Manufacturing method of resin laminate and manufacturing method of packaging container
A resin laminate with a modified polyester-polyolefin structure addresses VOC emissions and ensures strong bonding without adhesives, facilitating the manufacture of high-strength packaging containers.
Patent Information
- Application Number
- JP2020182471
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-10-30
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2040-10-30
AI Technical Summary
Existing resin laminates used for packaging containers generate volatile organic compounds (VOCs) during manufacturing due to the use of adhesives or anchor coating agents, and there is a lack of standardization for ensuring sufficient peel strength without these agents.
A resin laminate composed of a polyester first layer and a polyolefin second layer, where the first layer's surface is modified to create a C-N bond strength of 0.03 or more using sum frequency generation spectroscopy, allowing direct lamination without adhesives or anchor coating agents.
The laminate achieves sufficient peel strength while eliminating VOC emissions, enabling the production of packaging containers with enhanced bonding properties.
Smart Images

Figure 0007558756000002 
Figure 0007558756000003 
Figure 0007558756000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin laminate, a packaging container, a method for producing a resin laminate, and a method for producing a packaging container. [Background technology]
[0002] 2. Description of the Related Art Laminates of two or more types of resins (resin laminates) are used as materials for packaging containers for various liquid products such as liquid seasonings, liquid detergents, and liquid cosmetics.
[0003] Conventionally, as the above-mentioned resin laminate, a laminate having a structure in which two or more kinds of resin films are bonded together via an adhesive or an anchor coating agent is known. A resin laminate manufactured using an adhesive or an anchor coating agent can sufficiently increase the peel strength between the resin films. On the other hand, when an adhesive or an anchor coating agent is used, VOCs (volatile organic compounds) are generated during the manufacturing process of the resin laminate.
[0004] In response to this, in recent years, from the viewpoints of preserving the working environment and protecting the environment, techniques for producing resin laminates without emitting VOCs while ensuring peel strength have been studied. For example, a production method is known in which, when producing a laminate of a polyamide resin film and a polyester resin film, at least one of the opposing surfaces of both films is irradiated with an electron beam to bond them together, thereby bonding them under pressure without the use of an adhesive (see, for example, Patent Document 1). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2012-254594 A Summary of the Invention [Problem to be solved by the invention]
[0006] Patent Document 1 does not disclose any criteria for the degree of modification required for the film surface modified by electron beams to exhibit sufficient peel strength.
[0007] The present invention has been made in view of the above circumstances, and has an object to provide a resin laminate that exhibits sufficient peel strength without using an adhesive or an anchor coating agent. Another object is to provide a packaging container made of such a resin laminate. Another object is to provide a method for producing a resin laminate that ensures peel strength and suppresses VOC emissions. Another object is to provide a method for producing a packaging container that ensures peel strength and suppresses VOC emissions. [Means for solving the problem]
[0008] In order to solve the above problems, one aspect of the present invention includes the following aspects.
[0009] [1] A resin laminate comprising at least a first layer made of a polyester and a second layer made of a polyolefin, the first layer and the second layer being laminated in direct contact with each other, and a surface of the first layer that contacts the second layer has a C-N bond strength derived from an aromatic amine of 0.03 or more as measured by sum frequency generation spectroscopy.
[0010] [2] A packaging container made from the resin laminate described in [1].
[0011] [3] A method for producing a resin laminate, comprising at least a step of modifying the surface of a first layer made of polyester, and a step of directly laminating and bonding a second layer made of polyolefin to the modified surface, wherein in the modification step, the surface is modified until the strength of C-N bonds derived from aromatic amines, as determined by measurement using sum frequency generation spectroscopy, is 0.03 or more.
[0012] [4] A method for producing a packaging container, comprising: a step of producing a resin laminate by the method for producing a resin laminate described in [3]; and a step of molding the resin laminate into a container shape with the second layer of the resin laminate on the inside. Effect of the Invention
[0013] According to the present invention, it is possible to provide a resin laminate that exhibits sufficient peel strength without using an adhesive or an anchor coating agent. It is also possible to provide a packaging container made of such a resin laminate. It is also possible to provide a method for producing a resin laminate that ensures peel strength and does not generate VOCs. It is also possible to produce a packaging container while suppressing VOC emissions and while ensuring peel strength. [Brief description of the drawings]
[0014] [Figure 1] FIG. 1 is a schematic cross-sectional view showing a resin laminate 1 of the present embodiment. [Diagram 2] FIG. 2 is a schematic diagram showing a packaging container 50 formed using the resin laminate 1. As shown in FIG. [Diagram 3] FIG. 3 is a process diagram showing a method for producing the resin laminate 1 of the embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] 1 is a schematic cross-sectional view showing a resin laminate 1 of the present embodiment. The resin laminate 1 has a first layer 11 and a second layer 12. The resin laminate 1 may further have a printed layer 14 and an intermediate layer 15. The combined configuration of the first layer 11, the printed layer 14, and the intermediate layer 15 may be referred to as a substrate 10.
[0016] The first layer 11 is laminated in direct contact with the second layer 12. "Directly" means that no adhesive or anchor coating agent is present between the first layer 11 and the second layer 12, and "in direct contact" means that the first layer 11 and the second layer 12 are in contact with each other without the intervention of an adhesive or anchor coating agent.
[0017] (1st layer) The first layer 11 is made of a thermoplastic resin. The thermoplastic resin is preferably a polyester, such as polyethylene terephthalate, polyethylene naphthalate, polycarbonate, etc., with polyethylene terephthalate being preferred.
[0018] The first layer 11 may contain, in addition to polyester, an optional component such as a biodegradable resin or a component derived from biomass, as long as the effect of the invention is not impaired.
[0019] Biodegradable resins include polylactic acid (PLA), polybutylene succinate (PBS), polybutylene succinate adipate (PBSA), polybutylene adipate terephthalate (PBAT), and poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) copolymer resin (PHBH).
[0020] The thickness of the first layer 11 is preferably not less than 5 μm and not more than 100 μm.
[0021] One surface 11a of the first layer 11 is subjected to a modification treatment described below in a nitrogen atmosphere. Surface 11a is the surface of the first layer 11 that contacts the second layer 12. When surface 11a is modified in a nitrogen atmosphere, nitrogen molecules (N2) in the atmosphere react with the thermoplastic resin exposed on surface 11a to form new C-N bonds.
[0022] The modification treatment of surface 11a can be confirmed by sum frequency generation spectroscopy (SFG spectroscopy). Specifically, the strength of the C-N bond derived from aromatic amines on surface 11a measured by SFG spectroscopy is 0.03 or more. Also, the strength of the C-N bond derived from aromatic amines is 0.5 or less.
[0023] Specifically, SFG spectroscopy is performed under the following conditions: In this embodiment, the strength of the C-N bond derived from the aromatic amine measured using SFG spectroscopy is a value measured under the following conditions.
[0024] (Method of measuring the strength of CN bonds) The narrowband visible light ω1 used in the measurement is adjusted using a Spitfire ProXP (Spectra Physics, 3.5 W, 1 kHz) as an excitation light source and a filter for ω1 (center wavelength 795 nm, bandwidth 1.5 nm).
[0025] The broadband infrared light ω2 used in the measurement is adjusted using a Spitfire ProXP as an excitation light source and an ω2 filter (Spectra-Physics, TOPAS C and DFG1).
[0026] The infrared laser intensity of the light source is 3.6 mW for both the narrowband visible light ω1 and the broadband infrared light ω2. The narrowband visible light ω1 is s-polarized light, and the broadband infrared light ω2 is p-polarized light.
[0027] A sample film is irradiated with narrowband visible light ω1 and broadband infrared light ω2, and a sum frequency ω3 is generated from the sample film. The sum frequency ω3 is s-polarized light.
[0028] The sum frequency generated by the above operation is detected by the detector, which uses an HR320 (Jobin Yvon) spectrometer and a Spec10 (Princeton Instrument) CCD.
[0029] The sum frequency spectrum of the sample film obtained by the above method is obtained. The sum frequency spectrum is expressed as the sum frequency wave number (cm -1 ) versus sum frequency intensity (au).
[0030] In addition, no sample is placed at the sample film installation position, and the above operation is carried out for the background of the measurement device, and the sum frequency is measured once. Furthermore, the above operation is carried out on the gold mirror instead of the sample film, and the sum frequency is measured once.
[0031] The background sum-frequency spectrum is subtracted from the sum-frequency spectrum of the sample film, and the resulting spectrum is smoothed using the Savitzky-Golay transform. The resulting spectrum is called processed spectrum 1.
[0032] Similarly, subtract the background sum-frequency spectrum from the gold mirror sum-frequency spectrum, and perform smoothing processing on the resulting spectrum by Savitzky-Golay transform. The resulting spectrum is called processed spectrum 2.
[0033] Then, at each wavelength, the intensity of the sum frequency of processed spectrum 1 is divided by the intensity of the sum frequency of processed spectrum 2 to normalize the intensity of the sum frequency of processed spectrum 1 with the intensity of the sum frequency of processed spectrum 2, and a new spectrum is obtained. Peak fitting is performed on the obtained spectrum using a Lorentz function, and the "1286 cm" peak, which is assigned to the C-N bond derived from aromatic amines, is obtained. -1 The peak intensity in the "nearby" area is calculated.
[0034] The above operation was carried out on the sample film at 10 points at 0.5 mm intervals, and each was measured at 1286 cm -1 Among the 10 peak intensities, the data with the highest intensity is used as the data for the sample film.
[0035] In the resin laminate 1, the surface 11a is modified to such an extent that the strength of the C-N bond derived from aromatic amines measured by SFG spectroscopy is 0.03 or more. Since the strength of the C-N bond derived from aromatic amines measured by SFG spectroscopy for the surface 11a of the first layer 11 is 0.03 or more, the resin laminate 1 exhibits sufficient peel strength at the interface between the first layer 11 and the second layer 12.
[0036] The peel strength (unit: N / inch) can be measured in accordance with the measurement method specified in JIS K 6854-1 "Adhesives - Peel adhesion strength test method, Part 1: 90 degree peel."
[0037] The first layer 11 may have a metal vapor-deposited layer on the other surface 11b. Surface 11b is the surface of the first layer 11 opposite to the surface in contact with the second layer 12. The metal vapor-deposited layer may be, for example, an aluminum vapor-deposited layer.
[0038] (2nd layer) The second layer 12 is mainly made of polyolefin and may function as a sealant layer or adhesive layer when bonding the resin laminate 1 to another member (including another resin laminate 1).
[0039] The manufacturing method will be described later, but the second layer 12 may be a polyolefin film or an extruded polyolefin resin layer.
[0040] Polyolefins include polyethylene, polypropylene, and cyclic polyolefins.
[0041] The second layer 12 may contain, in addition to polyolefin, an optional component such as a biodegradable resin or a component derived from biomass, as long as the effect of the invention is not impaired.
[0042] Biodegradable resins include polylactic acid (PLA), polybutylene succinate (PBS), polybutylene succinate adipate (PBSA), polybutylene adipate terephthalate (PBAT), and poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) copolymer resin (PHBH).
[0043] The thickness of the second layer 12 is preferably 10 μm or more and 500 μm or less.
[0044] (Printing layer) The printed layer 14 is a layer on which characters and designs are printed using printing ink, a laser, or the like on a surface 14a of a film made of a thermoplastic resin.
[0045] The printing ink used for printing characters and patterns in the printing layer 14 may contain various ink binder resins such as thermoplastic resins, urethane resins, acrylic resins, etc. Furthermore, the printing ink contains additives such as various pigments, drying agents, stabilizers, etc.
[0046] In the printing layer 14, the letters and patterns are formed by a known printing method such as offset printing, gravure printing, screen printing, etc. The thickness of the part constituting the letters and patterns can usually be about 0.05 μm or more and 2.0 μm or less.
[0047] The thickness of the printed layer 14 is preferably 5 μm or more and 100 μm or less.
[0048] The surface 14a of the printing layer 14 may be subjected to an oxidation treatment. The fact that the surface 14a has been oxidized can be confirmed by sum frequency generation spectroscopy. In other words, the surface 14a may be oxidized to a degree that can be confirmed by sum frequency generation spectroscopy. The above-mentioned known methods can be used for the oxidation treatment.
[0049] (Middle class) The intermediate layer 15 is in contact with the surface 11b of the first layer 11 and the surface 14a of the printed layer 14, and is laminated with the first layer 11 and the printed layer 14.
[0050] Polyethylene can be used as the material for forming the intermediate layer 15. The polyethylene may be composed of only one type of polyethylene, or may be a mixed composition of two or more types of polyethylene.
[0051] The thickness of the intermediate layer 15 is preferably 10 μm or more and 500 μm or less.
[0052] Surface 15a of intermediate layer 15 facing printed layer 14 has been subjected to an oxidation treatment, typically ozone treatment. It can be confirmed by sum frequency generation spectroscopy that surface 15a has been subjected to the oxidation treatment. In other words, surface 15a has been oxidized to a degree that can be confirmed by sum frequency generation spectroscopy.
[0053] (packaging container) 2 is a schematic diagram showing a packaging container 50 formed using the above-mentioned resin laminate 1. In the packaging container 50, the second layer 12 of the resin laminate 1 faces the inside of the container, and the printed layer 14 is exposed to the outside of the container.
[0054] The packaging container 50 is obtained by overlapping two resin laminates 1 cut to a predetermined size with their second layers 12 facing each other, and heat-sealing three sides. In Fig. 2, the heat-sealed portion is indicated by the symbol A.
[0055] The packaging container 50 may also be a self-supporting standing pouch manufactured by a known method.
[0056] (Method of manufacturing resin laminate) The method for producing the resin laminate of this embodiment includes at least a step of modifying the surface of a first layer made of polyester under a nitrogen atmosphere, and a step of directly laminating and bonding a second layer made of polyolefin to the modified surface of the first layer. The following explains each in order.
[0057] (Modification process) The first layer to be treated in the modification step is made of polyester, and a resin film made of polyester can be suitably used for the first layer.
[0058] The surface of the first layer may be modified by plasma treatment or corona treatment. The modification step is carried out until the strength of the C-N bond derived from the aromatic amine is 0.03 or more when the surface of the first layer is measured by sum frequency generation spectroscopy. The modification method is not limited to plasma treatment or corona treatment as long as the same result is obtained.
[0059] When the above modification process is performed in a nitrogen atmosphere, some of the nitrogen molecules in the atmosphere go through a plasma state and react with the main chains and side chains of the polymer on the surface of the first layer. As a result, it is believed that nitrogen atoms derived from the nitrogen molecules in the atmosphere are introduced into the polymer on the surface of the first layer, generating C-N bonds. Since C-N bonds are polarized, it is expected that the polarity of the first layer surface after the above modification process will be higher than before the process. Furthermore, when the polyester contains an aromatic ring, it is believed that the aromatic ring reacts with a nitrogen atom to easily form an aromatic amine.
[0060] In the modification step, in order not to inhibit the formation of C—N bonds, the oxygen gas concentration in the atmosphere is preferably 2% or less by volume, and more preferably 50 ppm or less by volume.
[0061] It is also preferable not to introduce a gas containing oxygen atoms into the atmosphere. Examples of "gases containing oxygen atoms" include CO2 and N2O.
[0062] (Laminating process) The second layer used in the lamination process is made of polyolefin. Either a resin film made of polyolefin or a molten resin film made by melting polyolefin in an extrusion molding machine and extruding it into a film shape from a T-die can be used for the second layer.
[0063] When the produced resin laminate is used as a packaging material, the material of the second layer is preferably a heat-sealable polyolefin or polypropylene that can be used as a sealant layer.
[0064] When a resin film is used as the second layer, the second layer is overlaid on the surface of the modified first layer, and the laminate of the first and second layers is heated and pressed between two rolls, a heating roll and a pinch roll, to obtain a resin laminate.
[0065] When the second layer is a molten resin film, the second layer is melt-extruded and laminated onto the surface of the modified first layer. The laminate of the first and second layers is pressed between two rolls, a cooling roll and a pinch roll, while being cooled to obtain a resin laminate.
[0066] Alternatively, a multilayer laminate formed by overlaying a second layer on the surface of a first layer and then overlaying another resin film on the surface of the second layer may be compressed between two rolls, a cooling roll and a pinch roll, while being cooled to form a resin laminate. In this case, the second layer is attached to the first layer as well as to the other resin film.
[0067] The surface of the second layer that comes into contact with the first layer is preferably treated with ozone. When the second layer is a molten resin film, the surface of the molten resin film that comes into contact with the first layer is preferably treated with ozone before the molten resin film is superimposed on the modified surface of the first layer.
[0068] Ozone treatment is an oxidation treatment of the surface of the molten resin film using ozone. It is recommended to install an ozone generator downstream in the MD direction of the molten resin film discharged from the T-die and perform the ozone treatment before the molten resin film comes into contact with the first layer.
[0069] The method for generating ozone is not particularly limited, but it is preferable to carry out a UV / ozone treatment by irradiating with ultraviolet rays in the air.
[0070] In UV / ozone treatment, the surface of the second layer is irradiated with ultraviolet light using a light source that generates ultraviolet light, such as a low-pressure mercury lamp or a Xe excimer lamp. This breaks down the bonds in the polymer on the surface of the second layer. In addition, oxygen breaks down due to the ultraviolet light irradiation, generating ozone, which then oxidizes the surface of the second layer.
[0071] By subjecting the surface of the second layer to ozone treatment, the polymer on the surface is oxidized, and oxygen functional groups such as carbonyl groups and carboxy groups are generated on the surface of the second layer. These groups have high polarity, so they are strongly electrostatically attracted to the surface of the first layer that has been modified as described above, allowing the first and second layers to be bonded together effectively.
[0072] Fig. 3 is a process diagram showing a method for producing the resin laminate 1 of this embodiment. In the process diagram shown in Fig. 3, a plasma treatment is carried out as the modification treatment.
[0073] The resin laminate 1 described above is produced by laminating a first film and a second film without using an adhesive or an anchor coating agent. The first film corresponds to the "first layer" in the production method of the present invention, and the second film corresponds to the "second layer" in the production method of the present invention.
[0074] The base film 10F is a laminate of a first film 11F made of the same material as the first layer 11 and formed in a strip shape, a printed layer 14F formed in a strip shape with the same configuration as the printed layer 14, and an intermediate layer 15F formed in a strip shape with the same configuration as the intermediate layer 15. When the base film 10F is cut into sheets, it becomes the above-mentioned base material 10.
[0075] The base film 10F is sequentially unwound from a winding roll 10L wound in a roll shape, and is carried into the plasma processing device 110 via a transport roll 101.
[0076] The plasma processing apparatus 110 includes a chamber 111, a roll 112, a plasma generator 113, and transport rolls 114 and 115. The chamber 111 houses the roll 112, the plasma generator 113, and the transport rolls 114 and 115.
[0077] The base film 10F carried into the plasma processing apparatus 110 is wound around a roll 112 via a transport roll 114. In the chamber 111, an atmosphere suitable for conditions for generating plasma is formed.
[0078] The plasma generator 113 is disposed opposite the roll 112, and generates plasma in the space between the plasma generator 113 and the roll 112. One surface of the base film 10F (one surface 11a of the first film 11F) is plasma-treated by the generated plasma.
[0079] The plasma treatment is carried out under atmospheric pressure conditions using nitrogen (N2) as the atmospheric gas until the strength of the C-N bond derived from aromatic amine becomes 0.03 or more when the surface 11a of the first layer 11 of the base film 10F is measured by SFG spectroscopy.
[0080] Regarding the processing conditions such as the output of the plasma generator 113 and the transport speed of the base film 10F, it is advisable to confirm and determine the conditions in a preliminary experiment so that the strength of the C—N bond derived from the aromatic amine is 0.03 or more.
[0081] The substrate film 10F, one surface 11a of which has been plasma-treated, is conveyed out of the plasma processing device 110 via the conveyor rolls 115.
[0082] The plasma treatment of the one surface 11a of the base film 10F may be carried out continuously during the transport process as described above, or may be carried out in advance.
[0083] The base film 10F is fed via a transport roll 102 between a heating roll 104 and a backup roll 105, both of which are maintained at a predetermined temperature.
[0084] On the other hand, the second film 12F is formed in a strip shape and is made of the same material as the second layer 12. The second film 12F is preferably one selected from the group consisting of an unstretched polyethylene resin film, an unstretched polypropylene resin film, a cyclic polyolefin resin film, and a co-extruded film of unstretched polyethylene and unstretched polypropylene.
[0085] The second film 12F is continuously unwound from an unwinding roll 12L wound in a roll shape, and is supplied between a heating roll 104 and a backup roll 105 via a transport roll 103.
[0086] The heating roll 104 is set to a heating temperature higher than the melting point of the second film 12F. The base film 10F and the second film 12F are continuously bonded to each other by passing between the heating roll 104 and the backup roll 105 without applying any adhesive or anchor coating agent to the interface. In this way, the raw sheet 1F of the resin laminate 1 described above is obtained.
[0087] The raw web 1F is conveyed while being cooled by being sandwiched between cooling rolls 106 and 107. The raw web 1F is conveyed to a winding roll 1L and wound into a roll.
[0088] The raw web 1F is appropriately cut into sheets to form the above-mentioned resin laminate 1. The raw web 1F may be cut downstream in the process without being wound into a roll.
[0089] In this embodiment, the resin laminate 1 is obtained in the manner described above.
[0090] (Manufacturing method of packaging containers) The method for manufacturing a packaging container of this embodiment includes a step of manufacturing a resin laminate by the above-mentioned method for manufacturing a resin laminate, and a step of molding the resin laminate into a container shape with the second layer of the resin laminate on the inside.
[0091] The process for molding the resin laminate into a container can be, for example, a process in which two resin laminates cut to a predetermined size are stacked with the second layers facing each other, and three sides are heat-sealed. In the container obtained in this way, the second layer becomes the inside of the container.
[0092] Thereafter, the container is filled with the contents and the remaining side is sealed by heat sealing or the like to produce a packaging container filled with the contents.
[0093] According to the resin laminate 1 having the above-mentioned configuration, it is possible to provide a resin laminate that exhibits sufficient peel strength without using an adhesive or an anchor coating agent.
[0094] Furthermore, according to the packaging container having the above-mentioned configuration, by using the above-mentioned resin laminate as a material, the packaging container exhibits sufficient peel strength and suppresses VOC emissions.
[0095] Furthermore, according to the above-described method for producing a resin laminate, it is possible to produce a resin laminate while ensuring peel strength and suppressing VOC emissions.
[0096] Furthermore, according to the above-described method for producing a packaging container, it is possible to produce a packaging container while ensuring peel strength and suppressing VOC emissions.
[0097] Although the preferred embodiment of the present invention has been described above with reference to the accompanying drawings, the present invention is not limited to the above embodiment. The shapes and combinations of the components shown in the above embodiment are merely examples, and various modifications can be made based on design requirements, etc., without departing from the spirit of the present invention. EXAMPLES
[0098] The present invention will be described below with reference to examples, but the present invention is not limited to these examples.
[0099] (Method of measuring the strength of CN bonds) The strength of the CN bond on the plasma-treated surface was measured by the method described above in (Method for measuring the strength of the CN bond).
[0100] <Example 1> An aluminum-deposited polyethylene terephthalate film (thickness 12 μm) was used as the first layer. The surface on which the polyethylene terephthalate was exposed was subjected to plasma treatment (modification treatment) in an atmosphere filled with nitrogen gas. The intensity of the plasma treatment was 31.3 Wmin / m 2 It was decided.
[0101] The second layer was a polyethylene molten resin film (temperature 300° C., 20 μm). The surface of the second layer that was to be bonded to the first layer was subjected to ozone treatment.
[0102] The modified surface of the first layer was laminated with the ozone-treated surface of the second layer, and a polyethylene film (thickness 105 μm) was further laminated on the surface of the second layer opposite the surface in contact with the second layer to create a resin laminate.
[0103] The modified surface of the first layer was irradiated from the polyethylene film side with a laser beam used for measurement, and the strength of the C-N bond was measured to be 0.178. Note that narrowband visible light ω1 was irradiated at an incident angle of 38°, and broadband infrared light ω2 was irradiated at an incident angle of 46°.
[0104] <Example 2> Plasma treatment intensity: 60.0 Wmin / m 2 A resin laminate was produced in the same manner as in Example 1 except for the above. The C—N bond strength of the modified surface of the first layer was measured and found to be 0.034.
[0105] <Example 3> Plasma treatment intensity: 90.0 Wmin / m 2 A resin laminate was produced in the same manner as in Example 1 except for the above. The strength of the C—N bond on the modified surface of the first layer was measured and found to be 0.099.
[0106] <Example 4> Plasma treatment intensity: 120.0 Wmin / m 2 A resin laminate was produced in the same manner as in Example 1 except for the above. The C—N bond strength of the modified surface of the first layer was measured and found to be 0.155.
[0107] <Comparative Example 1> A resin laminate was produced in the same manner as in Example 1 above, except that the plasma treatment was not carried out. The strength of the C—N bonds on the modified surface of the first layer was measured and found to be below the detection limit.
[0108] (Peel test) The peel strength of the interface between the first layer and the second layer was measured in accordance with the measurement method specified in JIS K 6854-1 "Adhesives - Peel adhesion strength test method, Part 1: 90 degree peel."
[0109] The state when the first layer and the second layer were peeled off (peel mode) was evaluated as follows. Material failure: The peeling of the test piece was not localized at the interface between the first and second layers, and was accompanied by damage to either or both of the first and second layers. Interface: delamination of the specimen occurred at the interface between the first and second layers.
[0110] The evaluation results are shown in Table 1.
[0111] [Table 1]
[0112] The above results prove that the resin laminates according to the examples have sufficient peel strength without using an adhesive or anchor coating agent.
[0113] From the above results, it was confirmed that the present invention is useful. [Explanation of symbols]
[0114] 1...resin laminate, 11...first layer, 11a...surface in contact with second layer, 11F...first film (first layer), 12...second layer, 12F...second film (second layer), 50...packaging container
Claims
1. modifying the surface of the first layer made of polyester; A second layer made of polyolefin is directly laminated to the modified surface. and a step of combining the above-mentioned components, Prior to the modifying step, a preliminary experiment step is included in which a treatment condition for modifying the surface is determined until a strength of a C—N bond derived from an aromatic amine, as determined by a measurement using sum frequency generation spectroscopy, is 0.03 or more; A method for producing a resin laminate, wherein in the modifying step, the surface is modified based on the treatment conditions determined in the preliminary experiment step.
2. A step of producing a resin laminate by the method for producing a resin laminate according to claim 1; and molding the resin laminate into a container shape with the second layer of the resin laminate facing inside.
Citation Information
Patent Citations
Method for manufacturing laminate
JP2001260297A
Method for manufacturing laminated body
JP2003266626A
Apparatus for processing a sample in a droplet, and method for using the same.
JP2010510777A
Manufacturing method of laminate, laminate, and packaging container using the same
JP2011098549A
Laminate and method of manufacturing the same
JP2012254594A