Dispersion and method for producing laminate
A dispersion of tetrafluoroethylene polymer powder in a specified hydrocarbon or silicone oil medium addresses liquid physical property issues, providing stability and electrical performance in laminates.
Patent Information
- Application Number
- JP2020178938
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-10-26
- Publication Date
- 2024-10-02
- Estimated Expiration
- 2040-10-26
AI Technical Summary
Existing dispersions of tetrafluoroethylene polymers suffer from poor liquid physical properties, including thickening, foaming, and agglomeration during long-term storage, and poor handling properties such as wetting and spreading, especially when using polar or non-polar dispersion media.
A dispersion of tetrafluoroethylene polymer powder using a specified hydrocarbon or silicone oil as a dispersion medium, with specific properties such as fluorine content, viscosity, and particle size, which enhances dispersibility and stability, resulting in a balanced liquid physical state.
The dispersion achieves high stability, handling properties, and long-term storage stability, with laminates exhibiting excellent electrical properties.
Smart Images

Figure 0007559497000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a dispersion containing a powder of a specific tetrafluoroethylene-based polymer and a method for producing a laminate. [Background technology]
[0002] Tetrafluoroethylene-based polymers have excellent physical properties such as electrical insulation, water and oil repellency, chemical resistance, and heat resistance. A dispersion in which the powder is dispersed in a dispersion medium is useful as a material for forming resists, adhesives, electrical insulating layers, lubricants, inks, paints, etc. However, tetrafluoroethylene-based polymers have low surface energy, and the powder is prone to aggregation. For this reason, it is difficult to obtain a dispersion with balanced liquid properties. Patent Document 1 discloses a non-aqueous dispersion containing a specific additive with a view to improving the dispersibility of the dispersion. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] International Publication No. 2016 / 159102 Summary of the Invention [Problem to be solved by the invention]
[0004] However, the liquid properties other than dispersibility of the dispersion liquid described in Patent Document 1 are still insufficient. The present inventors have found that while a dispersion liquid using a polar dispersion medium is easy to increase the powder content, it is prone to thickening, foaming, and the powder tends to aggregate during long-term storage. In addition, the present inventors have found that a dispersion liquid using a non-polar dispersion medium is easy to suppress these tendencies, but is difficult to increase the powder content, and tends to have poor handling properties such as wettability and spreadability during coating.
[0005] As a result of intensive research, the present inventors have found that a dispersion in which a tetrafluoroethylene-based polymer powder is dispersed in a specific hydrocarbon or silicone oil as a dispersion medium has a high balance of various liquid physical properties, and that a laminate formed from such a dispersion exhibits the physical properties of the tetrafluoroethylene-based polymer to a high degree, and is particularly excellent in electrical properties. An object of the present invention is to provide a dispersion containing a powder of a specific tetrafluoroethylene-based polymer and a liquid compound which is a specific hydrocarbon or silicone oil, and a laminate formed therefrom. [Means for solving the problem]
[0006] The present invention has the following aspects. [1] A powder of a tetrafluoroethylene polymer having a fluorine content of 70% by mass or more and at least one oil selected from the group consisting of isoalkane, terpene, α-olefin, dimethyl silicone oil, and methylphenyl silicone oil, having a kinetic viscosity of 1000 mm 2 ·s -1 and a liquid compound having a boiling point of 100 to 300°C, in which the powder is dispersed. [2] The dispersion of [1], wherein the tetrafluoroethylene-based polymer has a carbonyl group-containing group. [3] The dispersion liquid according to [1] or [2], wherein the tetrafluoroethylene-based polymer is a polymer having 10 to 5,000 carbonyl-containing groups per 1×10 6 carbon atoms in the main chain. [4] The dispersion liquid according to any one of [1] to [3], wherein the powder has an average particle size of 20 μm or less. [5] The specific surface area of the powder is 25m 2 / g or less. [6] The dispersion liquid according to any one of [1] to [5], wherein the liquid compound is an isoalkane or a dimethylsilicone oil. [7] The dispersion liquid according to any one of [1] to [6], wherein the liquid compound is isododecane, isohexadecane, linear dimethyl silicone oil, or cyclic dimethyl silicone oil. [8] The dispersion liquid according to any one of [1] to [7], wherein the ratio of the content of the liquid compound to the content of the tetrafluoroethylene-based polymer powder is 1 or more. [9] The dispersion according to any one of [1] to [8], wherein the content of the tetrafluoroethylene-based polymer powder is 20 mass % or more.
[10] The dispersion according to any one of [1] to [9], further comprising an inorganic filler or an aromatic polymer.
[11] The dispersion according to any one of [1] to
[10] , further comprising a nonionic surfactant.
[12] Any of the dispersions [1] to
[10] having a viscosity of 50 to 10,000 mPa s.
[13] The dispersion liquid according to any one of [1] to
[12] , wherein a component dispersion layer rate is 60% or more.
[14] The dispersion according to any one of [1] to
[13] , having a foam volume ratio of less than 10%.
[15] A method for producing a laminate, comprising contacting a dispersion according to any one of the items [1] to
[14] with a surface of a substrate and heating the dispersion to form a polymer layer, thereby obtaining a laminate having the substrate and the polymer layer. Effect of the Invention
[0007] According to the present invention, a dispersion containing a powder of a specific tetrafluoroethylene-based polymer and a specific liquid compound and having well-balanced liquid properties (dispersion stability, handling properties, long-term storage properties, etc.) can be obtained. Also, a laminate exhibiting the properties of the tetrafluoroethylene-based polymer to a high degree can be obtained. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] The following terms have the following meanings. The "glass transition point (Tg) of a polymer" is a value measured by analyzing a polymer using a dynamic mechanical analysis (DMA) method. The "melting temperature (melting point) of a polymer" is the temperature corresponding to the maximum value of the melting peak measured by differential scanning calorimetry (DSC). "D50" is the average particle size of a powder or filler, and is the cumulative 50% diameter based on the volume of the target object determined by the laser diffraction / scattering method. In other words, the particle size distribution of the target object is measured by the laser diffraction / scattering method, and a cumulative curve is calculated with the total volume of the target group as 100%, and D50 is the particle size at the point on the cumulative curve where the cumulative volume is 50%. "D90" is the cumulative volume particle size of a powder or filler, and is the volume-based cumulative 90% diameter of a target object, which is calculated in the same manner as "D50". The "specific surface area" is a value calculated by measuring particles using a gas adsorption (constant volume method) BET multipoint method, and is determined using a NOVA4200e (manufactured by Quantachrome Instruments). The "viscosity" is a value measured for the dispersion using a Brookfield viscometer at 25° C. and a rotation speed of 30 rpm. The measurement is repeated three times, and the average value of the three measured values is used. The "thixotropy ratio" is a value calculated by dividing the viscosity η1 measured for the dispersion at 25°C and a rotation speed of 30 rpm using a Brookfield viscometer by the viscosity η2 measured at a rotation speed of 60 rpm. Each viscosity measurement is repeated three times, and the average value of the three measurements is used. "Kinematic viscosity" is a value measured for a liquid compound at 25°C using an Ubbelohde viscometer. The measurement is repeated three times, and the average value of the three measured values is used. The term "unit based on a monomer" refers to an atomic group based on the monomer formed by polymerization of the monomer. The unit may be a unit formed directly by a polymerization reaction, or may be a unit in which a part of the unit is converted into a different structure by treating the polymer. Hereinafter, the unit based on monomer a is also referred to simply as "monomer a unit." The "component dispersion layer ratio" is a value calculated by the following formula from the height of the entire liquid composition in the screw tube and the height of the dispersion layer before and after leaving the liquid composition in the screw tube when 18 mL of the liquid composition is placed in a screw tube with an internal volume of 30 mL and left to stand at 25°C for 14 days. If no component dispersion layer is observed after leaving the liquid composition to stand and there is no change in the state, the component dispersion layer ratio is considered to be 100%, assuming that there is no change in the height of the entire liquid composition. The higher the component dispersion layer ratio, the more excellent the dispersion stability. Component dispersion layer rate (%) = (height of dispersion layer) / (height of entire liquid composition) × 100 The "foam volume ratio" is the volume of the dispersion at 1013.25 hPa and 20°C (V N ) and the combined volume of the bubbles when it is decompressed to 0.003 MPa (V V ) and the value is calculated using the following formula: Foam volume ratio [%] = 100 × (V V -V N ) / V N It is.
[0009] The dispersion of the present invention (hereinafter also referred to as "the present dispersion") is a powder (hereinafter also referred to as "F powder") of a tetrafluoroethylene-based polymer (hereinafter also referred to as "F polymer") having a fluorine content of 70 mass% or more, and at least one selected from the group consisting of isoalkane, terpene, α-olefin, dimethyl silicone oil, and methylphenyl silicone oil having a kinetic viscosity of 1000 mm 2 ·s -1 and a liquid compound having a boiling point of 100 to 300° C. In this dispersion, the F powder is dispersed. In other words, this dispersion has a liquid compound with low surface tension and low polarity as a dispersion medium, is less prone to aggregation and thickening, and has a highly balanced liquid property profile including dispersion stability, handling properties, and long-term storage stability, and can also be said to be a dispersion in which F powder is dispersed in the above liquid compound.
[0010] The F polymer in the present invention is a polymer having a fluorine content of 70% by mass or more and containing units based on tetrafluoroethylene (TFE) (TFE units). The fluorine content of the F polymer is preferably 74% by mass or more. The upper limit of the fluorine atom content is preferably 76% by mass. Such an F polymer with a high fluorine content has excellent physical properties such as electrical properties and heat resistance, while having low surface tension and extremely low affinity with other components. According to the present invention, a dispersion of such an F polymer having excellent liquid physical properties can be obtained.
[0011] The F polymer may be either heat-fusible or non-heat-fusible, and is preferably a heat-fusible polymer. The melting temperature of the heat-fusible F polymer is preferably 200° C. or higher, more preferably 260° C. or higher. The melting temperature of the F polymer is preferably 325° C. or lower, more preferably 320° C. or lower. In this case, the present dispersion is likely to have excellent liquid physical properties, and it is easy to form a dense molded product from the present dispersion. The glass transition point of the F polymer is preferably 50° C. or higher, more preferably 75° C. or higher. The glass transition point of the F polymer is preferably 150° C. or lower, more preferably 125° C. or lower.
[0012] F polymer includes polytetrafluoroethylene (PTFE), the polymer that comprises TFE unit and the unit based on ethylene, the polymer that comprises TFE unit and the unit based on propylene, the polymer that comprises TFE unit and the unit based on perfluoro(alkyl vinyl ether) (PAVE) (PAVE unit) (PFA), the polymer that comprises TFE unit and the unit based on hexafluoropropylene (FEP), the polymer that comprises TFE unit and the unit based on fluoroalkylethylene, the polymer that comprises TFE unit and the unit based on chlorotrifluoroethylene, and PFA or FEP is preferred, and PFA is more preferred.The above-mentioned polymer may further comprise the unit based on other comonomers. As the PAVE, CF2=CFOCF3, CF2=CFOCF2CF3 or CF2=CFOCF2CF2CF3 (PPVE) is preferred, with PPVE being more preferred.
[0013] The PTFE may be a low-molecular-weight PTFE having a number-average molecular weight of 10,000 to 200,000. The number-average molecular weight of PTFE is a value calculated based on the following formula (1). Mn = 2.1 × 10 10 ×ΔHc -5.16 ... (1) In formula (1), Mn represents the number average molecular weight of PTFE, and ΔHc represents the heat of crystallization (cal / g) of PTFE measured by differential scanning calorimetry. PTFE may contain a small amount of units other than TFE units.
[0014] The F polymer preferably has a carbonyl group-containing group or a hydroxyl group-containing group, more preferably a carbonyl group-containing group. Such an F polymer powder suppresses electrostatic repulsion between powder particles, and is easily affected by the stabilizing effect of the permeation action of a liquid compound in a highly fluid state, which makes it easier to further improve the liquid properties of the dispersion. The carbonyl group-containing group or the hydroxyl group-containing group may be contained in a monomer unit in the F polymer, or may be contained in a terminal group of the main chain of the polymer. The latter embodiment includes an F polymer having the polar group as a terminal group derived from a polymerization initiator, a chain transfer agent, etc., and an F polymer that has been corona-treated, plasma-treated, ionizing-ray-treated, or radiation-treated.
[0015] The hydroxyl-containing group is preferably a group containing an alcoholic hydroxyl group, more preferably -CF2CH2OH or -C(CF3)2OH. The carbonyl group-containing group is a group containing a carbonyl group (>C(O)), and is preferably a carboxyl group, an alkoxycarbonyl group, an amide group, an isocyanate group, a carbamate group (-OC(O)NH2), an acid anhydride residue (-C(O)OC(O)-), an imide residue (-C(O)NHC(O)- etc.) or a carbonate group (-OC(O)O-), more preferably an acid anhydride residue. The number of carbonyl-containing groups in the F polymer is 1 × 10 6The number per particle is preferably 10 to 5000, more preferably 100 to 3000, and even more preferably 50 to 1500. In this case, the above-mentioned mechanism of action is promoted, and the liquid properties of the present dispersion are likely to be further improved.
[0016] The F polymer is preferably a polymer containing PAVE units, containing 1.5 to 5 mol % of PAVE units relative to all units, and having a melting temperature of 280 to 320°C, and more preferably a polymer containing 1.5 to 5 mol % of PAVE units, having a carbonyl group-containing group or a hydroxyl group, and having a melting temperature of 280 to 320°C. A preferred embodiment of the F polymer is a polymer containing TFE units, PAVE units, and a monomer having a carbonyl group-containing group or a hydroxyl group. The polymer preferably contains 90 to 98 mol% of TFE units, 1.5 to 9.97 mol% of PAVE units, and 0.01 to 3 mol% of units based on the above monomers, based on the total units. The monomer is preferably itaconic anhydride, citraconic anhydride, or 5-norbornene-2,3-dicarboxylic anhydride (also known as himic anhydride; hereinafter also referred to as "NAH"). Specific examples of such polymers include those described in WO 2018 / 16644.
[0017] The F powder in this method is a powder containing an F polymer, and may be a powder consisting of only an F polymer, or may be a powder containing an F polymer and a resin or an inorganic filler different from the F polymer. Note that the F powder (particularly the former F powder) may contain components used in the production of the F polymer (surfactants, residues of polymerization initiators, etc. used in polymerization). The content of the F polymer in the F powder is preferably 60% by mass or more, more preferably 80% by mass or more. The upper limit of the content of the F polymer is 100% by mass.
[0018] Examples of resins different from the F polymer include aromatic polyesters, polyamideimides, polyimides, polyphenylene ethers, polyphenylene oxides, and maleimides. Examples of inorganic substances include silicon oxide (silica), metal oxides (beryllium oxide, cerium oxide, alumina, soda alumina, magnesium oxide, zinc oxide, titanium oxide, etc.), boron nitride, and magnesium metasilicate (steatite). The F powder containing a resin or inorganic substance different from the F polymer preferably has a core-shell structure having an F polymer as a core and the above-mentioned resin or inorganic substance as a shell, or has a core-shell structure having an F polymer as a shell and the above-mentioned resin or inorganic substance as a core. Such an F powder is obtained, for example, by bonding (by collision, aggregation, etc.) a powder of the F polymer and a powder of the above-mentioned resin or inorganic substance.
[0019] The D50 of the F powder is preferably 20 μm or less, more preferably 10 μm or less, even more preferably 6 μm or less, and particularly preferably 3 μm or less. The D50 of the F powder is preferably 0.1 μm or more, more preferably 0.5 μm or more. The D90 of the F powder is preferably 100 μm or less, more preferably 10 μm or less, and even more preferably 8 μm or less. The specific surface area of F powder is 25m 2 / g or less is preferable, and 1 to 8m 2 / g is more preferable, and 1 to 3m 2 / g is more preferred. If the F powder has D50, D90 and specific surface area each within the above range, a dispersion having superior liquid properties can be obtained.
[0020] The liquid compound in the present invention is at least one compound selected from the group consisting of isoalkane, terpene, α-olefin, dimethyl silicone oil, and methylphenyl silicone oil, and has a kinetic viscosity of 1000 mm 2 ·s -1 or less, and has a boiling point of 100 to 300° C. Note that the liquid compound means a compound that is liquid at 1013.25 hPa and 25° C.
[0021] The kinetic viscosity of a liquid compound is 0mm 2 ·s -1 More than 0.1mm is preferable.2 ·s -1 More preferably, 1 mm or more 2 ·s -1 More preferably, the kinematic viscosity is 100 mm 2 ·s -1 Less than 10mm is preferable 2 ·s -1 The following is more preferred: The boiling point of the liquid compound is preferably 120° C. or higher, more preferably 150° C. or higher. The boiling point is preferably 250° C. or lower, more preferably 220° C. or lower. When the kinetic viscosity and boiling point of the liquid compound are each within the above ranges, the F powder is sufficiently wetted and spread easily due to the penetration action of the liquid compound in a highly fluid state, the liquid properties of the dispersion are further improved, and it is easy to obtain a dense molded product with excellent smoothness from the dispersion.
[0022] The liquid compound is preferably an isoalkane or dimethyl silicone oil. Isoalkanes are alkanes that have a branched chain on the main chain, and have a high level of balance between their affinity for the F polymer and their penetrating effect on the F powder due to their fluidity, making it easier to further improve the liquid properties of the dispersion. Dimethyl silicone oil or methylphenyl silicone oil (particularly dimethyl silicone oil) improves the dispersibility of the F powder due to its own surface activity, and tends to further improve the liquid properties of the present dispersion.
[0023] The isoalkane is preferably isodecane, isododecane, isotetradecane or isohexadecane, since these isoalkanes tend to enhance the above-mentioned mechanism of action. As the terpene, a monoterpene, a diterpene or a triterpene is preferable, and limonene or squalene is more preferable. The α-olefin is preferably 1-decene, 1-dodecene, 1-tetradecene or 1-hexadecene.
[0024] As the dimethyl silicone oil, linear dimethyl silicone oil or cyclic dimethyl silicone oil is preferable, since these silicone oils tend to enhance the above-mentioned mechanism of action. Examples of linear dimethyl silicone oils include hexamethyldisiloxane, octamethyltrisiloxane, decamethyltetrasiloxane, and octamethylcyclotetrasiloxane. Examples of cyclic dimethyl silicone oils include decamethylcyclopentasiloxane, hexamethylcyclotrisiloxane, octamethylcyclotetrasiloxane, and dodecamethylcyclohexasiloxane. Methylphenyl silicone oils include diphenyl dimethicone and diphenylsiloxyphenyl trimethicone.
[0025] The content of F powder in the present dispersion is preferably 20% by mass or more, more preferably 25% by mass or more, and even more preferably 30% by mass or more. The content of F powder is preferably 60% by mass or less, and more preferably 50% by mass or less. Even if the content of F powder in the dispersion is high, the present dispersion has excellent liquid physical properties due to the above-mentioned action mechanism, and can be easily formed into any molded product (such as a thick polymer layer) from it. The content of the liquid compound in the present dispersion is preferably 30% by mass or more, more preferably 50% by mass or more, and is preferably 80% by mass or less, more preferably 60% by mass or less. The ratio of the content of the liquid compound to the content of the F powder in the present dispersion is preferably 1 or more, more preferably 1.5 or more. The content ratio is preferably 4 or less, more preferably 3 or less. When the content of the liquid compound and the above ratio are each within the above range, the above-mentioned mechanism of action is likely to be enhanced, and the liquid properties of the present dispersion are likely to be further improved.
[0026] The viscosity of the present dispersion is preferably 50 mPa·s or more, more preferably 100 mPa·s or more. The viscosity of the present dispersion is preferably 10,000 mPa·s or less, more preferably 5,000 mPa·s or less, and even more preferably 1,000 mPa·s or less. In this case, the present dispersion has excellent coatability, and therefore it is easy to form a molded product such as a polymer layer having a desired thickness. The thixotropy ratio of the present dispersion is preferably 1.0 or more. The thixotropy ratio of the present dispersion is preferably 3.0 or less, more preferably 2.0 or less. In this case, the present dispersion is not only excellent in coatability but also in homogeneity, so that it is easy to form a molded product such as a dense polymer layer.
[0027] The component dispersion layer ratio of the present dispersion is preferably 60% or more, more preferably 70% or more. The upper limit of the component dispersion layer ratio is 100%. Since the present dispersion has excellent dispersion stability, it is easy to adjust the component dispersion layer ratio to such a level. The foam volume ratio of the present dispersion is preferably 10% or less, more preferably 5% or less. The foam volume ratio is preferably 0% or more. In this case, the molded product formed from the present dispersion is likely to be dense, and the components are likely to be uniformly distributed in the molded product. The foam volume ratio may be adjusted by degassing the present dispersion. Due to the above-mentioned mechanism of action, according to the present invention, a dispersion liquid having a viscosity, a thixotropic ratio, a component-dispersed layer ratio, and a foam volume ratio each falling within the above-mentioned ranges can be easily obtained.
[0028] The present dispersion preferably further contains an inorganic filler, in which case the liquid properties of the present dispersion are more likely to be improved, and the physical properties of the inorganic filler are more likely to be well exhibited in a molded product formed from the present dispersion. The inorganic filler is preferably an inorganic filler containing an oxide, a nitride, a metal element, an alloy, and carbon, more preferably an inorganic filler containing silicon oxide (silica), a metal oxide (beryllium oxide, cerium oxide, alumina, soda alumina, magnesium oxide, zinc oxide, titanium oxide, etc.), boron nitride, and magnesium metasilicate (steatite), and further preferably an inorganic filler containing an inorganic oxide containing at least one element selected from aluminum, magnesium, silicon, titanium, and zinc, particularly preferably an inorganic filler containing silica and boron nitride, and most preferably an inorganic filler containing silica. The inorganic filler may also be ceramics. One type of inorganic substance may be used, or two or more types may be mixed and used. When two or more types of inorganic fillers are mixed, two types of inorganic fillers containing silica may be used, or an inorganic filler containing silica and a metal oxide may be used.
[0029] The inorganic filler is preferably particulate, and the shape of the inorganic filler may be any of granular, needle-like (fibrous), and plate-like. Specific shapes of the inorganic filler include spherical, scaly, lamellar, flat, leaf-like, apricot kernel, columnar, cockscomb, equiaxial, leaf-like, mica-like, block-like, flat, wedge-like, rosette-like, mesh-like, and prismatic. The inorganic filler may be hollow, and may include hollow inorganic fillers and non-hollow inorganic fillers. The shape of the inorganic filler is preferably spherical or scaly. The inorganic filler preferably has a D50 of 20 μm or less, more preferably 10 μm or less, and even more preferably 5 μm or less.The inorganic filler preferably has a D50 of 0.01 μm or more, and more preferably 0.1 μm or more.
[0030] Specific examples of suitable inorganic fillers include silica fillers (such as the "Admafine (registered trademark)" series manufactured by Admatechs Co., Ltd.), zinc oxide surface-treated with an ester such as propylene glycol dicaprylate (such as the "FINEX (registered trademark)" series manufactured by Sakai Chemical Industry Co., Ltd.), spherical fused silica (such as the "SFP (registered trademark)" series manufactured by Denka Co., Ltd.), titanium oxide coated with polyhydric alcohol and inorganic substances (such as the "Tipaque (registered trademark)" series manufactured by Ishihara Sangyo Kaisha, Ltd.), and rutile-type titanium oxide surface-treated with alkylsilane (such as the "Tipaque (registered trademark)" series manufactured by Teika Co., Ltd.). JMT (registered trademark) series, etc.), hollow silica filler (Taiheiyo Cement Corporation's E-SPHERES series, Nippon Steel Mining Co., Ltd.'s Silinax series, Emerson & Cumming Co., Ltd.'s Ecocosfyer series, etc.), talc filler (Nippon Talc Co., Ltd.'s SG series, etc.), steatite filler (Nippon Talc Co., Ltd.'s BST series, etc.), boron nitride filler (Showa Denko KK's UHP series, Denka Company, Ltd.'s Denka Boron Nitride series (GP, HGP grades, etc.), etc.).
[0031] The surface of the inorganic filler may be treated with a silane coupling agent, such as 3-aminopropyltriethoxysilane, vinyltrimethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 3-methacryloxypropyltriethoxysilane, or 3-isocyanatepropyltriethoxysilane. When an inorganic filler is contained, the content of the inorganic filler in the present dispersion is preferably 5% by mass or more, more preferably 10% by mass or more, and is preferably 40% by mass or less, more preferably 30% by mass or less.
[0032] The present dispersion preferably further contains an aromatic polymer. The aromatic polymer may be dissolved or dispersed in the present dispersion. In this case, the liquid properties of the present dispersion are more likely to be improved, and the molded product formed from the present dispersion is more likely to have low linear expansion properties and UV absorption properties. The aromatic polymer is preferably an aromatic polyimide, an aromatic maleimide, an aromatic elastomer such as a styrene elastomer, or an aromatic polyamic acid, more preferably an aromatic polyimide, an aromatic maleimide, a polyphenylene ether, an aromatic elastomer such as a styrene elastomer, and even more preferably an aromatic polyimide or an aromatic polyamic acid. The aromatic polyimide may be thermoplastic or thermosetting. Thermoplastic polyimide means a polyimide in which imidization is completed and no further imidization reaction occurs.
[0033] Specific examples of aromatic polyimides include the "Neoplim (registered trademark)" series (manufactured by Mitsubishi Gas Chemical Company, Inc.), the "Spiccellia (registered trademark)" series (manufactured by Somar), the "Q-PILON (registered trademark)" series (manufactured by PI Technical Research Institute), the "WINGO" series (manufactured by Wingo Technology Co., Ltd.), the "Tomide (registered trademark)" series (manufactured by T&K Toka Corporation), the "KPI-MX" series (manufactured by Kawamura Sangyo Co., Ltd.), and the "Upia (registered trademark)-AT" series (manufactured by Ube Industries, Ltd.). Examples of the styrene elastomer include styrene-butadiene copolymer, hydrogenated styrene-butadiene copolymer, hydrogenated styrene-isoprene copolymer, styrene-butadiene-styrene block copolymer, styrene-isoprene-styrene block copolymer, hydrogenated styrene-butadiene-styrene block copolymer, and hydrogenated styrene-isoprene-styrene block copolymer. When an aromatic polymer is contained, the content of the aromatic polymer in the present dispersion is preferably 0.1% by mass or more, more preferably 1% by mass or more, and is preferably 20% by mass or less, more preferably 10% by mass or less.
[0034] The present dispersion preferably does not substantially contain a surfactant. Substantially free of a surfactant means that the concentration of the surfactant in the present dispersion does not exceed 1% by mass. The content of the surfactant in the present dispersion is less than 1% by mass, preferably 0.5% by mass or less, and more preferably 0% by mass. In this case, the present dispersion is likely to have excellent defoaming properties. In addition, the surfactant is unlikely to remain in a molded product formed from the present dispersion, and the molded product is likely to have excellent electrical properties. Due to the above-mentioned mechanism of action, such a dispersion can be easily obtained according to the present invention.
[0035] When the present dispersion contains a surfactant, the surfactant is preferably a nonionic surfactant. The hydrophilic site of the surfactant preferably has an oxyalkylene group or an alcoholic hydroxyl group. The oxyalkylene group may be composed of one type or two or more types. In the latter case, the different types of oxyalkylene groups may be arranged randomly or in a block form. The oxyalkylene group is preferably an oxyethylene group.
[0036] The hydrophobic portion of the surfactant preferably has an acetylene group, a polysiloxane group, a perfluoroalkyl group or a perfluoroalkenyl group, and more preferably has a polysiloxane group. In other words, the surfactant is preferably an acetylene-based surfactant, a silicone-based surfactant, or a fluorine-based surfactant, and more preferably a silicone-based surfactant. In this case, the surfactant interacts well with the F powder and the liquid compound, and the dispersion tends to have excellent dispersion stability.
[0037] In addition to the above-mentioned components, the present dispersion may further contain other components such as a thixotropic agent, a viscosity modifier, an antifoaming agent, a silane coupling agent, a dehydrating agent, a plasticizer, a weathering agent, an antioxidant, a heat stabilizer, a lubricant, an antistatic agent, a whitening agent, a colorant, a conductive agent, a release agent, a surface treatment agent, a flame retardant, and various fillers. The present dispersion can be produced by mixing the F powder with a liquid compound. The present dispersion is preferably produced by mixing the liquid compound with a paste obtained by kneading a liquid composition containing the F powder and the liquid compound.
[0038] The liquid compound used to prepare the liquid composition may be any of the above-mentioned liquid compounds or any liquid compound other than the above-mentioned liquid compounds. The liquid compound other than the liquid compound is preferably an amide, a ketone or an ester, and more preferably N-methyl-2-pyrrolidone, γ-butyrolactone, cyclohexanone or cyclopentanone. The liquid compound in the present dispersion is preferably the same liquid compound as that used in the preparation of the liquid composition, in which case the liquid properties of the present dispersion tend to be superior.
[0039] When the present dispersion contains an inorganic filler, an aromatic polymer, or a surfactant, they may be mixed at any stage in the production of the present dispersion, for example, they may be mixed with the liquid composition before kneading, they may be mixed with the liquid composition during kneading, they may be mixed with the paste after kneading, or they may be mixed with the mixture of the paste and the liquid compound. For the kneading, a Henschel mixer, a pressure kneader, a Banbury mixer, a planetary mixer, a twin-screw extrusion kneader, or a stone mill type kneader can be used. During kneading, it is preferable to knead the liquid composition so that the mass of the liquid composition does not change substantially, and it is preferable to knead in a closed system. It is preferable to knead the liquid composition so that the liquid content of the liquid composition does not evaporate during kneading. As a result, each component is kneaded uniformly, and a paste that is highly defoamed is obtained.
[0040] The paste obtained as described above has a high viscosity and is usually a semi-solid or solid paste. The viscosity of the paste is preferably 800 to 100,000 mPa·s, and more preferably 10,000 to 100,000 mPa·s. The solid content of the paste is preferably 40 to 90% by mass, more preferably 50 to 80% by mass. The solid content of the paste means the total amount of substances forming solid components in a molded product formed from the present dispersion obtained from the paste. For example, when the paste contains an F polymer, an inorganic filler, and an aromatic polymer, the total content of these components in the molded product is the solid content of the paste. Methods for mixing the paste and the liquid compound include a method of mixing the paste and the liquid compound in a kneader having a stirring tank and stirring blades used for kneading after kneading, a method of removing the paste from the kneader used for kneading and mixing the paste and the liquid compound in another kneader, etc. Either a batch type or a continuous type kneader can be used as the kneader.
[0041] This dispersion is brought into contact with the surface of a substrate and heated to form a layer made of the F polymer (hereinafter also referred to as the "F layer"), whereby a laminate having the substrate and the F layer can be produced. In producing the above laminate, it is sufficient that an F layer is formed on at least one surface of the substrate. An F layer may be formed on only one surface of the substrate, or an F layer may be formed on both surfaces of the substrate. The surface of the substrate may be treated with a silane coupling agent or the like. The dispersion is preferably brought into contact with the surface of the substrate by coating. For this application, a coating method such as spraying, roll coating, spin coating, gravure coating, microgravure coating, gravure offset, knife coating, kiss coating, bar coating, die coating, fountain-meyer bar, slot die coating, or the like can be used.
[0042] The F layer is preferably formed by removing the liquid compound by heating, and then baking the F polymer by further heating. The temperature for removing the liquid compound is preferably as low as possible, and is preferably a temperature lower than the boiling point of the liquid compound by 50 to 150° C. From the viewpoint of improving smoothness, it is preferable to blow air in the step of removing the liquid compound. After removing the liquid compound, it is preferable to form an F layer by heating the substrate to a temperature range where the F polymer is baked, and for example, it is preferable to bake the F polymer in the range of 300 to 400° C. In other words, it is preferable that the F layer contains a baked product of the F polymer.
[0043] As described above, the F layer is formed through the steps of coating the dispersion, drying, and baking. Each of these steps may be carried out once or twice or more. For example, the F layer may be formed by repeating the process of applying the above dispersion to the surface of the substrate, removing the liquid compound by heating to form a film twice, and then heating the thickened film to bake the F polymer. From the viewpoint of easily obtaining a thick F layer having excellent smoothness, it is preferable to carry out the steps of coating and drying the present dispersion twice. The thickness of the F layer is preferably 0.1 μm or more. The upper limit of the thickness is 200 μm. Within this range, an F layer with excellent crack resistance can be easily formed.
[0044] The peel strength between the F layer and the base layer is preferably 10 N / cm or more, more preferably 15 N / cm or more. The peel strength is preferably 100 N / cm or less. By using the present dispersion, the present laminate can be easily formed without impairing the physical properties of the F polymer in the F layer. The porosity of the F layer is preferably 5% or less, more preferably 4% or less. The porosity is preferably 0.01% or more, more preferably 0.1% or more. The porosity is determined by determining the void area of the F layer by image processing from an SEM photograph of the cross section of the molded product observed using a scanning electron microscope (SEM), and is the percentage (%) obtained by dividing the area occupied by the void area by the area of the F layer. The area occupied by the void area is determined by approximating the void area as a circle.
[0045] Examples of the material for the substrate include metal substrates (metal foils of copper, nickel, aluminum, titanium, alloys thereof, etc.), resin films (films of polyimide, polyarylate, polysulfone, polyarylsulfone, polyamide, polyetheramide, polyphenylene sulfide, polyaryletherketone, polyamideimide, liquid crystalline polyester, liquid crystalline polyesteramide, etc.), and prepregs (precursors of fiber-reinforced resin substrates). The shape of the substrate may be flat, curved or uneven, and may further be any of foil, plate, film and fiber.
[0046] Suitable embodiments of the laminate include a metal-clad laminate having a metal foil and an F layer formed on at least one surface thereof, and a multilayer film having a resin film and an F layer formed on at least one surface thereof. The metal foil in the metal clad laminate is preferably a copper foil. Such a metal clad laminate is particularly useful as a printed circuit board material. The resin film in the multi-layer film is preferably a polyimide film. Such a multi-layer film is useful as a wire covering material and a printed circuit board material.
[0047] On the side opposite to the substrate of the F layer, another substrate may be further laminated to form a multi-layer laminate. The structure of such a multilayer laminate may be substrate / F layer / other substrate / F layer / substrate, etc. Each layer may further contain glass cloth or a filler. Such laminates are useful as antenna parts, printed circuit boards, aircraft parts, automobile parts, sports equipment, food industry products, paints, cosmetics, and the like, and specifically, are useful as electric wire covering materials (aircraft electric wires, etc.), electrical insulating tapes, insulating tapes for oil drilling, materials for printed circuit boards, separation membranes (microfiltration membranes, ultrafiltration membranes, reverse osmosis membranes, ion exchange membranes, dialysis membranes, gas separation membranes, etc.), electrode binders (for lithium secondary batteries, for fuel cells, etc.), copy rolls, furniture, automobile dashboards, covers for home appliances, etc., sliding members (load bearings, sliding shafts, valves, bearings, gears, cams, belt conveyors, food transport belts, etc.), tools (shovels, files, saws, saws, etc.), boilers, hoppers, pipes, ovens, baking molds, chutes, dies, toilets, and container covering materials. EXAMPLES
[0048] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these. 1. Preparation of each ingredient [powder] Powder 1: Contains 97.9 mol% TFE units, 0.1 mol% NAH units, and 2.0 mol% PPVE units, in that order, and has a carbonyl group with a main chain carbon number of 1 × 10 6 Powder (D50: 2.1 μm, specific surface area: 3 m) made of polymer 1 (fluorine content: 76% by mass, melting temperature: 300 °C) with 1000 particles per particle 2 / g) Powder 2: Contains 97.5 mol% TFE units and 2.5 mol% PPVE units, in that order, and has a carbonyl group with a main chain carbon number of 1 × 10 6 Powder (D50: 1.8 μm, specific surface area: 6 m) made of polymer 2 (fluorine content: 76 mass%, melting temperature: 305 °C) with 40 particles per particle 2 / g)
[0049] [Liquid compound] Liquid compound 1: Isododecane (boiling point: 180°C) Liquid compound 2: Isohexadecane (boiling point: 287°C) Liquid compound 3: Decamethyltetrasiloxane (boiling point: 194°C) Liquid compound 4: Decamethylcyclopentanesiloxane (boiling point: 210°C) Liquid compound 5: Cyclohexane (boiling point: 81°C) In addition, the kinetic viscosity of each liquid compound is 5 mm 2 ·s -1 The following is the result. [Surfactants] Surfactant 1: Nonionic polyoxyalkylene-modified polydimethylsiloxane
[0050] 2. Dispersion liquid production example [Example 1] Powder 1 and liquid compound 1 were charged into a planetary mixer and kneaded to obtain paste 1 (viscosity: 28000 mPa·s) containing powder 1 (34 parts by mass) and liquid compound 1 (30 parts by mass). 36 parts by mass of liquid compound 1 was added to paste 1 in several batches and stirred, and the mixture was degassed for 1 minute at 2000 rpm using a planetary centrifugal mixer to obtain dispersion 1 (viscosity: 400 mPa·s).
[0051] [Examples 2-5, 7] Dispersions 2 to 5 and 7 were prepared in the same manner as in Example 1, except that the types of powder and liquid compound were changed. [Example 6] Powder 2, liquid compound 1, and surfactant 1 were charged into a planetary mixer and kneaded to obtain paste 6 (viscosity: 26,000 mPa·s) containing powder 2 (34 parts by mass), liquid compound 1 (30 parts by mass), and surfactant 1 (3 parts by mass). 33 parts by mass of liquid compound 1 was added to paste 6 in several batches and stirred, and the mixture was degassed for 1 minute at 2000 rpm using a planetary centrifugal mixer to obtain dispersion 6 (viscosity: 400 mPa·s).
[0052] 3. Example of laminate manufacturing Dispersion liquid 1 was applied to the surface of a long copper foil (thickness 18 μm) using a bar coater to form a wet film. The metal foil on which the wet film was formed was then passed through a drying oven at 110° C. for 5 minutes and dried by heating to obtain a dry film. The dry film was then heated at 380° C. for 3 minutes in a nitrogen oven. This produced a laminate 1 having a metal foil and a polymer layer (thickness: 10 μm) as a molded product containing a molten and baked product of powder 1 on its surface. Laminates 2 to 7 were produced in the same manner as for laminate 1, except that dispersion 1 was changed to dispersions 2 to 7.
[0053] 4. Evaluation 4-1. Evaluation of dispersion stability of dispersion liquid 18 mL of each dispersion was placed in a 30 mL screw tube and allowed to stand for 14 days at 25° C. The component dispersion layer ratio was calculated from the total height of the dispersion in the screw tube and the height of the component dispersion layer before and after standing using the following formula. Component dispersion layer rate (%) = (component dispersion layer height) / (total height of dispersion liquid) × 100 If no component dispersion layer is observed after standing and there is no change in state, it is assumed that there is no change in the overall height of the dispersion liquid, and the component dispersion layer rate is taken as 100%. The dispersion stability of the dispersion was evaluated according to the following criteria. [Evaluation Criteria] ◯: Component dispersion layer rate is 90% or more. △: The component dispersion layer rate is 60% or more and less than 80%. ×: The component dispersion layer rate is less than 60%.
[0054] 4-2. Evaluation of foam volume ratio of dispersion liquid For each dispersion, the volume of the dispersion at 1013.25 hPa and 20°C (V N ) and the combined volume of the bubbles when it is decompressed to 0.003 MPa (V V ) was measured, and the foam volume ratio was calculated according to the following formula. Foam volume ratio [%] = 100 × (V V -V N ) / V N The foam volume ratio of the dispersion was evaluated according to the following criteria. [Evaluation Criteria] ◯: Foam volume ratio is 5% or less. △: The foam volume ratio is more than 5% and 10% or less. ×: The foam volume ratio is more than 10%.
[0055] 4-3.Evaluation of dielectric tangent of laminate For each laminate, the copper foil of the laminate was removed by etching with an aqueous ferric chloride solution to produce a single polymer layer, and the dielectric tangent of the polymer layer (measurement frequency: 10 GHz) was measured using a split post dielectric resonance (SPDR) method and evaluated according to the following criteria. [Evaluation Criteria] ○: Dielectric tangent is 0.001 or less. △: The dielectric loss tangent is more than 0.001 and not more than 0.003. ×: The dielectric tangent is more than 0.003. The evaluation results are summarized in Table 1 below.
[0056] [Table 1] [Industrial Applicability]
[0057] As is clear from the above results, the dispersion containing a powder of a specified tetrafluoroethylene-based polymer and a specified hydrocarbon or silicone oil had excellent liquid physical properties, and the laminate obtained by contacting the substrate had excellent physical properties such as low dielectric tangent.
Claims
1. A powder of a tetrafluoroethylene polymer having a carbonyl group-containing group or a hydroxyl group-containing group and a fluorine content of 70% by mass or more, and at least one oil selected from the group consisting of isoalkane, terpene, α-olefin, dimethyl silicone oil, and methylphenyl silicone oil, having a kinetic viscosity of 1000 mm 2 ・s -1 and a liquid compound having a boiling point of 100 to 300°C, wherein the powder is dispersed in the dispersion.
2. The tetrafluoroethylene polymer has a main chain carbon number of 1×10 6 2. The dispersion according to claim 1, which is a polymer having 10 to 5,000 carbonyl group-containing groups per polymer.
3. The dispersion according to claim 1 or 2, wherein the powder has an average particle size of 20 μm or less.
4. The specific surface area of the powder is 25 m 2 The dispersion according to any one of claims 1 to 3, wherein the dispersion has a molecular weight of 1 / g or less.
5. The dispersion according to any one of claims 1 to 4, wherein the liquid compound is an isoalkane or a dimethylsilicone oil.
6. The dispersion according to any one of claims 1 to 5, wherein the liquid compound is isodecane, isododecane, isotetradecane, isohexadecane, linear dimethyl silicone oil or cyclic dimethyl silicone oil.
7. 7. The dispersion according to claim 1, wherein the ratio of the content of the liquid compound to the content of the tetrafluoroethylene-based polymer powder is 1 or more.
8. The dispersion according to any one of claims 1 to 7, wherein the content of the tetrafluoroethylene-based polymer powder is 20 mass% or more.
9. The dispersion of any one of claims 1 to 8, wherein the dispersion further comprises an inorganic filler or an aromatic polymer.
10. The dispersion according to any one of claims 1 to 9, further comprising a nonionic surfactant.
11. The dispersion according to any one of claims 1 to 9, having a viscosity of 50 to 10,000 mPa·s.
12. The dispersion according to any one of claims 1 to 11, wherein the component dispersion layer rate is 60% or more.
13. The dispersion according to any one of claims 1 to 12, wherein the foam volume ratio is 10% or less.
14. A method for producing a laminate, comprising contacting the dispersion according to any one of claims 1 to 13 with a surface of a substrate and heating the resulting mixture to form a polymer layer, thereby obtaining a laminate having the substrate and the polymer layer.
Citation Information
Patent Citations
Carbon electrode, method for forming same, and use thereof
CN110690450A
PTFE nano mask film and preparation method thereof
CN111378240A
PTFE isolating membrane for medical protective clothing and preparation method of PTFE isolating membrane
CN111423676A
Powder slurry composition
JP2003082220A
Surface treatment method for coating film surface and article treated by the method
JP2005334688A