Gravure inks, printed matter and laminates
The gravure ink formulation with a polyester-based urethane resin and isocyanate compound addresses the issues of printability, stability, and laminate strength, enhancing tearability in packaging bags.
Patent Information
- Application Number
- JP2021128162
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-08-04
- Publication Date
- 2024-10-02
- Estimated Expiration
- 2041-08-04
AI Technical Summary
Existing gravure inks face challenges in achieving good printability, ink stability, lamination strength, and tearability, particularly in packaging bags, where low adhesion can lead to peeling and poor tearability, causing design issues and content leakage.
A gravure ink formulation using a polyester-based urethane resin with a specific molecular weight distribution (Mw/Mn of 5 to 10) and a curing agent, such as an isocyanate compound, to enhance adhesion and tearability, combined with optional resins like cellulose and rosin, to improve laminate properties.
The solution provides gravure inks with excellent printability, stability, and balanced lamination strength and tearability, ensuring the integrity of packaging bags during handling and use.
Smart Images

Figure 0007559704000001 
Figure 0007559704000002 
Figure 0007559704000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a gravure ink, and more particularly to a gravure ink that is suitable for use in forming a laminate exhibiting excellent performance in terms of laminate strength and tear resistance. [Background technology]
[0002] Generally, packaging bags are sometimes provided with patterns such as pictures, and are provided with a printed layer made of ink to make the contents invisible. Examples of such inks include offset ink, flexographic ink, silk screen ink, gravure ink, and other printing inks. Among them, gravure ink has good productivity due to its printing speed and the ability to create high-definition patterns, and is often used in gravure printing.
[0003] The printed layer made of gravure ink is laminated by bonding (laminating) an adhesive layer and a thermoplastic substrate, in that order, onto the printed layer. The laminate is then heat-sealed to form a packaging bag, with the thermoplastic substrates of the outermost layers being heat-sealed together. Such packaging bags are often used in the food packaging field. If the adhesion between the layers of such packaging bags is low, peeling between the layers occurs during filling or transportation of the contents, resulting in problems such as a loss of design and leakage of the contents, and therefore laminated laminates in the food packaging field are required to have good adhesion strength.
[0004] In addition, in the case of food packaging bags, for example liquid sub-bags, the packaging bag is often torn open directly by hand to remove the contents. In this case, being able to tear and open the packaging bag without using tools such as scissors is a great advantage in terms of convenience, and therefore increases market value. However, if the packaging bag has poor tearability, particularly if the content of the packaging bag is liquid, problems arise such as excessive force being required to open the bag or the bag being torn in an unexpected direction, causing the contents to spill out, and therefore laminated products in the food packaging field are required to have good tearability (Patent Document 1).
[0005] As a conventional technique, for example, Patent Document 1 describes a technique in which a curing agent is used in an ink containing a polyurethane resin to increase the laminate strength and thereby exhibit easy tearing properties. However, it may still be difficult to increase the laminate strength simply by using a curing agent. On the other hand, Patent Document 2 describes a technique in which a silane coupling agent is used in addition to a curing agent. However, there is a concern that the use of a silane coupling agent in combination may deteriorate the stability of the ink over time and cause changes in the laminate strength. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2017-031298 A [Patent Document 2] JP 2019-199509 A Summary of the Invention [Problem to be solved by the invention]
[0007] An object of the present invention is to provide a gravure ink that has excellent printability and ink stability in addition to excellent lamination properties and tearability. [Means for solving the problem]
[0008] As a result of extensive investigations, the inventors have found that the above problems can be solved by using the gravure ink of the present invention, and have thus completed the present invention.
[0009] That is, the present invention provides a gravure ink containing a polyester-based urethane resin for use in forming a printed layer of a laminate having a printed layer, the gravure ink comprising: The polyester-based urethane resin has a molecular weight distribution (Mw / Mn) of more than 5 and not more than 10.
[0010] The present invention also relates to the above gravure ink, which further comprises a curing agent.
[0011] The present invention also relates to the above gravure ink, wherein the curing agent contains an isocyanate compound having a molecular weight distribution (Mw / Mn) of 1.5-5.
[0012] The present invention also relates to the above gravure ink, wherein the isocyanate compound has a weight average molecular weight of 800-8,000.
[0013] The present invention also relates to the above gravure ink, wherein the polyester-based urethane resin has a structure derived from at least one of sebacic acid, succinic acid and azelaic acid.
[0014] The present invention also relates to the above gravure ink, which further contains at least one resin selected from the group consisting of cellulose-based resins, vinyl chloride-based resins and rosin-based resins.
[0015] The present invention also relates to a printed matter having a printed layer formed on a substrate 1 from the above gravure ink.
[0016] The present invention also relates to a laminate having an adhesive layer and a substrate 2 in this order on the printed layer of the printed matter. Effect of the Invention
[0017] The present invention makes it possible to provide a gravure ink that has excellent printability and ink stability in addition to laminate properties and easy tearing properties. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] The following describes in detail the embodiments of the present invention. However, the description of the components described below is one example (representative example) of an embodiment of the present invention, and the present invention is not limited to these contents as long as it does not go beyond the gist of the present invention.
[0019] In the present invention, "gravure ink" may be abbreviated to "ink". In addition, an ink consisting of a mixture of "gravure ink" and "curing agent" is also called "gravure ink", but hereinafter may be abbreviated to "curable gravure ink" or "curable ink". A printing layer formed by printing "gravure ink" or "curable gravure ink" may be simply referred to as "printing layer" or "ink layer", but these terms are synonymous. Furthermore, "〇~△" means "〇 or more and △ or less".
[0020] The present invention will be described in detail below. The present invention provides a gravure ink containing a polyester-based urethane resin for use in forming a printed layer of a laminate having a printed layer, comprising: The molecular weight distribution (Mw / Mn) of the polyester-based urethane resin is more than 5 and not more than 10. This gravure ink is used to form a printing layer positioned as an intermediate layer of a laminate. By using a polyester-based urethane resin with a molecular weight distribution (Mw / Mn) of more than 5 and not more than 10, adhesion to substrates and the like is improved. Furthermore, by crosslinking and curing with a curing agent having a molecular weight distribution (Mw / Mn) of 1.5 to 5, for example, the printed layer containing the polyester-based urethane resin becomes strong, imparting durability to the entire laminate and making it easy to tear.
[0021] (Gravure ink containing polyester-based urethane resin) The gravure ink contains a polyester-based urethane resin as a binder resin. The gravure ink contains preferably 2 to 40% by mass, more preferably 3 to 30% by mass of the binder resin in 100% by mass of the gravure ink. The gravure ink is used by mixing with a curing agent described later.
[0022] (Polyester-based urethane resin) The polyester-based urethane resin used in the present invention refers to a urethane resin having a polyester-derived structural unit in the urethane resin. The polyester-based urethane resin preferably contains 40 mass% or more of polyester-derived structural units in the total mass of the polyester-based urethane resin, more preferably 50 mass% or more, even more preferably 60 mass% or more, and particularly preferably 65 mass% or more. The polyester-based urethane resin is not limited to the following, but examples thereof include a polyester-based urethane resin obtained by reacting a polyisocyanate with a polyol including a polyester polyol to obtain a urethane prepolymer having an isocyanate group at the end, and then reacting the urethane prepolymer with a polyamine (chain extender) and, if necessary, a reaction terminator. The urethane resin may be any resin having a urethane bond, and even if it has a urea bond in addition to the urethane bond, it falls under the concept of the urethane resin. To obtain a polyester-derived structural unit, for example, a polyester polyol is used as the polyol as described above.
[0023] (Polyisocyanate) The polyisocyanate preferably contains a diisocyanate, such as an aliphatic diisocyanate, such as tetramethylene diisocyanate, isopropylene diisocyanate, methylene diisocyanate, 2,2,4-trimethylhexamethylene diisocyanate, or 2,4,4-trimethylhexamethylene diisocyanate; Alicyclic diisocyanates such as cyclohexane-1,4-diisocyanate, hydrogenated xylylene diisocyanate, isophorone diisocyanate, lysine diisocyanate, dicyclohexylmethane-4,4'-diisocyanate, 1,3-bis(isocyanatomethyl)cyclohexane, methylcyclohexane diisocyanate, m-tetramethylxylylene diisocyanate, and dimer diisocyanate in which the carboxyl groups of dimer acid are converted to isocyanate groups; Examples of the diisocyanate include α,α,α',α'-tetramethylxylylene diisocyanate, 1,5-naphthylene diisocyanate, 4,4'-diphenylmethane diisocyanate, 4,4'-diphenyldimethylmethane diisocyanate, 4,4'-dibenzyl isocyanate, dimethyldiphenylmethane diisocyanate, tetramethyldiphenylmethane diisocyanate, 1,3-phenylene diisocyanate, 1,4-phenylene diisocyanate, m-xylylene diisocyanate, p-xylylene diisocyanate, o-xylylene diisocyanate, and aromatic diisocyanates such as 2,4-tolylene diisocyanate and 2,6-tolylene diisocyanate. Among these, from the viewpoints of easy reaction control and good balance of the performance of the resulting urethane resin, alicyclic or araliphatic diisocyanates are preferred, and isophorone diisocyanate and α,α,α',α'-tetramethylxylylene diisocyanate are particularly preferred. At least one diisocyanate may be used, and two or more diisocyanates may be used in combination.
[0024] (Polyol) As the polyol, polyester polyol is often used, but polyether polyol, polycarbonate polyol, polyolefin polyol, etc. can also be used. However, when introducing a polyester-derived structural unit into the urethane resin, the method of introducing the polyester structure is not particularly limited.
[0025] (Polyester polyol) The number average molecular weight of the polyester polyol is preferably 500 to 10,000. The number average molecular weight used for the polyol here is calculated from the hydroxyl value, which is a value calculated by esterifying or acetylating the hydroxyl groups in the resin, back titrating the remaining acid with an alkali, converting the amount of hydroxyl groups in 1 g of the resin into mg of potassium hydroxide according to JIS K0070. When the number average molecular weight of the polyol is 10,000 or less, the blocking resistance to plastic films is excellent. Also, when the number average molecular weight of the polyol is 500 or more, the flexibility of the urethane resin coating is excellent and the adhesion to plastic films is excellent. For the above reasons, the number average molecular weight is more preferably 1,000 to 5,000.
[0026] The polyester polyol is preferably a polyester diol. The diol is a compound having two hydroxyl groups in one molecule. Even when other polyols are used in combination, the diol is preferably used, and examples of the polyols include polyether diol, polycarbonate, and polybutadiene glycol. At least one diol may be used, and two or more diols may be used in combination.
[0027] The polyester diol is preferably a polyester diol which is a condensation product of a diol and a dicarboxylic acid. Suitable examples of the polyester diol include ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, 1,3-propanediol, 1,4-butanediol, 1,3-butanediol, 1,6-hexanediol, 1,8-octanediol, 1,9-nonanediol, neopentyl glycol, 3-methyl-1,5-pentanediol, 2-methyl-1,3-propanediol, 3,3,5-trimethylpentanediol, 2,4-diethyl-1,5-pentanediol, 1,12-octadecanediol, 1,2-alkanediol, 1,3-alkanediol, 1-monoglyceride, 2-monoglyceride, 1-monoglycerin ether, 2-monoglycerin ether, dimer diol, and hydrogenated dimer diol. The polyester polyol can be used alone or in combination of two or more kinds. The polyester diol is preferably a condensation product of a diol containing a branched diol and a dicarboxylic acid. Alternatively, the polyester diol may be a polyester diol obtained by a ring-opening reaction of a cyclic ester (such as a lactone). Suitable examples of the dicarboxylic acid include adipic acid, phthalic anhydride, isophthalic acid, terephthalic acid, maleic acid, fumaric acid, succinic acid, oxalic acid, malonic acid, pimelic acid, azelaic acid, sebacic acid, suberic acid, glutaric acid, 1,4-cyclohexyldicarboxylic acid, dimer acid, and hydrogenated dimer acid. Of these, adipic acid, succinic acid, sebacic acid, azelaic acid, and the like are preferred. Furthermore, a polyol having three or more hydroxyl groups and a polycarboxylic acid having three or more carboxyl groups can be used in combination as raw materials for the polyester polyol.
[0028] Among these, preferred specific examples include those containing structural units derived from polyesters composed of adipic acid, succinic acid, sebacic acid or other dibasic acids and diols having a branched structure, because this can improve adhesion to plastic substrates and the solubility of the ink composition. The diol having a branched structure is preferably a diol having a structure in which at least one hydrogen atom of an alkylene glycol is substituted with an alkyl group. Suitable examples of the diol having a branched structure include 1,2-propanediol, 1,3-butanediol, 2-methyl-1,3-propanediol, neopentyldiol, 1,4-pentanediol, 3-methyl-1,5-pentanediol, 2,5-hexanediol, 2-methyl-1,4-pentanediol, 2,4-diethyl-1,5-pentanediol, 2-butyl-2-ethyl-1,3-propanediol, 2-methyl-1,8-octanediol, 2,2,4-trimethyl-1,3-pentanediol, and 2,2,4-trimethyl-1,6-hexanediol. Among these, at least one selected from 1,2-propanediol, 3-methyl-1,5-pentanediol, neopentyl glycol, and 2-butyl-2-ethyl-1,3-propanediol is preferred, and the use of polyester polyols containing 1,2-propanediol and / or 3-methyl-1,5-pentanediol is even more preferred.
[0029] (Polyamine) The chain extender is preferably a polyamine. Suitable examples of the polyamine include, but are not limited to, ethylenediamine, propylenediamine, hexamethylenediamine, isophoronediamine, dicyclohexylmethane-4,4'-diamine, and dimer diamine in which the carboxyl group of dimer acid is converted to an amino group. These can be used alone or in combination of two or more. A reaction terminator may be used to suppress excessive reaction due to chain extension. Amino acids can also be used for chain extension. The term "amino acid" refers to a compound having both an amino group and an acidic functional group in one molecule, and preferred examples include glutamine, asparagine, lysine, diaminopropionic acid, ornithine, diaminobenzoic acid, and diaminobenzenesulfonic acid. In addition, since there is a high probability that the acidic group will not react with the isocyanate group during the synthesis process of the urethane resin, the acid value can be maintained in the urethane resin.
[0030] In the case of a urethane resin that can be produced only by the urethanization step, it is preferable to use a monoalcohol or a monoamine as the reaction terminator, and in the case of a urethane resin that is produced by carrying out a urethanization reaction step in addition to the urethanization step, it is preferable to use a monoamine. The monoalcohol is preferably a substituted or unsubstituted alcohol, and suitable examples thereof include methanol, ethanol, n-propanol, isopropyl alcohol, 1-butanol, etc. The monoamine is preferably a substituted or unsubstituted monoamine, and suitable examples thereof include n-butylamine, n-dibutylamine, octylamine, diethylamine, monoethanolamine, monopropanolamine, diethanolamine, dipropanolamine, etc. In addition, the compounds listed as the chain extenders can also be used as the reaction terminator, and at least one of them may be used, or two or more of them may be used in combination.
[0031] In producing a urethane prepolymer having an isocyanate group at its terminal, obtained by reacting a polyisocyanate with a polyol, the molar equivalent ratio of NCO of the polyisocyanate to OH of the polyol (molar equivalent of NCO of the polyisocyanate / molar equivalent of OH of the polyol compound) is preferably 1.3 to 3, and more preferably 1.5 to 2.
[0032] The polyester-based urethane resin preferably has an active hydrogen group such as a hydroxyl value and / or an amine value. This is to obtain a reaction site with the curing agent described below. The hydroxyl value is preferably 0.5 to 30 mgKOH / g, more preferably 1 to 20 mgKOH / g, and even more preferably 2 to 15 mgKOH / g. When the polyester-based urethane resin has an amine value, it is preferably 0.1 to 15 mgKOH / g, and even more preferably 1 to 12 mgKOH / g. On the other hand, the acid value of the polyester-based urethane resin is preferably 5 mgKOH / g or less, and even more preferably 3 mgKOH / g or less. This is because the acid value is poorly reactive with the curing agent described below.
[0033] The weight average molecular weight of the polyester-based urethane resin is preferably 20,000 to 100,000, more preferably 25,000 to 90,000, and even more preferably 30,000 to 80,000, in order to make the printed layer into a strong film by crosslinking with the curing agent described below, thereby achieving good laminate strength. The weight average molecular weight and the molecular weight distribution (Mw / Mn) described later can be measured by gel permeation chromatography (GPC). For example, Water2690 (manufactured by Waters) or HLC-8220 (manufactured by Tosoh Corporation) can be used as the GPC device, and PLgel, 5 μm, MIXED-D (manufactured by Polymer Laboratories) or TSKgel Super AW series (manufactured by Tosoh Corporation) can be used as the column. Tetrahydrofuran, 1,2,4-trichlorobenzene, N,N-dimethylformamide (with 0.01N lithium bromide added), etc. can be used as the developing solvent, and the flow rate is preferably 0.5 to 1.5 milliliters / minute. An RI detector or the like can be used for detection, and the measurement can be performed under conditions such as a sample injection concentration of 0.5 to 1.5 milligrams / milliliter and an injection amount of 0.1 to 1.0 microliter. The weight average molecular weight can be determined as a polystyrene equivalent value.
[0034] The molecular weight distribution (Mw / Mn) of the polyester urethane resin is more than 5 and not more than 10, preferably more than 5 and not more than 9, and more preferably 5.2 to 8.5. Mw represents the weight average molecular weight, and Mn represents the number average molecular weight. When Mw / Mn is within the above range, it is considered that the cohesive force and adhesive force are strengthened by crosslinking with the curing agent described below, and the resin shows sufficient resistance in boiling and retorting, and also exhibits easy tearing properties. Note that Mw, Mn, and Mw / Mn can be determined by gel permeation chromatography (GPC) as described above.
[0035] In order to set the molecular weight distribution (Mw / Mn) of polyester-based urethane resin within the above range, the selection of urethane synthesis raw materials, the solid content mass ratio, the dripping speed of reactive raw materials such as polyisocyanate in the synthesis reaction, the stirring speed and the shape of the stirring blade, and the reaction temperature can be appropriately set in the urethane resin synthesis to set the molecular weight distribution within the range. In addition, when a chain extension reaction is performed, it is effective to set the dripping speed and temperature range control to a certain range when reacting polyamine with urethane prepolymer. Reaction temperature control is important, and it is preferable to control it between 50 and 130 ° C in the synthesis of urethane prepolymer, and it is preferable to control it to a range of 10 to 50 ° C when reacting polyamine with urethane prepolymer. In addition, setting the charging ratio of the reaction raw materials to an appropriate ratio is also effective in keeping the molecular weight distribution within a predetermined range. Examples of the charging ratio include the NCO / OH ratio, which is the ratio of the hydroxyl groups of the polyol and hydroxy acid, and the isocyanate groups of the polyisocyanate, and the amino group / NCO ratio, which is the ratio of the amino group of the polyamine and the isocyanate group of the urethane prepolymer. In order to control the molecular weight distribution, it is preferable to use a polymerization terminator (also called a reaction terminator) to prevent excessive polymerization reaction. Suitable examples of the polymerization terminator include monoalcohols and monoamines. In addition, the molecular weight distribution of the polyester polyol also has an effect. By selecting a polyester polyol with a molecular weight distribution of about 2 to 10, it is easy to control the molecular weight distribution (Mw / Mn) of the polyester urethane resin within the above range. The amount of polyols having a relatively small molecular weight, for example, a weight average molecular weight of 800 or less, used is preferably 30 mass % or less, more preferably 20 mass % or less, and even more preferably 10 mass % or less, of the total mass of the polyester-based urethane resin.
[0036] <Concomitant Resin> The gravure ink used in the present invention may suitably contain a co-resin together with the urethane resin. Preferred embodiments of the co-resin are shown below. Examples of the resin include polyolefin resins such as polyethylene resins and chlorinated polypropylene resins, poly(meth)acrylic resins, vinyl chloride copolymer resins, polyvinyl acetate resins, vinyl chloride-vinyl acetate copolymers, polystyrene resins, styrene-butadiene copolymer resins, styrene-maleic acid copolymers, vinylidene fluoride resins, polyvinyl alcohol resins, polyvinyl acetal resins, polyvinyl butyral resins, polybutadiene resins, polyester resins, polyamide resins, alkyd resins, epoxy resins, polyester resins, thermosetting poly(meth)acrylic resins, melamine resins, urea resins, polyurethane resins, phenolic resins, xylene resins, maleic acid resins, cellulose resins such as nitrocellulose, ethyl cellulose, acetylbutyl cellulose, and ethyloxyethyl cellulose, rubber resins such as chlorinated rubber and cyclized rubber, petroleum resins, and natural resins such as rosin and casein. Among them, at least one resin selected from vinyl chloride copolymer resin, cellulose resin, poly(meth)acrylic resin, styrene-maleic acid copolymer and rosin resin is preferable, and vinyl chloride copolymer resin is more preferable.
[0037] The vinyl chloride copolymer resin is preferably a vinyl chloride-vinyl acetate copolymer resin, a vinyl chloride-acrylic copolymer resin, or the like. The weight-average molecular weight of the vinyl chloride copolymer resin is preferably 5,000 to 100,000, and more preferably 5,000 to 50,000. The content of the constituent unit derived from the vinyl acetate monomer in 100% by mass of the solid content of the vinyl chloride copolymer resin is preferably 70 to 95% by mass. The glass transition temperature is preferably 50°C to 90°C. The vinyl chloride copolymer resin preferably has a hydroxyl group, and the hydroxyl value is preferably 10 to 200 mgKOH / g. This is because the reactivity with the curing agent is improved, and the hydroxyl group is preferably derived from a hydroxyl group derived from a vinyl alcohol unit or an acrylic monomer having a hydroxyl group.
[0038] The mass ratio (urethane resin:co-used resin) of the urethane resin to at least one resin (co-used resin) selected from the group consisting of cellulose-based resins, vinyl chloride-based resins, and rosin-based resins is preferably 95:5 to 30:70, and more preferably 90:10 to 40:60, because this leads to good adhesion to the substrate, coating properties, laminate strength, etc.
[0039] (Coloring agent) The gravure ink used in the present invention may contain a colorant. The colorant preferably contains a pigment, and preferably contains 0.2 to 38% by mass in 100% by mass of the gravure ink. Any of organic pigments, inorganic pigments, and extender pigments can be used as the pigment, but inorganic pigments containing titanium oxide are preferred, and extender pigments such as silica, barium sulfate, kaolin, clay, calcium carbonate, and magnesium carbonate are preferred. Organic pigments made of organic compounds and organometallic complexes are preferred. The pigment may be either organic or inorganic, and examples of the inorganic pigment include yellow lead, titanium yellow, red iron oxide, cadmium red, ultramarine, and cobalt blue, while examples of the organic pigment include soluble azo, insoluble azo, azo, phthalocyanine, halogenated phthalocyanine, anthraquinone, anthanthrone, dianthraquinonyl, anthrapyrimidine, perylene, perinone, quinacridone, thioindigo, dioxazine, isoindolinone, quinophthalone, azomethine azo, flavanthrone, diketopyrrolopyrrole, isoindoline, indanthrone, and carbon black. Any pigment designated by the CI pigment number in the Color Index may be used.
[0040] (Titanium dioxide) The gravure ink used in the present invention is also preferably one containing titanium oxide. For example, when printing is performed for reverse printing of a laminated laminate, a white gravure ink is finally applied to the entire surface to promote crosslinking and hardening of the entire layer including other printed layers. In the present invention, the titanium oxide pigment may be one having a crystal structure of any of anatase type, rutile type, and brookite type. Among them, rutile type titanium oxide is preferred because it has good crosslinking and hardening properties. In the industrial production of titanium oxide, rutile ore or ilmenite ore (FeTiO3) is used as a raw material. There are two main production methods: the chlorine method and the sulfuric acid method, and either method may be used. In addition, in order to improve the crosslinking and hardening of the printed layer, it is preferable that the titanium oxide pigment is surface-treated, and in particular, that the titanium oxide pigment is surface-treated with at least one metal selected from the group consisting of Si, Al, Zn, Zr and oxides thereof.
[0041] The oil absorption as measured by the method specified in JIS K5101 is preferably 14 to 35 ml / 100 g, and more preferably 17 to 32 ml / 100 g. The average particle size (median particle size) as measured by a transmission electron microscope is preferably 0.2 to 0.3 μm. The total content of the titanium oxide pigment is preferably 10 to 60% by weight, and more preferably 10 to 45% by weight, based on 100% by weight of the ink. Multiple types of titanium oxide pigments may be used in combination.
[0042] (medium) The gravure ink used in the present invention may contain an organic solvent, water, or other medium. The medium is not limited, but suitable organic solvents include toluene and other aromatic organic solvents, methyl ethyl ketone and other ketone-based organic solvents, ethyl acetate, normal propyl acetate, and other ester-based organic solvents, ethanol, isopropanol, normal propanol, and other alcohol-based organic solvents. Water may be contained, and when an organic solvent is the main medium, it is preferable that the water content is 10 mass% or less.
[0043] (Additives) The gravure ink used in the present invention may further contain any additives as necessary, such as a filler, a stabilizer, a plasticizer, an antioxidant, a light stabilizer such as an ultraviolet absorber, a dispersant, a thickener, a drying agent, a lubricant, an antistatic agent, and a crosslinking agent.
[0044] <Hardening agent> In the present invention, the curing agent is mixed with the gravure ink and used as a curable gravure ink for printing. The curing agent may be an isocyanate-based compound, a carbodiimide-based compound, an epoxy-based compound, or the like, but is preferably one containing an isocyanate-based compound. When the polyester-based urethane resin has a hydroxyl group, an amino group, or other active hydrogen group, the curing agent crosslinks with the active hydrogen group, and when the polyester-based urethane resin does not have the active hydrogen group, the curing agent crosslinks with the isocyanate-based compound alone, thereby improving the laminate strength, tearability, etc. In the gravure ink used in combination with the curing agent, it is preferable that the polyester-based urethane resin has a hydroxyl group, an amino group, or other active hydrogen group.
[0045] Preferred embodiments of the isocyanate compound are shown below. The weight average molecular weight of the isocyanate compound is preferably 800 to 8000, more preferably 900 to 6000, and even more preferably 1000 to 4000. The molecular weight distribution (Mw / Mn) of the isocyanate compound is preferably 1.5 to 5, more preferably 2 to 4.5, and even more preferably 2 to 4. When the content is within the above range, it is believed that the cohesive strength and adhesive strength are strengthened by the action with the polyester-based urethane resin, resulting in good laminate strength and easy tearability.
[0046] The isocyanate compound is preferably a polyisocyanate including an adduct type polyisocyanate (adduct body), a biuret type polyisocyanate (biuret body), an isocyanurate type polyisocyanate (isocyanurate body), a bifunctional polyisocyanate, etc., and examples of the adduct body, biuret body and isocyanurate body include an adduct body obtained by reacting trimethylolpropane or other polyol with a diisocyanate, a biuret body in which a diisocyanate is dimerized and linked by a biuret bond, and an isocyanurate body obtained by a cyclic trimerization reaction of a diisocyanate. The diisocyanate may be selected from the above diisocyanates and preferably includes tolylene diisocyanate (TDI), diphenylmethane diisocyanate (MDI), hydrogenated diphenylmethane diisocyanate (hydrogenated MDI), hexamethylene diisocyanate (HDI), isophorone diisocyanate, xylylene diisocyanate (XDI), hydrogenated xylylene diisocyanate (hydrogenated XDI), etc. Adduct type polyisocyanate, biuret type polyisocyanate, and isocyanurate type polyisocyanate may be used in combination, and may also be used in combination with other polyisocyanates.
[0047] In order to set the weight average molecular weight and molecular weight distribution (Mw / Mn) of the isocyanate compound within the above range, it is possible to set the selection of diisocyanate, polyol, etc., the solid content mass ratio, the dripping speed of reactive raw materials such as polyisocyanate in the synthesis reaction, the stirring speed, the shape of the stirring blade, and the reaction temperature appropriately in the synthesis reaction. Note that it is effective to set the dripping speed and temperature range in a certain range when reacting polyamine and polyisocyanate in order to set the molecular weight distribution within the specified range. In addition, it is effective to set the molecular weight distribution within a predetermined range by setting the charging ratio of the reaction raw materials to an appropriate ratio. Examples of the charging ratio include the NCO / OH ratio, which is the ratio of the isocyanate group of the polyol and the polyisocyanate, and the amino group / NCO ratio, which is the ratio of the amino group of the polyamine and the isocyanate group of the polyisocyanate. Reaction temperature control is important, and in synthesis using polyol and polyisocyanate, it is preferable to control it between 50 and 130°C, and in reacting polyamine and polyisocyanate, it is preferable to control it in the range of 10 to 50°C. In addition, the solid content is also important, and it is preferable to set the solid content during the reaction to 40 to 80 mass%. The reaction solvent is also important, and it is preferable to use ethyl acetate, normal propyl acetate, or other ester-based organic solvents.
[0048] In the present invention, the mass ratio of the urethane resin (including polyester-based urethane resin) contained in the gravure ink to the isocyanate compound contained in the curing agent, i.e., urethane resin:isocyanate compound, is preferably 99:1 to 60:40, more preferably 98:2 to 65:35, and even more preferably 95:5 to 70:30. When a combined resin described below is contained in addition to the urethane resin, the mass ratio of the total amount of the urethane resin and the combined resin (total mass of the binder resin) to the isocyanate compound is preferably 99:1 to 60:40, more preferably 98:2 to 65:35, and even more preferably 95:5 to 70:30. This is because it is believed that within this range, the effects of crosslinking and substrate adhesion become good, and good laminate properties and easy tearability are exhibited.
[0049] (Curable gravure ink) The gravure ink of the present invention can be made into a curable gravure ink by mixing a curing agent. The curable gravure ink is preferably prepared by mixing 0.3 to 10% by mass of the curing agent with respect to 100% by mass of the gravure ink. The blending amount of the curing agent is more preferably 0.5 to 7% by mass, and even more preferably 0.8 to 5% by mass or 1 to 4% by mass with respect to 100% by mass of the gravure ink. The viscosity can be adjusted to an appropriate level for printing using an organic solvent, and the organic solvents mentioned above are preferably used as the organic solvent.
[0050] (Printed layer formed by printing "curable gravure ink") The printing layer refers to a printing layer formed from a curable gravure ink, and is formed by gravure printing. After printing, the printing layer is gradually crosslinked and cured by the curing agent. It is preferable to leave the layer still for about 1 to 24 hours after printing. The thickness of the printing layer is preferably 0.5 to 10 μm, and more preferably 0.8 to 8 μm.
[0051] <Gravure printing> (Photogravure version) A gravure plate is a cylindrical metal plate, and recesses for each color are created by engraving, etching, or laser. There are no restrictions on the use of engraving and laser, and they can be set arbitrarily to match the pattern. Lines per page are appropriately set at 100 to 300 lines, and the higher the line count, the finer the printing. The thickness of the printing layer is preferably 0.1 μm to 100 μm. (gravure printing machine) In a gravure printing press, one printing unit is equipped with the gravure plate and doctor blade. There are many printing units, and printing units corresponding to organic solvent-based printing inks and picture inks can be set, and each unit has an oven drying unit. Printing is performed by rotary printing, and a roll-to-roll printing method is used. The type of plate and the type of doctor blade are selected appropriately according to the specifications.
[0052] <Laminate> The laminate of the present invention comprises the above-mentioned printed layer as an intermediate layer of the laminate. A laminate having a configuration in which at least a substrate 1, a printed layer, and a substrate 2 (sealant) are laminated in this order is preferred. Substrate 1 and substrate 2 may be the same or different, but substrate 2 is preferably an unstretched polyolefin substrate (sealant) having heat sealability (see below). Specific examples of the layered configuration of the laminate include the following. In the following configuration indications (1) to (4), " / " indicates the boundary between each layer. (1) Substrate 1 / printed layer / adhesive layer / sealant (2) Substrate 1 / printed layer / adhesive layer / intermediate substrate layer / adhesive layer / sealant (3) Substrate 1 / printed layer / ink layer / adhesive layer / sealant (4) Substrate 1 / printed layer / ink layer / adhesive layer / intermediate substrate layer / adhesive layer / sealant The layer structure can be arbitrarily selected so that the printed layer can be seen from the substrate side.
[0053] <Base material 1> The substrate 1 is preferably a plastic film, which serves as the substrate on the outer layer side of the laminate, and is made of a light-transmitting material so that the printed layer can be visually recognized from the outside. Specifically, examples of the resin include polyolefin resins such as polyethylene (PE) and polypropylene (PP), cyclic polyolefin resins, polystyrene resins, acrylonitrile-styrene copolymer (AS) resins, acrylonitrile-butadiene-styrene copolymer (ABS) resins, poly(meth)acrylic resins, polycarbonate resins, polyvinyl alcohol resins, ethylene-vinyl alcohol copolymer (EVOH), saponified ethylene-vinyl ester copolymers, polyester resins such as polyethylene terephthalate (PET), polybutylene terephthalate (PBT), and polyethylene naphthalate (PEN), polyamide resins such as various nylons (Ny), polyurethane resins, acetal resins, cellulose resins, and polyvinylidene chloride resins (PVDC). The substrate 1 may be uniaxially or biaxially stretched. It may also be a composite film in which two or more of the above resin films are laminated. It may also be in a form in which a metal oxide such as silica or alumina is vapor-deposited.
[0054] From the viewpoint of boiling and retort treatment, the substrate 1 is preferably one having excellent heat resistance. As a resin constituting the substrate having excellent heat resistance, a polyester resin and / or a polyamide resin is suitable. Specific examples of the substrate 1 having excellent heat resistance include a polyester film alone, a polyamide film alone such as nylon, and a composite film containing at least one of a polyester film and a polyamide film. Examples of the composite film include a co-extruded stretched film having a structure of PET / Ny / PET, and PET / Ny from the outer layer side. In addition, it is also preferable to combine at least one of a polyester film and a polyamide film with at least one of an ethylene-vinyl alcohol copolymer film and a polyvinylidene chloride film as the composite film.
[0055] The thickness of the substrate 1 is not particularly limited and can be appropriately set depending on the application of the laminate, but is usually preferably about 5 to 50 μm, more preferably 10 to 30 μm.
[0056] The substrate 1 preferably has a total light transmittance according to JIS K7361-1:1997 of 85% or more, and more preferably 90% or more. The substrate also preferably has a haze according to JIS K7136:2000 of 1.5% or less, more preferably 1.0% or less, and even more preferably 0.5% or less.
[0057] (Gas barrier layer) The gas barrier layer can be provided anywhere between the substrate and the sealant, as necessary. The gas barrier layer plays a role in blocking the transmission of oxygen, water vapor, and the like between the packaged item in the laminate and the external environment of the laminate. The gas barrier layer may also be provided with a light-shielding property that blocks the transmission of visible light, ultraviolet rays, and the like. The gas barrier layer may be composed of only one layer, or may be composed of two or more layers.
[0058] Suitable examples of the gas barrier layer (vapor deposition film) include inorganic substances such as silicon (Si), aluminum (Al), magnesium (Mg), calcium (Ca), potassium (K), tin (Sn), sodium (Na), boron (B), titanium (Ti), lead (Pb), zirconium (Zr), yttrium (Y), etc., or vapor deposition films formed from oxides of these substances. Among these, inorganic oxides such as silicon oxide, aluminum oxide, magnesium oxide, etc. are preferred when the laminate is for use in a microwave oven. Examples of methods for forming a vapor-deposited film include physical vapor deposition (PVD) methods such as vacuum deposition, sputtering, and ion plating, and chemical vapor deposition (CVD) methods such as plasma chemical vapor deposition, thermal chemical vapor deposition, and photochemical vapor deposition.
[0059] The thickness of the vapor-deposited film varies depending on the material used, the required gas barrier performance, etc., but is usually preferably about 5 to 200 nm, more preferably 5 to 150 nm, and even more preferably 10 to 100 nm. In the case of inorganic oxides such as silicon oxide and aluminum oxide, the thickness is preferably about 5 to 100 nm, more preferably 5 to 50 nm, and even more preferably 10 to 30 nm.
[0060] <Intermediate base material layer> The laminate of the present invention may have an intermediate substrate layer between the printing layer and the sealant. The intermediate substrate layer is a layer that is provided as necessary for the purpose of improving the strength and processing suitability of the laminate. Examples of the constituent material of the intermediate substrate layer include a plastic film-like substrate. The substrate can be the same as the substrate described above. In consideration of heating in a microwave oven or retort processing, in order to increase the heat resistance of the laminate, it is preferable that the intermediate substrate layer has excellent heat resistance. A polyester substrate, a polyamide substrate, or the like is preferably used.
[0061] <Adhesive layer> In the laminate, the constituent layers are laminated via an adhesive layer from the viewpoint of improving the bonding strength between the layers. The adhesive layer can be formed by a method using a known adhesive for dry lamination. Examples of adhesives for dry lamination include polyvinyl acetate adhesives, polyacrylic ester adhesives, cyanoacrylate adhesives, ethylene copolymer adhesives, cellulose adhesives, polyester adhesives, polyamide adhesives, polyimide adhesives, amino resin adhesives such as urea resin and melamine resin, phenol resin adhesives, epoxy adhesives, polyurethane adhesives (for example, cured products of polyol and isocyanate compounds), reactive (meth)acrylic acid adhesives, rubber adhesives such as chloroprene rubber, nitrile rubber, styrene-butadiene rubber, silicone adhesives, and inorganic adhesives such as alkali metal silicates and low-melting point glasses. The adhesive is applied to a print layer, a sealant, or an intermediate substrate layer, and then laminated to each layer, substrate, or sealant. The thickness of the applied film is preferably 0.5 to 5 μm, and more preferably 1 to 4 μm.
[0062] <Base material 2 (sealant)> The inner layer of the sealant is in direct contact with the packaged product and plays a role in protecting the packaged product. In order to make the laminate into a bag, it is preferable that the innermost layer of the sealant has heat sealability. Examples of materials constituting the sealant include polyolefin resins such as low density polyethylene (LDPE), linear low density polyethylene (LLDPE), medium density polyethylene (MDPE), high density polyethylene (HDPE), ethylene-vinyl acetate copolymer, propylene homopolymer, and ethylene-propylene copolymer, and one or more of these resins can be used. The sealant may be composed of a single layer or two or more layers. In order to suppress shrinkage during heat sealing, the sealant is preferably a non-stretched film made of the above-mentioned resin.
[0063] From the viewpoint of heating during boiling or retort treatment, in order to enhance heat resistance, it is preferable that the sealant is made of a resin having excellent heat resistance, and specifically, propylene-based resins such as polypropylene and ethylene-propylene copolymers, and HDPE are preferred.
[0064] The thickness of the sealant is not particularly limited and is appropriately set depending on the application of the laminate and the type and properties of the packaged goods, but is usually preferably 10 to 200 μm. In the case of a pouch (particularly a retort pouch), the thickness of the sealant is preferably 20 to 150 μm, more preferably 30 to 100 μm.
[0065] (Method of manufacturing laminate) The laminate of the present invention is a method for producing a laminate having at least a substrate, a printed layer, an adhesive layer, and a sealant in this order, and includes a step of forming the printed layer by gravure printing a curable ink, which is a mixture of a pigment, a gravure ink containing a polyester-based urethane resin, and a curing agent containing an isocyanate compound, on the substrate. The adhesive layer may be formed by coating on the printed layer, or may be formed by coating on the sealant. A preferred embodiment is, for example, a mode in which an adhesive is applied onto the printed layer, and then a sealant is laminated. When the laminate further has an intermediate substrate layer, a preferred embodiment includes a step of first laminating the printed layer and the intermediate substrate layer with an adhesive, and then laminating the intermediate substrate layer and the sealant. The configuration is arbitrary and is not particularly limited. The laminate thus obtained is cut to a predetermined size, and the edges are heat-sealed with the sealants joined together to form a bag. The heat-sealing temperature is preferably 50 to 250°C, more preferably 80 to 180°C. The heat-sealing pressure is 1 to 5 kg / cm. 2 The conditions are as follows. One laminate may be folded and the edges may be heat sealed, or two or more laminates may be heat sealed. Also, a bag made of a laminate may be one in which all openings are heat sealed after the contents are packed. EXAMPLES
[0066] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. In the present invention, parts, % and ratios represent parts by mass, % by mass and mass ratios unless otherwise noted. It should be noted that Examples 1 and 2 are reference examples.
[0067] (Hydroxyl value) Calculated in accordance with JIS K0070. (Acid value) Calculated in accordance with JIS K0070. (amine value) The amine value was calculated by the following method in accordance with JIS K0070, in terms of the equivalent amount of hydrochloric acid and the equivalent amount of potassium hydroxide required to neutralize the amino groups contained in 1 g of resin. 0.5 to 2 g of sample was precisely weighed out (sample solid content: Sg). 50 mL of a mixed solution of methanol / methyl ethyl ketone = 60 / 40 (mass ratio) was added to the precisely weighed sample to dissolve it. Bromophenol blue was added to the resulting solution as an indicator, and the resulting solution was titrated with 0.2 mol / L ethanolic hydrochloric acid solution (titer: f). The point at which the color of the solution changed from green to yellow was set as the endpoint, and the titration amount (A mL) at this point was used to calculate the amine value according to the following (Equation 2). (Equation 2) Amine value = (A x f x 0.2 x 56.108) / S [mg KOH / g]
[0068] (Weight average molecular weight Mw, number average molecular weight Mn and molecular weight distribution Mw / Mn) The weight average molecular weight Mw, number average molecular weight Mn and molecular weight distribution Mw / Mn were determined by measuring the molecular weight distribution using a GPC (gel permeation chromatography) device (HLC-8220 manufactured by Tosoh Corporation) and calculating the molecular weight converted using polystyrene as a standard substance. The measurement conditions are shown below. Columns: The following columns were used in series connection: Tosoh Corporation TSKgel Super AW2500 Tosoh Corporation TSKgel Super AW3000 Tosoh Corporation TSKgel Super AW4000 Tosoh Corporation's TSK gelguard column Super AWH Detector: RI (differential refractometer) Measurement conditions: Column temperature 40℃ Eluent: Tetrahydrofuran Flow rate: 1.0mL / min
[0069] [Synthesis Example 1] (Synthesis of polyester-based urethane resin PU1) In a nitrogen gas atmosphere, in a reaction vessel equipped with an agitator, 100 parts of a polyester polyol (NPG:1,3-PD=60:40, sebacic acid:adipic acid=50:50) having a number average molecular weight of 2000, which is a condensation product of neopentyl glycol (hereinafter "NPG"), 1,3-propanediol (hereinafter "1,3-PD"), sebacic acid, and adipic acid, 1.0 part of 1,4-butanediol (hereinafter "1,4-BD"), 28.5 parts of isophorone diisocyanate (hereinafter "IPDI"), and 32.1 parts of ethyl acetate were reacted under a nitrogen gas flow at 80°C and a stirring speed of 150 rpm for 5 hours to obtain a solvent solution of a terminal isocyanate urethane prepolymer. Next, in another reactor with stirring blades, 11 parts of isophoronediamine (hereinafter "IPDA"), 1.0 part of N-(2-aminoethyl)ethanolamine (hereinafter "AEA"), 1.0 part of dibutylamine (hereinafter "DBA"), and 300.4 parts of a mixed solvent of ethyl acetate / isopropanol (hereinafter "IPA") = 60 / 40 were rapidly stirred at a stirring speed of 180 rpm and kept at 40 ° C., and the obtained terminal isocyanate prepolymer solution was added dropwise at 40 ° C. over 60 minutes, and then reacted at 80 ° C. for 1 hour. After the reaction was completed, the solid content was adjusted to 30 mass % with the ethyl acetate / IPA mixed solvent to obtain a polyester-based urethane resin PU1 solution.
[0070] [Synthesis Examples 2 to 5] (Synthesis of polyester-based urethane resins PU2 to PU5) Polyester-based urethane resins PU2 to PU5 were synthesized in the same manner as in Synthesis Example 1, except that the raw materials and blending ratios shown in Table 1 were used. Table 1 shows the Mw / Mn, hydroxyl value, amine value, and weight average molecular weight. The abbreviations in the table stand for the following. NPG, 1,3-PD / Sebacic acid, succinic acid: Neopentyl glycol (hereinafter "NPG"), 1,3-propanediol (hereinafter "1,3-PD"), sebacic acid, polyester polyol (NPG:1,3-PD=60:40, sebacic acid:succinic acid=50:50), which is a condensation product of sebacic acid and succinic acid. MPD / Sebacic acid: A polyester polyol that is a condensation product of 3-methyl-1,5-pentanediol (hereinafter, "MPD") and sebacic acid (hereinafter, "SA") PEG: Polyethylene glycol with a number average molecular weight of 1000 PPG: Polypropylene glycol with a number average molecular weight of 2000
[0071] [Comparative Synthesis Examples 1, 2 and 3] (Synthesis of urethane resins P1, P2 and P3) Urethane resin P1 was synthesized in the same manner as in Synthesis Example 1, except that the raw materials and blending ratios shown in Table 1 were used.
[0072] [Synthesis Example 6] (Synthesis of Curing Agent 1) In a nitrogen gas atmosphere, 15 parts of trimethylolpropane, 60.3 parts of toluene-2,4-diisocyanate, and 32.3 parts of ethyl acetate that had been previously dehydrated were reacted in a reaction vessel equipped with an agitator at 50°C and a stirring speed of 150 rpm for 3 hours to obtain a curing agent 1 with a solid content of 70% by mass. (Hardening agent 1 (adduct type)) Weight average molecular weight: 1200 Mw / Mn: 2.5
[0073] [Synthesis Example 7] (Synthesis of Curing Agent 2) Under a nitrogen gas atmosphere, 15 parts of trimethylolpropane, 29.8 parts of toluene-2,4-diisocyanate, and 99.3 parts of ethyl acetate that had been dehydrated in advance were reacted in a reaction vessel equipped with an agitator at 50°C and a stirring speed of 150 rpm for 3 hours to obtain a curing agent 2 with a solid content of 70% by mass. (Hardening agent 2 (adduct type)) Weight average molecular weight: 2500 Mw / Mn: 3.3
[0074] [Synthesis Example 8] (Synthesis of Curing Agent 3) Under a nitrogen gas atmosphere, 15 parts of ditrimethylolpropane, 39.7 parts of toluene-2,4-diisocyanate, and 23.4 parts of ethyl acetate were reacted in a reaction vessel equipped with a stirring blade at 80° C. and a stirring speed of 150 rpm for 3 hours to obtain a curing agent 3 having a solid content of 70 mass %. (Hardening agent 3 (adduct type)) Weight average molecular weight: 3500 Mw / Mn: 4.2
[0075] In the examples described below, in addition to the above curing agents, the following curing agents were also used. TLA-100: Asahi Kasei Corporation, isocyanurate type isocyanate curing agent Weight average molecular weight: 1300 Mw / Mn: 2.4 Solid content 70% by mass 24A-100: Asahi Kasei Corporation Biuret type isocyanate curing agent Weight average molecular weight: 1600 Mw / Mn: 3.2 Solid content 70% by mass E402-80B: Asahi Kasei Corporation Isocyanate-based hardener Weight average molecular weight: 4100 Mw / Mn: 3.4 Solid content 70% by mass
[0076] [Example 1] (Preparation of laminate S1) <Preparation of Gravure Ink S1> The polyester-based urethane resin PU1 obtained in Synthesis Example 1 was used to prepare the following gravure ink S1. Polyester urethane resin 40 parts by weight Vinyl chloride copolymer resin solution 10 parts by weight (Vinyl chloride-vinyl acetate copolymer resin, Solvine TA5R, manufactured by Nissin Chemical Co., Ltd., 30% solids in ethyl acetate solution) Phthalocyanine pigment 10 parts by weight (CI Pigment Blue 15:4) Organic solvent 40 parts by weight (Mixed solvent of normal propyl acetate / isopropanol = 70 / 30)
[0077] <Print> 100 parts by mass of the gravure ink S1 obtained above was diluted with a mixed solvent (methyl ethyl ketone "MEK":N-propyl acetate "NPAC":isopropanol "IPA" = 30:40:30) to a viscosity of 16 seconds (25°C, Zahn cup No. 3) to obtain a curable gravure ink S1. The ink was then printed on a corona discharge treated surface of a biaxially oriented NY (polyamide) substrate (N1102, manufactured by Toyobo Co., Ltd., film thickness 15 μm) at a printing speed of 100 m / min using a Helio 175 line solid plate (pressed type, 100% solid pattern) to obtain a printed matter S1.
[0078] <Extrusion lamination (EL method, imine)> A methanol solution of an imine-based anchor coat agent (Toyo-Morton EL420) was applied to the above printed matter at a solid content of 0.03 g / m 2 The film was coated, and then molten polyethylene (Japan Polyethylene Corporation, LC600A) was melted at 320°C using an extrusion laminator (Musashino Kikai Co., Ltd.) at a line speed of 100 m / min to laminate at a thickness of 18 μm. The film was then bonded to CPP (Futamura Chemical Co., Ltd., FCMN#20) to obtain a laminate.
[0079] <Extrusion lamination (EL method, isocyanate)> A methanol solution of an isocyanate-based anchor coating agent (Toyo Morton EL530) was applied to the above printed matter at a solid content of 0.3 g / m 2 The laminate was coated with molten polyethylene (Japan Polyethylene Corporation, LC600A) at 320°C and laminated at a thickness of 18 μm using an extrusion laminator (Musashino Kikai Co., Ltd.) at a line speed of 100 m / min. The laminate was then bonded to LLDPE (Mitsui Chemicals Tohcello Co., Ltd., TUX-FCD#40) to obtain a laminate.
[0080] [Examples 2 to 22] (Preparation of Laminates S2 to 22) The curable inks, printed matter and laminates S2 to 22 of Examples 2 to 22 were obtained in the same manner as in Example 1, except that the raw materials and compounding ratios shown in Table 2 were used and a curing agent was added and mixed by stirring. The abbreviations in the table are as follows: DLX5-8: ICI Novel Enterprises Nitrocellulose Weight average molecular weight 50,000 Nitrogen content 12.0% Glass transition temperature 150°C (Solid content 30% isopropanol solution) Hariestar P: Made by Harima Chemicals Co., Ltd. Rosin modified pentaerythritol ester, 30% solids in ethyl acetate solution BR-105: Mitsubishi Chemical Corporation acrylic resin, weight average molecular weight 60,000, glass transition point 50°C, acid value 3.5mgKOH / g, ethyl acetate solution with 30% solids 7018: Arakawa Chemical Co., Ltd. polyester resin, 30% solids solution Titanium oxide: Ishihara Sangyo Kaisha, Ltd. CR-90 Titanium oxide coated with silica and alumina, with an average particle size (median particle size) of 0.25 μm as measured by a transmission electron microscope.
[0081] [Comparative Examples 1 to 6] (Preparation of Laminates H1 to H6) Laminates H1 to H6 of Comparative Examples 1 to 6 were obtained in the same manner as in Example 1, except that the raw materials and the urethane resin and the ink were used in the blending ratios shown in Table 3.
[0082] (Measurement and Evaluation) The laminates of the examples and comparative examples were subjected to the following measurements and evaluations. The results are shown in Tables 2 and 3.
[0083] <Ink stability> The inks obtained in the above Examples and Comparative Examples were filled into glass bottles (100 g), sealed, and left to stand at 40°C for 7 days, and the presence or absence of separation or precipitation and the degree of change (increase) in the ink viscosity were evaluated. [Evaluation Criteria] A: No separation or precipitation, and no change in viscosity. (Good) B: Separation or precipitation of less than 5 mm or an increase in ink viscosity of less than 10% is observed (fairly good). C: Separation or precipitation of less than 1 cm or an increase in ink viscosity of less than 30% is observed (usable). D: Separation or hard sediment of less than 3 cm or increase in ink viscosity of less than 50% is observed (slightly poor). E: Defects such as separation of a transparent liquid phase of 3 cm or more, irreversible precipitation, or an increase in ink viscosity of 50% or more are observed. (Failure) The practical ratings are A, B and C.
[0084] <Printability> The printing inks of the examples and comparative examples were evaluated for plate fogging. The dilution solvent was NC201 solvent: ethyl acetate: IPA = 80:20, the viscosity was 16 seconds (25°C) using Zahn cup #3, and the area of plate fogging was visually determined after 90 minutes of idling on the printing press. Judgment criteria A (Excellent): The plate cover area is between 0% and 5%. B (Good): The plate cover area is 5% or more but less than 10%. C (Acceptable): The plate cover area is 10% or more but less than 15%. D (Not acceptable): The plate cover area is 15% or more but less than 30%. E (Poor): Plate cover area is 30% or more The practical ratings are A, B and C.
[0085] <Lamination strength> After the laminates obtained in the above examples and comparative examples were left at 40°C for 48 hours, the printed portions were cut to a width of 15 mm and the ink surface was peeled off from the substrate surface, after which the peel strength (lamination strength) was measured using an Intesco 201 universal tensile tester. [Evaluation Criteria] A: 1.6N or more (good) B: 1.2N or more but less than 1.6N (slightly good) C: 0.8N or more but less than 1.2N (practical) D: 0.4N or more but less than 0.8N (slightly poor) E: Less than 0.4N (defective) The practical ratings are A, B and C.
[0086] <Easy tearability> For the laminates obtained in the above Examples and Comparative Examples, samples were prepared in accordance with JIS K7128-1:1998, and evaluated for tear resistance using an Intesco 201 universal tensile tester. [Evaluation Criteria] A: Less than 0.5N (good) B: 0.5N or more but less than 1.0N (slightly good) C: 1.0N or more but less than 1.5N (practical) D: 1.5N or more but less than 2.0N (slightly poor) E: 2.0N or more (defective) The practical ratings are A, B and C.
[0087] [Table 1]
[0088] [Table 2]
[0089] [Table 3]
Claims
1. A gravure ink for use in forming a printed layer of a laminate having a printed layer, the gravure ink comprising a polyester-based urethane resin as a binder resin, The molecular weight distribution (Mw / Mn) of the polyester-based urethane resin is more than 5 and not more than 10, The gravure ink contains a curing agent, the curing agent contains an isocyanate compound having a molecular weight distribution (Mw / Mn) of 1.5 to 5; the polyester-based urethane resin contains structural units derived from a polyester composed of a dibasic acid including sebacic acid and a diol, The weight average molecular weight of the polyester-based urethane resin is 20,000 to 100,000; The gravure ink contains the polyester-based urethane resin in an amount of 2 to 40% by mass based on 100% by mass of the gravure ink.
2. A gravure ink as described in claim 1, wherein the mass ratio of the total mass of the binder resin to the isocyanate compound is 99:1 to 60:
40.
3. The gravure ink according to claim 1 or 2, wherein the weight average molecular weight of the isocyanate compound is 800 to 8,000.
4. The gravure ink according to any one of claims 1 to 3, wherein the polyester-based urethane resin further has a structure derived from succinic acid and / or azelaic acid.
5. The gravure ink according to any one of claims 1 to 4, further comprising at least one resin selected from the group consisting of cellulose-based resins, vinyl chloride-based resins and rosin-based resins.
6. A printed matter having a printed layer formed on a substrate 1 from the gravure ink according to any one of claims 1 to 5.
7. A laminate comprising the printed layer of the printed matter according to claim 6, and further comprising an adhesive layer and a substrate (2) in that order on the printed layer.
Citation Information
Patent Citations
Printing ink composition for laminate and easily tearable laminate
JP2017031298A
Solvent type gravure ink for laminate, printed matter, and laminate
JP2018076461A
Gravure ink for easy-tearing laminate, and easy-tearing laminate
JP2019199509A
Gravure or flexographic ink
JP2020002185A
Organic solvent-based printing ink, printed material, and laminate
JP2020090627A