Biaxially oriented film

A biaxially stretched film with specific polyester compositions addresses the limitations of existing films by providing enhanced heat resistance and moldability, suitable for flexible displays with improved durability and handling.

JP7559598B2Active Publication Date: 2024-10-02MITSUBISHI CHEM CORP
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2021022844
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-02-16
Publication Date
2024-10-02
Estimated Expiration
2041-02-16

AI Technical Summary

Technical Problem

Existing films, such as those made from polyethylene terephthalate (PET) and polyimide, face issues with heat resistance, bending resistance, and moldability, making them unsuitable for flexible displays that require high durability and ease of manufacturing.

Method used

A biaxially stretched film composed of two or more types of polyester, including polybutylene naphthalate resin (PBN) and another polyester, with specific properties like a hysteresis loss rate of 18.0% or less, glass transition temperature between 75°C and 150°C, and crystal melting temperature between 220°C and 300°C, ensuring excellent heat resistance and moldability.

Benefits of technology

The film exhibits superior heat resistance, folding durability, and moldability, making it suitable for flexible displays, particularly foldable applications, with improved handling properties and reduced anisotropy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007559598000002
    Figure 0007559598000002
  • Figure 0007559598000001
    Figure 0007559598000001
Patent Text Reader

Abstract

To provide a biaxial oriented film that is excellent in folding resistance, heat resistance and moldability.SOLUTION: A biaxial oriented film contains two or more polyesters, at least one of which is a polybutylene naphthalate resin (A). The film has a thickness of 20 μm or more and 250 μm or less. The film is subjected to a tensile cycle test up to a 1.5% tensile strain in each of a longitudinal direction (MD) and a width direction (TD), so that its hysteresis loss rates are 18.0% or less on average.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a biaxially oriented film. [Background technology]

[0002] Polyester has excellent properties such as heat resistance, weather resistance, mechanical strength, transparency, chemical resistance, and gas barrier properties, and is also readily available at a reasonable price, making it a versatile resin that is currently widely used in beverage and food containers and packaging materials, molded products, films, etc. The main type of polyester is polyethylene terephthalate (hereinafter sometimes referred to as "PET"), which has excellent mechanical properties, electrical properties, chemical resistance, etc. and has a wide range of uses, but has drawbacks such as poor heat resistance and folding resistance.

[0003] Also, polybutylene naphthalate (hereinafter sometimes referred to as "PBN"), which is made by polymerizing naphthalenedicarboxylic acid with 1,4-butanediol, is known as a material that uses naphthalenedicarboxylic acid as the acid component. PBN has excellent mechanical properties and impact resistance because it undergoes a crystal transition due to the conformation of the alkyl chain portion, but it has a low glass transition temperature of about 75°C and a low melting point of about 240°C, and therefore has problems with heat resistance. In addition, the crystallization rate is too fast, making it unsuitable for film formation by extrusion molding.

[0004] Meanwhile, in recent years, with the trend towards smaller and lighter electronic devices, there has been a trend towards using flexible substrates and flexible printed circuits. In line with this trend, there is also an increasing demand for flexibility in display applications, and there is a strong demand for films that have high heat resistance, excellent recovery properties, and excellent resistance to repeated bending.

[0005] Flexible displays include types such as foldable, bendable, rollable, and stretchable. A typical example of a flexible display comprises a substrate film made of a synthetic resin such as polyimide, and elements such as thin film transistors (TFTs) and organic light-emitting diodes (OLEDs) supported on the substrate film. In addition to the substrate film, optical films with excellent flexibility are used as components for the front panel of a flexible display, base film for touch sensors, and film for protecting the substrate film (hereinafter referred to as lower protective film), etc.

[0006] Thus, in recent years, resin films with excellent flexibility have been studied. For example, Patent Document 1 studies a film made of a cyclic olefin resin that is resistant to repeated bending.

[0007] Furthermore, Patent Documents 2 and 3 propose a polyimide film as a film having excellent heat resistance and bending resistance.

[0008] Furthermore, Patent Document 4 proposes a polyester copolymer having excellent heat resistance and injection moldability by blending 2,6-naphthalenedicarboxylic acid as the acid component and 1,4-butanediol and 1,4-cyclohexanedimethanol as the glycol component. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] JP 2014-104687 A [Patent Document 2] International Publication No. 2017 / 150377 [Patent Document 3] International Publication No. 2016 / 060213 [Patent Document 4] Japanese Patent Application Publication No. 5-209044 Summary of the Invention [Problem to be solved by the invention]

[0010] However, the film disclosed in Patent Document 1 has a low level of resistance to repeated folding, and does not satisfy market demands. Furthermore, cyclic olefins have poor coating and adhesive properties, making them difficult to laminate with other materials, making them unsuitable for use as materials for flexible displays.

[0011] In addition, although the polyimide film described in Patent Document 2 has high heat resistance, the molding temperature is 350° C. and the molding time is long, which makes it difficult to produce.

[0012] Although the polyimide film described in Patent Document 3 has flex resistance, the production process thereof involves a molding method using a coating of a solvent, which results in problems such as poor productivity and high costs.

[0013] Furthermore, although the polyester copolymer described in Patent Document 4 has excellent injection moldability, the crystallization rate is too fast, which deteriorates the film formability and stretchability, making it unsuitable for extrusion molding.

[0014] An object of the present invention is to solve the above problems and to provide a biaxially stretched film having excellent heat resistance, folding resistance and formability. [Means for solving the problem]

[0015] The present inventors have conducted extensive research to achieve the above object, and as a result have completed the present invention. In one aspect, the present invention is summarized as follows [1] to

[12] . The gist of the present invention is as follows. [1] A biaxially oriented film comprising two or more polyesters, at least one of which is a polybutylene naphthalate resin (A), having a thickness of 20 μm or more and 250 μm or less, and having an average hysteresis loss rate of 18.0% or less when subjected to a tensile cycle test up to 1.5% tensile strain in each of the longitudinal direction (MD) and the transverse direction (TD). [2] The biaxially stretched film according to the above [1], wherein the glass transition temperature of the polyester (B) other than the polybutylene naphthalate resin (A) is 75°C or higher and 150°C or lower. [3] The biaxially stretched film according to the above [2], wherein the crystalline melting temperature of the polyester (B) is 220°C or higher and 300°C or lower. [4] The biaxially stretched film according to the above [2] or [3], wherein the polyester (B) has a heat of crystalline fusion of 15 J / g or more and 60 J / g or less. [5] The biaxially stretched film according to any one of the above [2] to [4], wherein the polyester (B) is a polyethylene naphthalate-based resin. [6] The biaxially stretched film according to any one of the above [1] to [5], having an average residual strain of 0.110% or less when subjected to a tensile cycle test up to a tensile strain of 1.5% in each of the longitudinal direction (MD) and the transverse direction (TD). [7] The biaxially stretched film according to any one of the above [1] to [6], having a glass transition temperature of 75° C. or higher and 150° C. or lower. [8] The biaxially stretched film according to any one of the above [1] to [7], which has a crystalline melting temperature of 220° C. or higher and 300° C. or lower. [9] The biaxially stretched film according to any one of the above [1] to [8], having a heat of crystalline fusion of 10 J / g or more and 60 J / g or less.

[10] The biaxially stretched film according to any one of the above [1] to [9], which has a heat shrinkage rate of 5.0% or less in both the longitudinal direction (MD) and the transverse direction (TD) when heated at 150°C for 30 minutes.

[11] The biaxially stretched film according to any one of the above [1] to

[10] , which is for a display.

[12] A flexible display comprising the biaxially stretched film according to any one of the above [1] to

[11] . Effect of the Invention

[0016] The biaxially stretched film of the present invention has excellent heat resistance, folding resistance and formability. Therefore, the biaxially stretched film of the present invention can be suitably used for flexible displays and the like. [Brief description of the drawings]

[0017] [Figure 1] 1 is a profile of a stress-strain curve. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] The present invention will be described in detail below. However, the content of the present invention is not limited to the embodiments described below.

[0019] <Biaxially oriented film> A biaxially stretched film according to one embodiment of the present invention (hereinafter, sometimes referred to as "this film") contains two or more polyesters, at least one of which is a polybutylene naphthalate resin (A), has a thickness of 20 μm or more and 250 μm or less, and has an average hysteresis loss rate of 18.0% or less when subjected to a tensile cycle test up to 1.5% tensile strain in each of the longitudinal direction (MD) and the transverse direction (TD). Since the present film is a biaxially oriented film, it can be made thin, and since the hysteresis loss rate is adjusted to fall within a specific range by using a specific blend of polyesters, the film has excellent folding resistance. Furthermore, since the film uses a specific blend of polyesters to maintain high crystallinity, it also has excellent heat resistance and melt extrusion moldability.

[0020] In the present invention, the machine direction (MD) of the film refers to the direction in which the film travels during the film production process, that is, the winding direction of the film roll. The transverse direction (TD) of the film refers to a direction parallel to the film surface and perpendicular to the longitudinal direction, that is, a direction parallel to the central axis of the roll of the film.

[0021] The present inventors have found that the present film, which has a hysteresis loss rate of a specific value or less, has excellent heat resistance and folding resistance as a display film, and is suitable for flexible applications, particularly foldable applications. This film has a low hysteresis loss rate, which is believed to be why it has excellent recovery and folding resistance.

[0022] 1. Physical properties First, the physical properties of the film will be described.

[0023] (1) Hysteresis loss rate The film has an average hysteresis loss rate of 18.0% or less when subjected to a tensile cycle test up to 1.5% tensile strain in each of the machine direction (MD) and the transverse direction (TD) at 23°C, preferably 17.5% or less, more preferably 17.0% or less, and even more preferably 16.5% or less. The lower limit is not particularly limited, but is 0.100% or more. By setting the hysteresis loss rate to 18.0% or less, the restoring force of the film is increased and the bending resistance (folding resistance) of the film is maintained within a practical range.

[0024] Moreover, by taking the hysteresis loss rate as an average value in each of the machine direction (MD) and the transverse direction (TD), it can be used as an index of properties of the entire film. The hysteresis loss rate can be adjusted by the stretching conditions, etc. The hysteresis loss rate of the present film can be measured by the method described in the Examples in accordance with JIS K 7312:1996. More specifically, when a stress-strain curve like that shown in FIG. 1 is obtained by a tensile cycle test, the ratio of the area enclosed by abcef to the total area (abcda) is defined as the hysteresis loss rate.

[0025] Furthermore, the difference in hysteresis loss rate between the machine direction (MD) and the transverse direction (TD) of the present film at 23° C. is preferably 4.5% or less, more preferably 4.3% or less, and even more preferably 4.0% or less. The difference in hysteresis loss rate is expressed as an absolute value, and the smaller the better, but it is sufficient if it is 0% or more. When the difference in hysteresis loss rate between the machine direction (MD) and the transverse direction (TD) is within the above range, the bending resistance of the film and therefore the anisotropy of various properties of the film become small, so that the film is not restricted by the direction. Therefore, when the film is used as a component or during manufacturing steps such as secondary processing, it is no longer necessary to select a specific direction, which has the advantage of preventing an increase in the workload of workers. In addition, since defects in only a specific direction due to anisotropy are unlikely to occur, the film also has excellent handleability.

[0026] (2) Thickness The thickness of the present film is 20 to 250 μm, preferably 25 to 200 μm, and more preferably 30 to 150 μm. By making it 20 μm or more, the film strength can be kept within a practical range, and it can be suitably used for displays. By making it 250 μm or less, folding resistance is easily exhibited. The thickness can be adjusted by film formation and stretching conditions.

[0027] (3) Residual strain The biaxially stretched film of the present invention contains two or more polyesters, at least one of which is a polybutylene naphthalate resin (A), and preferably has an average residual strain of 0.110% or less when subjected to a tensile cycle test up to a tensile strain of 1.5% in each of the longitudinal direction (MD) and the transverse direction (TD). By setting the residual strain to 0.110% or less, the restoring force of the film is increased, and the bending resistance of the film is maintained within a practical range. From the above viewpoints, the average value of the residual strain is more preferably 0.108% or less, further preferably 0.106% or less, particularly preferably 0.104% or less, and particularly preferably 0.102% or less. The lower limit is not particularly limited, but is 0.010% or more. In addition, the residual strain can be used as an index of properties of the entire film by averaging the residual strain in both the machine direction (MD) and the transverse direction (TD). Moreover, the residual strain can be adjusted by adjusting the stretching conditions. The residual strain of the present film can be measured according to JIS K 7312:1996 by the method described in the Examples. More specifically, when a stress-strain curve such as that shown in FIG. 1 is obtained by a tensile cycle test, the value of f is defined as the residual strain.

[0028] Furthermore, the difference in the residual strain between the machine direction (MD) and the transverse direction (TD) of the present film at 23° C. is preferably 0.027% or less, more preferably 0.026% or less, and even more preferably 0.025% or less. The difference in the residual strain is expressed as an absolute value, and the smaller the better, but it is sufficient if it is 0% or more. When the difference in residual strain between the machine direction (MD) and the transverse direction (TD) is within the above range, the bending resistance of the film and, in turn, the anisotropy of various film properties are reduced, so that the film is not restricted by the direction. Therefore, when the film is used as a component or during manufacturing steps such as secondary processing, it is no longer necessary to select a specific direction, which has the advantage of preventing an increase in the workload of workers. In addition, since defects in only a specific direction due to anisotropy are unlikely to occur, the film also has excellent handleability.

[0029] (4) Glass transition temperature The glass transition temperature (Tg) of the present film is preferably from 75° C. to 150° C., more preferably from 76° C. to 140° C., and even more preferably from 77° C. to 130° C. If the glass transition temperature (Tg) of the present film is 75° C. or higher, the film will not deform even when used for display purposes, and therefore the film can be said to have excellent heat resistance. On the other hand, if the glass transition temperature (Tg) is 150° C. or lower, the material is also suitable for moldability. The glass transition temperature (Tg) of this film is measured using a differential scanning calorimeter (DSC) at a heating rate of 10°C / min according to JIS K7121 (2012).

[0030] (5) Crystal melting temperature The crystalline melting temperature (Tm) of the present film is preferably from 220° C. to 300° C., more preferably from 221° C. to 295° C., even more preferably from 222° C. to 290° C., and particularly preferably from 223° C. to 285° C. If the crystalline melting temperature (Tm) of the present film is within the above range, the present film has an excellent balance between heat resistance and melt extrusion moldability. Here, the crystalline melting temperature (Tm) of the present film is measured in accordance with JIS K7121 (2012) using a differential scanning calorimeter (DSC) at a heating rate of 10°C / min. The crystalline melting temperature (Tm) of the present film can be optimized by adjusting the cooling temperature from the molten state, the stretching ratio, the stretching temperature, and the heat treatment conditions after stretching during the production of the present film.

[0031] (6) Heat of crystal fusion The heat of crystalline fusion (ΔHm) of the present film is preferably 10 J / g to 60 J / g, more preferably 20 J / g to 55 J / g, even more preferably 25 J / g to 50 J / g, and particularly preferably 30 J / g to 45 J / g. If the heat of crystalline fusion (ΔHm) of the present film is within this range, the present film has an excellent balance between heat resistance and melt extrusion moldability. Here, the crystalline heat of fusion (ΔHm) of this film is measured at a heating rate of 10° C. / min using a differential scanning calorimeter (DSC) in accordance with JIS K7122 (2012).

[0032] (7) Heat shrinkage rate The heat shrinkage of the present film is preferably 5.0% or less in both the machine direction (MD) and the transverse direction (TD) when heated at 150° C. for 30 minutes. With a heat shrinkage of 5.0% or less, the present film has excellent heat resistance, particularly dimensional stability at high temperatures, and can be used without problems in practice. From this viewpoint, the heat shrinkage rate of the present film is more preferably 4.0% or less, further preferably 3.0% or less, and particularly preferably 2.5% or less. There is no particular lower limit, but it is 0.01% or more.

[0033] 2. Ingredients Next, the components constituting the present film will be described.

[0034] The present inventors have found that a biaxially stretched film containing a mixed polyester, which contains two or more polyesters that generally exhibit relatively higher yield stress and elastic modulus than polyethylene and polypropylene, at least one of which is a polybutylene naphthalate resin (A), has excellent folding resistance. Furthermore, the present inventors have found that if the hysteresis loss rate of the film is equal to or less than a specific value, the restoring force of the film increases and distortion is less likely to occur. Even though polyester is a material with a high yield stress and elastic modulus, if the stress or strain applied by deformation is large, deformation occurs and unresolved strain remains in the material. Generally, large strain occurs in the material when deformation exceeds the elastic deformation region. However, even if the deformation is within the elastic deformation region, residual strain may remain in the material, leaving traces of deformation such as folds or wrinkles, which may result in poor appearance or affect the material properties themselves. In other words, the smaller the hysteresis loss rate, the higher the recovery from deformation and the smaller the strain remaining in the material. Therefore, even when a deformation within the elastic deformation region or a large strain exceeding the elastic deformation region is applied, it is unlikely to leave a deformation mark and it is considered to have excellent deformation resistance. In the present invention, a specific mixed polyester, i.e., a mixed polyester containing two or more polyesters, at least one of which is a polybutylene naphthalate-based resin (A), is used, which makes it possible to keep the hysteresis loss rate of the film below a specific value, increase the restoring force of the film, thereby suppressing distortion of the material, and also provides heat resistance.

[0035] <Polybutylene naphthalate resin (A)> The PBN resin (A) constituting the present film may be either a homopolyester or a copolymer polyester, but from the viewpoint of folding endurance, a homopolyester is preferred. The PBN resin (A) may be a homopolyester or a copolymer polyester alone, or a blend of a homopolyester and a copolymer polyester. In the case of a homopolyester, it is obtained by polycondensing 2,6-naphthalenedicarboxylic acid as the dicarboxylic acid component (a-1) and 1,4-butanediol as the diol component (a-2).

[0036] On the other hand, in the case of a copolymer polyester, 2,6-naphthalenedicarboxylic acid is an essential component as the dicarboxylic acid component (a-1), and other copolymer components may be added thereto as necessary. Examples of other copolymerization components include aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid, phthalic acid, 1,4-naphthalenedicarboxylic acid, 1,5-naphthalenedicarboxylic acid, 2,5-furandicarboxylic acid, 2,4-furandicarboxylic acid, 3,4-furandicarboxylic acid, benzophenone dicarboxylic acid, 4,4'-diphenyldicarboxylic acid, 3,3'-diphenyldicarboxylic acid, and 4,4'-diphenylether dicarboxylic acid; aliphatic dicarboxylic acids such as cyclohexanedicarboxylic acid, oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, and dimer acid; and oxycarboxylic acids such as p-oxybenzoic acid. Among these, isophthalic acid, 2,5-furandicarboxylic acid, 2,4-furandicarboxylic acid, and 3,4-furandicarboxylic acid are preferred from the viewpoint of moldability. These copolymerization components can be used alone or in combination of two or more.

[0037] As the diol component (a-2), 1,4-butanediol is an essential component, and other copolymerization components may be copolymerized with this as necessary. Other copolymerization components include 1,4-cyclohexanedimethanol, ethylene glycol, diethylene glycol, propylene glycol, neopentyl glycol, polytetramethylene ether glycol, dimer diol, bisphenols (bisphenol compounds such as bisphenol A, bisphenol F, or bisphenol S, or derivatives thereof, or ethylene oxide adducts thereof), and one or more of these can be used. Among these, 1,4-cyclohexanedimethanol, polytetramethylene ether glycol, dimer diol, and bisphenols are preferred. In particular, from the viewpoint of maintaining the strength of the film, it is preferable to use 1,4-cyclohexanedimethanol or bisphenols, and it is particularly preferable to use 1,4-cyclohexanedimethanol. These copolymerization components can be used alone or in combination of two or more.

[0038] The copolymerized polyester constituting the PBN resin (A) is preferably a PBN copolymer containing a dicarboxylic acid component (a-1) and a diol component (a-2), the (a-1) component containing 2,6-naphthalenedicarboxylic acid units, and the (a-2) component containing 1,4-butanediol units and 1,4-cyclohexanedimethanol units.

[0039] The copolymer polyester contains, in the dicarboxylic acid component (a-1), preferably 0 mol % or more and 10 mol % or less, more preferably 0 mol % or more and 8 mol % or less, even more preferably 0 mol % or more and 6 mol % or less, particularly preferably 0 mol % or more and 4 mol % or less, and especially preferably 0 mol % or more and 2 mol % or less of other copolymer components. By adjusting the content of the other copolymerization component in the dicarboxylic acid component (a-1) to fall within the above numerical range, the glass transition temperature and crystalline melting temperature of the copolymerized polyester are improved, and thus the heat resistance of the present film is improved.

[0040] The copolymer polyester contains 2,6-naphthalenedicarboxylic acid units in the dicarboxylic acid component (a-1) at preferably 90 mol % or more, more preferably 92 mol % or more, even more preferably 94 mol % or more, particularly preferably 96 mol % or more, and especially preferably 98 mol % or more, and all of the dicarboxylic acid component (a-1) (100 mol %) may be 2,6-naphthalenedicarboxylic acid. By adjusting the content of 2,6-naphthalenedicarboxylic acid units in the dicarboxylic acid component (a-1) to fall within the above numerical range, the glass transition temperature and crystalline melting temperature of the copolymerized polyester are improved, and thus the heat resistance of the present film is improved.

[0041] The copolymer polyester contains another copolymer component in the diol component (a-2) in an amount of preferably 10 mol % or more and 90 mol % or less, more preferably 20 mol % or more and 85 mol % or less, even more preferably 30 mol % or more and 80 mol % or less, particularly preferably 40 mol % or more and 75 mol % or less, and especially preferably 50 mol % or more and 70 mol % or less. By setting the content of other copolymerization components in the diol component (a-2) within the above numerical range, the glass transition temperature and crystalline melting temperature of the copolymerized polyester are improved, and the heat resistance of the present film is improved. In addition, since the crystallinity can be controlled, the crystallization rate can be slowed down, and the extrusion moldability and stretching processability of the film can be improved. In addition, when the content is 90 mol% or less, the melting point does not become too high. Therefore, there is no need to set the molding temperature high, and there is no concern about thermal decomposition.

[0042] The copolymer polyester contains 1,4-butanediol in the diol component (a-2) in an amount of preferably 10 mol % or more and 90 mol % or less, more preferably 15 mol % or more and 80 mol % or less, even more preferably 20 mol % or more and 70 mol % or less, particularly preferably 25 mol % or more and 60 mol % or less, and especially preferably 30 mol % or more and 50 mol % or less. By setting the content of 1,4-butanediol in the diol component (a-2) within the above numerical range, the crystallinity of the copolymerized polyester is maintained, and the heat resistance of the present film is improved. On the other hand, if the content exceeds 90 mol%, the crystallization speed becomes too fast, and the extrusion film formability and film stretchability may be deteriorated.

[0043] From the viewpoint of heat resistance, the glass transition temperature (Tg(A)) of the PBN-based resin (A) is preferably 70°C or higher and 150°C or lower, more preferably 73°C or higher and 140°C or lower, and even more preferably 75°C or higher and 130°C or lower.

[0044] From the viewpoint of a balance between heat resistance and moldability, the crystalline melting temperature (Tm(A)) of the PBN resin (A) is preferably 220°C or higher and 300°C or lower, more preferably 230°C or higher and 290°C or lower, and even more preferably 235°C or higher and 280°C or lower.

[0045] <Polyester (B)> The present film is composed of a polyester mixture containing the PBN resin (A) and a polyester (B). The polyester (B) constituting the present film is a component that imparts heat resistance and moldability to the PBN resin (A), which is a folding-resistant component.

[0046] By mixing the polyester (B) with the PBN resin (A), it is possible to obtain a resin composition having a higher glass transition temperature than the PBN resin (A) alone, and a film with excellent heat resistance can be obtained. Furthermore, by adding the polyester (B), the crystallization rate of the PBN resin (A) can be controlled, and a film having excellent extrusion moldability and stretch processability can be obtained.

[0047] The polyester (B) may be one composed of a dicarboxylic acid component (b-1) and a diol component (b-2) as shown below. Examples of the dicarboxylic acid component (b-1) include terephthalic acid, isophthalic acid, orthophthalic acid, phthalic acid, 4,4'-diphenyldicarboxylic acid, 2,5-naphthalenedicarboxylic acid, 1,5-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, 2,7-naphthalenedicarboxylic acid, 1,4-cyclohexanedicarboxylic acid, 2-potassium sulfoterephthalic acid, 5-sodium sulfoisophthalic acid, adipic acid, azelaic acid, sebacic acid, dodecanedicarboxylic acid, glutaric acid, succinic acid, trimellitic acid, trimesic acid, pyromellitic acid, trimellitic anhydride, phthalic anhydride, p-hydroxybenzoic acid, trimellitic acid monopotassium salt, and ester-forming derivatives thereof.

[0048] Examples of the diol component (b-2) include ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,3-propanediol, 1,4-butanediol, 1,6-hexanediol, 2-methyl-1,5-pentanediol, neopentyl glycol, 1,4-cyclohexanedimethanol, p-xylylene glycol, bisphenol A-ethylene glycol adduct, diethylene glycol, triethylene glycol, polyethylene glycol, polypropylene glycol, polytetramethylene glycol, polytetramethylene oxide glycol, dimethylolpropionic acid, glycerin, trimethylolpropane, sodium dimethylolethylsulfonate, and potassium dimethylolpropionate. One or more of the above compounds may be appropriately selected and subjected to a conventional polycondensation reaction to synthesize a polyester. The polyester (B) includes a polyester corresponding to the above-mentioned PBN-based resin (A), but in the mixed polyester of the present invention, the polyester (B) used is different from the above-mentioned PBN-based resin (A).

[0049] The polyester (B) may be one or more kinds, but preferably satisfies the following conditions (glass transition temperature (Tg), crystalline melting temperature (Tm), crystalline melting heat (ΔHm)). As for the measurement method, Tg and Tm are measured according to JIS K7121 (2012), and ΔHm is measured according to JIS K7122 (2012). Specifically, they can be measured in the same manner as Tg, Tm, and ΔHm in the film described in the examples.

[0050] From the viewpoint of heat resistance, the glass transition temperature (Tg(B)) of the polyester (B) is preferably 75°C or higher and 150°C or lower, more preferably 77°C or higher and 145°C or lower, and even more preferably 80°C or higher and 140°C or lower.

[0051] From the viewpoint of the balance between heat resistance and moldability, the crystalline melting temperature (Tm(B)) of the polyester (B) is preferably 220°C or higher and 300°C or lower, more preferably 225°C or higher and 290°C or lower, even more preferably 230°C or higher and 280°C or lower, and particularly preferably 235°C or higher and 270°C or lower.

[0052] Furthermore, from the viewpoint of maintaining high crystallinity and thereby exhibiting excellent heat resistance and moldability, the crystalline heat of fusion (ΔHm(B)) of the polyester (B) is preferably 15 J / g or more and 60 J / g or less, and more preferably 20 J / g or more and 50 J / g or less.

[0053] Examples of the polyester (B) having a glass transition temperature (Tg(B)), crystalline melting temperature (Tm(B)) and crystalline melting heat (ΔHm(B)) within the above-mentioned ranges include polyethylene naphthalate-based resins and polycyclohexylene dimethylene terephthalate-based resins. From the viewpoint of heat resistance and compatibility with the PBN-based resin (A), it is preferable to contain a polyethylene naphthalate (hereinafter sometimes referred to as "PEN")-based resin.

[0054] (Polyethylene naphthalate resin) The PEN resin may be either a homopolyester or a copolymer polyester. A homopolyester and a copolymer polyester may be blended, and when a homopolyester and one copolymer polyester are blended, it is considered that two kinds of the polyester (B) are used.

[0055] In the case of a homopolyester, it is obtained by polycondensing 2,6-naphthalenedicarboxylic acid as a dicarboxylic acid component and ethylene glycol as a diol component.

[0056] On the other hand, in the case of a copolymer polyester, 2,6-naphthalenedicarboxylic acid is an essential dicarboxylic acid component, and other copolymer components may be added thereto as necessary. Examples of other copolymerization components include aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid, phthalic acid, 1,4-naphthalenedicarboxylic acid, 1,5-naphthalenedicarboxylic acid, 2,5-furandicarboxylic acid, 2,4-furandicarboxylic acid, 3,4-furandicarboxylic acid, benzophenone dicarboxylic acid, 4,4'-diphenyldicarboxylic acid, 3,3'-diphenyldicarboxylic acid, and 4,4'-diphenylether dicarboxylic acid; aliphatic dicarboxylic acids such as cyclohexanedicarboxylic acid, oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, and dimer acid; and oxycarboxylic acids such as p-oxybenzoic acid. Among these, isophthalic acid, 2,5-furandicarboxylic acid, 2,4-furandicarboxylic acid, and 3,4-furandicarboxylic acid are preferred from the viewpoint of moldability. These copolymerization components can be used alone or in combination of two or more.

[0057] As the diol component, ethylene glycol is an essential component, and other copolymerization components may be used as necessary, such as 1,2-propanediol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, neopentyl glycol, diethylene glycol, triethylene glycol, propylene glycol, polyalkylene glycol, 1,2-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, hydroquinone, spiroglycol, 2,2,4,4,-tetramethylcyclobutane-1,3-diol, isosorbide, 1,4-cyclohexanedimethanol, polytetramethylene ether glycol, dimer diol, and bisphenols (bisphenol compounds such as bisphenol A, bisphenol F, or bisphenol S, or derivatives thereof, or ethylene oxide adducts thereof), and among these, 1,4-cyclohexanedimethanol, polytetramethylene ether glycol, dimer diol, and bisphenols are preferred. In particular, from the viewpoint of maintaining the strength of the film, it is preferable to use bisphenols. As the bisphenol, it is preferable to use a bisphenol A-ethylene oxide adduct. These copolymerization components can be used alone or in combination of two or more.

[0058] The copolymer polyester constituting the PEN resin is preferably a polyethylene naphthalate copolymer containing 2,6-naphthalenedicarboxylic acid units as the dicarboxylic acid component and ethylene glycol units and bisphenol A-ethylene oxide adduct units as the diol components.

[0059] The copolymer polyester contains another copolymer component in the dicarboxylic acid component in an amount of preferably 0 mol % or more and 10 mol % or less, more preferably 0 mol % or more and 8 mol % or less, even more preferably 0 mol % or more and 6 mol % or less, particularly preferably 0 mol % or more and 4 mol % or less, and especially preferably 0 mol % or more and 2 mol % or less. By adjusting the content of the other copolymerization component in the dicarboxylic acid component to fall within the above numerical range, the glass transition temperature and crystalline melting temperature of the copolymerized polyester are improved, and thus the heat resistance of the present film is improved.

[0060] The copolymer polyester contains 2,6-naphthalenedicarboxylic acid units in the dicarboxylic acid component in an amount of preferably 90 mol % or more, more preferably 92 mol % or more, even more preferably 94 mol % or more, particularly preferably 96 mol % or more, and especially preferably 98 mol % or more, and all of the dicarboxylic acid component (100 mol %) may be 2,6-naphthalenedicarboxylic acid. By controlling the content of 2,6-naphthalenedicarboxylic acid units in the dicarboxylic acid component to fall within the above range, the glass transition temperature and crystalline melting temperature of the copolymerized polyester are improved, and thus the heat resistance of the present film is improved.

[0061] The copolymer polyester contains another copolymer component in the diol component in an amount of preferably 4 mol % or more and 70 mol % or less, more preferably 4.2 mol % or more and 60 mol % or less, even more preferably 4.4 mol % or more and 50 mol % or less, particularly preferably 4.6 mol % or more and 40 mol % or less, and especially preferably 4.8 mol % or more and 30 mol % or less. By adjusting the content of the other copolymerization component in the diol component to fall within the above range, the glass transition temperature and crystalline melting temperature of the copolymerized polyester are improved, and thus the heat resistance of the present film is improved. Furthermore, since the crystallinity can be controlled, the crystallization rate can be slowed down, and the extrusion moldability and stretch processability of the film can be improved. Furthermore, when the content is 70 mol % or less, the melting point does not become too high, and therefore there is no need to set the molding temperature high, and there is no concern about thermal decomposition.

[0062] The copolymer polyester contains ethylene glycol in the diol component in an amount of preferably 30 mol % or more and 96 mol % or less, more preferably 40 mol % or more and 95.8 mol % or less, even more preferably 50 mol % or more and 95.6 mol % or less, particularly preferably 60 mol % or more and 95.4 mol % or less, and especially preferably 70 mol % or more and 95.2 mol % or less. By adjusting the content of ethylene glycol in the diol component to fall within the above range, the crystallinity of the copolymerized polyester is maintained, and the heat resistance of the present film is improved.

[0063] From the viewpoint of a balance between heat resistance, folding resistance, and moldability, the content of the polyester (B) is preferably 50 parts by mass or more and 1,000 parts by mass or less, more preferably 55 parts by mass or more and 980 parts by mass or less, even more preferably 60 parts by mass or more and 950 parts by mass or less, and particularly preferably 65 parts by mass or more and 900 parts by mass or less, per 100 parts by mass of the PBN-based resin (A). When the content of the polyester (B) in the present film is 50 parts by mass or more, the crystallization rate can be slowed down, and therefore extrusion moldability and stretch processability during film production can be improved. When the content is 50 parts by mass or more, the glass transition temperature is increased, and the heat resistance of the present film can be improved. On the other hand, when the content of the polyester (B) is 1000 parts by mass or less, the folding resistance of the PBN resin (A) is not significantly impaired, and the folding resistance of the obtained present film is sufficient.

[0064] In the present invention, the present film can be allowed to contain resins other than the PBN resin (A) and the polyester (B) as long as the effects of the present invention are not impaired. Examples of other resins include polystyrene resins, polyvinyl chloride resins, polyvinylidene chloride resins, chlorinated polyethylene resins, polycarbonate resins, polyamide resins, polyacetal resins, acrylic resins, ethylene vinyl acetate copolymers, polymethylpentene resins, polyvinyl alcohol resins, cyclic olefin resins, polylactic acid resins, polybutylene succinate resins, polyacrylonitrile resins, polyethylene oxide resins, cellulose resins, polyimide resins, polyurethane resins, polyphenylene sulfide resins, polyphenylene ether resins, polyvinyl acetal resins, polybutadiene resins, polybutene resins, polyamideimide resins, polyamide bismaleimide resins, polyetherimide resins, polyetheretherketone resins, polyetherketone resins, polyethersulfone resins, polyketone resins, polysulfone resins, aramid resins, and fluorine-based resins.

[0065] The present film may contain particles for the main purpose of imparting easy slippage and preventing scratches during each process. The type of particles to be added is not particularly limited as long as it is a particle capable of imparting easy slippage, and specific examples include inorganic particles such as silica, calcium carbonate, magnesium carbonate, barium carbonate, calcium sulfate, calcium phosphate, magnesium phosphate, kaolin, aluminum oxide, and titanium oxide, and organic particles such as acrylic resin, styrene resin, urea resin, phenolic resin, epoxy resin, and benzoguanamine resin. Furthermore, precipitated particles obtained by precipitating and finely dispersing a part of a metal compound such as a catalyst during the production process of a polymer such as polyester can also be used.

[0066] The film may also contain additives that are generally used as appropriate, such as recycled resins resulting from trimming losses such as edges, pigments such as titanium oxide and carbon black, flame retardants, weathering stabilizers, heat stabilizers, antistatic agents, melt viscosity improvers, crosslinking agents, lubricants, nucleating agents, plasticizers, antioxidants, antioxidants, light stabilizers, ultraviolet absorbers, neutralizing agents, antifogging agents, antiblocking agents, slip agents, and colorants, which are added for the purpose of improving and adjusting moldability, productivity, and various physical properties of the porous film.

[0067] 3. Manufacturing method Next, a method for producing the present film will be described.

[0068] A method for producing the biaxially stretched film of the present invention will be described below. However, the following description is one example of the method for producing the present film, and the present film is not limited to films produced by this production method.

[0069] The method for producing the film according to one embodiment of the present invention is a method for producing a film by forming a resin composition containing a PBN resin (A) and a polyester (B) into a film and biaxially stretching the film.

[0070] The method of kneading the PBN resin (A), the polyester (B), other resins, and additives to obtain a resin composition is not particularly limited, but in order to obtain the resin composition as simply as possible, it is preferable to manufacture the resin composition by melt kneading using an extruder. In order to uniformly mix the raw materials constituting the resin composition, it is preferable to melt knead using a co-rotating twin screw extruder. The kneading temperature must be equal to or higher than the glass transition temperature (Tg) of all polymers used, and for crystalline resins, equal to or higher than the crystalline melting temperature (Tm) of the polymer. The higher the kneading temperature is, the easier it is for a part of the polymer to undergo an ester exchange reaction and the compatibility is improved, but if the kneading temperature is higher than necessary, the resin will decompose, which is not preferable. For this reason, the kneading temperature is preferably 255°C or higher and 340°C or lower, more preferably 260°C or higher and 330°C or lower, even more preferably 270°C or higher and 320°C or lower, and particularly preferably 280°C or higher and 310°C or lower. If the kneading temperature is within this range, the compatibility and melt moldability can be improved without causing decomposition of the polymer.

[0071] The obtained resin composition can be molded into a biaxially stretched film by a general molding method such as extrusion molding, injection molding, blow molding, vacuum molding, pressure molding, press molding, etc. In each molding method, the apparatus and processing conditions are not particularly limited. The present film is preferably produced, for example, by the following method.

[0072] From the resin composition obtained by mixing, a substantially amorphous and unoriented film (hereinafter, sometimes referred to as "unstretched film") is produced by an extrusion method. For the production of this unstretched film, for example, an extrusion method can be adopted in which the above-mentioned raw materials are melted by an extruder, extruded from a flat die or annular die, and then quenched to form a flat or annular unstretched film. In this case, a laminated structure using multiple extruders may be used in some cases.

[0073] Next, the unstretched film is stretched in the longitudinal direction (MD) of the film and in the transverse direction (TD) perpendicular to the MD, usually by 1.1 to 5.0 times in at least one direction, preferably by 1.1 to 5.0 times in each of the longitudinal and transverse directions, in terms of the stretching effect, film strength, etc.

[0074] As the method of biaxial stretching, any of the conventionally known stretching methods such as tenter-type sequential biaxial stretching, tenter-type simultaneous biaxial stretching, and tubular-type simultaneous biaxial stretching can be adopted. For example, in the case of the tenter-type sequential biaxial stretching method, the unstretched film is heated to a temperature range of Tg to Tg+50°C, where Tg is the glass transition temperature of the resin composition, and stretched in the longitudinal direction by 1.1 to 5.0 times, preferably 1.5 to 4.5 times, more preferably 2.0 to 4.0 times, by a roll-type longitudinal stretching machine, and then stretched in the transverse direction by 1.1 to 5.0 times, preferably 1.5 to 4.8 times, more preferably 2.0 to 4.6 times within the temperature range of Tg to Tg+50°C by a tenter-type transverse stretching machine, so that the film can be produced. If the stretching ratio is within the range, the film can be uniformly stretched, and orientation crystallization is induced, so that the strength of the film can be made within a range suitable for display applications. In the case of tenter-type simultaneous biaxial stretching or tubular-type simultaneous biaxial stretching, the film can be produced by stretching the film simultaneously in both the longitudinal and transverse directions by 1.1 to 5.0 times in each axial direction in the temperature range of, for example, Tg to Tg+50°C.

[0075] The biaxially stretched film stretched by the above method is subsequently heat-set. Heat-setting can impart dimensional stability at room temperature. In this case, the treatment temperature is preferably selected in the range of the crystalline melting temperature of the resin composition, Tm-1 to Tm-80°C. If the heat-setting temperature is within the above range, heat-setting is sufficiently performed, stress during stretching is alleviated, sufficient heat resistance and mechanical properties are obtained, and an excellent film without problems such as breakage or whitening of the film surface can be obtained.

[0076] In the present invention, in order to relieve the stress of crystallization shrinkage due to heat setting, it is preferable to perform relaxation in the width direction during heat setting by 0 to 15%, preferably 3 to 10%. Since the relaxation is performed sufficiently and the film is relaxed uniformly in the width direction, the shrinkage rate in the width direction becomes uniform, and a film with excellent dimensional stability at room temperature is obtained. In addition, since the relaxation is performed following the shrinkage of the film, there is no sagging of the film, no fluttering in the tenter, and no breakage of the film.

[0077] <Uses of this film> The biaxially stretched film of the present invention has excellent folding resistance, heat resistance and formability, and can be used as an optical film, a packaging film, various protective films, etc. In particular, from the viewpoint of folding resistance, it can be suitably used for flexible displays. In addition, the display is particularly preferably a foldable display. The display may be used in a mobile phone, a smartphone, a digital camera, a personal computer, etc. The type of display is not particularly limited, and may be any of a liquid crystal display, a plasma display, an organic electroluminescence display, etc., or may be a touch panel type display. As the display, an organic electroluminescence display is preferable.

[0078] <Another embodiment of the present invention> A biaxially stretched film according to another embodiment of the present invention comprises two or more polyesters, at least one of which is a polybutylene naphthalate resin (A), has a thickness of 20 μm or more and 250 μm or less, and has an average residual strain of 0.110% or less when subjected to a tensile cycle test up to 1.5% tensile strain in each of the longitudinal direction (MD) and the transverse direction (TD). The film having the above-mentioned structure maintains high crystallinity by using a specific blend of polyesters, and therefore has excellent formability, such as melt extrusion formability, and heat resistance. Furthermore, the restoring force of the film is increased, and the bending resistance of the film is improved, making the film suitable for flexible applications, particularly foldable applications. In another embodiment, the average hysteresis loss rate when a tensile cycle test is performed up to a tensile strain of 1.5% in each of the longitudinal direction (MD) and the transverse direction (TD) at 23°C is preferably 18.0% or less, but the average hysteresis loss rate does not necessarily have to be within the above range. The other configurations of the biaxially stretched film according to the other embodiment are as described above, and therefore will not be described again. EXAMPLES

[0079] The following examples are given, but the present invention is not limited to these in any way.

[0080] (1) Hysteresis loss rate In accordance with JIS K 7312:1996, the average hysteresis loss rate at 23°C was determined by the following method. The measuring device used was a tensile tester (Shimadzu Corporation tensile tester AG-1kNXplus). The test specimen was a rectangle cut from the film with a length of 100 mm and a width of 10 mm. The test specimen was chucked at both ends in the length direction with a chuck distance of 50 mm, raised to a strain of 1.5% at a crosshead speed of 0.5 mm / min, and then lowered to the initial position at the same speed to obtain a stress-strain curve from one cycle of tensile cycle test. The stress-strain curve had a profile as shown in Figure 1, and the hysteresis loss rate was calculated from the obtained stress-strain curve using the area A1 (abcda) of the curve obtained during the upward movement and the area A2 (abcef) which is the difference between the area A1 and the area of ​​the curve obtained during the downward movement, using the following formula 1. The test was performed three times, and the average value was calculated. The above tensile cycle test was performed in the longitudinal direction (MD) and the transverse direction (TD) of the film, respectively, and the average value was calculated. Hysteresis loss rate = (A2 / A1) x 100 (Formula 1)

[0081] (2) Residual strain In accordance with JIS K 7312:1996, the average value of residual strain at 23°C was determined by the following method. The measurement device used was a tensile tester (Shimadzu Corporation AG-1kNXplus tensile tester). The test pieces were cut from the film in a rectangle with a length of 100 mm in the measurement direction and a width of 10 mm. Both ends of the test piece in the length direction were chucked with a chuck distance of 50 mm, and the test piece was raised to a strain of 1.5% at a crosshead speed of 0.5 mm / min, and then lowered to the initial position at the same speed. From the stress-strain curve obtained from one cycle of tensile cycle test, the strain at the point where the stress was removed was taken as the residual strain. The test was performed three times, and the average value was calculated. The above tensile cycle test was performed in the machine direction (MD) and the transverse direction (TD) of the film, and the average value was calculated.

[0082] (3) Glass transition temperature (Tg) The obtained film was heated to the melting temperature at a heating rate of 10°C / min once and then cooled at a heating rate of 10°C / min in accordance with JIS K7121 (2012) using a Diamond DSC (manufactured by PerkinElmer Japan), and the glass transition temperature during the heating process at a heating rate of 10°C / min was measured.

[0083] (4) Crystal melting temperature (Tm) The crystalline melting temperature of the obtained film was measured in a heating process at a heating rate of 10° C. / min using a Diamond DSC (manufactured by PerkinElmer Japan) in accordance with JIS K7121 (2012).

[0084] (5) Heat of crystal fusion (ΔHm) The heat of crystal fusion of the obtained film was measured using a Diamond DSC (manufactured by PerkinElmer Japan) in a temperature rise process at a heating rate of 10° C. / min in accordance with JIS K7122 (2012).

[0085] (6) Formability In the extrusion molding, when the sheet was cooled and solidified by a cast roll to obtain a pre-stretched sheet, if a transparent film was obtained without crystallization and whitening, it was rated as ◯, and if a crystallization and whitening film was obtained, it was rated as ×.

[0086] (7) Heat shrinkage rate The film was cut into a rectangle 120 mm long and 10 mm wide in the measurement direction, and a mark was made 100 mm from the end. These test pieces were hung by clips at the end and heated at 150°C for 30 minutes. After cooling, the length from the end of the test piece to the mark was measured to obtain the thermal shrinkage. The measurements were performed in both the machine direction (MD) and the transverse direction (TD).

[0087] (8) Thickness The thickness of this film was measured at five random locations on the surface with a 1 / 1000 mm dial gauge, and the average was taken as the thickness.

[0088] [PBN resin (A)] As the PBN resin (A), a homo-PBN having a dicarboxylic acid component (a-1): 2,6-naphthalenedicarboxylic acid = 100 mol % and a diol component (a-2): 1,4-butanediol = 100 mol % was used (TQB-OT, manufactured by Teijin Ltd.). The PBN resin had a crystalline melting temperature (Tm) of 243°C and a glass transition temperature (Tg) of 77°C.

[0089] [Polyester (B)] As the polyester (B), a homo-PEN having a dicarboxylic acid component (b-1) of 2,6-naphthalenedicarboxylic acid = 100 mol % and a diol component (b-2) of ethylene glycol = 100 mol % was used (TN8065S, manufactured by Teijin Ltd.). The crystalline melting temperature (Tm) of the PEN-based resin was 263°C, the glass transition temperature (Tg) was 121°C, and the crystalline melting heat (ΔHm) was 43 J / g.

[0090] Example 1 Pellet-like (B) was added at a ratio of 90% by mass to 10% by mass of pellet-like (A) (900 parts by mass of (B) to 100 parts by mass of (A)), dry-blended, and then melt-kneaded in a Φ40 mm twin-screw extruder set at 285°C. The mixture was extruded as a film from a T-die with a gap of 1.0 mm, taken up by a cast roll at 105°C, and cooled and solidified to obtain a film-like material (cast film) with a thickness of approximately 450 μm. The resulting cast film was then passed through a longitudinal stretching machine and heated with an infrared heater (temperature near the heater: 170°C) to be stretched 2.8 times in the machine direction (MD).Then, the resulting longitudinally stretched film was passed through a transverse stretching machine (tenter) to be stretched 4.0 times in the width direction (TD) at a preheating temperature of 130°C, a stretching temperature of 135°C, and a heat setting temperature of 190°C.Then, the film was subjected to a 5% relaxation treatment in the width direction (TD) while being heat set in the tenter. The obtained film was subjected to measurements, and the results are shown in Table 1.

[0091] Example 2 A pellet-like (B) was added in a ratio of 80% by mass to 20% by mass of pellet-like (A) (400 parts by mass of (B) per 100 parts by mass of (A)), dry-blended, and then a cast film was obtained in the same manner as in Example 1, except that the cast roll temperature was set to 100°C. The resulting cast film was then passed through a longitudinal stretching machine and heated with an infrared heater (temperature near the heater: 160°C) to be stretched 2.8 times in the machine direction (MD).Then, the resulting longitudinally stretched film was passed through a transverse stretching machine (tenter) to be stretched 3.9 times in the width direction (TD) at a preheating temperature of 120°C, a stretching temperature of 125°C, and a heat setting temperature of 190°C, and then the film was relaxed by 5% in the tenter. The obtained film was subjected to measurements, and the results are shown in Table 1.

[0092] Example 3 A pellet-like (B) was added in a ratio of 70 mass% to 30 mass% of pellet-like (A) (233 mass parts of (B) per 100 mass parts of (A)), dry blended, and then a cast film was obtained in the same manner as in Example 1, except that the cast roll temperature was 95°C. The resulting cast film was then passed through a longitudinal stretching machine and heated with an infrared heater (temperature near the heater: 155°C) to be stretched 2.8 times in the machine direction (MD).Then, the resulting longitudinally stretched film was passed through a transverse stretching machine (tenter) to be stretched 3.9 times in the width direction (TD) at a preheating temperature of 115°C, a stretching temperature of 120°C, and a heat setting temperature of 190°C, and then the film was relaxed by 5% in the tenter. The obtained film was subjected to measurements, and the results are shown in Table 1.

[0093] Example 4 A pellet-like (B) was added in a ratio of 60 mass% to 40 mass% of pellet-like (A) (150 mass parts of (B) per 100 mass parts of (A)), dry blended, and then a cast film was obtained in the same manner as in Example 1, except that the cast roll temperature was 90°C. The resulting cast film was then passed through a longitudinal stretching machine and heated with an infrared heater (temperature near the heater: 145°C) to be stretched 2.8 times in the machine direction (MD).Then, the resulting longitudinally stretched film was passed through a transverse stretching machine (tenter) to be stretched 3.8 times in the width direction (TD) at a preheating temperature of 105°C, a stretching temperature of 110°C, and a heat setting temperature of 190°C, and then the film was relaxed by 5% in the tenter. The obtained film was subjected to measurements, and the results are shown in Table 1.

[0094] Example 5 A pellet-like (B) was added in a ratio of 50% by mass to 50% by mass of pellet-like (A) (100 parts by mass of (B) per 100 parts by mass of (A)), dry-blended, and then a cast film was obtained in the same manner as in Example 1, except that the cast roll temperature was 81°C. The resulting cast film was then passed through a longitudinal stretching machine and heated with an infrared heater (temperature near the heater: 135°C) to be stretched 2.8 times in the machine direction (MD).Then, the resulting longitudinally stretched film was passed through a transverse stretching machine (tenter) to be stretched 4.0 times in the width direction (TD) at a preheating temperature of 95°C, a stretching temperature of 100°C, and a heat setting temperature of 190°C, and then the film was relaxed by 5% in the tenter. The obtained film was subjected to measurements, and the results are shown in Table 1.

[0095] Example 6 A pellet-like (B) was added in a ratio of 40 mass% to 60 mass% of pellet-like (A) (67 mass parts of (B) per 100 mass parts of (A)), dry blended, and then a cast film was obtained in the same manner as in Example 1, except that the cast roll temperature was set to 70°C. The resulting cast film was then passed through a longitudinal stretching machine and heated with an infrared heater (temperature near the heater: 133°C) to be stretched 2.8 times in the machine direction (MD).Then, the resulting longitudinally stretched film was passed through a transverse stretching machine (tenter) to be stretched 3.7 times in the width direction (TD) at a preheating temperature of 95°C, a stretching temperature of 100°C, and a heat setting temperature of 190°C, and then the film was relaxed by 5% in the tenter. The obtained film was subjected to measurements, and the results are shown in Table 1.

[0096] Comparative Example 1 A cast film was obtained in the same manner as in Example 1, except that 100% by mass of a PEN-based resin was used as the polyester (B) and the temperature of the casting roll was set to 110°C. The resulting cast film was then passed through a longitudinal stretching machine and heated with an infrared heater (temperature near the heater: 175°C) to be stretched 2.6 times in the machine direction (MD).The resulting longitudinally stretched film was then passed through a transverse stretching machine (tenter) to be stretched 3.8 times in the width direction (TD) at a preheating temperature of 125°C, a stretching temperature of 130°C, and a heat setting temperature of 190°C, and then the film was relaxed by 5% in the tenter. The obtained film was subjected to measurements, and the results are shown in Table 1.

[0097] Comparative Example 2 An attempt was made to produce a cast film in the same manner as in Example 1, except that 100% by mass of PBN-based resin (A) was used and the temperature of the casting roll was set to 75°C. However, whitening due to crystallization occurred and an amorphous film could not be obtained. Therefore, the moldability in Table 1 was rated as x.

[0098] [Table 1]

[0099] As shown in the above examples, the mixed polyesters of Examples 1 to 6, by mixing the polyester (B), had a high glass transition temperature (Tg) and were excellent in heat resistance. Moreover, the films of Examples 1 to 6 have clearly lower hysteresis loss rates and residual strain values ​​than Comparative Example 1, and can be said to have greater recovery and superior folding resistance. Furthermore, in Comparative Example 2, the crystallization rate was too fast, which caused a problem in moldability, but in the films of Examples 1 to 6, film formation was possible without any problem, and therefore it can be said that the films are also excellent in moldability. [Industrial Applicability]

[0100] The biaxially stretched film of the present invention has excellent heat resistance, folding resistance and formability, and can therefore be suitably used for optical films, particularly for flexible displays. Therefore, the embodiments of the present disclosure are useful for flexible displays, such as foldable displays, bendable displays, rollable displays, and stretchable displays, that utilize the advantages of flexible display panels that can be folded, bent, or rolled.

Claims

1. Contains two or more polyesters, At least one of them is a polybutylene naphthalate-based resin (A), The thickness is 20 μm or more and 250 μm or less, A biaxially stretched film having an average hysteresis loss rate of 18.0% or less when subjected to a tensile cycle test up to 1.5% tensile strain in each of the machine direction (MD) and the transverse direction (TD), The polyester (B) other than the polybutylene naphthalate-based resin (A), The glass transition temperature of the polyester (B) is 75° C. or more and 150° C. or less, The crystalline melting temperature of the polyester (B) is 220° C. or higher and 300° C. or lower, The polyester (B) has a heat of crystalline fusion of 15 J / g or more and 60 J / g or less.

2. A polyester composition comprising two or more types of polyester, At least one of them is a polybutylene naphthalate-based resin (A), The thickness is 20 μm or more and 250 μm or less, A biaxially stretched film having an average hysteresis loss rate of 18.0% or less when subjected to a tensile cycle test up to 1.5% tensile strain in each of the machine direction (MD) and the transverse direction (TD), The polyester (B) other than the polybutylene naphthalate-based resin (A), The biaxially stretched film, wherein the polyester (B) is a polyethylene naphthalate resin.

3. A polyester composition comprising two or more types of polyester, At least one of them is a polybutylene naphthalate-based resin (A), The polyester (B) other than the polybutylene naphthalate-based resin (A), The thickness is 20 μm or more and 250 μm or less, A biaxially stretched film having an average hysteresis loss rate of 18.0% or less when subjected to a tensile cycle test up to 1.5% tensile strain in each of the machine direction (MD) and the transverse direction (TD), The glass transition temperature is 75° C. or more and 150° C. or less, The crystal melting temperature is 220° C. or more and 300° C. or less, A biaxially stretched film having a heat of crystalline fusion of 10 J / g or more and 60 J / g or less.

4. A biaxially stretched film as described in claim 1 or 3, wherein the polyester (B) is a polyethylene naphthalate resin or a polycyclohexylene dimethylene terephthalate resin.

5. A biaxially stretched film described in any one of claims 1 to 4, wherein the content of the polybutylene naphthalate resin (A) is 30 mass% or more out of a total of 100 mass% of the polybutylene naphthalate resin (A) and the polyester (B).

6. The biaxially stretched film according to any one of claims 1 to 5, wherein the average residual strain when subjected to a tensile cycle test up to a tensile strain of 1.5% in each of the machine direction (MD) and the transverse direction (TD) is 0.110% or less.

7. The biaxially stretched film according to any one of claims 1 to 6, wherein the heat shrinkage rate when heated at 150°C for 30 minutes is 5.0% or less in both the machine direction (MD) and the width direction (TD).

8. The biaxially stretched film according to any one of claims 1 to 7, which is for a display.

9. A flexible display comprising the biaxially stretched film according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • JP1975024366A

  • Copolyester

    JP1993209044A

  • Resin composition

    JP1995138461A

  • Polyester resin composition and molded product therefrom

    JP2001234048A