Light-shielding packaging
The laminated film with a white and silver layer integration in light-shielding packaging simplifies manufacturing, enhances visibility, and maintains effective light-shielding properties, addressing the complexity and visibility issues of conventional multi-layered solutions.
Patent Information
- Application Number
- JP2021009526
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-01-25
- Publication Date
- 2024-10-02
- Estimated Expiration
- 2041-01-25
AI Technical Summary
Conventional light-shielding packaging materials require multiple layers, increasing manufacturing steps and thickness, which complicates production and reduces visibility, while single-layer solutions compromise visibility or light-shielding effectiveness.
A laminated film structure with a white layer and a silver layer, each printed on the entire surface, providing high light-shielding properties and maintaining visibility, while reducing manufacturing steps by integrating these layers into a single package.
The laminated film structure achieves high light-shielding properties with reduced manufacturing complexity, maintaining interior visibility and allowing for metal detection and microwave heating, thus optimizing production efficiency and functionality.
Smart Images

Figure 0007559572000002 
Figure 0007559572000003 
Figure 0007559572000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a light-shielding package having light-shielding properties. [Background technology]
[0002] In order to prevent the deterioration of the contents due to light, packaging of medicines and food products using light-shielding packaging materials is required. Light-shielding properties can be obtained by including metal foil in the packaging material that forms the light-shielding packaging material. However, when used for medicines, there is a problem that metal detection for foreign matter cannot be used, and when used for food products, there is a problem that the packaging material cannot be heated in a microwave oven. For this reason, Patent Document 1 discloses a packaging material that has a light-shielding layer made of a resin that contains a light-shielding agent.
[0003] This packaging material has a thermal adhesive resin layer on the inner surface, and a first shielding layer, a light-shielding layer, and a second shielding layer are provided below the picture-printed layer. The first shielding layer is formed by printing with white ink, and shields the darkness caused by the color of the light-shielding layer, preventing a decrease in the color development of the picture-printed layer. The light-shielding layer is made of a resin containing a black shielding agent or a black and white shielding agent. The second shielding layer is made of a resin containing a white light-shielding agent. Placing the second shielding layer on the inner side of the light-shielding layer can improve the visibility of the inside of the package, and placing the light-shielding layer on the inner side of the second shielding layer can further shield the darkness caused by the color of the light-shielding layer. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2019-177948 A (pages 3-10, Figure 16) Summary of the Invention [Problem to be solved by the invention]
[0005] However, the conventional packaging materials described above have a problem in that the provision of a light-shielding layer requires a first and second shielding layer, which increases the number of steps required to manufacture the packaging material and the light-shielding packaging bag. In addition, when the second shielding layer is disposed on the inner side of the light-shielding layer, the thickness of the first shielding layer must be increased, which increases the number of steps required to manufacture the packaging material and the light-shielding packaging bag. On the other hand, when the light-shielding layer is disposed on the inner side of the second shielding layer, visibility of the inside of the package is reduced.
[0006] An object of the present invention is to provide a light-shielding package that provides good visibility of the inside and can reduce the number of manufacturing steps. [Means for solving the problem]
[0007] In order to achieve the above-mentioned object, the present invention provides a light-blocking packaging material formed of a laminated film having a thermal adhesive resin layer arranged on the inner surface, a picture printed layer forming a picture, and a light-blocking printed layer arranged on the inner side of the picture printed layer, and having a storage section for contents, wherein the light-blocking printed layer has a white layer formed by solid printing of white ink over the entire surface of the storage section, and a silver layer arranged on the inner side of the white layer and by solid printing of silver ink over the entire surface of the storage section, the white layer having a maximum transmittance of 40 to 44% for light having a wavelength of 300 to 800 nm, and the silver layer having a silver microparticle content of 37 to 47% by weight.
[0008] The present invention is also characterized in that, in the light-blocking packaging body of the above-mentioned configuration, the laminate is formed by sequentially laminating a first base material layer on which a gas-barrier transparent vapor-deposited film is vapor-deposited, a second base material layer, and the thermal adhesive resin layer, and the picture printed layer and the light-blocking printed layer are provided on the first base material layer.
[0009] The present invention is also characterized in that, in the light-blocking packaging body of the above-mentioned configuration, the laminate is formed by sequentially laminating a first base material layer on which a gas-barrier transparent vapor-deposited film is vapor-deposited, a second base material layer, and the thermal adhesive resin layer, and the picture printing layer and the light-blocking printing layer are provided on the second base material layer.
[0010] The present invention is also characterized in that, in the light-blocking packaging body of the above configuration, the laminated film is formed by sequentially laminating a first base material layer on which a gas-barrier transparent vapor-deposited film is vapor-deposited, a second base material layer, and the thermal adhesive resin layer, the pattern printed layer and the white layer being provided on the first base material layer, and the silver layer being provided on the second base material layer.
[0011] Furthermore, in the light-shielding packaging material of the present invention having the above-mentioned structure, the thickness of the white layer is 80 to 120% of the thickness of the silver layer. Effect of the Invention
[0012] According to the present invention, the light-blocking printed layer has a white layer solidly printed with white ink and a silver layer solidly printed with silver ink. Therefore, the two layers of the white layer and the silver layer provide high light-blocking properties and prevent a decrease in the color development of the picture-printed layer. This allows the manufacturing process of the light-blocking package to be reduced. In addition, the silver layer can increase the visibility of the inside of the storage section. [Brief description of the drawings]
[0013] [Figure 1] FIG. 1 is a perspective view showing a light-shielding package according to a first embodiment of the present invention; [Diagram 2] FIG. 1 is a cross-sectional view showing a laminated film forming a light-shielding package according to a first embodiment of the present invention. [Diagram 3] FIG. 11 is a cross-sectional view showing a laminated film forming a light-shielding package according to a second embodiment of the present invention. [Figure 4] FIG. 3 is a cross-sectional view showing a laminated film forming a light-shielding package according to a third embodiment of the present invention. [Diagram 5] FIG. 11 is a cross-sectional view showing a laminated film forming a light-shielding package according to a fourth embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] First Embodiment Hereinafter, an embodiment of the present invention will be described with reference to the drawings. Fig. 1 shows a perspective view of a light-shielding package according to the first embodiment. The light-shielding package 1 is a three-sided sealed bag having an opening 1a at the top end, and the contents such as food and medicine are stored in the storage section 5.
[0015] The light-shielding package 1 is formed by thermally bonding three peripheral sides (both side edges and bottom side) of two laminated films 10 with a sealing section 3. Alternatively, one laminated film 10 may be folded and two peripheral sides (both side edges) may be thermally bonded with a sealing section 3. After filling the light-shielding package 1 with the contents, the opening 1a is sealed by thermal bonding.
[0016] 2 shows a cross-sectional view of the laminated film 10. The laminated film 10 includes a first base material layer 11, a picture printed layer 14, a light-shielding printed layer 15, a second base material layer 20, and a thermal adhesive resin layer 22, in that order from the outer surface side.
[0017] The first base layer 11 is formed by depositing a transparent deposition film 11a on the inner surface of a base film made of resin. The base film may be made of polyester resin, polyamide resin, polyolefin resin, or a mixture of these. Specifically, a biaxially oriented polyethylene terephthalate film, a biaxially oriented nylon film, or the like may be used. The base film may also be a multi-layer film in which multiple resin films are laminated. The thickness of the first base layer 11 is about 5 to 50 μm.
[0018] The transparent vapor deposition film 11a is formed by vapor deposition of an oxide such as aluminum oxide or silicon oxide. This gives the light-shielding packaging body 1 gas barrier properties. Therefore, the light-shielding packaging body 1 for pharmaceutical use, which requires gas barrier properties, can be subjected to metal detection for foreign matter detection, and the light-shielding packaging body 1 for food use can be heated in a microwave oven.
[0019] The pattern-printed layer 14 is formed by printing a pattern on the first base layer 11 with a plurality of inks. The pattern-printed layer 14 can be printed by gravure printing, offset printing, letterpress printing, screen printing, or the like.
[0020] The light-shielding printed layer 15 is printed on the inner surface of the picture printed layer 14 by gravure printing, offset printing, letterpress printing, screen printing, or the like, and includes a white layer 15a and a silver layer 15b. The white layer 15a is formed by solid printing on the entire surface of the laminated film 10 with a white ink containing white fine particles such as titanium oxide, a hardener, and an anti-blocking agent. The silver layer 15b is disposed on the inner surface of the white layer 15a, and is formed by solid printing on the entire surface of the laminated film 10 with a silver ink containing silver fine particles of metal such as aluminum, a hardener, and an anti-blocking agent. It is sufficient that the white layer 15a and the silver layer 15b are solid printed on at least the entire surface of the storage section 5.
[0021] The light-shielding printed layer 15 can block light entering the storage section 5 from the outside. In addition, the white layer 15a arranged under the picture-printed layer 14 forms the background of the picture and blocks the darkness caused by the color of the silver layer 15b, thereby preventing a decrease in the color development of the picture-printed layer 14.
[0022] The amount of white ink applied to the white layer 15a and the amount of silver ink applied to the silver layer 15b are, for example, 6 g / m in a wet state. 2 The white layer 15a and the silver layer 15b are each printed in one coat and have approximately the same thickness. Therefore, the thickness of the white layer 15a is in the range of 80% to 120% of the thickness of the silver layer 15b.
[0023] The white layer 15a is formed with a maximum transmittance of 40-44% for light with a wavelength of 300-800 nm, and the silver layer 15b is formed with a silver fine particle content of 37-47% by weight. In the following description, when the term "transmittance" is used simply, it refers to the maximum transmittance for light with a wavelength of 300-800 nm.
[0024] The transmittance of the white layer 15a varies depending on the concentration and amount of application of the white ink. If the concentration or amount of application of the white ink is large and the transmittance of the white layer 15a is lower than 40%, sufficient laminate strength cannot be obtained. If the concentration or amount of application of the white ink is small and the transmittance of the white layer 15a is higher than 44%, sufficient light blocking properties of the light-blocking printed layer 15 cannot be obtained.
[0025] Furthermore, if the content of silver particles in the silver layer 15b is higher than 47% by weight, sufficient laminate strength cannot be obtained, and if it is lower than 37% by weight, the light-shielding printed layer 15 does not provide sufficient light-shielding properties.
[0026] The second base layer 20 is formed of a resin film. The resin forming the second base layer 20 may be a polyester resin, a polyamide resin, a polyolefin resin, or a mixture thereof. Specifically, a biaxially oriented polyethylene terephthalate film, a biaxially oriented nylon film, or the like may be used. The second base layer 20 may also be a multi-layer film in which a plurality of resin films are laminated. It is more preferable to form the second base layer 20 from a polyethylene terephthalate film, since the heat resistance of the laminated film 10 can be increased. The thickness of the second base layer 20 is about 5 to 50 μm.
[0027] The thermal adhesive resin layer 22 is formed of a resin film that can be melted and welded by heat. As a resin for forming the thermal adhesive resin layer 22, polyolefin resins (polyethylene, polypropylene, etc.), polyethylene terephthalate, polyacrylonitrile, etc. can be used. Specifically, a non-oriented polypropylene film can be preferably used. The thickness of the thermal adhesive resin layer 22 is not particularly limited, but is about 20 to 80 μm.
[0028] The first base material layer 11, on which the picture print layer 14 and the light-shielding print layer 15 are printed, and the second base material layer 20 are dry laminated with an adhesive layer 16 made of an adhesive. The second base material layer 20 and the heat adhesive resin layer 22 are dry laminated with an adhesive layer 21 made of an adhesive. The heat adhesive resin layer 22 may be formed by extrusion resin extruded onto the second base material layer 20.
[0029] The light-shielding package 1 formed by thermally bonding the heat-adhesive resin layer 22 of the laminated film 10 is provided with a light-shielding printed layer 15 having a white layer 15a and a silver layer 15b. This allows the light-shielding package 1 to have light-shielding properties, and prevents the contents from deteriorating due to light. In addition, the white layer 15a prevents the color development of the picture printed layer 14 from decreasing, and the silver layer 15b arranged on the inner surface side improves the visibility of the inside of the storage section 5. Furthermore, since the light-shielding printed layer 15 is formed of two layers, the white layer 15a and the silver layer 15b, the number of steps required for manufacturing the light-shielding package 1 can be reduced.
[0030] At this time, the white layer 15a is formed with a transmittance of 40 to 44%, and the silver layer 15b is formed with a silver fine particle content of 37 to 47% by weight. This allows the storage section 5 to be formed with a transmittance of 10% or less. In addition, the laminate film 10 forming the light-shielding packaging body 1 has a high lamination strength of 2N / 15mm or more, and delamination of the laminate film 10 can be prevented.
[0031] According to this embodiment, the light-shielding printed layer 15 has a white layer 15a solidly printed with white ink and a silver layer 15b solidly printed with silver ink. Therefore, the two layers of the white layer 15a and the silver layer 15b provide light-shielding properties and prevent the color development of the picture-printed layer 14 from decreasing. This reduces the number of steps required to manufacture the light-shielding package 1. In addition, the silver layer 15b improves the visibility of the inside of the storage section 5.
[0032] The white layer 15a has a transmittance of 40 to 44%, and the silver layer 15b has a silver fine particle content of 37 to 47% by weight, which provides the storage section 5 with high light blocking properties and prevents delamination of the laminated film 10.
[0033] Moreover, the laminated film 10 is formed by laminating a first base material layer 11 on which a transparent vapor-deposited film 11a is vapor-deposited, a second base material layer 20, and a thermal adhesive resin layer 22, and a light-blocking printed layer 15 is provided on the first base material layer 11. This makes it possible to easily realize the laminated film 10 and the light-blocking package 1 that are provided with the light-blocking printed layer 15.
[0034] In this embodiment, when the gas barrier property of the light-shielding package 1 is not required, the transparent vapor-deposited film 11a may be omitted.
[0035] <Second embodiment> Next, Fig. 3 shows a cross-sectional view of the laminated film 10 forming the light-shielding package 1 of the second embodiment. For ease of explanation, the same parts as those of the first embodiment shown in Figs. 1 and 2 above are given the same reference numerals. In this embodiment, the picture print layer 14 and the light-shielding print layer 15 of the laminated film 10 are provided on the second base material layer 20. The other parts are the same as those of the first embodiment.
[0036] The silver layer 15b of the light-blocking printing layer 15 is printed on the outer surface of the second base material layer 20, and a white layer 15a is printed on the outer surface of the silver layer 15b. In addition, a picture printed layer 14 is printed on the outer surface of the white layer 15a. The first base material layer 11 and the second base material layer 20 on which the picture printed layer 14 and the light-blocking printing layer 15 are printed are dry laminated by an adhesive layer 12 formed of an adhesive.
[0037] This embodiment can also provide the same effects as those of the first embodiment. In this embodiment, when the gas barrier property of the light-shielding package 1 is not required, the transparent vapor-deposited film 11a may be omitted.
[0038] <Third embodiment> Next, Fig. 4 shows a cross-sectional view of the laminated film 10 forming the light-shielding package 1 of the third embodiment. For ease of explanation, the same parts as those of the first embodiment shown in Figs. 1 and 2 above are given the same reference numerals. In this embodiment, the white layer 15a of the light-shielding printed layer 15 of the laminated film 10 is provided on the first base material layer 11, and the silver layer 15b is provided on the second base material layer 20. The other parts are the same as those of the first embodiment.
[0039] A picture printed layer 14 is printed on the inner surface side of the first base material layer 11, and a white layer 15a of the light-blocking printed layer 15 is printed on the inner surface of the picture printed layer 14. A silver layer 15b of the light-blocking printed layer 15 is printed on the outer surface side of the second base material layer 20. The first base material layer 11 on which the picture printed layer 14 and the white layer 15a are printed, and the second base material layer 20 on which the silver layer 15b is printed are dry laminated by an adhesive layer 12 formed of an adhesive.
[0040] In this embodiment, the same effect as in the first embodiment can be obtained. In addition, the white layer 15a and the silver layer 15b of the light-shielding printed layer 15 are dispersed, with the white layer 15a provided on the first base material layer 11 and the silver layer 15b provided on the second base material layer 20. This makes it possible to increase the white density of the background of the pattern formed by the picture printed layer 14. In addition, it is possible to reduce overprinting of ink and suppress a decrease in the lamination strength of the laminated film 10.
[0041] <Fourth embodiment> Next, Fig. 5 shows a cross-sectional view of a laminated film 10 forming a light-shielding package 1 of a fourth embodiment. For ease of explanation, the same parts as those of the first embodiment shown in Figs. 1 and 2 above are given the same reference numerals. In this embodiment, the transparent vapor-deposited film 11a (see Fig. 2) on the first base material layer 11 of the laminated film 10 is omitted, and a transparent vapor-deposited film 20a is provided on the second base material layer 20. In addition, a picture print layer 14 and a light-shielding print layer 15 are provided on the second base material layer 20. The other parts are the same as those of the first embodiment.
[0042] A transparent vapor-deposited film 20a is formed on the outer surface side of the second base material layer 20 by vapor-depositing an oxide. The silver layer 15b of the light-blocking printed layer 15 is printed on the transparent vapor-deposited film 20a, and the white layer 15a is printed on the outer surface of the silver layer 15b. In addition, the picture printed layer 14 is printed on the outer surface of the white layer 15a. The first base material layer 11 and the second base material layer 20 on which the picture printed layer 14 and the light-blocking printed layer 15 are printed are dry laminated by an adhesive layer 12 formed of an adhesive.
[0043] This embodiment can also provide the same effects as those of the first embodiment. In this embodiment, the picture printed layer 14 and the light-blocking printed layer 15 may be printed on the first base material layer 11. EXAMPLES
[0044] Next, the transmittance and laminate strength were examined for each example of the light-shielding package 1. Example 1 used the light-shielding package 1 of the first embodiment. The first base material layer 11 was a 12 μm-thick biaxially oriented polyethylene terephthalate film on which a transparent vapor-deposited film 11a of aluminum oxide was provided. The second base material layer 20 used a 12 μm-thick biaxially oriented polyethylene terephthalate film. The thermal adhesive resin layer 22 used a 60 μm-thick unstretched polypropylene film.
[0045] The white layer 15a and the silver layer 15b are gravure printed with Helio 175 L / inch, and the coating amount of the white ink and the silver ink is 6 g / m in wet state. 2 The transmittance of the white layer 15a is 44%, and the content of the silver particles in the silver layer 15b is 39% by weight. Aluminum particles are used as the silver particles. The white ink in the white layer 15a contains an appropriate amount of a hardener, and the silver ink in the silver layer 15b contains appropriate amounts of a hardener and an anti-blocking agent. EXAMPLES
[0046] In the light-shielding package 1 of Example 2, the content of the silver particles in the silver layer 15b of the laminated film 10 is 37% by weight. EXAMPLES
[0047] In the light-shielding package 1 of Example 3, the content of the silver particles in the silver layer 15b of the laminated film 10 is 47% by weight. EXAMPLES
[0048] In the light-shielding package 1 of Example 4, the transmittance of the white layer 15a of the laminated film 10 is set to 40%, and the content of the silver particles in the silver layer 15b is set to 47% by weight.
[0049] [Comparative Example 1] In the light-shielding package 1 of Comparative Example 1, the coating amount of the white ink on the white layer 15a and the silver ink on the silver layer 15b of the laminated film 10 was 7 g / m 2 The transmittance of the white layer 15a is set to 36%, and the content of the silver particles in the silver layer 15b is set to 39% by weight. The rest is the same as in Example 1.
[0050] [Comparative Example 2] In the light-shielding package 1 of Comparative Example 2, the transmittance of the white layer 15a of the laminated film 10 is set to 38%, and the content of the silver particles in the silver layer 15b is set to 39% by weight.
[0051] [Comparative Example 3] In the light-shielding package 1 of Comparative Example 3, the transmittance of the white layer 15a of the laminated film 10 is set to 39.5%, and the content of the silver particles in the silver layer 15b is set to 39% by weight.
[0052] [Comparative Example 4] The light-shielding package 1 of Comparative Example 4 has a transmittance of 50% for the white layer 15a of the laminated film 10, and a content of silver particles in the silver layer 15b of 39% by weight.
[0053] [Comparative Example 5] In the light-shielding package 1 of Comparative Example 5, the transmittance of the white layer 15a of the laminated film 10 is set to 47%, and the content of the silver particles in the silver layer 15b is set to 39% by weight.
[0054] [Comparative Example 6] The light-shielding package 1 of Comparative Example 6 has a transmittance of 44% for the white layer 15a of the laminated film 10, and a content of silver particles in the silver layer 15b of 33% by weight.
[0055] [Table 1]
[0056] Table 1 shows the results of examining the transmittance and laminate strength of the laminate film 10 of each Example and Comparative Example. In Table 1, the laminate strength of 2N / 15mm or more is indicated by "◯" and that of less than 2N / 15mm is indicated by "X".
[0057] Referring to Table 1, in Comparative Examples 1 to 3, when the transmittance of the white layer 15a is lower than 40%, the laminate strength is deteriorated. In addition, in Comparative Examples 4 to 6, when the transmittance of the white layer 15a is 47% or more and when the content of silver particles in the silver layer 15b is 33% or less, the transmittance of the laminate film 10 is high.
[0058] In contrast, in Examples 1 to 4, when the transmittance of the white layer 15a is 40% to 44% and the content of silver particles in the silver layer 15b is 37% to 47%, the laminate film 10 has a low transmittance of less than 10% and a high lamination strength of 2 N / 15 mm or more. [Industrial Applicability]
[0059] The present invention can be used as a light-shielding package for packaging medicines and food. [Explanation of symbols]
[0060] 1 Light-shielding packaging 1a opening 3. Seal Part 5 Storage area 10 Laminated film 11 First base layer 11a Transparent vapor deposited film 12, 16, 21 Adhesive layer 14 Picture printing layer 15 Light-shielding printing layer 15a White layer 15b Silver layer 20 Second base layer 22 Heat adhesive resin layer
Claims
1. A light-shielding package formed of a laminated film having a heat-adhesive resin layer disposed on the inner surface, a picture-printed layer forming a picture, and a light-shielding printed layer disposed on the inner surface side of the picture-printed layer, the light-shielding printed layer having a storage section for contents, the light-shielding printed layer having a white layer formed by solid printing with white ink over the entire surface of the storage section, and a silver layer disposed on the inner surface side of the white layer and by solid printing with silver ink over the entire surface of the storage section, the white layer having a maximum transmittance of 40 to 44% for light having a wavelength of 300 to 800 nm, the silver layer having a content of silver fine particles of 37 to 47% by weight, the laminated film has a first base material layer, a second base material layer located on the inner surface side of the first base material layer, and the thermal adhesive resin layer located on the inner surface side of the second base material layer, a gas barrier transparent vapor deposition film is formed on the outer surface side of the second base layer; An adhesive layer is formed between the first base material layer and the picture printed layer, and between the second base material layer and the thermal adhesive resin layer, The silver layer is printed on the outer surface side of the transparent vapor-deposited film, The white layer is printed on the outer surface side of the silver layer, A light-blocking package, characterized in that the picture print layer is printed on the outer surface side of the white layer.
2. A light-blocking package formed of a laminated film having a heat-adhesive resin layer disposed on the inner surface, a picture-printed layer forming a picture, and a light-blocking printed layer disposed on the inner side of the picture-printed layer, and having a storage section for contents, wherein the light-blocking printed layer has a white layer formed by solid printing of white ink over the entire surface of the storage section, and a silver layer disposed on the inner side of the white layer and by solid printing of silver ink over the entire surface of the storage section, the white layer has a maximum transmittance of 40 to 44% for light having a wavelength of 300 to 800 nm, and the silver layer has a silver microparticle content of 37 to 47% by weight, the laminated film has a first base material layer, a second base material layer located on the inner surface side of the first base material layer, and the thermal adhesive resin layer located on the inner surface side of the second base material layer, a gas barrier transparent vapor deposition film is formed on the outer surface side of the second base layer; an adhesive layer is formed between the silver layer and the transparent vapor deposition film, and between the second base layer and the thermal adhesive resin layer; The picture print layer is printed on the inner surface side of the first base material layer, The white layer is printed on the inner surface side of the picture print layer, A light-proof packaging body, characterized in that the silver layer is printed on the inner surface side of the white layer.
3. A light-shielding packaging body as described in claim 1 or claim 2, characterized in that the transparent vapor deposition film is formed only on the outer surface side of the second substrate layer.
4. 4. The light-shielding package according to claim 1, wherein the thickness of the white layer is 80 to 120% of the thickness of the silver layer.
Citation Information
Patent Citations
Shielding packaging material
JP1997314719A
Packaging bag
JP2004025555A
Packaging material having light shielding property and concealing property
JP2018172138A
Packaging material
JP2019177948A