Dispersants, dispersions and ink compositions, and methods of making same

A styrene-ethyleneoxy group-containing (meth)acrylic acid copolymer addresses the issues of poor dispersion and redispersibility in inks by providing stable and efficient dispersion of disperse dyes and pigments, ensuring they remain dispersed and easily redispersible.

JP7559912B1Active Publication Date: 2024-10-02NISSHIN CHEM IND CO LTD
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2023201961
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-11-29
Publication Date
2024-10-02
Estimated Expiration
2043-11-29

AI Technical Summary

Technical Problem

Existing dispersants for disperse dyes and pigments in inks require longer dispersion times, exhibit poor dispersion ability, and lack effective redispersibility, leading to aggregation and poor stability when the water content is lost.

Method used

A styrene-ethyleneoxy group-containing (meth)acrylic acid copolymer is used as a dispersant, formulated with specific monomer ratios and neutralized with a basic compound, to achieve efficient dispersion and redispersibility of disperse dyes and pigments in aqueous solvents.

Benefits of technology

The copolymer allows for stable dispersion and redispersibility of disperse dyes and pigments with improved wettability, even with small amounts, maintaining dispersion stability and preventing aggregation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007559912000001
    Figure 0007559912000001
  • Figure 0007559912000002
    Figure 0007559912000002
  • Figure 0007559912000003
    Figure 0007559912000003
Patent Text Reader

Abstract

The present invention aims to provide a dispersant that can disperse disperse dyes or pigments even in a small amount and that can exhibit wettability, a dispersion that can exhibit redispersibility, and an ink composition using these, as well as methods for producing these. [Solution] The present invention provides a dispersant, dispersion and ink composition, characterized in that it contains (A) a styrene-ethyleneoxy group-containing (meth)acrylic acid copolymer having a weight average molecular weight of 1,000 to 50,000, (a1) a copolymer having a styrene content of 1 to 40 mass%, and the surfactant content is less than 0.1 mass%, as well as methods for producing these.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a dispersant used for dispersing disperse dyes and pigments, a dispersion and an ink composition, and methods for producing these. [Background technology]

[0002] Conventionally, disperse dyes and pigments have been used as colorants for inks. When using disperse dyes and pigments in inks, the finely divided disperse dyes and pigments must be dispersed in water. However, since disperse dyes and pigments are insoluble in water, it is important to keep the disperse dyes and pigments in a dispersed state and stable for a long period of time.

[0003] Furthermore, inks containing water-insoluble colorants such as disperse dyes and pigments have the disadvantage that when they lose the moisture they contain for some reason and become dry, the pigment's dispersion state is broken and the pigment aggregates. Once the disperse dyes or pigments in the ink aggregate in this way, they cannot be returned to a dispersed state even by adding a liquid medium such as water (poor redispersibility), and there is a strong demand for an improvement in this regard.

[0004] As dispersants for ink, nonionic surfactants, anionic surfactants, polymeric surfactants, etc. have been proposed in the past. For example, Patent Document 1 and Patent Document 2 disclose that nonionic surfactants containing an acetylene group are useful as pigment dispersants. However, although nonionic surfactants containing an acetylene group are excellent in ink penetration and foam suppression, they have inferior dispersing ability compared to other dispersants, requiring a long time for dispersion, and no redispersion effect can be expected.

[0005] As a method for facilitating redispersion of pigments, for example, Patent Document 3 proposes a method in which the surface of pigment particles is coated with a silane coupling agent or a specific dispersant to suppress direct contact between pigment particles and strong aggregation and adhesion.

[0006] In addition, Patent Document 4 and Patent Document 5 disclose that a pigment dispersion using an acrylic polymer enhances the redispersibility of the ink, but the process is complicated, requiring crosslinking of the polymer in the pigment aqueous dispersion and living radical polymerization, etc. Therefore, there is a demand for the development of a dispersant that can be expected to more easily achieve the redispersion effect.

[0007] Furthermore, Patent Document 6 discloses a dispersion resin having a hydrophobic monomer, an acrylic monomer, and a hydrophilic vinyl monomer having a sulfonic acid group, but because the proportion of the hydrophobic monomer is high, the dispersion effect may not be achieved in aqueous inks.

[0008] Patent Document 7 discloses that an inkjet ink using a styrene-(meth)acrylic acid copolymer in combination with a specific acetylene glycol compound has high-quality and stable recording performance, and can increase the print density on the fabric surface while maintaining the storage stability of the ink. However, it does not explicitly state redispersibility after drying.

[0009] In addition, the present inventors have previously filed an application for an invention relating to a dispersant using a styrene-ethyleneoxy group-containing (meth)acrylic acid copolymer in combination with an acetylene surfactant (Patent Application No. 2022-155738). This dispersant can exhibit redispersibility, but since the effect is exhibited by using the two components in combination, there was room for further improvement in the styrene-ethyleneoxy group-containing (meth)acrylic acid copolymer. [Prior art documents] [Patent documents]

[0010] [Patent Document 1] JP 2000-290578 A [Patent Document 2] JP 2002-020673 A [Patent Document 3] International Publication No. 2013 / 008691 [Patent Document 4] JP 2019-210389 A [Patent Document 5] JP 2019-014879 A [Patent Document 6] Patent Publication No. 2022-052994 [Patent Document 7] International Publication No. 2014 / 129323 Summary of the Invention [Problem to be solved by the invention]

[0011] The present invention has been made in view of the above circumstances, and has an object to provide a dispersant that can disperse disperse dyes or pigments even in a small amount added and that can exhibit wettability, a dispersion that can exhibit redispersibility, and an ink composition using these, as well as methods for producing these. [Means for solving the problem]

[0012] As a result of intensive research conducted by the present inventors to achieve the above object, they discovered that when a specific styrene-ethyleneoxy group-containing (meth)acrylic acid copolymer is used as a dispersant, the addition of a small amount of the copolymer exhibits dispersibility and wettability, is excellent in fine particle formation of disperse dyes and pigments, and further exhibits redispersibility, which led to the creation of the present invention.

[0013] Accordingly, the present invention provides the following dispersant, dispersion and ink compositions, and methods for their preparation. 1. (a1) to (a3) ​​below, (a1) Styrene: 1 to 40% by mass (a2) Ethyleneoxy group-containing (meth)acrylic acid ester monomer: 1 to 59% by mass (a3) Monomers other than (a1) and (a2): 10 ~98% by mass A dispersant for dispersing a disperse dye or pigment in an aqueous solvent, comprising (A) a styrene-ethyleneoxy group-containing (meth)acrylic acid copolymer having a weight average molecular weight of 1,000 to 50,000, which is a polymer of the above-mentioned (a3) ​​component, wherein the monomer of the component (a3) ​​is a (meth)acrylic acid alkyl ester monomer or a radical polymerizable monomer having a functional group selected from the group consisting of a carboxy group, a hydroxy group, an epoxy group and a sulfonic acid group, and the surfactant content is less than 0.1 mass %. 2. The dispersant according to the above item 1, wherein the monomer of component (a3) ​​is a radical polymerizable monomer containing a functional group selected from the group consisting of a carboxy group, a hydroxy group and an epoxy group. 3. The dispersant according to the above 1 or 2, wherein the component (A) is a neutralized product with a basic compound having an octanol / water partition coefficient of -5.0 or more and 0 or less. 4. The dispersant according to 1 or 2 above, which does not contain an acetylene-based surfactant. 5. A dispersion comprising a dispersant, a disperse dye and / or a pigment, and an aqueous solvent, wherein the dispersant is the dispersant described in 1 or 2 above. 6. An ink composition comprising the dispersion described in 5 above. 7. A method for producing a dispersant according to 1 or 2 above, comprising a step of neutralizing the component (A) with a basic compound having an octanol / water partition coefficient of -5.0 or more and 0 or less. 8. A method for producing a dispersion, comprising the step of mixing and dispersing the dispersant according to 1 or 2 above, a disperse dye and / or a pigment, and an aqueous solvent. 9. The following steps (a) and (b) (a) a step of mixing and dispersing the dispersant described in 1 or 2 above, a disperse dye and / or a pigment, and an aqueous solvent to obtain a dispersion; (b) mixing the dispersion with at least one substance selected from the group consisting of water, a water-soluble organic solvent, a resin, an ultraviolet absorber, an antioxidant, a pH adjuster, a preservative, and a viscosity adjuster; A method for producing an ink composition comprising the steps of: Effect of the Invention

[0014] The dispersant of the present invention can disperse disperse dyes and pigments with a small amount of addition, regardless of the type of disperse dye or pigment. Furthermore, the dispersion and ink composition using this dispersant exhibits wettability and dispersion stability, and further exhibits redispersibility. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] The dispersant of the present invention contains (A) a styrene-ethyleneoxy group-containing (meth)acrylic acid copolymer having a weight average molecular weight of 1,000 to 50,000. The component (A) is preferably a neutralized product with a basic compound having an octanol / water partition coefficient of -5.0 or more and 0 or less.

[0016] The component (A) is a styrene-ethyleneoxy group-containing (meth)acrylic acid copolymer having a weight average molecular weight of 1,000 to 50,000. (a1) Styrene: 1 to 40% by mass (a2) Ethyleneoxy group-containing (meth)acrylic Acid Stel monomer: 1 to 59% by mass (a3) Monomers other than (a1) and (a2): 1 to 98% by mass The component (A) may be a random copolymer or a block copolymer.

[0017] The content of styrene, which is the component (a1), is 1 to 40% by mass, preferably 10 to 30% by mass, based on 100% by mass of the monomers of the components (a1) to (a3). By setting the content within the range of 1 to 40% by mass, the dispersion can have a redispersibility effect.

[0018] The ethyleneoxy group-containing (meth)acrylic compound (a2) Acid The ester monomer preferably has an added mole number of ethyleneoxy groups of 1 to 100 moles, more preferably 5 to 90 moles, and even more preferably 10 to 90 moles.

[0019] The ethyleneoxy group-containing (meth)acrylic compound (a2) Acid The weight average molecular weight of the ster monomer is preferably 100 to 5,000.

[0020] Specifically, the component (a2) is an acrylic acid modified with polyethylene glycol. Acid ester monomers. Specific examples include polyethylene glycol mono(meth)acrylate, methoxypolyethylene glycol mono(meth)acrylate, ethoxypolyethylene glycol mono(meth)acrylate, polyethylene glycol modified 2-isocyanatoethyl (meth)acrylate, polyethylene glycol-propylene glycol-mono(meth)acrylate, etc. Particularly preferred is polyethylene glycol mono(meth)acrylate.

[0021] The polyethylene glycol mono(meth)acrylate is represented by the following formula. [ka] (In the formula, R represents a hydrogen atom or an alkyl group having 1 to 20 carbon atoms, and p represents a positive number of 1 to 100.)

[0022] Examples of commercially available products of the component (a2) include Blenmer "PME-400", "PME-1000", "PME-4000", "PE-200", "PE-350", "AE-200", "AE-400", and "AME-400" manufactured by NOF Corporation; Light Ester "130MA" and "041MA", Light Acrylate "MTG-A" and "130A" manufactured by Kyoeisha Chemical Co., Ltd.; Fancryl "FA-400M(100)" manufactured by Showa Denko Materials Co., Ltd.; NK Ester "AM-90G", "AM-130G", "AM-230G", "M-90G", "M-130G", "M-230G", and "M-450G" manufactured by Shin-Nakamura Chemical Co., Ltd.; and VISIOMER "MPEG 750MA W", "MPEG 1005 MA W", "MPEG 2005 MA W", and "MPEG 5005 MA W" manufactured by Evonik.

[0023] The ethyleneoxy group-containing (meth)acrylic compound of the above component (a2) Acid The amount of the steric monomer is 1 to 59% by mass, and preferably 5 to 55% by mass, based on 100% by mass of the monomers (a1) to (a3). By keeping the content of the (a2) component within the range of 1 to 59% by mass, the effect of dispersing disperse dyes and pigments can be obtained when used as a dispersant.

[0024] The monomer other than (a1) to (a2) which is the component (a3) ​​is not particularly limited, but examples thereof include (meth)acrylic acid alkyl ester monomers and / or radical polymerizable monomers containing functional groups such as carboxyl groups, amide groups, hydroxyl groups, epoxy groups, and sulfonic acid groups. These can be used alone or in combination of two or more kinds, but it is preferable to contain at least one of radical polymerizable monomers containing functional groups such as carboxyl groups, amide groups, hydroxyl groups, epoxy groups, and sulfonic acid groups. Particularly preferable are (meth)acrylic acid alkyl ester monomers and / or carboxyl group-containing radical polymerizable monomers and hydroxyl group-containing radical polymerizable monomers.

[0025] The (meth)acrylic acid alkyl ester monomer is not particularly limited and may be one having a linear or branched structure, one having an alicyclic group, one having an aromatic ring group, etc., but the above-mentioned (a2) component, ethyleneoxy group-containing (meth)acrylic acid alkyl ester monomer, is preferably used. Acid Does not include steric monomers.

[0026] Examples of the (meth)acrylic acid alkyl ester monomer having a linear or branched structure include methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, iso-butyl (meth)acrylate, sec-butyl (meth)acrylate, tert-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, and stearyl (meth)acrylate.

[0027] Examples of the (meth)acrylic acid ester monomer having an alicyclic group include cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, adamantyl (meth)acrylate, and dicyclopentanyl (meth)acrylate.

[0028] Examples of the (meth)acrylic acid ester monomer having an aromatic ring group include benzyl (meth)acrylate and phenoxyethyl (meth)acrylate.

[0029] Examples of the carboxy group-containing radically polymerizable monomer include methacrylic acid, acrylic acid, carboxyethyl (meth)acrylate, fumaric acid, itaconic acid, maleic acid, crotonic acid, vinylbenzoic acid, maleic acid monobutyl ester, itaconic acid monomethyl ester, and itaconic acid butyl ester.

[0030] Examples of the amide group-containing radically polymerizable monomer include N-methoxymethylacrylamide, N-ethoxymethylacrylamide, and N-butoxymethylacrylamide.

[0031] Examples of the hydroxy group-containing radically polymerizable monomer include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 1-methyl-4-hydroxybutyl (meth)acrylate, and 1-methyl-4-hydroxypentyl (meth)acrylate.

[0032] Examples of the epoxy group-containing radically polymerizable monomer include glycidyl (meth)acrylate and methallyl glycidyl ether.

[0033] Examples of the sulfonic acid group-containing radically polymerizable monomer include sodium p-styrenesulfonate, lithium p-styrenesulfonate, Nt-butylacrylamidosulfonic acid, sodium 2-sulfoethyl methacrylate, polycyclic phenyl ether methacrylate sulfate, sodium N-sulfonate polyoxyalkylene methacrylate, and ammonium polyoxyalkylene alkenyl ether sulfonate.

[0034] Examples of commercially available sulfonic acid group-containing radically polymerizable monomers include Spinomer "NaSS" (sodium p-styrenesulfonate) and "LiSS" (lithium p-styrenesulfonate) manufactured by Tosoh Finechem Corporation, "ATBS" (Nt-butylacrylamidosulfonic acid) manufactured by Toagosei Co., Ltd., Antox "MS-2N-D" (sodium 2-sulfoethyl methacrylate) and "MS-60" (polycyclic phenyl ether methacrylate sulfate) manufactured by Nippon Nyukazai Co., Ltd., Eleminol "JS-20" and "RS-3000" (N-sulfonic acid sodium polyoxyalkylene methacrylate) manufactured by Sanyo Chemical Industries, and Latemul "PD-104" and "PD-105" (ammonium polyoxyalkylene alkenyl ether sulfonate) manufactured by Kao Corporation.

[0035] The content of monomers other than the components (a1) and (a2) is 1 to 98% by mass, and preferably 10 to 80% by mass, relative to 100% by mass of the monomers (a1) to (a3). If this content is less than 1% by mass, it becomes difficult to make the acrylic resin water-soluble, and if it exceeds 98% by mass, the effect of imparting redispersibility to the dispersion may be impaired.

[0036] The monomers of the components (a1) to (a3) ​​can be polymerized by a known polymerization method, such as solution polymerization, emulsion polymerization, suspension polymerization, and bulk polymerization. Among these known polymerization methods, solution polymerization is preferably used because of the simplicity of the equipment and operation.

[0037] In order to efficiently proceed with the polymerization reaction, a known polymerization initiator can be used. The polymerization initiator can be appropriately selected depending on the polymerization method, polymerization conditions, and solubility in the solvent, but from the viewpoint of safety and polymerization efficiency, the 10-hour half-life temperature is preferably 70 to 110°C. If the 10-hour half-life temperature is less than 70°C, the stability at room temperature is low, so there is a possibility of increasing the risk of fire. If the 10-hour half-life temperature is 110°C or more, the polymerization reaction requires a high temperature and a long time, so the production efficiency may decrease. Specifically, azobis compounds such as 2,2'-azobis-isobutyronitrile, organic peroxides such as benzoyl peroxide, inorganic peroxides such as sodium persulfate, and redox catalyst systems consisting of combinations of such oxidizing agents and reducing agents such as bisulfite can be mentioned, and these can be used alone or in combination of two or more.

[0038] A chain transfer agent can be added to adjust the molecular weight to a preferred range. Examples of the chain transfer agent include alcohols such as catechol, mercaptans such as n-dodecyl mercaptan, and halogenated carbons such as carbon tetrachloride, and these can be used alone or in combination of two or more. In consideration of the chain transfer constant and safety, it is preferable to select mercaptans, and high-boiling mercaptans such as n-dodecyl mercaptan are particularly preferable in that the odor of remaining mercaptans can be suppressed.

[0039] The use of a solvent is preferable because the polymer can be handled in a solution state and can be synthesized with a simple device. An appropriate solvent can be selected according to the polymerization method to be applied, polymerization conditions, solubility of the raw material, and the solvent composition of the dispersion composition using the dispersant, but when producing an aqueous dispersant, it is preferable to select one with a boiling point of 60 to 120 ° C. under standard conditions. If the boiling point is less than 60 ° C., it may be difficult to efficiently proceed with polymerization in a short time. On the other hand, if the boiling point is 120 ° C. or more, a large amount of energy may be required for distillation under reduced pressure. Examples of solvents that are preferably used include water (boiling point 100 ° C.), alcohols such as 2-propanol (boiling point 82 ° C.), esters such as ethyl acetate (boiling point 77 ° C.), ketones such as 2-butanone (boiling point 80 ° C.), aromatic hydrocarbons such as toluene (boiling point 111 ° C.), and ethers such as tetrahydrofuran (boiling point 66 ° C.), and these can be used alone or in combination of two or more. When producing an aqueous dispersion, water-miscible alcohols, ethers, and mixed solvents of these with other organic solvents and / or water are preferably used, and in consideration of safety and economy, 2-propanol and mixed solvents of 2-propanol with other organic solvents and / or water are more preferably used.

[0040] The styrene-ethyleneoxy group-containing (meth)acrylic acid copolymer obtained by polymerization is neutralized with a basic compound characterized by an octanol / water partition coefficient of -5.0 or more and 0 or less. By neutralizing a part or all of the functional groups of the polymer with a basic compound, the polymer is stabilized in a dissolved or dispersed state in a solvent. The basic compound may be added in the form of a monomer and then polymerized, or may be added after polymerizing a monomer having an acidic functional group.

[0041] Although it depends on the water solubility and acidity of the styrene-ethyleneoxy group-containing (meth)acrylic acid copolymer and the water solubility and basicity of the basic compound, the basic compound is preferably added so that the pH of a 20% aqueous solution of the styrene-ethyleneoxy group-containing (meth)acrylic acid copolymer is in the range of 7 to 13, more preferably so that the pH of a 20% aqueous solution of the styrene-ethyleneoxy group-containing (meth)acrylic acid copolymer is in the range of more than 7 to 11, and particularly preferably so that the pH of a 20% aqueous solution of the styrene-ethyleneoxy group-containing (meth)acrylic acid copolymer is in the range of 8 to 10. If the pH of the aqueous polymer solution is less than 7, the solubility of the polymer in water may be insufficient, and the polymer may precipitate or precipitate in water, which is not preferable. On the other hand, if the pH of the aqueous polymer solution is higher than 13, the polymer may deteriorate over time due to hydrolysis, which is not preferable.

[0042] The octanol / water partition coefficient (logPow) of the basic compound is within the range of -5.0 to 0, and preferably -4.0 to 0. Here, the octanol / water partition coefficient (logPow) in the present invention is a value obtained in accordance with "Measurement of partition coefficient (1-octanol / water) - flask shaking method" of JIS Z7260-107 (2000). The basic compound used in the present invention is a basic compound that is highly water-soluble and has hydrophilicity.

[0043] Furthermore, the basic compound can be appropriately selected in consideration of the compatibility with the dispersion system and the composition of the dispersion composition using the dispersant. By using a basic compound with a boiling point of 100° C. or more, the basic compound remains in the dried product, and re-solubility is increased when water is added. Examples of such basic compounds include organic amine compounds such as 2-amino-2-methyl-1-propanol (distribution coefficient = -0.74, boiling point 165°C), morpholine (distribution coefficient = -0.84, boiling point 129°C), 1-amino-2-propanol (distribution coefficient = -0.96, boiling point 159°C), 3-amino-1-propanol (distribution coefficient = -1.12, boiling point 187°C), diethanolamine (distribution coefficient = -1.43, boiling point 268°C), monoethanolamine (distribution coefficient = -1.31, boiling point 171°C), and triethanolamine (distribution coefficient = -1.59, boiling point 335°C), and alkali metal hydroxides such as sodium hydroxide (distribution coefficient = -3.88, boiling point 1390°C) and potassium hydroxide (distribution coefficient = -3.88, boiling point 1320°C).

[0044] The styrene-ethyleneoxy group-containing (meth)acrylic acid copolymer (A) obtained by the above method has a weight average molecular weight (Mw) of 1,000 to 50,000, preferably 3,000 to 30,000. If the weight average molecular weight (Mw) is less than 1,000, the dispersion stabilizing power for disperse dyes and pigments decreases, and if it is more than 50,000, the ability to disperse disperse dyes and pigments decreases and the viscosity of the ink may become too high, which is not preferable. The weight average molecular weight can be measured by GPC (gel permeation chromatography).

[0045] The acid value of the (A) styrene-ethyleneoxy group-containing (meth)acrylic acid copolymer is preferably 50 to 300, more preferably in the range of 100 to 250. If the acid value is less than 50, the solubility of the resin in water tends to be poor and the dispersion stabilizing power for disperse dyes and pigments tends to be poor, while if the acid value exceeds 300, the affinity with the aqueous medium becomes strong and the image after printing tends to easily bleed, which is not preferable. The acid value of the resin represents the number of mg of KOH required to neutralize 1 g of the resin, and is measured according to JIS-K 3054.

[0046] The dispersant of the present invention can be obtained by mixing the (A) component with other components such as an aqueous solvent as necessary, and is characterized in that the surfactant content in the dispersant is less than 0.1 mass%. In particular, it is preferable that the dispersant does not contain an acetylene-based surfactant. Even if the dispersant does not contain an acetylene-based surfactant, the desired performance can be obtained.

[0047] The dispersion of the present invention contains the above-mentioned (A) styrene-ethyleneoxy group-containing (meth)acrylic acid copolymer having a weight average molecular weight of 1,000 to 50,000, a disperse dye and / or pigment, and an aqueous solvent.

[0048] The components of the dispersion are described below. In the dispersion of the present invention, the amount of the dispersant is preferably 1 to 100 parts by mass, more preferably 3 to 80 parts by mass, and even more preferably 5 to 50 parts by mass, per 100 parts by mass of the disperse dye and pigment. If the amount of the dispersant is too small, the disperse dye and pigment cannot be sufficiently dispersed, and if the amount of the dispersant is too large, a large amount of dispersant that is not adsorbed to the disperse dye or pigment will be present in the dispersion, which is not preferable.

[0049] The disperse dye is not particularly limited and any known disperse dye can be used. Disperse dyes are classified into chemical structures such as benzene azo (monoazo, disazo), heterocyclic azo (thiazole azo, benzothiazole azo, pyridone azo, pyrazolone azo, thiophene azo, etc.), anthraquinone, and condensation (quinophthalone, styryl, coumarin, etc.), and have characteristics such as being poorly soluble in water because they do not have a water-soluble group, and having a molecular weight of 2,000 or less, which is smaller than other dyes.

[0050] Examples of disperse dyes that can be preferably used in the present invention are given below. CIDisperse Yellow 3, 4, 5, 7, 9, 13, 24, 30, 33, 34, 42, 44, 49, 50, 51, 54, 56, 58, 60, 63, 64, 66, 68, 71, 74, 76, 79, 82, 83, 85, 86, 88, 90, 91, 93, 98, 99, 100, 104, 114, 116, 118, 119, 122, 124, 126, 135, 140, 141, 149, 160, 162, 163, 164, 165, 179, 180, 182, 183, 186, 192, 198, 199, 202, 204, 210, 211, 215, 216, 218, 224, etc. yellow dyes; Orange dyes such as CI Disperse Orange 1, 3, 5, 7, 11, 13, 17, 20, 21, 25, 29, 30, 31, 32, 33, 37, 38, 42, 43, 44, 45, 47, 48, 49, 50, 53, 54, 55, 56, 57, 58, 59, 61, 66, 71, 73, 76, 78, 80, 89, 90, 91, 93, 96, 97, 119, 127, 130, 139, 142; CIDisperse Red 1, 4, 5, 7, 11, 12, 13, 15, 17, 27, 43, 44, 50, 52, 53, 54, 55, 56, 58, 59, 60, 65, 72, 73, 74, 75, 76, 78, 81, 82, 86, 88, 90, 91, 92, 93 , 96, 103, 105, 106, 107, 108, 110, 111, 113, 117, 118, 121, 122, 126, 127, 128, 131, 132, 134, 135, 137, 143, 145, 146, 151, 152, red dyes, such as 153, 154, 157, 159, 164, 167, 169, 177, 179, 181, 183, 184, 185, 188, 189, 190, 191, 192, 200, 201, 202, 203, 205, 206, 207, 210, 221, 224, 225, 227, 229, 239, 240, 257, 258, 277, 278, 279, 281, 288, 289, 298, 302, 303, 310, 311, 312, 320, 324, 328; Purple dyes such as CIDisperse Violet 1, 4, 8, 23, 26, 27, 28, 31, 33, 35, 36, 38, 40, 43, 46, 48, 50, 51, 52, 56, 57, 59, 61, 63, 69, 77; Green dyes such as CIDisperse Green 6:1, 9; Brown dyes such as CI Disperse Brown 1, 2, 4, 9, 13, 19, 21, 27; CIDisperse Blue 3, 7, 9, 14, 16, 19, 20, 26, 27, 35, 43, 44, 54, 55, 56, 58, 60, 62, 64, 71, 72, 73, 75, 79, 81, 82, 83, 87, 91, 93, 9 4, 95, 96, 102, 106, 108, 112, 113, 115, 118, 120, 122, 125, 128, 130, 139, 141, 142, 143, 146, 148, 149, 153, 1 Blue dyes, such as 54, 158, 165, 167, 171, 173, 174, 176, 181, 183, 185, 186, 187, 189, 197, 198, 200, 201, 205, 207, 211, 214, 224, 225, 257, 259, 267, 268, 270, 284, 285, 287, 288, 291, 293, 295, 297, 301, 315, 330, 333, 359, 360; Black dyes such as CI Disperse Black 1, 3, 10, and 24 can be preferably used.

[0051] Dyes manufactured by Nippon Kayaku Co., Ltd. include Kayaset Black KR, AN, Kayalon Polyester Black S-200, EX-SF 300, G-SF, BR-SF, 2B-SF 200, TA-SF 200, AUL-S, Kayaset Yellow K-CL, Kayalon Polyester Yellow 4G-E, Kayalon Polyester Light Yellow 5G-S, Kayaset Red K-BL, Kayacelon. Red E-BF, SMS-5, SMS-12, Kayalon Polyester Red TL-SF, BR-S, BL-E, HL-SF, 3BL-S200, AUL-S, Kayalon Polyester Light Red B-S200, Kayalon Polyester Rubine BL-S200, Kayaset Blue N, K-FL, MSB-13, Kayalon Polyester Blue BR-SF, TS, Kayalon Polyester Light Blue BGL-S200, Kayalon Polyester Turq Blue GL-S200, Kayalon Polyester Blue Green FCT-S, etc. can be preferably used. Dyes manufactured by Orient Chemical Industry Co., Ltd. include Valifast Black 3806, 3810, 3820, Oil Black BS, BY, B-85, 860, Water Yellow 6C, Valifast Yellow 1101, 1105, 3110, 3120, 4120, 4126, Oplas Yellow 130, 140, Oil Yellow GG-S, 105, 107, 129, 818, Water Red 27, Valifast Red 1306, 1355, 2303, 3311, 3320, Valifast Orange 3210, Valifast Brown 2402, Oil Red 5B, Oil Pink 312, Oil Brown BB, Valifast Blue 1601, 1603, 1605, 2606, 3806, 3820, and Oil Blue. #15, #613, 613, N14, BOS, etc. can be preferably used. Dyes manufactured by Sumitomo Chemical Co., Ltd. include Sumikaron Black S-BL, S-BF extra conc., S-RPD, S-XE 300%, Sumikaron Yellow SE-4G, SE-5G, SE-3GL conc., SE-RPD, Sumikaron Brilliant Flavine S-10G, Sumikaron Red. E-FBL, E-RPD(E), S-RPD(S), Sumikaron Brilliant Red S-BF, S-BLF, SE-BL, SE-BGL, SE-2BF, SE-3BL(N), Sumikaron Red E-FBL, E-RPD(E), S-RPD(S), Sumikaron Brilliant Red S-BF, S-BLF, SE-BL, SE-BGL, SE-2BF, SE-3BL(N), Sumikaron Brilliant Blue S-BL, Sumikaron Turquoise Blue S-GL, S-GLF grain, etc. can be preferably used. As dyes manufactured by BASF, Basacryl Black X-BGW, Naozapon Black X-51, X-55, Neozapon Yellow 081, Lurafix Yellow 138, Zapon Blue 807, Neozapon Blue 807, Lurafix Blue 590, 660, Orasol Black RLI, RL, CN, Oracet Yellow 8GF, GHS, Orasol Red G, Oracet Pink RP, Orasol Blue GL, GN, 2R, etc. can be preferably used. As dyes manufactured by Taoka Chemical Co., Ltd., Oleosol Fast Black AR, RL, Oleosol Fast Pink FB, Rhodamine A, B, B gran., Oleosol Fast Yellow 2G, Oleosol Fast Blue ELN, etc. can be preferably used. As dyes manufactured by Hodogaya Chemical Co., Ltd., Spilon Black BNH, MH special, etc. can be preferably used. As dyes manufactured by Mitsui Chemicals, Inc., PS Yellow GG, MS Yellow HD-180, PS Red G, MS Magenta VP, etc. can be preferably used. As a dye manufactured by Bayer, Ceres Blue GN 01 or the like can be preferably used. As dyes manufactured by Sumika Color Co., Ltd., TS Yellow 118 cake, ESC Yellow 155, Sumiplast Yellow HLR, GC, TS Turq Blue 618, 606, ESC Blue 655, 660, Sumiplast Blue S, OA, etc. can be preferably used.

[0052] The pigment is not particularly limited, and known pigments can be used. Examples of organic pigments include azo pigments such as soluble azo pigments, insoluble azo pigments, and condensed azo pigments, quinacrylonitrile pigments, perylene pigments, perinone pigments, isoindolinone pigments, isoindoline pigments, dioxazine pigments, thioindigo pigments, anthraquinone pigments, quinophthalone pigments, metal complex pigments, polycyclic pigments such as diketopyrrolopyrrole pigments, and phthalocyanine pigments. Examples of inorganic pigments include carbon black, metal oxides, metal hydroxides, metal sulfides, metal ferrocyanides, and metal chlorides, and examples of carbon black include furnace black, lamp black, acetylene black, and channel black.

[0053] Specific examples of pigments include red pigments such as CI Pigment Red 7, 9, 14, 41, 48:1, 48:2, 48:3, 48:4, 81:1, 81:2, 81:3, 122, 123, 146, 149, 168, 177, 178, 179, 187, 200, 202, 208, 210, 215, 224, 254, 255, and 264; Yellow pigments such as CI Pigment Yellow 1, 3, 5, 6, 14, 55, 60, 61, 62, 63, 65, 73, 74, 77, 81, 93, 97, 98, 104, 108, 110, 128, 138, 139, 147, 150, 151, 154, 155, 166, 167, 168, 170, 180, 188, 193, 194, 213; Orange pigments such as CI Pigment Orange 36, 38, 43; Blue pigments such as CI Pigment Blue 15, 15:2, 15:3, 15:4, 15:6, 16, 22, 60; Green pigments such as CI Pigment Green 7, 36, 58; Purple pigments such as CI Pigment Violet 19, 23, 32, 50; Examples of black pigments include CI Pigment Black 7. Of these, CI Pigment Red 122, CI Pigment Yellow 74, 128, 155, CI Pigment Blue 15:3, 15:4, 15:6, CI Pigment Green 7, 36, CI Pigment Violet 19, CI Pigment Black 7, etc. can be preferably used.

[0054] The type, particle size, processing method, etc. of the disperse dye and / or pigment contained in the dispersion can be appropriately selected depending on the purpose. The disperse dye and pigment contained in the dispersion may be used alone or in combination of two or more kinds.

[0055] The concentration of the disperse dye and pigment in the dispersion is preferably 1 to 50 mass %, more preferably 5 to 50 mass %, in 100 mass % of the dispersion. If the concentration of the disperse dye and pigment exceeds 50 mass %, the density of the disperse dye and pigment in the dispersion becomes high, and the free movement of the disperse dye and pigment is hindered, which may cause aggregation.

[0056] The aqueous solvent may be water and / or a water-soluble organic solvent, and may be a mixture of two or more. The water is preferably pure water or ion-exchanged water (deionized water). Examples of the water-soluble organic solvent include alcohols such as methyl alcohol, ethyl alcohol, n-propyl alcohol, isopropyl alcohol, n-butyl alcohol, sec-butyl alcohol, and tert-butyl alcohol; glycols such as ethylene glycol, propylene glycol, dipropylene glycol, butylene glycol, triethylene glycol, 1,2,6-hexanetriol, thiodiglycol, hexylene glycol, and diethylene glycol; glycol ethers such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, diethylene glycol methyl ether, diethylene glycol ethyl ether, triethylene glycol monomethyl ether, triethylene glycol monoethyl ether, and triethylene glycol monobutyl ether; polyhydric alcohols such as glycerin; and nitrogen-containing compounds such as N-methyl-2-pyrrolidone, 2-pyrrolidone, and 1,3-dimethyl-2-imidazolidinone. The proportion of water and the water-soluble organic solvent in the dispersion is preferably from 5 to 95% by mass, and more preferably from 30 to 90% by mass, based on 100% by mass of the dispersion.

[0057] The method for producing the dispersion of the present invention preferably includes a step of mixing and dispersing the above-mentioned dispersant, disperse dye and / or pigment, and aqueous solvent. For example, the dispersant, disperse dye and / or pigment, and aqueous solvent can be mixed using a mixer / disperser such as a paint shaker, a bead mill, a ball mill, a dissolver, or a kneader to obtain a dispersion. In addition, when a component that is solid at room temperature is used, it may be heated and mixed as necessary.

[0058] The static surface tension of the dispersion is desirably 60 mN / m or less, more desirably 50 mN / m or less.

[0059] The viscosity of the dispersion is preferably 50.0 mPa·s or less, and more preferably 30.0 mPa·s or less. The lower limit of the viscosity of the dispersion is preferably 1.0 mPa·s or more. The viscosity in this case is measured at 25°C.

[0060] The average particle size of the disperse dye and / or pigment in the dispersion depends on the type of disperse dye and / or pigment, but is desirably 500 nm or less, more desirably 300 nm or less. The average particle size here refers to the median diameter (D50).

[0061] Furthermore, the dispersion of the present invention has excellent dispersion stability, and the interfacial migration speed is preferably 3.0 μm / s or less, and more preferably 1.0 μm / s or less.

[0062] The dispersion of the present invention has excellent redispersibility. That is, when an ink containing a colorant insoluble in water, such as a disperse dye or pigment, is dried, the dispersed state of the disperse dye or pigment is broken and aggregation occurs. In general, once aggregated, the disperse dye or pigment in the ink cannot be returned to a dispersed state even if a liquid medium such as water is added, and redispersibility is often poor, but the dispersion of the present invention has excellent redispersibility. In the present invention, the dissolution rate of the dispersion into the dispersion medium is preferably 40% or more, more preferably 60% or more. The dissolution rate of the dispersion into the dispersion medium will be described in the examples below.

[0063] The ink composition of the present invention contains the above-mentioned dispersion of the present invention, and further contains a resin and other additives as desired. That is, the ink composition of the present invention comprises the following components (i) to (v): (i) Dispersants (ii) Disperse dyes and / or pigments (iii) Water and / or a water-soluble organic solvent (iv) Resin (v) One or more additives selected from the group consisting of ultraviolet absorbers, antioxidants, pH adjusters, preservatives, and viscosity adjusters. It is preferred that the composition contains

[0064] The concentration of the disperse dye and / or pigment in the ink composition is preferably from 0.1 to 20% by mass, and more preferably from 0.1 to 10% by mass, based on 100% by mass of the ink composition.

[0065] The proportion of water and / or the water-soluble organic solvent in the ink composition is preferably from 50 to 99 mass %, and more preferably from 60 to 95 mass %, based on 100 mass % of the ink composition.

[0066] The resin contained in the ink composition is preferably a polymer having a hydrophobic group and a hydrophilic group. This polymer preferably has at least one functional group selected from an alkyl group, a cycloalkyl group, and an aryl group as a hydrophobic group. In addition, it is preferable that the polymer has at least one functional group selected from a carboxy group, a sulfo group, a hydroxy group, an amino group, an amide group, and these functional groups as a hydrophilic group. Such a polymer can be obtained by polymerizing monomers or oligomers having functional groups such as an acryloyl group, a methacryloyl group, a vinyl group, and an allyl group.Specifically, styrene, tetrahydrofurfuryl acrylate, butyl methacrylate, (α,2,3 or 4)-alkylstyrene, (α,2,3 or 4)-alkoxystyrene, 3,4-dimethylstyrene, α-phenylstyrene, divinylbenzene, vinylnaphthalene, dimethylamino(meth)acrylate, dimethylaminoethyl(meth)acrylate, dimethylaminopropylacrylamide, N,N-dimethylaminoethyl acrylate, acryloylmorpholine, N,N-dimethylacrylamide, N-isopropylacrylamide, N,N-diethylacrylamide, methyl(meth)acrylate, ethyl(meth)acrylate, propyl(meth)acrylate, ethylhexyl(meth)acrylate, other alkyl(meth)acrylates, methoxydiethylene glycol(meth)acrylate, (meth)acrylates of diethylene glycol or polyethylene glycol having an ethoxy group, a propoxy group or a butoxy group, cyclohexyl(meth)acrylate, benzene In addition to monofunctional monomers such as diethyl (meth)acrylate, phenoxyethyl (meth)acrylate, isobornyl (meth)acrylate, hydroxyalkyl (meth)acrylate, other fluorine-, chlorine-, and silicon-containing (meth)acrylates, (meth)acrylamide, maleic acid amide, and (meth)acrylic acid, when a crosslinking structure is to be introduced, (mono-, di-, tri-, tetra-, or poly)ethylene glycol di(meth)acrylate, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1, Compounds having an acrylic group or a methacrylic group, such as (meth)acrylates of 8-octanediol and 1,10-decanediol, trimethylolpropane tri(meth)acrylate, glycerin (di, tri)(meth)acrylate, di(meth)acrylate of an ethylene oxide adduct of bisphenol A or F, neopentyl glycol di(meth)acrylate, pentaerythritol tetra(meth)acrylate, and dipentaerythritol hexa(meth)acrylate, can be used.

[0067] The proportion of the resin in the ink composition is not particularly limited, but is preferably 0 to 30% by mass, and more preferably 0 to 20% by mass, relative to 100% by mass of the ink composition. When a resin is blended in the ink composition, it is preferably 1% by mass or more.

[0068] In addition, various additives can be contained in the ink composition. Examples of additives include ultraviolet absorbers, antioxidants, pH adjusters, preservatives, viscosity adjusters, etc., which can be appropriately selected and blended in the ink composition. These additives can be blended separately from the disperse dye and / or pigment, water and / or water-soluble organic solvent, and resin, in the dispersion and the remainder in 100% by mass of the ink composition, specifically, in a ratio of 0 to 10% by mass in 100% by mass of the ink composition.

[0069] The method for producing the ink composition is not particularly limited, but may be the following steps (a) and (b): (a) a step of mixing and dispersing the above-mentioned dispersant, a disperse dye and / or a pigment, and an aqueous solvent to obtain a dispersion; (b) mixing the dispersion with at least one substance selected from the group consisting of water, a water-soluble organic solvent, a resin, an ultraviolet absorber, an antioxidant, a pH adjuster, a preservative, and a viscosity adjuster; It is preferable to employ a method including the steps of:

[0070] The ink composition is applied to a recording medium by an ink jet recording method, a recording method using a writing instrument such as a pen, or other printing method. The ink composition of the present invention is particularly preferably used in the ink jet recording method. EXAMPLES

[0071] (A) Styrene-ethyleneoxy group-containing (meth)acrylic acid copolymer was synthesized by a known and commonly used method as follows. In this production example, unless otherwise specified, "parts" means "parts by mass" and "%" means "% by mass".

[0072] <Production Example 1> [Preparation of aqueous polymer solution neutralized with sodium hydroxide] In a three-neck flask equipped with a thermocouple thermometer, a stirrer, and a reflux condenser, 33 parts of styrene (hereinafter referred to as ST), 44 parts of methyl methacrylate (hereinafter referred to as MMA), 33 parts of polyethylene glycol methacrylate (average EO addition mole number 23, NOF Corp. "Blenmer PME-1000". Hereinafter referred to as PEG (23) MA), 55 parts of methacrylic acid (hereinafter referred to as MAA), 3.3 parts of n-dodecyl mercaptan (hereinafter referred to as NDM) as a chain transfer agent, 1.65 parts of 2,2'-azobis-isobutyronitrile (hereinafter referred to as AIBN) as a polymerization initiator, and 169.95 parts of 2-propanol (hereinafter referred to as IPA) as a solvent were charged, and the operation of deoxidation and nitrogen replacement was repeated twice to make the flask a nitrogen atmosphere. Then, stirring was started and the inside temperature was heated until it reached 80 ° C. The internal temperature was kept at 80°C for 6 hours and stirring was continued. After 6 hours, 145.2 parts of IPA was slowly added, and the internal temperature was cooled to 25°C or less to obtain an unneutralized polymer (IPA solution) (hereinafter referred to as unneutralized solution A). The polymer content of the obtained unneutralized solution A was 35.2% as determined from the dry residue. The weight average molecular weight of the unneutralized polymer was 18,275 and the number average molecular weight was 6,991.

[0073] The weight average molecular weight and number average molecular weight in the present invention are values ​​calculated in terms of standard polystyrene, which are determined by drying an unneutralized polymer solution at 105° C. for 3 hours, dissolving it in tetrahydrofuran so that the polymer content is 1%, and filtering the solution through a 0.45 μm membrane filter using gel permeation chromatography (GPC) under the following conditions. Column: Shodex KF-802, Shodex KF806M (Showa Denko) Elution solvent: Tetrahydrofuran ·Flow rate: 1.0mL / min ·Injection volume: 10μL Column temperature: 40℃ Detector: RI detector

[0074] 140 parts of unneutralized solution A was weighed into a beaker and stirring was started. 6.0 parts of sodium hydroxide (distribution coefficient = -3.88, boiling point 1390 ° C.) was weighed into another beaker, and 150 parts of ion-exchanged water was added to prepare an aqueous sodium hydroxide solution. The entire amount of the prepared aqueous sodium hydroxide solution was added to the unneutralized solution A under stirring to neutralize the polymer, and the entire amount of the liquid was transferred to an eggplant flask. After 120 parts were distilled off using a rotary evaporator, 200 parts of ion-exchanged water was added, and 160 parts were further distilled off under reduced pressure to remove IPA from the solution. 31.64 parts of ion-exchanged water was added to make the total amount 252.80 parts, and an aqueous polymer solution neutralized with sodium hydroxide having a polymer content of 19.5% and a pH of 7.4 was obtained.

[0075] <Production Example 2, Comparative Production Example 1> The type of neutralizer in unneutralized solution A was changed as shown in Table 1, and the amount of neutralizer added was changed to an amount that gave a pH as shown in the table. Other than that, the same method as in Production Example 1 was used to produce the solution. The types of neutralizing agents in Table 1 are as follows. Sodium hydroxide (distribution coefficient = -3.88, boiling point 1390℃) 2-Amino-2-methyl-1-propanol (Partition coefficient = -0.74, boiling point 166°C) Ammonia (distribution coefficient = 0.23, boiling point -33°C)

[0076] <Production Example 3, Comparative Production Example 2> The production was carried out in the same manner as in Production Example 1, except that the content (charging ratio) of each component was changed as shown in Table 1. Furthermore, the neutralizing agent in the unneutralized solution of Production Example 3 was changed as shown in Table 1 to produce Comparative Production Example 2.

[0077] <Comparative Manufacturing Example 3> In a three-neck flask equipped with a thermocouple thermometer, a stirrer, and a reflux condenser, 135.3 parts of ST, 13.2 parts of polyethylene glycol methacrylate (average EO addition mole number 9, NOF Corp. "Blenmer PME-400". Hereinafter referred to as PEG (9) MA), 16.5 parts of vinyl sulfonic acid (hereinafter referred to as VSA), 3.3 parts of NDM, 1.65 parts of AIBN, 305.25 parts of N,N-dimethylformamide (hereinafter referred to as DMF), and 49.5 parts of ion-exchanged water were charged, and the flask was subjected to deoxidation and nitrogen replacement twice to create a nitrogen atmosphere. Then, stirring was started to dissolve VSA and AIBN, and the mixture was heated until the internal temperature reached 80°C. The internal temperature was kept at 80°C for 6 hours while stirring was continued to carry out the polymerization reaction. After the reaction was completed, the reaction liquid was dropped into IPA to precipitate the polymer. After removing the supernatant, the precipitate was collected and dried to obtain Unneutralized Polymer B. The weight average molecular weight of the obtained Unneutralized Polymer B was 18,517. In a separable flask equipped with a thermocouple thermometer, a stirrer, a reflux tube, and a pH electrode, 15 parts of unneutralized polymer B and 70 parts of ion-exchanged water were weighed and heated with stirring until the internal temperature reached 80°C. Sodium hydroxide was added thereto until the pH reached 8.0, and ion-exchanged water was further added to make the total amount 100 parts. Stirring was continued at 80°C for 3 hours. Unneutralized polymer B did not dissolve.

[0078] <Comparative Manufacturing Examples 4 and 5> Except for changing the type of neutralizer for unneutralized polymer B as shown in the table and changing the amount of neutralizer added to an amount that gave a pH as shown in the table, the unneutralized polymer B was produced in the same manner as in Comparative Production Example 3. In each case, stirring was continued at 80° C. for 3 hours, but the unneutralized polymer B did not dissolve.

[0079] [Table 1]

[0080] [Table 2]

[0081] The present invention will be described in detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples. In the following examples, parts and % respectively indicate parts by mass and % by mass.

[0082] [Example 1] 15 parts of Hostaperm Blue BT-617-D (manufactured by CLARIANT, Pigment Blue 15:4) as a blue pigment, 61.9 parts of ion-exchanged water as an aqueous solvent, 23.1 parts of the dispersant, and 300 parts of zirconia beads (diameter 0.3 mm) were placed in a plastic container (made of polypropylene, capacity 0.5 L) and dispersed for 1 hour using a PAINT SHAKER (manufactured by Asada Iron Works Co., Ltd.). After dispersion, the zirconia beads were filtered off to obtain a dispersion.

[0083] [Examples 2 and 3, Comparative Examples 1 to 5] In the same manner as in Example 1, dispersions of the respective examples having the compositions shown in Table 3 below were prepared.

[0084] The surface tension, viscosity, average particle size, dispersion stability, redispersibility (visual observation), and redispersibility / elution rate of each dispersion were measured by the following methods. The results are shown in Table 3.

[0085] <Surface tension> The static surface tension of the dispersion immediately after dispersion was measured at 25° C. using a DY-500 high-performance surface tensiometer (manufactured by Kyowa Interface Science Co., Ltd.).

[0086] <Viscosity> The viscosity (25° C.) of the dispersion immediately after dispersion was measured using a TVE-20 E-type viscometer (manufactured by Toki Sangyo Co., Ltd.).

[0087] <Average particle size> The average particle size (D50) of the dispersion immediately after dispersion was measured using an ELSZ-2000 Zeta potential / particle size / molecular weight measurement system (Otsuka Electronics Co., Ltd.).

[0088] <Dispersion stability> Dispersion stability was evaluated using a dispersion stability analyzer LUMiSizer (manufactured by LUM Corporation). This analysis was performed under conditions of a temperature of 25°C immediately after dispersion, a rotation speed of 4,000 rpm, and an analysis time of 50 minutes, and the interfacial migration speed (settling speed of particles) was measured. The smaller the interfacial migration speed, the better the dispersion stability.

[0089] <Redispersibility (visual inspection)> Immediately after dispersion, 100 μL of the dispersion was measured out with a micropipette into a petri dish and left to dry at room temperature (approximately 25°C) for approximately 15 hours. After drying, 3 mL of ion-exchanged water was added, and the state of redispersion of the dried dispersion in the ion-exchanged water was visually judged. The evaluation criteria for redispersibility are shown below. (Evaluation Criteria) ◎: The dried matter disappeared and was redispersed. ◯: Some dried matter remained, but was mostly redispersed. △: Most of the dried material remained, and some was redispersed. ×: Redispersion of the dried material was not confirmed.

[0090] <Redispersibility dissolution rate> Immediately after dispersion, 100 μL of the dispersion was measured out using a micropipette and placed in a petri dish, and the dispersion was allowed to dry for approximately 15 hours at room temperature (approximately 25°C). After drying, the mass of the dried dispersion (mass before redispersion) was measured using an electronic balance, and then 3 mL of ion-exchanged water was added and the dispersion was allowed to dry for 3 minutes at room temperature (approximately 25°C). After leaving the dispersion to stand, undissolved matter was removed using an 80 mesh filter cloth, and the resulting filtrate was dried in a dryer at 60°C for 3 hours. After drying, the dried material (redispersed mass) was returned to room temperature and measured using an electronic balance, and the dispersion elution rate in ion-exchanged water was calculated using the following formula [1]. Redispersibility Elution rate [%]=(Redispersion mass) / (Mass before redispersion)×100...[1]

[0091] [Table 3]

[0092] From Table 3 above, it can be seen that the elution rate can be improved by about 40% by changing from "neutralized by ammonia in Comparative Production Example 1" to "neutralized by sodium hydroxide in Production Example 1" and "neutralized by 2-amino-2-methyl-1-propanol in Production Example 2", and further, the elution rate can be improved by about 20% by changing from "neutralized by ammonia in Comparative Production Example 2" to "neutralized by sodium hydroxide in Production Example 3". Thus, by using as a dispersant a styrene-ethyleneoxy group-containing (meth)acrylic acid copolymer neutralized with a basic compound having an octanol / water distribution coefficient of -5.0 or more and 0 or less, a dispersion with excellent resolubility can be obtained.

Claims

1. The following (a1) to (a3): (a1) Styrene: 1 to 40% by mass (a2) Ethyleneoxy group-containing (meth)acrylic acid ester monomer: 1 to 59% by mass (a3) Monomers other than (a1) and (a2): 10 to 98% by mass a polymer of (A) a styrene-ethyleneoxy group-containing (meth)acrylic acid copolymer having a weight average molecular weight of 1,000 to 50,000, wherein the monomer of component (a3) ​​is a (meth)acrylic acid alkyl ester monomer or a radical polymerizable monomer having a functional group selected from the group consisting of a carboxy group, a hydroxy group, an epoxy group, and a sulfonic acid group, and the surfactant content is less than 0.1% by mass.

2. 2. The dispersant according to claim 1, wherein the monomer of component (a3) ​​is a radical polymerizable monomer containing a functional group selected from the group consisting of a carboxy group, a hydroxy group and an epoxy group.

3. 3. The dispersant according to claim 1, wherein the component (A) is a neutralized product with a basic compound having an octanol / water partition coefficient of -5.0 or more and 0 or less.

4. 3. The dispersant according to claim 1 or 2, which does not contain an acetylene-based surfactant.

5. A dispersion comprising a dispersant, a disperse dye and / or a pigment, and an aqueous solvent, wherein the dispersant is the dispersant according to claim 1 or 2.

6. An ink composition comprising the dispersion according to claim 5.

7. 3. The method for producing a dispersant according to claim 1, further comprising a step of neutralizing the component (A) with a basic compound having an octanol / water partition coefficient of −5.0 or more and 0 or less.

8. 3. A method for producing a dispersion, comprising the step of mixing and dispersing the dispersant according to claim 1 or 2, a disperse dye and / or a pigment, and an aqueous solvent.

9. The following steps (a) and (b) (a) mixing and dispersing the dispersant according to claim 1 or 2, a disperse dye and / or a pigment, and an aqueous solvent to obtain a dispersion; (b) mixing the dispersion with at least one substance selected from the group consisting of water, a water-soluble organic solvent, a resin, an ultraviolet absorber, an antioxidant, a pH adjuster, a preservative, and a viscosity adjuster; A method for producing an ink composition comprising the steps of:

Citation Information

Patent Citations

  • Dispersion stabilizer for highly concentrated coal-water slurry

    JP1987215695A

  • Preparation of water-based pigment dispersion

    JP2000290578A

  • Method for manufacturing pigment dispersion, pigment dispersion obtained thereby, ink jet recording ink using the same, and recording method and recorded matter therewith

    JP2002020673A

  • Aqueous emulsion polymers as dispersants

    JP2006506491A

  • Aqueous pigment dispersion liquid, ink composition and ink-jet recording method

    JP2010013576A