Conductive member, process cartridge and electrophotographic image forming apparatus

The conductive member with a matrix-domain structure and insulating resin particles addresses uneven charge distribution and electric field concentration, enhancing image quality and longevity in electrophotographic image forming apparatuses.

JP7558737B2Active Publication Date: 2024-10-01CANON KK
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2020163791
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-09-29
Publication Date
2024-10-01
Estimated Expiration
2040-09-29

AI Technical Summary

Technical Problem

Existing conductive members in electrophotographic image forming apparatuses experience issues with fogging and toner adhesion due to uneven charge distribution and electric field concentration, particularly when high voltages are applied, leading to reduced image quality and longevity.

Method used

A conductive member with a matrix-domain structure, where the domains are crosslinked rubber and conductive particles, are designed to have a specific shape and distribution to minimize electric field concentration and promote uniform charge transfer, incorporating insulating resin particles to prevent toner adhesion.

Benefits of technology

The solution effectively suppresses fogging and toner adhesion, ensuring high-quality and long-lasting electrophotographic images by maintaining uniform charge distribution and preventing electric field concentration, even under high voltage conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007558737000019
    Figure 0007558737000019
  • Figure 0007558737000020
    Figure 0007558737000020
  • Figure 0007558737000021
    Figure 0007558737000021
Patent Text Reader

Abstract

To provide a conductive member CM that can prevent fogging.SOLUTION: A CM comprises: a conductive support; and a conductive layer CL that has a matrix Mt including a cross-linked product of first rubber and a plurality of domains Dm in the Mt. The Dm includes a cross-linked product of second rubber and conductive particles, and some of the Dm are exposed to an outer surface of the CM to cause first convex parts. The outer surface of the CM is composed of the Mt and the exposed Dm. The CL further includes insulating resin particles IP, and some of the IP causes second convex parts on the outer surface of the CM. When the length of the longitudinal direction of the CL is L and the thickness of the CL is T, and for cross-sections in the thickness direction at three points including the center in the longitudinal direction of the CL and L / 4 directed from both ends to the center, when nine observation areas with 20-μm sides are placed at arbitrary three points in the thickness direction at a depth of 0.1-0.9 T, 80% by number or more of the Dm in the observation areas satisfy the following requirements. 1: the cross-sectional ratio of the conductive particles included in the Dm to the cross-section of the Dm is 20% or more. 2: when the peripheral length of the Dm is A and the envelope peripheral length of the Dm is B, A / B is 1.00-1.10.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure is directed to an electro-conductive member for electrophotography, a process cartridge, and an electrophotographic image forming apparatus. [Background technology]

[0002] In an image forming apparatus that employs an electrophotographic method (hereinafter referred to as an electrophotographic image forming apparatus), conductive members such as a charging member, a transfer member, a developing member, etc. The conductive member is composed of a conductive layer coated on the outer peripheral surface of a conductive support, and plays a role of transporting electric charge from the conductive support to the conductive member surface and imparting electric charge to a contacting object by discharging, etc. For example, the charging member is a member that generates a discharge between itself and the photoconductor to charge the surface of the photoconductor, while the transfer member is a member that transfers the developer from the photoconductor to a print medium or an intermediate transfer member, and at the same time generates a discharge to stabilize the developer after transfer. In response to the recent demand for high image quality of electrophotographic image forming apparatuses, it has been considered to increase the voltage applied to the conductive member in order to achieve high contrast. Under such high voltage application conditions, these conductive members are required to be more uniformly charged against contact objects such as photoconductors, intermediate transfer bodies, and print media. In addition, there is a demand for electrophotographic image forming apparatuses that are equipped with an energy-saving system that brings cleaning members such as cleaning blades into contact with light pressure, and a resource-saving simultaneous development and cleaning system that does not have a waste toner box, and that can output high-quality images for a long period of time. These systems are systems in which more residual toner than before enters the charging member, and they require a charging member that can maintain uniform charging without deterioration even when used for a long period of time exceeding several hundred thousand sheets.

[0003] Patent Document 1 describes a rubber composition having an island structure including a polymer continuous phase made of an ionically conductive rubber material and a polymer particle phase made of an electronically conductive rubber material, and the ionically conductive rubber material has a volume resistivity of 1×10 12The document discloses an electroconductive member that is mainly made of raw rubber A with a resistance of Ω·cm or less, and that the electronically conductive rubber material is made conductive by blending conductive particles into raw rubber B. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2002-3651 A [Patent Document 2] WO2019 / 203225 Summary of the Invention [Problem to be solved by the invention]

[0005] One aspect of the present disclosure is to provide a conductive member for electrophotography that can stably suppress the occurrence of "fogging" on an electrophotographic image for a long period of time. Another aspect of the present disclosure is directed to providing a process cartridge that contributes to stable formation of high-quality, long-life electrophotographic images. Still another aspect of the present disclosure is directed to providing an electrophotographic image forming apparatus that can stably form high-quality electrophotographic images over a long period of time. [Means for solving the problem]

[0006] According to one aspect of the present disclosure, A conductive layer provided on the outer surface of the support; A conductive member for electrophotography, comprising: the conductive member is in the form of a roller; the conductive layer has a matrix containing a crosslinked product of a first rubber and a plurality of domains dispersed in the matrix, The domain comprises a crosslinked product of a second rubber and a conductive particle, at least a portion of the domain is exposed on an outer surface of the conductive member to form a first protrusion on the outer surface of the conductive member; the outer surface of the conductive member is composed of the matrix and the domain exposed on the outer surface of the conductive member; the conductive layer further contains insulating resin particles, at least a portion of the resin particles cause second protrusions on an outer surface of the conductive member; When the conductive member is pressed against a transparent flat plate with a load of 500 g applied to the transparent flat plate, the second protrusion and the second protrusion are formed in the nip between the conductive member and the transparent flat plate. The transparent flat plate The spatial distance formed by contact with d is 3 μm or more and 30 μm or less, and there is no contact point between the first convex portion and the transparent flat plate within the nip, The transparent flat plate is a glass plate having a size of 20 mm square and a thickness of 2 mm. The distance d is determined by performing a scan measurement in the height direction of the nip and measuring the spatial volume V1 [μm] of the space formed between the conductive member and the glass surface of the transparent flat plate in an area of ​​the nip width L [μm] × the longitudinal direction A [μm] in the measurement range. 3 ] is calculated using the formula: d = V1 / (L × A), Directly on the outer surface of the conductive member , 1.5cm wide Platinum electrode In the circumferential direction of the conductive member When an AC voltage having an amplitude of 1 V and a frequency of 1.0 Hz was applied between the outer surface of the support and the platinum electrode in an environment of a temperature of 23° C. and a relative humidity of 50%, the impedance was 1.0×10 3 Ω or more 1.0×10 8 Ω or less 、 When the length of the conductive layer in the longitudinal direction is L and the thickness of the conductive layer is T, and observation regions of 20 μm square are placed at any three locations in a thickness region from the outer surface of the conductive layer to a depth of 0.1T to 0.9T on each of a cross section of the conductive layer in the thickness direction at three locations, namely, the center of the conductive layer in the longitudinal direction and L / 4 from both ends of the conductive layer toward the center, 80% or more by number of domains observed in each of all nine observation regions satisfy the following requirement (B1) and requirement (B2): 、 A conductive member characterized in that: Requirement (B1) The ratio of the cross-sectional area of ​​the conductive particles contained in a domain to the cross-sectional area of ​​the domain is 20% or more; Requirement (B2) When the perimeter of a domain is A and the envelope perimeter of the domain is B, A / B is 1.00 or more and 1.10 or less.

[0007] According to another aspect of the present disclosure, there is provided a process cartridge configured to be detachably mountable to a main body of an electrophotographic image forming apparatus, the process cartridge including the above-mentioned conductive member. According to yet another aspect of the present disclosure, there is provided an electrophotographic image forming apparatus comprising the above-described conductive member. Effect of the Invention

[0008] According to one embodiment of the present disclosure, it is possible to obtain a conductive member for electrophotography that can be used as a charging member capable of suppressing fogging even when used for a long period of time by increasing the charging bias. According to another aspect of the present disclosure, a process cartridge that contributes to the formation of high-quality, long-life electrophotographic images can be obtained. Furthermore, according to another aspect of the present disclosure, it is possible to obtain an electrophotographic image forming apparatus capable of forming high-quality electrophotographic images for a long period of time. [Brief description of the drawings]

[0009] [Figure 1] 1 is a cross-sectional view of a conductive member according to an embodiment of the present disclosure, taken in a direction perpendicular to the longitudinal direction. [Diagram 2] 1A and 1B are cross-sectional views perpendicular to the longitudinal direction of a conductive layer of a conductive member according to one embodiment of the present disclosure, where (a) shows a matrix-domain structure and a first protrusion, and (b) shows a second protrusion. [Diagram 3] FIG. 4 is an explanatory diagram of impedance measurement of a conductive layer of a conductive member. [Figure 4] FIG. 2 is a conceptual diagram illustrating the maximum Feret diameter of a domain according to the present disclosure. [Diagram 5] FIG. 2 is a conceptual diagram illustrating the envelope perimeter of a domain according to the present disclosure. [Figure 6] FIG. 1 is a conceptual diagram of a slice for measuring domain shape according to the present disclosure. [Figure 7] FIG. 2 is a cross-sectional view of a process cartridge according to an embodiment of the present disclosure. [Figure 8]1 is a cross-sectional view of an electrophotographic image forming apparatus according to one aspect of the present disclosure. [Figure 9] 1A is a schematic diagram of an apparatus for alternatively measuring the distance at a nip portion between a conductive member and a photoreceptor, and FIG. 1B is an enlarged view of the nip portion. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The present inventors attempted to obtain an electrophotographic image with higher contrast when forming an electrophotographic image using the charging member according to Patent Document 1. Specifically, the charging bias between the charging member and the electrophotographic photosensitive member was increased to a higher voltage (for example, -1500V or higher) than a general charging bias (for example, -1000V). As a result, for example, the reverse toner was developed even in the solid white portion on the photosensitive drum where the toner was not originally developed, and an image with so-called "fog" was formed. In addition, so-called transfer residual toner was attached to the surface of the charging member, and the charging performance was changed over time. The present inventors have studied the reason why the charging member according to Patent Document 1 causes fog on an electrophotographic image when the charging bias is increased. In the process, they focused on the role of the polymer particle phase made of an electronically conductive rubber material in the charging member according to Patent Document 1. That is, it is considered that the polymer particle phase imparts electronic conductivity to the elastic layer by transferring electrons between the polymer continuous phases present in the vicinity in the elastic layer. Then, they speculated that the occurrence of fog when the charging bias is increased is due to electric field concentration. Electric field concentration is a phenomenon in which current is concentrated at a specific location when electricity is applied.

[0011] That is, according to the observations of the present inventors, the polymer particle phase according to Patent Document 1 had an irregular shape and had unevenness on the outer surface. Between such polymer particle phases, the transfer of electrons is concentrated at the convex parts of the polymer particle phase, and the current flow from the vicinity of the conductive support to which the charging bias of the charging member is applied to the outer surface of the charging member becomes uneven. Therefore, the discharge from the outer surface of the charging member to the electrophotographic photosensitive member, which is the member to be charged, becomes uneven, and the surface potential of the electrophotographic photosensitive member also becomes uneven. As a result, it was presumed that fogging occurs in the electrophotographic image. Therefore, the present inventors have recognized that eliminating the concentration points of electron exchange between polymer particle phases when the charging bias is increased is effective in improving fogging of electrophotographic images. Based on this recognition, and as a result of extensive investigations, it was found that a conductive member having a support having a conductive outer surface and a conductive layer provided on the outer surface of the support and satisfying the following requirements (A) and (B) can effectively suppress fogging of an electrophotographic image even when a high charging bias is applied (Patent Document 2).

[0012] Requirement(A): The conductive layer has a matrix containing a cross-linked product of the first rubber and a plurality of domains (sea-island structure) dispersed in the matrix, the domains containing a cross-linked product of the second rubber and conductive particles.Furthermore, when a platinum electrode is directly provided on the outer surface of the conductive member and an AC voltage with an amplitude of 1 V and a frequency of 1.0 Hz is applied between the outer surface of the support and the platinum electrode in an environment of a temperature of 23°C and a relative humidity of 50%, the impedance is within the following range. 1.0×10 3 Ω or more 1.0×10 8 Ω or less.

[0013] Requirement (B): The length of the conductive layer in the longitudinal direction is L, and the thickness of the conductive layer is T. For each of the cross sections of the conductive layer in the thickness direction at the longitudinal center of the conductive layer and at three locations of L / 4 from both ends of the conductive layer toward the center, observation regions of 20 μm square are placed at any three locations in a thickness region from the outer surface of the elastic layer to a depth of 0.1T to 0.9T. At that time, 80% or more by number of the domains observed in each of all nine observation regions satisfy the following requirement (B1) and requirement (B2): Requirement (B1) The ratio of the cross-sectional area of ​​the conductive particles contained in a domain to the cross-sectional area of ​​the domain is 20% or more; Requirement (B2) When the perimeter of a domain is A and the envelope perimeter of the domain is B, A / B is 1.00 or more and 1.10 or less.

[0014] Each requirement is explained below. Regarding requirement (A): Requirement (A) expresses the degree of conductivity of the conductive layer. The conductivity of the conductive member is determined by the impedance at 1 Hz being 10 3 Ω or more 10 8 The impedance is within 10 3 By setting the impedance at 10 Ω or more, it is possible to suppress an excessive increase in the discharge current amount, and as a result, it is possible to prevent the occurrence of potential unevenness caused by abnormal discharge. 8 By setting the resistance to Ω or less, it is possible to suppress insufficient charging due to an insufficient total amount of discharged charge.

[0015] The impedance required for requirement (A) can be measured by the following method: In order to eliminate the influence of contact resistance between the charged member and the measurement electrode when measuring impedance, it is preferable to form a thin platinum film on the outer surface of the charged member, use the thin film as an electrode, and measure the impedance via two terminals, with the conductive support as a ground electrode. Examples of the method for forming the thin film include metal deposition, sputtering, application of a metal paste, application of a metal tape, etc. Among these, from the viewpoint of reducing the contact resistance with the charging member, the method of forming a platinum thin film by deposition is preferred. When forming a platinum thin film on the surface of a charged member, taking into consideration the simplicity of the process and the uniformity of the thin film, it is preferable to use a vacuum deposition apparatus that is provided with a mechanism for gripping the charged member and that is further provided with a rotation mechanism for a charged member having a cylindrical cross section. For charged members with a cylindrical cross section, it is preferable to form a platinum electrode with a width of about 10 mm in the longitudinal direction, which is the axial direction of the cylindrical shape, and to connect a metal sheet wrapped around the platinum electrode so as to come into contact with the platinum electrode to the measurement electrode protruding from the measurement device. This makes it possible to perform impedance measurement without being affected by the fluctuation of the outer diameter of the charged member or the surface shape. Aluminum foil, metal tape, etc. can be used as the metal sheet. The impedance measuring device may be any device capable of measuring impedance, such as an impedance analyzer, a network analyzer, a spectrum analyzer, etc. Among these, it is preferable to measure the impedance using an impedance analyzer because of the electric resistance range of the charging member. Figure 3 shows a schematic diagram of a state in which a measurement electrode is formed on a conductive member. In Figure 3, 31 is a conductive support, 32 is a conductive layer, 33 is a platinum vapor deposition layer which is a measurement electrode, and 34 is an aluminum sheet. Figure 3(a) shows a perspective view, and Figure 3(b) shows a cross-sectional view. As shown in this figure, it is important that the conductive layer 32 is sandwiched between the conductive support 31 and the conductor layer 33 of the measurement electrode.

[0016] Then, the aluminum sheet 34 is connected to the measuring electrode 33 and the conductive support 31 in an impedance measuring device (Solatron 126096W type dielectric impedance measuring system manufactured by Toyo Corporation, not shown), and impedance measurement is performed. The impedance is measured in an environment of a temperature of 23°C and a relative humidity of 50%, with an oscillating voltage of 1 Vpp and a frequency of 1.0 Hz, to obtain the absolute value of the impedance. The conductive member is divided into five equal regions in the longitudinal direction, and the above measurement is carried out five times in total, once in each region. The average value is regarded as the impedance of the conductive member.

[0017] Requirements (B) Among the requirements (B), the requirement (B1) specifies the amount of conductive particles contained in each of the domains contained in the conductive layer, and the requirement (B2) specifies that the outer peripheral surface of the domain has little or no irregularities. When the conductive member described in Patent Document 1 was analyzed, it was confirmed that the outer peripheral surface of the domain had irregularities or the domain had a shape with a high aspect ratio. As a result of intensive investigation, it was found that the above-mentioned problem of fogging during application of a high voltage can be dramatically suppressed by making the cross-sectional shape of the domain that appears in the cross section in the thickness direction of the conductive layer closer to a perfect circle with fewer irregularities, in other words, by making the domain closer to a sphere. As described above, in a conductive domain / non-conductive matrix configuration in which only the domains are conductive, multiple domains are conductive inside the conductive member, and charge is transferred between the domains. If a domain has a convex portion, the electric field is concentrated at the convex portion, making it easier for charge transfer between adjacent domains to occur at the convex portion, and an excessive current flows in the convex portion. In other words, charge is easier to flow from the convex portion of a domain to a domain close to the convex portion. This phenomenon causes strong localized discharge from the surface of the conductive member, which causes potential unevenness in the photoconductor when the conductive member is used as a charging member.

[0018] That is, it is effective to make the cross-sectional shape of the domain, which appears in a cross section in the thickness direction of the conductive layer, as close to a perfect circle as possible. Regarding requirement (B1), the present inventors have found that, when focusing on one domain, the amount of conductive particles contained in the domain affects the outer shape of the domain. That is, the inventors have found that as the amount of conductive particles packed in one domain increases, the outer shape of the domain becomes closer to a sphere. The more domains that are closer to a sphere, the fewer the concentration points of electron transfer between domains can be. As a result, the fogging of electrophotographic images observed in the charging member according to Patent Document 1 can be reduced. According to the study by the present inventors, a domain in which the ratio of the total cross-sectional area of ​​the conductive particles observed in a cross-section to the cross-sectional area of ​​the domain is 20% or more can have an outer shape that can significantly alleviate the concentration of electron transfer between domains. Specifically, the domain can have a shape closer to a sphere. The requirement (B2) specifies the degree of the presence of irregularities on the outer peripheral surface of a domain that may become points of concentration for the exchange of electrons. That is, when the perimeter of a domain is A and the envelope perimeter of the domain is B, when the value (A / B) of the requirement (B2) indicating the degree of unevenness is 1.00, it indicates that there is no unevenness, and the concentration of the electric field can be more reliably suppressed. Also, the larger the value of the requirement (B2), the more uneven the shape is. The larger this value, the more likely the electric field is to concentrate at the convex parts because the domain has an uneven shape. It has been found that the electric field concentration caused by the convex parts of the domain shape can be suppressed by setting the value of the requirement (B2) to 1.10 or less. The envelope perimeter is defined as the perimeter of the convex hull of the domain. Specifically, for example, as shown in FIG. 5, it is the perimeter (dashed line 52) when the convex parts of the domain 51 observed in the observation area are connected to each other and the perimeter of the concave parts is ignored.

[0019] From the above results, the inventors have found that when 80% or more of the domains in the cross section of the conductive layer observed in each of the nine observation regions simultaneously satisfy requirements (A) and (B), the electric field concentration inside the conductive member can be suppressed and uniform discharge can be achieved. As a result, fogging on the photoconductor when a high voltage is applied as a charging member can be suppressed. In requirement (B), the domain observation target is set to a depth of 0.1T to 0.9T from the outer surface of the conductive layer in the cross section in the thickness direction of the conductive layer. This is because it is considered that the movement of electrons from the conductive support side to the outer surface side of the conductive layer in the conductive layer is mainly controlled by the domains present within that range.

[0020] Here, the present inventors further studied the adhesion of toner, which may change the charging performance of the electrophotographic member according to Patent Document 2 over time. That is, the toner remaining on the photoconductor even after the transfer process (hereinafter, also referred to as "transfer residual toner") is often charged with the same polarity (positive polarity) as the polarity of the voltage in the transfer process. Therefore, the transfer residual toner that reaches the nip between the photoconductor and the charging member electrostatically adheres to the surface of the charging member. As a result, the surface of the charging member is gradually contaminated with the transfer residual toner, which may hinder stable discharge from the surface of the charging member. In order to suppress the electrostatic adhesion of the transfer residual toner to the outer surface of the charging member, it is effective to reverse the charge of the transfer residual toner.

[0021] Here, the present inventors have investigated reversing the charge of the transfer residual toner by using a conductive member having the above-mentioned requirements (A) and (B), which can effectively suppress fogging of an electrophotographic image even when a high charging bias is applied. As a result, in addition to the above-mentioned requirements (A) and (B), it has been found that exposing at least a part of the domain to the outer surface of the conductive member and generating a convex portion (hereinafter also referred to as a "first convex portion") derived from the domain on the outer surface of the conductive member (hereinafter also referred to as requirement (C)) is effective in reversing the charge of the transfer residual toner.

[0022] By exposing the domain on the outer surface of the conductive member and forming the first convex portion, the transfer residual toner that reaches the nip portion between the charging member and the photosensitive drum is likely to physically come into contact with the first convex portion. In addition, the positively charged transfer residual toner is electrostatically attracted to the first convex portion that accumulates negative charges. These actions increase the probability of contact between the transfer residual toner and the first convex portion. Then, negative charges are injected into the transfer residual toner that comes into contact with the first convex portion, and it is made negative. In addition, the domain that transfers the charge to the transfer residual toner by contacting with the transfer residual toner can receive a stable and continuous supply of charge from other domains present in the conductive layer. Therefore, it is considered that it is possible to more reliably make the transfer residual toner that reaches the nip portion negative.

[0023] Specifically, the height of the first convex portion on the outer surface of the conductive member is preferably 50 nm or more and 200 nm or less. By making the first convex portion 50 nm or more in height, the contact opportunity between the conductive first convex portion and the reverse toner can be increased. Furthermore, by making the first convex portion 100 nm or more in height, the contact opportunity can be further increased and reverse toner fogging can be reduced. On the other hand, since uneven discharge caused by the first convex portion is formed in the discharge area, the height of the first convex portion is preferably 200 nm or less.

[0024] The arithmetic mean value Dm of the distance between the wall surfaces of the domains on the outer surface of the conductive member (hereinafter, simply referred to as "domain distance Dm") is preferably 2.00 μm or less. By setting the domain distance Dm to 2.00 μm or less, the contact opportunity between the first protrusions and the inverted toner can be increased.

[0025] Therefore, the conductive member makes the domains closer to a perfect circle to suppress the concentration of the electric field in the conductive layer due to the requirements (A) and (B), and furthermore, due to the requirement (C), the reverse toner adhesion is suppressed by the injection charging caused by the convex parts derived from the domains. As a result, it is possible to significantly reduce fogging even when the charging bias is high.

[0026] Furthermore, the present inventors have studied configurations for stabilizing, for a longer period of time, the performance as a charging member of the electrophotographic member according to Patent Document 2. As a result, they have found that, in addition to the above requirements (A), (B), and (C), it is effective to suppress physical adhesion of the transfer residual toner to the convex portions (first convex portions) constituted by domains exposed on the outer surface of the conductive member. For example, in an electrophotographic image forming apparatus with high energy saving in which a cleaning member such as a cleaning blade is brought into contact with the photosensitive drum with less pressure, or in an electrophotographic image forming apparatus in which a waste toner box is eliminated and the photosensitive drum is cleaned simultaneously with development, more transfer residual toner can reach the charging member. In the use of an electrophotographic image forming apparatus for a long period of time in which the number of prints exceeds several hundred thousand sheets, the number of contacts between the charging member and the photosensitive drum increases, so that the transfer residual toner is crushed at the contact portion between the charging member and the photosensitive drum and strongly adheres to the surface of the charging member. Even with the electrophotographic member according to Patent Document 2, it was difficult to completely prevent the transfer residual toner from adhering as a result of the above-mentioned long-term use. And, when the transfer residual toner adheres to the first convex portion exposed on the outer surface of the conductive member, which has the function of uniform discharge, discharge from the first convex portion is hindered, and the flow of charge in the conductive layer, which should be uniform, is impeded, and the transfer residual toner can concentrate on the first convex portion to which it is not adhered. As a result, there are areas where the discharge is locally strong, which can cause fogging on the electrophotographic image.

[0027] Therefore, in the conductive member according to the present disclosure, the inventors have provided convex portions (hereinafter also referred to as "second convex portions") derived from insulating resin particles on the outer surface of the conductive member in addition to the first convex portions derived from the domains, thereby achieving a configuration that can prevent the residual toner from adhering to the first convex portions.

[0028] In the nip between the conductive member surface and the photosensitive drum, a space is formed by the second convex portion, and the distance can be determined by the following method. That is, when a transparent flat plate is brought into contact with the conductive member and a load of 500 g (the upper limit of the load on the charging member) is applied to the transparent flat plate, the height of the space formed by the contact between the second convex portion and the transparent flat plate in the nip between the conductive member and the flat plate is determined. In the present disclosure, this distance is 3 μm or more and 30 μm or less. Furthermore, there is no contact point between the first convex portion and the transparent flat plate in the nip, and they contact only at the second convex portion. This can suppress toner adhesion to the first convex portion. The transparent plate may be any plate having transparency that allows the second convex portion to be observed through the material, and that is not deformed by the above pressure. The thickness may be any thickness that allows the above pressure to be applied stably and does not affect transparency. A representative example is an inorganic transparent material, such as an optical glass plate made of BK7 or synthetic quartz. Optical glass has high smoothness and is suitable for such measurements.

[0029] The measurement of the spatial distance at the nip portion between the conductive member surface and the photosensitive drum by the second convex portion will be described in detail later, but is performed using a transparent glass plate 92 as a transparent flat plate for the conductive member as shown in Fig. 9(a). Furthermore, a predetermined load is applied using a jig having a configuration capable of measuring the load, and measurement can be performed from the glass plate 92 side with a device capable of scanning a height profile, such as a laser microscope.

[0030] If the spatial distance in the nip portion between the conductive member and the photosensitive drum is 3 μm or more, the destruction of the transfer residual toner at the contact portion can be suppressed. Furthermore, if the height is 5 μm or more, a gap that prevents the transfer residual toner from being deformed can be formed, which is preferable. On the other hand, since unevenness in discharge due to the first convex portion is formed in the discharge area, the spatial distance needs to be 30 μm or less.

[0031] Furthermore, the second convex portion is insulating so as not to disturb the uniformity of the electric field due to the domains in the conductive phase and to prevent the injection of electric charge from the second convex portion to the photosensitive drum. 10 The upper limit is not particularly limited, but it is generally 1.0×10 17 It is preferable that the resistivity is Ωcm or less.

[0032] In addition, since the second convex portion, which is on the order of micrometers, is close to the photosensitive drum, the amount of discharge is greater than in other places than the second convex portion, and the surface potential of the photosensitive drum becomes locally high, which may cause fogging. Therefore, an initial conductive member that has not been subjected to a durability test tends to have more fogging than a conductive member that does not have the second convex portion. However, to prevent the worsening of fogging caused by toner adhesion due to long-term use, a means of suppressing the adhesion of transfer residual toner by the second convex portion is extremely effective.

[0033] In addition, in order to avoid scraping off residual toner and promoting toner adhesion when the conductive member and the photosensitive drum slip and have a relative speed, such as when starting rotation, the second convex portions are preferably present in the form of dots on the outer surface of the conductive member.

[0034] <Transparent flat plate> In the present disclosure, the transparent flat plate is, for example, a glass plate having a material of BK7, surface precision of optically polished surfaces on both sides, parallelism of 1 arc minute or less, and a thickness of 2 mm.

[0035] <Conductive materials> As one embodiment of the conductive member for electrophotography according to the present disclosure, a conductive member having a roller shape (hereinafter, also referred to as a "conductive roller") will be described with reference to the drawings. 1 is a cross-sectional view perpendicular to the direction along the axis of the conductive roller (hereinafter also referred to as the "longitudinal direction"). The conductive roller 1 has a cylindrical conductive support 2 and a conductive layer formed on the outer periphery of the support 2, i.e., on the outer surface of the support. 2 shows an enlarged cross-sectional view of the conductive layer 3 in a direction perpendicular to the longitudinal direction of the conductive roller. The conductive layer 3 has a matrix-domain structure having a matrix 3a and domains 3b. The domains 3b contain conductive particles (not shown). A part of the domains 3b is exposed on the outer surface of the conductive member, i.e., the surface facing a member to be charged such as a photoconductor. The domains 3b exposed on the outer surface generate first protrusions 3-1 on the outer surface of the conductive member. Further, FIG. 2(b) shows a cross-sectional view at a lower magnification (for example, 1 / 30 magnification) than FIG. 2(a). As shown in FIG. 2(b), the conductive layer 3 is added with resin particles 3c, and a second convex portion 3-2 derived from the resin particles is formed to form a gap with the photosensitive drum. Note that the second convex portion 3-2 is shown in a case where the surface is polished and flattened to expose it as described later, but the second convex portion 3-2 is not necessarily flattened entirely, and may remain a spherical surface. In addition, the area of ​​the flat surface differs depending on the difference in the protrusion method, but the maximum height is controlled by this polishing. In FIG. 2(b), the first convex portion 3-1 due to the domain 3b is omitted because it is lower in height than the second convex portion 3-2. It is preferable that the first convex portion 3-1 is formed on the outer surface of the conductive layer other than the second convex portion 3-2 so as not to form a contact point at the nip portion with the transparent flat plate. The first protrusion 3-1 may be formed on a part of the surface of the second protrusion 3-2 (such as a peripheral part not in contact with the transparent flat plate) as long as the effect of the present disclosure is not impaired.

[0036] <How to check the matrix-domain structure> The presence of the matrix-domain structure can be confirmed, for example, as follows. Specifically, a thin piece of the conductive layer is prepared from the conductive member and then observed in detail. Examples of means for forming the thin piece include a sharp razor, a microtome, and an FIB. In addition, in order to favorably observe the matrix-domain structure, a pretreatment such as a dyeing treatment or a deposition treatment may be performed to favorably obtain a contrast between the conductive phase and the insulating phase. The thin piece after the formation of the fracture surface and the pretreatment can be observed with a laser microscope, a scanning electron microscope (SEM), or a transmission electron microscope (TEM).

[0037] The conductivity of the conductive member may be evaluated by impedance measurement at 1 Hz. Specifically, the impedance at 1 Hz is 10 3 Ω or more 10 8 It is preferable that the resistance is in the range of 10 Ω or less. 3 By setting the resistance to 10 Ω or more, it is possible to prevent the discharge current from becoming excessively large, which can prevent potential unevenness caused by abnormal discharge. 8 By setting the resistance to Ω or less, it is possible to suppress insufficient charging due to insufficient total amount of discharged charge.

[0038] <Conductive support> The material constituting the support can be appropriately selected from materials known in the field of electroconductive members for electrophotography and materials usable as electroconductive members, such as aluminum, stainless steel, conductive synthetic resins, iron, copper alloys, and other metals or alloys. Furthermore, these may be subjected to oxidation treatment or plating treatment with chromium, nickel, etc. As the type of plating, either electric plating or electroless plating can be used. From the viewpoint of dimensional stability, electroless plating is preferred. As the type of electroless plating used here, nickel plating, copper plating, gold plating, and various other alloy platings can be mentioned. The plating thickness is preferably 0.05 μm or more, and considering the balance between work efficiency and rust prevention ability, the plating thickness is preferably 0.10 μm or more and 30.00 μm or less. The cylindrical shape of the support may be a solid cylindrical shape or a hollow cylindrical shape (cylindrical shape). In addition, the outer diameter of the support is preferably in the range of 3 mm or more and 10 mm or less.

[0039] <Conductive layer> <Matrix> The matrix contains a first crosslinked rubber. The volume resistivity ρm of the matrix is ​​1.0×10 8 Ωcm or more 1.0×10 17 Ωcm or less is preferable. The volume resistivity of the matrix is ​​1.0×10 8 When the resistivity is Ωcm or more, the effect of the conductivity of the matrix on the transfer of charges between conductive domains can be suppressed. In particular, when the conductivity of the matrix is ​​high (volume resistivity is low) and it exhibits ionic conductivity, the matrix excessively promotes the transfer of charges between conductive domains, and when electric field concentration occurs due to a slight change in the domain shape, excessive current tends to flow. Therefore, in order to suppress the ionic conductivity of the matrix, the volume resistivity ρm should be set to 1.0×10 8 It is preferable that the resistivity is Ωcm or more. Volume resistivity ρm is 1.0×10 17 When the resistivity is Ωcm or less, the necessary conductivity can be obtained as a whole of the conductive layer without impeding the transfer of charges between the conductive domains, and therefore image defects due to insufficient charging can be prevented. The volume resistivity ρm is more preferably 1.0×10 10 Ωcm or more 1.0×10 17Within this range, the influence of the ionic conductivity of the matrix can be suppressed, and the volume resistivity required for the conductive member can be obtained. The most preferable range of the volume resistivity ρm is 1.0×10 12 Ωcm or more 1.0×10 17 Within this range, even when a high voltage is applied, electric field concentration can be significantly suppressed, and the volume resistivity required for the conductive member can be obtained.

[0040] <Volume resistivity of matrix ρm> The volume resistivity ρm of the matrix can be measured, for example, by cutting a slice of a given thickness (e.g., 1 μm) containing a matrix domain structure from the conductive layer and contacting the matrix in the slice with a microprobe of a scanning probe microscope (SPM) or an atomic force microscope (AFM). For example, as shown in Fig. 6(a), the slice is cut from the elastic layer so as to include at least a part of a cross section 62a that is flat with respect to the XZ plane, where the longitudinal direction of the conductive member is the X axis, the thickness direction of the conductive layer is the Z axis, and the circumferential direction is the Y axis. Alternatively, as shown in Fig. 6(b), the slice is cut so as to include at least a part of a YZ plane (e.g., 63a, 63b, 63c) perpendicular to the axial direction of the conductive member. For example, a sharp razor, a microtome, a focused ion beam method (FIB), etc. can be used. To measure the volume resistivity, one side of a thin piece cut from the conductive layer is grounded. Next, a tiny probe of a scanning probe microscope (SPM) or atomic force microscope (AFM) is brought into contact with the matrix on the side of the thin piece opposite the grounded side, a DC voltage of 50V is applied for 5 seconds, and the arithmetic mean value is calculated from the ground current value measured for 5 seconds, and the applied voltage is divided by this calculated value to calculate the electrical resistance value. Finally, the resistance value is converted to volume resistivity using the film thickness of the thin piece. At this time, the SPM or AFM can measure the film thickness of the thin piece at the same time as the resistance value. The volume resistivity value of the matrix in a cylindrical charging member is determined, for example, by cutting out one thin sample from each of the regions obtained by dividing the conductive layer into four in the circumferential direction and five in the longitudinal direction, obtaining the above-mentioned measurement values, and then calculating the arithmetic average value of the volume resistivities of a total of 20 samples.

[0041] <First Rubber> The first rubber is the component with the highest compounding ratio in the rubber mixture for forming the conductive layer, and the crosslinked product of the first rubber governs the mechanical strength of the conductive layer. Therefore, the first rubber is used to provide the conductive layer with the strength required for a conductive member for electrophotography after crosslinking, and is capable of phase separation with the second rubber described below to form a matrix-domain structure.

[0042] Preferred examples of the first rubber are given below. Examples include natural rubber (NR), isoprene rubber (IR), butadiene rubber (BR), styrene-butadiene rubber (SBR), butyl rubber (IIR), ethylene-propylene rubber (EPM), ethylene-propylene-diene terpolymer rubber (EPDM), chloroprene rubber (CR), acrylonitrile-butadiene rubber (NBR), hydrogenated NBR (H-NBR), and silicone rubber.

[0043] <Reinforcement material> In addition, reinforcing carbon black can be blended into the matrix as a reinforcing agent to the extent that it does not affect the conductivity of the matrix. Examples of reinforcing carbon black used here include FEF, GPF, SRF, and MT carbon, which have low conductivity. Furthermore, to the first rubber forming the matrix, fillers, processing aids, vulcanization aids, vulcanization accelerators, vulcanization acceleration aids, vulcanization retarders, antioxidants, softeners, dispersants, colorants, and the like, which are generally used as compounding agents for rubber, may be added as necessary.

[0044] <domain> The domain is conductive and includes a crosslinked second rubber and conductive particles. Here, the conductive property is defined as a volume resistivity of 1.0×10 8 This means that the resistance is less than Ωcm.

[0045] <Second Rubber> Specific examples of the second rubber include at least one selected from the group consisting of natural rubber (NR), isoprene rubber (IR), butadiene rubber (BR), acrylonitrile butadiene rubber (NBR), styrene butadiene rubber (SBR), butyl rubber (IIR), ethylene propylene rubber (EPM), ethylene propylene diene rubber (EPDM), crumbrene rubber (CR), nitrile rubber (NBR), hydrogenated nitrile rubber (H-NBR), silicone rubber, and urethane rubber (U).

[0046] <Conductive particles> Examples of conductive particles to be blended in the domain include carbon materials such as conductive carbon black and graphite, oxides such as titanium oxide and tin oxide, metals such as Cu and Ag, and electron conductors such as particles that are surface-coated with oxides or metals to make them conductive. If necessary, two or more types of these conductive particles may be blended in appropriate amounts. The conductive particles to be mixed in the domains are preferably added in an amount such that the ratio of the cross-sectional area of ​​the conductive particles to the cross-sectional area of ​​the domain is at least 20%, preferably 25% to 30%, as specified in requirement (B1). By being in the above range, the conductive particles can be densely packed in the domains. Furthermore, the external shape of the domain can be made closer to a sphere, and irregularities can be made small as specified in requirement (B2). Furthermore, a sufficient amount of charge can be supplied even under high-speed processing. Among the above conductive particles, conductive particles containing conductive carbon black as a main component are preferred because of their high conductivity, high affinity with rubber, and ease of control of the distance between conductive particles. The type of conductive carbon black to be blended into the domain is not particularly limited. Specific examples include gas furnace black, oil furnace black, thermal black, lamp black, acetylene black, and ketjen black. Among these, as described below, conductive particles having a DBP absorption of 40 cm 3 / 100g or more 80cm 3 Carbon black having a molecular weight of 100 g or less can be particularly preferably used.

[0047] <Shape of conductive domain> The inventors have discovered that by making the conductive domains closer to a circular shape, electric field concentration caused by the convex shape of the conductive domains is minimized, thereby suppressing excessive charge movement even when a high voltage is applied, enabling the photoconductor to be uniformly charged, and as a result, fogging can be suppressed. The shape of the domain is defined as three locations: the center of the conductive layer in the longitudinal direction, and two locations at L / 4 from both ends toward the center, where L is the length of the conductive layer in the longitudinal direction and T is the thickness of the conductive layer. For each of the three locations, a 20 μm square observation region is placed at any three locations in a thickness region from the outer surface of the conductive layer to a depth of 0.1 T to 0.9 T. The shape of the domain is defined as the shape of the domain observed in each of the nine observation regions. As explained above, the domain shape is preferably close to a circle. Specifically, 80% or more of the domains in a 20 μm square area of ​​a cross section of the conductive layer in the thickness direction must satisfy the following requirements (B1) and (B2). Requirement (B1): The ratio of the cross-sectional area of ​​the conductive particles contained in a domain to the cross-sectional area of ​​the domain is 20% or more; Requirement (B2): When the perimeter of a domain is A and the envelope perimeter of the domain is B, A / B is 1.00 or more and 1.10 or less.

[0048] The minimum ratio of the domain perimeter to the domain envelope perimeter in requirement (B2) is 1.00, and a ratio of 1.00 indicates that the domain is a perfect circle or an ellipse. If the ratio exceeds 1.10, the domain will have a large uneven shape, that is, electric field concentration will be likely to occur. If requirement (B2) is satisfied, the electric field concentration is suppressed, and it is possible to suppress fogging. The maximum Feret diameter Df is the value at which the length of the perpendicular line is the longest when the periphery of the observed domain 41 is sandwiched between two parallel lines and the two parallel lines are connected by a perpendicular line, as shown in FIG. The size of the domain is preferably within a certain range, and the maximum Feret diameter, which is an index representing the domain size, is preferably 0.1 μm or more and 5.0 μm or less. If the maximum Feret diameter is within this range, the domain is likely to have a circular shape. As a result, fogging is reduced. Also, by making the conductive domains finer, the discharge also becomes finer, which enables higher image quality.

[0049] <Method of measuring the maximum Feret diameter, area, perimeter, envelope perimeter, and number of domains> The method of measuring the maximum Feret diameter, area, perimeter, envelope perimeter, and number of domains of a domain may be carried out as follows. First, a slice is prepared in the same manner as in the measurement of the volume resistivity of the matrix described above. Then, a thin piece having a fracture surface can be formed by means of a freeze fracture method, a cross polisher method, a focused ion beam method (FIB), or the like. Considering the smoothness of the fracture surface and pretreatment for observation, the FIB method is preferred. In addition, in order to perform an observation of the matrix-domain structure favorably, a pretreatment such as a dyeing treatment or a deposition treatment may be performed to favorably obtain a contrast between the conductive phase and the insulating phase. The formed and pretreated thin sections can be observed using a scanning electron microscope (SEM) or a transmission electron microscope (TEM). Among these, it is preferable to observe using an SEM at 1,000 to 100,000 magnifications in terms of the accuracy of quantifying the area of ​​the domains. The maximum Feret diameter, area, perimeter, envelope perimeter, and number of domains of the domains can be measured by quantifying the photographed image. That is, the fracture surface image obtained by observation with an SEM is converted to 8-bit grayscale using image processing software (product name: ImageProPlus, manufactured by Media Cybernetics) or the like to obtain a monochrome image with 256 gradations. Next, the black and white of the image are inverted and binarized so that the domains in the fracture surface become white. Next, the maximum Feret diameter, area, perimeter, envelope perimeter, and number of domains may be calculated from each of the domain groups in the image. For the above measurement, slices are cut from a total of three locations, namely, the center of the longitudinal direction of the conductive layer, and two locations at L / 4 from both ends of the conductive layer toward the center, when the longitudinal length of the conductive layer of the conductive member is L. The direction in which the slices are cut is a direction perpendicular to the longitudinal direction of the conductive layer.

[0050] The reason for evaluating the shape of the domain in a cross section perpendicular to the longitudinal direction of the conductive layer as described above will be described with reference to FIG. 6 shows a diagram illustrating the shape of the conductive member 61 in three dimensions along three axes, specifically, the X, Y, and Z axes. In Fig. 6, the X axis indicates a direction parallel to the longitudinal direction (axial direction) of the conductive member, and the Y axis and Z axis indicate directions perpendicular to the axial direction of the conductive member.

[0051] FIG. 6(a) shows an image of a conductive member cut out at a cross section 62a parallel to an XZ plane 62. The XZ plane can rotate 360° around the axis of the conductive member. Considering that the conductive member rotates in contact with the photosensitive drum and discharges when passing through a gap with the photosensitive drum, the cross section 62a parallel to the XZ plane 62 indicates a surface on which discharge occurs simultaneously at a certain timing. Therefore, the surface potential of the photosensitive drum is formed by passing a surface equivalent to a certain amount of the cross sections 62a. Since a locally large discharge due to electric field concentration in the conductive member locally increases the surface of the photosensitive drum and becomes fog, an evaluation is required that correlates with the surface potential of the photosensitive drum formed by passing a set of the cross sections 62a rather than a single cross section 62a of a certain amount. Therefore, rather than analyzing a cross section where discharge occurs simultaneously at a certain moment like the cross section 62a, an evaluation is required on cross sections (63a to 63c) parallel to the YZ plane 63 perpendicular to the axial direction of the conductive member, which allows evaluation of the domain shape including the certain amount of the cross sections 62a. When the longitudinal length of the conductive layer is L, three cross sections 63a to 63c are selected: cross section 63b at the longitudinal center of the conductive layer, and two cross sections (63a and 63c) at L / 4 from both ends of the conductive layer toward the center. The observation positions of each of the cross sections 63a to 63c are as follows: when the thickness of the conductive layer is T, three arbitrary positions are specified in a thickness region from the outer surface of each of the cross sections to a depth of 0.1T to 0.9T. When an observation region of 20 μm square is placed at the three arbitrary positions, a total of nine positions are measured.

[0052] <Domain shape control> The formation of nearly circular domains in the matrix-domain structure is an important point in achieving the effects of the present disclosure. The formation of nearly circular domains and the reduction of size unevenness in the maximum Feret diameter suppress electric field concentration and domain deformation, thereby reducing resistance fluctuation. The present inventors have investigated methods for making the cross-sectional shape of the domain circular, that is, for making the domain shape closer to a sphere, and have found that this can be achieved by using the following two methods. -Reduce the domain size (maximum Feret diameter). -Increase the amount of carbon gel in the domain. The reason why the domains become closer to a spherical shape by reducing the domain size (maximum Feret diameter) is speculated to be as follows: Even with the same domain volume fraction, if the domain size is small, the surface area of ​​the domain increases, and as a result the interface with the matrix increases. Molecules near the interface have more different molecules surrounding them than inside the matrix, and therefore have greater free energy than the molecules inside the domain. In order to reduce this interfacial free energy, interfacial tension acts to make the interface smaller, and it is thought that the domains become closer to a spherical shape (circular in the cross section in the thickness direction of the conductive layer). As a result, electric field concentration can be suppressed.

[0053] -Method to reduce domain size (maximum Feret diameter) Regarding the dispersed particle diameter (domain size) D when two immiscible polymers are melt-kneaded, the Taylor formula, Wu's empirical formula, and Tokita's formula shown in the following formulas (4) to (7) have been proposed (see Sumitomo Chemical Technical Journal 2003-II, 42). · Taylor's formula Formula (4) D = [C σ / ηm γ] f(ηm / ηd) ·Wu's Empirical Formula Formula (5) γ D ηm / σ = 4(ηd / ηm) 0.84 ηd / ηm>1 Formula (6) γ D ηm / σ = 4(ηd / ηm) -0.84 ηd / ηm<1

[0054]

number

[0055] In the formulas (4) to (7), D: domain size, C: constant, σ: interfacial tension, ηm: viscosity of matrix, ηd: viscosity of domain, where γ is the shear rate, η is the viscosity of the mixture, P is the probability of collision and coalescence, φ is the domain phase volume, and EDK is the domain phase cleavage energy.

[0056] As shown in the above formula, the formation of nearly spherical domains can be controlled mainly by the following four points. 1.Interfacial tension difference between domain and matrix 2. Viscosity ratio of domain to matrix 3.Shear rate during mixing / energy during shear 4. Domain Volume Fraction

[0057] 1.Interfacial tension difference between domain and matrix Generally, when two types of polymers are mixed, phase separation occurs. This phenomenon occurs because the interaction between the same polymers is stronger than the interaction between different polymers, so the same polymers aggregate to reduce the free energy and stabilize. The interface of the phase-separated structure comes into contact with different polymers, so the free energy is higher than the interior, which is stabilized by the interaction between the same molecules. As a result, in order to reduce the free energy of the interface, interfacial tension is generated that tries to reduce the area of ​​contact with the different polymers. When this interfacial tension is small, the different polymers tend to mix more uniformly in order to increase the entropy. The state of uniform mixing is dissolution, and the SP value, which is an indicator of solubility, tends to correlate with the interfacial tension. In other words, the difference in interfacial tension between the domain and the matrix is ​​thought to correlate with the SP value difference of the rubber material that constitutes the domain and the matrix, so it is possible to control it by selecting the raw rubber of the matrix and the domain. The difference in absolute values ​​of the solubility parameters of the first rubber and the second rubber is 0.4 (J / cm 3 ) 0.5 More than 4.0(J / cm 3 ) 0.5 If the density is less than 0.4 (J / cm), a stable phase separation structure can be formed. 3 )0.5 2.2 (J / cm 3 ) 0.5 or less. Within this range, a stable phase separation structure can be formed, and the maximum Feret diameter of the domain can also be reduced.

[0058] 2. Viscosity ratio of domain to matrix The viscosity ratio of the domain to the matrix (ηd / ηm) can reduce the maximum Feret diameter of the domain the closer it is to 1. The viscosity ratio of the domain to the matrix can be adjusted by selecting the Mooney viscosity of the rubber raw material and by blending the type and amount of the filler. Also, it is possible by adding a plasticizer such as paraffin oil to the extent that it does not prevent the formation of the phase separation structure. In addition, the viscosity ratio can be adjusted by adjusting the temperature during kneading. Note that the viscosities of the domain and the matrix can be obtained by measuring the Mooney viscosity ML(1+4) based on JIS K6300-1:2013 at the rubber temperature during kneading. Also, it may be substituted with the catalog value of the raw rubber.

[0059] 3. Shear rate during mixing / Energy amount during shear The shear rate during mixing / energy amount during shear can reduce the maximum Feret diameter of the domain the greater it is. The shear rate can be increased by increasing the inner diameter of the stirring members such as the blades and screws of the kneader, reducing the gap from the end face of the stirring member to the inner wall of the kneader, or increasing the rotation speed. Also, to increase the energy during shear, it can be achieved by increasing the rotation speed of the stirring member or by increasing the viscosities of the domain raw rubber and the matrix raw rubber.

[0060] 4. Volume fraction of domain The volume fraction of the domain in the conductive layer correlates with the probability of collision and coalescence of the domain and the matrix. Specifically, reducing the volume fraction in the conductive layer decreases the probability of collision and coalescence of the domain and the matrix. That is, within the range where the required conductivity can be obtained, the domain size can be reduced by decreasing the volume fraction of the domain.

[0061] <Method for measuring SP value> The SP value of the rubber constituting the matrix and the domain can be calculated with high accuracy by creating a calibration curve using a material with a known SP value. The known SP value can also be a catalog value of the material manufacturer. For example, the SP value of NBR and SBR that can be used in the present disclosure is determined almost entirely by the content ratio of acrylonitrile and styrene, regardless of the molecular weight. Therefore, the content ratio of acrylonitrile or styrene of the rubber constituting the matrix and the domain is analyzed using analytical methods such as pyrolysis gas chromatography (Py-GC) and solid-state NMR. This allows the SP value to be calculated from a calibration curve obtained from a material with a known SP value. In addition, the SP value of isoprene rubber is determined by the isomer structure, such as 1,2-polyisoprene, 1,3-polyisoprene, 3,4-polyisoprene, cis-1,4-polyisoprene, trans-1,4-polyisoprene, etc. Therefore, like SBR and NBR, the isomer content ratio can be analyzed by Py-GC and solid-state NMR, etc., and the SP value can be calculated from materials with known SP values. The SP values ​​of materials with known SP values ​​were determined by the Hansen sphere method.

[0062] Next, we will explain why the domains become closer to a spherical shape by increasing the amount of carbon gel in the domains. Carbon gel is a particulate substance that is in a pseudo-crosslinked state due to rubber molecules being adsorbed onto the carbon black. Carbon gel does not dissolve even in organic solvents that dissolve raw rubber. In other words, it is three-dimensionally crosslinked due to physical and chemical adsorption of rubber molecules onto the carbon black surface, and is thought to behave as rubber particles. As a result, it is speculated that the rubber particles formed by the carbon gel act as nuclei to form domains. By increasing the amount of carbon gel, it is possible to suppress the uneven shape of the domains and electric field concentration, as required by the above-mentioned requirement (B2).

[0063] In order to increase the amount of carbon gel, it is preferable to compound a large amount of carbon black with respect to the rubber, and the amount of carbon black that functions as an adsorbent can be increased. As an index for blending a large amount of carbon black in the domain, we focused on DBP absorption. 3 / 100 g) is the volume of dibutyl phthalate (DBP) that can be adsorbed by 100 g of carbon black, and is measured in accordance with JIS K 6217. Generally, carbon black has a cluster-like high-order structure in which primary particles with an average particle size of 10 nm to 50 nm are aggregated. This cluster-like high-order structure is called structure, and its degree is expressed by the DBP absorption (cm 3 / 100g). Generally, carbon black with a developed structure has a high reinforcing effect on rubber, which makes it difficult to incorporate the carbon black into rubber and also makes the shear torque during kneading very high, making it difficult to fill in large amounts. The conductive carbon black used in this disclosure has a DBP absorption of 40 cm 3 / 100g or more 80cm 3 It is preferable to use carbon black having a DBP absorption of 100 g or less. By making the DBP absorption amount within the above range, a large amount of carbon black is blended into the rubber, and the amount of carbon gel increases. Furthermore, if the DBP absorption amount is within the above range, the conductive carbon black has a small structure, so that the carbon black disperses well in the rubber, and the carbon black aggregates little, and the carbon black alone has few irregularities. Therefore, it is easy to make the domain shape round. That is, it is easy to make it spherical. When carbon black with a developed structure is used, it is difficult to disperse uniformly in the rubber, and the carbon black tends to disperse in an aggregated state. Originally, carbon black has a tuft-like high-order structure as mentioned above, so it has an irregular shape, but when these aggregate, they tend to become a mass with a larger irregular structure. If this carbon black aggregate is present on the outer edge of the domain, it may affect the domain shape and form an irregular structure.

[0064] In addition, the amount of conductive carbon black to be added to the domain is preferably such that the arithmetic mean of the distance between adjacent carbons, C (hereinafter also referred to as the "arithmetic mean wall distance C"), is 110 nm or more and 130 nm or less. If the arithmetic mean wall distance C is 110 nm or more and 130 nm or less, the transfer of electrons between carbon black particles by the tunnel effect is possible between almost all carbon black particles in the domain. In other words, if the above arithmetic mean wall distance is satisfied, the volume resistivity of the domain becomes almost constant, and electric field concentration is suppressed. In addition, resistance fluctuation due to changes in the carbon black wall distance due to repeated image output is suppressed. Furthermore, the amount of carbon gel that shows crosslinked rubber properties increases in the rubber in which carbon black is dispersed, making it easier to maintain the shape, and making it easier to maintain the domain in a spherical shape during molding. As a result, electric field concentration and changes in the domain distance due to deformation of the domain convex parts are suppressed, making it easier to achieve uniform discharge. Furthermore, the arithmetic mean wall-to-wall distance C of the conductive carbon black is 110 nm or more and 130 nm or less, and the standard deviation of the distribution of the wall-to-wall distance of the conductive carbon black is σm. At that time, it is more preferable that the coefficient of variation σm / C of the wall-to-wall distance of the conductive carbon black is 0.0 or more and 0.3 or less. The coefficient of variation is a value indicating the variation of the wall-to-wall distance of the conductive carbon black, and is 0.0 when all the wall-to-wall distances of the conductive carbon black are the same. When the coefficient of variation σm / C is between 0.0 and 0.3, the variation in the wall distance between the carbon black particles is small, which allows electrons to be exchanged between the carbon black particles in the domains by the tunnel effect, making the volume resistivity more likely to be constant. Furthermore, because the carbon black particles are uniformly dispersed, uneven distribution of the conductive paths in the domains can be suppressed, which in turn suppresses electric field concentration in the domains. As a result, in addition to the domain shape, electric field concentration in the domains can be suppressed, making it easier to achieve more uniform discharge.

[0065] The arithmetic mean value C of the distance between the conductive carbon black walls in a domain and the ratio of the carbon black cross section to the domain cross section area may be measured as follows. First, a thin piece of the conductive layer is prepared. In order to conveniently observe the matrix-domain structure, a pretreatment such as a dyeing treatment or a deposition treatment may be performed to favorably obtain a contrast between the conductive phase and the insulating phase. The formed and pretreated thin section can be observed with a scanning electron microscope (SEM) or a transmission electron microscope (TEM). Among these, it is preferable to observe with an SEM at 1,000 to 100,000 magnifications in terms of the accuracy of quantifying the area of ​​the domains that are the conductive phase. The obtained observation image is binarized and analyzed using an image analyzer or the like to obtain the above arithmetic mean wall-to-wall distance and the above ratio.

[0066] <Method of forming first convex portion (convex portion derived from domain)> The convex portion (first convex portion) derived from the domain can be formed by grinding the surface of the conductive member. The inventors believe that the convex portion derived from the domain can be suitably formed by a grinding process using a grindstone because the conductive layer has a matrix-domain structure. The convex portion derived from the domain is preferably formed by a method of grinding with a grindstone using a plunge type grinder. The following is a speculated mechanism by which the domain-derived convex portion can be formed by grinding with a grindstone. First, the domain dispersed in the matrix is ​​filled with conductive particles such as carbon black, and has a higher reinforcing property than the matrix not filled with conductive particles. In other words, when grinding is performed with the same grindstone, the domain is more difficult to grind than the matrix because of its high reinforcing property, and convex portions are more likely to be formed. By utilizing the difference in grinding property caused by this difference in reinforcing property, convex portions derived from the domain can be formed. In particular, since the conductive member according to this embodiment has a configuration in which many conductive particles are filled in the domain, it is possible to preferably form the convex portion.

[0067] Here, we will explain the grinding wheel for the plunge type grinding machine used for grinding. The surface roughness of the grinding wheel can be selected appropriately depending on the grinding efficiency and the type of material that constitutes the conductive layer. The roughness of the grinding wheel surface can be adjusted by the type of abrasive grain, grain size, degree of bonding, binder, structure (abrasive grain ratio), etc. The above "grain size" refers to the size of the abrasive grain, for example #80. The number in this case refers to the number of meshes per inch (25.4 mm) used to select the abrasive grains, and the larger the number, the finer the abrasive grains. The above "bonding degree of the abrasive grains" refers to hardness, and is expressed by the letters A to Z. The closer to A, the softer the bond, and the closer to Z, the harder the bond. The more binder the abrasive grains contain, the harder the bond of the grindstone will be. The above "structure of the abrasive grains (abrasive grain ratio)" refers to the volume ratio of the abrasive grains to the total volume of the grindstone, and the size of this structure indicates the coarseness or density of the structure. The larger the number indicating the structure, the coarser the structure. A grindstone with a large structure number and large pores is called a porous grindstone, and has the advantage of preventing clogging and burnt stone.

[0068] In general, this grinding wheel can be manufactured by mixing raw materials (abrasive, binder, pore agent, etc.), pressing, drying, sintering, and finishing. As the abrasive grains, green silicon carbide (GC), black silicon carbide (C), white alumina (WA), brown alumina (A), zirconia alumina (Z), etc. can be used. These materials can be used alone or in combination. As the binder, vitrified (V), resinoid (B), resinoid reinforced (BF), rubber (R), silicate (S), magnesia (Mg), shellac (E), etc. can be used as appropriate depending on the application. Here, the outer diameter shape of the grinding wheel in the longitudinal direction is preferably an inverted crown shape in which the outer diameter gradually decreases from the end to the center so that the conductive roller can be polished into a crown shape. The outer diameter shape of the grinding wheel is preferably an arc curve or a higher order curve of second degree or higher in the longitudinal direction. In addition, the outer diameter shape of the grinding wheel may be a shape expressed by various mathematical formulas such as a quartic curve or a sine function. The outer diameter shape of the grinding wheel is preferably one in which the change in the outer diameter changes smoothly, but it may also be a shape in which the arc curve or the like is approximated to a polygonal shape by straight lines. The width of the grinding wheel in the axial direction is preferably equal to or greater than the axial width of the conductive roller. By appropriately selecting a grindstone in consideration of the factors listed above and carrying out the grinding step under conditions that promote the difference in grindability between the domain and the matrix, it is possible to form convex portions derived from the domain.

[0069] Specifically, conditions under which polishing is suppressed and conditions using abrasive grains with a dull cutting edge are preferred. For example, by shortening the time of the precision polishing step after rough cutting and polishing with a treated grindstone, protrusions derived from the domains can be suitably formed. The treated grindstone may be, for example, a grindstone that has been treated with a rubber member, specifically, a grindstone that has been dressed with a rubber member containing abrasive grains and then the surface of the grindstone is polished to wear down the abrasive grains.

[0070] <Method for measuring the height of the first convexity (convexity derived from the domain)> A thin piece including the surface is taken from the conductive layer, and a micro-probe is used to confirm and measure the convex shape caused by the domain. The surface profile and electrical resistance profile of the thin piece sampled from the conductive member are measured using an SPM. This makes it possible to confirm that the convex portion is the first convex portion originating from the domain. At the same time, the height of the convex portion can be quantified and evaluated from the shape profile. The specific procedure will be described later.

[0071] <Method for measuring the domain distance Dm on the outer surface of a conductive material> When the length of the conductive layer in the longitudinal direction is L and the thickness of the conductive layer is T, samples are cut out using a razor from three locations, the center of the longitudinal direction of the conductive layer and L / 4 from both ends of the conductive layer toward the center, so as to include the outer surface of the charged member. The size of the sample is 2 mm in the circumferential direction and the longitudinal direction of the charged member, and the thickness is T, which is the thickness of the conductive layer. For each of the three samples obtained, analysis areas of 50 μm square are placed at three arbitrary locations on the surface corresponding to the outer surface of the charged member, and the three analysis areas are photographed at a magnification of 5000 times using a scanning electron microscope (product name: S-4800, manufactured by Hitachi High-Technologies Corporation). Each of the nine photographed images obtained is binarized using image processing software (product name: LUZEX; manufactured by Nireco Corporation). The binarization procedure is as follows. The captured image is converted to 8-bit grayscale to obtain a monochrome image with 256 gradations. The captured image is then binarized so that the domains in the captured image become black, obtaining a binarized image of the captured image. Next, for each of the nine binarized images, the distance between the walls of the domains is calculated, and their arithmetic mean value is calculated. This value is called Dm. The distance between the walls is the distance between the walls of the closest domains, and can be found by setting the measurement parameter to the distance between adjacent walls in the image processing software.

[0072] <Method of forming second convex portions (convex portions derived from resin particles)> The method of forming the second convex portion derived from the resin particles can be, for example, a method of exposing particles that have been kneaded in advance during the polishing process of polishing the surface of the conductive member. The material of the particles is not particularly limited as long as the kneaded particles can be exposed on the outer surface, but it is preferable that the material can secure a gap with the photosensitive drum and has a hardness higher than that of the rubber material constituting the conductive layer. If the hardness of the conductive layer is too low, the second convex portion will sink in due to contact with the photosensitive drum, making it impossible to form a gap. Furthermore, in order not to disturb the uniformity of the electric field in the domain and to prevent the injection of electric charges from the second convex portion into the photosensitive drum, the second convex portion needs to be insulating. 10 It indicates that the volume resistivity is Ωcm or more. The method for measuring the volume resistivity will be described later. As a material for the resin particles that has a high volume resistivity and can ensure the above hardness, organic resin particles containing a polymer material are preferable. Here, the polymer material refers to a material with a high molecular weight, and refers to a polymer obtained by polymerizing a monomer such as a semi-synthetic polymer or a synthetic polymer, or a compound with a high molecular weight such as a natural polymer.

[0073] Examples of organic resin particles include polyamide resin, silicone resin, fluororesin, (meth)acrylic resin, styrene resin, polyethylene resin, phenolic resin, polyester resin, melamine resin, urethane resin, olefin resin, epoxy resin, naphthalene resin, furan resin, xylene resin, divinylbenzene polymer, styrene-divinylbenzene copolymer, polyacrylonitrile resin, copolymers, modified products, and derivatives thereof, ethylene-propylene-diene copolymer (EPDM), styrene-butadiene copolymer rubber (SBR), silicone rubber, urethane rubber, and isoprene rubber (IR). Examples of suitable thermoplastic elastomers include rubbers such as butyl rubber, acrylonitrile-butadiene copolymer rubber (NBR), chloroprene rubber (CR), and epichlorohydrin rubber; thermoplastic elastomers such as polyolefin-based thermoplastic elastomers, urethane-based thermoplastic elastomers, polystyrene-based thermoplastic elastomers, fluororubber-based thermoplastic elastomers, polyester-based thermoplastic elastomers, polyamide-based thermoplastic elastomers, polybutadiene-based thermoplastic elastomers, ethylene-vinyl acetate-based thermoplastic elastomers, polyvinyl chloride-based thermoplastic elastomers, and chlorinated polyethylene-based thermoplastic elastomers. The spatial distance between the photosensitive drum and the outer surface of the conductive member can be controlled by the number of organic resin particles added that form the second convex portion and the particle size distribution. That is, the number of columns that support the gap between the photosensitive drum and the outer surface of the conductive member is large, and resin particles that can form many of them can form the gap favorably. Therefore, the average particle size Dp of the resin particles forming the second convex portions is preferably 4 μm or more and 50 μm or less.

[0074] <Method for measuring the gap between the conductive member and the photosensitive drum> The distance of the gap between the conductive member formed by the second convex portion and the photosensitive drum can be measured using a jig shown in Figure 9(a) to simulate the state in which a space is formed between the conductive layer 96 and the glass plate 92 by the second convex portion 95 as shown in Figure 9(b). 9(b), the spatial distance d between the glass plate 92 and the conductive layer 96 may be measured by any method, such as an optical microscope, a laser microscope, or an electron scanning microscope, as long as the method can measure the distance d through the glass plate 92. However, a laser microscope may be used for measurement because it can precisely measure the second convex portion on the order of micrometers. A specific procedure will be described later.

[0075] <Method of manufacturing conductive member> An example of a method for producing a conductive member according to the present disclosure is shown below. In this example, the production method is characterized by including the following steps (A) to (C), but is not particularly limited as long as the configuration of the present disclosure can be achieved.

[0076] Step (A): preparing a carbon master batch (hereinafter also referred to as "CMB") for domain formation, comprising carbon black and rubber; Step (B): preparing a matrix-forming rubber composition (hereinafter also referred to as "MRC"); Step (C): A step of kneading the CMB and the MRC to prepare a rubber composition having a matrix-domain structure. Step (D): A step of forming a conductive layer on a conductive support by a known method such as extrusion molding, injection molding, or compression molding using the rubber composition prepared in steps (A) to (C). The conductive layer may be attached to the conductive support via an adhesive as required. The conductive layer formed on the conductive support may be vulcanized as required, polished, and then subjected to a surface treatment such as ultraviolet light treatment. Furthermore, resin particles that will become the second convex portions can be added in step (B) or (C). It is particularly preferable to add the resin particles in step (C).

[0077] <Process cartridge> FIG. 7 is a schematic cross-sectional view of an electrophotographic process cartridge 100 having a conductive member according to an embodiment of the present disclosure as a charging member (charging roller). This process cartridge is configured to integrate a developing device and a charging device and be detachable from the main body of an electrophotographic device. The developing device is configured to integrate at least a developing roller 103, a toner container 106, and a toner 109, and may include a toner supply roller 104, a developing blade 108, and an agitating blade 110 as necessary. The charging device is configured to integrate at least a photosensitive drum 1-1 and a charging roller 102, and may include a cleaning blade 105 and a waste toner container 107. The charging roller 102, the developing roller 103, the toner supply roller 104, and the developing blade 108 are each configured to be applied with a voltage.

[0078] <Electrophotographic image forming apparatus> FIG. 8 is a schematic diagram of an electrophotographic image forming apparatus 200 using a conductive member according to an embodiment of the present disclosure as a charging member (charging roller). This apparatus is a color electrophotographic apparatus in which the four process cartridges 100 are detachably mounted. Each process cartridge uses toner of each color, black, magenta, yellow, and cyan. A photosensitive drum 201 rotates in the direction of the arrow and is uniformly charged by a charging roller 202 to which a voltage is applied from a charging bias power supply, and an electrostatic latent image is formed on the surface by exposure light 211. Meanwhile, toner 209 stored in a toner container 206 is supplied to a toner supply roller 204 by an agitating blade 210 and conveyed onto a developing roller 203. Then, a developing blade 208 arranged in contact with the developing roller 203 uniformly coats the toner 209 on the surface of the developing roller 203, and the toner 209 is charged by frictional charging. The electrostatic latent image is developed by the toner 209 conveyed by the developing roller 203 arranged in contact with the photosensitive drum 101, and is visualized as a toner image.

[0079] The visualized toner image on the photosensitive drum is transferred by a primary transfer roller 212 to which a voltage is applied by a primary transfer bias power supply, onto an intermediate transfer belt 215 supported and driven by a tension roller 213 and an intermediate transfer belt drive roller 214. The toner images of each color are superimposed in order to form a color image on the intermediate transfer belt. A transfer material 219 is fed into the apparatus by a paper feed roller, and is transported between an intermediate transfer belt 215 and a secondary transfer roller 216. A voltage is applied to the secondary transfer roller 216 from a secondary transfer bias power supply, and the secondary transfer roller 216 transfers the color image on the intermediate transfer belt 215 onto the transfer material 219. The transfer material 219 onto which the color image has been transferred is fixed by a fixing device 218, and is then discarded outside the apparatus, completing the printing operation. Meanwhile, the toner remaining on the photosensitive drum without being transferred is scraped off by a cleaning blade 205 and stored in a waste toner storage container 207, and the above-mentioned process is repeated for the cleaned photosensitive drum 201. In addition, the toner remaining on the primary transfer belt without being transferred is also scraped off by a cleaning device 217. Although a color electrophotographic device is shown as an example, in a monochrome electrophotographic device (not shown), the process cartridge uses only black toner. A monochrome image is formed directly on the transfer material by the process cartridge and the primary transfer roller (no secondary transfer roller) without the intermediate transfer belt. The image is then fixed by the fixing device and the paper is discharged outside the device, completing the printing operation. EXAMPLES

[0080] Next, the conductive members in the examples and comparative examples of the present disclosure were produced using the materials shown below.

[0081] <nbr> NBR (1) (Product name: JSR NBR N230SV, Acrylonitrile content: 35%, Mooney viscosity ML (1+4) 100℃: 32, SP value: 20.0 (J / cm 3 ) 0.5 , manufactured by JSR Corporation, abbreviation: N230SV) NBR (2) (Product name: JSR NBR N215SL, Acrylonitrile content: 48%, Mooney viscosity ML (1+4) 100℃: 45, SP value: 21.7 (J / cm 3 ) 0.5 , manufactured by JSR Corporation, abbreviation: N215SL) NBR (3) (Product name: Nipol DN401LL, Acrylonitrile content: 18.0%, Mooney viscosity ML (1+4) 100℃: 32, SP value: 17.4 (J / cm 3 ) 0.5 , manufactured by Zeon Corporation, abbreviation: DN401LL) <Isoprene rubber IR> Isoprene rubber (product name: Nipol IR2200L, Mooney viscosity ML (1+4) 100℃: 70, SP value: 16.5 (J / cm 3 ) 0.5 , manufactured by Zeon Corporation, abbreviation: IR2200L) <Butadiene rubber BR> Butadiene rubber (1) (product name: UBEPOL BR130B, Mooney viscosity ML (1+4) 100℃: 29, SP value: 16.8 (J / cm 3 ) 0.5 , manufactured by Ube Industries, Ltd., abbreviation: BR130B) Butadiene rubber (2) (product name: UBEPOL BR150B, Mooney viscosity ML (1+4) 100℃: 40, SP value: 16.8 (J / cm 3 ) 0.5 , manufactured by Ube Industries, abbreviated name: BR150B) <sbr> SBR (1) (product name: Asaprene 303, styrene content: 46%, Mooney viscosity ML (1+4) 100℃: 45, SP value: 17.4 (J / cm 3 ) 0.5 , manufactured by Asahi Kasei Corporation, abbreviation: A303) SBR (2) (product name: Tufden 2003, styrene content: 25%, Mooney viscosity ML (1+4) 100℃: 33, SP value: 17.0 (J / cm 3 ) 0.5 , manufactured by Asahi Kasei Corporation, abbreviation: T2003) SBR (3) (product name: Tufden 2100R, styrene content: 25%, Mooney viscosity ML (1+4) 100℃: 78, SP value: 17.0 (J / cm 3 ) 0.5 , manufactured by Asahi Kasei Corporation, abbreviation: T2100R) SBR (4) (product name: Tufden 2000R, styrene content: 25%, Mooney viscosity ML (1+4) 100℃: 45, SP value: 17.0 (J / cm 3 ) 0.5 , manufactured by Asahi Kasei Corporation, abbreviation: T2000R) SBR (5) (product name: Tufden 1000, styrene content: 18%, Mooney viscosity ML (1+4) 100℃: 45, SP value: 16.8 (J / cm 3 ) 0.5 , manufactured by Asahi Kasei Corporation, abbreviation: T1000) <Chloroprene rubber (CR)> Chloroprene rubber (product name: SKYPRENE B31, Mooney viscosity ML (1+4) 100℃: 40, SP value: 17.4 (J / cm 3 ) 0.5 , manufactured by Tosoh Corporation, abbreviation: B31) <epdm> EPDM (product name: Esprene505A, Mooney viscosity ML (1+4) 100℃: 47, SP value: 16.0 (J / cm 3 ) 0.5 (Manufactured by Sumitomo Chemical Co., Ltd., abbreviation: E505A)

[0082] <Conductive particles> Carbon black (1) (Product name: TOKABLACK♯5500, DBP absorption capacity: 155 cm 3 / 100g, manufactured by Tokai Carbon Co., Ltd., abbreviation: #5500) Carbon black (2) (Product name: TOKABLACK♯7360SB, DBP absorption capacity: 87 cm 3 / 100g, manufactured by Tokai Carbon Co., Ltd., abbreviation: #7360) Carbon black (3) (Product name: TOKABLACK♯7270SB, DBP absorption capacity: 62 cm 3 / 100g, manufactured by Tokai Carbon Co., Ltd., abbreviation: #7270) Carbon black (4) (Product name: #44, DBP absorption capacity: 78 cm 3 / 100g, manufactured by Mitsubishi Chemical Corporation, abbreviation: #44) Carbon black (5) (product name: Asahi #35, DBP absorption capacity: 50 cm 3 / 100g, manufactured by Asahi Carbon Co., Ltd., abbreviation: #35) Carbon black (6) (Product name: #45L, DBP absorption capacity: 45cm 3 / 100g, manufactured by Mitsubishi Chemical Corporation, abbreviation: #45L) Tin oxide (product name: S-2000, manufactured by Mitsubishi Materials Electronic Chemicals Co., Ltd., abbreviation: tin oxide) <Vulcanizing agent> Vulcanizing agent (1) (product name: SULFAX PMC, sulfur content 97.5%, manufactured by Tsurumi Chemical Industry Co., Ltd., abbreviation: sulfur) <Vulcanization accelerator> Vulcanization accelerator (1) (product name: Sancerer TBZTD, tetrabenzyl thiuram disulfide, manufactured by Sanshin Chemical Industry Co., Ltd., abbreviation: TBZTD) Vulcanization accelerator (2) (trade name: Noccela TBT, tetrabutyl thiuram disulfide, manufactured by Ouchi Shinko Chemical Industry Co., Ltd., abbreviation: TBT) Vulcanization accelerator (3) (product name: Noccela EP-60, vulcanization accelerator mixture, manufactured by Ouchi Shinko Chemical Industry Co., Ltd., abbreviation: EP-60) Vulcanization accelerator (4) (trade name: SANTOCURE-TBSI, Nt-butyl-2-benzothiazole sulfenimide, manufactured by FLEXSYS, abbreviation: TBSI) <Filling agent> Filler (1) (product name: Nanox #30, calcium carbonate, manufactured by Maruo Calcium Co., Ltd., abbreviation: #30) Filler (2) (product name: Nipsil AQ, silica, manufactured by Tosoh Corporation, abbreviation: AQ) <Resin particles> Polyethylene particles 1 (product name: Mipelon XM-221U, polyethylene resin, average particle size 25 μm, manufactured by Mitsui Chemicals, Inc.) Polyethylene particles 2 (product name: Mipelon PM-200, polyethylene resin, average particle size 25 μm, manufactured by Mitsui Chemicals, Inc.) Acrylic particles (product name: Ganzpearl GM-2801, polymethacrylate resin, average particle size 28 μm, manufactured by Aica Kogyo Co., Ltd.) Acrylic particles 2 (product name: Ganzpearl GM-0401S, polymethacrylate resin, average particle size 28 μm, manufactured by Aica Kogyo Co., Ltd.) - Urethane particles (product name: Art Pearl C-300T, polyurethane resin, average particle size 22μm, manufactured by Negami Chemical Industries Co., Ltd.) Graphitized carbon particles (product name: Nika Beads PC-1020, graphitized carbon resin, average particle size 10 μm, manufactured by Nippon Carbon Co., Ltd.)

[0083] The conductive member, process cartridge, and electrophotographic image forming apparatus of the present disclosure will be specifically described below in detail, but the technical scope of the present disclosure is not limited thereto. First, a method for producing the conductive member in the examples and comparative examples of the present disclosure will be specifically described.

[0084] <Example 1> [1-1. Preparation of carbon master batch (CMB) for domain formation] The materials shown in Table 1 were mixed in a 6L pressure kneader (product name: TD6-15MDX, manufactured by Toshin Corporation) to obtain CMB for domain formation. The mixing conditions were a filling rate of 70 vol%, a blade rotation speed of 30 rpm, and 16 minutes.

[0085] [Table 1]

[0086] [1-2. Preparation of rubber composition for forming matrix] The materials shown in Table 2 were mixed in the amounts and types shown in Table 2 in a 6 L pressure kneader (product name: TD6-15MDX, manufactured by Toshin Co., Ltd.) to obtain a rubber composition for forming a matrix. The mixing conditions were a filling rate of 70 vol%, a blade rotation speed of 30 rpm, and 18 minutes.

[0087] [Table 2]

[0088] The materials of the types and amounts shown in Table 3 were mixed with an open roll to prepare a rubber composition for forming a conductive resin layer. An open roll with a roll diameter of 12 inches was used as the mixer. The mixing conditions were a front roll rotation speed of 10 rpm, a rear roll rotation speed of 8 rpm, a roll gap of 2 mm, and a total of 20 left and right turns, followed by 10 thin passes with a roll gap of 1.0 mm.

[0089] [Table 3]

[0090] <2. Molding of conductive materials> A round bar with a total length of 252 mm and an outer diameter of 6 mm was prepared, the surface of which was made of free-cutting steel and electroless nickel plating was applied. Next, an adhesive (product name: Metalock U-20, manufactured by Toyo Kagaku Kenkyusho Co., Ltd.) was applied to the entire circumference of the round bar, over a range of 230 mm, excluding 11 mm at each end, using a roll coater. In this example, the round bar coated with the adhesive was used as a conductive support. Next, a die with an inner diameter of 10.0 mm was attached to the tip of a crosshead extruder having a mechanism for feeding the conductive support and a mechanism for discharging the unvulcanized rubber roller, and the temperature of the extruder and the crosshead was adjusted to 100° C., and the conveying speed of the conductive support was adjusted to 60 mm / sec. Under these conditions, the rubber composition for forming a conductive resin layer was fed from the extruder, and the outer periphery of the conductive support was coated with the rubber composition for forming a conductive resin layer in the crosshead, to obtain an unvulcanized rubber roller. Next, the unvulcanized rubber roller was placed in a hot air vulcanizing furnace at 170°C and heated for 60 minutes to vulcanize the unvulcanized rubber composition, thereby obtaining a conductive roller having a conductive resin layer formed on the outer periphery of the conductive support. After that, 10 mm of each end of the conductive resin layer was cut off, making the longitudinal length of the conductive resin layer 232 mm.

[0091] [2-1. Conductive layer polishing] Next, the surface of the conductive layer was polished under the polishing conditions described below in Polishing Condition 1 to obtain a crown-shaped conductive member 1 having a diameter of 8.5 mm at the center and a diameter of 8.44 mm at each position 90 mm from the center to both ends. (polishing condition 1) A cylindrical grinding wheel (manufactured by Teiken Co., Ltd.) with a diameter of 305 mm and a length of 235 mm was prepared. The type, grain size, degree of bonding, bonding agent, and structure (abrasive grain ratio) of the abrasive grains are as follows: Abrasive material: GC (green silicon carbide), (JIS R6111-2002) Abrasive grain size: #80 (average grain size 177μm JIS B4130) Abrasive grain bond: HH (JIS R6210) · Binder: V4PO (vitrified) · Grain structure (abrasive grain ratio): 23 (abrasive grain content 16% JIS R6242) The polishing conditions were a grinding wheel rotation speed of 2100 rpm and a conductive member rotation speed of 250 rpm. In the rough cutting process, the grinding wheel was inserted into the conductive member at a penetration speed of 20 mm / sec, and penetrated 0.24 mm after contacting the outer peripheral surface of the conductive member. For the precision polishing process, the penetration speed was changed to 0.5 mm / sec, and after penetrating 0.01 mm, the grindstone was removed from the conductive member to complete the polishing. The polishing method used was the upper cut method, in which the grindstone and the conductive member rotate in the same direction.

[0092] Conductive members 2 to 51 were produced in the same manner as conductive member 1, except that the starting materials shown in Tables 4-1 to 4-5 and the polishing conditions shown below were changed. The parts by mass and physical properties of the starting materials used in producing each conductive member are shown in Tables 4-1 to 4-5.

[0093] Polishing conditions 2 to 5 are shown in detail below. (Polishing conditions 2) The polishing conditions were the same as those in 1, except that the penetration speed in the precision polishing process was 2.0 mm / sec. (Polishing condition 3) The polishing conditions were the same as those in 1, except that the penetration speed in the precision polishing process was 1.0 mm / sec. (polishing condition 4) The polishing conditions were the same as those in 1, except that the penetration speed in the precision polishing process was 0.2 mm / sec. (Polishing condition 5) The polishing conditions were the same as those in 1, except that the penetration speed in the precision polishing process was changed to 0.1 mm / sec, and polishing was continued for 4 seconds after penetration of 0.01 mm. The results are shown in Tables 5-1 to 5-5.

[0094] [Table 4-1]

[0095] [Table 4-2]

[0096] [Table 4-3]

[0097] [Table 4-4]

[0098] [Table 4-5]

[0099] <3. Characterization> Next, the characteristic evaluations for the following items in the examples and comparative examples of the present disclosure will be described below. <3-1. Confirmation of matrix-domain structure> The presence of a matrix-domain structure in the conductive layer was confirmed by the following method. A slice (500 μm thick) was cut out using a razor so that a cross section perpendicular to the longitudinal direction of the conductive layer of the conductive member could be observed. Then, platinum was vapor-deposited on the surface of the slice corresponding to the cross section of the conductive layer. The platinum-deposited surface of the slice was photographed at 1000 times using a scanning electron microscope (SEM) (product name: S-4800, manufactured by Hitachi High-Technologies Corporation) to obtain an SEM image. When a structure in which a plurality of domains are dispersed in a matrix and the matrix is ​​connected was confirmed in the SEM image, the matrix-domain structure was judged to be "present."

[0100] <3-2. How to measure the maximum Feret diameter, perimeter, and envelope perimeter of a domain> The maximum Feret diameter, perimeter, and envelope perimeter of the domain according to the present disclosure were measured as follows. First, a thin slice (thickness 1 μm) including a cross section of the entire thickness of the conductive layer was cut out from the conductive layer of the conductive member using a microtome (trade name: Leica EM FCS, manufactured by Leica Microsystems) so that a cross section perpendicular to the longitudinal direction of the conductive layer of the conductive member could be observed. The positions of the cutout from the conductive layer were the center in the longitudinal direction and three positions at L / 4 from both ends of the conductive layer toward the center, where L is the longitudinal length of the conductive layer and T is the thickness of the conductive layer. For each of the obtained flakes, platinum was vapor-deposited on the surface corresponding to the cross section of the elastic layer. Next, the platinum-deposited surface of the flakes was photographed at 5,000 times magnification using a scanning electron microscope (SEM) (trade name: S-4800, manufactured by Hitachi High-Technologies Corporation) to obtain an SEM image. The obtained SEM image was converted to 8-bit grayscale using image processing software (trade name: ImageProPlus, manufactured by Media Cybernetics) to obtain a monochrome image with 256 gradations. Next, the black and white of the image were inverted so that the domains in the monochrome image became white, and a binarization threshold was set for the brightness distribution of the image based on the algorithm of Otsu's discriminant analysis method, and a binarized image was obtained. For the obtained binary image, square observation areas with sides of 20 μm were placed at three arbitrary locations in a thickness region of 0.1T to 0.9T depth from the outer surface of the conductive layer (the surface opposite to the surface facing the support), where T is the thickness of the conductive layer, and the maximum Feret's diameter, perimeter A, and envelope perimeter B were calculated for each of the domains present in each observation area using the counting function of the image processing software. The A / B value was calculated using the perimeter and envelope perimeter measured for each domain observed in each observation area.The percentage of domains that satisfied requirement (B2) among all observed domains was then calculated.

[0101] <3-3.Measuring method for volume resistivity of matrix> The volume resistivity of the matrix was measured using a scanning probe microscope (SPM) (product name: Q-Scope250, manufactured by Quesant Instrument Corporation) in contact mode as follows. The measurement environment was a temperature of 23° C. and a humidity of 50% RH. First, a thin piece was cut out from the conductive layer in the same manner as in 3-2 above. Next, the thin piece was placed on the surface of a metal plate so that one surface of the piece corresponding to the cross section of the elastic layer was in contact with the surface of the metal plate. Then, the cantilever of the SPM was brought into contact with the portion of the surface of the piece opposite to the surface in contact with the metal plate, which corresponds to the matrix. Next, a voltage of 50 V was applied to the cantilever, and the current value was measured. In addition, the surface shape of the measurement piece was measured with the SPM, and the thickness of the measurement point was calculated from the obtained height profile. The volume resistivity of the measurement point was calculated from the thickness of the measurement point and the current value. The measurements were performed at three arbitrary points in the matrix portion of the thin piece in a region corresponding to a thickness region of 0.1T to 0.9T depth from the outer surface of the conductive layer (the surface opposite to the surface facing the support), where T is the thickness of the conductive layer. The arithmetic mean value of the volume resistivity calculated from the measurement results at a total of nine points obtained from each thin piece was taken as the volume resistivity of the matrix of the conductive member to be measured. The evaluation results are shown in Tables 5-1 and 5-2.

[0102] <3-4. Measurement method for DBP absorption of carbon black> The DBP absorption amount of carbon black was measured in accordance with Japanese Industrial Standards (JIS) K 6217. <3-5. Measurement method of arithmetic mean C, standard deviation σm, coefficient of variation σm / C of distance between conductive carbon black walls in a domain, and ratio of cross-sectional area of ​​carbon black contained in the domain to domain area> The arithmetic mean C of the distance between the conductive carbon black wall surfaces in a domain, the standard deviation σm, the coefficient of variation σm / C, and the ratio of the cross-sectional area of ​​the carbon black contained in the domain to the domain area were measured as follows. First, a portion of the platinum-deposited surface of the sample prepared in 3-2. above, corresponding to the observation area measuring 20 μm on a side placed on the binary image in the evaluation in 3-2. above, was photographed at a magnification of 20,000 times using a scanning electron microscope (SEM) (product name: S-4800, manufactured by Hitachi High-Technologies Corporation) to obtain an SEM image. The arithmetic mean wall-to-wall distance of the carbon black in the domain and the area of ​​the carbon black were obtained by quantifying the SEM image. That is, the SEM image was converted to 8-bit grayscale using an image analyzer (product name: LUZEX-AP, manufactured by Nireco Corporation) to obtain a monochrome image with 256 gradations. Next, the black and white of the image were inverted so that the domains in the fracture surface became white, and a binarization threshold was set for the brightness distribution of the image based on the algorithm of Otsu's discriminant analysis method to obtain a binarized image. Next, an observation area of ​​a size in which at least one domain can be accommodated was extracted from the binarized image. Then, the wall-to-wall distance Ci of the carbon black in the domain was calculated. Then, the arithmetic mean of the wall-to-wall distance was calculated to calculate the arithmetic mean wall-to-wall distance C. The cross-sectional area of ​​the domain and the cross-sectional area of ​​the carbon black in the domain were also calculated. From these results, the ratio (number %) of the number of domains that satisfy the requirement (B1) to the number of all domains observed was calculated. In addition, based on the results of 3-2 above, the percentage of domains that satisfy requirements (B1) and (B2) was calculated. In addition, the standard deviation σm was calculated from the distance between the conductive carbon black walls in the obtained domain and its arithmetic mean C. The standard deviation σm was divided by the arithmetic mean C to calculate the coefficient of variation σm / C. Furthermore, for domains satisfying requirements (B1) and (B2), the arithmetic mean values ​​of the wall distance C of the carbon black, the coefficient of variation σm / C, and the ratio of the cross-sectional area of ​​the carbon black to the cross-sectional area of ​​the domain were calculated. Furthermore, for domains satisfying requirements (B1) and (B2), the arithmetic mean value of A / B and the arithmetic mean value of the maximum Feret diameter were calculated. The results are shown in Tables 5-3 to 5-5.

[0103] <3-6. SP value of rubber constituting the matrix and domain> The SP value was measured using a conventional swelling method. That is, the rubbers constituting the matrix and domains were each separated using a manipulator or the like, immersed in solvents with different SP values, and the degree of swelling was measured from the change in mass of the rubber. The Hansen solubility parameter (HSP) was calculated by analyzing the swelling value for each solvent. It is possible to calculate with high accuracy by creating a calibration curve using materials with known SP values. The known SP value can also be the value in the catalog of the material manufacturer. The evaluation results are shown in Tables 5-1 and 5-2.

[0104] <3-7.Measuring method for impedance of conductive material> The impedance of the conductive member was measured by the following method. First, while rotating the conductive member, platinum was vapor-deposited onto its outer surface to create an electrode. At this time, masking tape was used to create an electrode with a width of 1.5 cm and uniformity in the entire circumference. By forming this type of electrode, the contribution of the contact area between the measurement electrode and the conductive member due to the surface roughness of the conductive member can be minimized. Next, an aluminum sheet was wrapped around the electrode so as to be in contact with the platinum vapor-deposited film, to form a measurement sample as shown in FIG. An impedance measuring device (Solatron 126096W, Toyo Corporation) was then connected to the aluminum sheet and to the conductive support. The impedance was measured at a temperature of 23°C and a relative humidity of 50%, with an oscillating voltage of 1 Vpp and a frequency of 1.0 Hz, to obtain the absolute value of the impedance. The conductive member (longitudinal length: 232 mm) was divided into 5 equal regions in the longitudinal direction, and a measurement electrode was formed at one arbitrary point in each region, for a total of 5 points, and the above measurement was performed. The average value was taken as the impedance of the conductive member. The evaluation results are shown in Tables 5-1 and 5-2.

[0105] <3-8. Measurement of the height of the first convexity (convexity derived from the domain)> A thin slice having a thickness of 1 μm is cut out from the conductive layer of the conductive member at a cutting temperature of −100° C. using a microtome (trade name: Leica EM FCS, manufactured by Leica Microsystems). At this time, the thin slice is perpendicular to the axis of the conductive support. The cutting positions from the conductive layer were set at three positions: the center in the longitudinal direction, and L / 4 from both ends of the conductive layer toward the center, where L is the longitudinal length of the conductive layer. Next, the surface of the conductive member was measured using an SPM (MFP-3D-Origin, Oxford Instruments Co., Ltd.) under the following conditions for the slice containing the surface of the conductive member obtained as described above. The electrical resistance profile and shape profile were measured by this measurement. Oxford Instruments MFP-3D-Origin Measurement mode: AM-FM mode Probe: Olympus OMCL-AC160TS ·Resonance frequency: 251.825~261.08kHz Spring constant: 23.59~25.18N / m Scan speed: 0.8~1.5Hz Scan size: 10μm, 5μm, 3μm Target Amplitude: 3V and 4V Set Point: All 2V Next, it was confirmed that the convex portions in the profile of the surface shape obtained by the above measurement were derived from domains having higher electrical conductivity than the surrounding area in the electrical resistance profile. Furthermore, the height of the first convex portion was calculated from the profile. The calculation method was to obtain the difference between the arithmetic mean value of the domain-derived shape profile and the arithmetic mean value of the adjacent matrix shape profile. The arithmetic mean value was calculated from the measurement values ​​of 20 randomly selected convex portions in each of the slices cut from the above three places. The values ​​are shown in Tables 5-3 to 5-5.

[0106] <3-9. Measurement of domain distance Dm on the outer surface of a conductive material> The domain distance Dm on the outer surface of the conductive member was measured as follows. When observing the outer surface of the conductive member and measuring Dm, a measurement sample was cut out with a razor from the surface of the conductive member to a length of about 2 mm in the circumferential direction and the longitudinal direction of the conductive layer of the conductive member, and a depth of about 500 μm including the surface of the conductive member. The positions of the cutouts from the conductive layer were the center in the longitudinal direction and three positions at L / 4 from both ends of the conductive layer toward the center, where L is the longitudinal length of the conductive layer. Platinum was vapor-deposited on the surface of the obtained slice corresponding to the outer surface of the conductive member. Next, a 5000x SEM image of the platinum-deposited surface of the slice was obtained using a scanning electron microscope (product name: S-4800, manufactured by Hitachi High-Technologies Corporation). A binarized image was obtained from the obtained SEM image using image processing software (product name: LUZEX, manufactured by Nireco Corporation). The binarization procedure was as follows. The observed image was converted to an 8-bit grayscale to obtain a monochrome image with 256 gradations. Then, the black and white of the image were inverted so that the domains in the fracture surface became white, and a binarization threshold was set for the brightness distribution of the image based on the algorithm of Otsu's discriminant analysis method to obtain a binarized image. Next, the distribution of the distance between the walls of the domains was calculated for the binarized image, and the arithmetic mean value Dm of the distribution was calculated. The distance between the walls is the shortest distance between the walls of adjacent domains. Specifically, in the image processing software, the measurement parameter was set as the distance between adjacent wall surfaces. Here, the arithmetic mean value of 10 observation images randomly selected on the outer surface of the conductive member was adopted as the distance between adjacent wall surfaces of the conductive member, and the values ​​are shown in Tables 5-3 to 5-5.

[0107] <3-10. Measurement of the space between the conductive member and the glass plate> A jig having the mechanism shown in FIG. 9(a) and a glass plate were used. A jig having a lower stage 91, an upper stage 93, and a load meter 94 shown in Fig. 9(a) was used. The lower stage was configured so that a charged member could be placed thereon and could be moved vertically up and down. In addition, the load applied when the conductive member was pressed against the glass plate could be detected by the load meter 94. The lower stage on which the conductive member was placed was moved vertically upward, and pressed against a 20 mm square, 2 mm thick glass plate (material: BK7, surface accuracy: double-sided optically polished surface, parallelism: within 1 arcmin) 92 set on the upper stage with a load of 500 g. Then, the surface shape of the conductive member pressed against the glass plate was measured from the glass plate side using a laser microscope (product name: VK-8700, manufactured by Keyence Corporation) with a stage modified so that the jig could be installed, and the contact surface between the conductive member and the glass plate was measured from the glass plate side. The observation magnification was 160 times. In the surface profile obtained in the shape measurement, the nip width (nip length in the circumferential direction) L μm was measured by pressing the glass of the cross-sectional profile, and the distance of the flat part was measured. Next, a scan measurement was performed in the height direction for the contact nip portion, and the spatial volume V1 (μm) of the space formed between the conductive member and the glass surface in the region of [nip width L μm] × [longitudinal direction A μm in the measurement range] was measured. 3 ) was calculated. Furthermore, the formula: d=V1 / (L×A) The spatial distance d was obtained by the method described above, and the average value was calculated. The above measurements were performed at three locations, one at the center of the conductive member in the longitudinal direction, and 90 mm from the center toward both ends, and three locations in the circumferential direction (at 120 degree intervals), for a total of nine locations. The arithmetic average of the measurements at these nine locations was calculated as the gap distance (μm) in the nip between the conductive member and the photosensitive drum. The evaluation results are shown in Tables 5-3 to 5-5.

[0108] <3-11. Measurement of volume resistivity ρp of the second convex portion (convex portion derived from resin particles)> The volume resistivity ρp of the second convex portion was measured as follows. When observing the outer surface of the conductive member and measuring ρp, a measurement sample was cut out with a razor from the surface of the conductive member, with a length of approximately 2 mm in the circumferential and longitudinal directions of the conductive layer of the conductive member, and a depth of approximately 500 μm including the surface of the conductive member. The electrical resistance profile was measured for the surface of the slice corresponding to the outer surface of the conductive member by the same method as in <Measurement of the height of the first convex portion (convex portion derived from the domain)>, and the volume resistivity ρp derived from the resin particles, which are the second convex portions, was measured. The above measurements were performed at a total of nine locations, including the center of the conductive member in the longitudinal direction, three locations 90 mm from the center toward both ends, and three locations in the circumferential direction (120 degree intervals). The arithmetic average value of the measurements at these nine locations was calculated as the volume resistivity ρp derived from the resin particles, which are the second convex portions. The evaluation results are shown in Table 5.

[0109] <4. Image evaluation> [4-1] Fog evaluation In order to confirm the uniformity of discharge when the prepared conductive member was used as a charging member, the following evaluation was carried out. First, a laser printer (product name: Laserjet M608dn, manufactured by HP) was prepared as an electrophotographic device. The laser printer was then modified so that any voltage could be applied to the charging member, developing member, and intermediate transfer belt from an external power source (product name: Model 615, manufactured by Trek Japan). In addition, the penetration depth of the cleaning blade into the photosensitive drum was reduced. Next, the conductive member, the modified electrophotographic image forming apparatus, and the process cartridge were left in an environment of 30°C and 80% RH for 48 hours. Then, the process cartridge incorporating the prepared conductive member as a charging member was loaded into the laser printer. Then, a direct current voltage of -1700V was applied to the conductive support of the conductive member, a voltage was applied to the developing member so that Vback (a voltage of the difference between the surface potential of the photoreceptor and the voltage applied to the developing member) was -350V, and further, an image forming condition was established such that the voltage applied to the intermediate transfer belt was 2000V. Then, a white solid image was output in an environment of a temperature of 30°C and a relative humidity of 80%, and the fog on the white solid image was observed and evaluated by the following method. The evaluation result at this time is also called the "initial fog number". Next, under the same environment, using the above laser printer, while maintaining the image formation conditions, 500,000 images (hereinafter also referred to as "E letter images") were formed in which the letter "E" of 4 points was printed so that the coverage rate of the area of ​​A4 size paper was 1%. Then, one solid white image was output. The fog on the obtained solid white image was observed and evaluated by the following method. The evaluation result at this time is also referred to as "number of fogs after durability test". Here, the developer installed in the laser printer is negatively charged. Therefore, when a solid white image is output, the developer does not transfer to the photoconductor or paper. However, as described above, when the charging bias is increased, a localized strong discharge from the charging member may cause an excessively charged portion on the surface of the photoconductor. A small amount of positively charged developer present in the developer transfers to the excessively charged portion of the photoconductor, and as a result, even when a solid white image is formed, black spots originating from the developer are observed, and so-called "fogging" occurs on the solid white image. This phenomenon is more likely to occur when Vback is large, such as -350V.

[0110] (Method of evaluating fogging) Nine random points on the solid white image were observed at 500x magnification using an optical microscope, and the number of black spots caused by toner particles present in a 400 μm square observation area was counted, and this number was taken as the number of fog spots on the paper. In the present disclosure, the initial fog count is preferably 200 or less, more preferably 150 or less. It is also preferable that the ratio of the fog count after durability testing to the initial fog count is suppressed to 130% or less, particularly 115% or less. The evaluation results are shown in Tables 5-1 and 5-3.

[0111] <Examples 2 to 5> Conductive members 2 to 5 were produced in the same manner as in Example 1, except that the polishing conditions in Example 1 were changed to polishing conditions 2 to 5, and evaluations were performed in the same manner as in Example 1. The results of each evaluation in Examples 2 to 5 are shown in Tables 5-1 and 5-3.

[0112] <Examples 6 to 57> Similarly to the conductive member 1 in Example 1, conductive members 6 to 57 were used as charging rollers, and evaluations were carried out in the same manner as in Example 1. The results of each evaluation in Examples 6 to 57 are shown in Tables 5-1 to 5-5.

[0113] <Example 58> Conductive member 58 was produced by subjecting conductive member 1 of Example 1 to ultraviolet treatment as a surface treatment. Otherwise, evaluations were performed in the same manner as in Example 1. The evaluation results are shown in Tables 5-2 and 5-5. (UV surface treatment) While rotating the conductive member, the surface of the conductive member was irradiated with ultraviolet light for 5 minutes using a low-pressure mercury lamp (Harrison Toshiba Lighting Co., Ltd.). The low-pressure mercury lamp mainly irradiated ultraviolet light with a wavelength of 254 nm, and the cumulative amount of ultraviolet light at this time was approximately 10,000 mJ / cm. 2 (UV intensity was 35mW / cm 2 ).

[0114] [Table 5-1]

[0115] [Table 5-2]

[0116] [Table 5-3]

[0117] [Table 5-4]

[0118] [Table 5-5]

[0119] <Comparative Example 1> A round bar similar to that in Example 1 was used as the conductive support, and the carbon master batch for domain formation (CMB), rubber composition for matrix formation (MRC), and rubber composition for conductive layer formation were changed to those shown in Table 6. A conductive layer was produced in the same manner as in Example 1, except that the MRC for matrix formation was not used. A surface layer was then formed on the conductive layer as described below to produce a conductive roller.

[0120] [Table 6-1]

[0121] [Table 6-2]

[0122] The raw materials in Tables 6-1 and 6-2 above are as follows. CG102: Epichlorohydrin rubber (EO-EP-AGE ternary compound) (Product name: Epichromer CG102, SP value: 18.5 (J / cm 3 )0.5, manufactured by Osaka Soda Co., Ltd. LV: Quaternary ammonium salt (product name: Adeka Cizer LV70, manufactured by ADEKA Corporation) P202: Aliphatic polyester plasticizer (product name: Polycizer P-202, manufactured by DIC Corporation) MB: 2-mercaptobenzimidazole (product name: Nocrac MB, manufactured by Ouchi Shinko Chemical Industry Co., Ltd.) TS: Tetramethylthiuram monosulfide (product name: Noccela TS, manufactured by Ouchi Shinko Chemical Industry Co., Ltd.) DM: Di-2-benzothiazolyl disulfide (DM) (product name: Noccela DM-P (DM), manufactured by Ouchi Shinko Chemical Industry Co., Ltd.) EC600JD: Ketjen Black (Product name: Ketjen Black EC600JD, manufactured by Lion Specialty Chemicals Co., Ltd.) PW380: Paraffin oil (product name: PW-380, manufactured by Idemitsu Kosan Co., Ltd.) 25-B-40: 2,5-dimethyl-2,5-di(t-butylperoxy)hexyne (trade name: Perhexa 25B-40, manufactured by Nippon Oil Corporation) TAIC-M60: Triallyl isocyanurate (product name: TAIC-M60, manufactured by Mitsubishi Chemical Corporation) Next, a surface layer was further provided on the conductive layer of the conductive layer roller obtained above according to the following method to produce a two-layer conductive member C1, which was evaluated in the same manner as in Example 1. The evaluation results are shown in Table 8. First, methyl isobutyl ketone was added to the caprolactone-modified acrylic polyol solution to adjust the solid content to 10% by mass. A mixed solution was prepared using the materials shown in Table 7 below for 1000 parts by mass of this acrylic polyol solution (100 parts by mass of solid content). At this time, the mixture of block HDI and block IPDI had "NCO / OH=1.0".

[0123] [Table 7]

[0124] Next, 210 g of the above mixed solution and 200 g of glass beads having an average particle size of 0.8 mm as media were mixed in a 450 mL glass bottle, and pre-dispersed for 24 hours using a paint shaker disperser to obtain a coating material for forming a surface layer. The conductive roller obtained above was immersed in the coating material for forming the surface layer by a dipping method with its lengthwise direction being vertical. The immersion time for the dip coating was 9 seconds, and the lifting speed was an initial speed of 20 mm / sec and a final speed of 2 mm / sec, during which the speed was changed linearly with respect to time. The obtained coating material was air-dried at room temperature for 30 minutes, then dried in a hot air circulation dryer set at 90°C for 1 hour, and further dried in a hot air circulation dryer set at 160°C for 1 hour.

[0125] [Table 8]

[0126] In this comparative example, the conductive member C1 has a two-layer structure of an ion-conductive conductive layer and an electron-conductive surface layer, but the surface layer does not have a matrix-domain structure. This reduces the uniformity of dispersion of the conductive particles, causing electric field concentration, making it easy for excess charge to flow through the conductive path. In addition, this comparative example has a second convex portion. Therefore, the initial number of fog particles on paper was 380, and the number of fog particles on paper after durability test was 409, resulting in a change rate of fog on paper of 108 percent.

[0127] <Comparative Example 2> A conductive member C2 was produced and evaluated in the same manner as in Example 1, except that the domain-forming CMB was changed to one shown in Table 6-1 and no matrix-forming MRC was used. The evaluation results are shown in Table 8. In this comparative example, the conductive layer of the conductive member C2 does not have a matrix-domain structure, and is composed only of domain material, so that electric field concentration occurs in the conductive layer, and excess charge is likely to flow in the conductive path. In addition, this comparative example has a second convex portion. Therefore, the initial number of fogs on paper was 484, and the number of fogs on paper after durability was 522, and the change rate of fog on paper was 108%.

[0128] <Comparative Example 3> A conductive member C3 was produced and evaluated in the same manner as in Example 1, except that the domain-forming CMB and the matrix-forming MRC were changed to those shown in Table 6-1. The evaluation results are shown in Table 8. In this comparative example, the conductive member C3 has a domain and a matrix, but the number of domains that satisfy the requirements (B1) and (B2) is small, and the domain shape is irregular, so excessive charge migration occurs due to electric field concentration resulting from the domain shape. In addition, this comparative example has a configuration with a second convex portion. Therefore, the initial number of fogs on paper was 412, and the number of fogs on paper after durability test was 440, and the rate of change in fog on paper was 107%.

[0129] <Comparative Example 4> A conductive member C4 was produced and evaluated in the same manner as in Example 1, except that the domain-forming CMB and the matrix-forming MRC were changed to those shown in Table 6-1. The evaluation results are shown in Table 8. In this comparative example, conductive particles are added to the matrix of the conductive member C4, so the volume resistivity is low, and the conductive member has a single conductive path, and the conductive layer is configured such that electric field concentration occurs and excess charge easily flows through the conductive path. In addition, this comparative example has a second convex portion. Therefore, the initial number of fog particles on the paper was 440, and the number of fog particles on the paper after the durability test was 476, and the change rate of fog on the paper was 108%.

[0130] <Comparative Example 5> A conductive member C5 was produced and evaluated in the same manner as in Example 1, except that the domain-forming CMB and the matrix-forming MRC were changed to those shown in Table 6-1. The evaluation results are shown in Table 8. In this comparative example, the conductive member C5 has a matrix-domain structure, but since no conductive agent is added to the domain, the volume resistivity is high, and since conductive particles are added to the matrix, the volume resistivity is low. In other words, since the conductive member has a single conductive path, electric field concentration occurs in the conductive layer, and excess charge is likely to flow in the conductive path. In addition, this comparative example has a second convex portion. Therefore, the initial number of fogs on paper was 420, and the number of fogs on paper after durability was 448, and the change rate of fog on paper was 107%.

[0131] <Comparative Example 6> A conductive member C6 was produced and evaluated in the same manner as in Example 1, except that the domain-forming CMB and the matrix-forming MRC were changed to those shown in Table 6-1. The evaluation results are shown in Table 8. In this comparative example, the conductive member C6 does not have a matrix-domain structure, but has a bicontinuous structure of the conductive phase and the insulating phase. In other words, since the conductive member has a single conductive path, electric field concentration occurs in the conductive layer, and excess charge is likely to flow in the conductive path. In addition, this comparative example has a second convex portion. Therefore, the initial number of fogs on paper was 428, and the number of fogs on paper after durability was 457, and the change rate of fog on paper was 107%.

[0132] <Comparative Example 7> A conductive member C7 was produced and evaluated in the same manner as in Example 1, except that the domain-forming CMB and the matrix-forming MRC were changed to those shown in Table 6-2. The evaluation results are shown in Table 8. In this comparative example, the conductive member C7 has a matrix-domain structure, but the domains that satisfy the requirements (B1) and (B2) account for 80% or less by number. The reason for this is thought to be that the amount of carbon black added to the domains is small, and the amount of carbon gel was not sufficient to form, so the domain shape was not spherical, resulting in large irregularities and a large aspect ratio. As a result, the conductive layer is configured such that electric field concentration occurs and excess charge easily flows through the conductive path. In addition, this comparative example has a configuration having a second convex portion. Therefore, the initial number of fogs on paper was 388, and the number of fogs on paper after durability was 395, resulting in a change rate of fog on paper of 102%.

[0133] <Comparative Example 8> A conductive member C8 was produced and evaluated in the same manner as in Example 1, except that the domain-forming CMB and the matrix-forming MRC were changed to those shown in Table 6-2. The evaluation results are shown in Table 8. In this comparative example, the conductive member C8 had a matrix-domain structure, but the number of domains satisfying the requirements (B1) and (B2) was 0%. This is believed to be due to the following two reasons. (1) Since reinforcing silica is added, the carbon master batch that forms the domains has a high viscosity, and the viscosity difference between the carbon master batch and the rubber composition for forming the matrix is ​​large. (2) The difference in SP value between the first rubber and the second rubber is large. Therefore, it is considered that the domain shape was not spherical, and the unevenness and aspect ratio became large. As a result, the electric field concentration occurred in the conductive layer, and the configuration made it easy for excess charge to flow in the conductive path. In addition, this comparative example had a configuration with a second convex portion. Therefore, the initial number of fog particles on the paper was 528, and the number of fog particles on the paper after the durability test was 541, and the rate of change in fog on the paper was 102 percent.

[0134] <Comparative Example 9> A conductive member C9 was produced and evaluated in the same manner as in Example 1, except that the domain-forming CMB was changed to rubber particles obtained by heat-vulcanizing the conductive layer-forming rubber of Comparative Example 2 alone and then freezing and pulverizing it, and the matrix-forming MRC was changed to that shown in Table 6-2. The evaluation results are shown in Table 8. In this comparative example, the conductive member C9 has a matrix-domain structure, but the domains that satisfy the requirements (B1) and (B2) accounted for 0% by number. The reason for this is that large, anisotropic conductive rubber particles formed by freeze pulverization are dispersed. As a result, electric field concentration occurs in the conductive layer, making it easy for excess charge to flow in the conductive path. In addition, this comparative example has a second convex portion. Therefore, the initial number of fog particles on paper was 504, and the number of fog particles on paper after durability test was 548, resulting in a change rate of fog on paper of 109%.

[0135] <Comparative Example 10> A conductive member C10 was produced and evaluated in the same manner as in Comparative Example 3, except that no resin particles were added. The evaluation results are shown in Table 8. In this comparative example, the circularity of the domain shape is low, and the volume resistivity of the matrix is ​​low, so the uniformity of the electric field in the conductive layer is low. Furthermore, since there is no second convex portion, toner adhesion was observed significantly after durability testing. Therefore, the initial number of fog particles on paper was 103, and the number of fog particles on paper after durability testing was 253, and the change rate of fog on paper was 246%.

[0136] <Comparative Example 11> A conductive member C11 was produced and evaluated in the same manner as in Example 1, except that no resin particles were added. The evaluation results are shown in Table 8. In this comparative example, the uniformity of the electric field in the conductive layer is high, but since there is no second convex portion, toner adhesion was observed significantly after durability testing. Therefore, the initial number of fog particles on paper was 29, and the number of fog particles on paper after durability testing was 201, and the change rate of fog on paper was 693%.

[0137] <Comparative Example 12> A conductive member C12 was produced and evaluated in the same manner as in Example 1, except that the resin particles were changed to graphitized carbon particles (product name: Nika Beads PC-1020, graphitized carbon resin, average particle size 10 μm, manufactured by Nippon Carbon Co., Ltd.). The evaluation results are shown in Table 8. In this comparative example, the use of non-insulating conductive resin particles results in low uniformity of the electric field in the conductive layer, while the distance from the photosensitive drum results in a significantly large number of initial fog particles. Therefore, the initial number of fog particles on paper was 350, and the number of fog particles on paper after durability testing was 424, resulting in a change rate of 108%. [Explanation of symbols]

[0138] 1 Conductive material 2. Conductive support 3 Conductive layer 3a Matrix 3b Domain 3c conductive particles< / epdm> < / sbr> < / nbr>

Claims

1. a support having an electrically conductive outer surface; A conductive layer provided on the outer surface of the support; A conductive member for electrophotography, comprising: the conductive member is in the form of a roller; the conductive layer has a matrix containing a crosslinked product of a first rubber and a plurality of domains dispersed in the matrix, The domain comprises a crosslinked product of a second rubber and a conductive particle, at least a portion of the domain is exposed on an outer surface of the conductive member to form a first protrusion on the outer surface of the conductive member; the outer surface of the conductive member is composed of the matrix and the domain exposed on the outer surface of the conductive member; the conductive layer further contains insulating resin particles, at least a portion of the resin particles cause second protrusions on an outer surface of the conductive member; when the conductive member is pressed against a transparent flat plate with a load of 500 g applied to the transparent flat plate, a distance d of a space formed by contact between the second convex portion and the transparent flat plate in a nip between the conductive member and the transparent flat plate is 3 μm or more and 30 μm or less, and no contact point between the first convex portion and the transparent flat plate exists in the nip, The transparent flat plate is a glass plate having a size of 20 mm square and a thickness of 2 mm. The distance d is determined by performing a scan measurement of the nip in the height direction, and calculating the spatial volume V1 [μm 3 ] of the space formed between the conductive member and the glass surface of the transparent flat plate in an area of ​​nip width L [μm] × longitudinal direction A [μm] in the measurement range, using the formula: d = V1 / (L × A); A platinum electrode having a width of 1.5 cm was provided directly on the outer surface of the conductive member in the circumferential direction of the conductive member, and an AC voltage having an amplitude of 1 V and a frequency of 1.0 Hz was applied between the outer surface of the support and the platinum electrode in an environment of a temperature of 23° C. and a relative humidity of 50%. The impedance was 1.0×10 3 Ω or more 1.0×10 8 Ω or less, When the length of the conductive layer in the longitudinal direction is L and the thickness of the conductive layer is T, and observation regions of 20 μm square are placed at any three locations in a thickness region from the outer surface of the conductive layer to a depth of 0.1T to 0.9T for each of a cross section of the conductive layer in the thickness direction at the center in the longitudinal direction of the conductive layer and three locations at L / 4 from both ends of the conductive layer toward the center, 80% or more by number of domains observed in each of all nine observation regions satisfy the following requirement (B1) and requirement (B2): A conductive member characterized by: Requirement (B1) The ratio of the cross-sectional area of ​​the conductive particles contained in a domain to the cross-sectional area of ​​the domain is 20% or more; Requirement (B2): When the perimeter of a domain is A and the envelope perimeter of the domain is B, A / B is 1.00 or more and 1.10 or less.

2. The volume resistivity ρm of the matrix is ​​1.0×10 8 Ωcm or more 1.0×10 17 The conductive member according to claim 1 , having a resistivity of Ωcm or less.

3. The conductive member according to claim 1 or 2, wherein the average of the maximum Feret diameter Df of the domains satisfying the requirements (B1) and (B2) is in the range of 0.1 μm or more and 5.0 μm or less.

4. The conductive member according to any one of claims 1 to 3, wherein the ratio of the cross-sectional area of ​​the conductive particles to the cross-sectional area of ​​the domain in the requirement (B1) is 25% or more and 30% or less.

5. The conductive member according to any one of claims 1 to 4, wherein the conductive particles are conductive carbon black.

6. The DBP absorption of the conductive carbon black is 40 cm 3 / 100g or more 80cm 3 The conductive member according to claim 5 , wherein the surface roughness is 100 g or less.

7. The conductive member according to claim 5 or 6, wherein the conductive carbon black contained in each of the domains satisfying the requirement (B1) and the requirement (B2) has an arithmetic mean wall-to-wall distance C of 110 nm or more and 130 nm or less, and σm / C is 0.0 or more and 0.3 or less, where σm is a standard deviation of the wall-to-wall distance of the conductive carbon black.

8. The difference between the absolute values ​​of the solubility parameters of the first rubber and the second rubber is 0.4 (J / cm 3 ) 0.5 4.0 (J / cm 3 ) 0.5 The conductive member according to any one of claims 1 to 7, wherein:

9. The conductive member according to any one of claims 1 to 8, wherein the height of the first projections is not less than 50 nm and not more than 200 nm.

10. The conductive member according to any one of claims 1 to 9, wherein an arithmetic mean value Dm of a distance between wall surfaces of the domains forming the first convex portion is 2.00 µm or less.

11. The volume resistivity ρm of the matrix is ​​1.0×10 10 Ωcm or more 1.0×10 17 The conductive member according to any one of claims 1 to 10, having a resistivity of Ωcm or less.

12. The volume resistivity ρm of the matrix is ​​1.0×10 12 Ωcm or more 1.0×10 17 The conductive member according to any one of claims 1 to 11, having a resistivity of Ωcm or less.

13. The volume resistivity ρp of the resin particles that generate the second convex portions is 1.0×10 10 Ωcm or more 1.0×10 17 The conductive member according to any one of claims 1 to 12, having a resistivity of Ωcm or less.

14. The conductive member according to any one of claims 1 to 13, wherein the average particle size Dp of the resin particles that form the second convex portions is 4 µm or more and 50 µm or less.

15. A process cartridge that is detachably mountable to a main body of an electrophotographic image forming apparatus, 15. A process cartridge for electrophotography, comprising the conductive member according to claim 1.

16. 16. The process cartridge according to claim 15, wherein the conductive member is provided as a charging member.

17. 15. An electrophotographic image forming apparatus comprising the conductive member according to claim 1.

18. 18. The electrophotographic image forming apparatus according to claim 17, wherein the conductive member is provided as a charging member.

Citation Information

Patent Citations

  • Semiconductive rubber composition, electrified member, electrophotographic device and process cartridge

    JP2002003651A

  • Charging member, method for manufacturing charging member, electrophotographic device, and process cartridge

    JP2019191564A

  • Image forming apparatus

    JP2021067729A

  • Conductive member, process cartridge, and electrophotographic image forming apparatus

    JP2021067924A

  • Conductive member, process cartridge, and electrophotographic image forming device

    WO2019203225A1