Oxide sintered body, its manufacturing method, and sputtering target material

The oxide sintered body of tin, tantalum, and niobium oxides addresses the issue of defects in transparent conductive films by ensuring low porosity and high density, enhancing sputtering performance and film quality.

JP7557648B2Active Publication Date: 2024-09-27MITSUI MINING & SMELTING CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2024070413
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-09-01
Filing Date
2024-04-24
Publication Date
2024-09-27
Estimated Expiration
2042-07-01

AI Technical Summary

Technical Problem

Existing tin oxide-based transparent conductive films suffer from defects such as pinholes, leading to abnormal discharge and cracking during sputtering, which affects the quality and performance of display devices.

Method used

An oxide sintered body composed of tin, tantalum, and niobium oxides is produced with a low pore area ratio, small pore sizes, and high density to prevent abnormal discharge and cracking, achieved through a method involving separate slurries, spray drying, and controlled sintering.

Benefits of technology

The solution effectively suppresses abnormal discharge and cracking during sputtering, resulting in higher-quality transparent conductive films with reduced defects and improved performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007557648000001
    Figure 0007557648000001
Patent Text Reader

Abstract

To provide an oxide sintered body having few defects such as pinholes, and hardly causing abnormal discharge or cracking when used as a sputtering target material, and a manufacturing method thereof, and the sputtering target material.SOLUTION: The oxide sintered body contains tin element, tantalum element and niobium element. An area ratio of pores per unit area in cross-sectional observation of the oxide sintered body is 1% or less. A maximum equivalent circular diameter of the pores in cross-sectional observation of the oxide sintered body is 20 μm or less. A maximum Feret diameter of the pores in cross-sectional observation of the oxide sintered body is 50 μm or less. A flexural strength of the oxide sintered body measured in accordance with JIS R1601 is 180 MPa or more.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an oxide sintered body and a method for producing the same, and also to a sputtering target material made of an oxide sintered body. [Background technology]

[0002] Tin oxide-based transparent conductive films are used in a wide range of applications, including display devices such as liquid crystal displays, plasma displays, and organic electroluminescence (EL). Sputtering is known as one of the methods for forming tin oxide-based transparent conductive films. When forming conductive films using sputtering, if there are many defects such as pinholes in the sputtering target material, this can cause abnormal discharge during sputtering, and can also cause particles to be generated during sputtering, and breakage or cracks in the target material.

[0003] For the purpose of preventing abnormal discharge from occurring during sputtering, the applicant previously proposed a method for producing a sputtering target in which an unsintered compact containing SnO2 as the main component, Nb2O5, and Ta2O5 is prepared and the compact is sintered at 1550°C to 1650°C (see Patent Document 1). For the same purpose, the applicant previously proposed a sputtering target containing Ta2O5, Nb2O5, and the balance SnO2 and unavoidable impurities (see Patent Document 2). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2007-131891 A [Patent Document 2] JP 2008-248278 A Summary of the Invention

[0005] According to the techniques described in Patent Documents 1 and 2, it is possible to suppress abnormal discharge and cracking of the target material during sputtering. However, further improvement in the performance of display devices using tin oxide-based transparent conductive films is required, and even higher quality tin oxide-based transparent conductive films are also required. Therefore, there is a demand for high-quality sputtering target materials used to manufacture tin oxide-based transparent conductive films, in which the occurrence of abnormal discharge and cracking of the target material during sputtering is reduced compared to conventional methods. Therefore, an object of the present invention is to provide an oxide sintered body which has few defects such as pinholes and which is less likely to cause abnormal discharge or cracks when used as a sputtering target material, a method for producing the same, and a sputtering target material.

[0006] The present invention is an oxide sintered body containing tin, tantalum and niobium, The above-mentioned problem has been solved by providing an oxide sintered body in which the area ratio of pores per unit area in cross-sectional observation of the oxide sintered body is 1% or less.

[0007] The present invention also provides a sputtering target material comprising the above-mentioned oxide sintered body.

[0008] Further, the present invention provides a method for preparing a slurry of tin oxide, a slurry of tantalum oxide, and a slurry of niobium oxide separately, The slurries are mixed to prepare a mixed slurry, The mixed slurry is subjected to a spray drying method to produce a granulated product. Producing a compact using the granules, A method for producing an oxide sintered body, comprising sintering the molded body, The present invention also provides a method for producing an oxide sintered body, in which a dispersant is contained in each of the tin oxide slurry, the tantalum oxide slurry, and the niobium oxide slurry. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The present invention relates to an oxide sintered body and a sputtering target material using the same. The oxide sintered body of the present invention is a sintered body of multiple metal oxides. In detail, the oxide sintered body of the present invention contains tin element (hereinafter, also simply referred to as "Sn"), tantalum element (hereinafter, also simply referred to as "Ta"), and niobium element (hereinafter, also simply referred to as "Nb") as metals. These metal elements are present in the sintered body in the form of oxides of the respective metals, or in the form of composite oxides of at least two metal elements selected from these three metal elements.

[0010] As described in the above-mentioned Patent Document 1, since SnO2 is a substance that is difficult to sinter, it has been difficult to manufacture a dense sintered body containing SnO2. Due to this, sintered bodies containing SnO2 known so far tend to have holes, which are defective parts. In contrast, one of the characteristics of the oxide sintered body of the present invention is that the presence of holes is extremely reduced. The holes are defective parts observed in the cross section of the oxide sintered body of the present invention. In this specification, the cross section of the oxide sintered body refers to a surface obtained by cutting the oxide sintered body by a predetermined means. The pores are open in the cross section and extend toward the inside of the oxide sintered body. The pores include both through holes and bottomed holes. In this specification, the pores refer to defective areas of a size that can be recognized when the cross section of the oxide sintered body is observed with a microscope at a magnification of 200 times (observation field: 445.3 μm × 634.6 μm).

[0011] The degree of the presence of holes in the oxide sintered body of the present invention is extremely low, preferably 1% or less in terms of the area ratio of holes per unit area in cross-sectional observation of the oxide sintered body (hereinafter also referred to as "hole area ratio"). Due to such a low degree of the presence of holes, when the oxide sintered body of the present invention is used as, for example, a sputtering target material, the occurrence of abnormal discharge during sputtering is effectively suppressed. In addition, the generation of particles during sputtering and the occurrence of cracks and breaks in the target material are effectively prevented. From the viewpoint of making these advantages more prominent, the hole area ratio is more preferably 0.9% or less, even more preferably 0.8% or less, even more preferably 0.7% or less, particularly preferably 0.6% or less, and especially preferably 0.5% or less. The closer the hole area ratio value is to zero, the more preferable it is. From this viewpoint, the hole area ratio is preferably greater than 0% and not greater than 1%, more preferably 0.02% or more and not greater than 0.9%, even more preferably 0.04% or more and not greater than 0.8%, even more preferably 0.06% or more and not greater than 0.7%, particularly preferably 0.08% or more and not greater than 0.6%, and especially preferably 0.1% or more and not greater than 0.5%. A method for measuring the hole area ratio will be described in the Examples below. A method for setting the hole area ratio to the above-mentioned value or less will also be described below.

[0012] The oxide sintered body of the present invention is also characterized in that when holes are observed in the cross section, the size of the holes is suppressed. In detail, the maximum equivalent circle diameter of the holes in the cross section of the oxide sintered body is extremely small, 20 μm or less. Since the size of the holes is suppressed in this way, when the oxide sintered body of the present invention is used as a sputtering target material, for example, the generation of particles during sputtering and the generation of cracks and breaks in the target material are effectively prevented. From the viewpoint of making these advantages more prominent, the maximum equivalent circle diameter of the holes is more preferably 18 μm or less, more preferably 16 μm or less, even more preferably 15 μm or less, particularly preferably 13 μm or less, and particularly preferably 12 μm or less. The closer the maximum equivalent circle diameter of the holes is to zero, the more preferable it is. From this viewpoint, the maximum equivalent circle diameter of the hole is preferably more than 0 μm and not more than 20 μm, more preferably 1 μm or more and not more than 18 μm, even more preferably 2 μm or more and not more than 16 μm, even more preferably 3 μm or more and not more than 15 μm, particularly preferably 4 μm or more and not more than 13 μm, and especially preferably 5 μm or more and not more than 12 μm. A method for measuring the maximum equivalent circular diameter of the holes will be described in the Examples below. A method for making the maximum equivalent circular diameter of the holes equal to or smaller than the above-mentioned value will also be described below.

[0013] In addition to the maximum circle equivalent diameter of the hole being equal to or less than the above-mentioned value, the oxide sintered body of the present invention has a maximum Feret diameter of the hole being extremely small, 50 μm or less. The Feret diameter is the size of a rectangle circumscribing the measurement target. By setting the maximum Feret diameter of the hole to the above-mentioned value or less, when the oxide sintered body of the present invention is used as, for example, a sputtering target material, the occurrence of abnormal discharge during sputtering is effectively suppressed. In addition, the generation of particles during sputtering and the occurrence of cracks and breaks in the target material are effectively prevented. From the viewpoint of making these advantages more prominent, the maximum Feret diameter of the hole is more preferably 45 μm or less, more preferably 40 μm or less, even more preferably 35 μm or less, particularly preferably 30 μm or less, particularly preferably 28 μm or less, and most preferably 26 μm or less. The closer the maximum Feret diameter of the hole is to zero, the more preferable it is. From this viewpoint, the maximum Feret diameter of the hole is preferably more than 0 μm and not more than 50 μm, more preferably 2 μm or more and not more than 45 μm, even more preferably 3 μm or more and not more than 40 μm, even more preferably 4 μm or more and not more than 35 μm, particularly preferably 6 μm or more and not more than 30 μm, particularly preferably 8 μm or more and not more than 28 μm, and most preferably 10 μm or more and not more than 26 μm. The method for measuring the maximum Feret diameter of the hole will be described in the Examples below. Also, a method for making the maximum Feret diameter of the hole equal to or smaller than the above-mentioned value will be described later.

[0014] The oxide sintered body of the present invention preferably satisfies at least one of the above-mentioned (i) pore area ratio, (ii) maximum circle equivalent diameter, and (iii) maximum Feret diameter, and more preferably satisfies a combination of at least two of (i)-(iii), and even more preferably satisfies all of (i)-(iii).

[0015] In addition to the above (i)-(iii), the oxide sintered body of the present invention is also characterized by a high relative density. In detail, the oxide sintered body of the present invention preferably has a high relative density of 99.6% or more. By exhibiting such a high relative density, when the oxide sintered body of the present invention is used as a sputtering target material and sputtering is performed using the target material, it is possible to suppress abnormal discharge during sputtering, which is preferable. From this viewpoint, the oxide sintered body of the present invention preferably has a relative density of 99.8% or more, more preferably 100.0% or more, even more preferably 100.2% or more, and particularly preferably 100.3% or more. There is no particular limit to the upper limit of the relative density, but it is preferably 105% or less, more preferably 104% or less, even more preferably 103% or less, and even more preferably 102% or less. The oxide sintered body of the present invention having such a relative density is suitably manufactured by the method described below. The relative density is measured according to the Archimedes method. A specific measurement method will be described in the examples described below.

[0016] The oxide sintered body of the present invention is also characterized by its high strength. In detail, the oxide sintered body of the present invention preferably has a high flexural strength of 180 MPa or more. By exhibiting such a high flexural strength, the oxide sintered body of the present invention is preferable because, when it is used as a sputtering target material and sputtering is performed using the target material, even if an abnormal discharge occurs unintentionally during sputtering, the target material is less likely to break or crack. From this viewpoint, the oxide sintered body of the present invention has a flexural strength of more preferably 190 MPa or more, even more preferably 200 MPa or more, even more preferably 210 MPa or more, particularly preferably 220 MPa or more, particularly preferably 230 MPa or more, and most preferably 240 MPa or more. There is no particular limit to the upper limit of the flexural strength, but it is preferably 300 MPa or less, even more preferably 290 MPa or less, even more preferably 280 MPa or less, and even more preferably 270 MPa or less. The oxide sintered body of the present invention having such a flexural strength is suitably manufactured by the method described below. The flexural strength is measured in accordance with JIS R1601. A specific measurement method will be described in the Examples below.

[0017] The oxide sintered body of the present invention is preferably low in bulk resistivity because DC sputtering can be easily performed when the oxide sintered body is used as a sputtering target material. From this viewpoint, the bulk resistivity of the oxide sintered body is preferably 10 Ω·cm or less. The bulk resistivity is measured in AUTO RANGE mode using Loresta (registered trademark) HP MCP-T410 (serial 4-point probe TYPE ESP) manufactured by Mitsubishi Chemical Corporation. The measurement points are five points in total, near the center and at the four corners of the oxide sintered body, and the arithmetic average value of each measurement value is taken as the bulk resistivity of the sintered body.

[0018] As described above, the oxide sintered body of the present invention contains Sn, Ta, and Nb as metal elements. The oxide sintered body of the present invention preferably contains SnO2 as a main component and Ta2O5 and Nb2O5 as subcomponents from the viewpoint of improving the properties of the transparent conductive film formed from the oxide sintered body. From the viewpoint of making this advantage more prominent, the total amount of Ta2O5 and Nb2O5 in the oxide sintered body is preferably 1.15 mass% or more and 12.0 mass% or less, more preferably 3.5 mass% or more and 10 mass% or less, even more preferably 4.0 mass% or more and 8.0 mass% or less, and even more preferably 5.0 mass% or more and 7.0 mass% or less.

[0019] The ratio of Ta2O5 to Nb2O5 in the oxide sintered body of the present invention, expressed as a mass ratio of Nb2O5 / Ta2O5, is preferably 0.15 to 0.90, more preferably 0.15 to 0.60, even more preferably 0.16 to 0.43, and even more preferably 0.17 to 0.33, from the viewpoint of improving the properties of the transparent conductive film formed from the oxide sintered body and from the viewpoint of improving the sintered density of the oxide sintered body.

[0020] The specific ratios of Sn, Ta, and Nb in the oxide sintered body of the present invention are preferably such that Sn is 80 mass% or more and less than 100 mass% in terms of SnO2, Ta is preferably more than 0 mass% and 10 mass% or less in terms of Ta2O5, and Nb is preferably more than 0 mass% and 10 mass% or less in terms of Nb2O5. Furthermore, Sn is preferably 88 mass % or more and 98.85 mass % or less in terms of SnO2, Ta is preferably 1 mass % or more and 8 mass % or less in terms of Ta2O5, and Nb is preferably 0.15 mass % or more and 4 mass % or less in terms of Nb2O5. In particular, Sn is preferably 90% by mass or more and 96.5% by mass or less in terms of SnO2, Ta is preferably 3% by mass or more and 7% by mass or less in terms of Ta2O5, and Nb is preferably 0.5% by mass or more and 3% by mass or less in terms of Nb2O5. By containing Sn, Ta and Nb in this ratio in the oxide sintered body of the present invention, the properties of the transparent conductive film formed from the oxide sintered body are improved, which is preferable. The proportions of SnO2, Ta2O5, and Nb2O5 are values ​​based on mass including the amount of inevitable impurities contained in the oxide sintered body.

[0021] Next, a preferred method for producing the oxide sintered body of the present invention will be described. The oxide sintered body of the present invention is produced by sintering raw material powders. As the raw material powders, tin oxide powder, tantalum oxide powder, and niobium oxide powder are used. As the tin oxide powder, SnO2 powder is preferably used. As the tantalum oxide powder, Ta2O5 powder is preferably used. As the niobium oxide powder, Nb2O5 powder is preferably used. The proportion of each oxide powder used is preferably adjusted so that the proportions of SnO2, Ta2O5, and Nb2O5 contained in the target oxide sintered body are within the above-mentioned ranges.

[0022] From the viewpoint of ensuring sufficient dispersibility in the dispersion medium, the particle size of each oxide powder is preferably 0.3 μm or more and 1.2 μm or less, more preferably 0.4 μm or more and 1.1 μm or less, and even more preferably 0.5 μm or more and 0.9 μm or less, expressed as a volume cumulative particle size D50 at 50 volume % cumulative volume as measured by a laser diffraction scattering particle size distribution measurement method.

[0023] In the present manufacturing method, the inventors have found that it is advantageous to prepare a slurry of each oxide powder separately and mix the slurries to prepare a mixed slurry, in that it is possible to successfully manufacture an oxide sintered body in which the generation of pores is suppressed. This procedure will be described in detail below. First, a slurry of each oxide powder is prepared separately. As the dispersion medium used for preparing the slurry, a liquid capable of dispersing each oxide powder can be used. Examples of such dispersion medium include water and various organic solvents. As the organic solvent, for example, ethanol can be used. Among these dispersion mediums, it is preferable to use water from the viewpoint of economy and ease of handling. When the proportion of the dispersion medium in the slurry is set to preferably 20 mass% or more and 70 mass% or less, more preferably 30 mass% or more and 60 mass% or less, and even more preferably 35 mass% or more and 55 mass% or less, relative to the mass of the oxide powder, the oxide powder is sufficiently dispersed in the dispersion medium.

[0024] The concentration of each oxide powder in the slurry is preferably 58% by mass or more and 84% by mass or less, more preferably 62% by mass or more and 77% by mass or less, and even more preferably 64% by mass or more and 74% by mass or less, taking into consideration the dispersibility of the oxide powder in the dispersion medium. From the viewpoint of increasing the dispersibility of each oxide powder contained in the slurry, it is preferable to mix a dispersant into each slurry. As the dispersant, an appropriate one can be used according to the type of oxide powder. For example, polycarboxylates such as ammonium polycarboxylate, sodium polycarboxylate, and polycarboxylate amine salts; quaternary cationic polymers; nonionic surfactants such as polyalkylene glycols; and cationic surfactants such as quaternary ammonium salts can be used. These dispersants can be used alone or in combination of two or more. Among these dispersants, it is preferable to use polycarboxylates because of their high dispersibility of the oxide powder, and it is particularly preferable to use ammonium polycarboxylate. The type of dispersant contained in each slurry may be the same or different.

[0025] The concentration of the dispersant to be added to each slurry is appropriately selected according to the concentration and type of the oxide powder contained in the slurry. When the concentration of the dispersant in the slurry is set to preferably 0.01% by mass or more and 0.04% by mass or less, more preferably 0.015% by mass or more and 0.035% by mass or less, and even more preferably 0.02% by mass or more and 0.03% by mass or less, based on the mass of the oxide powder, satisfactory dispersibility is exhibited. The concentration of the dispersant in each slurry may be the same or different.

[0026] A binder may be added to each slurry. By adding a binder, the strength of the granulated material can be made appropriate when the granulated material is obtained using the mixed slurry described below. As the binder, for example, various organic polymer materials can be used. As the organic polymer material, for example, polyvinyl alcohol, acrylic emulsion binder, etc. can be used. The concentration of the binder to be mixed in each slurry is appropriately selected according to the concentration and type of the oxide powder contained in the slurry. The strength of the granulated product can be made appropriate by setting the concentration of the binder in the slurry to preferably 0.2% by mass or more and 0.8% by mass or less, more preferably 0.3% by mass or more and 0.7% by mass or less, and even more preferably 0.4% by mass or more and 0.6% by mass or less, based on the mass of the oxide powder. The concentration of the binder in each slurry may be the same or different.

[0027] The slurry is prepared by mixing the components constituting the slurry. For mixing, it is preferable to use a media mill such as a ball mill or a bead mill, since the oxide powder can be sufficiently dispersed in the dispersion medium.

[0028] After preparing each slurry by the above procedure, the slurries are then mixed to prepare a mixed slurry. The mixing ratio of each slurry is preferably adjusted so that the ratio of SnO2, Ta2O5, and Nb2O5 contained in the target oxide sintered body falls within the above-mentioned range. In order to mix the slurries to obtain a mixed slurry, it is preferable to use a media mill such as a ball mill or a bead mill, but the method is not limited to this.

[0029] The following advantages are obtained by preparing a slurry of each oxide powder and mixing the slurries to obtain a mixed slurry. In this manufacturing method, as described later, it is preferable to obtain a granulated material by a spray-drying method using a mixed slurry. In order to smoothly carry out the spray-drying method, it is advantageous to increase the amount of dispersant blended in the mixed slurry to reduce the viscosity of the mixed slurry. However, if the blending amount of the dispersant is increased, the granulated material obtained by the spray-drying method tends to be hard and difficult to crush. If such a granulated material is used to compression-mold a molded body for producing an oxide sintered body, defective parts are likely to occur in the molded body due to the fact that the granulated material is difficult to crush during the compression process. If such a molded body is fired, the obtained sintered body will not be dense, and defective parts will occur. On the other hand, if the amount of dispersant mixed in the mixed slurry is reduced in order to make the granules easier to crush, the viscosity of the mixed slurry tends to increase, which makes it difficult to produce granules with a uniform shape. If such granules are used for compression molding, defects tend to occur in the molded body, and the sintered body will not be dense and will have defects. In response to this, the inventors have found that by adding a dispersant to each oxide powder slurry and then mixing the slurries to obtain a mixed slurry, the increase in viscosity of the mixed slurry can be suppressed even if the amount of dispersant added is reduced, and a mixed slurry with good dispersibility can be obtained. The sintered body manufactured using such a mixed slurry is dense and has suppressed occurrence of defective portions.

[0030] There is another advantage to preparing a slurry of each oxide powder and mixing the slurries to obtain a mixed slurry, which will be described below. In the conventional technology, for example, the technology described in Patent Documents 1 and 2 described above, when producing an oxide sintered body containing a plurality of metal elements, the oxide powders of each metal element were dispersed in a dispersion medium all at once to prepare a slurry. When the slurry was prepared in this manner, the dispersant blended in the slurry acted preferentially on a specific oxide, and the inventors found that the dispersibility in the dispersion medium differed between the oxides. If the dispersibility differed, the state of the oxide powder in the granulated product produced from the slurry, for example, the degree of crushability, became non-uniform, which caused the disadvantage that holes were likely to occur in the finally obtained oxide sintered body. The reason for the difference in dispersibility is that the interaction between the dispersant and each oxide powder differs depending on the type of oxide powder. Therefore, in the present production method, in order to prevent the difference in dispersibility in the dispersion medium between the oxides, instead of dispersing each oxide powder in a dispersion medium all at once, a method is adopted in which each oxide powder is dispersed in a dispersion medium separately for each oxide powder, and a dispersant is blended in the dispersion medium at that time. By employing this method, the dispersant acts reliably on each oxide powder, so that differences in dispersibility of each oxide powder in the mixed slurry are unlikely to occur.

[0031] Once the mixed slurry is prepared, the mixed slurry is subjected to a spray-drying method to produce a granulated product. In the granulation by the spray-drying method, it is preferable to produce a granulated product having a particle size represented by a volume cumulative particle size D50 at 50% of cumulative volume by a laser diffraction scattering particle size distribution measurement method of 30 μm to 60 μm, particularly 35 μm to 55 μm, and particularly 40 μm to 50 μm, in terms of the ease of crushing the granulated product. The ease of crushing the granulated product is advantageous in that holes are less likely to be generated when the granulated product is used to produce an oxide sintered body. The volume cumulative particle size D50 of the granulated product is a particle size measured without ultrasonic dispersion treatment.

[0032] Once the granules are obtained, they are filled into a mold to produce a compact. For molding, a cold pressing method such as cold isostatic pressing can be used. The pressure during molding is 600 kg / cm. 2 More than 1200kg / cm2 It is preferable to set the above range in order to obtain a dense molded body. When the molded body is obtained, the molded body may be subjected to a degreasing step as necessary. By subjecting the molded body to the degreasing step, organic substances contained in the molded body, such as dispersants and binders, can be removed. The degreasing step is performed by heating the molded body, for example, in an air atmosphere at 500°C to 900°C.

[0033] When the molded body is obtained in this way, it is then fired. The firing of the molded body can generally be carried out in an oxygen-containing atmosphere. It is particularly convenient to fire the molded body in an air atmosphere. The firing temperature is preferably 1500°C or more and 1700°C or less, more preferably 1520°C or more and 1680°C or less, and even more preferably 1550°C or more and 1650°C or less. The firing time is preferably 1 hour or more and 100 hours or less, more preferably 2 hours or more and 50 hours or less, and even more preferably 3 hours or more and 30 hours or less. The temperature increase rate and the temperature decrease rate are each independently preferably 5°C / hour or more and 500°C / hour or less, more preferably 10°C / hour or more and 200°C / hour or less, and even more preferably 20°C / hour or more and 100°C / hour or less.

[0034] The oxide sintered body obtained by the above method is dense and the formation of pores is suppressed. Therefore, the oxide sintered body has a low pore area ratio and a small maximum equivalent circle diameter and maximum Feret diameter.

[0035] The oxide sintered body thus obtained can be processed to a predetermined size by grinding or the like to obtain a sputtering target material. The obtained sputtering target material is bonded to a backing plate to obtain a sputtering target. For example, stainless steel, copper, titanium, or the like can be used as the backing plate. For example, a low melting point solder such as indium can be used to bond the target material to the backing plate. The sputtering target thus obtained is suitable for use in the manufacture of a sputtered film, such as a transparent conductive film. The sputtered film formed using this sputtering target can have the same composition as the sputtering target material. The specific resistance of the sputtered film is preferably low, at 9 mΩ·cm or less. EXAMPLES

[0036] The present invention will be described in more detail below with reference to examples, but the scope of the present invention is not limited to these examples.

[0037] Example 1 SnO2 powder with a particle size D50 of 0.7 μm, Ta2O5 powder with a particle size D50 of 0.6 μm, and Nb2O5 powder with a particle size D50 of 0.9 μm were prepared. The particle size D50 was measured using a particle size distribution measuring device MT3300EXII manufactured by Microtrackbell Co., Ltd. Water was used as the dispersion medium. The refractive index of the measurement material was 2.20. Each oxide powder was placed in a separate pot, and 0.5% by mass of polyvinyl alcohol, 0.02% by mass of ammonium polycarboxylate, and 50% by mass of water were added relative to the mass of each oxide powder, and mixed using a ball mill for 20 hours to prepare each slurry. The prepared slurries were mixed together and mixed for 60 minutes using a ball mill to obtain a mixed slurry. The mixing ratio of each slurry was 96.5 mass% SnO2, 3.0 mass% Ta2O5, and 0.5 mass% Nb2O5 relative to the total of each powder.

[0038] The mixed slurry was supplied to a spray dryer, and spray drying was carried out under the conditions of an atomizer rotation speed of 14000 rpm, an inlet temperature of 200° C., and an outlet temperature of 80° C. to obtain granules. The particle size D50 of the granules was 45 μm. The obtained granules were filled into a 158 mm x 640 mm mold and subjected to a pressure of 800 kg / cm 2 The obtained green body was heated at 750°C for 6 hours in the air to be degreased. The degreased green body was sintered to produce a sintered body. The sintering was performed in an atmosphere with an oxygen concentration of 20 vol%, at a sintering temperature of 1600°C for 8 hours, with a temperature increase rate of 50°C / h and a temperature decrease rate of 50°C / h. The sintered body thus obtained was cut to obtain an oxide sintered body having a width of 100 mm, a length of 240 mm, a thickness of 8 mm, and a surface roughness Ra of 1.0 μm. A #170 grindstone was used for the cutting.

[0039] [Examples 2 and 3] The SnO2 powder, Ta2O5 powder, and Nb2O5 powder were mixed so that the ratio of each powder to the total powder was as shown in Table 1 below. Other than this, an oxide sintered body was obtained in the same manner as in Example 1.

[0040] Comparative Example 1 The same SnO2 powder, Ta2O5 powder, and Nb2O5 powder as in Example 1 were prepared. Each powder was weighed so that SnO2 was 94 mass %, Ta2O5 was 5 mass %, and Nb2O5 was 1 mass % based on the total mass of the powders, and then dry mixed for 21 hours. A 4% by mass aqueous solution of polyvinyl alcohol was added in an amount of 6% by mass relative to the mixed powder. After mixing the polyvinyl alcohol and the mixed powder in a mortar, the mixture was passed through a 5.5 mesh sieve to obtain a mixed powder for molding. Other than these, the oxide sintered body was obtained in the same manner as in Example 1.

[0041] Comparative Example 2 The same SnO2 powder, Ta2O5 powder, and Nb2O5 powder as in Example 1 were prepared. All the powders were placed in a pot, and 0.5% by mass of polyvinyl alcohol, 0.02% by mass of ammonium polycarboxylate, and 50% by mass of water were added to the total amount of powder, and mixed for 20 hours using a ball mill to prepare a mixed slurry. The ratio of each powder in the mixed slurry was 94% by mass of SnO2, 5% by mass of Ta2O5, and 1% by mass of Nb2O5 relative to the total amount of each powder. A sintered oxide body was obtained in the same manner as in Example 1 except for this.

[0042] Comparative Example 3 In this comparative example, the concentration of ammonium polycarboxylate, which is the dispersant used in Example 2, was increased from 0.02% by mass to 0.05% by mass. Except for this, an oxide sintered body was obtained in the same manner as in Example 2.

[0043] 〔evaluation〕 For the oxide sintered bodies obtained in the examples and comparative examples, the pore area ratio, maximum equivalent circle diameter, maximum Feret diameter, relative density, and flexural strength were measured by the following methods. In addition, sputtering targets were manufactured using the oxide sintered bodies obtained in the examples and comparative examples, and the degree of abnormal discharge and the degree of cracking of the targets when sputtering was performed using the targets were evaluated by the following methods. The results are shown in Table 1 below.

[0044] [Hole area ratio, maximum circle equivalent diameter and maximum Feret diameter] (1) Preparation of cross section of oxide sintered body The cut surface obtained by cutting the oxide sintered body was polished stepwise using emery paper #180, #400, #800, #1000, and #2000, and finally buffed to a mirror finish. (2) Measurement of pore area ratio, maximum circle equivalent diameter and maximum Feret diameter A BSE-COMP image (hereinafter also referred to as "SEM image") was taken of the cross section of the oxide sintered body at a magnification of 200 times and within a range of 445.3 μm × 634.6 μm using a scanning electron microscope (SU3500, manufactured by Hitachi High-Technologies Corporation). The SEM image was traced using particle analysis software ("Particle Analysis Version 3.0", manufactured by Sumitomo Metal Technology Co., Ltd.) and image recognition was performed using a scanner. This image was binarized. At this time, the conversion value was set so that one pixel was displayed in μm units. Next, the area and the sum of the areas of all the holes shown in the SEM images were calculated. The percentage of the sum of the areas of the holes relative to the field area (445.3 μm × 634.6 μm) was calculated. The arithmetic mean value of the percentages measured for 10 different SEM images was calculated, and this arithmetic mean value was defined as the hole area ratio in the present invention. In addition, the equivalent circular diameter of the pores was calculated based on the area of ​​the pores measured in the process of calculating the pore area ratio. The maximum equivalent circular diameter of the pores was determined as the maximum equivalent circular diameter of the pores among all the equivalent circular diameters measured in 10 different SEM images. In addition to the above operations, the horizontal Feret diameter (μm) was calculated based on the total number of pixels in the horizontal direction for all holes shown in the SEM images, and the vertical Feret diameter (μm) was calculated based on the total number of pixels in the vertical direction. The maximum value of all the horizontal and vertical Feret diameters measured for 10 different SEM images was taken as the maximum Feret diameter of the holes.

[0045] [Relative density] The relative density was measured based on the Archimedes method. Specifically, the mass of the oxide sintered body in air was divided by the volume (mass of the sintered body in water / specific gravity of water at the measurement temperature) to obtain the theoretical density ρ (g / cm3) based on the following formula (1). 3 The percentage of the density was taken as the relative density (unit: %). ρ={(C1 / 100) / ρ1+(C2 / 100) / ρ2+(C3 / 100) / ρ3} -1 (1) In formula (1), C1 to C3 respectively indicate the content (mass%) of the constituent substances of the target material, and ρ1 to ρ3 respectively indicate the density (g / cm 3 ) is shown. In the present invention, the contents (mass%) of the constituent substances of the target material are considered to be SnO2, Ta2O5, and Nb2O5, for example. C1: Mass% of SnO2 in the target material ρ1: Density of SnO2 (6.95g / cm 3 ) C2: mass% of Ta2O5 in the target material ρ2: Density of Ta2O5 (8.74g / cm 3 ) C3: Mass% of Nb2O5 in the target material ρ3: Density of Nb2O5 (4.47g / cm 3 ) The theoretical density ρ can be calculated by applying The mass % of SnO2, the mass % of Ta2O5, and the mass % of Nb2O5 can be determined from the results of analysis of each element in the target material by ICP-OES analysis.

[0046] [Folding strength] An Autograph (registered trademark) AGS-500B manufactured by Shimadzu Corporation was used. A sample piece (total length 36 mm or more, width 4.0 mm, thickness 3.0 mm) cut out from the oxide sintered body was subjected to measurement according to the three-point bending strength measurement method of JIS R1601.

[0047] [Extent of abnormal discharge and target cracking] A sputtering target was prepared using the oxide sintered body obtained in the examples and comparative examples, and the target was attached to a DC magnetron sputtering device to perform sputtering. The sputtering conditions were as follows. ·Achieved vacuum level: 3×10 -6 Pa Sputtering pressure: 0.4Pa Oxygen partial pressure: 1×10 -3 Pa ·Power input time: 2W / cm 2 Duration: 25 hours The number of arcs that occurred during sputtering under the above conditions was counted using an arc counter attached to the power supply. The arc counter used was a μArc Monitor MAM Genesis MAM Data Collector Ver. 2.02 (manufactured by LANDMARK TECHNOLOGY). The evaluation criteria were as follows: A: Less than 5 arcing events B: Number of arcing events is 5 or more but less than 30 C: Arcing count is 30 or more While sputtering was being carried out under the above conditions, the target was also visually observed to evaluate whether or not cracks had occurred.

[0048] [Table 1]

[0049] As is clear from the results shown in Table 1, when the oxide sintered bodies obtained in the respective Examples are used as sputtering target materials, abnormal discharge is less likely to occur during sputtering, and the target is less likely to crack, compared to the case where the oxide sintered bodies obtained in the Comparative Examples are used as sputtering target materials. In contrast, in Comparative Example 1, in which a green body for sintering was produced without using the spray drying method, the green body could not be made dense, and a large number of pores were generated in the oxide sintered body produced from the green body. In addition, in Comparative Example 2 in which a slurry was not prepared for each raw material powder, the granulated material was non-uniform, the green body could not be made dense, and the oxide sintered body produced from the green body had a large number of holes. In Comparative Example 3, in which the amount of dispersant was greater than in Comparative Example 2, the granules were uniform, but were hard and difficult to crush. As a result, the compact could not be made dense, and the oxide sintered body produced from the compact had many holes. [Industrial Applicability]

[0050] According to the present invention, there are provided an oxide sintered body which has few pores or, even if pores are present, has a small size, and which is less likely to cause abnormal discharge or cracks when used as a sputtering target material, a manufacturing method thereof, and a sputtering target material. When sputtering is performed using the oxide sintered body according to the present invention, it is possible to form a film while suppressing the occurrence of abnormal discharge and cracks during sputtering, as compared with the case of using a conventional oxide sintered body, so that the generation of unnecessary defective products can be suppressed, and the generation of waste can be reduced. In other words, it is possible to reduce the energy cost for disposing of such waste. This leads to the sustainable management and efficient use of natural resources, and the achievement of decarbonization (carbon neutrality).

Claims

1. An oxide sintered body containing tin, tantalum and niobium, The area ratio of holes per unit area in a cross-sectional observation of the oxide sintered body is 1% or less, A sputtering target material made of an oxide sintered body, having a flexural strength of 180 MPa or more as measured in accordance with JIS R1601.

2. An oxide sintered body containing tin, tantalum and niobium, The maximum circle equivalent diameter of a hole in a cross-sectional observation of the oxide sintered body is 20 μm or less, A sputtering target material made of an oxide sintered body, having a flexural strength of 180 MPa or more as measured in accordance with JIS R1601.

3. An oxide sintered body containing tin, tantalum and niobium, The maximum Feret diameter of a hole in a cross-sectional observation of the oxide sintered body is 50 μm or less, A sputtering target material made of an oxide sintered body, having a flexural strength of 180 MPa or more as measured in accordance with JIS R1601.

4. An oxide sintered body containing tin, tantalum and niobium, The area ratio of holes per unit area in a cross-sectional observation of the oxide sintered body is 1% or less, The maximum equivalent circle diameter of the hole is 20 μm or less, The maximum Feret diameter of the hole is 50 μm or less, A sputtering target material made of an oxide sintered body, having a flexural strength of 180 MPa or more as measured in accordance with JIS R1601.

5. SnO 2 80% by mass or more and less than 100% by mass of tin element in terms of Ta 2 O 5 Tantalum element in an amount of more than 0 mass% and not more than 10 mass% in terms of Nb 2 O 5 The sputtering target material according to claim 1 , further comprising: a niobium element in an amount of more than 0 mass % and not more than 10 mass % in terms of niobium content.

6. SnO 2 90% by mass or more and 96.5% by mass or less of tin element in terms of Ta 2 O 5 Tantalum element in an amount of 3 mass% or more and 7 mass% or less in terms of Nb 2 O 5 The sputtering target material according to claim 5 , further comprising: 0.5 mass % or more and 3 mass % or less of niobium element, calculated as a niobium content of 0.5 mass % or more and 3 mass % or less.

7. T 2 O 5 and Nb 2 O 5 The ratio of Nb 2 O 5 / Ta 2 O 5 The sputtering target material according to claim 5 , wherein the mass ratio of the metal oxide to the metal oxide is 0.15 or more and 0.90 or less.

8. 6. The sputtering target material according to claim 5, which has a relative density of 99.6% or more as measured by the Archimedes method.

9. 5. The sputtering target material according to claim 1, which has a bulk resistivity of 10 Ω·cm or less.

10. A method for producing a sputtered film using a sputtering target material described in any one of claims 1 to 4.

11. A method for producing the sputtering target material according to any one of claims 1 to 4. A tin oxide slurry, a tantalum oxide slurry, and a niobium oxide slurry are separately prepared; The slurries are mixed to prepare a mixed slurry, The mixed slurry is subjected to a spray drying method to produce a granulated product. Producing a compact using the granules, A method for producing a sputtering target material, comprising sintering the molded body, a dispersant content of 0.01 mass % or more and 0.04 mass % or less relative to the mass of oxide powder contained in the tin oxide slurry, the tantalum oxide slurry, and the niobium oxide slurry, respectively.

12. The method of claim 11 , wherein the dispersing agent is a polycarboxylate.

13. An oxide sintered body containing tin, tantalum, and niobium, The alloy contains tin element of 90% by mass or more and 96.5% by mass or less in terms of SnO 2 , tantalum element of 3% by mass or more and 7% by mass or less in terms of Ta 2 O 5 , and niobium element of 0.5% by mass or more and 3% by mass or less in terms of Nb 2 O 5 , The area ratio of holes per unit area in a cross-sectional observation of the oxide sintered body is 1% or less, An oxide sintered body having a flexural strength of 180 MPa or more as measured in accordance with JIS R1601.

14. An oxide sintered body containing tin, tantalum, and niobium, The alloy contains tin element of 90% by mass or more and 96.5% by mass or less in terms of SnO 2 , tantalum element of 3% by mass or more and 7% by mass or less in terms of Ta 2 O 5 , and niobium element of 0.5% by mass or more and 3% by mass or less in terms of Nb 2 O 5 , The maximum circle equivalent diameter of a hole in a cross-sectional observation of the oxide sintered body is 20 μm or less, An oxide sintered body having a flexural strength of 180 MPa or more as measured in accordance with JIS R1601.

15. An oxide sintered body containing tin, tantalum, and niobium, The alloy contains tin element of 90% by mass or more and 96.5% by mass or less in terms of SnO 2 , tantalum element of 3% by mass or more and 7% by mass or less in terms of Ta 2 O 5 , and niobium element of 0.5% by mass or more and 3% by mass or less in terms of Nb 2 O 5 , The maximum Feret diameter of a hole in a cross-sectional observation of the oxide sintered body is 50 μm or less, An oxide sintered body having a flexural strength of 180 MPa or more as measured in accordance with JIS R1601.

16. An oxide sintered body containing tin, tantalum, and niobium, The alloy contains tin element of 90% by mass or more and 96.5% by mass or less in terms of SnO 2 , tantalum element of 3% by mass or more and 7% by mass or less in terms of Ta 2 O 5 , and niobium element of 0.5% by mass or more and 3% by mass or less in terms of Nb 2 O 5 , The area ratio of holes per unit area in a cross-sectional observation of the oxide sintered body is 1% or less, The maximum equivalent circle diameter of the hole is 20 μm or less, The maximum Feret diameter of the hole is 50 μm or less, An oxide sintered body having a flexural strength of 180 MPa or more as measured in accordance with JIS R1601.

17. The oxide sintered body according to claim 13, wherein a ratio of Ta 2 O 5 to Nb 2 O 5 , expressed as a mass ratio of Nb 2 O 5 / Ta 2 O 5 , is 0.15 or more and 0.90 or less.

18. An oxide sintered body described in any one of claims 13 to 16, having a relative density measured based on the Archimedes method of 99.6% or more.

19. An oxide sintered body described in any one of claims 13 to 16, having a bulk resistivity of 10 Ω·cm or less.

20. A method for producing a sputtered film using the oxide sintered body described in any one of claims 13 to 16 as a sputtering target material.

21. A method for producing an oxide sintered body according to any one of claims 13 to 16, comprising the steps of: A tin oxide slurry, a tantalum oxide slurry, and a niobium oxide slurry are separately prepared; The slurries are mixed to prepare a mixed slurry, The mixed slurry is subjected to a spray drying method to produce a granulated product. Producing a compact using the granules, A method for producing an oxide sintered body, comprising sintering the molded body, a dispersant in an amount of 0.01 mass % or more and 0.04 mass % or less relative to the mass of oxide powder contained in the tin oxide slurry, the tantalum oxide slurry, and the niobium oxide slurry, respectively.

22. The method of claim 21, wherein the dispersant is a polycarboxylate.

Citation Information

Patent Citations

  • Preparation of ceramic raw material and apparatus therefor

    JP1992187555A

  • Material for forming thin film

    JP2000273622A

  • SnO2-BASED SPUTTERING TARGET AND MANUFACTURING METHOD THEREFOR

    JP2007131891A

  • Method of manufacturing ceramic

    JP2008150224A

  • SnO2-BASE SPUTTERING TARGET AND SPUTTER FILM

    JP2008248278A