Plastic container lids made from recycled plastic
A balanced plastic composition using polyethylene, polypropylene, polybutyl terephthalate, and olefin thermoplastic elastomers addresses the recycling challenges of POM and PBT, ensuring container lids maintain integrity and functionality.
Patent Information
- Application Number
- JP2021010665
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-01-26
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2041-01-26
AI Technical Summary
Plastic waste materials, particularly those containing polyacetal (POM) and polybutylene terephthalate (PBT), are not suitable for recycling due to their high mechanical strength, leading to issues like cracking when used in container lids, despite being collected in large quantities with polyethylene (PE) and polypropylene (PP).
A plastic molded product using polyethylene and/or polypropylene as a main material, combined with polybutyl terephthalate and/or polyacetal resin as an auxiliary material, and an olefin thermoplastic elastomer as an additive, achieving a balanced flexibility and hardness through injection molding.
The solution provides a plastic molded product with improved impact resistance and appropriate pull-out load, suitable for container lids, maintaining integrity under impact and temperature stress.
Smart Images

Figure 0007558564000003 
Figure 0007558564000001 
Figure 0007558564000002
Abstract
Description
[Technical field]
[0001] The present invention relates to plastic molded products such as plastic containers and container lids, and more particularly to plastic molded products made using waste plastic materials. [Background technology]
[0002] In recent years, the recycling of containers and packaging has progressed, and for plastic molded products, attempts to recycle waste materials reproduced during the manufacturing process (pre-consumer materials) and materials collected after use by consumers (post-consumer materials) are becoming more widespread. Recycling methods include material recycling, in which waste plastic is melted and pelletized to be used again as plastic material, and chemical recycling, in which waste plastic is chemically treated and used as a chemical raw material. Of these, material recycling is a promising recycling method because it places less strain on the environment, is inexpensive, and has high utilization efficiency.
[0003] However, the materials used in plastic products are not uniform, and include a variety of materials, such as olefin-based materials such as polyethylene and polypropylene, ester-based materials such as polystyrene, and materials with high mechanical strength called engineering plastics such as polyacetal, polyamide, and polycarbonate. Some materials are suitable for material recycling, while others are not. Material recycling can be achieved relatively easily if the plastic raw materials that make up the waste are suitable for material recycling, but there are many cases where materials that are not suitable for material recycling are mixed into the materials collected as waste, and many plastic products are made by mixing multiple materials and composite materials such as elastomers, and in this case, even if they are pelletized and reused, they may not meet the characteristics required for the intended plastic molded product.
[0004] In other words, in material recycling, if the recycled plastic material does not satisfy the characteristics required for the desired plastic product, recycling cannot be realized as intended.
[0005] To address these problems, Patent Document 1 discloses a technology for improving the impact resistance and flexibility of recycled plastic products by adding 1 to 50% by weight of an elastic polymer such as recycled rubber, styrene-butadiene rubber, ethylene-propylene rubber, styrene-butadiene-styrene block polymer, or styrene-isoprene-styrene block polymer to recycled plastics containing polyethylene resin, polypropylene resin, and polystyrene resin, relative to 50 to 99% by weight of the recycled plastic. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2009-1693 A DISCLOSURE OF THEINVENTION [Problem to be solved by the invention]
[0007] Currently, most plastic materials collected as waste are polyethylene (PE) and polypropylene (PP), with a certain amount of polyacetal (POM) and polybutylene terephthalate (PBT) present, though less. When POM or PBT is added to PE or PP and pelletized to produce recycled plastic material for molding, molding is possible, but it has been found that the properties (physical properties) of the molded product are different from those of recycled plastic molded products that do not contain POM or PBT, and may not be suitable for the intended use. For example, when manufacturing a container lid as a molded product, the container lid is required to not easily fall off the container when fitted to the container, that is, to have an appropriate pull-out load and not break when dropped. However, if hard resins such as POM or PBT are added, they are likely to break when dropped, making them unsuitable as a lid material.
[0008] The present invention has been made to solve the above-mentioned problems, and aims to provide a molded product made from waste plastics that is suitable for containers and container lids, and in particular to provide a molded product that satisfies specified performance requirements using waste plastic materials including POM, PBT, etc. [Means for solving the problem]
[0009] The plastic molded product of the present invention, which solves the above problems, is a plastic molded product obtained by injection molding a plastic raw material including plastic waste, characterized in that the plastic waste contains polyethylene and / or polypropylene as a main material, polybutyl terephthalate and / or polyacetal resin as a secondary material, and the plastic raw material contains polyethylene and an olefin-based thermoplastic elastomer () as an additive resin. Metallocene plastomer and / or metallocene polyethylene are particularly preferred as the additive resin.
[0010] The plastic container lid material of the present invention is obtained by injection molding plastic raw materials including plastic waste, the plastic waste contains polyethylene and / or polypropylene as a main material, polybutyl terephthalate and / or polyacetal resin as a secondary material, the plastic raw materials further contain additive resins, and is characterized in that the number of cracks occurring during a drop test (5°C, dropped from a height of 70 cm, 10 samples) is zero. Note that the drop height of 70 cm in this drop test is based on the average height of an average person's waist or the average height of a table on which a plastic container is placed. The temperature is set to 5°C in winter, which is a temperature that is harsher than room temperature. Effect of the Invention
[0011] According to the present invention, by using plastic waste material containing polyethylene and / or polypropylene as a main material and polybutyl terephthalate and / or polyacetal resin as a secondary material, it is possible to provide a plastic molded product with a good balance between flexibility and hardness. In particular, it is possible to provide a plastic molded product having the performance required for a lid material. [Brief description of the drawings]
[0012] [Figure 1] FIG. 1 shows the structure of a lid material produced in an embodiment, with the upper part being a cross-sectional view of the lid material and the lower part being a view from the opening side of the lid. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] Hereinafter, embodiments of the plastic molded product and the lid material of the present invention will be described.
[0014] The plastic molded product (including the lid material) of the present invention is produced by using waste plastic material (recycled material) as the plastic raw material, adding an additive resin to this, and subjecting it to injection molding.
[0015] Plastic waste includes recycled plastic products after use and waste materials that remain after the injection molding process, and includes polyethylene, polypropylene, and mixtures of these as main materials, and polyacetal resin, polybutylene phthalate, and other engineering plastics and mixtures of these as secondary materials.
[0016] The ratio of PE to PP and the ratio of POM to PBT in the mixture are not particularly limited, but the ratio of the secondary material to the main material is preferably 70:30 to 90:10 by weight, and the secondary material is preferably less than 30% by weight, more preferably 25% by weight or less. If the amount of the secondary material exceeds 30% by weight, the impact absorption property decreases, and even if an additive resin is added, the material is likely to crack when subjected to an impact such as a drop at low temperatures.
[0017] As the additive resin, it is preferable to use polyethylene or an olefin elastomer, and LDPE, LLDPE, or its α-olefin polymer is more preferable. In particular, polyethylene synthesized by a metallocene catalyst (metallocene polyethylene) and polyethylene-α-olefin copolymer (metallocene plastomer) in which α-olefins such as butene-1, hexene-1, and 4-methylpentene-1 are copolymerized with polyethylene by a metallocene catalyst are preferable. Metallocene polyethylene and metallocene plastomer have less branching and are more flexible and rigid than ordinary polyethylene (LDPE). By adding them as additive resin, it is possible to improve the impact resistance of plastic waste materials that contain the above-mentioned high mechanical strength engineering plastics as secondary materials. However, if the amount of additive resin is too large, it is more likely to crack when impacted. In addition, when the plastic molded product is a lid material for a container, it is required that it does not come off the container when holding the lid, that is, that the pull-out load is high, but if the additive resin exceeds 30% by weight, the pull-out load tends to decrease.
[0018] Therefore, the amount of the added resin is preferably not more than 30% by weight, more preferably 25% by weight or less, based on 100% by weight of the plastic waste. The lower limit of the amount is preferably 10% by weight or more, more preferably more than 10% by weight.
[0019] The plastic molded product of the present invention basically uses the above-mentioned plastic waste material and additive resin as plastic materials, but may also contain plastic materials other than recycled plastics and resins other than PE and PP, such as PA (nylon) and SBC (styrene-based thermoplastic elastomer). Furthermore, known additives such as pigments, ultraviolet absorbers, and antistatic agents may be added.
[0020] The plastic molded product of the present invention is made by crushing plastic materials (plastic waste) separated by type of resin from plastic waste using a crusher (e.g., a resin ball pressure crusher) and feeding them to a normal injection molding machine together with added resins. After crushing, the plastic waste may be melted and pelletized. In addition, plastic waste may be supplied in a form in which PP and PE are not separated, and such plastic waste may also be used. Additives are added to granular (including powdered) or pelletized plastic waste as necessary, and the plastic is fed to a normal injection molding machine. The injection molding conditions vary depending on the shape and structure of the molded product, but molding can be performed under the same conditions as those for injection molding of normal PE or PP.
[0021] For example, when the molded product is a relatively small part such as a container lid, the mold temperature is set to 60° C., the holding pressure is set to 30 to 50 MPa, and the cycle time is set to 15 to 30 seconds / set to obtain an injection molded product.
[0022] The plastic molded product of the present invention is molded using plastic waste materials with different properties and additive resins, and can provide a molded product with excellent impact resistance that is not inferior to products using PP or PE alone, compared to products using only plastics with different properties. In particular, when the plastic molded product is a lid material for a container, a product with an appropriate pull-out load required for the lid material can be obtained. The pull-out load means the load required when the lid material is fitted to the container and the fitting between the container and the lid material is released by an external force. The lid material does not come off the container just by holding it, and can be removed from the container by applying an appropriate force, so an appropriate pull-out load is required in relation to the container.
[0023] As an example, in a lid 10 (diameter: 34.8 mm, height: 34.8 mm, thickness: 1.3 mm, weight: approximately 3.5 g) having a structure in which a protrusion 11 is provided on the inner periphery and this protrusion 11 engages with a recess formed on the outer periphery of the mouth of a container as shown in Fig. 1, when the lid is fitted to the container, the container is fixed with the bottom side, and the lid is pulled up at a predetermined pulling speed (200 mm / min), the load (pull-out load) at which the lid comes out of the container is preferably 50 N or more and 70 N or less. This makes it possible to provide a lid that will not easily come off even when the container is lifted by holding only the lid, for a container whose total weight including the container and contents is approximately 250 g.
[0024] In addition, due to its excellent impact resistance, it will not break or crack even if it is hit by an object or dropped under normal use conditions. Specifically, when a lid with the above structure is dropped to the floor from a height of 70 cm at a low temperature (5°C), zero cracks occurred in 10 samples.
[0025] As described above, according to the present invention, it is possible to provide plastic products with good properties, particularly lids for containers, by using multiple types of plastic waste. This makes it possible to increase the recycling efficiency of plastic waste and significantly reduce the amount of waste material disposed of, compared to recycling only PE or PP. EXAMPLES
[0026] Hereinafter, examples in which the plastic molded article of the present invention is used as a container lid material will be described. In the following description, unless otherwise specified, "%" means "% by weight."
[0027] 1. Manufacturing of lid material <Example 1> As plastic waste, recycled molded products and waste materials generated during injection molding are collected, and mixed material of PE and PP (unsorted material): Main material A, mixed material of PBT and POM (unsorted material): Secondary materialAfter crushing and turning into powder (granules), 80% of material A and 20% of material B were mixed together to prepare a plastic raw material for injection molding.
[0028] In addition, metallocene polyethylene (product name: Harmolex, manufactured by Japan Polyethylene Co., Ltd.) and metallocene-based polyethylene (product name: Kernel, manufactured by Japan Polyethylene Co., Ltd.) were mixed in a weight ratio of 90:10, and this was added as additive resin C at 10% to 100% of the plastic waste.
[0029] The plastic raw material with the added resin was injection molded under the molding conditions of mold temperature: 60°C, cycle time: 16.4 seconds / set, and holding pressure: 40 MPa to produce a container lid (diameter: 34.8 mm, height: 34.8 mm, thickness: 1.3 mm, weight: approximately 3.5 g) with the shape shown in Figure 1. This lid fits onto the container by the projections on the inner periphery engaging with the recesses of the container.
[0030] <Examples 2 to 4> The addition ratio of the additive was changed as shown in Table 1, and the rest was the same as in Example 1, and injection molding was carried out to produce container lid materials. [Table 1]
[0031] <Example 5> The additive was added at a ratio of 30% to 100% of the plastic waste material, and injection molding was carried out in the same manner as in Example 1 to produce a container lid material. However, the conditions for injection molding were a cycle time of 34.5 seconds and a holding pressure of 45 MPa.
[0032] <Example 6> The same plastic waste material as in Example 1 (main material A + secondary material B) was used, and 10% of metallocene-based polyethylene (product name: Harmolex, manufactured by Japan Polyethylene Corporation) was added as additive resin C to 100% of this plastic waste material. Injection molding was performed in the same manner as in Example 1 to produce a container lid material.
[0033] <Example 7> The same plastic waste material as in Example 1 (main material A + secondary material B) was used, and 10% of metallocene plastomer (product name: Kernel, manufactured by Japan Polyethylene Corporation) was added as additive resin C to 100% of this plastic waste material. Injection molding was performed in the same manner as in Example 1 to produce a container lid material.
[0034] <Comparative Example 1> Using 100% plastic waste material (a mixture of 90% recycled PP and 10% POM) and without adding any additional resin, injection molding was performed to produce a container lid material. The conditions for injection molding were cycle time: 25.8 seconds / set, and holding pressure: 35 MPa.
[0035] <Comparative Example 2> A container lid material was produced by injection molding without adding any additives using the same plastic waste material as in Example 1. The conditions for injection molding were cycle time: 25.8 seconds / set, and holding pressure: 35 MPa.
[0036] <Comparative Example 3> A container lid material was produced by injection molding in the same manner as in Example 1, except that the ratio of main material A to auxiliary material B was changed to main material A: 70% and auxiliary material B: 30%.
[0037] <Reference example 1, reference example 2> Using only the main material A, a container lid material was produced by injection molding.
[0038] 2. Evaluation of molded products A visual evaluation of solvent resistance, a pull-out load evaluation, and a drop test were performed on the container lid materials produced in Examples 1 to 6 and Comparative Examples 1 to 3. Furthermore, for Reference Examples 1 and 2, a pull-out load evaluation and a drop test were performed.
[0039] The visual evaluation of solvent resistance was carried out by a coating test in which the surface of the molded product was wiped with a cloth soaked in alcohol (left for 24 hours after coating) and an immersion test in which the product was immersed in a container of alcohol for three days, and the appearance was visually observed to confirm the occurrence of "silvering" (surface haze). The results were for 10 samples, and if even one of them showed silvering, it was marked as "X", and if none showed silvering, it was marked as "O".
[0040] In the drop test, the molded products were dropped upside down from heights of 50cm, 60cm, and 70cm from the floor (P tile) in an environment of room temperature (RT) and 5℃, and the lid material was visually observed to see if it had any cracks. The results were rated as "Good" if none of the 10 samples had any cracks, "Good" if at least one crack was found but not all, and "Poor" if more than 80% had cracks.
[0041] The pull-out load was measured at room temperature and at 37°C, when the container was fixed with the lid fitted and the lid was pulled up at a speed of 200mm / min, and the load at which the lid came out of the container was measured. Note that when using the container, it is important that the lid does not come out easily when lifting or moving the container by holding only the lid, and the standard (reference specification) for the pull-out load in the container manufacturing industry is considered to be 50N or more, even in a high temperature environment (37°C).
[0042] The evaluation results of the above molded products are shown in Table 2. [Table 2]
[0043] As shown in Reference Examples 1 and 2, when only the main material PP (Reference Example 1) or PP+PE (Reference Example 2) was used, excellent results were shown in both the drop test and pull-out load. In contrast, as shown in Comparative Examples 1 and 2, when 10% or more of a secondary material (POM or PBT) was mixed, the pull-out load decreased and the product was more likely to crack when dropped.
[0044] On the other hand, the molded products of Examples 1 to 7, in which the main material and the secondary material were mixed and an additive resin was added, all showed better results in the pull-out load and drop test than those of Comparative Examples 1 and 2.
[0045] Specifically, as a result of the drop test, at room temperature, no cracks occurred in any of the samples except for Comparative Example 3, but at 5°C, cracks occurred when dropped from 60 cm in Comparative Examples 2 and 3. Furthermore, in Example 1, which contains 10% added resin, cracks occurred 2 to 3 times out of 10 times in a drop test from 70 cm, and it was found that the amount of added resin is preferably more than 10%.
[0046] With regard to the removal load (37°C), all of the examples except for Example 5 showed high values of 50N or more (above the reference standard), but Comparative Example 1 showed about 42N, and Comparative Examples 2 and 3 showed values of 40N or less. Furthermore, Example 5, in which the amount of added resin was 30%, also showed a removal load of 40N or less, and it is considered that the amount of added resin to be used as a lid material should be 30%. Not to exceed It has been found that it is preferable to
[0047] Furthermore, a comparison between Example 1 and Comparative Example 3 revealed that even if the amount of added resin was the same (10%), when the amount of secondary material (PBT / POM) was large, the required performance as a lid material was insufficient in both the drop test and pull-out load, and the amount of PBT or POM in the waste material was preferably less than 30%.
[0048] Furthermore, it was confirmed that the molded products of Examples 1 to 7 all had good solvent resistance to alcohol. On the other hand, as shown in Table 2, "silver" was confirmed on the top surface of the lid material of the molded products of Comparative Examples 1 and 2. In Comparative Examples 2 and 3, since the total plastic material contained a large amount of PBT, it is considered that the "silver" occurred due to insufficient drying of the PBT. [Explanation of symbols]
[0049] 10: Lid material, 11: Protrusion
Claims
1. A lid material for plastic containers obtained by injection molding a plastic raw material including plastic waste, The plastic waste material is mainly composed of polyethylene and / or polypropylene. Contains pyrene and, as a secondary material, polyacetal resin; The plastic raw material contains, as an additive resin, one or more selected from polyethylene and / or olefin-based thermoplastic elastomers in an amount of 10% by weight or more and less than 30% by weight based on 100% by weight of the plastic waste material; A lid material for plastic containers, characterized in that it produces zero cracks during a drop test (5°C, dropped from a height of 70 cm, 10 samples).
2. The plastic container lid material according to claim 1, A lid for plastic containers, characterized in that the removal load (37°C) when the lid for containers is fitted onto the container is 50N or more.
3. A lid material for a plastic container as described in claim 1, A lid material for plastic containers, characterized in that the secondary material contains polyacetal resin and polybutyl terephthalate.
4. The plastic container lid material according to claim 1 or 3, A lid material for plastic containers, characterized in that the proportion of the main material in the plastic waste is 70% by weight or more and 90% by weight or less, and the proportion of the secondary material is 10% by weight or more and 30% by weight or less.
5. The plastic container lid material according to claim 1, A lid material for plastic containers, characterized in that the added resin is metallocene polyethylene and / or metallocene plastomer.
Citation Information
Patent Citations
Compatibilizing agent, modifier for plastic recycling use, recycling plastic material and molded form therefrom
JP2001220473A
Producing method for regenerated polyolefin resin composition and the same
JP2001246621A
Polyethylene / Polyalkylene terephthalate composition retaining physical characteristics, even when being reused in extrusion molding, extrusion molding method therefor and moldings
JP2003261751A
Thermoplastic resin composition, method for producing the same and molded product of the same
JP2004204210A
Sandwich molded product
JP2005305981A