Urethane (meth)acrylate polymer

The urethane (meth)acrylate polymer with a bisbenzotriazolylphenol skeleton incorporated via a urethane bond addresses the issue of ultraviolet absorber bleed-out, enhancing weather resistance and transparency in curable compositions, and providing a coating film with superior scratch resistance.

JP7559806B2Active Publication Date: 2024-10-02MITSUBISHI CHEM CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2022108317
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2017-03-17
Filing Date
2022-07-05
Publication Date
2024-10-02
Estimated Expiration
2038-03-16

AI Technical Summary

Technical Problem

Existing curable compositions suffer from ultraviolet absorber bleed-out, leading to poor weather resistance and transparency due to the ultraviolet absorber not being incorporated into the polymer skeleton or being incorporated via unstable ester bonds, which cause hydrolysis.

Method used

A urethane (meth)acrylate polymer with a bisbenzotriazolylphenol skeleton incorporated via a chemically stable urethane bond, preventing bleed-out and enhancing weather resistance and transparency.

Benefits of technology

The urethane (meth)acrylate polymer prevents ultraviolet absorber bleed-out, resulting in improved weather resistance and transparency, with a curable composition that forms a coating film with excellent scratch resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007559806000001
    Figure 0007559806000001
  • Figure 0007559806000002
    Figure 0007559806000002
  • Figure 0007559806000003
    Figure 0007559806000003
Patent Text Reader

Abstract

To provide a urethane (meth)acrylate polymer that can prevent the bleeding out of an ultraviolet absorber and can provide a coating film that is excellent in weather resistance, scratch resistance, and transparency. [Solution] A urethane (meth)acrylate polymer having a chemical structure represented by the following formula (1) and a polyol structure such as ethylene glycol. TIFF2022133387000021.tif47166 [wherein A is a single bond, or a methylene group which may have a substituent, an alkylene group, an -O- group, an -NH- group, an -S- group, an -SO- group or an -SO2- group, R 1 , R 2 , R 3 and R 4 are independently a hydrogen atom, an alkyl group, an alkoxy group, an aryl group, or a halogen atom; R 5 and R 6 each independently represents an alkylene group, an alkoxylene group, or an arylene group.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a urethane (meth)acrylate polymer and a curable composition containing the same, which have excellent transparency, weather resistance, and scratch resistance after the curable composition is applied to a substrate and cured. The present invention also relates to a cured product, a laminate, and a decorative film using the urethane (meth)acrylate polymer and the curable composition. [Background technology]

[0002] Radical polymerization type curable compositions cure in a short time when irradiated with active energy rays, and can provide films and molded articles that are excellent in chemical resistance, scratch resistance, weather resistance, heat resistance, etc., and are therefore used in coating compositions that cover the surfaces of automobiles, home appliances, woodworking products, plastic molded articles, transfer materials, etc.

[0003] For example, Patent Document 1 discloses a coating composition to which a bisbenzotriazolylphenol compound is added as an ultraviolet absorber.

[0004] Patent Document 2 discloses a coating composition in which an ultraviolet absorber having a specific structure is incorporated into the polymer skeleton.

[0005] Patent Document 3 discloses a curable resin composition in which a bisbenzotriazolylphenol-based ultraviolet absorber is incorporated into the polymer skeleton via an ester bond. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2000-017204 A [Patent Document 2] JP 2000-053913 A [Patent Document 3] JP 2000-109652 A Summary of the Invention [Problem to be solved by the invention]

[0007] However, in the coating composition described in Patent Document 1, the ultraviolet absorber is not incorporated into the polymer backbone, and therefore the ultraviolet absorber bleeds out from the coating film, resulting in insufficient transparency and weather resistance of the coating film. The coating composition described in Patent Document 2 has insufficient weather resistance because the ultraviolet absorbing performance of the ultraviolet absorbent is insufficient. In the curable composition described in Patent Document 3, since the ultraviolet absorber is incorporated into the polymer skeleton via an ester bond, hydrolysis originating from the ester bond occurs, causing the ultraviolet absorber to bleed out, and the weather resistance is insufficient.

[0008] The present invention solves the above-mentioned problems, and has an object to provide a urethane (meth)acrylate polymer that can prevent bleed-out of an ultraviolet absorber and give a coating film that is excellent in weather resistance, scratch resistance and transparency, and a curable composition containing the same. [Means for solving the problem]

[0009] That is, the above object of the present invention can be achieved by the following means [1] to

[18] : [1] A urethane (meth)acrylate polymer having a chemical structure represented by the following formula (1). [ka] [In the formula, A represents a single bond, or a methylene group, an alkylene group, an -O- group, an -NH- group, an -S- group, an -SO- group, or an -SO2- group which may have a substituent. 1 , R 2 , R 3 and R 4 R independently represents a hydrogen atom, an alkyl group, an alkoxy group, an aryl group, or a halogen atom. 5 and R 6 each independently represents an alkylene group, an alkoxylene group, or an arylene group. [2] The urethane (meth)acrylate polymer according to [1], wherein the formula (1) is the following formula (2): [ka] [3] The urethane (meth)acrylate polymer according to [1] or [2], having a chemical structure represented by the following formula (3): [ka] (In formula (3), X 1 is an aliphatic structure having a molecular weight of 500 or less, and n is an integer of 2 to 8. ) [4] The urethane (meth)acrylate polymer according to [3], which contains, as the chemical structure represented by the formula (3), at least one of a chemical structure represented by the following formula (4-1) and a chemical structure represented by the following formula (4-2): [ka] (In formulas (4-1) and (4-2), X 1 is X in formula (3). 1 is equivalent to [5] Any of [1] to [4], having a weight average molecular weight (Mw) of 500 to 30,000. The urethane (meth)acrylate polymer according to claim 1. [6] The urethane (meth)acrylate polymer according to any one of [1] to [5], wherein the ratio of the chemical structure represented by formula (1) in the urethane (meth)acrylate polymer is 5 to 60% by weight. [7] A curable composition comprising the urethane (meth)acrylate polymer according to any one of [1] to [6] and an organic solvent. [8] The curable composition according to [7], wherein the organic solvent has a solubility parameter of 8.0 to 11.5. [9] The curable composition according to [7] or [8], wherein the curable composition has a solid content concentration of 5 to 90% by weight.

[10] The curable composition according to any one of [7] to [9], wherein the ratio of the chemical structure represented by formula (1) in the polymerization components of the curable composition is 5 to 60% by weight.

[11] A cured product of the curable composition according to any one of [7] to

[10] .

[12] A laminate having a substrate and a cured product of the curable composition according to any one of [7] to

[10] above.

[13] A headlamp lens having a substrate on which a cured product of the curable composition according to

[11] is formed.

[14] A glazing material having a substrate and a cured product of the curable composition described in

[11] on the substrate.

[15] A decorative film having a substrate and a cured product of the curable composition according to

[11] on the substrate.

[16] A method for producing a film, comprising the steps of: applying the urethane (meth)acrylate polymer according to any one of [1] to [6] or the curable composition according to any one of [7] to

[10] onto a substrate; irradiating the urethane (meth)acrylate polymer or the curable composition with active energy rays to obtain a laminate having a cured product; and stretching the laminate.

[17] A method for producing a urethane (meth)acrylate polymer, comprising reacting the following compound (A) with the following compound (B) to obtain a precursor of a urethane polymer, and then reacting the precursor with the following compound (C): Compound (A): Polyisocyanate Compound (B): A polyol represented by the following formula (5): [ka] [In the formula, A represents a single bond, or a methylene group, an alkylene group, an -O- group, an -NH- group, an -S- group, an -SO- group, or an -SO2- group which may have a substituent. 1 , R 2 , R 3 and R 4 each independently represents a hydrogen atom, an alkyl group, an alkoxy group, an aryl group, or a halogen atom. R 5 and R 6 each independently represents an alkylene group, an alkoxylene group, or an arylene group. Compound (C): A compound having a hydroxyl group and a (meth)acryloyl group

[18] A method for producing a urethane (meth)acrylate polymer according to

[17] , comprising reacting the following compound (D) in addition to the compound (A) and the compound (B) to obtain a precursor of a urethane polymer, and then reacting the precursor with the compound (C). Compound (D): Aliphatic polyol having a molecular weight of 500 or less Effect of the Invention

[0010] According to the present invention, the bleeding out of the ultraviolet absorbing agent is prevented, and the weather resistance, scratch resistance, and transparency are improved. The present invention provides a urethane (meth)acrylate polymer capable of forming an excellent coating film, and a curable composition containing the same. It is also possible to provide a laminate and a decorative film having a layer made of the cured product on the surface thereof. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] In the present invention, "(meth)acrylate" is a general term for acrylate and methacrylate, and means either or both of acrylate and methacrylate, and the same applies to "(meth)acryloyl" and "(meth)acryl".

[0012] [Urethane (meth)acrylate polymer] The urethane (meth)acrylate polymer of the present invention has a chemical structure represented by the following formula (1). [ka]

[0013] In formula (1), A is a single bond or a methylene group, an alkylene group, an -O- group, an -NH- group, an -S- group, an -SO- group, or an -SO2- group, which may have a substituent. From the viewpoints of transparency of the cured product containing the urethane (meth)acrylate polymer of the present invention and prevention of bleeding out of the ultraviolet absorbent from the cured product, a methylene group or an alkylene group is preferred, and a methylene group is more preferred.

[0014] In formula (1), R1 , R 2 , R 3 and R 4 may be independently any one of a hydrogen atom, an alkyl group, an alkoxy group, an aryl group, and a halogen atom. From the viewpoints of the transparency of the cured product of the urethane (meth)acrylate polymer or the curable composition of the present invention and of preventing the bleed-out of the bisbenzotriazolylphenol skeleton from the cured product, a hydrogen atom, an alkyl group, and an alkoxy group are preferred.

[0015] In formula (1), R 5 and R 6 may be the same or different and may be any one of an alkylene group, an alkoxylene group, and an arylene group. From the viewpoints of transparency of the cured product of the urethane (meth)acrylate polymer or the curable composition of the present invention and prevention of bleeding out of the bisbenzotriazolylphenol skeleton from the cured product, an alkylene group or a methylene group is preferred.

[0016] The urethane (meth)acrylate polymer of the present invention has a bisbenzotriazolylphenol skeleton that acts as an ultraviolet absorber incorporated in the molecular chain of the polymer via a chemically stable urethane bond. The bisbenzotriazolylphenol skeleton has a structure in which benzotriazolylphenol is dimerized, and therefore has high ultraviolet absorbing power per unit weight, and can impart high weather resistance with a small amount. Furthermore, in the present invention, since the bisbenzotriazolylphenol skeleton is incorporated via a urethane bond, the bisbenzotriazolylphenol skeleton is less likely to bleed out due to hydrolysis or the like, and therefore the composition has excellent long-term weather resistance.

[0017] The urethane (meth)acrylate polymer of the present invention and the curable composition using the same are cured. From the viewpoints of transparency of the resulting cured film and prevention of bleeding out of the bisbenzotriazolylphenol skeleton from the cured product, the chemical structure represented by formula (1) is preferably a chemical structure represented by the following formula (2). [ka]

[0018] In order to obtain a cured product having excellent transparency, weather resistance, and scratch resistance, the ratio of the chemical structure represented by the formula (1) in the urethane (meth)acrylate polymer of the present invention is preferably 5% by weight or more, more preferably 20% by weight or more, and is preferably 60% by weight or less, more preferably 35% by weight or less.

[0019] The urethane (meth)acrylate polymer of the present invention preferably has a chemical structure represented by the following formula (3).

[0020] The urethane (meth)acrylate polymer of the present invention contains at least one of a chemical structure represented by the following formula (4-1) and a chemical structure represented by the following formula (4-2) as the chemical structure represented by formula (3), thereby making it possible to improve the transparency of the cured product, and to improve the solubility of the urethane (meth)acrylate polymer in an organic solvent when the urethane (meth)acrylate polymer having a bisbenzotriazolylphenol skeleton is made into a curable composition. [ka]

[0021] In formula (3), X 1 is not particularly limited as long as it has an aliphatic structure with a molecular weight of 500 or less. However, it is preferably an aliphatic structure having a molecular weight of 400 or less, and more preferably an aliphatic structure having a molecular weight of 300 or less. 1 is preferably an aliphatic structure having a molecular weight of 14 or more, More preferably, it is an aliphatic structure having 28 or more X 1 represents the aliphatic structure of compound (B) described below. and may be a straight-chain aliphatic structure, a branched-chain aliphatic structure, or an alicyclic structure.

[0022] In the formula (3), n is an integer of 2 to 8, preferably 2 to 6, and more preferably 2 to 4.

[0023] Specifically, when the value of n is 2, the chemical structure represented by formula (3) is the following formula (4-1), and when the value of n is 3, the chemical structure represented by formula (3) is the following formula (4-2).

[0024] That is, more specifically, it is preferable that the chemical structure represented by formula (3) includes at least one of a chemical structure represented by the following formula (4-1) and a chemical structure represented by the following formula (4-2).

[0025] The urethane (meth)acrylate polymer of the present invention preferably contains, as the chemical structure represented by formula (3), at least one of a chemical structure represented by the following formula (4-1) and a chemical structure represented by the following formula (4-2). [ka] (In formulas (4-1) and (4-2), X 1 is X in formula (3). 1 is equivalent to

[0026] Furthermore, the urethane (meth)acrylate polymer of the present invention contains a structural unit derived from a compound having a hydroxyl group and a (meth)acryloyl group. Examples of the compound having a hydroxyl group and a (meth)acryloyl group include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, cyclohexane dimethanol mono(meth)acrylate, an addition reaction product of 2-hydroxyethyl (meth)acrylate and caprolactone, an addition reaction product of 4-hydroxybutyl (meth)acrylate and caprolactone, bisphenol A diglycidyl ether diacrylate, glycol mono(meth)acrylate, glycerin (meth)acrylate, glycerin di(meth)acrylate, pentaerythritol di(meth)acrylate, pentaerythritol tri(meth)acrylate, and dipentaerythritol penta(meth)acrylate.

[0027] [Weight average molecular weight (Mw)] The weight average molecular weight (Mw) of the urethane (meth)acrylate polymer of the present invention is preferably 500 or more, more preferably 10,000 or more, and more preferably 30,000 or less. 20,000 or less is more preferable. When the weight average molecular weight of the urethane (meth)acrylate polymer is within the above range, the transparency of the urethane (meth)acrylate polymer or the curable composition in a solution state and the scratch resistance of the cured film are good.

[0028] The weight average molecular weight was measured by gel permeation chromatography (GPC) using the method shown in the Examples.

[0029] An example of a method for producing the urethane (meth)acrylate polymer of the present invention will be described below. The urethane (meth)acrylate polymer of the present invention can be obtained by reacting the following compound (A) with the following compound (B) to obtain a urethane polymer precursor, and then reacting this with the following compound (C). Compound (A): Polyisocyanate Compound (B): A polyol represented by the following formula (5): [ka] [In the formula, A represents a single bond, or a methylene group, an alkylene group, an -O- group, an -NH- group, an -S- group, an -SO- group, or an -SO2- group which may have a substituent. 1 , R 2 , R 3 and R 4 R independently represents a hydrogen atom, an alkyl group, an alkoxy group, an aryl group, or a halogen atom. 5 and R 6 each independently represents an alkylene group, an alkoxylene group, or an arylene group. Compound (C): A compound having a hydroxyl group and a (meth)acryloyl group

[0030] In addition, the urethane (meth)acrylate polymer of the present invention may be prepared by reacting a polyol other than compound (B) in addition to compound (A) and compound (B) to obtain a urethane polymer precursor, and then reacting compound (C).

[0031] Examples of polyols other than the compound (B) include diols having a linear aliphatic structure such as ethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, 1,12-dodecanediol, 1,14-tetradecanediol, and 1,16-hexadecanediol; propylene glycol, 1,2-butanediol, 1,3-butanediol, 2,3-butanediol, 2-methyl-1,3-propanediol, neo Examples of the diols include those having a branched aliphatic structure, such as pentyl glycol, 1,2-pentanediol, 3-methyl-1,5-pentanediol, and 1,8-nonanediol; those compounds having a branched aliphatic structure and three or more hydroxyl groups bonded thereto, such as trimethylolpropane, glycerin, sorbitol, mannitol, and pentaerythritol; and those having an alicyclic structure, such as cyclopropanediol, cyclohexanediol, cyclohexanedimethanol, hydrogenated bisphenol A, tricyclodecanediol, and adamantyldiol. Of these, an aliphatic polyol having a molecular weight of 500 or less (hereinafter referred to as compound (D)) is preferred.

[0032] Furthermore, in the present invention, when the compound (A) and the compound (B) are reacted to obtain a precursor of the urethane polymer, a compound having two or more active hydrogens reactive with an isocyanate group may be added as a chain extender.

[0033] [Compound (A)] Examples of the polyisocyanate of the compound (A) include linear aliphatic polyisocyanates, aromatic polyisocyanates, alicyclic polyisocyanates, etc. Among these, linear alicyclic polyisocyanates are preferred from the viewpoint of improving the weather resistance and hardness of the resulting cured product.

[0034] Examples of the chain aliphatic polyisocyanate include aliphatic diisocyanates such as tetramethylene diisocyanate, hexamethylene diisocyanate, trimethylhexamethylene diisocyanate, and dimer acid diisocyanate, and aliphatic triisocyanates such as tris(isocyanatehexyl)isocyanurate. In order to improve the weather resistance and hardness of the resulting cured product, a linear or branched alkyl group having 1 to 6 carbon atoms is used. Preferably, the aryl group is a phenyl group. These may be used alone or in combination of two or more.

[0035] Examples of the aromatic polyisocyanate include aromatic diisocyanates such as tolylene diisocyanate, xylylene diisocyanate, diphenylmethane diisocyanate, m-phenylene diisocyanate, and naphthalene diisocyanate. From the viewpoint of increasing the mechanical strength of the cured film of the urethane (meth)acrylate polymer or the curable composition, the aromatic polyisocyanate is preferably tolylene diisocyanate and diphenylmethane diisocyanate. These may be used alone or in combination of two or more.

[0036] Examples of polyisocyanates having an alicyclic structure include diisocyanates having an alicyclic structure such as bis(isocyanatemethyl)cyclohexane, cyclohexane diisocyanate, bis(isocyanatecyclohexyl)methane, and isophorone diisocyanate, and triisocyanates having an alicyclic structure such as tris(isocyanateisophorone)isocyanurate. Among these, isophorone diisocyanate is preferred as the alicyclic polyisocyanate. These may be used alone or in combination of two or more.

[0037] The alicyclic structure preferably has 5 or more carbon atoms, and more preferably has 6 or more carbon atoms. Also, the alicyclic structure preferably has 15 or less carbon atoms, and more preferably has 13 or less carbon atoms. Furthermore, the alicyclic structure is preferably a cycloalkylene group. The compound (A) may be used alone or in combination of two or more kinds.

[0038] In order to obtain a cured product having excellent transparency, weather resistance, and scratch resistance, the compound (A) is preferably 5% by weight or more, more preferably 25% by weight or more, in the urethane (meth)acrylate polymer of the invention, and is preferably 60% by weight or less, more preferably 50% by weight or less, in order to obtain a cured product having excellent transparency, weather resistance, and scratch resistance.

[0039] [Compound (B)] The compound (B) is a polyol represented by the following formula (5). [ka] [In the formula, A represents a single bond, or a methylene group, an alkylene group, an -O- group, an -NH- group, an -S- group, an -SO- group, or an -SO2- group which may have a substituent. 1 , R 2 , R 3 and R 4 R independently represents a hydrogen atom, an alkyl group, an alkoxy group, an aryl group, or a halogen atom. 5 and R 6 each independently represents an alkylene group, an alkoxylene group, or an arylene group.

[0040] From the viewpoints of improving the transparency of the cured product obtained by curing the urethane (meth)acrylate polymer of the present invention and the curable composition using the same and preventing the bleed-out of the bisbenzotriazolylphenol skeleton from the cured product, it is preferable that the compound (B) represented by the formula (5) is a polyol represented by the following formula (10). [ka]

[0041] In order to obtain a cured product having excellent transparency, weather resistance, and scratch resistance, the ratio of the chemical structure represented by the formula (5) in the urethane (meth)acrylate polymer of the present invention is preferably 5% by weight or more, more preferably 20% by weight or more, and is preferably 60% by weight or less, more preferably 35% by weight or less.

[0042] As the compound (B), a commercially available product, Dynesorb T-33 manufactured by Daiwa Kasei Co., Ltd., can be used.

[0043] From the viewpoint of improving the weather resistance of the cured film of the present invention, the compound (B) is preferably 5% by weight or more, more preferably 25% by weight or more, based on the total polyol components used as raw materials for the urethane (meth)acrylate polymer, and is preferably 95% by weight or less, more preferably 90% by weight or less, from the viewpoints of excellent transparency in a solution state, transparency of the cured film, and scratch resistance.

[0044] [Compound (C)] The compound (C) having a hydroxyl group and a (meth)acryloyl group has a (meth)acryloyl group, and therefore forms a crosslinked structure with other components upon irradiation with active energy rays, thereby suppressing the bleeding out of the bisbenzotriazolylphenol skeleton that acts as an ultraviolet absorber.

[0045] Examples of the compound (C) include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, cyclohexanedimethanol mono(meth)acrylate, an addition reaction product of 2-hydroxyethyl (meth)acrylate and caprolactone, an addition reaction product of 4-hydroxybutyl (meth)acrylate and caprolactone, bisphenol A diglycidyl ether diacrylate, glycol mono(meth)acrylate, glycerin (meth)acrylate, glycerin di(meth)acrylate, pentaerythritol di(meth)acrylate, pentaerythritol tri(meth)acrylate, and dipentaerythritol penta(meth)acrylate.

[0046] Among these, from the viewpoints of improving the mechanical strength of the resulting cured film and the curability of the urethane (meth)acrylate polymer, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, pentaerythritol di(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol penta(meth)acrylate, and the like are preferred.

[0047] The compound (C) may be an epoxy (meth)acrylate having a chain aliphatic structure having 2 to 12 carbon atoms. Examples of raw materials for synthesizing the epoxy (meth)acrylate include ethylene glycol diglycidyl ether, 1,3-propanediol diglycidyl ether, 1,4-butanediol diglycidyl ether, 1,5-pentanediol diglycidyl ether, 1,6-hexanediol diglycidyl ether, 1,7-heptanediol diglycidyl ether, 1,8-octanediol diglycidyl ether, 1,9-nonanediol diglycidyl ether, 1,10-decanediol diglycidyl ether, and the like. glycidyl ether, 1,11-undecanediol diglycidyl ether, 1,12-dodecanediol diglycidyl ether, and other epoxy compounds having a linear aliphatic structure; and epoxy compounds having a branched aliphatic structure, such as propylene glycol diglycidyl ether, neopentyl glycol diglycidyl ether, 3-methyl-1,5-pentanediol diglycidyl ether, trimethylolpropane triglycidyl ether, glycerin triglycidyl ether, and pentaerythritol tetraglycidyl ether.

[0048] Among these, from the viewpoint of the curability of the urethane (meth)acrylate polymer, the epoxy compound is preferably an epoxy compound having a chain aliphatic structure having 4 to 6 carbon atoms, such as 1,4-butanediol diglycidyl ether, 1,5-pentanediol diglycidyl ether, or 1,6-hexanediol diglycidyl ether.

[0049] Compound (C) can be obtained by carrying out ring-opening addition reaction of a compound having a (meth)acryloyl group and a carboxyl group with the epoxy compound. As the compound having a (meth)acryloyl group and a carboxyl group, a compound having a (meth)acryloyl group and a carboxyl group can be used. Examples of the compound include (meth)acrylic acid; carboxyalkyl (meth)acrylates such as carboxymethyl (meth)acrylate, carboxyethyl (meth)acrylate, carboxypropyl (meth)acrylate, and carboxypropyl (meth)acrylate; and reaction products of hydroxyalkyl (meth)acrylates such as hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, and hydroxybutyl (meth)acrylate with carboxylic anhydrides such as phthalic anhydride, succinic anhydride, and maleic anhydride. These may be used alone or in combination of two or more.

[0050] Among these, acrylic acid is preferred as the compound having a (meth)acryloyl group and a carboxyl group from the viewpoint of the curability of the urethane (meth)acrylate polymer.

[0051] Examples of the epoxy (meth)acrylate of the compound (C) include KAYARAD (registered trademark) R-167 (manufactured by Nippon Kayaku Co., Ltd.), NK Oligo EA-5520, and EA-5321 (manufactured by Shin-Nakamura Chemical Co., Ltd.), etc. The compound (C) may be used alone or in combination of two or more.

[0052] In order to further increase the scratch resistance of the cured film of the curable composition of the present invention and to obtain good stretchability after curing, the compound (C) is preferably 4% by weight or more, more preferably 8% by weight or more, based on the total polyol components used as raw materials for the urethane (meth)acrylate polymer, and is preferably 25% by weight or less, more preferably 18% by weight or less.

[0053] [Compound (D)] The compound (D) is an aliphatic polyol having a molecular weight of 500 or less.

[0054] Examples of the compound (D) include diols having a linear aliphatic structure, such as ethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, 1,12-dodecanediol, 1,14-tetradecanediol, and 1,16-hexadecanediol; diols having a branched aliphatic structure, such as propylene glycol, 1,2-butanediol, 1,3-butanediol, 2,3-butanediol, 2-methyl-1,3-propanediol, neopentyl glycol, 1,2-pentanediol, 3-methyl-1,5-pentanediol, and 1,8-nonanediol; trimethylolpropane, glycol, and the like. Examples of such compounds include compounds having a branched aliphatic structure and three or more hydroxyl groups bonded thereto, such as lycerin, sorbitol, mannitol, and pentaerythritol; and diols having an alicyclic structure, such as cyclopropanediol, cyclohexanediol, cyclohexanedimethanol, hydrogenated bisphenol A, tricyclodecanediol, and adamantyldiol.

[0055] Among these, those having a linear aliphatic structure are preferred from the viewpoint of excellent scratch resistance of the cured film, and it is particularly preferred to use at least one selected from ethylene glycol, 1,4-butanediol, and 1,12-dodecanediol. Among these, ethylene glycol is preferred from the viewpoint of chemical resistance, and 1,12-dodecanediol is preferred from the viewpoint of scratch resistance and flexibility. In order to further improve the weather resistance of the cured film, it is necessary to introduce more compound (B) into the urethane (meth)acrylate polymer. For this purpose, it is preferred that compound (D) contains a diol having a branched aliphatic structure. As the diol having a branched aliphatic structure, propylene glycol, 1,3-butanediol, neopentyl glycol, 3-methyl-1,5-pentanediol, etc. are more preferred from the viewpoint of complementing the solution transparency and the low solubility of the ultraviolet absorbing skeleton, and 1,3-butanediol, neopentyl glycol, 3-methyl-1,5-pentanediol, etc. are even more preferred. The compound (D) may be used alone or in combination of two or more.

[0056] From the viewpoint of improving the chemical resistance and scratch resistance of the cured product of the urethane (meth)acrylate polymer of the present invention, the compound (D) is preferably 3% by weight or more, and more preferably 10% by weight or more, based on the total polyol components used as raw materials for the urethane (meth)acrylate polymer.

[0057] In order to increase the content of the formula (1) in the urethane (meth)acrylate polymer, the compound (D) is preferably 99.95% by weight or less, and more preferably 90% by weight or less, of the total polyol components used as raw materials for the urethane (meth)acrylate polymer.

[0058] [Polyols other than the compound (B) and the compound (D)] Examples of polyols other than the compound (B) and the compound (D) include aromatic polyols having a molecular weight of 500 or less, high molecular weight polyols having a molecular weight of more than 500, and the like.

[0059] Examples of the polyol having an aromatic structure and a molecular weight of 500 or less include bishydroxyethoxybenzene, bishydroxyethyl terephthalate, and bisphenol A. These may be used alone or in combination of two or more.

[0060] Examples of the high molecular weight polyol having a molecular weight of more than 500 include polyether polyol, polyester polyol, polyether ester polyol, polycarbonate polyol, polyolefin polyol, and silicone polyol, etc. These may be used alone or in combination of two or more.

[0061] When the high molecular weight polyol is used, polycarbonate polyol is preferred. Polycarbonate polyol can be obtained by reacting at least one carbonate compound selected from the group consisting of alkylene carbonate, diaryl carbonate, and dialkyl carbonate with at least one of diols and polyether polyols. Examples of the diols include ethylene glycol, propylene glycol, 1,4-butanediol, neopentyl glycol, 3-methyl-1,5-pentanediol, 1,6-hexanediol, 1,9-nonanediol, 1,4-cyclohexanedimethanol, 1,12-dodecanediol, diethylene glycol, dipropylene glycol, polybutadiene diol, etc. Among these, polycarbonate polyols having good scratch resistance are preferred. From the viewpoint of the convenience, it is preferable to include at least one selected from 1,4-butanediol, 1,5-pentanediol, and 1,6-hexanediol. Polycarbonate polyol can be obtained as a commercially available product. Examples of commercially available products include Duranol (registered trademark) T4671 (manufactured by Asahi Kasei Corporation), Duranol (registered trademark) T4691 (manufactured by Asahi Kasei Corporation), Duranol (registered trademark) 5651 (manufactured by Asahi Kasei Corporation), and Duranol (registered trademark) 6001 (manufactured by Asahi Kasei Corporation).

[0062] [Chain extender] Furthermore, in the present invention, when the compound (A) and the compound (B) are reacted to obtain a precursor of the urethane polymer, a compound having two or more active hydrogens reactive with an isocyanate group may be added as a chain extender.

[0063] Examples of the chain extender include low molecular weight diamine compounds having a number average molecular weight of 500 or less, such as aromatic diamines such as 2,4- or 2,6-tolylenediamine, xylylenediamine, and 4,4'-diphenylmethanediamine; ethylenediamine, 1,2-propylenediamine, 1,6-hexanediamine, 2,2-dimethyl-1,3-propanediamine, 2-methyl-1,5-pentanediamine, 2,2,4- or 2,4,4-trimethylhexanediamine, and 2-butyl- Aliphatic diamines such as 2-ethyl-1,5-pentanediamine, 1,8-octanediamine, 1,9-nonanediamine, and 1,10-decanediamine; and alicyclic diamines such as 1-amino-3-aminomethyl-3,5,5-trimethylcyclohexane, 4,4'-dicyclohexylmethanediamine, isopropylidenecyclohexyl-4,4'-diamine, 1,4-diaminocyclohexane, 1,3-bisaminomethylcyclohexane, and tricyclodecanediamine. These may be used alone or in combination of two or more.

[0064] In addition, when a chain extender is used, the amount of all polyols used is preferably 70 mol % or more, more preferably 95 mol % or more, based on the total amount of compounds used, including compound (B), compound (C), other polyol components, and the chain extender.

[0065] In the present invention, it is preferable to react the compound (B) with a polyol other than the compound (B) under conditions in which the isocyanate group is in excess to obtain a precursor of a urethane polymer having an isocyanate terminal, and then react the precursor of the urethane polymer having an isocyanate terminal with the compound (C).

[0066] When the compound (C) has two or more hydroxyl groups, the compound (C) is preferably used in an excess amount based on the total isocyanate groups of the urethane (meth)acrylate polymer.

[0067] In terms of being able to control the molecular weight of the urethane (meth)acrylate polymer, when producing the urethane (meth)acrylate polymer, the amount of the compound (C) used is preferably 2 mol% or more, more preferably 10 mol% or more, based on the total amount of the compound (C) and the compound containing a functional group that reacts with an isocyanate group in the other raw materials. Also, it is preferably 70 mol% or less, more preferably 50 mol% or less. If the proportion of the compound (C) is high, the molecular weight of the urethane (meth)acrylate polymer tends to be small, and if the proportion of the compound (C) is low, the molecular weight of the urethane (meth)acrylate polymer tends to be large.

[0068] In the method for producing the urethane (meth)acrylate polymer of the present invention, an organic solvent can be used for the purpose of adjusting the viscosity. As the organic solvent, any known organic solvent can be used as long as the effects of the present invention can be obtained. Preferable organic solvents include toluene, xylene, ethyl acetate, butyl acetate, cyclohexanone, methyl ethyl ketone, Examples of the organic solvent include methyl isobutyl ketone, N-methylpyrrolidone, and dimethylformamide. The organic solvent may be used alone or in combination of two or more. The organic solvent can usually be used in an amount of 300% by weight or less based on the total mass of the urethane (meth)acrylate polymer.

[0069] In the production of urethane (meth)acrylate polymers, a catalyst can be used in the urethanization reaction. Examples of the catalyst include tin-based catalysts such as dibutyltin laurate, dibutyltin dioctate, dioctyltin dilaurate, and dioctyltin dioctate; and bismuth-based catalysts such as bismuth tris(2-ethylhexanoate). Among these, dioctyltin dilaurate and bismuth tris(2-ethylhexanoate) are preferred in terms of environmental adaptability, catalytic activity, storage stability, and the like. The catalyst may be used alone or in combination of two or more. The amount of catalyst used is preferably 2,000 ppm or less, more preferably 1,000 ppm or less, based on the total amount of raw materials charged. Also, it is preferably 10 ppm or more, more preferably 30 ppm or more.

[0070] In addition, it is preferable to use a polymerization inhibitor in combination when producing a urethane (meth)acrylate polymer. Examples of the polymerization inhibitor include phenols such as hydroquinone, methylhydroquinone, hydroquinone monoethyl ether, and dibutylhydroxytoluene, amines such as phenothiazine and diphenylamine, copper salts such as copper dibutyldithiocarbamate, manganese salts such as manganese acetate, nitro compounds, and nitroso compounds. Among these, the polymerization inhibitor is preferably a phenol. The polymerization inhibitor may be used alone or in a mixture of two or more. The amount of the polymerization inhibitor used is preferably 3,000 ppm or less, more preferably 1,000 ppm or less, based on the total amount of the raw materials charged. In addition, it is preferably 50 ppm or more, more preferably 100 ppm or more.

[0071] In the production of a urethane (meth)acrylate polymer, the reaction temperature of the urethane-forming reaction is preferably 20° C. or higher, more preferably 40° C. or higher, in order to increase the reaction rate and improve production efficiency. Also, the reaction temperature is preferably 120° C. or lower, more preferably 100° C. or lower, in order to prevent side reactions such as allophanate-forming reactions from occurring. Also, when the reaction system contains the organic solvent, the reaction temperature is preferably equal to or lower than the boiling point of the organic solvent. The reaction time is usually 5 to 20 hours.

[0072] [Curable composition] The curable composition of the present invention preferably contains the urethane (meth)acrylate polymer and an organic solvent.

[0073] In the curable composition of the present invention, the content of the urethane (meth)acrylate polymer is preferably 40% by weight or more, more preferably 60% by weight or more, based on the total amount of all components (solids) in the curable composition excluding the organic solvent. The upper limit of the content of the urethane (meth)acrylate polymer is 100% by weight. When the content of the urethane (meth)acrylate polymer is within the above range, the curing speed and surface curability of the curable composition are good, and no tackiness remains, which is preferable.

[0074] Furthermore, in order to obtain a cured product with excellent transparency, weather resistance, and scratch resistance, the structural ratio of the compound represented by the formula (1) in the polymerization components of the curable composition is preferably 10% by weight or more, and more preferably 25% by weight or less.

[0075] The polymerizable component of the curable composition is a component having an unsaturated double bond polymerizable by active energy rays, and means a urethane (meth)acrylate polymer, an active energy ray curable polymer, an active energy ray reactive monomer, and the like contained in the curable composition. .

[0076] [Organic solvents] The organic solvent can be used to adjust the viscosity of the coating material when forming a coating film of the curable composition of the present invention. The solid content of the curable composition is preferably 5 to 90% by weight, more preferably 10% by weight or more, and more preferably 15% by weight or more, and is preferably 80% by weight or less, and more preferably 60% by weight or less.

[0077] The organic solvent may be a known organic solvent. From the viewpoint of the solubility of the urethane (meth)acrylate polymer, the solubility parameter (hereinafter referred to as "SP value") of the organic solvent is preferably 8.0 or more, and from the viewpoint of the transparency of the solution, the solubility parameter is preferably 11.5 or less. Examples of the organic solvent include toluene (SP value: 9.1), xylene (SP value: 9.1), ethyl acetate (SP value: 8.7), butyl acetate (SP value: 8.7), cyclohexanone (SP value: 9.8), methyl ethyl ketone (SP value: 9.0), methyl isobutyl ketone (SP value: 8.7), N-methylpyrrolidone (SP value: 11.2), and isopropyl alcohol (SP value: 11.5). In the present invention, the SP value is calculated by the method proposed by Fedors et al. Specifically, the "POLYMER This value is determined by referring to "ENGINEERING AND SCIENCE, FEBRUARY, 1974, Vol. 14, No. 2, ROBERT F. FEDORS. (pp. 147-154)." When a mixed solvent is used, the SP value means the value of the mixture.

[0078] [Other ingredients] The curable composition of the present invention may contain, as other components, an active energy ray reactive monomer, an active energy ray curable polymer (excluding the urethane (meth)acrylate polymer of the present invention), a polymerization initiator, a photosensitizer, an epoxy compound, other additives, and the like.

[0079] As the active energy ray reactive monomer, any known active energy ray reactive monomer can be used within the scope of the effect of the present invention. These active energy ray reactive monomers are used for the purpose of adjusting the hydrophilicity / hydrophobicity of the urethane (meth)acrylate polymer of the present invention, the hardness of the cured product when the obtained composition is cured, the elongation of the cured product, and other physical properties. The active energy ray reactive monomers may be used alone or in combination of two or more.

[0080] Examples of the active energy ray reactive monomer include vinyl ethers, (meth)acrylamides, and (meth)acrylates. Specific examples of the active energy ray reactive monomer include aromatic vinyl monomers such as styrene, α-methylstyrene, α-chlorostyrene, vinyl toluene, and divinylbenzene; vinyl ester monomers such as vinyl acetate, vinyl butyrate, N-vinylformamide, N-vinylacetamide, N-vinyl-2-pyrrolidone, N-vinylcaprolactam, and divinyl adipate; vinyl ethers such as ethyl vinyl ether and phenyl vinyl ether; and allyl monomers such as diallyl phthalate, trimethylolpropane diallyl ether, and allyl glycidyl ether. Compounds: (meth)acrylamides such as (meth)acrylamide, N,N-dimethylacrylamide, N,N-dimethylmethacrylamide, N-methylol (meth)acrylamide, N-methoxymethyl (meth)acrylamide, N-butoxymethyl (meth)acrylamide, Nt-butyl (meth)acrylamide, (meth)acryloylmorpholine, and methylene bis (meth)acrylamide; (meth)acrylic acid, methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, i-butyl (meth)acrylate, t-butyl (meth)acrylate, hexyl (meth)acrylate, and 2-Ethylhexyl, lauryl (meth)acrylate, stearyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, morpholyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, glycidyl (meth)acrylate, dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, benzyl (meth)acrylate, cyclohexyl (meth)acrylate, (meth)acrylic monofunctional (meth)acrylates such as phenoxyethyl (meth)acrylate, tricyclodecane (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, dicyclopentanyl (meth)acrylate, allyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, isobornyl (meth)acrylate, and phenyl (meth)acrylate; and ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, and triethylene glycol di(meth)acrylate. , tetraethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate (n=5-14), propylene glycol di(meth)acrylate, dipropylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, tetrapropylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate (n=5-14), 1,3-butylene glycol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, poly(meth)acrylate butylene glycol (n=3-16), poly(1-methylbutylene glycol) di(meth)acrylate (n=5-20), 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, neopentyl glycol hydroxypivalate di(meth)acrylate, dicyclopentanediol di(meth)acrylate, tricyclodecane di(meth)acrylate, bisphenol A diglycidyl ether di(meth)acrylate, 1,4-Cyclohexanedimethanol diglycidyl ether di(meth)acrylate, ethylene glycol diglycidyl ether di(meth)acrylate, 1,4-butanediol diglycidyl ether di(meth)acrylate, 1,6-hexanediol diglycidyl ether di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, dipentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, trimethylolpropane trioxyethyl(meth)acrylate, trimethylolpropane trioxypropyl(meth)acrylate Polyfunctional (meth)acrylates such as acrylate, trimethylolpropane polyoxyethyl (meth)acrylate, trimethylolpropane polyoxypropyl (meth)acrylate, tris(2-hydroxyethyl)isocyanurate tri(meth)acrylate, tris(2-hydroxyethyl)isocyanurate di(meth)acrylate, ethylene oxide-added bisphenol A di(meth)acrylate, ethylene oxide-added bisphenol F di(meth)acrylate, propylene oxide-added bisphenol A di(meth)acrylate, propylene oxide-added bisphenol F di(meth)acrylate, tricyclodecane dimethanol di(meth)acrylate, bisphenol A epoxy di(meth)acrylate, and bisphenol F epoxy di(meth)acrylate; and the like.

[0081] Among these, monofunctional (meth)acrylates having a ring structure in the molecule, such as (meth)acryloylmorpholine, tetrahydrofurfuryl (meth)acrylate, benzyl (meth)acrylate, cyclohexyl (meth)acrylate, trimethylcyclohexyl (meth)acrylate, phenoxyethyl (meth)acrylate, tricyclodecane (meth)acrylate, dicyclopentenyl (meth)acrylate, isobornyl (meth)acrylate, and (meth)acrylamide, are preferred, since the viscosity of the curable composition is low and the coating properties are good. Also, di(meth)acrylate-1,4-butene is preferred, since the mechanical strength of the resulting cured film is good. Polyfunctional (meth)acrylates such as hexanediol, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, tricyclodecane di(meth)acrylate, 1,4-cyclohexanedimethanol diglycidyl ether di(meth)acrylate, ethylene glycol diglycidyl ether di(meth)acrylate, 1,4-butanediol diglycidyl ether di(meth)acrylate, 1,6-hexanediol diglycidyl ether di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, and dipentaerythritol hexa(meth)acrylate are preferred. Furthermore, polyether (meth)acrylates such as polyethylene glycol di(meth)acrylate (n=5 to 14), polypropylene glycol di(meth)acrylate (n=5 to 14), polybutylene glycol di(meth)acrylate (n=3 to 16), and poly(1-methylbutylene glycol) di(meth)acrylate (n=5 to 20) are preferred in terms of providing good extensibility of the resulting cured film.

[0082] From the viewpoint of adjusting the viscosity of the curable composition and adjusting the physical properties such as hardness of the obtained cured product, the content of the active energy ray reactive monomer is preferably 50% by weight or less, and more preferably 30% by weight or less, based on the total amount of all components (solid contents) excluding the organic solvent of the curable composition.

[0083] Examples of the active energy radiation curable polymer include epoxy (meth)acrylate polymers, acrylic (meth)acrylate polymers, polyester (meth)acrylate polymers, polycarbonate (meth)acrylate polymers, polybutadiene (meth)acrylate polymers, and polyether (meth)acrylate (excluding those described in the active energy radiation reactive monomers). The active energy radiation curable polymers may be used alone or in combination of two or more.

[0084] The polymerization initiator is mainly used for the purpose of improving the polymerization efficiency of a polymerization reaction that proceeds by irradiation with active energy rays such as ultraviolet rays, electron beams, etc. As the polymerization initiator, any known photoradical polymerization initiator can be used as long as the effects of the present invention can be obtained. The polymerization initiator may be used alone or in combination of two or more. Furthermore, a photoradical polymerization initiator and a photosensitizer may be used in combination.

[0085] Examples of the photoradical polymerization initiator include benzophenone, 2,4,6-trimethylbenzophenone, 4,4-bis(diethylamino)benzophenone, 4-phenylbenzophenone, methyl orthobenzoyl benzoate, thioxanthone, diethylthioxanthone, isopropylthioxanthone, chlorothioxanthone, 2-ethylanthraquinone, t-butylanthraquinone, diethoxyacetophenone, 2-hydroxy-2-methyl-1-phenylpropan-1-one, benzyl dimethyl ketal, 1-hydroxycyclohexyl phenyl ketone, benzoin methyl ether, benzoin ethyl ether, and benzoin isopropyl. ether, benzoin isobutyl ether, methyl benzoyl formate, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one, 2,6-dimethylbenzoyldiphenylphosphine oxide, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, bis(2,6-dimethoxybenzoyl)-2,4,4-trimethylpentylphosphine oxide, bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide, and 2-hydroxy-1-[4-[4-(2-hydroxy-2-methyl-propionyl)-benzyl]-phenyl]-2-methyl-propan-1-one.

[0086] Among these, benzophenone and benzophenone are preferred because they have a fast curing rate and can sufficiently increase the crosslink density. 2-Hydroxy-2-methyl-1-phenylpropan-1-one, 1-hydroxycyclohexyl phenyl ketone, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, and 2-hydroxy-1-[4-[4-(2-hydroxy-2-methyl-propionyl)-benzyl]-phenyl]-2-methyl-propan-1-one are preferred, and 1-hydroxycyclohexyl phenyl ketone, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, and 2-hydroxy-1-[4-[4-(2-hydroxy-2-methyl-propionyl)-benzyl]-phenyl]-2-methyl-propan-1-one are more preferred.

[0087] In addition, when the curable composition contains a compound having a cationic polymerizable group such as an epoxy group together with a radical polymerizable group, the curable composition may contain a cationic photopolymerization initiator together with the photoradical polymerization initiator as a polymerization initiator. Any known cationic photopolymerization initiator can be used as long as it does not significantly impair the effects of the present invention.

[0088] The content of the polymerization initiator is preferably 10% by weight or less, and more preferably 5% by weight or less, based on the total weight of the polymerization components of the curable composition, in order to prevent a decrease in mechanical strength due to initiator decomposition products.

[0089] The photosensitizer can be used for the same purpose as the polymerization initiator. Examples of the photosensitizer include ethanolamine, diethanolamine, triethanolamine, N-methyldiethanolamine, methyl 4-dimethylaminobenzoate, ethyl 4-dimethylaminobenzoate, amyl 4-dimethylaminobenzoate, and 4-dimethylaminoacetophenone. The photosensitizer may be used alone or in combination of two or more.

[0090] In the curable composition of the present invention, the content of the photosensitizer is preferably 10% by weight or less, and more preferably 5% by weight or less, based on the total weight of the polymerization components of the curable composition, in order to prevent a decrease in mechanical strength due to a decrease in crosslink density.

[0091] Examples of the additives include fillers such as silica, alumina, calcium carbonate, mica, zinc oxide, titanium oxide, talc, kaolin, metal oxides, metal fibers, iron, lead, and metal powder; carbon materials such as carbon fibers, carbon black, graphite, carbon nanotubes, and fullerenes such as C60; modifiers such as antioxidants, heat stabilizers, ultraviolet absorbers, hindered amine light stabilizers (HALS), surface hydrophilizing agents, antistatic agents, slipping agents, plasticizers, release agents, defoamers, leveling agents, antisettling agents, surfactants, thixotropy-imparting agents, flame retardants, flame retardant assistants, polymerization inhibitors, and silane coupling agents; and colorants such as pigments, dyes, and hue adjusters. The additives may be used alone or in combination of two or more.

[0092] In the curable composition of the present invention, the content of the additive is preferably 10% by weight or less, and more preferably 5% by weight or less, based on the total weight of the polymerization components of the curable composition, in order to prevent a decrease in mechanical strength due to a decrease in crosslink density.

[0093] The method for incorporating the additives into the curable composition of the present invention is not particularly limited, and examples thereof include conventionally known mixing and dispersing methods, etc. In order to disperse the additives in the curable composition more reliably, examples thereof include a method of treating with a two-roll mill, a three-roll mill, a bead mill, a ball mill, a sand mill, a pebble mill, a tron ​​mill, a sand grinder, a segmented barrier lighter, a planetary mixer, a high-speed impeller disperser, a high-speed stone mill, a high-speed impact mill, a kneader, a homogenizer, an ultrasonic disperser, etc.

[0094] [viscosity] The viscosity of the curable composition of the present invention is preferably 5 mPa·s or more, more preferably 10 mPa·s or more, from the viewpoints of handling property, coatability, moldability, three-dimensional modeling property, etc., and is preferably 50,000 mPa·s or less, more preferably 10,000 mPa·s or less. The viscosity of the curable composition can be adjusted, for example, by the content of the urethane (meth)acrylate polymer according to the present invention, the types of the additives, and the blending ratio thereof. The viscosity was measured at 25°C using an E-type viscometer (rotor 1°34'×R24).

[0095] [Coating method] The urethane (meth)acrylate polymer of the present invention or the curable composition of the present invention can be applied by known methods such as a bar coater method, an applicator method, a curtain flow coater method, a roll coater method, a spray method, a gravure coater method, a comma coater method, a reverse roll coater method, a lip coater method, a die coater method, a slot die coater method, an air knife coater method, a dip coater method, etc., among which the bar coater method and the gravure coater method are preferred. The urethane (meth)acrylate polymer of the present invention can also be used alone by the above-mentioned coating method.

[0096] Examples of substrates to which the urethane (meth)acrylate polymer of the present invention or the curable composition of the present invention is applied include polyesters such as polyethylene terephthalate and polybutylene terephthalate; polyolefins such as polypropylene and polyethylene; and various plastics such as nylon, polycarbonate, and (meth)acrylic polymers, glass, and metal. Among these, polyethylene terephthalate is preferred. The shape of these substrates may be flat, such as a film or sheet, or may be molded into various shapes.

[0097] [Cured product / laminate] The cured product of the present invention can be obtained by irradiating the urethane (meth)acrylate polymer of the present invention or the curable composition of the present invention with active energy rays. Examples of the active energy rays include infrared rays, visible light rays, ultraviolet rays, X-rays, electron beams, α rays, β rays, γ rays, etc. From the viewpoint of equipment cost and productivity, it is preferable to use electron beams or ultraviolet rays. As the light source, an electron beam irradiation device, an ultra-high pressure mercury lamp, a high pressure mercury lamp, a medium pressure mercury lamp, a low pressure mercury lamp, a metal halide lamp, an Ar laser, a He-Cd laser, a solid laser, a xenon lamp, a high frequency induction mercury lamp, sunlight, etc. can be used.

[0098] The amount of irradiation of active energy rays can be appropriately selected depending on the type of active energy rays. For example, when curing is performed by irradiation with electron beams, the amount of irradiation is preferably 1 to 15 Mrad. When curing is performed by irradiation with ultraviolet rays, the amount of irradiation is preferably 50 to 1,500 mJ / cm. 2 It is preferable that:

[0099] When the urethane (meth)acrylate polymer of the present invention or the curable composition of the present invention is cured, it may be cured in an atmosphere of air or an inert gas such as nitrogen or argon, or may be irradiated in a closed space between a film or glass and a metal mold.

[0100] The thickness of the cured product is appropriately determined depending on the intended use, but from the viewpoint of good expression of design and functionality after three-dimensional processing, the thickness of the cured product is preferably 1 μm or more, and more preferably 2 μm or more. Also, from the viewpoint of good curability and three-dimensional processing suitability, the thickness of the cured product is preferably 100 μm or less, more preferably 50 μm or less, and even more preferably 20 μm or less.

[0101] The laminate of the present invention can be obtained by curing the urethane (meth)acrylate polymer of the present invention or the curable composition of the present invention on a substrate. A layer other than the cured product may be present between the substrate and the cured product of the present invention, or may be present on the outside of the laminate of the present invention. The laminate may have multiple layers of the substrate and the cured product of the present invention.

[0102] As a method for obtaining a laminate having a plurality of cured layers, known methods such as a method of laminating all layers in an uncured state and then curing with active energy rays, a method of curing or semi-curing a lower layer with active energy rays and then coating an upper layer and curing it again with active energy rays, a method of coating each layer on a substrate and then laminating the layers together in an uncured or semi-cured state, etc. are applicable, but from the viewpoint of increasing the adhesion between layers, a method of laminating in an uncured state and then curing with active energy rays is preferred. As a method for laminating in an uncured state, known methods such as sequential coating in which a lower layer is coated and then an upper layer is coated in layers, and simultaneous multi-layer coating in which two or more layers are coated in layers at the same time from multiple slits can be applied, but are not limited thereto.

[0103] The laminate of the present invention can be suitably used as a film to replace paint. For example, it can be effectively applied to various components such as interior and exterior building materials, automobiles, home appliances, and information and electronic materials. In addition, the laminate of the present invention can be suitably used for glazing components and decorative films because it can impart the weather resistance, bleed-out resistance, and scratch resistance required for surface protection with a single layer, and the process is simple. In the present invention, the decorative film refers to a film to which designs and decorations such as wood grain, metallic finish, uneven shapes such as embossing, various patterns, characters, etc. have been added by printing, painting, vapor deposition, coloring, etc. The urethane (meth)acrylate polymer of the present invention or the curable composition of the present invention is applied to the surface of a molded article such as polycarbonate, and then irradiated with active energy rays to form a cured product. The molded article is suitably used for automobile headlamp lenses and automobile polymer glass.

[0104] Since the cured product of the present invention has excellent stretchability, the laminate of the present invention can be stretched and used as a film. A method for producing the film preferably includes a step of applying the urethane (meth)acrylate polymer of the present invention or the curable composition of the present invention onto a substrate, a step of irradiating the curable composition with active energy rays to obtain a laminate having a cured product, and a step of stretching the laminate.

[0105] In the film manufacturing method, the step of applying the urethane (meth)acrylate polymer or the curable composition of the present invention onto a substrate and the step of irradiating the urethane (meth)acrylate polymer or the curable composition with active energy rays to obtain a cured product can each be performed under the conditions described above. In addition, in the film manufacturing method, the cured product can be stretched by heating it under conditions of usually 60 to 200°C, preferably 100 to 180°C. When the film is used as a decorative film, the decorative film can be formed by known methods such as insert molding, in-mold molding, overlay molding, blow molding, and vacuum molding. EXAMPLES

[0106] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples in any way.

[0107] [Methods for measuring physical properties and characteristics] The urethane (meth)acrylate polymer and the cured film were evaluated by the following methods. <Molecular weight> The gel was analyzed by GPC (Tosoh Corporation, "HLC-8120GPC") using tetrahydrofuran (T The weight average molecular weight Mw and number average molecular weight Mn of the urethane (meth)acrylate polymer were measured using a column of TSKgel super H1000+H2000+H3000 with a flow rate of 0.5 mL / min and a column oven temperature of 40°C.

[0108] <Transparency evaluation of curable composition> The curable compositions obtained in the examples were allowed to stand for one day, and then their appearance was visually confirmed to determine whether they were transparent, opaque, or insoluble, thereby evaluating the transparency of the curable compositions.

[0109] <Evaluation of the cured product> (Evaluation sample) The curable compositions obtained in the examples and comparative examples were applied onto a polyethylene terephthalate film using a bar coater, then dried at 80°C for 2 minutes, and then irradiated with a 160W high-pressure mercury lamp at an accumulated irradiation dose of 1000mJ / cm using an ultraviolet irradiator (US5-X1802-X1202, Iwasaki Electric Co., Ltd.). 2 It was cured by exposure to ultraviolet light (wavelength 315 to 380 nm). After further curing at 23° C. for one day, a laminate with a thickness of about 5 μm was obtained.

[0110] (Evaluation of coating appearance) The appearance of the coating film on the obtained laminate was visually confirmed to be transparent or opaque, and the haze value H was measured. The haze value H was measured using a haze meter ("HAZE METER HM-65W" manufactured by Murakami Color Research Laboratory Co., Ltd.) in accordance with JIS K7105.

[0111] (Weather resistance test (metal weather test)) The color tone b0 of the coating film on the obtained laminate was measured using a spectrophotometer (manufactured by Konica Minolta, Inc., product name "Spectrophotometer CM-5"). A meter (manufactured by Daipla Wintes Co., Ltd., product name "Daipla Metal Weather KU-R4Ci-W") was used, and the irradiation intensity was 80 mW / cm 2 Under the irradiation of the following (1), (2), and (3) ) was performed for 4 hours each, totaling 12 hours as one cycle, and accelerated weather resistance tests were performed for 168 hours (14 cycles) and 336 hours (28 cycles). After the tests, the cured products were visually observed, and the color tone b1 and haze value H of the cured products after the accelerated weather resistance tests were measured. The color tone of the cured product was evaluated as b1-b0. (1) Temperature 63℃, humidity 70% (2) Temperature 70℃, humidity 90% (3) Temperature 30°C, humidity 98% (10-second showers before and after (3))

[0112] (Transmittance measurement) The transmittance (360 nm, 380 nm) of the coating film on the obtained laminate was measured using a spectrophotometer (manufactured by Hitachi High-Technologies Corporation, product name "Ratio Beam Spectrophotometer U-1900"), with a polyethylene terephthalate film (treated for easy adhesion) as the baseline.

[0113] (Evaluation of scratch resistance) The haze value H1 of the coating film on the obtained laminate before the scratch resistance test was measured. The surface of the coating film on the laminate was abraded with steel wool #0000 at 200 gf (area 4 cm ) using a Gakushin abrasion tester (manufactured by Toyo Seiki Co., Ltd.) at 23°C and 55% RH. 2 Place the weight of the The haze value H2 was measured after 15 round trips. A haze value H2 of 30 or less was determined to be excellent in scratch resistance. The haze value was measured using a haze meter ("HAZE METER HM-65W" manufactured by Murakami Color Research Laboratory Co., Ltd.) in accordance with JIS K7105.

[0114] [Raw materials and solvents] The raw materials and solvents used in the following Examples and Comparative Examples and their abbreviations are as follows: (Compound (A)) IPDI: Isophorone diisocyanate (Evonik Degussa Japan, product name "VESTANAT IPDI")

[0115] (Compound (B)) T-33: Polyol represented by the following formula (10) (manufactured by Daiwa Kasei Co., Ltd., product name "Dynesorb T-33") [ka] T-35: Polyol represented by the following formula (11) (manufactured by Daiwa Kasei Co., Ltd., product name "Dynesorb T-35") [ka]

[0116] (Compound (C): Compound having a hydroxyl group and a (meth)acryloyl group) HEA: 2-hydroxyethyl acrylate (Osaka Organic Chemicals, product name "HEA") (Compound (D)) 3MPD: 3-Methyl-1,5-pentanediol

[0117] (Organic solvent) MEK: Methyl ethyl ketone (SP value: 9.0) PGM: Propylene glycol monomethyl ether (SP value: 11.3)

[0118] (Multifunctional acrylate) V-300: A mixture containing 40 to 45% by weight of pentaerythritol triacrylate and 35 to 40% by weight of pentaerythritol tetraacrylate as another compound (catalog value) ("Viscoat (registered trademark) 300" manufactured by Osaka Organic Chemicals)

[0119] (Photoradical polymerization initiator) Omn184: 1-hydroxy-cyclohexyl-phenyl-ketone (manufactured by IGM, "Omnirad (registered trademark) 184")

[0120] (UV absorber) TINUVIN479: Hydroxyphenyltriazine (HPT) UV absorber (manufactured by BASF)

[0121] (Leveling agent) Polyflow No. 75: (Kyoeisha Chemical Co., Ltd.)

[0122] [Synthesis Example 1] In a four-neck flask equipped with a stirrer, reflux condenser, dropping funnel, and thermometer, 102 g of IPDI and 101 g of T-33 were placed, and further 203 g of methyl ethyl ketone, 0.20 g of dioctyltin dilaurate, and 0.25 g of methyl hydroquinone were placed and reacted for about 2 hours until the suspension became transparent while heating to 80 ° C. in an oil bath. After the completion of the urethane reaction, the mixture was cooled to 60 ° C., and then 0.05 g of dioctyltin dilaurate was added, and a mixture of 297 g of V-300 and 297 g of methyl ethyl ketone was added dropwise over 1 hour to carry out the reaction. The reaction was carried out for 8 hours while heating to 70 ° C. in an oil bath, and the end point of the urethane reaction was confirmed by the disappearance of the peak derived from the isocyanate (NCO) group in the infrared absorption spectrum, to obtain a urethane acrylate polymer. The weight average molecular weight and number average molecular weight of the obtained urethane acrylate polymer were measured. The obtained results are shown in Table 1. Hereinafter, this urethane acrylate polymer will be referred to as "U-1."

[0123] [Synthesis Example 2] In a four-neck flask equipped with a stirrer, reflux condenser, dropping funnel, and thermometer, 247g of IPDI and 79g of 3MPD were added, and 326g of methyl ethyl ketone and 0.10g of dioctyltin dilaurate were added and reacted for 2 hours while heating to 80°C in an oil bath. Then, 116g of T-33, 116g of methyl ethyl ketone, and 0.12g of dioctyltin dilaurate were added, and the reaction was continued for about 2 hours until the suspension became transparent. After the completion of the urethane reaction, the mixture was cooled to 60°C, and then 0.28g of dioctyltin dilaurate and 0.25g of methyl hydroquinone were added, and a mixture of 57g of HEA and 57g of methyl ethyl ketone was added dropwise over 1 hour to start the reaction. The reaction was carried out for 8 hours while heating to 70°C in an oil bath, and the end point of the urethane reaction was confirmed by the disappearance of the peak derived from the isocyanate (NCO) group in the infrared absorption spectrum, to obtain a urethane acrylate polymer. The weight average molecular weight and number average molecular weight of the obtained urethane acrylate polymer were measured. The results are shown in Table 1. Hereinafter, this urethane acrylate polymer is referred to as "U-2".

[0124] [Synthesis Example 3] In a four-neck flask equipped with a stirrer, reflux condenser, dropping funnel, and thermometer, 223 g of IPDI and 59 g of 3MPD were added, and 282 g of methyl ethyl ketone and 0.08 g of dioctyltin dilaurate were added and reacted for 2 hours while heating to 80 ° C. in an oil bath, and then 174 g of T-33, 175 g of methyl ethyl ketone, and 0.14 g of dioctyltin dilaurate were added and reacted for about 2 hours until the suspension became transparent. After the completion of the urethane reaction, the mixture was cooled to 60 ° C., and then 0.27 g of dioctyltin dilaurate and 0.25 g of methyl hydroquinone were added, and a mixture of 43 g of HEA and 43 g of methyl ethyl ketone was added dropwise over 1 hour to start the reaction. The reaction was carried out for 8 hours while heating to 70 ° C. in an oil bath, and the end point of the urethane reaction was confirmed by the disappearance of the peak derived from the isocyanate (NCO) group in the infrared absorption spectrum, to obtain a urethane acrylate polymer. The weight average molecular weight and number average molecular weight of the obtained urethane acrylate polymer were measured. The results are shown in Table 1. Hereinafter, this urethane acrylate polymer is referred to as "U-3".

[0125] [Synthesis Example 4] In a four-neck flask equipped with a stirrer, reflux condenser, dropping funnel, and thermometer, add IPDI 154g of 3MPD and 27g of 3MPD were added, and 181g of methyl ethyl ketone and 0.05g of dioctyltin dilaurate were added and reacted for 2 hours while heating to 80°C in an oil bath. Then, 258g of T-35, 258g of methyl ethyl ketone, and 0.17g of dioctyltin dilaurate were added and reacted for 2 hours. After the completion of the urethane reaction, the mixture was cooled to 60°C, and 0.28g of dioctyltin dilaurate and 0.25g of methyl hydroquinone were added, and a mixture of 59g of HEA and 59g of methyl ethyl ketone was added dropwise over 1 hour to start the reaction. The reaction was carried out for 8 hours while heating to 70°C in an oil bath, and the end point of the urethane reaction was confirmed by the disappearance of the peak derived from the isocyanate (NCO) group in the infrared absorption spectrum, to obtain a urethane acrylate polymer. The weight average molecular weight and number average molecular weight of the obtained urethane acrylate polymer were measured. The obtained results are shown in Table 1. Hereinafter, this urethane acrylate polymer will be referred to as "U-4."

[0126] [Example 1] A flask was charged with 56.9 g of urethane acrylate polymer "U-1" (solid content: 50% by weight), 1.4 g of Irg184 as a polymerization initiator, 0.1 g of Polyflow No. 75 as a leveling agent, 1.6 g of MEK, and 40.0 g of PGM, and stirred at 25°C for 1 hour to obtain a curable composition. The obtained curable composition was used to evaluate transparency. The obtained results are shown in Table 1.

[0127] [Examples 2 to 5 and Comparative Examples 1 to 7] The same procedure as in Example 1 was carried out except that the composition of the curable composition was changed as shown in Table 1. The results obtained for each evaluation item are shown in Table 1. Note that U-2 was used instead of U-1 in Examples 2 and 3, U-3 in Examples 4 and 5, and U-4 in Comparative Example 1.

[0128] [Table 1]

[0129] [Table 2]

[0130] Comparative Example 1, in which T-35 was introduced into the urethane (meth)acrylate structure instead of T-33, had an ester bond in the UV-absorbing skeleton compared to Example 2, and therefore hydrolysis originating from the ester bond occurred, leading to an increase in the b1-b0 value in the metal weather test (28-cycle weather resistance) and a decrease in weather resistance.

[0131] In addition, in Comparative Examples 2 and 3, in which the dihydroxy compound T-33 was added to the curable composition, the solution became cloudy, the solution appearance was unacceptable, and a good coating film was not obtained. On the other hand, in Comparative Examples 4 and 5, in which T-35 was added, the weather resistance was insufficient. Furthermore, in Comparative Example 6, in which Tinuvin 479 was added, the b1-b0 value in the metal weather test (28 cycle weather resistance) increased, and the weather resistance decreased. In Comparative Example 7, the coating appearance and weather resistance were poor.

[0132] Although the present invention has been described in detail and with reference to specific embodiments, it is apparent to those skilled in the art that various changes and modifications can be made without departing from the spirit and scope of the present invention. This application is based on a Japanese patent application (Patent Application No. 2017-052242) filed on March 17, 2017, the contents of which are incorporated herein by reference. [Industrial Applicability]

[0133] The cured product and laminate obtained by using the urethane (meth)acrylate polymer or the curable composition of the present invention can be suitably used as a film to replace paint. For example, it can be effectively applied to various components such as interior and exterior building materials, automobiles, home appliances, and information and electronic materials. In particular, the cured film according to the embodiment of the present invention can be suitably used as a decorative film with the cured film as a topcoat layer.

Claims

1. A chemical structure represented by the following formula (2), and Ethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, 1,12-dodecanediol, 1,14-tetradecanediol, 1,16-hexadecanediol, propylene glycol, 1,2-butanediol, 1,3-butanediol, 2,3-butanediol one or more polyol structures selected from the group consisting of phenol, 2-methyl-1,3-propanediol, neopentyl glycol, 1,2-pentanediol, 3-methyl-1,5-pentanediol, 1,8-nonanediol, trimethylolpropane, glycerin, sorbitol, mannitol, pentaerythritol, cyclopropanediol, cyclohexanediol, cyclohexanedimethanol, hydrogenated bisphenol A, tricyclodecanediol, and adamantyldiol. having A urethane (meth)acrylate polymer, in which the ratio of the chemical structure represented by the formula (2) is 5 to 60% by weight. [Formula 1]

2. The urethane (meth)acrylate polymer according to claim 1, having a weight average molecular weight (Mw) of 500 to 30,000.

3. A curable composition comprising the urethane (meth)acrylate polymer according to claim 1 or 2 and an organic solvent.

4. The curable composition according to claim 3, wherein the organic solvent has a solubility parameter of 8.0 to 11.

5.

5. The curable composition according to claim 3 or 4, wherein the solid content concentration of the curable composition is 5 to 90% by weight.

6. The curable composition according to any one of claims 3 to 5, wherein the ratio of the chemical structure represented by formula (2) in the polymerization components of the curable composition is 5 to 60% by weight.

7. A cured product of the curable composition according to any one of claims 3 to 6.

8. A laminate having a cured product of the curable composition according to any one of claims 3 to 6 on a substrate.

9. A headlamp lens having a substrate and a cured product of the curable composition according to claim 7 on the substrate.

10. A glazing material having a substrate and a cured product of the curable composition according to claim 7 .

11. A decorative film comprising a substrate and a cured product of the curable composition according to claim 7 on the substrate.

12. A method for producing a film, comprising: a step of applying the urethane (meth)acrylate polymer according to claim 1 or 2 or the curable composition according to any one of claims 3 to 6 onto a substrate; a step of irradiating the urethane (meth)acrylate polymer or the curable composition with active energy rays to obtain a laminate having a cured product; and a step of stretching the laminate.

13. A method for producing a urethane (meth)acrylate polymer, comprising the steps of: The urethane (meth)acrylate polymer has a chemical structure represented by the following formula (2), and the ratio of the chemical structure represented by the formula (2) in the urethane (meth)acrylate polymer is 5 to 60% by weight: A method for producing a urethane (meth)acrylate polymer, comprising reacting the following compound (A), a polyol represented by the following formula (10), and the following compound (D) to obtain a precursor of a urethane polymer, and then reacting the precursor with the following compound (C). Compound (A): Polyisocyanate [Case 2] [C3] Compound (C): A compound having a hydroxyl group and a (meth)acryloyl group Compound (D): Aliphatic polyol having a molecular weight of 500 or less

Citation Information

Patent Citations

  • Paint composition

    JP2000017204A

  • Coating material of high resistance to weather

    JP2000053913A

  • Ultraviolet-screening activation energy ray curable composition, curable coating material and molded product coated therewith

    JP2000109652A

  • Urethane (Meth)Acrylate containing ultraviolet- absorbing functional group, and composition thereof

    JP2003137964A

  • Curable resin composition

    JP2015017211A