Method for producing positive electrode active material for lithium ion secondary battery
By using oxidized metallic nickel powder to form a layered structure with lithium and other metals, the method addresses the inefficiencies and emissions of traditional nickel sulfate or nickel hydroxide processes, achieving a simpler, more efficient production of high-capacity positive electrode active materials for lithium-ion batteries.
Patent Information
- Application Number
- JP2023117559
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-03-30
- Filing Date
- 2023-07-19
- Publication Date
- 2024-10-02
- Estimated Expiration
- 2042-03-17
AI Technical Summary
The production of positive electrode active materials for lithium-ion batteries using nickel sulfate or nickel hydroxide as precursors is costly, complex, and leads to high greenhouse gas emissions due to the processing and transportation of these compounds, which have low bulk density and require extensive handling.
A method utilizing highly purified metallic nickel powder, oxidized to at least 50% oxygen content, is mixed with lithium and other metal compounds, then fired to form a layered structure, eliminating the need for acid dissolution and coprecipitation steps, thereby reducing transportation volume and manufacturing complexity.
This approach reduces energy consumption and greenhouse gas emissions by simplifying the manufacturing process and minimizing the volume handled, while maintaining high nickel content and capacity, resulting in a more efficient production of positive electrode active materials.
Smart Images

Figure 0007559884000003 
Figure 0007559884000004 
Figure 0007559884000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a positive electrode active material for a lithium ion secondary battery. [Background technology]
[0002] Lithium-ion batteries are widely used in various fields such as electronics, automobiles, and infrastructure. In particular, in automobiles, lithium-ion batteries are used as the power source for electric vehicles (EVs) and are an important core component. From the viewpoint of extending the driving range, the energy density of lithium-ion batteries is improving year by year, and high-capacity ternary layered materials are used as the positive electrode active material used in the batteries. The ternary layered materials are composite oxides of metal elements such as Ni, Co, Mn, or Al and Li (hereinafter referred to as lithium metal composite oxides), and the higher the atomic ratio of Ni in the metal elements, the higher the capacity. Therefore, high-Ni materials are expected as positive electrode active materials for EV batteries. Furthermore, from the viewpoint of maintaining a sustainable global environment and cost and resource conservation measures, materials that reduce Co, which is expensive and has a small amount of reserves, are expected, and the movement to improve the Ni ratio as a substitute for Co will further promote high-Ni materials in the future.
[0003] Patent Document 1 describes a method for producing a positive electrode active material using a metal hydroxide as a precursor. The process of producing a positive electrode active material by reacting a metal hydroxide with a Li source is widely adopted. Patent Document 2 describes a manufacturing method in which a nickel source is melted, nickel particles obtained by an atomization method are dissolved in a sulfuric acid aqueous solution to obtain nickel sulfate, a hydroxide containing Ni is obtained by a crystallization method, and a positive electrode active material for a secondary battery is obtained by a coprecipitation method using this hydroxide. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2015-002120 A [Patent Document 2] International Publication No. 2020 / 066262 Summary of the Invention [Problem to be solved by the invention]
[0005] As described in Patent Documents 1 and 2, the positive electrode active material is produced by reacting a Li source with synthesized transition metal hydroxide particles by a coprecipitation reaction. In the coprecipitation reaction, an aqueous solution of nickel sulfate or the like is used as a raw material, which is produced by dissolving nickel bullion that has been refined to a high purity in acid to avoid impurities. Nickel sulfate is produced by refining nickel from nickel ore mined from a mine and processing it by dissolving it in acid, which is a problem of high processing costs. In addition, since nickel sulfate is a hexahydrate, the mass % of Ni is about 20 to 25%, which is a small bulk specific gravity, and to compensate for this, the volume handled in the manufacturing process of the positive electrode material becomes large. At the same time, the transportation cost also increases. For these reasons, more energy is required for transportation and manufacturing, and the manufacturing process becomes complicated and long. As a result, there is a problem that greenhouse gases (GHG) emitted also increase.
[0006] Therefore, the present invention aims to provide a method for producing a positive electrode active material for a lithium ion secondary battery that uses nickel ingots that are highly refined to avoid impurities, while reducing the volume of material handled in the transportation and manufacturing process of the positive electrode material, thereby reducing the energy used in transportation and manufacturing and eliminating the complexity of the manufacturing process. As a result, the present invention aims to provide a method for producing a positive electrode active material for a lithium ion secondary battery that reduces GHG emissions. [Means for solving the problem]
[0007] The method for producing a positive electrode active material for a lithium ion secondary battery of the present invention includes a mixing step of mixing metallic nickel powder, a compound containing lithium, and a compound containing a metal element M other than lithium and nickel to obtain a mixed powder, an oxidation step of oxidizing the metallic nickel powder in the mixed powder to an oxidation rate of 50% or more, a crushing and mixing step of crushing the oxidized powder containing the oxidized metallic nickel powder to obtain a crushed mixed powder, and a firing step of sintering the crushed mixed powder to obtain a layered structured positive electrode active material for a lithium ion secondary battery in which the ratio of Ni to all metal elements other than Li is 60 atomic % or more. The lithium-containing compound is lithium carbonate, and the oxidation step is carried out at a temperature equal to or lower than the melting point of lithium carbonate. The present invention is characterized by the above.
[0008] The method for producing a positive electrode active material for a lithium ion secondary battery of the present invention is characterized in that, in the oxidation step, the metallic nickel powder is oxidized while preventing sintering of the metallic nickel powder with each other by a compound containing lithium having a melting point higher than the thermal oxidation temperature of the oxidation step.
[0009] The method for producing a positive electrode active material for a lithium ion secondary battery of the present invention is characterized by comprising a mixing step of mixing metallic nickel powder, at least a portion of which has already been oxidized and has an oxygen content of 300 ppm or more, a compound containing lithium, and a compound containing a metal element M other than lithium and nickel, to obtain a mixed powder, and a firing step of sintering the mixed powder to obtain a positive electrode active material for a lithium ion secondary battery having a layered structure in which the proportion of Ni relative to all metal elements other than Li is 60 atomic % or more.
[0011] In this case, it is preferable that the primary particle D50 of the pulverized and mixed powder after the pulverizing and mixing step is 0.17 μm or less.
[0012] In addition, the specific surface area of the primary particles of the pulverized mixed powder after the pulverization and mixing process is 28 m 2 It is preferable that the molecular weight is 1 / g or more. Effect of the Invention
[0013] According to the present invention, by using metallic nickel powder, it is possible to reduce the energy used for transportation and production, and to eliminate the complexity of the production process. As a result, it is possible to provide a method for producing a positive electrode active material for a lithium ion secondary battery with reduced GHG emissions. [Brief description of the drawings]
[0014] [Figure 1] 1 is a flowchart showing an example of a method for producing a positive electrode active material for a lithium ion secondary battery according to the present invention. [Diagram 2] FIG. 2 is a schematic diagram showing an example of production of metallic nickel powder by a water atomization method. [Diagram 3] 4 is a flowchart showing another example of the method for producing a positive electrode active material for a lithium ion secondary battery according to the present invention. [Figure 4] 4 is a flowchart showing another example of the method for producing a positive electrode active material for a lithium ion secondary battery according to the present invention. [Diagram 5] 1 is a scanning electron microscope (SEM) image of the positive electrode active material of Example 2. [Figure 6] 1 is an SEM image of the positive electrode active material of Example 3. [Figure 7] 1 is an SEM image of the positive electrode active material of Example 4. [Figure 8] 1 is an X-ray diffraction (XRD) pattern of Example 2. [Figure 9] 1 is an XRD pattern of Example 3. [Figure 10] 1 is an XRD pattern of Example 4. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] <Method of manufacturing positive electrode active material for lithium ion secondary battery> Hereinafter, a method for producing a positive electrode active material for a lithium ion secondary battery according to this embodiment (hereinafter referred to as a method for producing a positive electrode active material) will be described.
[0016] [Method of manufacturing metallic nickel powder] Before explaining the method for producing the positive electrode active material, a method for producing metallic nickel powder will be exemplified. In this embodiment, metallic nickel powder produced by, for example, the atomization method or the carbonyl method can be used. The atomization method or the carbonyl method is preferable because it is possible to obtain metallic nickel powder with a small amount of impurity elements. In order to avoid short-circuiting of the battery, high-purity raw materials are used for the battery components. In particular, since iron (Fe) is an impurity element that is likely to cause a short circuit, it is preferable that the Fe content of the metallic nickel powder is 100 ppm or less. More preferably, it is 30 ppm or less, and even more preferably, it is 10 ppm or less. In addition, high-purity briquettes and cathodes of grade Class I are suitable as high-purity nickel sources. In this embodiment, high-purity metallic nickel powder with few impurities is obtained without dissolving these briquettes and cathodes in acid.
[0017] Fig. 2 is a schematic diagram of the production of metallic nickel powder by the water atomization method. In this embodiment, the method is not limited to the water atomization method, but is shown as an example of the production method. Here, there is a first step in which nickel briquettes or cathodes are melted in a melting furnace 1 to obtain molten nickel 2, and a second step in which high-pressure water 3 is sprayed onto the molten nickel 2 to obtain metallic nickel powder 4 by an atomization method. Gas can also be used as the medium sprayed onto the molten nickel instead of high-pressure water. In that case, it is called a gas atomization method. By using these atomization methods, metallic nickel powder of high purity can be obtained.
[0018] This embodiment is characterized in that the metallic nickel powder is used as a raw material for the positive electrode active material without being dissolved in acid. At the stage of production by the atomization method, the metallic nickel powder is already partially oxidized. In order to promote the oxidation, the high pressure water 3 in FIG. 2 can be an acidic solution in addition to water. In addition to inert gas such as argon or nitrogen, gas containing oxygen may be used when injecting gas. The metallic nickel powder being partially oxidized by the atomization method means that, for example, the oxygen content is preferably 300 ppm or more. In addition, when the oxidation step is carried out separately, a mixed powder with a higher oxidation rate can be obtained. In this case, the oxygen concentration in the metallic nickel powder is preferably 3,000 ppm or more, more preferably 5,000 ppm or more, and even more preferably 10,000 ppm or more.
[0019] Another method for obtaining metallic nickel powder is the carbonyl process. In the carbonyl process, nickel briquettes or the like are reacted with carbon monoxide gas to obtain gaseous nickel carbonyl, which is then thermally decomposed under reduced pressure and low temperature to obtain metallic nickel powder. High-purity metallic nickel powder can also be obtained by using the carbonyl process.
[0020] The particle size of the metallic nickel powder is preferably in the range of several μm to several tens of μm. When the pulverization process is omitted during the production of the positive electrode active material, the average particle size D50 of the metallic nickel powder is preferably in the range of 5 to 30 μm, more preferably 5 to 20 μm, and even more preferably 5 to 15 μm. The particle size of the metallic nickel powder can be controlled by the injection pressure of the injected water or gas in the atomization method, and can be controlled by the thermal decomposition conditions in the carbonyl method. Powders exceeding 100 μm can be removed by sieve classification and returned to dissolution (recycled).
[0021] [Method of manufacturing positive electrode active material I] Hereinafter, a manufacturing method I of a positive electrode active material using the metallic nickel powder will be described. As shown in the flow chart of FIG. 1, this manufacturing method I includes a step of sintering a mixed powder obtained by mixing metallic nickel powder, a compound containing Li, and a compound containing a metal element M other than Li and Ni to obtain a positive electrode active material having a layered structure. In this embodiment, as described above, metallic nickel powder is used as the nickel raw material, so that an acid dissolution step and a coprecipitation step are not required. Furthermore, since metallic nickel powder is used as the nickel raw material, the volume handled in the transportation and manufacturing process of the positive electrode active material can be reduced compared to compounds such as nickel sulfate and nickel hydroxide. Specifically, when the Ni content per unit volume of each compound is expressed in mass%, nickel sulfate (Ni(SO)4·6H2O) is 5% and nickel hydroxide (Ni(OH)2) is 29%, while the Ni content of metallic nickel is 100%, and the Ni content per unit volume is high. As a result, in this embodiment, the volume handled in the transportation and manufacturing process of the positive electrode active material is about 1 / 20 compared to nickel sulfate and about 1 / 3 compared to nickel hydroxide, making it possible to reduce fuel consumption during transportation and improve production efficiency by saving space during production and reducing driving force. These things lead to a reduction in GHG emissions, and as a result, it is possible to manufacture the positive electrode active material while suppressing GHG. The Ni content per unit volume is preferably close to 100%, and for example, a metal nickel powder with a specific gravity of 8 g / cm 3 It is preferable that the metallic nickel powder contains metallic nickel and the remainder is in an oxidized state, and does not contain elements other than unavoidable impurities. In this case, the oxygen content of the metallic nickel powder is 7.3 mass % or less.
[0022] The composition of the positive electrode active material is not particularly limited, but the specific composition of this embodiment will be described later. Basically, if the ratio of Ni to all metal elements other than Li contained in the positive electrode active material is 60% or more in atomic ratio, the redox potential of Ni is relatively low, so that it is easy to develop high capacity at a predetermined potential and can meet the required battery characteristics. More preferably, it is 80% or more, which is preferable because an even higher capacity can be expected. In addition, since the ratio of nickel to all metal elements other than Li is 60% or more in atomic ratio, in the firing process, the firing reaction proceeds while lithium and the metal element M are diffused into the particles with each particle of the metal nickel powder as a nucleus, so it is considered that the powder properties of the positive electrode active material after firing can be easily controlled depending on the particle size of the metal nickel powder. In addition, the metal nickel powder used is at least partially oxidized. This is because at least a part of the metal nickel powder is oxidized at the stage before firing, so that the firing reaction to form a layered structure proceeds quickly when firing in an atmosphere containing oxygen.
[0023] Since the positive electrode active material is sintered in an oxygen-containing atmosphere to obtain a layered structure positive electrode active material for lithium ion secondary batteries, a step of oxidizing the metallic nickel powder may be actively introduced in order to perform the sintering reaction quickly. For example, an oxidation step may be separately provided in which the metallic nickel powder is exposed to an air atmosphere or thermally oxidized in the air or an oxidizing atmosphere. This will be explained with reference to the manufacturing method II. In addition, when the metallic nickel powder is manufactured by the water atomization method, heat drying is required, but this drying step can also serve as the oxidation step. In this case, the upper limit of the oxygen concentration in the metallic nickel powder is preferably determined in consideration of the amount of Ni per unit volume during transportation.
[0024] In FIG. 1, in the process of mixing metallic nickel powder, a compound containing lithium, and a compound containing a metal element M other than lithium and nickel to obtain a mixed powder, the metallic nickel powder can be used as it is as an atomized powder. The atomized powder may be pulverized to adjust to an appropriate particle size before use. In addition, lithium hydroxide and lithium carbonate can be used as the compound containing lithium. Considering reactivity with metals, lithium hydroxide having a low melting point is considered, but lithium hydroxide is a deleterious substance, so lithium carbonate is preferable in consideration of environmental and safety aspects. Next, examples of the compound containing a metal element M other than lithium and nickel include oxides, carbonates, hydroxides, phosphates, and the like. For convenience, the term "compound" also includes pure metals. Since the positive electrode active material is a composite oxide of lithium and metal, the raw material is preferably a pure metal, oxide, carbonate, or hydroxide. The metal element M is preferably an element containing at least one of, for example, Co, Mn, Al, Ti, Mg, Zr, Nb, and Mo. In addition, in consideration of the reactivity with the metallic nickel powder during the firing process, the average particle size of the compound containing the metal element M is preferably equal to or smaller than that of the metallic nickel powder.
[0025] The raw material powders are mixed using a V-type mixer, stirring mixer, attritor, media mill, etc. In order to mix uniformly, it is preferable to be able to break down the agglomerates of each raw material powder. The mixing method may be either a dry method in which only the raw material powders are mixed, or a wet method in which a liquid is used as a dispersion medium.
[0026] Next, the mixed powder is sintered to obtain a layered positive electrode active material in a sintering step. An electric furnace or a gas furnace is used for sintering the mixed powder. The sintering atmosphere preferably contains 20% or more oxygen by volume, and when the Ni content is 80% or more of the total metal elements, the oxygen concentration is preferably 90% or more. The firing process preferably includes a pre-firing stage held at 450° C. to 730° C., and a main firing stage held at 750° C. to 900° C. The preferred firing temperature and holding time are adjusted according to the composition blended during raw material mixing, and firing is performed so that the physical properties (specific surface area, etc.) of the target positive electrode active material after firing fall within a preferred range.
[0027] In this embodiment, the metallic nickel powder is at least partially oxidized and the oxidized metallic nickel powder is used in the process of sintering the mixed powder and obtaining a layered structure positive electrode active material for lithium ion secondary batteries. This may be expressed as partially containing an oxide. This may be an acidic solution or an oxygen-containing gas as described in the process of obtaining metallic nickel powder, an oxidizing medium may be used in the process of obtaining the mixed powder, and an oxidizing process may be provided or an oxidizing atmosphere may be exposed in the sintering process. In addition, a process of exposing the metallic nickel powder to at least the air atmosphere may be added when moving between each process.
[0028] [Method of manufacturing positive electrode active material II] Next, a manufacturing method II of a positive electrode active material using the metallic nickel powder described above will be described. As shown in the flow charts of FIG. 3 and FIG. 4, this manufacturing method II is characterized in that metallic nickel powder and a compound containing at least lithium are mixed, and an oxidation step is performed on this mixed powder. That is, the positive electrode active material is obtained by firing in an atmosphere containing oxygen to obtain a layered structure positive electrode active material, but this manufacturing method differs from manufacturing method I in that an oxidation step is introduced in which metallic nickel powder is actively oxidized in order to rapidly perform the firing reaction. The oxidation step is preferably performed in an oxidizing atmosphere because the time required for the oxidation treatment is short. Furthermore, in the case of thermal oxidation, the temperature is preferably about 100 to 700°C, preferably 400 to 680°C, and more preferably 600 to 680°C. This is because the oxidation rate is increased by setting the temperature at 600 to 680°C. Moreover, the oxidation rate by the oxidation step is preferably 50% or more, and more preferably 65% or more. If the oxidation rate is high and there is little residual metallic nickel component after oxidation, the powder is easily pulverized in the subsequent pulverizing and mixing step, and a pulverized mixed powder of a predetermined pulverized particle size can be obtained in the pulverizing and mixing step described below.
[0029] In addition, when the metallic nickel powder and the lithium-containing compound are mixed and then the oxidation step is carried out, the lithium-containing compound acts as an inclusion, which can prevent the metallic nickel powder from sintering with itself, and the powder state can be maintained even after the oxidation step, which is preferable. In addition, the amount of the lithium-containing compound mixed with the metallic nickel powder is preferably 25 mass% or more of the lithium-containing compound used in the production. This is because by mixing 25 mass% or more and then carrying out thermal oxidation, the metallic nickel powder can be prevented from sintering with itself.
[0030] The lithium-containing compound preferably has a melting point higher than the thermal oxidation temperature. If the melting point of the lithium-containing compound is higher than the thermal oxidation temperature, sintering of the metallic nickel powders in the oxidation step can be prevented. Therefore, the lithium-containing compound used in this manufacturing method is preferably lithium carbonate. The melting point of lithium carbonate is 724°C, which allows the thermal oxidation temperature to be as high as 720°C, preventing sintering of the powders and shortening the oxidation step. The average particle size of the Li-containing compound is preferably several μm to several hundreds μm, and more preferably several μm to several tens of μm.
[0031] The particle size of the metallic nickel powder is preferably in the range of several μm to several tens of μm, as described above in the production of metallic nickel powder. However, in this production method II, the metallic nickel powder has an average particle size of preferably 5 to 30 μm, more preferably 5 to 20 μm, and even more preferably 5 to 15 μm, in order to enable uniform mixing of the metallic nickel powder and the lithium-containing compound in the mixing step and to increase the oxidation rate in the oxidation step.
[0032] Next, a compound containing lithium and a metal element M other than nickel is mixed. When an oxidation step is introduced, after the oxidation step, as shown in Fig. 3, an oxide powder containing oxidized metallic nickel powder and a compound containing lithium and a metal element M other than nickel are mixed to obtain a mixed powder. Note that the oxidation step may be performed on a mixed powder obtained by mixing a metallic nickel powder and a compound containing lithium with a compound containing lithium and further mixing the compound containing lithium and a metal element M other than nickel, as shown in Fig. 4. However, in terms of reducing the amount of processing in the oxidation step, the step of mixing a compound containing lithium and a metal element M other than nickel after the oxidation step shown in Fig. 3 is preferable. The compound containing a metal element M other than Li and Ni is similar to that in Production Method I, and therefore a description thereof will be omitted, but the composition of the positive electrode active material will be exemplified below.
[0033] Next, a process of pulverizing and mixing the mixed powder containing the oxide powder is introduced for the purpose of promoting the firing reaction (this process may be called a mixing and pulverizing process). This process corresponds to the process of obtaining the mixed powder in the manufacturing method I. The pulverization and mixing can be carried out using an attritor, a media mill, etc. It is preferable to use a media mill, and it is more preferable to use a bead mill, since the mixed powder can be pulverized to submicron size.
[0034] The D50 of the primary particles of the mixed powder (pulverized mixed powder) after pulverization and mixing is preferably 0.17 μm or less. When the D50 of the primary particles is 0.17 μm or less, the sintering reaction is promoted and the voids in the positive electrode active material are suppressed. As a result, the particle strength of the positive electrode active material is high and the cycle characteristics are good. In addition, the D95 of the primary particles of the pulverized mixed powder is preferably 0.26 μm or less. When the D95 of the primary particles is 0.26 μm or less, the sintering reaction is promoted and the voids in the positive electrode active material are suppressed. As a result, the particle strength of the positive electrode active material is high and the cycle characteristics are good.
[0035] The specific surface area of the pulverized mixed powder is 28m 2 The specific surface area of the pulverized mixed powder is preferably 28 m 2 When the sintering rate is 1 / g or more, the firing reaction is promoted and the generation of voids in the positive electrode active material is suppressed, resulting in high particle strength of the positive electrode active material and good cycle characteristics.
[0036] Next, a firing step of firing the mixed powder or the pulverized mixed powder to obtain a layered structure positive electrode active material for a lithium ion secondary battery will be described. The raw material mixed powder or pulverized mixed powder is fired in an electric furnace or gas furnace. The firing atmosphere preferably contains 20% or more oxygen by volume, and when the Ni content is 80% or more of the total metal elements, the oxygen concentration is preferably 90% or more. The firing process includes a pre-firing stage in which the temperature is maintained at 450° C. to 730° C., and a main firing stage in which the temperature is maintained at 750° C. to 900° C. The preferred firing temperature and holding time are adjusted according to the composition blended during raw material mixing, and firing is performed so that the physical properties (specific surface area, etc.) of the target positive electrode active material are within a preferred range after firing.
[0037] For the purpose of removing impurities, the synthesized lithium transition metal composite oxide may be subjected to a washing step of washing with deionized water or the like, a drying step of drying the washed lithium transition metal composite oxide, etc., after the firing step. The synthesized lithium transition metal composite oxide may also be subjected to a crushing step of crushing the lithium transition metal composite oxide, a classification step of classifying the lithium transition metal composite oxide into a predetermined particle size, etc.
[0038] Next, the composition of the positive electrode active material of this embodiment will be described. As described above, the composition of the positive electrode active material of this embodiment is not particularly limited, but a preferred composition will be described below. First, the positive electrode active material according to this embodiment is represented by the following formula (1). Li 1+a NiMO 2+α (1) (In the formula (1), M is a metal element other than Li and Ni, the proportion of Ni in all metal elements is 60 atomic % or more, and a and α are numbers that satisfy -0.1≦a≦0.2 and -0.2≦α≦0.2.)
[0039] The positive electrode active material according to this embodiment has a composition in which the ratio of Ni to all metal elements other than Li is 60 atomic % or more, and thus can realize a high energy density and a high charge / discharge capacity. The ratio of Ni to all metal elements other than Li can be an appropriate value within the range of 60 atomic % or more and 100 atomic % or less. Since the positive electrode active material contains nickel at such a high ratio, Ni 2+ Ni 3+ It is important that the oxidation reaction to oxidize to is carried out efficiently.
[0040] A more preferred specific composition of the positive electrode active material according to this embodiment is represented by formula (2). Li 1+a Ni b Co c M1 d X e O 2+α (2) [wherein, in formula (2), M1 represents at least one selected from Al and Mn, X represents one or more metal elements other than Li, Ni, Co, Al, and Mn, and a, b, c, d, e, and α are numbers that respectively satisfy -0.1≦a≦0.2, 0.7≦b≦1.0, 0≦c≦0.20, 0≦d≦0.20, 0≦e≦0.1, b+c+d+e=1, and -0.2<α<0.2.]
[0041] The positive electrode active material represented by the formula (2) has a high Ni content and therefore can exhibit a higher charge / discharge capacity than LiCoO2, etc., in the range up to about 4.3 V. In addition, since the Ni content is high, the raw material cost is lower than LiCoO2, etc., and the raw materials are easily available, making this a positive electrode active material.
[0042] Here, the meanings of the numerical ranges of a, b, c, d, e and α in the above formulas (1) and (2) will be explained.
[0043] In the formula, a is -0.1 or more and 0.2 or less. a represents the stoichiometric ratio of the lithium composite compound represented by the general formula LiM'O2, that is, the amount of lithium deficiency or excess from Li:M':O=1:1:2. If the amount of lithium is too small, the charge / discharge capacity of the positive electrode active material decreases. On the other hand, if the amount of lithium is too large, the charge / discharge cycle characteristics deteriorate. If a is within the above numerical range, it is possible to achieve both a high charge / discharge capacity and good charge / discharge cycle characteristics.
[0044] a may be -0.02 or more and 0.07 or less. If a is -0.02 or more, a sufficient amount of lithium is secured to contribute to charging and discharging, so that the charge and discharge capacity of the positive electrode active material can be increased. If a is 0.07 or less, charge compensation due to the valence change of the transition metal is sufficiently performed, so that both high charge and discharge capacity and good charge and discharge cycle characteristics can be achieved.
[0045] The coefficient b of nickel is 0.7 or more and 1.0 or less. When b is 0.7 or more, a sufficiently high charge / discharge capacity can be obtained compared to the case where other transition metals are used. Therefore, when b is in the above-mentioned numerical range, a positive electrode active material exhibiting a high charge / discharge capacity can be produced at a low cost compared to LiCoO2, etc.
[0046] b is preferably 0.8 or more and 0.95 or less, more preferably 0.85 or more and 0.95 or less. The larger b is 0.8 or more, the higher the charge / discharge capacity can be obtained. Also, the smaller b is 0.95 or less, the smaller the lattice distortion or crystal structure change associated with the insertion or desorption of lithium ions becomes, and the less likely the cation mixing in which nickel is mixed into the lithium site or the decrease in crystallinity occurs during firing, so that the deterioration of the charge / discharge capacity and the charge / discharge cycle characteristics is suppressed.
[0047] The coefficient c of cobalt is 0 or more and 0.20 or less. When cobalt is added, the crystal structure is stabilized, and the effect of suppressing cationic mixing in which nickel is mixed into the lithium site is obtained. Therefore, the charge-discharge cycle characteristics can be improved without significantly impairing the charge-discharge capacity. On the other hand, if the cobalt is excessive, the raw material cost increases, and the manufacturing cost of the positive electrode active material increases. If c is in the above numerical range, it is possible to achieve both high charge-discharge capacity and good charge-discharge cycle characteristics with good productivity.
[0048] c may be 0.01 or more and 0.20 or less, or 0.03 or more and 0.20 or less. The larger c is 0.01 or more, the more sufficient the effect of the elemental substitution of cobalt is obtained, and the more improved the charge-discharge cycle characteristics are. In addition, if c is 0.20 or less, the raw material cost becomes cheaper, and the productivity of the positive electrode active material becomes better.
[0049] The coefficient d of M1 is 0 or more and 0.20 or less. When at least one element (M1) selected from the group consisting of manganese and aluminum is substituted, the layered structure is more stable even if lithium is released by charging. On the other hand, when these elements (M1) are excessive, the ratio of other transition metals such as nickel is reduced, and the charge / discharge capacity of the positive electrode active material is reduced. When d is within the above-mentioned numerical range, the crystal structure of the positive electrode active material is kept stable, and good charge / discharge cycle characteristics, thermal stability, etc. can be obtained in addition to a high charge / discharge capacity.
[0050] Manganese is particularly preferred as the element represented by M1. When manganese is substituted as an element, a higher charge / discharge capacity can be obtained compared to when aluminum is substituted as an element. In addition, when the lithium composite compound is sintered, manganese also reacts with lithium carbonate as shown in the following formula (3). This reaction suppresses the coarsening of crystal grains and allows the oxidation reaction of nickel to proceed at high temperatures, so that a positive electrode active material exhibiting a high charge / discharge capacity can be efficiently obtained.
[0051] Li2CO3+2M´O+0.5O2→2LiM´O2+CO2···(3) (In the formula (3), M' represents a metal element such as Ni, Co, or Mn.)
[0052] The coefficient d of M1 is preferably 0.02 or more, more preferably 0.04 or more. The larger the coefficient d of M1, the more sufficient the effect of element substitution with at least one element selected from the group consisting of manganese and aluminum can be obtained. When M1 is manganese, it is possible to proceed with the oxidation reaction of nickel at a higher temperature, and a positive electrode active material exhibiting a high charge / discharge capacity can be obtained more efficiently. In addition, the coefficient d of M1 is preferably 0.18 or less. If the coefficient d of M1 is 0.18 or less, the charge / discharge capacity is kept high even if the element is substituted.
[0053] The coefficient e of X is 0 or more and 0.10 or less. X represents one or more metal elements other than Li, Ni, Co, Al, and Mn, and when at least one element selected from the group consisting of magnesium, titanium, zirconium, molybdenum, and niobium is substituted, various performances such as charge-discharge cycle characteristics can be improved while maintaining the activity of the positive electrode active material. On the other hand, if these elements (X) are excessive, the ratio of other transition metals such as nickel decreases, and the charge-discharge capacity of the positive electrode active material decreases. If e is within the above numerical range, it is possible to achieve both high charge-discharge capacity and good charge-discharge cycle characteristics.
[0054] In the formulas (1) and (2), α is set to be −0.2 or more and 0.2 or less. α represents the stoichiometric ratio of the lithium composite compound represented by the general formula LiM′O2, that is, the amount of oxygen in excess or deficiency from Li:M′:O=1:1:2. When α is within the above-mentioned numerical range, the crystal structure has few defects, and a high charge / discharge capacity and good charge / discharge cycle characteristics can be obtained. EXAMPLES
[0055] The present invention will be specifically described below with reference to examples, but the technical scope of the present invention is not limited thereto. The measurement means for the characteristic values and the preliminary experiment of the oxidation process will be described below, and then the examples will be described.
[0056] (Average particle size, specific surface area) The D50 and D95 of the primary particles of the pulverized mixed powder and the secondary particles of the fired powder of the positive electrode active material were measured using a laser diffraction particle size distribution analyzer. The specific surface area was measured by the BET method using gas adsorption with an automatic specific surface area measurement device.
[0057] (Oil absorption amount) The oil absorption of the powder sample was measured according to JIS K5101-13-1, and NMP (N-methylpyrrolidone) was used as the solvent. 5.0 g of the powder sample was weighed out and placed in a mountain shape on a flat tray. NMP was sucked up with a poly dropper (2 mL capacity) and the mass was measured. Next, NMP was dropped onto the powder sample while kneading with a spatula, and the dropping and kneading were continued until the powder sample became clay-like overall. When there was an excess of NMP, it was visible that the droplets were not absorbed by the powder sample and remained on the surface, and the amount of NMP dropped up to this point was converted to the oil absorption per 100 g of powder sample.
[0058] (X-ray diffraction pattern) The X-ray diffraction (XRD) pattern in the X-ray powder diffraction measurement of the positive electrode active material was measured using an X-ray diffractometer "X'Pert PRO MPD" (PANalyticalsei) under the conditions of a CuKα radiation source, a tube voltage of 45 kV, a tube current of 40 mA, a sampling interval of 0.02° / step, a divergence slit of 0.5°, a scattering slit of 0.5°, a receiving slit of 0.15 mm, and a scanning range of 15°≦2θ≦80°.
[0059] [Oxidation process of metallic nickel powder] (Preliminary experiment 1) Metallic nickel powder (manufactured by Nippon Atomize Processing) produced by the water atomization method with D50 of 8 μm and lithium carbonate were weighed so that the molar ratio of metal elements was Li:Ni, 1.03:0.85. A total of 5 kg of these raw material powders were put into a V-shaped mixer with a volume of 45 L and mixed for 90 minutes to obtain a raw material mixed powder. Next, this raw material mixed powder was heat-treated at 650 °C for 10 hours in a sintering furnace in an air atmosphere to obtain an oxidized powder. The weight of the obtained oxidized powder was 18% greater than that of the raw material mixed powder. From this weight increase rate, it was confirmed that 70% of the metallic nickel powder was nickel oxide. In other words, the oxidation rate was 70%. In addition, some of the oxidized powder was caked. This was crushed in a mortar to obtain an oxidized powder with D50 of 8 μm.
[0060] (Preliminary experiment 2) Except for using metallic nickel powder (manufactured by Vale) produced by the carbonyl method with a D50 of 8 μm, the same oxidation process as in preliminary experiment 1 was carried out to obtain an oxidized powder with a D50 of 8 μm. The oxidation rate of this metallic nickel powder was 70%.
[0061] (Preliminary experiment 3) Except for using metallic nickel powder with a D50 of 67 μm, the same oxidation process as in Preliminary Experiment 1 was carried out to obtain oxidized powder with a D50 of 32 μm. The oxidation rate of this metallic nickel powder was 10%.
[0062] Preliminary experiments 1, 2, and 3 showed that when the D50 of the metallic nickel powder is small, the oxidation rate is high, and when the D50 is at least 8 μm or less, an oxidized powder with a high oxidation rate of 70% or more can be obtained.
[0063] (Preliminary experiment 4) The same oxidation process as in Preliminary Experiment 1 was carried out, except that the metallic nickel powder and lithium carbonate were weighed out so that the molar ratio of the metallic elements was Li:Ni 0.26:0.85. Although some of the oxidized powder was caked, oxidized powder with a D50 of 8 μm was obtained by crushing it in a mortar. Note that the metallic nickel powder and lithium carbonate with a molar ratio of the metallic elements Li:Ni 0.26:0.85 means that the metallic nickel powder and 25 mass% of the lithium-containing compound used in the production were mixed.
[0064] (Preliminary experiment 5) Metallic nickel powder and lithium carbonate were weighed out so that the molar ratio of the metal elements, Li:Ni, was 0:0.85. In other words, only metallic nickel was oxidized. The rest of the oxidation process was the same as in Preliminary Experiment 1. The metallic nickel powder was sintered and could not be crushed in a mortar.
[0065] Preliminary experiments 1, 4, and 5 confirmed that sintering of metallic nickel powder can be prevented by mixing metallic nickel powder with 25 mass% or more of the lithium-containing compounds used in production and then performing an oxidation treatment.
[0066] [Example 1] In Example 1, manufacturing method I was carried out. That is, a plate-shaped metallic nickel having an Fe content of 30 ppm was melted in a melting furnace, and a metallic nickel powder having an average particle size of 8 μm was obtained by a water atomization method in which high-pressure water was sprayed onto the molten nickel that had flowed out and fallen. The oxygen content of this metallic nickel powder was measured with an oxygen / nitrogen analyzer and found to be 3,000 ppm. In addition to the obtained metallic nickel powder, the following raw materials were prepared. Lithium hydroxide was prepared as a compound containing lithium, and cobalt oxide, manganese oxide, and titanium oxide were prepared as compounds containing a metallic element M other than lithium and nickel. Each raw material was weighed so that the molar ratio of the metallic elements was Li:Ni:M of 1.03:0.85:0.15. A total of 5 kg of these raw material powders were charged into a V-type mixer with a volume of 45 L and mixed for 90 minutes to obtain a raw material mixed powder. Next, this raw material mixed powder was pre-calcined in an oxygen gas atmosphere in a sintering furnace at 500°C for 10 hours in an oxygen stream, and then sintered at 820°C for 10 hours. Between each step, the metallic nickel powder was transported in an environment exposed to the air, without being enclosed in a vacuum or non-oxidizing atmosphere. As a result, a positive electrode active material made of a lithium metal composite oxide was obtained.
[0067] In Example 1, the positive electrode active material mainly composed of nickel was produced using metallic nickel powder, thereby reducing impurities. In addition, in the conventional coprecipitation process, nickel bullion is processed into a water-soluble compound such as nickel sulfate, and then processed into an aqueous solution of nickel sulfate (acid dissolution process), and further, nickel hydroxide powder is produced from this aqueous solution of nickel sulfate by coprecipitation (coprecipitation process), and this nickel hydroxide powder is used as a precursor. In this embodiment, metallic nickel powder produced directly from nickel bullion without processing into compounds such as nickel sulfate and nickel hydroxide is used as a precursor. Therefore, the acid dissolution process and the coprecipitation process are not necessary, and the positive electrode active material can be produced easily. In addition, the volume handled in the transportation and manufacturing process of the positive electrode material can be reduced.
[0068] [Example 2] In Example 2, manufacturing method II was carried out. That is, lithium carbonate, metallic nickel powder, cobalt carbonate, manganese carbonate, titanium oxide, and aluminum oxide were prepared as raw materials, and each raw material was weighed so that the molar ratio of metal elements Li:Ni:Co:Mn:Ti:Al was 1.03:0.85:0.03:0.09:0.03:0.01. For the metallic nickel powder, metallic nickel powder with D50 of 8 μm produced by the water atomization method described above was used. First, metallic nickel powder and lithium carbonate were put into a V-type mixer and mixed for 90 minutes to obtain a raw material mixed powder. Next, this raw material mixed powder was oxidized in a sintering furnace in an air atmosphere at 650°C for 10 hours (oxidation process) to obtain an oxidized powder containing oxidized metallic nickel powder. The obtained oxidized powder was mixed with metal element M consisting of cobalt carbonate, manganese carbonate, titanium oxide, and aluminum oxide, and pure water was added to this so that the solid content ratio was 30 mass%. Then, a raw material slurry was prepared by wet pulverization (wet mixing) in a pulverizer so that the primary particle D50 was 0.30 μm (pulverization and mixing process). Next, the obtained raw material slurry was spray-dried with a nozzle-type spray dryer (Okawahara Kakoki Co., Ltd., ODL-20 type) to obtain granules with D50 of about 10 μm (granulation process). The dried granules were then fired to obtain a lithium transition metal composite oxide (fired process). Specifically, the sample was pre-fired at 700°C for 24 hours in an oxygen gas atmosphere in a firing furnace. The sample was then fired at 840°C for 10 hours in an oxygen gas atmosphere in a firing furnace, to obtain a lithium transition metal composite oxide. The fired powder obtained by the firing process was classified using a sieve with a mesh size of 53 μm, and the powder that fell under the sieve was used as the positive electrode active material of the sample.
[0069] [Example 3] A positive electrode active material was produced in the same manner as in Example 2, except that a raw material slurry was prepared by wet pulverization (wet mixing) using a pulverizer so that the D50 of the primary particles was 0.17 μm.
[0070] [Example 4] A positive electrode active material was produced in the same manner as in Example 2, except that a raw material slurry was prepared by wet pulverization (wet mixing) using a pulverizer so that the D50 of the primary particles was 0.13 μm.
[0071] The specific surface areas of the granules of Examples 2 to 4 were measured. The results are shown in Table 1. The positive electrode active materials of Examples 2 to 4 were also subjected to SEM observation and X-ray diffraction measurement. The photographs are shown in Figs. 5 to 7. The X-ray diffraction patterns are shown in Figs. 8 to 10. Furthermore, the specific surface areas and oil absorption amounts of the positive electrode active materials of Examples 2 to 4 were measured. The results are also shown in Table 1.
[0072] (Preparation of positive electrode) Next, a lithium ion secondary battery was produced using the synthesized positive electrode active material as a positive electrode material, and the discharge capacity and capacity retention rate of the lithium ion secondary battery were measured. First, the produced positive electrode active material, a carbon-based conductive material, and a binder dissolved in advance in N-methyl-2-pyrrolidone (NMP) were mixed in a mass ratio of 94:4.5:1.5. Then, the uniformly mixed positive electrode mixture slurry was applied to a positive electrode current collector made of aluminum foil with a thickness of 15 μm in an amount of 13 mg / cm. 2 The positive electrode mixture slurry applied to the positive electrode current collector was then heat-treated at 120°C to remove the solvent, thereby forming a positive electrode mixture layer. The positive electrode mixture layer was then pressurized by a hot press and punched into a circular shape with a diameter of 15 mm to form a positive electrode.
[0073] (Initial capacity, charge / discharge cycle characteristics (capacity retention rate)) Next, a lithium ion secondary battery was produced using the produced positive electrode, negative electrode, and separator. Metallic lithium punched into a circle with a diameter of 16 mm was used as the negative electrode. A porous separator made of polypropylene with a thickness of 30 μm was used as the separator. The positive electrode and the negative electrode were opposed to each other in a non-aqueous electrolyte via the separator, and a lithium ion secondary battery was assembled. As the non-aqueous electrolyte, a solution was used in which LiPF6 was dissolved at 1.0 mol / L in a solvent in which ethylene carbonate and dimethyl carbonate were mixed at a volume ratio of 3:7.
[0074] The lithium ion secondary battery thus prepared was charged at a constant current / constant voltage of 38A / kg based on the weight of the positive electrode mixture and an upper limit potential of 4.3V in an environment of 25°C. Then, the battery was discharged to a lower limit potential of 2.5V at a constant current of 40A / kg based on the weight of the positive electrode mixture, and the charge capacity and discharge capacity were measured. Then, the battery was charged at a constant current / constant voltage of 190A / kg based on the weight of the positive electrode mixture and an upper limit potential of 4.3V. Then, a total of 30 cycles of discharge to a lower limit potential of 2.5V at a constant current of 190A / kg based on the weight of the positive electrode mixture were performed, and the discharge capacity after 30 cycles was measured. The ratio of the discharge capacity after 10 cycles to the initial capacity was calculated as the capacity retention rate. The results are shown in Table 1.
[0075] [Table 1-1]
[0076] [Table 1-2]
[0077] 5 to 7, it was found that the secondary particle diameter of the positive electrode active materials of Examples 2 to 4 was about 10 μm and the primary particle diameter was about 400 nm. In addition, compared with the positive electrode active material of Example 2 in which the D50 of the primary particles of the mixed powder (pulverized mixed powder) after pulverization and mixing was 0.30 μm, the positive electrode active materials of Examples 3 and 4 in which the D50 of the primary particles of the mixed powder (pulverized mixed powder) after pulverization and mixing was 0.17 μm or less had fewer voids, and it was confirmed that when the D50 of the primary particles of the mixed powder (pulverized mixed powder) after pulverization and mixing was 0.17 μm or less, the firing reaction was promoted and the voids in the positive electrode active material could be suppressed.
[0078] From the XRD patterns in FIGS. 8 to 10, the positive electrode active materials of Examples 2 to 4 all exhibited peaks assigned to the 003 plane near 2θ=18°, the 101 plane near 2θ=36°, the 006 plane and the 012 plane near 2θ=38°, the 104 plane near 2θ=44°, the 015 plane near 2θ=48°, and the 107 plane near 2θ=58°. This confirmed that the positive electrode active materials belonged to the space group R3-m and were lithium metal composite oxides with a layered structure.
[0079] As can be seen from Table 1, the positive electrode active materials of Examples 2 to 4 have high capacities, such as a charge capacity of 222 Ah / kg and a discharge capacity of 195 Ah / kg or more. In addition, the capacity retention rate is 81% or more, and the cycle characteristics are good. In other words, it was confirmed that the method for producing a positive electrode active material of the present invention can obtain a positive electrode active material with high capacity and good cycle characteristics using metallic nickel powder as a raw material without processing it into compounds such as nickel sulfate or nickel hydroxide. In addition, the primary particles after pulverization and mixing have D50 of 0.17 μm or less, D95 of 0.26 μm or less, and a specific surface area of 28 m 2 It was confirmed that the capacity retention rates of the positive electrode active materials of Examples 3 and 4, which had a capacity retention rate of 84% or more / g or more, were even better.
[0080] From the above, in this embodiment, the nickel raw material does not need to be processed into compounds such as nickel sulfate and nickel hydroxide, compared to the conventional coprecipitation process. In other words, an acid dissolution process and a coprecipitation process are not required, and the positive electrode active material can be manufactured easily. In addition, since the positive electrode active material can be manufactured by directly using metallic nickel powder or by oxidizing the metallic nickel powder without going through compounds such as nickel sulfate and nickel hydroxide, the manufacturing process is short and the transportation between manufacturing processes is small. Furthermore, metallic nickel powder has a high nickel content and a large specific gravity compared to nickel sulfate, nickel hydroxide, etc., so the volume to be transported is small, and the energy required for transportation can be reduced. As a result, greenhouse gas (GHG) emissions can be reduced by about 30 to 40%, and as a result, the positive electrode active material can be manufactured while suppressing GHG emissions. [Explanation of symbols]
[0081] 1: Melting furnace 2: Molten nickel 3: High pressure water jet 4: Metallic nickel powder
Claims
1. Metallic nickel powder; A compound containing lithium; a mixing step of mixing the lithium and the compound containing a metal element M other than nickel to obtain a mixed powder; an oxidation step of oxidizing the metallic nickel powder of the mixed powder to an oxidation rate of 50% or more; A grinding and mixing step of grinding the oxide powder containing the oxidized metallic nickel powder to obtain a ground and mixed powder; and a calcination step of calcining the pulverized mixed powder to obtain a layered structure positive electrode active material for a lithium ion secondary battery in which a ratio of Ni to all metal elements other than Li is 60 atomic % or more, wherein the lithium-containing compound is lithium carbonate, and the oxidation step is carried out at a temperature equal to or lower than a melting point of lithium carbonate.
2. 2. The method for producing a positive electrode active material for a lithium ion secondary battery according to claim 1, characterized in that, in the oxidation step, the metallic nickel powder is oxidized while preventing sintering of the metallic nickel powder with each other by using a compound containing lithium having a melting point higher than a thermal oxidation temperature of the oxidation step.
3. 3. The method for producing a positive electrode active material for a lithium ion secondary battery according to claim 1, wherein the pulverized mixed powder has a primary particle D50 of 0.17 μm or less after the pulverization and mixing step.
4. The specific surface area of the primary particles of the pulverized mixed powder after the pulverization and mixing step is 28 m 2 3. The method for producing a positive electrode active material for a lithium ion secondary battery according to claim 1, wherein the active material has a molecular weight of 1 / g or more.
Citation Information
Patent Citations
Preparation method for environmentally-friendly lithium battery cathode material
CN108923038A
Positive electrode active material for lithium secondary battery and its manufacturing method
JP2011113869A
Nickel cobalt manganese composite hydroxide, and method for manufacturing the same
JP2015002120A
Production method of cathode active material for lithium ion secondary battery
JP2018088310A
Method for manufacturing positive electrode active material for lithium ion secondary battery, and positive electrode active material for lithium ion secondary battery