Packaging and method for manufacturing the same

A laminate sheet with a propylene resin base layer and ethylene vinyl alcohol copolymer barrier layer, thermoformed below the melting point, addresses the challenge of achieving both transparency and barrier properties in packaging, ensuring effective protection for food containers.

JP7558695B2Active Publication Date: 2024-10-01IDEMITSU UNITECH CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2020114143
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-07-02
Filing Date
2020-07-01
Publication Date
2024-10-01
Estimated Expiration
2040-07-01

AI Technical Summary

Technical Problem

Existing packaging materials lack both excellent barrier properties against water vapor and oxygen while maintaining high transparency, particularly in applications like food containers that require microwave heating.

Method used

A laminate sheet composed of a base layer containing propylene resin with smectica crystals and a barrier layer, such as ethylene vinyl alcohol copolymer resin, is thermoformed below the melting point of the propylene resin to create a package with internal haze of 15% or less, ensuring both high transparency and effective barrier properties.

Benefits of technology

The package achieves both excellent barrier properties and high transparency, effectively preventing oxidative deterioration and moisture absorption, maintaining food quality and appearance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007558695000004
    Figure 0007558695000004
  • Figure 0007558695000005
    Figure 0007558695000005
  • Figure 0007558695000006
    Figure 0007558695000006
Patent Text Reader

Abstract

To provide a package that has both excellent barrier properties and high transparency.SOLUTION: A package of this invention is obtained by thermoforming a laminated sheet obtained by laminating at least 2 layers of a substrate layer 41 containing a propylene-based resin containing a smectic-crystal and a barrier layer 42 at a temperature below the melting point of the propylene-based resin, wherein the internal haze is 15% or less, the ratio of the internal haze of the package to the internal haze of the laminated sheet before thermoforming is 1 or less, and the isotactic pentad fraction of the propylene-based resin is 85 mol% or more and 99 mol% or less.SELECTED DRAWING: Figure 4
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a package. [Background technology]

[0002] In packaging, highly transparent polyethylene terephthalate (PET) resin, biaxially oriented polystyrene (OPS) resin, polypropylene (PP) resin, etc. are often used because they provide excellent visibility of the contents. For example, when packaging is used as a food container, the number of packaging that is heated in a microwave oven has increased in recent years, and polypropylene-based resins with high oil resistance and heat resistance are used. For example, Patent Document 1 describes a method for producing a molded article, including the step of producing a molded article using a laminate having (a) a first layer containing polypropylene and a second layer containing one or more selected from the group consisting of polyethylene, polyamide, ethylene-vinyl alcohol copolymer, and ethylene-vinyl acetate copolymer. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2018-127006 A Summary of the Invention [Problem to be solved by the invention]

[0004] Furthermore, in order to protect the contents (for example, in the case of food containers, to reduce food waste and maintain the flavor), packaging is required to have barrier properties against water vapor and oxygen. However, there is no packaging material that has excellent barrier properties while maintaining high transparency. The laminate described in Patent Document 1 is a laminate for decorating a resin molded body, and Patent Document 1 does not disclose a laminate for imparting high transparency and excellent barrier properties to a molded body. In addition, in the laminate described in Patent Document 1, the second layer is also a layer that is expected to be separated from the first layer before molding.

[0005] An object of the present invention is to provide a packaging material that combines excellent barrier properties with high transparency. [Means for solving the problem]

[0006] According to one aspect of the present invention, there is provided a packaging body obtained by thermoforming a laminate sheet comprising at least two layers, a base layer containing a propylene-based resin containing smectite crystals, and a barrier layer, at a temperature equal to or lower than the melting point of the propylene-based resin.

[0007] In one embodiment of the packaging body of the present invention, the internal haze of the packaging body may be 15 percent or less, and the ratio of the internal haze of the packaging body to the internal haze of the laminated sheet before thermoforming may be 1 or less.

[0008] In the package according to one aspect of the present invention, the propylene-based resin may have an isotactic pentad fraction of 85 mol % or more and 99 mol % or less.

[0009] In one embodiment of the packaging material according to the present invention, the crystallization rate of the propylene-based resin at 130° C. is 2.5 min -1 It may be the following.

[0010] In the packaging material according to one aspect of the present invention, the propylene-based resin may have an exothermic peak of 1.0 J / g or more on the low temperature side of a maximum endothermic peak in a differential scanning calorimetry curve.

[0011] In the packaging material according to one aspect of the present invention, the base layer may not contain a nucleating agent.

[0012] In the packaging body according to one aspect of the present invention, the laminate sheet may have a thickness of 0.2 mm or more and 1.2 mm or less.

[0013] In the packaging body according to one aspect of the present invention, the barrier layer may contain an ethylene-vinyl alcohol copolymer resin.

[0014] The packaging body according to one aspect of the present invention may be used for packaging food products. Effect of the Invention

[0015] According to one aspect of the present invention, a package having both excellent barrier properties and high transparency can be provided. [Brief description of the drawings]

[0016] [Figure 1] FIG. 2 is an enlarged cross-sectional view of a laminate sheet forming a package according to one embodiment of the present invention. [Diagram 2] FIG. 2 is an enlarged cross-sectional view of a laminate sheet forming a package according to one embodiment of the present invention. [Diagram 3] FIG. 2 is an enlarged cross-sectional view of a laminate sheet forming a package according to one embodiment of the present invention. [Figure 4] 1 is a schematic diagram of a package according to an embodiment of the present invention. [Diagram 5] FIG. 2 is a schematic diagram showing a manufacturing apparatus for manufacturing the laminate sheet of Example 1. [Figure 6] FIG. 2 is a schematic diagram showing a manufacturing apparatus for manufacturing the laminated sheet of Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] Hereinafter, an embodiment of the present invention will be described in detail with reference to the accompanying drawings. In this specification and the drawings, components having substantially the same functional configurations are denoted by the same reference numerals, and duplicated explanations will be omitted.

[0018] [First embodiment] In the first embodiment, a packaging body according to one aspect of the present invention, a laminate sheet forming the packaging body, and a container including the packaging body will be described.

[0019] [Laminated sheet] 1 is an enlarged cross-sectional view of a laminate sheet forming the packaging body of the present embodiment. The packaging body of the present embodiment is formed by thermoforming a laminate sheet 1 having at least two layers, a base layer 2 and a barrier layer 3, laminated together.

[0020] (base material layer) The base layer 2 contains a propylene-based resin. The propylene-based resin may be a polymer containing at least propylene. Examples of the polymer containing propylene include homopolypropylene and a copolymer of propylene and an olefin. The copolymer of propylene and an olefin may be a block copolymer or a random copolymer. Alternatively, it may be a mixture thereof (a mixture containing a block copolymer and a random copolymer). From the viewpoint of heat resistance and hardness, the propylene-based resin in the present embodiment is preferably homopolypropylene.

[0021] The propylene-based resin forming the base layer 2 contains Smectic crystals as a crystalline structure. Smectic crystals are a metastable intermediate phase, and each domain size is small, so they have excellent transparency. In addition, since they are in a metastable state, the laminated sheet 1 containing Smectic crystals softens with a lower amount of heat compared to a sheet containing α crystals, which are highly crystallized, and therefore has excellent moldability.

[0022] The propylene-based resin may contain other crystal forms such as β crystals, γ crystals, and amorphous portions in addition to the Smectic crystals. For example, 30% by mass or more, 50% by mass or more, 70% by mass or more, or 90% by mass or more of the propylene-based resin may be Smectic crystals, and the rest may be other crystal forms.

[0023] The presence of smectic crystals in a propylene-based resin can be confirmed, for example, by small-angle X-ray scattering analysis.

[0024] The propylene-based resin preferably has an isotactic pentad fraction of 85 mol % or more and 99 mol % or less. If the isotactic pentad fraction is 85 mol % or more, the laminate sheet 1 has excellent rigidity. If the isotactic pentad fraction is 99 mol % or less, the laminate sheet 1 has excellent transparency. The isotactic pentad fraction is the fraction of pentad units (units in which five consecutive propylene monomers are isotactically bonded) in the molecular chain of the resin composition. The method for measuring this fraction is described, for example, in Macromolecules, Vol. 8 (1975), p. 687, 13 It can be measured by C-NMR.

[0025] Propylene-based resin has a crystallization rate of 2.5 min at 130℃. -1 It is preferable that the crystallization rate is 2.5 min -1 When the crystallization rate is equal to or less than this, rapid hardening of the part in contact with the mold during thermoforming can be suppressed, and deterioration of the design can be prevented. The crystallization rate can be measured by the method described in the Examples.

[0026] In the differential scanning calorimetry curve, the propylene-based resin preferably has an exothermic peak of 1.0 J / g or more, more preferably an exothermic peak of 1.5 J / g or more, on the low-temperature side of the maximum endothermic peak. The upper limit of the exothermic peak is not particularly limited. The upper limit of the exothermic peak is usually 10 J / g or less. The exothermic peak can be measured using a differential scanning calorimeter.

[0027] The base layer 2 may contain, in addition to the propylene-based resin, a resin other than the propylene-based resin, an additive, and the like. It is preferable that the base layer 2 does not contain a nucleating agent. When the base layer 2 does not contain a nucleating agent, the number of α crystals and spherulites in the base layer 2 does not increase, and the crystallinity of the base layer 2 does not increase. Examples of the nucleating agent include sorbitol-based crystal nucleating agents, etc. Examples of commercially available products include Gelall MD (New Japan Chemical Co., Ltd.) and Rikemaster FC-2 (Riken Vitamin Co., Ltd.).

[0028] Thickness T of base layer 2 B1 is not particularly limited. B1 is appropriately set depending on the application of the packaging body.

[0029] (Barrier layer) The barrier layer 3 is a layer having oxygen barrier properties that suppresses oxidative deterioration of the contents. The barrier layer 3 is formed of at least one resin selected from the group consisting of ethylene vinyl alcohol copolymer resin (EVOH), polyvinylidene chloride resin (PVDC), and polyacrylonitrile resin (PAN). Alternatively, as described later, when the barrier layer 3 is formed by a method of coating the material of the barrier layer 3 on the base layer 2, examples of the material for forming the barrier layer 3 include a coating material selected from the group consisting of inorganic materials such as silica, alumina, aluminum, and silicon nitride, organic materials such as polyvinyl alcohol (PVA), and organic-inorganic hybrid materials such as silica / PVA.

[0030] The barrier layer 3 preferably contains an ethylene-vinyl alcohol copolymer resin (EVOH). A barrier layer containing EVOH provides high oxygen barrier properties. From the viewpoints of transparency and thermoformability, the EVOH preferably has an ethylene copolymerization ratio of 38 mol % or more and 47 mol % or less.

[0031] When the barrier layer 3 contains ethylene-vinyl alcohol copolymer resin (EVOH), the package obtained by thermoforming the laminate sheet 1 has excellent oxygen barrier properties. The base material layer 2 of the laminate sheet 1 according to this embodiment has high water vapor barrier properties. Therefore, in the laminate sheet 1, the base material layer 2 suppresses the deterioration of the oxygen barrier properties of the barrier layer 3 formed of ethylene-vinyl alcohol copolymer resin (EVOH) due to contact with water or water vapor, and as a result, the oxygen barrier properties of the package obtained by thermoforming the laminate sheet 1 having the barrier layer 3 are excellent.

[0032] When the barrier layer 3 is formed of ethylene-vinyl alcohol copolymer resin (EVOH), the thickness T of the entire laminate sheet 1 and the thickness T of the barrier layer 3 are B2 The ratio of [(T B2 / T) × 100] is preferably 2% or more and 15% or less. When this ratio is 2% or more, excellent oxygen barrier properties are easily obtained, and when it is 15% or less, the laminate sheet 1 is easily thermoformed and an increase in the cost of the laminate sheet 1 can be suppressed.

[0033] The barrier layer 3 may contain, in addition to EVOH, resins other than EVOH, additives, and the like.

[0034] The thickness of the laminate sheet 1 is appropriately set depending on the application of the packaging material. For example, the thickness of the laminate sheet 1 can be set to 0.2 mm or more and 1.2 mm or less.

[0035] The laminate sheet 1 may contain an antifogging agent as necessary. When the laminate sheet 1 contains an antifogging agent, at least one of the base layer 2 and the barrier layer 3 may contain the antifogging agent. The antifogging agent is not particularly limited, but is preferably at least one selected from the group consisting of sucrose fatty acid esters, glycerin fatty acid esters, fatty acid tertiary amides, higher alcohol fatty acid esters, and propylene glycol fatty acid esters, and among these, from the viewpoints of transparency and antifogging properties, sucrose fatty acid esters are preferred, and partial ester compounds of sucrose and aliphatic monocarboxylic acids having 12 to 22 carbon atoms are more preferred. One type of antifogging agent may be used alone, or two or more types may be used in combination.

[0036] Furthermore, the laminate sheet used in the packaging material is not limited to a two-layer structure consisting of a base layer 2 and a barrier layer 3 as in the laminate sheet 1, but may be a multi-layer structure of three or more layers. A laminate sheet having a multi-layer structure of three or more layers may have other layers in addition to the base layer and the barrier layer. For example, there is a laminate sheet having other layers (not shown) between the base layer 2 and the barrier layer 3 in the laminate sheet 1 of FIG. 1. Examples of other layers include an adhesive layer or an anti-fogging layer containing an anti-fogging agent.

[0037] When the laminate sheet has an anti-fogging layer, the anti-fogging layer is preferably formed from a resin composition containing an anti-fogging agent and a binder component. The binder component is not particularly limited, but is preferably an acrylic adhesive, and from the viewpoint of transparency, moldability, and stickiness of the anti-fogging layer, is more preferably a hydrophilic acrylic resin. The hydrophilic acrylic resin is not particularly limited, but a copolymer such as polyacrylic acid ester can be adopted. Here, examples of the acrylic acid ester constituting the polyacrylic acid ester include methyl ester, ethyl ester, butyl ester, octyl ester, and 2-ethylhexyl ester of acrylic acid. And, as the polyacrylic acid ester, a copolymer obtained by copolymerizing these acrylic acid esters with at least one monomer selected from the group consisting of, for example, methacrylic acid ester, styrene, acrylonitrile, vinyl chloride, and vinyl acetate can be adopted. Also, as the polyacrylic acid ester, a copolymer obtained by copolymerizing these acrylic acid esters with at least one functional monomer selected from the group consisting of, for example, acrylic acid, acrylamide, methylol acrylamide, and hydroxydialkyl methacrylate can be adopted.

[0038] The laminate sheet used in the packaging material may have a plurality of base layers 2. For example, as shown in Fig. 2, the laminate sheet 1A may be formed by laminating a first base layer 2A, a barrier layer 3, and a second base layer 2B in this order. When the laminate sheet used in the packaging material has a plurality of base layers 2, the propylene-based resins in the plurality of base layers 2 may be the same or different from each other. Also, for example, the laminate sheet may have other layers between the first base layer and the barrier layer, and between the barrier layer and the second base layer, respectively. For example, as shown in Fig. 3, the laminate sheet 1B may have a first base layer 2A, a first adhesive layer 4A, a barrier layer 3, a second adhesive layer 4B, and a second base layer 2B laminated in this order. In these laminate sheets 1A and 1B, the first base layer 2A and the second base layer 2B correspond to the above-mentioned base layer 2. The laminate sheet used for the packaging body preferably has a structure in which the barrier layer is sandwiched between multiple base layers, such as laminate sheet 1A or laminate sheet 1B, by having a first base layer 2A on one side of the barrier layer 3 and a second base layer 2B on the other side of the barrier layer 3. By having the barrier layer sandwiched between multiple base layers in the laminate sheet, it is easier to prevent the oxygen barrier function of the barrier layer from being deteriorated by water vapor, and as a result, the oxygen barrier property of the packaging body obtained by thermoforming the laminate sheet is even more excellent.

[0039] [Laminated sheet manufacturing] The laminate sheet 1 according to this embodiment can be manufactured, for example, by the method described in Example 1. Alternatively, the barrier layer 3 may be formed by, for example, manufacturing the base layer 2 by the manufacturing apparatus described in Example 1, and then coating the base layer 2 with the material for the barrier layer 3.

[0040] [container] FIG. 4 is a cross-sectional view showing the container of this embodiment. As shown in Fig. 4, the container 50 of this embodiment is composed of a container body 30 and a lid 40. In the container 50 of this embodiment, the lid 40 uses a package obtained by forming the above-mentioned laminated sheet 1, specifically by heating. In the package obtained by thermoforming the laminated sheet 1, the base layer 2 and the barrier layer 3 are not separated from each other and are used as elements constituting the package. The container described in this embodiment may be appropriately selected from a variety of containers, such as a container that is opened by interlayer peeling with a notch, a container that is opened by cohesive peeling without a notch, and the like.

[0041] [Container body configuration] As shown in FIG. 4, the container body 30 is composed of a base layer 31 and a surface layer 32. The base layer 31 of the container body 30 is not particularly limited as long as it is basically a thermoformable material. Examples of the material include polypropylene, polystyrene, polyamide, polyethylene terephthalate, polycarbonate, and polyethylene naphthalate. These materials may be used alone or in combination. Polypropylene is preferably used. Examples of polypropylene include homopolypropylene, block copolymers or random copolymers of propylene and ethylene, and block copolymers or random copolymers of propylene, ethylene, and butene. Additionally, polymer alloys such as polypropylene and polystyrene, and rubber-modified polystyrene, can be used to improve stiffness and moldability. Furthermore, the base material layer 31 of the container body 30 may contain various additives in the resin, for example, inorganic filler to improve rigidity.

[0042] Furthermore, the base layer 31 of the container body 30 may be configured not only from a single layer, but also by laminating a plurality of layers, as necessary. For example, it may include an adhesive resin layer or the like. The surface layer 32 of the container body 30 is preferably made of a polypropylene resin or a polyethylene resin in consideration of oil resistance, chemical resistance, and heat resistance. The container body 30 is obtained by forming a resin sheet composed of a base layer 31 and a surface layer 32 into a desired shape having a flange 30a shown in Fig. 4. Examples of the forming method include vacuum forming and pressure forming.

[0043] [Lid configuration] As shown in FIG. 4, the lid 40 is composed of a base layer 41 and a barrier layer 42. The lid body 40 is formed using the laminate sheet 1 of the present embodiment. Therefore, the base material layer 41 of the lid body 40 is composed of the base material layer 2 of the laminate sheet 1 described above, and the barrier layer 42 of the lid body 40 is composed of the barrier layer 3 of the laminate sheet 1 described above. The lid 40 is obtained by forming the laminated sheet 1 of this embodiment into a desired shape having a flange 40a shown in FIG. 4. Examples of forming methods include vacuum forming and compressed air forming. In this case, the lid 40 is thermoformed at a temperature below the melting point of the propylene-based resin in the base layer 2 of the laminated sheet 1. By thermoforming the lid 40 at a temperature below the melting point of the propylene-based resin, a fine crystal structure is maintained, resulting in a highly transparent lid. Patent Document 1, which relates to a method for manufacturing a decorated molded body, does not describe the thermoforming of the laminated sheet at a temperature below the melting point of the propylene-based resin in the base layer to obtain a package in order to maintain high transparency. The melting point of the propylene-based resin in the base layer of the laminate sheet can be measured by differential scanning calorimetry (DSC). The lid 40 in this embodiment is formed using the laminate sheet 1 of this embodiment, and therefore has excellent barrier properties. In addition, it has good transparency and also has excellent performance in various physical properties such as cold impact resistance, heat resistance, and rigidity.

[0044] [Method of sealing the container body and the lid] When sealing the container body 30 and the lid body 40 together, the flange 30a of the container body 30 and the flange 40a of the lid body 40 are overlapped, and the overlapped flanges 30a, 40a are heat-sealed from the lid body side with a seal bar to tightly seal them together. The sealing temperature is preferably 170° C. or higher and 220° C. or lower, and more preferably 180° C. or higher and 200° C. or lower. If the sealing temperature is 170° C. or higher, the sealing time can be shortened and productivity can be improved. Also, if the sealing temperature is 220° C. or lower, there is no risk of the base layer melting and causing edge cuts. The sealing pressure is preferably 1 MPa or more and 5 MPa or less, and the sealing time is preferably 0.5 seconds or more and 5 seconds or less, and more preferably 2 MPa or more and 4 MPa or less, and the sealing time is more preferably 1 second or more and 3 seconds or less. If the sealing pressure is 1 MPa or more, sufficient sealing strength can be obtained. Also, if the sealing pressure is 5 MPa or less, there is no risk of edge cutting. By carrying out heat sealing under the above heat sealing conditions, a container having high sealability can be obtained.

[0045] From the viewpoint of improving transparency, the internal haze of the lid body 40 as the packaging body of the container 50 is preferably 15% or less. It is also preferable that the ratio of the internal haze of the lid body 40 as the packaging body to the internal haze of the laminated sheet 1 before thermoforming (the ratio of the internal haze of the packaging body (lid body 40) to the internal haze of the laminated sheet 1 before thermoforming) is 1 or less. It is more preferable that the container 50 has an internal haze of the lid body 40 as a packaging body of 15% or less, and a ratio of the internal haze of the lid body 40 as a packaging body / the internal haze of the laminated sheet before thermoforming of 1 or less. If the internal haze of the lid body 40 as a packaging body is 15% or less, and the ratio of the internal haze of the lid body 40 as a packaging body / the internal haze of the laminated sheet before thermoforming of 1 or less, the container 50 becomes a container with higher transparency. The internal haze is the haze of the resin itself measured excluding the influence of the surface roughness of the sheet, etc. The internal haze can be measured by a haze meter NDH2000 (manufactured by Nippon Denshoku Industries Co., Ltd.) in accordance with JIS-K-7136.

[0046] The container 50 is used for food applications, for example, by filling the interior thereof with food products, seasonings, food ingredients, beverages, etc., for secondary packaging of medicines, and for daily necessities. Furthermore, the container 50 can be used to fill various packaged items, such as not only solids but also liquids and mixtures thereof.

[0047] [Effects of this embodiment] The container 50 according to this embodiment includes, as a packaging material, a lid 40 formed by thermoforming a laminated sheet formed by stacking at least two layers, a base layer 41 and a barrier layer 42. The base layer 41 contains a propylene-based resin containing smectite crystals, and the lid 40 is thermoformed at a temperature equal to or lower than the melting point of the propylene-based resin. This results in the container 50 having both excellent barrier properties and high transparency.

[0048] [Variations] Although the best configuration for carrying out the present invention has been disclosed in the above description, the present invention is not limited thereto. That is, the present invention has been mainly described with reference to specific embodiments, but those skilled in the art can make various modifications to the above-described embodiments in terms of materials, quantities, and other detailed configurations without departing from the scope of the technical idea and purpose of the present invention. Therefore, the descriptions limiting the materials, layer structures, etc. disclosed above are merely illustrative for the purpose of facilitating understanding of the present invention, and do not limit the present invention. For this reason, descriptions in which some or all of the limitations on the materials, etc. are removed are included in the present invention.

[0049] For example, in the above embodiment, the container 50 in which the packaging body is the lid body 40 is exemplified, but the packaging body in the container may be the container body or the like. In the above embodiment, the container 50 having the lid 40 as a package formed by heating the laminated sheet 1 has been described as an example, but the present invention is not limited to such an embodiment. For example, the container body may be a package formed by heating the laminated sheet 1. In this case, both the lid and the container body may be a combination of packages formed by heating the laminated sheet 1, or the container body may be a package formed by heating the laminated sheet 1, and the lid may be a general-purpose film.

[0050] The container 50 may be circular, rectangular, elliptical, or of any other suitable shape. Furthermore, the lid 40 is exemplified as being dome-shaped, but may be in the form of a flat sheet.

[0051] The method for joining the container body 30 and the lid 40 is not limited to heat sealing, and various joining methods can be used, such as ultrasonic welding, adhesion using an adhesive, etc. Furthermore, the configuration for opening the container body 30 and the lid body 40 may be either an interlayer peeling opening or a cohesive peeling opening. Furthermore, the heat sealing of the flange 30a of the container body 30 and the flange 40a of the lid body 40 is not limited to forming a ring-shaped heat seal portion along the outer peripheral edge to provide airtightness, but may also be performed by partial heat sealing so that the heat seal portions are scattered in the outer circumferential direction.

[0052] Furthermore, the laminated sheet forming the lid 40 has been described as having a two-layer structure of the base material layer 41 and the barrier layer 42, but the base material layer 41 may be a sheet having a multi-layer structure of two or more layers. The laminated sheet forming the lid 40 may be a sheet having a multi-layer structure of three or more layers, which has another layer between the base layer 41 and the barrier layer 42. Examples of the other layer include an adhesive layer. The laminated sheet forming the lid 40 may be a sheet in which a first base material layer, a barrier layer, and a second base material layer are laminated in this order. Furthermore, the container body 30 may also have a multi-layer structure of three or more layers.

[0053] Furthermore, in addition to the container 50 configured by the container body 30 and the lid body 40, a configuration in which a joined portion is interposed between the container body 30 and the lid body 40 may also be used. EXAMPLES

[0054] EXAMPLES Hereinafter, examples of the present invention will be described, but the present invention is not limited to these examples.

[0055] Example 1 [Laminated sheet manufacturing] Using the manufacturing apparatus 10 shown in FIG. 5, a laminated sheet 1B was manufactured as follows. The following three types of molten resins (resins obtained by melting the resin for the base material layer, the resin for the barrier layer, and the resin for the adhesive layer) were co-extruded from a T-die 11 of an extruder as a sheet-like material 1a, and the sheet-like material 1a was sandwiched between a metallic endless belt 25 and a fourth cooling roll 22 on a first cooling roll 21. In this state, the sheet-like material 1a was pressed against the first cooling roll 21 and the fourth cooling roll 22 at a circular arc portion corresponding to the central angle θ1 of the first cooling roll 21, and was rapidly cooled. Next, the sheet-like material 1a was sandwiched between the metallic endless belt 25 and the fourth cooling roll 22 in a circular arc portion corresponding to approximately the lower half of the fourth cooling roll 22 and pressed together, and the sheet-like material 1a was further quenched by spraying cooling water onto the back side of the metallic endless belt 25 using a cooling water spray nozzle 26. The sprayed cooling water was collected in a water tank 27 and the collected water was discharged through a drainage groove 27a. After being planarly pressed and cooled by the fourth cooling roll 22, the sheet-like material 1a in close contact with the metallic endless belt 25 was moved onto the second cooling roll 23 with the rotation of the metallic endless belt 25. Here, the sheet-like material 1a, which was guided by the peeling roll 29 and pressed toward the second cooling roll 23, was planarly pressed by the metallic endless belt 25 at a circular arc portion corresponding to approximately the upper half of the second cooling roll 23, as described above, and was cooled again. Note that water adhering to the back surface of the metallic endless belt 25 was removed by the water absorbing roll 28 provided midway from the fourth cooling roll 22 to the second cooling roll 23. The sheet-like material 1 a (laminate sheet 1 B) cooled on the second cooling roll 23 was then peeled off from the metallic endless belt 25 by a peeling roll 29 . The surface of the first cooling roll 21 is covered with an elastic material 21a made of nitrile-butadiene rubber (NBR). The surface of the second cooling roll 23 is also covered with an elastic material (not shown) made of nitrile-butadiene rubber (NBR). In addition, the temperature of the metallic endless belt 25 can be adjusted by a cooling means (not shown) such as a water-cooling type built into the third cooling roll 24 or the like.

[0056] The manufacturing conditions for the laminated sheet 1B are as follows. Base layer resin: Homopolypropylene F-300SP (Prime Polymer Co., Ltd.) (melting point: 160°C, isotactic pentad fraction: [mmmm] = 94%) Barrier layer resin: Ethylene-vinyl alcohol copolymer resin G-Soarnol (Mitsubishi Chemical Co., Ltd.) Adhesive layer resin: Modic P674V (manufactured by Mitsubishi Chemical Corporation) Extruder diameter: 150mm T-die 11 width (die edge size): 1400mm Thickness of laminated sheet 1B: 0.3mm - Laminated sheet 1B take-up speed: 25m / min Surface temperature of the fourth cooling roll 22 and the metal endless belt 25: 17°C ·Cooling rate: 10,800℃ / min (180℃ / sec) Nucleating agent: None

[0057] In the obtained laminate sheet 1B, the thickness T of the base layer relative to the thickness T of the entire laminate sheet 1B is B1 The ratio of [(T B1 / T)×100] was 92%. B2 The ratio of [(T B2 / T) × 100] was 4%. Furthermore, the obtained laminated sheet 1B was a five-layer sheet having a first base material layer, a first adhesive layer, a barrier layer, a second adhesive layer, and a second base material layer laminated in this order.

[0058] (Melting Point) The melting point of the resin (polypropylene) of the base material layer was measured as follows. Using a differential scanning calorimeter (DSC) (Diamond DSC, manufactured by PerkinElmer Japan Co., Ltd.), the polypropylene was heated from 50° C. to 200° C. at 10° C. / min, held at 220° C. for 5 minutes, and cooled from 220° C. to 50° C. at 10° C. / min. The temperature showing the maximum value of the endothermic peak obtained at this time was taken as the melting point of the polypropylene.

[0059] (crystallization rate) The crystallization rate of the polypropylene used in the base layer was measured using a differential scanning calorimeter (DSC) (Diamond DSC manufactured by PerkinElmer Japan Co., Ltd.). Specifically, the polypropylene was heated from 50°C to 230°C at 10°C / min, held at 230°C for 5 minutes, cooled from 230°C to 130°C at 80°C / min, and then held at 130°C for crystallization. Measurement of the change in heat quantity was started when the temperature reached 130°C, and a DSC curve was obtained. The crystallization rate was calculated from the obtained DSC curve by the following steps (i) to (iv). (i) The baseline was determined by approximating the change in heat quantity from a point 10 times the time from the start of measurement to the peak top to a point 20 times the time by a straight line. (ii) The intersection points between the tangent line having a slope at the inflection point of the peak and the baseline were determined to determine the start and end times of crystallization. (iii) The time from the obtained crystallization start time to the peak top was measured as the crystallization time. (iv) The crystallization rate was calculated from the reciprocal of the obtained crystallization time. The crystallization rate of the polypropylene used in the base layer is 0.9 min -1 It was.

[0060] [Container molding] The laminate sheet 1B produced as described above was heated by an infrared heater to a temperature below the melting point of the resin of the base layer, and then pressed against a mold using vacuum and compressed air to cool, thereby forming a cup container with a diameter of 95 mm.

[0061] Comparative Example 1 A container was formed using the same materials and method as in Example 1, except that a laminated sheet 71 was produced under the following production conditions using the production apparatus shown in FIG. In this production apparatus, molten resins co-extruded from a T-die 72 of an extruder were brought into close contact with a cooling roll 76 by an air knife 74 and cooled by cooling rolls 76 and 78 to produce a laminated sheet 71 . [Manufacturing conditions] Extruder diameter: 30mm Width of T-die 72: 350mm Take-up speed of laminated sheet 71: 2.1 m / min Surface temperature of cooling rolls 76 and 78: 30℃

[0062] (Water vapor barrier evaluation) The molded cup container with a diameter of 95 mm was filled with 80 g of water, sealed, and stored under dry conditions at 40°C. The moisture loss mass (%) was measured after 1 day, 4 days, and 6 days of storage. The moisture mass in the cup container immediately after filling and sealing was 80 g, and the moisture mass in the cup container measured after 1 day, 4 days, and 6 days of storage was taken as Wx (unit: g), and the moisture loss mass (%) was calculated by the formula moisture loss mass (%) = {(80-Wx) / 80} x 100. The results are shown in Table 1.

[0063] (Oxygen barrier evaluation) The molded cup container with a diameter of 95 mm was filled with nitrogen and sealed, and retorted at 120°C for 30 minutes. The oxygen concentration (%) inside the cup container was measured 2 and 4 hours after retort treatment. The oxygen concentration inside the cup container was measured using a non-destructive oxygen concentration meter manufactured by PreSens, measuring the oxygen sensor chip attached to the barrier film when the cup container sample was made from outside the cup container in a non-destructive state. The results are shown in Table 2.

[0064] (Internal Haze Rating) The internal haze of the laminated sheet and the cup container was measured using a haze meter (NDH-2000, manufactured by Nippon Denshoku Industries Co., Ltd.). The internal haze of the laminated sheet was measured with a haze meter after applying silicone oil to both sides of the sheet and then sandwiching the sheet between glass plates to eliminate the influence of the outside of the sheet. The internal haze of a cup container was measured with a haze meter after applying silicone oil to both sides (inside and outside) of the bottom of the container and then sandwiching the bottom of the container between glass plates to eliminate the influence of the outside of the container. The results are shown in Table 3.

[0065] [Table 1]

[0066] [Table 2]

[0067] [Table 3]

[0068] From the results shown in Table 1, it can be seen that the cup container of Example 1 is a cup container superior in water vapor barrier property compared to the cup container of Comparative Example 1. Furthermore, the cup container of Example 1 has superior water vapor barrier properties compared to the cup container of Comparative Example 1, and therefore can suppress temporary deterioration of barrier properties due to moisture absorption by EVOH when heat sterilization such as retort treatment is performed. Therefore, the results shown in Table 2 show that the cup container also has superior oxygen barrier properties when used for heat sterilization. Furthermore, it can be seen from the results shown in Table 3 that the laminate sheet and cup container of Example 1 are superior in transparency to the laminate sheet and cup container of Comparative Example 1. The laminate sheet according to Example 1 includes a base layer and a barrier layer manufactured under the above-mentioned manufacturing conditions and using the above-mentioned materials, and the barrier layer is formed of an ethylene-vinyl alcohol copolymer resin. The base layer has excellent water vapor barrier properties, and the barrier layer formed of an ethylene-vinyl alcohol copolymer resin has excellent oxygen barrier properties. Therefore, it can be said that the cup container as a package thermoformed using the laminate sheet has both excellent water vapor barrier properties and oxygen barrier properties. Furthermore, by thermoforming the laminate sheet according to Example 1 at a temperature equal to or lower than the melting point of the polypropylene resin of the base layer, a cup container having excellent transparency could be obtained.

[0069] Although the embodiment of the present invention has been described in detail above with reference to the accompanying drawings, the present invention is not limited to such examples. It is clear that a person having ordinary knowledge in the technical field to which the present invention pertains can conceive of various modified or amended examples within the scope of the technical ideas described in the claims, and it is understood that these also naturally belong to the technical scope of the present invention. [Explanation of symbols]

[0070] 1, 1A, 1B... laminated sheet, 1a... sheet-like material, 2, 41... base layer, 2A... first base layer, 2B... second base layer, 3, 42... barrier layer, 4A... first adhesive layer, 4B... second adhesive layer, 10... manufacturing apparatus, 11... T-die, 21... first cooling roll, 21a... elastic material, 22... fourth cooling roll, 23... second cooling roll, 24... third cooling roll, 25... metal endless belt, 26... cooling water spray nozzle, 27... water tank, 27a... drainage groove, 28... water absorption roll, 29... peeling roll, 30... container body, 30a, 40a... flange, 31... base layer, 32... surface layer, 40... lid, 50... container, θ1... central angle.

Claims

1. A substrate layer containing a propylene-based resin containing smectic crystals having an isotactic pentad fraction of 85 mol % or more and 99 mol % or less; and Barrier Layer At least two layers of the above are laminated, The propylene-based resin and the resin that forms the barrier layer are co-extruded into a sheet, and the sheet is pressed between one cooling roll and another cooling roll to obtain a laminated sheet, which is then thermoformed at a temperature equal to or lower than the melting point of the propylene-based resin.

2. The internal haze of the package is 15 percent or less, and the ratio of the internal haze of the package to the internal haze of the laminate sheet before thermoforming is 1 or less. The package of claim 1.

3. The pressing is performed by sandwiching the sheet-like material co-extruded into a sheet between a metal belt and the first cooling roll. The package according to claim 1 or 2.

4. The crystallization rate of the propylene-based resin at 130° C. is 2.5 min -1 Below is the The packaging body according to any one of claims 1 to 3.

5. The propylene-based resin has an exothermic peak of 1.0 J / g or more on the low-temperature side of a maximum endothermic peak in a differential scanning calorimetry curve. The packaging body according to any one of claims 1 to 4.

6. The substrate layer does not contain a nucleating agent. The packaging body according to any one of claims 1 to 5.

7. The thickness of the laminated sheet is 0.2 mm or more and 1.2 mm or less. The packaging body according to any one of claims 1 to 6.

8. the barrier layer contains at least one resin selected from the group consisting of an ethylene-vinyl alcohol copolymer resin, a polyvinylidene chloride resin, and a polyacrylonitrile resin; A package according to any one of claims 1 to 7.

9. The internal haze of the package is 5 percent or less. A package according to any one of claims 1 to 8.

10. The isotactic pentad fraction is 94 mol% or more and 99 mol% or less. A package according to any one of claims 1 to 9.

11. The laminate sheet has a plurality of base layers containing the propylene-based resin. A package according to any one of claims 1 to 10.

12. The laminate sheet includes a first base material layer and a second base material layer as the plurality of base material layers, a first base material layer on one surface side of the barrier layer, a second base material layer on the other surface side of the barrier layer, and a structure in which the barrier layer is sandwiched between the plurality of base material layers; The package of claim 11.

13. The laminate sheet is obtained by co-extruding the propylene-based resin contained in the first base material layer, a resin forming the barrier layer, and the propylene-based resin contained in the second base material layer into a sheet, and pressing the sheet with the first cooling roll and another cooling roll different from the first cooling roll. The package of claim 12.

14. The laminate sheet includes the first base material layer, the second base material layer, the barrier layer, a first adhesive layer, and a second adhesive layer, the first base material layer, the first adhesive layer, the barrier layer, the second adhesive layer, and the second base material layer are laminated in this order; The package according to claim 12 or 13.

15. The temperature of the first cooling roll is less than 30° C. A package according to any one of claims 1 to 14.

16. The packaging body according to any one of claims 1 to 15, which is used for packaging food products.

17. a step of pressing a sheet-like product obtained by co-extruding a propylene-based resin and a resin for a barrier layer into a sheet shape between one cooling roll and another cooling roll different from the one cooling roll; A step of thermoforming a laminate sheet obtained by laminating at least two layers, a substrate layer containing the propylene-based resin containing smectic crystals having an isotactic pentad fraction of 85 mol% to 99 mol%, and the barrier layer, at a temperature equal to or lower than the melting point of the propylene-based resin containing smectic crystals. A method for producing a package, comprising:

18. The pressing step is performed by sandwiching the sheet-like material between a metal belt and the first cooling roll. A method for producing the package according to claim 17.

19. The surface temperature of the first cooling roll is less than 30° C. A method for producing the package according to claim 17 or 18.

Citation Information

Patent Citations

  • Polypropylene sheet and manufacture thereof

    JP1986130018A

  • Polypropylene group laminated sheet

    JP1986144345A

  • Laminated oriented polyolefin film

    JP1998016153A

  • Polypropylene sheet for packaging medicine

    JP1999172059A

  • Molded object obtained from antifogging polyolefin sheet and molded object for food packaging