Sputtering target material
By controlling crystal orientation and temperature gradients during target material production, the method ensures uniformity and quality of large-diameter KNN films, addressing defects and improving device reliability.
Patent Information
- Application Number
- JP2021203146
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-12-15
- Publication Date
- 2024-09-27
- Estimated Expiration
- 2041-04-20
AI Technical Summary
Existing methods for producing large-diameter KNN films on substrates suffer from localized defective regions due to non-uniform crystal orientation and temperature gradients, leading to variations in film quality.
The method involves controlling the crystal orientation and temperature gradient during the production of the target material by creating a specific temperature profile during firing, ensuring random crystal orientation and uniformity across the sputtering surface, thereby preventing abnormal discharge and local defects.
This approach results in a large-diameter KNN film with uniform film quality and consistent characteristics, enhancing the yield and reliability of piezoelectric devices by eliminating local defective areas.
Smart Images

Figure 0007557454000005 
Figure 0007557454000006 
Figure 0007557454000004
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a piezoelectric laminate, a method for manufacturing a piezoelectric laminate, a sputtering target material, and a method for manufacturing a sputtering target material. [Background technology]
[0002] Piezoelectric bodies are widely used in functional electronic components such as sensors, actuators, etc. As the piezoelectric body, a piezoelectric body containing potassium, sodium, niobium, and oxygen has been proposed, and a laminate (hereinafter, piezoelectric laminate) having a piezoelectric film (KNN film) formed by a sputtering method using such a piezoelectric body has been proposed (see, for example, Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2011-146623 A Summary of the Invention [Problem to be solved by the invention]
[0004] Patent Document 1 discloses that the half-width of the X-ray rocking curve of the (001) plane when X-ray diffraction measurement is performed on the KNN film is set within a range of 0.5° to 2.5° by controlling the magnetic field strength of the surface exposed to the plasma of the target material used when depositing a KNN film on a substrate by sputtering and the crystal orientation of the film that serves as the base of the KNN film. Patent Document 1 also discloses that the KNN film is deposited by sputtering while the substrate is rotated and revolved in order to improve the in-plane uniformity of the film quality of the KNN film.
[0005] However, in the technology described in Patent Document 1, it was found that when a KNN film is formed on a large-diameter substrate having a diameter of 3 inches or more by a sputtering method using a large-diameter target material having a diameter of 3 inches or more, as used in mass production, a region (defective region) in which the half-width falls outside the above range appears locally on the main surface of the KNN film. In other words, it was found that in the technology described in Patent Document 1, a region in which the film quality (film characteristics) is locally deteriorated appears on the main surface of the KNN film. This is a new problem that was first identified through the intensive research of the inventors and others.
[0006] The present disclosure aims to provide a piezoelectric laminate having a large-diameter piezoelectric film with uniform film quality and no localized defective areas over the entire area of its main surface except for the peripheral edge, and to provide related techniques thereof. [Means for solving the problem]
[0007] According to one aspect of the present disclosure, A substrate having a major surface with a diameter of 3 inches or more; a piezoelectric film formed on the substrate, the piezoelectric film containing potassium, sodium, niobium, and oxygen and made of an alkali niobium oxide having a perovskite structure; The present invention provides a piezoelectric laminate and related technologies, in which the half-width of the X-ray rocking curve for the (001) plane, when subjected to X-ray diffraction measurement of the piezoelectric film, is within a range of 0.5° to 2.5° over the entire inner area excluding the peripheral portion of the main surface of the piezoelectric film. Effect of the Invention
[0008] According to the present disclosure, it is possible to obtain a piezoelectric laminate having a large-diameter piezoelectric film with uniform film quality, without any localized defective regions appearing over the entire area of the main surface except for the peripheral edge portion. [Brief description of the drawings]
[0009] [Figure 1] FIG. 2 is a diagram showing an example of a cross-sectional structure of a piezoelectric laminate according to an embodiment of the present disclosure. [Diagram 2]1A and 1B are diagrams illustrating modified examples of the cross-sectional structure of the piezoelectric laminate according to an embodiment of the present disclosure. [Diagram 3] FIG. 2 is a plan view of the principal surface of the piezoelectric film showing measurement points of X-ray diffraction. [Figure 4] 1 is a diagram illustrating an example of a schematic configuration of a piezoelectric device module according to an embodiment of the present disclosure. [Diagram 5] FIG. 1 is a diagram showing an example of a schematic configuration of a sputtering target material according to one embodiment of the present disclosure. [Figure 6] FIG. 2 is a schematic diagram of a molding device used when producing a sputtering target material, and a graph showing the temperature distribution in a processing chamber. [Figure 7] 11A and 11B are diagrams illustrating a modified example of the cross-sectional structure of the piezoelectric device module according to an embodiment of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] <Knowledge gained by the inventors> It is known that the quality of the KNN film formed on a substrate by the sputtering method is strongly affected by the strength of the electromagnetic field on the surface of the target material used in the sputtering film formation that is exposed to plasma (hereinafter also referred to as the "sputtering surface") and the crystal orientation (crystal orientation) of the film (underlying film) that is the underlayer of the KNN film. In order to improve the in-plane uniformity of the quality of the KNN film, the KNN film is sputtered while the substrate is rotated and revolved. However, even if the strength of the electromagnetic field on the sputtering surface and the crystal orientation of the underlayer are adjusted (controlled) or the sputtering film is formed while the substrate is rotated and revolved, when the KNN film is formed on a large substrate with a diameter of 3 inches or more using a target material with a sputtering surface with a diameter of 3 inches or more, as used in mass production, the inventors have discovered a new problem that a defective region, whose film quality is locally inferior to the surroundings, inevitably appears on the main surface of the KNN film. The defective region here refers to a localized region in which, for example, when X-ray diffraction measurement is performed on a KNN film, the full width at half maximum (FWHM(001)) of the X-ray rocking curve for the (001) plane does not fall within the range of 0.5° to 2.5°.
[0011] The inventors have conducted extensive research into the above problem. As a result, they have found that in a target material having a large diameter sputtering surface, there are areas in the sputtering surface where the crystal orientation is not random, and that abnormal discharge occurs in such areas during sputtering deposition, which causes the above-mentioned defective areas to appear in the main surface of the KNN film deposited on the substrate. The "area where the crystal orientation is not random" can also be called an area where the crystal orientation is reduced, and specifically, when X-ray diffraction measurement is performed on the sputtering surface, it refers to an area where the ratio R of the X-ray diffraction peak intensity from the (110) plane to the X-ray diffraction peak intensity from the (001) plane is not within the range of 0.3 to 5.
[0012] The inventors have conducted intensive research into the mechanism by which "regions in which the crystal orientation is not random" appear locally on the sputtering surface of a target material. The KNN target material can be produced by, for example, compressing and molding a mixture of a powder made of a potassium (K) compound, a powder made of a sodium (Na) compound, and a powder made of a niobium (Nb) compound in a predetermined ratio to produce a molded body, and then firing the obtained molded body. However, when firing the molded body, even if an attempt is made to adjust the temperature so that the temperature within the surface of the molded body (within the surface that will become the sputtering surface) is uniform, it is difficult to make the temperature within the surface of the molded body completely uniform. In particular, when producing a target material having a sputtering surface with a diameter of 3 inches or more, it is practically very difficult to make the temperature within the surface of the molded body completely uniform. If there is a temperature gradient (temperature unevenness) exceeding a certain critical value in the surface of the molded body during sintering, that is, if the temperature in the surface of the molded body is not completely uniform, in the region where the temperature gradient is large, crystals (crystal grains) tend to grow along the temperature gradient in the creeping direction on the surface of the molded body, compared to the region where the temperature gradient is small. As a result, when the surface (sputter surface) of the molded body after sintering is viewed from above in the vertical direction, a region where crystals (e.g., crystal grains with a diameter of more than 30 μm) that have grown large in the creeping direction are locally present will appear, and in that region, the orientation of the crystals will not be random (the exposed surface of the large grown crystals will be greatly influenced) compared to other regions (regions where many crystals with a diameter of less than 30 μm are gathered). In this way, the non-orientation of the crystals on the sputter surface of the target material will be locally reduced.
[0013] The inventors have conducted extensive research into a method for avoiding the phenomenon of localized deterioration of the non-orientation of crystals on the sputtering surface of a target material. As a result, they have discovered that by intentionally creating a temperature gradient in the thickness direction of a molded body when firing the molded body, it is possible to suppress crystal growth in the creeping direction on the surface of the molded body even if there are temperature unevenness within the surface of the molded body, and thus it is possible to avoid localized deterioration of the non-orientation of crystals on the sputtering surface.
[0014] The present disclosure has been made based on the above-mentioned findings and problems obtained by the inventors.
[0015] <One aspect of the present disclosure> Hereinafter, one embodiment of the present disclosure will be described with reference to the drawings.
[0016] (1) Structure of the piezoelectric laminate 1, a laminate 10 having a piezoelectric film according to this embodiment (hereinafter also referred to as piezoelectric laminate 10) includes a substrate 1, a lower electrode film 2 provided on the substrate 1, a piezoelectric film (piezoelectric thin film) 3 provided on the lower electrode film 2, and an upper electrode film 4 provided on the piezoelectric film 3. Note that in this embodiment, an example will be described in which one laminate structure (a structure formed by laminating at least the lower electrode film 2, the piezoelectric film 3, and the upper electrode film 4) is provided on one substrate 1.
[0017] The substrate 1 has a main surface with a diameter of 3 inches or more. The substrate 1 has a circular outer shape in a plan view. The outer shape of the substrate 1 (the planar shape of the main surface of the substrate 1) can be various shapes such as a circle, an ellipse, a rectangle, or a polygon. In this case, the substrate 1 preferably has a main surface with an inscribed circle having a diameter of 3 inches or more. As the substrate 1, a single crystal silicon (Si) substrate 1a on which a surface oxide film (SiO2 film) 1b such as a thermal oxide film or a CVD (Chemical Vapor Deposition) oxide film is formed, that is, a Si substrate having a surface oxide film, can be suitably used. As the substrate 1, as shown in FIG. 2, a Si substrate 1a having an insulating film 1d formed on its surface from an insulating material other than SiO2 can also be used. As the substrate 1, a Si substrate 1a on which a Si(100) surface or a Si(111) surface is exposed on the surface, that is, a Si substrate without a surface oxide film 1b or an insulating film 1d can also be used. Also, a metal substrate made of a metal material such as an SOI (Silicon On Insulator) substrate, a quartz glass (SiO2) substrate, a gallium arsenide (GaAs) substrate, a sapphire (Al2O3) substrate, stainless steel (SUS), etc. may be used as the substrate 1. The thickness of the single crystal Si substrate 1a may be, for example, 300 μm or more and 1000 μm or less, and the thickness of the surface oxide film 1b may be, for example, 1 nm or more and 4000 nm or less.
[0018] The lower electrode film 2 can be formed using, for example, platinum (Pt). The lower electrode film 2 is a polycrystalline film. Hereinafter, a polycrystalline film formed using Pt is also referred to as a Pt film. It is preferable that the (111) plane of the Pt film is parallel to the main surface of the substrate 1 (including the case where the (111) plane is inclined at an angle of ±5° or less with respect to the main surface of the substrate 1), that is, the Pt film is oriented in the (111) plane direction. The Pt film being oriented in the (111) plane direction means that no peaks other than those due to the (111) plane are observed in the X-ray diffraction pattern obtained by X-ray diffraction (XRD) measurement. Thus, it is preferable that the main surface of the lower electrode film 2 (the surface serving as the base of the piezoelectric film 3) is composed of a Pt (111) plane. The lower electrode film 2 can be formed using a sputtering method, a vapor deposition method, or the like. The lower electrode film 2 can be formed using various metals such as gold (Au), ruthenium (Ru), or iridium (Ir), alloys mainly composed of these metals, or metal oxides such as strontium ruthenate (SrRuO3, abbreviated as SRO) or lanthanum nickelate (LaNiO3, abbreviated as LNO), in addition to Pt. The lower electrode film 2 can be a single layer film formed using the above-mentioned various metals or metal oxides. The lower electrode film 2 may be a laminate of a Pt film and a film made of SRO provided on the Pt film, or a laminate of a Pt film and a film made of LNO provided on the Pt film. Note that, between the substrate 1 and the lower electrode film 2, an adhesion layer 6 mainly composed of, for example, titanium (Ti), tantalum (Ta), titanium oxide (TiO2), nickel (Ni), ruthenium oxide (RuO2), iridium oxide (IrO2), zinc oxide (ZnO), or the like may be provided in order to enhance the adhesion between them. The adhesion layer 6 can be formed by using a method such as sputtering, vapor deposition, etc. The thickness of the lower electrode film 2 (when the lower electrode film 2 is a laminate, the total thickness of each layer) can be, for example, 100 nm to 400 nm, and the thickness of the adhesion layer 6 can be, for example, 1 nm to 200 nm.
[0019] The piezoelectric film 3 is, for example, a film made of an alkali niobium oxide containing potassium (K), sodium (Na), niobium (Nb), and oxygen (O).1-x Na x ) A film can be formed using an alkali niobate oxide represented by NbO3, that is, potassium sodium niobate (KNN). The coefficient x [= Na / (K + Na)] in the above composition formula can be in the range of 0 < x < 1, preferably 0.4 ≦ x ≦ 0.7. The piezoelectric film 3 becomes a polycrystalline film of KNN (hereinafter also referred to as the KNN film 3). The crystal structure of KNN is a perovskite structure. That is, the KNN film 3 has a perovskite structure. Further, it is preferable that more than half of the crystal groups constituting the KNN film 3 have a columnar structure. In this specification, the crystal system of KNN is regarded as a tetragonal system. The KNN film 3 can be formed using a technique such as a sputtering method. The thickness of the KNN film 3 can be, for example, 0.5 μm or more and 5 μm or less.
[0020] The KNN film 3 can contain any one or more elements (dopants) such as lithium (Li), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), bismuth (Bi), antimony (Sb), vanadium (V), indium (In), Ta, molybdenum (Mo), tungsten (W), chromium (Cr), Ti, zirconium (Zr), hafnium (Hf), scandium (Sc), yttrium (Y), lanthanum (La), cerium (Ce), praseodymium (Pr), neodymium (Nd), samarium (Sm), europium (Eu), gadolinium (Gd), terbium (Tb), dysprosium (Dy), holmium (Ho), erbium (Er), thulium (Tm), ytterbium (Yb), lutetium (Lu), copper (Cu), zinc (Zn), silver (Ag), manganese (Mn), iron (Fe), cobalt (Co), Ni, aluminum (Al), Si, germanium (Ge), tin (Sn), gallium (Ga). The concentration of these elements in the KNN film 3 can be, for example, 5 at% or less (when containing a plurality of the above elements, the total concentration is 5 at% or less).
[0021] The crystals constituting the KNN film 3 are preferably preferentially oriented in the (001) plane direction with respect to the main surface of the substrate 1 (Si substrate 1a when the substrate 1 is, for example, a Si substrate 1a having a surface oxide film 1b or an insulating film 1d, etc.). That is, the main surface of the KNN film 3 (the surface serving as the base of the upper electrode film 4) is preferably mainly composed of the KNN (001) plane. For example, by directly depositing the KNN film 3 on a Pt film (lower electrode film 2) whose main surface is mainly composed of a Pt (111) plane, the KNN film 3 whose main surface is mainly composed of a KNN (001) plane can be easily obtained.
[0022] In this specification, the crystals constituting the KNN film 3 are oriented in the (001) plane direction means that the (001) plane of the crystals constituting the KNN film 3 is parallel or approximately parallel to the main surface of the substrate 1. In addition, the crystals constituting the KNN film 3 are preferentially oriented in the (001) plane direction means that there are many crystals whose (001) plane is parallel or approximately parallel to the main surface of the substrate 1. For example, it is preferable that 80% or more of the crystals constituting the KNN film 3 are oriented in the (001) plane direction with respect to the main surface of the substrate 1. That is, the orientation rate of the crystals constituting the KNN film 3 in the (001) plane direction is, for example, preferably 80% or more, and more preferably 90% or more. In addition, the "orientation rate" in this specification is a value calculated by the following (Equation 1) based on the peak intensity of the X-ray diffraction pattern (2θ / θ) obtained by performing XRD measurement on the KNN film 3.
[0023] (Number 1) Orientation rate (%) = {(001) peak intensity / ((001) peak intensity + (110) peak intensity)} × 100
[0024] In addition, the "(001) peak intensity" in the above (Equation 1) is the intensity of a diffraction peak due to a crystal oriented in the (001) plane direction (i.e., a crystal whose (001) plane is parallel to the main surface of the substrate 1) among the crystals constituting the KNN film 3 in the X-ray diffraction pattern obtained by performing XRD measurement on the KNN film 3, and is the intensity of a peak that appears within a range of 2θ of 20° to 23°. In addition, when multiple peaks appear within a range of 2θ of 20° to 23°, it is the intensity of the highest peak. In addition, the "(110) peak intensity" in the above (Equation 1) is the intensity of a diffraction peak due to a crystal oriented in the (110) plane direction (i.e., a crystal whose (110) plane is parallel to the main surface of the substrate 1) among the crystals constituting the KNN film 3 in the X-ray diffraction pattern obtained by performing XRD measurement on the KNN film 3, and is the intensity of a peak that appears within a range of 2θ of 30° to 33°. When multiple peaks appear within the range of 2θ of 30° to 33°, the intensity is that of the highest peak.
[0025] The KNN film 3 has a principal surface (upper surface) with a diameter of 3 inches or more, i.e., a large diameter principal surface. In the KNN film 3, no local defective regions appear in the entire inner area except for the peripheral area in the principal surface of the KNN film 3, and the film quality is uniform. Specifically, when the KNN film 3 is subjected to XRD measurement, the value of the half-width (FWHM(001)) of the X-ray rocking curve of the (001) plane is within the range of 0.5° to 2.5° in the entire inner area except for the peripheral area in the principal surface of the KNN film 3. Here, "the FWHM(001) value is within the range of 0.5° to 2.5° in the entire inner area excluding the peripheral area on the main surface of the KNN film 3" means that, as shown in FIG. 3, the FWHM(001) value is within the range of 0.5° to 2.5° in all points when XRD measurement is performed at 1 cm intervals in a grid pattern on the main surface of the KNN film 3 in the area 3b inside the outer peripheral area 3a 5 mm from the edge (area excluding the outer peripheral area 3a 5 mm from the edge). In FIG. 3, the measurement points of FWHM(001) are indicated by ● marks. In addition, hereinafter, "the entire inner area excluding the peripheral area on the main surface of the KNN film 3" is also referred to as "the entire main surface of the KNN film 3".
[0026] Since the FWHM(001) value is within the range of 0.5° to 2.5° over the entire main surface of the KNN film 3, the film characteristics of the KNN film 3 can be made uniform (in-plane uniform) over the entire main surface of the KNN film 3. This makes it possible to prevent variations in characteristics from occurring among a plurality of piezoelectric elements 20 (piezoelectric device modules 30) (to be described later) obtained from one piezoelectric laminate 10. As a result, the yield and reliability of the piezoelectric elements 20 (piezoelectric device modules 30) can be improved.
[0027] The upper electrode film 4 can be formed using various metals such as Pt, Au, Al, Cu, or alloys thereof. The upper electrode film 4 can be formed using a method such as a sputtering method, a vapor deposition method, a plating method, or a metal paste method. The upper electrode film 4 does not have a large effect on the crystal structure of the KNN film 3, unlike the lower electrode film 2. Therefore, the material, crystal structure, and film formation method of the upper electrode film 4 are not particularly limited. Note that, in order to increase the adhesion between the KNN film 3 and the upper electrode film 4, an adhesion layer mainly composed of, for example, Ti, Ta, TiO2, Ni, RuO2, IrO2, or the like may be provided. The thickness of the upper electrode film 4 can be, for example, 100 nm to 5000 nm, and when an adhesion layer is provided, the thickness of the adhesion layer can be, for example, 1 nm to 200 nm.
[0028] (2) Structure of the piezoelectric device module FIG. 4 shows a schematic diagram of a device module 30 having a KNN film 3 (hereinafter also referred to as a piezoelectric device module 30). By forming the above-mentioned piezoelectric laminate 10 into a predetermined shape, an element (device) 20 (element 20 having a KNN film 3, hereinafter also referred to as a piezoelectric element 20) as shown in FIG. 4 is obtained. The piezoelectric device module 30 includes at least a piezoelectric element 20 and a voltage application means 11a or a voltage detection means 11b connected to the piezoelectric element 20. The voltage application means 11a is a means for applying a voltage between the lower electrode film 2 and the upper electrode film 4, and the voltage detection means 11b is a means for detecting a voltage generated between the lower electrode film 2 and the upper electrode film 4. As the voltage application means 11a and the voltage detection means 11b, various known means can be used.
[0029] By connecting the voltage application means 11a between the lower electrode film 2 and the upper electrode film 4 of the piezoelectric element 20, the piezoelectric device module 30 can function as an actuator. By applying a voltage between the lower electrode film 2 and the upper electrode film 4 by the voltage application means 11a, the KNN film 3 can be deformed. This deformation action can operate various members connected to the piezoelectric device module 30. In this case, examples of applications of the piezoelectric device module 30 include heads for inkjet printers, MEMS mirrors for scanners, and vibrators for ultrasonic generators.
[0030] By connecting the voltage detection means 11b between the lower electrode film 2 and the upper electrode film 4 of the piezoelectric element 20, the piezoelectric device module 30 can function as a sensor. When the KNN film 3 deforms in response to a change in some physical quantity, a voltage is generated between the lower electrode film 2 and the upper electrode film 4 due to the deformation. By detecting this voltage with the voltage detection means 11b, it is possible to measure the magnitude of the physical quantity applied to the KNN film 3. In this case, examples of applications of the piezoelectric device module 30 include an angular velocity sensor, an ultrasonic sensor, a pressure sensor, and an acceleration sensor.
[0031] The piezoelectric device module 30 (piezoelectric element 20) is made from a piezoelectric laminate 10 having a KNN film 3 whose FWHM(001) value is within the range of 0.5° to 2.5° over the entire main surface. This makes it possible to prevent variations in characteristics between multiple piezoelectric elements 20 (piezoelectric device modules 30) obtained from one piezoelectric laminate 10. In other words, multiple piezoelectric elements 20 (piezoelectric device modules 30) with uniform characteristics can be obtained from one piezoelectric laminate 10.
[0032] For example, in a plurality of piezoelectric device modules 30 obtained by processing one piezoelectric laminate 10 in which a Ti layer (thickness: 2 nm) as an adhesion layer 6, a Pt film (thickness: 200 nm) as a lower electrode film 2, a KNN film 3 (thickness: 2 μm), a RuO2 layer (thickness: 30 nm) as an adhesion layer for enhancing adhesion between the KNN film 3 and the upper electrode film 4, and a Pt film (thickness: 100 nm) as the upper electrode film 4 are sequentially provided on a large-diameter substrate 1, when an electric field of −100 kV / cm is applied between the lower electrode film 2 and the upper electrode film 4, the piezoelectric constants -e 31 10C / m 2 For example, when an electric field of −150 kV / cm is applied between the lower electrode film 2 and the upper electrode film 4 in the plurality of piezoelectric device modules 30, the leakage current density of all the piezoelectric device modules 30 can be increased to 1×10 -5 A / cm 2 Here, in this specification, "applying an electric field of -100 kV / cm or -150 kV / cm between the lower electrode film 2 and the upper electrode film 4" means applying a negative voltage to the upper electrode film 4 so that an electric field of 100 kV / cm or 150 kV / cm is generated between the upper electrode film 4 and the lower electrode film 2 in the upward thickness direction of the KNN film 3 (direction from the lower electrode film 2 to the upper electrode film 4) with the upper electrode film 4 side being negative and the lower electrode film 2 side being earthed.
[0033] In this way, the characteristics of the plurality of piezoelectric elements 20 (piezoelectric device modules 30) are made uniform, thereby improving the yield and reliability of the piezoelectric elements 20 (piezoelectric device modules 30).
[0034] (3) Methods for manufacturing piezoelectric laminates, piezoelectric elements, and piezoelectric device modules A method for manufacturing the above-mentioned piezoelectric laminate 10, piezoelectric element 20, and piezoelectric device module 30 will now be described.
[0035] (Deposition of adhesion layer and bottom electrode film) First, a large-diameter substrate 1 with a main surface having a diameter of 3 inches or more is prepared, and an adhesion layer 6 (e.g., a Ti layer) and a lower electrode film 2 (e.g., a Pt film) are formed in this order on one of the main surfaces of the substrate 1 by, for example, a sputtering method. Note that a substrate 1 on which the adhesion layer 6 and the lower electrode film 2 have been formed in advance on one of the main surfaces may be prepared.
[0036] The conditions for providing the adhesive layer 6 are exemplified as follows. Temperature (substrate temperature): 100°C or higher and 500°C or lower, preferably 200°C or higher and 400°C or lower Discharge power: 1000W or more and 1500W or less, preferably 1100W or more and 1300W or less Atmosphere: Argon (Ar) gas atmosphere Ambient pressure: 0.1 Pa or more and 0.5 Pa or less, preferably 0.2 Pa or more and 0.4 Pa or less Time: 30 seconds to 3 minutes, preferably 45 seconds to 2 minutes
[0037] The conditions for forming the lower electrode film 2 are exemplified as follows. Temperature (substrate temperature): 100°C or higher and 500°C or lower, preferably 200°C or higher and 400°C or lower Discharge power: 1000W or more and 1500W or less, preferably 1100W or more and 1300W or less Atmosphere: Ar gas atmosphere Ambient pressure: 0.1 Pa or more and 0.5 Pa or less, preferably 0.2 Pa or more and 0.4 Pa or less Time: 3 minutes or more and 10 minutes or less, preferably 4 minutes or more and 8 minutes or less, more preferably 5 minutes or more and 6 minutes below
[0038] (KNN membrane production) After the deposition of the adhesion layer 6 and the lower electrode film 2 is completed, the KNN film 3 is deposited on the lower electrode film 2 by a sputtering method such as RF magnetron sputtering. At this time, a target material 100, which will be described later, is used, which contains K, Na, Nb, and O and is made of a sintered body of an alkali niobium oxide having a perovskite structure. The target material 100 has a sputtering surface 101 having a diameter of 3 inches or more and having random crystal orientations over the entire inner area except for the periphery. The target material 100 will be described in detail later. The composition ratio of the KNN film 3 can be adjusted, for example, by controlling the composition of the target material 100.
[0039] The following conditions are exemplified as conditions for forming the KNN film 3. The film formation time can be appropriately set depending on the thickness of the KNN film 3. Discharge power: 2000W or more and 2400W or less, preferably 2100W or more and 2300W or less Atmosphere: Ar gas + oxygen (O2) gas mixture Ambient pressure: 0.2 Pa or more and 0.5 Pa or less, preferably 0.2 Pa or more and 0.4 Pa or less Partial pressure of Ar gas relative to O gas (Ar / O partial pressure ratio): 30 / 1 to 20 / 1, preferably 27 / 1 to 22 / 1 Film-forming temperature: 500°C or higher and 700°C or lower, preferably 550°C or higher and 650°C or lower Film-forming speed: 0.5 μm / hr or more and 2 μm / hr or less, preferably 0.5 μm / hr or more and 1.5 μm / hr or less
[0040] By using a target material 100 described later having a sputtering surface 101 with random crystal orientation over the entire inner area except for the periphery, and depositing the KNN film 3 under the above-mentioned conditions, it is possible to prevent abnormal discharge from occurring over the entire sputtering surface during sputtering deposition. This makes it possible to prevent localized defective regions from appearing on the main surface of the KNN film 3 even when depositing a large-diameter KNN film 3 on a large-diameter substrate 1 (on a large-diameter lower electrode film 2 deposited on a large-diameter substrate 1). In other words, it is possible to obtain a large-diameter KNN film 3 having uniform film quality over the entire main surface. Specifically, it is possible to obtain a large-diameter KNN film 3 whose FWHM(001) value is within the range of 0.5° to 2.5° over the entire main surface.
[0041] (Deposition of upper electrode film) After the deposition of the KNN film 3 is completed, the upper electrode film 4 is deposited on the KNN film 3 by, for example, a sputtering method. The conditions for depositing the upper electrode film 4 can be the same as those for depositing the above-mentioned lower electrode film 2. This results in a piezoelectric stack 10 as shown in FIG.
[0042] (Fabrication of piezoelectric elements and piezoelectric device modules) The obtained piezoelectric laminate 10 is then shaped into a predetermined shape by etching or the like (micromachining is performed into a predetermined pattern). This results in a piezoelectric element 20 as shown in Fig. 4, and a piezoelectric device module 30 is obtained by connecting a voltage application means 11a or a voltage detection means 11b to the piezoelectric element 20. As an etching method, for example, a dry etching method such as reactive ion etching, or a wet etching method using a predetermined etching solution can be used.
[0043] When the piezoelectric stack 10 is formed by dry etching, a photoresist pattern serving as an etching mask for dry etching is formed on the piezoelectric stack 10 (for example, the upper electrode film 4) by a photolithography process or the like. As the etching mask, a precious metal film (metal mask) such as a Cr film, Ni film, Pt film, or Ti film may be formed by a sputtering method. Then, dry etching is performed on the piezoelectric stack 10 (the upper electrode film 4, the KNN film 3, etc.) using a gas containing a halogen element as an etching gas. The halogen element includes chlorine (Cl), fluorine (F), etc. As the gas containing a halogen element, BCl3 gas, SiCl4 gas, Cl2 gas, CF4 gas, C4F8 gas, etc. can be used.
[0044] When forming the piezoelectric laminate 10 by wet etching, a silicon oxide (SiO x ) film, etc. Then, the piezoelectric stack 10 is immersed in an etching solution that contains an alkaline aqueous solution of a chelating agent and does not contain hydrofluoric acid, for example, to perform wet etching on the piezoelectric stack 10 (upper electrode film 4, KNN film 3, etc.). Note that as the etching solution that contains an alkaline aqueous solution of a chelating agent and does not contain hydrofluoric acid, an etching solution that is a mixture of ethylenediaminetetraacetic acid as a chelating agent, ammonia water, and hydrogen peroxide water can be used.
[0045] (4) Target material composition The configuration of the sputtering target material 100 used in sputtering the KNN film 3 will be described in detail below with reference to Fig. 5. The target material 100 is fixed to a backing plate via an adhesive such as In, and then mounted in a sputtering device so that the sputtering surface 101 is irradiated with plasma. As described above, the "sputtering surface" refers to the surface of the target material 100 that is exposed to plasma during sputtering (the surface that ions collide with during sputtering).
[0046] FIG. 5 is a schematic configuration diagram showing an example of the target material 100 according to this aspect. In FIG. 5, the target material 100 is illustrated with the sputtering surface 101 facing upward.
[0047] The target material 100 contains K, Na, Nb, and O, and is composed of a sintered body of an alkali niobate oxide having a perovskite structure, that is, a KNN sintered body. The target material 100 has a composition within the range of 0 < Na / (K + Na) < 1, preferably 0.4 ≦ Na / (K + Na) ≦ 0.7. The target material 100 is composed of a plurality of KNN crystal grains.
[0048] The target material 100 may contain, as a dopant, any one or more elements of Li, Mg, Ca, Sr, Ba, Bi, Sb, V, In, Ta, Mo, W, Cr, Ti, Zr, Hf, Sc, Y, La, Ce, Pr, Nd, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu, Cu, Zn, Ag, Mn, Fe, Co, Ni, Al, Si, Ge, Sn, Ga. The concentration of the above elements in the target material 100 can be, for example, 5 at% or less (when containing a plurality of kinds of elements, the total concentration is 5 at% or less).
[0049] The target material 100 has a circular outer shape. That is, the target material 100 has a circular sputtering surface 101 in plan view. The diameter of the sputtering surface 101 can be, for example, 3 inches or more. Note that the outer shape of the target material 100 (the planar shape of the sputtering surface 101) can be various shapes such as an ellipse, a rectangle, or a polygon in addition to a circle. In this case, the diameter of the inscribed circle of the sputtering surface 101 can be, for example, 3 inches or more. Thus, the target material 100 has a sputtering surface 101 with a diameter of 3 inches or more, that is, a large-diameter sputtering surface 101.
[0050] The target material 100 is configured so that, when an XRD measurement is performed on the sputtering surface 101, the ratio R of the (110) peak intensity to the (001) peak intensity (=(110) peak intensity / (001) peak intensity) is within the range of 0.3 to 5, preferably 1.2 to 5, and more preferably 1.2 to 3, throughout the entire inner area of the sputtering surface 101 excluding the peripheral portion.
[0051] The "(001) peak intensity" here refers to the X-ray diffraction peak intensity from the (001) plane when the sputtering surface 101 is subjected to XRD measurement, that is, in the X-ray diffraction pattern obtained by performing XRD measurement on the sputtering surface 101, the intensity of a diffraction peak due to crystals oriented in the (001) plane orientation among the crystals constituting the target material 100, and the intensity of a peak that appears within a 2θ range of 20° to 23°. In addition, when multiple peaks appear within a 2θ range of 20° to 23°, the intensity of the highest peak is used. The "(110) peak intensity" here refers to the X-ray diffraction peak intensity from the (110) plane when the sputtering surface 101 is subjected to XRD measurement, that is, in the X-ray diffraction pattern obtained by performing XRD measurement on the sputtering surface 101, the intensity of a diffraction peak due to crystals oriented in the (110) plane orientation among the crystals constituting the target material 100, and the intensity of a peak that appears within a 2θ range of 30° to 33°. When multiple peaks appear within the range of 2θ of 30° to 33°, the intensity is that of the highest peak.
[0052] Furthermore, "the ratio R is within the range of 0.3 to 5 in the entire inner area of sputtering surface 101 excluding the peripheral portion" means that the value of ratio R is 0.3 to 5 in all points (37 points in the case of a sputtering surface 101 with a diameter of 3 inches) when XRD measurement is performed in a grid pattern at 1 cm intervals on the area of sputtering surface 101 excluding the area 5 mm from the edge (periphery) (area inside the area 5 mm from the edge). Hereinafter, "the entire inner area of sputtering surface 101 excluding the peripheral portion" will also be referred to as "the entire sputtering surface".
[0053] Thus, in the target material 100, even in the large-diameter sputtering surface 101, there are no regions where the crystal orientation is not locally random, i.e., there are no regions where the crystal orientation is locally reduced, and the crystal orientation is random over the entire sputtering surface. Preferably, in the target material 100, no regions where crystal grains with a grain size exceeding 30 μm are locally concentrated are observed over the entire sputtering surface and the entire surface parallel to the sputtering surface 101 except for the peripheral portion (hereinafter also referred to as "the entire surface parallel to the sputtering surface 101"). More preferably, in the target material 100, no crystal grains with a grain size exceeding 30 μm are observed over the entire sputtering surface and the entire surface parallel to the sputtering surface 101. That is, the target material 100 is composed of crystal grains having a grain size of, for example, 0.1 μm or more and 30 μm or less, preferably 0.1 μm or more and 20 μm or less, and more preferably 0.1 μm or more and 10 μm or less, over the entire sputtering surface and the entire surface parallel to the sputtering surface 101.
[0054] By sputtering the KNN film 3 on the substrate 1 having a diameter of 3 inches or more using such a target material 100, it is possible to prevent abnormal discharge from occurring over the entire sputtering surface during sputtering. As a result, it is possible to obtain a large-diameter KNN film 3 whose FWHM(001) value is within the range of 0.5° to 2.5° over the entire main surface.
[0055] The relative density of the target material 100 is 60% or more, preferably 70% or more, and more preferably 80% or more, over the entire sputtering surface. The relative density (%) here is a value calculated by (actual density / KNN theoretical density)×100. The KNN theoretical density is 4.51 g / cm 3The flexural strength of the target material 100 is 10 MPa or more, preferably 30 MPa or more, more preferably 40 MPa or more, and even more preferably 50 MPa or more, over the entire sputtering surface. The flexural strength here is a value measured by a three-point bending test (based on JIS R1601:2008). In this way, by having a relative density of 60% or more over the entire sputtering surface and a flexural strength of 10 MPa or more, it is possible to reliably avoid abnormal discharge occurring over the entire sputtering surface during sputtering film formation using the target material 100.
[0056] In addition, it is preferable that the target material 100 has a high resistance. For example, it is preferable that the volume resistivity of the target material 100 is 1000 kΩcm or more. This makes it possible to obtain a KNN film 3 having good insulating properties. The upper limit of the volume resistivity is not particularly limited, but can be, for example, 100 MΩcm or less.
[0057] (5) Manufacturing method of target material Hereinafter, a method for manufacturing a target material 100 in which the ratio R falls within the range of 0.3 to 5 over the entire sputtering surface will be described in detail with reference to FIG.
[0058] In the production sequence of the target material 100 in this embodiment, A process (mixing process) of mixing a powder of a K compound, a powder of a Na compound, and a powder of a Nb compound in a predetermined ratio to obtain a mixture; A process in which a specific pressure (load) is applied to the mixture to form it into a molded body with a diameter of 3 inches or more (compression molding process); A process (sintering process) of heating and sintering the molded body for 1 hour to 5 hours under conditions in which the temperature within the surface of the molded body is 800°C or more and 1150°C or less over the entire surface and has a temperature gradient that increases at a rate of 10°C / mm or more in the direction from the front to the back surface, to obtain a sintered body; In this embodiment, the case where the compression molding process and the firing process are carried out simultaneously (all at once) will be described.
[0059] In addition, after the mixing process and before the compression molding process, A process of pre-firing the mixture at a temperature lower than the heating temperature in the firing process (pre-firing process); A process of crushing the mixture after the calcination (crushing process); In this case, in the compression molding process, a predetermined pressure is applied to the mixture that has been pulverized after the preliminary firing.
[0060] After the firing treatment, the sintered body may be further subjected to a treatment of heating at a predetermined temperature (heat treatment).
[0061] (Mixing process) A powder made of a K compound, a powder made of a Na compound, and a powder made of a Nb compound are mixed in a predetermined ratio to obtain a mixture.
[0062] Specifically, first, a powder made of a K compound, a powder made of a Na compound, and a powder made of a Nb compound are prepared.
[0063] The K compound is at least one selected from the group consisting of K oxides, K composite oxides, and K compounds that become oxides when heated (e.g., carbonates, oxalates). As the powder consisting of a K compound, for example, potassium carbonate (K2CO3) powder can be used.
[0064] The Na compound is at least one selected from the group consisting of Na oxides, Na composite oxides, and Na compounds that become oxides by heating (e.g., carbonates, oxalates). As the powder consisting of a Na compound, for example, sodium carbonate (Na2CO3) powder can be used.
[0065] The Nb compound is at least one selected from the group consisting of an oxide of Nb, a composite oxide of Nb, and a compound of Nb that becomes an oxide by heating. As the powder consisting of a Nb compound, for example, niobium oxide (Nb2O5) powder can be used.
[0066] In addition, when preparing a target material 100 containing a predetermined dopant, a powder made of a compound of one or more elements selected from the group consisting of Li, Mg, Ca, Sr, Ba, Bi, Sb, V, In, Ta, Mo, W, Cr, Ti, Zr, Hf, Sc, Y, La, Ce, Pr, Nd, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu, Cu, Zn, Ag, Mn, Fe, Co, Ni, Al, Si, Ge, Sn, and Ga is prepared. The powder of the compound of each of the above elements is at least one selected from the group consisting of an oxide powder of each of the above elements, a composite oxide powder of each of the above elements, and a compound (e.g., carbonate, oxalate) of each of the above elements that becomes an oxide by heating.
[0067] Then, the mixing ratio of each of the powders is adjusted and each powder is weighed so that the composition of the target material 100 becomes a predetermined composition. The weighing may be performed in the air, but is preferably performed in an inert gas atmosphere such as Ar gas or nitrogen (N2) gas in order to avoid deviation in the composition ratio of the target material 100. In addition, in order to reliably avoid deviation in the composition ratio of the target material 100, it is preferable to weigh each powder after sufficiently drying (dehydrating).
[0068] Next, the powders are mixed (wet mixed) using a mixer such as a ball mill, a bead mill, etc. The mixing conditions are exemplified as follows. Solvent: organic solvent such as ethanol or water Mixing time: 5 hours or more and 30 hours or less, preferably 10 hours or more and 26 hours or less Mixed atmosphere: Air
[0069] By mixing under the above conditions, it is possible to prevent the powder from agglomerating, and as a result, it is possible to make the composition of the target material 100 uniform over the entire sputtering surface and over the entire surface parallel to the sputtering surface 101.
[0070] (Pre-calcination and crushing process) After the mixing process is completed, the mixture obtained by the mixing process is pre-calcined by heating at a temperature lower than the heating temperature in the calcination process described below (pre-calcination process).
[0071] The conditions for carrying out the calcination are exemplified as follows. Heating temperature: 650° C. or higher and 1100° C. or lower, preferably 700° C. or higher and 900° C. or lower, more preferably 700° C. or higher and lower than 800° C., and lower than the heating temperature in the firing treatment described below. Heating time: 1 hour or more and 50 hours or less, preferably 5 hours or more and 40 hours or less, more preferably 10 hours or more and 35 hours or less
[0072] After the preliminary firing process is completed, the mixture after the preliminary firing is mixed while being pulverized using a ball mill or the like (pulverization process).
[0073] The conditions for pulverization are exemplified as follows. Grinding (mixing) time: 3 hours or more and 10 hours or less, preferably 5 hours or more and 9 hours or less The other conditions can be the same as those in the above-mentioned mixing process.
[0074] (Compression molding process / firing process) After the preliminary firing and crushing processes are completed, the mixture obtained by crushing and mixing after the preliminary firing is subjected to a predetermined pressure to be molded (compression molding) to obtain a molded body (compression molding process), and the molded body is heated and fired under predetermined conditions to obtain a sintered body (firing process) are simultaneously performed using a molding device 200 shown in Fig. 6. In other words, hot press sintering is performed in which firing is performed while compression molding is performed.
[0075] The molding device 200 shown in FIG. 6 is made of SUS or the like, and includes a chamber 203 with a processing chamber 201 formed therein. A jig (mold) 208 in which a mixture 210 is filled (stored) is provided in the processing chamber 201. The jig 208 is made of a material such as graphite, and is configured to be capable of forming a molded body (sintered body) with a diameter of 3 inches or more. A pressing means 217 (e.g., a hydraulic press pressing means 217) configured to be capable of applying a predetermined pressure to the mixture 210 filled in the jig 208 is provided in the processing chamber 201. A heater 207 is provided in the processing chamber 201 to heat the mixture 210 in the jig 208 to a desired temperature. The heater 207 is configured such that an upper heater 207a, a central heater 207b, and a lower heater 207c are arranged in order from the top to the bottom of the processing chamber 201, and an inner heater 207d for heating an inner zone of the jig 208 and an outer heater 207e for heating an outer zone of the jig 208 are arranged in order. Each of the upper heater 207a, the central heater 207b, and the lower heater 207c has a cylindrical shape, and each of the inner heater 207d and the outer heater 207e has a doughnut shape, and is configured so that the temperature can be controlled individually. In addition, a temperature sensor 209 for measuring the temperature inside the processing chamber 201 is provided inside the processing chamber 201. Each member of the molding device 200 is connected to a controller 280 configured as a computer, and is configured so that the procedures and conditions described below are controlled by a program executed on the controller 280.
[0076] The compression molding process and the firing process can be carried out using the above-mentioned molding apparatus 200, for example, in the following procedure.
[0077] First, mixture 210 obtained by crushing and mixing after calcination is filled into jig 208. Then, a predetermined pressure is applied to mixture 210 in jig 208 by pressing means 217 in a direction perpendicular to the pressing surface as shown by the outlined arrow in FIG. 6 to form a molded body.
[0078] Examples of conditions for carrying out the compression molding include the following conditions. Applied pressure (load): 100kgf / cm 2 More than 500kgf / cm 2 below Pressurization time: 1 hour or more and 5 hours or less, preferably 2 hours or more and 4 hours or less Atmosphere: inert gas atmosphere or vacuum atmosphere
[0079] The load during compression molding is 100kgf / cm 2 More than 500kgf / cm 2 By setting the load at or below 100 kgf / cm, it is possible to obtain a target material 100 having a predetermined mechanical strength while avoiding damage to the jig 208. 2 If the compression pressure is less than 500 kgf / cm, the compression may be insufficient, resulting in a sintered body with low mechanical strength. If the mechanical strength is low, cracks may easily occur during the production of the target material 100, which may result in a decrease in yield. Furthermore, when a target material 100 made of such a sintered body is used, cracks may occur in the target material 100 even during the formation of the KNN film 3, which may result in localized deterioration in the physical properties of the KNN film 3, such as the crystal quality and film thickness. Furthermore, if the load is less than 500 kgf / cm, the compression pressure may be insufficient, resulting in a decrease in the mechanical strength of the sintered body. If ... 2 If the load exceeds this value, the jig 208 is likely to be damaged.
[0080] While the compression molding process is being carried out under the above-mentioned conditions, the molded body is heated and fired under predetermined conditions.
[0081] The firing process is performed by heating the molded body (mixture 210) for 1 hour to 5 hours under the conditions that the temperature (firing temperature) in the surface of the molded body (mixture 210 in jig 208) is 800°C or more and 1150°C or less over the entire surface, and the temperature gradient increases at 10°C / mm or more in the direction from the surface to the back of the molded body. At this time, the molded body (mixture 210) is heated while controlling the temperatures of heaters 207a to 207c based on the temperature detected by temperature sensor 209 so that the temperature in the processing chamber 201 (molded body, mixture 210) has a desired temperature distribution (for example, so that the temperature distribution in the processing chamber 201 is a distribution as shown in the graph of FIG. 6), and while controlling the temperatures of heaters 207d and 207e based on the temperature detected by temperature sensor 209 so that the temperature in the surface of the molded body becomes uniform. In this specification, the front surface of the molded body is the surface of the target material 100 that will become the sputtering surface 101, and the back surface of the molded body is the surface opposite to the front surface of the molded body.
[0082] The firing conditions are exemplified as follows. Firing temperature: 800°C or higher and 1150°C or lower, preferably 900°C or higher and 1150°C or lower, more preferably 1000°C or higher and 1150°C or lower Temperature gradient: A gradient that rises at 10° C. / mm or more in the direction from the front surface to the back surface of the molded body, preferably 10° C. / mm or more and 15° C. / mm or less Firing time (heating time): 1 hour or more and 5 hours or less, preferably 2 hours or more and 3 hours or less
[0083] The timing of starting and ending the heating (firing) is not particularly limited. Heating may be started simultaneously with the start of pressurization, may be started before the start of pressurization, or may be started after the start of pressurization. Heating may be ended simultaneously with the end of pressurization, may be ended before the end of pressurization, or may be ended after the end of pressurization.
[0084] By carrying out compression molding and sintering under the above-mentioned conditions, it is possible to obtain a large-diameter target material 100 in which the crystal orientation is random across the entire sputtering surface. Specifically, it is possible to obtain a large-diameter sintered body in which the ratio R is within the range of 0.3 to 5 across the entire surface that will become the sputtering surface 101. As a result, it is possible to obtain a large-diameter target material 100 in which the ratio R is within the range of 0.3 to 5 across the entire sputtering surface.
[0085] In particular, by intentionally providing a temperature gradient that rises at 10° C. / mm or more in the direction from the front surface to the back surface of the molded body during firing, a large-diameter target material 100 can be obtained in which the ratio R is within the range of 0.3 to 5 in the entire sputtering surface. This is because, by intentionally providing the above-mentioned temperature gradient during firing, even if a temperature gradient (temperature unevenness) that exceeds a predetermined critical value occurs in the surface of the molded body during firing, it is possible to suppress crystal growth (solid-phase growth) in the creeping direction (hereinafter also simply referred to as the "creeping direction") on the surface of the molded body along the temperature gradient in the surface of the molded body. This makes it possible to avoid, for example, the appearance of a region in which crystal grains with a grain size exceeding 30 μm are locally concentrated. It is also possible to avoid the appearance of crystal grains with a grain size exceeding 30 μm. As a result, even in the case of a large-diameter sputtering surface 101, it is possible to avoid the local appearance of a region in which the ratio R is not within the range of 0.3 to 5. In other words, it is possible to avoid a local decrease in the non-orientation of the crystals on the sputtering surface 101.
[0086] Furthermore, by intentionally applying the above-mentioned temperature gradient during firing, it is possible to obtain the effect of suppressing crystal growth in the lateral direction, and therefore it is also possible to obtain a target material 100 in which no crystals with a grain size exceeding 30 μm are observed over the entire sputtering surface and the entire surface parallel to the sputtering surface 101. In other words, it is also possible to obtain a target material 100 in which the entire sputtering surface and the entire surface parallel to the sputtering surface 101 are composed of crystals with a grain size of 0.1 μm or more and 30 μm or less, preferably 0.1 μm or more and 20 μm or less, and more preferably 0.1 μm or more and 10 μm or less.
[0087] If the temperature gradient is less than 10° C. / mm, it becomes difficult to obtain the effect of suppressing crystal growth in the lateral direction during firing.
[0088] The temperature gradient can be, for example, 15° C. / mm or less. This makes it possible to obtain a target material 100 in which the crystal orientation does not differ significantly between the front and back surfaces, that is, the crystal orientation is almost the same. As a result, it becomes possible to make the various physical properties and characteristics, such as the crystal quality, of the KNN film 3 uniform among a plurality of piezoelectric laminates 10 fabricated using one target material 100. In other words, it is possible to prevent the various physical properties and characteristics of the KNN film 3 from changing from run-to-run during the fabrication of the piezoelectric laminate 10. As a result, it is possible to further improve the yield and reliability of the piezoelectric elements 20 and the piezoelectric device modules 30.
[0089] In addition, by heating the molded body (mixture 210) while controlling the temperatures of heaters 207d and 207e based on the temperature detected by temperature sensor 209 so that the temperature in the surface of the molded body becomes uniform (uniform in-plane), that is, so that a temperature gradient is minimized in the surface of the molded body, the effect of suppressing crystal growth in the lateral direction can be reliably obtained. As a result, a large-diameter target material 100 in which the ratio R is within the range of 0.3 to 5 over the entire sputtering surface can be reliably obtained.
[0090] By setting the firing temperature to 800°C or more and 1150°C or less over the entire surface of the molded body and setting the firing time to 1 hour or more and 5 hours or less, sufficient firing (sintering) can be performed while suppressing crystal growth in the lateral direction. As a result, a target material 100 can be obtained in which the ratio R is within the range of 0.3 to 5 over the entire sputtering surface and which has sufficient mechanical strength.
[0091] If the firing temperature is less than 800°C (including the case where the firing temperature is not 800°C or higher over the entire surface of the molded body) or if the firing time is less than one hour, firing may be insufficient, resulting in a sintered body with low mechanical strength. Therefore, cracks are likely to occur in the target material 100 during the preparation of the target material 100 or during the deposition of the KNN film 3.
[0092] Furthermore, when the firing temperature exceeds 1150°C or the firing time exceeds 5 hours, even if a predetermined temperature gradient is applied in the thickness direction of the molded body, the crystal growth in the lateral direction cannot be suppressed, and the crystals may grow large. As a result, regions in which the crystal orientation is not random may appear locally on the sputtering surface 101.
[0093] Furthermore, by carrying out compression molding and sintering under the above-mentioned conditions, and in particular by intentionally applying the above-mentioned temperature gradient during sintering, it is possible to obtain a target material 100 having a relative density of 60% or more and a flexural strength of 10 MPa or more over the entire sputtering surface.
[0094] (Heat treatment) After the compression molding process and the firing process are completed, the obtained sintered body is subjected to a predetermined heat treatment using the above-mentioned molding device 200. The heat treatment is preferably performed while controlling the temperature of the heaters 207a to 207e based on the temperature detected by the temperature sensor 209 so that the temperature in the surface of the sintered body (the surface that becomes the sputtering surface 101) becomes uniform (uniform in-plane).
[0095] The heat treatment conditions are exemplified as follows. Temperature: 600°C or higher and 900°C or lower, preferably 700°C or higher and 800°C or lower Atmosphere: air or oxygen-containing atmosphere Time: 1 hour or more and 20 hours or less, preferably 5 hours or more and 15 hours or less
[0096] Even if the carbon (C) contained in the jig 208 reacts with the O in the mixture 210 during the firing process, causing oxygen deficiency in the sintered body, the oxygen deficiency in the sintered body can be replenished by performing the heat treatment under the above-mentioned conditions. As a result, it is possible to obtain a target material 100 with a higher resistance. For example, it is possible to obtain a target material 100 with a volume resistivity of 1000 kΩcm or more.
[0097] (Finishing process) After the heat treatment is completed, the outer shape and thickness of the heat treated molded body are adjusted as necessary, and the surface is polished to improve the surface condition, thereby obtaining a target material 100 as shown in FIG.
[0098] (6) Effects The present disclosure provides one or more of the following advantages:
[0099] (a) In the KNN film 3 according to this embodiment, even if the film has a large diameter (diameter of 3 inches or more), no local defective regions appear over the entire main surface. That is, the KNN film 3 has an FWHM(001) value in the range of 0.5° to 2.5° over the entire main surface. Therefore, the KNN film 3 has uniform film quality over the entire main surface, and the film characteristics of the KNN film 3 are uniform over the entire main surface of the KNN film 3. As a result, it is possible to prevent variations in characteristics from occurring among a plurality of piezoelectric elements 20 and piezoelectric device modules 30 obtained by processing one piezoelectric laminate 10. This makes it possible to improve the yield and reliability of the piezoelectric elements 20 and piezoelectric device modules 30.
[0100] (b) By sputtering the KNN film 3 using the target material 100 in which the ratio R is within the range of 0.3 to 5 over the entire sputtering surface, it is possible to avoid abnormal discharge occurring over the entire sputtering surface during sputtering. As a result, even when a large-diameter KNN film 3 is sputtered on a large-diameter substrate 1, it is possible to avoid the appearance of local defective regions over the entire main surface of the KNN film 3. In other words, by depositing the KNN film 3 using the above-mentioned target material 100, it is possible to obtain a large-diameter KNN film 3 in which the FWHM(001) value is within the range of 0.5° to 2.5° over the entire main surface.
[0101] Here, as an evaluation method of the crystal orientation (crystal orientation) of the sputtering surface, for example, a method of calculating and evaluating the ratio R at a total of nine points, including one point at the center of the sputtering surface, four points at 1 / 2 the radius at 90° intervals, and four points at a predetermined distance inside from the outer periphery at 90° intervals, may be considered. However, this evaluation method has fewer evaluation points than the present embodiment, so the crystal orientation of the entire sputtering surface may not be accurately evaluated. In particular, in the case of a large-diameter target material having a sputtering surface with a diameter of 3 inches or more, even if an area where the ratio R is not within the range of 0.3 to 5 (an area where the crystal orientation is not random) appears locally, the area may not be found.
[0102] In contrast, in the target material 100 according to the present embodiment, the ratio R is within the range of 0.3 to 5 at all points (e.g., 37 points on a sputtering surface 101 with a diameter of 3 inches) when XRD measurements are performed in a grid pattern at 1 cm intervals in the region excluding the peripheral portion, which is a region 5 mm from the edge of the sputtering surface 101. By sputtering the KNN film 3 on the large-diameter substrate 1 using such a target material 100, it is possible to obtain a large-diameter KNN film 3 whose FWHM(001) value is within the range of 0.5° to 2.5° over the entire main surface.
[0103] (c) In the above-mentioned firing process, the molded body is heated under conditions with a temperature gradient of 10° C. / mm or more from the front surface to the back surface of the molded body, thereby suppressing crystal growth in the creeping direction. As a result, a large-diameter target material 100 can be obtained in which the ratio R is within the range of 0.3 to 5 over the entire sputtering surface.
[0104] (d) In the above-mentioned firing process, the firing temperature is 800° C. or more and 1150° C. or less over the entire surface of the molded body, and the molded body is heated for 1 hour or more and 5 hours or less under the conditions having the above-mentioned temperature gradient, whereby a large-diameter target material 100 can be obtained in which the ratio R is within the range of 0.3 to 5 over the entire sputtering surface and which has sufficient mechanical strength.
[0105] (7) Variations This aspect can be modified as in the following modified examples. In the following description of the modified examples, the same components as those in the above aspect are given the same reference numerals, and the description thereof will be omitted. The above aspect and the following modified examples can be combined in any combination.
[0106] (Variation 1) The piezoelectric stack 10 does not necessarily have to include the lower electrode film 2. In other words, the piezoelectric stack 10 may be configured to include a large-diameter substrate 1, a large-diameter KNN film 3 formed on the substrate 1, and an upper electrode film 4 (electrode film) formed on the KNN film 3.
[0107] 7 shows a schematic diagram of a piezoelectric device module 30 fabricated using the piezoelectric laminate 10 according to this modification. The piezoelectric device module 30 is configured to include at least a piezoelectric element 20 obtained by forming the piezoelectric laminate 10 into a predetermined shape, and a voltage application means 11a and a voltage detection means 11b connected to the piezoelectric element 20. In this modification, the piezoelectric element 20 has pattern electrodes formed by forming an electrode film into a predetermined pattern. For example, the piezoelectric element 20 has a pair of positive and negative pattern electrodes 4p1 on the input side, and a pair of positive and negative pattern electrodes 4p2 on the output side. An example of the pattern electrodes 4p1 and 4p2 is an interdigital transducer (abbreviated as IDT).
[0108] By connecting the voltage application means 11a between the pattern electrodes 4p1 and the voltage detection means 11b between the pattern electrodes 4p2, the piezoelectric device module 30 can function as a filter device such as a surface acoustic wave (SAW) filter. By applying a voltage between the pattern electrodes 4p1 by the voltage application means 11a, a SAW can be excited in the KNN film 3. The frequency of the SAW to be excited can be adjusted, for example, by adjusting the pitch of the pattern electrode 4p1. For example, the shorter the pitch of the IDT as the pattern electrode 4p1, the higher the frequency of the SAW, and the longer the pitch, the lower the frequency of the SAW. Of the SAWs excited by the voltage application means 11a and propagating through the KNN film 3 to reach the pattern electrodes 4p2, a SAW having a predetermined frequency (frequency component) determined according to the pitch of the IDT as the pattern electrode 4p2 generates a voltage between the pattern electrodes 4p2. By detecting this voltage with the voltage detection means 11b, it is possible to extract a SAW having a predetermined frequency from among the excited SAWs. Note that the term "predetermined frequency" used here may include not only a predetermined frequency but also a predetermined frequency band whose center frequency is a predetermined frequency.
[0109] In this modified example, by sputtering the KNN film 3 using the target material 100 having a ratio R in the range of 0.3 to 5 over the entire sputtering surface, it is possible to obtain a large-diameter KNN film 3 having an FWHM(001) value in the range of 0.5° to 2.5° over the entire main surface.
[0110] Also in this modification, the FWHM(001) value is within the range of 0.5° to 2.5° over the entire main surface of the large-diameter KNN film 3. This allows the film characteristics of the KNN film 3 to be uniform over the entire main surface of the KNN film 3. This also makes it possible to prevent variations in characteristics between a plurality of piezoelectric elements 20 (piezoelectric device modules 30) obtained from one piezoelectric laminate 10 in this modification. As a result, the yield and reliability of the piezoelectric elements 20 (piezoelectric device modules 30) can be improved.
[0111] (Variation 2) In the above embodiment, a case has been described in which a powder made of a compound of K (e.g., K2CO3 powder), a powder made of a compound of Na (e.g., Na2CO3 powder), and a powder made of a compound of Nb (e.g., Nb2O5 powder) are mixed in a predetermined ratio in the mixing process for producing the target material 100, but the present invention is not limited to this. For example, in the mixing process, a powder made of a compound containing K and Nb and a powder made of a compound containing Na and Nb may be mixed in a predetermined ratio to obtain a mixture.
[0112] The compound containing K and Nb is at least one selected from the group consisting of an oxide (composite oxide) containing K and Nb, and a compound containing K and Nb that becomes an oxide by heating (e.g., carbonate, oxalate). As the powder of the compound containing K and Nb, for example, KNbO3 powder can be used. KNbO3 powder can be obtained by, for example, mixing a compound of K (e.g., K2CO3 powder) and a compound of Nb (e.g., Nb2O5 powder), calcining the mixture, and pulverizing and mixing the calcined mixture using a ball mill or the like.
[0113] The compound containing Na and Nb is at least one selected from the group consisting of an oxide containing Na and Nb (composite oxide) and a compound containing Na and Nb that becomes an oxide by heating (e.g., carbonate, oxalate). As the powder of the compound containing Na and Nb, for example, NaNbO3 powder can be used. NaNbO3 powder can be obtained by mixing a compound of Na (e.g., Na2CO3 powder) and a compound of Nb (e.g., Nb2O5 powder), calcining the mixture, and pulverizing and mixing the calcined mixture using a ball mill or the like.
[0114] In this case, the composition of the target material 100 can be controlled by adjusting the mixing ratio of KNbO3 powder and NaNbO3 powder, the mixing ratio of K compounds and Nb compounds when producing the KNbO3 powder, and the mixing ratio of Na compounds and Nb compounds when producing the NaNbO3 powder.
[0115] In this modified example, the calcination conditions for producing the KNbO3 powder and the NaNbO3 powder can be the same as the calcination treatment conditions of the above-mentioned embodiment, and the mixing conditions can be the same as the mixing treatment conditions of the above-mentioned embodiment.
[0116] In this modified example, the molded body is heated for 1 hour to 5 hours in the firing process under conditions in which the temperature in the surface of the molded body is 800° C. or more and 1150° C. or less over the entire surface, and the temperature gradient increases at 10° C. / mm or more in the direction from the surface to the back surface of the molded body, thereby obtaining a large-diameter target material 100 in which the ratio R is within a range of 0.3 to 5 over the entire sputtering surface. In addition, by sputtering the KNN film 3 using this target material 100, a large-diameter KNN film 3 in which the FWHM(001) value is within a range of 0.5° to 2.5° over the entire main surface can be obtained.
[0117] (Variation 3) In the above-mentioned embodiment and modified example, the mixing method of each powder in the mixing process and the pulverization process is a wet mixing method, but the present invention is not limited to this. The mixing method in the mixing process may be a dry mixing method. In other words, in the mixing process, each powder may be mixed using a mixer such as an attritor.
[0118] (Variation 4) In the above embodiment, an example in which compression molding and sintering are performed simultaneously, i.e., hot press sintering, has been described, but the present invention is not limited thereto. For example, sintering may be performed after compression molding. That is, for example, using a molding device 200 shown in FIG. 6, a predetermined pressure may be applied to the mixture 210 in a jig 208 to perform compression molding to obtain a molded body, and then the molded body may be heated and sintered under predetermined conditions to obtain a sintered body.
[0119] The conditions for the compression molding process in this modified example are exemplified as follows. Temperature: room temperature (25°C) or higher, preferably 25°C to 50°C Other conditions may be the same as those for the compression molding process described above.
[0120] In this modified example, the firing treatment involves heating the molded body for 1 hour to 5 hours under conditions in which the temperature within the surface of the molded body is 800° C. or more and 1150° C. or less over the entire surface, and the temperature gradient increases from the surface to the back surface of the molded body at a rate of 10° C. / mm or more. Other conditions for the firing treatment in this modified example can be the same as those for the firing treatment in the above-mentioned embodiment.
[0121] In this modified example, by carrying out the firing process under the above-mentioned conditions, it is possible to obtain a large-diameter target material 100 in which the ratio R is within a range of 0.3 to 5 over the entire sputtering surface. In addition, by sputtering the KNN film 3 using this target material 100, it is possible to obtain a large-diameter KNN film 3 in which the FWHM(001) value is within a range of 0.5° to 2.5° over the entire main surface.
[0122] (Variation 5) In the above-mentioned embodiment and modified example, a series of processes from compression molding to heat treatment are performed in one molding apparatus 200, but the present invention is not limited to this. The compression molding, firing, and heat treatment may each be performed in a different apparatus, or two of these processes may be performed in the same apparatus and the other processes may be performed in a different apparatus.
[0123] (Variation 6) In the above embodiment, the example of carrying out the pre-baking process, the crushing process, and the heat treatment has been described, but the present invention is not limited thereto. These processes may be carried out as necessary. That is, as long as it is possible to obtain a large-diameter target material 100 in which the ratio R is within the range of 0.3 to 5 over the entire sputtering surface, these processes may not be carried out.
[0124] (Variation 7) In the above embodiment, the heater 207 is configured with the upper heater 207a, the center heater 207b, and the lower heater 207c, as well as the inner heater 207d and the outer heater 207e, but is not limited thereto. As long as the temperature inside the surface of the molded body is kept at 800° C. or more and 1150° C. or less over the entire surface, and the baking process can be performed under conditions with a temperature gradient that rises at 10° C. / mm or more in the direction from the surface to the back surface of the molded body, the configuration of the heater 207 is not particularly limited.
[0125] (Variation 8) For example, the heating in each of the pre-baking treatment, the baking treatment, and the heat treatment may be performed in multiple steps. This modification also makes it possible to obtain a large-diameter target material 100 in which the ratio R is within the range of 0.3 to 5 over the entire sputtering surface.
[0126] (Variation 9) For example, the jig 208 may be connected to a rotation mechanism via a rotation shaft and configured to be freely rotatable. Then, the heat treatment of the above-mentioned embodiment and modification, the firing treatment of modification 4, etc. may be performed while rotating the jig 208 by the rotation mechanism via the rotation shaft. This makes it easier to heat the molded body or sintered body uniformly in-plane, and makes it easier to make the physical properties of the target material 100 uniform across the entire sputtering surface.
[0127] (Variation 10) For example, an orientation control layer for controlling the orientation of the crystals constituting the KNN film 3 may be provided between the lower electrode film 2 and the KNN film 3, i.e., directly under the KNN film 3. When the lower electrode film 2 is not provided, an orientation control layer may be provided between the substrate 1 and the KNN film 3. The orientation control layer may be formed using a material different from the material constituting the lower electrode film 2, such as a metal oxide, such as SRO, LNO, or strontium titanate (SrTiO3, abbreviated as STO). It is preferable that the crystals constituting the orientation control layer are preferentially oriented in the (100) plane with respect to the main surface of the substrate 1. This makes it possible to easily and reliably achieve an orientation rate of the KNN film 3 of, for example, 80% or more, preferably 90% or more.
[0128] (Variation 11) In the above embodiment, an example in which one laminated structure is formed on one substrate 1 has been described, but the present invention is not limited thereto. For example, a plurality of laminated structures may be formed on one substrate 1. In this case, it is preferable that each of the plurality of laminated structures has a lower electrode film 2, a KNN film 3, and an upper electrode film 4. In the embodiment according to the first modification, it is preferable that each of the plurality of laminated structures has a KNN film 3 and an electrode film 4. The substrate 1 on which one or more laminated structures are formed is also referred to as a piezoelectric laminated substrate.
[0129] (Variation 12) For example, when the above-mentioned piezoelectric laminate 10 is molded into the piezoelectric element 20, the substrate 1 may be removed from the piezoelectric laminate 10, so long as the piezoelectric device module 30 produced using the piezoelectric laminate 10 (piezoelectric element 20) can be applied to a desired application such as a sensor or actuator. EXAMPLES
[0130] Hereinafter, experimental results that support the effects of the above-mentioned embodiment will be described.
[0131] (Sample 1, 2) For samples 1 and 2, the molding apparatus 200 shown in FIG. 6 was used to produce samples containing a predetermined concentration of Mn (K 1-x Na x ) A target material with a diameter of 3 inches was prepared from sintered NbO3.
[0132] Samples 1 and 2 were each produced by performing a mixing process, a calcination / pulverization process, a compression molding process, a calcination process, and a heat treatment. The compression molding process and the calcination process were also performed simultaneously (all at once). In the mixing process, K2CO3 powder, Na2CO3 powder, and Nb2O5 powder were mixed so that the Na / (K+Na) value was 0.55, and MnO powder was mixed so that Mn was contained at a specified concentration to produce a mixture. In the compression molding process, a load of 300 kgf / cm was applied. 2 In the firing process, the molded body was heated for 3 hours under the conditions that the temperature (firing temperature) in the surface of the molded body was 900°C over the entire surface and the temperature gradient increased from the surface to the back surface at 10°C / mm. Other conditions in each process were set to the predetermined conditions within the range of the treatment conditions described in the above-mentioned embodiment.
[0133] (Samples 3-8) In Samples 3 to 8, the temperature gradient increasing in the direction from the front surface to the back surface of the molded body during the firing treatment was changed from that of Sample 1. Specifically, the temperature gradient was set to 12° C. / mm in Samples 3 and 4, 15° C. / mm in Samples 5 and 6, 5° C. / mm in Sample 7, and 7° C. / mm in Sample 8. The rest of the temperature gradient was the same as that in Sample 1.
[0134] (Samples 9-13) In Samples 9 to 13, the firing temperature in the firing treatment was changed from that of Sample 1. Specifically, in Sample 9, the firing temperature was 750°C over the entire surface of the molded body, in Sample 10, the firing temperature was 800°C over the entire surface of the molded body, in Sample 11, the firing temperature was 1000°C over the entire surface of the molded body, in Sample 12, the firing temperature was 1150°C over the entire surface of the molded body, and in Sample 13, the firing temperature was 1200°C over the entire surface of the molded body. The rest were the same as those in the preparation of Sample 1.
[0135] (Samples 14-17) In Samples 14 to 17, the load in the compression molding process was changed from that in Sample 1. Specifically, in Sample 14, the load was 100 kgf / cm 2 For sample 15, the load was 200 kgf / cm 2 For sample 16, the load was 400 kgf / cm 2 For sample 17, the load was 500 kgf / cm 2 The other conditions were the same as those in the preparation of Sample 1.
[0136] (Samples 18-23) In Samples 18 to 23, the time for heating the molded body in the firing treatment (firing time) was changed from Sample 1. Specifically, the firing time was 0.5 hours in Sample 18, 1 hour in Sample 19, 2 hours in Sample 20, 4 hours in Sample 21, 5 hours in Sample 22, and 5.5 hours in Sample 23. The rest were the same as those in the preparation of Sample 1.
[0137] (Sample 24) Sample 24 does not contain dopants such as Mn (K 1-x Na x) A target material with a diameter of 3 inches was prepared from a NbO3 sintered body. Specifically, in the mixing process, K2CO3 powder, Na2CO3 powder, and Nb2O5 powder were mixed so that the value of Na / (K+Na) was 0.55, and no MnO powder was mixed to prepare the mixture. The rest of the process was the same as that for Sample 1.
[0138] (Sample 25) In the case of Sample 25, the compression molding process was performed, and then the firing process was performed. In other words, the compression molding process and the heat treatment were performed separately. The other steps were the same as those used in the preparation of Sample 1.
[0139] (Sample 26) In the case of Sample 26, the compression molding process and the firing process were separately carried out. The other steps were the same as those in the case of producing Sample 24.
[0140] (Sample 27, 28) In samples 27 and 28, (K 1-x Na x ) The composition of the NbO3 sintered body, i.e., the composition of the target material, was changed from Sample 1. Specifically, in Sample 27, K2CO3 powder, Na2CO3 powder, and Nb2O5 powder were mixed in the mixing process so that the value of Na / (K+Na) was 0.40. In Sample 28, a mixture was prepared by mixing K2CO3 powder, Na2CO3 powder, and Nb2O5 powder so that the value of Na / (K+Na) was 0.70. The rest of the process was the same as that for Sample 1.
[0141] (Sample 29-32) Samples 29 to 32 contain Cu as a dopant at a predetermined concentration (K 1-x Na x) A target material having a diameter of 4 inches was prepared from a sintered NbO3 body. Specifically, in the mixing process for Samples 29 to 32, CuO powder was mixed in a predetermined ratio instead of MnO powder to prepare a mixture. In Sample 30, the temperature gradient in the firing process was set to 12°C / mm, in Sample 31, the temperature gradient was set to 3°C / mm, and in Sample 32, the temperature gradient was set to 8°C / mm. The rest of the process was the same as that for Sample 1.
[0142] (Sample 33-36) Samples 33 to 26 contain Cu at a predetermined concentration and Mn at a predetermined concentration (K 1-x Na x ) A target material having a diameter of 6 inches was prepared from a NbO3 sintered body. Specifically, in the mixing process for Samples 33 to 36, a mixture was prepared by mixing CuO powder and MnO powder in a predetermined ratio. In addition, in Sample 34, the temperature gradient in the firing process was set to 14°C / mm, in Sample 35, the temperature gradient was set to 4°C / mm, and in Sample 36, the temperature gradient was set to 9°C / mm. The rest of the process was the same as that for Sample 1.
[0143] <Evaluation> The target materials of Samples 1 to 36 were evaluated for cracking and the ratio R, and the KNN films formed by sputtering using each sample were also evaluated.
[0144] (Crack rating) Each sample was visually evaluated for the presence or absence of cracks. As a result, it was confirmed that cracks occurred in Sample 9 and Sample 18, and that no cracks occurred in the other samples except for Samples 9 and 18. From this, it can be confirmed that if the firing temperature is less than 800°C or the firing time is less than 1 hour, firing is insufficient, resulting in a sintered body with low mechanical strength.
[0145] (Evaluation of ratio R) For each of the samples except for Samples 9 and 18 in which cracks had occurred, XRD measurement was performed on the sputtered surface of the target material, and the ratio R of the (110) peak intensity to the (001) peak intensity was calculated. The XRD measurement was performed in a lattice pattern at 1 cm intervals on the area excluding the area 5 mm from the edge of the sputtered surface. That is, XRD measurement was performed at 37 points for samples with a diameter of 3 inches (Samples 1 to 28), XRD measurement was performed at 69 points for samples with a diameter of 4 inches (Samples 29 to 32), and XRD measurement was performed at 147 points for samples with a diameter of 6 inches (Samples 33 to 36). The ratio R was calculated for all points of the XRD measurement points. The calculation results are shown in Table 1 below. In addition, in the evaluation of the ratio R in Table 1, the "passed measurement points" is the number of measurement points where the ratio R is in the range of 0.3 to 5, and the "pass rate" is the ratio of the number of passed measurement points to the number of all measurement points (= number of passed measurement points / total number of measurement points).
[0146] (Evaluation of KNN membrane) Except for Samples 9 and 18 in which cracks had occurred, the remaining samples were used to form KNN films according to the following procedure.
[0147] In the sputtering deposition using Samples 1, 3, 5, 7, 8, 10-17, 19-28, a Si substrate having a diameter of 4 inches, a thickness of 510 μm, a surface oriented in the (100) plane, and a thermally oxidized film (SiO2 film) having a thickness of 200 nm was prepared as a substrate. Then, on this substrate (on the thermally oxidized film), a Ti layer (thickness: 2 nm) as an adhesion layer, a Pt film (oriented in the (111) plane with respect to the main surface of the substrate, thickness: 200 nm) as a lower electrode film, and a KNN film having a diameter of 4 inches (preferentially oriented in the (001) plane with respect to the surface of the substrate, thickness: 2 μm) as a piezoelectric film were deposited in this order by RF magnetron sputtering.
[0148] In the sputtering deposition using Samples 2, 4, 6, 29 to 36, a Si substrate having a diameter of 6 inches, a thickness of 610 μm, a surface oriented in a (100) plane, and a thermal oxide film (SiO2 film) having a thickness of 200 nm formed on the surface was prepared as a substrate. Then, on this substrate (on the thermal oxide film), a Ti layer (thickness: 2 nm) as an adhesion layer, a Pt film (oriented in a (111) plane with respect to the main surface of the substrate, thickness: 200 nm) as a lower electrode film, and a KNN film having a diameter of 6 inches (preferentially oriented in a (001) plane with respect to the surface of the substrate, thickness: 2 μm) as a piezoelectric film were deposited in this order by RF magnetron sputtering.
[0149] The conditions for depositing the Ti layer were as follows: Temperature (substrate temperature): 300℃ Discharge power: 1200W Atmosphere: Ar gas atmosphere Ambient pressure: 0.3Pa Film deposition speed: A 2.5 nm thick Ti layer is deposited in 30 seconds.
[0150] The conditions for forming the Pt film were as follows: Temperature (substrate temperature): 300℃ Discharge power: 1200W Atmosphere: Ar gas atmosphere Ambient pressure: 0.3Pa Time: 5 minutes
[0151] The target materials used in forming the KNN films were the samples other than the above samples 9 and 18. The conditions in forming the KNN films were as follows. Discharge power: 2200W Atmosphere: Ar gas + O2 gas mixture atmosphere Ambient pressure: 0.3Pa Ar / O2 partial pressure ratio: 25 / 1 Temperature (substrate temperature): 600℃ Film forming speed: 1μm / hr
[0152] Then, the sputter-deposited KNN film was subjected to XRD measurement to obtain the value of FWHM(001). The XRD measurement was performed in a grid pattern at 1 cm intervals on the area excluding a 5 mm area from the edge of the main surface (upper surface) of the KNN film. That is, the XRD measurement was performed at 69 points for the KNN film with a diameter of 4 inches, and at 147 points for the KNN film with a diameter of 6 inches. The measurement results are shown in Table 1 below. In addition, in the evaluation of the KNN film in Table 1, the "passed measurement points" are the number of measurement points whose FWHM(001) value is within the range of 0.5° to 2.5°, and the "pass rate" is the ratio of the number of passed measurement points to the number of all measurement points (= number of passed measurement points / total number of measurement points).
[0153] [Table 1]
[0154] From Table 1, it can be confirmed that in both the target material containing at least one of Mn and Cu as a dopant and the target material not containing a dopant, the temperature in the surface of the molded body is 800°C or more and 1150°C or less over the entire surface, and the molded body is heated for 1 hour or more and 5 hours or less under the condition of a temperature gradient rising at 10°C / mm or more in the direction from the front surface to the back surface of the molded body, thereby obtaining a target material in which the ratio R is within the range of 0.3 to 5 over the entire sputtering surface (see Samples 1 to 6, 10 to 12, 19 to 22, 24, 29, 30, 33, and 34). In other words, it can be confirmed that the target material in which the crystal orientation is random over the entire sputtering surface can be obtained by performing the firing process under the above conditions.
[0155] Furthermore, the inventors have confirmed that if the temperature gradient in the firing process is 15°C / mm or less, the crystal orientation can be made approximately the same between the sputtering surface and the surface opposite to the sputtering surface of the target material while keeping the ratio R within the range of 0.3 to 5 over the entire sputtering surface.
[0156] Also, from Table 1, it can be seen that when the temperature gradient in the firing process is less than 10°C / mm, the pass rate of the ratio R is less than 1, that is, there are cases where a target material having a ratio R within the range of 0.3 to 5 over the entire sputtering surface cannot be obtained (see Samples 7, 8, 31, 32, 35, and 36). This is thought to be because it becomes difficult to obtain the effect of suppressing crystal growth in the creeping direction of the molded body surface during firing.
[0157] Also, from Table 1, it can be seen that when the firing temperature exceeds 1150°C or the firing time exceeds 5 hours, the pass rate of the ratio R is less than 1 over the entire sputtering surface, that is, there are cases where a target material with a ratio R falling within the range of 0.3 to 5 cannot be obtained (see Samples 13 and 23). This is thought to be because when the firing temperature exceeds 1150°C or the firing time exceeds 5 hours, crystal growth in the lateral direction cannot be suppressed even when firing is performed under conditions with the above-mentioned temperature gradient, and therefore regions where the crystal orientation is not random are locally generated on the sputtering surface.
[0158] Also, from Table 1, the load in the compression molding process is 100 kgf / cm 2 More than 500kgf / cm 2 It has been confirmed that within the following range, it is possible to obtain a target material with random crystal orientation over the entire sputtering surface while avoiding the occurrence of cracks (see Samples 14 to 17). The inventors have also confirmed that the jig used during compression molding was not damaged as long as the load during compression molding was within the above range.
[0159] Furthermore, from Table 1, it can be seen that even when the firing process is performed after the compression molding process, by carrying out the specified firing process, it is possible to obtain a target material with random crystal orientation over the entire sputtering surface (see Samples 25 and 26).
[0160] Furthermore, Table 1 confirms that, regardless of the KNN composition in the target material, by performing a specified firing process, a target material with random crystal orientation can be obtained across the entire sputtering surface (see samples 27 and 28).
[0161] Also, from Table 1, it can be confirmed that by sputtering a KNN film on a large-diameter substrate using a target material whose ratio R is within the range of 0.3 to 5 over the entire sputtering surface, a large-diameter KNN film whose FWHM(001) value is within the range of 0.5° to 2.5° over the entire main surface can be obtained. Furthermore, from Table 1, it can be confirmed that when a KNN film is sputtered on a large-diameter substrate using a target material whose ratio R is within the range of 0.3 to 5 over the entire sputtering surface, the pass rate is less than 1, that is, a large-diameter KNN film whose FWHM(001) value is within the range of 0.5° to 2.5° over the entire main surface cannot be obtained. That is, it can be confirmed that a localized defective area appears in the main surface of the KNN film.
[0162] <Preferred aspects of the present disclosure> Preferred aspects of the present disclosure will be described below.
[0163] (Appendix 1) According to one aspect of the present disclosure, A substrate having a major surface with a diameter of 3 inches or more; a piezoelectric film formed on the substrate, the piezoelectric film containing potassium, sodium, niobium, and oxygen and made of an alkali niobium oxide having a perovskite structure; The piezoelectric laminate has an X-ray rocking curve half-width for the (001) plane, measured by X-ray diffraction on the piezoelectric film, within a range of 0.5° to 2.5° over the entire inner area of the main surface of the piezoelectric film, excluding the peripheral portion.
[0164] (Appendix 2) The laminate according to claim 1, preferably The piezoelectric film contains one or more of the following dopants: Li, Mg, Ca, Sr, Ba, Bi, Sb, V, In, Ta, Mo, W, Cr, Ti, Zr, Hf, Sc, Y, La, Ce, Pr, Nd, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu, Cu, Zn, Ag, Mn, Fe, Co, Ni, Al, Si, Ge, Sn, and Ga.
[0165] (Appendix 3) The laminate according to claim 1 or 2, preferably A lower electrode film is formed between the substrate and the piezoelectric film.
[0166] (Appendix 4) The laminate according to any one of Supplementary Notes 1 to 3, preferably An upper electrode film is formed on the piezoelectric film.
[0167] (Appendix 5) According to another aspect of the present disclosure, A step of preparing a sputtering target material made of a sintered body of an alkali niobium oxide having a perovskite structure, the alkali niobium oxide containing potassium, sodium, niobium, and oxygen; providing a substrate having a major surface with a diameter of 3 inches or more; and forming a piezoelectric film on the substrate using the sputtering target material, the piezoelectric film being made of the alkali niobium oxide, the half-width of the X-ray rocking curve of the (001) plane being within a range of 0.5° to 2.5° in the entire inner area excluding the peripheral portion of the main surface when subjected to X-ray diffraction measurement. A method for manufacturing a piezoelectric stack is provided.
[0168] (Appendix 6) According to yet another aspect of the present disclosure, A substrate having a major surface with a diameter of 3 inches or more; A lower electrode film formed on the substrate; a piezoelectric film formed on the lower electrode film, the piezoelectric film containing potassium, sodium, niobium, and oxygen and made of an alkali niobium oxide having a perovskite structure; an upper electrode film formed on the piezoelectric film; The piezoelectric element (piezoelectric device module) is provided such that, when X-ray diffraction measurement is performed on the piezoelectric film, the half-width of the X-ray rocking curve for the (001) plane is within a range of 0.5° or more and 2.5° or less over the entire inner area excluding the peripheral portion of the main surface of the piezoelectric film.
[0169] (Appendix 7) According to yet another aspect of the present disclosure, A substrate having a major surface with a diameter of 3 inches or more; a piezoelectric film formed on the substrate, the piezoelectric film containing potassium, sodium, niobium, and oxygen and made of an alkali niobium oxide having a perovskite structure; An electrode film formed on the piezoelectric film, The piezoelectric element (piezoelectric device module) is provided such that, when X-ray diffraction measurement is performed on the piezoelectric film, the half-width of the X-ray rocking curve for the (001) plane is within a range of 0.5° or more and 2.5° or less over the entire inner area excluding the peripheral portion of the main surface of the piezoelectric film.
[0170] (Appendix 8) According to yet another aspect of the present disclosure, A sputtering target material comprising a sintered body of an alkali niobium oxide having a perovskite structure, the sputtering target material comprising: The diameter of the surface (sputtering surface) that will be exposed to plasma during the film formation process by sputtering is 3 inches or more, The sputtering target material has a ratio of the intensity of the X-ray diffraction peak from the (110) plane to the intensity of the X-ray diffraction peak from the (001) plane, when X-ray diffraction measurement is performed on the surface to be exposed to the plasma, within a range of 0.3 to 5 throughout the entire inner area, excluding the peripheral portion, of the surface to be exposed to the plasma.
[0171] (Appendix 9) According to yet another aspect of the present disclosure, A sputtering target material comprising a sintered body of an alkali niobium oxide having a perovskite structure, the sputtering target material comprising: When used as a target material for film formation by sputtering, a piezoelectric film was formed on a substrate with a diameter of 3 inches or more. A sputtering target material is provided which, when X-ray diffraction measurement is performed on the piezoelectric film, produces a piezoelectric film in which the half-width of the X-ray rocking curve for the (001) plane is within a range of 0.5° or more and 2.5° or less over the entire inner area excluding the peripheral portion of the main surface of the piezoelectric film.
[0172] (Appendix 10) The target material according to claim 8 or 9, preferably The dopant contains one or more of Li, Mg, Ca, Sr, Ba, Bi, Sb, V, In, Ta, Mo, W, Cr, Ti, Zr, Hf, Sc, Y, La, Ce, Pr, Nd, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu, Cu, Zn, Ag, Mn, Fe, Co, Ni, Al, Si, Ge, Sn, and Ga.
[0173] (Appendix 11) The target material according to any one of appendixes 8 to 10, preferably In the entire area of the surface exposed to plasma during the film formation process by sputtering and in the entire area of any surface parallel to this surface, no area is observed in which crystal grains having a grain size exceeding 30 μm are densely concentrated. That is, the entire area of the surface exposed to plasma during the film formation process by sputtering and in the entire area of any surface parallel to this surface are composed of crystal grains having a grain size of 0.1 μm to 30 μm, preferably 0.1 μm to 20 μm, and more preferably 0.1 μm to 10 μm.
[0174] (Appendix 12) The target material according to any one of claims 8 to 11, preferably The relative density is 60% or more over the entire surface that is exposed to plasma during the film formation process by sputtering.
[0175] (Appendix 13) The target material according to any one of appendixes 8 to 12, preferably The flexural strength is 10 MPa or more over the entire surface that is exposed to plasma during film formation by sputtering.
[0176] (Appendix 14) The target material according to any one of appendixes 8 to 13, preferably The volume resistivity is 1000 kΩcm or more.
[0177] (Appendix 15) According to yet another aspect of the present disclosure, A method for producing a sputtering target material made of a sintered body of an alkali niobium oxide having a perovskite structure, the method comprising the steps of: (a) mixing a powder of a potassium compound, a powder of a sodium compound, and a powder of a niobium compound in a predetermined ratio to obtain a mixture; (b) applying a predetermined pressure to the mixture to form a molded body having a diameter of 3 inches or more; (c) heating and firing the molded body for 1 hour to 5 hours under conditions in which the temperature within the surface, which is the surface that will be exposed to plasma when performing a film formation process by sputtering (the surface that will become the sputtered surface), is 800°C or more and 1150°C or less over the entire surface, and the temperature gradient increases at 10°C / mm or more in the direction from the surface to the back surface, which is the surface opposite to the surface, to obtain a sintered body; By carrying out the above steps, a sputtering target material having a surface (sputtering surface) exposed to the plasma with a diameter of 3 inches or more is obtained. A method for making a sputtering target material is provided.
[0178] (Appendix 16) According to yet another aspect of the present disclosure, A method for producing a sputtering target material made of a sintered body of an alkali niobium oxide having a perovskite structure, the method comprising the steps of: (a) mixing a powder of a compound containing potassium and niobium with a powder of a compound containing sodium and niobium in a predetermined ratio to obtain a mixture; (b) applying a predetermined pressure to the mixture to form a molded body having a diameter of 3 inches or more; (c) heating and firing the molded body for 1 hour to 5 hours under conditions in which the temperature within the surface, which is the surface that will be exposed to plasma when performing a film formation process by sputtering (the surface that will become the sputtered surface), is 800°C or more and 1150°C or less over the entire surface, and the temperature gradient increases at 10°C / mm or more in the direction from the surface to the back surface, which is the surface opposite to the surface, to obtain a sintered body; By carrying out the above steps, a sputtering target material having a surface (sputtering surface) exposed to the plasma with a diameter of 3 inches or more is obtained. A method for making a sputtering target material is provided.
[0179] (Appendix 17) The method according to claim 15 or 16, preferably comprising (b) and (c) are carried out simultaneously, i.e. (c) is carried out while (b) is carried out.
[0180] (Appendix 18) The method according to any one of appendices 15 to 17, preferably comprising: After (a) and before (b), (d) heating the mixture at a temperature lower than the heating temperature of the molded body in (c) to calcinate it; (e) pulverizing the mixture after the calcination; In step (b), a predetermined pressure is applied to the pre-calcined and pulverized mixture to form the molded body.
[0181] (Appendix 19) The method according to any one of appendices 15 to 18, preferably comprising: After (c), (f) A step of heating the sintered body at a predetermined temperature is further carried out. [Explanation of symbols]
[0182] 1 Board 3 Piezoelectric film (KNN film) 10 Piezoelectric laminate 100 Target material 101 Sputter surface
Claims
1. A sputtering target material comprising a sintered body of an alkali niobium oxide having a perovskite structure, the sputtering target material comprising: The diameter of the surface that will be exposed to plasma during the film formation process by sputtering is 3 inches or more; when X-ray diffraction measurement is performed on the surface to be exposed to the plasma, a ratio of the intensity of the X-ray diffraction peak from the (110) plane to the intensity of the X-ray diffraction peak from the (001) plane is within a range of 0.3 to 5 inclusive over the entire inner area of the surface to be exposed to the plasma, excluding a peripheral portion within a region 5 mm from the edge; A sputtering target material, wherein the entire inner area, excluding the peripheral portion, of a surface to be exposed to the plasma, and the entire inner area, excluding the peripheral portion of a region 5 mm from the edge, of any surface parallel to the surface to be exposed to the plasma, are composed of crystal grains having a grain size of 0.1 μm or more and 30 μm or less.
2. 2. The sputtering target material according to claim 1, wherein the surface exposed to the plasma has a relative density of 60% or more over the entire inner area excluding the peripheral edge portion.
3. 3. The sputtering target material according to claim 1, wherein the surface exposed to the plasma has a flexural strength of 10 MPa or more over the entire inner area excluding the peripheral edge portion.
4. 4. The sputtering target material according to claim 1, wherein the surface to be exposed to the plasma has a volume resistivity of 1000 kΩcm or more over the entire inner area excluding the peripheral edge portion.
5. The sputtering target material according to any one of claims 1 to 4, containing as a dopant at least one of Li, Mg, Ca, Sr, Ba, Bi, Sb, V, In, Ta, Mo, W, Cr, Ti, Zr, Hf, Sc, Y, La, Ce, Pr, Nd, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu, Cu, Zn, Ag, Mn, Fe, Co, Ni, Al, Si, Ge, Sn, and Ga.
Citation Information
Patent Citations
Target for high frequency sputtering
JP1985021862A
Piezoelectric thin film element and piezoelectric thin film device
JP2011146623A
Substrate with piezoelectric film, method for manufacturing the same and film forming device
JP2012167316A
Piezoelectric ceramic sputtering target, non-lead piezoelectric thin film and piezoelectric thin film element using the same
JP2017179416A
Potassium sodium niobate sputtering target
JP2020183574A