Resin film and method for producing same

A resin film with controlled crystallinity and α-type crystal ratio in a polyvinylidene fluoride and polymethacrylate ester resin composition prevents whitening during heating and cooling, ensuring high transparency and chemical resistance for decorative films in automobile interiors.

JP7559039B2Active Publication Date: 2024-10-01DENKA CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2022500361
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-02-10
Filing Date
2021-02-04
Publication Date
2024-10-01
Estimated Expiration
2041-02-04

AI Technical Summary

Technical Problem

Resin films containing polyvinylidene fluoride resin tend to whiten and change appearance when subjected to heating and cooling processes such as thermal lamination and film insert molding, which is a common issue in producing decorative films for automobile interiors with complex designs.

Method used

A resin composition comprising 50 to 80 parts by mass of polyvinylidene fluoride resin and 20 to 50 parts by mass of polymethacrylate ester resin, with controlled crystallinity and α-type crystal ratio, is used to create a resin film with a thickness of 5 to 200 μm, achieving a HAZE of 20% or less and a total light transmittance of 90% or more, and rapid cooling to suppress α-type crystal formation.

Benefits of technology

The resin film maintains high transparency and does not easily whiten during heating and cooling processes, making it suitable for applications like film insert molding and lamination, while maintaining excellent chemical resistance and transparency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007559039000006
    Figure 0007559039000006
  • Figure 0007559039000001
    Figure 0007559039000001
  • Figure 0007559039000002
    Figure 0007559039000002
Patent Text Reader

Abstract

Provided is a resin film containing a polyvinylidene fluoride-based resin which is highly transparent and is less likely to whiten even when the resin is heated and cooled. The resin film is composed of a resin composition containing 50-80 parts by mass of a polyvinylidene fluoride-based resin, and 20-50 parts by mass of a polymethacrylic acid ester-based resin, with respect to 100 parts by mass of the total of the polyvinylidene fluoride-based resin and the polymethacrylic acid ester-based resin, wherein: the crystallinity of the resin composition is 15-35%; the percentage of an α-type crystal to the total mass of the α-type crystal and a β-type crystal in the resin composition is 0-15 mass%; and the resin film has an average thickness of 5-200 μm, and has a HAZE of at most 20% as measured according to JIS K7136:2000.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin film containing a polyvinylidene fluoride resin and a method for producing the same, and in particular to a resin film containing a polyvinylidene fluoride resin that can be suitably used for lamination onto a substrate and a method for producing the same. [Background technology]

[0002] Resin films containing polyvinylidene fluoride resins have excellent weather resistance and chemical resistance, and are therefore suitable for use as the outermost layer of decorative films used in the interior or exterior of automobiles, or electrical appliance components, etc. Decorative films are generally produced through a process of bonding a decorative layer to a film of the outermost layer. Common bonding techniques include lamination using an adhesive and thermal lamination.

[0003] In recent years, designs have become more diverse and complex, particularly in automotive interiors, and the outermost layer of a decorative film is required to have high transparency so as not to impair color and texture. For this reason, technologies have been developed to improve the transparency of resin films containing polyvinylidene fluoride resins.

[0004] Patent Document 1 (WO 2011 / 142453) proposes a film containing a vinylidene fluoride resin (A) and an acrylic resin (B), in order to provide a film with high crystallinity, transparency, and surface smoothness, and having an arithmetic mean roughness on at least one surface of 0.1 to 20 nm, a crystalline heat of fusion of 18 to 40 J / g measured by a differential scanning calorimeter, and a haze value of 3.5 or less.

[0005] Patent Document 2 (JP 2012-187934 A) describes the successful production of a novel fluororesin film that can be used for vehicle interior and exterior component applications and has excellent transparency, surface hardness, chemical resistance, and stain resistance, by using a fluorine-based (meth)acrylic resin containing a fluorine-containing alkyl (meth)acrylate component. This document specifically discloses a fluororesin laminated acrylic resin film in which a fluororesin film layer is laminated on at least one side of a film layer made of an acrylic resin (A), and the fluororesin film layer is formed from a fluororesin (C) containing a fluorine-based (meth)acrylic resin (B) that contains a fluorine-containing alkyl (meth)acrylate polymer component.

[0006] Also known is a technique for improving the properties of a resin film containing a vinylidene fluoride resin by controlling the crystal form of the vinylidene fluoride resin.

[0007] Patent Document 3 (International Publication No. 2019 / 107302) discloses a vinylidene fluoride resin multilayer film including two layers, a surface layer laminated on a back layer, the surface layer containing 80% by mass or more of vinylidene fluoride resin and 20% by mass or less of methacrylic acid ester resin, the crystallinity of the surface layer being 45% or more, the ratio of α crystals to the total crystal components of the vinylidene fluoride resin being 60% or more, the thickness of the surface layer being 15 μm or more, and the back layer containing 90% by mass or more of methacrylic acid ester resin. It is said that the film can suppress discoloration of the film due to acid rain and discoloration of the film due to the generation of a polyene structure by a hindered amine light stabilizer contained in the decorative film for a long period of time under high temperature and high humidity environments. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] International Publication No. 2011 / 142453 [Patent Document 2] JP 2012-187934 A [Patent Document 3] International Publication No. 2019 / 107302 Summary of the Invention [Problem to be solved by the invention]

[0009] As mentioned above, decorative films are often produced through a process of attaching a decorative layer to the outermost film by thermal lamination. In addition, methods for covering the surface of automotive interior parts with decorative films include film insert molding, in-mold molding, and vacuum lamination molding. Among these, film insert molding is the mainstream. Film insert molding has the advantage that the decorative film can follow parts with more complex shapes compared to in-mold molding and vacuum lamination molding, since the decorative film is heated and preformed, and a good surface covering state can be achieved.

[0010] However, it has been found that when a resin film containing a polyvinylidene fluoride resin is used in a process involving heating and cooling, such as thermal lamination and film insert molding, there is a problem that the resin film whitens and changes in appearance. The above-mentioned prior art lacks awareness of whitening, and there is still room for improvement in the resin film containing a polyvinylidene fluoride resin from the viewpoint of preventing whitening.

[0011] Therefore, in one embodiment, an object of the present invention is to provide a resin film containing a polyvinylidene fluoride resin that is highly transparent and does not easily whiten even when heated and cooled, and a method for producing the same. [Means for solving the problem]

[0012] As a result of various studies conducted to achieve the above-mentioned object, the inventors discovered that controlling the crystallinity and the ratio of α-type crystals in a resin composition containing a polyvinylidene fluoride resin is advantageous in preventing whitening of a resin film, and thus arrived at the present invention, which is exemplified below.

[0013] [1] A resin film made of a resin composition containing 50 to 80 parts by mass of a polyvinylidene fluoride resin and 20 to 50 parts by mass of a polymethacrylate resin relative to 100 parts by mass in total of the polyvinylidene fluoride resin and the polymethacrylate resin, The degree of crystallinity of the resin composition is 15% to 35%, The ratio of α-type crystals to the total mass of α-type crystals and β-type crystals in the resin composition is 0 to 15% by mass, The average thickness of the resin film is 5 to 200 μm, The haze of the resin film measured according to JIS K7136:2000 is 20% or less. Resin film. [2] The resin film according to [1], wherein at least one surface has an arithmetic mean roughness Ra of 100 nm or less as measured in accordance with JIS B0601:2001. [3] The resin film according to [1] or [2], having a haze of 5% or less as measured in accordance with JIS K7136:2000. [4] The resin film according to any one of [1] to [3], which has a total light transmittance of 90% or more as measured in accordance with JIS K7375:2008. [5] The resin film according to any one of [1] to [4], wherein the resin film has a change in haze value ΔHAZE of 5% or less when heated in air from 25°C to 170°C at an average heating rate of 3.5°C / sec, placed in a temperature environment of 25°C within 1 second after the temperature reached 170°C, and then allowed to cool to 25°C in air, as measured in accordance with JIS K7136:2000. [6] a surface layer made of a resin composition containing 50 to 80 parts by mass of a polyvinylidene fluoride resin and 20 to 50 parts by mass of a polymethacrylate resin relative to 100 parts by mass in total of the polyvinylidene fluoride resin and the polymethacrylate resin; a back layer laminated on the front layer, the back layer being composed of a resin composition containing 0 to 30 parts by mass of a polyvinylidene fluoride resin and 70 to 100 parts by mass of a polymethacrylate resin relative to 100 parts by mass in total of the polyvinylidene fluoride resin and the polymethacrylate resin; A resin film comprising: The crystallinity of the resin composition constituting the surface layer is 15% to 35%; The ratio of α-type crystals to the total mass of α-type crystals and β-type crystals in the resin composition constituting the surface layer is 0 to 15% by mass, The average thickness of the surface layer is 5 to 200 μm, The average thickness of the back surface layer is 5 to 300 μm, The haze of the resin film measured according to JIS K7136:2000 is 20% or less. Resin film. [7] The resin film according to [6], wherein at least one of the outer surface of the front layer and the outer surface of the back layer has an arithmetic average roughness Ra of 100 nm or less as measured in accordance with JIS B0601:2001. [8] The resin film according to [6] or [7], having a haze of 5% or less as measured in accordance with JIS K7136:2000. [9] The resin film according to any one of [6] to [8], which has a total light transmittance of 90% or more as measured in accordance with JIS K7375:2008.

[10] The resin film according to any one of [6] to [9], wherein the resin film has a change in haze value ΔHAZE of 5% or less before and after heating in air from 25°C to 170°C at an average heating rate of 3.5°C / sec, placing in a temperature environment of 25°C within 1 second after the temperature reaches 170°C, and cooling in air to 25°C, as measured in accordance with JIS K7136:2000.

[11] The resin film according to any one of [6] to

[10] , wherein the resin composition constituting the back surface layer contains 0.1 to 10 parts by mass of an ultraviolet absorber per 100 parts by mass in total of the polyvinylidene fluoride resin and the polymethacrylate ester resin.

[12] The resin film according to

[11] , wherein the ultraviolet absorber contains a triazine-based compound, a benzotriazole-based compound, or a mixture thereof.

[13] The resin film according to any one of [6] to

[12] , wherein the resin composition constituting the back surface layer contains 0.1 to 10 parts by mass of crosslinked (meth)acrylic acid ester-based resin particles per 100 parts by mass in total of the polyvinylidene fluoride-based resin and the polymethacrylic acid ester-based resin.

[14] The resin film according to any one of [1] to

[13] , which is used for lamination with a substrate.

[15] The resin film according to

[14] , wherein the 60° specular gloss of the surface of the substrate to be laminated with the resin film is 100 to 600 as measured in accordance with JIS Z8741:1997, and L* at a light receiving angle of 15° in the L*a*b* color space in accordance with JIS Z8781-4:2013 is 0 to 20.

[16] The resin film according to any one of [1] to

[13] , which is used for thermoforming.

[17] a step of melt-extrusion molding a resin composition containing 50 to 80 parts by mass of a polyvinylidene fluoride resin and 20 to 50 parts by mass of a polymethacrylate resin relative to a total of 100 parts by mass of the polyvinylidene fluoride resin and the polymethacrylate resin from a T-die at a temperature of 200°C to 260°C into a film having an average thickness of 5 to 200 μm; A step of contacting at least one surface of the melt-extruded film with the surface of a metal roll adjusted to a temperature of 30 to 50°C within 6 seconds after being extruded from the outlet of the T-die, and cooling the film; A method for producing a resin film comprising the steps of:

[18] a first resin composition containing 50 to 80 parts by mass of a polyvinylidene fluoride resin and 20 to 50 parts by mass of a polymethacrylate resin relative to 100 parts by mass in total of the polyvinylidene fluoride resin and the polymethacrylate resin; a second resin composition containing 0 to 30 parts by mass of a polyvinylidene fluoride resin and 70 to 100 parts by mass of a polymethacrylate resin relative to 100 parts by mass in total of the polyvinylidene fluoride resin and the polymethacrylate resin; a step of melt-co-extrusion molding the first resin composition into a film shape from a T-die at a temperature of 200° C. to 260° C. so that the first resin composition has an average thickness of 5 to 200 μm and the second resin composition has an average thickness of 5 to 300 μm; a step of contacting at least a surface of the melt-coextruded film on the side of the first resin composition with a surface of a metal roll adjusted to a temperature of 30 to 50° C. within 6 seconds after the film is extruded from an outlet of the T-die, and cooling the film; A method for producing a resin film comprising the steps of:

[19] The method for producing a resin film according to

[17] or

[18] , wherein the surface of the metal roll has an arithmetic mean roughness Ra of 100 nm or less as measured in accordance with JIS B0601:2001. Effect of the Invention

[0014] According to one embodiment of the present invention, a resin film containing a polyvinylidene fluoride resin that is highly transparent and does not easily whiten even when heated and cooled can be obtained. Therefore, the resin film according to one embodiment of the present invention can be suitably used in processes involving heating and cooling, such as film insert molding. The resin film can be attached to a substrate and used, for example, as the outermost layer of a decorative film. [Brief description of the drawings]

[0015] [Figure 1] FIG. 4 is a schematic cross-sectional view showing a laminated structure of a resin film according to a second embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] Hereinafter, embodiments of the present invention will be described. The embodiments described below are illustrative of typical embodiments of the present invention, and are not intended to narrow the technical scope of the present invention.

[0017] 1. First Embodiment The resin film according to the first embodiment can be composed of a resin composition containing 50 to 80 parts by mass of polyvinylidene fluoride resin and 20 to 50 parts by mass of polymethacrylate resin, relative to a total of 100 parts by mass of polyvinylidene fluoride resin and polymethacrylate resin.

[0018] In one embodiment, the crystallinity of the resin composition can be 15% to 35%. By setting the lower limit of the crystallinity to 15% or more, preferably 20% or more, excellent chemical resistance can be exhibited. In addition, by setting the upper limit of the crystallinity to 35% or less, preferably 30% or less, the total amount of α-type crystals can be suppressed, and the effect of preventing whitening is enhanced.

[0019] In this specification, the crystallinity of the resin composition is calculated from the integrated value of the crystalline melting enthalpy (J / g) of the melting peak from the spectrum measured based on JIS K 7121:2012, and calculated by the formula: (crystallinity (%)) = (crystalline melting enthalpy (J / g) per unit mass of the resin composition) / (crystalline melting enthalpy (J / g) per unit mass of the PVDF crystal) × 100 (%), where (crystalline melting enthalpy per unit mass of the PVDF crystal) = 104.6 J / g.

[0020] From the viewpoint of preventing whitening, it is desirable that the ratio of α-type crystals to the total mass of α-type crystals and β-type crystals in the resin composition is small. Specifically, the ratio is preferably 0 to 15 mass%, more preferably 0 to 10 mass%, further preferably 0 to 8 mass%, and even more preferably 0 to 5 mass%.

[0021] In this specification, the ratio of α-type crystals to the total mass of α-type crystals and β-type crystals in a resin composition is determined based on the characteristic absorption wave number of α-type crystals of 765 cm from the infrared absorption spectrum of the resin composition obtained by a reflection method. -1 Absorption intensity (peak height (α)) at the characteristic absorption wavenumber of 840 cm for β-type crystals -1 The absorption intensity (peak height (β)) at each point is measured and calculated using the following formula. Ratio of α-type crystals (%) = (α) / ((α)+(β))×100(%)

[0022] The thickness of the resin film according to the first embodiment is preferably 5 to 200 μm, more preferably 5 to 100 μm, even more preferably 5 to 40 μm, and particularly preferably 10 to 20 μm. When the resin film is 5 μm or more, the film formability is improved and the protective function when used as a surface layer can be improved, and when the resin film is 200 μm or less, whitening becomes less noticeable and transparency can be improved and costs can be reduced. The resin film according to the first embodiment may be formed of a single layer or multiple layers, but it is desirable that the total average thickness falls within the above-mentioned thickness.

[0023] The haze of the resin film according to the first embodiment, measured based on JIS K7136:2000, is, from the viewpoint of enhancing transparency, preferably 20% or less, more preferably 10% or less, even more preferably 5% or less, and most preferably 2% or less, and can be, for example, in the range of 0.1 to 20%.

[0024] The resin film according to the first embodiment can have a feature that the change in haze before and after heating is small. For example, the change amount ΔHAZE of the haze value measured based on JIS K7136:2000 after heating in air from 25°C to 170°C at an average heating rate of 3.5°C / sec, placing in a temperature environment of 25°C within 1 second after reaching 170°C, and cooling to 25°C in air can be 5% or less, preferably 3% or less, more preferably 1% or less, for example, 0.5 to 5%. ΔHAZE is expressed by ΔHAZE(%)=|HAZEa-HAZEb|, where HAZEb(%) is the haze value before heating and HAZEa(%) is the haze value after heating.

[0025] The total light transmittance of the resin film according to the first embodiment, measured based on JIS K7375:2008, is preferably 80% or more, more preferably 85% or more, and even more preferably 90% or more, from the viewpoint of increasing transparency, and can be, for example, 80 to 95%.

[0026] The arithmetic average roughness Ra measured in accordance with JIS B0601:2001 on at least one surface, preferably both surfaces, of the resin film according to the first embodiment is, from the viewpoint of enhancing transparency, preferably 100 nm or less, more preferably 90 nm or less, and can be, for example, 70 to 100 nm.

[0027] The mixing ratio of the polyvinylidene fluoride resin and the polymethacrylic acid ester resin in the resin composition constituting the resin film according to the first embodiment is preferably 50 to 80 parts by mass: 20 to 50 parts by mass, more preferably 60 to 75 parts by mass: 25 to 40 parts by mass, based on 100 parts by mass of the total of the polyvinylidene fluoride resin and the polymethacrylic acid ester resin. When the polyvinylidene fluoride resin is 50 parts by mass or more based on 100 parts by mass of the total of the polyvinylidene fluoride resin and the polymethacrylic acid ester resin, properties such as chemical resistance, weather resistance, and contamination resistance can be improved. In addition, by containing a small amount of polymethacrylic acid ester resin in the resin film, it is possible to prevent the ratio of α-type crystals from becoming large, and when the resin film according to the first embodiment is used as a surface layer by laminating it on a back layer described later, it is possible to improve adhesion and adhesion.

[0028] The resin composition constituting the resin film according to the first embodiment may contain other resins, plasticizers, heat stabilizers, antioxidants, light stabilizers, crystal nucleating agents, antiblocking agents, sealability improvers, release agents, colorants, pigments, foaming agents, flame retardants, etc., as appropriate, within the scope of the present invention. However, in general, the total content of the polyvinylidene fluoride resin and the polymethacrylic acid ester resin in the resin composition constituting the resin film is 80% by mass or more, typically 90% by mass or more, more typically 95% by mass or more, and may be 100% by mass. The resin composition constituting the resin film according to the first embodiment may contain an ultraviolet absorber, but it is preferable not to contain it from the viewpoint of cost and bleed-out.

[0029] In this specification, the term "polyvinylidene fluoride resin" refers to a homopolymer of vinylidene fluoride, as well as a copolymer of vinylidene fluoride and a monomer copolymerizable with vinylidene fluoride. Examples of monomers copolymerizable with vinylidene fluoride include vinyl fluoride, tetrafluoroethylene, hexafluoropropylene, hexafluoroisobutylene, trifluorochloroethylene, various fluorinated alkyl vinyl ethers, and further known vinyl monomers such as styrene, ethylene, butadiene, and propylene, which can be used alone or in combination of two or more kinds. Among these, at least one selected from vinyl fluoride, tetrafluoroethylene, hexafluoropropylene, and trifluorochloroethylene is preferred, and hexafluoropropylene is more preferred.

[0030] Polymerization reactions for obtaining polyvinylidene fluoride resins include known polymerization reactions such as radical polymerization and anionic polymerization. Polymerization methods include known polymerization methods such as suspension polymerization and emulsion polymerization. The degree of crystallinity, mechanical properties, etc. of the resulting resin change depending on the polymerization reaction and / or polymerization method.

[0031] The lower limit of the melting point of the polyvinylidene fluoride resin is preferably 150° C. or higher, more preferably 160° C. or higher. The upper limit of the melting point of the polyvinylidene fluoride resin is preferably 170° C. or lower, which is equal to the melting point of polyvinylidene fluoride (PVDF).

[0032] The lower limit of the glass transition point (Tg) of the polymethacrylic acid ester resin is preferably 70° C. or higher, more preferably 80° C. or higher. The upper limit of the Tg of the polymethacrylic acid ester resin is preferably 120° C. or lower.

[0033] The melting point of the polyvinylidene fluoride resin and the Tg of the polymethacrylate resin can be measured by heat flux differential scanning calorimetry (heat flux DSC). For example, they can be obtained from the DSC curve (first run) obtained by heating a sample of 1.5 mg from room temperature to 200°C at a heating rate of 10°C / min using a differential scanning calorimeter DSC3100SA manufactured by Bruker AXS.

[0034] In this specification, the term "polymethacrylate ester-based resin" refers to a homopolymer of a methacrylate ester such as methyl methacrylate, a copolymer of a methacrylate ester and a monomer copolymerizable with a methacrylate ester, and a particle size of less than 1 μm in a resin film (including particles so fine that the particle size cannot be specified and particles that form a matrix phase). In other words, resin particles having a particle size of 1 μm or more in a resin film are not included in the polymethacrylate ester-based resin in this specification. The particle size of a resin particle refers to the diameter of the smallest circle that can surround the resin particle when the resin film is clamped and fixed in a small metal vice, cut with a single-edged knife so that the cross section of the resin film is smooth, and the cross section of the resin film is observed at a magnification of 2000 times with the resin film clamped in the vice using a confocal laser microscope (e.g., Keyence VK-X110).

[0035] Examples of monomers copolymerizable with methacrylic acid esters include (meth)acrylic acid esters such as butyl acrylate, butyl methacrylate, ethyl acrylate, and ethyl methacrylate; aromatic vinyl monomers such as styrene, α-methylstyrene, p-methylstyrene, o-methylstyrene, t-butylstyrene, divinylbenzene, and tristyrene; cyanide vinyl monomers such as acrylonitrile and methacrylonitrile; glycidyl group-containing monomers such as glycidyl (meth)acrylate; vinyl carboxylate-based monomers such as vinyl acetate and vinyl butyrate; olefin-based monomers such as ethylene, propylene, and isobutylene; diene-based monomers such as 1,3-butadiene and isoprene; unsaturated carboxylic acid-based monomers such as maleic acid, maleic anhydride, and (meth)acrylic acid; and enone-based monomers such as vinyl methyl ketone. These may be used alone or in combination of two or more. Among these, a homopolymer of methyl methacrylate or an acrylic rubber modified acrylic copolymer in which an acrylic rubber mainly composed of butyl methacrylate is copolymerized with a monomer mainly composed of methyl (meth)acrylate is preferred for reasons of compatibility with polyvinylidene fluoride resins, film strength, and adhesion and cohesion with the back layer.

[0036] Examples of the copolymer include random copolymers, graft copolymers, block copolymers (e.g., linear types such as diblock copolymers, triblock copolymers, gradient copolymers, and the like, star-shaped copolymers polymerized by the arm-first method or the core-first method, etc.), copolymers obtained by polymerization using macromonomers, which are polymerizable functional compounds (macromonomer copolymers), and mixtures thereof. Among these, graft copolymers and block copolymers are preferred from the viewpoint of resin productivity.

[0037] Polymerization reactions for obtaining polymethacrylate resins include known polymerization reactions such as radical polymerization, living radical polymerization, living anionic polymerization, and living cationic polymerization. Polymerization methods include known polymerization methods such as bulk polymerization, suspension polymerization, emulsion polymerization, and solution polymerization. The mechanical properties of the resulting resin change depending on the polymerization reaction and polymerization method.

[0038] The resin film according to the first embodiment can be produced, for example, by carrying out the following steps. Step 1: A step of melt-extrusion molding a resin composition containing 50 to 80 parts by mass of polyvinylidene fluoride resin and 20 to 50 parts by mass of polymethacrylate resin, relative to a total of 100 parts by mass of polyvinylidene fluoride resin and polymethacrylate resin, from a T-die at a temperature of 200°C to 260°C into a film having an average thickness of 5 to 200 μm. Step 2: A step of contacting at least one surface of the melt-extruded film with the surface of a metal roll whose temperature is adjusted to 30 to 50°C within 6 seconds after being extruded from the outlet of the T-die, thereby cooling the film.

[0039] From the viewpoint of controlling the crystallinity of the resin composition to an appropriate range and reducing the ratio of α-type crystals, it is desirable to rapidly cool the molten resin composition extruded from the T-die at a temperature of 200°C to 260°C. Specifically, after the resin composition is extruded into a film form from the outlet of the T-die, it is desirable to contact the surface of a metal roll whose temperature is adjusted to 30 to 50°C, preferably 40 to 45°C, within 6 seconds, preferably within 4 seconds. Since α-type crystals are likely to be generated and grow at around 140°C, rapid cooling under these conditions allows the temperature to pass through around 140°C quickly, so that the generation of α-type crystals can be effectively suppressed. As a method for adjusting the temperature of the metal roll surface, for example, a method of circulating a cooling medium such as cooling water inside the metal roll can be mentioned.

[0040] Examples of the melt extrusion molding method include a T-die method in which a film is formed using a T-die and a method using an inflation die. During cooling, it is more preferable to place a rubber touch roll opposite the metal roll and pinch the molten resin composition extruded from the outlet of the die between the metal roll (cast roll) and the touch roll, from the viewpoint of transferring the smooth surface of the metal roll to the film.

[0041] From the viewpoint of reducing the surface roughness of the resin film, it is desirable that the surface roughness of the metal roll is small, and furthermore, it is desirable that the surface roughness of the touch roll is also small. This is because the surface roughness of the metal roll and the touch roll is reflected in the surface roughness of the resin film. Therefore, the arithmetic mean roughness Ra of the surface of the metal roll measured according to JIS B0601:2001 is preferably 100 nm or less, more preferably 80 nm or less, even more preferably 60 nm or less, even more preferably 40 nm or less, even more preferably 20 nm or less, and can be, for example, 10 to 100 nm. The arithmetic mean roughness Ra of the surface of the touch roll measured according to JIS B0601:2001 is preferably 150 nm or less, more preferably 120 nm or less, and can be, for example, 100 to 150 nm.

[0042] 2. Second Embodiment 1 shows a schematic cross-sectional view illustrating the laminated structure of a resin film (100) according to the second embodiment. The resin film (100) comprises at least a surface layer (110) and a back layer (120) laminated on the surface layer (110), in that order. Typically, the surface layer (110) and the back layer (120) are directly bonded to each other, with no other resin layer interposed between them.

[0043] The haze of the resin film according to the second embodiment, measured based on JIS K7136:2000, is preferably 20% or less, more preferably 10% or less, even more preferably 5% or less, and most preferably 2% or less, from the viewpoint of increasing transparency, and can be, for example, in the range of 0.1 to 20%.

[0044] The resin film according to the second embodiment can have a feature that the change in haze before and after heating is small. For example, the change amount ΔHAZE of the haze value measured based on JIS K7136:2000 after heating in air from 25°C to 170°C at an average heating rate of 3.5°C / sec, placing in a temperature environment of 25°C within 1 second after reaching 170°C, and cooling to 25°C in air can be 5% or less, preferably 3% or less, more preferably 1% or less, for example, 0.5 to 5%. ΔHAZE is expressed by ΔHAZE(%)=|HAZEa-HAZEb|, where HAZEb(%) is the haze value before heating and HAZEa(%) is the haze value after heating.

[0045] The total light transmittance of the resin film according to the second embodiment, measured based on JIS K7375:2008, is preferably 80% or more, more preferably 85% or more, and even more preferably 90% or more, from the viewpoint of increasing transparency, and can be, for example, 80 to 95%.

[0046] From the viewpoint of enhancing transparency, the resin film according to the second embodiment preferably has an arithmetic average roughness Ra, measured in accordance with JIS B0601:2001, of at least one, and preferably both, of the outer surface of the front layer and the outer surface of the back layer, of 100 nm or less, more preferably 90 nm or less, and can be, for example, 70 to 100 nm.

[0047] The surface layer can be composed of a resin composition containing 50 to 80 parts by mass of polyvinylidene fluoride resin and 20 to 50 parts by mass of polymethacrylic acid ester resin, relative to 100 parts by mass in total of polyvinylidene fluoride resin and polymethacrylic acid ester resin. The same description as that of the resin composition constituting the resin film according to the first embodiment applies to the embodiment of the resin composition constituting the surface layer, including the composition, crystallinity, ratio of α-type crystals, thickness, haze, and total light transmittance, and therefore the description thereof will be omitted.

[0048] The thickness of the back surface layer is preferably 5 to 300 μm, more preferably 5 to 100 μm, even more preferably 10 to 75 μm, and particularly preferably 25 to 35 μm. When the back surface layer is 5 μm or more, the film formability is improved and the adhesiveness during thermal lamination described below can be improved, and when the thickness is 300 μm or less, the thermoformability and transparency can be improved and the cost can be reduced. The back surface layer may be formed as a single layer or multiple layers, but it is desirable that the total average thickness falls within the above-mentioned thickness.

[0049] The back surface layer can be composed of a resin composition containing 0 to 30 parts by mass of polyvinylidene fluoride resin and 70 to 100 parts by mass of polymethacrylate resin, relative to a total of 100 parts by mass of polyvinylidene fluoride resin and polymethacrylate resin.

[0050] The mixing ratio of the polyvinylidene fluoride resin and the polymethacrylic acid ester resin in the resin composition constituting the back surface layer is preferably 0-30 parts by mass:70-100 parts by mass, more preferably 20-30 parts by mass:70-80 parts by mass, based on 100 parts by mass of the total of the polyvinylidene fluoride resin and the polymethacrylic acid ester resin. When the polymethacrylic acid ester resin is 70 parts by mass or more based on 100 parts by mass of the total of the polyvinylidene fluoride resin and the polymethacrylic acid ester resin, the adhesion to other layers such as the decorative layer described below can be improved. In addition, by containing a small amount of the polyvinylidene fluoride resin in the back surface layer, the weather resistance and the adhesion and adhesion to the surface layer can be improved.

[0051] The types, melting points and polymerization reactions of the polyvinylidene fluoride resins and polymethacrylate ester resins in the resin composition constituting the back layer are the same as those of the polyvinylidene fluoride resins and polymethacrylate ester resins in the resin composition constituting the surface layer, so the explanation is omitted here.

[0052] Since the content of the polyvinylidene fluoride resin in the resin composition constituting the back surface layer is small, typically, α-type crystals and β-type crystals are not generated in the back surface layer, and therefore, it is not necessary to specify the crystallinity and the ratio of α-type crystals in the back surface layer.

[0053] In addition to the polyvinylidene fluoride resin and the polymethacrylate resin, the resin composition constituting the back surface layer may appropriately contain ultraviolet absorbers, other resins, plasticizers, heat stabilizers, antioxidants, light stabilizers, crystal nucleating agents, antiblocking agents, sealability improvers, release agents, colorants, pigments, foaming agents, flame retardants, etc., within the scope of the present invention. However, the total content of the polyvinylidene fluoride resin and the polymethacrylate resin in the back surface layer is generally 80% by mass or more, typically 90% by mass or more, more typically 95% by mass or more, and may be 100% by mass.

[0054] The resin composition constituting the back surface layer preferably contains an ultraviolet absorbing agent. When the resin composition constituting the back surface layer contains an ultraviolet absorbing agent, ultraviolet rays are blocked and weather resistance can be effectively improved. Examples of ultraviolet absorbing agents include, but are not limited to, hydroquinone-based, triazine-based, benzotriazole-based, benzophenone-based, cyanoacrylate-based, oxalic acid-based, hindered amine-based, salicylic acid derivatives, etc., which can be used alone or in combination of two or more. Among them, it is preferable to contain a triazine-based compound, a benzotriazole-based compound, or a mixture thereof in terms of the durability of the ultraviolet ray blocking effect.

[0055] The content of the ultraviolet absorber in the resin composition constituting the back surface layer is preferably 0.1 to 10 parts by mass relative to 100 parts by mass of the total of the polyvinylidene fluoride resin and the polymethacrylic acid ester resin of the back surface layer. By making the content of the ultraviolet absorber in the resin composition constituting the back surface layer 0.1 parts by mass or more, preferably 1 part by mass or more, more preferably 2 parts by mass or more, relative to 100 parts by mass of the total of the polyvinylidene fluoride resin and the polymethacrylic acid ester resin, it is possible to expect a further improvement effect in weather resistance and an ultraviolet absorbing effect, and by making the content of the ultraviolet absorber in the resin composition constituting the back surface layer 10 parts by mass or less, more preferably 5 parts by mass or less, relative to 100 parts by mass of the total of the polyvinylidene fluoride resin and the polymethacrylic acid ester resin, it is possible to prevent the ultraviolet absorber from bleeding out to the film surface, prevent a decrease in adhesion with the surface layer, and realize cost reduction.

[0056] The resin composition constituting the back surface layer may contain crosslinked (meth)acrylic acid ester-based resin particles. When the resin composition constituting the back surface layer contains a small amount of crosslinked (meth)acrylic acid ester-based resin particles, it is possible to produce a resin film that is slightly cloudy white and has little change in appearance. By making the resin film slightly cloudy white from the beginning, a wider range of design expression is possible. The content of the crosslinked (meth)acrylic acid ester-based resin particles in the resin composition constituting the back surface layer is preferably 0.1 to 10 parts by mass per 100 parts by mass of the total of the polyvinylidene fluoride-based resin and the polymethacrylic acid ester-based resin. Examples of the crosslinked (meth)acrylic acid ester-based resin particles include, but are not limited to, crosslinked polymethyl methacrylate, crosslinked polyethyl methacrylate, crosslinked polynormal butyl methacrylate, etc., which can be used alone or in combination of two or more. Among them, it is preferable to contain polymethyl methacrylate because the difference in refractive index with the back surface layer is small.

[0057] In this specification, the crosslinked (meth)acrylic acid ester-based resin particles refer to those having a particle size of 1 μm or more in a resin film. The particle size of a resin particle refers to the diameter of the smallest circle that can surround the resin particle when the resin film is observed by the above-mentioned method. Therefore, even if the crosslinked (meth)acrylic acid ester-based resin particles have a particle size of less than 1 μm in a resin film, they are considered to be polymethacrylic acid ester-based resins if they satisfy the above-mentioned definition of polymethacrylic acid ester-based resins.

[0058] The arithmetic mean particle size of the crosslinked (meth)acrylic acid ester resin particles in the resin film is preferably from 1 to 4 μm, more preferably from 1.5 to 3.5 μm, from the viewpoints of film appearance and film formability.

[0059] A laminate in which a surface layer and a back layer are laminated can be manufactured by, for example, a melt co-extrusion molding method in which multiple resins are bonded and laminated in a molten state using multiple extruders. The melt co-extrusion molding method includes the multi-manifold die method, in which multiple resins are formed into a sheet and then each layer is brought into contact and bonded at the tip inside a T-die, the feed block die method, in which multiple resins are bonded in a merging device (feed block) and then spread into a sheet, and the dual slot die method, in which multiple resins are molded into a sheet and then each layer is brought into contact and bonded at the tip outside the T-die. It can also be manufactured by an inflation molding method using a round die.

[0060] The resin film according to the second embodiment can be produced, for example, by carrying out the following steps. Step 1: a first resin composition containing 50 to 80 parts by mass of a polyvinylidene fluoride resin and 20 to 50 parts by mass of a polymethacrylate resin relative to 100 parts by mass in total of the polyvinylidene fluoride resin and the polymethacrylate resin; a second resin composition containing 0 to 30 parts by mass of a polyvinylidene fluoride resin and 70 to 100 parts by mass of a polymethacrylate resin relative to 100 parts by mass in total of the polyvinylidene fluoride resin and the polymethacrylate resin; A process of melt co-extrusion molding into a film shape from a T-die at a temperature of 200°C to 260°C so that the first resin composition has an average thickness of 5 to 200 µm and the second resin composition has an average thickness of 5 to 300 µm. Step 2: A process of contacting at least the surface of the melt coextruded film on the side of the first resin composition with the surface of a metal roll whose temperature is adjusted to 30 to 50°C within 6 seconds after the film is extruded from the outlet of the T-die, thereby cooling the film.

[0061] From the viewpoint of controlling the crystallinity of the first resin composition to an appropriate range and reducing the ratio of α-type crystals, it is desirable to rapidly cool the laminate of the first resin composition and the second resin composition in a molten state extruded into a film form from a T-die at a temperature of 200°C to 260°C from the surface on the first resin composition side. Specifically, it is desirable to contact at least the surface on the first resin composition side of the melt-coextruded film with the surface of a metal roll adjusted to a temperature of 30 to 50°C, preferably 40 to 45°C, within 6 seconds, preferably within 4 seconds, after extrusion from the outlet of the T-die. As a method for adjusting the temperature of the metal roll surface, for example, a method of circulating a cooling medium such as cooling water inside the metal roll can be mentioned.

[0062] During cooling, it is more preferable to place a rubber touch roll opposite the metal roll and pinch the laminate of the first resin composition and the second resin composition in a molten state extruded from the outlet of the T-die between the metal roll and the touch roll, from the viewpoint of transferring a smooth surface to the film.

[0063] From the viewpoint of reducing the surface roughness of the resin film, it is desirable that the surface roughness of the metal roll is small, and furthermore, it is desirable that the surface roughness of the touch roll is also small. This is because the surface roughness of the metal roll and the touch roll is reflected in the surface roughness of the resin film. Therefore, the arithmetic mean roughness Ra of the surface of the metal roll measured according to JIS B0601:2001 is preferably 100 nm or less, more preferably 80 nm or less, even more preferably 60 nm or less, even more preferably 40 nm or less, even more preferably 20 nm or less, and can be, for example, 10 to 100 nm. The arithmetic mean roughness Ra of the surface of the touch roll measured according to JIS B0601:2001 is preferably 150 nm or less, more preferably 120 nm or less, and can be, for example, 100 to 150 nm.

[0064] (3. Resin film laminated with substrate) A substrate may be laminated to each of the resin films according to the first and second embodiments. Thus, in one embodiment of the present invention, a resin film is provided in which a substrate is laminated on either one surface of the resin film according to the first embodiment. In another embodiment of the present invention, a resin film is provided in which a substrate is laminated on the front layer and / or back layer of the resin film according to the second embodiment. It is preferable that the average total thickness of the resin film laminated with the substrate is 50 to 1000 μm in terms of workability and cost in bonding to automobile interior parts.

[0065] Examples of the substrate include layers such as a decorative layer, a protective layer, an adhesive layer, a printed layer, and a metal deposition layer. The substrate may be used as a single layer, or may be used by combining and laminating two or more types. In a typical embodiment, a resin film is provided in which a decorative layer is laminated on the back surface layer of the resin film according to the second embodiment. In another typical embodiment, a resin film is provided in which a printed layer is formed on the back surface layer of the resin film according to the second embodiment, and another substrate (such as a decorative layer) is laminated on the printed layer. As the decorative layer, for example, an acrylic resin, a polycarbonate resin, a polyvinyl chloride resin, a polyester resin, or a resin composition containing these resins can be used. In addition, additives such as pigments can be appropriately added to the decorative layer.

[0066] In addition, the resin films according to the first and second embodiments can be multi-layered with films such as isotactic or syndiotactic polypropylene, high density polyethylene, low density polyethylene, polystyrene, polyethylene terephthalate, ethylene-vinyl acetate copolymer (EVA) as layers other than the decorative layer, and various decorative treatments such as embossing can be performed.

[0067] As described above, the resin film according to the first embodiment and the second embodiment can have the characteristics of having high transparency and being difficult to whiten. Therefore, by applying the resin film to a substrate surface having high brightness and glossiness where whitening is easily noticeable, this characteristic can be effectively utilized. Therefore, in a preferred embodiment, the 60° specular gloss of the substrate on the bonding surface with the resin film measured based on JIS Z8741:1997 is 100 to 600, typically 300 to 550, and the L* at a light receiving angle of 15° in the L*a*b* color space based on JIS Z8781-4:2013 is 0 to 20, typically 0 to 5.

[0068] Examples of the method for laminating the substrate to the resin film according to the first embodiment and the second embodiment include adhesive lamination and heat lamination. Other known lamination methods can also be adopted. In addition, the resin film according to the first embodiment and the second embodiment can be used for heat molding. Examples of the heat molding method include a method in which a substrate is bonded to one or both sides of the resin film, and then vacuum molding, pressure molding, and vacuum pressure molding are used.

[0069] Examples of methods for surface coating articles such as automobile interior parts with decorative films include film insert molding, in-mold molding, and vacuum lamination molding (including vacuum and pressure molding such as TOM molding). Among them, film insert molding has the advantage that the decorative film can follow parts with more complex shapes compared to in-mold molding and vacuum lamination molding, since the decorative film is heated and preformed, and a good surface coating state can be achieved. Although film insert molding involves heating and cooling, the resin films according to the first and second embodiments are not easily whitened even when heated and cooled, so film insert molding can be suitably applied. EXAMPLES

[0070] The present invention will be described in detail below based on examples and comparative examples.

[0071] <1. Single layer film> (1-1.Materials) As polyvinylidene fluoride resin (PVDF), Kynar 1000HD (PVDF homopolymer with a melting point of 168° C.) manufactured by Arkema was prepared. As a polymethacrylate resin (PMMA), Sumipex MGSS (polymethylmethacrylate with a Tg of 101° C.) manufactured by Sumitomo Chemical Co., Ltd. was prepared.

[0072] (1-2. Film Production) According to the test number, each compound was obtained after kneading with a φ30 mm twin screw extruder according to the composition described in Table 1. Each compound obtained was melt extrusion molded using a φ40 mm T-die type single screw extruder, and the extruded film-like resin composition was sandwiched and cooled between a metal roll and a rubber touch roll through which cooling water flows, to obtain a film of a predetermined average thickness described in Table 1. At this time, the temperature of the resin composition at the outlet (lip) of the T-die was fixed at 210°C, and the time until one surface of the film was contacted with the surface of the metal roll after being extruded from the outlet of the T-die was fixed at 4 seconds, and the crystallization degree and the ratio of α-type crystals of the resin composition constituting the film were controlled by changing the surface roughness of the touch roll. In addition, in Comparative Example 6, the surface roughness of the film in contact with the touch roll was changed by changing the surface roughness of the touch roll.

[0073] (1-3. Average film thickness) For each film (800 mm in width direction) produced under the above conditions, a laser microscope (Keyence, VK-X100) was used to observe the cross section of the film at a magnification of 2000 times, and the film thickness was measured based on the distance between two points. Measurements were performed at 17 points at 50 mm intervals in the film width direction (TD) at one arbitrary point in the machine direction (MD), and the average value was taken as the measured value. The results are shown in Table 1.

[0074] (1-4. Surface roughness) For each film produced under the above conditions, the arithmetic mean roughness Ra of both sides of the film was measured based on JIS B0601:2001. The arithmetic mean roughness Ra was measured using a laser microscope (Keyence Corporation, VK-X100) at a magnification of 1000 times on the film surface. The results are shown in Table 1. The arithmetic mean roughness Ra of the metal roll surface based on JIS B0601:2001 was measured using a contact type surface roughness meter (Mitutoyo Corporation, SJ210) and was 0.013 μm. The arithmetic mean roughness Ra of the touch roll surface based on JIS B0601:2001 was measured using a contact type surface roughness meter (Mitutoyo Corporation, SJ210) and was 0.116 μm (however, Comparative Example 6 was 3.712 μm).

[0075] (1-5. Crystallinity) The crystallinity of the resin composition constituting each film produced under the above conditions was measured based on the crystalline fusion enthalpy by the method described above. The crystalline fusion enthalpy was measured using a DSC (BRUKER, DSC3100SA) under the condition that a 1.5 mg film sample was sealed in an aluminum pan and heated from room temperature to 200°C at a heating rate of 10°C / min. The results are shown in Table 1.

[0076] (1-6. α type crystal ratio) The ratio of α-type crystals in the resin composition constituting each film produced under the above conditions was measured based on the infrared absorption spectrum by the method described above. The infrared absorption spectrum was measured using a JASCO FT-IR (FT / IR4600) with an accumulation number of 64 times. The results are shown in Table 1.

[0077] (1-7.Total light transmittance) For each film produced under the above conditions, the total light transmittance was measured based on JIS K7375:2008 using a haze meter NDH7000 (manufactured by Nippon Denshoku Industries Co., Ltd.) The results are shown in Table 1.

[0078] (1-8.HAZE) For each film prepared under the above conditions, a haze meter NDH7000 (manufactured by Nippon Denshoku Industries Co., Ltd.) was used to measure the haze value (before heating) based on JIS K7136:2000 at 25°C. Next, for each film prepared under the above conditions, it was heated in air from 25°C to 170°C at an average heating rate of 3.5°C / sec, and within 1 second after reaching 170°C, it was placed in a temperature environment of 25°C and allowed to cool to 25°C in air. For the film that had undergone the heating and cooling, a haze meter NDH7000 (manufactured by Nippon Denshoku Industries Co., Ltd.) was used to measure the haze value (after heating) based on JIS K7136:2000. The results are shown in Table 1.

[0079] (1-9. Bleaching resistance) Each film produced under the above conditions was heated in air to 170°C at an average heating rate of 3.5°C / sec, and within 1 second of reaching 170°C, it was placed in a 25°C environment and allowed to cool to 25°C in air. The whitening state of the film before and after heating was visually evaluated according to the following criteria. The results are shown in Table 1. 〇: No whitening was observed ×: Whitening was confirmed

[0080] (1-10. Chemical resistance 1) Each film produced under the above conditions was cut into a 10 cm square, and 5 g of a chemical (sunscreen cream, product name: Neutrogena Ultra Sheer SPF45) was applied to the surface of the film that had come into contact with the metal roll surface. After leaving the film to stand at 55°C for 4 hours, the surface was wiped off and the appearance was checked. Evaluation was based on the following criteria. The results are shown in Table 1. ◎: No change in appearance ○: Slight traces of chemicals remain and slight wrinkles appear. ×: The film becomes cloudy and significantly deforms.

[0081] (1-11. Chemical resistance 2) 0.2 mL of a chemical (engine oil, product name: HONDA Ultra U) was dropped onto the surface of each film produced under the above conditions that had come into contact with the metal roll, and the film was left to stand at room temperature for 1.5 hours, then wiped off, and then left to stand for a further 3 hours at 80°C before the appearance was checked. Evaluation was based on the following criteria. The results are shown in Table 1. ◎: No change in appearance ○: Slight traces of chemicals remain and slight wrinkles appear. ×: The film becomes cloudy and significantly deforms.

[0082] (1-12. Film forming properties) The film formability of each film produced under the above conditions was evaluated according to the following criteria. The results are shown in Table 1. ◎: No problem at all ○: The film is not stiff enough, causing poor winding. ×: Film formation is difficult due to the occurrence of holes and breaks in the film.

[0083] [Table 1-1]

[0084] [Table 1-2]

[0085] <2. Laminated film> (2-1.Materials) ·For surface layer As polyvinylidene fluoride resin (PVDF), Kynar 1000HD (PVDF homopolymer with a melting point of 168° C.), manufactured by Arkema, was prepared. As a polymethacrylate resin, Sumipex MGSS (polymethyl methacrylate with a Tg of 101° C.) manufactured by Sumitomo Chemical Co., Ltd. was prepared. For back layer As polyvinylidene fluoride resin (PVDF), Kynar 720 (a homopolymer of vinylidene fluoride, melting point 169° C.) manufactured by Arkema was prepared. As the polymethacrylate resin, a polymethacrylate resin containing rubber components of butyl acrylate (n-BA) and butyl methacrylate (BMA) was prepared, the product name of which is Hi-pet HBS000 manufactured by Mitsubishi Chemical Corporation. As a triazine-based ultraviolet absorbing agent, Tinuvin 1600 (trade name) manufactured by BASF was prepared. As the crosslinked acrylic ester-based fine particles, GM-0105 (volume median particle diameter: 2 μm) manufactured by Aica Kogyo Co., Ltd. was prepared. The volume median particle diameter of the crosslinked (meth)acrylic ester-based resin particles used as the raw material refers to the 50% volume particle diameter of the cumulative particle size distribution curve on a volume basis obtained by measurement using a laser diffraction / scattering method. Since there were substantially no particles with a particle diameter of less than 1 μm, it is acceptable to consider that the total amount blended into the raw material constitutes the crosslinked (meth)acrylic ester-based resin particles in the resin film.

[0086] (2-2. Film Production) According to the test number, the compounds for the surface layer and the back layer were obtained after kneading with a φ30 mm twin screw extruder according to the composition described in Table 2. The compounds for the surface layer and the compounds for the back layer were melt-extruded using two φ40 mm single screw extruders and a feed block type T-die type multi-layer extruder equipped with a feed block and a T-die at the tip, and the extruded film-like resin composition was sandwiched between a metal roll and a rubber touch roll through which cooling water flows, and cooled to obtain a film of a predetermined average thickness described in Table 2. At this time, the temperature of the resin composition at the outlet (lip) of the T-die was fixed at 210 ° C., and the time until the surface of the surface layer side of the film was contacted with the surface of the metal roll (however, in Comparative Example 12, the touch roll) after extrusion from the outlet of the T-die was fixed at 4 seconds, and the surface temperature of the metal roll ("metal roll temperature" in the table) was changed to control the crystallinity and the ratio of α-type crystals of the resin composition constituting the surface layer of the film. In Comparative Example 12, the surface roughness of the film's contact surface with the touch roll (front layer side) was changed by changing the surface roughness of the touch roll. In Comparative Example 13, the surface roughness of the film's contact surface with the touch roll (back layer side) was changed by changing the surface roughness of the touch roll.

[0087] (2-3. Average film thickness) For each film (800 mm in width direction) produced under the above conditions, a laser microscope (Keyence, VK-X100) was used to observe the cross section of the film at a magnification of 2000 times, and the thickness of the front layer and back layer was measured based on the distance between two points. Measurements were performed at 17 points at 50 mm intervals in the film width direction (TD) at one arbitrary point in the machine direction (MD), and the average value was taken as the measured value. The results are shown in Table 2.

[0088] (2-4. Surface roughness) For each film produced under the above conditions, the arithmetic mean roughness Ra based on JIS B0601:2001 was measured on both sides of the film. The arithmetic mean roughness Ra was measured using a laser microscope (Keyence Corporation, VK-X100) at a magnification of 2000 times. The results are shown in Table 2. The arithmetic mean roughness Ra based on JIS B0601:2001 on the metal roll surface was measured using a contact type surface roughness meter (Mitutoyo Corporation, SJ210) and was 0.013 μm. The arithmetic mean roughness Ra based on JIS B0601:2001 on the touch roll surface was measured using a contact type surface roughness meter (Mitutoyo Corporation, SJ210) and was 0.116 μm (however, Comparative Example 12 was 3.712 μm).

[0089] (2-5. Crystallinity) The crystallinity of the resin composition constituting the surface layer of each film produced under the above conditions was measured based on the enthalpy of fusion of crystals by the method described above. The enthalpy of fusion of crystals was measured using a DSC (BRUKER, DSC3100SA) under the condition that 1.5 mg of a sample of the film was sealed in an aluminum pan and heated from room temperature to 200°C at a heating rate of 10°C / min. The results are shown in Table 2. The lower layer does not crystallize because it contains a large amount of polymethacrylic acid ester resin. Therefore, even if the measurement is performed in the state of a laminated film, the enthalpy of fusion of the crystals obtained is essentially an evaluation of only the crystals of the surface layer.

[0090] (2-6. α type crystal ratio) The ratio of α-type crystals in the resin composition constituting the surface layer of each film produced under the above conditions was measured based on the infrared absorption spectrum by the method described above. The infrared absorption spectrum was measured using a JASCO FT-IR (FT / IR4600) with an accumulation number of 64. The results are shown in Table 2.

[0091] (2-7.Total light transmittance) For each film produced under the above conditions, the total light transmittance was measured based on JIS K7375:2008 using a haze meter NDH7000 (manufactured by Nippon Denshoku Industries Co., Ltd.) The results are shown in Table 2.

[0092] (2-8.HAZE) For each film prepared under the above conditions, a haze meter NDH7000 (manufactured by Nippon Denshoku Industries Co., Ltd.) was used to measure the haze value (before heating) based on JIS K7136:2000 at 25°C. Next, for each film prepared under the above conditions, it was heated in air from 25°C to 170°C at an average heating rate of 3.5°C / sec, and within 1 second after reaching 170°C, it was placed in a temperature environment of 25°C and allowed to cool to 25°C in air. For the film that had undergone the heating and cooling, a haze meter NDH7000 (manufactured by Nippon Denshoku Industries Co., Ltd.) was used to measure the haze value (after heating) based on JIS K7136:2000. The results are shown in Table 2.

[0093] (2-9. Bleaching resistance) Each film produced under the above conditions was heated in air to 170°C at an average heating rate of 3.5°C / sec, and within 1 second of reaching 170°C, it was placed in a 25°C environment and allowed to cool to 25°C in air. The whitening state of the film before and after heating was visually evaluated according to the following criteria. The results are shown in Table 2. 〇: No whitening was observed ×: Whitening was confirmed

[0094] (2-10. Chemical resistance 1) Each film produced under the above conditions was cut into a 10 cm square, and 5 g of a chemical (sunscreen cream, product name: Neutrogena Ultra Sheer SPF45) was applied to the film surface (i.e., the surface of the surface layer) that had come into contact with the metal roll surface, and after leaving it to stand at 55°C for 4 hours, it was wiped off and the appearance was confirmed. Evaluation was performed according to the following criteria. The results are shown in Table 2. ◎: No change in appearance ○: Slight traces of chemicals remain and slight wrinkles appear. ×: The film becomes cloudy and significantly deforms.

[0095] (2-11. Chemical resistance 2) 0.2 mL of a chemical (engine oil, product name: HONDA Ultra U) was dropped onto the surface of each film produced under the above conditions that had come into contact with the metal roll surface (i.e., the surface of the surface layer), and the film was left to stand at room temperature for 1.5 hours, then wiped off, and then further left to stand at 80°C for 3 hours before the appearance was checked. Evaluation was performed according to the following criteria. The results are shown in Table 2. ◎: No change in appearance ○: Slight traces of chemicals remain and slight wrinkles appear. ×: The film becomes cloudy and significantly deforms.

[0096] (2-12. Bleeding out of UV absorbers) Each film prepared under the above conditions was subjected to a total of four heat cycle tests, with each cycle consisting of exposure to the following environments: -30°C x 7h → 23°C x 1h → 80°C x 15h → 23°C x 1h. After the heat cycle tests, the surface of the back layer was observed at a magnification of 2000 times using a laser microscope to see if the UV absorber had bled out. The results are shown in Table 2. ○: No bleed out ×: Bleed out

[0097] (2-13. Film forming properties) The film formability was evaluated based on the appearance of each film produced under the above conditions according to the following criteria. The results are shown in Table 2. ◎: No problem at all ○: Slight holes etc. occur, but film formation is possible ×: Film formation is difficult due to significant hole formation or film breakage.

[0098] (2-14. Peel strength with white polyvinyl chloride film) The back layer side of each film prepared under the above conditions was thermally laminated to a white polyvinyl chloride film (manufactured by Kyowa Leather Co., Ltd.) at a roll temperature of 140°C and a line speed of 0.5 m / min. The obtained film laminated with the substrate was cut into a width of 10 mm, and a 180° peel test was performed by peeling the film from the white polyvinyl chloride film in a direction perpendicular to the width direction at a speed of 50 mm / min using a Strograph (manufactured by Toyo Seiki Co., Ltd., STROGRAPH VE10). The maximum value of the peel strength at this time was taken as the measured value. The results are shown in Table 2.

[0099] <Consideration> In Examples 1 to 16, the composition of the resin composition constituting the resin film, the degree of crystallinity, the ratio of α-type crystals, the average thickness, and the haze were all suitable, so that a resin film with high transparency and resistance to whitening even when heated and cooled was obtained. In addition, the resin film had excellent chemical resistance. In Example 15, crosslinked acrylic acid ester-based fine particles were added to the back layer, so that the surface roughness of the outer surface of the back layer was slightly larger than that of the other Examples. In Example 16, the compatibility of the ultraviolet absorber was deteriorated due to the increase in the ratio of PVDF in the back layer, and bleeding out of the ultraviolet absorber was observed. In Comparative Examples 1, 2, 8, and 9, the composition of the resin composition constituting the resin film was inappropriate, so that the ratio of α-type crystals was high and whitening occurred due to heating. In Comparative Examples 3 and 10, the average thickness of the resin film was too thin, making film formation difficult. In Comparative Examples 4 and 11, whitening was observed due to the resin film having an excessively thick average thickness. In Comparative Example 5, the composition of the resin composition constituting the resin film was inappropriate, so that the crystallinity of the resin composition constituting the resin film did not increase, and the chemical resistance was poor. In Comparative Example 6, the surface roughness of the resin film at the contact surface with the touch roll was large, resulting in insufficient transparency. In Comparative Example 12, the outer surface of the surface layer of the resin film had high surface roughness, resulting in insufficient transparency. In Comparative Examples 7 and 14, the temperature of the metal roll during cooling was high, so the ratio of α-type crystals increased, causing whitening. In Comparative Example 13, the amount of crosslinked acrylic ester-based fine particles added was too large, and the surface roughness of the outer surface of the back surface layer was large, resulting in insufficient transparency.

[0100] [Table 2-1]

[0101] [Table 2-2]

[0102] [Table 2-3] [Explanation of symbols]

[0103] 100 Resin Film 110 Surface layer 120 Back layer

Claims

1. A resin film made of a resin composition containing 50 to 80 parts by mass of a polyvinylidene fluoride resin and 20 to 50 parts by mass of a polymethacrylate resin relative to 100 parts by mass in total of the polyvinylidene fluoride resin and the polymethacrylate resin, The crystallinity of the resin composition is 15% to 35%; The ratio of α-type crystals to the total mass of α-type crystals and β-type crystals in the resin composition is 0 to 10% by mass, The average thickness of the resin film is 5 to 200 μm, The haze of the resin film measured according to JIS K7136:2000 is 20% or less. Resin film.

2. The resin film according to claim 1, wherein at least one surface has an arithmetic mean roughness Ra of 100 nm or less as measured in accordance with JIS B0601:2001.

3. 3. The resin film according to claim 1, which has a haze of 5% or less as measured in accordance with JIS K7136:2000.

4. The resin film according to any one of claims 1 to 3, having a total light transmittance of 90% or more as measured based on JIS K7375:2008.

5. The resin film according to any one of claims 1 to 4, wherein the resin film is heated in air from 25°C to 170°C at an average heating rate of 3.5°C / sec, placed in a temperature environment of 25°C within 1 second after the temperature reaches 170°C, and then cooled in air to 25°C. The change in haze value ΔHAZE measured according to JIS K7136:2000 is 5% or less.

6. a surface layer made of a resin composition containing 50 to 80 parts by mass of a polyvinylidene fluoride resin and 20 to 50 parts by mass of a polymethacrylate resin relative to 100 parts by mass in total of the polyvinylidene fluoride resin and the polymethacrylate resin; a back surface layer laminated on the front surface layer, the back surface layer being composed of a resin composition containing 0 to 30 parts by mass of a polyvinylidene fluoride resin and 70 to 100 parts by mass of a polymethacrylate resin relative to 100 parts by mass in total of the polyvinylidene fluoride resin and the polymethacrylate resin; A resin film comprising: The degree of crystallinity of the resin composition constituting the surface layer is 15% to 35%; the ratio of α-type crystals to the total mass of α-type crystals and β-type crystals in the resin composition constituting the surface layer is 0 to 10% by mass, The average thickness of the surface layer is 5 to 200 μm, The average thickness of the back surface layer is 5 to 300 μm, The haze of the resin film measured according to JIS K7136:2000 is 20% or less. Resin film.

7. The resin film according to claim 6, wherein at least one of the outer surface of the front layer and the outer surface of the back layer has an arithmetic average roughness Ra of 100 nm or less as measured in accordance with JIS B0601:2001.

8. The resin film according to claim 6 or 7, which has a haze of 5% or less as measured in accordance with JIS K7136:2000.

9. The resin film according to any one of claims 6 to 8, having a total light transmittance of 90% or more as measured based on JIS K7375:2008.

10. The resin film according to any one of claims 6 to 9, wherein the change in haze value ΔHAZE measured according to JIS K7136:2000 before and after an operation of heating in air from 25°C to 170°C at an average heating rate of 3.5°C / sec, placing in a temperature environment of 25°C within 1 second after the temperature reaches 170°C, and cooling to 25°C in air is 5% or less.

11. The resin film according to any one of claims 6 to 10, wherein the resin composition constituting the back surface layer contains 0.1 to 10 parts by mass of an ultraviolet absorber per 100 parts by mass of the total of the polyvinylidene fluoride resin and the polymethacrylic acid ester resin.

12. The resin film according to claim 11, wherein the ultraviolet absorbing agent comprises a triazine-based compound, a benzotriazole-based compound, or a mixture thereof.

13. The resin film according to any one of claims 6 to 12, wherein the resin composition constituting the back surface layer contains 0.1 to 10 parts by mass of crosslinked (meth)acrylic acid ester-based resin particles per 100 parts by mass of the total of the polyvinylidene fluoride-based resin and the polymethacrylic acid ester-based resin.

14. The resin film according to any one of claims 1 to 13, which is used for lamination with a substrate.

15. The 60 ° specular gloss measured based on JIS Z8741: 1997 on the bonding surface of the substrate with the resin film is 100 to 600, and L* at a light receiving angle of 15 ° in the L*a*b* color space based on JIS Z8781-4: 2013 is 0 to 20. The resin film according to claim 14.

16. The resin film according to any one of claims 1 to 13, which is used for hot forming.

17. a step of melt-extrusion molding a resin composition containing 50 to 80 parts by mass of a polyvinylidene fluoride resin and 20 to 50 parts by mass of a polymethacrylate resin relative to a total of 100 parts by mass of the polyvinylidene fluoride resin and the polymethacrylate resin from a T-die at a temperature of 200° C. to 260° C. into a film having an average thickness of 5 to 200 μm; a step of contacting at least one surface of the melt-extruded film with the surface of a metal roll adjusted to a temperature of 30 to 50° C. within 4 seconds after being extruded from the outlet of the T-die, and cooling the film; The method for producing a resin film according to any one of claims 1 to 5, comprising:

18. a first resin composition containing 50 to 80 parts by mass of a polyvinylidene fluoride resin and 20 to 50 parts by mass of a polymethacrylate resin relative to 100 parts by mass in total of the polyvinylidene fluoride resin and the polymethacrylate resin; a second resin composition containing 0 to 30 parts by mass of a polyvinylidene fluoride resin and 70 to 100 parts by mass of a polymethacrylic acid ester resin relative to 100 parts by mass in total of the polyvinylidene fluoride resin and the polymethacrylic acid ester resin; a step of melt-co-extrusion molding the first resin composition into a film shape from a T-die at a temperature of 200° C. to 260° C. so that the first resin composition has an average thickness of 5 to 200 μm and the second resin composition has an average thickness of 5 to 300 μm; a step of contacting at least a surface of the melt-coextruded film on the side of the first resin composition with a surface of a metal roll adjusted to a temperature of 30 to 50° C. within 4 seconds after the film is extruded from an outlet of the T-die, and cooling the film; The method for producing a resin film according to any one of claims 6 to 13, comprising:

19. The method for producing a resin film according to claim 17 or 18, wherein the surface of the metal roll has an arithmetic mean roughness Ra of 100 nm or less as measured in accordance with JIS B0601:2001.

Citation Information

Patent Citations

  • Manufacture of vinylidene fluoride resin film which is superior in transparency

    JP1994091734A

  • Resin composition and laminated resin plate

    JP2005112972A

  • Method for manufacturing of propylene resin film

    JP2011218646A

  • Fluororesin-laminated acrylic resin film and molded article including the same

    JP2012187934A

  • Film, method for producing same, laminated film or sheet, and laminate

    WO2011142453A1