Preparation method of high-superposition low-loss Fe-Si-Al metal magnetic powder core
By adjusting the composition and particle size of the ferrosilicon aluminum powder and using the passivation method of the multi-layer composite insulating layer, the problem of low DC superposition performance of the ferrosilicon aluminum magnetic powder core is solved, and a high superposition and low loss ferrosilicon aluminum metal magnetic powder core is realized The preparation of the output inductor line filter and power factor corrector are suitable for devices such as output inductor line filters and power factor correctors.
Patent Information
- Application Number
- CN202411277686.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-12
- Publication Date
- 2024-11-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The DC superposition performance of the ferrosilicon aluminum magnetic powder core in high DC and AC bias fields is relatively low, which limits its application, and the prior art is difficult to improve the DC superposition performance on the basis of reducing losses.
By adjusting the composition and particle size of aerosolized iron-silicon aluminum powder, the passivation method of a multi-layer composite insulating layer is adopted to optimize the concentration and pH of the passivation liquid, and the gap between the insulating layer is repaired by combining nano-oxidized powder to prepare high superposition and low loss ferrosilicon aluminum metal magnetic powder core.
The magnetic permeability is about 60, the core loss is below 150mW/cm3, and the DC superposition characteristic reaches 68.5%, which significantly improves the overall performance of the ferrosilicon aluminum magnetic powder core.
Smart Images

Figure CN119008216A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of metal soft magnetism, and in particular to a method for preparing a high-overlapping low-loss Sendust metal magnetic powder core. Background Art
[0002] With the rapid development of science and technology, the miniaturization and lightness of equipment have led to the miniaturization and high power density of electronic devices. Therefore, it is necessary to use magnetic powder core materials with high magnetic flux density, high DC bias performance, and high frequency and low loss. As a soft magnetic material with good high-frequency performance and low cost, Sendust magnetic powder core has been widely used in devices such as output inductor line filters and power factor correctors. Its market demand is increasing day by day. However, due to the factors of the material itself, the DC superposition performance of Sendust material is the lowest among all alloy magnetic powder cores, which seriously limits the application of Sendust material in high DC and AC bias fields. How to improve the DC superposition performance while reducing its loss has become a major challenge in today's research.
[0003] The patent application with publication number CN 114551021 A discloses a method for preparing a low-loss FeSiAl-based composite soft magnetic powder core. By selecting 400-mesh atomized FeSiAl magnetic powder and 200-mesh FeNi magnetic powder, and according to the alloy composition mass percentage of 55%:45%, a low-loss 60μ FeSiAl-based composite soft magnetic powder core is prepared. The core has the advantages of low loss and high DC bias performance. The DC bias performance of the powder core under 100Oe is higher than 70%, and the volume loss Pcv under 50kHz and 100mT is lower than 100mW / cm 3 The performance of the magnetic powder core is very good, but the addition of iron-nickel magnetic powder has deviated from the component elements of sendust powder, and the price is high. Patent application publication number CN109979740A discloses a low-loss sendust metal magnetic powder core insulation coating method, including the following steps: preparation of metal soft magnetic powder, phosphating treatment, drying, insulation coating, drying and screening, pressing and molding, annealing and sintering. Although the invention can obtain the following magnetic powder core performance: magnetic permeability 60-70, low core loss 270mW / cm 3 The test conditions are 50kHz, 100mT, but there is no mention of improving the DC superposition characteristics. Summary of the invention
[0004] In order to solve the above technical problems, the purpose of the present invention is to provide a method for preparing a high-overlay low-loss Sendust metal powder core, and the powder composition and particle size of the magnetic powder core are adjusted to obtain a Sendust metal powder core with low loss and high DC bias performance.
[0005] In order to achieve the above object, the technical solution provided by the present invention is:
[0006] A high-overlap low-loss iron-silicon-aluminum metal magnetic powder core, comprising the following components and weight contents:
[0007] Gas atomized iron silicon aluminum powder 1 30% to 50%;
[0008] Gas atomized iron silicon aluminum powder 2 50% to 70%;
[0009] The atomized sendust powder 1 is composed of the following components and weight contents: Al 5.4%, Si 9.6%, Fe 81%; the atomized sendust powder 2 is composed of the following components and weight contents: Al 5.0-6.0%, Si 7.8-9.0%, and the rest is Fe.
[0010] Preferably, the atomized Sendust powder 1 has a particle size range of -200 to +400 mesh, and the atomized Sendust powder 2 has a particle size range of -400 mesh.
[0011] The method for preparing the high-overlap low-loss FeSiAl metal powder core as described above comprises the following specific steps:
[0012] Step 1: Atomization powder making: weigh the raw materials according to the component ratio, put them into a vacuum medium frequency furnace for smelting, pour the molten steel into the atomization equipment, and use high-pressure nitrogen to impact the steel liquid, so as to obtain gas-atomized sendustine powder 1 and gas-atomized sendustine powder 2;
[0013] Step 2: Particle size ratio: The atomized sendust powder 1 and the atomized sendust powder 2 in step 1 are screened according to the particle size intervals, and the required powder particle sizes of the atomized sendust powder 1 and the atomized sendust powder 2 are selected for particle size ratio, and mixed in proportion to obtain the original powder to be passivated;
[0014] Step 3: Insulation coating: Add the prepared passivation solution to the original powder to be passivated in step 2, stir evenly, then put it on a heating furnace to fry and dry, cool to form a passivated powder, then add 1.0wt.% silicone resin acetone solution to the passivated powder, stir evenly, heat and fry to dry, then place it in an oven for drying, take it out and cool it to obtain the sendust powder with insulation coating;
[0015] Step 4: Pressing and molding: adding a release agent and auxiliary materials to the insulatingly coated sendust powder, stirring evenly, and pressing into a ring shape to obtain a ring sample;
[0016] Step 5: Heat treatment: placing the annular sample in a tube furnace for heat treatment under a protective atmosphere to obtain a magnetic core;
[0017] Step 6: Impregnation and spraying: Put the magnetic core into the impregnation liquid mixed with epoxy resin and acetone in proportion, soak for a certain period of time, clean it, put it into the oven for baking, and then put it into the coating machine for spraying to obtain a high stacking and low loss iron silicon aluminum metal powder core.
[0018] Preferably, in step 3, the passivation solution is composed of the following components by weight: 0.1%-0.3% weak acid, 0.2%-0.8% sodium nitrate solution, 0.3%-5% nano-oxidation powder, and the rest is deionized water, and the pH value of the passivation solution is controlled to be 4-7. The sodium nitrate solution is a commercially available 80-90% sodium nitrate solution.
[0019] Preferably, the weak acid is one or more of oxalic acid, acetic acid and boric acid.
[0020] Preferably, the nano oxide powder is one or more of zinc oxide powder, aluminum oxide powder and silicon dioxide powder.
[0021] Preferably, in step three, the oven temperature is 150-200° C., and the drying time is 20-30 min.
[0022] Preferably, in step 4, the auxiliary material is glass powder, and the release agent is one or more of zinc stearate, calcium stearate, and paraffin.
[0023] Preferably, in step 4, the mass ratio of the insulating coated sendust powder, the release agent and the glass powder is 100:0.6:0.2, and the molding pressure is 800-1200 MPa.
[0024] Preferably, in step five, the annealing temperature is 600-700°C, the heating rate is 10°C / min, the holding time is 1 hour, the annealing atmosphere is a mixture of one or more of hydrogen, nitrogen and argon, and rapid cooling is performed after the holding is completed.
[0025] Compared with the prior art, the technical solution provided by the present invention has the following significant effects: a high-overlapping, low-loss sendust metal magnetic powder core of the present invention, the magnetic powder core comprises atomized sendust powder 1 and atomized sendust powder 2, and the powders of the two components are sieved at different particle sizes to select the sendust powder with better comprehensive performance; in the preparation method of the magnetic powder core, the passivation method is optimized to form a main and auxiliary composite insulation layer, so that the insulation layer is more uniform and dense, the concentration and pH value of the passivation solution are controlled in a targeted manner, and the magnetic powders with different components are effectively corroded and passivated, wherein sodium nitrate is used as an oxidizing salt to in-situ passivate the magnetic powder, the reaction is relatively mild, and the main insulation layer is effectively formed, and then nano-oxidation powder is used for the auxiliary insulation layer to repair the gaps in the main insulation layer to prepare a magnetic powder core with a magnetic permeability of about 60 and a core loss of 150mW / cm 3The following is a sendust metal powder core with high superposition and low loss performance, with a DC superposition characteristic of up to 68.5%. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 The DC-Bias curve of the Sendust metal powder core product of Example 1;
[0027] Figure 2 This is a loss curve diagram of the Sendust metal powder core product of Example 1. DETAILED DESCRIPTION
[0028] The following will describe the insulation coating method of low-loss Sendust metal powder core in conjunction with embodiments.
[0029] Embodiment 1:
[0030] This embodiment 1 discloses a high-overlap low-loss iron silicon aluminum metal magnetic powder core, including the following components and weight contents:
[0031] Gas atomized sendust powder 1 50%;
[0032] Gas atomized sendust powder 2 50%;
[0033] The atomized sendust powder 1 is composed of the following components and weight contents: Al 5.4%, Si 9.6%, Fe 81%; the atomized sendust powder 2 is composed of the following components and weight contents: Al 5.0%, Si 8.2%, and the rest is Fe.
[0034] This embodiment 1 also discloses a method for preparing a high-overlap low-loss iron silicon aluminum metal powder core, and the specific steps are as follows:
[0035] Step 1: using a vacuum gas atomization smelting furnace to smelt gas atomized Sendust powder 1 and gas atomized Sendust powder 2;
[0036] Step 2: Screen the atomized sendust powder 1 in step 1 to obtain powder with a mesh size of -200 to +400, and screen the atomized sendust powder 2 to obtain powder with a mesh size of -400, and mix the powders in a ratio of 1:1 to form raw powder to be passivated;
[0037] Step 3: prepare a passivation solution with a pH of 5 according to the ratio of acetic acid accounting for 0.1%, sodium nitrate solution accounting for 0.8%, nano zinc dioxide powder accounting for 0.3%, and the rest being deionized water, pour the original powder to be passivated into the passivation solution, heat in a 90°C water bath, stir until the solution evaporates to dryness, then add the passivated powder into a 1.0wt.% silicone resin acetone solution, stir evenly, heat and fry until dry, then place in an oven at 180°C to dry for 20 minutes, take out and cool;
[0038] Step 4: Add 0.6wt% zinc stearate and 0.2wt% glass powder into the cooled powder, mix well, and press into shape at a molding pressure of 1200MPa.
[0039] Step 5: sintering the sample in an argon atmosphere furnace at 600° C. for 1 hour to obtain a magnetic core;
[0040] Step 6: Place the magnetic core in 40% epoxy resin acetone impregnation liquid, soak for a certain period of time, clean it, place it in an oven for baking, and then place it in a coating machine for spraying to obtain the Sendust metal magnetic powder core.
[0041] Comparative Example 1:
[0042] This embodiment 1 discloses a high-overlap low-loss iron silicon aluminum metal magnetic powder core, which is composed of the following components and weight contents:
[0043] Gas atomized sendust powder 1 10%;
[0044] Gas atomized sendust powder 2 90%;
[0045] The atomized sendust powder 1 is composed of the following components and weight contents: Al 5.4%, Si 9.6%, Fe 81%; the atomized sendust powder 2 is composed of the following components and weight contents: Al 5.0%, Si 8.2%, and the rest is Fe.
[0046] This embodiment 1 also discloses a method for preparing a high-overlap low-loss iron silicon aluminum metal powder core, and the specific steps are as follows:
[0047] Step 1: using a vacuum gas atomization smelting furnace to smelt gas atomized Sendust powder 1 and gas atomized Sendust powder 2;
[0048] Step 2: Screen the atomized sendust powder 1 in step 1 to obtain powder of -200 to +400 mesh, and screen the atomized sendust powder 2 to obtain powder of -400 mesh, and mix the powders according to a ratio of 1:9 to form raw powder to be passivated;
[0049] Step 3: prepare a passivation solution with a pH of 5 by mixing acetic acid at 0.1%, sodium nitrate solution at 0.8%, nano zinc dioxide powder at 0.3%, and the rest at deionized water, pour the original powder to be passivated into the passivation solution, heat in a 90°C water bath, stir until the solution evaporates to dryness, then add the passivated powder into a 1.0wt.% silicone resin acetone solution, stir evenly, heat and fry until dry, then place in an oven at 180°C for 20 minutes, take out and cool;
[0050] Step 4: Add 0.6wt% zinc stearate and 0.2wt% glass powder into the cooled powder, mix well, and press into shape at a molding pressure of 1200MPa.
[0051] Step 5: sintering the sample in an argon atmosphere furnace at 600° C. for 1 hour to obtain a magnetic core;
[0052] Step 6: Place the magnetic core in 40% epoxy resin acetone impregnation liquid, soak for a certain period of time, clean it, place it in an oven for baking, and then place it in a coating machine for spraying to obtain the Sendust metal magnetic powder core.
[0053] Embodiment 2:
[0054] This embodiment 1 discloses a high-overlap low-loss iron silicon aluminum metal magnetic powder core, which is composed of the following components and weight contents:
[0055] Gas atomized sendust powder 1 40%;
[0056] Gas atomized sendust powder 2 60%;
[0057] The atomized sendust powder 1 is composed of the following components and weight contents: Al 5.4%, Si 9.6%, Fe 81%; the atomized sendust powder 2 is composed of the following components and weight contents: Al 5.0%, Si 8.9%, and the rest is Fe.
[0058] This embodiment 1 also discloses a method for preparing a high-overlap low-loss iron silicon aluminum metal powder core, and the specific steps are as follows:
[0059] Step 1: using a vacuum gas atomization smelting furnace to smelt gas atomized Sendust powder 1 and gas atomized Sendust powder 2;
[0060] Step 2: Screen the atomized sendust powder 1 in step 1 to obtain powder with a mesh size of -200 to +400, and screen the atomized sendust powder 2 to obtain powder with a mesh size of -400, and mix the powders in a ratio of 4:6 to form raw powder to be passivated;
[0061] Step 3: prepare a passivation solution with a pH of 4 by mixing acetic acid at 0.3%, sodium nitrate solution at 0.5%, nano-silicon dioxide powder at 0.5%, and the rest at deionized water, pour the original powder to be passivated into the passivation solution, heat in a 90°C water bath, stir until the solution evaporates to dryness, then add the passivated powder into a 0.9wt.% silicone resin acetone solution, stir evenly, heat and fry until dry, then place in an oven at 150°C for 30 minutes, take out and cool;
[0062] Step 4: Add 0.6wt% zinc stearate and 0.2wt% glass powder into the cooled powder, mix well, and press into shape at a molding pressure of 1200MPa.
[0063] Step 5: sintering the sample in an argon atmosphere furnace at 600° C. for 1 hour to obtain a magnetic core;
[0064] Step 6: Place the magnetic core in 40% epoxy resin acetone impregnation liquid, soak for a certain period of time, clean it, place it in an oven for baking, and then place it in a coating machine for spraying to obtain the Sendust metal magnetic powder core.
[0065] Comparative Example 2:
[0066] This embodiment 1 discloses a high-overlap low-loss iron silicon aluminum metal magnetic powder core, which is composed of the following components and weight contents:
[0067] Gas atomized sendust powder 1 90%;
[0068] Gas atomized sendust powder 2 10%;
[0069] The atomized sendust powder 1 is composed of the following components and weight contents: Al 5.4%, Si 9.6%, Fe 81%; the atomized sendust powder 2 is composed of the following components and weight contents: Al 5.0%, Si 8.9%, and the rest is Fe.
[0070] This embodiment 1 also discloses a method for preparing a high-overlap low-loss iron silicon aluminum metal powder core, and the specific steps are as follows:
[0071] Step 1: using a vacuum gas atomization smelting furnace to smelt gas atomized Sendust powder 1 and gas atomized Sendust powder 2;
[0072] Step 2: Screen the atomized sendust powder 1 in step 1 to obtain powder of -200 to +400 mesh, and screen the atomized sendust powder 2 to obtain powder of -400 mesh, and mix the powders according to a ratio of 9:1 to form raw powder to be passivated;
[0073] Step 3: prepare a passivation solution with a pH of 4 by mixing acetic acid at 0.3%, sodium nitrate solution at 0.5%, nano-silicon dioxide powder at 0.5%, and the rest at deionized water, pour the original powder to be passivated into the passivation solution, heat in a 90°C water bath, stir until the solution evaporates to dryness, then add the passivated powder into a 0.9wt.% silicone resin acetone solution, stir evenly, heat and fry until dry, then place in an oven at 150°C for 30 minutes, take out and cool;
[0074] Step 4: Add 0.6wt% zinc stearate and 0.2wt% glass powder into the cooled powder, mix well, and press into shape at a molding pressure of 1200MPa.
[0075] Step 5: sintering the sample in an argon atmosphere furnace at 600° C. for 1 hour to obtain a magnetic core;
[0076] Step 6: Place the magnetic core in 40% epoxy resin acetone impregnation liquid, soak for a certain period of time, clean it, place it in an oven for baking, and then place it in a coating machine for spraying to obtain the Sendust metal magnetic powder core.
[0077] The performance of the sendust metal powder core samples obtained in Example 1, Example 2 and Comparative Example 1 and Comparative Example 2 was tested, wherein the DC-Bias curve of the sendust metal powder core sample of Example 1 is as shown in Figure 1 As shown, the loss curve of the sendust metal powder core sample of Example 1 is as follows Figure 2 The specific test results of each embodiment and comparative example are shown in Table 1 below:
[0078] Table 1: Test data of magnetic permeability, core loss and DC superposition characteristics of each Sendust metal powder core sample
[0079] Group Magnetic permeability (20kHz, 1.0V) <![CDATA[Pcv(mW / cm 3 )(50kHz / 100mT)]]> DC-Bias(100Oe) Example 1 59.1 148 68.1% Comparative Example 1 57.5 225 71% Example 2 58.8 144 68.5% Comparative Example 2 59.2 124 60.2%
[0080] The above test results show that the magnetic permeability of the sendust metal powder core prepared by the present invention is about 60, and the core loss can be controlled at 150mW / cm 3 The DC superposition characteristic is as high as 68.5%, and the comprehensive performance is excellent, indicating that this method can obtain a high-superposition-performance, low-loss Sendust metal powder core, which can be used in devices such as output inductor line filters and power factor correctors.
[0081] This implementation mode is only an exemplary description of this patent and does not limit its protection scope. Personnel in this field may also make partial changes to it. As long as it does not exceed the spirit of this patent, it shall be regarded as an equivalent replacement of this patent and shall be within the protection scope of this patent.
Claims
1. A high-overlay low-loss Sendust metal powder core, characterized in that: Includes the following components and weight contents: Gas atomized iron silicon aluminum powder 1 30% to 50%; Gas atomized iron silicon aluminum powder 2 50% to 70%; The atomized sendust powder 1 is composed of the following components and weight contents: Al 5.4%, Si 9.6%, Fe 81%; the atomized sendust powder 2 is composed of the following components and weight contents: Al 5.0-6.0%, Si 7.8-9.0%, and the rest is Fe.
2. The high-overlap low-loss Sendust metal powder core according to claim 1, characterized in that: The atomized Sendust powder 1 has a particle size range of -200 to +400 meshes, and the atomized Sendust powder 2 has a particle size range of -400 meshes.
3. A method for preparing a high-overlap low-loss Sendust metal powder core according to any one of claims 1 to 2, characterized in that: The specific steps are as follows: Step 1: Atomization powder making: weigh the raw materials according to the component ratio, put them into a vacuum medium frequency furnace for smelting, pour the molten steel into the atomization equipment, and use high-pressure nitrogen to impact the steel liquid, so as to obtain gas-atomized sendustine powder 1 and gas-atomized sendustine powder 2; Step 2: Particle size ratio: The atomized sendust powder 1 and the atomized sendust powder 2 in step 1 are screened according to the particle size intervals, and the required powder particle sizes of the atomized sendust powder 1 and the atomized sendust powder 2 are selected for particle size ratio, and mixed in proportion to obtain the original powder to be passivated; Step 3: Insulation coating: Add the prepared passivation solution to the original powder to be passivated in step 2, stir evenly, then put it on a heating furnace to fry and dry, cool to form a passivated powder, then add 1.0wt.% silicone resin acetone solution to the passivated powder, stir evenly, heat and fry to dry, then place it in an oven for drying, take it out and cool it to obtain the sendust powder with insulation coating; Step 4: Pressing and molding: adding a release agent and auxiliary materials to the insulatingly coated sendust powder, stirring evenly, and pressing into a ring shape to obtain a ring sample; Step 5: Heat treatment: placing the annular sample in a tube furnace for heat treatment under a protective atmosphere to obtain a magnetic core; Step 6: Impregnation and spraying: Put the magnetic core into the impregnation liquid mixed with epoxy resin and acetone, soak for a certain period of time, clean it, put it into the oven for baking, and then put it into the coating machine for spraying to obtain a high stacking and low loss iron silicon aluminum metal powder core.
4. The method for preparing a low-loss and high-overlay sendust metal powder core according to claim 3, characterized in that: In step three, the passivation solution is composed of the following components by weight: 0.1%-0.3% weak acid, 0.2%-0.8% sodium nitrate solution, 0.3%-5% nano-oxidation powder, and the rest is deionized water, and the pH value of the passivation solution is controlled to be 4-7.
5. The method for preparing a low-loss and high-overlay sendust metal powder core according to claim 4, characterized in that: The weak acid is one or more of oxalic acid, acetic acid and boric acid.
6. The method for preparing a low-loss and high-overlay sendust metal powder core according to claim 4, characterized in that: The nano-oxide powder is one or more of zinc oxide powder, aluminum oxide powder and silicon dioxide powder.
7. The method for preparing a low-loss, high-overlay sendust metal powder core according to claim 3, characterized in that: In the step 3, the oven temperature is 150-200° C., and the drying time is 20-30 minutes.
8. The method for preparing a low-loss and high-overlay sendust metal powder core according to claim 3, characterized in that: In the step 4, the auxiliary material is glass powder, and the release agent is one or more of zinc stearate, calcium stearate, and paraffin.
9. The method for preparing a low-loss and high-overlay sendust metal powder core according to claim 8, characterized in that: In step 4, the mass ratio of the insulating coated sendust powder, the release agent, and the glass powder is 100:0.6:0.2, and the molding pressure is 800-1200 MPa.
10. The method for preparing a low-loss and high-overlay sendust metal powder core according to claim 3, characterized in that: In the step 5, the annealing temperature is 600-700° C., the heating rate is 10° C. / min, the holding time is 1 hour, the annealing atmosphere is a mixture of one or more gases selected from hydrogen, nitrogen, and argon, and rapid cooling is performed after the holding is completed.
Citation Information
Patent Citations
Preparation method for ferrosilicon aluminum magnetic powder core
CN102436895A
Blueing insulation coating method for metal soft magnetic powder cores
CN107452495A
FeSiAl magnetic core and preparation method thereof
CN108597714A
Preparation method of high-permeability aerosolized iron silicon aluminum magnetic powder core
CN109285685A
Manufacturing method of low-power-consumption iron-nickel-molybdenum magnetic powder core
CN114496544A
Cited By
MHz-level low-loss Fe-Si-Al magnetic powder core and preparation method thereof
CN120299851A
A MHz-level low-loss sendust magnetic powder core and its preparation method
CN120299851B
MHz-level low-loss Fe-Si-Al magnetic powder core and infiltration diffusion preparation method thereof
CN121171776A