Biomimetic nerve graft and method for preparing same

A chitosan-based biomimetic nerve graft with a helical structure and nanofiber coating addresses the balance of mechanical support and biocompatibility, facilitating nerve regeneration with reduced immune reaction.

JP7560189B2Active Publication Date: 2024-10-02NANTONG UNIV
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023551258
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-10-18
Filing Date
2022-11-10
Publication Date
2024-10-02
Estimated Expiration
2042-11-10

AI Technical Summary

Technical Problem

Current methods for constructing biomimetic nerve grafts face challenges in achieving a balance between microenvironmental stability and functional reconstruction, with existing materials lacking sufficient mechanical performance, biocompatibility, and causing immune reactions.

Method used

A biomimetic nerve graft composed of a helical scaffold coated with a nanofiber membrane and filled with guide fibers and human-derived bone marrow stromal extracellular matrix (hBMSC-ECM), all made from chitosan, is produced using cast molding and electrospinning techniques, ensuring mechanical support and biocompatibility while guiding neural growth.

Benefits of technology

The graft provides sufficient mechanical backup, nutrient transport, and directional alignment for nerve regeneration, with chitosan's biodegradability minimizing immune response and maintaining a favorable microenvironment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007560189000001
    Figure 0007560189000001
  • Figure 0007560189000002
    Figure 0007560189000002
  • Figure 0007560189000003
    Figure 0007560189000003
Patent Text Reader

Abstract

The present invention aims to provide a biomimetic nerve graft and a method for its preparation. [Solution] The biomimetic nerve graft includes a helical scaffold, a nanofiber membrane, a guide fiber and hBMSC-ECM, the nanofiber membrane covers the surface of the helical scaffold, the guide fiber and hBMSC-ECM are provided in the lumen of the helical scaffold, and the raw materials of the helical scaffold, the nanofiber membrane and the guide fiber are all chitosan. The preparation method includes preparing the helical scaffold by a cast molding method, coating the surface of the helical scaffold with a nanofiber membrane by an electrospinning method, preparing the guide fiber by a template method, and filling the guide fiber and hBMSC-ECM inside the helical tube whose surface is coated with the nanofiber membrane. The method provided by the present invention is simple, low-cost, ensures sufficient mechanical backup, good adaptability and inductivity, provides sufficient space for nutrient transport in nerve regeneration, provides microenvironmental elements for nerve regeneration, and provides a biomimetic nerve graft with good biocompatibility and low immunogenicity.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the field of biomaterials technology, in particular to a biomimetic nerve graft and a method for its preparation. [Background technology]

[0002] Peripheral nerve deficiency is a common clinical disease with poor prognosis and high mortality rate, which significantly affects the quality of life of patients. Although autologous nerve grafting is currently still considered the "gold standard" for repairing peripheral nerve defects, the clinical use of autologous nerve grafting is limited by problems such as a finite donor nerve source, functional loss of nerves at the donor site, size mismatch between donor and recipient nerves, and functional mispairing of nerve bundles.

[0003] Tissue engineering scaffold materials have the advantages of adjustable structure size, abundant material sources, and good processability, providing a new treatment for the recovery of injured nerves. Advances in micro- and nano-fabrication technologies, such as electrospinning, microetching, 3D printing, and phase separation, have enabled the construction of biomimetic tissue-engineered nerve grafts with porous, ordered, multi-channel, multi-layered, or multi-branched structures. In addition, a large amount of research work in the construction process of nerve grafts over the past 20 years has shown that nerve tissue engineering scaffolds with directional microstructures can induce directional alignment and growth of nerve cells (Non-Patent Document 1). Although researchers have made some progress in the construction of biomimetic tissue-engineered nerve grafts in recent years, there are still some challenges in the reconstruction of the microenvironment. There is still no standard reconstruction method that can achieve a perfect balance between stability and functional reconstruction in the microenvironment of biomimetic nerve grafts.

[0004] Natural biomaterials have the advantages of good biocompatibility, easy absorption, and the ability to promote cell adhesion and proliferation, and are widely used in the preparation of grafts for nerve regeneration. However, natural biomaterials themselves have poor mechanical properties and are prone to rupture and collapse, which significantly affect the stability of the microenvironment in nerve regeneration. Good mechanical performance is a prerequisite for maintaining the stability of the microenvironment, and in order to provide sufficient mechanical backup for the reconstruction of the microenvironment in nerve regeneration, the mechanical performance of nerve grafts can be improved by adding crosslinking agents or synthetic polymers with excellent mechanical performance. However, crosslinking agents, especially chemical crosslinking agents, are highly toxic and difficult to remove, and the biocompatibility of synthetic polymers such as polycaprolactone (PCL) and polylactic acid (PLA) is far inferior to that of natural materials, and neither of them is suitable for the reconstruction of the microenvironment or the recovery of nerve function by biomimetics. How to prepare nerve grafts with excellent mechanical performance and excellent biocompatibility is an issue that needs to be resolved in the construction process of biomimetic nerve grafts. [Prior art documents] [Non-patent literature]

[0005] [Non-Patent Document 1] Rao Feng. Aligned chitosan nanofiber hydrogel grafted with peptides mimicking bioactive brain-derived neurotrophic factor and vascular endothelial growth factor repair long-distance sciatic nerve defects in rats.Theranostics,2020, 10(4):1590-1603 Summary of the Invention [Problem to be solved by the invention]

[0006] The present invention aims to provide a biomimetic nerve graft and its preparation method which overcomes the shortcomings in the prior art, and the method is simple, low cost, ensures sufficient mechanical backup, provides sufficient space for nutrient transport in nerve regeneration, and obtains a biomimetic nerve graft with good biocompatibility and low immunogenicity. [Means for solving the problem]

[0007] The technical solutions provided by the present invention are as follows:

[0008] In a first embodiment, a biomimetic nerve graft is provided, which includes a helical scaffold, a nanofibrous membrane, a guide fiber, and human-derived bone marrow stromal extracellular matrix (hBMSC-ECM), in which the nanofibrous membrane covers the surface of the helical scaffold, the guide fiber and the hBMSC-ECM are disposed within the lumen of the helical scaffold, and the raw materials of the helical scaffold, the nanofibrous membrane, and the guide fiber are all chitosan.

[0009] Furthermore, the spiral scaffold has an inner diameter of 1-6 mm, a length of 1-6 cm, and a pitch of 0.5-5 mm.

[0010] Furthermore, the guide fibers are 1 to 3 cm long and 3 to 28 in number.

[0011] In a second aspect, there is provided a method for preparing a biomimetic nerve graft according to the first aspect, comprising: A step of producing a spiral scaffold using chitosan as a raw material by a cast molding method; A step of using chitosan as a raw material and coating the surface of a spiral scaffold with a single layer of nanofiber membrane by electrospinning to obtain a spiral tube whose surface is coated with the nanofiber membrane; A step of preparing a guide fiber using a template method with chitosan as a raw material; and filling the inside of the spiral tube, the surface of which is coated with a nanofiber membrane, with a guide fiber and hBMSC-ECM to obtain a biomimetic nerve graft.

[0012] Furthermore, the process for producing the spiral scaffold includes: Preparing a chitosan solution having a concentration of 4 wt% to 7 wt%; injecting a chitosan solution into a threaded core mold; The core mold containing the chitosan solution is placed in a 5-20% NaOH solution for hardening and shaping, and then washed with water, dried, and demolded to obtain a semi-finished spiral scaffold. The spiral scaffold semi-finished product is immersed in an acetic anhydride solution containing 5 wt% methanol for 6 hours to acetylate it, and then fixed with a 5-20% NaOH solution at room temperature for 12 hours, washed and dried to obtain a spiral scaffold.

[0013] Furthermore, the process for producing a spiral tube whose surface is coated with a nanofiber membrane is as follows: A blend solution of chitosan and polyethylene oxide having a total concentration of 3 wt% to 5 wt% is prepared, and the mass ratio of chitosan to polyethylene oxide is 100:5 to 20; Putting the chitosan and polyethylene oxide blend solution into an electrospinning device, placing the spiral scaffold on a tubular collector, and performing electrospinning to coat a single layer of nanofiber membrane on the surface of the spiral scaffold; The spiral scaffold coated with the nanofiber membrane is placed in a 5-20% NaOH solution for hardening and stabilizing, and then washed with water to remove the polyethylene oxide, thereby obtaining a spiral tube whose surface is coated with the nanofiber membrane.

[0014] Furthermore, the set parameters for electrospinning were: voltage 5–35 kV, flow rate 0.1–2 mL / h, collector distance 5–35 cm, and collector rotation speed 5–150 r. pm This includes being.

[0015] Furthermore, the manufacturing process of the guide fiber includes: preparing a chitosan solution with a concentration of 4 wt% to 7 wt%; injecting the chitosan solution into a mold provided with grooves; placing the mold with the chitosan solution in a 5% to 20% NaOH solution for hardening and shaping, then washing with water, drying, and demolding to obtain the guide fiber.

[0016] Furthermore, the grooves of the mold include communicating inner grooves and outer grooves. The cross-sectional shapes of the communicating inner grooves and outer grooves are in the shape of an inverted Chinese character 'pin'. The width of the outer groove is 100 to 500 μm, the height of the outer groove is 20 to 50 μm, the width of the inner groove is the same as the height of the outer groove, the height of the inner groove is 25 to 240 μm, the width of the outer groove is the sum of twice the height of the inner groove and the width of the inner groove, the lengths of the inner groove and the outer groove are the same, both being 1 to 3 cm.

[0017] Furthermore, the manufacturing process of hBMSC-ECM includes: coating a Petri dish with a mesenchymal stem cell (MSC) adhesion reagent diluted 100-fold with DPBS solution; seeding human bone marrow mesenchymal cells (hBMSC) after resuscitation onto the coated Petri dish, adding complete medium, culturing in an incubator at 37°C and 5% CO2, and changing the medium once every two days; when the cell saturation density reaches 80%, changing to a complete medium containing ascorbic acid (50 μg / mL), performing liquid exchange while shielding from light once every two days, removing the culture solution after 10 days, washing with DPBS three or more times, then performing hypotonic treatment with ultrapure water at 37°C for 10 minutes, removing the ultrapure water, adding cell lysate and reacting for 5 minutes, washing with DPBS, reacting with deoxyribonuclease (0.1 mg / mL) at 37°C for 2 hours, and finally washing with DPBS and storing at 4°C.

Advantages of the Invention

[0018] Compared with the prior art, the present invention has the following beneficial effects.

[0019] (1) The biomimetic nerve graft provided by the present invention comprises a spiral scaffold, a nanofiber membrane, a guide fiber, and hBMSC-ECM, and the nanofiber membrane covers the surface of the spiral scaffold, ensuring that the biomimetic nerve graft has sufficient mechanical backup and good adaptability, and providing sufficient space for nutrient transport in nerve regeneration. The guide fiber and hBMSC-ECM are provided in the spiral scaffold lumen and play a good guiding role, which is favorable for the directional alignment and growth of nerve cells, and provides microenvironmental elements in nerve regeneration, which is favorable for the regeneration of damaged nerves.

[0020] (2) The helical scaffold, nanofiber membrane, and guide fiber of the biomimetic nerve graft provided by the present invention are all made of chitosan, a natural biodegradable material with the advantages of good biocompatibility and low immunogenicity. The biomimetic nerve graft is naturally biodegraded during the nerve repair process, and the decomposition products are completely absorbed by the human body, avoiding immune system reactions.

[0021] (3) The preparation method of the biomimetic nerve graft provided by the present invention combines cast molding and electrospinning technologies, in which a spiral scaffold is fabricated using a cast molding method, and the surface of the spiral scaffold is coated with a single layer of nanofiber membrane using an electrospinning method. This enables the biomimetic nerve graft to simultaneously realize mechanical backup and nutrient transport for nerve regeneration, and further reduces the total mass of the biomimetic nerve graft, greatly reducing immune rejection.

[0022] (4) The preparation method of biomimetic nerve grafts provided by the present invention involves techniques such as cast molding, template method and electrospinning, all of which are simple and easy to implement, low cost, and the production process is safe and controllable. [Brief description of the drawings]

[0023] [Figure 1] 1 is a scanning electron microscope (SEM) image of the nanofiber membrane in Example 1. [Diagram 2] 1 is an SEM image of a spiral tube whose surface is coated with a nanofiber membrane in Example 1. [Diagram 3] FIG. 2 is a schematic diagram of a cross-sectional view of a mold groove for producing a guide fiber in an embodiment. [Figure 4] 1 is a SEM image of the guide fiber in Example 2. [Diagram 5] 1 shows the DNA content of hBMSCs-ECM before and after decellularization in Example 2. [Figure 6] 1 shows HE staining images of the helical scaffold biodegraded for 6 weeks after acetylation in Example 2. [Figure 7] Immunofluorescence images of transverse fragments at the distal end of regenerated nerves and axonal density at the distal end of regenerated nerves taken 8 weeks after repairing a 10 mm gap in a rat sciatic nerve using the nerve graft in Example 2 (TEN: biomimetic nerve group; AUTO: autologous nerve group; SHAM: sham-operated group; the same below). [Figure 8] 1 shows transmission electron microscope images (scale: left 50 μm, right 0.2 μm) of regenerated nerve cross sections of three animal groups taken 12 weeks after the surgery in Example 2, and histograms of the number of myelin layers and myelin thickness in the three groups. [Figure 9] FIG. 1 shows compound muscle action potential, conduction velocity, proximal amplitude and distal amplitude maps obtained 12 weeks after surgery in Example 2. [Figure 10] FIG. 13 is a CatWalk gait analysis diagram 12 weeks after surgery in Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0024] The present invention will be further described below with reference to the accompanying drawings. The following examples are merely for the purpose of more clearly illustrating the technical solution of the present invention, and are not intended to limit the scope of the present invention.

[0025] Example 1 (1) Chitosan was dissolved in a 2% acetic acid solution and stirred for 30 minutes to completely dissolve it, obtaining a chitosan solution with a concentration of 4 wt%. The chitosan solution was poured into a core mold with a screw thread, which had a length of 1 cm, a diameter of 2 mm, a screw thread pitch of 1 mm, and a line width of 0.5 mm. The core mold with the chitosan solution was placed in a 5% NaOH solution to harden and mold, and after molding, it was washed with water, dried, and demolded to obtain a semi-finished spiral scaffold. The semi-finished spiral scaffold was acetylated by immersing it in an acetic anhydride solution containing 5 wt% methanol for 6 hours, and then fixed using a 5% NaOH solution at room temperature for 12 hours, washed, and dried to obtain a spiral scaffold.

[0026] (2) An appropriate amount of polyethylene oxide was dissolved in a 50% acetic acid solution, and chitosan powder was added to prepare an electrospinning solution. The final total concentration of chitosan and polyethylene oxide was 3 wt%, and the mass ratio of chitosan to polyethylene oxide was 100:20. The spiral scaffold was placed on a rotatable tubular collector, and the electrospinning solution was placed in the syringe of the electrospinning device, and the voltage was 5 kV, the flow rate was 0.1 mL / h, the collector distance was 5 cm, and the collector rotation speed was 5 r pm The spiral scaffold was electrospinned at a temperature of 100° C. to coat a single layer of nanofiber membrane (as shown in FIG. 1) on the surface thereof, thereby obtaining a spiral tube (as shown in FIG. 2) coated with a nanofiber membrane on its surface.

[0027] (3) The chitosan solution from step (1) was poured into a mold with grooves. The grooves included an inner groove and an outer groove that communicated with each other, and the cross-sectional shape was as shown in Figure 3. The groove length was 1 cm, the width a of the outer groove was 100 μm, the height c of the outer groove was 20 μm, the inner groove was located at the center of the outer groove, the width of the inner groove was c, the height b of the inner groove was 40 μm, and the width of the outer groove was twice the height of the inner groove and the sum of the width of the inner groove. The mold with the chitosan solution was placed in a 10% NaOH solution and hardened and molded, washed with water after molding, and demolded after drying to obtain a guide fiber.

[0028] (4) The MSC colonization reagent diluted 100-fold with DPBS solution was coated on a Petri dish, and the resuscitated hBMSCs were inoculated onto the coated Petri dish and incubated in a complete medium (NutriStem® MSC XF basal medium: NutriStem® MSC The cells were cultured in a 37℃, 5% CO2 incubator with a medium change every two days. When the cell saturation density reached about 80%, the medium was changed to a complete medium containing ascorbic acid (50μg / mL). The medium was changed every two days in the dark. After 10 days, the culture medium was removed, washed with DPBS three times or more, and then hypotonic treatment was performed with ultrapure water at 37℃ for 10 minutes. The ultrapure water was then removed, and a cell lysis solution (3% TritonX-100, 2% sodium dodecyl sulfate) was added and reacted for 5 minutes. The cells were washed with DPBS, and after washing, the cells were reacted with deoxyribonuclease (0.1mg / mL) at 37℃ for 2 hours. Finally, the cells were washed with DPBS to decellularize the cells and obtain hBMSC-ECM.

[0029] (5) A biomimetic nerve graft containing guide fibers within the wall of a spiral scaffold tube was obtained by filling the inside of a spiral tube with 28 guide fibers and hBMSC-ECM, whose surface was coated with a nanofiber membrane.

[0030] Example 2 (1) Chitosan was dissolved in a 2% acetic acid solution and stirred for 2 hours to completely dissolve it, obtaining a chitosan solution with a concentration of 6 wt%. The chitosan solution was poured into a core mold with a screw thread, which had a length of 4 cm, a diameter of 2 mm, a screw thread pitch of 1 mm, and a line width of 0.5 mm. The core mold with the chitosan solution was placed in a 5% NaOH solution to harden and mold, and after molding, it was washed with water, dried, and demolded to obtain a semi-finished spiral scaffold. The semi-finished spiral scaffold was acetylated by immersing it in an acetic anhydride solution containing 5 wt% methanol for 6 hours, and then fixed using a 10% NaOH solution at room temperature for 12 hours, washed, and dried to obtain a spiral scaffold.

[0031] (2) An appropriate amount of polyethylene oxide was dissolved in a 50% acetic acid solution, and chitosan powder was added to prepare an electrospinning solution. The final total concentration of chitosan and polyethylene oxide was 4 wt%, and the mass ratio of chitosan to polyethylene oxide was 100:20. The spiral scaffold was placed on a rotatable tubular collector, and the electrospinning solution was placed in the syringe of the electrospinning device, and the electrospinning was performed under the following conditions: voltage 20 kV, flow rate 0.1 mL / h, collector distance 15 cm, and collector rotation speed 100 r pm The spiral scaffold was coated with a single layer of nanofiber membrane by electrospinning, to obtain a spiral tube coated with a nanofiber membrane on its surface.

[0032] (3) The chitosan solution from step (1) was poured into a mold with a groove. The shape of the groove was the same as in Example 1. The length of the groove was 3 cm, a was 250 μm, b was 100 μm, and c was 50 μm. The mold with the chitosan solution was placed in a 10% NaOH solution to harden and mold, washed with water after molding, and demolded after drying to obtain a guide fiber (as shown in FIG. 4).

[0033] (4) The MSC colonization reagent diluted 100-fold with DPBS solution was coated on a Petri dish, and the resuscitated hBMSCs were inoculated onto the coated Petri dish and incubated in a complete medium (NutriStem® MSC XF basal medium: NutriStem® MSC The cells were cultured in a 37℃, 5% CO2 incubator with a medium change every two days. When the cell saturation density reached about 80%, the medium was changed to a complete medium containing ascorbic acid (50μg / mL). The medium was changed every two days in the dark. After 10 days, the culture medium was removed, washed with DPBS three times or more, and then hypotonic treatment was performed with ultrapure water at 37℃ for 10 minutes. The ultrapure water was then removed, and a cell lysis solution (3% TritonX-100, 2% sodium dodecyl sulfate) was added and reacted for 5 minutes. The cells were washed with DPBS, and after washing, the cells were reacted with deoxyribonuclease (0.1mg / mL) at 37℃ for 2 hours. Finally, the cells were washed with DPBS to decellularize the cells and obtain hBMSC-ECM.

[0034] (5) Five guide fibers and hBMSC-ECM were packed inside a spiral tube whose surface was coated with a nanofiber membrane to obtain a biomimetic nerve graft containing guide fibers within the spiral scaffold tube wall.

[0035] The hBMSC-ECM in the biomimetic nerve graft prepared in this example contained bioactive components such as fibronectin, laminin, and type I collagen, which have a promoting effect on nerve regeneration, and DNA was hardly detected in it (as shown in Figure 5). After the semi-finished spiral scaffold was acetylated, the acetylation degree increased from the original 4.73% to 74.77%, and it had good biodegradability (as shown in Figure 6). The diameter of the electrospun nanofiber membrane covering the outer layer was about 100 nm.

[0036] The biomimetic nerve graft prepared in this example was used to repair a 10 mm defect in the sciatic nerve of a rat. The results of immunofluorescence images (as shown in FIG. 7) and transmission electron microscope images (as shown in FIG. 8) of the regenerated nerve distal transverse fragment 8 weeks after surgery showed that the biomimetic nerve graft had good nerve regeneration function and its effect of promoting nerve regeneration was comparable to that of autologous nerve. The functional test 12 weeks after surgery (as shown in FIG. 9 and FIG. 10) showed that the biomimetic nerve had good repair effect on the damaged nerve, and its repair effect was similar to that of autologous nerve.

[0037] Example 3 (1) Chitosan was dissolved in a 2% acetic acid solution and stirred for 4 hours to completely dissolve it, obtaining a chitosan solution with a concentration of 7 wt%. The chitosan solution was poured into a core mold with a screw thread, which had a length of 6 cm, a diameter of 5 mm, a screw thread pitch of 10 cm, and a line width of 5 mm. The core mold with the chitosan solution was placed in a 20% NaOH solution to harden and mold, and after molding, it was washed with water, dried, and demolded to obtain a semi-finished spiral scaffold. The semi-finished spiral scaffold was acetylated by immersing it in an acetic anhydride solution containing 5 wt% methanol for 6 hours, and then fixed using a 20% NaOH solution at room temperature for 12 hours, washed, and dried to obtain a spiral scaffold.

[0038] (2) An appropriate amount of polyethylene oxide was dissolved in a 50% acetic acid solution, and chitosan powder was added to prepare an electrospinning solution. The final total concentration of chitosan and polyethylene oxide was 5 wt%, and the mass ratio of chitosan to polyethylene oxide was 100:5. The spiral scaffold was placed on a rotatable tubular collector, and the electrospinning solution was placed in the syringe of the electrospinning device. The voltage was 35 kV, the flow rate was 2 mL / h, the collector distance was 35 cm, and the collector rotation speed was 150 r pm The spiral scaffold was coated with a single layer of nanofiber membrane by electrospinning, to obtain a spiral tube coated with a nanofiber membrane on its surface.

[0039] (3) The chitosan solution from step (1) was poured into a mold with a groove. The shape of the groove was the same as in Example 1. The length of the groove was 1 cm, a was 500 μm, b was 225 μm, and c was 50 μm. The mold with the chitosan solution was placed in a 20% NaOH solution and hardened and molded. After molding, it was washed with water, dried, and then demolded to obtain a guide fiber.

[0040] (4) The MSC colonization reagent diluted 100-fold with DPBS solution was coated on a Petri dish, and the resuscitated hBMSCs were inoculated onto the coated Petri dish and incubated in a complete medium (NutriStem® MSC XF basal medium: NutriStem® MSC The cells were cultured in a 37℃, 5% CO2 incubator with a medium change every two days. When the cell saturation density reached about 80%, the medium was changed to a complete medium containing ascorbic acid (50μg / mL). The medium was changed every two days in the dark. After 10 days, the culture medium was removed, washed with DPBS three times or more, and then hypotonic treatment was performed with ultrapure water at 37℃ for 10 minutes. The ultrapure water was then removed, and a cell lysis solution (3% TritonX-100, 2% sodium dodecyl sulfate) was added and reacted for 5 minutes. The cells were washed with DPBS, and after washing, the cells were reacted with deoxyribonuclease (0.1mg / mL) at 37℃ for 2 hours. Finally, the cells were washed with DPBS to decellularize the cells and obtain hBMSC-ECM.

[0041] (5) Three guide fibers and hBMSC-ECM were packed inside a spiral tube whose surface was coated with a nanofiber membrane to obtain a biomimetic nerve graft containing guide fibers within the spiral scaffold tube wall.

[0042] The above is only a preferred embodiment of the present invention, and those skilled in the art may make some improvements and modifications without departing from the technical principles of the present invention, and such improvements and modifications should be considered as belonging to the protection scope of the present invention.

[0043] [Note] [Appendix 1] A biomimetic nerve graft comprising a spiral scaffold, a nanofibrous membrane, a guide fiber, and hBMSC-ECM, wherein the nanofibrous membrane covers the surface of the spiral scaffold, the guide fiber and the hBMSC-ECM are disposed within the lumen of the spiral scaffold, and the spiral scaffold, the nanofibrous membrane, and the guide fiber are all made from chitosan.

[0044] [Appendix 2] 2. The biomimetic nerve graft described in appendix 1, wherein the spiral scaffold has an inner diameter of 1-6 mm, a length of 1-6 cm, and a pitch of 0.5-5 mm.

[0045] [Appendix 3] The biomimetic nerve graft described in Appendix 1, characterized in that the guide fibers are 1 to 3 cm long and have a quantity of 3 to 28 fibers.

[0046] [Appendix 4] A method for preparing a biomimetic nerve graft according to any one of claims 1 to 3, comprising: A step of producing a spiral scaffold using chitosan as a raw material by a cast molding method; A step of using chitosan as a raw material and coating the surface of the spiral scaffold with a single layer of nanofiber membrane by electrospinning to obtain a spiral tube whose surface is coated with the nanofiber membrane; A step of preparing a guide fiber using a template method with chitosan as a raw material; A method for preparing a biomimetic nerve graft, comprising the steps of: filling the inside of a spiral tube, the surface of which is covered with a nanofiber membrane, with the guide fiber and hBMSC-ECM to obtain a biomimetic nerve graft.

[0047] [Appendix 5] The process for producing the spiral scaffold comprises: Preparing a chitosan solution having a concentration of 4 wt% to 7 wt%; injecting the chitosan solution into a threaded core mold; The core mold carrying the chitosan solution is placed in a 5 to 20% NaOH solution for hardening and shaping, and then washed with water, dried, and demolded to obtain a semi-finished spiral scaffold. 5. The method for preparing the biomimetic nerve graft according to claim 4, further comprising: immersing the semi-finished spiral scaffold in an acetic anhydride solution containing 5 wt% methanol for 6 hours to acetylate it, and then fixing it with a 5-20% NaOH solution at room temperature for 12 hours, washing and drying it to obtain the spiral scaffold.

[0048] [Appendix 6] The process for producing a spiral tube having a surface coated with a nanofiber membrane includes the steps of: A blend solution of chitosan and polyethylene oxide having a total concentration of 3 wt% to 5 wt% is prepared, and the mass ratio of chitosan to polyethylene oxide is 100:5 to 20; Putting the chitosan and polyethylene oxide blend solution into an electrospinning device, placing the spiral scaffold on a tubular collector, and performing electrospinning to coat a layer of the nanofiber membrane on the surface of the spiral scaffold; and placing the spiral scaffold covered with the nanofiber membrane in a 5-20% NaOH solution to harden and mold it, and then washing with water to remove polyethylene oxide, thereby obtaining a spiral tube whose surface is covered with a nanofiber membrane.

[0049] [Appendix 7] The electrospinning parameters were: voltage 5-35 kV, flow rate 0.1-2 mL / h, collector distance 5-35 cm, and collector rotation speed 5-150 r. pm A method for preparing a biomimetic nerve graft as described in Appendix 6, comprising:

[0050] [Appendix 8] The process for producing the guide fiber includes the steps of: Preparing a chitosan solution having a concentration of 4 wt% to 7 wt%; pouring the chitosan solution into a mould having a groove; After placing the mold impregnated with the chitosan solution into a 5 - 20% NaOH solution for curing and shaping, washing with water, drying, and demolding, the guide fiber is obtained, and the method for preparing the biomimetic nerve graft according to appended note 4 is characterized by including this step.

[0051] [Appended Note 9] The groove of the mold includes a communicating inner groove and an outer groove. The cross - sectional shapes of the communicating inner groove and the outer groove are in the shape of an inverted Chinese character "pin". The width of the outer groove is 100 - 500 μm, the height of the outer groove is 20 - 50 μm, the width of the inner groove is the same as the height of the outer groove, the height of the inner groove is 25 - 240 μm, the width of the outer groove is the sum of twice the height of the inner groove and the width of the inner groove, and the lengths of the inner groove and the outer groove are the same, both being 1 - 3 cm. The method for preparing the biomimetic nerve graft according to appended note 8 is characterized by this.

[0052] [Appended Note 10] The preparation process of the hBMSC - ECM is as follows: Coating a Petri dish with an MSC adhesion reagent diluted 100 - fold with DPBS solution; Inoculating the resuscitated hBMSC onto the coated Petri dish, adding a complete medium, culturing in an incubator at 37°C and 5% CO₂, and changing the medium once every two days; When the cell saturation density reaches 80%, changing to a complete medium containing ascorbic acid, performing liquid exchange under light shielding once every two days, removing the culture solution after 10 days, washing with DPBS three or more times, then performing hypotonic treatment with ultrapure water at 37°C for 10 minutes, removing the ultrapure water, adding a cell lysate and reacting for 5 minutes, washing with DPBS, reacting with deoxyribonuclease at 37°C for 2 hours, and finally washing with DPBS and storing at 4°C. The method for preparing the biomimetic nerve graft according to appended note 4 is characterized by including this.

Claims

1. A biomimetic nerve graft comprising a spiral scaffold, a nanofibrous membrane, a guide fiber, and a human-derived bone marrow stromal extracellular matrix, wherein the nanofibrous membrane covers the surface of the spiral scaffold, the guide fiber and the human-derived bone marrow stromal extracellular matrix are provided within the lumen of the spiral scaffold, and the spiral scaffold, the nanofibrous membrane, and the guide fiber are all made from chitosan.

2. The biomimetic nerve graft of claim 1, wherein the helical scaffold has an inner diameter of 1-6 mm, a length of 1-6 cm, and a pitch of 0.5-5 mm.

3. The biomimetic nerve graft of claim 1, wherein the guide fibers are 1-3 cm long and 3-28 in number.

4. A method for preparing a biomimetic nerve graft according to any one of claims 1 to 3, comprising: A step of producing a spiral scaffold using chitosan as a raw material by a cast molding method; A step of using chitosan as a raw material and coating the surface of the spiral scaffold with a single layer of nanofiber membrane by electrospinning to obtain a spiral tube whose surface is coated with the nanofiber membrane; A step of preparing a guide fiber using a template method with chitosan as a raw material; and filling the inside of the spiral tube, the surface of which is covered with a nanofiber membrane, with the guide fiber and human bone marrow stromal extracellular matrix to obtain a biomimetic nerve graft.

5. The process for producing the spiral scaffold comprises: Preparing a chitosan solution having a concentration of 4 wt % to 7 wt %; injecting the chitosan solution into a threaded core mold; The core mold carrying the chitosan solution is put into a 5-20% NaOH solution for hardening and shaping, and then washed with water, dried, and demolded to obtain a semi-finished spiral scaffold. The method for preparing the biomimetic nerve graft according to claim 4, further comprising: immersing the semi-finished spiral scaffold in an acetic anhydride solution containing 5 wt% methanol for 6 hours for acetylation, and then fixing the semi-finished spiral scaffold with a 5-20% NaOH solution for 12 hours at room temperature, washing and drying to obtain the spiral scaffold.

6. The process for producing a spiral tube having a surface coated with a nanofiber membrane includes the steps of: A blend solution of chitosan and polyethylene oxide having a total concentration of 3 wt% to 5 wt% is prepared, and the mass ratio of chitosan to polyethylene oxide is 100:5 to 20; Putting the chitosan and polyethylene oxide blend solution into an electrospinning device, placing the spiral scaffold on a tubular collector, and performing electrospinning to coat a layer of the nanofiber membrane on the surface of the spiral scaffold; The method for preparing a biomimetic nerve graft according to claim 4, further comprising: placing the spiral scaffold covered with the nanofiber membrane in a 5-20% NaOH solution for hardening and stabilizing, and then washing with water to remove polyethylene oxide, thereby obtaining a spiral tube whose surface is covered with a nanofiber membrane.

7. The method for preparing a biomimetic nerve graft according to claim 6, characterized in that the setting parameters of the electrospinning include: voltage 5-35 kV, flow rate 0.1-2 mL / h, collector distance 5-35 cm, and collector rotation speed 5-150 rpm.

8. The process for producing the guide fiber includes the steps of: Preparing a chitosan solution having a concentration of 4 wt % to 7 wt %; Injecting the chitosan solution into a mold provided with grooves; Placing the mold with the chitosan solution into a 5-20% NaOH solution for hardening and shaping, then washing with water, drying, and demolding to obtain the guide fiber, characterized by including the above steps, which is the method for preparing a biomimetic nerve graft according to claim 4.

9. The grooves of the mold include communicating inner grooves and outer grooves. The cross-sectional shapes of the communicating inner grooves and outer grooves are in the shape of an inverted Chinese character "pin". The width of the outer groove is 100-500 μm, the height of the outer groove is 20-50 μm, the width of the inner groove is the same as the height of the outer groove, the height of the inner groove is 25-240 μm, the width of the outer groove is the sum of twice the height of the inner groove and the width of the inner groove, and the lengths of the inner groove and the outer groove are the same, both being 1-3 cm. This is the method for preparing a biomimetic nerve graft according to claim 8.

10. The preparation process of the human-derived bone marrow stromal cell extracellular matrix is as follows: Coating a Petri dish with a mesenchymal stem cell adhesion reagent diluted 100 times with DPBS solution; Inoculating the human-derived bone marrow stromal cells after resuscitation onto the coated Petri dish, adding a complete medium, and culturing in an incubator at 37°C and 5% CO 2 Exchanging the medium once every two days; When the cell saturation density reaches 80%, changing to a complete medium containing ascorbic acid, performing liquid exchange under light shielding once every two days, removing the culture solution after 10 days, washing more than three times with DPBS, then performing hypotonic treatment at 37°C with ultrapure water for 10 minutes and then removing the ultrapure water, adding a cell lysate and reacting for 5 minutes, washing with DPBS, reacting with deoxyribonuclease at 37°C for 2 hours, and finally washing with DPBS and storing at 4°C. This is the method for preparing a biomimetic nerve graft according to claim 4.

Citation Information

Patent Citations

  • Artificial nerve implant with path for guiding growth

    CN101433475A

  • Flexible peripheral neurological deficit repairing duct and preparation method thereof

    CN109701075A

  • Chitosan medical nerve and productive method thereof

    CN1385217A

  • Tissue engineered peripheral nerve graft

    CN1580255A

  • Implantable nerve conduit having a polymer fiber spiral guidance channel

    US20140379009A1