Printing ink and method for producing printed matter using the same
The printing ink formulation with urethane (meth)acrylate and polyfunctional (meth)acrylate addresses adhesion and print quality issues, ensuring strong adhesion to plastic films and maintaining performance through hot water treatment, while producing high-quality prints.
Patent Information
- Application Number
- JP2020531174
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-12-20
- Filing Date
- 2020-05-19
- Publication Date
- 2024-10-02
- Estimated Expiration
- 2040-05-19
AI Technical Summary
Existing active energy ray-curable lithographic printing inks face issues with adhesion to plastic films, particularly during hot water treatment, and deteriorate in print quality due to the addition of urethane compounds, which impair ink viscosity and cohesive force.
A printing ink formulation containing urethane (meth)acrylate and hydroxyl group-containing polyfunctional (meth)acrylate, with specific viscosity and tack values, along with a resin having ethylenically unsaturated groups and hydrophilic groups, to enhance adhesion and flexibility, and a method involving active energy ray irradiation for curing.
The ink exhibits excellent adhesion to plastic films, maintains adhesion performance during hot water treatment, and produces high-quality prints with improved stain resistance and leveling properties.
Smart Images

Figure 0007559554000001 
Figure 0007559554000002 
Figure 0007559554000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a printing ink, a method for producing a printed matter using the same, and a printed matter. [Background technology]
[0002] Lithographic printing is a printing method that is widely used as a system for producing printed matter at high speed, in large quantities, and at low cost. In recent years, the use of active energy ray-curable lithographic printing inks, which are instantly cured by irradiating them with active energy rays from mercury lamps, metal halide lamps, light-emitting diodes, electron beams, etc., has spread to many fields due to its advantages in terms of equipment, safety, environment, and productivity.
[0003] Traditionally, lithographic printing methods have often used paper as a substrate, but printing on plastic films, etc. is becoming more common as substrates become more diverse. In particular, in recent years, studies have begun on the application of this method to printing on flexible packaging, which uses thin plastic films as a substrate and is used for everyday items, food, medicines, etc.
[0004] Since active energy ray-curable lithographic printing inks can be cured at room temperature in a short time, they are considered to be the optimal material for forming an ink film on a plastic film with poor heat resistance. However, when active energy ray-curable lithographic printing inks are used to print on a substrate such as a thin plastic film, the adhesion between the ink and the surface of the plastic film may be insufficient. For this reason, development of active energy ray-curable lithographic printing inks with excellent adhesion to plastic films is underway (see Patent Document 1).
[0005] In addition, since the thin plastic films used in flexible packaging are flexible and easily bent, the ink film needs to be flexible as well as to adhere firmly to the surface of the thin film. In order to improve the flexibility of active energy ray-curable lithographic printing inks, an embodiment using a polymerizable urethane acrylate with excellent flexibility has been disclosed (see Patent Document 2). [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Patent Application Publication No. 3-252472 [Patent Document 2] International Publication No. 2015 / 141552 Summary of the Invention [Problem to be solved by the invention]
[0007] Even when printing is performed on a plastic film using the active energy ray-curable lithographic printing ink with improved adhesion disclosed in Patent Document 1, the adhesion between the ink and the plastic film may be insufficient depending on the composition and surface condition of the plastic film.
[0008] The active energy ray-curable lithographic printing ink with improved flexibility disclosed in Patent Document 2 had a tendency to show a marked decrease in adhesion to plastic films when subjected to heat treatments such as boiling and retorting, which are essential for food packaging applications.
[0009] Furthermore, adding urethane compounds to inks had the problem of deteriorating print quality (resistance to scumming and leveling).
[0010] Therefore, the present invention aims to overcome the problems of the conventional technology, to provide a printing ink that exhibits good adhesion to plastic films, does not lose its adhesion even during hot water treatment, and can produce printed matter of good print quality, which is particularly suitable for active energy ray-curable lithographic printing, and to provide a method for producing printed matter using the same. [Means for solving the problem]
[0011] The inventors have come up with this invention based on the fact that when a urethane compound is added to an ink, the urethane compound is incompatible with the ink, impairing the Newtonian properties of the ink, and that the cohesive force is increased by the urethane bond, thereby increasing the ink viscosity and tack value, thereby deteriorating print quality (resistance to scumming and leveling).
[0012] That is, the present invention provides a printing ink containing (a) a urethane (meth)acrylate and (c) another polymerizable monomer, Contains at least a hydroxyl group The printing ink contains a hydrophilic multifunctional (meth)acrylate, and is characterized in that the ink tack value is 5.0 or more and 18.0 or less, and the viscosity (C) at 20 rpm and the viscosity (B) at 50 rpm measured at 35°C with a cone-plate type rotational viscometer are both 5 Pa s or more and 100 Pa s or less, and the viscosity ratio (B) / (C) is 0.60 or more and 1.00 or less.
[0013] The printing ink of the present invention preferably further contains a resin.
[0015] The present invention also relates to a method for producing a printed matter by lithographic printing using the printing ink of the present invention, which is characterized by comprising a step of irradiating the ink with active energy rays after transferring the ink to a substrate to be printed.
[0016] The present invention also relates to a method for producing a printed matter by lithographic printing using the printing ink of the present invention, characterized in that a waterless lithographic plate is used as the lithographic plate. Effect of the Invention
[0019] According to the printing ink of the present invention and the method for producing a printed matter using the same, it is possible to obtain a printed matter having good print quality, which exhibits good adhesion to plastic films and does not lose its adhesion performance even during hot water treatment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] The present invention will be specifically described below. In explaining the scope of the present invention, the word "obtained (product)" is used after indicating raw materials, but it is not limited to the product obtained by the reaction of the indicated raw materials, and also includes the indicated raw materials and products having the same structure as the product obtainable by the reaction.
[0021] The printing ink of the present invention contains (a) a urethane (meth)acrylate. Note that "(meth)acrylate" is a general term including acrylate and methacrylate.
[0022] The hydrogen bonds between the urethane bonds contained in the (a) urethane (meth)acrylate form hard segments that can impart toughness to the ink film, and can also provide good adhesion to the surface of a plastic film or the like by forming strong bonds. In addition, the acrylic groups contained in the (a) urethane (meth)acrylate cause a curing reaction when irradiated with active energy rays, and can therefore provide heat resistance to the ink film. Furthermore, the (a) urethane (meth)acrylate contains a polyol, which forms soft segments and can provide flexibility to the ink film.
[0023] (a) Urethane (meth)acrylate can be synthesized by reacting (meth)acrylic acid having a hydroxyl group with a polyisocyanate compound and a polyol compound.
[0024] (a) Urethane (meth)acrylate preferably has at least an ether structure in the polyol. Polyether polyol is particularly preferred because it is water resistant, has a low solubility parameter (SP value), has good compatibility with the resin constituting the ink, and is inexpensive. The polyhydric alcohols used as raw materials for polyether polyols are not particularly limited, but include low molecular weight alcohol compounds such as ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,2-butanediol, 1,3-butanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 3-methyl-1,5-pentanediol, neopentyl glycol, 1,8-octanediol, 1,9-nonanediol, diethylene glycol, dipropylene glycol, 1,4-cyclohexanedimethanol, ethylene oxide or propylene oxide adduct of bisphenol A, trimethylolpropane, glycerin, and pentaerythritol, and low molecular weight amino alcohol compounds such as monoethanolamine and diethanolamine. Among them, polytetramethylene ether glycol (PTMG) having a 1,4-butanediol structure is particularly preferred because it has a high cohesive force and enhances the physical properties of the ink coating film. On the other hand, polypropylene glycol is also particularly preferred because the branching keeps the cohesive force low, thereby maintaining the ink flowability and suppressing an increase in tack.
[0025] It is also preferable that the (a) urethane (meth)acrylate has at least one of an ester structure and a polycarbonate structure. When the urethane (meth)acrylate has at least one of an ester structure and a polycarbonate structure, the heat resistance and coating film properties of the ink can be effectively improved by these rigid structures. In addition, these rigid structures suppress entanglement of the molecular chains formed, keep the ink viscosity low, and improve the ink fluidity, thereby obtaining good transferability during printing.
[0026] The alcohol that gives the ester structure is preferably a polyhydric alcohol, and the dicarboxylic acid that gives the ester structure is not particularly limited, but includes phthalic acid, isophthalic acid, terephthalic acid, adipic acid, oxalic acid, maleic acid, fumaric acid, sebacic acid, etc. Among these, isophthalic acid and adipic acid are particularly preferred because they are relatively inexpensive, have good heat resistance, and maintain good compatibility with ink.
[0027] Examples of carbonate polyols that give urethane having a carbonate structure include pentamethylene carbonate diol, hexamethylene carbonate diol, hexane carbonate diol, and decane carbonate diol. However, due to the high cohesive strength of the carbonate bond, as the amount of carbonate bond increases, the viscosity increases and the compatibility with ink deteriorates. Therefore, pentamethylene carbonate diol or hexamethylene carbonate diol, which have a branched chain that suppresses the hydrogen bond strength of the carbonate bond, are particularly preferred.
[0028] (a) The polyisocyanate compound used as the raw material for the urethane (meth)acrylate is not particularly limited, but it is preferable to use a diisocyanate in order to suppress the viscosity of the urethane compound formed by the reaction of the hydroxyl group of the polyol with the isocyanate group of the polyisocyanate compound, and to maintain compatibility with the resin and monomer in the ink. The diisocyanate is not particularly limited. For example, compounds having an aromatic ring structure include toluene diisocyanate, diphenylmethane diisocyanate, and xylylene diisocyanate. Compounds having an alicyclic structure include isophorone diisocyanate, 4,4-methylenebiscyclohexyl diisocyanate (so-called hydrogenated MDI), and hydrogenated xylylene diisocyanate. Compounds having an aliphatic structure include hexamethylene diisocyanate. These diisocyanates can be used alone or in combination of two or more.
[0029] The isocyanate constituting the (a) urethane (meth)acrylate preferably has an aromatic ring structure or an alicyclic structure in order to provide excellent coating properties, and more preferably has an alicyclic structure in order to provide resistance to yellowing due to heat.
[0030] The raw material for providing the urethane (meth)acrylate acrylate (a) contained in the ink of the present invention is preferably an acrylate ester having a hydroxyl group. The hydroxyl group-containing acrylate ester is not particularly limited, but is preferably an acrylate ester having two or more acrylic groups in terms of improving heat resistance and water resistance. The hydroxyl group-containing acrylate ester having two or more acrylic groups is not particularly limited, but may be poly(meth)acrylates of polyhydric alcohols such as trimethylolpropane, glycerin, pentaerythritol, diglycerin, ditrimethylolpropane, isocyanuric acid, and dipentaerythritol, and their alkylene oxide adducts. More specifically, di(meth)acrylate of trimethylolpropane, di(meth)acrylate of glycerin, di- or tri(meth)acrylate of pentaerythritol, di- or tri(meth)acrylate of diglycerin, di- or tri(meth)acrylate of ditrimethylolpropane, di-, tri-, tetra- or penta(meth)acrylate of dipentaerythritol, and their ethylene oxide adducts, propylene oxide adducts, tetraethylene oxide adducts, etc. can be mentioned. Among these, pentaerythritol triacrylate can be particularly preferably used. These hydroxyl-containing acrylic acid esters having two or more acrylic groups can be used alone or in combination of two or more.
[0031] The polyisocyanate compound is not particularly limited, but it is preferable to use a diisocyanate in order to suppress the viscosity of the urethane compound formed by the reaction of the hydroxyl group in the resin such as (b) resin having an ethylenically unsaturated group and a hydrophilic group and (c) other polymerizable monomer with the isocyanate group of the polyisocyanate compound, which will be described later, and to maintain compatibility with the resin and monomer in the ink. Examples of diisocyanates include compounds having an aromatic ring structure such as toluene diisocyanate, diphenylmethane diisocyanate, and xylylene diisocyanate. Examples of compounds having an alicyclic structure include isophorone diisocyanate (IPDI), 4,4-methylenebiscyclohexyl diisocyanate (so-called hydrogenated MDI), and hydrogenated xylylene diisocyanate. Examples of compounds having an aliphatic structure include hexamethylene diisocyanate. These diisocyanates can be used alone or in combination of two or more. Diisocyanates preferably have an aromatic ring structure or an alicyclic structure because they have excellent coating properties, and diisocyanates with an alicyclic structure are preferred because they have excellent yellowing resistance and weather resistance. Among them, IPDI is particularly preferred because it has a bulky structure, which reduces the cohesive force of the urethane compound, thereby suppressing viscosity, and because the suppression of cohesive force results in excellent compatibility with the resin and monomer in the ink, and also shows high adhesion. In addition, aromatic ring structures are preferred because of their excellent reactivity and the fact that raw materials are available at low cost.
[0032] The urethane (meth)acrylate (a) contained in the ink of the present invention is also preferably in the following form. (1) A compound having at least a urethane structure obtained from a polyisocyanate having an aromatic ring structure or an alicyclic structure, and an ester structure obtained from a carboxylic acid. (2) A compound having at least a urethane bond structure obtained from a diisocyanate having an alicyclic structure and an ester structure obtained from adipic acid or isophthalic acid. (3) A compound having a urethane structure obtained from a polyisocyanate having at least an aromatic ring structure or an alicyclic structure, and a carbonate structure consisting of a carbonate dipolyol. (4) A compound having a urethane structure obtained from a diisocyanate having at least an alicyclic structure, and a carbonate structure selected from at least one selected from polypentamethylene carbonate diol and polyhexamethylene carbonate diol. (5) A compound having a urethane structure and an acrylic group, obtained by reacting a hydroxyl group-containing acrylic ester with an isocyanate compound. (6) A compound having a urethane structure and an acrylic group, which is obtained by reacting pentaerythritol triacrylate with a diisocyanate compound having an aromatic ring structure.
[0033] The weight-average molecular weight of the (a) urethane (meth)acrylate is preferably 100 or more because the hot water resistance of the active energy ray-curable lithographic printing ink is improved, and since the soft segment ratio of polyol components in one molecule is at least a certain level, the coating film is given flexibility and the adhesion is improved, so the weight-average molecular weight is more preferably 300 or more, even more preferably 500 or more, even more preferably 800 or more, even more preferably 1,000 or more, and even more preferably 1,500 or more. In addition, by maintaining compatibility with the ink, the fluidity of the ink is maintained, and good coating film appearance (leveling property) and background smear resistance can be obtained during printing, and Newtonian behavior as described below can be imparted, so the weight-average molecular weight is preferably 10,000 or less, more preferably 7,000 or less, and even more preferably 5,000 or less. The weight-average molecular weight of the resin can be calculated by measuring it in terms of polystyrene using gel permeation chromatography (GPC).
[0034] The urethane bond fraction of the (a) urethane (meth)acrylate is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 15% by mass or more, in order to suppress the entanglement of molecular chains due to rigid urethane bonds and suppress the increase in viscosity of the ink, and to obtain the effect of improving the cohesive force of the ink coating film and improving the adhesion strength by forming hydrogen bonds with the substrate surface. On the other hand, in order to maintain the appropriate fluidity of the ink by exhibiting good compatibility with (b) resins such as resins having ethylenically unsaturated groups and hydrophilic groups, and (c) inks containing other polymerizable monomers, the urethane bond fraction is preferably 40% by mass or less, more preferably 30% by mass or less, and even more preferably 20% by mass or less. The bond fraction can be calculated from the ratio of the CH peak area of the internal standard substance to the NH peak area derived from the urethane bond, the ratio of the number of protons of the internal standard substance and the urethane bond, and the molecular weight of the urethane bond and the molecular weight of the internal standard substance, as measured by proton nuclear magnetic resonance (1H-NMR).
[0035] The content of the (a) urethane (meth)acrylate in the total amount of the ink is preferably 1% by mass or more, more preferably 3% by mass or more, more preferably 5% by mass or more, and even more preferably 7% by mass or more in order to obtain good adhesion. In addition, by making the content 30% by mass or less, more preferably 20% by mass or less, and even more preferably 15% by mass or less, good compatibility with the resin can be maintained. This suppresses the increase in tackiness of the ink, and allows a printed matter with good positional accuracy of the pattern to be obtained. In addition, since the ink fluidity can be suitably maintained, it is preferable because a printed matter with excellent coating appearance (leveling property) and no background scumming (transfer of ink to non-image areas) can be obtained.
[0036] In the printing ink of the present invention, the ratio of the (a) urethane (meth)acrylate to the (c) other polymerizable monomers described below is preferably 40% by mass or less, more preferably 35% by mass or less, in order to maintain good compatibility as an ink. By maintaining good compatibility, it is possible to obtain the effects of suppressing the increase in tack of the ink, good coating appearance, and background stain resistance, as described above. In addition, in order to develop good adhesion between the substrate and the ink, the content is preferably 3% by mass or more, more preferably 7% by mass or more. In addition, by having the content of the urethane (meth)acrylate within the above range, it is possible to maintain good ink fluidity and hot water resistance of the cured ink coating.
[0037] The printing ink of the present invention preferably further contains a resin, which can provide the ink with a flowability suitable for printing, such as preventing the ink from scattering (misting) during printing.
[0038] Resins contained in the printing ink of the present invention include, but are not limited to, acrylic resins, styrene-acrylic resins, styrene-maleic acid resins, rosin-modified maleic acid resins, rosin-modified acrylic resins, epoxy resins, polyester resins, polyurethane resins, phenolic resins, etc. Among the main chain structures derived from the above-listed resins, main chain structures derived from acrylic resins, styrene-acrylic resins, and styrene-maleic acid resins are preferably used in terms of ease of availability of monomers that are raw materials for the resins, low cost, ease of synthesis, compatibility with other ink components, pigment dispersibility, etc.
[0039] In addition, the resin contained in the printing ink of the present invention is particularly preferably a resin having (b) an ethylenically unsaturated group and a hydrophilic group. The ethylenically unsaturated group of the resin reacts with the acrylic group contained in the urethane (meth)acrylate (a) to form a strong covalent bond when irradiated with active energy rays, thereby improving the resistance of the ink film to hot water treatment and the like. In addition, the hydrophilic group strongly interacts with the urethane bond contained in the urethane (meth)acrylate (a), thereby significantly improving the resistance of the ink film to hot water treatment and the like. This is presumably due to the interaction between the hydrophilic groups in the ink, which increases the cohesive force of the ink. Furthermore, the increased cohesive force of the ink improves the ink repellency to non-image areas, which results in improved anti-scumming properties. In addition, the ethylenically unsaturated group forms a crosslinked structure by reacting with radical species, thereby improving the sensitivity of the printing ink of the present invention to active energy rays.
[0040] Preferred examples of the hydrophilic group of the (b) resin having an ethylenically unsaturated group and a hydrophilic group include a hydroxyl group, an amino group, a mercapto group, a carboxyl group, a sulfo group, a phosphate group, etc. Among these, a carboxyl group or a hydroxyl group, which have good interaction with the urethane bond of the (a) compound, is more preferred, and it is particularly preferred that the resin contains both a carboxyl group and a hydroxyl group.
[0041] The acid value of the (b) resin having an ethylenically unsaturated group and a hydrophilic group is preferably 30 mgKOH / g or more, more preferably 60 mgKOH / g or more, and even more preferably 75 mgKOH / g or more, because the ink has good pigment dispersibility and improves background stain resistance. In addition, the acid value is preferably 250 mgKOH / g or less, more preferably 200 mgKOH / g or less, and even more preferably 150 mgKOH / g or less, because the resin exhibits solubility in polyfunctional (meth)acrylates and maintains the fluidity of the ink by suppressing the increase in viscosity caused by polar groups. The acid value of the resin can be determined in accordance with the neutralization titration method in Section 3.1 of the test method of JIS K 0070:1992.
[0042] The iodine value of the resin having (b) an ethylenically unsaturated group and a hydrophilic group is preferably 0.5 mol / kg or more, more preferably 1.0 mol / kg or more, and even more preferably 1.5 mol / kg or more, because the curing sensitivity to active energy rays is good. Also, the iodine value is preferably 3.0 mol / kg or less, more preferably 2.5 mol / kg or less, and even more preferably 2.0 mol / kg or less, because the storage stability of the ink is improved. The iodine value of the resin having an ethylenically unsaturated group and a hydrophilic group can be adjusted by the amount of the ethylenically unsaturated group. The iodine value of the resin can be determined by the method described in JIS K 0070:1992, Test Method, Section 6.0.
[0043] Specific examples of the (b) resin skeleton having an ethylenically unsaturated group and a hydrophilic group include (meth)acrylic acid copolymer, (meth)acrylic acid-(meth)acrylic acid ester copolymer, styrene-(meth)acrylic acid copolymer, styrene-(meth)acrylic acid-(meth)acrylic acid ester copolymer, styrene-maleic acid copolymer, styrene-maleic acid-(meth)acrylic acid copolymer, and styrene-maleic acid-(meth)acrylic acid ester copolymer.
[0044] Among the above-listed resins, the resin having an ethylenically unsaturated group and a hydrophilic group and having a main chain structure derived from a resin selected from the group consisting of acrylic resin, styrene-acrylic resin, and styrene-maleic acid resin can be prepared by the following method.
[0045] A resin having a hydrophilic group can be obtained by polymerizing or copolymerizing a compound selected from among a carboxyl group-containing monomer such as (meth)acrylic acid, itaconic acid, crotonic acid, maleic acid, fumaric acid, vinyl acetate, or an acid anhydride thereof, a hydroxyl group-containing monomer such as 2-hydroxyethyl (meth)acrylate, an amino group-containing monomer such as dimethylaminoethyl (meth)acrylate, a mercapto group-containing monomer such as 2-(mercaptoacetoxy)ethyl (meth)acrylate, a sulfo group-containing monomer such as (meth)acrylamido t-butylsulfonic acid, a phosphoric acid group-containing monomer such as 2-(meth)acryloxyethyl acid phosphate, a (meth)acrylic acid ester, styrene, (meth)acrylonitrile, vinyl acetate, and the like, using a polymerization initiator. Furthermore, an ethylenically unsaturated compound having a glycidyl group or an isocyanate group, acrylic acid chloride, methacrylic acid chloride or allyl chloride can be added to the active hydrogen-containing group, mercapto group, amino group, hydroxyl group or carboxyl group, in the resin having a hydrophilic group, to obtain a resin having an ethylenically unsaturated group and a hydrophilic group, although the method is not limited to these methods.
[0046] Specific examples of ethylenically unsaturated compounds having a glycidyl group include glycidyl (meth)acrylate, allyl glycidyl ether, glycidyl crotonate, and glycidyl isocrotonate.
[0047] Specific examples of the ethylenically unsaturated compound having an isocyanate group include (meth)acryloyl isocyanate and (meth)acryloylethyl isocyanate.
[0048] The weight average molecular weight of the (b) resin having an ethylenically unsaturated group and a hydrophilic group is preferably 100,000 or less, more preferably 75,000 or less, and even more preferably 50,000 or less, in order to maintain the fluidity of the ink. In addition, the weight average molecular weight is preferably 5,000 or more, more preferably 15,000 or more, and even more preferably 20,000 or more, in order to improve the resistance to hot water treatment and the background staining resistance of the printed matter printed with the active energy ray-curable lithographic printing ink. The weight average molecular weight of the resin can be obtained by measuring in terms of polystyrene using gel permeation chromatography (GPC).
[0049] The content of the resin (b) having an ethylenically unsaturated group and a hydrophilic group in the printing ink of the present invention is preferably 5% by mass or more and 50% by mass or less. By having the content of the resin within the above range, the resistance of the ink film to hot water treatment can be maintained at a good level.
[0050] The printing ink of the present invention contains (c) other polymerizable monomers. Here, compounds belonging to (a) and compounds belonging to resin compounds such as (b) are not classified as (c) other polymerizable monomers. By containing (c) other polymerizable monomers, ink physical properties such as viscosity and leveling required for lithographic printing can be adjusted. In addition, the (c) other polymerizable monomers crosslink the (a) urethane (meth)acrylate and (b) resin having an ethylenically unsaturated group and a hydrophilic group through an addition reaction by irradiation with active energy rays, so that the resistance of the ink coating to hot water treatment and the like can be further improved.
[0051] From the viewpoint of compatibility with the resin (b) having an ethylenically unsaturated group and a hydrophilic group, the (c) other polymerizable monomer preferably contains a hydrophilic polyfunctional (meth)acrylate, and particularly preferably contains at least a hydroxyl group-containing polyfunctional (meth)acrylate. The hydroxyl group interacts with the urethane bond in the (a) urethane (meth)acrylate and the hydrophilic group in the resin (b) having an ethylenically unsaturated group and a hydrophilic group in the ink, so that good resistance to hot water treatment and the like can be obtained. In addition, the ink can have good pigment dispersibility in the ink, improving the ink flowability. The improved ink flowability shows good transferability during printing.
[0052] The hydroxyl value of the hydroxyl group-containing polyfunctional (meth)acrylate is preferably 50 mgKOH / g or more, more preferably 75 mgKOH / g or more, and even more preferably 100 mgKOH / g or more, because the pigment dispersibility is improved. The hydroxyl value is preferably 200 mgKOH / g or less, more preferably 180 mgKOH / g or less, and even more preferably 160 mgKOH / g or less, because the viscosity increase caused by polar groups is suppressed and the fluidity can be kept good.
[0053] Examples of raw materials for the polyfunctional (meth)acrylate having a hydroxyl group include polyhydric alcohols such as trimethylolpropane, glycerin, pentaerythritol, diglycerin, ditrimethylolpropane, isocyanuric acid, and dipentaerythritol. These are esterified with (meth)acrylate to obtain a polyfunctional (meth)acrylate having a hydroxyl group. An alkylene oxide may be added.
[0054] Examples of polyfunctional (meth)acrylates having a hydroxyl group include di(meth)acrylate of trimethylolpropane, di(meth)acrylate of glycerin, di- or tri(meth)acrylate of pentaerythritol, di- or tri(meth)acrylate of diglycerin, di- or tri(meth)acrylate of ditrimethylolpropane, di-, tri-, tetra- or penta(meth)acrylate of dipentaerythritol, and ethylene oxide adducts, propylene oxide adducts, and tetraethylene oxide adducts of these.
[0055] Among the above, pentaerythritol tri(meth)acrylate, diglycerin tri(meth)acrylate, and ditrimethylolpropane tri(meth)acrylate are particularly preferred because they provide the ink of the present invention with excellent pigment dispersibility and flowability.
[0056] The content of the (c) other polymerizable monomer in the ink of the present invention is preferably 10% by mass or more, more preferably 15% by mass or more, and even more preferably 20% by mass or more, in order to effectively improve the hot water treatment resistance of the ink film. In addition, by making it preferably 70% by mass or less, more preferably 60% by mass or less, and even more preferably 50% by mass or less, it is possible to suppress the increase in viscosity caused by polar groups, maintain good fluidity, suppress the increase in tackiness of the ink, and obtain good coating appearance (leveling property) and scum resistance.
[0057] The (c) other polymerizable monomer contained in the ink of the present invention preferably contains a (meth)acrylate having an alicyclic skeleton or an aliphatic skeleton having 6 to 18 carbon atoms. By adding the (meth)acrylate having an alicyclic skeleton or an aliphatic skeleton having 6 to 18 carbon atoms, the viscosity and surface free energy of the ink are reduced, improving the ink transferability and adhesion to the substrate that is to be printed.
[0058] Of the (meth)acrylates having an alicyclic skeleton or an aliphatic skeleton having 6 to 18 carbon atoms, (meth)acrylates having an aliphatic skeleton having 6 to 18 carbon atoms are preferred for improving ink transferability to a substrate.
[0059] Among (meth)acrylates having an alicyclic skeleton or an aliphatic skeleton having 6 to 18 carbon atoms, (meth)acrylates having an alicyclic skeleton are preferred because they have a smaller volumetric shrinkage during curing due to irradiation with active energy rays, improving adhesion to the substrate. The alicyclic skeleton is more preferably a condensed ring skeleton, because it is more rigid, has a smaller volumetric shrinkage during curing, and improves the physical properties of the cured film, such as scratch resistance. Examples of the alicyclic skeleton include a norbornane skeleton, an adamantane skeleton, a tricyclodecane skeleton, and a dicyclopentadiene skeleton, and the tricyclodecane skeleton is particularly preferred.
[0060] When the (meth)acrylate having an alicyclic skeleton or an aliphatic skeleton having 6 to 18 carbon atoms is added, the amount is preferably 1% by mass or more, more preferably 5% by mass or more, and even more preferably 10% by mass or more, based on the ink of the present invention in order to improve ink transferability and adhesion to the substrate. In addition, the amount is preferably 40% by mass or less, more preferably 35% by mass or less in order to suppress a decrease in the ink viscosity and maintain smear resistance.
[0061] The (meth)acrylate having an alicyclic skeleton or an aliphatic skeleton having 6 to 18 carbon atoms has good curing sensitivity to active energy rays, and the strength of the cured film is increased, thereby improving adhesion, so that it is preferable that the (meth)acrylate has two or more (meth)acrylate-derived structures.
[0062] In order to improve ink transferability to a substrate, the (meth)acrylate having an aliphatic skeleton having 6 to 18 carbon atoms preferably has 6 or more carbon atoms, more preferably 8 or more carbon atoms, and even more preferably 10 or more carbon atoms. (b) In order to suppress a decrease in compatibility with a resin having an ethylenically unsaturated group and a hydrophilic group, and a hydrophilic polyfunctional (meth)acrylate, an increase in the viscosity of the ink, and a decrease in ink transferability, the (meth)acrylate preferably has 18 or less carbon atoms, more preferably 16 or less carbon atoms, and even more preferably 14 or less carbon atoms.
[0063] The ratio of the (meth)acrylate having an aliphatic skeleton having 6 to 18 carbon atoms relative to the total amount of the hydrophilic polyfunctional (meth)acrylate (1.00 part by mass) is preferably 0.02 parts by mass or more, more preferably 0.04 parts by mass or more, and even more preferably 0.06 parts by mass or more, in order to maintain a suitable compatibility with the hydrophilic polyfunctional (meth)acrylate and improve ink transferability. For the same reason, the ratio of the (meth)acrylate having an aliphatic skeleton having 6 to 18 carbon atoms relative to the total amount of the hydrophilic polyfunctional (meth)acrylate (1.00 part by mass) is preferably 0.30 parts by mass or less, more preferably 0.20 parts by mass or less, even more preferably 0.15 parts by mass or less, and even more preferably 0.12 parts by mass or less.
[0064] The ratio of the (meth)acrylate having an aliphatic skeleton having 6 to 18 carbon atoms relative to the total amount of the (b) resin having an ethylenically unsaturated group and a hydrophilic group (1.00 part by mass) is preferably 0.10 parts by mass or more, more preferably 0.15 parts by mass or more, and even more preferably 0.20 parts by mass or more, in order to maintain a suitable compatibility with the (b) resin having an ethylenically unsaturated group and a hydrophilic group and to improve ink transferability. For the same reason, the ratio of the (meth)acrylate having an aliphatic skeleton having 6 to 18 carbon atoms relative to the total amount of the (b) resin having an ethylenically unsaturated group and a hydrophilic group (1.00 part by mass) is preferably 0.60 parts by mass or less, more preferably 0.45 parts by mass or less, and even more preferably 0.30 parts by mass or less.
[0065] Specific examples of the (meth)acrylate having an alicyclic skeleton or an aliphatic skeleton having 6 to 18 carbon atoms include, in the case of a monofunctional (meth)acrylate having an aliphatic skeleton having 6 to 18 carbon atoms, hexyl (meth)acrylate, octyl (meth)acrylate, nonyl (meth)acrylate, dodecyl (meth)acrylate, stearyl (meth)acrylate, and isostearyl (meth)acrylate; and examples of the (meth)acrylate having an alicyclic skeleton include isobornyl (meth)acrylate, norbornyl (meth)acrylate, norbornane-2-methanol (meth)acrylate, cyclohexyl (meth)acrylate, tricyclopentenyl (meth)acrylate, tricyclopentenyloxy (meth)acrylate, and tricyclodecane monomethylol (meth)acrylate.
[0066] As bifunctional (meth)acrylates having an aliphatic skeleton with 6 to 18 carbon atoms, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, 1,7-heptanediol di(meth)acrylate, 1,8-octanediol di(meth)acrylate, 1,10-decanediol di(meth)acrylate, 1,11-undecanediol di(meth)acrylate, 1,12-dodecanediol di(meth)acrylate, 1,13-tridecanediol di(meth)acrylate, 1,14-tridecanediol di(meth)acrylate, 1,15-tridecanediol di(meth)acrylate, 1,16-tridecanediol di(meth)acrylate, 1,1 ...tridecanediol di(meth)acrylate, 1,18-tridecanediol di(meth)acrylate, 1,19-tridecanediol di(meth)acrylate, 1,20-tridecanediol di(meth)acrylate, 1,21-tridecanediol di(meth)acrylate, 1,22-tridecanediol di(meth)acrylate, 1,23-tridecanediol di(meth)acrylate, 1,24-tridecanediol di(meth)acrylate, 1,25-tridecanediol di(meth)acrylate, 1, Examples of the (meth)acrylate having an alicyclic skeleton include dicyclopentadiene dimethanol di(meth)acrylate and tricyclodecane dimethanol di(meth)acrylate. In addition, the polyester di(meth)acrylate may have an aliphatic skeleton having 6 to 18 carbon atoms as a repeating unit. The polyester di(meth)acrylate may contain two or more of these. Among the above, tricyclodecane dimethanol di(meth)acrylate is particularly preferred because it has a small volume shrinkage during curing, a condensed ring skeleton, and is bifunctional. Also, 1,10-decane diol di(meth)acrylate is particularly preferred in order to maintain a suitable degree of compatibility with (b) resins having ethylenically unsaturated groups and hydrophilic groups, and hydrophilic polyfunctional (meth)acrylates, and to improve ink transferability. The functionality here refers to the number of (meth)acrylate-derived structures.
[0067] The ink of the present invention preferably contains a pigment consisting of an organic pigment and / or an inorganic pigment. Specific examples of organic pigments include phthalocyanine pigments, soluble azo pigments, insoluble azo pigments, lake pigments, quinacridone pigments, isoindoline pigments, threne pigments, metal complex pigments, etc., and specific examples thereof include phthalocyanine blue, phthalocyanine green, azo red, monoazo red, monoazo yellow, disazo red, disazo yellow, quinacridone red, quinacridone magenta, isoindoline yellow, etc.
[0068] Examples of inorganic pigments include titanium oxide, zinc oxide, alumina white, calcium carbonate, barium sulfate, red iron oxide, cadmium red, yellow lead, zinc yellow, iron blue, ultramarine, oxide-coated glass powder, oxide-coated mica, oxide-coated metal particles, aluminum powder, gold powder, silver powder, copper powder, zinc powder, stainless steel powder, nickel powder, organic bentonite, iron oxide, carbon black, and graphite.
[0069] In the case of inks to be printed as a base color for transparent plastic films, white pigments such as titanium dioxide, zinc oxide, and alumina white, which impart hiding properties, are preferred.
[0070] The particle size of the white pigment is preferably 200 nm or more and 300 nm or less, at which point the transmittance of visible light is most reduced due to scattering.
[0071] The pigment concentration in the printing ink of the present invention is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 15% by mass or more, in order to obtain a printing density, if the pigment is an organic pigment or carbon black having a specific gravity of 2 or less. Also, in order to improve the fluidity of the ink and obtain good transferability, it is preferably 50% by mass or less, more preferably 45% by mass or less, and even more preferably 40% by mass or less. If the pigment is an inorganic pigment having a specific gravity of more than 2, it is preferably 20% by mass or more, more preferably 30% by mass or more, and even more preferably 40% by mass or more, in order to obtain a printing density. Also, in order to improve the fluidity of the ink and obtain good transferability, it is preferably 70% by mass or less, more preferably 60% by mass or less, and even more preferably 50% by mass or less.
[0072] The printing ink of the present invention preferably contains an acylphosphine oxide compound. The acylphosphine oxide compound also absorbs light in the long wavelength region of 350 nm or more, and therefore has high sensitivity even in a system containing a pigment that absorbs or reflects ultraviolet light. In addition, the acylphosphine oxide compound has a photobleaching effect in which light absorption disappears after one reaction, and this effect shows excellent internal curing properties. In addition, the acylphosphine oxide compound generally has low solubility in polyfunctional (meth)acrylates, so it does not diffuse uniformly in the ink, and as a result, there are cases in which the improvement in sensitivity commensurate with the amount added is not observed, or the ink fluidity is reduced due to precipitation of the acylphosphine oxide compound. On the other hand, the acylphosphine oxide compound exhibits high compatibility with the polyfunctional (meth)acrylates having a hydroxyl group, so it diffuses uniformly in the medium, and as a result, the sensitivity to active energy rays is improved.
[0073] Specific examples of the acylphosphine oxide compound include 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide, 2,6-dimethylbenzoyl-diphenyl-phosphine oxide, 2,6-dimethoxybenzoyl-diphenyl-phosphine oxide, benzoyl-diphenyl-phosphine oxide, 2,4,6-trimethylbenzoyl-bis(4-methoxyphenyl)phosphine oxide, 2,6-dimethylbenzoyl-bis(4-methoxyphenyl)phosphine oxide, 2,6-dimethoxybenzoyl-bis(4-methoxyphenyl)phosphine oxide, 2,4,6-trimethylbenzoyl-4-methoxyphenyl-phenyl-phosphine oxide, 2,6-dimethylbenzoyl-4-methoxyphenyl-phenyl-phosphine oxide, 2,6-dimethoxybenzoyl-4-methoxyphenyl-phenyl-phosphine oxide, Examples of such compounds include 2,4,6-trimethylbenzoyl-dicyclohexyl-phosphine oxide, 2,6-dimethylbenzoyl-dicyclohexyl-phosphine oxide, 2,6-dimethoxybenzoyl-dicyclohexyl-phosphine oxide, benzoyl-bis(2,4,6-trimethylphenyl)phosphine oxide, bis(2,4,6-trimethylbenzoyl)-phenyl-phosphine oxide, bis(2,6-dimethylbenzoyl)-phenyl-phosphine oxide, bis(2,6-dimethoxybenzoyl)-phenyl-phosphine oxide, bis(2,4,6-trimethylbenzoyl)-2,4,4-trimethylpentyl-phosphine oxide, bis(2,6-dimethoxybenzoyl)-2,4,4-trimethylpentyl-phosphine oxide, and bis(2,6-dimethylbenzoyl)-2,4,4-trimethylpentyl-phosphine oxide. Among these, 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide, bis(2,4,6-trimethylbenzoyl)-phenyl-phosphine oxide, and bis(2,6-dimethoxybenzoyl)-2,4,4-trimethylpentyl-phosphine oxide, which are easily available, are particularly preferred.
[0074] In order to improve the curing sensitivity to light of 350 nm or more, the printing ink of the present invention preferably contains the acylphosphine oxide compound in an amount of 1 mass % or more, more preferably 3 mass % or more, and even more preferably 5 mass % or more. In order to improve the storage stability of the ink and maintain good fluidity, the amount is preferably 20 mass % or less, more preferably 15 mass % or less, and even more preferably 10 mass % or less.
[0075] The printing ink of the present invention may contain a sensitizer. Specific examples of the sensitizer include 2-methylthioxanthone, 2-chlorothioxanthone, 2,4-diethylthioxanthone, isopropylthioxanthone, 2,4-dichlorothioxanthone, 2,3-bis(4-diethylaminobenzal)cyclopentanone, 2,6-bis(4-dimethylaminobenzal)cyclohexanone, 2,6-bis(4-dimethylaminobenzal)-4-methylcyclohexanone, 4,4-bis(dimethylamino)-benzophenone (also known as Michler's ketone), 4,4-bis(diethylamino)-benzophenone, 4,4-bis(dimethylamino)chalcone, 4,4-bis(diethylamino)chalcone, p-dimethylaminocinnamylidene indanone, p-dimethylaminobenzylidene Indanone, 2-(p-dimethylaminophenylvinylene)-isonaphthothiazole, 1,3-bis(4-dimethylaminobenzal)acetone, 1,3-carbonyl-bis(4-diethylaminobenzal)acetone, 3,3-carbonyl-bis(7-diethylaminocoumarin), N-phenyl-N-ethylethanolamine, N-phenylethanolamine, N-tolyldiethanolamine, isoamyl dimethylaminobenzoate, isoamyl diethylaminobenzoate, methyl diethylaminobenzoate, ethyl diethylaminobenzoate, isoamyl diethylaminobenzoate, 3-phenyl-5-benzoylthiotetrazole, and 1-phenyl-5-ethoxycarbonylthiotetrazole.
[0076] When a sensitizer is added, the content thereof is preferably 0.1% by mass or more of the printing ink, more preferably 1% by mass or more, and even more preferably 3% by mass or more, since the printing ink can obtain good sensitivity, and is preferably 20% by mass or less of the active energy ray-curable lithographic printing ink, more preferably 15% by mass or less, and even more preferably 10% by mass or less, since the storage stability of the active energy ray-curable lithographic printing ink is improved.
[0077] The ink of the present invention preferably contains a polymerization inhibitor. Specific examples of the polymerization inhibitor include hydroquinone, a monoester of hydroquinone, N-nitrosodiphenylamine, phenothiazine, pt-butylcatechol, N-phenylnaphthylamine, 2,6-di-t-butyl-p-methylphenol, chloranil, pyrogallol, etc. When a polymerization inhibitor is added, the content is preferably 0.001% by mass or more of the active energy ray-curable lithographic printing ink because the active energy ray-curable lithographic printing ink can obtain good storage stability, and is preferably 5% by mass or less because good sensitivity can be obtained.
[0078] The printing ink of the present invention may contain one or more components selected from silicone fluid, alkyl (meth)acrylate, vegetable oil, fatty acid ester derived from vegetable oil, hydrocarbon solvent, and fluorocarbon, and in particular may contain one or more components selected from silicone fluid, alkyl (meth)acrylate, hydrocarbon solvent, and fluorocarbon.
[0079] The above-mentioned components have the effect of reducing ink adhesion to the silicone rubber, which is the non-printing area of a waterless lithographic printing plate. The reason for the reduction in ink adhesion to silicone rubber is presumed to be as follows. That is, the above-mentioned components contained in the ink diffuse from the ink upon contact with the silicone rubber surface, and cover the silicone rubber surface in the form of a thin film. It is presumed that the thin film thus formed prevents the ink from adhering to the silicone rubber surface, and prevents scumming on the silicone rubber surface.
[0080] Among the above-mentioned components, alkyl (meth)acrylate is preferable because it cures when irradiated with active energy rays, and therefore improves the water resistance of the cured ink film and at the same time improves the sensitivity to active energy rays. Specific compounds of the above-mentioned components are as follows.
[0081] Examples of silicone liquids include dimethyl silicone, methyl phenyl silicone, alkyl modified silicone, polyether modified silicone, aralkyl modified silicone, fatty acid amide modified silicone, fatty acid ester modified silicone, fluoroalkyl modified silicone, methyl hydrogen silicone, silanol modified silicone, alcohol modified silicone, amino modified silicone, epoxy modified silicone, epoxy polyether modified silicone, phenol modified silicone, carboxy modified silicone, and mercapto modified silicone.
[0082] Examples of the alkyl (meth)acrylate include nonyl (meth)acrylate, decyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate, tridecyl (meth)acrylate, tetradecyl (meth)acrylate, pentadecyl (meth)acrylate, hexadecyl (meth)acrylate, heptadecyl (meth)acrylate, octadecyl (meth)acrylate, isooctadecyl (meth)acrylate, etc. The alkyl group of the alkyl (meth)acrylate preferably has 5 to 24 carbon atoms, more preferably 6 to 21 carbon atoms.
[0083] Examples of vegetable oils include soybean oil, linseed oil, safflower oil, tung oil, tall oil, and dehydrated castor oil.
[0084] Examples of fatty acid esters derived from vegetable oils include alkyl esters of fatty acids having an alkyl main chain of about 15 to 20 carbon atoms, such as stearic acid, isostearic acid, hydroxystearic acid, oleic acid, linoleic acid, linolenic acid, and eleostearic acid, and the like, having an alkyl chain of about 1 to 10 carbon atoms, such as methyl, ethyl, propyl, isopropyl, butyl, isobutyl, tert-butyl, and 2-ethylhexyl.
[0085] Examples of the hydrocarbon solvent include polyolefin oil, naphthenic oil, and paraffin oil.
[0086] Fluorocarbons include 1,1,1,2,2-pentafluoroethane, 1,1,1,2,2,3,3,4,4-nonafluorobutane, 1,1,1,2,2,3,3,4,4,5,5,6,6-tridecafluorohexane, 1,1,1,2,2,3,3,4,4,5,5,6,6,7,7,8,8-heptadecafluorooctane, 1,1,1,2,3,3,3-heptafluoropropane, Examples of the fluoroalkyl groups include 1,1,1,2,3,3,4,4-octafluoro-2-trifluoromethylbutane, 1,1,1,2,3,3,4,4,5,5,6,6-dodecafluoro-2-trifluoromethylhexane, 1,1,2,2-tetrafluoroethane, 1,1,2,2,3,3,4,4-octafluorobutane, and 1,1,2,2,3,3,4,4,5,5,6,6-dodecafluorohexane.
[0087] The printing ink of the present invention preferably contains at least one component selected from the silicone liquid, vegetable oil, fatty acid ester derived from vegetable oil, hydrocarbon solvent, and fluorocarbon in an amount of at least 0.5% by mass in order to improve the smear resistance. More preferably, it contains at least 1% by mass, and even more preferably, it contains at least 2% by mass. In addition, the printing ink of the present invention preferably contains at most 10% by mass in order to improve the storage stability of the active energy ray-curable lithographic printing ink. More preferably, it contains at most 8% by mass, and even more preferably, it contains at most 5% by mass.
[0088] The printing ink of the present invention preferably contains a pigment dispersant to enhance the dispersibility of the pigment. The optimal content varies depending on the density, particle size, surface area, etc. of the pigment used, but the pigment dispersant acts on the surface of the pigment and suppresses the aggregation of the pigment. This enhances the pigment dispersibility and improves the flowability of the active energy ray-curable lithographic printing ink.
[0089] Specific examples of the pigment dispersant include "Anti-Terra-U", "Anti-Terra-203 / 204", "Disperbyk-101, 102, 103, 106, 107, 110, 111, 115, 118, 130, 140, 142, 145, 161, 162, 163, 164, 165, 166, 167, 168, 170, 171, 174, 180, 181, 182, 184, 185, 187, 190, 191, 192, 193, 194, 195, 196, 197, 198, 199, 200, 201, 202, 203, 204, 205, 206, 207, 208, 209, 300, 309, 310, 311, 312, 313, 314, 315, 316, 317, 318, 319, 320, 321, 322, 323, 324, 325, 326, 327, 328, 329, 330, 331, 332, 333, 334, 335, 336, 337, 338, 339, 340, 341, 342, 343, 344, 345, 346, 347, 348, 349, 350, 351, 9, 2000, 2001, 2008, 2009, 2010, 2012, 2013, 2015, 2022, 2025, 2026, 2050, 2055, 2060, 2061, 2070, 2096, 2150, 2151, 2152, 2155, 2163, 2164, 2200, 2205, 9067, 9076, "Bykumen", "BYK-P104, P105", "P104S, 240S", and "Lactimon".
[0090] "Bykumen" and "Lactimon" are registered trademarks.
[0091] Other examples include Efka 44, 46, 47, 48, 49, 54, 63, 64, 65, 66, 71, 701, 764, 766, and Efka Polymer 100, 150, 400, 401, 402, 403, 450, 451, 452, 453, and 745 manufactured by Efka Chemicals; Flowlen TG-710, Flownon SH-290, SP-1000, and Polyflow No. 50E and No. 300 manufactured by Kyoeisha Chemical; and Disparlon 325, KS-860, 873SN, 874, 1401, #2150, and #7004 manufactured by Kusumoto Chemicals.
[0092] "EFKA", "Florent", "Floron" and "Disparlon" are registered trademarks.
[0093] Further examples include "Demol RN, N, MS, C, SN-B, EP", "Homogenol L-18", "Emulgen 920, 930, 931, 935, 950, 985", and "Acetamine 24, 86" manufactured by Kao Corporation, "Solsperse 5000, 13940, 17000, 24000GR, 32000, 33000, 39000, 41000, 53000" manufactured by Avecia, and "Ajisper PB821, 822, 824" manufactured by Ajinomoto Fine-Techno Co., Ltd.
[0094] "Demol," "Homogenol," "Emulgen," "Acetamine," "Solsperse," and "Ajisper" are registered trademarks.
[0095] The content of the pigment dispersant is preferably from 5% by mass to 50% by mass with respect to the pigment, since this improves the fluidity of the active energy ray-curable lithographic printing ink.
[0096] The printing ink of the present invention may contain additives such as wax, antifoaming agent, transfer improver, leveling agent, etc., as required.
[0097] The viscosity of the printing ink of the present invention is measured at 35°C using a cone-plate type rotational viscometer. In the cone-plate type rotational viscometer, the shape of the cone and plate is such that the apex of the cone is in vertical point contact with the flat plate surface. A measurement sample is sandwiched between the cone and the plate surface, and the viscosity is measured based on the torque applied to the cone when the cone rotates.
[0098] The viscosity (A) at a rotation speed of 0.5 rpm is preferably 5 Pa·s or more and 100 Pa·s or less. When the viscosity (A) is 5 Pa·s or more, the ink tends to exhibit good transferability between rollers. It is more preferably 10 Pa·s or more, and even more preferably 20 Pa·s or more. Furthermore, when the viscosity (A) is 100 Pa·s or less, the ink has good fluidity and, in the case of a white ink in particular, the hiding power is improved. It is more preferably 80 Pa·s or less, and even more preferably 60 Pa·s or less.
[0099] Furthermore, the viscosity (B) at a rotation speed of 50 rpm is preferably 10 Pa·s or more and 40 Pa·s or less. By having the viscosity (B) of 10 Pa·s or more, it is possible to improve the smear resistance of the ink. It is more preferably 15 Pa·s or more, and even more preferably 20 Pa·s or more. By having the viscosity (B) of 40 Pa·s or less, it is possible to improve the transferability of the ink to the lithographic printing plate (the ink adhesion to the image area). It is more preferably 35 Pa·s or less, and even more preferably 30 Pa·s or less.
[0100] Furthermore, the viscosity (C) at a rotation speed of 20 rpm is preferably 10 Pa·s or more and 40 Pa·s or less. By having the viscosity (C) of 10 Pa·s or more, it is possible to improve the smear resistance of the ink. It is more preferable that the viscosity (C) is 15 Pa·s or more, and even more preferable that the viscosity is 20 Pa·s or more. By having the viscosity (C) of 40 Pa·s or less, it is possible to improve the transferability of the ink to the lithographic printing plate (the ink adhesion to the image area). It is more preferable that the viscosity is 35 Pa·s or less, and even more preferable that the viscosity is 30 Pa·s or less.
[0101] The viscosity ratio (B) / (A), which is the ratio of the viscosity (A) to the viscosity (B), is preferably 0.25 or more and 0.4 or less, more preferably 0.30 or more and 0.4 or less, and even more preferably 0.35 or more and 0.4 or less. When the viscosity ratio (B) / (A) is within the above range, it is possible to achieve both smear resistance and fluidity of the ink, and when the ink is used, a high-quality printed matter with a smooth image area and no smear can be obtained.
[0102] The viscosity ratio (B) / (C), which is the ratio of the viscosity (B) to the viscosity (C), is preferably 0.60 or more and 1.00 or less, more preferably 0.70 or more and 1.00 or less, and even more preferably 0.80 or more and 1.00 or less. When the viscosity ratio (B) / (C) is within the above range, stable performance is exhibited over a wide range of printing speeds and printing conditions, and good quality printed matter can be obtained without scumming.
[0103] The printing ink of the present invention preferably contains a surfactant. When the active energy ray-curable lithographic printing ink contains a surfactant, for example, during water-based lithographic printing, an appropriate amount of dampening water (generally said to be 10 to 20% by mass of the total amount of ink) is incorporated and emulsified, thereby increasing the repellency of non-printing areas against dampening water and improving the scumming resistance of the ink.
[0104] The ratio of hydrophilic groups to hydrophobic groups in the surfactant is represented by the HLB value. The HLB value here is a value that indicates the degree of affinity of the surfactant for water and oil, and takes values from 0 to 20, with the closer to 0 the higher the lipophilicity, and the closer to 20 the higher the hydrophilicity. The HLB value of the surfactant is preferably 8 or more, and more preferably 10 or more, since it dissolves water. Also, it is preferably 18 or less, and more preferably 16 or less, since it dissolves in the active energy ray-curable lithographic printing ink.
[0105] Specific examples of the surfactant include polyoxyethylene alkyl ether, polyoxyethylene lauryl ether, polyoxyethylene oleyl ether, polyoxyethylene stearyl ether, polyoxyethylene cetyl ether, polyoxyethylene palmitic ether, polyoxypropylene alkyl ether, polyoxypropylene lauryl ether, polyoxypropylene oleyl ether, polyoxypropylene stearyl ether, polyoxypropylene cetyl ether, polyoxypropylene palmitic ether, polyoxyalkylene alkyl ether, polyoxyalkylene lauryl ether, polyoxyalkylene oleyl ether, polyoxyalkylene stearyl ether, polyoxyalkylene cetyl ether, polyoxyalkylene palmitic ether, and mono-, di- and tri-sorbitol sorbitan acid. mono-, di-, and trialkyl ethers of polyoxyethylene sorbitan acid, mono-, di-, and trilauryl ethers of sorbitan acid, mono-, di-, and trioleyl ethers of sorbitan acid, mono-, di-, and tristearyl ethers of sorbitan acid, mono-, di-, and tricetyl ethers of sorbitan acid, mono-, di-, and tripalmitin ethers of sorbitan acid, mono-, di-, and trialkyl ethers of polyoxyethylene sorbitan acid, mono-, di-, and trilauryl ethers of polyoxyethylene sorbitan acid, mono-, di-, and trioleyl ethers of polyoxyethylene sorbitan acid, mono-, di-, and tristearyl ethers of polyoxyethylene sorbitan acid, mono-, di-, and tricetyl ethers of polyoxyethylene sorbitan acid, mono-, di-, and tripalmitin ethers of polyoxyethylene sorbitan acid, and polyether-modified silicone oils, and those having an HLB value of 8 or more and 18 or less are preferably used.
[0106] When the printing ink of the present invention is used for water-based lithographic printing, the content of the surfactant in the ink is preferably 0.01% by mass or more, more preferably 0.05% by mass or more, and even more preferably 0.1% by mass or more, so that the dampening water is absorbed and the emulsified state is stabilized. Also, the content is preferably 5% by mass or less, more preferably 3% by mass or less, and even more preferably 1% by mass or less, so that the printing ink does not absorb too much dampening water during printing and become miscible with the dampening water.
[0107] The printing ink of the present invention preferably has an ink tack value of 5.0 or more in order to maintain ink transferability to a printing substrate. Also, in order to obtain a printed matter with excellent positional accuracy, the ink tack value is preferably 18.0 or less, more preferably 15.0 or less, and even more preferably 12.0 or less. The ink tack value is an index representing the viscosity of the ink, and is measured by an inkometer.
[0108] The printing ink of the present invention has the excellent effect of exhibiting good adhesion to plastic films and not losing its adhesion performance even during hot water treatment, and therefore overcomes the problem of conventional active energy ray-curable lithographic printing inks that lack adhesion between the ink and the surface of a substrate such as a plastic film. In other words, the printing ink of the present invention can be suitably used as an active energy ray-curable lithographic printing ink.
[0109] The method for producing the printing ink of the present invention will now be described.
[0110] The printing ink of the present invention can be obtained by dissolving (a) a urethane acrylate, (b) a resin such as a resin having an ethylenically unsaturated group and a hydrophilic group, (c) a polymerizable monomer, preferably a pigment, and other components by heating at 5 to 100°C as necessary, and then homogeneously mixing and dispersing the mixture with a stirrer or kneader such as a kneader, a three-roll mill, a ball mill, a planetary ball mill, a bead mill, a roll mill, an attritor, a sand mill, a gate mixer, a paint shaker, a homogenizer, or a planetary stirrer. After mixing and dispersing, or during the mixing and dispersing process, degassing is preferably performed under vacuum or reduced pressure conditions.
[0111] A method for producing a printed matter using the printing ink of the present invention will now be described. First, a printed matter having an ink coating film can be obtained by applying the printing ink of the present invention to a substrate to be printed by a lithographic printing method.
[0112] Examples of the substrate include art paper, coated paper, cast paper, synthetic paper, newsprint, aluminum-deposited paper, metal, and plastic film. However, since the printing ink of the present invention has excellent transferability to plastic film, it is preferable to use plastic film as the substrate. Also, plastic film laminated paper in which a plastic film is laminated on paper, and metal-deposited plastic film in which metal such as aluminum, zinc, and copper is deposited on plastic can be preferably used. Examples of the plastic film include polyethylene terephthalate, polyethylene, polyester, polyamide, polyimide, polystyrene, polypropylene, polycarbonate, and polyvinyl acetal. Among them, at least one selected from the group consisting of polypropylene, polyethylene, polyester, and polyamide, particularly polypropylene, is preferable because it shows good transferability of the ink of the present invention.
[0113] In order to impart easy adhesion to these plastic films, it is preferable to subject the films to surface treatment such as coating with a primer resin, corona discharge treatment, or plasma treatment.
[0114] In the method for producing a printed matter according to the present invention, it is preferable to use a substrate having a nitrogen element concentration of 0.5 atomic % or more and 10.0 atomic % or less on the printed surface side of the substrate. The nitrogen element concentration is preferably 0.5 atomic % or more because the functional group derived from a compound containing nitrogen atoms such as an amino group present on the substrate surface can improve the transferability of the ink and the adhesion between the ink and the substrate by intermolecular forces such as hydrogen bonds between the resin having a hydrophilic group in the ink and the polyfunctional (meth)acrylate. In addition, the nitrogen element concentration is preferably 10.0 atomic % or less in order to prevent yellowing due to exposure to active energy rays or long-term exposure to ultraviolet rays.
[0115] In the present invention, the nitrogen element concentration on the substrate surface is the average nitrogen element concentration on the substrate surface, and can be measured by a general composition analysis method such as X-ray photoelectron spectroscopy (XPS) or Rutherford backscattering analysis (RBS). A preferred analysis method is X-ray photoelectron spectroscopy, in which the excitation X-ray is monochromatic Al Kα1,2 ray, the X-ray diameter is 200 μm, and the photoelectron escape angle, i.e., the inclination of the detector relative to the film surface, is 45° or 60°. The inclination of the detector can be appropriately selected depending on the film thickness of the easy-adhesion layer described later.
[0116] In the method for producing a printed matter of the present invention, it is preferable that the substrate has an easy-adhesion layer containing an organic substance on the surface of the printed side. The transferability of the ink and the adhesion between the ink and the substrate are improved by intermolecular forces such as hydrogen bonds between the functional groups derived from the organic substance in the easy-adhesion layer and the resin having an acidic group in the ink and the polyfunctional (meth)acrylate.
[0117] The easy-adhesion layer preferably contains at least one compound selected from amines, amides, isocyanates, and urethanes. Among them, it is preferable to have at least a urethane structure, since the presence of a urethane bond forms a hard segment in the easy-adhesion layer, which allows the formation of a coating film with high cohesive strength, and the hydrogen bond strength of the urethane bond can improve the adhesion to the ink.
[0118] Examples of the amines in the easy-adhesion layer include ethylenediamine, propylenediamine, hexamethylenediamine, phenylenediamine, tolylenediamine, diphenyldiamine, diaminodiphenylmethane, diaminodiphenylmethane, diaminocyclohexylmethane, ethylenediaminetetraacetic acid, N,N-dimethylaminoethyl (meth)acrylate, N,N-diethylaminoethyl (meth)acrylate, N,N-dimethylaminopropyl (meth)acrylate, and other N,N-dialkylaminoalkyl (meth)acrylates, 2-(methacryloyloxy)ethyl trimethylammonium chloride, 2-(methacryloyloxy)ethyl Examples of the acryloyloxyalkyl trialkyl ammonium salts include trimethylammonium bromide and 2-(methacryloyloxy)ethyl trimethylammonium dimethyl phosphate, (meth)acryloylaminoalkyl trialkyl ammonium salts such as methacryloylaminopropyl trimethylammonium chloride and methacryloylaminopropyl trimethylammonium bromide, tetraalkyl (meth)acrylates such as tetrabutylammonium (meth)acrylate, and trialkylbenzylammonium (meth)acrylates such as trimethylbenzylammonium (meth)acrylate.
[0119] Examples of the amides in the easy-adhesion layer include aliphatic amides such as ethylene bisstearic acid amide and hexamethylene bisstearic acid amide, and N,N-dialkylaminoalkyl (meth)acrylamides such as N,N-dimethylaminoethyl (meth)acrylamide, N,N-diethylaminoethyl (meth)acrylamide, and N,N-dimethylaminopropyl (meth)acrylamide. Examples of isocyanates include tolylene diisocyanate, diphenylmethane-4,4'-diisocyanate, meta-xylylene diisocyanate, hexamethylene-1,6-diisocyanate, 1,6-diisocyanatehexane, an adduct of tolylene diisocyanate and hexanetriol, an adduct of tolylene diisocyanate and trimethylolpropane, polyol-modified diphenylmethane-4,4'-diisocyanate, carbodiimide-modified diphenylmethane-4,4'-diisocyanate, isophorone diisocyanate, 1,5-naphthalene diisocyanate, 3,3'-bitrylene-4,4' diisocyanate, 3,3'dimethyldiphenylmethane-4,4'-diisocyanate, and metaphenylene diisocyanate.
[0120] Examples of isocyanates in the easy-adhesion layer include aromatic diisocyanates such as tolylene diisocyanate and diphenylmethane-4,4-diisocyanate, aromatic aliphatic diisocyanates such as xylylene diisocyanate, alicyclic diisocyanates such as isophorone diisocyanate, 4,4-dicyclohexylmethane diisocyanate, and 1,3-bis(isocyanatemethyl)cyclohexane, aliphatic diisocyanates such as hexamethylene diisocyanate and 2,2,4-trimethylhexamethylene diisocyanate, and polyisocyanates in which one or more of these compounds are added to trimethylolpropane or the like in advance. These may be used alone or in combination of two or more. For example, the surface layer containing an amine compound and an isocyanate compound includes a case in which an amine group and an isocyanate group are present in one compound.
[0121] As the urethane in the easy-adhesion layer, for example, one obtained by a known polymerization method of a polyol and an isocyanate compound may be used. The constituent components include at least a polyol and an isocyanate compound, and may further include a chain extender as necessary. Examples of polyols include polyester polyols obtained by reacting polyvalent carboxylic acids (e.g., malonic acid, succinic acid, adipic acid, sebacic acid, fumaric acid, maleic acid, terephthalic acid, isophthalic acid, etc.) or their acid anhydrides with polyhydric alcohols (e.g., ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, butanediol, 1,3-butanediol, 1,4-butanediol, 2,3-butanediol, neopentyl glycol, 1,6-hexanediol, etc.), polyethylene glycol, polypropylene glycol, polyethylene propylene glycol, polytetramethylene ether glycol, polyhexamethylene ether glycol, and other polyether polyols, polycarbonate polyols, polyolefin polyols, and acrylic polyols.
[0122] The content of amines, amides, isocyanates and urethanes contained in the easy-adhesion layer is not particularly limited, but when the entire easy-adhesion layer is taken as 100 mass%, it is preferably 0.1 mass% or more and 80 mass% or less, more preferably 1.0 mass% or more and 50 mass% or less, and particularly preferably 5 mass% or more and 20 mass% or less.
[0123] The easy-adhesion layer may further contain a resin component. The resin component is not particularly limited as long as it has adhesiveness to the substrate, but for example, polyester, polycarbonate, epoxy resin, alkyd resin, acrylic resin, urea resin, etc. can be suitably used. Polyester and acrylic resin are preferred, and polyester having a phthalic acid skeleton is particularly preferred. The above-mentioned urethanes may also be included as urethane resins. Two or more different resins may also be used in combination.
[0124] The easy-adhesion layer may appropriately contain various additives such as a crosslinking agent, a plasticizer, a heat stabilizer, a weather stabilizer, organic or inorganic fine particles, a wax agent, an antioxidant, a weathering agent, an antistatic agent, a pigment, etc., within a range that does not impair the properties as a film. Examples of the crosslinking agent that can be used include a melamine-based crosslinking agent, an aziridine-based crosslinking agent, an epoxy-based crosslinking agent, a methylolated or alkylolated urea-based crosslinking agent, an acrylamide-based crosslinking agent, a polyamide-based crosslinking agent, an oxazoline-based crosslinking agent, a carbodiimide-based crosslinking agent, an isocyanate-based crosslinking agent, various silane coupling agents, and various titanate-based coupling agents.
[0125] The thickness of the easy-adhesion layer can be adjusted appropriately according to the optical properties and productivity, but is preferably 10 nm or more and 5000 nm or less. More preferably, it is 50 nm or more and 3000 nm or less, and particularly preferably, it is 100 nm or more and 1000 nm or less. When the thickness is 10 nm or more, it is possible to uniformly coat the substrate without defects, and uniform adhesion can be imparted. Also, when the thickness is 5000 nm or less, adverse effects on optical properties can be reduced.
[0126] When used for flexible packaging, the thickness of the substrate is preferably 5 μm or more, more preferably 10 μm or more, in terms of the mechanical strength of the substrate required for printing, and is preferably 50 μm or less, more preferably 30 μm or less, in order to reduce the cost of the substrate.
[0127] The printing ink of the present invention can be applied to a substrate by well-known methods such as flexographic printing, offset printing, gravure printing, screen printing, and bar coater. Planographic printing is particularly preferred, and there are two types of planographic printing: water-based printing and waterless printing. Waterless printing does not use dampening water, so high-resolution patterns can be printed because the reproducibility of printing dots is good, and it is a printing method with excellent environmental impact. As the substrate, either sheets or roll films can be used. When printing on thin films for flexible packaging, it is preferable to use roll films and print by roll-to-roll printing.
[0128] A waterless plate coated with silicone rubber can be used as the lithographic plate used when printing the printing ink of the present invention. The amount of this silicone rubber layer formed before development is 2.6 g / m2 in order to obtain good resistance to scumming and printing durability that enables printing of a large number of processed quantities with one plate. 2 More than 3.0 g / m is preferable. 2 More preferably, the thickness is 8.0 g / m or more to obtain good image reproducibility. 2 Less than 6.5 g / m is preferred 2 The following is more preferable: When the coating amount of the silicone rubber layer is within the above range, a large amount of printing can be performed without scumming, and printed matter with good image reproducibility can be obtained.
[0129] The thickness of the ink coating (cured ink film) on the printed matter is preferably 0.1 to 50 μm. By keeping the thickness of the ink coating within this range, it is possible to reduce the ink cost while maintaining good print quality.
[0130] The method may further include a step of irradiating the ink coating film printed on the substrate with active energy rays after transferring the ink to the substrate to be printed. By irradiating active energy rays, the ink coating film on the printed matter can be instantly cured. As the active energy rays, any ray having the excitation energy required for the curing reaction can be used, and for example, ultraviolet rays and electron beams are preferably used. When electron beams are used, the coating film can be cured without adding a photopolymerization initiator to the ink, so that it is particularly suitable for applications in which migration of low molecular weight compounds to the contents, such as pharmaceutical packaging and food packaging, is to be avoided. When curing with electron beams, an electron beam device having an energy beam of 100 to 500 keV is preferably used.
[0131] The amount of electron beam irradiation is preferably 5 kGy or more, more preferably 10 kGy or more, and even more preferably 20 kGy or more in order to ensure good curing of the ink coating film. In addition, in order to prevent deterioration and discoloration of the printing substrate due to electron beam irradiation, it is preferably 80 kGy or less, more preferably 50 kGy or less. The acceleration voltage that contributes to the penetration depth of the electron beam is preferably 80 kV or more and 300 kV or less.
[0132] When curing with ultraviolet light, ultraviolet irradiation devices such as high-pressure mercury lamps, xenon lamps, metal halide lamps, light-emitting diodes (LEDs), etc. are preferably used. From the viewpoints of power saving and cost reduction, it is preferable to use light-emitting diodes that emit emission lines with wavelengths of 350 to 420 nm.
[0133] The printed matter of the present invention preferably includes at least a substrate, the printing ink of the present invention, an adhesive, and a heat-melting film called a sealant film. The sealant film is not particularly limited, but examples thereof include a non-oriented polypropylene film (CPP) or a linear low-density polyethylene film (LLDPE) having a thickness of 20 to 120 μm. The sealant film has a role of forming a pouch into which contents are put by heat-sealing the periphery of the printed matter in a state in which the sealant film faces the printed matter to form a bag. In addition, by appropriately selecting the material and thickness of the sealant film, it is possible to protect the contents and maintain physical properties that can withstand subsequent processes.
[0134] The printed laminate may include a hot water treatment step after the formation of the laminate. Examples of the hot water treatment step include boiling treatment, which is generally performed under a normal pressure environment at 100°C or less, and retort treatment, which is performed under a pressurized environment at 100°C or more. Retort treatment is often performed under a pressurized environment at 120°C. Conventionally, such a hot water treatment step may reduce the adhesive strength between the substrate and the printing ink, but the printing ink of the present invention can provide a printed matter whose adhesive performance does not decrease even during hot water treatment. The adhesive strength of the printed matter of the present invention is preferably 1.0N / 15mm or more, more preferably 1.5N / 15mm or more, even more preferably 2.0N / 15mm or more, and even more preferably 3.0N / 15mm or more, or the failure mode is substrate breakage (i.e., substrate breakage occurs before peeling). EXAMPLES
[0135] The present invention will be described in more detail below with reference to examples, although the present invention is not limited to these.
[0136] <Measurement and evaluation methods> (1) Measurement of weight average molecular weight The weight average molecular weight of the resin was measured by gel permeation chromatography (GPC) using tetrahydrofuran as the mobile phase. The GPC used was HLC-8220 (Tosoh Corporation), and the columns were TSKgel SuperHM-H (Tosoh Corporation), TSKgel SuperHM-H (Tosoh Corporation), and TSKgel SuperH2000 (Tosoh Corporation), connected in this order, and RI detection was performed using an RI detector built into the GPC. A calibration curve was created using polystyrene standard material, and the weight average molecular weight of the sample was calculated. The method for preparing the measurement sample will be described below. The sample was diluted with tetrahydrofuran so that the concentration was 0.25% by mass, and the diluted solution was stirred at 100 rpm for 5 minutes in a mix rotor (MIX-ROTAR VMR-5, manufactured by AS ONE Corporation) to dissolve the sample, and then filtered through a 0.2 μm filter (Z227536-100EA, manufactured by SIGMA Corporation), and the filtrate was used as the measurement sample. The measurement conditions are as follows: The injection volume was 10 μL, the analysis time was 30 minutes, the flow rate was 0.4 mL / min, and the column temperature was 40° C.
[0137] (2) Adhesion evaluation The ink was applied to the substrate film at a coating amount of 1 g / m using an RI tester PI-600 (manufactured by Tester Sangyo Co., Ltd.). 2 The ink was transferred so that the ink cured film was formed as shown in FIG. 1, and an electron beam was irradiated at a belt conveyor speed of 9 m / min using an electron beam irradiation device EC250 / 30 / 90LS (accelerating voltage 125 kV, irradiation dose 30 kGy) manufactured by Iwasaki Electric Co., Ltd., to obtain a substrate film having an ink cured film. When the electron beam irradiation dose was less than 5 kGy, tack remained in the cured film due to insufficient curing of the ink, and when the electron beam irradiation dose was more than 80 kGy, yellowing of the substrate film was observed. Takelac A-626 / Takenate A-65 (mixed at a mass ratio of 16 / 1, both manufactured by Mitsui Chemicals, Inc.) was applied as an adhesive onto the ink cured film by a bar coat method, and after drying at 80°C for 1 minute, the coating amount was 4.0 g / m 2 The substrate film coated with the adhesive was laminated with a linear low-density polyethylene LL-XHT50 (manufactured by Futamura Chemical Co., Ltd., thickness 50 μm) as a sealant using a hand roller, and then aged at 40° C. for 72 hours to obtain a film laminate of sealant / adhesive / cured ink film / substrate film. "Takelac" and "Takenate" are registered trademarks.
[0138] Two sheets of the film laminate (10 cm x 10 cm square) were prepared and stacked so that the sealants were in contact with each other, and then a heat sealer TP-701-B (manufactured by Tester Sangyo Co., Ltd.) was used to seal three of the four sides at a heater temperature of 180°C, a pressure of 0.1 MPa, and a time of 1.0 second to produce a bag with one side open. 50 ml of pure water was poured into this bag, and the air was sufficiently removed, and the remaining side was sealed with the sheet sealer to obtain a pouch formed of the film laminate with pure water inside.
[0139] The pouch was placed in a water bath set to 95° C. and subjected to hot water treatment for 30 minutes. After the hot water treatment, the sealed portion of the pouch was cut off and the water inside was removed to obtain a film laminate after hot water treatment.
[0140] For the film laminate before and after the hot water treatment, a piece 15 mm wide and 50 mm long was cut out. Using a Tensilon universal material testing machine (manufactured by A&D, model number "RTG-1210"), the base film and sealant were clamped between the top and bottom chucks to measure the peel strength using the 90 degree T-type peel method (JIS K 6854-3), and the load value at the first maximum point was taken as the laminate peel strength. The test environment was a temperature of 25°C and humidity of 50%, and the test speed was 300mm / min. The main failure mode in each Example and Comparative Example was interfacial peeling between the substrate film and the ink, but cases in which the substrate broke are marked with an asterisk ("*") in the table.
[0141] (3) Compatibility The appearance of the coating liquid when the urethane (meth)acrylate described in each Example and Comparative Example was added to the resin varnish obtained from the resin, polymerizable monomer 1, polymerizable monomer 2, and polymerization inhibitor described in each Example and Comparative Example in the formulation described in each Example and Comparative Example was evaluated as follows: SS for completely transparent and very good, S for transparent and good, A for almost transparent and good, B for slightly cloudy but no problem for practical use, and C for cloudy.
[0142] (4) Viscosity The viscosity of the ink was measured at 35°C using a cone-plate type rotational viscometer with a cone diameter of 40 mm and an inclination angle of 1.0°.
[0143] (5) Coating appearance The appearance of the coating on the printed matter was visually evaluated using an RI tester PI-600 (manufactured by Tester Sangyo Co., Ltd.). Those without any defects in appearance such as uneven printing were rated as A, those with some defects in appearance but no practical problems were rated as B, and those with significant defects in appearance were rated as C.
[0144] (6) Tack value 1.3 ml of the prepared ink was applied to the roller of an inkmeter INKOGRAPH TYPE-V (manufactured by Tester Sangyo Co., Ltd.), which was operated at a roller temperature of 38° C. and a rotation speed of 400 rpm, and the tack value was measured after 1 minute.
[0145] (7) Resistance to staining 0.5 g of the ink of each Example and Comparative Example was placed on the roller of an RI tester PI-600 (manufactured by Tester Sangyo Co., Ltd.) and transferred to the non-image area of a waterless lithographic printing plate TAC-VG-5 (manufactured by Toray Industries, Inc.). The transferred ink was then transferred to white coated paper, and the color density was measured using a reflection densitometer SpectroEye (manufactured by GretagMacbeth). A color density of less than 0.1 was judged to be particularly good in terms of smear resistance (S); 0.1 to less than 0.2 was judged to be good (A); 0.2 to less than 0.3 was judged to be acceptable (B); and 0.3 or more was judged to be C.
[0146] (8) Evaluation of ink transfer A waterless lithographic printing plate (TAC-VG5, Toray Industries, Inc.) with a strip-shaped solid image of 400 mm (printing direction) x 900 mm (printing width direction) in the center of a plate of 854 mm (printing direction) x 1,070 mm (printing width direction) was attached to an offset rotary printing press (CI-8, COMEXI, Inc.), and 1,000 m was printed on polyester film PTM12 (Unitika, thickness 12 μm) using the inks described in the Examples and Comparative Examples at a printing speed of 200 m / min and an ink supply of 50%, and the reflection density of the solid area was evaluated using a reflection densitometer (GretagMacbeth, SpectroEye, Status E) with high-quality paper as the paper white (reflection density 0 as the reference). A higher reflection density of the solid area indicates better transferability.
[0147] (9) Urethane bond fraction Measurements were carried out using proton nuclear magnetic resonance (H-NMR) under the following conditions. Equipment: ECZ600R (manufactured by JEOL Ltd.) Observation frequency: 600MHz Accumulation count: 512 times Temperature: 20℃ Sample composition: 10 mg of urethane acrylate. 1000 mg of N,N-dimethylformamide-d7 (deuterated solvent). 5 mg of 3,5-dinitrobenzoic acid (internal standard).
[0148] The mass of the urethane acrylate in the measurement sample was a (g), the mass of the internal standard was A (g), the signal integral value derived from the NH of the urethane bond when the signal integral value derived from the CH of the internal standard was normalized to 1 was b, and the molecular weights of the urethane bond and the internal standard were 59.0 and 212.1, respectively, and the urethane bond fraction (mass%) was calculated from formula (1).
[0149]
number
[0150] <Base film> The base films shown in the table are as follows. PA: Polyamide film ONM15 (manufactured by Unitika, thickness 15 μm) OPP: Polypropylene film P2111 (Toyobo Co., Ltd., thickness 20 μm) PET: Polyester film (thickness 12 μm) having an easy-adhesion layer containing urethane bonds.
[0151] <Ink raw materials> (Urethane (meth)acrylate) As the urethane (meth)acrylate, a substance having the following composition was used. Urethane acrylate 1: A urethane acrylate consisting of alicyclic diisocyanate (hydrogenated XDI), carboxylic acid (isophthalic acid and adipic acid), polyol, and 2-hydroxyethyl acrylate, with a weight average molecular weight (Mw) of 3,600 and a urethane bond fraction of 8 mass%. Urethane acrylate 2: A urethane acrylate consisting of an aromatic diisocyanate (TDI) and a multifunctional acrylate having a hydroxyl group (pentaerythritol triacrylate), with Mw 850 and a urethane bond fraction of 14 mass%. Urethane acrylate 3: A urethane acrylate consisting of alicyclic diisocyanate (IPDI), polyether polyol (polytetramethylene ether glycol), and 2-hydroxyethyl acrylate, with Mw 3300 and a urethane bond fraction of 15 mass%. Urethane acrylate 4: A urethane acrylate consisting of alicyclic diisocyanate (IPDI), polyether polyol, and 2-hydroxyethyl acrylate, with Mw 13,000 and a urethane bond fraction of 4 mass%. Urethane acrylate 5: A urethane acrylate consisting of alicyclic diisocyanate (IPDI), polyester polyol, and 2-hydroxyethyl acrylate, having Mw 3800 and a urethane bond fraction of 13 mass%. Urethane acrylate 6: A urethane acrylate consisting of alicyclic diisocyanate (IPDI), polyester polyol (polypropylene glycol), and 2-hydroxyethyl acrylate, with Mw 2000 and a urethane bond fraction of 17 mass%. Urethane acrylate 7: A urethane acrylate consisting of alicyclic diisocyanate (IPDI), polyether polyol, and 2-hydroxyethyl acrylate, with Mw 8600 and a urethane bond fraction of 8 mass%.
[0152] (resin) Resin 1: 0.55 equivalents of glycidyl methacrylate was added to the carboxyl groups of a copolymer obtained from 25% by mass of methyl methacrylate, 25% by mass of styrene, and 50% by mass of methacrylic acid to obtain Resin 1 having ethylenically unsaturated groups and hydrophilic groups. The obtained Resin 1 had a weight average molecular weight of 34,000, an acid value of 105 mgKOH / g, and an iodine value of 2.0 mol / kg.
[0153] Resin 2: A resin consisting of a copolymer having neither an ethylenically unsaturated group nor a hydrophilic group, obtained from 25% by mass of methyl methacrylate, 25% by mass of styrene, and 50% by mass of methacrylic acid. The weight average molecular weight was 30,000.
[0154] (Polymerizable monomer) Polymerizable monomer 1: Mixture of pentaerythritol triacrylate and pentaerythritol tetraacrylate "Miramer" (registered trademark) M340 (manufactured by MIWON Co., Ltd.). Contains hydroxyl groups, hydroxyl value 115 mg KOH / g Polymerizable monomer 2: Tricyclodecane dimethanol diacrylate "Miramer" (registered trademark) M262 (manufactured by MIWON). No hydroxyl group, hydroxyl value 0 mg KOH / g Polymerizable monomer 3: 1,6-hexanediol diacrylate (Kyoeisha Chemical Co., Ltd., Light Acrylate 1.6HX-A). No hydroxyl group, hydroxyl value 0 mgKOH / g Polymerizable monomer 4: 1,10-decanediol diacrylate (NK Ester A-DOD-N, manufactured by Shin-Nakamura Chemical Co., Ltd.). No hydroxyl group, hydroxyl value 0 mgKOH / g.
[0155] (Other additives) Polymerization inhibitor: p-methoxyphenol (Wako Pure Chemical Industries, Ltd.) Pigment: Seikacyanine Blue 4920 (manufactured by Dainichi Seika Chemicals Co., Ltd.) Extender pigment: Microace P-8 (manufactured by Nippon Talc Co., Ltd.) Wax: Polytetrafluoroethylene fine powder "KTL-4N" (registered trademark) (manufactured by Kitamura Co., Ltd.).
[0156] [Example 1] The ink composition shown in Table 1, which includes resin, polymerizable monomer 1, polymerizable monomer 2, polymerization inhibitor, pigment, urethane acrylate 1, extender pigment, and wax, was weighed out and passed three times using a triple roll mill "EXAKT" (registered trademark) M-80S (manufactured by EXAKT) with the "gap 1" setting, to obtain a printing ink.
[0157] The obtained printing ink was used to prepare a film laminate before and after hot water treatment as described above, and the adhesion was evaluated. The laminate peel strength was good at 1.8 N / 15 mm before hot water treatment, and was also good at 1.9 N / 15 mm after hot water treatment. The appearance of the coating was good with no abnormalities such as printing unevenness.
[0158] [Examples 2 to 6] Except for changing the composition of the ink as shown in Table 1, the same operation as in Example 1 and the evaluation of adhesion were carried out. By increasing the content of urethane acrylate 1, the laminate peel strength before and after hot water treatment tended to improve compared to Example 1. Furthermore, when the content of resin and urethane acrylate was reduced, the tack tended to decrease. Furthermore, good adhesion was obtained even when a different urethane acrylate 2 was added. The solid part density in the ink transfer evaluation of Example 2 was 1.4.
[0159] [Example 7] Except for changing the composition of the ink as shown in Table 1, the same operation and evaluation of adhesion as in Example 1 were carried out. Example 10 contains polymerizable monomer 3 (1,6-hexanediol diacrylate). The laminate peel strength before hot water treatment was 2.4 N / 15 mm, and after hot water treatment it was 2.6 N / 15 mm, showing very good adhesion. In addition, the solid area density in the ink transfer evaluation was 1.6.
[0160] [Example 8] Except for changing the composition of the ink as shown in Table 1, the same operation and evaluation of adhesion as in Example 1 were carried out. Example 11 contains polymerizable monomer 4 (1,10-decanediol diacrylate). The laminate peel strength before hot water treatment was 2.7 N / 15 mm, and after hot water treatment was 2.7 N / 15 mm, showing very good adhesion. In addition, the solid area density in the ink transfer evaluation was 1.7.
[0161] [Examples 9 to 11] The ink composition was fixed as shown in Table 1, and the film substrates to be printed were polyamide, polypropylene, and polyester, respectively. The same operations and adhesion evaluations as in Example 1 were carried out. Example 9 showed very good adhesion of 3.3 N / 15 mm before hot water treatment and 3.4 N / 15 mm after hot water treatment. Examples 10 and 11 showed particularly good adhesion, with an adhesion higher than 3 N / 15 mm and a failure mode of substrate breakage.
[0162] [Example 12] The same operations and evaluation of adhesion were carried out as in Example 1, except that the ink composition was changed as shown in Table 2. This also showed good adhesion, 1.8 N / 15 mm before hot water treatment and 1.7 N / 15 mm after hot water treatment.
[0163] [Examples 13 to 16] The same operations and evaluation of adhesion as in Example 1 were carried out except that the ink composition was changed as shown in Table 2. Good adhesion was shown for all urethane acrylates.
[0164] [Comparative Example 1] The same operations and evaluation of adhesion as in Example 1 were carried out, except that the ink composition was changed as shown in Table 2. It was found that with the ink not containing urethane acrylate, the laminate peel strength before hot water treatment was insufficient at 1.4 N / 15 mm, and further deteriorated to 0.9 N / 15 mm after hot water treatment.
[0165] [Comparative Example 2] Except for changing the composition of the ink as shown in Table 2, the same operation and evaluation of adhesion were carried out as in Example 1. It was found that the appearance of the coating film and the resistance to smearing were deteriorated in the ink with a low tack of 4.0 and a small ink viscosity ratio (B) / (C) of 0.55. This is thought to be because the tack due to the cohesive force of the ink was not adequately maintained, which deteriorated the ink transferability and impaired the Newtonian properties.
[0166] [Comparative Example 3] Except for changing the ink composition as shown in Table 2, the same operations and adhesion evaluation were carried out as in Example 1. For the ink with a high content of urethane acrylate 1 of 35 mass%, the laminate peel strength before hot water treatment was 3.2 N / 15 mm, and after hot water treatment it was 3.6 N / 15 mm, showing very good adhesion, but it was found that the appearance of the coating film deteriorated. This is thought to be because the tack value of the ink increased significantly due to the high content of urethane acrylate.
[0167] The compositions of the components used in the examples and comparative examples and the evaluation results are shown in Tables 1 and 2.
[0168] [Table 1]
[0169] [Table 2]
[0170] [Examples 17 to 22] Waterless planographic plates were prepared with the following amounts of silicone rubber layer formed before development. After development, the halftone dot image reproducibility was evaluated visually using a loupe at a magnification of 50x. Example 17: 2.6 g / m 2 Example 18: 3.0 g / m 2 Example 19: 4.5 g / m 2 Example 20: 6.0 g / m 2 Example 21: 8.0 g / m 2 Example 22: 9.0 g / m 2 As a result, good image reproducibility was obtained in Examples 20 and 21, and even better image reproducibility was obtained in Examples 17 to 19. In Example 22, dot loss was observed during lithographic development, but this was at a level that was not problematic in practice. Furthermore, when printing durability was evaluated using the printing ink and substrate in Example 9, good printing durability was confirmed in Example 17, and even better printing durability was confirmed in Examples 18 to 22.
Claims
1. A printing ink comprising (a) a urethane (meth)acrylate and (c) another polymerizable monomer, wherein the (c) other polymerizable monomer comprises a hydrophilic polyfunctional (meth)acrylate containing at least a hydroxyl group, the ink having an ink tack value of 5.0 or more and 18.0 or less, and a viscosity (C) at 20 rpm and a viscosity (B) at 50 rpm, both of which are 5 Pa s or more and 100 Pa s or less, as measured at 35°C using a cone-plate type rotational viscometer, and a viscosity ratio (B) / (C) of 0.60 or more and 1.00 or less.
2. The printing ink according to claim 1, further comprising a resin.
3. 3. The printing ink according to claim 2, wherein the acid value of the resin is from 105 mg KOH / g to 250 mg KOH / g.
4. 4. The printing ink according to claim 1, wherein the (a) urethane (meth)acrylate is contained in an amount of 1 to 30% by mass relative to 100% by mass of the ink.
5. The printing ink according to any one of claims 1 to 4, wherein the (a) urethane (meth)acrylate has a weight average molecular weight (Mw) of 500 to 10,000.
6. The printing ink according to any one of claims 1 to 5, wherein the urethane (meth)acrylate (a) has a urethane bond fraction of 5 mass % or more and 40 mass % or less.
7. The printing ink according to any one of claims 1 to 6, wherein the (a) urethane (meth)acrylate has at least an ether structure in a polyol.
8. The printing ink according to any one of claims 2 to 7, wherein the resin is (b) a resin having an ethylenically unsaturated group and a hydrophilic group.
9. 9. The printing ink according to claim 1, wherein the ratio of (a) the urethane (meth)acrylate to (c) the other polymerizable monomers is 3% by mass or more and 40% by mass or less.
10. A method for producing a printed matter by lithographic printing using the printing ink according to any one of claims 1 to 9, comprising a step of transferring the ink to a substrate to be printed and then irradiating the substrate with active energy rays.
11. The method for producing a printed matter according to claim 10 , wherein the base material comprises at least one selected from the group consisting of polypropylene, polyethylene, polyester, and polyamide.
12. The method for producing a printed matter according to claim 10 or 11, wherein the substrate is a plastic film having an easy-adhesion layer containing an organic substance on the surface on the printing side.
13. The method for producing a printed matter according to claim 12 , wherein the easy-adhesion layer has at least a urethane structure.
14. The method for producing a printed matter according to any one of claims 11 to 13, wherein the active energy rays are electron beams or LED-UV rays.
15. A method for producing a printed matter by lithographic printing using the printing ink according to any one of claims 1 to 9, characterized in that a waterless lithographic plate is used as the lithographic plate.
Citation Information
Patent Citations
Ultraviolet-or electron ray-curing type water-free ink for lithography
JP1991252472A
Active energy-curable ink composition for water-free lithographic printing
JP1994172695A
Activating energy ray curing type printing ink
JP1995292304A
Activation-energy ray setting resin composition and coating material
JP1998030012A
Resin composition for active energy ray curing type ink
JP2001348516A