Method for producing pigment composition
The described method effectively reduces coarse particles and improves storage stability and production efficiency in pigment compositions by using specific dispersion techniques and liquid media with resin components, addressing issues of nozzle clogging and stability in existing technologies.
Patent Information
- Application Number
- JP2020116969
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-07-07
- Publication Date
- 2024-10-02
- Estimated Expiration
- 2040-07-07
AI Technical Summary
Existing methods for producing pigment compositions fail to effectively reduce the number of coarse particles, leading to issues such as nozzle clogging during printing and decreased storage stability, while also being inefficient in production.
A method involving the use of a rotor-stator type processing machine, bead mill, or ultrasonic dispersion machine to disperse a raw material composition, followed by a step of colliding the composition with a hard body, utilizing a liquid medium with specific Hansen Solubility Parameters (ΔD 15 to 20, ΔP 4 to 17, ΔH 6 to 43) to promote wetting and dispersion, and combining this with a resin component to enhance adsorption and stability.
The method significantly reduces coarse particles to 1.0 μm or more, improves storage stability by preventing particle settling, and enhances production efficiency by minimizing processing time and reducing nozzle clogging.
Smart Images

Figure 0007559385000002 
Figure 0007559385000003 
Figure 0007559385000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a pigment composition. [Background technology]
[0002] Pigment compositions are used in various printing processes such as inkjet printing, etc. As a method for producing a pigment composition, a method is known in which a raw material composition containing a pigment component and a liquid medium is treated with a dispersing machine to obtain the pigment composition (for example, see Patent Document 1 below). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2001-262038 A Summary of the Invention [Problem to be solved by the invention]
[0004] In order to obtain good ejection stability by suppressing clogging of ejection nozzles during printing, it is required that the pigment composition contains a small number of coarse particles.
[0005] In order to reduce the number of coarse particles, it is effective to subject a raw material composition containing a pigment, a resin component such as a pigment dispersion resin, and a liquid medium to a long-term dispersion treatment or to repeatedly feed the composition into a disperser and treat it.
[0006] However, in the above-mentioned methods, there are cases where the production efficiency of pigment compositions, inks, etc. cannot be improved.
[0007] The problem that the present invention aims to solve is to provide a method for producing a pigment composition, which can reduce the number of coarse particles that may be contained in the pigment composition, prevent a decrease in storage stability due to an increase in the number of coarse particles over time, and improve the production efficiency of the pigment composition. [Means for solving the problem]
[0008] The present invention provides a method for producing a pigment composition in which the pigment component is dispersed in a liquid medium by the resin component, the method comprising: step A producing a first raw material composition by mixing a resin component, a pigment component, a basic compound, and a liquid medium; step B producing a second raw material composition by treating the first raw material composition with a rotor-stator type processor, a bead mill processor, an ultrasonic disperser, or a disperser; and step C treating the second raw material composition with a disperser having a configuration for colliding the second raw material compositions with each other or a configuration for colliding the second raw material composition with a hard body, the method comprising the steps of: 1 ) and the polarity term (δP 1 ) and hydrogen bond terms (δH 1 The present invention relates to a method for producing a pigment composition, comprising: a liquid medium (a) having Effect of the Invention
[0009] According to the method for producing a pigment composition of the present invention, it is possible to reduce the number of coarse particles having a particle diameter of 1.0 μm or more that may be contained in the pigment composition, prevent a decrease in storage stability due to an increase in the number of coarse particles over time, and simultaneously improve the production efficiency of the pigment composition. [Brief description of the drawings]
[0010] [Figure 1] FIG. 2 is a schematic cross-sectional view showing an example of a rotor-stator type processing machine. [Diagram 2] FIG. 2 is a schematic side view showing an example of a stator in a rotor-stator type processing machine. [Diagram 3] FIG. 2 is a schematic diagram for explaining a pulverization or crushing process in a rotor-stator type processor. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Hereinafter, an embodiment of the present invention will be described in detail. However, the present invention is not limited to the following embodiment, and various modifications can be made within the scope of the present invention.
[0012] In this specification, a numerical range indicated using "~" indicates a range including the numerical values described before and after "~" as the minimum and maximum values, respectively. In the numerical ranges described in stages in this specification, the upper limit or lower limit of a numerical range of a certain stage can be arbitrarily combined with the upper limit or lower limit of a numerical range of another stage. In the numerical ranges described in this specification, the upper limit or lower limit of the numerical range may be replaced with a value shown in the examples. "A or B" may include either A or B, or may include both. Unless otherwise specified, the materials exemplified in this specification may be used alone or in combination of two or more types. When a plurality of substances corresponding to each component are present in the composition, the content of each component in the composition means the total amount of the plurality of substances present in the composition, unless otherwise specified. The term "process" includes not only independent processes, but also processes that cannot be clearly distinguished from other processes as long as the intended action of the process is achieved. The term "(meth)acrylic acid" is a general term for acrylic acid and the corresponding methacrylic acid, and the same applies to other similar expressions such as "(meth)acrylate."
[0013] The method for producing a pigment composition of the present invention is a method for producing a pigment composition in which the pigment component is dispersed in a liquid medium by the resin component, the method comprising the steps of: Step A producing a first raw material composition by mixing a resin component, a pigment component, a basic compound, and a liquid medium; Step B producing a second raw material composition by treating the first raw material composition with a rotor-stator type processor, a bead mill processor, an ultrasonic disperser, or a disperser; and Step C treating the second raw material composition with a disperser having a configuration for colliding the second raw material compositions with each other or a configuration for colliding the second raw material composition with a hard body, the method comprising the steps of: 1) and the polarity term (δP 1 ) and hydrogen bond terms (δH 1 ) and (a) a liquid medium (a).
[0014] The pigment composition obtained by the above method refers to a pigment component dispersed in a liquid medium such as water by a resin component such as the pigment dispersion resin (specifically, an aqueous pigment dispersion). The pigment composition may be used as a material for producing an ink, or the pigment composition itself may be used as an ink. For example, the pigment composition is preferably used for producing a printing ink or the printing ink, and more preferably used for producing an inkjet printing ink or the inkjet printing ink.
[0015] When the pigment composition is used for producing the inkjet printing ink, the ratio of solid content of the pigment composition to the total amount of the pigment composition is preferably in the range of 1 mass % to 60 mass %, and more preferably in the range of 10 mass % to 30 mass %.
[0016] First, step A of the present invention will be described.
[0017] Step A is a step of producing a first raw material composition by mixing a resin component, a pigment component, a basic compound, and a liquid medium.
[0018] In the step A, the liquid medium is a dispersion term (ΔD 1 ) and polar term (δP 1 ) and the hydrogen bond term (δH 1 ) and a liquid medium (a) having the above structure are used.
[0019] The dispersion term (δD 1 ) is preferably in the range of 12 to 24, more preferably 14 to 21, and particularly preferably 16 to 19.
[0020] The polar term (ΔP1 ) is preferably in the range of 4 to 17, more preferably 6 to 15, and particularly preferably 8 to 13.
[0021] The hydrogen bond term (δH 1 ) is preferably in the range of 6 to 43, more preferably 9 to 35, and particularly preferably 9 to 30.
[0022] Dispersion term (δD 1 ) and polar term (δP 1 ) and the hydrogen bond term (δH 1 As the liquid medium having these, for example, triethylene glycol, glycerin, 2-pyrrolidone, 1-(2-hydroxyethyl)-2-pyrrolidone, dipropylene glycol, propylene glycol, 1,5-pentanediol, etc. can be used alone or in combination of two or more kinds.
[0023] It is preferable that the liquid medium (a) satisfies at least one of the following, from the viewpoint of easily and efficiently reducing the number of coarse particles and easily shortening the time required to obtain a pigment composition having desired physical properties of the solid content (e.g., the number of coarse particles, particle size, etc.) through the step C.
[0024] When the pigment component contains carbon black, the liquid medium (a) preferably contains at least one selected from the group consisting of N-(2-hydroxyethyl)pyrrolidone, 2-pyrrolidone, triethylene glycol, and glycerin.
[0025] When the pigment component contains a magenta pigment, the liquid medium (a) preferably contains at least one selected from the group consisting of 2-pyrrolidone, triethylene glycol, dipropylene glycol, and glycerin.
[0026] When the pigment component contains a cyan pigment, the liquid medium (a) preferably contains at least one selected from the group consisting of dipropylene glycol, N-(2-hydroxyethyl)pyrrolidone, 2-pyrrolidone, triethylene glycol, and glycerin.
[0027] When the pigment component contains a yellow pigment, the liquid medium (a) preferably contains at least one selected from the group consisting of propylene glycol, N-(2-hydroxyethyl)pyrrolidone, 2-pyrrolidone, triethylene glycol, and glycerin.
[0028] In addition, the dispersion term of the liquid medium (δD 1 ) and polar term (δP 1 ) and the hydrogen bond term (δH 1 ) are values recorded in the computer software Hansen Solubility Parameters in Practice 4th Edition 4.1.07 (HSPiP).
[0029] Dispersion term (δD 1 ) and polar term (δP 1 ) and the hydrogen bond term (δH 1 By using a liquid medium containing the liquid medium (a) having the above-mentioned properties, wetting of the pigment component and swelling and dissolution of the resin component are promoted. As a result, it is possible to obtain an ink having even better storage stability and which is more likely to prevent clogging of the ink ejection nozzle in the initial stage of ink ejection, and a pigment composition used in the production of the ink.
[0030] The liquid medium (a) is preferably used in the range of 10 to 90% by mass with respect to the total amount of the liquid medium contained in the pigment composition, and using it in the range of 15 to 80% by mass makes it easier for the pigment component and the resin component to wet, swell, or dissolve in the liquid medium, promotes the adsorption of the pigment component to the surface, and makes it easier to maintain a good dispersion of the resin. As a result, it is easy to obtain excellent storage stability that prevents the occurrence of sedimentation of solids in the pigment composition over time, it is easy to prevent the occurrence of sedimentation of solids in the ink over time, it is easy to suppress the occurrence of clogging of the ink ejection nozzle at the beginning of ink ejection (it is easy to obtain excellent initial ejection stability), and it is easy to suppress the occurrence of clogging of the ink ejection nozzle over time (it is easy to obtain excellent ejection stability over time).
[0031] As the liquid medium, it is preferable to use a liquid medium (b) other than the liquid medium (a) in combination with the liquid medium (a) because the resin components such as the pigment dispersion resin are easily adsorbed to the surface of the pigment component. In particular, when a high-pressure homogenizer is used in producing the pigment composition of the present invention, or when an inkjet printing ink obtained using the pigment composition is applied to a thermal type inkjet printing method described later, it is preferable to use the liquid medium (a) in combination with the liquid medium (b) described later.
[0032] Examples of the liquid medium (b) include an aqueous medium (water, etc.), an organic solvent, etc. When a high-pressure homogenizer is used as the dispersing machine used in the present invention, a water-soluble organic solvent is preferably used among the organic solvents because high pressure is applied, and a high-boiling point solvent having a boiling point of 100° C. or more is more preferably used.
[0033] Examples of water include ion-exchanged water such as ion-exchanged water, ultrafiltered water, reverse osmosis water, and distilled water; ultrapure water, etc. As the water, it is preferable to use water that has been sterilized by ultraviolet irradiation, addition of hydrogen peroxide, etc., from the viewpoint of easily preventing the growth of mold or bacteria when the pigment composition or ink is stored for a long period of time.
[0034] The water is preferably used in an amount of 10 to 90% by mass, based on the total amount of the liquid medium contained in the pigment composition of the present invention, and is preferably used in an amount of 15 to 80% by mass in terms of producing an aqueous ink.
[0035] The organic solvent may be a water-soluble organic solvent, which can efficiently wet the surface of the pigment component and can easily adsorb a resin component (e.g., a neutralized resin) dissolved in water to the pigment component, thereby shortening the time required to achieve desired physical properties.
[0036] Examples of water-soluble organic solvents include glycols such as ethylene glycol, diethylene glycol, tetraethylene glycol, tripropylene glycol, polyethylene glycol, and polypropylene glycol; diols such as butanediol, pentanediol, and hexanediol; glycol esters such as propylene glycol laurate; diethylene glycol monoethyl, diethylene glycol monobutyl, diethylene glycol monohexyl, and carbitol; glycol ethers such as cellosolve containing propylene glycol ether, dipropylene glycol ether, or triethylene glycol ether; alcohols (excluding glycols) such as methanol, ethanol, isopropyl alcohol, 1-propanol, 2-propanol, 1-butanol, 2-butanol, butyl alcohol, and pentyl alcohol; lactones such as sulfolane, esters, ketones, and γ-butyrolactone; lactams such as N-(2-hydroxyethyl)pyrrolidone and 2-pyrrolidone. The water-soluble organic solvents can be used alone or in combination of two or more.
[0037] In addition, as the water-soluble organic solvent, it is preferable to use a high-boiling point solvent having a boiling point of 100° C. or more, such as triethylene glycol, glycerin, 2-pyrrolidone, 1-(2-hydroxyethyl)-2-pyrrolidone, dipropylene glycol, propylene glycol, or 1,5-pentanediol, which promotes wetting of the pigment and makes it easier for the resin to be adsorbed onto the pigment, thereby improving storage stability, etc.
[0038] The content of the water-soluble organic solvent is preferably 10 to 500 parts by mass, more preferably 15 to 200 parts by mass, and more preferably 15 to 150 parts by mass, relative to 100 parts by mass of the pigment component contained in the first raw material composition. In these cases, it is easy to obtain excellent storage stability that prevents the occurrence of sedimentation of solids in the pigment composition over time, it is easy to prevent the occurrence of sedimentation of solids in the ink over time, it is easy to suppress the occurrence of clogging of the ink ejection nozzle at the beginning of ink ejection (it is easy to obtain excellent initial ejection stability), and it is easy to suppress the occurrence of clogging of the ink ejection nozzle over time (it is easy to obtain excellent ejection stability over time).
[0039] The liquid medium contained in the pigment composition is preferably used in a range of 40 to 95% by mass, and more preferably in a range of 60 to 90% by mass, based on the total amount of the pigment composition of the present invention, in terms of producing an aqueous ink.
[0040] Examples of the resin component used in the step A include a pigment dispersing resin and a binder resin.
[0041] As the resin component, a conventionally known resin can be used, for example, a radical polymer can be used, and it is preferable to use a radical polymer having an aromatic ring structure or a heterocyclic structure. In this case, the resin component such as the pigment dispersion resin is easily adsorbed to the pigment component by the π-π interaction between the resin component such as the pigment dispersion resin and the pigment component, and it is easy to obtain excellent storage stability that prevents the occurrence of sedimentation of solids over time in the pigment composition, it is easy to prevent the occurrence of sedimentation of solids over time in the ink, it is easy to suppress the occurrence of clogging of the ink discharge nozzle at the beginning of ink discharge (it is easy to obtain excellent initial discharge stability), and it is easy to suppress the occurrence of clogging of the ink discharge nozzle over time (it is easy to obtain excellent discharge stability over time).
[0042] Examples of the aromatic cyclic structure or heterocyclic structure include a cyclic structure introduced into a radical polymer by using a monomer having an aromatic cyclic structure or a heterocyclic structure. The aromatic cyclic structure is preferably a benzene ring structure, and more preferably a structure derived from styrene. By using a resin component that is a radical polymer having an aromatic cyclic structure or a heterocyclic structure, it is possible to increase the adsorption of a resin component such as a pigment dispersion resin to a pigment component, and it is easy to obtain excellent storage stability that prevents the occurrence of precipitation of solids over time in the pigment composition, and it is easy to prevent the occurrence of precipitation of solids over time in the ink, and it is easy to suppress the occurrence of clogging of the ink ejection nozzle at the beginning of ink ejection (it is easy to obtain excellent initial ejection stability), and it is easy to suppress the occurrence of clogging of the ink ejection nozzle over time (it is easy to obtain excellent ejection stability over time).
[0043] As the radical polymer usable as the resin component of the pigment dispersion resin, for example, a polymer obtained by radically polymerizing various monomers can be used.
[0044] As the monomer, when an aromatic ring structure is to be introduced into a resin component such as a pigment dispersion resin, a monomer having an aromatic ring structure can be used, and when a heterocyclic structure is to be introduced, a monomer having a heterocyclic structure can be used.
[0045] Examples of monomers having an aromatic ring structure include styrene, p-tert-butyldimethylsiloxystyrene, o-methylstyrene, p-methylstyrene, p-tert-butylstyrene, p-tert-butoxystyrene, m-tert-butoxystyrene, p-tert-(1-ethoxymethyl)styrene, m-chlorostyrene, p-chlorostyrene, p-fluorostyrene, α-methylstyrene, p-methyl-α-methylstyrene, vinylnaphthalene, and vinylanthracene.
[0046] Examples of the monomer having a heterocyclic structure include vinylpyridine monomers such as 2-vinylpyridine and 4-vinylpyridine.
[0047] When a polymer having both an aromatic cyclic structure and a heterocyclic structure is used as the radical polymer, a monomer having an aromatic cyclic structure and a monomer having a heterocyclic structure can be used in combination as the monomer.
[0048] As the resin component of the pigment dispersion resin, etc., a radical polymer having an aromatic ring structure is preferable, and therefore, as the monomer, a monomer having an aromatic ring structure is preferable, and at least one selected from the group consisting of styrene, α-methylstyrene, and tert-butylstyrene is more preferable.
[0049] From the viewpoint of further increasing the adsorption of resin components such as a pigment dispersion resin to the pigment component, the content of the monomer having an aromatic cyclic structure or a heterocyclic structure is preferably 20 mass % or more, more preferably 40 mass % or more, and even more preferably 50 to 95 mass %, based on the total amount of monomers.
[0050] As the resin component such as the pigment dispersing resin, a monomer having an acid group can be used as the monomer from the viewpoint of producing a radical polymer having an acid value in the range described below.
[0051] Examples of monomers having an acid group include monomers having a carboxy group, a sulfo group, a phosphoric acid group, etc. As the monomer having an acid group, a monomer having a carboxy group is preferable, and at least one selected from the group consisting of acrylic acid and methacrylic acid is more preferable. In these cases, it is easy to obtain excellent storage stability that prevents the occurrence of precipitation of solids over time in the pigment composition, it is easy to prevent the occurrence of precipitation of solids over time in the ink, it is easy to suppress the occurrence of clogging of the ink ejection nozzle at the beginning of ink ejection (it is easy to obtain excellent initial ejection stability), and it is easy to suppress the occurrence of clogging of the ink ejection nozzle over time (it is easy to obtain excellent ejection stability over time).
[0052] From the viewpoint of easily obtaining a radical polymer having an acid value in the range described below, the content of the monomer having an acid group is preferably 5 to 80 mass%, more preferably 5 to 60 mass%, and even more preferably 5 to 50 mass%, based on the total amount of monomers usable for producing the resin component.
[0053] As monomers usable for producing resin components such as pigment dispersion resins, in addition to the above-mentioned monomers, other monomers can be used as necessary. Examples of other monomers include methyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, sec-butyl (meth)acrylate, tert-butyl (meth)acrylate, 2-ethylbutyl (meth)acrylate, 1,3-dimethylbutyl (meth)acrylate, hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, 2-methylbutyl (meth)acrylate, pentyl (meth)acrylate, heptyl (meth)acrylate, nonyl (meth)acrylate, 3-ethoxypropyl (meth)acrylate, 3-ethoxy ... Examples of the monomers include acrylate, dimethylaminoethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, ethyl-α-(hydroxymethyl) (meth)acrylate, dimethylaminoethyl (meth)acrylate, hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, phenyl (meth)acrylate, benzyl (meth)acrylate, phenylethyl (meth)acrylate, diethylene glycol (meth)acrylate, triethylene glycol (meth)acrylate, polyethylene glycol (meth)acrylate, glycerin (meth)acrylate, bisphenol A (meth)acrylate, dimethyl maleate, diethyl maleate, vinyl acetate, and the like. These monomers can be used alone or in combination of two or more. As the other monomers, such acrylates or methacrylates can be used alone, or acrylates and methacrylates can be used in combination.
[0054] As the resin component such as the pigment dispersion resin, a polymer having a linear structure formed by radical polymerization of a monomer, a polymer having a branched (grafted) structure, a polymer having a crosslinked structure, etc. can be used. The monomer sequence in each polymer is not particularly limited, and a polymer having a random type sequence or a block type sequence can be used.
[0055] The polymer having a crosslinked structure can be produced by using a monomer having a crosslinkable functional group as the monomer. Examples of the monomer having a crosslinkable functional group include poly(meth)acrylates of polyhydric alcohols such as ethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, poly(oxyethyleneoxypropylene) glycol di(meth)acrylate, and tri(meth)acrylate of alkylene oxide adduct of glycerin; glycidyl (meth)acrylate; and divinylbenzene.
[0056] As the resin component such as the pigment dispersion resin, a polymer having a structural unit derived from the above-mentioned monomer can be used, but a polymer obtained by polymerizing only a monomer having an anionic group and a monomer having an aromatic cyclic structure or a heterocyclic structure is preferred.
[0057] As the resin component such as the pigment dispersion resin, a polymer having a structural unit derived from styrene and a structural unit derived from (meth)acrylic acid is preferred, and at least one selected from the group consisting of a styrene-(meth)acrylic acid copolymer and a styrene-(meth)acrylic acid ester-(meth)acrylic acid copolymer is more preferred. The polymer having a structural unit derived from styrene and a structural unit derived from (meth)acrylic acid preferably has an acid value in the range described below. The aromatic ring moiety in the structural unit derived from styrene is firmly adsorbed to the surface of the pigment component, and the carboxyl group in the structural unit derived from (meth)acrylic acid has good affinity with water, so that good dispersion stabilization is easily obtained. This makes it easy to obtain excellent storage stability that prevents the occurrence of precipitation of solids over time in the pigment composition, makes it easy to prevent the occurrence of precipitation of solids over time in the ink, makes it easy to suppress the occurrence of clogging of the ink discharge nozzle at the beginning of ink discharge (easy to obtain excellent initial discharge stability), and makes it easy to suppress the occurrence of clogging of the ink discharge nozzle over time (easy to obtain excellent discharge stability over time).
[0058] As the styrene-(meth)acrylic acid copolymer, any of styrene-acrylic acid copolymer, styrene-methacrylic acid copolymer, and styrene-acrylic acid-methacrylic acid copolymer can be used, but at least one selected from the group consisting of styrene-acrylic acid copolymer and styrene-acrylic acid-methacrylic acid copolymer is preferred. In this case, it is easy to adjust the adsorption force with the pigment component and the dispersing force in water, and as a result, it is easy to obtain excellent storage stability that prevents the occurrence of sedimentation of solids over time in the pigment composition, it is easy to prevent the occurrence of sedimentation of solids over time in the ink, it is easy to suppress the occurrence of clogging of the ink discharge nozzle at the beginning of ink discharge (it is easy to obtain excellent initial discharge stability), and it is easy to suppress the occurrence of clogging of the ink discharge nozzle over time (it is easy to obtain excellent discharge stability over time).
[0059] In the styrene-(meth)acrylic acid copolymer, the total amount of the structural units derived from styrene, the structural units derived from acrylic acid, and the structural units derived from methacrylic acid is preferably 80 to 100 mass%, more preferably 90 to 100 mass%, based on the total amount of the structural units of the styrene-(meth)acrylic acid copolymer.
[0060] The radical polymerization rate (reaction rate) of each monomer during radical polymerization is assumed to be approximately the same, and the proportion of each monomer used (feeding ratio) is assumed to be the same as the proportion of structural units derived from each monomer that constitutes the radical polymer.
[0061] The radical polymer can be produced, for example, by radically polymerizing the above-mentioned monomers by a method such as bulk polymerization, solution polymerization, suspension polymerization, or emulsion polymerization.
[0062] When producing the radical polymer, known and commonly used polymerization initiators, chain transfer agents (polymerization degree regulators), surfactants, antifoaming agents, etc. may be used as necessary.
[0063] Examples of the polymerization initiator include 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobisisobutyronitrile, 1,1'-azobis(cyclohexane-1-carbonitrile), benzoyl peroxide, dibutyl peroxide, butyl peroxybenzoate, etc. The content of the polymerization initiator is preferably 0.1 to 10 mass% based on the total amount of monomers used in the production of the radical polymer.
[0064] When using a radical polymer obtained by solution polymerization, the resin component such as a pigment dispersion resin can be a radical polymer obtained by removing the solvent contained in the radical polymer solution obtained by solution polymerization, followed by drying and pulverization to form fine particles. When a water-soluble organic solvent and a basic compound are used in combination, the resin component, which is a finely-divided radical polymer, is neutralized by the basic compound in the 0th step, dissolved in a liquid medium containing a water-soluble organic solvent, and adsorption to the surface of the pigment component wetted with the liquid medium proceeds. As a result, it is easy to obtain excellent storage stability that prevents the occurrence of sedimentation of solids in the pigment composition over time, it is easy to prevent the occurrence of sedimentation of solids in the ink over time, it is easy to suppress the occurrence of clogging of the ink ejection nozzle at the beginning of ink ejection (it is easy to obtain excellent initial ejection stability), and it is easy to suppress the occurrence of clogging of the ink ejection nozzle over time (it is easy to obtain excellent ejection stability over time).
[0065] As the resin component such as a pigment dispersion resin, a resin component classified using a mesh sieve having a mesh size (diameter) of 1 mm or less is preferable.
[0066] The acid value of the resin component such as the pigment dispersion resin is preferably 60 to 300 mgKOH / g, more preferably 80 to 250 mgKOH / g, further preferably 100 to 200 mgKOH / g, and particularly preferably 120 to 180 mgKOH / g. In these cases, the adsorption of the resin component such as the pigment dispersion resin to the pigment component can be increased, and since it is easy to obtain a moderate affinity to the liquid medium (for example, a liquid medium containing water and a water-soluble organic solvent), it is easy to maintain a good dispersion state. Therefore, it is easy to obtain excellent storage stability that prevents the occurrence of sedimentation of solids in the pigment composition over time, it is easy to prevent the occurrence of sedimentation of solids in the ink over time, it is easy to suppress the occurrence of clogging of the ink discharge nozzle at the beginning of ink discharge (it is easy to obtain excellent initial discharge stability), and it is easy to suppress the occurrence of clogging of the ink discharge nozzle over time (it is easy to obtain excellent discharge stability over time).
[0067] The acid value is preferably an acid value derived from an anionic group such as a carboxy group, a sulfo group, a phosphate group, etc. The acid value is a value measured in accordance with the Japanese Industrial Standards "K0070:1992. Testing method for acid value, saponification value, ester value, iodine value, hydroxyl value and unsaponifiable matter of chemical products" except that tetrahydrofuran is used instead of diethyl ether as a solvent, and refers to the amount (mg) of potassium hydroxide required to completely neutralize 1 g of a resin component such as a pigment dispersion resin.
[0068] The weight average molecular weight of the resin component such as the pigment dispersion resin is preferably 2000 to 40000, more preferably 5000 to 30000, further preferably 5000 to 25000, and particularly preferably 8000 to 12000. In these cases, aggregation with adjacent pigment components is suppressed, and excellent storage stability that prevents the occurrence of precipitation of solids in the pigment composition over time is easily obtained, the occurrence of precipitation of solids in the ink over time is easily prevented, clogging of the ink discharge nozzle at the beginning of ink discharge is easily suppressed (excellent initial discharge stability is easily obtained), and clogging of the ink discharge nozzle over time is easily suppressed (excellent long-term discharge stability is easily obtained). The "weight average molecular weight" is a value measured by GPC (gel permeation chromatography) and is a value converted into the molecular weight of polystyrene used as a standard substance.
[0069] The resin component used in the step A preferably has a neutralization rate of 0 to 10% by mass. That is, the resin component preferably has all or most of the acid groups of the resin component not neutralized by a basic compound. The resin component preferably has a neutralization rate of 0 to 10% by mass, more preferably 0 to 5% by mass, and preferably 0 to 0.1% by mass. The use of 0% by mass is preferable because it improves the shear force on the raw material composition, makes it easier for the resin component to be adsorbed by the pigment component, and improves the storage stability of the pigment composition.
[0070] Here, the neutralization rate refers to a value calculated by the following formula.
[0071] Neutralization rate [%] = ((mass of basic compound [g] × 56 × 1000) / (acid value of resin component × equivalent of basic compound × (mass of resin component [g])) × 100
[0072] On the other hand, the acid groups of the resin component contained in the first raw material composition obtained through step A are neutralized by a basic compound during step A. The neutralization rate of the resin component contained in the first raw material composition is preferably in the range of 50 to 100% by mass, more preferably in the range of 80 to 100% by mass, and even more preferably in the range of 90 to 100% by mass.
[0073] When the neutralization rate of the pigment dispersion resin contained in the first raw material composition obtained through the step A is within the above range, the resin component is easily dissolved or dispersed in a liquid medium containing water, the adsorption of the pigment component to the surface is promoted, and a good dispersion state is easily maintained. As a result, it is easy to obtain excellent storage stability that prevents the occurrence of sedimentation of solids in the pigment composition over time, it is easy to prevent the occurrence of sedimentation of solids in the ink over time, it is easy to suppress the occurrence of clogging of the ink discharge nozzle at the beginning of ink discharge (it is easy to obtain excellent initial discharge stability), and it is easy to suppress the occurrence of clogging of the ink discharge nozzle over time (it is easy to obtain excellent discharge stability over time).
[0074] The content of the resin component such as the pigment dispersion resin is preferably 5 to 200 parts by mass, more preferably 10 to 100 parts by mass, relative to 100 parts by mass of the pigment component contained in the first raw material composition. This makes it easy to maintain a good dispersion state due to sufficient affinity with a liquid medium (for example, water), and since the resin component such as the pigment dispersion resin is easily adsorbed to the pigment component, it is easy to obtain excellent storage stability that prevents the occurrence of sedimentation of solids in the pigment composition over time, it is easy to prevent the occurrence of sedimentation of solids in the ink over time, it is easy to suppress the occurrence of clogging of the ink discharge nozzle at the beginning of ink discharge (it is easy to obtain excellent initial discharge stability), and it is easy to suppress the occurrence of clogging of the ink discharge nozzle over time (it is easy to obtain excellent discharge stability over time). In addition, the amount of the resin component such as the free pigment dispersion resin that is not adsorbed to the pigment component is reduced, and the dischargeability of the ink is easily improved. Furthermore, it is easy to suppress the aggregation of the pigment component due to the resin component such as the free pigment dispersion resin, and it is easy to stabilize the ink.
[0075] Next, the basic compound used in the step A will be described.
[0076] The basic compound can be used to neutralize acid groups contained in the resin components such as the pigment dispersing resin.
[0077] As the basic compound, inorganic basic compounds, organic basic compounds, etc. can be used. As the inorganic basic compound, hydroxides of alkali metals such as potassium and sodium; carbonates of alkali metals such as potassium and sodium; hydroxides of alkaline earth metals such as calcium and barium; carbonates of calcium and barium, etc. can be mentioned. As the organic basic compound, amino alcohols such as triethanolamine, N,N-dimethanolamine, N-ethylethanolamine, dimethylethanolamine, and N-butyldiethanolamine; morpholines such as morpholine, N-methylmorpholine, and N-ethylmorpholine; piperazines such as N-(2-hydroxyethyl)piperazine and piperazine hexahydrate; and ammonium hydroxide can be mentioned. As the basic compound, alkali metal hydroxides (potassium hydroxide, sodium hydroxide, lithium hydroxide, etc.) are preferable, and potassium hydroxide is more preferable, from the viewpoint of improving the dispersion stability of the pigment component adsorbed by the resin component such as the pigment dispersion resin in a liquid medium such as water, since they have excellent neutralization efficiency of the resin component such as the pigment dispersion resin.
[0078] When the basic compound is used in the step A, it is preferable that the basic compound is used in a form that is dissolved or dispersed in water in advance.
[0079] The basic compound is used in an amount such that the neutralization rate of the resin component contained in the first raw material composition is in the range of preferably 50 to 100 mass%, more preferably 80 to 100 mass%, and particularly preferably 90 to 100 mass%, in order to improve the solubility of the resin component in the liquid medium.
[0080] Next, the pigment component used in the step A will be described.
[0081] As the pigment component, at least one selected from the group consisting of pigments and pigment derivatives can be used.
[0082] As the pigment, inorganic or organic pigments can be used. Examples of inorganic pigments include iron oxide, carbon black (e.g., carbon black produced by known methods such as contact method, furnace method, and thermal method), and titanium oxide. Examples of organic pigments include azo pigments (insoluble azo pigments (monoazo pigments, disazo pigments, pyrazolone pigments, etc.), benzimidazolone pigments, beta naphthol pigments, naphthol AS pigments, condensed azo pigments, etc.), polycyclic pigments (quinacridone pigments, perylene pigments, perinone pigments, anthraquinone pigments, dioxazine pigments, thioindigo pigments, isoindolinone pigments, isoindoline pigments, quinophthalone pigments, diketopyrrolopyrrole pigments, etc.), phthalocyanine pigments, dye chelates (basic dye chelates, acid dye chelates, etc.), nitro pigments, nitroso pigments, and aniline black. These inorganic and organic pigments can be suitably used in the production of printing inks (e.g., inkjet printing inks). The pigments may be used alone or in combination of two or more.
[0083] Examples of carbon black that can be used include #2300, #980, #960, #900, #52, #45L, #45, #40, #33, MA100, MA8, and MA7 manufactured by Mitsubishi Chemical Corporation; Regal series and Monarch series manufactured by Cabot Corporation; and Color Black FW1, Color Black series, Printex series, Special Black series, and NIPEX series manufactured by Orion Engineered Carbons Co., Ltd.
[0084] As the pigment, yellow pigments such as CI Pigment Yellow 1, 2, 12, 13, 14, 16, 17, 73, 74, 75, 83, 93, 95, 97, 98, 109, 110, 114, 120, 128, 129, 138, 150, 151, 154, 155, 174, 180, and 185 can be used.
[0085] As the pigment, magenta pigments such as CI Pigment Red 5, 7, 12, 48(Ca), 48(Mn), 57(Ca), 57:1, 112, 122, 123, 146, 149, 150, 168, 176, 184, 185, 202, 209, 213, 269, and 282 can be used.
[0086] As the pigment, cyan pigments such as CI Pigment Blue 1, 2, 3, 15, 15:1, 15:2, 15:3, 15:4, 15:6, 16, 22, 60, 63, and 66 can be used.
[0087] As the pigment, orange pigments such as CI Pigment Orange 5, 13, 16, 17, 34, 36, 43, 51, 64, and 71 can be used.
[0088] As the pigment, violet pigments such as CI Pigment Violet 1, 3, 5:1, 16, 19, 23, and 38 can be used.
[0089] As the pigment, green pigments such as CI Pigment Green 1, 4, 7, 8, 10, 17, 18, 36, 50, and 58 can be used.
[0090] As the pigment, a dry pigment (pigment in a dry powder state) or a wet pigment (pigment in a wet cake state) can be used. As the magenta pigment, a wet pigment is preferred from the viewpoint of efficiently reducing the number of coarse particles and easily shortening the time required to obtain a pigment composition having the desired physical properties of the solid content (number of coarse particles, particle diameter, etc.) through the step C. As the cyan pigment, a dry pigment is preferred from the viewpoint of efficiently reducing the number of coarse particles and easily shortening the time required to obtain a pigment composition having the desired physical properties of the solid content (number of coarse particles, particle diameter, etc.) through the step C. As the pigment, a mixture or solid solution containing two or more kinds can also be used.
[0091] As the pigment component, the above-mentioned pigments can be used in combination with pigment derivatives.
[0092] As the pigment derivative, a compound in which a functional group is introduced into a pigment can be used. Examples of pigments that provide the pigment derivative include phthalocyanine pigments, azo pigments, anthraquinone pigments, quinacridone pigments, and diketopyrrolopyrrole pigments. Examples of functional groups include carboxy groups, sulfo groups, amino groups, nitro groups, acid amide groups, carbonyl groups, carbamoyl groups, phthalimide groups, and sulfonyl groups. The pigment derivative can impart dispersion stability to the pigment composition or ink that can prevent the generation of coarse particles over time and the occurrence of precipitation of pigment components and the like over time.
[0093] The primary particle size of the pigment component is preferably 1.0 μm or less, and more preferably 0.01 to 0.5 μm, from the viewpoint of more effectively suppressing sedimentation of the pigment component over time. The primary particle size refers to the number average particle size measured using a transmission electron microscope (TEM).
[0094] The pigment component is preferably 1 to 50% by mass, more preferably 10 to 30% by mass, and even more preferably 15 to 25% by mass, based on the total amount of the first raw material composition. In these cases, since it is easy to obtain appropriate fluidity, efficient and uniform treatment can be performed in each process, excellent storage stability that prevents the occurrence of sedimentation of solids in the pigment composition over time is easily obtained, the occurrence of sedimentation of solids in the ink over time is easily prevented, clogging of the ink discharge nozzle at the beginning of ink discharge and the like is easily suppressed (excellent initial discharge stability is easily obtained), and clogging of the ink discharge nozzle over time is easily suppressed (excellent discharge stability over time is easily obtained).
[0095] In the step A, a liquid medium containing the liquid medium (a), a resin component, a pigment component, and a basic compound are mixed. Examples of the step A include the following (i) to (iii). (i) A step of mixing a liquid medium containing the liquid medium (a) with a basic compound or an aqueous solution thereof to produce a mixture, and then supplying the resin component such as the pigment dispersion resin and the pigment component separately to the mixture, or supplying a mixture of the resin component such as the pigment dispersion resin and the pigment component in advance and mixing them. (ii) A step of mixing a liquid medium containing the liquid medium (a) with a resin component such as the pigment dispersion resin and a pigment component to produce a mixture, and then mixing the mixture with a basic compound or an aqueous solution thereof. (iii) A step of mixing a liquid medium containing the liquid medium (a) with a pigment component to produce a mixture, mixing a resin component such as the pigment dispersion resin with the mixture to produce a mixture, and mixing a basic compound or an aqueous solution thereof with the mixture.
[0096] In step A, a resin component such as a pigment dispersion resin having an acid group and a neutralization rate of 0 to 10% by mass is used as the resin component, and the resin component, a basic compound, and a liquid medium are mixed to produce a first raw material composition in which the acid group of the resin component is neutralized, since the shear force on the raw material composition is improved, the resin component is easily adsorbed by the pigment component, and the storage stability of the pigment composition is improved. Therefore, it is preferable that the resin component such as the pigment dispersion resin is supplied to the container in a solid (powder) form rather than in the form of a water dispersion or aqueous solution that has been neutralized in advance.
[0097] Next, the step B will be described.
[0098] The step B is a step of producing a second raw material composition by treating the first raw material composition obtained in the step A with a treating machine described below.
[0099] The step B is a step of pulverizing or crushing the aggregated pigment. The term "crushing" refers to, for example, a process of breaking up agglomerates. The term "cracking" refers to, for example, a process of breaking up aggregates.
[0100] Using the first raw material composition previously treated in step B as the second raw material composition used in step C described below is preferable in that it is possible to significantly reduce the number of times the second raw material composition is repeatedly fed into the disperser for treatment in step C, and as a result, it is possible to significantly improve the production efficiency of the pigment composition and the ink.
[0101] On the other hand, if a raw material composition containing a large amount of coarse particles obtained without going through steps A and B is treated with the disperser in step C, there is a concern that problems such as clogging of pipes in the disperser may occur. Therefore, from the viewpoint of avoiding such problems, it is effective to use a raw material composition obtained through steps A and B in which preliminary pulverization or preliminary crushing is performed as a pretreatment prior to the step of dispersing the pigment component in a liquid medium with a resin component such as a pigment dispersion resin using the disperser in step C.
[0102] Examples of the processing machine that can be used in step B include a rotor-stator type processing machine, a bead mill processing machine, an ultrasonic disperser, a disperser, and the like. Use of a rotor-stator type processing machine is preferred because it allows the pigment to be pulverized or disintegrated more efficiently, and as a result, a pigment composition having a reduced number of coarse particles can be efficiently produced.
[0103] In the rotor-stator type processor, as described below, a shear force is applied between the rotor and the stator to the first raw material composition containing coarse particles, so that the coarse particles are pulverized or disintegrated. Therefore, by carrying out the step C after carrying out the step B using the rotor-stator type processor, the number of coarse particles in the pigment composition can be reduced more efficiently, and the number of coarse particles having a particle diameter of 1.0 μm or more can be further reduced. In addition, by carrying out the step C after carrying out the step B using the rotor-stator type processor, the increase in the processing time required to obtain a pigment composition having a small number of coarse particles can be suppressed, and a pigment composition having a small number of coarse particles can be obtained with good productivity. In addition, by carrying out the step C after carrying out the step B using the rotor-stator type processor, the number of coarse particles having a particle diameter of 0.5 μm or more can also be reduced. When evaluating the reduction rate of the number of coarse particles, the reduction rate of the number of coarse particles when a first raw material composition having the same composition is pulverized or disintegrated is compared. When treating the pigment composition with various types of treating machines, the performance difference between the treating machines can be compared by using a rotation speed that is about 80% of the maximum rotation speed.
[0104] By carrying out step B using the rotor stator type processor and then carrying out step C, it is possible to efficiently reduce the number of coarse particles in the pigment composition while reducing the viscosity of the pigment composition. By carrying out step B using the rotor stator type processor and then carrying out step C, it is possible to reduce the particle size of the solid content in the pigment composition obtained by the pulverization or crushing treatment. By carrying out step B using the rotor stator type processor and then carrying out step C, it is possible to obtain excellent storage stability (dispersion stability of the solid content) in the pigment composition obtained by the pulverization or crushing treatment.
[0105] By carrying out step B using the rotor-stator type processor and then carrying out step C, it is possible to obtain a high print density when compared under conditions where the composition of the pigment composition and the mass ratio of the resin component such as the pigment dispersion resin to the pigment component are the same. Also, by carrying out step B using the rotor-stator type processor and then carrying out step C, it is possible to obtain a high adsorption rate of the resin component such as the pigment dispersion resin to the pigment component.
[0106] In the present invention, it is possible to efficiently further reduce the number of coarse particles in the pigment composition by using a rotor-stator type processor, a bead mill processor, an ultrasonic processor, or a disperser in step B to prepare a second raw material composition in which the pigment has been ground or disintegrated in advance, and by carrying out step C. In addition, by using a rotor-stator type processor, a bead mill processor, or an ultrasonic processor in step B to prepare a second raw material composition in which the pigment has been ground or disintegrated in advance, and by carrying out step C, it is possible to shorten the time required to produce a pigment composition having the desired physical properties of the solid content (number of coarse particles, particle size, etc.).
[0107] The temperature in the treatment step using the treatment machine in the step B is preferably in the following range from the viewpoint of efficiently reducing the number of coarse particles, shortening the time required to obtain a pigment composition having the desired physical properties (number of coarse particles, particle diameter, etc.) of the solid content through the step C, and promoting the dissolution of the resin component such as the pigment dispersion resin, which easily improves the adsorption rate of the resin component such as the pigment dispersion resin to the pigment component, and easily obtaining excellent storage stability. The temperature is preferably 25°C or higher, more preferably 30°C or higher, even more preferably 40°C or higher, particularly preferably 50°C or higher, extremely preferably 55°C or higher, and very preferably 60°C or higher. The temperature is preferably 80°C or lower, more preferably 75°C or lower, even more preferably 70°C or lower, particularly preferably 65°C or lower, and extremely preferably 60°C or lower. From these viewpoints, the temperature is preferably 25 to 80°C, more preferably 50 to 80°C, and even more preferably 60 to 80°C.
[0108] The rotor-stator type processor usable in the step B includes a rotor having a rotatable blade portion and a stator having a wall portion disposed on the outer periphery of the blade portion. The processor may be any of a pulverizer, a crusher, a disperser, etc. The rotor and stator may be of any shape that is commercially available, and may be used in combination with different shapes or the same shape. Since the transportability of the raw material composition, the shear rate (refining ability), the amount of heat generated during refining, etc. differ depending on the shape, the combination can be selected according to the properties of the first raw material composition. Usually, a rotor with a large number of teeth is easier to refining and generates a large amount of heat.
[0109] FIG. 1 (FIG. 1(a) and FIG. 1(b)) is a schematic cross-sectional view showing an example of a rotor-stator type processor. The rotor-stator type processor 100 shown in FIG. 1 includes a central shaft 10, a rotor 20, and a stator 30. Constituent materials of the central shaft 10, the rotor 20, and the stator 30 include metal materials, ceramics, and the like.
[0110] The central shaft 10 is an elongated member that extends, for example, in the vertical direction. The central shaft 10 supports the rotor 20 and the stator 30.
[0111] The rotor 20 has an annular (e.g., circular) blade portion 22 extending in the longitudinal direction of the central axis 10 on the outer periphery of the rotor 20, and a connection portion 24 connecting the blade portion 22 and the central axis 10. The blade portion 22 can rotate around the central axis 10. The blade portion 22 has an opening (through hole) 22a penetrating the blade portion 22, and has, for example, a plurality of openings 22a at intervals (e.g., equal intervals) along the circumferential direction of the blade portion 22. The opening direction of the openings 22a may be inclined with respect to the radial direction. The end of the openings 22a on the upper side in the vertical direction may be open without any member constituting the rotor 20 being disposed therein. The number, arrangement, and shape of the openings 22a are not particularly limited.
[0112] The arrangement and shape of the blade part in the rotor of the rotor-stator type processing machine are not particularly limited. For example, the blade part is not limited to an annular member arranged on the outer periphery of the rotor, and may have a shape extending from the center to the outer periphery of the rotor. The rotor may have a plurality of blade parts extending from the center to the outer periphery of the rotor. The blade part extending from the center to the outer periphery of the rotor may have a streamlined shape.
[0113] The stator 30 has an annular (e.g., circular) wall portion 32 extending in the longitudinal direction of the central axis 10 at the outer periphery of the stator 30, and a connection portion 34 connecting the wall portion 32 and the central axis 10. The wall portion 32 is disposed on the outer periphery side of the blade portion 22 in the rotor-stator type processor 100. The wall portion 32 has an opening (through hole) 32a penetrating the wall portion 32, and has, for example, a plurality of openings 32a spaced apart (e.g., equally spaced) along the circumferential direction of the wall portion 32. The opening direction of the openings 32a may be inclined with respect to the radial direction.
[0114] The number, arrangement and shape of the openings in the wall of the stator are not particularly limited. Figure 2 is a schematic side view showing an example of a stator (wall of the stator) in a rotor-stator type processing machine. Examples of the wall of the stator include a wall having an array of openings (e.g., rectangular openings such as square openings) (Figure 2(a)), a wall having a plurality of rectangular openings arranged in a row (Figure 2(b)), and a wall having a plurality of circular (e.g., perfect circle) openings arranged in a row (Figure 2(c)). Examples of the shape of the opening include a rectangular shape (square, rectangular, etc.), a circular shape (perfect circle, ellipse, etc.), and the like.
[0115] The stator may have a plurality of annular (e.g., annular) walls extending in the longitudinal direction of the central axis at the outer periphery of the stator. For example, the stator may have the above-mentioned wall 32 as a first wall, a second wall disposed on the outer periphery of the first wall in the rotor-stator type processor, and a third wall disposed on the outer periphery of the second wall in the rotor-stator type processor. The number of walls is not particularly limited, and may be four or more.
[0116] Fig. 3 is a schematic diagram for explaining the pulverization or disintegration process in the rotor-stator type processor, and is a schematic diagram showing an enlarged portion of the outer periphery of the rotor-stator type processor 100 shown in Fig. 1. In the rotor-stator type processor 100, for example, a first raw material composition containing a pigment component and a liquid medium is supplied around the central axis 10, and then, as shown in Fig. 3, the first raw material composition passes through the opening 22a of the blade portion 22 of the rotor 20 (flow path F1 in the figure) and reaches the space between the blade portion 22 and the wall portion 32 of the stator 30. In this space, a shear force caused by the rotational motion of the blade portion 22 is applied to the coarse particles P (solid content), so that the coarse particles P are pulverized or disintegrated. Thereafter, a portion of the composition containing the crushed or disintegrated particles flows out through the openings 32a of the wall 32 (flow path F2 in the figure) to the outer periphery of the wall 32, and the remainder of the composition advances further through the space between the blade portion 22 and the wall 32, where the particles are further crushed or disintegrated by shear force. As a result, the pigment component contained in the first raw material composition is crushed or disintegrated by the crushing or disintegrating process of the rotor-stator type processor 100.
[0117] The shear rate (refining ability) given by the treatment section constituted by the rotor and the stator is set to 50,000 s from the viewpoints of easily efficiently reducing the number of coarse particles, easily reducing the particle size of the solid content after treatment, easily reducing the viscosity of the pigment composition, and easily obtaining excellent storage stability in the pigment composition. -1 More than 75000s is preferable. -1 More than 90,000 is preferable. -1 More preferably, 100,000s-1 More than 120,000s is particularly preferable. -1 More than 150,000s is highly preferable. -1 More than 170,000s are highly preferred -1 More preferably, the upper limit of the share rate is, for example, 400,000 s -1 may be less than or equal to 250000s -1 From these viewpoints, the share rate may be 50,000 to 400,000 s -1 is preferred. -1 ] can be obtained by dividing the peripheral speed of the rotor blades [m / s] by the distance [m] between the blades and the stator wall.
[0118] The rotor-stator type processor may have a plurality of processing sections (pulverizing sections or disintegrating sections) each composed of a rotor and a stator. By flowing the first raw material composition from a processing section with a low shear rate toward a processing section with a high shear rate, clogging is easily suppressed, and the number of coarse particles is easily reduced efficiently. The rotor-stator type processor may have a plurality of processing sections along a central axis extending in the vertical direction (may have a multi-stage processing section). When the rotor-stator type processor has a plurality of processing sections along the central axis, it is preferable to arrange the processing sections with a higher shear rate vertically downward from the viewpoint of easily reducing the number of coarse particles efficiently.
[0119] The rotor-stator type processor may be an in-line processor or a batch processor. In an in-line processor, the first raw material composition is continuously supplied, and for example, a processor is installed in the middle of a processing path (for example, a grinding processing path and a crushing processing path, for example, a pipe), and the first raw material composition can be continuously processed (grinding or crushing). In an in-line processor, the first raw material composition is forced to pass through the processor in its entirety, so that the first raw material composition can be uniformly processed in a short time compared to a batch processor in which only the rotor periphery is mainly processed. With an in-line processor, the number of coarse particles can be efficiently reduced, and therefore clogging of the pipes of the processor used in the step B can be easily suppressed. With an in-line processor, the viscosity of the pigment composition can be easily reduced. In an in-line processor, the raw material composition may be circulated. With a batch processor, the raw material composition is intermittently supplied, and the first raw material composition is replaced for each processing (grinding or crushing).
[0120] Examples of rotor-stator type processors include "magic LAB" manufactured by IKA Co., Ltd. (in-line type, maximum peripheral speed: 41 m / s, maximum rotation speed: 26000 rpm); "VERSO" manufactured by Silverson Nippon Co., Ltd. (high shear in-line mixer, in-line type, maximum peripheral speed: 20 m / s, maximum rotation speed: 10000 rpm); and "L5M-A" manufactured by Silverson Nippon Co., Ltd. (batch type, maximum peripheral speed: 20 m / s, maximum rotation speed: 10000 rpm). Processors manufactured by IKA Co., Ltd. that can be used include processors equipped with a UTR module (ULTRA-TURRAX), DR module (DISPAX-REACTOR), MK module, MKO module, and CMX module. The DR module has three stages of processors (stages) consisting of rotors and stators, and the shear rate can be adjusted by the combination of rotors and stators, making it easy to efficiently reduce the number of coarse particles. For example, by using 2P / 4M / 6F processing units in this order from the top in the vertical direction, processing units with higher share rates can be arranged vertically downward.
[0121] The rotor-stator type processor preferably has a maximum rotation speed in the range of 1,000 to 30,000 rpm, more preferably in the range of 3,000 to 25,000 rpm, and is particularly preferably in the range of 8,000 to 20,000 rpm, from the viewpoints of efficiently reducing the number of coarse particles, reducing the particle size of the solid content after treatment, reducing the viscosity of the pigment composition, and achieving excellent storage stability of the pigment composition.
[0122] The rotor-stator type treating machine to be used is preferably one having a maximum peripheral speed in the range of 5 m / s to 60 m / s, more preferably one having a maximum peripheral speed in the range of 10 m / s to 60 m / s, and is particularly preferably one having a maximum peripheral speed in the range of 15 m / s to 60 m / s, from the viewpoints of easily efficiently reducing the number of coarse particles, easily reducing the particle size of the solid content after treatment, easily reducing the viscosity of the pigment composition, and easily obtaining excellent storage stability of the pigment composition.
[0123] The raw material supply unit in the pigment composition production apparatus according to the present embodiment is not particularly limited as long as it can supply the first raw material composition to the rotor-stator type processor. The raw material supply unit may be a pipe or a pump that supplies the raw material supply unit.
[0124] As the bead mill dispersing machine, for example, a paint shaker, a bead mill, a sand mill, a basket mill, a dyno mill, an SC mill, a nano mill, a spike mill, an agitator mill, etc. can be used.
[0125] As the ultrasonic disperser, a Hielcher product named "UP200St" or the like can be used.
[0126] As the disperser, a device named "Homo Disper" manufactured by Primix Corporation, a device named "Disper Mat" manufactured by Eiko Seiki Co., Ltd., or the like can be used.
[0127] Next, the step C will be described.
[0128] The step C is a step of treating the second raw material composition obtained in the step B with a dispersing machine having a configuration for colliding the second raw material composition with itself or a configuration for colliding the second raw material composition with a hard body.
[0129] Among the dispersers used in the step C, as a disperser having a configuration for colliding the second raw material compositions with each other, it is particularly preferable to use a disperser having a configuration for colliding the second raw material compositions with each other obliquely in order to simultaneously reduce the number of coarse particles in the pigment composition, reduce the dispersed particle diameter, and improve the production efficiency of the pigment composition. More specifically, by using a disperser having a configuration for colliding the second raw material compositions with each other obliquely, the number of times (so-called number of passes) in which the second raw material composition is repeatedly charged into the disperser and processed can be significantly reduced from the conventional approximately 10 to 30 times to preferably 1 to 8 times, more preferably 1 to 5 times, and particularly preferably 1 to 3 times. In particular, when carbon black is used as a pigment component, a pigment composition that achieves both a reduction in the number of coarse particles and a reduction in the dispersed particle diameter with only one pass can be obtained. An example of a configuration for colliding the second raw material compositions with each other obliquely is an oblique collision chamber. When the disperser is used, the second raw material compositions can be collided with each other by pressurizing and spraying the raw material compositions from multiple directions.
[0130] An example of the oblique impingement chamber is a chamber with the device name "Starburst" manufactured by Sugino Machine Co., Ltd. The oblique impingement chamber is preferable because it can avoid wear of the hard body described below during long-term use and can obtain a shear force superior to that of a single nozzle chamber.
[0131] Specifically, the dispersing machine may be manufactured by Sugino Machine Co., Ltd. under the name "Starburst."
[0132] In addition, the dispersing machine used in the present invention is preferably a so-called high-pressure homogenizer capable of applying a pressure in the range of 50 to 245 MPa when spraying the second raw material composition, in order to simultaneously reduce the number of coarse particles in the pigment composition and improve the production efficiency of the pigment composition. The pressure is more preferably 80 to 200 MPa, further preferably 100 to 200 MPa, and particularly preferably 130 to 200 MPa. When the pigment component contains carbon black, a pigment composition can be obtained that is inkjet-ejectable at low pressure and has excellent storage stability, and it is easy to achieve a long life of the device and an improvement in the production volume per unit time.
[0133] The second raw material composition may contain solids such as pigment components and resin components, a liquid medium, and other additives. The pigment composition may contain the same type of components as the raw material composition. The solids concentration of the raw material composition is preferably in the range of 1 to 60 mass%, more preferably in the range of 10 to 50 mass%, and particularly preferably in the range of 15 to 40 mass%, based on the total amount of the raw material composition.
[0134] The pigment composition obtained by the above-mentioned method can be used as ink by diluting it to a desired concentration with the above-mentioned liquid medium and / or adding additives such as a resin component (binder such as acrylic resin or polyurethane resin), a drying inhibitor, a penetrant, a surfactant, a preservative, a viscosity adjuster, a pH adjuster, a chelating agent, a plasticizer, an antioxidant, an ultraviolet absorber, etc. After obtaining the ink, it may be subjected to a centrifugation treatment or a filtration treatment.
[0135] Examples of the ink include paints for automobiles or building materials, and printing inks such as inkjet printing ink, offset ink, gravure ink, flexo ink, and silk screen ink. When the ink is used as an inkjet printing ink, the content of the pigment component in the ink is preferably 1 to 10 mass % based on the total amount of the ink.
[0136] Examples of the drying inhibitor include glycerin, ethylene glycol, diethylene glycol, triethylene glycol, triethylene glycol mono-n-butyl ether, polyethylene glycol with a molecular weight of 2000 or less, propylene glycol, dipropylene glycol, tripropylene glycol, 1,3-propylene glycol, isopropylene glycol, isobutylene glycol, 1,4-butanediol, 1,3-butanediol, 1,5-pentanediol, 1,6-hexanediol, mesoerythritol, and pentaerythritol. The drying inhibitor can be the same compound as the water-soluble organic solvent used in the raw material composition. Therefore, if a water-soluble organic solvent is already used in the raw material composition, it can also function as a drying inhibitor.
[0137] The penetrant can be used for the purpose of improving the permeability into the recording medium or adjusting the dot diameter on the recording medium. Examples of the penetrant include lower alcohols such as ethanol and isopropyl alcohol; glycol monoethers of alkyl alcohols such as ethylene glycol hexyl ether, diethylene glycol butyl ether, and propylene glycol propyl ether.
[0138] The surfactant can be used to adjust the ink properties such as surface tension. The surfactant is not particularly limited, and examples thereof include various anionic surfactants, nonionic surfactants, cationic surfactants, amphoteric surfactants, etc., and at least one selected from the group consisting of anionic surfactants and nonionic surfactants is preferred. The surfactant can be used alone or in combination of two or more types.
[0139] Examples of the anionic surfactant include alkylbenzenesulfonates, alkylphenylsulfonates, alkylnaphthalenesulfonates, higher fatty acid salts, sulfates of higher fatty acid esters, sulfonates of higher fatty acid esters, sulfates and sulfonates of higher alcohol ethers, higher alkyl sulfosuccinates, polyoxyethylene alkyl ether carboxylates, polyoxyethylene alkyl ether sulfates, alkyl phosphates, polyoxyethylene alkyl ether phosphates, etc. Specific examples of these include dodecylbenzenesulfonates, isopropylnaphthalenesulfonates, monobutylphenylphenol monosulfonates, monobutylbiphenylsulfonates, dibutylphenylphenol disulfonates, etc.
[0140] Examples of nonionic surfactants include polyoxyethylene alkyl ethers, polyoxyethylene alkylphenyl ethers, polyoxyethylene fatty acid esters, sorbitan fatty acid esters, polyoxyethylene sorbitan fatty acid esters, polyoxyethylene sorbitol fatty acid esters, glycerin fatty acid esters, polyoxyethylene glycerin fatty acid esters, polyglycerin fatty acid esters, sucrose fatty acid esters, polyoxyethylene alkylamines, polyoxyethylene fatty acid amides, fatty acid alkylol amides, alkyl alkanol amides, acetylene glycol, oxyethylene adducts of acetylene glycol, polyethylene glycol polypropylene glycol block copolymers, etc. Among these, at least one selected from the group consisting of polyoxyethylene nonylphenyl ethers, polyoxyethylene octylphenyl ethers, polyoxyethylene dodecylphenyl ethers, polyoxyethylene alkyl ethers, polyoxyethylene fatty acid esters, sorbitan fatty acid esters, polyoxyethylene sorbitan fatty acid esters, fatty acid alkylol amides, acetylene glycol, oxyethylene adducts of acetylene glycol, and polyethylene glycol polypropylene glycol block copolymers is preferred.
[0141] Other surfactants that can be used include silicone surfactants such as polysiloxane oxyethylene adducts; fluorine-based surfactants such as perfluoroalkyl carboxylates, perfluoroalkyl sulfonates, and oxyethylene perfluoroalkyl ethers; and biosurfactants such as spiculisporic acid, rhamnolipid, and lysolecithin. EXAMPLES
[0142] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. <Preparation of styrene-acrylic acid copolymer> (Styrene-acrylic acid copolymer A) After 100g of methyl ethyl ketone was charged into a reaction vessel equipped with a stirring device, a dropping device, and a reflux device, the inside of the reaction vessel was replaced with nitrogen while stirring. Next, the reaction vessel was heated, and a mixture of 77g of styrene, 10g of acrylic acid, 13g of methacrylic acid, and 8g of a polymerization catalyst (manufactured by Wako Pure Chemical Industries, Ltd., product name: V-59) was dropped from the dropping device over 2 hours while the reaction vessel was heated and the methyl ethyl ketone was refluxed. The temperature of the reaction vessel was kept at 80°C during the dropping. After the dropping was completed, the reaction was continued for another 25 hours at the same temperature. After the reaction was completed, the reaction vessel was allowed to cool, and then methyl ethyl ketone was added to obtain a solution with a solid content concentration of 50% by mass. Furthermore, this solution was dried and then pulverized into powder of 1 mm or less to obtain a styrene-acrylic acid copolymer A. The acid value of the styrene-acrylic acid copolymer A was 150 mgKOH / g, and the weight average molecular weight was 8800.
[0143] The weight average molecular weight is a value measured by GPC (gel permeation chromatography) and converted into the molecular weight of polystyrene used as a standard substance. The measurement was performed using the following apparatus and conditions.
[0144] Liquid delivery pump: LC-9A (Shimadzu Corporation) System controller: SLC-6B (Shimadzu Corporation) Auto injector: S1L-6B (Shimadzu Corporation) Detector: RID-6A (Shimadzu Corporation) Data processing software: Sic480II Data Station (System Instruments) Column: GL-R400 (guard column) + GL-R440 + GL-R450 + GL-R400M (Hitachi Chemical Co., Ltd.) Elution solvent: THF (tetrahydrofuran) Elution flow rate: 2mL / min Column temperature: 35℃
[0145] <Preparation of Pigment Composition> (Black pigment composition) [Example A1] First, 110.0 g of triethylene glycol (ΔD 16.5, ΔP 12.5, ΔH 18.5), 232.2 g of ion-exchanged water, and 17.8 g of 34% by mass potassium hydroxide aqueous solution were mixed to prepare a mixture. 100.0 g of black pigment (manufactured by Mitsubishi Chemical Corporation, carbon black, #960, dry pigment) and 40 g of the above-mentioned styrene-acrylic acid copolymer A were mixed to prepare a first raw material composition (pigment concentration: 20% by mass, solid concentration: 28% by mass).
[0146] Next, in the step B, the first raw material composition was charged into a rotor-stator type processor (manufactured by IKA Corporation, equipment name: magic LAB, 3-stage type, processing section (rotor and stator) of 2P / 4M / 6F from the top in the vertical direction, in-line type). Next, the first raw material composition was heated to 60° C. and then stirred at a peripheral speed of 34 m / s (shear rate: 170,000 s -1 ), and five passes were performed at a rotation speed of 20,000 rpm to prepare a second raw material composition (slurry).
[0147] Next, in step C, the second raw material composition was sprayed and collided at a pressure of 140 MPa using a high-pressure homogenizer (manufactured by Sugino Machine Co., Ltd., equipment name: Starburst, oblique collision chamber) in one pass to obtain a pigment composition.
[0148] [Example A2] A pigment composition was obtained in the same manner as in Example A1, except that dipropylene glycol (ΔD 17.0, ΔP 8.4, ΔH 15.9) was used instead of triethylene glycol.
[0149] [Example A3] A pigment composition was obtained in the same manner as in Example A1, except that 1,5-pentanediol (δD 17.0, δP 8.9, δH 19.8) was used instead of triethylene glycol.
[0150] [Example A4] A pigment composition was obtained in the same manner as in Example A1, except that propylene glycol (ΔD 16.8, ΔP 10.4, ΔH 21.3) was used instead of triethylene glycol.
[0151] [Comparative Example A1] A pigment composition was obtained in the same manner as in Example A1, except that triethylene glycol was replaced with methyl ethyl ketone (ΔD 16.0, ΔP 9.0, ΔH 5.1).
[0152] [Comparative example A2] A pigment composition was obtained in the same manner as in Example A1, except that ethylene glycol (ΔD 16.8, ΔP 15.8, ΔH 27.7) was used instead of triethylene glycol.
[0153] [Comparative example A3] A pigment composition was obtained in the same manner as in Example A1, except that triethylene glycol was replaced with N-methyl-2-pyrrolidone (ΔD 18.0, ΔP 12.3, ΔH 7.2).
[0154] <Evaluation of Pigment Composition> The number of coarse particles, particle size, viscosity, storage stability, and print density of the pigment compositions obtained in the Examples and Comparative Examples and the raw material compositions in the process of production were measured by the following methods. The results are shown in Tables 1 and 2.
[0155] (Number of coarse particles) The number of particles with a diameter of 1.0 μm or more and the number of particles with a diameter of 0.5 μm or more were measured using a particle size distribution meter (Particle Sizing Systems, Accusizer 780 APS, number counting method) in the following manner. The pigment composition was diluted with ion-exchanged water so that the sensitivity was in the range of 1000 to 4000 particles / mL. Next, the number of particles with a diameter of 1.0 μm or more and the number of particles with a diameter of 0.5 μm or more contained in the diluted pigment composition were measured three times using the particle size distribution meter. Next, the average value of the values obtained by multiplying the measured particle number by the dilution concentration was calculated as the number of coarse particles.
[0156] (Particle size) The pigment composition was placed in a cell of about 4 mL. The particle size was measured by detecting the scattered light of a laser beam using a Nanotrac particle size distribution analyzer "UPA150" manufactured by Microtrac Bell Co., Ltd., in an environment of 25°C. The particle sizes measured were the volume average particle size (Mv), number average particle size (Mn), D50, D90, and D95.
[0157] (viscosity) 1.0 mL of the pigment composition was placed in a sample cup, and the viscosity of the pigment composition was measured in an environment of 25° C. using a TV-20 viscometer manufactured by Toki Sangyo Co., Ltd.
[0158] (Storage stability) Immediately after production, the volume average particle size (Mv), viscosity, and number of coarse particles having a diameter of 0.5 μm of the pigment composition were measured by the methods described above.
[0159] Next, the pigment composition was sealed in a polypropylene container and then stored for 4 weeks at 60° C. After the storage, the volume average particle size (Mv), viscosity, and number of coarse particles having a diameter of 0.5 μm of the pigment composition were measured by the above-mentioned methods.
[0160] The rate of change in the volume average particle diameter (Mv), viscosity, and number of coarse particles having a diameter of 0.5 μm of the pigment composition after the storage relative to the volume average particle diameter (Mv), viscosity, and number of coarse particles having a diameter of 0.5 μm of the pigment composition immediately after production was calculated.
[0161] Those whose rate of change was within 10% were evaluated as having excellent storage stability, those whose rate of change was more than 10% but not more than 15% were evaluated as having good storage stability, and those whose rate of change was more than 15% were evaluated as having insufficient storage stability.
[0162] [Table 1] [Explanation of symbols]
[0163] 10...central shaft, 20...rotor, 22...blade portion, 22a...opening, 24...connection portion, 30...stator, 32...wall portion, 32a...opening, 34...connection portion, 100...rotor-stator type processing machine, F1, F2...flow path.
Claims
1. A method for producing a pigment composition in which the pigment component is dispersed in a liquid medium by the resin component, the method comprising the steps of: a step A of producing a first raw material composition by mixing a resin component, a pigment component, a basic compound, and a liquid medium; a step B of producing a second raw material composition by processing the first raw material composition with a rotor-stator type processing machine; and a step C of processing the second raw material composition with a dispersing machine having a configuration in which the second raw material compositions collide with each other, the method comprising the steps of: 1 ) and polar terms (δP 1 ) and the hydrogen bond term (δH 1 13. A method for producing a pigment composition for an ink-jet printing ink, comprising the steps of:
2. 2. The method for producing a pigment composition according to claim 1, wherein the liquid medium (a) is triethylene glycol, 2-pyrrolidone, 1-(2-hydroxyethyl)-2-pyrrolidone, dipropylene glycol, propylene glycol, 1,5-pentanediol or glycerin.
3. 3. The method for producing a pigment composition according to claim 1, wherein a mass ratio of the liquid medium (a) to a total amount of the liquid medium contained in the pigment composition is in the range of 15 to 80 mass %.
4. The method for producing a pigment composition according to any one of claims 1 to 3, wherein the disperser having a configuration for colliding the second raw material compositions with each other is an oblique collision type disperser.
5. 5. The method for producing a pigment composition according to claim 4, wherein the oblique collision type disperser is configured to collide the second raw material compositions with each other at a pressure in the range of 50 to 245 MPa.
6. 6. The method for producing a pigment composition according to claim 5, wherein the number of times (number of passes) in which the second raw material composition is repeatedly fed into a disperser having a configuration in which the second raw material compositions are collided obliquely with each other is in the range of 1 to 8.
7. A method for producing a pigment composition described in claim 1 or 2, wherein the acid value of the resin component is in the range of 60 to 300 mg KOH / g, and the weight average molecular weight of the resin component is in the range of 5,000 to 25,000.
Citation Information
Patent Citations
Production of water-based pigment recording liquid
JP1999131004A
Method of producing aqueous pigment dispersion
JP2001262038A
Manufacturing method of aqueous pigment dispersion
JP2018002835A