Deep drawing processing base paper and deep drawing products

A base paper for deep drawing processing, optimized with specific fiber length, modulus, and elongation, addresses the limitations of pulp mold containers by enhancing extensibility and shape reproducibility, offering an environmentally friendly alternative to plastic containers.

JP7559669B2Active Publication Date: 2024-10-02OJI HLDG CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2021079116
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-05-07
Publication Date
2024-10-02
Estimated Expiration
2041-05-07

AI Technical Summary

Technical Problem

Conventional pulp mold containers face challenges in productivity, water resistance, oil resistance, and limited shapeability due to poor stretchability and ductility, while plastic containers pose environmental concerns. Existing solutions like using alkyl ketene dimer on paper surfaces for extensibility lead to adhesion issues with laminate films.

Method used

The base paper for deep drawing processing is formulated with specific fiber length, Young's modulus, elongation, and curl values, combined with a thermoplastic resin layer, to enhance extensibility, reduce cracking, and improve shape reproducibility, using pulp as the primary material.

Benefits of technology

The solution results in a paper with high extensibility, reduced cracking, and excellent shape reproducibility, producing deep-drawn products with reduced environmental impact.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007559669000002
    Figure 0007559669000002
  • Figure 0007559669000003
    Figure 0007559669000003
  • Figure 0007559669000001
    Figure 0007559669000001
Patent Text Reader

Abstract

To provide a base paper for deep drawing that has low environmental load, has high extensibility, prevents cracking in the paper surface during deep drawing, and has high shape reproducibility, and a deep-drawn product including the same.SOLUTION: Base paper for deep drawing has a paper substrate layer composed of a paper substrate. The constituent pulp of the paper substrate has a length-weighted mean fiber length of 0.60 mm or more and 2.40 mm or less. Out of Young's moduli of the base paper in the longitudinal direction and the transverse direction, the greater one is defined as A and the smaller one is defined as B, where A is 2,600 N / mm2 or less and the ratio C of Young's moduli represented by the formula (1): C=A / B is 1.00 or more and 1.80 or less. The base paper has elongations at break of 3.0% or more in the longitudinal direction and the transverse direction, respectively, and the geometric mean of the elongations at break in the longitudinal direction and the transverse direction is 4.0% or more.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a base paper for deep drawing processing and a deep drawing product. [Background technology]

[0002] Conventionally, plastic containers have been used in large quantities as food containers or packaging materials for various industrial products because they are easy to mold, can be mass-produced, and can be manufactured at low cost. For example, polystyrene foam containers obtained by molding expanded polystyrene beads or press-molding expanded polystyrene sheets, polypropylene containers, polyethylene terephthalate containers, polyvinyl chloride containers, etc. are widely used as these plastic containers. However, such plastic containers have the problem that they place a heavy burden on the environment when they are disposed of. That is, when they are buried in landfills, they remain in the ground semi-permanently without decomposing, and when they are incinerated, they easily damage incinerators due to their high combustion calories, are difficult to completely burn, and in particular, when polyvinyl chloride is used, there is a risk of generating highly corrosive hydrogen chloride gas.

[0003] Therefore, in recent years, in consideration of environmental issues, recycling issues, and resource conservation, there has been a demand for containers made of pulp that are recyclable, have low combustion calories when discarded, are biodegradable, and have a low environmental impact, as an alternative to the above-mentioned plastic containers.

[0004] Pulp-molded containers have been used as three-dimensional molded products made of pulp or a material mainly made of pulp. Pulp-molded containers have been widely used as packaging containers. However, the production of pulp molds takes time, and there have been problems with productivity. Furthermore, it has been difficult to impart sufficient water resistance and oil resistance to pulp-molded containers, which are often required for food tray containers.

[0005] Other than pulp moulding, a method of press-molding a base sheet mainly made of pulp such as paperboard under heating is known as a method of obtaining a molded product mainly made of pulp. In this method, a base sheet with lines drawn in advance is loaded between a male and female mold, and press-molded by heat and pressure. This press molding method has high productivity because a molded product can be obtained with one press. However, unlike resins and metals, base sheets mainly made of paper pulp generally have poor extensibility, stretchability, and elasticity. Therefore, if deep press molding is performed to mold a tray with a certain depth, the base sheet may not be able to withstand the stretching and may break. As a result, when ordinary paperboard or the like is used as a base material, only molded containers with almost no depth, such as so-called paper plates, can be manufactured, and the shape of the molded product obtained is very limited.

[0006] In order to solve such problems, for example, Patent Document 1 describes a multi-layered base paper for molded containers consisting of two or more layers, in which a mixture of starch and alkyl ketene dimer is coated on the surfaces of the front and back layers. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2014-167192 A Summary of the Invention [Problem to be solved by the invention]

[0008] The base paper for molded containers described in Patent Document 1 has an improved extensibility by using a coating layer containing alkyl ketene dimer (AKD) on the surface. However, when alkyl ketene dimer (AKD) is used on the surface of the paper substrate, there is a problem that the adhesion between the paper substrate and the laminate film is reduced, causing the laminate film to peel off.

[0009] The present invention aims to provide a base paper for deep-draw molding that has a low environmental impact, high extensibility, is less susceptible to cracks on the paper surface during deep-draw molding, and has high shape reproducibility for the molding die, and a deep-draw molded product using the same. [Means for solving the problem]

[0010] The inventors have found that the above problem can be solved by setting the length-weighted average fiber length of the pulp constituting the base paper for deep drawing processing within a specific range, setting the maximum values ​​of the Young's modulus in the longitudinal direction and the Young's modulus in the transverse direction of the base paper to be equal to or less than a specific value and setting the ratio thereof within a specific range, and further setting the breaking elongation in the longitudinal direction and the transverse direction and the geometric mean of the breaking elongation in the longitudinal direction and the transverse direction within specific ranges. That is, the present invention provides the following: <1> ~ <6> Regarding. <1> A base paper for deep drawing processing, the base paper having a paper base layer made of a paper base material, The length-weighted average fiber length of the pulp constituting the base paper is 0.60 mm or more and 2.40 mm or less, and the Young's modulus of the base paper in the longitudinal direction and the transverse direction, the larger of which is designated as A and the smaller of which is designated as B, is 2,600 N / mm 2 and the ratio C of Young's modulus represented by the following formula (1) is 1.00 or more and 1.80 or less, C=A / B (1) The base paper for deep drawing processing has a longitudinal and transverse breaking elongation of 3.0% or more, and a geometric mean of the longitudinal and transverse breaking elongations of 4.0% or more. <2> The Young's modulus ratio C is 1.00 or more and 1.50 or less. <1> The deep drawing forming base paper described in the above. <3> The curl value of the pulp constituting the paper base material is 7% or more and 12% or less. <1> or <2> The deep drawing forming base paper described in the above. <4> The base paper has a basis weight of 100 g / m 2 More than 500g / m 2 The paper thickness is 0.10 mm or more and 0.90 mm or less, and the density is 0.60 g / cm 3 More than 1.2g / cm3 Below is the <1> ~ <3> 10. The deep drawing forming base paper according to claim 9, <5> A thermoplastic resin layer is further provided on at least one surface of the paper base layer. <1> ~ <4> 10. The deep drawing forming base paper according to claim 9, <6> <1> ~ <5> A deep-drawn product obtained by using the deep-drawn forming base paper according to any one of the above. Effect of the Invention

[0011] According to the present invention, there are provided a deep-drawing base paper that has low environmental impact, high extensibility, is less susceptible to cracks on the paper surface during deep-drawing, and has high shape reproducibility, and a deep-drawing molded product using the same. Note that "high shape reproducibility" or "excellent shape reproducibility" means that the shape of the obtained molded product is highly similar to the shape of the mold used during molding, and that a molded product close to the desired shape is obtained. [Brief description of the drawings]

[0012] [Figure 1] FIG. 1 is a schematic diagram of deep drawing processing by pressing. [Diagram 2] 1A and 1B are a plan view and a front view of a molded product produced in an example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] [Base paper for deep drawing processing] The deep drawing base paper of this embodiment (hereinafter simply referred to as "base paper") has a paper base layer made of a paper base material, and the length-weighted average fiber length of the pulp constituting the paper base material is 0.60 mm or more and 2.40 mm or less. When the larger of the Young's modulus in the longitudinal direction and the Young's modulus in the transverse direction of the base paper is A and the smaller Young's modulus is B, A is 2,600 N / mm 2 and the Young's modulus ratio C, expressed by the following formula (1), is 1.00 or more and 1.80 or less, the breaking elongation in the longitudinal direction and the transverse direction of the base paper is each 3.0% or more, and the geometric mean of the breaking elongation in the longitudinal direction and the transverse direction is 4.0% or more. C=A / B (1) According to the deep drawing forming base paper of this embodiment, a deep drawing forming base paper is provided which has a low environmental impact, high extensibility, is less susceptible to cracks on the paper surface when deep drawing, and has high shape reproducibility. Compared with conventional plastic containers, the deep-draw molded product is obtained using the deep-draw molding base paper of this embodiment, which has a paper base layer mainly made of pulp, and thus the environmental load is reduced. The reason why cracks are less likely to occur on the paper base surface during deep drawing and shape reproducibility is high is thought to be as follows: Since the paper base is a non-uniform sheet of pulp fibers, there are a mixture of areas with many inter-fiber bonds and where cracks are less likely to occur during deep drawing, and areas with few inter-fiber bonds and where breakage and cracks are likely to occur during deep drawing. It is thought that by setting the length-weighted average fiber length of the pulp constituting the paper base layer within a specific range, both the strength of the paper base and the suppression of cracks during deep drawing are achieved. Furthermore, by setting the larger of the Young's modulus in the longitudinal direction and the transverse direction of the base paper to a specific value or less and setting the above-mentioned Young's modulus ratio C to be 1.00 or more and 1.80 or less, a paper base material with appropriate flexibility is obtained, which suppresses the occurrence of cracks during deep drawing and improves the ability to conform to the forming mold during forming, thereby obtaining excellent shape reproducibility. Furthermore, it is believed that by setting the longitudinal and transverse breaking elongations of the base paper and the geometric mean of the longitudinal and transverse breaking elongations to a specific value or more, the occurrence of cracks on the paper substrate surface during deep drawing is further suppressed. Note that in deep drawing, it is necessary to suppress the occurrence of cracks on the paper substrate surface due to short-term stretching, while in the measurement of breaking elongation, the base paper is broken over a longer period of time than in deep drawing, so that using a base paper with excellent breaking elongation does not necessarily suppress cracks on the paper surface during deep drawing, but a base paper that does not satisfy the above breaking elongation requirements does not provide sufficient molding processability. Deep drawing is a molding method for obtaining a three-dimensional molded product from a single sheet without processing such as cutting, bonding, etc. Examples of deep drawing include press molding, vacuum molding, and compressed air molding. The present invention will now be described in further detail.

[0014] The deep drawing forming base paper has a paper base layer made of a paper base material. The deep drawing forming base paper has at least one paper base layer, and may have two or more paper base layers. Among these, it is preferable to have 1 to 5 paper base layers, and it is more preferable to have 1 to 3 paper base layers. Examples of a paper base paper having two or more paper base layers include polysand paper having a polyethylene film sandwiched between two paper base layers (paper base material / polyethylene film / paper base material) and polysand paper having a polyethylene film sandwiched between three paper base layers (paper base material / polyethylene film / paper base material / polyethylene film / paper base material). A thermoplastic resin layer may be provided on one or both sides of the paper substrate or polysand paper. That is, the deep drawing base paper may be composed of only a paper substrate layer, but it is preferable that in addition to the paper substrate layer, at least one side of the paper substrate layer has a thermoplastic resin layer. When the deep drawing product is made, the thermoplastic resin layer preferably has a thermoplastic resin layer at least on the food contact surface. A thermoplastic resin layer may also be provided on the surface opposite to the food contact surface.

[0015] [Paper base layer] The paper base layer is made of a paper base material, and the paper base material contains pulp as a raw material. The manufacturing method and type of pulp are not particularly limited. <Raw pulp> In this embodiment, the pulp constituting the paper base material is preferably natural pulp fiber from the viewpoint of reducing the environmental load, and as the natural pulp fiber, wood fiber (chemical pulp, mechanical pulp), non-wood fiber, waste paper pulp, etc. are arbitrarily used as necessary. Among wood fibers, examples of chemical pulp include kraft pulp, which uses caustic soda and sodium sulfide during wood chip cooking, and sulfite pulp, which uses sulfurous acid and hydrogen sulfite. These pulps may be unbleached or bleached (bleached). Examples of mechanical pulp include ground wood pulp (GP) obtained by grinding logs with a grinder, refiner ground wood pulp (RGP) obtained by grinding (refining) waste wood from a lumber mill with a refiner, and thermomechanical pulp (TMP) obtained by heating and refining wood chips. Among these wood fiber pulps, long fiber pulps obtained from coniferous trees such as pine, larch, cedar, fir, and cypress are preferably used to improve the stretchability and strength of the paper base material. Also, short fiber pulps obtained from broad-leaved trees such as eucalyptus, acacia, birch, beech, maple, elm, and chestnut can be used in combination, provided that the effects of the present invention are not impaired.

[0016] Examples of non-wood fibers that can be used in this embodiment include bast fibers such as paper mulberry, mitsumata, gampi, flax, taiman, kenaf, choma, jute, and sunn hemp, seed hair fibers such as cotton and cotton linters, leaf fibers such as Manila hemp, sisal, and esparto, and stem fibers such as bamboo, rice straw, wheat straw, and sugarcane bagasse. Paper mulberry, mitsumata, kenaf, Manila hemp, sisal, cotton, and cotton linters are particularly suitable because they have long fiber lengths and can improve the stretchability and strength of the base paper of this embodiment. The cooking of non-wood fibers can be carried out in the same manner as for wood fibers. Examples of waste paper pulp that can be used in this embodiment include waste cardboard and waste magazine paper.

[0017] These pulp fibers can be used alone or in combination of two or more kinds. In addition, synthetic resin fibers can be mixed as necessary within a range that does not impair the effects of the present invention. Examples of synthetic resin fibers that can be used include polyethylene fibers, polypropylene fibers, polyamide fibers, polyethylene terephthalate fibers, polybutylene terephthalate fibers, and polylactic acid fibers.

[0018] In this embodiment, from the viewpoint of obtaining the desired length-weighted average fiber length described later, it is preferable that the raw material pulp contains coniferous pulp, and it is also preferable to use only coniferous pulp, or it is also preferable to use a combination of coniferous pulp and hardwood pulp.

[0019] <Pulp characteristics> (length-weighted average fiber length) The length-weighted average fiber length of the pulp constituting the paper base material is 0.60 mm or more, preferably 0.70 mm or more, and more preferably 0.80 mm or more, from the viewpoint of obtaining the paper strength as a base paper, and although there is no particular upper limit, a length of 2.40 mm or less is realistic from a practical standpoint. The length-weighted average fiber length of the fibers constituting the paper base material is calculated by disintegrating the base paper using the method described in the Examples and measuring the fiber length of the resulting pulp slurry using a fiber length measuring device (e.g., Valmet, Model FS-5, with UHD base unit). The length-weighted average fiber length is calculated from the fiber lengths measured by selecting fibers having a length of 0.2 mm or more and 7.6 mm or less.

[0020] (Percentage of fine fibers) In the pulp constituting the paper base material, the proportion of fine fibers having a fiber length of 0.2 mm or less is preferably 8% or more, more preferably 9% or more, even more preferably 10% or more, still more preferably 12% or more, and preferably 35% or less, more preferably 32% or less, even more preferably 30% or less, still more preferably 28% or less, and still more preferably 26% or less. When the ratio of the number of fine fibers is within the above range, the presence of the fine fibers increases interfiber bonding, which further suppresses the occurrence of cracks during deep drawing, and is also preferable because the decrease in breaking elongation due to the increase in the fine fibers is suppressed. The number of fine fibers with a fiber length of 0.2 mm or less in the pulp fiber constituting the paper base material is calculated by disintegrating the base paper using the method described in the Examples, measuring the fiber length of the resulting pulp slurry with a fiber length measuring device (e.g., Valmet Model FS-5 with UHD base unit). Fibers with a fiber length of 0.2 mm or less and a fiber width of 75 μm or less are defined as fine fibers, and the ratio of the number of fine fibers to the number of measured pulp fibers is calculated.

[0021] In order to bring the length-weighted average fiber length and the proportion of fine fibers in the pulp constituting the paper base material within the above ranges, appropriate adjustments can be made by selecting the raw pulp, whether or not filtration is performed in the chemical and mechanical treatment of the pulp, and selecting the concentration and beating load of the beating treatment. Furthermore, for the purpose of increasing the proportion of fine fibers, powdered pulp obtained by mechanically pulp fiber crushing may be added. Furthermore, when manufacturing the paper base material, the proportion of fine fibers remaining in the paper base material during papermaking can be increased by adding a retention aid that is a cationic polymer in the papermaking process, so that the proportion of fine fibers remaining in the paper base material during papermaking can be increased by adding a cationic polymer in the papermaking process.

[0022] (Curl value) From the viewpoint of increasing interfiber bonds and setting the breaking elongation of the base paper within the desired range, the curl value of the pulp constituting the paper base material is preferably 5% or more, more preferably 5.5% or more, even more preferably 6% or more, still more preferably 6.5% or more, particularly preferably 7% or more, and is preferably 12% or less, more preferably 11% or less, and even more preferably 10% or less. The curl value (also called curl index) of the pulp constituting the paper base material is expressed as follows, using the length of the pulp fibers when stretched straight (L1) and the length of the fibers in a curled state (L2): Curl value (%) = (L1-L2) / L1 x 100 Here, the fiber length (L1) and the fiber length (L2) are calculated as length-weighted average values ​​of the fiber lengths measured by selecting fibers with L1 of 0.2 mm or more and 7.6 mm or less. The above-mentioned length-weighted average fiber length is the length-weighted average fiber length of L1. L1 and L2 are calculated by image processing. L1 is calculated by image processing so that the fiber length is at its longest, and L2 is calculated by image processing so that the fiber length is at its longest in the curled (bent) state. In addition, the curl value tends to increase by increasing the concentration of the pulp slurry during beating, so the curl value of the pulp constituting the base paper can be adjusted by adjusting the concentration of the pulp slurry during beating. The curl value of the pulp constituting the paper base material is calculated by disintegrating the base paper using the method described in the Examples, and measuring the curl value of the resulting pulp slurry using a fiber length measuring device (e.g., Valmet, model FS-5, with UHD base unit).

[0023] (Canadian Standard Freeness) The Canadian Standard Freeness (CSF) of the pulp constituting the paper base material, measured in accordance with JIS P 8121-2:2012, is preferably 200 mL or more, more preferably 400 mL or more, even more preferably 600 mL or more, from the viewpoint of suppressing the occurrence of cracks during molding and improving shape reproducibility during molding, and is preferably 800 mL or less, more preferably 750 mL or less, even more preferably 700 mL or less.

[0024] <Optional ingredients> The paper base material may contain optional components as necessary, such as anionic, cationic, nonionic or amphoteric retention agents, drainage improvers, dry strength agents, wet strength agents, fillers, internal additives such as sizing agents, dyes, fluorescent whitening agents, etc. Examples of the dry strength agent include cationic starch, polyacrylamide, carboxymethyl cellulose, etc. The content of the dry strength agent is not particularly limited, and the amount used may be appropriately adjusted according to the characteristics of the pulp used, the papermaking method, etc. Examples of the wet strength agent include polyamide polyamine epichlorohydrin, urea formaldehyde resin, and melamine formaldehyde resin. Examples of the filler include inorganic fillers such as talc, kaolin, calcined kaolin, calcium carbonate, calcium sulfate, barium sulfate, titanium dioxide, zinc oxide, alumina, magnesium carbonate, magnesium oxide, silica, white carbon, bentonite, zeolite, sericite, and smectite, and organic fillers such as acrylic resins and vinylidene chloride resins. Examples of the sizing agent include internal sizing agents such as rosin sizing agents, synthetic sizing agents, and petroleum resin-based sizing agents, and surface sizing agents such as styrene / acrylic acid copolymers and styrene / methacrylic acid copolymers.

[0025] <Manufacturing method of paper base material> The method for producing the paper base material preferably includes a step of making paper from a slurry containing the above-mentioned raw material pulp. The papermaking method is not particularly limited, and examples thereof include an acidic papermaking method in which papermaking is carried out at a pH of about 4.5, and a neutral papermaking method in which papermaking is carried out at a pH of about 6 to about 9. In the papermaking process, chemicals for the papermaking process such as a pH adjuster, an antifoaming agent, a pitch control agent, and a slime control agent can be appropriately added as necessary. The papermaking machine is not particularly limited, and examples thereof include continuous papermaking machines of the Fourdrinier type, cylinder type, and tilt type, and multi-layer papermaking machines that combine these.

[0026] In this embodiment, in the papermaking process, the jet / wire ratio (J / W ratio), which is the ratio of the flow velocity of the paper material sprayed onto the wire (J) to the papermaking wire running speed (W), is preferably close to 1.0 from the viewpoint of setting the above-mentioned Young's modulus ratio C in the desired range, and is preferably 0.95 or more, more preferably 0.98 or more, even more preferably 1.00 or more, and is preferably 1.08 or less, more preferably 1.05 or less, even more preferably 1.02 or less.

[0027] (Clupak Processing) The paper base may be subjected to Clupak treatment, which is a process that imparts stretchability by minutely shrinking the paper on the paper machine. The specific manufacturing method is to install a Clupak device in a part of the papermaking machine dryer, pass the wet paper between an endless thick elastic rubber blanket with nip rolls and a heated dryer, and the blanket, which has been stretched in advance, shrinks the running paper web, increasing the breaking elongation. The shrinkage that is created is then dried and fixed so that it does not stretch in the subsequent process. In the Clupak device, the longitudinal breaking elongation of the paper can be adjusted mainly by the ratio of the production speed on the inlet side of the Clupak device to the production speed on the outlet side of the Clupak device.

[0028] <Characteristics of paper base material> The paper base material may be a single-layer paper or a multi-layer paper, preferably a single-layer to seven-layer paper, more preferably a single-layer to five-layer paper. Furthermore, the paper substrate may be a multi-layer paper in which two or more paper layers are laminated with an adhesive. The total thickness of the paper base layer is preferably 50 μm or more, more preferably 60 μm or more, even more preferably 80 μm or more, and is preferably 500 μm or less, more preferably 450 μm or less, even more preferably 400 μm or less, and even more preferably 350 μm or less. The total thickness of the paper base layers refers to the total thickness when the deep drawing base paper has two or more paper base layers, for example, when polysand paper is used. The thickness of the paper substrate is measured in accordance with JIS P 8118:2014.

[0029] The paper substrate preferably has a basis weight of 30 g / m 2 More preferably, 50 g / m 2 More preferably, 100 g / m 2 More preferably, 150 g / m 2 More preferably, 180 g / m 2 and preferably 500 g / m 2 Less than 400 g / m 2 Less than 350 g / m 2 More preferably, 300 g / m or less 2 The following is the result. The basis weight of the paper base material is measured in accordance with JIS P 8124:2011.

[0030] The density of the paper substrate is preferably less than 0.4 g / cm 3 More preferably, 0.5 g / cm 3 More preferably, 0.6 g / cm 3 More preferably, 0.65 g / cm 3 and preferably 1.2 g / cm 3 Less than or equal to 1.1 g / cm 3 More preferably, 1.0 g / cm 3 The following is the result. In addition, when the paper base is Clupak-treated, the density of the paper base is preferably 0.4 g / cm 3 More preferably, 0.5 g / cm 3 More preferably, 0.6 g / cm 3 More preferably, 0.65 g / cm 3 and preferably 1.2 g / cm 3 Less than or equal to 1.1 g / cm 3More preferably, 1.0 g / cm 3 More preferably, 0.9 g / cm 3 Less than 0.85 g / cm 3 The following is the result. The density of the paper substrate is calculated from the thickness and basis weight of the paper substrate.

[0031] From the viewpoint of reducing the environmental impact, the content of the paper base material in the deep drawing forming base paper is preferably 30% by mass or more, more preferably 40% by mass or more, even more preferably 50% by mass or more, still more preferably 52% by mass or more, and particularly preferably 55% by mass or more, relative to the total mass of the base paper, and the upper limit is not particularly limited and may be 100% by mass.

[0032] [Other layers] <Pigment coating layer> The deep drawing base paper of this embodiment may have a coating layer containing a pigment and an adhesive on at least one side of the paper base layer as necessary. By providing such a coating layer, it is possible to impart good printability to the surface of the deep drawing base paper. Furthermore, a printing layer may be provided using any ink such as dye ink or pigment ink using a commonly used printing machine. As the pigment used in the pigment coating layer, any known pigment such as calcium carbonate, kaolin, clay, talc, titanium oxide, plastic pigment, etc. can be used. The adhesive used in the pigment coating layer may be any known adhesive such as starch, casein, SBR latex, polyvinyl alcohol, or the like. These pigment coating layers can be formed as a single layer or multiple layers. The total coating weight is 20 g / m2. 2 More than 30g / m 2 It is preferable that the thickness of the coating layer is about 1 / 2 mm or less. When such a coating layer is provided, it is more preferable that the layer immediately below the pigment coating layer has a higher degree of beating and a smoother surface. Such a coating layer can be applied using various known coating devices. It is also possible to provide a printing layer on such a pigment coating layer.

[0033] <Water-resistant coating layer> The deep drawing forming base paper of this embodiment can be provided with a water-resistant coating layer on one or both sides as necessary to prevent liquid seepage or leakage. This water-resistant coating layer can be provided directly on the paper substrate, or on the pigment coating layer or print layer, and can be provided at any desired location. The water-resistant coating layer may be provided by coating a water-resistant paint.

[0034] Water-resistant paints that are applied to the surface of paper substrates and the like to impart water resistance include emulsions of waxes such as microcrystalline wax and paraffin wax, latexes such as SBR latex and polyvinylidene chloride latex, acrylic emulsions, self-emulsifying polyolefins, and various synthetic resin emulsions such as polyethylene copolymer resin emulsions. The coating equipment for these water-resistant coating materials is not particularly limited and may be any of commonly used bar coaters, air knife coaters, roll coaters, blade coaters, gate rolls, size presses, etc. In addition, the total coating amount of these coating materials is 1.0 g / m 2 More than 20.0g / m 2 The coating layer may be formed as a single layer or multiple layers.

[0035] <Thermoplastic resin layer> The deep-drawing base paper of this embodiment preferably further has a thermoplastic resin layer on at least one side of the paper substrate layer. The thermoplastic resin layer may be provided directly on the paper substrate, or on the pigment coating layer or print layer. By providing the thermoplastic resin layer, the deep-drawing molded product can be provided with water resistance and gas barrier properties against nitrogen, oxygen, water vapor, etc. Therefore, when the deep-drawing molded product is a food container, the thermoplastic resin layer is preferably provided at least on the food contact surface, and is preferably provided as the outermost layer of the food contact surface. The thermoplastic resin used in the thermoplastic resin layer is not particularly limited as long as it is a thermoplastic resin that can be laminated on the paper base layer, and may be appropriately selected from known thermoplastic resins. Examples of thermoplastic resins include polyester-based resins such as polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polylactic acid, and polybutylene succinate; polyolefin-based resins such as polyvinyl chloride, polyvinylidene chloride, polybutene, polybutadiene, ethylene-vinyl acetate copolymer, polyethylene, polypropylene, ethylene-propylene copolymer, and polymethylpentene; polycarbonate resins; polyurethane resins; polyamide resins such as nylon; polystyrene resins; polyacrylonitrile resins; poly(meth)acrylate resins, polyvinyl alcohol, and ethylene-vinyl alcohol copolymers. Among these, polyolefins such as polyethylene, polypropylene, and ethylene-propylene copolymers; polyesters such as polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polylactic acid, and polybutylene succinate, polyamide resins, and ethylene-vinyl alcohol copolymers are preferred. Among the above thermoplastic resins, polyethylene is preferred due to its excellent extrusion lamination properties and water resistance. Polyethylene (PE) is broadly classified into linear low-density polyethylene (LLDPE), low-density polyethylene (LDPE), medium-density polyethylene (MDPE), and high-density polyethylene (HDPE). Among these, low-density polyethylene (LDPE) is preferred due to its excellent extrusion lamination properties. The thermoplastic resin layer may be provided using a laminated film of a thermoplastic resin. For example, it is preferable to use a multi-layer laminated film having at least one layer of polyamide resin, ethylene-vinyl alcohol copolymer, polyvinyl alcohol, etc., which have excellent gas barrier properties against oxygen, water vapor, nitrogen, etc. When the base paper has a thermoplastic resin layer having nitrogen gas barrier properties, it is preferably used as a base paper for deep-drawing molded products filled with inert gas. When the base paper for deep-drawing processing of this embodiment has at least one thermoplastic resin layer formed from a resin having excellent gas barrier properties, a molded product having excellent gas barrier properties can be obtained. The thermoplastic resin layer having excellent gas barrier properties is preferably provided on the food contact surface side. In addition, it is preferable to have a polyolefin layer such as polypropylene or polyethylene, which has excellent water resistance and lamination properties. These resins may be used alone or in combination of two or more. The resin layer may be foamed during or after molding to form a foamed resin layer.

[0036] The method for laminating the thermoplastic resin layer may be appropriately selected from commonly used methods such as wet lamination, hot melt lamination, extrusion lamination, dry lamination, and thermal lamination.

[0037] <Characteristics of base paper for deep drawing processing> (Young's Modulus) Of the Young's modulus in the longitudinal direction and the transverse direction of the deep drawing base paper, the larger Young's modulus is A and the smaller Young's modulus is B. A is 2,600 N / mm 2 or less, and the ratio C of Young's modulus represented by the following formula (1) is 1.00 or more and 1.80 or less. C=A / B (1) The larger of the Young's modulus in the longitudinal direction and the transverse direction, Young's modulus A, is 2,600 N / mm 2 less than 2,200 N / mm 2 Less than or equal to 2,000N / mm 2 Less than or equal to 1,800N / mm2 Less than 1,500N / mm 2 The lower limit is not particularly limited, but is preferably 800 N / mm 2 More than 1,000N / mm 2 More preferably, 1,200N / mm 2 That's all. Furthermore, the Young's modulus ratio C (the ratio of A to B, C=A / B) represented by the above formula (1) is 1.00 or more and 1.80 or less, preferably 1.50 or less, more preferably 1.40 or less, even more preferably 1.30 or less, and still more preferably 1.25 or less. When the Young's modulus A is within the above range, the deep drawing base paper is easily stretched during deep drawing, so that the occurrence of cracks is suppressed. When the Young's modulus ratio C is within the above range, the difference in Young's modulus between the longitudinal direction and the transverse direction is small, so that the base paper is easily stretched both longitudinally and transversely, so that the formability is good. In addition, the shape reproducibility is excellent, and the strength of the molded product is increased, so that this is preferable.

[0038] (Elongation at break) In order to suppress the occurrence of cracks during deep drawing, the breaking elongation of the base paper for deep drawing is 3.0% or more in both the longitudinal and transverse directions, and the geometric mean of the breaking elongations in the longitudinal and transverse directions is 4.0% or more. The machine direction means the paper-making direction, and the cross direction means the direction perpendicular to the paper-making direction. The breaking elongation in the longitudinal direction and the transverse direction is preferably 3.4% or more, more preferably 5.0% or more, even more preferably 7.0% or more, still more preferably 8.0% or more, and particularly preferably 9.0% or more. There is no upper limit, but from the viewpoint of manufacturability, it is preferably 20% or less, more preferably 15% or less, and even more preferably 12% or less. The geometric mean of the longitudinal and transverse breaking elongations is preferably 4.5% or more, more preferably 5.0% or more, even more preferably 7.0% or more, and even more preferably 10.0% or more. There is no particular upper limit, but from the viewpoint of manufacturability, it is preferably 20% or less, more preferably 16% or less, and even more preferably 12% or less. The breaking elongation of the deep drawing base paper is measured in accordance with JIS P 8113:2006, and is measured on the base paper that has been left to stand for one day or more in an environment of 23±5°C and 50±10% RH and has been temperature and humidity regulated. Details are as described in the Examples.

[0039] (paper thickness) The thickness of the base paper for deep drawing molding (thickness of the base paper) is preferably 0.10 mm or more, more preferably 0.20 mm or more, even more preferably 0.30 mm or more, still more preferably 0.35 mm or more, from the viewpoints of strength as a molded product and suppression of breakage during deep drawing molding, and is preferably 0.90 mm or less, more preferably 0.70 mm or less, even more preferably 0.60 mm or less, and still more preferably 0.50 mm or less. The thickness of the deep drawing base paper is measured in accordance with JIS P 8118:2014.

[0040] (Basic weight) The basis weight of the deep drawing base paper is preferably 100 g / m from the viewpoint of strength as a molded product and suppression of breakage during deep drawing. 2 More preferably, 150 g / m 2 More preferably, 200 g / m 2 More preferably, 225 g / m 2 and preferably 500 g / m 2 Less than 450g / m 2 Less than 400 g / m 2 or less, even more preferably 385 g / m 2 The following is the result. The basis weight of the deep drawing base paper is measured in accordance with JIS P 8124:2011.

[0041] (density) The density of the deep drawing base paper is preferably 0.60 g / cm from the viewpoint of strength as a molded product and suppression of breakage during deep drawing. 3 More preferably, 0.65 g / cm 3 and preferably 1.2 g / cm 3 Less than or equal to 1.1 g / cm 3 More preferably, 1.0 g / cm 3 The following is the result. The density of the base paper is calculated from the paper thickness and basis weight.

[0042] [Deep drawing molded products] The deep-drawn product of the present embodiment is made using the above-mentioned deep-draw base paper. That is, the deep-drawn product of the present embodiment is obtained by, for example, pressing, vacuum forming, or pressure forming the above-mentioned base paper. <Manufacturing method for deep drawn products> (1) Base paper moisture adjustment Examples of the manufacturing method of the deep-drawn molded product of this embodiment include a manufacturing method called press molding, in which a deep-drawn base paper is punched into a container blank sheet, the blank sheet is sandwiched between a press mold consisting of a male mold and a female mold, and molded by heating and pressurization. Other examples include vacuum molding, in which a male mold or a female mold alone is used under heating to create a vacuum between the mold and the blank sheet, and the sheet is molded by being in close contact with the mold, and pressure molding, in which a male mold or a female mold is used under heating to sandwich a sheet between one mold and a pressure device on the other, and the sheet is molded by being in close contact with the mold by the pressure from the pressure device. In this case, it is preferable to adjust the moisture content of the deep drawing base paper in advance. The moisture content of the base paper is preferably 10% to 20%, more preferably 11% to 17%, even more preferably 12% to 15%, and most preferably 12.5% ​​to 14.5%. The moisture content of the base paper here refers to the mass % of moisture relative to the bone dry mass of the entire deep drawing base paper including the thermoplastic resin layer. When the moisture content of the base paper is in this preferred range, the base paper is plasticized to improve formability and the damage of the paper layer during forming can be reduced. As a result, a drawn product with greater depth, a smooth and beautiful appearance, and high rigidity can be obtained. Methods for adjusting the moisture content of base paper include adding moisture to the base paper immediately before press forming, and humidifying the paper after it leaves the dryer during papermaking to produce the base paper, and transporting and storing the paper in a state where the moisture is maintained.

[0043] (2) Molding method Next, a process for producing a molded product from a blank sheet will be described. In this embodiment, when deep drawing is performed by pressing, a pair of press dies is used. The pair of hot press dies is a convex die having a shape corresponding to the internal volume of the molded product, and a concave die having a shape corresponding to the external shape of the molded product. The pair of press dies can press the molded product by moving at least one die back and forth or up and down. For the sake of convenience, the following description will be given using a method (FIG. 1) in which the convex die is the upper die and the concave die is the lower die, and the upper die moves downward to perform pressing. In Fig. 1(A), a convex mold (male mold) 1 is used as the upper mold, a concave mold (female mold) 2 is used as the lower mold, a blank sheet 3 made by punching a base paper for deep drawing processing into a desired shape is sandwiched between the convex mold 1 and the concave mold 2, and the blank sheet is pressure molded (press molded) into the desired shape by moving the convex mold (male mold) 1 from above to below. At this time, as described above, it is preferable to perform pressure molding under heat. As shown in (B), a molded product is obtained by moving the convex mold (male mold) 1 upward. When deep drawing is performed by vacuum forming, the sheet is formed into a shape that matches the mold using only one of the female and male molds. Preferably, the blank sheet is molded by closely contacting the mold with the blank sheet by reducing the pressure in the gap between the blank sheet and the mold under heating, and if necessary, after cooling, air is blown in to remove the molded product. When deep drawing is performed by pressure forming, either a male or female die and a pressure device (also called a pressure box) are used to form the sheet into a shape that matches the die. A blank sheet is sandwiched between the die and the pressure device, and the sheet is pressed against the die by pressure from the pressure device, preferably under heating, and then the formed product is removed after cooling as necessary.

[0044] The blank sheet may be heated by high-frequency heating, hot air heating, infrared heating, or the like. The entire mold may also be heated. In this case, a means for heating the mold is required. As a mold heating means, an electric heating device is generally provided on the mold to heat it, but there is also a means for connecting a high-frequency oscillator to the mold and applying high-frequency waves to dry it. Electric heating and high-frequency heating may also be used in combination.

[0045] In addition, the heating temperature during molding is preferably in the range of 100°C to 150°C, more preferably 110°C to 140°C. If the heating temperature is 100°C or higher, molding is performed in a short time, improving productivity. If the heating temperature is 150°C or lower, the occurrence of blisters is suppressed, even when the moisture content of the base paper is particularly high. The deep drawing base paper can be brought to the above-mentioned specified temperature when set in the heated press machine, vacuum machine, or compressed air machine. As another method, a method is also possible in which electromagnetic waves such as microwaves are applied to the moisture-containing deep drawing base paper to raise its temperature, and then the deep drawing base paper is introduced into the press machine, vacuum machine, or compressed air machine.

[0046] Once the deep drawing process is complete, the molded product may be removed from the die and air-cooled. However, in order to improve dimensional stability, it is also preferable to fix the hot molded product in the cooling die for a certain period of time and cool it.

[0047] The material of the mold may be any known material, such as aluminum, aluminum alloys, brass, iron, stainless steel, or ceramic.

[0048] The method of operating the mold can be any of a hydraulic press, an air cylinder, and a cam mechanism. In this embodiment, the specific method of controlling the clearance between the upper and lower molds is to control the pressure by computer control or to control the position of the stopper according to the thickness of the molded product when using hydraulic or air pressure. When using a cam mechanism, it is possible to control it by a pre-designed cam shape and the lowering speed of the mold. The press time during press molding is preferably from 2 seconds to 30 seconds in terms of moldability and workability.

[0049] <Shape of molded product> The deep-drawn product of the present embodiment is a product obtained by forming one sheet of deep-draw base paper. The product is preferably obtained by drawing with a pair of press dies having a convex (male) and a concave (female) mold. The molded article is preferably a container, and typically has an open top and a flange at the top edge. The flange may also be formed by curling.

[0050] The outer shape of the container in plan view is a square, a rectangle, a circle, an ellipse, etc. In each shape, the corners are usually rounded. Figure 2 shows an example of a deep-drawn container of this embodiment as a plan view (A) and a front view (B). EXAMPLES

[0051] The features of the present invention will be described in more detail below with reference to examples and comparative examples. The materials, amounts used, ratios, processing contents, processing procedures, etc. shown in the following examples can be appropriately changed without departing from the spirit of the present invention. Therefore, the scope of the present invention should not be interpreted as being limited by the specific examples shown below.

[0052] [Evaluation and Analysis] The raw pulp and deep drawing base paper of the examples and comparative examples were evaluated and analyzed as follows.

[0053] [Raw pulp] <Measurement of Canadian Standard Freeness (CSF)> The Canadian Standard Freeness (CSF) of the raw pulp was measured in accordance with JIS P 8121-2:2012.

[0054] [Base paper for deep drawing processing] <Thickness (paper thickness)> The thickness of the deep drawing base paper was measured in accordance with JIS P 8118:2014. When a resin layer was present, the thickness of each of the paper base layer and the thermoplastic resin layer was measured from an observation image of the cross section of the deep drawing base paper under an electron microscope (SEM).

[0055] <Basic weight> The basis weight of the deep drawing base paper was measured in accordance with JIS P 8124:2011.

[0056] <density> The density of the deep drawing base paper was calculated from the thickness and basis weight obtained by the above-mentioned measuring method.

[0057] <Measurement of length-weighted average fiber length, percentage of fine fibers, and curl value> The deep drawing base papers of the Examples and Comparative Examples were cut into 40 cm squares, which were then soaked in ion-exchanged water adjusted to a concentration of 2%, and left to soak for 24 hours. After soaking for 24 hours, the pulp was disintegrated into fibers using a standard disintegrator (Kumagaya Riki Kogyo Co., Ltd.) until no undisintegrated fibers remained. When the pulp had a resin layer, the slurry (dispersion of pulp fibers) after disintegration was removed from the resin layer and the length-weighted average fiber length (ISO), fine fiber content (Fines A), and curl value were measured using a fiber length measuring instrument (Model FS-5 with UHD base unit, Valmet). The "length-weighted average fiber length (ISO)" is the length-weighted average fiber length calculated by selecting fibers that are 0.2 mm or more and 7.6 mm or less. In addition, the "fine fiber content (Fine A)" is the percentage of fine fibers with a fiber width of 75 μm or less and a length of 0.2 mm or less among the defibrated pulp fibers.

[0058] <Elongation at break> In accordance with JIS P 8113:2006 (Testing methods for tensile properties of paper and paperboard), the base paper was left to stand for at least one day in an environment of 23±5°C and 50±10% humidity, and the temperature and humidity were conditioned. The base paper was then cut into samples 15 mm wide and 150 mm long to prepare samples. The sample was attached to a tensile testing machine (model RTC-1210A, manufactured by A&D Co., Ltd.) with a chuck distance of 100 mm, and a tensile test was performed at a speed of 20 mm / min to measure the breaking elongation in both the T (longitudinal direction) and Y (transverse direction).

[0059] <Young's modulus> Tensile tests were carried out in the same manner as for the breaking elongation, except that the speed was changed to 240 mm / min, in both the T (machine direction) and Y (transverse direction) directions. The slope of the elongation of the obtained chart from 0 to 1% was calculated to obtain Young's modulus.

[0060] <Formability: Suppression of crack generation> The deep drawing base paper of the examples and comparative examples was cut out to obtain blank sheets. The blank sheets were pressed at a pressure of 35 kgf / cm using a molding die and a press molding machine (FVT400, manufactured by Wakisaka Engineering Co., Ltd.). 2 The mixture was pressed at a temperature of 150°C for a press time of 5 seconds into a tray shape as shown in Figure 2. 200 molded pieces were produced and evaluated as follows. The evaluation criteria are as follows: (Evaluation Criteria) A: Of the molded paper trays, the percentage of paper trays without cracks is 98% or more. B: The percentage of molded paper trays without cracks is 95% or more and less than 98%. C: The percentage of the molded paper trays that have no cracks is 90% or more but less than 95%. D: The percentage of the molded paper trays without cracks is less than 90%.

[0061] <Moldability: Shape reproducibility> The molded paper tray was placed on a desk and the center of one of the four long sides was pressed with a finger until it touched the desk, and the following evaluation was performed. The evaluation criteria are as follows: A: Press your finger against the ground and it will stop within two shakes. B: Press your finger against the ground and it will come to a stop after shaking 3 to 5 times. C: Press your finger against the ground and shake it six or more times before it comes to a stop. When the shape reproducibility of the molding die is high, a flat bottom surface is formed, but when the shape reproducibility is poor, the bottom surface is not flat and has a bulge. As a result, when the shape reproducibility is high, the mold stops with little shaking, but when the shape reproducibility is poor, the mold stops with many shakings.

[0062] [Pulp preparation] <Preparation of Pulp 1> Pulp 1 was prepared by using NUKP (unbleached softwood kraft pulp) made by pulping (cooking) wood and beating it at a low concentration (slurry concentration at time of beating: 2% by mass) until the CSF (Canadian Standard Freeness) became 650 mL.

[0063] <Preparation of Pulp 2> Pulp 2 was prepared by using NBKP (bleached softwood kraft pulp) made by pulping (cooking) and bleaching wood. In the first stage of beating, the pulp concentration was set to 30 mass%, and in the second stage, low concentration beating (slurry concentration at beating: 2 mass%) was used until the CSF (Canadian Standard Freeness) was 600 mL. In addition, the proportion of fine fibers in bleached kraft pulp tends to decrease due to repeated dehydration treatments during the bleaching process. Furthermore, when high concentration beating is performed, the curl value tends to increase.

[0064] <Preparation of Pulp 3> Pulp 3 (CSF 650 mL) was prepared in the same manner as pulp 1, except that the first stage of beating was changed to high-consistency beating (pulp concentration at beating: 30% by mass) and the second stage of beating was changed to low-consistency beating.

[0065] <Preparation of Pulp 4> Pulp 4 (CSF 550 mL) was prepared in the same manner as Pulp 1, except that in the preparation of Pulp 1, 30 parts by mass of NBKP (softwood bleached kraft pulp) and 70 parts by mass of LBKP (hardwood bleached kraft pulp) were used as the raw material pulp. Furthermore, softwood pulp tends to have longer fiber length than hardwood pulp.

[0066] [Examples and Comparative Examples] <Production of paper base material (Examples 1 to 5)> The pulp shown in Table 1 was used, and 0.2 parts by mass of a synthetic sizing agent (SPS400, manufactured by Arakawa Chemical Industries Co., Ltd.), 1.0 parts by mass of aluminum sulfate, 0.5 parts by mass of a polyacrylamide resin (DS4433, manufactured by Seiko PMC Corporation) as a retention agent, and 0.025 parts by mass of nonionic polyacrylamide (Percol 47, manufactured by Allied Colloids Co., Ltd.) as a polymer flocculant (retention agent) were added to 100 parts by mass of pulp in terms of solid content to prepare a paper stock. The above paper stock was used to make paper at a papermaking speed of 600 m / min on a wet papermaking machine (Bellform III type, manufactured by Mitsubishi Heavy Industries Co., Ltd.) equipped with an expansion device (manufactured by Clupac), to obtain a paper base material with a crepe applied to the surface of the paper. The basis weight of the single sheet of paper used in each example was 68 g / m 2 , and Example 2 is 69 g / m 2 , and Example 3 is 67 g / m 2 , and Example 4 is 63 g / m 2 , and Example 5 is 73 g / m 2 It was.

[0067] <Production of Polysand Paper (Examples 1 to 5)> One side of the paper base material (single paper) obtained as described above was melt-extrusion coated with LDPE (LC-522, manufactured by Japan Polyethylene Corporation) to a thickness of 20 μm, and the same paper base material (single paper) was laminated to the coated surface. One side of the paper base material was similarly melt-extrusion coated with LDPE to a thickness of 20 μm, and the same paper base material (single paper) was laminated to the coated surface, resulting in a polysand paper with three paper base layers (paper base material / LDPE / paper base material / LDPE / paper base material).

[0068] <Production of Paper Base Material (Example 6, Comparative Examples 1 to 3)> The pulp shown in Table 1 was used, and 0.2 parts by mass of a synthetic sizing agent (SPS400, manufactured by Arakawa Chemical Industries Co., Ltd.), 1.0 parts by mass of aluminum sulfate, 0.02 parts by mass of a cationic retention agent (ND-300, manufactured by Hymo Co., Ltd.) as a retention agent, and 0.025 parts by mass of a nonionic polyacrylamide (Percoll 47, manufactured by Allied Colloids Co., Ltd.) as a polymer flocculant were added to 100 parts by mass of pulp in terms of solid content to prepare a paper stock. Using the above paper stock, paper was made at a papermaking speed of 600 m / min on a wet papermaking machine (Bellform III type, manufactured by Mitsubishi Heavy Industries Co., Ltd.) to obtain a paper base material. In Example 6, paper was made at a J / W ratio of 1, and in Comparative Examples 1 to 3, paper was made at a J / W ratio of 1.1. The basis weight of the single sheet is 278 g / m 2 , Comparative Example 1 is 338 g / m 2 , Comparative Example 2 is 303 g / m 2 , Comparative Example 3 is 297 g / m 2 It was.

[0069] [Examples 1, 2, 4, 5, 6, Comparative Examples 2 and 3] The coating amount after heat drying on paper substrate is 10g / m 2 A coating liquid prepared by mixing 100 parts by mass of an aqueous acrylic adhesive (EA-G34, manufactured by Toyo-Morton Co., Ltd.) with 3 parts by mass of a curing agent (CAT-EP8, manufactured by Toyo-Morton Co., Ltd.) was applied using a reverse roll coater so that the coating liquid would be as follows: Next, a thermoplastic resin film was wet laminated onto the surface coated with the adhesive. The thermoplastic resin films L1 and L2 were as follows: L1 and L2 were laminated so that the PA was on the paper substrate side. L1: CEL-4264D (Sumitomo Bakelite Co., Ltd., laminated film of PE (polyethylene) / PA (polyamide) / EVOH (ethylene-vinyl alcohol copolymer) / PA (polyamide)), thickness = 60 μm L2: Diamiron MFC673 (manufactured by Mitsubishi Chemical Corporation, laminated film of PP (polypropylene) / EVOH (ethylene-vinyl alcohol copolymer) / PA (polyamide)), thickness = 60 μm In Examples 1, 2, 5, and 6 and Comparative Examples 2 and 3, a thermoplastic resin layer was also provided on the side opposite to the side on which L1 or L2 was provided. Specifically, the coating amount after thermal drying was 10 g / m on the side opposite to the side on which L1 or L2 was provided. 2 A coating liquid prepared by mixing 100 parts by mass of an aqueous acrylic adhesive (EA-G34, manufactured by Toyo-Morton Co., Ltd.) with 3 parts by mass of a curing agent (CAT-EP8, manufactured by Toyo-Morton Co., Ltd.) was applied using a reverse roll coater so that the coating liquid would be as follows: Next, a thermoplastic resin film was wet laminated onto the surface coated with the adhesive.

[0070] [Example 3, Comparative Example 1] In Example 3, the obtained polysand paper was used as it is as a base paper for deep drawing processing. In Comparative Example 1, the obtained paper base material was used as it is as base paper for deep drawing processing.

[0071] The obtained deep drawing base paper was subjected to the above-mentioned evaluations. The results are shown in the table below.

[0072] [Table 1]

[0073] From the results of the Examples and Comparative Examples, it is clear that the deep drawing base paper of the present invention suppresses the occurrence of cracks during deep drawing, has excellent shape reproducibility, and is excellent in deep drawing processability. [Industrial Applicability]

[0074] The deep drawing base paper of the present invention is suitable for use in deep drawing products because it suppresses the occurrence of cracks during deep drawing and has excellent shape reproducibility.

Claims

1. It is a base paper for deep drawing processing, The base paper has a paper base layer made of a paper base material, The length-weighted average fiber length of the pulp constituting the paper base material is 0.60 mm or more and 2.40 mm or less, Of the Young's modulus in the longitudinal direction and the transverse direction of the base paper, the larger Young's modulus is A and the smaller Young's modulus is B. A is 2,600 N / mm 2 and The Young's modulus ratio C represented by the following formula (1) is 1.00 or more and 1.80 or less, C = A / B (1) The base paper has a longitudinal and transverse breaking elongation of 3.0% or more, and a geometric mean of the longitudinal and transverse breaking elongations of 4.0% or more. Base paper for deep drawing processing.

2. The deep drawing base paper according to claim 1, wherein the Young's modulus ratio C is 1.00 or more and 1.50 or less.

3. The deep drawing base paper according to claim 1 or 2, wherein the curl value of the pulp constituting the paper base material is 5% or more and 12% or less.

4. The base paper has a basis weight of 100 g / m 2 More than 500g / m 2 The paper thickness is 0.10 mm or more and 0.90 mm or less, and the density is 0.60 g / cm 3 1.2g / cm or more 3 The deep drawing forming base paper according to any one of claims 1 to 3, wherein

5. The deep drawing base paper according to any one of claims 1 to 4, further comprising a thermoplastic resin layer on at least one surface of the base paper.

6. A deep drawing molded product obtained using the deep drawing molding base paper according to any one of claims 1 to 5.

Citation Information

Patent Citations

  • Molding paper suitable for vacuum molding or pressure molding

    JP2003293300A

  • Support base for image recording material, method for manufacturing the same, and image recording material

    JP2004226951A

  • Support for image recording material and image-recording material

    JP2006070381A

  • Base paper for molded vessel

    JP2014167192A

  • 3d moldable sheet material

    JP2018534393A