Manufacturing method of the joint body
A laminate of base materials with amorphous thermoplastic resins addresses the limitations of conventional adhesives by providing rapid bonding, long open time, and high adhesive strength, enhancing recyclability and repairability.
Patent Information
- Application Number
- JP2023530137
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-06-24
- Filing Date
- 2022-06-24
- Publication Date
- 2024-10-02
- Estimated Expiration
- 2042-06-24
AI Technical Summary
Conventional adhesives for joining dissimilar materials face challenges such as long bonding process times, short open times, and inadequate adhesive strength, particularly with thermosetting epoxy resins and hot melt adhesives.
A method involving a laminate of base materials with a solid bonding agent composed of amorphous thermoplastic resins like thermoplastic epoxy resin or phenoxy resin, which are heated and pressurized to melt and bond, ensuring a short process time, long open time, and high adhesive strength.
The method achieves rapid bonding, long open time, and excellent adhesiveness, with recyclability and repairability, utilizing the phase change of the solid bonding agent without chemical reactions.
Smart Images

Figure 0007559950000002 
Figure 0007559950000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a bonded body suitable for applications in which different types of materials must be bonded easily and firmly. [Background technology]
[0002] In recent years, from the viewpoint of reducing the weight and improving the performance of products, the use of multi-material parts has been progressing in various fields such as automobile parts, medical equipment, and home appliances. Multi-materialization is a method of reducing the weight and increasing the strength of materials by combining materials with different functions and properties (hereinafter referred to as dissimilar materials). To realize multi-materialization, technology to firmly bond dissimilar materials is essential.
[0003] As a means for firmly joining different materials, a liquid adhesive, such as thermosetting epoxy resin adhesive (Patent Document 1, etc.), is widely used. Bonding using a liquid adhesive requires a coating step of coating a liquid resin composition and a curing step of curing the resin composition by polymerization reaction after coating. For this reason, when bonding is performed using a liquid adhesive, there is a problem that it takes a long time to apply the resin composition in the application process, and the polymerization reaction takes a long time in the curing process (i.e., the bonding process takes a long time), resulting in a lack of convenience. In this specification, the bonding process time means the time from the start point when at least one of the substrates constituting the bonded body comes into contact with the bonding agent or adhesive to the end point when the fabrication of the bonded body is completed. For example, this includes the time required for the step of applying a liquid adhesive to the substrate and the drying step, the time required for the step of placing a solid bonding agent, and the time required to bond the substrates together (for example, the time required to harden the adhesive layer).
[0004] A technology has also been disclosed in which a thermosetting epoxy resin composition is impregnated into or applied to a substrate, and then semi-cured to produce a laminate having an adhesive layer made of a thermosetting epoxy resin-based adhesive in a semi-cured state (hereinafter, referred to as B-stage), which is then used to manufacture a bonded body (Patent Document 2, etc.). However, even when a laminate having a B-stage adhesive layer is used, a curing step is required to polymerize and cure the B-stage adhesive layer, which results in a long bonding process time. Furthermore, the B-stage adhesive layer has problems in that it has poor storage stability, cannot be stored at room temperature for long periods, must be stored at low temperatures, and has a short open time, resulting in a lack of convenience. In this specification, the open time refers to the time limit from when a bonding agent or adhesive is applied or placed on substrate A until when substrate B is completely placed. Within the open time, the adhesive strength of the bonding agent or adhesive does not decrease, and substrate A and substrate B can be bonded with sufficient adhesive strength. The longer the open time, the longer the time limit from when a bonding agent or adhesive is applied or placed on substrate A until when substrate B is completely placed, which is more convenient.
[0005] Hot melt adhesives, which are thermoplastic adhesives, are also used as a means of joining dissimilar materials (Patent Document 3, etc.). Hot melt adhesives are solid at room temperature and liquefied by heating and melting. The liquefied hot melt adhesive is applied to the adherend, and a bond is formed by cooling and solidifying. Since hot melt adhesives bond by utilizing a phase change that does not involve a polymerization reaction, no application process is required, and they have a fast curing time (i.e., a short joining process time), making them highly convenient. In addition, hot melt adhesives can be stored for long periods at room temperature, and are also highly convenient in that they have a long open time.
[0006] However, conventional hot melt adhesives are made of crystalline resins or resins containing crystalline resins in order to reduce the melt viscosity, so the adhesive resin has high cohesive force and cannot have sufficient interaction with the substrate. In addition, when melted and bonded, the viscosity becomes low at high temperatures, so it tends to flow out from the bonding surface, and the viscosity is difficult to control, so the film thickness is not stable. Due to these factors, there is a problem that conventional hot melt adhesives cannot stably obtain high adhesive strength. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2019-157018 A [Patent Document 2] Japanese Patent Application Publication No. 10-17685 [Patent Document 3] Japanese Patent Application Publication No. 10-168417 Summary of the Invention [Problem to be solved by the invention]
[0008] As described above, among the conventional technologies, thermosetting epoxy resin adhesives with excellent adhesive properties, whether in liquid or B-stage form, have at least one of the problems of a long bonding process time and a short open time, and hot melt adhesives with a short bonding process time and a long open time have the problem that high adhesive strength cannot be stably obtained.
[0009] The present invention has been made in view of the above technical background, and has an object to provide a bonding technique which has a short bonding process time, a long open time, and excellent adhesiveness. [Means for solving the problem]
[0010] In order to achieve the above object, the present invention provides the following means. In this specification, bonding means joining two objects together, and adhesion and welding are subordinate concepts. Adhesion means joining two adherends (objects to be bonded) via an organic material such as tape or adhesive (thermosetting resin, thermoplastic resin, etc.). Welding means joining by utilizing entanglement and crystallization due to molecular diffusion that occurs in the process of melting the surface of a thermoplastic resin or the like by heat, and contact pressure and cooling, or by utilizing intermolecular interactions with the base material that occur during melting.
[0011] <Method of manufacturing the bonded body> [1] A method for producing a bonded body, comprising: a pre-bonding process for preparing a laminate by arranging a substrate A, a solid bonding agent mainly composed of an amorphous thermoplastic resin which is at least one of a thermoplastic epoxy resin and a phenoxy resin, and a substrate B in that order; and a bonding process for heating and pressurizing the laminate to melt the solid bonding agent and bond the substrate A and the substrate B together, wherein the amorphous thermoplastic resin has an epoxy equivalent of 1,600 or more or does not contain an epoxy group, and the amorphous thermoplastic resin has a heat of fusion of 15 J / g or less. [2] The method for producing a bonded body according to [1], wherein the heating and pressurizing are carried out under conditions of 100 to 400° C. and 0.01 to 20 MPa. [3] The method for producing a bonded body according to [1] or [2], wherein the solid bonding agent before melting has any shape selected from the group consisting of a film, a rod, a pellet, and a powder. [4] The method for producing a bonded body according to any one of [1] to [3], wherein the base material A is made of at least one of a resin or a metal, and the base material B is made of at least one of a resin or a metal.
[0012] <zygote> [5] A bonded body obtained by bonding a base material A and a base material B with an adhesive layer therebetween, the adhesive layer being formed by disposing a solid adhesive agent mainly composed of an amorphous thermoplastic resin, which is at least one of a thermoplastic epoxy resin and a phenoxy resin, between the base material A and the base material B, melting the solid adhesive by heating and pressurizing, and solidifying the solid adhesive, the amorphous thermoplastic resin having an epoxy equivalent of 1,600 or more or the amorphous thermoplastic resin does not contain an epoxy group, and the amorphous thermoplastic resin having a heat of fusion of 15 J / g or less. [6] The bonded body according to [5], wherein the heating and pressurizing are carried out under conditions of 100 to 400° C. and 0.01 to 20 MPa. [7] The bonded body according to [5] or [6], wherein the base material A is made of at least one of a resin or a metal, and the base material B is made of at least one of a resin or a metal. Effect of the Invention
[0013] According to the present invention, it is possible to provide a bonding technique with a short bonding process time, a long open time, and excellent adhesiveness.
Brief Description of the Drawings
[0014] [Figure 1] It is an explanatory diagram showing the configuration of a bonded body in one embodiment of the present invention.
Embodiments for Carrying Out the Invention
[0015] [Method for Manufacturing a Bonded Body] The method for manufacturing a bonded body of the present invention will be described in detail. In the following description, the description of "a~b" indicating a numerical range means a numerical range including the endpoints a and b. That is, it means "a or more and b or less" (when a < b), or "a or less and b or more" (when a > b).
[0016] The method for manufacturing a bonded body of the present invention includes a pre-bonding step of arranging a base material A, a solid bonding agent mainly composed of an amorphous thermoplastic resin which is at least one of a thermoplastic epoxy resin and a phenoxy resin, and a base material B in this order to prepare a laminate, and a bonding step of heating and pressurizing the laminate to melt the solid bonding agent and bond the base material A and the base material B. In the pre-bonding step, neither the bonding of the base material A and the solid bonding agent nor the bonding of the base material B and the solid bonding agent is performed, and these are performed in the next bonding step. The solid bonding agent may have tackiness. When the solid bonding agent has tackiness, the solid bonding agent is temporarily fixed to the base material in the pre-bonding step.
[0017] Hereinafter, each step will be described.
[0018] <Pre-bonding Step> In the pre-bonding step, a base material A, a solid bonding agent mainly composed of an amorphous thermoplastic resin which is at least one of a thermoplastic epoxy resin and a phenoxy resin, and a base material B are arranged in this order to prepare a laminate. In the laminate, neither the base material A and the solid adhesive, nor the solid adhesive and the base material B are bonded together, and each is formed by overlapping independent members. The term "solid" in the solid binder means that the solid binder is solid at room temperature, that is, has no fluidity at 23° C. without pressure. The solid adhesive preferably has the property of being able to retain its shape without deformation for 30 days or more under no pressure at 23° C., and furthermore, not changing in quality. The "main component" means a component that is contained in the largest amount of resin components in the solid bonding agent and that accounts for 50% by mass or more of the resin components in the solid bonding agent. The solid bonding agent preferably contains 50% by mass or more of the resin components, more preferably 70% by mass or more, even more preferably 80% by mass or more, and particularly preferably 90% by mass or more.
[0019] (Solid adhesive) The solid bonding agent is mainly composed of an amorphous thermoplastic resin which is at least one of a thermoplastic epoxy resin and a phenoxy resin, wherein the amorphous thermoplastic resin has an epoxy equivalent of 1,600 or more or the amorphous thermoplastic resin does not contain an epoxy group, and the heat of fusion of the amorphous thermoplastic resin is 15 J / g or less. The amorphous resin in the present invention is a resin that has a melting point (Tm) but does not have a clear endothermic peak associated with melting in a measurement using a differential scanning calorimeter (DSC), or the endothermic peak is very small. The heat of fusion is calculated from the area of the endothermic peak of the DSC and the weight of the thermoplastic resin component. When an inorganic filler or the like is contained in the solid bonding agent, it is calculated from the weight of the resin component excluding the inorganic filler. Specifically, the amorphous thermoplastic resin in the present invention refers to the following. A sample is weighed out to 2-10 mg, placed in an aluminum pan, and heated from 23°C to 200°C or higher at 10°C / min using a DSC (DSC8231 manufactured by Rigaku Corporation) to obtain a DSC curve. Next, when the heat of fusion is calculated from the area of the endothermic peak at the time of melting obtained from the DSC curve and the weighed value, the resin has a heat of fusion of 15 J / g or less.
[0020] In order to fully impart the properties of an amorphous thermoplastic resin to the solid bonding agent, the content of the amorphous thermoplastic resin in the resin components in the solid bonding agent is preferably 60 mass % or more, more preferably 70 mass % or more, even more preferably 80 mass % or more, and most preferably 90 mass % or more.
[0021] The heat of fusion is 15 J / g or less, preferably 11 J / g or less, more preferably 7 J / g or less, and even more preferably 4 J / g or less, and most preferably the endothermic peak upon melting is below the detection limit. The epoxy equivalent is 1,600 or more, preferably 2,000 or more, more preferably 5,000 or more, and even more preferably 9,000 or more, and most preferably above the detection limit so that substantially no epoxy groups are detected.
[0022] In a solid adhesive containing an amorphous thermoplastic resin, which is at least one of a thermoplastic epoxy resin and a phenoxy resin, as a main component, the epoxy equivalent of the amorphous thermoplastic resin is 1,600 or more or the amorphous thermoplastic resin does not contain an epoxy group, and the heat of fusion of the amorphous thermoplastic resin is 15 J / g or less, the solid adhesive does not undergo a sudden drop in viscosity when heated, as seen in conventional hot melt adhesives, and does not reach a low viscosity state (0.001 to 100 Pa s) even in a high temperature range exceeding 200°C. Therefore, the solid adhesive does not flow out of the laminate even in a molten state, the thickness of the adhesive layer can be stably secured, and high adhesive strength can be stably obtained. The epoxy equivalent weight (weight of the resin containing 1 mole of epoxy groups) referred to here is the epoxy equivalent weight of the thermoplastic epoxy resin or phenoxy resin component contained in the solid adhesive before bonding, and is a value (unit: g / eq.) measured by the method specified in JIS-K7236:2001. Specifically, a potentiometric titration device was used, cyclohexanone was used as the solvent, brominated tetraethylammonium acetate solution was added, and a 0.1 mol / L perchloric acid-acetic acid solution was used, and the solvent-diluted product (resin varnish) was calculated as a solid content equivalent value from the non-volatile content. In the case of a mixture of two or more resins, it can also be calculated from the content and epoxy equivalent weight of each resin.
[0023] The melting point of the amorphous thermoplastic resin, which is the main component of the solid bonding agent, is preferably 50 to 400° C., more preferably 60 to 350° C., and even more preferably 70 to 300° C. By having a melting point in the range of 50 to 400° C., the solid bonding agent is efficiently deformed and melted by heating and effectively wets and spreads over the bonding surface, resulting in high adhesive strength. In this specification, the melting point of an amorphous thermoplastic resin means the temperature range in the process where the resin softens from a substantially solid state, acquires thermoplastic properties, and becomes meltable and adhesive.
[0024] Conventional thermosetting adhesives have problems in that it is difficult to disassemble the bonded body, making it difficult to separate and recycle the different materials that make up the bonded body (i.e., poor recyclability), and it is difficult to reattach the bonded body when there is a misalignment of the bonded part during the manufacturing process of the bonded body, or when the contents or the adherend have a defect and need to be replaced (i.e., poor repairability), resulting in a lack of convenience.However, the solid adhesive can be softened and melted by heat and can be easily peeled off, so it has excellent recyclability.In addition, since the solid adhesive is thermoplastic, it can be reversibly softened, melted and hardened repeatedly, and has excellent repairability.
[0025] <Thermoplastic epoxy resin> The thermoplastic epoxy resin is preferably a polymer of (a) a difunctional epoxy resin monomer or oligomer and (b) a difunctional compound having two identical or different functional groups selected from the group consisting of a phenolic hydroxyl group, a carboxyl group, a mercapto group, an isocyanate group, and a cyanate ester group. By using such a compound, the polymerization reaction for forming a linear polymer proceeds preferentially, making it possible to obtain a thermoplastic epoxy resin having the desired properties.
[0026] The (a) difunctional epoxy resin monomer or oligomer refers to an epoxy resin monomer or oligomer having two epoxy groups in the molecule. Specific examples of the (a) include bisphenol A type epoxy resins, bisphenol F type epoxy resins, bifunctional phenol novolac type epoxy resins, bisphenol AD type epoxy resins, biphenyl type epoxy resins, bifunctional naphthalene type epoxy resins, bifunctional alicyclic epoxy resins, bifunctional glycidyl ester type epoxy resins (e.g., diglycidyl phthalate, diglycidyl tetrahydrophthalate, dimer acid diglycidyl ester, etc.), bifunctional glycidyl amine type epoxy resins (e.g., diglycidyl aniline, diglycidyl toluidine, etc.), bifunctional heterocyclic epoxy resins, bifunctional diarylsulfone type epoxy resins, hydroquinone type epoxy resins (e.g., hydroquinone diglycidyl ether, 2,5-di-tert-butyl ether, etc.), t-Butylhydroquinone diglycidyl ether, resorcin diglycidyl ether, etc.), bifunctional alkylene glycidyl ether compounds (e.g. butanediol diglycidyl ether, butenediol diglycidyl ether, butynediol diglycidyl ether, etc.), bifunctional glycidyl group-containing hydantoin compounds (e.g. 1,3-diglycidyl-5,5-dialkylhydantoin, 1-glycidyl-3-(glycidoxyalkyl)-5,5-dialkylhydantoin, etc.), bifunctional glycidyl group-containing siloxanes (e.g. 1,3-bis(3-glycidoxypropyl)-1,1,3,3-tetramethyldisiloxane, α,β-bis(3-glycidoxypropyl)polydimethylsiloxane, etc.) and modified products thereof. Among these, bisphenol A type epoxy resins, bisphenol F type epoxy resins, and biphenyl type epoxy resins are preferred in terms of reactivity and workability. Examples of the bifunctional compound having a phenolic hydroxyl group in (b) include mononuclear aromatic dihydroxy compounds having one benzene ring, such as catechol, resorcin, and hydroquinone; bisphenols, such as bis(4-hydroxyphenyl)propane (bisphenol A), bis(4-hydroxyphenyl)methane (bisphenol F), and bis(4-hydroxyphenyl)ethane (bisphenol AD); compounds having a condensed ring, such as dihydroxynaphthalene; Examples include bifunctional phenol compounds having an allyl group introduced therein, such as resorcinol, diallyl bisphenol A, and triallyl dihydroxybiphenyl, and dibutyl bisphenol A. Specific examples of the (b) carboxyl group-containing compound include adipic acid, succinic acid, malonic acid, cyclohexanedicarboxylic acid, phthalic acid, isophthalic acid, and terephthalic acid. Examples of the (b) bifunctional compound having a mercapto group include ethylene glycol bisthioglycolate and ethylene glycol bisthiopropionate. Specific examples of the (b) isocyanate group-containing bifunctional compound include diphenylmethane diisocyanate (MDI), isophorone diisocyanate (IPDI), hexamethylene diisocyanate (HMDI), and tolylene diisocyanate (TDI). Specific examples of the (b) cyanate ester group-containing bifunctional compound include 2,2-bis(4-cyanatophenyl)propane, 1,1-bis(4-cyanatophenyl)ethane, and bis(4-cyanatophenyl)methane. Among the above (b), a bifunctional compound having a phenolic hydroxyl group is preferred from the viewpoint of obtaining a thermoplastic polymer, a bifunctional compound having two phenolic hydroxyl groups and a bisphenol structure or a biphenyl structure is preferred from the viewpoint of heat resistance and adhesiveness, and bisphenol A, bisphenol F or bisphenol S is preferred from the viewpoint of heat resistance and cost.
[0027] When the (a) is a bisphenol A type epoxy resin, a bisphenol F type epoxy resin, a bisphenol S type epoxy resin, or a biphenyl type epoxy resin, and the (b) is bisphenol A, bisphenol F, or bisphenol S, the polymer obtained by polymerization of the (a) and (b) has a main chain having a paraphenylene structure and an ether bond as a main skeleton, the main chain being linked by an alkylene group, and a structure in which a hydroxyl group generated by polyaddition is arranged in a side chain. The linear structure of the paraphenylene skeleton can increase the mechanical strength of the polymer after polymerization, and the hydroxyl groups arranged in the side chains can improve adhesion to the substrate. As a result, high adhesive strength can be achieved while maintaining the workability of thermosetting resins. Furthermore, in the case of thermoplastic resins, recycling and repair are possible by softening and melting with heat, improving the recyclability and repairability that are problems with thermosetting resins.
[0028] Phenoxy resin Phenoxy resin is a polyhydroxy polyether synthesized from bisphenols and epichlorohydrin, and has thermoplastic properties. For the production of phenoxy resin, a method of direct reaction of dihydric phenols with epichlorohydrin and a method of addition polymerization reaction of diglycidyl ether of dihydric phenols with dihydric phenols are known, but the phenoxy resin used in the present invention may be obtained by either method. In the case of direct reaction of dihydric phenols with epichlorohydrin, examples of dihydric phenols include phenols such as bisphenol A, bisphenol F, bisphenol S, biphenol, biphenylenediol, and fluorenediphenyl; and aliphatic glycols such as ethylene glycol, propylene glycol, and diethylene glycol. Among them, bisphenol A, bisphenol F, and bisphenol S are preferred from the viewpoints of cost, adhesiveness, viscosity, and heat resistance. These may be used alone or in combination of two or more. Phenoxy resin has a chemical structure similar to that of epoxy resin, with a paraphenylene structure and an ether bond as the main skeleton, a main chain connecting these, and a structure in which hydroxyl groups are arranged in the side chains.
[0029] <Thermoplastic epoxy resin and phenoxy resin> The thermoplastic epoxy resin and the phenoxy resin preferably have a weight average molecular weight of 10,000 to 500,000, more preferably 18,000 to 300,000, and even more preferably 20,000 to 200,000, which is a value calculated in terms of polystyrene by GPC (gel permeation chromatography). The weight average molecular weight is calculated from the elution peak position detected by GPC, and each is a value of the molecular weight in terms of standard polystyrene. When the weight average molecular weight is within this range, the balance between thermoplasticity and heat resistance is good, and a bonded body can be efficiently obtained by melting, and the heat resistance is also high. When the weight average molecular weight is 10,000 or more, the heat resistance is excellent, and when it is 500,000 or less, the viscosity during melting is low and the adhesiveness is high.
[0030] <Method for manufacturing solid adhesive> The method for producing the solid adhesive is not particularly limited, but for example, it can be obtained by heating and polymerizing a monomer or oligomer of a bifunctional epoxy compound. A solvent may be added during polymerization to reduce the viscosity and make it easier to stir. If a solvent is added, it must be removed, and the solid adhesive may be obtained by drying or polymerization, or both, on a release film or the like. If necessary, other additives can be blended within a range that does not impair the object of the present invention. The blending amount of the additives with respect to the total amount of the amorphous thermoplastic resin is preferably 50% by volume or less, more preferably 30% by volume or less, even more preferably 20% by volume or less, and most preferably 10% by volume or less. The volume % of the additives represents the volume ratio of the volume of the additives contained before polymerization of the solid bonding agent based on the volume of the total amount of the amorphous thermoplastic resin, and the volume of the additives can be obtained by dividing the weight of the additives contained by the true specific gravity of the additives.
[0031] Examples of the additives include viscosity adjusters, inorganic fillers, organic fillers (resin powders), antifoaming agents, coupling agents such as silane coupling agents, pigments, etc., and these can be used alone or in combination of two or more. As the viscosity modifier, for example, a reactive diluent or the like can be used. Examples of inorganic fillers include spherical fused silica, metal powders such as iron, silica sand, talc, calcium carbonate, mica, acid clay, diatomaceous earth, kaolin, quartz, titanium oxide, silica, phenolic resin microballoons, and glass balloons. The solid bonding agent thus obtained has a small or substantially no content of unreacted monomers or terminal epoxy groups, and therefore has excellent storage stability and can be stored for long periods at room temperature.
[0032] The form of the solid adhesive is not particularly limited, but it is preferable that the solid adhesive has any shape selected from the group consisting of a film, a rod, a pellet, and a powder. In particular, at least one side of the outer shape is preferably 5 mm or less, more preferably 3 mm or less, even more preferably 1 mm or less, even more preferably 0.5 mm or less, and most preferably 0.3 mm or less. By sandwiching a solid adhesive having at least one side of the outer shape of 5 mm or less between the substrate A and the substrate B and applying heat and pressure, the solid adhesive spreads efficiently over the bonding surface, and high adhesive strength is obtained.
[0033] The solid adhesive may have tackiness to the extent that it does not impair the adhesive strength or heat resistance. In this case, the solid adhesive is temporarily fixed to the substrate in the laminate preparation step.
[0034] <Joining process> In the bonding step, the laminate is heated and pressurized to melt the solid bonding agent, and then the temperature is lowered to solidify the solid bonding agent, thereby bonding the base material A and the base material B together.
[0035] The heating temperature is preferably 100 to 400° C., more preferably 120 to 350° C., and even more preferably 150 to 300° C. By heating at 100 to 400° C., the solid bonding agent efficiently deforms and melts, and effectively wets and spreads over the bonding surface, resulting in high adhesive strength. The pressure of the pressurization is preferably 0.01 to 20 MPa, more preferably 0.1 to 10 MPa, and even more preferably 0.2 to 5 MPa. By applying a pressure of 0.01 to 20 MPa, the solid adhesive agent is efficiently deformed and effectively wets and spreads on the adhesion surface, thereby obtaining a high adhesive strength. When at least one of the substrates A and B is a thermoplastic resin, applying a pressure of 0.01 to 20 MPa makes the solid adhesive agent and the substrate compatible, thereby obtaining a strong adhesive strength.
[0036] The main components of the solid adhesive, thermoplastic epoxy resin and phenoxy resin, have low cohesive strength within the resin and contain hydroxyl groups, which give them strong interaction with the base material and enable them to bond dissimilar materials with greater adhesive strength than conventional crystalline hot melt adhesives.
[0037] The bonding of the substrate A and the substrate B utilizes the phase change (solid to liquid to solid) of the solid bonding agent and does not involve a chemical reaction, so bonding can be completed in a shorter time than with conventional thermosetting epoxy resins.
[0038] [zygote] One embodiment of the bonded body of the present invention is shown in Fig. 1. The bonded body 1 shown in Fig. 1 is formed by bonding and integrating a substrate A3 and a substrate B4 via an adhesive layer 2 formed by melting and solidifying a solid bonding agent, the solid adhesive agent being mainly composed of an amorphous thermoplastic resin, which is at least one of a thermoplastic epoxy resin and a phenoxy resin, and the amorphous thermoplastic resin has an epoxy equivalent of 1,600 or more or does not contain an epoxy group and has a heat of fusion of 15 J / g or less. The bonded body of the present invention shows excellent bonding strength even when it is a bonded body of different materials. Since the bonding strength is affected by many factors, such as the thickness of the adhesive layer, the molecular weight and chemical structure of the polymer constituting the adhesive, mechanical properties, and viscoelastic properties, in addition to the strength of the interfacial interaction between the adhesive layer and the substrate, the details of the mechanism by which the bonded body of the present invention exhibits excellent bonding strength are not clear, but it is speculated that the main factors are the low cohesive force in the amorphous thermoplastic resin constituting the adhesive layer 2 and the presence of hydroxyl groups in the resin, which form chemical bonds and intermolecular forces such as hydrogen bonds and van der Waals forces at the interfaces between the adhesive layer and the substrate A and between the adhesive layer and the substrate B. However, in the bonded body, the state or characteristics of the interface of the bonded body is a very thin chemical structure at the nanometer level or less, which is difficult to analyze, and it is impossible or impractical with current technology to identify it and express it in a way that distinguishes it from those that do not use a solid bonding agent.
[0039] The bonded structure of the present invention in which the adhesive layer is made of a thermoplastic resin has excellent recyclability and repairability, and can be easily disassembled into base material A and base material B by heating the bonded structure.
[0040] Each of the substrate A and the substrate B is preferably made of at least one of resin and metal. The metal is preferably at least one selected from the group consisting of aluminum, iron, copper, magnesium, and alloys thereof. From the viewpoints of adhesive strength and base material strength, and of the strength of the interfacial adhesive strength with the solid bonding agent, at least one of an aluminum alloy and an iron alloy is particularly preferable, since a strong bond can be obtained. The resin is preferably one selected from the group consisting of thermoplastic resins, thermosetting resins, and fiber-reinforced plastics (FRP), and from the viewpoints of adhesive strength, cost, and ease of molding, it is more preferably a thermoplastic resin. The combination of the base material A and the base material B is not particularly limited. The shapes of the substrate A and the substrate B are not particularly limited.
[0041] A high adhesive strength may be obtained by subjecting the substrate A and substrate B to a pretreatment suitable for each substrate. As the pretreatment, a pretreatment for cleaning the surface of the substrate or a pretreatment for making the surface uneven is preferable. Specifically, when the substrate is made of aluminum, glass, ceramic, or iron, at least one selected from the group consisting of degreasing treatment, UV ozone treatment, blasting treatment, polishing treatment, plasma treatment, and etching treatment is preferable, and when the substrate is made of FRP, polypropylene, polycarbonate, polymethyl methacrylate, polyetherimide, polyamide, or polybutylene terephthalate, at least one selected from the group consisting of degreasing treatment, UV ozone treatment, blasting treatment, polishing treatment, plasma treatment, and corona discharge treatment is preferable. The pretreatment may be performed by one type alone or by two or more types. As the specific method of these pretreatments, known methods can be used. EXAMPLES
[0042] Next, specific examples of the present invention will be described, but the present invention is not particularly limited to these examples. In the following examples, base material A and base material B are collectively referred to as bonding base materials.
[0043] <Joining base material> The following bonding materials were used: PA6 (6-nylon) A test piece measuring 10 mm in width, 45 mm in length, and 3 mm in thickness was obtained by injection molding using Amilan CM3001G-30 manufactured by Toray Industries, Inc. The test piece was used without surface treatment. In order to efficiently heat the material during ultrasonic welding, linear protrusions with a height of 0.5 mm and an equilateral triangular cross section were created 2.5 mm from the edge. <PBT (Polybutylene terephthalate)> SABIC 20-1001 was injection molded to obtain test pieces with a width of 18 mm, length of 45 mm, and thickness of 1.5 mm. They were used without surface treatment. <PC (Polycarbonate)> SABIC 121R was injection molded to obtain test pieces with a width of 10 mm, a length of 45 mm, and a thickness of 3 mm. They were used without surface treatment. "iron" The surface of the SPCC-SD was blasted to obtain a test piece measuring 10 mm in width, 45 mm in length, and 2.3 mm in thickness. "aluminum" The surface of A6061-T6 was blasted to obtain a test piece with a width of 10 mm, a length of 45 mm, and a thickness of 3 mm.
[0044] <Weight average molecular weight, heat of fusion and epoxy equivalent of thermoplastic epoxy resin and phenoxy resin> The weight average molecular weight, heat of fusion and epoxy equivalent of the solid bonding agent were determined as follows.
[0045] (Weight average molecular weight) The thermoplastic epoxy resin and the phenoxy resin were dissolved in tetrahydrofuran, and the measurement was carried out under the following conditions using Prominence 501 (manufactured by Showa Science Co., Ltd., Detector: Shodex (registered trademark) RI-501 (manufactured by Showa Denko K.K.)). Column: Showa Denko LF-804 x 2 Column temperature: 40℃ Sample: 0.4% by mass of resin in tetrahydrofuran Flow rate: 1ml / min Eluent: Tetrahydrofuran Calibration method: Conversion using standard polystyrene
[0046] (Heat of fusion) 2 to 10 mg of thermoplastic epoxy resin and phenoxy resin were weighed out and placed in an aluminum pan, and the temperature was raised from 23°C to 200°C at 10°C / min using a DSC (DSC8231 manufactured by Rigaku Corporation) to obtain a DSC curve. The heat of fusion was calculated from the area of the endothermic peak at the time of melting in the DSC curve and the weighed value.
[0047] (epoxy equivalent) The values were measured according to JIS K-7236:2001 and converted into values based on the resin solid content. In the case of simple mixtures that did not involve reactions, the values were calculated from the epoxy equivalent and content of each.
[0048] <Example 1> (Solid adhesive P-1) In a reaction apparatus equipped with a stirrer, a reflux condenser, a gas inlet tube, and a thermometer, 1.0 equivalent (203 g) of jER (registered trademark) 1007 (manufactured by Mitsubishi Chemical Corporation, bisphenol A type epoxy resin, weight average molecular weight about 10,000), 1.0 equivalent (12.5 g) of bisphenol S, 2.4 g of triphenylphosphine, and 1,000 g of methyl ethyl ketone were charged, and the temperature was raised to 100 ° C. while stirring under a nitrogen atmosphere. After visually confirming that the mixture had dissolved, the mixture was cooled to 40 ° C. to obtain a resin composition with a solid content of about 20 mass %. The solvent was removed from the mixture, and the mixture was heated at 160 ° C. for 2 hours to obtain a solid adhesive (P-1) in the form of a film with a thickness of 100 μm and a solid content of 100 mass %. The weight average molecular weight was about 37,000. The epoxy equivalent was above the detection limit. No endothermic peak was detected during melting in DSC. (zygote) The following three types of junctions were prepared. In addition, for the open time evaluation, a bonded body for open time evaluation was also prepared in the same manner as described in the "Metal-Metal" section below, except that the solid bonding agent was placed on the aluminum substrate (substrate A) and left to stand for three days, and then the PC substrate (substrate B) was placed on top. 《Resin / Resin》 The solid adhesive P-1 cut to a size of 10 x 15 mm was placed on the PBT substrate, which was the substrate A, and then the PA6 substrate, which was the substrate B, was placed on top of it so that the triangular protrusions were placed on top of it. The overlap between these substrates was 10 mm wide and 5 mm deep. The solid adhesive P-1 was placed so as to cover the entire overlapping area between the substrates. In other words, the substrates A and B were not in direct contact with each other, and the solid adhesive was placed between them to prepare an unbonded laminate. In this specification, "promptly thereafter" means within about 30 minutes. Ultrasonic waves were applied using an ultrasonic welding machine (Seidensha Electronics Co., Ltd., oscillator JII930S, press JIIP30S) to bond the test pieces together by heating and pressure. The amount of penetration was 0.6 mm, and the ultrasonic application time was within 1 second. (The process ended when the penetration was complete, even if it took less than 1 second.) The subsequent holding time was 1 second. A pressure of 110 N (pressure 2.2 MPa) and an oscillation frequency of 28.5 kHz were used. Resin and metal The solid adhesive P-1 cut to a size of 10 x 15 mm was placed on the aluminum base material, which was the base material A, and then the PC base material, which was the base material B, was quickly placed on top of it. The overlapping area between these base materials was 10 mm wide and 5 mm deep. The solid adhesive P-1 was placed so as to cover the entire overlapping area between the base materials. In other words, the base material A and the base material B were not in direct contact with each other, but the solid adhesive was interposed between them, and an unbonded laminate was prepared. A high-frequency induction welding machine (Seidensha Denshi Kogyo Co., Ltd., oscillator UH-2.5K, press JIIP30S) was used to heat the metal by high-frequency induction, and the test pieces were joined together by heating and pressurization. The applied pressure was 110 N (pressure 2.2 MPa), and the oscillation frequency was 900 kHz. The oscillation time was 6 seconds. 《Metal / metal》 The solid adhesive P-1 cut to a size of 10 x 15 mm was placed on the aluminum base material, which was the base material A, and then the iron base material, which was the base material B, was placed on top of it immediately. The overlapping area between these base materials was 10 mm wide and 5 mm deep. The solid adhesive P-1 was placed so as to cover the entire overlapping area between the base materials. In other words, the base materials A and B were not in direct contact with each other, but the solid adhesive was interposed between them, and an unbonded laminate was prepared. A high-frequency induction welding machine (Seidensha Denshi Kogyo Co., Ltd., oscillator UH-2.5K, press JIIP30S) was used to heat the metal by high-frequency induction, and the test pieces were joined together by heating and pressurization. The applied pressure was 110 N (pressure 2.2 MPa), and the oscillation frequency was 900 kHz. The oscillation time was 5 seconds.
[0049] <Example 2> (Solid adhesive P-2) In a reaction apparatus equipped with a stirrer, a reflux condenser, a gas inlet tube, and a thermometer, 20 g of Enotote (registered trademark) YP-50S (manufactured by Nippon Steel Chemical & Material Co., Ltd., phenoxy resin, weight average molecular weight about 50,000) and 80 g of cyclohexanone were charged, and the temperature was raised to 60°C while stirring, and it was confirmed that it had dissolved visually, and it was cooled to 40°C to obtain a resin composition with a solid content of 20% by mass. The solvent was removed from this to obtain a solid adhesive (P-2) in the form of a film with a thickness of 100 μm and a solid content of 100% by mass. The weight average molecular weight was 50,000, and the epoxy equivalent was above the detection limit. No heat of fusion peak was detected in DSC. (zygote) Three types of bonded bodies and a bonded body for open time evaluation were produced in the same manner as in Example 1, except that P-2 was used as the solid bonding agent.
[0050] <Example 3> (Solid adhesive P-3) The resin composition P-2 and crystalline epoxy resin YSLV-80XY (manufactured by Nippon Steel Chemical & Material Co., Ltd.) were mixed in a mass ratio of 98 to 2 to obtain a solid bonding agent (P-3). The weight average molecular weight was 36,000, the epoxy equivalent was 9600 g / eq, and the heat of fusion was 2 J / g. (zygote) Three types of bonded bodies and a bonded body for open time evaluation were produced in the same manner as in Example 1, except that P-3 was used as the solid bonding agent.
[0051] <Example 4> (Solid adhesive P-4) The resin composition P-2 and a crystalline epoxy resin YSLV-80XY (manufactured by Nippon Steel Chemical & Material Co., Ltd.) were mixed in a mass ratio of 94 to 6 to obtain a solid bonding agent (P-4). The weight average molecular weight was 35,000, the epoxy equivalent was 2100 g / eq, and the heat of fusion was 4 J / g. (zygote) Three types of bonded bodies and a bonded body for open time evaluation were produced in the same manner as in Example 1, except that P-4 was used as the solid bonding agent.
[0052] <Example 5> (Solid adhesive P-5) The resin composition P-2 and crystalline epoxy resin YSLV-80XY (manufactured by Nippon Steel Chemical & Material Co., Ltd.) were mixed in a mass ratio of 89:11 to obtain a solid bonding agent (P-5). The weight average molecular weight was 33,000, the epoxy equivalent was 1700 g / eq, and the heat of fusion was 11 J / g. (zygote) Three types of bonded bodies and a bonded body for open time evaluation were produced in the same manner as in Example 1, except that P-5 was used as the solid bonding agent.
[0053] <Example 6> (Solid adhesive P-6) In a reaction apparatus equipped with a stirrer, a reflux condenser, a gas inlet tube, and a thermometer, 1.0 equivalent (203 g) of jER (registered trademark) 1007 (manufactured by Mitsubishi Chemical Corporation, bisphenol A type epoxy resin, molecular weight about 4060), 0.6 equivalent (12.5 g) of bisphenol S (molecular weight 250), 2.4 g of triphenylphosphine, and 1,000 g of methyl ethyl ketone were charged, and the mixture was heated to 100°C while stirring under a nitrogen atmosphere. After visually confirming that the mixture had dissolved, the mixture was cooled to 40°C to obtain a resin composition with a solid content of about 20% by mass. The solvent was removed from the mixture, and the mixture was heated at 160°C for 2 hours to obtain a solid adhesive (P-6) in the form of a film with a thickness of 100 μm and a solid content of 100% by mass. The weight average molecular weight was about 30,000, and the epoxy equivalent was above the detection limit. No heat of fusion peak was detected in the DSC. (zygote) The method for producing the bonded bodies was the same as in Example 1, except that P-6 was used as the solid bonding agent, and three types of bonded bodies and a bonded body for open time evaluation were produced.
[0054] <Comparative Example 1> (Solid adhesive Q-1) Two liquid components of the thermosetting liquid epoxy adhesive E-250 (Konishi Co., Ltd., a two-liquid type consisting of bisphenol-type epoxy resin and amine curing agent) were mixed, applied to a release film, and cured at 100°C for 1 hour. The mixture was then cooled and peeled off from the release film to obtain a 100μm thick solid adhesive film (Q-1). No heat of fusion peak was detected by DSC. The epoxy equivalent and weight average molecular weight could not be measured because the material was insoluble in solvents. (zygote) Three types of bonded bodies and a bonded body for open time evaluation were produced in the same manner as in Example 1, except that Q-1 was used as the solid bonding agent.
[0055] <Comparative Example 2> (Solid adhesive Q-2) An amorphous polycarbonate film (Iupilon (registered trademark) FE2000, manufactured by Mitsubishi Engineering Plastics Corporation, thickness 100 μm) was used as the solid joint Q-2. No heat of fusion peak was detected in DSC. (zygote) Three types of bonded bodies and a bonded body for open time evaluation were produced in the same manner as in Example 1, except that Q-2 was used as the solid bonding agent.
[0056] <Comparative Example 3> (Solid adhesive Q-3) Crystalline epoxy resin YSLV-80XY (manufactured by Nippon Steel Chemical & Material Co., Ltd.) was used as the solid bonding agent (Q-3). The epoxy equivalent was 192 g / eq. The weight average molecular weight was 340. The heat of fusion was 70 J / g. (zygote) Three types of bonded bodies and a bonded body for open time evaluation were produced in the same manner as in Example 1, except that Q-3 was used as the solid bonding agent.
[0057] <Comparative Example 4> (zygote) Two liquid components of thermosetting liquid epoxy adhesive E-250 (Konishi Corporation, a two-liquid type consisting of bisphenol-type epoxy resin and amine curing agent) were mixed, applied to three types of substrates A and B similar to those in Example 1, and bonded together within one minute. After that, the substrates were fixed with clips and left to stand in an oven at 100°C for one hour to cure the adhesive components, and then cooled to room temperature to produce three types of bonded bodies. In addition, a bonded specimen for open time evaluation was also prepared in the same manner as above, except that the thermosetting liquid epoxy adhesive E-250 was applied to substrate A and substrate B, and then left to stand for 3 days before bonding.
[0058] <Comparative Example 5> In a flask, 1.0 equivalent (203 g) of jER (registered trademark) 1007 (manufactured by Mitsubishi Chemical Corporation, bisphenol A type epoxy resin, weight average molecular weight about 10,000), 1.0 equivalent (12.5 g) of bisphenol S, 2.4 g of triphenylphosphine, and 1,000 g of methyl ethyl ketone were charged and stirred at room temperature to obtain a liquid resin composition with a solid content of about 20 mass%. The liquid resin composition was bar-coated on each of three types of substrate B similar to those in Example 1, dried at room temperature for 30 minutes, and then left to stand in an oven at 160 ° C. for 2 hours to form a solid thermoplastic epoxy resin polymer coating layer with a thickness of 100 μm on the surface of the substrate B. The weight average molecular weight of the coating layer was about 40,000. The epoxy equivalent was above the detection limit. No heat of fusion peak was detected in DSC. (zygote) Three types of bonded bodies were produced in the same manner as in Example 1, except that the base material A was placed directly on the base material B having the coating layer. In addition, for the open time evaluation, a joint for open time evaluation was also prepared in the same manner as above, except that a thermoplastic epoxy resin polymer coating layer was formed on the surface of substrate B, allowed to stand for 3 days, and then laminated with substrate A.
[0059] <Comparative Example 6> A reactor equipped with a stirrer, a reflux condenser, a gas inlet tube, and a thermometer was charged with 20 g of FENOTOTE (registered trademark) YP-50S (manufactured by Nippon Steel Chemical & Material Co., Ltd., phenoxy resin, weight average molecular weight about 50,000) and 80 g of cyclohexanone, and the temperature was raised to 60°C while stirring. Dissolution was confirmed visually, and the mixture was cooled to 40°C to obtain a liquid resin composition with a solid content of 20% by mass. The liquid resin composition was bar-coated on each of three types of substrate B similar to those in Example 1, and the substrate was left to stand in an oven at 70°C for 30 minutes to form a phenoxy resin coating layer with a thickness of 100 μm on the surface of the substrate B. The weight average molecular weight of the coating layer was about 50,000. The epoxy equivalent was above the detection limit. No heat of fusion peak was detected in DSC. (zygote) Three types of bonded bodies were produced in the same manner as in Example 1, except that the base material A was placed directly on the base material B having the phenoxy resin coating layer. In addition, for the open time evaluation, a joint for open time evaluation was also prepared in the same manner as above, except that a phenoxy resin coating layer was formed on the surface of substrate B, which was then left to stand for 3 days, and then laminated with substrate A.
[0060] <Comparative Example 7> (zygote) Three types of bonded bodies and a bonded body for open time evaluation were prepared in the same manner as in Example 1, except that a crystalline polyamide-based hot melt adhesive film NT-120 (manufactured by Nihon Matai Co., Ltd., thickness 100 μm) was used as the solid bonding agent. The heat of fusion was 60 J / g.
[0061] [Shear adhesive strength] The bonded bodies obtained in Examples 1 to 6 and Comparative Examples 1 to 7 were allowed to stand at the measurement temperature (23°C or 80°C) for 30 minutes or more, and then a tensile shear adhesive strength test was performed in an atmosphere of 23°C and 80°C in accordance with ISO19095 using a tensile testing machine (Universal testing machine autograph "AG-X plus" (manufactured by Shimadzu Corporation); load cell 10 kN, tensile speed 10 mm / min) to measure the bond strength. The measurement results are shown in Table 1.
[0062] [Joining process time] The bonding process time was measured as follows. The time from the start point when at least one of the substrates that constitute the bonded body came into contact with the bonding agent to the end point when the fabrication of the bonded body was completed was measured. The heating and pressing times were averaged for the three types of bonded bodies.
[0063] [Recyclability] Each of the aluminum and iron joints was placed on a hot plate at 200°C and heated for 1 minute, after which it was judged whether it could be easily peeled off with a force of 1 N or less. If it could be peeled off, it was judged as good (○), and if it could not be peeled off, it was judged as unsuitable (×).
[0064] [Repairability] Of the aluminum and iron test pieces (with a layer of the bonding solid remaining on the surface of substrate A or B or both) whose bonding surfaces had broken after the tensile shear strength test at 23°C, substrate A was placed on substrate B, and a bonded structure was produced in the same manner as in Example 1, to obtain a repaired bonded structure. The shear adhesive strength of the repaired bonded structure at 23°C was measured in the same manner as in the test method described above, and if it was 80% or more of the first shear adhesive strength, it was judged as good (◯), and if it was less than 80%, it was judged as unsuitable (×).
[0065] [Open Time Evaluation] The tensile shear adhesive strength test was carried out at 23° C. using the bonded bodies for open time evaluation. If the shear adhesive strength was 80% or more compared to the test pieces prepared by the methods of the examples and comparative examples, it was rated as good (◯), and if it was less than 80%, it was rated as unsuitable (×). A good open time evaluation (◯) means that the open time is long and the convenience is excellent.
[0066] [Table 1] [Industrial Applicability]
[0067] The joined body obtained by the manufacturing method of the present invention can be used, for example, as door side panels, bonnet roofs, tailgates, steering hangers, A-pillars, B-pillars, C-pillars, D-pillars, crash boxes, power control unit (PCU) housings, electric compressor components (inner wall portions, intake port portions, exhaust control valve (ECV) insertion portions, mount boss portions, etc.), lithium ion battery (LIB) spacers, battery cases, LED headlamps, and other automotive parts, as well as smartphones, notebook computers, tablet computers, smart watches, large liquid crystal televisions (LCD-TVs), and outdoor LED lighting structures, but is not limited to these exemplified uses. [Explanation of symbols]
[0068] 1. Joint 2 Adhesive layer 3. Substrate A 4. Substrate B
Claims
1. a pre-bonding process of preparing a laminate by arranging a substrate A (excluding woven fabrics and nonwoven fabrics made of natural or synthetic fibers), a film, and a substrate B (excluding woven fabrics and nonwoven fabrics made of natural or synthetic fibers) in this order; a bonding step of heating and pressurizing the laminate to melt the film and bond the base material A and the base material B together, The film contains a resin component in an amount of 50% by mass or more, The epoxy equivalent of the resin component is 1,600 or more, or the resin component does not contain an epoxy group, and the heat of fusion of the resin component is 15 J / g or less, The resin component contains 80% by mass or more of an amorphous thermoplastic resin which is at least one of a thermoplastic epoxy resin and a phenoxy resin, The thermoplastic epoxy resin is (a) a polymer of a bifunctional epoxy resin monomer or oligomer and (b) a bifunctional compound having two identical or different functional groups selected from the group consisting of a phenolic hydroxyl group, a carboxyl group, a mercapto group, an isocyanate group, and a cyanate ester group (excluding bisphenols and polyhydroxy polyethers synthesized from epichlorohydrin), The phenoxy resin is a polyhydroxy polyether synthesized from a bisphenol and epichlorohydrin, The film is produced by removing the solvent from a resin composition dissolved in a solvent to form a film, The bonding is performed by heating the molten film to wet and spread on the adhesive surfaces of the substrate A and the substrate B, and then solidifying on the adhesive surfaces. the content of the amide-based compound in the film is less than 1% by mass relative to 100% by mass of the amorphous thermoplastic resin; The content of γ-butyrolactone in the film is less than 1% by mass relative to 100% by mass of the amorphous thermoplastic resin. A method for manufacturing a joint body.
2. The method for producing a bonded body according to claim 1, wherein the heating and pressing are carried out under conditions of 100 to 400° C. and 0.01 to 20 MPa.
3. 3. The method for producing a joined body according to claim 1, wherein the base material A is made of at least one of a resin and a metal, and the base material B is made of at least one of a resin and a metal.
4. A bonded body obtained by bonding a substrate A (excluding woven fabrics and nonwoven fabrics made of natural or synthetic fibers) and a substrate B (excluding woven fabrics and nonwoven fabrics made of natural or synthetic fibers) via an adhesive layer, the adhesive layer is formed by disposing a film between the substrate A and the substrate B, applying heat and pressure to melt the film, and solidifying the film; The film contains a resin component in an amount of 50% by mass or more, The epoxy equivalent of the resin component is 1,600 or more, or the resin component does not contain an epoxy group, and the heat of fusion of the resin component is 15 J / g or less, The resin component contains 80% by mass or more of an amorphous thermoplastic resin which is at least one of a thermoplastic epoxy resin and a phenoxy resin, The thermoplastic epoxy resin is (a) a polymer of a bifunctional epoxy resin monomer or oligomer and (b) a bifunctional compound having two identical or different functional groups selected from the group consisting of a phenolic hydroxyl group, a carboxyl group, a mercapto group, an isocyanate group, and a cyanate ester group (excluding bisphenols and polyhydroxy polyethers synthesized from epichlorohydrin), The phenoxy resin is a polyhydroxy polyether synthesized from a bisphenol and epichlorohydrin, The film is produced by removing the solvent from a resin composition dissolved in a solvent to form a film, The bonding is performed by heating the molten film to wet and spread on the adhesive surfaces of the substrate A and the substrate B, and then solidifying on the adhesive surfaces. the content of the amide-based compound in the film is less than 1% by mass relative to 100% by mass of the amorphous thermoplastic resin; The content of γ-butyrolactone in the film is less than 1% by mass relative to 100% by mass of the amorphous thermoplastic resin. zygote.
5. 5. The bonded body according to claim 4, wherein the heating and pressing are carried out under conditions of 100 to 400° C. and 0.01 to 20 MPa.
6. 6. The joined body according to claim 4, wherein the substrate A is made of at least one of a resin and a metal, and the substrate B is made of at least one of a resin and a metal.
Citation Information
Patent Citations
Adhesion and surface working method for cloth
JP1981053072A
Bonding method of metal plate
JP1981089520A
Prepreg and laminate
JP1998017685A
Hot-melt adhesive
JP1998168417A
Phenoxy resin composition and adhesive composition using the same
JP2017052907A