Nonaqueous dispersion, method for producing laminate, and molded product
The combination of a tetrafluoroethylene polymer and inorganic filler in a non-aqueous dispersion with specific properties addresses stability and aggregation issues, enabling molded articles with enhanced physical properties and uniform distribution.
Patent Information
- Application Number
- JP2021556073
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-04-24
- Filing Date
- 2020-11-06
- Publication Date
- 2024-10-02
- Estimated Expiration
- 2040-11-06
AI Technical Summary
Existing non-aqueous dispersions face challenges in maintaining dispersion stability and expressing high physical properties when the content of inorganic fillers and polymers is increased, leading to sedimentation, aggregation, and reduced rigidity in molded products.
A non-aqueous dispersion containing a tetrafluoroethylene polymer with specific particle size and melt viscosity, combined with an inorganic filler of predetermined particle size and shape, along with a liquid dispersion medium, ensures high content of both components while maintaining excellent dispersion stability and blendability.
The solution allows for the formation of molded articles with high physical properties, including electrical properties, heat resistance, and low linear expansion, while ensuring uniform distribution and stability of the components.
Smart Images

Figure 0007559767000001 
Figure 0007559767000002 
Figure 0007559767000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a non-aqueous dispersion containing a specified tetrafluoroethylene-based polymer and an inorganic filler, a method for producing a laminate having a polymer layer formed from the non-aqueous dispersion, and a molded product having specified microvoids. [Background technology]
[0002] Tetrafluoroethylene-based polymers such as polytetrafluoroethylene (PTFE), copolymers of tetrafluoroethylene and perfluoro(alkyl vinyl ether) (PFA), and copolymers of tetrafluoroethylene and hexafluoropropylene (FEP) have excellent physical properties such as mold releasability, electrical properties, water and oil repellency, chemical resistance, weather resistance, and heat resistance, and are used for various industrial applications. A non-aqueous dispersion containing PTFE powder is known as a coating agent used to impart these physical properties to the surface of a substrate. Patent Document 1 further describes a method for improving the dispersion stability by adding Al 2 O 3 , SiO 2 , CaCO 3 , ZrO 2 , SiC, Si 3 N 4 and ZnO.
[0003] Patent Documents 2 and 3 disclose a non-aqueous dispersion (thermosetting composition) containing an uncured epoxy resin as a main component, and containing PTFE powder and a silica filler as filling components. These patent documents describe the physical properties (viscosity, dispersibility, etc.) of non-aqueous dispersions based on the epoxy resin before curing as the main component, and the physical properties (linear expansion, adhesion, electrical properties, etc.) of polymer layers formed therefrom. However, these patent documents do not describe at all aspects in which various polymers are used in place of the epoxy resin. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2016-194017 A [Patent Document 2] JP 2017-165876 A [Patent Document 3] JP 2016-166347 A Summary of the Invention [Problem to be solved by the invention]
[0005] If the content of the inorganic filler contained in the non-aqueous dispersion is increased, it is expected that the physical properties based on the inorganic filler will be highly expressed in the molded product formed therefrom. However, as described in paragraph 0019 of Patent Document 1, if the content of the inorganic filler in the non-aqueous dispersion is increased, the dispersion stability is reduced, making it difficult to obtain a molded product with sufficient properties. The present inventors have found that such a tendency becomes more pronounced when the respective contents of PTFE and inorganic filler in the non-aqueous dispersion are increased, and becomes even more pronounced when other components (such as the various components described in paragraph 0019 of Patent Document 1) are blended in. Therefore, there has been a problem that a molded product having high physical properties based on the tetrafluoroethylene polymer (electrical properties, heat resistance, etc.) and physical properties based on the inorganic filler (low linear expansion, electrical properties, etc.) cannot be formed from such a non-aqueous dispersion.
[0006] In addition, it was thought that by using various polymers instead of the epoxy resin in the non-aqueous dispersions containing epoxy resins described in Patent Documents 2 and 3, the formed polymer layer could be imparted with properties based on the added polymer and silica in addition to the properties based on the tetrafluoroethylene polymer. In order to favorably express the properties based on each component in the polymer layer, it is preferable to increase the contents of each of the three components in the non-aqueous dispersion as much as possible. However, the inventors have discovered that in this case, the viscosity of the non-aqueous dispersion is likely to increase and sediment or aggregates are likely to form, and not only are the physical properties of the formed polymer layer not fully expressed, but the rigidity is significantly reduced.
[0007] The present inventors have found that by using a powder of a specific tetrafluoroethylene-based polymer and an inorganic filler of a specific particle size, even if the content of both is high, a non-aqueous dispersion excellent in dispersion stability and blendability with other polymers such as aromatic polymers can be obtained, and that a molded product having high physical properties of the tetrafluoroethylene-based polymer and the inorganic filler can be obtained from such a non-aqueous dispersion. Furthermore, the present inventors have also found that when the non-aqueous dispersion contains other polymers, the molded product also has high physical properties of the other polymers. An object of the present invention is to provide such a non-aqueous dispersion and to provide a dense molded product having excellent physical properties (electrical characteristics, low linear expansion, heat resistance, etc.). [Means for solving the problem]
[0008] [1] Melt viscosity at 380℃ is 1×10 6 A non-aqueous dispersion comprising a powder of a tetrafluoroethylene-based polymer having a viscosity of not more than Pa s, an inorganic filler having an average particle size of more than 0.10 μm, and a liquid dispersion medium, wherein the content of the polymer and the content of the inorganic filler each exceed 5 mass%. [2] The nonaqueous dispersion of [1], wherein the tetrafluoroethylene-based polymer is a polymer containing units based on tetrafluoroethylene and units based on perfluoro(alkyl vinyl ether). [3] The nonaqueous dispersion of [1] or [2], wherein the powder has an average particle size of 6 μm or less and is substantially free of particles having a particle size of 10 μm or more. [4] The nonaqueous dispersion according to any one of [1] to [3], wherein the inorganic filler is an inorganic filler containing silicon oxide or magnesium metasilicate. [5] The nonaqueous dispersion of any of [1] to [4], wherein the inorganic filler is a nearly spherical inorganic filler having an average particle size of more than 0.10 μm and less than 10 μm and substantially free of particles having a particle size of 25 μm or more, or a scaly inorganic filler having an average major axis of 1 μm or more and an aspect ratio of 5 or more. [6] The nonaqueous dispersion liquid according to any one of [1] to [5], wherein the liquid dispersion medium is at least one liquid dispersion medium selected from the group consisting of amides, ketones, and esters. [7] The nonaqueous dispersion according to any one of [1] to [6], wherein the content of the inorganic filler is equal to or less than the content of the tetrafluoroethylene-based polymer. [8] Melt viscosity at 380°C is 1×10 6 A non-aqueous dispersion comprising a powder of a tetrafluoroethylene-based polymer having an average particle size of 10 μm or less and Pa s or less, an aromatic polymer, and an inorganic filler, wherein the content of the tetrafluoroethylene-based polymer, the content of the aromatic polymer, and the content of the inorganic filler are each more than 5 mass%. [9] The nonaqueous dispersion according to [8], wherein the aromatic polymer is an aromatic polyimide, an aromatic polyamic acid, an aromatic polyester, or a polyphenylene ether.
[10] The nonaqueous dispersion according to [8] or [9], wherein the aromatic polymer is a liquid crystal polymer.
[11] The nonaqueous dispersion of any of [8] to
[10] , wherein the inorganic filler is a filler containing at least one inorganic compound selected from the group consisting of boron nitride, aluminum nitride, beryllium oxide, silicon oxide, cerium oxide, aluminum oxide, magnesium oxide, zinc oxide, and titanium oxide.
[12] The non-aqueous dispersion liquid according to any one of [8] to
[11] , containing at least one non-aqueous dispersion medium selected from the group consisting of aromatic hydrocarbons, amides, ketones and esters.
[13] A method for producing a laminate, comprising applying any one of the nonaqueous dispersions of [1] to
[12] to a surface of a substrate, heating the substrate, forming a polymer layer, and obtaining a laminate having the substrate and the polymer layer in this order.
[14] A molded article comprising a tetrafluoroethylene-based polymer containing units based on perfluoro(alkyl vinyl ether) and an inorganic filler having an average particle size greater than 0.10 μm, the molded article having a porosity of 5 vol.% or less.
[15] The molded product according to
[14] , wherein the mass ratio of the content of the inorganic filler to the content of the tetrafluoroethylene-based polymer is 1.5 or less. Effect of the Invention
[0009] According to the present invention, a non-aqueous dispersion is obtained which contains a high content of both tetrafluoroethylene-based polymer and inorganic filler and has excellent dispersion stability and blendability with other polymers, etc., and can mold a molded product having high physical properties. Also, a molded product having such high physical properties can be obtained. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The following terms have the following meanings. "Average particle size (D50)" is the cumulative 50% volume diameter of an object (powder or inorganic filler) that is dispersed in water and measured using a laser diffraction / scattering particle size distribution measuring device (LA-920, manufactured by Horiba, Ltd.). In other words, the particle size distribution of the object is measured using the laser diffraction / scattering method, the total volume of the powder particle group is set to 100%, and a cumulative curve is calculated. The average particle size (D50) is the particle size at the point on the cumulative curve where the cumulative volume is 50%. The "98% cumulative volume particle size (D98)", "90% cumulative volume particle size (D90)" and "10% cumulative volume particle size (D10)" are the volume-based cumulative 98% diameter and volume-based cumulative 10% diameter of powder or inorganic filler obtained in a similar manner. The "particle size distribution" is a distribution shown by a curve plotting the particle amount (%) in each particle size interval determined in the same manner. The term "melting temperature (melting point)" refers to the temperature corresponding to the maximum value of the melting peak, as determined by analyzing a polymer by differential scanning calorimetry (DSC). The "glass transition point" is a value measured by analyzing a polymer using a dynamic mechanical analysis (DMA) method. The "specific surface area" is a value determined by analyzing the inorganic filler by gas adsorption method (BET method). The term "approximately spherical inorganic filler" refers to an inorganic filler in which, when observed with a scanning electron microscope (SEM), the proportion of spherical particles with a ratio of minor axis to major axis of 0.7 or more accounts for 95% or more. The "aspect ratio of an inorganic filler" is a ratio obtained by dividing the average particle size (D50) by the short axis length (length in the short direction) of the inorganic filler. For example, the aspect ratio of a scaly anisotropic filler is obtained by dividing its D50 by its average short axis (average value of the short axis diameter). "Viscosity" refers to the viscosity of a liquid measured using a Brookfield viscometer at 25°C and a rotation speed of 30 rpm. The "thixotropy ratio" is a value calculated by dividing the viscosity of a liquid measured at a rotation speed of 30 rpm by the viscosity of the liquid measured at a rotation speed of 60 rpm. The "porosity" is the ratio (%) of the area of voids in the cross section of a molded article observed with a scanning electron microscope (SEM). "Ten-point average roughness (Rzjis)" is defined in Appendix JA of JIS B 0601:2013. The "dielectric tangent" is a value measured by the SPDR method in an environment of 24°C, 50% RH, and a frequency of 10 GHz. The term "unit based on monomer" refers to an atomic group based on the monomer formed by polymerization of the monomer. The unit may be a unit formed directly by a polymerization reaction, or may be a unit in which a part of the unit is converted to a different structure by treating the polymer. Hereinafter, the unit based on monomer a is also referred to simply as "monomer a unit."
[0011] The non-aqueous dispersion of the present invention (hereinafter also referred to as "the present dispersion") has a melt viscosity of 1×10 6 It contains a powder (hereinafter also referred to as "F powder") of a tetrafluoroethylene-based polymer (hereinafter also referred to as "F polymer") having a modulus of less than Pa·s, and an inorganic filler.
[0012] A first embodiment of the present dispersion (hereinafter also referred to as "the present dispersion (1)") contains F powder and an inorganic filler having an average particle size of more than 0.10 μm. Hereinafter, the F polymer in the present dispersion (1) will also be referred to as F polymer (1), the F powder as F powder (1), and the inorganic filler as filler (1). In this dispersion (1), the content of the F polymer (1) and the content of the filler (1) are each more than 5 mass %. In this dispersion (1), the F powder (1) and the filler (1) are dispersed.
[0013] This dispersion (1) contains a large amount of each of the F polymer (1) and the filler (1), has excellent dispersion stability, and can form a molded product (such as the molded product of the present invention described later) that has high physical properties of each of the F polymer (1) and the filler (1). The reason for this is not necessarily clear, but is thought to be as follows. F Polymer (1) has a low melt viscosity at 380°C, and compared with non-thermofusible tetrafluoroethylene polymers, it is less susceptible to physical stress (shear stress, etc.) and changes in state over time, and F Powder (1) has high dispersion stability. It can be said that the present dispersion liquid (1) contains a large amount of such F powder (1), and is in a state in which the interaction between the filler (1) having an average particle size exceeding a predetermined value and the F powder (1) is relatively likely to be enhanced. In other words, if a large amount of inorganic filler having an average particle size equal to or smaller than a predetermined value is contained, the aggregation action between such inorganic fillers themselves is simply enhanced and dispersibility is impaired, but if it is filler (1), the loose aggregation action (interaction) with the F powder (1) contained in a large amount is relatively enhanced, and pseudo secondary particles are formed at least in part of both, resulting in stabilization. As a result, it is believed that the present dispersion (1) has excellent dispersion stability and blendability when other components are added.
[0014] From the present dispersion (1), a molded product having both physical properties at a high level can be formed. The reason is not entirely clear, but is thought to be as follows. The F polymer (1) can be said to be a crystalline polymer containing TFE units, and is prone to forming minute spherulites in the molded product. Due to the microscopic uneven structure of the surface of such spherulites, the filler (1) and the spherulites are not completely in contact with each other in the molded product, and are uniformly distributed at least partially through minute voids. In other words, it is considered that such minute voids act as a buffer, and the physical properties of both (F polymer (1) and filler (1)) in the molded product are highly expressed. Specifically, if the filler (1) is an inorganic filler with a low linear expansion coefficient such as a silica filler, the molded product can be highly equipped with the resistance to warping due to the filler (1) and the various physical properties (heat resistance, electrical properties, etc.) due to the F polymer (1). Such a molded article can be suitably used as a printed circuit board material or a component thereof.
[0015] The F polymer (1) in the dispersion (1) contains units based on tetrafluoroethylene (TFE) (TFE units) and has a melt viscosity of 1×10 at 380° C. 6 The polymer (1) F may consist of TFE units alone or may contain TFE units and other units. The melt viscosity of F polymer (1) at 380°C is 5 x 10 5 Pa s or less is preferable, and 1×10 5 The melt viscosity is preferably 1×10 Pa·s or less. 2 Pa s or more is preferable, and 1×10 3 It is more preferable that the viscosity is Pa·s or more. In this case, the affinity between the F powder (1) and the filler (1) is easily improved. As the F polymer (1), a polymer containing a TFE unit and a PAVE unit is preferred. PAVE is CF 2 =CFOCF 3 (PMVE), CF 2 =CFOCF 2 CF 3 or CF 2 =CFOCF 2 CF 2 CF 3 (PPVE) is preferred. The melting temperature (melting point) of the F polymer (1) is preferably from 260 to 320°C, more preferably from 285 to 320°C. The glass transition point of the F polymer (1) is preferably from 75 to 125°C, more preferably from 80 to 100°C.
[0016] The F polymer (1) preferably further has units based on monomers other than the TFE unit and the PAVE unit. Examples of the monomer include olefins (such as ethylene and propylene), chlorotrifluoroethylene, fluoroolefins (such as hexafluoropropylene and fluoroalkylethylene), and monomers having an oxygen-containing polar group, which will be described later. Specific examples of fluoroalkylethylenes include CH 2 =CH(CF 2 ) 2 F, C.H. 2 =CH(CF 2 ) 4 F, C.H. 2 =CF(CF 2 ) 2 H, C.H. 2 =CF(CF 2 ) 4 Examples include H.
[0017] The F polymer (1) preferably has an oxygen-containing polar group. The oxygen-containing polar group may be contained in a unit contained in the F polymer (1) or may be contained in a terminal group of the polymer main chain. The latter F polymer (1) may be an F polymer having a polar functional group as a terminal group derived from a polymerization initiator, a chain transfer agent, etc., or an F polymer having an oxygen-containing polar group prepared by plasma treatment or ionizing radiation treatment. If the F polymer (1) has an oxygen-containing polar group, the dispersibility of the F powder (1) in the present dispersion liquid is excellent. The oxygen-containing polar group is preferably a hydroxyl group-containing group, a carbonyl group-containing group, or a phosphono group-containing group, and from the viewpoints of the dispersibility of the dispersion and the adhesion of the surface of the molded article, a hydroxyl group-containing group or a carbonyl group-containing group is more preferable, and a carbonyl group-containing group is particularly preferable. The hydroxyl group-containing group is preferably an alcoholic hydroxyl group-containing group, -CF 2 CH 2 OH, -C(CF 3 ) 2 OH or 1,2-glycol group (-CH(OH)CH 2 OH) is more preferred. The carbonyl group-containing group is a carboxyl group, an alkoxycarbonyl group, an amide group, an isocyanate group, a carbamate group (-OC(O)NH 2 ), an acid anhydride residue (-C(O)OC(O)-), an imide residue (-C(O)NHC(O)- etc.) or a carbonate group (-OC(O)O-).
[0018] The F polymer (1) having an oxygen-containing polar group particularly preferably has a unit based on a monomer having an oxygen-containing polar group. Such an F polymer (1) is likely to improve the adhesion and heat resistance of the molded product. The monomer is preferably a monomer having a hydroxyl group-containing group or a carbonyl group-containing group, and more preferably a monomer having a carbonyl group-containing group. The monomer having a carbonyl group-containing group is preferably itaconic anhydride, citraconic anhydride, 5-norbornene-2,3-dicarboxylic anhydride (also called himic anhydride; hereinafter also referred to as "NAH") or maleic anhydride, and more preferably NAH. The F polymer (1) is preferably a polymer containing TFE units and PAVE units, containing 1 to 10 mol % of PAVE units based on all units, and having a melting temperature of 260 to 320°C, and more preferably a polymer containing TFE units, PAVE units, and units based on a monomer having an oxygen-containing polar group, a polymer consisting of 95.0 to 98.0 mol % TFE units and 2.0 to 5.0 mol % PAVE units, or a polymer containing TFE units and PMVE units.
[0019] These polymers are particularly resistant to physical stress and changes in state over time, and have excellent dispersibility. In addition, they tend to relatively increase their interaction with the filler (1), which makes it easier to improve the dispersion stability of the dispersion. Furthermore, dense spherulites are easily formed in the molded product, and the physical properties of the molded product are easily improved. Specifically, a molded product is easily formed that has high physical properties (heat resistance, electrical properties, etc.) due to the F polymer (1) and high physical properties (low linear expansion coefficient, dielectric properties, etc.) due to the filler (1), and such a molded product can be suitably used as a printed circuit board material or a member thereof.
[0020] The F powder (1) in the present dispersion (1) may contain components other than the F polymer (1), and is preferably composed of the F polymer (1). Examples of the components other than the F polymer (1) include liquid crystal polyester, polyamideimide, polyimide, polyphenylene ether, and polyphenylene oxide.
[0021] The F powder (1) may form a complex with an inorganic substance. As the inorganic substance, oxides, nitrides, metal elements, alloys and carbon are preferred, silicon oxide (silica), metal oxides (beryllium oxide, cerium oxide, alumina, soda alumina, magnesium oxide, zinc oxide, titanium oxide, etc.), boron nitride and magnesium metasilicate (steatite) are more preferred, silica and boron nitride are even more preferred, and silica is particularly preferred. In this case, the dispersibility of the present dispersion liquid (1) is likely to be improved. The complex of the F powder (1) and an inorganic substance is preferably a particle having an F polymer (1) as a core and an inorganic substance on the surface of the core. Such particles are obtained, for example, by bonding (collision, aggregation, etc.) a powder of the F polymer (1) and a powder of an inorganic substance. The inorganic substance may be contained in the filler (1). In other words, the F powder (1) and the filler (1) may form a complex.
[0022] F powder (1) may be used alone or in the form of a mixture of two kinds. F powder (1) may be a mixture of a powder of a polymer containing, relative to the total units, 90 to 98 mol % of TFE units, 1 to 9.97 mol % of PAVE units, and 0.01 to 3 mol % of units based on a monomer having an oxygen-containing polar group, and a powder of PTFE. In this case, the PTFE is preferably a low molecular weight PTFE.
[0023] The D50 of the F powder (1) is preferably 0.1 μm or more, more preferably 0.3 μm or more, and even more preferably 1 μm or more. The D50 of the F powder (1) is preferably 6 μm or less, more preferably 4 μm or less, and even more preferably 3 μm or less. In this case, the interaction between the F powder (1) and the filler (1) is enhanced, and the dispersion stability of the present dispersion liquid (1) is likely to be further improved. It is preferable that F powder (1) does not substantially contain coarse particles. The particle diameter of the coarse particles in F powder (1) is preferably 10 μm or more, more preferably 6 μm or more. In other words, the 98% particle diameter of F powder (1) is preferably less than 10 μm, more preferably less than 6 μm. If the dispersion liquid (1) does not contain coarse particles, the interaction between F powder (1) and filler (1) is enhanced, and the dispersion stability is likely to be improved.
[0024] The content of F powder (1) in the present dispersion liquid (1) is more than 5% by mass, preferably 7% by mass or more, more preferably 10% by mass or more, and even more preferably 25% by mass or more. The content of F powder (1) is preferably 50% by mass or less, more preferably 40% by mass or less, and even more preferably 30% by mass or less. In this case, the dispersibility of F powder (1) in the present dispersion liquid (1) is excellent. If the content of F powder (1) is within this range, the interaction between F powder (1) and filler (1) is relatively increased, and the dispersion stability is easily improved. In addition, the physical properties of F polymer (1) in the molded product are easily manifested significantly.
[0025] The filler (1) in the present dispersion (1) is preferably a nitride filler or an inorganic oxide filler, more preferably a boron nitride filler, a beryllium oxide filler (beryllia filler), a silicon oxide filler (silica filler), a metal oxide (cerium oxide, alumina, soda alumina, magnesium oxide, zinc oxide, titanium oxide, etc.) filler or a magnesium metasilicate filler (steatite filler), and even more preferably a silica filler or a magnesium metasilicate filler (steatite filler). These fillers may be fired ceramic fillers. Such a filler (1) is likely to enhance the interaction with the F powder (1), and the dispersion stability of the present dispersion (1) is likely to be improved. In addition, in the molded product, the physical properties based on the filler (1) are likely to be significantly expressed.
[0026] The filler (1) may be used alone or in combination with two or more different types of D50 or different kinds. The filler (1) preferably contains silicon oxide or magnesium metasilicate (steatite). Silicon oxide and steatite are likely to enhance the interaction with the F polymer (1), and the filler (1) containing them is likely to further improve the dispersion stability of the present dispersion liquid (1). In addition, the physical properties of silicon oxide or steatite are likely to be significantly expressed in the molded product. The content of silicon oxide or magnesium metasilicate in the filler (1) is preferably 50% by mass or more, more preferably 75% by mass, and the content of silicon oxide or magnesium metasilicate is preferably 100% by mass or less, more preferably 90% by mass or less. When the filler (1) is added to water, the pH of the water may be acidic, neutral or alkaline, and is preferably neutral or alkaline.
[0027] At least a part of the surface of the filler (1) is preferably surface-treated. Examples of surface treatment agents used for such surface treatment include polyhydric alcohols (trimethylolethane, pentaerythritol, propylene glycol, etc.), saturated fatty acids (stearic acid, lauric acid, etc.), esters thereof, alkanolamines, amines (trimethylamine, triethylamine, etc.), paraffin wax, silane coupling agents, silicones, polysiloxanes, oxides of aluminum, silicon, zirconium, tin, titanium, antimony, etc., hydroxides thereof, hydrated oxides thereof, and phosphates thereof.
[0028] The filler (1) is preferably an inorganic filler that has been surface-treated with a silane coupling agent. Such a filler (1) has excellent affinity with the F powder (1) and is likely to improve the dispersibility of the present dispersion (1). In addition, when the F polymer (1) is melted and sintered to form a molded product from the present dispersion (1) containing the filler, the filler (1) is thermally decomposed to generate gas, which promotes the flow of the filler (1) and is likely to improve the uniformity of the molded product. The silane coupling agent is preferably a silane coupling agent having a functional group, and more preferably 3-aminopropyltriethoxysilane, vinyltrimethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 3-methacryloxypropyltriethoxysilane, or 3-isocyanatopropyltriethoxysilane.
[0029] The D50 of the filler (1) is more than 0.10 μm, preferably 0.15 μm or more, and more preferably 0.30 μm or more. The D50 of the filler (1) is preferably less than 10 μm, more preferably 1.8 μm or less, and even more preferably 1.5 μm or less. In this case, the dispersibility of the F powder (1) in the present dispersion liquid (1) is excellent. If the D50 of the filler (1) is within this range and is close to the D50 of the F powder (1), the interaction between the two is relatively increased, and the dispersion stability is likely to be improved.
[0030] It is preferable that the filler (1) does not substantially contain coarse particles. The particle size of the coarse particles in the filler (1) is preferably 25 μm or more, more preferably 20 μm or more, and even more preferably 10 μm or more. In other words, the 98% particle size of the filler (1) is preferably less than 25 μm, more preferably less than 20 μm, and even more preferably less than 10 μm. In this case, the dispersibility of the filler (1) in the present dispersion liquid (1) is excellent. If the present dispersion liquid (1) does not contain coarse particles, the interaction between the F powder (1) and the filler (1) is enhanced, and the dispersion stability is likely to be improved.
[0031] The D50 of the filler (1) is preferably equal to or less than the D50 of the F powder (1). In this case, the interaction between the two is relatively increased, and the dispersion stability is likely to be improved. Furthermore, the filler (1) is more likely to be distributed more uniformly in the molded product, and its physical properties are more likely to be significantly exhibited. Specifically, it is preferable that the D50 of the filler (1) is more than 0.10 μm and 1 μm or less, and the D50 of the F powder (1) is 1 μm or more and 3 μm or less. The specific surface area of the filler (1) is 1 to 20 m 2 / g is preferable, and 5 to 8m 2 / g is more preferable. In this case, the filler (1) becomes more easily wetted in the present dispersion (1), and the interaction with the F powder (1) is easily enhanced. In addition, in a molded product formed from the present dispersion (1), the filler (1) and the F polymer (1) are more easily distributed uniformly, and the physical properties of both are easily expressed in a well-balanced manner.
[0032] The shape of the filler (1) is preferably approximately spherical. In spherical particles that account for 95% or more of the approximately spherical filler (1), the ratio of the short diameter to the long diameter is preferably 0.8 or more, more preferably 0.9 or more. The above ratio is preferably less than 1. If the filler (1) is highly approximately spherical, the filler (1) becomes more easily wetted in the dispersion liquid (1) and the interaction with the F powder (1) is easily enhanced. Furthermore, in the molded product, the filler (1) and the F polymer (1) are more easily distributed, and the physical properties of both are easily expressed in a balanced manner.
[0033] The filler (1) preferably has a scaly shape. The aspect ratio of the scaly filler (1) is preferably 5 or more, more preferably 10 or more. The aspect ratio is preferably 1000 or less. The average major axis (average value of diameter in the longitudinal direction) of the scaly filler (1) is preferably 1 μm or more, more preferably 3 μm or more. The average major axis is preferably 20 μm or less, more preferably 10 μm or less. The average minor axis is preferably 0.01 μm or more, more preferably 0.1 μm or more. The average minor axis is preferably 1 μm or less, more preferably 0.5 μm or less. In this case, the filler (1) becomes more easily wetted in the dispersion liquid (1), and the interaction with the F powder (1) is easily enhanced. Furthermore, in the molded product, the filler (1) and the F polymer (1) are more easily distributed, and the physical properties of both are easily expressed in a well-balanced manner. The scaly filler (1) may have a single-layer structure or a multi-layer structure.
[0034] The internal structure of the filler (1) may be dense, hollow, or honeycomb. The hollow filler (1) preferably has a hollow ratio (average volume ratio of voids per particle) of 40 to 80%. The hollow filler (1) preferably has a particle strength of 20 MPa or more. The particle strength is the particle strength when the remaining rate of hollow filler after pressure pressing is 50%. The particle strength can be calculated from the apparent density of the hollow filler and the apparent density of the pellet obtained by pressure pressing the mesosphere filler.
[0035] The filler (1) is preferably a sintered inorganic filler (an inorganic filler that has been sintered), in other words, preferably in the form of a ceramic. The water content of the filler (1) is preferably 0.3% by mass or less, more preferably 0.1% by mass or less. The water content is preferably 0% by mass or more. In this case, the filler (1) becomes more easily wetted in the dispersion liquid (1), and the interaction with the F powder (1) is easily enhanced. In addition, the filler (1) and the F polymer (1) are more easily distributed in the molded product, and the physical properties of both are easily expressed in a balanced manner.
[0036] Specific examples of suitable filler (1) include silica fillers having a D50 of more than 0.10 μm (such as the "Adma Fine" series manufactured by Admatechs Co., Ltd.), zinc oxide having a D50 of more than 0.10 μm and surface-treated with an ester such as propylene glycol dicaprylate (such as the "FINEX" series manufactured by Sakai Chemical Industry Co., Ltd.), nearly spherical fused silica fillers having a D50 of more than 0.10 μm and 0.5 μm or less and a 98% particle size of less than 1 μm (such as the "SFP" series manufactured by Denka Co., Ltd.), and D50-treated fillers coated with polyhydric alcohol and inorganic substances. Examples of fillers include rutile-type titanium dioxide fillers with a D50 of more than 0.10 μm and less than 0.5 μm (such as the "Tipaque" series manufactured by Ishihara Sangyo Co., Ltd.), rutile-type titanium dioxide fillers with a D50 of more than 0.10 μm that have been surface-treated with alkylsilane (such as the "JMT" series manufactured by Teika Corporation), steatite fillers with a D50 of more than 0.10 μm (such as the "BST" series manufactured by Nippon Talc Co., Ltd.), and boron nitride fillers with a D50 of more than 0.10 μm (such as the "UHP" series manufactured by Showa Denko KK, and the "HGP" series and "GP" series manufactured by Denka Co., Ltd.).
[0037] A preferred embodiment of the inorganic filler contained in the present dispersion (1) includes a filler (1) (hereinafter also referred to as "filler (11)") and an inorganic filler (hereinafter also referred to as "different filler") having a D50 of less than 1 μm and smaller than that of the filler (11). In this case, the improvement in the dispersion stability of the present dispersion (1) by the filler (11) and the ability to form a dense molded product by the different filler are balanced, and the physical properties (water resistance, low linear expansion, electrical properties, etc.) of the obtained molded product are more likely to be improved. The different filler may be an inorganic filler having a D50 smaller than that of the filler (11), and may be the same as or different from the filler (11).
[0038] The D50 of the filler (11) is preferably 1 μm or more, and more preferably 1 μm or more and less than 10 μm. Moreover, if the different filler has a D50 of more than 0.10 μm, it is preferably a filler having a smaller D50 than the filler (11), and more preferably a silica filler. If the different filler has a D50 of 0.10 μm or less, it is preferably a silica filler. The different filler preferably has a D50 of 0.01 μm or more and less than 1 μm.
[0039] In addition, the filler (1) in such a preferred embodiment may have a multi-modal particle size distribution. In this case, it is preferable that the peak in the particle size distribution attributable to the filler (11) is the highest, from the viewpoint of facilitating the formation of a dense molded product. Specifically, the filler (1) is preferably contained in a state having a bimodal particle size distribution having peaks in the region of 0.8 μm or less and the region of 1 μm or more, and more preferably contained in the above-mentioned state having a bimodal particle size distribution in which the latter peak is higher than the former peak.
[0040] In addition, in such a preferred embodiment, the filler (1) may be contained such that at least a part of it adheres to the surface of the F powder (1) or at least a part of the F powder (1) adheres to the surface. In this case, the dispersion liquid (1) can be said to contain a composite of the F powder (1) and the filler (1), and the dispersion stability is further improved, and the physical properties (water resistance, low linear expansion, electrical properties, etc.) of the molded product formed therefrom are likely to be further improved.
[0041] In this preferred embodiment, the mass ratio of the content of the different filler to the content of the filler (11) is preferably 0.1 or more, more preferably 0.4 or more. Moreover, the mass ratio is preferably 1 or less, more preferably 0.8 or less. In this case, the dispersion stability of the dispersion (1) and the physical properties of the molded product are easily balanced.
[0042] The content of the filler (1) in the dispersion (1) is more than 5% by mass, preferably 10% by mass or more, more preferably 20% by mass or more, and even more preferably 25% by mass or more. The content of the filler (1) is preferably 50% by mass or less, more preferably 40% by mass or less, and even more preferably 30% by mass or less. When the content of the filler (1) is within this range, the interaction between the F powder (1) and the filler (1) is relatively enhanced, and the dispersion stability is likely to be improved. In addition, the physical properties of the filler (1) are likely to be significantly expressed in the molded product.
[0043] The content of the filler (1) in the dispersion (1) is preferably equal to or less than the content of the F polymer (1). In this case, a molded product is likely to be formed in which the F polymer (1) serves as a matrix and the filler (1) is uniformly distributed, and the physical properties of both are likely to be well balanced. Specifically, it is preferable that the content of the filler (1) is from 5% by mass to 25% by mass, and the content of the F polymer (1) is from more than 25% by mass to 50% by mass.
[0044] It is preferable that the present dispersion (1) further contains another resin (polymer) different from the F polymer (1). In this case, in the molded product obtained from the present dispersion (1), the other resin is uniformly dispersed, and the properties based on the other resin tend to be well exhibited. The other resin may be a thermosetting resin or a thermoplastic resin. Examples of other resins include epoxy resins, maleimide resins, urethane resins, fluororesins, elastomers, polyimides, polyamic acids, polyamideimides, polyphenylene ethers, polyphenylene oxides, liquid crystal polyesters, and fluoropolymers other than F polymers.
[0045] The other resin is preferably a polyimide or a polyamic acid, more preferably a thermoplastic polyimide. In this case, the molded product has a reduced porosity and is dense, and the physical properties of the F polymer (1) and the filler (1) tend to be significantly exhibited. In addition, when a molded product is formed from the dispersion (1), the powder fall of the F powder (1) is suppressed, and the adhesiveness tends to be improved. In this case, the content of polyimide or polyamic acid in the present dispersion (1) is preferably 1 to 30 mass %, more preferably 5 to 25 mass %. The mass ratio of the content of polyimide to the content of F polymer (1) is preferably 1.0 or less, more preferably 0.1 to 0.7. When the present dispersion (1) contains another resin, it may be produced by mixing the present dispersion (1) with a powder of the other resin, or it may be produced by mixing the present dispersion (1) with a varnish containing the other resin. The other resin is preferably an aromatic polymer. The definition and scope of the aromatic polymer, including preferred embodiments thereof, are the same as those of the aromatic polymer (AR polymer) in the present dispersion (2) described later.
[0046] The liquid dispersion medium in the present dispersion liquid (1) is a non-aqueous liquid dispersion medium, which functions as a dispersion medium for the F powder (1) and the filler (1) and is a liquid compound that is inactive at 25° C. Such liquid compounds may be used alone or in combination of two or more kinds. The boiling point of the liquid compound is preferably 125 to 250° C. In this case, when a molded product is formed from the dispersion (1), the F powder (1) and the filler (1) are easily packed closely together, and the physical properties of the molded product are easily improved.
[0047] The liquid compound is preferably at least one selected from the group consisting of amides, ketones and esters, specific examples of which include N,N-dimethylformamide, N,N-dimethylacetamide, 3-methoxy-N,N-dimethylpropanamide, 3-butoxy-N,N-dimethylpropanamide, N-methyl-2-pyrrolidone, γ-butyrolactone, cyclohexanone, cyclopentanone, butyl acetate, and methyl isopropyl ketone. When the present dispersion (1) further comprises an aromatic polymer, in particular an aromatic thermoplastic polyimide, the liquid compound preferably comprises an amide and a ketone or an ester, more preferably 3-methoxy-N,N-dimethylpropanamide, 3-butoxy-N,N-dimethylpropanamide or N-methyl-2-pyrrolidone and cyclohexanone, cyclopentanone, γ-butyrolactone or butyl acetate. The content of the liquid dispersion medium in the present dispersion liquid (1) is preferably 25% by mass or more, more preferably 30% by mass or more. The content of the liquid dispersion medium is preferably 70% by mass or less, more preferably 60% by mass or less. When the content of the liquid dispersion medium is within this range, the interaction between the F powder (1) and the filler (1) is enhanced, and the dispersion stability of the present dispersion liquid (1) is likely to be improved.
[0048] The present dispersion (1) preferably further contains a surfactant, and more preferably contains a nonionic surfactant. The nonionic surfactant preferably has an alcoholic hydroxyl group or an oxyalkylene group (hereinafter also referred to as "AO group") as a hydrophilic site, and more preferably has an alcoholic hydroxyl group and an AO group as a hydrophilic site. Such a surfactant has improved affinity (interaction) with the liquid dispersion medium via the AO group, and is likely to increase the dispersibility of the present dispersion (1). The AO group may be composed of one kind of AO group, or may be composed of two or more kinds of AO groups. In the latter case, the different kinds of AO groups may be arranged randomly or in blocks.
[0049] The hydrophobic portion of the surfactant is preferably an acetylene-containing group, a perfluoroalkyl group, or a perfluoroalkenyl group. Specifically, the surfactant is preferably an acetylene-based surfactant, a silicone-based surfactant or a fluorine-based surfactant, and more preferably a silicone-based surfactant. In this case, since the F powder (1) and the filler (1) interact with the surfactant to a high degree, not only is the dispersion stability of the dispersion (1) more likely to be improved, but the physical properties of both (the F polymer (1) and the filler (1)) are more likely to be significantly expressed in the molded product.
[0050] The weight average molecular weight of the nonionic surfactant is preferably 1,000 to 80,000. When the nonionic surfactant has an AO group, the content of the AO group is preferably 10% by mass or more, more preferably 20% by mass or more. The content of the AO group is preferably 50% by mass or less. In this case, the affinity of the nonionic surfactant to the liquid dispersion medium is further improved, and the dispersibility of the F powder (1) and the filler (1) in the present dispersion liquid (1) is likely to be further improved. When the nonionic surfactant has an alcoholic hydroxyl group, the hydroxyl value is preferably 100 mgKOH / g or less, more preferably 50 mgKOH / g or less, and more preferably 10 mgKOH / g or more.
[0051] When the nonionic surfactant is a fluorine-based surfactant, the fluorine content is more preferably from 20 to 50 mass %. The nonionic fluorine-based surfactant is preferably a copolymer of a compound represented by the following formula (F) and a compound represented by the following formula (H). CH 2 =CHR F -C(O)OQ F -X F (F) CH 2 =CHR H -C(O)-(Q H ) m -OH (H) R F represents a hydrogen atom or a methyl group. Q F represents an alkylene group or an oxyalkylene group. X F represents a perfluoroalkyl group or a perfluoroalkenyl group. R Hrepresents a hydrogen atom or a methyl group. Q H represents an oxyalkylene group. m represents an integer of 1 to 120.
[0052] Specific examples of the compound represented by formula (F) include CH 2 =C(CH 3 )C(O)OCH 2 CH 2 (CF 2 ) 4 F, C.H. 2 =C(CH 3 )C(O)OCH 2 CH 2 (CF 2 ) 6 F, C.H. 2 =C(CH 3 )C(O)OCH 2 CH 2 CH 2 CH 2 OCF(CF 3 )C(=C(CF 3 ) 2 )(CF(CF 3 ) 2 ), C.H. 2 =C(CH 3 )C(O)OCH(CH 3 )OCH 2 (CF 2 ) 6 Examples include F. Specific examples of the compound represented by formula (H) include CH 2 =C(CH 3 )C(O)(OCH 2 CH 2 ) 4 OH, CH 2 =C(CH 3 )C(O)(OCH 2 CH 2 ) 9 OH, CH 2 =C(CH 3 )C(O)(OCH 2 CH 2 ) 23 OH is an example. The amount of each compound (monomer) used in producing the copolymer may be appropriately determined depending on the type of compound and the physical properties of the surfactant described above (fluorine content, AO group content, hydroxyl value, etc.).
[0053] Specific examples of such nonionic surfactants include the "Ftergent" series (manufactured by Neos), the "Surflon" series (manufactured by AGC Seimi Chemical Co., Ltd.), the "Megafac" series (manufactured by DIC Corporation), the "Unidyne" series (manufactured by Daikin Industries, Ltd.), "BYK-347", "BYK-349", "BYK-378", "BYK-3450", "BYK-3451", "BYK-3455", "BYK-3456" (manufactured by BYK Japan), and "KF-6011" and "KF-6043" (manufactured by Shin-Etsu Chemical Co., Ltd.). When the present dispersion (1) contains a surfactant, the content of the surfactant in the present dispersion (1) is preferably 1 to 15 mass %. When the content of the surfactant is within this range, the interaction between the F powder (1) and the filler (1) is enhanced, and the dispersion stability of the present dispersion (1) is likely to be further improved.
[0054] In addition to the above-mentioned components, the present dispersion (1) may contain additives such as a thixotropic agent, an antifoaming agent, a silane coupling agent, a dehydrating agent, a plasticizer, a weathering agent, an antioxidant, a heat stabilizer, a lubricant, an antistatic agent, a brightening agent, a colorant, a conductive agent, a release agent, a surface treatment agent, a viscosity regulator, a flame retardant, an organic filler, etc. Due to the above-mentioned mechanism of action, the present dispersion (1) has excellent dispersion stability even when it contains such additives, and the physical properties of the F polymer (1) and the filler (1) are highly expressed in the molded product formed therefrom.
[0055] The water content of the present dispersion (1) is preferably 20,000 ppm or less, more preferably 8,000 ppm or less, and even more preferably 5,000 ppm or less. The water content of the present dispersion (1) is preferably 0 ppm or more. In this case, the dispersion stability of the present dispersion (1) is more likely to be improved. The viscosity of the present dispersion (1) is preferably 50 mPa·s or more, and more preferably 100 mPa·s or more. The viscosity of the present dispersion (1) is preferably 1000 mPa or less, and more preferably 800 mPa or less. In this case, the dispersion stability of the present dispersion (1) is more likely to be improved. The thixotropy ratio of the present dispersion (1) is preferably 1.0 or more. The thixotropy ratio of the present dispersion (1) is preferably 3.0 or less, and more preferably 2.0 or less. Due to the above-mentioned mechanism of action, the present dispersion (1) easily forms such a liquid composition having excellent thixotropy.
[0056] The present dispersion (1) can be produced by mixing the F powder (1), the filler (1), and a liquid dispersion medium, and is preferably produced by separately preparing a non-aqueous dispersion containing the F powder (1) and a non-aqueous dispersion containing the filler (1) and mixing the two. In this case, the interaction between the F powder (1) and the filler (1) is enhanced, making it easy to prepare the present dispersion (1) with excellent dispersion stability. In this case, each non-aqueous dispersion preferably contains the above-mentioned surfactant. In addition, when other resins such as aromatic polymers are further contained in the present dispersion liquid (1), it is preferable to add them at the same time when dispersing the F powder (1) in the liquid dispersion medium in advance, or to add them in advance to the liquid dispersion medium before dispersing the F powder (1).
[0057] A specific method for producing the dispersion (1) includes mixing the F powder (1), the filler (1), a different filler, and a liquid dispersion medium. In this mixing, the F powder (1) and the liquid dispersion medium may be mixed in advance to form a non-aqueous dispersion, or the filler (11) and the different filler may be mixed in advance.
[0058] A second embodiment of the present dispersion (hereinafter also referred to as "present dispersion (2)") contains an F polymer powder having an average particle size of 10 μm or less, an aromatic polymer (hereinafter also referred to as "AR polymer"), an inorganic filler, and a liquid dispersion medium. Hereinafter, the F polymer in the present dispersion (2) will be referred to as F polymer (2), the F powder as F powder (2), and the inorganic filler as filler (2). In this dispersion (2), the F powder (2) and the filler (2) are each dispersed, and the AR polymer is dissolved or highly dispersed. The content of the F polymer (2), the content of the AR polymer, and the content of the filler (2) each exceed 5% by mass. This dispersion (2) is a non-aqueous dispersion with high contents of each of the three components (F polymer (2), AR polymer, and filler (2); the same applies below), and has excellent dispersibility, and the polymer layer (molded product) obtained from it has excellent physical properties based on the three components and is excellent in rigidity. The reason for this is not necessarily clear, but is thought to be as follows.
[0059] Although the AR polymer and inorganic filler themselves show a certain dispersibility or solubility in the non-aqueous dispersion, when their contents are high, the stability and properties of the non-aqueous dispersion tend to deteriorate. Specifically, when the AR polymer content is high, the viscosity and thixotropy ratio of the non-aqueous dispersion tend to increase, and the stability of the non-aqueous dispersion tends to deteriorate. In addition, when the inorganic filler content is high, the inorganic filler itself tends to aggregate or settle, and the stability of the non-aqueous dispersion tends to deteriorate. If a large amount of tetrafluoroethylene-based polymer powder, which has low surface tension, is further dispersed in such a non-aqueous dispersion, it will induce aggregation of each component and phase separation of the non-aqueous dispersion. This tendency becomes more pronounced when physical stress (shear stress, etc.) is applied to the non-aqueous dispersion in order to disperse the powder.
[0060] On the other hand, F polymer (2) has a melt viscosity within a specified range and has plasticity, and its powder is not easily affected by physical stress and has excellent dispersibility. The dispersion (2) contains a high content of such fine powder of the F polymer (2). In other words, the dispersion (2) contains the F polymer (2) densely (at a high density), so that the interaction between the three components tends to increase gradually. Therefore, the dispersion (2) is considered to have excellent dispersion stability and handleability. Furthermore, the three components tend to be densely and uniformly packed in the polymer layer formed therefrom. Therefore, the molded product (polymer layer, etc.) formed from the dispersion (2) is considered to have excellent rigidity such as folding resistance and low linear expansion while having the physical properties of the three components at a high level. The above-mentioned effects are more significantly exhibited in a preferred embodiment of the present dispersion (2) described below.
[0061] The definitions and scope of F polymer (2) and F powder (2), including preferred embodiments, are the same as those of F polymer (1) and F powder (1). The F polymer (2) may be polytetrafluoroethylene having a number average molecular weight of 10,000 to 200,000 (hereinafter, also referred to as "low molecular weight PTFE"). The number average molecular weight of the low molecular weight PTFE is a value calculated based on the following formula (1). Mn = 2.1 × 10 10 ×ΔHc -5.16 ... (1) In formula (1), Mn represents the number average molecular weight of the low molecular weight PTFE, and ΔHc represents the heat of crystallization (cal / g) of the low molecular weight PTFE measured by differential scanning calorimetry. When the F polymer (2) is a low molecular weight PTFE, the physical properties of the low molecular weight PTFE are expressed in the molded product (polymer layer, etc.), and the molded product tends to have excellent heat resistance and chemical resistance. In addition, a molded product with little unevenness in heat conductivity can be formed.
[0062] The melting temperature of the F polymer (2) is preferably from 280 to 325°C, more preferably from 285 to 320°C. The F polymer (2) is preferably a polymer containing TFE units and PAVE units, containing 1 to 5 mol % of PAVE units based on all units, and having a melting temperature of 260 to 320°C, and is more preferably a polymer (1) having an oxygen-containing polar group, containing TFE units, PAVE units, and units based on a monomer having an oxygen-containing polar group, or a polymer (2) containing TFE units and PAVE units, containing 2.0 to 5.0 mol % of PAVE units based on all units, and not having an oxygen-containing polar group. These F polymers (2) not only have excellent dispersion stability in their powder form, but also tend to distribute densely and uniformly in molded articles formed from the present dispersion (2). Furthermore, they tend to form fine spherulites in the polymer layer, which tends to increase adhesion with other components. As a result, molded articles that have high physical properties of each of the three components are more easily formed.
[0063] The polymer (1) preferably contains, based on all units, 90 to 98 mol % of TFE units, 1 to 9.97 mol % of PAVE units, and 0.01 to 3 mol % of units based on a monomer having a polar functional group. Specific examples of polymer (1) include the polymers described in WO 2018 / 16644.
[0064] The content of PAVE units in the polymer (2) is preferably 2.1 mol % or more, more preferably 2.2 mol % or more, based on all units. The polymer (2) is composed only of TFE units and PAVE units, and preferably contains 95.0 to 98.0 mol % of TFE units and 2.0 to 5.0 mol % of PAVE units based on all units. In addition, the polymer (2) having no oxygen-containing polar group is 1×10 of the number of carbon atoms constituting the polymer main chain. 6 This means that the number of oxygen-containing polar groups in the polymer per unit is less than 500. The number of the oxygen-containing polar groups is preferably 100 or less, more preferably 50 or less. The lower limit of the number of the oxygen-containing polar groups is usually 0. The polymer (2) may be produced by using a polymerization initiator or a chain transfer agent that does not generate an oxygen-containing polar group as a terminal group of the polymer chain, or by fluorinating an F polymer having an oxygen-containing polar group (such as an F polymer having an oxygen-containing polar group derived from a polymerization initiator at the terminal group of the main chain of the polymer). Examples of the fluorination method include a method using fluorine gas (see JP 2019-194314 A, etc.).
[0065] The D50 of the F powder (2) is preferably 8 μm or less, more preferably 4 μm or less, and the D50 of the powder is preferably 0.01 μm or more, more preferably 0.1 μm or more. Moreover, D90 of the F powder (2) is preferably 10 μm or less, and more preferably 6 μm or less. When D50 and D90 are within this range, the fluidity and dispersibility of the F powder (2) become good, and the electrical properties (low dielectric constant, etc.) and heat resistance of the resulting polymer layer are most easily exhibited.
[0066] The AR polymer in the present dispersion (2) is a polymer other than the F polymer (2) and is preferably a polymer having an aromatic ring in the main chain or a prepolymer forming such a polymer. The AR polymer is preferably thermoplastic. The dielectric loss tangent of the AR polymer is preferably 0.005 or less, more preferably 0.003 or less. The dielectric loss tangent of a polymer that is a precursor of another aromatic polymer, such as an aromatic polyamic acid described later, is the dielectric loss tangent of the aromatic polymer formed from the precursor. The AR polymer may be at least one selected from the group consisting of aromatic polyimide, aromatic polyamic acid, aromatic polyamideimide, aromatic polyester, polyphenylene ether, phenol resin, and diallyl phthalate resin. Among these, the AR polymer is preferably an aromatic polyimide, an aromatic polyamic acid, an aromatic polyester, or a polyphenylene ether, and more preferably an aromatic polyimide or an aromatic polyamic acid.
[0067] Examples of aromatic polyesters include liquid crystal polyesters. Examples of liquid crystal polyesters include the polymers described in paragraphs
[0010] to
[0015] of JP-A-2000-248056. Specific examples of aromatic polyesters include polymers of dicarboxylic acids (terephthalic acid, isophthalic acid, diphenyl ether-4,4'-dicarboxylic acid, acetic anhydride, etc.), dihydroxy compounds (4,4'-biphenol, etc.), aromatic hydroxycarboxylic acids (4-hydroxybenzoic acid, 6-hydroxy-2-naphthoic acid, 2-hydroxy-6-naphthoic acid, etc.), aromatic diamines, aromatic hydroxyamines, aromatic aminocarboxylic acids, etc. Specific examples of aromatic polyesters include a reaction product of 4-hydroxybenzoic acid and 6-hydroxy-2-naphthoic acid, a reaction product of 6-hydroxy-2-naphthoic acid, terephthalic acid and acetaminophen, a reaction product of 4-hydroxybenzoic acid, terephthalic acid and 4,4'-biphenol, and a reaction product of 2-hydroxy-6-naphthoic acid, 4,4'-dihydroxybiphenyl, terephthalic acid and 2,6-naphthalenedicarboxylic acid. The liquid crystal polyester may be either a solvent-soluble type or a solvent-insoluble type. The melting point of the liquid crystal polyester is preferably 280 to 340°C.
[0068] An aromatic polyimide is a unit based on a carboxylic dianhydride and a diamine, and has units formed by an imidization reaction between the two compounds (units having an imide structure; hereinafter, also referred to as "imide units"). The aromatic polyimide may be composed only of imide units, or may have imide units and units formed by an amidation reaction between the above-mentioned two compounds (units having an amic acid structure; hereinafter, also referred to as "amic acid units"). On the other hand, an aromatic polyamic acid is an aromatic polyimide precursor consisting of only amic acid units. In such aromatic polyimides or aromatic polyamic acids (hereinafter, these are also collectively referred to as "PIs"), at least one of the carboxylic dianhydride and the diamine, and at least a part of them, is an aromatic compound. The carboxylic dianhydride and the diamine may each be used alone or in combination of two or more. As the carboxylic dianhydride, it is preferable to use at least one aromatic carboxylic dianhydride.
[0069] The PIs preferably contain units based on an aromatic tetracarboxylic acid dianhydride and an aromatic diamine or an aliphatic diamine having a structure in which two or more arylene groups are linked via a linking group. Such PIs tend to have a higher affinity with the F polymer (2), and not only increase the dispersibility of the present dispersion (2), but also tend to improve the adhesiveness of the molded product formed therefrom. In other words, such PIs tend to function as a dispersant in the present dispersion (2) and as an adhesive component in the polymer layer.
[0070] The aromatic tetracarboxylic acid dianhydride is preferably a compound represented by the following formulae AN1 to AN6. [ka]
[0071] The aromatic diamine preferably has a structure in which 2 to 4 arylene groups are linked together, in which case the polarity of the PIs is balanced, making it easier to exhibit the above tendency. The arylene group is preferably a phenylene group, in which a hydrogen atom may be substituted with a hydroxyl group, a fluorine atom or a trifluoromethyl group. The linking group in the aromatic diamine is preferably an ether oxygen atom, a propane-2,2-diyl group, or a perfluoropropane-2,2-diyl group. The linking group may be one type or two or more types, and more preferably an ether oxygen atom is essential. In this case, the PIs are more likely to exhibit the above tendency due to their steric effect.
[0072] The aromatic diamine is preferably a compound represented by the following formulae DA1 to DA6. [ka]
[0073] Examples of the aliphatic diamine include alicyclic diamines (1,3-bis(aminomethyl)cyclohexane, 1,4-bis(aminomethyl)cyclohexane, 1,2-diaminocyclohexane, bis(4-aminocyclohexyl)methane, 2,2-bis(4-aminocyclohexyl)propane, 2,2-bis(4-aminocyclohexyl)hexafluoropropane, isophoronediamine, and norbornanediamine).
[0074] The AR polymer is preferably a liquid crystal polymer (such as the liquid crystal polyesters mentioned above). A molded product formed from the dispersion (2) containing the three components densely is likely to be filled with the three components at a high content and uniformly, and while it has the inherent physical properties of a liquid crystal polymer (mechanical properties such as strength, elasticity, and vibration absorption, and electrical properties such as dielectric properties), it is likely to be suppressed from decreasing in tensile strength and thermal expansion due to its anisotropy. In particular, when the F polymer (2) is the above-mentioned polymer (1) or (2), this tendency is likely to be enhanced due to its adhesion.
[0075] The AR polymer may be a polymer that dissolves in a liquid dispersion medium to form a solution, or may be a polymer that disperses in a liquid dispersion medium to form a dispersion, in which case the D50 of the AR polymer particles is preferably 1 to 40 μm, more preferably 5 to 20 μm. The solubility of the AR polymer at 25° C. is preferably 10 g or less, more preferably 5 g or less, per 100 g of the liquid dispersion medium, and more preferably 1 g or more. When such an AR polymer is used, during preparation or storage of the present dispersion (2) which is carried out at a low temperature range such as room temperature, the AR polymer is partially dispersed in particulate form, and therefore the interparticle interactions between the three components are enhanced, which tends to further improve the dispersion stability and liquid properties of the present dispersion (2).
[0076] The solubility of the AR polymer in the liquid dispersion medium at the boiling point is preferably 20 g or more, more preferably 25 g or more, per 100 g of the liquid dispersion medium. The solubility is preferably 10 g or less. Specifically, when a liquid dispersion medium with a boiling point of more than 150° C. is used, the solubility of the AR polymer at 150° C. is preferably 20 g or more, more preferably 25 g or more, per 100 g of the liquid dispersion medium. If such an AR polymer is used, when the present dispersion (2) is heated in the below-described method for producing a laminate, the AR polymer is highly dissolved and the formation of a matrix with the F polymer (2) is promoted, so that a molded product having excellent electric properties (dielectric constant, dielectric tangent, etc.) can be obtained more efficiently.
[0077] The filler (2) in the present dispersion (2) may be selected depending on the physical properties to be imparted to the molded product formed from the present dispersion (2). The definition and scope of the filler (2), including preferred embodiments, are the same as those of the filler (1). The dielectric tangent of the filler (2) is 0.005 or less, preferably 0.003 or less, and more preferably 0.001 or less. As the filler (2), a silica filler is preferred.
[0078] The shape of the filler (2) may be particulate (granular, spherical), non-particulate (scale, layered), or fibrous. The D50 of the spherical filler (2) is preferably 0.01 to 10 μm, in which case the filler (2) has better dispersibility in the dispersion liquid (2) and is more likely to be distributed uniformly in the molded product. In the fibrous filler (2), the length is the fiber length and the diameter is the fiber diameter. The fiber length is preferably 1 to 10 μm. The fiber diameter is preferably 0.01 to 1 μm. In order to further improve the UV processability of a molded product formed from the present dispersion (2) while highly suppressing the occurrence of warping, the filler (2) is preferably a spherical filler. The definition and scope of the liquid dispersion medium contained in the present dispersion liquid (2), including preferred embodiments, are the same as those of the liquid dispersion medium contained in the present dispersion liquid (1). From the viewpoint of improving dispersion stability, the present dispersion liquid (2) preferably contains a surfactant. The definition and scope of the surfactant contained in the present dispersion (2), including preferred embodiments, are the same as those of the surfactant contained in the present dispersion (1).
[0079] The present dispersion (2) preferably contains water at 50 ppm or more. A small amount of water is expected to increase the affinity between the components contained in the present dispersion (2). The water content is more preferably 100 ppm or more. The upper limit of the water content (ratio) in the present dispersion (2) is preferably 5000 ppm or less, more preferably 1000 ppm or less. The viscosity of the present dispersion (2) is preferably 10,000 mPa·s or less, and more preferably 10 to 1,000 mPa·s. The thixotropy ratio of the present dispersion (2) is preferably 1-2.
[0080] The present dispersion (2) may contain additives to the extent that the effects of the present invention are not impaired. Examples of additives include the same additives that may be contained in the present dispersion (1).
[0081] The content of the F polymer (2) in the present dispersion (2) is more than 5% by mass, preferably 10% by mass or more, more preferably 12% by mass or more. The upper limit of the content of the F polymer (2) is preferably 30% by mass. The content of the AR polymer in the present dispersion (2) is more than 5% by mass, preferably 10% by mass or more, and more preferably 20% by mass or more. The upper limit of the content of the AR polymer is preferably 40% by mass. The content of the filler (2) in the dispersion (2) is more than 5 mass%, preferably 10 mass% or more, more preferably 12 mass% or more. The upper limit of the content of the filler (2) is preferably 30 mass%.
[0082] The total content of the F polymer (2), the AR polymer and the filler (2) in the present dispersion (2) is preferably 30 to 75 mass%, more preferably 30 to 60 mass%, which further improves the dispersion stability of the present dispersion (2) and makes it easier for the properties of the formed molded product based on the three components to be well balanced. Furthermore, the ratio of the content of the F polymer (2) to the content of the AR polymer is preferably 0.25 to 1.0, and the ratio of the content of the filler (2) to the content of the AR polymer is preferably 0.25 to 1.0. The content of the liquid dispersion medium in the present dispersion (2) is preferably from 10 to 70 mass %, more preferably from 30 to 70 mass %. When the present dispersion (2) contains a surfactant, the content thereof is preferably 1 to 15% by mass, in which case the inherent physical properties of the F polymer (2) in the molded product are more likely to be improved.
[0083] Specific embodiments of the present dispersion (2) include an embodiment in which the content of the F polymer (2) is less than the content of the AR polymer, and an embodiment in which the content of the F polymer (2) is greater than the content of the AR polymer. In the former embodiment, the respective contents of the F polymer (2), the AR polymer, the filler (2) and the liquid dispersion medium are preferably, in this order, more than 5% by mass and less than 30% by mass, 10% by mass or more and less than 40% by mass, more than 5% by mass and less than 30% by mass, and more than 0% by mass and less than 80% by mass. In the latter embodiment, the respective contents of the F polymer (2), the AR polymer, the filler (2) and the liquid dispersion medium are preferably, in this order, 10% by mass or more and 30% by mass or less, more than 5% by mass and 20% by mass or less, more than 5% by mass and 30% by mass or less, and 20% by mass or more and less than 80% by mass.
[0084] The present dispersion (2) can be produced by the same method as the above-mentioned method for producing the present dispersion (1) containing an AR polymer.
[0085] The manufacturing method of the present invention (hereinafter also referred to as "this method") is a method in which the present dispersion is applied to the surface of a substrate and heated to form a polymer layer as a molded product, thereby obtaining a laminate having the substrate and the polymer layer in this order. In this method, the present dispersion is applied to the surface of a substrate to form a liquid coating, which is then heated to dry and then baked to form a polymer layer. That is, the polymer layer is a layer containing at least an F polymer and an inorganic filler. When the polymer layer further contains an AR polymer, the AR polymer in the polymer layer may be the AR polymer itself contained in the present dispersion, or may be an AR polymer in which an imidization reaction has progressed due to heating in the formation of the polymer layer. Examples of the coating method include spraying, roll coating, spin coating, gravure coating, microgravure coating, gravure offset, knife coating, kiss coating, bar coating, die coating, fountain-meyer bar, slot die coating, and comma coating.
[0086] The heating temperature (atmosphere temperature) when drying the liquid coating in this method is lower than the melting temperature of the F polymer and may be set according to the boiling point of the solvent contained in the dispersion, and is preferably 90 to 250°C, more preferably 100 to 200°C. The heating time is preferably from 0.1 to 10 minutes, and more preferably from 0.5 to 5 minutes. The heating in drying may be performed in one step, or in two or more steps at different temperatures. Also, a portion of the polar solvent may remain in the dried coating.
[0087] The temperature (atmosphere temperature) when baking the dried coating in this method is equal to or higher than the melting temperature of the F polymer and may be set according to the type of F polymer, and is preferably 300 to 400°C, more preferably 320 to 390°C, and even more preferably 340 to 380°C. The heating time is preferably from 30 seconds to 5 minutes. Furthermore, the heating in the firing may be carried out in one stage, or in two or more stages at different temperatures.
[0088] The heating means for the drying and firing may be a method using a ventilated drying oven or a method using a heat ray irradiation oven such as infrared ray irradiation oven. The atmospheric state at that time may be either normal pressure or reduced pressure. The atmosphere at this time may be any of an oxidizing gas (oxygen gas, etc.) atmosphere, a reducing gas (hydrogen gas, etc.) atmosphere, and an inert gas (helium gas, neon gas, argon gas, nitrogen gas, etc.) atmosphere.
[0089] The substrate in this method is preferably a metal foil or a heat-resistant resin film. The ten-point average roughness of the surface of the metal foil is preferably 0.5 μm or less, more preferably less than 0.1 μm. The ten-point average roughness of the surface of the metal foil is preferably 0.01 μm or more. In this case, the polymer layer and the metal foil are more strongly adhered to each other. For this reason, the dielectric loss tangent (Df) is more likely to decrease significantly in the laminate (polymer layer-coated metal foil) or in a printed circuit board obtained by processing the laminate. Specifically, when the substrate in this method is a metal foil, the dielectric loss tangent of the laminate at a frequency of 10 GHz is preferably 0.0020 or less, more preferably 0.0015 or less, and is preferably 0.0001 or more. Examples of materials for the metal foil include copper, copper alloys, stainless steel, nickel, nickel alloys (including alloy 42), aluminum, aluminum alloys, titanium, and titanium alloys. The metal foil is preferably a rolled copper foil or an electrolytic copper foil.
[0090] The surface of the metal foil may be subjected to an anti-rust treatment (formation of an oxide film such as chromate). The surface of the metal foil may also be treated with a silane coupling agent. The treatment area may be a part of the surface of the metal foil or the entire surface. The thickness of the metal foil is preferably from 0.1 to 20 μm, and more preferably from 0.5 to 10 μm. The thickness of the polymer layer is preferably 1 to 20 μm, more preferably 2 to 18 μm, and further preferably 5 to 15 μm, in which case swelling of the interface between the polymer layer and the metal foil due to heating is suppressed and transmission loss in the high frequency range is significantly improved.
[0091] The metal foil may be a carrier-attached metal foil containing two or more layers of metal foil. The carrier-attached metal foil may be a carrier-attached copper foil consisting of a carrier copper foil (thickness: 10 to 35 μm) and an ultra-thin copper foil (thickness: 2 to 5 μm) laminated on the carrier copper foil via a release layer. By using such a carrier-attached copper foil, it is possible to form a fine pattern by a modified semi-additive (MSAP) process. The release layer is preferably a metal layer containing nickel or chromium, or a multi-layer metal layer in which such metal layers are laminated. A specific example of the metal foil with a carrier is "FUTF-5DAF-2" manufactured by Fukuda Metal Foil & Powder Co., Ltd.
[0092] The heat-resistant resin film is a film containing one or more types of heat-resistant resin, and may be a single-layer film or a multi-layer film. The heat-resistant resin film may have glass fibers, carbon fibers, or the like embedded therein. When the substrate is a heat-resistant resin film, it is preferable to form a polymer layer on both sides of the substrate. In this case, since the polymer layer is formed on both sides of the heat-resistant resin film, the linear expansion coefficient of the laminate is significantly reduced, and warping is unlikely to occur. Specifically, the absolute value of the linear expansion coefficient of the laminate in this embodiment is preferably 1 to 25 ppm / °C.
[0093] Examples of the heat-resistant resin include polyimide, polyarylate, polysulfone, polyarylsulfone, aromatic polyamide, aromatic polyetheramide, polyphenylene sulfide, polyaryletherketone, polyamideimide, liquid crystal polyester, and liquid crystal polyesteramide, and polyimide (particularly, aromatic polyimide) is preferred. In this case, the aromatic rings of the AR polymer in the polymer layer and the aromatic rings of the aromatic polyimide in the heat-resistant resin film (substrate) are stacked, which is believed to improve the adhesion of the polymer layer to the heat-resistant resin film. In addition, in this case, the polymer layer and the heat-resistant resin film are not integrated in a compatible manner, but exist as independent layers. For this reason, the low water absorption of the F polymer complements the high water absorption of the AR polymer, and the laminate is believed to exhibit low water absorption (high water barrier properties).
[0094] In the laminate which is a heat-resistant resin film having polymer layers on both sides, the thickness (total thickness) is preferably 25 μm or more, more preferably 50 μm or more, and is preferably 150 μm or less. In such a configuration, the ratio of the total thickness of the two polymer layers to the thickness of the heat-resistant resin film is preferably 0.5 or more, more preferably 0.8 or more, and is preferably 5 or less. In this case, the properties of the heat-resistant resin film (high yield strength, low plastic deformation property) and the properties of the polymer layer (low water absorbency) are exhibited in a well-balanced manner.
[0095] A preferred embodiment of the laminate produced by this method, in which the substrate is a heat-resistant resin film, is a three-layer film in which the heat-resistant resin film is a polyimide film having a thickness of 20 to 100 μm, and a polymer layer, a polyimide film, and a polymer layer are laminated in this order in direct contact with each other. In this embodiment, the thicknesses of the two polymer layers are the same, and are preferably 15 to 50 μm. The ratio of the total thickness of the two polymer layers to the thickness of the polyimide film is preferably 0.5 to 5. The laminate of this embodiment is most likely to exhibit the effects of the laminate described above.
[0096] The outermost surface of the polymer layer of the laminate may be further subjected to annealing treatment, corona treatment, plasma treatment, ozone treatment, excimer treatment or silane coupling treatment in order to further improve its linear expansion property and adhesiveness. On the outermost surface of the polymer layer of the laminate, another substrate may be further laminated. Other substrates include a heat-resistant resin film, a prepreg which is a precursor of a fiber-reinforced resin plate, a laminate having a heat-resistant resin film layer, and a laminate having a prepreg layer. Note that a prepreg is a sheet-like substrate in which a base material (tow, woven fabric, etc.) of reinforcing fibers (glass fibers, carbon fibers, etc.) is impregnated with a thermosetting resin or a thermoplastic resin. The heat-resistant resin film may be the heat-resistant resin film described above.
[0097] As a method for lamination, a method of hot pressing the laminate and another substrate can be mentioned. When the other substrate is a prepreg, the heat press conditions are preferably a temperature of 120 to 300°C, a vacuum atmosphere of 20 kPa or less, and a press pressure of 0.2 to 10 MPa.When the other substrate is a heat-resistant resin film, the heat press conditions are preferably a temperature of 310 to 400°C. The laminate of the present invention has a polymer layer having excellent electrical properties, and is therefore suitable as a printed circuit board material. Specifically, the laminate of the present invention can be used as a flexible metal-clad laminate or a rigid metal-clad laminate for the manufacture of a printed circuit board, and is particularly suitable for use as a flexible metal-clad laminate for the manufacture of a flexible printed circuit board.
[0098] A printed circuit board is obtained by etching the metal foil of a laminate (polymer-layered metal foil) whose base material is metal foil to form a transmission circuit. Specifically, a printed circuit board can be manufactured by a method of processing a metal foil into a desired transmission circuit by etching the metal foil, or by a method of processing a metal foil into a desired transmission circuit by electrolytic plating (semi-additive method (SAP method), MSAP method, etc.). A printed circuit board manufactured from a polymer-layered metal foil has a transmission circuit formed from the metal foil and a polymer layer in this order. Specific examples of the configuration of a printed circuit board include transmission circuit / polymer layer / prepreg layer and transmission circuit / polymer layer / prepreg layer / polymer layer / transmission circuit. In the manufacture of such a printed circuit board, an interlayer insulating film may be formed on a transmission circuit, a solder resist may be laminated on the transmission circuit, or a coverlay film may be laminated on the transmission circuit. The present dispersion may be used as a material for these interlayer insulating films, solder resists, and coverlay films.
[0099] A specific embodiment of the printed board is a multi-layer printed circuit board in which the printed board is multi-layered. A preferred embodiment of the multilayer printed circuit board is one in which the outermost layer of the multilayer printed circuit board is a polymer layer, and the multilayer printed circuit board has one or more structures in which a metal foil or a transmission circuit, a polymer layer, and a prepreg layer are laminated in this order. The number of the above structures is preferably two or more. A transmission circuit may be further disposed between the polymer layer and the prepreg layer. The multilayer printed circuit board of this embodiment has particularly excellent heat resistance and processability due to the outermost polymer layer. Specifically, even at 288°C, interfacial swelling between the polymer layer and the prepreg layer and interfacial peeling between the metal foil (transmission circuit) and the polymer layer are unlikely to occur. In particular, even when the metal foil forms the transmission circuit, the polymer layer is firmly attached to the metal foil (transmission circuit), so warping is unlikely to occur and the heat resistance and processability are excellent.
[0100] A preferred embodiment of the multilayer printed circuit board is one in which the outermost layer of the multilayer printed circuit board is a prepreg layer, and the multilayer printed circuit board has one or more structures in which a metal foil or a transmission circuit, a polymer layer, and a prepreg layer are laminated in this order. The number of the above structures is preferably two or more. A transmission circuit may be further disposed between the polymer layer and the prepreg layer. The multilayer printed circuit board of this embodiment has excellent heat resistance and processability even if it has a prepreg layer as the outermost layer. Specifically, even at 300°C, interfacial swelling between the polymer layer and the prepreg layer and interfacial peeling between the metal foil (transmission circuit) and the polymer layer are unlikely to occur. In particular, even if the metal foil forms the transmission circuit, the polymer layer is firmly attached to the metal foil (transmission circuit), so that the board is unlikely to warp and has excellent heat resistance and processability. In other words, according to the present invention, printed circuit boards having various configurations can be easily obtained in which the respective interfaces are firmly adhered to each other without the need for various surface treatments, and in which interfacial swelling and peeling due to heating, particularly in the outermost layer, are suppressed.
[0101] The molded product of the present invention (hereinafter also referred to as "the molded product") contains an F polymer and an inorganic filler having an average particle size of more than 0.10 μm, and has a porosity of 5 volume % or less. This molded product can also be said to be a dense (solid) molded product in which inorganic filler is highly filled in the polymer layer having the F polymer as the matrix polymer. A preferred embodiment of the present molded product is one that contains the F polymer (1), the filler (11), and a different filler and has a porosity of 5% by volume or less. In such an embodiment, the voids in the polymer layer are filled with the different filler, making it easier to further reduce the porosity. The molded product may be in the form of a layer, a film, a plate, or a block.
[0102] The definitions and ranges of the F polymer and inorganic filler in the present molded product, including preferred embodiments, are the same as those in the present dispersion (1) and the present dispersion (2). In the present molded product, the content of the F polymer and the content of the inorganic filler are preferably 30-70% by mass and 30-70% by mass, respectively. In the present molded product, the mass ratio of the content of the inorganic filler to the content of the F polymer is preferably 1.5 or less, more preferably 1 or less. In other words, the content of the inorganic filler in the present molded product is preferably equal to or less than the content of the F polymer. The ratio is preferably 0.1 or more, more preferably 0.5 or more. When the molded article contains a different filler, the mass ratio of the content of the different filler to the content of the filler (11) is preferably 0.1-1. When the molded product contains other resins, the content of the other resins is preferably 1 to 10% by mass. The definition and range of the other resins, including their preferred embodiments, are the same as those of the other resins in the dispersion liquid (1). The other resins are preferably aromatic polymers, more preferably aromatic polyimides. When the other resins are aromatic polyimides, the mass ratio of the aromatic polyimide content to the F polymer content is preferably 1.0 or less, more preferably 0.1 to 0.7.
[0103] The voids in the present molded product are preferably present at the interface between the F polymer and the inorganic filler. The porosity of the molded product is 5% by volume or less, preferably 4% by volume or less, and more preferably 3% by volume or less.The porosity of the molded product is preferably 0.01% by volume or more, and more preferably 0.1% by volume or more. If the arrangement of the voids and the porosity in the present molded product are in the above-mentioned state and range, respectively, the voids make it easy for the physical properties of the F polymer and the inorganic filler to be significantly expressed in the molded product. Specifically, it is easy to form a molded product that has high physical properties due to the F polymer (heat resistance, electrical properties, etc.) and high physical properties due to the inorganic filler (low linear expansion coefficient, dielectric properties, etc.), and such a molded product can be suitably used as a printed circuit board material.
[0104] The present molded product is preferably formed from the present dispersion. The method for forming the present molded product from the present dispersion includes the above-mentioned present method. In this case, the present molded product, which is a polymer layer, can be easily formed on the surface of the substrate. The definition and scope of the laminate having the present molded product on the surface of the substrate, including preferred embodiments, are the same as those of the laminate in the present method. EXAMPLES
[0105] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these. 1. Example of Dispersion and Molded Product Production (Part 1) 1-1. Preparation of each ingredient [powder] Powder 11: Powder consisting of polymer 11 (melting temperature: 300°C) containing TFE units, NAH units and PPVE units in the order of 98.0 mol%, 0.1 mol% and 1.9 mol% and having an oxygen-containing polar group (D50: 2.0 μm, 98% particle size: 4.9 μm) Powder 12: Powder consisting of polymer 12 (melting temperature: 305°C) containing 98.7 mol% TFE units and 1.3 mol% PPVE units, in that order, and having no oxygen-containing polar group (D50: 2.4 μm, 98% particle size: 5.8 μm) Powder 13: Powder made of polymer 12 and containing particles with a particle diameter of 10 μm or more (D50: 2.6 μm, D98: 10.5 μm) Powder 14: Powder made of PTFE (D50: 2.4 μm, 98% particle size: 6.3 μm) The melt viscosity of polymer 11 and polymer 12 at 380°C was 1×10 6 It is less than Pa·s.
[0106] [Filler] Filler 11: Made of silicon oxide, with a specific surface area of 7 m 2 / g, nearly spherical silica filler (D50: 0.4 μm, 98% particle size: 1.0 μm) Filler 12: Made of silicon oxide, specific surface area 5m 2 / g, nearly spherical silica filler (D50: 0.9 μm, 98% particle size: 3.1 μm) Filler 13: Made of silicon oxide, with a specific surface area of 14 m 2 / g, nearly spherical silica filler (D50: 0.08 μm, 98% particle size: 0.2 μm) Filler 14: Scaly steatite filler (D50: 4.8 μm, average major axis: 5.7 μm, average minor axis: 0.3 μm, aspect ratio: 20, Nippon Talc Co., Ltd. "BST") Filler 15: Made of silicon oxide, specific surface area 3m 2 / g, nearly spherical silica filler (D50: 1.5 μm, 98% particle size: 3.3 μm) The surface of each filler was treated with vinyltrimethoxysilane.
[0107] [Non-aqueous solvent] NMP: N-methyl-2-pyrrolidone [Surfactants] Surfactant 11: CH 2 =C(CH 3 )C(O)OCH 2 CH 2 (CF 2 ) 6 F and CH 2 =C(CH 3 )C(O)(OCH 2 CH 2 ) 23 A nonionic polymer having an alcoholic hydroxyl group and an oxyalkylene group, which is a copolymer with OH and has a fluorine content of 35% by mass. [Varnishes of other polymers] Varnish 11: Thermoplastic polyimide (PI11) dissolved in NMP
[0108] 1-2. Example of dispersion liquid production (Example 1-1) First, the powder 11, the varnish 11, the surfactant 11, and NMP were put into a pot, and then zirconia balls were put into the pot. Then, the pot was rolled at 150 rpm for 1 hour to prepare a liquid composition. Next, the Filler 11, the Surfactant 11, and NMP were charged into the pot, and then the zirconia balls were charged into the pot. Thereafter, the pot was rolled at 150 rpm for 1 hour to prepare a liquid composition. Then, both liquid compositions were poured into a pot, and zirconia balls were poured into the pot. The pot was then rolled at 150 rpm for 1 hour to obtain Dispersion 1-1 (viscosity: 400 mPa s) containing Powder 11 (11 parts by mass), Filler 11 (11 parts by mass), PI11 (7 parts by mass), Surfactant 11 (4 parts by mass), and NMP (67 parts by mass).
[0109] (Example 1-2) Dispersion 1-2 containing Powder 11 (7 parts by mass), Powder 14 (4 parts by mass), Filler 11 (11 parts by mass), PI11 (7 parts by mass), Surfactant 11 (4 parts by mass) and NMP (67 parts by mass) was obtained in the same manner as in Example 1-1, except that Powder 14 was used in addition to Powder 11. (Example 1-3) Dispersion 1-3 containing Powder 12 (11 parts by mass), Filler 11 (11 parts by mass), PI11 (7 parts by mass), Surfactant 1 (4 parts by mass) and NMP (67 parts by mass) was obtained in the same manner as in Example 1-1, except that Powder 12 was used instead of Powder 11.
[0110] (Example 1-4) First, the powder 12, the varnish 11, the surfactant 11, and NMP were put into a pot, and then zirconia balls were put into the pot. Then, the pot was rolled at 150 rpm for 1 hour to obtain a liquid composition. Next, Filler 11 was added to this liquid composition, and the pot was rolled at 150 rpm for 1 hour to obtain Dispersion 1-4 containing Powder 12 (11 parts by weight), Filler 11 (11 parts by weight), PI11 (7 parts by weight), Surfactant 11 (4 parts by weight) and NMP (67 parts by weight). (Example 1-5) Dispersion 1-5 was obtained in the same manner as in Example 1-1, except that Powder 13 was used instead of Powder 11.
[0111] (Example 1-6) A dispersion 1-6 was obtained in the same manner as in Example 1-1, except that Powder 12 was used instead of Powder 11 and Filler 12 was used instead of Filler 11. (Example 1-7) Dispersion 17 was obtained in the same manner as in Example 11, except that Powder 14 was used instead of Powder 11. (Example 1-8) Except for using Powder 12 instead of Powder 11 and Filler 13 instead of Filler 11, the same procedure as in Example 1-1 was carried out to obtain Dispersion 1-8.
[0112] (Example 1-9) A dispersion 1-9 containing powder 14 (11 parts by mass), filler 11 (3 parts by mass), PI11 (7 parts by mass), surfactant 11 (4 parts by mass) and NMP (75 parts by mass) was obtained in the same manner as in Example 1-1, except that powder 14 was used instead of powder 11 and the amounts of filler 11 and NMP used were changed. (Example 1-10) A dispersion 1-10 containing powder 11 (11 parts by mass), filler 11 (11 parts by mass), PI11 (1 part by mass), surfactant 11 (4 parts by mass) and NMP (73 parts by mass) was obtained in the same manner as in Example 1-1, except that the amounts of varnish 11 and NMP used were changed. (Example 1-11) A dispersion 1-11 was obtained in the same manner as in Example 1-1, except that Filler 14 was used instead of Filler 11. (Example 1-12) Dispersion 1-12 was obtained in the same manner as in Example 1-1, except that 3 parts by mass of Filler 11 and 8 parts by mass of Filler 15 were used instead of 11 parts by mass of Filler 11. The types of powder, polymer, and filler in each dispersion are summarized in Table 1 below.
[0113] [Table 1]
[0114] 1-3. Example of laminate manufacturing Dispersion 1-1 was applied to the surface of a long copper foil (thickness: 18 μm) using a bar coater to form a wet film. The metal foil on which the wet film was formed was then passed through a drying oven at 120° C. for 5 minutes and dried by heating to obtain a dry film. The dry film was then heated at 380° C. for 3 minutes in a nitrogen oven. This produced a laminate 1-1 having a metal foil and a polymer layer (thickness: 5 μm) as a molded product containing a molten and fired product of powder 1 and filler 1 on its surface.
[0115] Laminates 1-2 to 1-12 were obtained in the same manner as laminate 1-1, except that dispersions 1-2 to 1-12 were used instead of dispersion 1-1. The porosity of the polymer layer of each of laminates 1-1 and 1-10 was 5% or less, and the porosity of the polymer layer of laminate 1-1 was lower than that of laminate 1-10.
[0116] 1-4.Evaluation 1-4-1. Dispersion stability of dispersion liquid Each of Dispersions 1-1 to 1-10 was stored in a container at 25° C. for one week, after which its dispersibility was visually confirmed and the dispersion stability was evaluated according to the following criteria. [Dispersion stability] ⊚: No aggregates were visible. ◯: Fine aggregates were visible on the side walls of the container. They were uniformly redispersed when lightly stirred. △: Settling of aggregates is visible at the bottom of the container. When sheared and stirred, the aggregates are uniformly redispersed. ×: Settling of aggregates was visible at the bottom of the container. Redispersion was difficult even with stirring under shear.
[0117] 1-4-2. Surface smoothness of polymer layer (molded product) The surface of the polymer layer of each of the laminates 1-1 to 1-10 was visually inspected and the surface smoothness was evaluated according to the following criteria. ◯: The entire surface of the polymer layer is smooth. Δ: Missing polymer or filler is visible at the surface edge of the polymer layer. ×: Irregularities due to missing polymer or filler are visible over the entire surface of the polymer layer.
[0118] 1-4-3. Linear expansion coefficient of polymer layer (molded product) For each of the laminates 1-1, 1-2, 1-3, and 1-9, the copper foil was removed by etching with an aqueous solution of ferric chloride to prepare a single polymer layer, and a square test piece measuring 180 mm square was cut out. The linear expansion coefficient of the test piece was measured in the range of 25 to 260°C according to the measurement method specified in JIS C 6471:1995. ○: Less than 30 ppm / ℃. ×: More than 30 ppm / ℃.
[0119] 1-4-4. Dielectric tangent of polymer layer (molded product) For each of the laminates 1-1, 1-2, 1-3 and 1-9, the copper foil was removed by etching with an aqueous ferric chloride solution to produce a single polymer layer, and the dielectric tangent of the polymer layer (measurement frequency: 10 GHz) was measured using the SPDR (split post dielectric resonance) method. ⊚: The dielectric tangent is less than 0.0010. ○: The dielectric tangent is 0.0010 or more and 0.0019 or less. △: The dielectric tangent is more than 0.0019 and not more than 0.0025. ×: The dielectric tangent is more than 0.0025. The evaluation results are summarized in Table 2 below.
[0120] [Table 2]
[0121] Dispersion 1-11 was evaluated in the same manner as the above dispersion, and the dispersion stability was evaluated as "◎". Furthermore, laminate 1-11 was evaluated in the same manner as the above laminate, and the surface smoothness was evaluated as "◯", the linear expansion coefficient was 26 ppm / ℃, the dielectric constant was 2.2, and the dielectric loss tangent was 0.0015. The porosity of the polymer layer of laminate 1-11 was 5% or less, and the porosity of the polymer layer of laminate 1-1 was lower than that of laminate 1-11. The dielectric constant was measured using the same device and conditions as the dielectric loss tangent.
[0122] Dispersion 1-12 was evaluated in the same manner as the above dispersion, and the dispersion stability was evaluated as "A". Furthermore, laminate 1-12 was evaluated in the same manner as the above laminate, and the surface smoothness was evaluated as "A", the linear expansion coefficient was 25 ppm / °C, and the dielectric constant was 2.2. Furthermore, the porosity of the polymer layer of laminate 1-12 was 5% or less, which was lower than the porosity of the polymer layer of laminate 1-1.
[0123] 2. Example of Dispersion and Molded Product Production (Part 2) 2-1. Preparation of each ingredient [powder] Powder 21: Powder of low molecular weight PTFE (number average molecular weight: 20,000) (D50: 2 μm) Powder 22: Powder (D50: 2 μm) of a polymer (melting temperature: 305°C) containing TFE units and PPVE units at 97.5 mol% and 2.5 mol%, respectively, and having no polar functional groups. Powder 23: Powder (D50: 2 μm) of a polymer (melting temperature: 300°C) containing TFE units, NAH units, and PPVE units at 98.0 mol%, 0.1 mol%, and 1.9 mol%, respectively, and having polar functional groups. The melt viscosity of each polymer at 380°C is 1×10 6 It is less than Pa·s.
[0124] [AR polymer] ·PI21 precursor solution (Polyamic acid solution 21) First, dimethylacetamide (DMAc), 2.3 g of paraphenylenediamine (p-PDA), 1.5 g of 4,4'-diamino-2,2'-bis(trifluoromethyl)biphenyl (TFMB), and 0.7 g of 1,3-bis(4-aminophenoxy)benzene (TPE-R) were added to a reaction vessel, and the mixture was stirred at 25°C to obtain a solution. Next, 6.4 g of bis(1,3-dioxo-1,3-dihydroisobenzofuran-5-carboxylic acid) 1,4-phenylene (TAHQ) and 4.1 g of s-3,3',4,4'-biphenyltetracarboxylic dianhydride (s-BPDA) were gradually added to the resulting solution, which was then stirred at 25°C for 3 hours to obtain a PI21 precursor solution.
[0125] Next, the PI21 precursor solution was applied to the roughened surface of the copper foil using a bar coater so that the thickness of the resin film after imidization was 25 μm, and then dried at 130 ° C for 10 minutes. The copper foil was then cooled to 25 ° C, and then heated stepwise to 360 ° C (physical temperature) to obtain a PI21 film. After being held at 360 ° C for 2 hours, it was naturally cooled to 25 ° C, and the copper foil was removed by etching to prepare a film alone. The dielectric tangent of the film was measured and found to be 0.0037.
[0126] ·PI22 precursor solution (Polyamic acid solution 22) A PI22 precursor solution was prepared in the same manner as the PI21 precursor solution, except that only p-PDA and s-BPDA were used as monomers. A resin film containing PI22 was formed in the same manner as the PI21 precursor solution, and its dielectric loss tangent was measured to be 0.0075.
[0127] PES21 (liquid crystalline aromatic polyester 21) First, 84.7 g of 2-hydroxy-6-naphthoic acid, 41.6 g of 4-hydroxyacetanilide, 5.8 g of isophthalic acid, 62.0 g of diphenyl ether-4,4'-dicarboxylic acid, and 81.7 g of acetic anhydride were charged into a reactor under a nitrogen atmosphere. Next, the temperature inside the reactor was raised to 150°C over 15 minutes and refluxed for 3 hours. Then, while distilling off the by-product acetic acid and unreacted acetic anhydride, the temperature was raised to 320°C over 170 minutes, and the reaction was continued until an increase in torque was observed. The contents of the reactor were then collected, cooled to 25°C, pulverized, and then held at 240°C for 3 hours under a nitrogen atmosphere to undergo a solid-state reaction to obtain a powder of PES1. 100 g of PES1 was added to N-methyl-2-pyrrolidone (NMP) and dissolved by heating to 140°C to obtain a brown, transparent solution of PES21. The PES21 solution was cast onto copper foil using a film applicator, then heated to 100°C, and then further heated from 250°C to 350°C over 12 minutes, and then allowed to cool to form a film. The copper foil was removed by etching to obtain a 25μm-thick PES21 film, and its dielectric tangent was measured to be 0.0027.
[0128] PES22 (liquid crystalline aromatic polyester 22) PES22 obtained by reacting 2-hydroxy-6-naphthoic acid, 4,4'-dihydroxybiphenyl, terephthalic acid, and 2,6-naphthalenedicarboxylic acid in the following order at ratios of 60 mol%, 20 mol%, 15.5 mol%, and 4.5 mol% was pulverized to obtain PES22 powder (D50: 16 μm). 100 g of PES22 powder was added to N-methyl-2-pyrrolidone (NMP) to obtain a PES22 dispersion in which the PES22 powder was dispersed. The PES22 dispersion was cast onto copper foil using a film applicator, then heated to 100°C, and then further heated from 250°C to 350°C over 12 minutes, after which it was allowed to cool to form a film. The copper foil was removed by etching to obtain a 25μm-thick PES22 film, and its dielectric tangent was measured to be 0.0007. The solubility of PES22 in DMAc (boiling point: 165° C.) was 10 g or less at 25° C. and 20 g or more at 150° C. In addition, the PES22 used was in powder form.
[0129] ·PPE21 (Polyphenylene Ether 21) A PPE21 solution was prepared by dissolving polyphenylene ether resin (SABIC, "Noryl1640") in toluene. The PPE21 solution was cast onto the surface of copper foil using a film applicator, then heated to 100°C and allowed to cool to form a PPE21 film. The copper foil was removed by etching to obtain a 25 μm-thick PPE21 film, and its dielectric tangent was measured to be 0.0040.
[0130] [Inorganic filler] Filler 21: Silica filler surface-treated with an aminosilane coupling agent (average particle size: 5 μm; Denka, "FB-7SDC") [Surfactants] Surfactant 21:CH 2 =C(CH 3)C(O)OCH 2 CH 2 (CF 2 ) 6 F and CH 2 =C(CH 3 )C(O)(OCH 2 CH 2 ) 23 Copolymer of OH
[0131] 2-2. Preparation of dispersion liquid In a pot, DMAc, powder 21, filler 21, and surfactant 21 were added to the PI21 precursor solution and mixed, and the mixture was stirred at 2000 rpm for 1 hour using a homodisper to obtain dispersion 2-1 containing 25% by mass of PI21 precursor, 13% by mass of powder 21, 13% by mass of filler 21, and 1% by mass of surfactant 21. Dispersions 2-2 to 2-9 were obtained in the same manner as Dispersion 2-1, except that the types or amounts of the powder, AR polymer, and non-aqueous dispersion medium were changed as shown in Table 3 below.
[0132] [Table 3]
[0133] 2-3. Evaluation of redispersibility of dispersion liquid Each dispersion was left to stand for one month, allowed to settle, and then shaken at 100 rpm for one hour using a rotary shaker (manufactured by Yamato Scientific Co., Ltd., "SA-320") After that, the dispersion was filtered through a 100 μm mesh and evaluated according to the following criteria. Good (Acceptable): No agglomerates in the mesh. × (Fail): Aggregates are observed on the mesh. The results are shown in Table 4 below.
[0134] [Table 4]
[0135] 2-4. Preparation of resin film (molded object) Using each dispersion, a resin film having a thickness of 100 μm was produced under the same conditions as those for producing the resin film described above. 2-5. Evaluation of resin film (molded product) 2-5-1. Linear expansion coefficient Each resin film was left to stand for 24 hours or more in an atmosphere of 23°C and 50% RH, and then a sample with a width of 5 mm and a length of 15 mm was cut out. The sample was then heated at a load of 5 N and a heating rate of 2°C / min using a thermomechanical analyzer (Shimadzu Corporation, "TMA-60"). The dimensional change of the sample from 30°C to 200°C was then measured, and the linear expansion coefficient (ppm / °C) was calculated.
[0136] 2-5-2. Folding resistance The folding endurance (MIT) of each resin film was measured in accordance with JIS P 8115. The equipment used was an MIT folding fatigue tester, D-type (manufactured by Toyo Seiki Seisakusho), with a test speed of 175 cpm, a bending angle of 135°, a load of 1 kg, and a clamp radius of 0.38 mm. The number of times each resin film broke was then measured. 2-5-3.Dielectric tangent Each resin film was left to stand for 24 hours or more in an atmosphere of 23° C. and 50% RH. Thereafter, the dielectric loss tangent of each resin film was measured using a network analyzer according to the SPDR method (10 GHz). The results are shown in Table 5 below.
[0137] [Table 5] [Industrial Applicability]
[0138] The non-aqueous dispersion of the present invention has excellent dispersion stability and can be used to produce molded products (films, impregnated products such as prepregs, laminates, etc.) that have the physical properties based on the F polymer and the characteristics based on the inorganic filler. The molded product of the present invention is useful as antenna parts, printed circuit boards, aircraft parts, automobile parts, sports equipment, food industry products, paints, cosmetics, etc., and specifically, it is useful as electric wire covering materials (aircraft electric wires, etc.), electrical insulating tapes, insulating tapes for oil drilling, materials for printed circuit boards, separation membranes (microfiltration membranes, ultrafiltration membranes, reverse osmosis membranes, ion exchange membranes, dialysis membranes, gas separation membranes, etc.), electrode binders (for lithium secondary batteries, for fuel cells, etc.), copy rolls, furniture, automobile dashboards, covers for home appliances, etc., sliding members (load bearings, sliding shafts, valves, bearings, gears, cams, belt conveyors, food transport belts, etc.), tools (shovels, files, saws, saws, etc.), boilers, hoppers, pipes, ovens, baking molds, chutes, dies, toilets, and container covering materials.
Claims
1. Melt viscosity at 380°C is 1 x 10 6 The powder contains a tetrafluoroethylene-based polymer having an average particle size of 10 μm or less and a viscosity of Pa·s or less, an aromatic polymer, and an inorganic filler, wherein the content of the tetrafluoroethylene-based polymer, the content of the aromatic polymer, and the content of the inorganic filler are each more than 5 mass%, the inorganic filler is a filler containing at least one inorganic compound selected from the group consisting of boron nitride, aluminum nitride, beryllium oxide, silicon oxide, cerium oxide, aluminum oxide, magnesium oxide, zinc oxide, and titanium oxide; the total content of the tetrafluoroethylene-based polymer, the aromatic polymer, and the inorganic filler is 30 to 75% by mass, the ratio of the content of the tetrafluoroethylene-based polymer to the content of the aromatic polymer is 0.25 to 1.0; The non-aqueous dispersion has a ratio of the content of the inorganic filler to the content of the aromatic polymer of 0.25 to 1.
0.
2. 2. The non-aqueous dispersion according to claim 1, wherein the aromatic polymer is an aromatic polyimide, an aromatic polyamic acid, an aromatic polyester, or a polyphenylene ether.
3. The non-aqueous dispersion according to claim 1 or 2, wherein the aromatic polymer is a liquid crystal polymer.
4. The non-aqueous dispersion according to any one of claims 1 to 3, which contains at least one non-aqueous dispersion medium selected from the group consisting of aromatic hydrocarbons, amides, ketones and esters.
5. A method for producing a laminate, comprising applying the nonaqueous dispersion according to any one of claims 1 to 4 to a surface of a substrate, heating the resulting substrate, forming a polymer layer, and obtaining a laminate having the substrate and the polymer layer in this order.
Citation Information
Patent Citations
Fluoropolymer nonaqueous dispersion
JP2011225710A
Resin composition, low dielectric constant resin sheet, prepreg, metal foil-clad laminate, high frequency circuit board and multilayer wire board
JP2016166347A
Non-aqueous dispersion of polytetrafluoroethylene
JP2016194017A
Resin composition
JP2017165876A
Resin powder, method for producing same, complex, molded article, method for producing ceramic molded article, metal laminated plate, print substrate, and prepreg