max 0.4%, preferably max 0.2%); Ti (max 0.1%, preferably max 0.05%); It is a Mg-free aluminum alloy containing unavoidable impurities (<0.05% each, <0.15% in total, preferably <0.02% each, <0.05% in total) and aluminum.
[0048] The Si content in the coated cladding layer can be 2% to 5% (e.g., 2.5% to 4.0%, or 3.0% to 3.9%). Optionally, the Si content can be about 0.2%, about 0.25%, about 0.3%, about 0.35%, about 0.4%, about 0.45%, or about 0.5%.
[0049] The Fe content in the coating cladding layer can be up to 0.5% (e.g., up to 0.3%, 0.05%-0.5%, 0.1%-0.4%, 0.15%-0.4%, or 0.2%-0.35%). Optionally, the Fe content can be about 0.05%, about 0.1%, about 0.15%, about 0.2%, about 0.25%, about 0.3%, about 0.35%, about 0.4%, about 0.45%, or about 0.5%.
[0050] The Mn in the coated cladding layer can be up to 0.2% (e.g., up to 0.10%, 0.05%-0.2%, 0.1%-0.2%, or 0.15%-0.2%). Optionally, the Mn content can be about 0.05%, about 0.1%, about 0.15%, or about 0.2%.
[0051] The Cu in the coating cladding layer can be up to 0.1% (e.g., up to 0.05%, 0.01%-0.1%, 0.05%-0.1%, or 0.06%-0.1%). Optionally, the Cu content can be about 0.01%, about 0.02%, about 0.03%, about 0.04%, about 0.05%, about 0.06%, about 0.07%, about 0.08%, about 0.09%, or about 0.1%.
[0052] The Zn in the coating layer can be up to 0.4% (e.g., up to 0.3%, up to 0.2%, up to 0.1%, 0.01%-0.4%, 0.05%-0.4%, 0.06%-0.35%, 0.1%-0.35%, or 0.15%-0.3%). Optionally, the Zn content can be about 0.05%, about 0.1%, about 0.15%, about 0.2%, about 0.25%, about 0.3%, about 0.35%, or about 0.4%.
[0053] The Ti in the coating cladding layer can be up to 0.1% (e.g., up to 0.05%, 0.01%-0.1%, 0.05%-0.1%, or 0.06%-0.1%). Optionally, the Ti content can be about 0.01%, about 0.02%, about 0.03%, about 0.04%, about 0.05%, about 0.06%, about 0.07%, about 0.08%, about 0.09%, or about 0.1%.
[0054] The overlying cladding layer also contains aluminum and impurities as described above.
[0055] In one embodiment, the coated cladding layer comprises (in wt%): Si (2% to 5%), Fe (max. 0.5%), Mn (max. 0.2%), Cu (max. 0.1%), Zn (max. 0.4%), Ti (max. 0.1%), A Mg-free aluminum alloy consisting of the incidental impurities (<0.05% each and <0.15% total), aluminum, and having the desired narrower ranges as described and claimed herein.
[0056] In some examples, the Al-Si braze cladding layer comprises (in wt%): Si (7% to 13%, preferably 10% to 13%, more preferably 11% to 13%); Mg (max 0.5%, preferably 0.02%-0.5%, more preferably 0.02%-0.20%); Fe (max 0.7%, preferably max 0.5%); Cu (max 0.3%, preferably max 0.1%); Mn (max 0.8%, preferably max 0.2%); Zn (max 2%, preferably max 0.3%); Ti (max. 0.25%); It has a composition consisting of aluminum and unavoidable impurities (<0.05% each, <0.2% in total).
[0057] In certain embodiments, the Al-Si brazing cladding layer may further comprise up to 0.3%, preferably 0.1% to 0.3%, more preferably 0.11% to 0.20% Bi to promote joint formation during brazing.
[0058] The Si in the Al-Si brazing cladding layer can be 7% to 13% (eg, 10% to 13%, 11% to 13%, 7.5% to 12.5%, or 8% to 12%). Optionally, the Si content is about 7%, about 7.05%, about 7.1%, about 7.15%, about 7.2%, about 7.25%, about 7.3%, about 7.35%, about 7.4%, about 7.45%, about 7.5%, about 7.55%, about 7.6%, about 7.65%, about 7.7%, about 7.75%, about 7.8%, about 7.85%, about 7.9%, about 7.95%, about 8%, about 8.05%, about 8.1%, about 8.15%, about 8.2%, about 8.25%, about 8.3%, about 8.35%, about 8.4%, about 8.45%, about 8.5%, about 8. 55%, approx. 8.6%, approx. 8.65%, approx. 8.7%, approx. 8.75%, approx. 8.8%, approx. 8.85%, approx. 8.9%, approx. 8.95%, approx. 9%, approx. 9.05%, approx. 9.1%, approx. 9.15%, approx. 9.2%, approx. 9.25%, approx. 9.3%, approx. 9.35%, approx. 9.4%, approx. 9.45%, approx. 9.5%, approx. 9.55%, approx. 9.6%, approx. 9.65%, approx. 9.7%, approx. 9.75%, approx. 9.8%, approx. 9.85%, approx. 9.9%, approx. 9.95%, approx. 10%, approx. 10.05%, approx. 10.1%, approx. 10.15%, approx. 1 0.2%, approx. 10.25%, approx. 10.3%, approx. 10.35%, approx. 10.4%, approx. 10.45%, approx. 10.5%, approx. 10.55%, approx. 10.6%, approx. 10.65%, approx. 10.7%, approx. 10.75%, approx. 10.8%, approx. 10.85%, approx. 10.9%, approx. 10.95%, approx. 11%, approx. 11.05%, approx. 11.1%, approx. 11.15%, approx. 11.2%, approx. 11.25%, approx. 11.3%, approx. 11.35%, approx. 11.4%, approx. 11.45%, approx. 11.5%, approx. 11.55%, approx. 11.6%, It can be about 11.65%, about 11.7%, about 11.75%, about 11.8%, about 11.85%, about 11.9%, about 11.95%, about 12%, about 12.05%, about 12.1%, about 12.15%, about 12.2%, about 12.25%, about 12.3%, about 12.35%, about 12.4%, about 12.45%, about 12.5%, about 12.55%, about 12.6%, about 12.65%, about 12.7%, about 12.75%, about 12.8%, about 12.85%, about 12.9%, about 12.95%, or about 13%.
[0059] The Mg in the Al-Si brazing cladding layer can be up to 0.5% (e.g., 0.01%-0.5%, 0.02%-0.5%, 0.02%-0.4%, 0.02%-0.3%, 0.02%-0.2%, 0.05%-0.5%, 0.1%-0.5%, 0.1%-0.4%, or 0.1%-0.3%). Optionally, the Mg content can be about 0.01%, about 0.02%, about 0.03%, about 0.04%, about 0.05%, about 0.06%, about 0.07%, about 0.08%, about 0.09%, about 0.1%, about 0.15%, about 0.2%, about 0.25%, about 0.3%, about 0.35%, about 0.4%, about 0.45%, or about 0.5%.
[0060] The Fe in the Al-Si brazing cladding layer can be up to 0.7% (e.g., up to 0.5%, 0.05%-0.35%, 0.06%-0.35%, 0.1%-0.3%, or 0.15%-0.25%). Optionally, the Fe content can be about 0.01%, about 0.05%, about 0.1%, about 0.15%, about 0.2%, about 0.25%, about 0.3%, about 0.35%, about 0.4%, about 0.45%, about 0.5%, about 0.55%, about 0.6%, about 0.65%, or about 0.7%.
[0061] The Cu in the Al-Si brazing cladding layer can be up to 0.3% (e.g., up to 0.2%, up to 0.1%, up to 0.09%, up to 0.04%, 0.05%-0.3%, 0.1%-0.25%, or 0.15%-0.2%). Optionally, the Cu content can be about 0.01%, about 0.05%, about 0.1%, about 0.15%, about 0.2%, about 0.25%, or about 0.3%.
[0062] The Mn in the Al-Si brazing cladding layer can be up to 0.8% (e.g., up to 0.6%, up to 0.4%, up to 0.2%, 0.05%-0.8%, 0.1%-0.7%, 0.2%-0.6%, or 0.25%-0.55%). Optionally, the Mn content can be about 0.01%, about 0.05%, about 0.1%, about 0.15%, about 0.2%, about 0.25%, about 0.3%, about 0.35%, about 0.4%, about 0.45%, about 0.5%, about 0.55%, about 0.6%, about 0.65%, about 0.7%, about 0.75%, or about 0.8%.
[0063] The Zn in the Al-Si brazing cladding layer can be up to 2% (e.g., up to 1%, up to 0.5%, up to 0.3%, 0.01%-0.3%, 0.05%-0.3%, or 0.05%-0.2%). Optionally, the Zn content can be about 0.01%, about 0.02%, about 0.03%, about 0.04%, about 0.05%, about 0.06%, about 0.07%, about 0.08%, about 0.09%, about 0.1%, about 0.11%, about 0.12%, about 0.13%, about 0.14%, about 0.15%, about 0.16%, about 0.17%, about 0.18%, about 0.19%, or about 0.2%.
[0064] The Ti in the Al-Si brazing cladding layer can be up to 0.25% (e.g., up to 0.20%, up to 0.09%, up to 0.04%, 0.05%-0.25%, 0.1%-0.25%, or 0.15%-0.2%). Optionally, the Ti content can be about 0.01%, about 0.05%, about 0.1%, about 0.15%, about 0.2%, or about 0.25%.
[0065] The Bi in the Al-Si brazing cladding layer can be up to 0.3% Bi, (e.g., up to 0.20%, up to 0.09%, up to 0.04%, 0.1%-0.3%, preferably 0.11%-0.20%, 0.05%-0.3%, 0.1%-0.25%, or 0.15%-0.2%). Optionally, the Bi content can be about 0.01%, about 0.05%, about 0.1%, about 0.15%, about 0.2%, about 0.25%, or about 0.3%.
[0066] The Al-Si braze cladding layer also contains aluminum and impurities as discussed above.
[0067] In some examples, the Al-Si braze cladding layer comprises (in wt%): Si (7% to 13%, preferably 10% to 13%, more preferably 11% to 13%); Mg (max 0.5%, preferably 0.02%-0.5%, more preferably 0.02%-0.20%); Fe (max 0.7%, preferably max 0.5%); Cu (max 0.3%, preferably max 0.1%); Mn (max 0.8%, preferably max 0.2%); Zn (max 2%, preferably max 0.3%); Bi (max 0.3%, preferably 0.1%-0.3%); Ti (max. 0.25%); It has a composition consisting of aluminum and unavoidable impurities (<0.05% each, <0.2% in total).
[0068] In some examples of the aluminum alloy multi-layer brazing sheet material described herein, both sides of the 3xxx alloy core layer are provided with an overlay clad layer and an Al-Si braze clad layer. When both sides of the 3xxx alloy core layer are similarly clad, the brazing sheet material has a five-layer configuration.
[0069] In one embodiment, the aluminum alloy multi-layer brazing sheet material does not include or has no aluminum alloy layer between the 3xxx alloy core layer and the Al-Si brazing clad layer, which prevents diffusion of Mg from the 3xxx alloy core layer to the Al-Si brazing clad layer.
[0070] The aluminum alloy multi-layer brazing sheet material described herein can be manufactured through various techniques. For example, the aluminum alloy multi-layer brazing sheet material can be manufactured by roll bonding, as will be understood by those skilled in the art. The process generally includes the following steps: Casting different aluminum alloys to obtain blocks for rolling; Milling any face of the block to remove surface segregation zones resulting from the casting process and improve the flatness of the product; Preheat the brazing block to 400℃~550℃; hot rolling the block carrying the coating layer and the Al-Si braze clad layer to a desired thickness to obtain a plurality of hot rolled clad liners; Alternatively, hot rolling a block of the coating layer and the Al-Si brazing cladding layer to an intermediate thickness, laminating the two materials at the intermediate thickness, and hot rolling the laminate to obtain a hot rolled clad liner of the required thickness consisting of two layers; Optionally, homogenizing the aluminum core alloy block at 500°C to 630°C for at least 1 hour, preferably 1 to 20 hours; combining the core alloy block, at least on one side, and optionally on both sides, with rolled clad liner(s) to obtain a sandwich; Preheat the sandwich to 400°C-550°C; hot rolling the sandwich to an intermediate thickness, e.g. 2-10 mm; cold rolling the hot rolled sandwich to a desired final thickness to obtain a multi-layer brazing sheet product; and Optionally, this may include annealing at 200° C. to 480° C. to obtain the multilayer brazing sheet product in the desired temper, for example O, H1x, H2x or H3x temper.
[0071] Alternatively, but less preferably, one or more of the coating cladding layer and the Al-Si brazing cladding layer can be applied onto the 3xxx alloy core layer by thermal spraying techniques. In other cases, the aluminum alloy core layer and the Al-Si alloy brazing cladding layer can be produced by casting techniques, for example, as disclosed in International Patent Document WO-2004 / 112992, which is incorporated herein by reference in its entirety, and the coating cladding layer can then be applied, for example, by roll bonding or thermal spraying techniques.
[0072] In one embodiment, the aluminum alloy multi-layer brazing sheet material thus obtained is treated with an alkaline or acidic etchant to remove the surface oxide film prior to the brazing process to facilitate the flux-free CAB brazing operation.
[0073] Preferably, the outer surface of the aluminum alloy multi-layer brazing sheet material is treated with an acid etching solution. The acid etching solution preferably contains H2SO4 in an amount of 10 g / L to 25 g / L (e.g., 12 g / L to 16 g / L, or 14 g / L). The acid etching solution may also contain HF in an amount of 0.5 g / L to 5 g / L (e.g., 1 g / L to 3 g / L, or 2 g / L of HF (5%)).
[0074] The acidic etching solution may contain at least one of the following inorganic acids: H2SO4, H3PO4, HCl, HF, and / or HNO3. Preferably, the acidic etching solution is a mixture of H2SO4 and HF. The acidic etching solution is generally in the form of a solution, and the content of inorganic acid is generally 0.5-20 wt% (e.g., 1-20 wt%, 2-18 wt%, 3-16 wt%, 4-15 wt%, 5-12.5 wt%, or 6-10 wt%).
[0075] According to another embodiment, the etching solution may be alkaline. The alkaline etching solution may include at least one of the following: NaOH and / or KOH. The alkaline etching solution is typically in the form of a solution, and the alkali content is typically 0.5-20 wt% (e.g., 1-20 wt%, 2-18 wt%, 3-16 wt%, 4-15 wt%, 5-12.5 wt%, or 6-10 wt%).
[0076] The alkaline etching solution may further contain a surfactant (e.g., anionic surfactants such as alkylbenzenesulfonates, alkyl sulfates, alkyl ether sulfates, etc.; cationic surfactants such as monoalkyl quaternary series; nonionic surfactants such as those having ester, ether or amide bonds (e.g., glycol esters); or amphoteric surfactants such as imidazoline derivatives or polypeptides) or a complexing agent (e.g., sodium gluconate, sorbitol, mucic acid or gum arabic).
[0077] Alkaline etchants generally require rinsing with an acid, such as nitric acid or sulfuric acid.
[0078] The surface treatment with the etching solution generally lasts for 1 second to 5 minutes, preferably 3 seconds to 80 seconds, and more preferably 5 seconds to 50 seconds.
[0079] The temperature during this surface treatment is generally 20°C to 100°C, preferably 30°C to 80°C, and more preferably 50°C to 80°C.
[0080] The amount of aluminum in the outer clad layer removed during surface treatment is 1 to 1000 mg / m per side. 2 , preferably 5 to 500 mg / m per side 2 More preferably, it is 5 to 300 mg / m per side. 2 It is.
[0081] The aluminum alloy multi-layer brazing sheet material described herein has a standard thickness in the final gauge ranging from about 0.05 mm to 4 mm, preferably from about 0.2 mm to 2 mm, and more preferably from about 0.2 mm to 1.5 mm.
[0082] In one embodiment, each coating clad layer has a thickness that is about 0.5% to 10%, preferably 0.5% to 5%, of the total thickness of the multi-layer brazing sheet, and each Al-Si brazing clad layer has a thickness that is about 3% to 25%, preferably about 4% to 15%, of the total thickness of the aluminum alloy multi-layer brazing sheet.
[0083] In one embodiment, the coating cladding layer has a thickness in the range of 4 μm to 80 μm, preferably in the range of 5 μm to 50 μm.
[0084] It is important to keep the thickness of the coating clad layer thin compared to the thickness of the Al-Si brazing clad layer. The coating clad layer has a thickness X1, the Al-Si brazing clad layer has a thickness X2, and the thickness ratio of the Al-Si alloy brazing clad layer to the coating clad layer (X2 to X1) is 2 or more to 1. In one embodiment, the thickness ratio is 2.5 or more to 1, preferably X2≧3.X1, for example, the thickness ratio is 2.5 to 1, or 3 to 1, or 3.5 to 1.
[0085] Preferably, the sum of the thickness of the coating clad layer applied to one side of the alloy core layer and the Al-Si brazing clad layer is in the range of about 5% to 25%, preferably 5% to 15%, of the total thickness of the multilayer brazing sheet material.
[0086] In one embodiment, the aluminum alloy multi-layer brazing sheet material is provided in the O temper and is fully annealed.
[0087] In one embodiment, the aluminum alloy multi-layer brazing sheet material is provided in H3x, H2x or H1x tempers, where x is 1, 2, 3, 4, 5, 6, 7 or 8, such as H14, H18, H22, H24 and H26 tempers.
[0088] As a specific example, aluminum alloy multi-layer brazing sheet material is provided in H24, H16 or O tempers.
[0089] Also described herein is the use of the aluminum alloy multi-layer brazing sheet material or product for the manufacture of heat exchangers (e.g., automotive) by flux-free controlled atmosphere brazing (CAB) operations. Thus, the aluminum alloy multi-layer brazing sheet material is suitable for application in heat exchangers such as radiators for powertrain and engine cooling, low temperature radiators, direct air-to-air charge air coolers ("CAC") or intercoolers, air-to-water CACs, water-to-air CACs, air-to-refrigerant CACs, refrigerant-to-air CACs, air-to-refrigerant evaporators, air-to-refrigerant condensers, water-to-refrigerant evaporators, water-to-refrigerant condensers, heater cores, exhaust gas coolers, exhaust gas recirculation systems, hybrid cooling systems, two-phase cooling systems, oil coolers, fuel coolers, materials for battery cooling systems, chillers, cold plates, heat recovery systems, and the like.
[0090] In a further aspect, there is provided herein an article having at least two shaped members, e.g. formed by bending, folding, tube forming or deep drawing, joined together in a flux-free controlled atmosphere brazing (CAB) operation, in particular an automotive heat exchanger incorporating an aluminium alloy multilayer braze material according to the present invention as at least one of the shaped members.
[0091] In another aspect, provided herein is a method for manufacturing an assembly of brazed components, comprising the steps in the following order: providing or forming components, at least one of which is made from an aluminum alloy multi-layer brazing sheet product as described or claimed herein, preferably the multi-layer brazing sheet is treated with an alkaline or acidic etchant; assembling the components to build an assembly, preferably by holding one side of the inventive multi-layer brazing sheet having a covering cladding layer inside the assembly so that the brazing sheet forms a structure, preferably a hollow structure; assembling the components to build an assembly, preferably by holding one side of the inventive multi-layer brazing sheet having a covering cladding layer inside the assembly; brazing the assembly without the application of a brazing flux in an inert gas atmosphere (e.g., argon or nitrogen) at a brazing temperature (usually in the range of about 540°C to 615°C, e.g., about 590°C or about 600°C) for a time sufficient to melt and spread the Al-Si braze (e.g., about 1 to 10 minutes, preferably 1 to 6 minutes, typically around about 2 minutes or 4 minutes residence time) to form a fillet between the assembly and other components of the assembly, wherein the oxygen content of the dry inert gas atmosphere is controlled to the lowest possible level, preferably below 200 ppm, more preferably below 100 ppm, even more preferably below 40 ppm; and cooling the brazed assembly, typically to below 100°C (e.g., ambient temperature).
[0092] Ideally, when assembling components to build an assembly suitable for joining by brazing, one side of the multi-layer brazing sheet product having a thin clad layer as described herein is held inside the assembly to form the brazing sheet into a structure. As long as the brazing sheet product as described herein is used, there is no need to apply brazing flux to obtain a good joint after the brazing operation.
[0093] In a preferred embodiment, the inert brazing gas atmosphere during the brazing operation should be dry, meaning that the dew point is less than minus 40° C., more preferably minus 45° C. or less. EXAMPLES
[0094] 1A and 1B illustrate the arrangement of an aluminum alloy multi-layer brazing sheet product 4 as described herein. The coating clad layer 2 and the Al-Si alloy brazing clad layer 1 can be applied to both sides or only one side of the core layer 3, where the coating clad layer 2 forms the outer layer of the aluminum alloy multi-layer brazing sheet product. When both sides are clad, the multi-layer brazing sheet product has five layers including the alloy core layer, as shown in FIG. 1A. When one side is clad with a brazing material, the multi-layer brazing sheet product has a three-layer configuration, as shown in FIG. 1B.
[0095] FIG. 2 is an isometric view of a portion of a brazed heat exchanger assembly. As shown in FIG. 2, a brazed aluminum heat exchanger 12 according to the present invention may include a plurality of fluid transport tubes 6 made from a multi-layer brazing sheet as described herein. The ends of the fluid transport tubes 6 open into a header plate 8 and a tank 10 (FIG. 2 shows one end of the fluid transport tubes 6, one header plate 8, and one tank 10). Coolant circulates from the tank 10 through the fluid transport tubes 6 into another tank (not shown). As shown, a plurality of cooling fins 5 are positioned between the fluid transport tubes 6 to dissipate heat therefrom, thereby facilitating heat exchange to cool the fluid within the tubes.
[0096] Real-life examples Example 1 is an aluminum alloy multi-layer brazing sheet product for brazing in an inert gas atmosphere without the use of a flux, comprising a core layer made of a 3xxx alloy containing 0.20-0.75 wt% Mg, the core layer having a coating clad layer containing 2-5 wt% Si on one or both sides of the 3xxx alloy core layer, and an Al-Si brazing clad layer containing 7-13 wt% Si located between the 3xxx alloy core layer and the coating clad layer, wherein the coating clad layer has a thickness of X1 and the Al-Si brazing clad layer has a thickness of X2, where X2≧2X1.
[0097] Example 2 is an aluminum alloy multi-layer brazing sheet product as described in any preceding or subsequent example, wherein the 3xxx alloy core layer contains 0.20%-0.60% Mg.
[0098] Example 3 is the aluminum alloy multi-layer brazing sheet product of any one of the preceding or following examples, wherein the 3xxx alloy core layer contains 0.20% to 0.30% Mg.
[0099] Example 4 is the aluminum alloy multi-layer brazing sheet product of any one of the preceding or following examples, wherein the 3xxx alloy core layer contains 0.40%-0.55% Mg.
[0100] Example 5 is the aluminum alloy multi-layer brazing sheet product of any one of the preceding or subsequent examples, wherein the coating cladding layer is Bi-free and Li-free.
[0101] Example 6 is a coating cladding layer that is Mg-free, Bi-free and Li-free, with the following (wt%): Si (2%-5%); Fe (max. 0.5%); Mn (max. 0.2%); Cu (max. 0.1%); Zn (max. 0.4%); Ti (max. 0.1%); 5. The aluminum alloy multi-layer brazing sheet product of any preceding or subsequent example, comprising: incidental impurities (<0.05% each, <0.15% total); and aluminum.
[0102] Example 7 is an aluminum alloy multi-layer brazing sheet product as described in any one of the preceding or following examples, wherein the Si content of the coated cladding layer is 2.5% to 4.0%.
[0103] Example 8 is a 3xxx alloy core layer having (wt%): Mn (0.5%-1.8%); Mg (0.20%-0.75%); Cu (max. 1.1%); Si (max. 0.4%); Fe (max. 0.7%); Cr(max. 0.3%); Sc(max. 0.3%); Zr and / or V (max 0.3%); Ti (max. 0.25%); Zn (max. 1.2%); 5. The aluminum alloy multi-layer brazing sheet product of any preceding or subsequent example, comprising: unavoidable impurities (max 0.05% each, max 0.2% total); and aluminum.
[0104] Example 9 is a 3xxx alloy core layer having (wt%): Mn (0.5%-1.8%); Mg (0.20%-0.75%); Cu (max. 1.1%); Si (max. 0.2%); Fe (max. 0.7%); Cr(max. 0.3%); Sc(max. 0.3%); Zr and / or V (max 0.3%); Ti (max. 0.25%); Zn (max. 1.2%); 5. The aluminum alloy multi-layer brazing sheet product of any preceding or subsequent example, comprising: unavoidable impurities (max 0.05% each, max 0.2% total); and aluminum.
[0105] Example 10 is the aluminum alloy multi-layer brazing sheet product of any one of the preceding or subsequent examples, wherein the 3xxx alloy core layer has a Si content of less than 0.10%.
[0106] Example 11 is the aluminum alloy multi-layer brazing sheet product of any preceding or subsequent example, wherein the Cu content of the 3xxx alloy core layer is up to 0.15%.
[0107] Example 12 is an aluminum alloy multi-layer brazing sheet product as described in any preceding or subsequent example, wherein the Cu content of the 3xxx alloy core layer is in the range of 0.15% to 1.1%.
[0108] Example 13 shows an Al-Si braze cladding layer with (wt%): Si (7%-13%); Mg (max. 0.5%); Fe (max. 0.7%); Cu (max. 0.3%); Mn (max. 0.8%); Zn (max. 2%); Bi (max 0.3%); Ti (max. 0.25%); 5. The aluminum alloy multi-layer brazing sheet product of any preceding or subsequent example, comprising: incidental impurities (<0.05% each, <0.2% total); and aluminum.
[0109] Example 14 is the aluminum alloy multi-layer brazing sheet product of any preceding or subsequent example, wherein the Al-Si brazing cladding layer contains 10% to 13% Si.
[0110] Example 15 is the aluminum alloy multi-layer brazing sheet product of any one of the preceding or following examples, wherein the Al-Si brazing cladding layer comprises 0.02% to 0.5% Mg.
[0111] Example 16 is the aluminum alloy multi-layer brazing sheet product of any one of the preceding or subsequent examples, wherein the aluminum alloy multi-layer brazing sheet product is surface treated with an alkaline or acidic etching solution prior to the brazing process.
[0112] Example 17 is the aluminum alloy multi-layer brazing sheet product of any one of the preceding or subsequent examples, wherein the coating clad layer has a thickness of X1 and the Al-Si brazing clad layer has a thickness of X2, where X2≧2.5X1.
[0113] Example 18 is the aluminum alloy multi-layer brazing sheet product of any preceding or subsequent example, wherein X2≧3X1.
[0114] Example 19 is a process for manufacturing a brazed heat exchanger, comprising providing at least one aluminum alloy multi-layer brazing sheet product of any preceding or subsequent example, and brazing by flux-free controlled atmosphere brazing (CAB).
[0115] Example 20 is the process of any one of the preceding examples, wherein the aluminum alloy multi-layer brazing sheet is surface treated with an alkaline or acidic etchant prior to the brazing process.
[0116] Example 21 is the use of an aluminum alloy multi-layer brazing sheet product as described in any one of the preceding or following examples to manufacture a heat exchanger device in a flux-free controlled atmosphere brazing (CAB) operation.
[0117] All patents, publications and abstracts cited above are incorporated herein by reference in their entirety. Various embodiments of the invention have been described in the fulfillment of various objectives of the invention. It should be recognized that these embodiments are merely illustrative of the principles of the invention. Numerous modifications and adaptations thereof will be readily apparent to those skilled in the art without departing from the spirit and scope of the invention as defined in the following claims. Some of the embodiments of the present disclosure are described in [Item 1] to [Item 20] below. [Item 1] An aluminum alloy multi-layer brazing sheet product for brazing in an inert gas atmosphere without the use of flux, comprising: a core layer made of a 3xxx alloy containing 0.20 wt% to 0.75 wt% Mg, the core layer being provided with a cladding layer containing 2 wt% to 5 wt% Si on one or both sides of the 3xxx alloy core layer; An Al-Si brazing clad layer containing 7 wt% to 13 wt% Si located between the 3xxx alloy core layer and the coating clad layer; Here, the covering clad layer is X 1 and the Al-Si brazing cladding layer has a thickness of X 2 has a thickness of X 2 ≧2X 1 The aluminum alloy multi-layer brazing sheet product. [Item 2] 2. The aluminum alloy multi-layer brazing sheet product according to item 1, wherein the 3xxx alloy core layer contains 0.20% to 0.60% Mg. [Item 3] 3. The aluminum alloy multilayer brazing sheet product according to item 1 or 2, wherein the 3xxx alloy core layer contains 0.20% to 0.30% Mg. [Item 4] 3. The aluminum alloy multilayer brazing sheet product according to item 1 or 2, wherein the 3xxx alloy core layer contains 0.40% to 0.55% Mg. [Item 5] 5. The aluminum alloy multilayer brazing sheet product according to any one of items 1 to 4, wherein the coating clad layer is Bi-free and Li-free. [Item 6] The coated clad layer is Mg-free, Bi-free and Li-free, and has the following (wt%): Si (2%-5%); Fe (max. 0.5%); Mn (max. 0.2%); Cu (max. 0.1%); Zn (max. 0.4%); Ti (max. 0.1%); 6. The aluminum alloy multilayer brazing sheet product according to any one of items 1 to 5, comprising inevitable impurities (each <0.05%, total <0.15%), and aluminum. [Item 7] 7. The aluminum alloy multilayer brazing sheet product according to item 6, wherein the Si content of the coating clad layer is 2.5% to 4.0%. [Item 8] The 3xxx alloy core layer comprises (wt%): Mn (0.5%-1.8%); Mg (0.20%-0.75%); Cu (max. 1.1%); Si (max. 0.4%); Fe (max. 0.7%); Cr(max. 0.3%); Sc(max. 0.3%); Zr and / or V (max 0.3%); Ti (max. 0.25%); Zn (max. 1.2%); 8. The aluminum alloy multilayer brazing sheet product according to any one of items 1 to 7, comprising unavoidable impurities (each at a maximum of 0.05%, and a total at a maximum of 0.2%), and aluminum. [Item 9] 9. The aluminum alloy multi-layer brazing sheet product according to item 8, wherein the 3xxx alloy core layer has a Si content of less than 0.10%. [Item 10] 10. The aluminum alloy multilayer brazing sheet product according to item 8 or 9, wherein the Cu content of the 3xxx alloy core layer is max 0.15%. [Item 11] 10. The aluminum alloy multilayer brazing sheet product according to item 8 or 9, wherein the Cu content of the 3xxx alloy core layer is in the range of 0.15% to 1.1%. [Item 12] The Al-Si braze cladding layer comprises (wt%): Si (7%-13%); Mg (max. 0.5%); Fe (max. 0.7%); Cu (max. 0.3%); Mn (max. 0.8%); Zn (max. 2%); Bi (max 0.3%); Ti (max. 0.25%); 12. The aluminum alloy multilayer brazing sheet product according to any one of items 1 to 11, comprising unavoidable impurities (<0.05% each, <0.2% in total), and aluminum. [Item 13] Item 13. The aluminum alloy multilayer brazing sheet product according to item 12, wherein the Al-Si brazing cladding layer contains 10% to 13% Si. [Item 14] 14. The aluminum alloy multilayer brazing sheet product according to item 12 or 13, wherein the Al-Si brazing cladding layer contains 0.02% to 0.5% Mg. [Item 15] 15. The aluminum alloy multilayer brazing sheet product according to any one of items 1 to 14, wherein the aluminum alloy multilayer brazing sheet product is surface-treated with an alkaline or acidic etching solution before a brazing step. [Item 16] The coating clad layer is X 1 and the Al-Si braze cladding layer has a thickness of X 2 has a thickness of X 2 ≧2.5X 1 16. The aluminum alloy multilayer brazing sheet product according to any one of items 1 to 15, [Item 17] X 2≧3X 1 17. The aluminum alloy multilayer brazing sheet product according to item 16, [Item 18] 1. A process for manufacturing a brazed heat exchanger, comprising the steps of: Providing at least one aluminum alloy multilayer brazing sheet product according to any one of items 1 to 17; and b. brazing using flux-free controlled atmosphere brazing (CAB). [Item 19] 19. The process according to item 18, wherein the aluminum alloy multi-layer brazing sheet is surface treated with an alkaline or acid etching solution before the brazing step. [Item 20] 18. Use of the aluminium alloy multilayer brazing sheet product according to any one of items 1 to 17 for manufacturing a heat exchanger device in a flux-free controlled atmosphere brazing (CAB) operation.
Claims
1. An aluminum alloy multi-layer brazing sheet product for brazing in an inert gas atmosphere without the use of flux, comprising: a core layer made of a 3xxx-series aluminum alloy containing 0.20 wt% to 0.75 wt% Mg, the core layer being provided with a clad layer made of an aluminum alloy containing 2 wt% to 5 wt% Si on one or both sides of the 3xxx-series aluminum alloy core layer; an Al-Si brazing clad layer made of an aluminum alloy containing 7 wt % to 13 wt % Si and up to 0.5 wt % Mg, located between the 3xxx-series aluminum alloy core layer and the coating clad layer; Here, the covering clad layer is X 1 and the Al-Si brazing cladding layer has a thickness of X 2 and has a thickness of X 2 ≧2X 1 and The coating clad layer is Mg-free and: The aluminum alloy multi-layer brazing sheet product, wherein an oxide film on the surface of the aluminum alloy multi-layer brazing sheet product has been removed.
2. 2. The aluminum alloy multi-layer brazing sheet product according to claim 1, wherein the 3xxx-series aluminum alloy core layer contains 0.20 wt % to 0.60 wt % Mg.
3. 3. The aluminum alloy multi-layer brazing sheet product according to claim 1, wherein the 3xxx-series aluminum alloy core layer contains 0.20 wt % to 0.30 wt % Mg.
4. 3. The aluminum alloy multi-layer brazing sheet product according to claim 1, wherein the 3xxx-series aluminum alloy core layer contains 0.40 wt % to 0.55 wt % Mg.
5. The aluminum alloy multi-layer brazing sheet product according to any one of claims 1 to 4, wherein the coating clad layer is Bi-free and Li-free.
6. The coated clad layer is Mg-free, Bi-free and Li-free, and has the following properties: Si (2wt% to 5wt%); Fe (maximum 0.5wt%); Mn (maximum 0.2wt%); Cu (maximum 0.1wt%); Zn (maximum 0.4wt%); Ti (maximum 0.1wt%); 6. The aluminum alloy multi-layer brazing sheet product according to claim 1, comprising unavoidable impurities (each <0.05 wt%, total <0.15 wt%), and the balance being aluminum.
7. 7. The aluminum alloy multi-layer brazing sheet product according to claim 6, wherein the Si content of the coating clad layer is 2.5 wt % to 4.0 wt %.
8. The 3xxx-series aluminum alloy core layer comprises: Mn (0.5wt% to 1.8wt%); Mg (0.20wt% to 0.75wt%); Cu (maximum 1.1wt%); Si (maximum 0.4wt%); Fe (maximum 0.7wt%); Cr (maximum 0.3wt%); Sc (maximum 0.3wt%); Zr and / or V (up to 0.3 wt%); Ti (maximum 0.25wt%); Zn (maximum 1.2wt%); 8. The aluminum alloy multi-layer brazing sheet product according to claim 1, comprising unavoidable impurities (max. 0.05 wt % each, max. 0.2 wt % in total), and the balance being aluminum.
9. 9. The aluminum alloy multi-layer brazing sheet product according to claim 8, wherein the 3xxx-series aluminum alloy core layer has a Si content of less than 0.10 wt%.
10. 10. The aluminum alloy multilayer brazing sheet product according to claim 8 or 9, wherein the 3xxx-series aluminum alloy core layer has a Cu content of up to 0.15 wt%.
11. 10. The aluminum alloy multilayer brazing sheet product according to claim 8, wherein the Cu content of the 3xxx-series aluminum alloy core layer is in the range of 0.15 wt % to 1.1 wt %.
12. The Al-Si braze cladding layer comprises: Si (7wt% to 13wt%); Mg (maximum 0.5wt%); Fe (maximum 0.7wt%); Cu (maximum 0.3wt%); Mn (maximum 0.8wt%); Zn (maximum 2wt%); Bi (maximum 0.3wt%); Ti (maximum 0.25wt%); 12. The aluminum alloy multi-layer brazing sheet product according to any one of claims 1 to 11, consisting essentially of unavoidable impurities (<0.05 wt% each, <0.2 wt% in total), and the balance being aluminum.
13. 13. The aluminum alloy multi-layer brazing sheet product of claim 12, wherein the Al-Si brazing cladding layer comprises 10 wt% to 13 wt% Si.
14. 14. The aluminum alloy multi-layer brazing sheet product according to claim 12 or 13, wherein the Al-Si brazing cladding layer comprises 0.02 wt % to 0.5 wt % Mg.
15. The cladding layer is X 1 and the Al-Si brazing cladding layer has a thickness of X 2 and has a thickness of X 2 ≧2.5X 1 The aluminum alloy multi-layer brazing sheet product according to any one of claims 1 to 14.
16. X 2 ≧3X 1 16. The aluminum alloy multi-layer brazing sheet product of claim 15,
17. 1. A process for manufacturing a brazed heat exchanger, comprising the steps of: Providing at least one aluminum alloy multilayer brazing sheet product according to any one of claims 1 to 16; brazing by flux-free controlled atmosphere brazing (CAB); The manufacturing process.
18. Use of the aluminium alloy multi-layer brazing sheet product according to any one of claims 1 to 16 for manufacturing heat exchange equipment in a flux-free controlled atmosphere brazing (CAB) operation.
Citation Information
Patent Citations
Aluminum alloy brazing sheet
EP1306207A1
Brazed sheet product having clad layer and ferrous alloy coating layer and method for manufacturing same
JP2006509635A
Aluminum brazing sheet
JP2013505135A
Aluminum alloy blazing sheet
JP2018197395A
Multilayer aluminum brazing sheet material
JP2023505586A