Composite polymer electrolyte membrane, catalyst-layered electrolyte membrane, membrane electrode assembly, and solid polymer electrolyte fuel cell
The composite polymer electrolyte membrane, combining a polymer electrolyte with a porous base material and nonionic fluorosurfactant, addresses the durability issues of existing membranes by improving mechanical stability and reducing proton resistance, thus enhancing fuel cell performance and sustainability.
Patent Information
- Application Number
- JP2020549721
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-09-20
- Filing Date
- 2020-09-11
- Publication Date
- 2024-10-02
- Estimated Expiration
- 2040-09-11
AI Technical Summary
Existing polymer electrolyte membranes in fuel cells suffer from insufficient dry-wet cycle durability due to mechanical properties that degrade under hydration and dehydration cycles, leading to wrinkles, sagging, and rupture, and they are costly and difficult to recycle.
A composite polymer electrolyte membrane is developed by combining a polymer electrolyte with a porous base material, such as a fluorine-based or aromatic hydrocarbon porous substrate, to enhance mechanical properties in both dry and hydrated states, with a nonionic fluorosurfactant improving affinity and durability.
The composite membrane exhibits improved dry-wet cycle durability, mechanical stability, and reduced proton resistance, enhancing fuel cell performance and longevity while being more cost-effective and environmentally friendly.
Smart Images

Figure 0007559556000001 
Figure 0007559556000002 
Figure 0007559556000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a composite polymer electrolyte membrane, a catalyst layer-attached composite polymer electrolyte membrane having catalyst layers sandwiched between both sides of the composite polymer electrolyte membrane, a membrane electrode assembly including the composite polymer electrolyte membrane, and a solid polymer electrolyte fuel cell including the composite polymer electrolyte membrane. [Background technology]
[0002] Fuel cells are a type of power generation device that extracts electrical energy by electrochemically oxidizing fuels such as hydrogen and methanol, and have been attracting attention in recent years as a clean energy supply source. Among them, solid polymer fuel cells have a low standard operating temperature of around 100°C and a high energy density, so they are expected to be used in a wide range of applications as power generation devices for relatively small-scale distributed power generation facilities and mobile objects such as automobiles and ships. They are also attracting attention as power sources for small mobile and portable devices, and are expected to be installed in mobile phones and personal computers, replacing secondary batteries such as nickel-metal hydride batteries and lithium-ion batteries.
[0003] Fuel cells are usually constructed as a unit, with a cell in which a membrane electrode assembly (MEA) is sandwiched between separators. The MEA has catalyst layers on both sides of an electrolyte membrane, and gas diffusion layers on both sides of the catalyst layers. In the MEA, a pair of electrode layers is formed by the catalyst layers and gas diffusion layers arranged on either side of the electrolyte membrane, one of which is the anode electrode and the other is the cathode electrode. Electricity is generated by an electrochemical reaction when a fuel gas containing hydrogen comes into contact with the anode electrode and air comes into contact with the cathode electrode. The electrolyte membrane is mainly composed of a polymer electrolyte material. Polymer electrolyte materials are also used as binders for the catalyst layers.
[0004] Conventionally, fluorine-based polymer electrolyte "Nafion" (registered trademark) (manufactured by Chemours Corporation) has been widely used as a polymer electrolyte material. "Nafion" (registered trademark) exhibits high proton conductivity at low humidification through proton-conducting channels resulting from a cluster structure. On the other hand, "Nafion" (registered trademark) is very expensive because it is manufactured through a multi-stage synthesis, and in addition, there is a problem that fuel crossover is large due to the above-mentioned cluster structure. In addition, under fuel cell operating conditions, dry-wet cycles are repeated, and in particular, the electrolyte membrane repeats swelling and shrinking. At that time, since the electrolyte membrane is restrained by a separator, etc., wrinkles and sagging occur, and the membrane breaks due to local stress concentration, and there is a problem that the mechanical strength and dry-wet cycle durability of the membrane are lost. In addition, problems such as a low softening point and inability to be used at high temperatures, problems with waste disposal after use, and difficulties in recycling materials have been pointed out. In order to overcome such problems, development of inexpensive hydrocarbon-based electrolyte membranes with excellent membrane properties that can replace "Nafion" (registered trademark) has been active in recent years.
[0005] In such solid polymer electrolyte fuel cells, in order to improve the long-term durability of the fuel cell, it is important to improve the mechanical properties of the electrolyte membrane and, in turn, the wet-dry cycle durability. Until now, the electrolyte membrane has had an insufficient wet-dry cycle durability, and as described above, the electrolyte membrane breaks due to wrinkles or slack in the wet-dry cycle, resulting in a loss of wet-dry cycle durability. Therefore, in order to improve the mechanical properties and wet-dry cycle durability of the electrolyte membrane, a composite electrolyte membrane has been proposed in which a polymer electrolyte is composited with a porous substrate such as a nanofiber or a microporous membrane.
[0006] Patent Document 1 describes a membrane in which swelling is suppressed by combining a hydrocarbon-based polymer electrolyte with a nanofiber (hereinafter, NF) nonwoven fabric of polybenzimidazole (hereinafter, PBI). Patent Document 2 describes a membrane in which swelling is suppressed by combining a fluorine-based electrolyte with a soluble PBI NF nonwoven fabric. Patent Document 3 describes a membrane in which proton conductivity and mechanical properties are improved by combining a sulfonated polyimide with an acid-permeated PBI NF nonwoven fabric. Patent Document 4 describes a membrane in which mechanical properties are improved by combining a sulfonated polyarylene with expanded porous polytetrafluoroethylene (ePTFE). [Prior art documents] [Patent documents]
[0007] [Patent Document 1] International Publication No. 2017 / 141878 [Patent Document 2] Special Publication No. 2017-532716 [Patent Document 3] JP 2015-28850 A [Patent Document 4] JP 2005-166557 A Summary of the Invention [Problem to be solved by the invention]
[0008] However, in Patent Document 1, the thickness ratio of the PBI NF nonwoven fabric to the composite polymer electrolyte membrane thickness is small, and the mechanical properties in the water-containing state are insufficient, so that it cannot necessarily be said that the wet-dry cycle durability is excellent. In Patent Document 2, the solvent-soluble PBI NF nonwoven fabric is composited without drying after spinning, and the PBI NF nonwoven fabric swells, deforms, and softens due to the solvent in the film-forming process, so that the mechanical properties in the water-containing state are insufficient and the wet-dry cycle durability is insufficient. In Patent Document 3, the water absorption is increased by permeating the nanofiber nonwoven fabric with an acid, so that the mechanical properties in the water-containing state are insufficient and the wet-dry cycle durability is insufficient. In Patent Document 4, the membrane is formed by permeating ePTFE, which is a hydrophobic and lipophobic compound, and an N-methylpyrrolidone (NMP) solution of polyarylene, which does not contain fluorine atoms and has extremely low affinity with ePTFE, so that the membrane actually has a large amount of voids, and therefore the mechanical properties are insufficient, especially in the water-containing state, and the wet-dry cycle durability is insufficient.
[0009] In view of the above background, the present invention aims to provide an electrolyte membrane which combines a polymer electrolyte with a porous substrate, has good mechanical properties both in a dry state and in a wet state, and can improve the wet / dry cycle durability of a fuel cell. [Means for solving the problem]
[0010] In order to solve the above problems, the composite polymer electrolyte membrane of the present invention has the following configuration. The composite polymer electrolyte membrane comprises a polymer electrolyte and a porous substrate, and has a dry tensile modulus per width of 100 N / cm or more and a wet tensile modulus per width of 35 N / cm or more.
[0011] The catalyst-layered electrolyte membrane of the present invention has the following configuration. The composite polymer electrolyte membrane with a catalyst layer is obtained by sandwiching the composite polymer electrolyte membrane with catalyst layers on both sides.
[0012] The membrane electrode assembly of the present invention has the following configuration. A membrane electrode assembly comprising the above composite polymer electrolyte membrane.
[0013] The polymer electrolyte fuel cell of the present invention has the following configuration. A solid polymer electrolyte fuel cell comprising the above composite polymer electrolyte membrane.
[0014] The polymer electrolyte composite membrane of the present invention preferably has a wet tensile modulus per cross-sectional area of 400 MPa or more.
[0015] The polymer electrolyte composite membrane of the present invention preferably has a wet tensile modulus / dry tensile modulus of 0.3 or more.
[0016] The polymer electrolyte composite membrane of the present invention preferably has a wet tensile elongation at break of 60% or more.
[0017] The polymer electrolyte composite membrane of the present invention preferably has a wet tensile breaking strength of 5 N / cm or more.
[0018] In the polymer electrolyte composite membrane of the present invention, the porous substrate is preferably a fluorine-containing porous substrate.
[0019] In the polymer electrolyte composite membrane of the present invention, the porous substrate preferably has an oxygen atom content of 10 mass % or less.
[0020] In the polymer electrolyte composite membrane of the present invention, the polymer electrolyte is preferably a hydrocarbon polymer having an ionic group.
[0021] The polymer electrolyte composite membrane of the present invention preferably further contains a nonionic fluorine-based surfactant.
[0022] In the composite polymer electrolyte membrane containing the above-mentioned nonionic fluorosurfactant of the present invention, the nonionic fluorosurfactant is preferably a compound having a fluorine-containing group consisting of a fluorinated alkyl group, a fluorinated alkenyl group or a fluorinated aryl group, and a nonionic solvent-philic group.
[0023] In the composite polymer electrolyte membrane of the present invention, the porous substrate is preferably an aromatic hydrocarbon-based porous substrate.
[0024] In the composite polymer electrolyte membrane of the present invention, the porous substrate is preferably a polyazole-based porous substrate.
[0025] In the composite polymer electrolyte membrane of the present invention, the porous substrate is preferably made of polybenzimidazole.
[0026] The polymer electrolyte composite membrane of the present invention preferably has a haze value of 20% or more and 45% or less when a light beam is transmitted through the membrane in the thickness direction.
[0027] The polymer electrolyte composite membrane of the present invention preferably has a diffuse transmittance of 20% or more and 40% or less when a light beam is transmitted through the membrane in the thickness direction. Effect of the Invention
[0028] The electrolyte membrane of the present invention has good mechanical properties both in a dry state and in a wet state, and can improve the dry / wet cycle durability of a fuel cell. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0029] The present invention will be described in detail below. In the following description, the symbol "to" indicates a range including both ends of the symbol.
[0030] <Electrolyte membrane> The electrolyte membrane of the present invention is an electrolyte membrane having a composite layer formed by combining a polymer electrolyte and a porous substrate, and has mechanical properties of a dry tensile modulus per width of 100 N / cm or more and a wet tensile modulus per width of 35 N / cm or more. In fuel cells and the like, two separators are usually compressed using a screw or the like to bring each component into close contact with each other, thereby reducing resistance and improving power generation performance. However, if the dry tensile modulus per width is less than 100 N / cm, the electrolyte membrane is easily deformed and perforated by external forces received from the catalyst layer, gas diffusion layer, etc., resulting in insufficient wet and dry cycle durability. In addition, if the wet tensile modulus per width is less than 35 N / cm, the softening of the electrolyte membrane in a wet state cannot be suppressed, resulting in insufficient wet and dry cycle durability as a fuel cell. As described later, the porous substrate is preferably composed mainly of a hydrophobic compound, and more preferably of a fluorine-based polymer compound having excellent water resistance and chemical resistance. In addition, a porous substrate made of an aromatic hydrocarbon-based polymer compound having hydrophobicity and excellent elastic modulus and breaking strength can also be suitably used. By using a porous substrate mainly composed of a hydrophobic compound, it becomes easier to suppress softening of the electrolyte membrane in a water-containing state and improve the wet tensile modulus. By using a polymer electrolyte membrane having such excellent mechanical properties, it is possible to improve the dry / wet cycle durability of the fuel cell. In the present invention, the dry tensile modulus per width and the wet tensile modulus per width are calculated using the methods described in (15) and (16) in the Examples section, respectively.
[0031] The electrolyte membrane preferably has a wet tensile modulus per width of 40 N / cm or more, more preferably 45 N / cm or more, and even more preferably 48 N / cm or more. If the wet tensile modulus per width is 40 N / cm or more, softening of the electrolyte membrane in a wet state can be suppressed, and the dry-wet cycle durability of the fuel cell can be further improved.
[0032] The electrolyte membrane preferably has a wet tensile modulus per cross-sectional area of 400 MPa or more, more preferably 450 MPa or more, and even more preferably 500 MPa or more. If the wet tensile modulus per cross-sectional area is 400 MPa or more, it is possible to suppress softening of the electrolyte membrane in a wet state, and not only to improve the dry-wet cycle durability of the fuel cell, but also to improve proton conductivity by thinning the electrolyte membrane while maintaining high mechanical properties, thereby reducing the resistance of the fuel cell and improving its output. The wet tensile modulus per cross-sectional area is calculated using the method described in (16) in the Examples section.
[0033] The electrolyte membrane preferably has a wet tensile modulus / dry tensile modulus, i.e., the wet tensile modulus per width divided by the dry tensile modulus per width, of 0.3 or more, more preferably 0.35 or more. If the wet tensile modulus / dry tensile modulus is 0.3 or more, the difference in mechanical properties between the dry state and the wet state becomes small, so that the generation of wrinkles and sagging during wet / dry cycles can be suppressed, and the wet / dry cycle durability of the fuel cell can be improved.
[0034] The electrolyte membrane preferably has a wet tensile breaking elongation of 60% or more, more preferably 100% or more, and even more preferably 140% or more. If the wet tensile breaking elongation is 60% or more, the electrolyte membrane is less likely to break even in a wet state where it is softened, even if it is subjected to stress concentration due to wrinkles or slackness caused by wet-dry cycles, and the wet-dry cycle durability of the fuel cell can be improved. The wet tensile breaking elongation is calculated using the method described in (16) in the Examples section.
[0035] The electrolyte membrane preferably has a wet tensile breaking strength of 5 N / cm or more, more preferably 5.5 N / cm or more, and even more preferably 6 N / cm or more. If the wet tensile breaking strength is 5 N / cm or more, the electrolyte membrane is less likely to break even in a wet state where it is softened, even if it is subjected to stress concentration due to wrinkles or slackness caused by wet-dry cycles, and the wet-dry cycle durability of the fuel cell can be improved. The wet tensile breaking elongation is calculated using the method described in (16) in the Examples section.
[0036] The filling rate of the polymer electrolyte in the composite layer is preferably 50% or more, and more preferably 60% or more. When the filling rate of the composite layer is 50% or more, a continuous proton conductive path is formed in the entire composite polymer electrolyte membrane, thereby improving the power generation performance. The filling rate of the composite layer in the present invention is a value indicating the ratio of the polymer electrolyte to the total volume of the composite layer, and can be calculated from the ion exchange capacity (IEC). Specifically, the filling rate is carried out by the method described in (4) in the Examples section.
[0037] The electrolyte membrane may have a polymer electrolyte layer formed on both sides or one side of the composite layer that is not composited with a reinforcing material such as a porous substrate. By having such a layer, the adhesion between the electrolyte membrane and the electrodes can be improved and interfacial peeling can be suppressed. When a polymer electrolyte layer that is not composited with a reinforcing material is formed in contact with both sides or one side of the composite layer, the polymer electrolyte constituting the layer is preferably the same polymer as the polymer electrolyte filled in the composite layer.
[0038] The electrolyte membrane of the present invention has a composite layer, which allows a reduction in the rate of dimensional change in the plane direction. The reduction in the rate of dimensional change in the plane direction reduces stress caused by swelling and shrinkage that occurs at the edge portions of the electrolyte membrane during wet-dry cycles when used as an electrolyte membrane for a fuel cell, and makes it easier to improve durability. The rate of dimensional change λ in the plane direction of the electrolyte membrane xy is preferably 10% or less, more preferably 8% or less, and even more preferably 5% or less.
[0039] In addition, it is preferable that the anisotropy of the dimensional change rate in the plane direction of the electrolyte membrane is small in MD and TD. TD MD dimensional change rate λ MD The ratio λ MD / λ TD However, 0.5≦λ MD / λ TD It is preferable that the relationship satisfies ≦2.0. Here, MD is an abbreviation for Machine Direction, and means the direction in which the porous substrate, coater, or coated substrate is moved in the electrolyte membrane production process described later. Which of the porous substrate, coater, and coated substrate is moved is appropriately determined according to the coating process and is not particularly limited. When applying a process in which multiple elements among the porous substrate, coater, and coated substrate are moved, all elements are usually moved in the same direction, but a process in which they are moved in different directions may also be applied. In this case, it is determined whether the elements are moved in the order of (1) the coated substrate, (2) the coater, and (3) the porous substrate, and the same direction as the highest-ranked element among the elements being moved is defined as MD. TD is an abbreviation for Traverse Direction, and is a direction perpendicular to MD in the plane direction of the electrolyte membrane.
[0040] TD dimensional change rate λ TD Dimensional change rate λ in MD MD The ratio (λ MD / λ TD ) is 0.5≦λ MD / λ TD When the ratio is ≦2.0, the cell design of the fuel cell is not restricted, and even at an edge perpendicular to the direction in which the dimensional change is greater in the MD or TD direction, the concentration of stress due to swelling and shrinkage is small. Therefore, the edge is less likely to become the starting point of electrolyte membrane rupture, and the dry-wet cycle durability can be improved.
[0041] Here, the dimensional change rate is an index showing the change in the dimensions of the electrolyte membrane in a dry state and in a wet state, and is specifically measured by the method described in (6) in the Examples section.
[0042] The thickness of the composite layer in the electrolyte membrane is not particularly limited, but is preferably 0.5 μm or more, more preferably 1 μm or more. Also, it is preferably 50 μm or less, more preferably 40 μm or less. When the composite layer is 0.5 μm or more and 50 μm or less, it is possible to obtain a composite polymer electrolyte membrane having high proton conductivity, suppressing electrical short circuits and fuel permeation, and excellent wet-dry cycle durability.
[0043] The electrolyte membrane preferably has a haze of 20% to 45%, more preferably 30% to 45%, and even more preferably 35% to 45% when light is transmitted in the thickness direction. When a material having a refractive index different from that of the polymer electrolyte, such as a porous substrate, is present in the electrolyte membrane, light may be scattered at the interface between the polymer electrolyte and the material having a different refractive index, resulting in haze. If the haze is 20% to 45%, the polymer electrolyte responsible for the conduction of protons and the porous substrate responsible for improving mechanical properties such as elastic modulus, elongation at break, and strength at break are combined in a good balance to obtain an electrolyte membrane having excellent proton conductivity and mechanical properties, and the fuel cell can achieve both excellent output and dry-wet cycle durability. The haze is calculated using the method described in (17) in the Examples section.
[0044] The electrolyte membrane preferably has a diffuse transmittance of 20% to 40%, more preferably 30% to 40%, when light is transmitted in the thickness direction. If the diffuse transmittance is 20% to 40%, an electrolyte membrane having excellent proton conductivity and mechanical properties can be obtained, and the fuel cell can achieve both excellent output and dry-wet cycle durability. The diffuse transmittance is calculated using the method described in (17) in the Examples section.
[0045] [Polymer electrolyte] The polymer electrolyte used in the present invention is a polymer having proton conductivity due to the presence of an ionic group, and may be either a fluorine-based polymer electrolyte or a hydrocarbon-based polymer.
[0046] Here, the fluorine-based polymer electrolyte means one in which most or all of the hydrogen atoms in the alkyl and / or alkylene groups in the polymer are replaced with fluorine atoms. Representative examples of fluorine-based polymer electrolytes having ionic groups include commercially available products such as "Nafion" (registered trademark) (manufactured by Chemours), "Aquivion" (registered trademark) (manufactured by Solvay), "Flemion" (registered trademark) (manufactured by AGC Corporation), and "Aciplex" (registered trademark) (manufactured by Asahi Kasei Corporation).
[0047] These fluorine-based polymer electrolytes are generally very expensive and tend to have large gas crossover. Therefore, from the viewpoints of mechanical strength, dry-wet cycle durability, chemical stability, etc., the polymer electrolyte used in the present invention is preferably a hydrocarbon-based polymer. That is, in the present invention, the polymer electrolyte is preferably a hydrocarbon-based polymer having an ionic group. In particular, in the composite membrane of the present invention, an embodiment in which the polymer electrolyte is a hydrocarbon-based polymer is particularly preferable in that it has excellent mechanical properties both in a dry state and in a hydrated state.
[0048] The hydrocarbon polymer is preferably an aromatic hydrocarbon polymer having an aromatic ring in the main chain. Here, the aromatic ring may include not only a hydrocarbon aromatic ring consisting of only carbon atoms and hydrogen atoms such as a benzene ring or a naphthalene skeleton, but also a heterocycle such as a pyridine ring, an imidazole ring, or a thiol ring. In addition, the polymer may be partially constituted by an aliphatic unit together with the aromatic ring unit.
[0049] Specific examples of aromatic hydrocarbon polymers include polymers having a structure selected from polysulfone, polyethersulfone, polyphenylene oxide, polyarylene ether polymer, polyphenylene sulfide, polyphenylene sulfide sulfone, polyparaphenylene, polyarylene polymer, polyarylene ketone, polyether ketone, polyarylene phosphine oxide, polyether phosphine oxide, polybenzoxazole, polybenzothiazole, polybenzimidazole, polyamide, polyimide, polyetherimide, and polyimide sulfone in the main chain together with an aromatic ring. Note that polysulfone, polyethersulfone, polyether ketone, etc. referred to here are general terms for structures having sulfone bonds, ether bonds, and ketone bonds in the molecular chain, and include polyether ketone ketone, polyether ether ketone, polyether ether ketone ketone, polyether ketone ether ketone ketone, and polyether ketone sulfone. The hydrocarbon skeleton may have a plurality of structures among these structures. Among these, the aromatic hydrocarbon polymer is most preferably a polymer having a polyetherketone skeleton, that is, a polyetherketone polymer.
[0050] The polymer electrolyte is preferably one that forms a bicontinuous or lamellar phase separation structure. Such a phase separation structure can be formed, for example, in a molded article made of a blend of two or more incompatible polymers, such as a hydrophilic polymer having an ionic group and a hydrophobic polymer having no ionic group, or in a polymer having a segment (S E1 ) and a segment that does not contain an ionic group (S E2) can be expressed in block copolymers consisting of two or more incompatible segments. In the cocontinuous and lamellar phase separation structures, both the hydrophilic and hydrophobic domains form continuous phases, so that continuous proton-conducting channels are formed, and it is easy to obtain an electrolyte membrane with excellent proton conductivity. At the same time, a continuous hydrophobic skeleton is also formed, so that it is easy to obtain an electrolyte membrane with excellent mechanical properties not only in a dry state but also in a hydrated state. Here, a domain means a mass formed by the aggregation of similar substances or segments in one membrane.
[0051] As the polymer electrolyte, in particular, a segment containing an ionic group (S E1 ) and a segment that does not contain an ionic group (S E2 ) is preferably a block copolymer having one or more of each of the above. Here, the segment is a partial structure in a copolymer polymer chain consisting of repeating units exhibiting specific properties, and has a molecular weight of 2,000 or more. By using a block copolymer, it is possible to express a bicontinuous or lamellar phase separation structure having fine domains compared to a polymer blend, and thus it is possible to achieve better power generation performance and wet / dry cycle durability.
[0052] Hereinafter, the segment containing an ionic group (S E1 ) or the polymer is called an "ionic block" and the segment that does not contain ionic groups (S E2 ) or polymer may be referred to as a “nonionic block”. However, the expression “containing no ionic groups” in this specification does not exclude an embodiment in which the segment or polymer contains a small amount of ionic groups within a range that does not inhibit the formation of a phase-separated structure.
[0053] Such block copolymers have a molar composition ratio of ionic block to nonionic block (S E1 / S E2) is preferably 0.20 or more, more preferably 0.33 or more, and even more preferably 0.50 or more. E1 / S E2 The molar composition ratio (S) is preferably 5.00 or less, more preferably 3.00 or less, and even more preferably 2.50 or less. E1 / S E2 When the molar composition ratio (S) is 0.20 or more or 5.00 or less, a composite polymer electrolyte membrane having high proton conductivity under low humidity conditions and excellent hot water resistance and dry-wet cycle durability can be obtained. E1 / S E2 ) represents the ratio of the number of moles of repeating units present in the ionic block to the number of moles of repeating units present in the nonionic block. The "number of moles of repeating units" is the value obtained by dividing the number average molecular weight of the ionic block and the number average molecular weight of the nonionic block by the molecular weight of the corresponding structural unit.
[0054] The ionic group of the polymer electrolyte may be an ionic group having proton exchange ability. As such functional groups, sulfonic acid groups, sulfonimide groups, sulfate groups, phosphonic acid groups, phosphoric acid groups, and carboxylic acid groups are preferably used. The polymer may contain two or more types of ionic groups. Among them, from the viewpoint of high proton conductivity, it is more preferable that the polymer has at least one selected from sulfonic acid groups, sulfonimide groups, and sulfate groups, and from the viewpoint of raw material cost, it is most preferable that the polymer has a sulfonic acid group.
[0055] The ion exchange capacity (IEC) of the polymer electrolyte is preferably 0.1 meq / g or more and 5.0 meq / g or less in terms of the balance between proton conductivity and water resistance. The IEC is more preferably 1.4 meq / g or more, and even more preferably 1.7 meq / g or more. The IEC is more preferably 3.5 meq / g or less, and even more preferably 3.0 meq / g or less. When the IEC is 0.1 meq / g or more and 5.0 meq / g or less, both excellent proton conductivity and water resistance can be achieved.
[0056] Here, IEC is the molar amount of ionic groups introduced per unit dry weight of the polymer electrolyte, and the larger this value is, the more the amount of ionic groups introduced is. In the present invention, IEC is defined as a value obtained by neutralization titration. The calculation of IEC by neutralization titration is performed by the method described in (2) in the Examples section.
[0057] In the present invention, it is particularly preferable to use an aromatic hydrocarbon-based block copolymer as the polymer electrolyte, and more preferably a polyetherketone-based block copolymer. Among them, a polyetherketone-based block copolymer containing a segment including a structural unit containing an ionic group as shown in the following general formula (S1) and a segment including a structural unit not containing an ionic group as shown in the following general formula (S2) can be particularly preferably used.
[0058] [ka]
[0059] In general formula (S1), Ar 1 ~Ar 4 represents any divalent arylene group, Ar 1 and / or Ar 2 contains an ionic group, and Ar 3 and Ar 4 may or may not contain an ionic group. 1 ~Ar 4 may be optionally substituted, and two or more types of arylene groups may be used independently. * represents a bonding site with general formula (S1) or another structural unit.
[0060] [ka]
[0061] In general formula (S2), Ar 5 ~Ar 8 represents any divalent arylene group, which may be optionally substituted but does not contain an ionic group. 5~Ar 8 may independently use two or more types of arylene groups. * represents a bonding site with general formula (S2) or another structural unit.
[0062] Here, Ar 1 ~Ar 8 Preferred divalent arylene groups include, but are not limited to, hydrocarbon arylene groups such as phenylene, naphthylene, biphenylene, and fluorenediyl groups, and heteroarylene groups such as pyridinediyl, quinoxalinediyl, and thiophenediyl. Here, the term "phenylene group" may be classified into three types, o-phenylene, m-phenylene, and p-phenylene, depending on the bonding site between the benzene ring and other structural units, and unless otherwise specified in this specification, it is used as a general term for these. The same applies to other divalent arylene groups such as "naphthylene group" and "biphenylene group". Ar 1 ~Ar 8 is preferably a phenylene group and a phenylene group containing an ionic group, and most preferably a p-phenylene group and a p-phenylene group containing an ionic group. 5 ~Ar 8 may be substituted with a group other than an ionic group, but is preferably unsubstituted in terms of proton conductivity, chemical stability, and dry-wet cycle durability.
[0063] In order to obtain sufficient dimensional stability, mechanical strength, dry-wet cycle durability, fuel barrier properties, and solvent resistance, the polymer electrolyte is preferably an aromatic hydrocarbon polymer having crystallinity. Here, "having crystallinity" means that the polymer electrolyte has a crystallizable property such that it can be crystallized when heated, or that the polymer electrolyte is already crystallized.
[0064] The presence or absence of crystallinity is confirmed by differential scanning calorimetry (DSC) or wide-angle X-ray diffraction. In the present invention, it is preferable that the heat of crystallization measured by differential scanning calorimetry after film formation is 0.1 J / g or more, or the crystallinity measured by wide-angle X-ray diffraction is 0.5% or more. That is, when no crystallization peak is observed by differential scanning calorimetry, it is considered that the polymer electrolyte has already crystallized or is amorphous. If the polymer electrolyte has already crystallized, the crystallinity measured by wide-angle X-ray diffraction will be 0.5% or more.
[0065] Aromatic hydrocarbon-based polymers having crystallinity may have poor processability for forming electrolyte membranes. In such cases, a protective group may be introduced into the aromatic hydrocarbon-based polymer to temporarily suppress the crystallinity. Specifically, the aromatic hydrocarbon-based polymer having crystallinity can be used as a polymer electrolyte in the present invention by forming a membrane in a state where a protective group is introduced and then removing the protective group.
[0066] [Porous base material] The porous substrate used in the present invention is classified into a hydrocarbon-based porous substrate mainly composed of a hydrocarbon-based polymer compound and a fluorine-based porous substrate mainly composed of a fluorine-based polymer compound. Examples of the hydrocarbon-based polymer compound include polyethylene (PE), polypropylene (PP), polystyrene (PS), polyacrylate, polymethacrylate, polyvinyl chloride (PVC), polyvinylidene chloride (PVdC), polyester, polycarbonate (PC), polysulfone (PSU), polyethersulfone (PES), polyphenylene oxide (PPO), polyarylene ether polymer, polyphenylene sulfide (PPS), polyphenylene sulfide sulfone, polyparaphenylene (PPP), polyarylene polymer, polyarylene ketone, polyether ketone (PEK), polyarylene phosphine oxide, polyether phosphine oxide, polybenzoxazole (P Examples of the fluorine-based polymer compound include, but are not limited to, polytetrafluoroethylene (PTFE), polyhexafluoropropylene, tetrafluoroethylene-hexafluoropropylene copolymer (FEP), ethylene-tetrafluoroethylene copolymer (ETFE), polyvinylidene fluoride (PVdF), polychlorotrifluoroethylene (PCTFE), perfluoroalkoxy fluorine resin (PFA), and ethylene-chlorotrifluoroethylene copolymer (ECTFE). From the viewpoints of water resistance, chemical resistance, and mechanical properties, PE, PP, PPS, PEK, PBO, PBT, PBI, PTFE, polyhexafluoropropylene, FEP, and PFA are preferred.
[0067] Since the fluorine-based porous substrate generally consists mainly of a fluorine-based polymer compound that is extremely hydrophobic, it is highly effective in imparting water resistance to the electrolyte membrane, improving mechanical properties in a water-containing state, and suppressing dimensional change by combining with a polymer electrolyte, and since fluorine-containing polymer compounds generally have low solubility in chemicals and are stable against chemical reactions, it is preferable because it can impart chemical resistance and chemical durability to the electrolyte membrane. From the viewpoint of chemical resistance and chemical durability, PTFE, polyhexafluoropropylene, FEP, and PFA are more preferable, and PTFE is particularly preferable because it has high mechanical strength due to molecular orientation.
[0068] From the viewpoint of water resistance, the porous substrate is preferably a fluorine-based porous substrate containing 50% or more by mass of fluorine atoms, more preferably a fluorine-based porous substrate containing 60% or more by mass of fluorine atoms, and particularly preferably a fluorine-based porous substrate containing 70% or more by mass of fluorine atoms. The fluorine atom content in the porous substrate is a value measured by ion chromatography of a solution in which the gas generated by burning the porous substrate is absorbed, and specifically, it can be measured by the method described in (10) in the Examples section below.
[0069] The oxygen atom content of the porous substrate is preferably 10% by mass or less, more preferably 8% or less, and even more preferably 5% or less, as measured by X-ray photoelectron spectroscopy (XPS). When the oxygen atom content is within the above-mentioned preferred range, the water absorption of the porous substrate does not increase, and dimensional change when the electrolyte membrane absorbs water can be suppressed. The oxygen atom content of the porous substrate can be specifically measured by the method described in (14) in the Examples section below.
[0070] Aromatic hydrocarbon-based porous substrates mainly composed of hydrocarbon-based polymer compounds having aromatic rings in the main chain are generally hydrophobic compounds and have excellent elastic modulus and breaking strength, and therefore can be suitably used. Among them, PPS, PBO, PBT, PBI, and PEK are more preferable from the viewpoint of elastic modulus, breaking strength, and chemical durability, and polyazole compounds PBO, PBT, and PBI are particularly preferable from the viewpoint of chemical resistance and processability, and PBI is the most preferable from the viewpoint of cost and distribution volume.
[0071] In addition, when analyzing the porous substrate present in the electrolyte membrane after it has been composited with the polymer electrolyte, it is possible to extract only the porous substrate by immersing the electrolyte membrane in a solvent that dissolves only the polymer electrolyte.
[0072] Examples of the form of the porous substrate include a stretched microporous membrane obtained by stretching a raw material film in the membrane surface direction to form fine pores; a wet-coagulated microporous membrane obtained by preparing a raw material solution, forming a membrane, and then immersing the membrane in a poor solvent for the raw material while still containing the solvent and coagulating it; a nonwoven fabric made of solution-spun fibers spun from a raw material solution; and a nonwoven fabric made of melt-spun fibers spun from the raw material of the porous substrate.
[0073] Methods for solution spinning include a dry spinning method in which high pressure is applied from a spinneret to extrude the raw material solution into a fibrous form and then dried with hot air; a wet spinning method in which the raw material solution extruded into a fibrous form is immersed in a poor solvent for the raw material and solidified; and electrospinning in which the raw material solution is extruded into a space to which a high voltage is applied and pulled into a fibrous form by static electricity.
[0074] The melt spinning method includes melt blow spinning, in which a molten porous substrate material is discharged from a nozzle in the form of fibers.
[0075] The porous substrate preferably has a structure in which thick fibrous nodes are aligned approximately parallel in the in-plane direction, which makes it possible to obtain an electrolyte membrane having excellent mechanical properties in the direction parallel to the nodes, particularly in a water-containing state.
[0076] The porous substrate preferably includes nodes with an aspect ratio calculated from the length / diameter of 10 or more, more preferably includes nodes with an aspect ratio of 20 or more, and even more preferably includes nodes with an aspect ratio of 50 or more. A porous substrate including nodes with an aspect ratio of 10 or more has a structure in which a strong hydrophobic skeleton is continuous, and therefore can obtain an electrolyte membrane with excellent mechanical properties by suppressing softening of the entire membrane not only in a dry state but also in a hydrated state in which a polymer electrolyte usually softens due to water absorption, and can improve the wet / dry cycle durability as a fuel cell.
[0077] The average diameter of the nodes is preferably 0.01 μm or more, more preferably 0.1 μm or less, and even more preferably 0.2 μm or less. Also, it is preferably 10 μm or less, more preferably 5 μm or less, and even more preferably 2 μm or less. When the average diameter of the nodes is 0.01 μm or more and 10 μm or less, softening of the electrolyte membrane in a water-containing state can be suppressed, and an electrolyte membrane having high proton conductivity can be obtained, so that a fuel cell having high output can be manufactured.
[0078] The porous substrate preferably has thin fibrous fibrils that connect the nodes in the in-plane direction to form a ladder-like structure. More preferably, the fibrils include those aligned approximately perpendicular to the nodes. By having such a structure, an electrolyte membrane can be obtained that has excellent mechanical properties, especially in a water-containing state, not only in the direction parallel to the nodes in the in-plane direction but also in the direction perpendicular to the nodes.
[0079] The diameter ratio calculated from the average diameter of the nodes / the average diameter of the fibrils is preferably 2 or more, more preferably 3 or more, and even more preferably 5 or more. The diameter ratio is preferably 20 or less, and more preferably 10 or less. When a porous substrate having a diameter ratio of 2 to 20 is used, an electrolyte membrane having high proton conductivity can be obtained by suppressing inhibition of proton conduction by the nodes, so that a fuel cell having high output can be manufactured, and at the same time, a composite polymer electrolyte membrane having small anisotropy and excellent mechanical properties can be manufactured because swelling in a direction perpendicular to and / or parallel to the nodes can be suppressed.
[0080] The structure of the porous substrate, such as the node orientation and average diameter, and the fibril orientation and average diameter, can be analyzed using a scanning electron microscope (SEM) by the method described in (18) in the Examples section.
[0081] There is no particular limitation on the thickness of the porous substrate used in the present invention, and this should be determined depending on the application of the electrolyte membrane. However, a membrane thickness of 0.5 μm or more and 50 μm or less is practically used, and a membrane thickness of 1 μm or more and 40 μm or less is preferably used.
[0082] The porosity of the porous substrate before being composited with the polymer electrolyte is not particularly limited, but is preferably 50 to 98%, more preferably 70 to 98%, from the viewpoint of achieving both proton conductivity and mechanical strength of the resulting electrolyte membrane. The porosity Y1 (volume %) of the porous substrate is defined as the value calculated by the following formula.
[0083] Y1 = (1-Db / Da) x 100 (Here, Da is the specific gravity of the raw material constituting the porous substrate, and Db is the specific gravity of the entire porous substrate.) [Nonionic fluorosurfactant] In the electrolyte membrane of the present invention, it is preferable to contain a nonionic fluorine-based surfactant (hereinafter, sometimes simply referred to as "surfactant"). By using a nonionic fluorine-based surfactant, the affinity between the polymer electrolyte and the porous substrate is improved, which not only makes it easier to manufacture the electrolyte membrane, but also strengthens the interfacial bond between the polymer electrolyte and the porous substrate in the electrolyte membrane, thereby suppressing the interfacial peeling between the two due to the volume change of the electrolyte membrane in the dry-wet cycle, thereby improving the dry-wet cycle durability of the fuel cell. In particular, when a hydrocarbon-based polymer electrolyte and a fluorine-based porous substrate are used, it is more preferable because the affinity between the two can be significantly improved.
[0084] The surfactant is preferably a compound having a fluorine-containing group consisting of a fluorinated alkyl group, a fluorinated alkenyl group or a fluorinated aryl group in which a hydrogen atom in an alkyl group, an alkenyl group or an aryl group is substituted with a fluorine atom, and a non-ionic solvent-philic group (hydrophilic group or lipophilic group).
[0085] The fluorine-containing group is preferably a perfluoroalkyl group, a perfluoroalkenyl group or a perfluoroaryl group in which all hydrogen atoms in an alkyl group, an alkenyl group or an aryl group have been substituted with fluorine atoms.
[0086] As the fluorine-containing group, a fluorinated alkenyl group or a fluorinated aryl group is more preferable because of its excellent surface activity, and a fluorinated alkenyl group is even more preferable because it has a flexible structure and exhibits high surface activity.
[0087] The fluorine-containing group preferably has 2 or more carbon atoms, more preferably 4 or more carbon atoms, and particularly preferably 6 or more carbon atoms. The number of carbon atoms is preferably 20 or less, more preferably 15 or less, and particularly preferably 10 or less. When the number of carbon atoms is within the above preferred range, the fluorine-containing group has appropriate volatility and water solubility and remains in the electrolyte membrane, resulting in excellent wet-dry cycle durability, while being less susceptible to phase separation from the polymer electrolyte and therefore excellent wet-dry cycle durability.
[0088] Specific examples of fluorinated alkyl groups include, but are not limited to, an ethyl fluoride group, a propyl fluoride group, a butyl fluoride group, a pentyl fluoride group, a hexyl fluoride group, a heptyl fluoride group, an octyl fluoride group, a nonyl fluoride group, and a decyl fluoride group.
[0089] Examples of the fluorinated alkenyl group include, but are not limited to, an ethenyl fluoride group, a propenyl fluoride group, a butenyl fluoride group, a pentenyl fluoride group, a hexenyl fluoride group, a heptenyl fluoride group, an octenyl fluoride group, a nonenyl fluoride group, and a decenyl fluoride group.
[0090] Among them, hexyl fluoride, heptyl fluoride, octyl fluoride, nonyl fluoride, decyl fluoride, hexenyl fluoride, heptenyl fluoride, octenyl fluoride, nonenyl fluoride, and decenyl fluoride are more preferable because they have low volatility and water solubility and tend to remain in the electrolyte membrane. Here, the "ethyl fluoride group" may be one of five types of functional groups, namely, monofluoroethyl, difluoroethyl, trifluoroethyl, tetrafluoroethyl, and pentafluoroethyl, depending on the number of fluorine atoms contained in one functional group, and in this specification, the "ethyl fluoride group" is used as a general term for these. The same applies to other functional groups such as "propyl fluoride group" and "butyl fluoride group". In addition, in the case of the difluoroethyl group, which is a functional group having two carbon atoms and two fluorine atoms, there are three structural isomers, namely, 1,1-difluoroethyl group, 1,2-difluoroethyl group, and 2,2-difluoroethyl group, and in this specification, the term "difluoroethyl group" is used as a general term for these. The same applies to other functional groups such as "trifluoroethyl group" and "tetrafluoroethyl group". In addition, in the case of "fluorinated butyl group", the term "butyl group" is a general term indicating a functional group consisting of a skeleton having four carbon atoms, and there are four types of structures, namely, butyl group, 1-methylpropyl group, 2-methylpropyl group, and 1,1-dimethylethyl group, and in this specification, the term "butyl group" is used as a general term for these. The same applies to other functional groups such as "fluorinated pentyl group" and "fluorinated hexyl group".
[0091] The structure of the fluorine-containing group can be linear, branched, cyclic, etc., but among them, a branched structure is preferable because the interaction between the fluorine compounds is weakened and the surface tension is easily reduced. In the present invention, a surfactant having a fluorine-containing group having a structure represented by the following formula (F1) is particularly preferable.
[0092] [ka]
[0093] In formula (F1), * represents a bonding point to another atomic group.
[0094] As the nonionic fluorine-based surfactant, a compound having 10% by mass or more of fluorine atoms in one molecule is preferably used. A compound having 20% by mass or more of fluorine atoms is more preferable, and a compound having 40% by mass or more of fluorine atoms is even more preferable. When the content of fluorine atoms in one molecule is within the above-mentioned preferred range, the compound has excellent affinity with the porous substrate, and a sufficient effect of improving power generation performance can be obtained. In addition, since the compound has low solubility in water and acid and is difficult to dissolve in water and acid generated during the operation of an electrochemical cell such as a fuel cell, the compound does not dissolve from the electrolyte membrane, and the affinity between the polymer electrolyte and the catalyst layer can be prevented from decreasing.
[0095] The philic group can be a hydrophilic group or a lipophilic group, but is preferably a hydrophilic group.
[0096] The hydrophilic group is not particularly limited as long as it is a nonionic group having a hydrophilic element selected from the group consisting of oxygen, nitrogen, phosphorus, sulfur, and boron, but is preferably a group containing a polyether group, a carboxylate group, a sulfonate group, a phosphite group, or a phosphate group, and is more preferably a group containing a polyether group because it has excellent affinity with the polymer electrolyte and excellent chemical stability by forming a hydrogen bond with the ionic group. Among them, the hydrophilic group is preferably a group having a polyalkyl ether structure shown in the following general formula (C1) or a polyacrylate structure shown in the following general formula (C2), and is more preferably a polyalkyl ether shown in the following general formula (C1) because it has particularly excellent affinity with the polymer electrolyte.
[0097] [ka]
[0098] In general formula (C1), q and r are natural numbers satisfying r=2q, and s is an integer of 1 to 1,000, meaning the number of repetitions of the alkyl ether structure. In general formula (C2), R is at least one group selected from an alkyl group having 1 to 20 carbon atoms, an alkenyl group having 1 to 20 carbon atoms, and an aryl group having 6 to 20 carbon atoms, and t is an integer of 1 to 1,000, meaning the number of repetitions of the acrylate structure. When s or t is 2 or more in (C1) or (C2), the multiple alkyl ether structures or acrylate structures may be the same or different.
[0099] The lipophilic group includes fluorine-free alkyl groups, alkenyl groups, alkynyl groups, and phenyl groups.
[0100] In the present invention, the nonionic fluorine-based surfactant is preferably a compound having a vapor pressure of less than 2 kPa at 150° C., more preferably a compound having a vapor pressure of 1 kPa or less at 150° C., and most preferably a compound having no boiling point, i.e., a compound that starts thermal decomposition without boiling. In particular, in the present invention, it is preferable that the surfactant is a compound having a 5% weight loss temperature of 150° C. or more in thermogravimetric differential thermal analysis. Such a surfactant does not volatilize or decompose during membrane formation, and can be left in the electrolyte membrane.
[0101] In the present invention, the nonionic fluorine-based surfactant is preferably a compound having a weight-average molecular weight of 1,000 or more, more preferably a compound having 1,500 or more, and even more preferably a compound having 2,000 or more. In addition, the nonionic fluorine-based surfactant is preferably a compound having a weight-average molecular weight of 10,000 or less, more preferably a compound having 8,000 or less, and even more preferably a compound having 5,000 or less. When the weight-average molecular weight of the surfactant is within the above-mentioned preferred range, the surfactant has a moderate volatility and is difficult to dissolve in a solvent such as water, so that the surfactant maintains affinity with the polymer electrolyte and the porous substrate and the catalyst layer described below, and is difficult to peel or break at the interface between the two, and has excellent durability. On the other hand, the surfactant is difficult to aggregate alone in the electrolyte membrane to form an island-like phase separation structure, and is difficult to break at the interface between the surfactant and the polymer electrolyte or the porous substrate, and has excellent durability.
[0102] The surfactant preferably has a molecular weight of the fluorine-containing group of 200 or more, more preferably 400 or more, and even more preferably 1,000 or more. The molecular weight of the fluorine-containing group is preferably 5,000 or less, more preferably 3,000 or less, and even more preferably 2,000 or less. When the molecular weight of the fluorine-containing group is within the above preferred range, the flexibility and degree of freedom of the molecular chain in the fluorine-containing group are excellent, so that the surfactant maintains affinity with the porous substrate and catalyst layer, is resistant to peeling and breaking at the interface with the polymer electrolyte, and has excellent durability, while the surfactant is unlikely to aggregate alone in the electrolyte membrane to form an island-like phase separation structure, and is resistant to breaking at the interface between the surfactant and the polymer electrolyte or porous substrate, and has excellent durability.
[0103] In the case of a surfactant having a hydrophilic group as a solvent group, the molecular weight of the hydrophilic group is preferably 100 or more, more preferably 200 or more, and even more preferably 500 or more. The molecular weight of the hydrophilic group is preferably 4,000 or less, more preferably 2,500 or less, and even more preferably 1,500 or less. When the molecular weight of the hydrophilic group is in the above preferred range, the flexibility and degree of freedom of the molecular chain in the hydrophilic group are excellent, so that the affinity with the polymer electrolyte is maintained, and the polymer electrolyte is not easily broken at the interface with the porous substrate and has excellent durability, while the water solubility is moderate, so that the polymer electrolyte is not easily dissolved in water or acid generated during the operation of an electrochemical cell such as a fuel cell, and elution from the electrolyte membrane is prevented, so that the affinity between the polymer electrolyte and the porous substrate is maintained, and the polymer electrolyte is not easily broken at the interface between the porous substrate and the polymer electrolyte during dimensional change and has excellent durability.
[0104] Moreover, the surfactant is preferably a compound that is not soluble in any of water, 10% sulfuric acid, and 10% aqueous sodium hydroxide solution, more preferably a compound that is not soluble in water, and most preferably a compound that is not soluble in any of these. Here, "not soluble" means that the saturated solubility at 25°C is less than 0.1% by mass. When the surfactant is not soluble in the solvent and / or solution, it becomes difficult to dissolve in water or acid generated during the operation of an electrochemical cell such as a fuel cell, and elution from the electrolyte membrane can be suppressed, so that the affinity between the polymer electrolyte and the porous substrate or catalyst layer can be maintained, and thus the decrease in durability caused by peeling or breaking at the interface between the polymer electrolyte and the porous substrate or catalyst layer during dimensional changes can be suppressed.
[0105] Examples of the nonionic fluorine-based surfactants used in the present invention include "Megafac" (registered trademark) F-251, F-253, F-281, F-430, F-477, F-551, F-552, F-553, F-554, F-555, F-556, F-557, F-558, F-559, F-560, F-561, F-562, F-563, F-564, F-565, F-566, F-567, F-568, F-569, F-570, F-571, F-572, F-573, F-574, F-575, F-576, F-577, F-578, F-579, F-580, F-581, F-582, F-583, F-584, F-585, F-586, F-587, F-588, F-589 ... F-563, F-565, F-568, F-570, F-572, F-574, F-575, F-576, R-40, R-40-LM, R-41, R-94, RS-56, RS-72-K, RS-75, RS-76-E, RS-76-NS, DS-21, F444, TF-2066, AGC's "Surflon" (registered trademark) S-141, S-145, S-241, S-242, S-243, S-386, S-420, S-611, S-651, and "Ftergent" (registered trademark) 251, 208M, 212M, 215M, 250, 209F, 222F, 245F, 208G, 218GL, 240G, 212P, 220P, 228P, FTX-218, and DF manufactured by Neos Co., Ltd. X-18, 710FL, 710FM, 710FS, 730FL, 730FM, 610FM, 683, 601AD, 601ADH2, 602A, 650AC, 681, Mitsubishi Materials Electronic Chemicals Co., Ltd.'s EF-PP31N04, EF-PP31N09, EF-PP31N15, EF-PP31N22, 3M's FC-4430, FC-4432, OMNOVA Examples of such polyurethane foams include PF-151N, PF-636, PF-6320, PF-656, PF-6520, PF-652-NF, and PF-3320 manufactured by Solvay Solutions, TG-9131 and "Zeffle" (registered trademark) GH-701 manufactured by Daikin Industries, Ltd., and "Fluorolink" (registered trademark) A10-P manufactured by Solvay Japan K.K.
[0106] The content of the nonionic fluorine-based surfactant in the electrolyte membrane is preferably 0.005 or more, more preferably 0.01 or more, as a mass ratio to the total amount of the polymer electrolyte contained in the electrolyte membrane. Also, it is preferably 0.20 or less, more preferably 0.10 or less. When the ratio is within the above preferred range, the affinity between the polymer electrolyte and the porous substrate or catalyst layer is maintained, and the polymer electrolyte is not easily peeled off or broken at the interface between the porous substrate or catalyst layer during dimensional change, resulting in excellent durability, while the amount of surfactant is appropriate and the proton conductivity of the electrolyte membrane is excellent. The surfactant content here means the amount of surfactant remaining in the completed electrolyte membrane, excluding the amount of surfactant that has fallen off during the manufacturing process.
[0107] The nonionic fluorine-based surfactant contained in the electrolyte membrane can be analyzed by dissolving the surfactant in a predetermined solvent together with the polymer electrolyte membrane. The polymer electrolyte membrane solution and the dried product obtained by removing the solvent are analyzed by infrared spectroscopy (IR), 1 H nuclear magnetic resonance (NMR) analysis, 19 By carrying out F-NMR analysis, MALDI-MS analysis, and pyrolysis GC / MS analysis, the chemical structure of each surfactant can be analyzed and the surfactant content can be calculated. It is also preferable to carry out general purification treatment such as solvent extraction or reprecipitation on the solution and the dried product to extract only the nonionic fluorine-based surfactant and then carry out the analysis.
[0108] The solvent used in the analysis of the nonionic surfactant can be appropriately selected depending on the type of the polymer electrolyte constituting the electrolyte membrane and the nonionic surfactant. For example, aprotic polar solvents such as N,N-dimethylacetamide, N,N-dimethylformamide, N-methyl-2-pyrrolidone, dimethyl sulfoxide, sulfolane, 1,3-dimethyl-2-imidazolidinone, and hexamethylphosphontriamide, carbonate-based solvents such as ethylene carbonate and propylene carbonate, alkylene glycol monoalkyl ethers such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, propylene glycol monomethyl ether, and propylene glycol monoethyl ether, alcohol-based solvents such as methanol, ethanol, propanol, and butanol, acetone, and the like can be used. Suitable solvents include ketone solvents such as ketone, methyl ethyl ketone, and methyl isobutyl ketone, ester solvents such as γ-butyrolactone, ethyl acetate, butyl acetate, and ethyl lactate, hydrocarbon solvents such as hexane and cyclohexane, aromatic hydrocarbon solvents such as benzene, toluene, and xylene, halogenated hydrocarbon solvents such as chloroform, dichloromethane, 1,2-dichloroethane, perchloroethylene, chlorobenzene, and dichlorobenzene, ether solvents such as diethyl ether, tetrahydrofuran, and 1,4-dioxane, nitrile solvents such as acetonitrile, nitrated hydrocarbon solvents such as nitromethane and nitroethane, and water. A mixed solvent of two or more of these solvents may also be used. Here, "propanol" has a structure in which one of the hydrogen atoms contained in the propane molecule is replaced with a hydroxyl group, and there are two structural isomers, 1-propanol and 2-propanol, but "propanol" is used as a general term for these in this specification. The same applies to other solvents such as "butanol" and "xylene."
[0109] If the electrolyte membrane is insoluble, a different analytical method can be used. The chemical structure and content of the surfactant can be analyzed by performing IR analysis, solid-state NMR analysis, MALDI-MS analysis, and pyrolysis GC / MS analysis on the electrolyte membrane itself that contains the nonionic fluorosurfactant. It is also suitable to immerse the electrolyte membrane in a solvent to dissolve and extract only the nonionic fluorosurfactant before analysis.
[0110] The nonionic fluorosurfactant used in the present invention is preferably one that does not contain metals as impurities. Here, the metals include, but are not limited to, simple metal elements, metal ions, nonionic metal compounds, metal oxides, etc. When the nonionic fluorosurfactant does not contain metals, the hydrophilic group or lipophilic group of the nonionic fluorosurfactant is less likely to interact with the metals, so that the nonionic fluorosurfactant has a high degree of freedom even in the polymer electrolyte membrane and can retain its function as a surfactant, thereby suppressing the decrease in durability caused by peeling and breaking at the interface between the polymer electrolyte and the porous substrate or catalyst layer when the dimensions change.
[0111] [Catalyst layer] The catalyst layer is a layer containing catalyst particles formed on both sides of the electrolyte membrane, and is generally a layer containing catalyst particles and a polymer electrolyte made of a fluorine-based polymer electrolyte. As the fluorine-based polymer electrolyte, the above-mentioned ones can be used.
[0112] In the catalyst-layered electrolyte membrane of the present invention, it is preferable that the catalyst layer contains a perfluoro-based polymer having an ionic group in terms of power generation performance and chemical durability. By using a perfluoro-based polymer having an ionic group, the acidity of the ionic group contained in the catalyst layer is increased, and the proton conductivity is further improved, and since the perfluoro-based polymer has a large number of chemically stable C-F bonds, the chemical durability of the catalyst layer can be further improved.
[0113] As the catalyst particles, catalyst-supported carbon particles in which a catalyst substance is supported on carbon particles are generally used. As the catalyst substance, in addition to platinum, platinum group elements such as palladium, ruthenium, iridium, rhodium, and osmium, as well as metals such as iron, lead, copper, chromium, cobalt, nickel, manganese, vanadium, molybdenum, gallium, and aluminum, or alloys thereof, oxides, double oxides, etc. are exemplified. The type of carbon particles is not particularly limited as long as it is in the form of fine particles, has electrical conductivity, and does not corrode or deteriorate due to reaction with the catalyst, but carbon black, graphite, activated carbon, carbon fiber, carbon nanotubes, and fullerene particles can be used.
[0114] The mass ratio of the polymer electrolyte content to the catalyst particle content in the catalyst layer is preferably in the range of 0.2 to 2.5, particularly preferably 0.5 to 2.0. When the mass ratio of the polymer electrolyte content to the catalyst particle content is in the above-mentioned preferred range, the catalyst layer is less likely to crack, while gas diffusibility is not impaired, and power generation performance is excellent.
[0115] The thickness of the catalyst layer is preferably 0.03 μm to 2,000 μm. To facilitate obtaining good power generation performance and durability, the thickness of the catalyst layer is more preferably 0.5 μm or more, and particularly preferably 1 to 30 μm.
[0116] <Method of manufacturing electrolyte membrane> In the present invention, the electrolyte membrane can be produced as a first embodiment by impregnating a porous substrate with a polymer electrolyte solution, and then drying to remove the solvent contained in the polymer electrolyte solution. At this time, a method in which the nonionic fluorine-based surfactant is mixed in advance with the polymer electrolyte solution and then impregnated into the porous substrate is also suitable. Details of the polymer electrolyte, porous substrate, and nonionic fluorine-based surfactant used in the first embodiment and the production method of the second embodiment described below are as described above, so they will be omitted here.
[0117] As described above, the content of the surfactant in the polymer electrolyte solution is preferably 0.005 or more, more preferably 0.01 or more, as a mass ratio to the total amount of the polymer electrolyte. Also, it is preferably 0.20 or less, more preferably 0.10 or less. When the ratio is within the above preferred range, the affinity between the polymer electrolyte and the catalyst layer is maintained, and the effect of improving the power generation performance is sufficiently obtained, while the amount of the surfactant is appropriate and the proton conductivity of the electrolyte membrane is excellent.
[0118] In addition, in the present invention, as a second embodiment, the electrolyte membrane can also be produced by impregnating a porous substrate to which a nonionic fluorine-based surfactant has been applied in advance with a polymer electrolyte solution, and then drying the porous substrate to remove the solvent contained in the polymer electrolyte solution.
[0119] In this case, the surfactant can be applied to the porous substrate by the following method. (1) A method of controlling the amount of the surfactant applied by removing excess solution while pulling up a porous substrate immersed in the surfactant solution; (2) A method of casting a surfactant solution onto a porous substrate, (3) A method in which a porous substrate is attached onto a supporting substrate on which a surfactant solution has been cast and then impregnated.
[0120] When the impregnation is carried out by the method (3), the solvent can be dried in the state as it is. When the impregnation is carried out by the method (1) or (2), a method in which the solvent of the fluorine-containing nonionic surfactant solution is dried in a state in which the porous substrate is attached to a separately prepared supporting substrate is preferred from the viewpoint of reducing wrinkles and unevenness in thickness of the porous substrate and improving the quality.
[0121] When the surfactant is liquid or oily, the surfactant itself may be impregnated instead of the surfactant solution. However, it is preferable to use a surfactant solution dissolved in a specified solvent in order to adjust the viscosity so that the surfactant can easily penetrate into the porous substrate, or to dilute the surfactant so that an excessive amount of the surfactant is not applied.
[0122] Examples of a method for casting and applying the surfactant solution include knife coating, direct roll coating, Mayer bar coating, gravure coating, reverse coating, air knife coating, spray coating, brush coating, dip coating, die coating, vacuum die coating, curtain coating, flow coating, spin coating, screen printing, and inkjet coating.
[0123] In the second embodiment, the surfactant is preferably added in an amount of 1% by mass or more, more preferably 5% by mass or more, based on the mass of the porous substrate being 100% by mass. Similarly, it is preferably added in an amount of 30% by mass or less, more preferably 20% by mass or less. When the amount of surfactant added is within the above-mentioned preferred range, the affinity between the polymer electrolyte and the porous substrate is maintained and composite formation is easy, while the amount of surfactant becomes appropriate and the pores of the porous substrate are not easily blocked, resulting in excellent proton conductivity of the composite electrolyte membrane.
[0124] In the second embodiment, the contact angle of the solvent used for the polymer electrolyte solution on the surface of the porous substrate is preferably 120° or less, more preferably 80° or less, and even more preferably 50° or less, due to the addition of the surfactant. When the contact angle is within the above-mentioned preferred range, the polymer electrolyte solution is easily impregnated into the surfactant-containing porous substrate.
[0125] Furthermore, in the second embodiment, it is preferable to use, as the surfactant, a compound that is insoluble in the solvent of the polymer electrolyte solution to be impregnated. When such a surfactant is used, the surfactant is prevented from diffusing from the surface of the porous substrate or the surface of the composite electrolyte membrane in contact with the catalyst layer to the polymer electrolyte during impregnation with the polymer electrolyte solution, and the surfactant can be fully exerted as a function of the surfactant while preventing a decrease in proton conductivity due to the presence of the surfactant in the polymer electrolyte.
[0126] In the first and second embodiments, the concentration of the polymer electrolyte solution is preferably 3 to 40% by mass, more preferably 5 to 25% by mass. If the concentration is within this range, the number of coating times required to sufficiently fill the voids in the porous substrate with the polymer electrolyte can be reduced to about 1 to 2 times, and a composite layer with excellent surface smoothness can be easily obtained.
[0127] The viscosity of the polymer electrolyte solution is preferably 100 to 50,000 mPa s, and more preferably 300 to 10,000 mPa s. When the viscosity is in the above preferred range, the polymer electrolyte can be easily filled into the voids of the porous substrate, the thickness of the electrolyte membrane can be easily made uniform, and the surface smoothness of the electrolyte membrane is excellent.
[0128] The solvent used in the polymer electrolyte solution can be appropriately selected depending on the type of polymer. Examples of the solvent include aprotic polar solvents such as N,N-dimethylacetamide, N,N-dimethylformamide, N-methyl-2-pyrrolidone, dimethyl sulfoxide, sulfolane, 1,3-dimethyl-2-imidazolidinone, and hexamethylphosphontriamide, carbonate solvents such as ethylene carbonate and propylene carbonate, alkylene glycol monoalkyl ethers such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, propylene glycol monomethyl ether, and propylene glycol monoethyl ether, and alcohol solvents such as methanol, ethanol, propanol, and butanol. Suitable solvents include ketone solvents such as acetone, methyl ethyl ketone, and methyl isobutyl ketone, ester solvents such as γ-butyrolactone, ethyl acetate, butyl acetate, and ethyl lactate, hydrocarbon solvents such as hexane and cyclohexane, aromatic hydrocarbon solvents such as benzene, toluene, and xylene, halogenated hydrocarbon solvents such as chloroform, dichloromethane, 1,2-dichloroethane, perchloroethylene, chlorobenzene, and dichlorobenzene, ether solvents such as diethyl ether, tetrahydrofuran, and 1,4-dioxane, nitrile solvents such as acetonitrile, nitrated hydrocarbon solvents such as nitromethane and nitroethane, and water. A mixed solvent of two or more of these solvents may also be used.
[0129] The method for impregnating the porous substrate with the polymer electrolyte solution includes the following methods. (1) A method of controlling the membrane thickness by removing excess solution while pulling up a porous substrate immersed in a polymer electrolyte solution; (2) A method of casting a polymer electrolyte solution onto a porous substrate, (3) A method in which a porous substrate is attached to a supporting substrate on which a polymer electrolyte solution has been cast and then impregnated.
[0130] The solvent can be dried in the state where the impregnation is performed by the method (3). When the impregnation is performed by the method (1) or (2), the method of drying the solvent of the polymer electrolyte solution in a state where the porous substrate is attached to a separately prepared support substrate is preferable from the viewpoint of reducing wrinkles and unevenness in thickness of the electrolyte membrane and improving the membrane quality.
[0131] Applicable methods for casting and applying the polymer electrolyte solution include knife coating, direct roll coating, Mayer bar coating, gravure coating, reverse coating, air knife coating, spray coating, brush coating, dip coating, die coating, vacuum die coating, curtain coating, flow coating, spin coating, screen printing, inkjet coating, etc. Here, the device used for casting and applying the polymer electrolyte solution is called a coater.
[0132] After the polymer electrolyte solution is applied onto the substrate, a drying process is performed to form an electrolyte membrane. In the drying process, the coating film of the polymer electrolyte solution impregnated into the porous substrate is heated to evaporate the solvent. The heating means is not particularly limited as long as the solvent can be evaporated, and for example, a heating device such as an oven or heater, or a device that controls the temperature near the electrolyte membrane using infrared rays, hot air, or the like can be used. Heat may also be conducted to the coating film via the substrate. The heating temperature range is preferably close to the boiling point of the solvent and equal to or lower than the glass transition temperature of the electrolyte membrane. It is also possible to remove the solvent only by reducing pressure or introducing an air flow without heating.
[0133] The drying time and drying temperature in the drying step can be appropriately determined experimentally, but it is preferable to dry at least to the extent that the film can be a self-supporting film even when peeled off from the substrate. The drying method can be selected from known methods such as heating the substrate, hot air, and infrared heaters. The drying temperature is preferably 200°C or less, more preferably 150°C or less, taking into consideration the decomposition of the polymer electrolyte and surfactant.
[0134] The polymer electrolyte in the solution may be one in which the ionic group forms a salt with an alkali metal or alkaline earth metal cation. In this case, it is also preferable to have a step of exchanging the alkali metal or alkaline earth metal cation with a proton after forming a film on a substrate and drying the film. This step is more preferably a step of contacting the formed film with an acidic aqueous solution. Moreover, the contact is even more preferably a step of immersing the formed film in the acidic aqueous solution. In this step, the protons in the acidic aqueous solution are replaced with cations ionically bonded to the ionic group, and the remaining water-soluble impurities, residual monomers, solvents, residual salts, etc. are simultaneously removed. The acidic aqueous solution is not particularly limited, but it is preferable to use sulfuric acid, hydrochloric acid, nitric acid, acetic acid, trifluoromethanesulfonic acid, methanesulfonic acid, phosphoric acid, citric acid, etc. The temperature and concentration of the acidic aqueous solution should also be appropriately determined, but from the viewpoint of productivity, it is preferable to use an aqueous sulfuric acid solution of 3 mass% or more and 30 mass% or less at a temperature of 0 ° C. or more and 80 ° C. or less.
[0135] [Method for producing a catalyst-layered electrolyte membrane] The catalyst coated electrolyte membrane (hereinafter, CCM) of the present invention is formed by forming catalyst layers on both sides of the electrolyte membrane of the present invention. The method for forming the catalyst layers is not particularly limited, but a method of applying and drying a catalyst layer ink or a method of transferring a catalyst layer using a catalyst layer decal in which a catalyst layer is formed in advance on a decal base material and then drying the same is preferred because the process is simple and the process cost can be reduced.
[0136] In the case of the method of applying the catalyst layer ink, the application method is not particularly limited as long as it is a method that can apply the ink in the desired shape, and the methods described above in the application step of the polymer electrolyte solution can be used.
[0137] The solvent contained in the catalyst layer ink is not particularly limited as long as it is a solvent that disperses the polymer electrolyte and the catalyst-supported carbon particles, but a solvent that is easy to evaporate and remove by heating is preferable. For example, a solvent with a boiling point of 140° C. or less is preferable. Specific examples of the solvent for the catalyst layer ink include water, alcohols such as methanol, ethanol, propanol, butanol, and pentanol, ketones such as acetone, methyl ethyl ketone, pentanone, hexanone, heptanone, cyclohexanone, methylcyclohexanone, acetonylacetone, and diisobutyl ketone, ethers such as tetrahydrofuran, dioxane, diethylene glycol dimethyl ether, anisole, methoxytoluene, and dibutyl ether, esters such as methyl acetate, ethyl acetate, normal propyl acetate, isopropyl acetate, butyl acetate, methyl lactate, ethyl lactate, and butyl lactate, and other dimethylformamide, dimethylacetamide, N-methylpyrrolidone, ethylene glycol, diethylene glycol, diacetone alcohol, and 1-methoxy-2-propanol, which may be used alone or in combination.
[0138] In the case of the method of transferring using a catalyst layer decal, first, a catalyst layer ink is applied onto a substrate, and a drying process is performed as necessary to prepare a catalyst layer decal. Then, the electrolyte membrane is sandwiched between the catalyst layer decal on the cathode electrode side and the catalyst layer decal on the anode electrode side, and hot-pressed so that the surfaces of the decals on which the catalyst layers are provided are in contact with the electrolyte membrane, thereby obtaining an electrolyte membrane with a catalyst layer. The temperature and pressure of the hot press may be appropriately selected depending on the thickness of the electrolyte membrane, the moisture content, the catalyst layer, and the decal substrate, but from the viewpoints of industrial productivity and suppression of thermal decomposition of the electrolyte membrane material, it is preferable to perform the hot press at a temperature in the range of 0°C to 250°C, and more preferably at a temperature higher than the glass transition temperature of the polymer electrolyte contained in the catalyst layer and 200°C or lower. The pressure in the hot press is preferably as low as possible from the viewpoint of protecting the electrolyte membrane and the electrodes, and in the case of flat press, a pressure of 10 MPa or lower is preferable.
[0139] As the decal substrate used when applying the catalyst layer ink, a resin film or substrate similar to the substrate used when forming the electrolyte membrane can be used, as well as fluororesins such as PTFE, polyhexafluoropropylene, ETFE, ethylene-hexafluoropropylene copolymer, FEP, PFA, PVdF, etc. From the viewpoints of heat resistance, solvent resistance, chemical stability and releasability, it is preferable to use a fluororesin film.
[0140] The catalyst layer can be dried by the same method as described above for drying the polymer electrolyte solution.
[0141] The membrane electrode assembly of the present invention and the polymer electrolyte fuel cell of the present invention use the electrolyte membrane of the present invention. EXAMPLES
[0142] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these. The various measurement conditions are as follows.
[0143] (1) Molecular weight of the polymer The number average molecular weight and weight average molecular weight of the polymer solution were measured by GPC. Tosoh Corporation's HLC-8022GPC was used as an integrated device of an ultraviolet detector and a differential refractometer. Two Tosoh Corporation's TSK gel SuperHM-H (inner diameter 6.0 mm, length 15 cm) were used as GPC columns. Measurements were performed in N-methyl-2-pyrrolidone solvent (N-methyl-2-pyrrolidone solvent containing 10 mmol / L lithium bromide) at a flow rate of 0.2 mL / min, and the number average molecular weight and weight average molecular weight were calculated in terms of standard polystyrene.
[0144] (2) Ion exchange capacity (IEC) The measurement was performed by neutralization titration. The measurement was performed three times and the average value was taken.
[0145] After the proton exchange and thorough washing with pure water, the moisture on the surface of the electrolyte membrane was wiped off, and the membrane was vacuum dried at 100° C. for 12 hours or more, and the dry weight was determined.
[0146] 50 mL of a 5% by mass aqueous solution of sodium sulfate was added to the electrolyte membrane, and the membrane was allowed to stand for 12 hours for ion exchange.
[0147] The resulting sulfuric acid was titrated using 0.01 mol / L aqueous sodium hydroxide solution. A 0.1 w / v% commercially available phenolphthalein solution for titration was added as an indicator, and the end point was when the solution turned a light reddish purple color.
[0148] The ion exchange capacity (IEC) was calculated by the following formula.
[0149] IEC (meq / g) = [concentration of sodium hydroxide solution (mmol / mL) × amount dropped (mL)] / dry weight of sample (g) (3) Cross-sectional SEM measurement of electrolyte membrane Cross-sectional SEM measurement was carried out under the following conditions. From the obtained image, the white area in the center was regarded as the composite layer, and the black areas on both sides were regarded as separate outer layers, and their thicknesses were measured.
[0150] Equipment: Field emission scanning electron microscope (FE-SEM) S-4800 (Hitachi High-Technologies Corporation) Accelerating voltage: 2.0 kV Pretreatment: Cross-sectional samples prepared by the BIB method were coated with Pt and then measured.
[0151] BIB method: A cross-sectional specimen preparation device that uses an argon ion beam.
[0152] A shielding plate is placed directly above the sample, and a broad argon ion beam is irradiated from above to etch the sample, creating an observation surface / analysis surface (cross section).
[0153] (4) Filling rate of the polymer electrolyte in the composite layer (filling rate of the composite layer) According to the above item (3), the cross section of the electrolyte membrane was observed using SEM, and the thickness T1 of the composite layer consisting of the polymer electrolyte and the porous substrate, and the thicknesses T2 and T3 of other layers on the outside of the composite layer, if any, were calculated. The specific gravity of the polymer electrolyte forming the composite layer was designated D1, the specific gravity of the polymer electrolyte forming the other layer on the outside of the composite layer was designated D2 and D3, respectively, and the specific gravity of the electrolyte membrane was designated D. The IEC of the polymers forming each layer was designated I1, I2, I3, and the IEC of the electrolyte membrane was designated I, and the filling rate Y2 (volume %) of the polymer electrolyte in the composite layer was calculated by the following formula.
[0154] Y2=[(T1+T2+T3)×D×I-(T2×D2×I2+T3×D3×I3)] / (T1×D1×I1)×100 (5) Observation of phase-separated structures by transmission electron microscope (TEM) tomography A sample piece of the electrolyte membrane was immersed in a 2% by mass aqueous solution of lead acetate as a staining agent and left to stand at 25°C for 48 hours for staining. The stained sample was taken out, embedded in epoxy resin, and fixed by irradiating visible light for 30 seconds. A 100 nm thin section was cut using an ultramicrotome at room temperature and observed under the following conditions.
[0155] Equipment: High-resolution field emission electron microscope (HRTEM) JEM2100F manufactured by JEOL Ltd. Image acquisition: Digital Micrograph System: Marker method Accelerating voltage: 200kV Magnification: 30,000x Tilt angle: +61°~-62° Reconstruction resolution: 0.71nm / pixel The marker method was used for the 3D reconstruction process. Au colloidal particles applied to a collodion film were used as a positioning marker when performing 3D reconstruction. Using the marker as a reference, the sample was tilted at 1° intervals in the range of +61° to -62°, and TEM images were taken from a series of continuous tilt images. Based on the marker, CT reconstruction processing was performed based on a total of 124 TEM images, and the 3D phase separation structure was observed.
[0156] (6) Dimensional change rate by hot water test (λ xy )measurement The electrolyte membrane was cut into a square of about 5 cm x about 5 cm, and left to stand for 24 hours in a temperature- and humidity-controlled atmosphere of 23°C ± 5°C and 50±5% RH, after which the MD length and TD length (MD1 and TD1) were measured with a caliper. The electrolyte membrane was immersed in hot water at 80°C for 8 hours, and then the MD length and TD length (MD2 and TD2) were measured again with a caliper, and the dimensional change rate (λ) of MD and TD in the planar direction was calculated. MD and λ TD ) and the dimensional change rate in the planar direction (λ xy ) (%) was calculated according to the following formula:
[0157] λ MD =(MD2-MD1) / MD1×100 λ TD =(TD2-TD1) / TD1×100 λ xy =(λ MD +λ TD ) / 2.
[0158] (7) Proton conductivity The electrolyte membrane was immersed in pure water at 25°C for 24 hours, and then held in a thermohygrostat at 80°C and 25% RH for 30 minutes, and the proton conductivity was measured by a constant potential AC impedance method. As a measuring device, an electrochemical measuring system manufactured by Solartron (Solartron 1287 Electrochemical Interface and Solartron 1255B Frequency Response Analyzer) was used, and constant potential impedance measurement was performed by a two-terminal method to obtain the proton conductivity. The AC amplitude was 50 mV. A membrane with a width of 10 mm and a length of 50 mm was used as a sample. The measuring tool was made of phenolic resin, and the measuring part was left open. Platinum plates (thickness 100 μm, 2 sheets) were used as electrodes. The electrodes were arranged on the front and back sides of the sample membrane with an interelectrode distance of 10 mm, parallel to each other and perpendicular to the longitudinal direction of the sample membrane.
[0159] (8) Fabrication of membrane electrode assembly (MEA) using electrolyte membrane A catalyst ink was prepared by adjusting the mass ratio of platinum catalyst-supported carbon particles TEC10E50E (platinum support rate 50 mass%) manufactured by Tanaka Kikinzoku Kogyo Co., Ltd. and "Nafion" (registered trademark) manufactured by Chemours Corporation to 2:1, and the catalyst ink was applied to a commercially available polytetrafluoroethylene film with a platinum amount of 0.3 mg / cm. 2 A catalyst decal was prepared by applying the coating liquid as follows:
[0160] Two of the above catalyst decals were cut into 5 cm squares, stacked facing each other so as to sandwich the electrolyte membrane, and hot-pressed at 150°C and 5 MPa for 3 minutes to obtain an electrolyte membrane with a catalyst layer. A commercially available gas diffusion electrode 24BCH manufactured by SGL was cut into a 5 cm square and sandwiched the obtained electrolyte membrane with a catalyst layer to produce an MEA with one side as the cathode and the other as the anode.
[0161] (9) Wet / dry cycle durability The MEA prepared in (8) above was placed in a JARI standard cell Ex-1 (electrode area 25 cm) manufactured by Eiwa Co., Ltd. 2 ), and with the cell temperature at 80°C, nitrogen at 160% RH was supplied to both electrodes for two minutes, and then nitrogen at 0% RH (dew point below -20°C) was supplied to both electrodes for two minutes. The hydrogen permeation amount was measured every 1,000 cycles, and the point at which the hydrogen permeation current exceeded 10 times the initial current was regarded as the dry-wet cycle durability.
[0162] The hydrogen permeation amount was measured by supplying hydrogen as fuel gas to one electrode and nitrogen to the other electrode, and the test was performed under humidification conditions: hydrogen gas 90% RH, nitrogen gas: 90% RH. The open circuit voltage was held until it reached 0.2 V or less, and the voltage was swept from 0.2 to 0.7 V at 1 mV / sec, and the current value at 0.7 V was taken as the hydrogen permeation current.
[0163] (10) Measurement of fluorine atom content in porous substrate According to the following conditions, a porous substrate sample was weighed and burned in a combustion tube of an analyzer. The generated gas was absorbed in a solution, and then a portion of the absorbed solution was analyzed by ion chromatography.
[0164] <Combustion and absorption conditions> System: AQF-2100H, GA-210 (Mitsubishi Chemical Corporation) Electric furnace temperature: Inlet 900℃, Outlet 1000℃ Gas: Ar / O 2 200mL / min, O 2 400mL / min Absorbing liquid: H 2 O 2 0.1%, internal standard Br 8μg / mL Absorbed liquid volume: 20mL <Ion chromatography - anion analysis conditions> System: ICS1600 (DIONEX) Mobile phase: 2.7mmol / L Na 2 CO 3 / 0.3mmol / L NaHCO 3 Flow rate: 1.50mL / min Detector: Electrical conductivity detector Injection volume: 20μL (11) Chemical structure analysis of surfactants Infrared spectroscopy (IR) analysis, 1 H nuclear magnetic resonance (NMR) analysis, 19 F-NMR analysis, MALDI-MS analysis, and pyrolysis GC / MS analysis were performed to analyze the chemical structures of various surfactants, and the contents of fluorine atoms and hydrophilic elements (total of oxygen, nitrogen, phosphorus, sulfur, and boron) were calculated.
[0165] (12) Measurement of weight-average molecular weight of surfactants The weight average molecular weight of the surfactant was measured by gel permeation chromatography (GPC) analysis under the following conditions.
[0166] Apparatus: Gel permeation chromatography (GPC) (instrument no. GPC-27) Detector: UV-visible absorption spectrometer (Shimadzu Corporation SPD-20AV) Column: TSKgel Super HZM-N x 2 SuperHZ4000, 2500, 1000 each 1 piece Solvent: Tetrahydrofuran (THF) Flow rate: 0.45mL / min Column temperature: 40℃ Injection volume: 0.02mL Standard samples: Tosoh Corporation and Agilent monodisperse polyethylene glycol (PEG) Data processing: GPC data processing system manufactured by Toray Research Center, Inc. (13) Amount of surfactant contained in electrolyte membrane According to the following conditions, the electrolyte membrane was weighed and burned in the combustion tube of the analyzer, the generated gas was absorbed in a solution, and a part of the absorbed solution was analyzed by ion chromatography. The contribution of the surfactant was calculated by excluding the contribution of the polymer electrolyte not containing the surfactant, which was measured in advance, and the contribution of the porous substrate, which was measured in advance by (10), from this analytical value, and the amount of surfactant contained in the composite electrolyte membrane was calculated from the amount of fluorine atoms contained in the surfactant, and the ratio of the surfactant to the polymer electrolyte contained in the composite membrane (surfactant / polymer electrolyte) was obtained.
[0167] <Combustion and absorption conditions> System: AQF-2100H, GA-210 (Mitsubishi Chemical Corporation) Electric furnace temperature: Inlet 900℃, Outlet 1000℃ Gas: Ar / O 2 200mL / min, O 2 400mL / min Absorbing liquid: H 2 O 2 0.1%, internal standard Br 8μg / mL Absorbed liquid volume: 20mL <Ion chromatography - anion analysis conditions> System: ICS1600 (DIONEX) Mobile phase: 2.7mmol / L Na 2 CO 3 / 0.3mmol / L NaHCO 3 Flow rate: 1.50mL / min Detector: Electrical conductivity detector Injection volume: 20μL (14) Measurement of oxygen content in porous substrates using XPS A porous substrate cut into a 5 mm square was rinsed with ultrapure water, dried at room temperature and 67 Pa for 10 hours, cooled with liquid nitrogen for 30 minutes, and processed twice for 5 minutes in a freeze grinder to prepare a sample. The composition of the prepared sample was measured, and the oxygen atom content was calculated. The measurement device and conditions were as follows.
[0168] Measuring device: Quantera SXM Excited X-ray: monochromatic Al Kα 1 ,Kα 2 Rays (1,486.6 eV) X-ray diameter: 200μm Photoelectron escape angle: 45° (15) Mechanical properties of electrolyte membrane in dry state The electrolyte membrane to be tested was set in the device, and a tensile test was performed under the following conditions. The values of tensile strength and tensile elongation were taken as the values at the moment when the maximum point stress was shown during the test. The elastic modulus was taken as the value calculated to be maximum using any two points where the strain was 0.35%. When calculating the tensile modulus per width (N / cm), the force (N) output in the tensile test was divided by the membrane width (cm) to obtain the strength (N / cm), and the difference in strength (N / cm) at the two arbitrary points was further divided by a strain of 0.0035 (a dimensionless quantity) to obtain the tensile modulus per width (N / cm). When calculating the tensile modulus per cross-sectional area (MPa), the force (N) output in the tensile test was divided by the membrane cross-sectional area (mm 2 The stress (MPa) was calculated by dividing the difference in stress (MPa) between the two arbitrary points by the strain of 0.0035 (a dimensionless quantity), and the tensile modulus (MPa) per cross-sectional area was calculated. The maximum stress and modulus were calculated as the average value of five tests.
[0169] Measuring device: Autograph AG-IS (Shimadzu Corporation) Load range: 100N Pulling speed: 100mm / min Test piece: width 10mm x length 50mm Distance between samples: 30 mm Test temperature and humidity: 23±1℃, 60±10%RH Number of tests: n=5 (16) Mechanical properties of electrolyte membranes in a wet state The electrolyte membrane specimens were cut to the size of test pieces and immersed in ultrapure water at 23°C for 24 hours. A tensile test was then carried out under the same conditions and method as in (15), and the tensile strength, tensile elongation, and elastic modulus were calculated.
[0170] (17) Measurement of haze and diffuse transmittance The electrolyte membrane sample was cut to a size of 5 cm x 5 cm, and the haze measurement was performed under the following conditions. 1 , device scattering rate T 3 After determining the total light transmittance T 2 and the sample scattering rate T 4 Measure the diffuse transmittance T d and haze were calculated.
[0171] Measuring device: Haze meter HGM-20P (manufactured by Suga Test Instruments Co., Ltd.) (18) SEM Observation of Porous Substrate The porous substrate to be used as a specimen was cut to a size of 2 mm x 2 mm, and after platinum ion sputtering, SEM observation was performed to observe the morphology of the porous substrate in the planar direction. The orientation of the nodes and fibrils contained in the porous substrate was determined based on the structure observed during SEM observation in an arbitrary 15 μm x 15 μm range. The average diameter of the nodes and fibrils was calculated by measuring the diameter of the nodes and fibrils at 100 points in an arbitrary 15 μm x 15 μm range and calculating the average value. Ion sputtering and SEM observation were performed using the following equipment and conditions.
[0172] <Ion sputtering> Sputtering equipment: Ion sputter E-1045 (manufactured by Hitachi High-Technologies Corporation) Metal type: Pt Ion emission current: 15mA Sputtering time: 60 seconds <SEM observation> Measuring device: Scanning electron microscope S-5500 (manufactured by Hitachi High-Technologies Corporation) Accelerating voltage: 5 kV Observation magnification: 2,000 - 20,000 times [Synthesis Example 1] (Synthesis of 2,2-bis(4-hydroxyphenyl)-1,3-dioxolane (K-DHBP) represented by the following chemical formula (G1)) 49.5 g of 4,4'-dihydroxybenzophenone, 134 g of ethylene glycol, 96.9 g of trimethyl orthoformate, and 0.50 g of p-toluenesulfonic acid monohydrate were charged and dissolved in a 500 mL flask equipped with a stirrer, a thermometer, and a distillation tube. Then, the mixture was kept warm and stirred at 78 - 82 °C for 2 hours. Further, the internal temperature was gradually raised to 120 °C, and heating was continued until the distillation of methyl formate, methanol, and trimethyl orthoformate completely stopped. After the reaction solution was cooled to room temperature, the reaction solution was diluted with ethyl acetate, and the organic layer was washed with 100 mL of 5% aqueous potassium carbonate solution, separated, and the solvent was distilled off. 80 mL of dichloromethane was added to the residue to precipitate crystals, which were filtered and dried to obtain 52.0 g of 2,2-bis(4-hydroxyphenyl)-1,3-dioxolane represented by the following chemical formula (G1). When this crystal was analyzed by GC, it was found to be 99.9% 2,2-bis(4-hydroxyphenyl)-1,3-dioxolane and 0.1% 4,4'-dihydroxybenzophenone.
[0173] [Chemical formula]
[0174] [Synthesis Example 2] (Synthesis of disodium-3,3'-disulfonate-4,4'-difluorobenzophenone represented by the following chemical formula (G2)) 109.1 g of 4,4'-difluorobenzophenone (reagent from Sigma-Aldrich Japan) was added to fuming sulfuric acid (50% SO 3The mixture was reacted at 100°C for 10 hours in 150mL of ethyl acetate (Fujifilm Wako Pure Chemical Industries, Ltd.) reagent. The mixture was then poured little by little into a large amount of water, neutralized with NaOH, and 200g of table salt (NaCl) was added to precipitate the compound. The resulting precipitate was filtered and recrystallized with an aqueous ethanol solution to obtain disodium-3,3'-disulfonate-4,4'-difluorobenzophenone represented by the following chemical formula (G2). The purity was 99.3%.
[0175] [ka]
[0176] [Synthesis Example 3] (Synthesis of oligomer a1 not containing an ionic group represented by the following general formula (G3)) In a 1,000 mL three-neck flask equipped with a stirrer, a nitrogen inlet tube, and a Dean-Stark trap, 16.59 g (120 mmol) of potassium carbonate (Sigma-Aldrich Japan (same) reagent), 25.8 g (100 mmol) of K-DHBP obtained in the above Synthesis Example 1, and 20.3 g (93 mmol) of 4,4'-difluorobenzophenone (Sigma-Aldrich Japan (same) reagent) were placed. After nitrogen replacement, 300 mL of N-methylpyrrolidone (NMP) and 100 mL of toluene were added, dehydrated at 160 ° C, heated to remove toluene, and polymerized at 180 ° C for 1 hour. Reprecipitation purification was performed in a large amount of methanol to obtain an oligomer (terminal: hydroxyl group) that does not contain ionic groups. The number average molecular weight was 10,000.
[0177] In a 500mL three-neck flask equipped with a stirrer, nitrogen inlet tube, and Dean-Stark trap, 1.1g (8mmol) of potassium carbonate (Sigma-Aldrich Japan (same) reagent) and 20.0g (2mmol) of the oligomer (terminal: hydroxyl group) not containing an ionic group were placed, and after nitrogen replacement, 100mL of NMP and 30mL of toluene were added, dehydration was performed at 100°C, and the temperature was raised to remove toluene, and 4.0g (12mmol) of decafluorobiphenyl (Sigma-Aldrich Japan (same) reagent) was added, and the reaction was performed at 105°C for 1 hour. Purification was performed by reprecipitation with a large amount of isopropyl alcohol, and an oligomer a1 (terminal: fluoro group) not containing an ionic group represented by the following general formula (G3) was obtained. The number average molecular weight was 11,000.
[0178] [ka]
[0179] [Synthesis Example 4] (Synthesis of oligomer a2 containing an ionic group represented by the following general formula (G4)) A 1,000mL three-neck flask equipped with a stirrer, nitrogen inlet tube, and Dean-Stark trap was charged with 27.6g (200mmol) of potassium carbonate (Sigma-Aldrich Japan (same) reagent), 12.9g (50mmol) of K-DHBP obtained in Synthesis Example 1, 9.3g (50mmol) of 4,4'-biphenol (Sigma-Aldrich Japan (same) reagent), 39.3g (93mmol) of disodium-3,3'-disulfonate-4,4'-difluorobenzophenone obtained in Synthesis Example 2, and 17.9g (82mmol) of 18-crown-6 (Fujifilm Wako Pure Chemical Industries, Ltd. reagent), and after nitrogen replacement, 300mL of NMP and 100mL of toluene were added, and the mixture was dehydrated at 170°C, heated to remove toluene, and polymerization was carried out at 180°C for 1 hour. The product was purified by reprecipitation with a large amount of isopropyl alcohol to obtain an oligomer a2 (terminal: hydroxyl group) containing an ionic group represented by the following general formula (G4). The number average molecular weight was 16,000.
[0180] [ka]
[0181] (In general formula (G4), M represents H, Na or K.) [Synthesis Example 5] (Synthesis of neopentyl 3-(2,5-dichlorobenzoyl)benzenesulfonate represented by the following chemical formula (G5)) 245g (2.1mol) of chlorosulfonic acid was placed in a 3L three-neck flask equipped with a stirrer and a condenser, followed by 105g (420mmol) of 2,5-dichlorobenzophenone, and the mixture was allowed to react in a 100℃ oil bath for 8 hours. After the specified time, the reaction solution was slowly poured into 1,000g of crushed ice and extracted with ethyl acetate. The organic layer was washed with saline and dried over magnesium sulfate, after which the ethyl acetate was distilled off to obtain pale yellow crude crystals of 3-(2,5-dichlorobenzoyl)benzenesulfonic acid chloride. The crude crystals were used in the next step without purification.
[0182] 41.1 g (462 mmol) of 2,2-dimethyl-1-propanol (neopentyl alcohol) was added to 300 mL of pyridine and cooled to about 10°C. The crude crystals obtained above were gradually added thereto over about 30 minutes. After the entire amount was added, the mixture was stirred for another 30 minutes to react. After the reaction, the reaction solution was poured into 1,000 mL of hydrochloric acid water, and the precipitated solid was collected. The obtained solid was dissolved in ethyl acetate, washed with an aqueous solution of sodium bicarbonate and saline, dried over magnesium sulfate, and the ethyl acetate was distilled off to obtain crude crystals. This was recrystallized from methanol to obtain white crystals of 3-(2,5-dichlorobenzoyl)benzenesulfonate neopentyl represented by the following chemical formula (G5).
[0183] [ka]
[0184] [Synthesis Example 6] (Synthesis of an oligomer not containing an ionic group represented by the following general formula (G6)) In a 1L three-neck flask equipped with a stirrer, a thermometer, a cooling tube, a Dean-Stark tube, and a three-way cock for nitrogen introduction, 49.4g (0.29mol) of 2,6-dichlorobenzonitrile, 88.4g (0.26mol) of 2,2-bis(4-hydroxyphenyl)-1,1,1,3,3,3-hexafluoropropane, and 47.3g (0.34mol) of potassium carbonate were weighed out. After replacing with nitrogen, 346mL of sulfolane and 173mL of toluene were added and stirred. The flask was placed in an oil bath and heated to reflux at 150℃. The water generated by the reaction was azeotroped with toluene and removed from the system using a Dean-Stark tube, and the reaction was continued until almost no water was generated after about 3 hours. After removing most of the toluene while gradually increasing the reaction temperature, the reaction was continued at 200℃ for 3 hours. Next, 12.3 g (0.072 mol) of 2,6-dichlorobenzonitrile was added, and the mixture was further reacted for 5 hours.
[0185] The resulting reaction solution was allowed to cool, and then diluted with 100 mL of toluene. The precipitate of the by-product inorganic compound was removed by filtration, and the filtrate was poured into 2 L of methanol. The precipitated product was filtered, collected, dried, and dissolved in 250 mL of tetrahydrofuran. This was reprecipitated in 2 L of methanol to obtain 107 g of the target oligomer represented by the following general formula (G6). The number average molecular weight was 11,000.
[0186] [ka]
[0187] [Synthesis Example 7] (Synthesis of polyethersulfone (PES)-based block copolymer precursor b4' consisting of a segment represented by the following chemical formula (G8) and a segment represented by the following general formula (G9)) 1.62 g of anhydrous nickel chloride and 15 mL of dimethyl sulfoxide were mixed and adjusted to 70° C. 2.15 g of 2,2′-bipyridyl was added thereto and stirred at the same temperature for 10 minutes to prepare a nickel-containing solution.
[0188] Here, 1.49 g of 2,5-dichlorobenzenesulfonic acid (2,2-dimethylpropyl) and 0.50 g of Sumika Excel PES5200P (manufactured by Sumitomo Chemical Co., Ltd., Mn = 40,000, Mw = 94,000) represented by the following general formula (G7) were dissolved in 5 mL of dimethyl sulfoxide to obtain a solution, to which 1.23 g of zinc powder was added and adjusted to 70 ° C. The nickel-containing solution was poured into this, and a polymerization reaction was carried out at 70 ° C. for 4 hours. The reaction mixture was added to 60 mL of methanol, and then 60 mL of 6 mol / L hydrochloric acid was added and stirred for 1 hour. The precipitated solid was separated by filtration and dried, and 1.62 g of a block copolymer precursor b4' containing a gray-white segment represented by the following chemical formula (G8) and the following general formula (G9) was obtained in a yield of 99%. The weight average molecular weight was 230,000.
[0189] [ka]
[0190] [Synthesis Example 8] (Synthesis of Polybenzimidazole (PBI)) Under a nitrogen atmosphere, polyphosphoric acid (PAA) was used as the polymerization solvent, 22.7 g (106 mol) of 3,3'-diaminobenzidine (DAB) and 27.3 g (106 mol) of 4,4'-oxybisbenzoic acid (OBBA) were weighed out, and PAA was added so that the amount was 3 mass%, and the temperature was gradually increased while stirring, and the mixture was stirred at 140 ° C for 12 hours to perform polycondensation. After the reaction, the mixture was cooled to room temperature, poured into ion-exchanged water to solidify, and then neutralized with an aqueous sodium hydroxide solution. After filtering and washing with ion-exchanged water, the mixture was dried under reduced pressure at 80 ° C overnight to obtain the desired polybenzimidazole. The weight average molecular weight was 430,000. [Polymer electrolyte solution A] A polymer electrolyte solution comprising a block copolymer b1 obtained by copolymerizing an oligomer represented by the general formula (G4) as a segment containing an ionic group and an oligomer represented by the general formula (G3) as a segment not containing an ionic group. In a 500mL three-neck flask equipped with a stirrer, nitrogen inlet tube, and Dean-Stark trap, 0.56g (4mmol) of potassium carbonate (Sigma-Aldrich Japan (same) reagent) and 16g (1mmol) of oligomer a2 (terminal: hydroxyl group) containing an ionic group obtained in Synthesis Example 4 were placed, and after nitrogen replacement, 100mL of N-methylpyrrolidone (NMP) and 30mL of cyclohexane were added, and after dehydration at 100°C, the temperature was raised to remove cyclohexane, and 11g (1mmol) of oligomer a1 (terminal: fluoro group) not containing an ionic group obtained in Synthesis Example 3 was placed, and the reaction was carried out at 105°C for 24 hours. Block copolymer b1 was obtained by reprecipitation purification in a large amount of isopropyl alcohol. The weight average molecular weight was 340,000. The ion exchange capacity (IEC) of this block copolymer b1 was 2.1.
[0191] The obtained block copolymer b1 was dissolved in 5% by mass N-methylpyrrolidone (NMP) solution, and the polymerization stock solution was directly centrifuged at 25°C for 30 minutes at a centrifugal force of 20,000G in an inverter compact high-speed refrigerated centrifuge (model number 6930) manufactured by Kubota Manufacturing Co., Ltd., with an angle rotor RA-800. The precipitated solid (cake) and the supernatant liquid (coating liquid) were neatly separated, and the supernatant liquid was collected. Next, the mixture was distilled under reduced pressure at 80°C while stirring, and pressure filtered using a 1μm polypropylene filter to obtain polymer electrolyte solution A (polymer electrolyte concentration 13% by mass). The viscosity of polymer electrolyte solution A was 1,300mPa·s. [Polymer electrolyte solution B] A polymer electrolyte solution comprising a block copolymer b2 obtained by copolymerizing an oligomer represented by the general formula (G4) as a segment containing an ionic group and an oligomer represented by the general formula (G3) as a segment not containing an ionic group. Block copolymer b2 was synthesized in the same manner as for block copolymer b1, except that 20 g (1.25 mmol) of oligomer a2 having an ionic group obtained in Synthesis Example 4 was used. The weight average molecular weight of this block copolymer b2 was 370,000, and the ion exchange capacity (IEC) was 2.4. In addition, polymer electrolyte solution B, obtained in the same manner as polymer electrolyte solution A, except that block copolymer b2 was used instead of block copolymer b1, had a viscosity of 1,600 mPa s. [Polymer electrolyte solution C] A polymer electrolyte solution comprising a block copolymer b3 obtained by copolymerizing an oligomer represented by the general formula (G4) as a segment containing an ionic group and an oligomer represented by the general formula (G3) as a segment not containing an ionic group. Block copolymer b3 was synthesized in the same manner as for polymer electrolyte solution A, except that 25.6 g (1.6 mmol) of oligomer a2 having an ionic group obtained in Synthesis Example 4 was used. The weight average molecular weight of this block copolymer b3 was 390,000 and the ion exchange capacity (IEC) was 2.7. In addition, polymer electrolyte solution C, obtained in the same manner as polymer electrolyte solution A, except that block copolymer b3 was used instead of block copolymer b1, had a viscosity of 1,800 mPa s. [Polyelectrolyte solution D] Polyelectrolyte solution D consisting of random copolymers In a 5L reaction vessel equipped with a stirrer, nitrogen inlet tube, and Dean-Stark trap, 129g of 2,2-bis(4-hydroxyphenyl)-1,3-dioxolane synthesized in Synthesis Example 1, 93g of 4,4'-biphenol (Sigma-Aldrich Japan (same) reagent), and 422g (1.0mol) of disodium-3,3'-disulfonate-4,4'-difluorobenzophenone synthesized in Synthesis Example 2 were placed, and after nitrogen replacement, 3,000g of N-methyl-2-pyrrolidone (NMP), 450g of toluene, and 232g of 18-crown-6 (Fujifilm Wako Pure Chemical Co., Ltd. reagent) were added, and after confirming that all the monomers had dissolved, 304g of potassium carbonate (Sigma-Aldrich Japan (same) reagent) was added, and the mixture was dehydrated at 160°C while refluxing, and then heated to remove toluene, and desalting polycondensation was carried out at 200°C for 1 hour. The resulting random copolymer had a weight average molecular weight of 320,000 and an ion exchange capacity (IEC) of 2.1.
[0192] Next, NMP was added to dilute the polymerization stock solution so that the viscosity of the polymerization stock solution became 500 mPa·s, and the polymerization stock solution was directly centrifuged at 25°C for 30 minutes at a centrifugal force of 20,000 G with an angle rotor RA-800 attached to a Kubota Manufacturing Co., Ltd. inverter compact high-speed refrigerated centrifuge (model number 6930). The precipitated solid (cake) and the supernatant liquid (coating liquid) were neatly separated, so the supernatant liquid was collected. Next, the mixture was distilled under reduced pressure at 80°C while stirring to remove NMP until the polymer concentration became 14% by mass, and then pressure-filtered through a 5 μm polyethylene filter to obtain polymer electrolyte solution D. The viscosity of this polymer electrolyte solution D was 1,000 mPa·s. [Polymer electrolyte solution E] A polymer electrolyte solution comprising a polyarylene-based block copolymer represented by the following general formula (G10): 540 mL of dry N,N-dimethylacetamide (DMAc) was added under nitrogen to a mixture of 135.0 g (0.336 mol) of neopentyl 3-(2,5-dichlorobenzoyl)benzenesulfonate, 40.7 g (5.6 mmol) of the oligomer not containing an ionic group represented by general formula (G6) synthesized in Synthesis Example 6, 6.71 g (16.8 mmol) of 2,5-dichloro-4'-(1-imidazolyl)benzophenone, 6.71 g (10.3 mmol) of bis(triphenylphosphine)nickel dichloride, 35.9 g (0.137 mol) of triphenylphosphine, 1.54 g (10.3 mmol) of sodium iodide, and 53.7 g (0.821 mol) of zinc.
[0193] The reaction system was heated with stirring (finally heated to 79°C) and reacted for 3 hours. An increase in viscosity in the system was observed during the reaction. The polymerization reaction solution was diluted with 730 mL of DMAc, stirred for 30 minutes, and filtered using Celite as a filter aid.
[0194] The filtrate was concentrated with an evaporator, 43.8 g (0.505 mol) of lithium bromide was added to the filtrate, and the mixture was reacted at an internal temperature of 110° C. for 7 hours under a nitrogen atmosphere. After the reaction, the mixture was cooled to room temperature and poured into 4 L of acetone to coagulate. The coagulated product was collected by filtration, air-dried, pulverized in a mixer, and washed with 1,500 mL of 1N hydrochloric acid while stirring. After filtration, the product was washed with ion-exchanged water until the pH of the washing solution became 5 or more, and then dried overnight at 80° C. to obtain 23.0 g of the desired polyarylene-based block copolymer. The weight-average molecular weight of the polyarylene-based block copolymer after deprotection was 190,000, and the ion exchange capacity (IEC) was 2.0. The obtained polyarylene-based block copolymer was dissolved in an organic solvent of N-methyl-2-pyrrolidone / methanol=30 / 70 (mass%) so as to be 0.1 g / g, to obtain a polymer electrolyte solution E. The viscosity of polymer electrolyte solution E was 1,200 mPa·s.
[0195] [ka]
[0196] [Polymer electrolyte solution F] Polymer electrolyte solution F made of polyethersulfone-based block copolymer 0.23 g of the block copolymer precursor b4' obtained in Synthesis Example 7 was weighed out and added to a mixed solution of 0.16 g of lithium bromide monohydrate and 8 mL of NMP, and reacted at 120°C for 24 hours. The reaction mixture was poured into 80 mL of 6 mol / L hydrochloric acid and stirred for 1 hour. The precipitated solid was separated by filtration. The separated solid was dried to obtain a gray-white block copolymer b4 consisting of a segment represented by the general formula (G9) and a segment represented by the following chemical formula (G11). The weight average molecular weight of the obtained polyethersulfone-based block copolymer was 190,000, and the ion exchange capacity (IEC) was 2.0. The obtained polyethersulfone-based block copolymer was dissolved in an organic solvent of N-methyl-2-pyrrolidone / methanol = 30 / 70 (mass%) so as to have a concentration of 0.1 g / g, to obtain a polymer electrolyte solution F. The viscosity of the polymer electrolyte solution F was 1,300 mPa·s.
[0197] [ka]
[0198] [Porous polytetrafluoroethylene (ePTFE) substrate P1] "POREFLON" (registered trademark) WP-010-80 (manufactured by Sumitomo Electric Fine Polymer Co., Ltd.) was stretched 10 times in the horizontal direction and then heat-treated at 365°C. It was then stretched twice in the vertical direction to produce an ePTFE porous substrate P1 with a film thickness of 9 μm and a porosity of 80%. SEM observation revealed a structure having nodes with an average diameter of 0.9 μm approximately parallel to the vertical direction and fibrils with an average diameter of 0.2 μm approximately parallel to the horizontal direction. [Polytetrafluoroethylene (ePTFE) porous substrate P2] "POREFLON" (registered trademark) HP-045-30 (manufactured by Sumitomo Electric Fine Polymer Co., Ltd.) was simultaneously biaxially stretched 3 times in the lengthwise and widthwise directions to produce an ePTFE porous substrate P2 with a film thickness of 8 μm and a porosity of 89%. SEM observation revealed a structure in which fibrils with an average diameter of 0.3 μm formed an irregular spider web shape. [Hydrophilized ePTFE porous base material P2'] In a glove box with a dew point of -80°C, ePTFE porous substrate B was immersed in a solution consisting of 30 g of a 1% solution of metallic sodium-naphthalene complex / tetrahydrofuran (THF) and 70 g of THF, and after 3 seconds was removed and immediately washed thoroughly with THF to produce a hydrophilized ePTFE porous substrate P2' with a film thickness of 8 μm and a porosity of 88%. [Porous substrate P3 made of PBI fibers] The PBI obtained in Synthesis Example 8 was dissolved in dimethyl sulfoxide (DMSO) to a concentration of 8% by weight, and spun using an electrospinning unit manufactured by Kato Tech Co., Ltd. under conditions of a voltage of 20 kV, a syringe pump discharge rate of 0.12 mL / hour, and a distance between the syringe and the target of 100 mm, and a nanofiber nonwoven fabric was simultaneously produced. The obtained nanofiber nonwoven fabric was dried under reduced pressure at 80°C for 1 hour, and then laminated on a 125 μm thick "Kapton" (registered trademark) substrate and heated at 400°C for 10 minutes in a nitrogen atmosphere to obtain a porous substrate P3 made of PBI fibers with an average fiber diameter of 160 nm and a thickness of 7 μm. The porosity was 86%. [Porous polytetrafluoroethylene (ePTFE) substrate P4] "Tetratex" (registered trademark) TX1356 (manufactured by Donaldson Co.) was used as the porous substrate P4. The film thickness was 8 μm and the porosity was 85%.
[0199] <Production of electrolyte membrane> [Example 1] 0.26 g of polyoxyethylene ether surfactant "Ftergent" (registered trademark) 208G (manufactured by Neos Co., Ltd.) (fluorine atom content 54 mass%, hydrophilic element content 11 mass%, weight average molecular weight 1,800) was dissolved in 100 g of polymer electrolyte solution A to prepare an electrolyte-surfactant mixed solution with a mass ratio of polymer electrolyte to surfactant (hereinafter "surfactant / electrolyte") of 0.02. Using a knife coater, this electrolyte-surfactant mixed solution was cast onto a glass substrate, and the ePTFE porous substrate P1 was attached. After holding at room temperature for 1 hour, the ePTFE porous substrate P1 was sufficiently impregnated with the electrolyte-surfactant mixed solution A, and then dried at 100 ° C. for 4 hours. The electrolyte-surfactant mixed solution A was cast onto the upper surface of the dried membrane again, held at room temperature for 1 hour, and then dried at 100 ° C. for 4 hours to obtain a film-like polymer. After immersing in a 10% by mass aqueous sulfuric acid solution at 80° C. for 24 hours to carry out proton exchange and deprotection reactions, the membrane was thoroughly washed by immersing in a large excess of pure water for 24 hours to obtain an electrolyte membrane (thickness: 9 μm). [Example 2] An electrolyte membrane (thickness: 9 μm) was obtained in the same manner as in Example 1, except that an electrolyte-surfactant mixed solution with a surfactant / electrolyte ratio of 0.10 was used. [Example 3] An electrolyte membrane (thickness: 9 μm) was obtained in the same manner as in Example 1, except that an electrolyte-surfactant mixed solution with a surfactant / electrolyte ratio of 0.01 was used. [Example 4] An electrolyte membrane (thickness: 9 μm) was obtained in the same manner as in Example 1, except that polymer electrolyte solution B was used instead of polymer electrolyte solution A. [Example 5] An electrolyte membrane (thickness: 9 μm) was obtained in the same manner as in Example 1, except that polymer electrolyte solution C was used instead of polymer electrolyte solution A. [Example 6] An electrolyte membrane (thickness: 10 μm) was obtained in the same manner as in Example 1, except that polymer electrolyte solution D was used instead of polymer electrolyte solution A. [Example 7] An electrolyte membrane (thickness: 10 μm) was obtained in the same manner as in Example 1, except that polymer electrolyte solution E was used instead of polymer electrolyte solution A. [Example 8] An electrolyte membrane (thickness: 10 μm) was obtained in the same manner as in Example 1, except that polymer electrolyte solution F was used instead of polymer electrolyte solution A. [Example 9] An electrolyte membrane (thickness: 10 μm) was obtained in the same manner as in Example 1, except that a polyoxyethylene ether surfactant "Ftergent" (registered trademark) FTX-218 (manufactured by Neos Corporation) (fluorine atom content: 46% by mass, hydrophilic element content: 14% by mass, weight average molecular weight: 1,900) was used instead of "Ftergent" (registered trademark) 208G. [Example 10] An electrolyte membrane (thickness 10 μm) was obtained in the same manner as in Example 1, except that a low metal-containing grade polyoxyethylene ether surfactant "Ftergent" (registered trademark) DFX-18 (manufactured by Neos Co., Ltd.) (fluorine atom content 46 mass%, hydrophilic element content 14 mass%, weight average molecular weight 1,900) was used instead of "Ftergent" (registered trademark) 208G. [Example 11] An electrolyte membrane (thickness 10 μm) was obtained in the same manner as in Example 1, except that a fluorine-containing hydrophilic group / lipophilic group-containing oligomer surfactant "Ftergent" (registered trademark) 710FS (manufactured by Neos Corporation) (fluorine atom content 16 mass%, hydrophilic element content 30 mass%, weight average molecular weight 3,500) was used instead of "Ftergent" (registered trademark) 208G. [Example 12] An electrolyte membrane (thickness: 8 μm) was obtained in the same manner as in Example 1, except that the ePTFE porous substrate P2 was used instead of the ePTFE porous substrate P1. [Example 13] An electrolyte membrane (thickness 9 μm) was obtained in the same manner as in Example 1, except that a fluorine-containing hydrophilic group / lipophilic group-containing oligomer surfactant "Megafac" (registered trademark) F-555 (manufactured by DIC Corporation) was used instead of "Ftergent" (registered trademark) 208G. [Example 14] Using a knife coater, the polymer electrolyte solution A was cast onto a glass substrate, and the PBI porous substrate P3 was attached. The substrate was held at room temperature for 1 hour to allow the PBI porous substrate P3 to be fully impregnated with the polymer electrolyte solution A, and then dried at 100°C for 4 hours. The polymer electrolyte solution A was cast onto the upper surface of the dried membrane again, held at room temperature for 1 hour, and then dried at 100°C for 4 hours to obtain a film-like polymer. The substrate was immersed in a 10% by mass aqueous sulfuric acid solution at 80°C for 24 hours to carry out proton substitution and deprotection reactions, and then immersed in a large excess of pure water for 24 hours to thoroughly wash the substrate, obtaining an electrolyte membrane (film thickness 8 μm). [Example 15] An electrolyte membrane (thickness: 9 μm) was obtained in the same manner as in Example 1, except that the ePTFE porous substrate P4 was used instead of the ePTFE porous substrate P1. [Comparative Example 1] Using a knife coater, 100 g of the polymer electrolyte solution A was cast onto a glass substrate, and then dried at 100° C. for 4 hours to obtain a film-like polymer. The polymer was then immersed in a 10% by mass aqueous sulfuric acid solution at 80° C. for 24 hours to carry out proton substitution and deprotection reactions, and then immersed in a large excess of pure water for 24 hours to thoroughly wash the polymer, obtaining an electrolyte membrane (thickness: 10 μm). [Comparative Example 2] An attempt was made to prepare an electrolyte membrane in the same manner as in Example 1, except that "Ftergent" (registered trademark) 208G was not used. However, the polymer electrolyte solution A did not penetrate into the porous substrate, and an electrolyte membrane could not be obtained. [Comparative Example 3] An electrolyte membrane (thickness: 10 μm) was obtained in the same manner as in Comparative Example 1, except that polymer electrolyte solution B was used instead of polymer electrolyte solution A. [Comparative Example 4] An electrolyte membrane (thickness: 10 μm) was obtained in the same manner as in Comparative Example 1, except that polymer electrolyte solution C was used instead of polymer electrolyte solution A. [Comparative Example 5] An electrolyte membrane (thickness: 8 μm) was obtained in the same manner as in Example 5, except that the ePTFE porous substrate P2 was used instead of the ePTFE porous substrate P1. [Comparative Example 6] An electrolyte membrane (thickness: 10 μm) was obtained in the same manner as in Comparative Example 1, except that polymer electrolyte solution D was used instead of polymer electrolyte solution A. [Comparative Example 7] An electrolyte membrane (thickness: 10 μm) was obtained in the same manner as in Comparative Example 1, except that polymer electrolyte solution E was used instead of polymer electrolyte solution A. [Comparative Example 8] A composite electrolyte membrane (thickness: 10 μm) was obtained in the same manner as in Comparative Example 1, except that polymer electrolyte solution F was used instead of polymer electrolyte solution A. [Comparative Example 9] An electrolyte membrane (thickness: 10 μm) was obtained in the same manner as in Comparative Example 2, except that a hydrophilized ePTFE porous substrate P2′ was used instead of the ePTFE porous substrate P1. [Comparative Example 10] An attempt was made to prepare an electrolyte membrane in the same manner as in Example 1, except that a surfactant "Triton" (registered trademark) X-100 (non-fluorinated surfactant) (fluorine atom content: 0, hydrophilic element content: 27% by mass, weight average molecular weight: 700) was used instead of "Ftergent" (registered trademark) 208G. However, the polymer electrolyte solution A did not penetrate into the porous substrate, and an electrolyte membrane could not be obtained. [Comparative Example 11] An electrolyte membrane (thickness 10 μm) was obtained in the same manner as in Example 1, except that a surfactant perfluorooctane sulfonic acid (PFOS) (anionic fluorosurfactant) (fluorine atom content 65 mass%, hydrophilic element content 16 mass%, weight average molecular weight 500) was used instead of "Ftergent" (registered trademark) 208G.
[0200] The electrolyte membranes produced in Examples 1 to 12, Comparative Example 1, Comparative Examples 3 to 9, and Comparative Example 11 were measured for ion exchange capacity (IEC), polymer electrolyte filling rate in the composite layer, and dimensional change rate λ xyThe properties of the electrolyte membrane were evaluated, including proton conductivity, mechanical properties in a dry state, mechanical properties in a wet state, haze, diffuse transmittance, and wet / dry cycle durability. The ionic group-containing polymer membrane that constitutes the electrolyte membrane was evaluated for the presence or absence of a phase separation structure, and the porous substrate was evaluated for its fluorine atom content, oxygen atom content, and porosity. The results of these evaluations are shown in Tables 1 and 2. Regarding wet / dry cycle durability, in cases where the hydrogen permeation current did not exceed 10 times the initial current even after 20,000 cycles, the evaluation was discontinued at 20,000 cycles.
[0201] [Table 1]
[0202] Note 1) Polymer electrolyte A: block copolymer b1, polymer electrolyte B: block copolymer b2, polymer electrolyte C: block copolymer b3, polymer electrolyte D: random copolymer, polymer electrolyte E: polyarylene-based block copolymer, polymer electrolyte F: polyethersulfone-based block copolymer b4 Note 2) Porous substrate P1: Polytetrafluoroethylene (ePTFE) with a thickness of 9 μm and a porosity of 80%. Porous substrate P2: Polytetrafluoroethylene (ePTFE) with a thickness of 8 μm and a porosity of 89%. Porous substrate P2': Hydrophilic ePTFE with a thickness of 8 μm and a porosity of 88%. Porous substrate P3: Polybenzimidazole (PBI) with a thickness of 7 μm and a porosity of 86%. Porous substrate P4: Polytetrafluoroethylene (ePTFE) with a thickness of 8 μm and a porosity of 85%.
[0203] [Table 2] [Industrial Applicability]
[0204] The electrolyte membrane of the present invention can be applied to various applications. For example, it can be applied to medical applications such as artificial skin, filtration applications, ion exchange resin applications such as chlorine-resistant reverse osmosis membranes, various structural material applications, electrochemical applications, humidification membranes, anti-fogging membranes, antistatic membranes, oxygen removal membranes, solar cell membranes, and gas barrier membranes. Among them, it can be preferably used for various electrochemical applications. Examples of electrochemical applications include solid polymer fuel cells, redox flow batteries, water electrolysis devices, chloroalkali electrolysis devices, electrochemical hydrogen pumps, and water electrolysis hydrogen generation devices.
[0205] In solid polymer electrolyte fuel cells, electrochemical hydrogen pumps, and water electrolysis hydrogen generation devices, the electrolyte membrane is used with a catalyst layer, an electrode substrate, and a separator laminated in sequence on both sides. In particular, an electrolyte membrane with a catalyst layer and a gas diffusion substrate laminated in sequence on both sides (i.e., a layer structure of gas diffusion substrate / catalyst layer / electrolyte membrane / catalyst layer / gas diffusion substrate) is called a membrane electrode assembly (MEA). The electrolyte membrane of the present invention is suitably used as the electrolyte membrane constituting the CCM and MEA.
Claims
1. A composite polymer electrolyte membrane comprising a polymer electrolyte and a porous substrate, the composite polymer electrolyte membrane having a dry tensile modulus per width of 100 N / cm or more and a wet tensile modulus per width of 35 N / cm or more.
2. 2. The polymer electrolyte composite membrane according to claim 1, having a wet tensile modulus per cross-sectional area of 400 MPa or more.
3. 3. The polymer electrolyte composite membrane according to claim 1, wherein the wet tensile modulus / dry tensile modulus is 0.3 or more.
4. 4. The composite polymer electrolyte membrane according to claim 1, which has a wet tensile elongation at break of 60% or more.
5. 5. The composite polymer electrolyte membrane according to claim 1, which has a wet tensile breaking strength of 5 N / cm or more.
6. The composite polymer electrolyte membrane according to any one of claims 1 to 5, wherein the porous substrate is a fluorine-containing porous substrate.
7. 7. The composite polymer electrolyte membrane according to claim 1, wherein the oxygen atom content of the porous substrate is 10% by mass or less.
8. 8. The composite polymer electrolyte membrane according to claim 1, wherein the polymer electrolyte is a hydrocarbon polymer having an ionic group.
9. The composite polymer electrolyte membrane according to any one of claims 1 to 8, further comprising a nonionic fluorine-based surfactant.
10. 10. The composite polymer electrolyte membrane according to claim 9, wherein the nonionic fluorine-based surfactant is a compound having a fluorine-containing group consisting of a fluorinated alkyl group, a fluorinated alkenyl group or a fluorinated aryl group, and a nonionic solvent-philic group.
11. 6. The composite polymer electrolyte membrane according to claim 1, wherein the porous substrate is an aromatic hydrocarbon-based porous substrate.
12. The composite polymer electrolyte membrane according to claim 11 , wherein the porous substrate is a polyazole-based porous substrate.
13. 13. The composite polymer electrolyte membrane according to claim 11, wherein the porous substrate is made of polybenzimidazole.
14. 14. The composite polymer electrolyte membrane according to claim 1, which has a haze value of 20% or more and 45% or less when a light beam is transmitted through the membrane in the thickness direction.
15. 15. The composite polymer electrolyte membrane according to claim 1, which has a diffuse transmittance of 20% or more and 40% or less when a light beam is transmitted through the membrane in the thickness direction.
16. 16. A catalyst layer-attached composite polymer electrolyte membrane comprising the composite polymer electrolyte membrane according to claim 1 and catalyst layers sandwiched between both sides of the membrane.
17. A membrane electrode assembly comprising the composite polymer electrolyte membrane according to any one of claims 1 to 15.
18. A solid polymer fuel cell comprising the composite polymer electrolyte membrane according to any one of claims 1 to 15.
Citation Information
Patent Citations
Polymer electrolyte composite membrane, its manufacturing method and solid polymer type fuel cell using it
JP2005166557A
Composite membrane consisting of partial element
JP2005342718A
Reinforced electrolyte membrane for fuel cell, membrane-electrode conjugant for fuel cell, and solid polymer fuel cell equipped with the conjugant
JP2008288193A
Composite polyelectrolyte membrane
JP2013062240A
Composite membrane and method for producing the same
JP2015028850A