Electroless nickel-phosphorus plating bath

The electroless nickel-phosphorus plating bath with specific compositions and additives addresses the issue of crack resistance in nickel-phosphorus films after heat treatment, ensuring improved hardness and thermal stability for electronic and automotive parts.

JP7560093B2Active Publication Date: 2024-10-02OKUNO CHEM IND CO LTD

Patent Information

Application Number
JP2020097178
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-06-03
Publication Date
2024-10-02
Estimated Expiration
2040-06-03

AI Technical Summary

Technical Problem

Existing electroless nickel-phosphorus plating films suffer from insufficient crack resistance after heat treatment, particularly in applications requiring improved hardness and thermal stability.

Method used

A low-phosphorus and sulfur-free electroless nickel-phosphorus plating bath comprising a water-soluble nickel compound, a reducing agent with a concentration of 13 g/L or less, and phosphorous acid or phosphites with a concentration of 30 g/L or more, along with optional additives like glutamic acid and gluconate, to achieve a peak intensity ratio Ni(111)/Ni(200) less than 1.0 and Vickers hardness of 800 HV or less after heat treatment.

Benefits of technology

The solution effectively suppresses cracking and enhances crack resistance in electroless nickel-phosphorus plating films, maintaining excellent film properties even after heat treatment, suitable for applications in electronic parts and automobile components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007560093000002
    Figure 0007560093000002
  • Figure 0007560093000003
    Figure 0007560093000003
  • Figure 0007560093000004
    Figure 0007560093000004
Patent Text Reader

Abstract

To provide an electroless nickel-phosphorus plating bath capable of forming a plating film that resists cracking even when subjected to heat treatment and exhibits excellent crack resistance after the heat treatment; to additionally provide an electroless nickel-phosphorus plating method capable of forming a plating film that resists cracking even when subjected to heat treatment and exhibits excellent crack resistance after the heat treatment; and to furthermore provide an electroless nickel-phosphorus plating film that resists cracking even when subjected to heat treatment and exhibits excellent crack resistance after the heat treatment.SOLUTION: An electroless nickel-phosphorus plating bath contains (1) a water-soluble nickel compound, (2) a reducer, and (3) one selected from the group consisting of phosphorous acid and phosphite, a content of the reducer being 13 g / L or less, a content of the one selected form phosphorous acid and phosphite being 30 g / L or more.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an electroless nickel-phosphorus plating bath. [Background technology]

[0002] Electroless nickel plating has excellent film properties and can form a uniform film even on objects with complex shapes, and is therefore widely used in a variety of fields, including electronic components and automobile parts.

[0003] Electroless nickel plating is classified into, for example, electroless nickel-phosphorus plating, electroless nickel-boron plating, etc., depending on the type of reducing agent contained in the plating bath. For electroless nickel plating, electroless nickel-phosphorus plating baths containing hypophosphite or the like as a reducing agent are widely used. Electroless nickel-phosphorus plating is classified into three types according to the phosphorus content (phosphorus content) contained in the plating film: low phosphorus (phosphorus content is about 0.1 to 5 mass%), medium phosphorus (phosphorus content is about 6 to 9 mass%), and high phosphorus (phosphorus content is about 10 to 13 mass%). Since the film properties differ depending on the phosphorus content in the electroless nickel-phosphorus plating film, an appropriate type of plating film is selected according to various applications.

[0004] In addition, it is known that the crystal structure of the electroless nickel-phosphorus plating film varies depending on the content; for example, low phosphorus types are microcrystalline, while high phosphorus types are amorphous single phase. After electroless nickel-phosphorus plating film is formed, heat treatment is performed to improve the hardness, but the higher the phosphorus content, the higher the temperature and longer the treatment time. Heat treatment causes a change in the crystal structure, and Ni3P is formed in the film, improving the film hardness. On the other hand, in the case of plating film with a high phosphorus content, cracks may occur when heat treatment is performed because the relative precipitation amount of Ni3P phase due to the structural change is large. To avoid such cracks in the plating film, low phosphorus electroless nickel-phosphorus plating baths are used.

[0005] In addition to being classified according to the phosphorus content, electroless nickel plating baths are also classified according to whether or not they contain a sulfur compound as an additive. When a plating bath contains a sulfur compound, it has advantages such as improved deposition speed and improved throwing power. On the other hand, when a plating bath contains a sulfur compound, it has problems such as a decrease in corrosion resistance of the plating film and embrittlement of the plating film due to sulfur segregation to the grain boundaries after heat treatment.

[0006] Therefore, in order to emphasize the film properties of the electroless nickel plating film, electroless nickel plating baths that do not contain sulfur compounds (sulfur-free) are used.

[0007] In light of the above-mentioned conventional techniques, development of low-phosphorus and sulfur-free electroless nickel plating baths is underway (see, for example, Patent Documents 1 to 3, etc.). [Prior art documents] [Patent documents]

[0008] [Patent Document 1] JP 2008-248318 A [Patent Document 2] JP 2013-014809 A [Patent Document 3] JP 2008-285752 A

[0009] However, Patent Documents 1 to 3 have a problem that the crack resistance of the electroless nickel-phosphorus plating film after heat treatment is insufficient. Since the articles on which the electroless nickel-phosphorus plating is formed are used for various purposes, the above-mentioned low-phosphorus type electroless nickel-phosphorus plating film is required to suppress the occurrence of cracks even if the hardness is improved by heat treatment, and further crack resistance is required. Summary of the Invention [Problem to be solved by the invention]

[0010] The present invention aims to provide an electroless nickel-phosphorus plating bath capable of forming a plating film that is suppressed from cracking even when heat treatment is performed and has excellent crack resistance after heat treatment. The present invention also aims to provide an electroless nickel-phosphorus plating method capable of forming a plating film that is suppressed from cracking even when heat treatment is performed and has excellent crack resistance after heat treatment. A further object of the present invention is to provide an electroless nickel-phosphorus plating film that is suppressed from cracking even when heat treatment is performed and has excellent crack resistance after heat treatment. [Means for solving the problem]

[0011] As a result of intensive research aimed at solving the above-mentioned problems, the inventors have found that the above-mentioned object can be achieved by configuring an electroless nickel-phosphorus plating bath containing (1) a water-soluble nickel compound, (2) a reducing agent, and (3) at least one selected from the group consisting of phosphorous acid and a phosphite, wherein the content of the reducing agent and the content of the at least one selected from the group consisting of phosphorous acid and a phosphite are within specific ranges, and have thus completed the present invention.

[0012] That is, the present invention relates to the following electroless nickel-phosphorus plating bath, electroless nickel-phosphorus plating method, and electroless nickel-phosphorus plating film. 1.(1) Water-soluble nickel compounds, (2) a reducing agent, and (3) containing at least one selected from the group consisting of phosphorous acid and phosphites; The content of the reducing agent is 13 g / L or less, The content of at least one selected from the group consisting of phosphorous acid and phosphites is 30 g / L or more. Electroless nickel-phosphorus plating bath. 2. The electroless nickel-phosphorus plating bath according to Item 1, wherein the reducing agent is at least one selected from the group consisting of hypophosphorous acid and hypophosphites. 3. The electroless nickel-phosphorus plating bath according to item 1 or 2, wherein the at least one selected from the group consisting of phosphorous acid and phosphites is added externally. 4. The electroless nickel-phosphorus plating bath according to any one of items 1 to 3, further comprising at least one selected from the group consisting of glutamic acid and glutamic acid salts. 5. The electroless nickel-phosphorus plating bath according to any one of items 1 to 4, further comprising at least one selected from the group consisting of glycine and gluconates. 6. The electroless nickel-phosphorus plating bath according to any one of items 1 to 5, which is substantially free of sulfur compounds. 7. An electroless nickel-phosphorus plating method comprising a step of contacting an object to be plated with an electroless nickel-phosphorus plating bath to form an electroless nickel-phosphorus plating film, The electroless nickel-phosphorus plating bath comprises (1) Water-soluble nickel compounds, (2) a reducing agent, and (3) containing at least one selected from the group consisting of phosphorous acid and phosphites; The content of the reducing agent is 13 g / L or less, The content of at least one selected from the group consisting of phosphorous acid and phosphites is 30 g / L or more. Electroless nickel-phosphorus plating method. 8. The electroless nickel-phosphorus plating method according to item 7, wherein the electroless nickel-phosphorus plating film has a measured peak intensity ratio Ni(111) / Ni(200) of Ni(111) to Ni(200) of less than 1.0 in analysis by X-ray diffraction after heat treatment. 9. The electroless nickel-phosphorus plating method according to item 7 or 8, wherein the Vickers hardness of the electroless nickel-phosphorus plating film after heat treatment is 800 HV or less. 10. An electroless nickel-phosphorus plating film, in which the measured peak intensity ratio Ni(111) / Ni(200) of Ni(111) to Ni(200) in analysis by X-ray diffraction after heat treatment is less than 1.0. Item 11. The electroless nickel-phosphorus plating film according to item 10, having a Vickers hardness of 800 HV or less after heat treatment at a temperature of 400 ° C. Effect of the Invention

[0013] The electroless nickel-phosphorus plating bath of the present invention is capable of suppressing the occurrence of cracks even when subjected to heat treatment, and is capable of forming a plating film having excellent crack resistance after heat treatment. The electroless nickel-phosphorus plating method of the present invention is capable of suppressing the occurrence of cracks even when subjected to heat treatment, and is capable of forming a plating film having excellent crack resistance after heat treatment. Furthermore, the electroless nickel-phosphorus plating film of the present invention is capable of suppressing the occurrence of cracks even when subjected to heat treatment, and is excellent in crack resistance after heat treatment. [Brief description of the drawings]

[0014] [Figure 1] 1 is a photograph showing the surface of an electroless nickel-phosphorus plating film formed using the electroless nickel-phosphorus plating bath of Example 1, heat-treated, and then subjected to an Erichsen test. [Diagram 2] 1 is a photograph showing the surface of an electroless nickel-phosphorus plating film formed using the electroless nickel-phosphorus plating bath of Comparative Example 1, heat-treated, and then subjected to an Erichsen test. [Diagram 3] 1 is a photograph showing the surface of an electroless nickel-phosphorus plating film formed using the electroless nickel-phosphorus plating bath of Comparative Example 2, heat-treated, and then subjected to an Erichsen test. [Figure 4] 1 is a photograph showing the surface of an electroless nickel-phosphorus plating film formed using the electroless nickel-phosphorus plating bath of Comparative Example 3, heat-treated, and then subjected to an Erichsen test. [Diagram 5] FIG. 2 is a diagram showing the results of XRD analysis of an electroless nickel-phosphorus plating film formed using the electroless nickel-phosphorus plating bath of Example 1 and subjected to heat treatment. [Figure 6] FIG. 2 is a diagram showing the results of XRD analysis of an electroless nickel-phosphorus plating film formed using the electroless nickel-phosphorus plating bath of Comparative Example 1 and subjected to heat treatment. [Figure 7] FIG. 13 is a diagram showing the results of XRD analysis of an electroless nickel-phosphorus plating film formed using the electroless nickel-phosphorus plating bath of Comparative Example 2 and subjected to heat treatment. [Figure 8] FIG. 13 is a diagram showing the results of XRD analysis of an electroless nickel-phosphorus plating film formed using the electroless nickel-phosphorus plating bath of Comparative Example 3 and subjected to heat treatment. [Figure 9] FIG. 2 is a diagram showing the results of XRD analysis of an electroless nickel-phosphorus plating film formed using the electroless nickel-phosphorus plating bath of Example 1 and before heat treatment. [Figure 10] FIG. 2 is a diagram showing the results of XRD analysis of an electroless nickel-phosphorus plating film formed using the electroless nickel-phosphorus plating bath of Comparative Example 1 and before heat treatment. [Figure 11] FIG. 1 is a diagram showing the results of XRD analysis of an electroless nickel-phosphorus plating film formed using the electroless nickel-phosphorus plating bath of Comparative Example 2 and before heat treatment. [Figure 12] FIG. 13 is a diagram showing the results of XRD analysis of an electroless nickel-phosphorus plating film formed using the electroless nickel-phosphorus plating bath of Comparative Example 3 and before heat treatment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] The present invention will be described in detail below.

[0016] In this specification, "low phosphorus" means that the phosphorus content in the plating film is 0.1 to 5 mass%, "medium phosphorus" means that the phosphorus content in the plating film is 6 to 9 mass%, and "high phosphorus" means that the phosphorus content in the plating film is 10 to 13 mass%. The phosphorus content in the plating film is a value measured by an X-ray fluorescence analyzer.

[0017] 1. Electroless nickel-phosphorus plating bath The electroless nickel-phosphorus plating bath of the present invention is an electroless nickel-phosphorus plating bath comprising (1) a water-soluble nickel compound, (2) a reducing agent, and (3) at least one selected from the group consisting of phosphorous acid and phosphites, in which the content of the reducing agent is 13 g / L or less, and the content of the at least one selected from the group consisting of phosphorous acid and phosphites is 30 g / L or more. The electroless nickel-phosphorus plating bath of the present invention includes the above (1) to (3), and satisfies both the requirement that the content of the reducing agent is 13 g / L or less, and the requirement that the content of at least one selected from the group consisting of phosphorous acid and phosphites is 30 g / L or more, so that the measured peak intensity ratio Ni(111) / Ni(200) of Ni(111) and Ni(200) in the analysis by X-ray diffraction method after heat treatment of the electroless nickel-phosphorus plating film formed can be made less than 1.0, the hardness of the electroless nickel-phosphorus plating film after heat treatment is reduced, and the electroless nickel-phosphorus plating film after heat treatment exhibits excellent crack resistance. Even if the content of the reducing agent is 13 g / L or less, if the content of at least one selected from the group consisting of phosphorous acid and phosphites is less than 30 g / L, the electroless nickel-phosphorus plating film after heat treatment cannot exhibit the excellent crack resistance. In addition, even if the content of at least one selected from the group consisting of phosphorous acid and phosphites is 30 g / L or more, if the content of the reducing agent exceeds 13 g / L, the excellent crack resistance cannot be exhibited. That is, the electroless nickel-phosphorus plating bath of the present invention contains the above (1) to (3), and by setting the content of the reducing agent to 13 g / L or less and the content of at least one selected from the group consisting of phosphorous acid and phosphites to 30 g / L or more, the measured peak intensity of Ni(200) becomes dominant in the analysis by X-ray diffraction method after heat treatment of the electroless nickel-phosphorus plating film formed, the hardness of the electroless nickel-phosphorus plating film after heat treatment can be reduced, and the electroless nickel-phosphorus plating film after heat treatment can exhibit excellent crack resistance.

[0018] (Water-soluble nickel compounds) The water-soluble nickel compound is not particularly limited, and known nickel compounds used in electroless nickel-phosphorus plating baths can be used. Examples of water-soluble nickel compounds include water-soluble nickel inorganic salts such as nickel sulfate, nickel chloride, nickel hypophosphite, and nickel carbonate; water-soluble nickel organic salts such as nickel acetate and nickel malate, and hydrates thereof. More specifically, nickel sulfate hexahydrate can be used. The water-soluble nickel compound can be used alone or in combination of two or more kinds. When two or more water-soluble nickel compounds are used in combination, the mixing ratio is not particularly limited and can be determined appropriately.

[0019] The concentration of the water-soluble nickel compound in the electroless nickel-phosphorus plating bath is not particularly limited as long as it is within a range in which an electroless nickel-phosphorus plating film can be formed, and can be appropriately adjusted. The concentration of the water-soluble nickel compound can be, for example, about 0.01 to 100 g / L, preferably 0.5 to 50 g / L, more preferably 1 to 10 g / L, and even more preferably 2 to 7 g / L, in terms of nickel metal. When the lower limit of the concentration of the water-soluble nickel compound is within the above range in terms of nickel metal, the deposition rate is further improved. When the upper limit of the concentration of the water-soluble nickel compound is within the above range in terms of nickel metal, the bath stability is further improved.

[0020] (reducing agent) The reducing agent is not particularly limited, and known reducing agents used in electroless nickel-phosphorus plating baths can be used. The reducing agent can be, for example, at least one selected from the group consisting of hypophosphorous acid, hypophosphites (e.g., sodium salts, potassium salts, ammonium salts, etc.), and hydrates thereof; other reducing agents such as dimethylamine borane, diethylamine borane, trimethylamine borane, sodium borohydride, hydrazine, etc. As the at least one selected from the group consisting of hypophosphorous acid and hypophosphites, more specifically, sodium hypophosphite monohydrate, etc. is preferably used.

[0021] The reducing agent is preferably at least one selected from the group consisting of hypophosphorous acid and hypophosphites. The reducing agent may be a combination of at least one selected from the group consisting of hypophosphorous acid and hypophosphites with another reducing agent.

[0022] The reducing agent may be used alone or in combination of two or more. When two or more reducing agents are used in combination, the mixing ratio is not particularly limited and may be appropriately determined.

[0023] The concentration of the reducing agent in the electroless nickel-phosphorus plating bath is 13 g / L or less. If the concentration of the reducing agent exceeds 13 g / L, the measured peak intensity ratio Ni(111) / Ni(200) of Ni(111) and Ni(200) in the analysis of the electroless nickel-phosphorus plating film after the heat treatment by the X-ray diffraction method becomes 1.0 or more, so that the hardness of the electroless nickel-phosphorus plating film after the heat treatment increases and the crack resistance decreases. The concentration of the reducing agent is preferably 11 g / L or less, more preferably 10 g / L or less, even more preferably 8 g / L or less, and particularly preferably 7 g / L or less. The concentration of the reducing agent is preferably 0.1 g / L or more, more preferably 1 g / L or more, even more preferably 2 g / L or more, and particularly preferably 3 g / L or more. If the lower limit of the concentration of the reducing agent is in the above range, the deposition rate of the electroless nickel-phosphorus plating film is further improved and the deposition is sufficient.

[0024] (Ratio of Ni mass / reducing agent mass) In the electroless nickel-phosphorus plating bath, the mass ratio of the nickel metal to the reducing agent (mass of Ni / mass of reducing agent) is preferably 0.05 to 5.0, more preferably 0.1 to 3.0, even more preferably 0.5 to 2.0, and particularly preferably 0.7 to 1.5. By setting the mass ratio of the nickel metal to the reducing agent within the above range, the productivity of the low-phosphorus electroless nickel-phosphorus plating film is further improved. In particular, if the mass ratio of the nickel metal to the reducing agent is less than 0.05, the phosphorus content in the plating film becomes high, and it may not be possible to form a low-phosphorus electroless nickel-phosphorus plating film, and if it exceeds 5.0, it may be possible to form a low-phosphorus electroless nickel-phosphorus plating film, but the deposition rate of the plating film may decrease, and production efficiency may decrease, so it is preferable to set it within the above range.

[0025] (Phosphorous acid (salt)) In this specification, "at least one selected from the group consisting of phosphorous acid and phosphites" is also referred to as "phosphorous acid (salt)".

[0026] The electroless nickel-phosphorus plating bath of the present invention is characterized by containing phosphorous acid (salt), and even if the electroless nickel-phosphorus plating bath is a low-phosphorus and sulfur-free electroless nickel-phosphorus plating bath, by containing phosphorous acid (salt), a plating film excellent in crack resistance can be obtained even if a heat treatment is performed to improve the hardness after the plating film is formed. In addition, by adding phosphorous acid (salt) to the electroless nickel-phosphorus plating bath, it is possible to suppress excessive adsorption of the stabilizer (galling) and stabilize the deposition rate of the plating.

[0027] The phosphorous acid (salt) is not particularly limited, and known phosphorous acid (salt) used in electroless nickel-phosphorus plating baths can be used. Examples of phosphorous acid (salt) include phosphorous acid, phosphites (e.g., sodium salt, potassium salt, ammonium salt, etc.), and hydrates thereof. More specifically, disodium hydrogen phosphite pentahydrate can be used. The phosphorous acid (salt) can be used alone or in combination of two or more kinds. When two or more kinds of phosphorous acid (salt) are used in combination, the mixing ratio is not particularly limited and can be determined appropriately.

[0028] The concentration of phosphorous acid (salt) in the electroless nickel-phosphorus plating bath is 30 g / L or more. If the concentration of phosphorous acid (salt) is less than 30 g / L, the measured peak intensity ratio Ni(111) / Ni(200) of Ni(111) and Ni(200) in the analysis by X-ray diffraction method after heat treatment of the electroless nickel-phosphorus plating film formed is 1.0 or more, so that the hardness of the electroless nickel-phosphorus plating film after heat treatment increases and the crack resistance decreases. The concentration of phosphorous acid (salt) is preferably 40 g / L or more, more preferably 50 g / L or more, even more preferably 70 g / L or more, and particularly preferably 90 g / L or more. In addition, the concentration of phosphorous acid (salt) is preferably 200 g / L or less, more preferably 170 g / L or less, even more preferably 150 g / L or less, particularly preferably 130 g / L or less, most preferably 120 g / L or less, and most preferably 110 g / L or less. When the upper limit of the phosphorous acid (salt) concentration is within the above range, structural changes in the electroless nickel-phosphorus plating film before and after heat treatment are suppressed, so that an increase in hardness after heat treatment is further suppressed, and cracking of the electroless nickel-phosphorus plating film after heat treatment is suppressed, thereby further improving the crack resistance.

[0029] (External addition of phosphorous acid (salt)) In the electroless nickel-phosphorus plating bath, the phosphorous acid (salt) is preferably added externally so that the concentration of the phosphorous acid (salt) falls within the above range.

[0030] In the electroless nickel-phosphorus plating bath of the present invention, "phosphorous acid (salt) derived from hypophosphorous acid (salt) contained as a reducing agent" is not considered to be "phosphorous acid (salt) contained in the electroless nickel-phosphorus plating bath of the present invention." In the electroless nickel-phosphorus plating bath of the present invention, it is preferable that the phosphorous acid (salt) is added externally, that is, added separately from the reducing agent.

[0031] (Glutamic acid (salt)) In this specification, "at least one selected from the group consisting of glutamic acid and glutamic acid salts" is also referred to as "glutamic acid (salt)".

[0032] The electroless nickel-phosphorus plating bath of the present invention may contain glutamic acid (salt). Even if the electroless nickel-phosphorus plating bath is a low-phosphorus and sulfur-free electroless nickel-phosphorus plating bath, the inclusion of glutamic acid (salt) further improves the crack resistance of the electroless nickel-phosphorus plating film after heat treatment.

[0033] The glutamic acid (salt) is not particularly limited, and a known glutamic acid (salt) used in an electroless nickel-phosphorus plating bath can be used. Examples of the glutamic acid (salt) include glutamic acid and glutamic acid salts (e.g., sodium salt, potassium salt, ammonium salt, etc.). The glutamic acid (salt) can be used alone or in combination of two or more kinds. When two or more kinds of reducing agents are used in combination, the mixing ratio is not particularly limited and can be determined appropriately.

[0034] The concentration of glutamic acid (salt) in the electroless nickel-phosphorus plating bath is not particularly limited as long as it is within a range in which a low-phosphorus type electroless nickel-phosphorus plating film can be formed, and can be appropriately adjusted. The concentration of glutamic acid (salt) can be, for example, about 1 to 100 g / L, preferably about 2 to 50 g / L, and more preferably about 3 to 20 g / L. Even if the electroless nickel-phosphorus plating bath is a low-phosphorus and sulfur-free electroless nickel-phosphorus plating bath, the crack resistance of the electroless nickel-phosphorus plating film after heat treatment is further improved by having a glutamic acid (salt) concentration of about 1 to 100 g / L.

[0035] (Glycine and Gluconate) The electroless nickel-phosphorus plating bath of the present invention preferably contains glycine and gluconate as complexing agents. By using specific complexing agents in combination in this way, decomposition of the plating bath is suppressed even in continuous use, and a low-phosphorus and sulfur-free electroless nickel-phosphorus plating bath having even better bath stability can be obtained.

[0036] The gluconate is not particularly limited, and any known gluconate used in electroless nickel-phosphorus plating baths can be used. Examples of gluconate include sodium salts, potassium salts, and ammonium salts.

[0037] The concentration of glycine in the electroless nickel-phosphorus plating bath is not particularly limited and can be adjusted appropriately. The electroless nickel-phosphorus plating bath preferably contains about 1 to 100 g / L of glycine. The concentration of glycine can be, for example, about 1 to 100 g / L, preferably about 2 to 50 g / L, and more preferably about 3 to 30 g / L. When the lower limit of the concentration of glycine (complexing agent) is within the above range, the bath stability is further improved. When the upper limit of the concentration of glycine (complexing agent) is within the above range, the deposition rate is further improved.

[0038] The concentration of gluconate in the electroless nickel-phosphorus plating bath is not particularly limited and can be adjusted appropriately. The electroless nickel-phosphorus plating bath preferably contains 0.1 to 100 g / L of gluconate. The concentration of gluconate can be, for example, about 0.1 to 100 g / L, preferably about 0.5 to 50 g / L, and more preferably about 1 to 20 g / L. When the lower limit of the concentration of gluconate is within the above range, the bath stability is further improved. When the upper limit of the concentration of gluconate is within the above range, the deposition rate is further improved.

[0039] (Ratio of glycine mass / gluconate mass) In the electroless nickel-phosphorus plating bath, the mass ratio of glycine to gluconate (mass of glycine / mass of gluconate) is preferably about 1 to 20, and more preferably about 2 to 15. When the lower limit of the mass ratio of glycine to gluconate is within the above range, the phosphorus content in the electroless nickel-phosphorus plating film is further reduced, making it easier to form a low-phosphorus electroless nickel-phosphorus plating film. When the upper limit of the mass ratio of glycine to gluconate is within the above range, the stability of the plating bath is further improved when the plating bath is used continuously.

[0040] (Ratio of Ni mass / glycine mass) In the electroless nickel-phosphorus plating bath, the mass ratio of nickel metal to glycine (mass of Ni / mass of glycine) is preferably about 0.1 to 5, and more preferably about 0.2 to 2. By setting the mass ratio of nickel metal to glycine within the above range, a low-phosphorus electroless nickel-phosphorus plating film can be formed more efficiently. In particular, if the mass ratio of nickel metal to glycine is less than 0.1, a low-phosphorus electroless nickel-phosphorus plating film can be formed, but the deposition rate of the plating film may decrease and the production efficiency may decrease, and if it exceeds 5, the stability may decrease, so it is preferable to set it within the above range.

[0041] (Other complexing agents) In addition to the above-mentioned complexing agents, glycine and gluconate, the electroless nickel-phosphorus plating bath of the present invention may contain a complexing agent (hereinafter, referred to as "other complexing agent") used in electroless nickel plating baths. Examples of such other complexing agents include monocarboxylic acids such as formic acid and acetic acid or their salts (e.g., sodium salts, potassium salts, ammonium salts, etc.); dicarboxylic acids such as malonic acid, succinic acid, adipic acid, maleic acid, fumaric acid or their salts (e.g., sodium salts, potassium salts, ammonium salts, etc.); hydroxycarboxylic acids such as malic acid, lactic acid, glycolic acid, citric acid or their salts (e.g., sodium salts, potassium salts, ammonium salts, etc.); ethylenediaminediacetic acid, ethylenediaminetetraacetic acid or their salts (e.g., sodium salts, potassium salts, ammonium salts, etc.); and amino acids such as alanine and arginine (excluding glycine). The complexing agent may be used alone or in combination of two or more. When two or more complexing agents are used in combination, the mixing ratio is not particularly limited and can be determined appropriately.

[0042] The concentration of the other complexing agent in the electroless nickel-phosphorus plating bath is not particularly limited and can be appropriately adjusted. The concentration of the other complexing agent can be, for example, about 0.5 to 100 g / L.

[0043] (Sulfur compounds) The electroless nickel-phosphorus plating bath of the present invention is preferably substantially free of sulfur compounds as additives (sulfur-free). By being substantially free of sulfur compounds, the electroless nickel-phosphorus plating bath can provide a sulfur-free electroless nickel-phosphorus plating film.

[0044] In this specification, the term "sulfur compound" refers to a compound that has the property of causing sulfur to codeposit in the plating film when electroless nickel-phosphorus plating is performed. Therefore, for example, nickel sulfate (sulfate ion), which is a water-soluble nickel compound, and sulfuric acid used as a pH adjuster, etc., are not compounds that have the property of causing sulfur to codeposit in the plating film when electroless nickel-phosphorus plating is performed, and therefore are not included in the "sulfur compound" defined in this specification.

[0045] In this specification, "substantially free of" sulfur compounds means that the sulfur content in the electroless nickel-phosphorus plating film formed when an electroless nickel-phosphorus plating bath is used is about 0.001 to 0.005 mass% or less. The sulfur content in the electroless nickel-phosphorus plating film can be measured by a carbon-sulfur analyzer using a combustion method. Therefore, "substantially free of" sulfur compounds does not exclude the case where the concentration of sulfur compounds in the electroless nickel-phosphorus plating bath is so small that the sulfur component contained in the electroless nickel-phosphorus plating film does not exceed the above-mentioned numerical range, and does not only mean that the plating bath does not contain any sulfur compounds.

[0046] That is, in the electroless nickel-phosphorus plating bath of the present invention, the electroless nickel-phosphorus plating film may contain a trace amount of sulfur compounds to the extent that the sulfur component does not exceed the above-mentioned numerical range, and it is preferable that the electroless nickel-phosphorus plating film does not contain any sulfur compounds at all. Examples of sulfur compounds include thiosulfuric acid or its salts (e.g., sodium salt, etc.) used as an accelerator, and thiourea used as a stabilizer.

[0047] The electroless nickel-phosphorus plating bath of the present invention is capable of carrying out a plating process at a deposition rate equivalent to that of a plating bath containing a sulfur compound, even though the electroless nickel-phosphorus plating bath of the present invention is substantially free of sulfur compounds as an additive.

[0048] (stabilizers, pH adjusters, surfactants, etc.) In addition to the above-mentioned components, the electroless nickel-phosphorus plating bath of the present invention may contain, if necessary, known additives used in electroless nickel plating baths, such as stabilizers, pH adjusters, surfactants, etc.

[0049] Examples of the stabilizer include lead compounds (e.g., lead nitrate, lead acetate, etc.), cadmium compounds (e.g., cadmium nitrate, cadmium acetate, etc.), thallium compounds (e.g., thallium sulfate, thallium nitrate, etc.), antimony compounds (e.g., antimony chloride, potassium antimonyl tartrate, etc.), tellurium compounds (e.g., telluric acid, tellurium chloride, etc.), chromium compounds (e.g., chromium oxide, chromium sulfate, etc.), iron compounds (e.g., iron sulfate, iron chloride, etc.), manganese compounds (e.g., manganese sulfate, manganese nitrate, etc.), bismuth compounds (e.g., bismuth nitrate, bismuth acetate, etc.), tin compounds (e.g., tin sulfate, tin chloride, etc.), selenium compounds (e.g., selenic acid, selenious acid, etc.), cyanides (e.g., methyl cyanide, isopropyl cyanide, etc.), allyl compounds (e.g., allylamine, diallylamine, etc.), and the like.

[0050] The stabilizer may be used alone or in combination of two or more. When two or more stabilizers are used in combination, the mixing ratio is not particularly limited and may be appropriately determined.

[0051] The concentration of the stabilizer in the electroless nickel-phosphorus plating bath is not particularly limited, and may be, for example, about 0.10 to 100 mg / L. In order to further improve the stability of the electroless nickel-phosphorus plating bath, it is preferable to set the concentration of the stabilizer to about 0.10 mg / L or more. When the concentration of the stabilizer is 100 mg / L or less, the occurrence of areas on the treated object where a plating film is not formed (unprecipitated areas) is further suppressed.

[0052] Examples of pH adjusters that can be used include acids such as hydrochloric acid, sulfuric acid, and phosphoric acid; and alkalis such as sodium hydroxide, potassium hydroxide, and aqueous ammonia.

[0053] The pH of the electroless nickel-phosphorus plating bath of the present invention is preferably about 3 to 12, and more preferably about 4 to 9. The pH of the plating bath can be adjusted using the above-mentioned pH adjuster. When the lower limit of the pH is within the above range, the occurrence of undeposited material is further suppressed. When the upper limit of the pH is within the above range, the bath stability is further improved.

[0054] As the surfactant, various surfactants such as nonionic, anionic, cationic, and amphoteric surfactants can be used. For example, aromatic or aliphatic sulfonic acid alkali salts, aromatic or aliphatic carboxylic acid alkali metal salts, etc. can be mentioned. The surfactant can be used alone or in combination of two or more. When two or more surfactants are used in combination, the mixing ratio is not particularly limited and can be appropriately determined.

[0055] The concentration of the surfactant in the electroless nickel-phosphorus plating bath is not particularly limited, and may be, for example, about 0.01 to 1000 mg / L. In order to further improve the effect of preventing pits in the electroless nickel-phosphorus plating bath, it is preferable to set the concentration of the surfactant to about 0.01 mg / L or more. When the concentration of the surfactant is 1000 mg / L or less, the decrease in deposition property due to foaming is further suppressed.

[0056] (Low phosphorus and sulfur-free electroless nickel-phosphorus plating bath) The electroless nickel-phosphorus plating bath of the present invention is preferably a low-phosphorus electroless nickel-phosphorus plating bath. "Low phosphorus" refers to a plating film having a phosphorus content of 0.1 to 5 mass%, and the phosphorus content can be measured by an X-ray fluorescence analyzer.

[0057] A low-phosphorus electroless nickel-phosphorus plating bath is preferred because it further suppresses cracking of the electroless nickel-phosphorus plating film, even when a heat treatment is carried out after the plating film is formed using the low-phosphorus electroless nickel-phosphorus plating bath.

[0058] The electroless nickel-phosphorus plating bath of the present invention, when it is low in phosphorus and sulfur-free, has excellent bath stability in which decomposition of the plating bath is further suppressed even when it is used continuously. In general, whether or not an electroless nickel-phosphorus plating bath can be used continuously is an important factor when using a plating bath industrially, and this point is advantageous.

[0059] When a plating film is formed using the electroless nickel-phosphorus plating bath of the present invention, embrittlement is suppressed even when heat treatment is performed, and the plating film has good film properties such as good solder wettability.

[0060] The electroless nickel-phosphorus plating bath of the present invention is low in phosphorus (phosphorus content is about 0.1 to 5 mass%) and sulfur-free (no sulfur compounds are contained), and even if a heat treatment is carried out to improve the hardness of a plating film formed using this bath, a plating film having excellent crack resistance (no cracks are generated) can be obtained.

[0061] The present invention is preferably a low-phosphorus and sulfur-free electroless nickel-phosphorus plating bath, and by using this, it is possible to obtain a plating film that is excellent in crack resistance (does not generate cracks) even if a heat treatment is performed to improve the hardness after the plating film is formed.

[0062] When plating flat plates such as iron or aluminum plates, cracks do not usually occur simply by performing heat treatment. However, when plating is performed on a substrate with a copper circuit bonded to ceramics, a substrate with an aluminum circuit bonded to ceramics, or an aluminum electrode on a wafer, cracks may occur simply by performing heat treatment. One of the reasons for this is thought to be the difference in thermal expansion coefficient between the substrate with a copper or aluminum circuit bonded to ceramics, the electrode, etc., and the plating film.

[0063] In the present invention, the object to be plated can be suitably applied to electrodes of a wafer of a power module, a substrate in which a copper circuit or an aluminum circuit is bonded to a ceramic, etc. In the manufacture of these plated objects, soldering is often performed, and the temperature may be as high as about 350 degrees, for example. In the process of performing the soldering, the hardness of the formed plating film may increase.

[0064] By using the electroless nickel-phosphorus plating bath of the present invention, when forming a plating film on electrodes of wafers in power modules, substrates in which a copper circuit or an aluminum circuit is bonded to a ceramic, or the like, it is possible to obtain an electroless nickel-phosphorus plating film having excellent crack resistance even if the hardness of the formed plating film increases.

[0065] (Method of manufacturing electroless nickel-phosphorus plating bath) As described above, the electroless nickel-phosphorus plating bath of the present invention contains (1) a water-soluble nickel compound, (2) a reducing agent, and (3) phosphorous acid (salt), and the phosphorous acid (salt) is preferably added externally.

[0066] The electroless nickel-phosphorus plating bath of the present invention is preferably produced by a method for producing the electroless nickel-phosphorus plating bath, the method including a step of adding the phosphorous acid (salt).

[0067] In the electroless nickel-phosphorus plating bath of the present invention, as described above, it is preferable not to consider "phosphorous acid (salt) derived from hypophosphorous acid (salt) contained as a reducing agent" as "phosphorous acid (salt) contained in the electroless nickel-phosphorus plating bath of the present invention." In the electroless nickel-phosphorus plating bath of the present invention, it is preferable that the phosphorous acid (salt) is added externally, that is, added separately from the reducing agent.

[0068] 2. Electroless nickel-phosphorus plating method The electroless nickel-phosphorus plating method of the present invention is an electroless nickel-phosphorus plating method including a step of contacting an object to be plated with an electroless nickel-phosphorus plating bath to form an electroless nickel-phosphorus plating film, the electroless nickel-phosphorus plating bath containing (1) a water-soluble nickel compound, (2) a reducing agent, and (3) at least one selected from the group consisting of phosphorous acid and phosphites, the content of the reducing agent being 13 g / L or less, and the content of the at least one selected from the group consisting of phosphorous acid and phosphites being 30 g / L or more. In the electroless nickel-phosphorus plating method of the present invention, the electroless nickel-phosphorus plating bath of the present invention described above may be used.

[0069] The electroless nickel-phosphorus plating method of the present invention includes a step of contacting an object to be plated with the electroless nickel-phosphorus plating bath to form an electroless nickel-phosphorus plating film. In this specification, this step may be referred to as a "plating step."

[0070] The object to be plated is not particularly limited, and various materials that have been conventionally used for electroless nickel plating can be used. Examples of the object to be plated include metals that are catalytic to the reduction precipitation of electroless nickel plating, such as iron, cobalt, nickel, palladium, or alloys thereof. Metals that are not catalytic to the reduction precipitation of electroless nickel plating, such as copper and aluminum, glass, ceramics, etc., can also be used. In this case, a metal catalyst nucleus such as a palladium nucleus can be attached to the object to be plated before the plating process according to a conventional method.

[0071] In the plating step, the method of bringing the object to be plated into contact with the electroless nickel-phosphorus plating bath is not particularly limited and can be carried out according to a conventional method. For example, the plating step includes a method of immersing the object to be plated in the electroless nickel-phosphorus plating bath.

[0072] The plating conditions (eg, bath temperature, plating time, etc.) are not particularly limited as long as they are conditions that allow a low-phosphorus type electroless nickel-phosphorus plating film to be formed, and can be determined appropriately.

[0073] The bath temperature of the electroless nickel-phosphorus plating bath in the plating step can be appropriately determined depending on the composition of the plating bath, etc. The bath temperature of the electroless nickel-phosphorus plating bath in the plating step can be, for example, about 25° C. or higher, preferably about 40 to 100° C., and more preferably about 70 to 95° C. When the lower limit of the bath temperature is within the above range, the deposition rate of the plating film is further improved, and production efficiency is improved.

[0074] The treatment time in the plating step is not particularly limited, and may be the time required for forming an electroless nickel-phosphorus plating film of a required thickness on the object to be plated. Specifically, the treatment time in the plating step may be appropriately determined depending on the composition of the plating bath, the type of the object to be plated, etc., and may be, for example, about 1 to 1,000 minutes, preferably 5 to 600 minutes.

[0075] Furthermore, the electroless nickel-phosphorus plating method of the present invention may include other steps, if necessary, in addition to the plating step described above. Such other steps include a heat treatment step in which the electroless nickel-phosphorus plating film is subjected to a heat treatment.

[0076] According to the electroless nickel-phosphorus plating method of the present invention, it is possible to provide an electroless nickel-phosphorus plating film having good film properties, such as suppressed embrittlement even when subjected to heat treatment and good solder wettability.

[0077] When the electroless nickel-phosphorus plating bath of the present invention is substantially free of sulfur compounds, according to an electroless nickel-phosphorus plating method using the electroless nickel-phosphorus plating bath, the electroless nickel-phosphorus plating film formed is substantially free of sulfur components, and therefore embrittlement due to heat treatment of the electroless nickel-phosphorus plating film formed is suppressed.

[0078] Therefore, the electroless nickel-phosphorus plating bath and the electroless nickel-phosphorus plating method using the plating bath of the present invention can be preferably applied to members that are heat treated for the purpose of improving the hardness of the plating film, members that are used in a heat-exposed environment such as the joining of electronic components, etc. Examples of such members include members used at joints where solder joining or sintering is performed, semiconductor parts in a high-temperature operating environment, etc.

[0079] The heat treatment method is not particularly limited, and may be a heat treatment method that is usually applied to a member having an electroless nickel-phosphorus plating film formed thereon. Examples of such heat treatment methods include heating with a high-temperature blower dryer, and heating in the air, in a vacuum, in a nitrogen atmosphere, or in a hydrogen reducing atmosphere using a reflow furnace.

[0080] The heat treatment temperature and the heat treatment time are not particularly limited, and the heat treatment may be performed at a temperature and time required for the bonding application. The heat treatment temperature is preferably 200 to 500° C., and more preferably 230 to 400° C. The heat treatment time is preferably 0.1 to 60 minutes, and more preferably 0.5 to 30 minutes.

[0081] In the electroless nickel-phosphorus plating film formed by the electroless nickel-phosphorus plating method of the present invention, the measured peak intensity ratio Ni(111) / Ni(200) of Ni(111) and Ni(200) in the analysis by X-ray diffraction method after heat treatment is preferably less than 1.0, more preferably 0.5 or less, even more preferably 0.1 or less, and particularly preferably 0.01 or less. When Ni(111) / Ni(200) is in the above range, the hardness of the electroless nickel-phosphorus plating film after heat treatment is further reduced, and the crack resistance is further improved. In addition, the lower limit value of Ni(111) / Ni(200) is preferably as low as possible, and may be, for example, 0 or 0.001.

[0082] In this specification, the analysis by X-ray diffraction method (XRD analysis) can be performed by subjecting the electroless nickel-phosphorus plating film to XRD analysis using an XRD measurement device (SmartLab manufactured by RIGAKU Corporation). Also, in this specification, the analysis by X-ray diffraction method (XRD analysis) of the electroless nickel-phosphorus plating film after heat treatment can be performed by subjecting the electroless nickel-phosphorus plating film to heat treatment under conditions of 400°C and 30 minutes, and then performing XRD analysis using the above measurement device.

[0083] The measured peak intensity ratio Ni(111) / Ni(200) can be adjusted to less than 1.0 by forming an electroless nickel-phosphorus plating film using the electroless nickel-phosphorus plating bath of the present invention and heat treating the film. That is, by forming an electroless nickel-phosphorus plating film using the electroless nickel-phosphorus plating bath of the present invention, the measured peak intensity of Ni(200) before heat treatment becomes dominant over the measured peak intensity of Ni(111), and is less than 1.0. In addition, the value of Ni(111) / Ni(200) can be reduced by reducing the content of the reducing agent in the electroless nickel-phosphorus plating bath of the present invention, and the value of Ni(111) / Ni(200) can be increased by increasing the content of the reducing agent. In addition, the value of Ni(111) / Ni(200) can be reduced by increasing the content of phosphorous acid (salt) in the electroless nickel-phosphorus plating bath of the present invention, and the value of Ni(111) / Ni(200) can be increased by reducing the content of phosphorous acid (salt). Electroless nickel-phosphorus plating films with a Ni(111) / Ni(200) ratio of less than 1.0 are inhibited from undergoing structural changes due to heat treatment, and can maintain a Ni(111) / Ni(200) ratio of less than 1.0 even after heat treatment.

[0084] The Vickers hardness of the electroless nickel-phosphorus plating film formed by the electroless nickel-phosphorus plating method of the present invention after heat treatment is preferably 800HV or less, more preferably 700HV or less, and even more preferably 600HV or less. By setting the upper limit of the Vickers hardness within the above range, the electroless nickel-phosphorus plating film after heat treatment is not too hard, and the crack resistance is further improved. In addition, the lower limit of the Vickers hardness may be the lower limit required for the electroless nickel-phosphorus plating film, and is, for example, about 200HV or about 300HV.

[0085] In this specification, the Vickers hardness is a value measured by heat treating the formed electroless nickel-phosphorus plating film at 400°C for 30 minutes, and measuring the surface of the heat-treated electroless nickel-phosphorus plating film at room temperature (25°C) using a micro Vickers hardness tester (HM-200, manufactured by Mitutoyo Corporation) (load 0.49 N).

[0086] The Vickers hardness can be adjusted to the above range by forming an electroless nickel-phosphorus plating film using the electroless nickel-phosphorus plating bath of the present invention described above and subjecting it to heat treatment. In addition, the Vickers hardness decreases by decreasing the content of the reducing agent in the electroless nickel-phosphorus plating bath of the present invention, and increases by increasing the content of the reducing agent. In addition, the Vickers hardness decreases by increasing the content of phosphorous acid (salt) in the electroless nickel-phosphorus plating bath of the present invention, and increases by decreasing the content of phosphorous acid (salt).

[0087] 3. Electroless nickel-phosphorus plating film The electroless nickel-phosphorus plating film of the present invention is an electroless nickel-phosphorus plating film in which the measured peak intensity ratio Ni(111) / Ni(200) of Ni(111) to Ni(200) is less than 1.0 in analysis by X-ray diffraction after heat treatment. By virtue of the above-mentioned configuration, the electroless nickel-phosphorus plating film of the present invention has an even lower hardness and an even more improved crack resistance.

[0088] The electroless nickel-phosphorus plating film of the present invention preferably has a Vickers hardness of 800 HV or less after heat treatment.

[0089] The electroless nickel-phosphorus plating film of the present invention can be formed by the above-mentioned method for forming an electroless nickel-phosphorus plating film of the present invention. The configuration and characteristics of the electroless nickel-phosphorus plating film of the present invention are the same as those described for the electroless nickel-phosphorus plating film formed by the above-mentioned electroless nickel-phosphorus plating method. EXAMPLES

[0090] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples.

[0091] 1. Preparation of electroless nickel-phosphorus plating bath The electroless nickel-phosphorus plating baths of the examples and comparative examples were prepared according to the compositions shown in Table 1.

[0092] An aluminum plate (A5052 material) was used as the plated object, and the plated object was immersed in each of the prepared electroless nickel-phosphorus plating baths (bath temperature 90° C.) to form an electroless nickel-phosphorus plating film having a thickness of 3 μm. The immersion time was 60 minutes in Example 1 and Comparative Example 3, and 30 minutes in Comparative Examples 1 and 2.

[0093] The phosphorus content in the electroless nickel-phosphorus plating film thus formed was measured using an X-ray fluorescence analyzer.

[0094] The sulfur content of the electroless nickel-phosphorus plating film was measured using a carbon-sulfur analyzer that uses the combustion method. When the sulfur content of the electroless nickel-phosphorus plating film was below the detection limit (0.0005 mass%), it was indicated as "ND".

[0095] (Vickers hardness test) The formed electroless nickel-phosphorus plating film was heat-treated by heating at 400°C for 30 minutes using a high-temperature constant-temperature dryer (Advantec DRH453WA), and the Vickers hardness of the surface of the electroless nickel-phosphorus plating film after heat treatment was measured at room temperature (25°C) using a micro Vickers hardness tester (Mitutoyo HM-200) (load 0.49 N).

[0096] The results are shown in Table 1.

[0097] [Table 1]

[0098] From Table 1, it was confirmed that the plating bath of Example 1 was a plating bath with a low phosphorus content in the plating film, and the sulfur content of the plating bath of Example 1 was below the detection limit.

[0099] 2. Evaluation of electroless nickel-phosphorus plating film properties Using the prepared electroless nickel-phosphorus plating bath, an iron plate was used as the substrate and immersed in the electroless nickel-phosphorus plating bath at a bath temperature of 90°C to form an electroless nickel-phosphorus plating film with a thickness of 3 μm.

[0100] (Erichsen tester indentation test (crack resistance evaluation)) The electroless nickel-phosphorus plating film formed on the iron plate as described above was heat treated at a temperature of 400°C for 30 minutes. The electroless nickel-phosphorus plating film after heat treatment was pressed 0.5 mm into the film using an Erichsen testing machine, and the state of cracks occurring on the convex side of the electroless nickel-phosphorus plating film after pressing was confirmed at a magnification of 500 times using a digital microscope (Keyence VHX-2000). The results are shown in Figures 1 to 4.

[0101] Fig. 1 is a photograph of the surface of an electroless nickel-phosphorus plating film when the film was subjected to an Erichsen test after being formed and heat-treated using the electroless nickel-phosphorus plating bath of Example 1. From the results of Fig. 1, it was found that the electroless nickel-phosphorus plating film formed using the electroless nickel-phosphorus plating bath of Example 1 and heat-treated suppressed the occurrence of cracks and had excellent crack resistance.

[0102] 2, 3, and 4 are photographs of the surfaces of electroless nickel-phosphorus plating films formed using the electroless nickel-phosphorus plating baths of Comparative Examples 1, 2, and 3, respectively, and subjected to an Erichsen test after heat treatment. From the results of Fig. 2 to Fig. 4, it was found that the electroless nickel-phosphorus plating films formed using the electroless nickel-phosphorus plating baths of Comparative Examples 1 to 3 and subjected to heat treatment cracked and did not exhibit sufficient crack resistance.

[0103] (Analysis by X-ray diffraction method (XRD analysis)) The electroless nickel-phosphorus plating film formed on the iron plate as described above was heat treated at 400°C for 30 minutes. The electroless nickel-phosphorus plating film after heat treatment was subjected to XRD analysis using an XRD measurement device (SmartLab manufactured by RIGAKU Corporation). The results are shown in Figures 5 to 8. In addition, the electroless nickel-phosphorus plating film before heat treatment was also subjected to XRD analysis in the same manner. The results are shown in Figures 9 to 12.

[0104] Fig. 5 is a diagram showing the results of XRD analysis performed after an electroless nickel-phosphorus plating film was formed and heat-treated using the electroless nickel-phosphorus plating bath of Example 1. From the results of Fig. 5, it was confirmed that in the electroless nickel-phosphorus plating film formed using the electroless nickel-phosphorus plating bath of Example 1 and heat-treated, the measured intensity of Ni(200) (2θ(deg) is around 51) is dominant over the measured intensity of Ni(111) (2θ(deg) is around 45), and the measured peak intensity ratio Ni(111) / Ni(200) is less than 1.0.

[0105] 6, 7, and 8 are diagrams showing the results of XRD analysis performed on electroless nickel-phosphorus plating films formed using the electroless nickel-phosphorus plating baths of Comparative Examples 1, 2, and 3, respectively, and then heat-treated. From the results of Fig. 6 to Fig. 8, it was confirmed that in the electroless nickel-phosphorus plating films formed using the electroless nickel-phosphorus plating baths of Comparative Examples 1 to 3 and then heat-treated, the measured intensity of Ni(200) was not dominant over the measured intensity of Ni(111), and the measured peak intensity Ni(111) / Ni(200) was 1.0 or more.

[0106] Fig. 9 is a diagram showing the results of XRD analysis performed before heat treatment on an electroless nickel-phosphorus plating film formed using the electroless nickel-phosphorus plating bath of Example 1. From the results of Fig. 9, the electroless nickel-phosphorus plating film before heat treatment formed using the electroless nickel-phosphorus plating bath of Example 1 has substantially the same measurement peak in the XRD analysis result as the electroless nickel-phosphorus plating film after heat treatment, and the structural change of the electroless nickel-phosphorus plating film before and after heat treatment is suppressed, so it is considered that the electroless nickel-phosphorus plating film of Example 1 has a suppressed increase in hardness after heat treatment, and cracking of the electroless nickel-phosphorus plating film after heat treatment is suppressed, thereby improving the crack resistance.

[0107] 10, 11, and 12 are diagrams showing the results of XRD analysis of electroless nickel-phosphorus plating films formed using the electroless nickel-phosphorus plating baths of Comparative Example 1, Comparative Example 2, and Comparative Example 3, respectively, before heat treatment. From the results of Figs. 10 to 12, it was found that the electroless nickel-phosphorus plating films formed using the electroless nickel-phosphorus plating baths of Comparative Example 1 to Comparative Example 3 before heat treatment had different measurement peak intensities in the XRD analysis results from the electroless nickel-phosphorus plating films after heat treatment. That is, the measurement peak intensity of Ni(111) after heat treatment was stronger than the measurement peak intensity of Ni(111) before heat treatment, and it was found that the structure of the electroless nickel-phosphorus plating film before and after heat treatment had changed. From this, it is considered that the hardness of the electroless nickel-phosphorus plating films of Comparative Examples 1 to 3 increased after heat treatment, making them more susceptible to cracking, and that the crack resistance was reduced.

Claims

1. (1) a water-soluble nickel compound, (2) a reducing agent, and (3) containing at least one selected from the group consisting of phosphorous acid and phosphites; The content of the reducing agent is 8 g / L or less, The content of at least one selected from the group consisting of phosphorous acid and phosphites is 30 g / L or more. Electroless nickel-phosphorus plating bath.

2. 2. The electroless nickel-phosphorus plating bath according to claim 1, wherein the reducing agent is at least one selected from the group consisting of hypophosphorous acid and hypophosphites.

3. 3. The electroless nickel-phosphorus plating bath according to claim 1, further comprising at least one selected from the group consisting of glutamic acid and glutamate salts.

4. The electroless nickel-phosphorus plating bath according to any one of claims 1 to 3, further comprising at least one selected from the group consisting of glycine and gluconate.

5. An electroless nickel-phosphorus plating bath as described in any of claims 1 to 4, wherein the content of the water-soluble nickel compound is 0.5 g / L or more as nickel metal.

6. 6. The electroless nickel-phosphorus plating bath according to claim 1, which is substantially free of sulfur compounds.

7. 1. An electroless nickel-phosphorus plating method comprising the steps of contacting an object to be plated with an electroless nickel-phosphorus plating bath to form an electroless nickel-phosphorus plating film, The electroless nickel-phosphorus plating bath comprises (1) a water-soluble nickel compound, (2) a reducing agent, and (3) containing at least one selected from the group consisting of phosphorous acid and phosphites; The content of the reducing agent is 13 g / L or less, The content of at least one selected from the group consisting of phosphorous acid and phosphites is 30 g / L or more. Electroless nickel-phosphorus plating method.

8. 8. The electroless nickel-phosphorus plating method according to claim 7, wherein the electroless nickel-phosphorus plating film has a measured peak intensity ratio Ni(111) / Ni(200) of Ni(111) to Ni(200) of less than 1.0 in an analysis by X-ray diffraction method after heat treatment.

9. 9. The electroless nickel-phosphorus plating method according to claim 7, wherein the Vickers hardness of the electroless nickel-phosphorus plating film after the heat treatment is 800 HV or less.

10. The electroless nickel-phosphorus plating film has a peak intensity ratio Ni(111) / Ni(200) of Ni(111) to Ni(200) of less than 1.0 when analyzed by X-ray diffraction after heat treatment.

11. The electroless nickel-phosphorus plating film according to claim 10, having a Vickers hardness of 800 HV or less after heat treatment at a temperature of 400° C. for 30 minutes.

Citation Information

Patent Citations

  • Anticorrosive wearable electrodeposit clad layer of Ni-W-P ternary alloy and manufacturing technique and electroplate liquid thereof

    CN101445946A

  • Process for treating chemical nickel-plating ageing solution

    CN105149610A

  • Oxidation of hypophosphite ion

    JP1994263414A

  • Electroless nickel-phosphorus plating solution

    JP1996176837A

  • Nickel-photsphorus thin film and electroless nickel-phosphorus plating liquid

    JP1997228061A

Cited By

  • Electroless nickel plating deposit, electroless nickel plating bath and method for producing an electroless nickel plating deposit

    DE102026107208A1

  • Electroless nickel plating film, electroless nickel plating bath, and method for manufacturing electroless nickel plating film

    JP2026160911A

  • Electroless nickel plating film, electroless nickel plating bath, and method for producing electroless nickel plating film

    JP7733848B1