Non-oriented metal flat plate product, method for producing non-oriented metal flat plate product, and use of non-oriented metal flat plate product

A steel alloy with enhanced Mn and Cr content and surface layer distribution addresses the challenges of high-frequency magnetic performance and mechanical integrity in non-oriented electrical steel, ensuring efficient operation and cold rolling capability.

JP7559220B2Active Publication Date: 2024-10-01THYSSENKRUPP STEEL EUROPE AG PATENTE PATENT DEPARTMENT
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2023509808
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-09-01
Filing Date
2021-06-04
Publication Date
2024-10-01
Estimated Expiration
2041-06-04

AI Technical Summary

Technical Problem

Existing non-oriented electrical steel strips and sheets face challenges in achieving high magnetic polarization, low remagnetization loss, and high magnetic induction while maintaining mechanical integrity, particularly at high frequencies, due to high silicon and aluminum content leading to brittleness and poor cold rolling ability.

Method used

A steel alloy composition with increased manganese (Mn) and chromium (Cr) content, combined with specific elemental distribution in the surface layer, enhances magnetic properties and mechanical strength, allowing for thinner products with improved cold rolling capability.

Benefits of technology

The alloy composition achieves high magnetic polarization and low remagnetization losses, with improved mechanical properties, enabling efficient operation in high-frequency electromagnetic fields and facilitating cold rolling processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007559220000001
    Figure 0007559220000001
  • Figure 0007559220000002
    Figure 0007559220000002
  • Figure 0007559220000003
    Figure 0007559220000003
Patent Text Reader

Abstract

The present invention relates to a non-oriented flat metal product, and in particular to a non-oriented flat metal product having a relatively high weight ratio of Mn and Cr. The present invention also relates to a method for producing the product and to its use.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to non-oriented metal flat products, methods for making the flat products, and uses. [Background technology]

[0002] In the context of the development described below, the term metal flat product includes in particular rolled products, such as steel strip, steel sheet, steel section or steel blanks, produced by casting. In particular, the invention relates to flat products formed as electrical steel strip and to flat products formed as electrical steel sheet.

[0003] Non-oriented flat products, particularly non-oriented electrical steel strip or sheet, are required in many electronics applications.

[0004] Non-oriented electrical steel strip or sheet, often also called "NO electrical steel strip" or "NO electrical steel sheet" (NGO = Non Grain Oriented), is used, for example, as a substrate for the manufacture of parts of rotating electrical machines. In such applications, non-oriented metal plate-shaped products are used to control and amplify the direction of electromagnetic fields. Typical fields of application for such strip or sheet are rotors and stators in electric motors and generators.

[0005] In the case of many electric motors, for example those developed for so-called electromobility applications that are becoming increasingly important, it is desirable to operate them at high revolutions per unit of time. In order to operate electric motors at high revolutions per unit of time, the frequency of the alternating electromagnetic fields required as the fundamental basis for driving the motor is high. For this reason, there is an increasing demand for materials that are intended to be used in alternating electromagnetic fields of relatively high frequency.

[0006] In the development of electric motors that operate in high frequency alternating magnetic fields, material developers are faced with the challenge of increasing the efficiency of the electric motors. Against this background, there is a need for non-oriented metal flat products, in particular non-oriented electrical steel strip and non-oriented electrical steel sheet, that have relatively low remagnetization losses at relatively high frequencies, relatively high magnetic polarization and magnetic induction, and relatively high magnetic permeability.

[0007] The combination of said properties is well achieved in proven electrical steel strips and sheets by a high weight proportion of silicon and / or aluminum in the starting alloys of the electrical steel strips and sheets. However, the high proportion of said elements generally entails the disadvantage that previously known NO electrical steel strips or sheets having the properties referred to as a result of a high silicon and / or aluminum content have a relatively high brittleness and therefore disadvantages in terms of processability, e.g. cold rolling ability. For example, breakages of said steel strips may occur more frequently during the cold rolling of the NO electrical steel strips. Summary of the Invention [Problem to be solved by the invention]

[0008] Against the above mentioned background, it is an object of the present invention to provide an alternative to known flat steel products, which meets given requirements equally well or better in terms of magnetic properties, the flat products to be provided being usable even at very low final thicknesses, for example less than 0.35 mm. [Means for solving the problem]

[0009] The present invention provides a flat product having the features as defined in claim 1. The present invention further provides a method having the features as defined in claim 7. The present invention further comprises a flat product having the features as defined in claim 13 and a use having the features as defined in claim 15. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] We provide a non-oriented metal plate product comprising a steel having the following alloying composition, the elements being given in weight percentage, or wt% for brevity: C: 0.0020~0.005 Si: 2.6~2.9 Al: 0.5~0.8 Mn: 1.1 to 1.3 Cr: 0.7 to 1.6, preferably 0.9 to 1.6, particularly preferably 1.0 to 1.6 N: 0.0001~0.0060 S: 0.0001 to 0.0035 Ti: 0.001 to 0.010 P: 0.004~0.060 Optional ingredients: 0.001~0.15 The balance is Fe and unavoidable impurities.

[0011] It is to be understood that the specification of the balance refers to the fact that the weight percentages of all alloy components, including the balance, add up to 100 wt%.

[0012] In particular, Ni, Cu, Sn, Co, Zr, Nb, V, and Mo may be included as optional components as long as the total weight ratio of these elements does not exceed the upper limit stated above.

[0013] Due to this process, Mg and Ca may be contained in a ratio of 0.0005wt% to 0.005wt%, and in the context of this description, are included in the above-mentioned unavoidable impurities.

[0014] A very important step in order to provide a flat product which combines advantageous magnetic properties with advantageous mechanical properties has been achieved by significantly increasing the Mn and Cr contents of the flat product having the alloy specification according to the invention compared to known compositions of electrical steel strip or sheet.

[0015] Surprisingly, the increased Mn content and the increased Cr content not only result in a magnetic property profile within the desired numerical range compared to materials with higher Si and / or Al contents and lower Mn and / or Cr contents, but also in a more advantageous behavior under mechanical stress, e.g. during cold rolling, both results being explained in detail below and demonstrated in the description of the manufactured examples.

[0016] With regard to the magnetic properties, it has been surprisingly shown that the material according to the invention combines a relatively high magnetic polarization with relatively low remagnetization losses.

[0017] Preferably, the non-oriented flat product is a non-oriented electrical steel strip or sheet, each made of a steel having an alloy composition according to the present invention.

[0018] The flat product according to the invention preferably has magnetic polarization and remagnetization losses to which the following relationships apply selectively or cumulatively: Abs[P 1.0;1000 ×d / (J 200;1000 ×([Mn]+[Cr])^2)]<9, and / or P 1.0;400 < 16 W / kg, and / or P 1.0;1000 <70 W / kg

[0019] The mathematical symbols in the above formula are selected as follows: Abs[]: Absolute value of the value in square brackets P 1.0;1000 : Remagnetization loss in a material in an alternating electromagnetic field with a remagnetization frequency of 1000 Hz and a magnetic flux density of 1.0 T (W / kg) P 1.0;400 : Remagnetization loss in a material in an alternating electromagnetic field with a remagnetization frequency of 400 Hz and a magnetic flux density of 1.0 T (W / kg) J 200;1000 Magnetic polarization in a 1000Hz alternating electromagnetic field at a magnetic field strength of 200A / m d: material thickness (mm)

[0020] All the numerical values ​​of the above values ​​are intended to be used as dimensionless numerical values, i.e. without units, within the square brackets of the formula, which has been empirically found to be valid for the preferred samples according to the invention, in summarizing the results obtained and using the dimensionless numerical values ​​associated with the above formula symbols with the above units.

[0021] Relational formula P 1.0;400 <16 W / kg indicates that the material has a remagnetization loss (W / kg) of less than 16 W / kg in an alternating electromagnetic field having a remagnetization frequency of 400 Hz and a magnetic flux density of 1.0 T.

[0022] Relational formula P 1.0;1000 <16 W / kg indicates that the material has a remagnetization loss of less than 70 W / kg in an alternating electromagnetic field having a remagnetization frequency of 1000 Hz and a magnetic flux density of 1.0 T.

[0023] Alternatively or additionally, J 200;1000 It is preferable to apply >1.0. 200;1000 >1.0 indicates that the magnetic polarization is greater than 1.0 T at a magnetic field strength of 200 A / m in a 1000 Hz alternating electromagnetic field.

[0024] Methods for determining the magnetic polarization and magnetic field strength are known to the person skilled in the art, for example by Epstein frame for determining the magnetic polarization, in particular according to DIN EN60404-2:2009-01: Magnetic materials Part 2: Methods for determining the magnetic properties of electrical steel strips and sheets using the Epstein frame.

[0025] Preferably, the plate-shaped product may alternatively or additionally be characterized in that the following relationship is maintained at a temperature of ≧18° C. and ≦28° C., preferably ≧20° C. and ≦24° C.: 2.2≦([Mn]+[Cr]) 2 ×[ρ spec ]≦5.5 In the above formula, [Mn] represents the dimensionless value of the Mn content (wt%), [Cr] represents the dimensionless value of the Cr content (wt%), [ρ spec ] is the specific electrical resistivity (Ωmm 2 / m) is a dimensionless value.

[0026] It has been found that flat products which satisfy the above relationship between the specific electrical resistivity and the Mn and Cr contents combine the above desired properties at a particularly desired level. The above relationship relates the weight ratio of Mn in the steel alloy to the weight ratio of Cr in the steel alloy. As a result, for a given resistivity, it is achieved that, on the one hand, a minimum content is also in the sum of Mn and Cr, which results in a given specific resistivity and related electromagnetic properties, and, on the other hand, a maximum content of Mn or Cr is not exceeded, even in the sum of Mn and Cr, which results in related disadvantages in the electromagnetic properties.

[0027] Particularly preferred flat products may alternatively or additionally be characterized in that they exhibit the observed surprising property of having a surface layer with increased Mn and Cr content as a result of annealing in the manufacturing process, i.e. Mn and Cr accumulate in layers at the edges of the flat product compared to the interior of the flat product.

[0028] This means, for example, that there is a depth range from the surface of the flat product to a point where the Mn and Cr contents are higher in the above-defined dimensions than in the interior of the flat product, and of course this depth range exists on both sides of the flat product, i.e. the upper and lower sides.

[0029] A flat plate-like product is preferred in which, when the content of Mn and Cr in the edge layer, i.e., the boundary region up to the surface, is integrated over the volume of the boundary region, the value is 0.2 or more relative to the content of Al and Si.

[0030] Particularly preferred is a flat plate-like product in which the value of the Mn and Cr contents, obtained by integrating the volume of this boundary region from the surface to a depth of 0.95 micrometers, is 0.2 or more relative to the Al and Si contents.

[0031] That is, after final annealing, in a surface layer of 0 μm to 0.95 μm, i.e., a maximum depth of 0.95 μm from the surface, the ratio of the sum of the volume integral mass densities of Mn and Cr to the sum of the volume integral mass densities of Si and Al is preferably 0.2 or more.

[0032] This can be expressed as a formula as follows.

[0033]

number

[0034] In the above formula, [Mn] represents the dimensionless value of the Mn content (wt%), [Cr] represents the dimensionless value of the Cr content (wt%), [Al] represents the dimensionless value of the Al content (wt%), [Si] represents the dimensionless value of the Si content (wt%), The integral boundaries indicate depths (in micrometers) below the surface, and the integral symbol indicates that the ratio of the sum of the Mn and Cr contents to the sum of the Al and Si contents is greater than 0.2 up to a depth of 0.95 μm and over the entire surface of a preferred flat product according to the invention.

[0035] Surprisingly, the results of the depth resolved elemental analysis show that the elemental composition according to the invention provides the prerequisites for a distinct enrichment of Mn and Cr in the near-surface region of the flat product. The special feature of enrichment of the elements Mn and Cr in the near-surface region was experimentally determined for the samples after final annealing by Glow-Discharge Optical Emission Spectroscopy (GDOES) according to the test specification ISO 11505:2012-12.

[0036] Due to the special and novel element distribution in the surface layer up to 0.95 μm depth of the inventive flat products having higher Mn and Cr contents than conventional high silicon electrical steel strip flat products, it is possible to prevent to a certain extent the formation of embrittled ordered phases (D03 type structure) known to those skilled in the art, which would be caused by the high Si and Al contents at the surface and would be brought about by Mn and Cr related "disturbances" of the atomic lattice order. As a result of the fact that the proportional weight excess as mentioned above in the sense of the resulting high Mn and Cr content relative to the Si and Al contents necessarily reduces to a certain extent the known Si and Al induced brittle phases, the adverse effect of these brittle phases on the formability known to those skilled in the art is consequently eliminated, and therefore the inventive flat products and their developments have a high processability during cold rolling, punching and cladding, and generally during forming.

[0037] Particularly preferably, the flat plate product according to the invention has a specific electrical resistivity of 0.60 Ωmm at a temperature of 28° C. 2 / m~0.70Ωmm 2 / m, more preferably 0.60Ωmm 2 / m~0.65Ωmm 2 / m. The specific electrical resistivity of the above specification correlates with good magnetic properties obtained.

[0038] Particularly preferably, the maximum thickness of the flat product is less than 0.35 mm, particularly preferably between 0.19 mm and 0.31 mm. In one embodiment, the flat product is a metal sheet or strip, the thickness of which meets the above criteria everywhere. As mentioned above, the thickness of the flat product is preferably thin, since a thinner thickness reduces remagnetization losses more than a thicker thickness. It turns out that the expected excellent cold rollability improves the processability of the flat product according to the invention and is therefore particularly advantageous.

[0039] One of the methods described below may be used to produce a material having the advantages based on the alloy specifications described at the beginning. For example, the method according to the invention described below produces a flat plate product having a particularly advantageous combination of properties. The following steps are carried out: A) melting a melt containing an elemental composition according to the alloy specification described above. B) casting the melt to form a rollable primary product, in particular a primary strip, slab or thin slab; C) hot rolling the primary product at a final rolling temperature of 820°C to 890°C. D) Pickling step E) Optionally, annealing the hot rolled strip. F) Cold rolling step G) Final annealing step

[0040] Within the scope of the present invention, final annealing is understood to mean the annealing of the flat product according to the invention at the end of the manufacturing method described above, i.e. in the last method step before carrying out the insulating lacquer coating.

[0041] Particularly advantageous properties are obtained if the primary product is heated to a preheat temperature of up to 1200° C. at the start of hot rolling. Step D) is carried out after step C).

[0042] It is particularly preferable to coil the hot-rolled strip at a coiling temperature between 500° C. and 750° C. in step C) or after step D), if step D) is performed, before step E), if step E) is performed, and / or before step F).

[0043] The annealing of the hot rolled strip in step E) is preferably carried out at a temperature between 700° C. and 790° C. The annealing of the hot rolled strip is preferably carried out for a period of at least 12 hours and at most 36 hours.

[0044] As a result of the cold rolling in step F), the flat product has particularly advantageous properties when the total cold rolling reduction is between 75% and 90%. It is particularly preferred to roll the flat product to a thickness of between 0.19 mm and 0.31 mm. More preferably, the rolling is carried out in not more than 4 passes.

[0045] A final anneal at a preferred temperature of 930° C. to 1070° C. has been shown to give advantageous properties. A final anneal time of up to 300 seconds is particularly preferred. A final anneal time of at least 50 seconds is preferred.

[0046] The final annealing is preferably carried out in a continuously operating furnace through which the flat product passes, such as a horizontal continuous furnace.

[0047] It is particularly preferred to carry out the above-mentioned final annealing in one step rather than in two steps.

[0048] It is particularly preferred to carry out steps A) to G) in alphabetical order.

[0049] Another aspect of the present application is a flat plate product, or a development thereof, that may be obtained using any of the methods described above.

[0050] Yet another aspect of the present application is the use of a stamped piece obtained by stamping one of the flat products described above as a lamella in a rotating electrical machine. EXAMPLES

[0051] The invention will now be explained in more detail with reference to exemplary embodiments.

[0052] Three electrical steel strips according to the invention were produced, hereinafter referred to as Variation 1, Variation 2 and Variation 3. The compositions of Variations 1, 2 and 3 are given in Table 1. Further variations are referred to as Reference Examples 1, 2 and 3. Examples 1, 2 and 3 serve as comparative samples not according to the invention, and their alloy compositions are also given in Table 1.

[0053] From the alloys shown in the table, low sulfur and nitrogen contents were adjusted by ladle refining, and each slab was produced by continuous injection or thin slab injection. Then, strips were produced from each slab by hot rolling, pickling, hot rolled strip annealing, cold rolling, and final annealing. In the examples, the material was heated up to 1200°C before hot rolling, and rolled to a hot rolled strip thickness of 1.3 mm to 1.9 mm at a final rolling temperature of 820°C to 890°C and a coiling temperature of 500°C to 750°C.

[0054] The produced hot rolled strip was pickled and then annealed at 700-790°C for 24 hours. This step is not necessarily part of the present invention, i.e. it is an optional step. The annealed hot rolled strip was formed in up to 4 passes with a total cold reduction of 75-90% to a final thickness of 0.19mm-0.31mm (+ / - 8%).

[0055] Final annealing is carried out at a maximum temperature of 930℃ to 1070℃.

[0056] Table 1 shows the manufacturing parameters of Modifications 1 to 3 and Reference Examples 1 to 3.

[0057] [Table 1]

[0058] After the final annealing, the specific electrical resistivity of the samples was measured using a Wheatstone measuring bridge according to DIN EN 60404-13:2015-01.

[0059] [Table 2]

[0060] Table 3 shows the properties of the prepared Samples 1 to 3 and Reference Examples 1 to 3.

[0061] The magnetic value P at 1.0T, 1000Hz and the magnetic value J at 200A / m, 1000Hz were measured on a 60×60mm 2 The measurements were made using a panel of 100 mm x 100 mm. In each case, the average values ​​of the vertical and horizontal values ​​were calculated.

[0062] In particular, it was found that in addition to very good magnetic polarization, a desired small magnetic remagnetization loss P occurs at 1.0 T and 1000 Hz at a field strength of 200 A / m, which is approximately in the order of magnitude of the results obtained with the reference sample.

[0063] [Table 3]

[0064] Table 4 shows the following properties of samples 1.1, 2.1, 2.2, 2.3, 3.1 produced from analyses 1-3 and reference samples 1.1, 1.2, 2.1, 3.1-3.5 produced from reference analyses 1-3. The numbers after the dots indicate that multiple samples were randomly made from one sample for optical analysis to verify the robustness of the tests performed. For example, five samples were made from reference material 3 and numbered 3.1-3.5.

[0065] The special feature of the surface layer of the flat products, enriched in the elements Mn and Cr, was determined by glow discharge spectroscopy according to test specification ISO 11505:2012-12. Measurements were performed on the upper (OS) and lower (US) sides of the samples. In addition, measurements were made across a bandwidth at the sample edges (R1 / R2) and at the center (M). Mass measurement curves were obtained over a sample depth of 0-12 μm, from which integral evaluations of the mass density from the surface (0 μm) to a sample depth of 0.95 μm were made for Mn, Cr, Al, and Si.

[0066] [Table 4-1] [Table 4-2] [Table 4-3]

Claims

1. Each of the components, expressed as percent by weight, or wt%, is C: 0.0020-0.005, Si: 2.6 to 2.9, Al: 0.5-0.8, Mn: 1.1 to 1.3, Cr: 0.7-1.6, N: 0.0001 to 0.0060, S: 0.0001 to 0.0035, Ti: 0.001 to 0.010, P: 0.004 to 0.060, and The balance is Fe and unavoidable impurities. It consists of: A non-oriented metal flat product in which the ratio of the total Mn and Cr content (kg / m^3) to the total Al and Si content (kg / m^3) is 0.2 or more in the boundary region from the surface to a depth of 0.95 μm.

2. Specific electrical resistance at 28°C is 0.60 Ωmm 2 / m≦ρ spec ≦0.70Ωmm 2 2. The flat product according to claim 1, wherein the thickness of the flat plate is 1 / m.

3. Abs [P 1.0;1000 ×d / (J 200;1000 × ([Mn] + [Cr])^2) < 9, and / or P 1.0;400 < 16 W / kg, and / or P 1.0;1000 < 70 W / kg, and / or J>1.0T at 200A / m, 1000Hz and The thickness of the flat product is 0.19 mm to 0.31 mm. The flat product according to claim 1 or 2.

4. At temperatures between 18°C ​​and 28°C, 2.2≦([Mn]+[Cr]) 2 × [ρ spec]≦5.5 Fulfilling In the above formula, [Mn] represents a dimensionless value of the Mn content (wt%), [Cr] represents a dimensionless value of the Cr content (wt%), [ρ spec ] is the specific electrical resistivity (Ωmm) of the cold rolled strip after final annealing 2 / m) represents a dimensionless value, A flat product according to any one of claims 1 to 3.

5. 5. The flat product according to claim 1, having a thickness d of d<0.35 mm.

6. 6. The flat product according to claim 5, wherein the thickness d is in the range of 0.19 mm<d<0.35 mm.

7. A method for producing a non-oriented metal flat product according to any one of claims 1 to 6, comprising the steps of: A) melting a melt comprising the elemental composition according to claim 1; B) casting the melt to form a rollable primary product, primary strip, slab, or thin slab; C) hot rolling the primary product at a final rolling temperature of 820°C to 890°C; D) a pickling step; E) annealing the hot rolled strip; F) a cold rolling step; G) a final annealing step; Including, The step E) of annealing the hot-rolled strip is carried out at a temperature of 700-790°C for 12-36 hours, and the flat product is produced in a boundary region from the surface to a depth of 0.95 μm, in which the ratio of the total content of Mn and Cr (kg / m^3) to the total content of Al and Si (kg / m^3) is 0.2 or more.

8. 8. The method of claim 7, wherein the primary product is heated to a preheat temperature of 1200°C or less at the start of the hot rolling step.

9. 9. The method according to claim 7 or 8, wherein after step C), the hot rolled strip is coiled at a coiling temperature of 500°C to 750°C.

10. 10. The method according to any one of claims 7 to 9, wherein the cold rolling step F) is carried out with a total cold rolling reduction of 75% to 90%.

11. 11. The method of claim 10, wherein the flat product is rolled in no more than four passes to a thickness of 0.19 mm to 0.31 mm.

12. A method according to any one of claims 7 to 11, wherein the final annealing step is carried out at a temperature between 930°C and 1070°C.

13. Use of a punched out of a flat product according to any one of claims 1 to 6 as a lamella in a rotating electrical machine.

Citation Information

Patent Citations

  • Non-oriented electrical steel sheets and method for manufacturing the same

    CN104726794A

  • Nonoriented silicon steel sheet having excellent blanking workability

    JP2002080948A

  • Continuous casting method for non-oriented electrical steel strip

    JP2006501361A

  • Method for continuously casting non-oriented electrical steel strip

    JP2011094233A

  • Non-oriented electrical steel sheet having excellent high frequency core loss, and method of producing the same

    JP2011219795A