Paper barrier laminate with resin layer and paper barrier container
A paper barrier laminate with cellulose nanofibers and resin layers addresses the limitations of existing packaging materials by providing high oxygen barrier properties and bending resistance, suitable for industrial use and recycling.
Patent Information
- Application Number
- JP2020035175
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-03-02
- Publication Date
- 2024-10-02
- Estimated Expiration
- 2040-03-02
AI Technical Summary
Existing packaging materials, particularly those containing aluminum foil or petroleum-based resins, face issues such as metal detection interference, microwave oven incompatibility, resource depletion, and difficulty in recycling, while paper-based materials lack sufficient gas barrier properties due to high permeability and brittleness when used alone or with thin film coatings.
A paper barrier laminate comprising a paper base material with a barrier layer containing cellulose nanofibers and resin layers on both sides, coated to a specific thickness and flexibility-enhancing water-soluble polymers, which maintains high oxygen barrier properties even after bending.
The laminate achieves high oxygen barrier properties suitable for industrial production, ensuring effective gas barrier performance and bending resistance, while being environmentally friendly and recyclable.
Smart Images

Figure 0007560258000003 
Figure 0007560258000004 
Figure 0007560258000005
Abstract
Description
[Technical field]
[0001] The present invention is suitable for packaging food, toiletry products, medicines, etc. , with a resin layer The present invention relates to a paper barrier laminate and a paper barrier container formed using the paper barrier laminate. [Background technology]
[0002] Many foods, toiletry products, medicines, etc. require packaging containers with oxygen barrier properties to prevent the contents from oxidizing and deteriorating due to oxygen in the air. In addition, when contents containing volatile chemicals such as fragrances and medicinal ingredients are stored in a packaging container, the material of the packaging container is required to have properties that suppress the permeation of volatile chemicals so that the contents do not deteriorate or change in quality due to the volatile chemicals permeating the packaging container and diffusing to the outside during transportation or storage. Another problem is odor transfer, whereby external odors permeate packaging containers and transfer to the contents during transportation or storage. From this perspective, packaging container materials are required to have gas barrier properties that prevent the permeation of oxygen, aromas, odors, etc.
[0003] Until now, plastic containers have been widely used as packaging containers. However, plastic is a finite resource, mostly derived from petroleum, and generates high combustion heat when disposed of. Problems such as environmental hormones have been pointed out. With the recent trend toward environmental conservation and the enforcement of the Container and Packaging Recycling Law, it has become necessary to switch from plastic materials to materials derived from renewable natural resources such as paper. Conventionally, gas barrier materials that suppress the permeation of gases such as oxygen and odors have been made of aluminum foil, resin films such as polyvinylidene chloride resins, or films coated with these resins, ceramic vapor deposition films, etc. Laminates in which such gas barrier materials are laminated on a substrate are used as packaging materials (see, for example, Patent Document 1).
[0004] The above-mentioned aluminum foil is widely used as a gas barrier material because of its excellent gas barrier properties. However, when the packaging material contains metal such as aluminum foil, there is a problem that metal detection cannot be performed in the inspection of the product (particularly the contents). In addition, there is a problem that a microwave oven cannot be used when heating the contents. Furthermore, when discarding a packaging container after use, it is desirable to separate and collect the materials for recycling, but it is impossible, especially in an ordinary household, to peel off and separate the aluminum foil from the packaging material that constitutes the packaging container, making it difficult to separate and collect the aluminum and reuse it. If packaging materials containing aluminum foil are incinerated, the incineration residue will be large, which may damage the incinerator.
[0005] On the other hand, gas barrier materials made of resin films or ceramic vapor deposition films can solve the problems of metal detection and microwave oven use mentioned above, but there are concerns about the depletion of petroleum-based resources, so there is a need to switch to renewable resources. Paper is an example of a material derived from renewable natural resources. Because paper has a porous structure and is highly gas permeable, it cannot be used alone as a gas barrier material. Therefore, the use of a laminate (paper barrier laminate) in which a barrier layer with gas barrier properties is laminated onto a paper base material is being considered as a packaging material. As a method for laminating a barrier layer on a paper substrate, for example, a method of laminating a film including a barrier layer onto a paper substrate has been considered. However, in this method, a barrier layer including synthetic resins derived from petroleum is laminated onto paper, which is a renewable natural resource-derived material, so the thickness of the resin layer is thicker than that of the paper substrate, making it impossible to move away from petroleum resources.
[0006] As a new gas barrier material, cellulose-based materials are attracting attention. Cellulose, which accounts for about half of the biomass materials produced on Earth, is biodegradable and has excellent physical properties such as gas barrier properties, strength, elastic modulus, dimensional stability, heat resistance, and crystallinity. Therefore, cellulose is expected to be applied to functional materials. Examples of cellulose-based materials include cellulose nanofibers obtained by dispersing cellulose produced by oxidation reaction using a 2,2,6,6-tetramethylpiperidine-1-oxy radical (hereinafter referred to as "TEMPO") catalyst, as described in Patent Document 2 and Patent Document 3, cellulose nanofibers obtained by introducing a carboxymethyl group into a glucose unit and then dispersing the cellulose, as described in Patent Document 4, and cellulose nanofibers obtained by mechanical fiberization after enzyme treatment and alkali treatment, as described in Patent Document 5. By coating and laminating these cellulose-based materials on a substrate, a gas barrier material capable of suppressing oxygen permeability can be obtained. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2004-299203 A [Patent Document 2] JP 2008-308802 A [Patent Document 3] JP 2008-1728 A [Patent Document 4] JP 2013-185122 A [Patent Document 5] Japanese Patent Application Publication No. 6-10288 Summary of the Invention [Problem to be solved by the invention]
[0008] A barrier layer containing cellulose nanofibers is formed by coating and film formation on a substrate. However, because cellulose nanofibers are hard and brittle, the barrier layer is easily cracked. Therefore, the barrier layer containing cellulose nanofibers cannot withstand the stress of bending and folding when processing and molding into packaging materials, etc., and cracks occur, making it impossible to maintain the barrier properties. In particular, when a thin barrier layer is used in consideration of profitability, the deterioration of the barrier properties due to processing and molding becomes significant. In light of the above circumstances, the present invention aims to provide a paper barrier laminate that has high oxygen barrier properties, even when the barrier layer is a thin film suitable for industrial production, and a paper barrier container formed using the paper barrier laminate. [Means for solving the problem]
[0009] One aspect of the present invention is a paper barrier laminate comprising a paper base material and a barrier layer containing cellulose nanofibers, the paper barrier laminate having resin layers on both sides thereof, and a coating amount of the barrier layer of 0.3 g / m 2 More than 3.0g / m 2 The paper barrier laminate is characterized in that the ratio (B / A) of oxygen permeability before (A) and after (B) of the paper barrier laminate having the resin layer is 3.0 or less, and is within the range described below. Bending treatment: In accordance with JIS K5600-5-1, the film is wrapped around a mandrel having a diameter of 8 mm for 2 seconds with the surface on which the barrier layer is formed facing outward, and then returned to its original state. Effect of the Invention
[0010]
[0023] According to the paper barrier laminate according to one aspect of the present invention, even a thin barrier layer suitable for industrial production can be provided with high oxygen barrier properties. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 is a cross-sectional view illustrating a schematic example of a configuration of a paper barrier laminate according to an embodiment of the present invention. [Diagram 2]FIG. 1 is a cross-sectional view illustrating a schematic configuration of another example of a paper barrier laminate according to an embodiment of the present invention. [Diagram 3] FIG. 1 is a perspective view illustrating a schematic example of a configuration of a paper barrier container according to an embodiment of the present invention. [Figure 4] FIG. 1 is a cross-sectional view showing a schematic configuration of a paper barrier laminate according to a first embodiment of the present invention. [Diagram 5] FIG. 1 is a cross-sectional view showing a schematic configuration of a paper barrier laminate according to a first embodiment of the present invention. [Figure 6] FIG. 11 is a cross-sectional view showing a schematic configuration of a paper barrier laminate according to a second embodiment of the present invention. [Figure 7] FIG. 11 is a cross-sectional view showing a schematic configuration of a paper barrier laminate according to a second embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] "Paper barrier laminate" The configuration of a paper barrier laminate according to an embodiment of the present invention will be described with reference to Figs. 1 and 2. Fig. 1 is a cross-sectional view that shows a schematic example of the configuration of a paper barrier laminate 100 of this embodiment. The paper barrier laminate 100 shown in Fig. 1 comprises a paper substrate 10 and a barrier layer 20 formed on the paper substrate 10. Fig. 2 is a cross-sectional view that shows a schematic example of another configuration of the paper barrier laminate 100 of this embodiment. Fig. 2 shows a barrier layer 20 that is made up of two layers: a layer 21 that contains cellulose nanofibers and a water-soluble polymer, and a layer 22 that contains only a water-soluble polymer. Note that "a layer that contains a water-soluble polymer as a main component" refers to "layer 22 that contains only a water-soluble polymer" in Fig. 2. Furthermore, the above-mentioned "main component" means that the water-soluble polymer is contained in an amount of 75 mass% or more.
[0013] The paper that is the material for the paper substrate 10 is not particularly limited and can be appropriately selected depending on the application of the paper barrier laminate 100. For example, examples include ordinary high-quality paper, various types of coated paper, backing paper, impregnated paper, cardboard, art paper, coated paper, kraft paper, coated cardboard, ivory paper, card paper, cup base paper, etc. Furthermore, the smoothness of the surface 10a of the paper base material 10 on which the barrier layer 20 is formed is preferably 5.0 μm or less. By making the smoothness of the surface 10a on which the barrier layer 20 is formed 5.0 μm or less, a smooth barrier layer 20 can be formed even with a small coating amount of the barrier layer 20 as described below. This results in high gas barrier properties.
[0014] There is no particular limitation on the method for controlling the smoothness of the paper base material 10 to 5.0 μm or less, and any known method can be used. For example, it may be controlled by the pulp fibers used and the calendering conditions in the papermaking process. The smoothness of the paper substrate 10 was measured in accordance with JIS P8151 "Paper and paperboard-Surface roughness and smoothness test method (air leak method)-Print-surf tester method" using a clamp pressure of 1000 kPa and a soft backing. Here, JIS P8151 specifies the method for measuring surface roughness using a Print-surf tester.
[0015] The barrier layer 20 is formed on one surface 10a of the paper base material 10. The barrier layer 20 may be formed on both surfaces of the paper base material 10 (the one surface 10a and the other surface 10b). The barrier layer 20 may contain cellulose nanofibers (CNF) and a water-soluble polymer and be configured to exhibit gas barrier properties as a layer, or may contain only cellulose nanofibers (CNF) without containing a water-soluble polymer and be configured to exhibit gas barrier properties as a layer. By containing a water-soluble polymer in addition to the cellulose nanofibers, the flexibility of the barrier layer 20 is improved and the bending resistance is increased.
[0016] The coating weight of the barrier layer 20 is 0.3 g / m 2 More than 3.0g / m 2 It is preferable that the range is 0.5 g / m 2 More than 2.8g / m 2 More preferably, it is within the range of 0.8 g / m 2 More than 2.5g / m 2It is particularly preferable that the coating weight of the barrier layer 20 is within the following range: 2 More than 3.0g / m 2 By ensuring that the content is within the following range, it is possible to exhibit gas barrier properties while maintaining good profitability.
[0017] The paper barrier laminate 100 of this embodiment is folded after a resin layer 30 (described later) is formed on both sides by extrusion lamination, and it is preferable that the ratio B / A of the oxygen permeability (A) before the folding process to the oxygen permeability (B) after the folding process is 3.0 or less. An oxygen permeability ratio B / A of 3.0 or less increases bending resistance. The above-mentioned extrusion lamination is performed on both sides of the paper barrier laminate 100 using low-density polyethylene (LDPE) as the resin material. The folding process conforms to JIS K5600-5-1, and involves wrapping the paper barrier laminate 100 around a mandrel with a diameter of 8 mm for 2 seconds with the side on which the barrier layer 20 is formed facing outwards, and then returning it to its original position to complete the process. The oxygen permeability is measured in an environment with a temperature of 30°C and a humidity of 40% RH.
[0018] In addition, the paper barrier laminate 100 of this embodiment has an oxygen permeability of 20 cc / m when the resin layer 30 is formed on both sides by extrusion lamination. 2 ·day or less is preferable, and 10cc / m 2 ·day or less. Oxygen permeability is preferably 20cc / m 2 ·day or less, preferably 10cc / m 2 The fact that the oxygen barrier properties are high is demonstrated by the fact that the oxygen barrier properties are less than 100%. The above-mentioned extrusion lamination is performed using low density polyethylene (LDPE) as the resin material on both sides of the paper barrier laminate 100. The oxygen permeability is measured in an environment with a temperature of 30°C and a humidity of 40% RH. In addition, in the paper barrier laminate 100 of this embodiment, the resin layer 30 may be formed only on the side of the barrier layer 20 opposite the paper substrate 10 by extrusion lamination, or the resin layer 30 may be formed only on the other side 10b of the paper substrate 10.
[0019] The aforementioned CNFs are fine cellulose fibers obtained by micronizing natural cellulose. Methods for measuring the average diameter of CNF include a method of observing the shape using an apparatus such as an atomic force microscope (AFM) or a scanning electron microscope (SEM) and measuring the fiber diameters of any number of samples and taking the average, and a method of measuring the diameter from the results of particle size measurements of a coating liquid containing cellulose fibers using an apparatus such as a particle size distribution meter. The average fiber diameter in this embodiment may be measured by either method. The average fiber diameter of the CNF used as the barrier material of the barrier layer 20 is preferably within a range of, for example, 2 nm to 1000 nm. In this case, the barrier layer 20 can be formed as a dense film with sufficiently small voids. In other words, the barrier layer 20 with excellent gas barrier properties can be formed.
[0020] Gas barrier properties are exhibited by the barrier layer 20 blocking the permeation of gas (air). For the gas barrier properties to be exhibited, it is important that the barrier layer 20 is dense enough to prevent the permeation of the molecules of the gas to be blocked, and that the multiple voids are not interconnected. CNF has high rigidity, and the fibers are firmly bound to each other due to the hydrogen bonding effect of the hydroxyl groups and carboxyl groups present in large numbers in the molecule, so that a dense film can be formed. In addition, CNF is thought to easily exhibit high gas barrier properties because it has high crystallinity and small molecular movement.
[0021] Anion-modified CNF can be preferably used as the CNF used in the barrier layer 20. CNF can be obtained by mechanically defibrating cellulose fibers. By performing anion modification before defibration, electrostatic repulsion is generated between the CNF fibers, so that the defibration can be performed with lower energy, and CNF can be obtained efficiently. In addition, anion modification can further reduce the fiber diameter of CNF, which is suitable for forming a dense film with excellent gas barrier properties. Examples of the anion-modified group of CNF include a carboxyl group, a carboxymethyl group, a phosphate ester group, etc. The carboxyl group and the carboxymethyl group are preferred in order to obtain high gas barrier properties.
[0022] The method for introducing a carboxyl group into a cellulose molecule can be appropriately selected from among known methods. For example, a method can be used in which a TEMPO (2,2,6,6-tetramethylpiperidine-1-oxy radical) catalyst is used, and oxidation is performed using an oxidizing agent such as sodium hypochlorite or a bromide such as sodium bromide while adjusting the pH. According to the above method, the hydroxyl group at the C6 position of the glucose unit on the surface of the cellulose microfibril is selectively carboxylated. In the TEMPO oxidized cellulose obtained by this method, electrostatic repulsion between fibers is increased, making it easier to disperse, so a dispersion of cellulose nanofibers can be obtained by performing a minor defibration treatment in water. TEMPO oxidized cellulose can be made into nanofibers while maintaining the high crystallinity of the raw cellulose, making it suitable as a barrier material.
[0023] The amount of carboxyl groups introduced into the cellulose molecules is preferably in the range of 0.1 mmol / g to 3.5 mmol / g, more preferably in the range of 1.0 mmol / g to 1.8 mmol / g, based on the mass of the cellulose. The amount of carboxyl groups can be measured by conductometric titration of cellulose. If the carboxyl group content is less than 0.1 mmol / g, dispersibility may decrease, making it difficult for the barrier layer 20 to fully exhibit gas barrier properties. If the carboxyl group content exceeds 3.5 mmol / g, the crystallinity of the cellulose may decrease, resulting in decreased oxygen barrier properties and water resistance under high humidity conditions. That is, when the amount of carboxy groups is within the range of 0.1 mmol / g to 3.5 mmol / g, the electrostatic repulsion effect of the carboxy groups increases dispersion stability, making it easier to uniformly form the barrier layer 20 on the paper substrate 10. As a result, the uniformly formed barrier layer is preferred because it is more likely to exhibit sufficient gas barrier properties and is also suitably prevented from decreasing in oxygen barrier properties and water resistance under high humidity conditions.
[0024] The method of introducing carboxymethyl groups into cellulose molecules can be appropriately selected from known methods. For example, a cellulose raw material is used as a starting material, and a mixed medium of 3 to 20 times by mass of a lower alcohol, specifically methanol, ethanol, N-propyl alcohol, isopropyl alcohol, N-butanol, isobutanol, tertiary butanol, etc., alone or a mixture of two or more of them and water is used as a solvent. The mixing ratio of the lower alcohol in the mixed medium is 60 to 95% by mass. A mercerizing agent is used in an amount of 0.5 to 20 times by mole of an alkali metal hydroxide, specifically sodium hydroxide or potassium hydroxide, per glucose residue of the starting material, and the starting material, solvent, and mercerizing agent are mixed to perform a mercerization treatment at a reaction temperature of 0 to 70°C, preferably 10 to 60°C, and for a reaction time of 15 minutes to 8 hours, preferably 30 minutes to 7 hours. Thereafter, monochloroacetic acid or sodium monochloroacetate (carboxymethylating agent) is added at 0.05 to 10.0 times the molar amount per glucose residue, and an etherification reaction is carried out at a reaction temperature of 30 to 90°C, preferably 40 to 80°C, for a reaction time of 30 minutes to 10 hours, preferably 1 hour to 4 hours, to obtain cellulose having a carboxymethyl group introduced therein.
[0025] The degree of substitution of the carboxymethyl group introduced into the cellulose molecule is preferably within the range of 0.1 to 0.5. With a degree of substitution within the range of 0.1 to 0.5, an appropriate fiber diameter is obtained, and the electrostatic repulsion effect of the carboxymethyl group increases dispersion stability, making it easier to uniformly form the barrier layer 20 on the paper substrate 10. As a result, the uniformly formed barrier layer is preferred because it is more likely to fully exhibit gas barrier properties and is also preferably prevented from decreasing in oxygen barrier properties and water resistance under high humidity conditions.
[0026] The water-soluble polymer is not particularly limited, but for example, polyvinyl alcohol, ethylene vinyl alcohol, carboxymethyl cellulose, etc. are preferable, and the degree of polymerization and the amount of functional groups are not limited. From the viewpoint of imparting flexibility, at least one of polyvinyl alcohol and carboxymethyl cellulose is particularly preferable. Furthermore, the addition of a water-soluble polymer can reduce the viscosity of the coating liquid used to form the barrier layer 20, thereby efficiently forming the barrier layer 20. From the viewpoint of maintaining high gas barrier properties, polyvinyl alcohol is particularly preferable.
[0027] The barrier layer 20 may have a different mass ratio of CNF to water-soluble polymer between the paper substrate 10 side and the opposite side. For example, the mass ratio of CNF may gradually increase from the paper substrate 10 side to the opposite side. Furthermore, as shown in Fig. 2, the barrier layer 20 may be formed by laminating two or more layers, and preferably includes a layer 22 containing a water-soluble polymer as a main component and a layer 21 containing CNF and a water-soluble polymer. The presence of the layer 22 containing a water-soluble polymer as a main component makes it easier to maintain the barrier properties even if a crack occurs in the layer 21 containing CNF and a water-soluble polymer. The layer 22 containing a water-soluble polymer as a main component may be a layer containing only a water-soluble polymer.
[0028] Conversely to the above configuration, the barrier layer 20 may have a gradually decreasing mass ratio of CNF from the paper substrate 10 side to the opposite side. Furthermore, the barrier layer 20 may have, from the paper substrate 10 side, a layer 21 containing CNF and a water-soluble polymer, and a layer 22 containing a water-soluble polymer as a main component, in this order. The mass ratio of CNF to water-soluble polymer in the barrier layer 20 is preferably in the range of 5 / 95 to 99 / 1, more preferably in the range of 5 / 95 to 99 / 1, and particularly preferably in the range of 10 / 90 to 90 / 10. Having the mass ratio in this range allows for high productivity, high oxygen barrier properties, and flex resistance.
[0029] The barrier layer 20 can be formed by coating the paper substrate 10 with a coating liquid containing the material for the barrier layer 20. The CNF and water-soluble polymers that are the materials for the barrier layer 20 can be dissolved or dispersed in a medium whose main component is water, and can be easily made into a coating liquid. Various known methods can be used to apply the coating liquid for forming the barrier layer. Specifically, a gravure coater, a dip coater, a reverse coater, a wire bar coater, a die coater, etc. can be used. By using a wet film-forming method, a coating film of the aqueous coating liquid can be formed uniformly on the surface of the paper substrate 10. Water is preferred as the medium, but a solvent such as alcohol can be added as appropriate to improve drying efficiency and coatability.
[0030] The paper barrier laminate 100 of this embodiment can be used as a material for various paper containers formed into desired shapes such as cups, bottles, boxes, etc. 3 shows, as an example of a paper container of this embodiment, a cup-shaped paper barrier container 200 formed from the paper barrier laminate 100. The paper barrier container 200 of this embodiment has a substantially circular bottom member 201 and a body member 202 that is joined to the bottom member 201 to form the side surfaces.
[0031] When producing the paper barrier container 200, first, a heat-sealable thermoplastic resin layer 30 is formed on both sides of the sheet-like paper barrier laminate 100, and then the bottom member 201 and body material 202 are punched out using a die. Next, the bottom member 201 and body material 202 are joined together and formed into a cup shape using a known cup forming machine. Furthermore, a separately produced lid member 203 is joined to the upper opening of the body material 202 in a peelable manner to seal the opening, completing the paper barrier container 200. As the bottom member 201 and body material 202 can be easily joined by heat sealing, the paper barrier container 200 can be easily formed.
[0032] The lid material 203 is not essential to the paper barrier container 200 of this embodiment, and may not be provided if not necessary. Furthermore, the lid material 203 does not necessarily have to be formed from the paper barrier laminate 100 of this embodiment, and may be formed in part or in whole using other barrier sheet materials. Similarly, in the paper barrier container 200 of this embodiment, as long as the paper barrier laminate 100 of this embodiment is used in at least a portion, the bottom member 201 and the body material 202 may be formed in part or in whole using other barrier sheet materials. Furthermore, when forming the paper barrier container 200, there is no particular limitation on the arrangement of the barrier layer 20. That is, the barrier layer 20 may be arranged on the inner surface side of the paper barrier container 200 relative to the paper substrate 10, or the barrier layer 20 may be arranged on the outer surface side of the paper substrate 10.
[0033] [Example] (First embodiment) The paper barrier laminate 100 and the paper barrier container 200 of this embodiment will be further described using examples and comparative examples. However, the technical scope of the present invention is not limited in any way by the specific contents of these examples. First, a procedure for preparing the water-based coating liquid for forming the barrier layer 20 will be described.
[0034] [Preparation of water-based coating solution 1-1] 30 g of softwood kraft pulp was immersed in 600 g of water and dispersed in a mixer. To the dispersed pulp slurry were added 0.3 g of TEMPO and 3 g of NaBr, which had been dissolved in advance in 200 g of water, and the mixture was further diluted with water to a total volume of 1400 mL. The temperature inside the system was kept at 20°C, and an aqueous solution of sodium hypochlorite was measured and added dropwise to give a concentration of 10 mmol per 1 g of cellulose. After the start of the dropwise addition of the sodium hypochlorite aqueous solution, the pH began to decrease, but the pH of the system was maintained at 10 by continually adding dropwise 0.5N sodium hydroxide aqueous solution. After 4 hours, when the amount of the 0.5N aqueous sodium hydroxide solution dropped reached 2.8 mmol / g, 30 g of ethanol was added to stop the reaction. 0.5N hydrochloric acid was added to the reaction system to lower the pH to 2. The oxidized pulp was filtered and repeatedly washed with 0.01N hydrochloric acid or water to obtain the oxidized pulp. The oxidized pulp was subjected to conductometric titration with 0.1N sodium hydroxide solution using an automatic titrator (DKK-TOA, AUT-701), and the calculated amount of carboxyl groups was 1.6 mmol / g. The obtained oxidized pulp was diluted with water and adjusted to pH 9 with 0.5N sodium hydroxide solution to obtain a 1% oxidized pulp suspension. This suspension was dispersed for 2 hours with a high-speed mixer to obtain aqueous coating solution 1-1 as a dispersion containing CNF as a barrier material.
[0035] [Preparation of water-based coating solution 1-2] To a mixer, 200 g (dry mass) of bleached, unbeaten conifer-derived kraft pulp (brightness 85%) and 111 g (dry mass) of sodium hydroxide were added, and water was added so that the pulp solids content became 20% (w / v). After stirring for 30 minutes at 30° C., 216 g (effective ingredient equivalent) of sodium monochloroacetate was added. After stirring for 30 minutes, the temperature was raised to 70° C. and stirring was continued for 1 hour. The reaction product was then removed, neutralized and washed to obtain a carboxymethylated pulp with a degree of carboxymethyl substitution per glucose unit of 0.25. The carboxymethylated pulp was then adjusted to 1% solids with water and stirred for approximately 60 minutes using a high-speed rotating mixer to obtain aqueous coating solution 1-2 as a dispersion containing CNF as a barrier material.
[0036] [Preparation of water-based coating solution 1-3] A 4% solids aqueous solution of commercially available polyvinyl alcohol (PVA) (molecular weight 100,000, saponification degree 98%) was prepared and used as aqueous coating solution 1-3. [Preparation of water-based coating solution 1-4] An aqueous solution of 4% solids content of commercially available carboxymethyl cellulose (CMC) (product name: F10LC, manufactured by Nippon Paper Industries Co., Ltd.) was prepared and used as aqueous coating solution 1-4. [Preparation of water-based coating solution 1-5] The above-mentioned aqueous coating liquid 1-1 was mixed with the aqueous coating liquid 1-3 so that the mass ratio of cellulose to PVA was 1: 1. The mixture was further stirred with a magnetic stirrer for 3 hours to obtain an aqueous coating liquid 1-5 as a PVA-added cellulose fine fiber dispersion.
[0037] [Preparation of water-based coating solution 1-6] The above-mentioned aqueous coating liquid 1-2 was mixed with the aqueous coating liquid 1-3 so that the mass ratio of cellulose to PVA was 1: 1. The mixture was further stirred with a magnetic stirrer for 3 hours to obtain an aqueous coating liquid 1-6 as a PVA-added cellulose fine fiber dispersion. [Preparation of water-based coating solution 1-7] The above-mentioned aqueous coating liquid 1-2 was mixed with the aqueous coating liquid 1-3 so that the mass ratio of cellulose to PVA was 25: 75. The mixture was further stirred with a magnetic stirrer for 3 hours to obtain an aqueous coating liquid 1-7 as a PVA-added cellulose fine fiber dispersion.
[0038] [Preparation of water-based coating solution 1-8] The above-mentioned aqueous coating liquid 1-2 was mixed with the aqueous coating liquid 1-4 so that the mass ratio of cellulose to CMC was 1: 1. The mixture was further stirred with a magnetic stirrer for 3 hours to obtain an aqueous coating liquid 1-8 as a CMC-added cellulose fine fiber dispersion. [Evaluation of water-based coating solutions 1-1 and 1-2] The aqueous coating solutions 1-1 and 1-2 containing CNF were diluted to a concentration of 0.01%, applied to mica, and the fiber morphology was observed by AFM. The average width of 10 random fibers was calculated and used as the average fiber diameter. The average fiber diameter of CNF in the aqueous coating solution 1-1 calculated by the above method was 4 nm. The average fiber diameter of CNF in the aqueous coating solution 1-2 was 6 nm.
[0039] Next, the manufacturing procedures for the paper barrier laminate 100 and the paper barrier container 200 in each example and comparative example will be described. [Example 1-1] Basis weight 260g / m 2 The uncoated cup base paper was used as the paper substrate 10. One surface 10a of the paper substrate 10 was coated with a bar coater to a dry coating amount of 1.6 g / m 2 The aqueous coating solution 1-3 was applied so that the thickness of the coated substrate was 0.6 g / m2, and the coated substrate was dried in an oven at 120°C for 5 minutes. 2 The aqueous coating liquid 1-6 was applied so as to obtain a paper barrier laminate 100, and the paper barrier laminate 100 was dried for 5 minutes in an oven at 120° C. As a result, a barrier layer 20 was formed on one surface 10a of the paper substrate 10.
[0040] [Bending process] Next, the barrier surface of the paper barrier laminate 100 was subjected to a corona treatment, and then an LDPE resin (Novatec LD LC520, manufactured by Japan Polyethylene Co., Ltd.) was supplied by extrusion lamination to form a resin layer 30. Furthermore, the other surface 10b of the paper substrate 10 was subjected to a corona treatment, and then the same LDPE resin was supplied onto the paper substrate 10 by extrusion lamination to form a resin layer 30 on the other surface 10b as well. The thickness of the resin layer 30 on the barrier layer 20 side was 30 μm, and the thickness of the resin layer 30 on the side opposite the barrier layer 20 was 20 μm. The corona treatment is a treatment carried out to increase the adhesion between layers. In this way, a paper barrier laminate 101 equipped with a resin layer 30, as shown in FIG. 4, was produced. The paper barrier laminate 101 of Example 1-1 that had been subjected to extrusion lamination was subjected to a folding process in accordance with JIS K5600-5-1. Specifically, in an environment of 25°C and 50% RH, the paper barrier laminate 101 was wrapped around a mandrel with a diameter of 8 mm for 2 seconds so that the surface on which the barrier layer 20 was formed was facing outward, and then returned to its original state. The folding direction was perpendicular to the paper-making direction of the paper.
[0041] [Oxygen permeability (isobaric method) (cc / m 2 ·day)] Using an oxygen permeability measuring device MOCON (OX-TRAN2 / 21, manufactured by Modern Controls), the oxygen permeability of the paper barrier laminate 101 before and after folding treatment was measured in an atmosphere of 30°C and 40% RH (relative humidity). The oxygen permeability before and after folding was as follows. Before bending (A): 3.8cc / m 2 ·day After bending (B): 4.1cc / m 2 ·day B / A: 1.1 [Profitability] The profitability was evaluated based on the coating amount of the barrier layer 20. The evaluation criteria were as follows. ○:2.7g / m 2 below △:2.7g / m 2 Super 3.0g / m 2 below ×:3.0g / m 2 super From the standpoint of profitability, "○" and "△" were deemed to be acceptable.
[0042] [Examples 1-2 to 1-18, Comparative Examples 1-1 to 1-2] The paper barrier laminates 101 of Examples 1-2 to 1-18 and Comparative Examples 1-1 to 1-2 were produced and their oxygen permeability was measured in the same manner as in Example 1-1, except that the aqueous coating liquid and dry coating amount were shown in Table 1. In addition, the profitability was also evaluated for the paper barrier laminates 101 of Examples 1-2 to 1-18 and Comparative Examples 1-1 to 1-2. In Examples 1-10 to 1-18, the paper barrier laminates 101 were produced in the same manner as in Examples 1-1 to 1-9, except that the resin layer 30 was not formed on the other surface 10b of the paper base material 10. Figure 5 shows the configuration of the paper barrier laminates 101 of Examples 1-10 to 1-19, which were subjected to extrusion lamination.
[0043] [Table 1]
[0044] As shown in Table 1, in Comparative Examples 1-1 and 1-2, which do not contain a water-soluble polymer in the barrier layer 20, the value of B / A, which is the ratio of oxygen transmission rates before and after the folding treatment, is 3.0 or more, and the barrier properties are significantly deteriorated by folding. In addition, the profitability of Comparative Example 1-2 is also low. On the other hand, in Examples 1-1 to 1-18 in which a water-soluble polymer was added to the barrier layer 20, the oxygen permeability ratio B / A before and after the folding treatment was all 3.0 or less, suppressing deterioration of the barrier layer 20 due to folding. Therefore, the paper barrier laminate 100 of this example (paper barrier laminate 101 including the resin layer 30) is a paper barrier laminate that is sufficiently suitable for processing such as cup molding, even though it has a thin barrier layer 20. Furthermore, the paper barrier laminates 101 of Examples 1-1 to 1-18 are good paper barrier laminates from the standpoint of profitability as well.
[0045] (Second Example) The paper barrier laminate 100 and the paper barrier container 200 of this embodiment will be further described using examples and comparative examples. However, the technical scope of the present invention is not limited in any way by the specific contents of these examples. First, a procedure for preparing the water-based coating liquid for forming the barrier layer 20 will be described.
[0046] [Preparation of water-based coating solution 2-1] 30 g of softwood kraft pulp was immersed in 600 g of water and dispersed in a mixer. To the dispersed pulp slurry were added 0.3 g of TEMPO and 3 g of NaBr, which had been dissolved in advance in 200 g of water, and the mixture was further diluted with water to a total volume of 1400 mL. The temperature inside the system was kept at 20°C, and an aqueous solution of sodium hypochlorite was measured and added dropwise to give a concentration of 10 mmol per 1 g of cellulose. After the start of the dropwise addition of the sodium hypochlorite aqueous solution, the pH began to decrease, but the pH of the system was maintained at 10 by continually adding dropwise 0.5N sodium hydroxide aqueous solution. After 4 hours, when the amount of the 0.5N aqueous sodium hydroxide solution dropped reached 2.8 mmol / g, 30 g of ethanol was added to stop the reaction. 0.5N hydrochloric acid was added to the reaction system to lower the pH to 2. The oxidized pulp was filtered and repeatedly washed with 0.01N hydrochloric acid or water to obtain the oxidized pulp. The oxidized pulp was subjected to conductometric titration with 0.1N sodium hydroxide solution using an automatic titrator (DKK-TOA, AUT-701), and the calculated amount of carboxyl groups was 1.6 mmol / g. The obtained oxidized pulp was diluted with water and adjusted to pH 9 with 0.5N sodium hydroxide solution to obtain a 1% oxidized pulp suspension. This suspension was dispersed for 2 hours with a high-speed mixer to obtain aqueous coating solution 2-1 as a dispersion containing CNF as a barrier material.
[0047] [Preparation of water-based coating solution 2-2] To a mixer, 200 g (dry mass) of bleached, unbeaten conifer-derived kraft pulp (brightness 85%) and 111 g (dry mass) of sodium hydroxide were added, and water was added so that the pulp solids content became 20% (w / v). After stirring for 30 minutes at 30° C., 216 g (effective ingredient equivalent) of sodium monochloroacetate was added. After stirring for 30 minutes, the temperature was raised to 70° C. and stirring was continued for 1 hour. The reaction product was then removed, neutralized and washed to obtain a carboxymethylated pulp with a degree of carboxymethyl substitution per glucose unit of 0.25. The carboxymethylated pulp was then adjusted to 1% solids with water, and this was stirred for approximately 60 minutes using a high-speed rotating mixer to obtain aqueous coating solution 2-2 as a dispersion containing CNF as a barrier material.
[0048] [Preparation of water-based coating solution 2-3] A 4% solids aqueous solution of commercially available polyvinyl alcohol (PVA) (molecular weight 100,000, saponification degree 98%) was prepared and used as aqueous coating solution 2-3. [Preparation of water-based coating solution 2-4] The above-mentioned aqueous coating liquid 2-1 was mixed with the aqueous coating liquid 2-3 so that the mass ratio of cellulose to PVA was 1: 1. The mixture was further stirred with a magnetic stirrer for 3 hours to obtain an aqueous coating liquid 2-4 as a PVA-added cellulose fine fiber dispersion. [Preparation of water-based coating solution 2-5] The above-mentioned aqueous coating liquid 2-2 was mixed with the aqueous coating liquid 2-3 so that the mass ratio of cellulose to PVA was 1: 1. The mixture was further stirred with a magnetic stirrer for 3 hours to obtain an aqueous coating liquid 2-5 as a PVA-added cellulose fine fiber dispersion.
[0049] [Evaluation of water-based coating solutions 2-1 and 2-2] The aqueous coating solutions 2-1 and 2-2 containing CNF were diluted to a concentration of 0.01%, applied to mica, and the fiber morphology was observed by AFM. The average width of 10 random fibers was calculated, and this was taken as the average fiber diameter. The average fiber diameter of CNF in the aqueous coating solution 2-1 calculated by the above method was 4 nm. The average fiber diameter of CNF in the aqueous coating solution 2-2 was 6 nm.
[0050] Next, the manufacturing procedures for the paper barrier laminate 100 and the paper barrier container 200 in each example and comparative example will be described. [Example 2-1] Basis weight 260g / m 2 The uncoated cup base paper was used as the paper substrate 10. The smoothness of the paper substrate 10 was 3.8 μm. One surface 10a of the paper substrate 10 was coated with a dry coating amount of 1.5 g / m2 using a bar coater. 2 The aqueous coating liquid 2-5 was applied so as to obtain a paper barrier laminate 100, and the paper barrier laminate 100 was dried for 5 minutes in an oven at 120° C. As a result, a barrier layer 20 was formed on one surface 10a of the paper substrate 10.
[0051] [Oxygen permeability (isobaric method) (cc / m 2 ·day)] Next, the barrier surface of the paper barrier laminate 100 was subjected to a corona treatment, and then an LDPE resin (Novatec LD LC520, manufactured by Japan Polyethylene Co., Ltd.) was supplied by extrusion lamination to form a resin layer 30. Furthermore, the other surface 10b of the paper substrate 10 was subjected to a corona treatment, and then the same LDPE resin was supplied onto the paper substrate 10 by extrusion lamination to form a resin layer 30 on the other surface 10b as well. The thickness of the resin layer 30 on the barrier layer 20 side was 30 μm, and the thickness of the resin layer 30 on the side opposite the barrier layer 20 was 20 μm. The corona treatment is a treatment carried out to increase the adhesion between layers. In this way, a paper barrier laminate 101 equipped with a resin layer 30, as shown in FIG. 6, was produced. The oxygen permeability of the paper barrier laminate 101 of Example 2-1, which had been subjected to extrusion lamination, was measured in an atmosphere of 30°C and 40% RH (relative humidity) using an oxygen permeability measuring device MOCON (OX-TRAN2 / 21, manufactured by Modern Controls). As a result, the oxygen permeability was 4.1 cc / m 2 ·day.
[0052] [Profitability] In the same manner as in the first example, the profitability was evaluated from the coating amount of the barrier layer 20. The evaluation criteria were as follows. ○:2.7g / m 2 below △:2.7g / m 2 Super 3.0g / m 2 below ×:3.0g / m 2 super From the standpoint of profitability, "○" and "△" were deemed to be acceptable.
[0053] [Example 2-2] A paper barrier laminate 100 was produced in the same manner as in Example 2-1, except that the water-based coating liquid 2-4 was used, and the oxygen permeability was measured. The oxygen permeability was 3.3 cc / m 2 ·day. [Example 2-3] The paper base material 10 has a basis weight of 260 g / m 2 A paper barrier laminate 100 was produced in the same manner as in Example 2-1, except that a paperboard for paper containers with a smoothness of 5.7 μm was used, and the oxygen permeability was measured. The oxygen permeability was 15.0 cc / m 2 ·day. [Example 2-4] A paper barrier laminate 101 was produced and its oxygen permeability was measured in the same manner as in Example 2-1, except that the resin layer 30 was not formed on the other surface 10b of the paper substrate 10. The oxygen permeability was 4.1 cc / m 2 7 shows the structure of the paper barrier laminate 101 of Example 2-4 which was subjected to extrusion lamination.
[0054] [Example 2-5] A paper barrier laminate 101 was produced and its oxygen permeability was measured in the same manner as in Example 2-2, except that the resin layer 30 was not formed on the other surface 10b of the paper substrate 10. The oxygen permeability was 3.3 cc / m 2 7 shows the structure of the paper barrier laminate 101 of Example 2-5 which was subjected to extrusion lamination. [Example 2-6] A paper barrier laminate 101 was produced and its oxygen permeability was measured in the same manner as in Example 2-3, except that the resin layer 30 was not formed on the other surface 10b of the paper substrate 10. The oxygen permeability was 15.0 cc / m 2 7 shows the structure of the paper barrier laminate 101 of Example 2-6 which was subjected to extrusion lamination.
[0055] [Comparative Example 2-1] The coating weight of the barrier layer 20 is 0.2 g / m 2 A paper barrier laminate 101 was produced and its oxygen permeability was measured in the same manner as in Example 2-1, except that the oxygen permeability was 280.0 cc / m 2 ·day. [Comparative Example 2-2] The coating weight of the barrier layer 20 is 3.1 g / m 2 A paper barrier laminate 101 was produced and its oxygen permeability was measured in the same manner as in Example 2-1, except that the oxygen permeability was 3.0 cc / m 2 ·day.
[0056] [Table 2]
[0057] As shown in Table 2, in Examples 2-3 and 2-6 in which the smoothness of the paper substrate 10 is greater than 5.0 μm, the oxygen permeability is 10 cc / m 2 Larger than day, and although there are no problems with use, the barrier properties tend to be low. On the other hand, in Examples 2-1 and 2-2 in which the smoothness of the paper base material 10 was 5.0 μm or less, the oxygen permeability was 10 cc / m 2Even though the barrier layer 20 is a thin film, the surface of the paper base material 10 is smooth, so there are few defects in the barrier layer 20, and the barrier property is high. Furthermore, the paper barrier laminates 101 of Examples 2-1 to 2-6 are also good paper barrier laminates from the standpoint of profitability. In addition, in the paper barrier laminate 101 of Comparative Example 2-1, the coating amount of the barrier layer 20 was 0.3 g / m 2 The oxygen permeability is extremely high because the oxygen permeability is below 100%. Furthermore, the paper barrier laminate 101 of Comparative Example 2-2 has a good oxygen permeability, but is not preferable from the viewpoint of profitability.
[0058] The above describes one embodiment of the present invention and examples. However, the technical scope of the present invention is not limited to the contents of the above embodiment, and various modifications and deletions can be made to each component without departing from the spirit of the present invention. In addition to the above-mentioned layers, the barrier laminate of the present invention may be provided with a printed layer for imparting a desired design effect or information, an antistatic layer, or the like, as necessary. [Explanation of symbols]
[0059] 10 Paper base material 20 Barrier Layer 21 Layer containing CNF and water-soluble polymer 22 Layer containing only water-soluble polymers 30 Resin layer 100 Paper Barrier Laminate 101 Paper barrier laminate with resin layer 200 Paper Barrier Containers
Claims
1. A paper barrier laminate comprising a paper substrate and a barrier layer containing cellulose nanofibers; and a resin layer formed on both sides of the paper barrier laminate, The coating weight of the barrier layer is 0.3 g / m 2 3.0g / m or more 2 Within the following range: the ratio of oxygen permeability (B / A) before (A) and after (B) of the paper barrier laminate provided with the resin layer is subjected to a folding treatment by the following method is 3.0 or less, The barrier layer further comprises a water-soluble polymer, A paper barrier laminate comprising a resin layer, characterized in that in the barrier layer, the mass ratio of the cellulose nanofiber to the water-soluble polymer (cellulose nanofiber / water-soluble polymer) is different between the paper substrate side and the opposite side. Folding treatment: According to JIS K5600-5-1, the film is wound around a mandrel having a diameter of 8 mm for 2 seconds with the surface on which the barrier layer is formed facing outward, and then returned to its original state.
2. A paper barrier laminate comprising a paper substrate and a barrier layer containing cellulose nanofibers; and a resin layer formed on both sides of the paper barrier laminate, The coating weight of the barrier layer is 0.3 g / m 2 3.0g / m or more 2 Within the following range: the ratio of oxygen permeability (B / A) before (A) and after (B) of the paper barrier laminate provided with the resin layer is subjected to a folding treatment by the following method is 3.0 or less, The barrier layer further comprises a water-soluble polymer, A paper barrier laminate with a resin layer, characterized in that the barrier layer is formed by laminating, from the paper base material side, a layer containing the water-soluble polymer as a main component, and a layer containing the cellulose nanofibers and the water-soluble polymer, in that order. Folding treatment: According to JIS K5600-5-1, the film is wound around a mandrel having a diameter of 8 mm for 2 seconds with the surface on which the barrier layer is formed facing outward, and then returned to its original state.
3. A paper barrier laminate comprising a paper substrate and a barrier layer containing cellulose nanofibers; and a resin layer formed on both sides of the paper barrier laminate, The coating weight of the barrier layer is 0.3 g / m 2 3.0g / m or more 2 Within the following range: the ratio of oxygen permeability (B / A) before (A) and after (B) of the paper barrier laminate provided with the resin layer is subjected to a folding treatment by the following method is 3.0 or less, The barrier layer further comprises a water-soluble polymer, A paper barrier laminate with a resin layer, characterized in that the barrier layer is formed by laminating, in this order from the paper base material side, a layer containing the cellulose nanofibers and the water-soluble polymer, and a layer containing the water-soluble polymer as a main component. Folding treatment: According to JIS K5600-5-1, the film is wound around a mandrel having a diameter of 8 mm for 2 seconds with the surface on which the barrier layer is formed facing outward, and then returned to its original state.
4. The oxygen permeability of the paper barrier laminate is 20 cc / m 2 4. A paper barrier laminate comprising the resin layer according to claim 1, wherein the resin layer has a viscosity of 0.01 to 0.1 s, and a viscosity of ...
5. 5. A paper barrier laminate comprising the resin layer according to any one of claims 1 to 4, characterized in that the smoothness of the surface of the paper base material on which the barrier layer is formed is 5.0 µm or less, as measured by the following method. Measurement of smoothness: According to JIS P8151 "Paper and paperboard -- Surface roughness and smoothness test method (air leak method) -- Print surf tester method", the measurement was performed with a clamp pressure of 1000 kPa and a soft backing.
6. 6. A paper barrier laminate comprising a resin layer according to any one of claims 1 to 5, characterized in that a mass ratio of the cellulose nanofiber to the water-soluble polymer in the barrier layer (cellulose nanofiber / water-soluble polymer) is 5 / 95 to 99 / 1.
7. The paper barrier laminate provided with a resin layer according to claim 1, characterized in that the barrier layer is a laminate in which at least two or more layers are laminated.
8. 8. A paper barrier laminate comprising a resin layer according to any one of claims 1 to 7, wherein the water-soluble polymer is at least one of polyvinyl alcohol and carboxymethyl cellulose.
9. 9. A paper barrier laminate comprising a resin layer according to any one of claims 1 to 8, characterized in that the cellulose nanofiber is anionically modified cellulose nanofiber.
10. 10. A paper barrier laminate comprising a resin layer according to any one of claims 1 to 9, characterized in that the cellulose nanofiber has a carboxy group per cellulose mass in the range of 0.1 mmol / g to 3.5 mmol / g.
11. 11. A paper barrier laminate comprising a resin layer according to any one of claims 1 to 10, characterized in that a portion of the OH groups of the cellulose nanofibers is substituted with carboxymethyl groups, and the degree of substitution is within the range of 0.1 or more and 0.5 or less.
12. A paper barrier container, formed using a paper barrier laminate comprising the resin layer according to any one of claims 1 to 11.
Citation Information
Patent Citations
Production of fine fibrous cellulose
JP1994010288A
Paper laminate having barrier property and its production method
JP2003094574A
Packaging material for aromatic
JP2004299203A
Fine cellulose fiber
JP2008001728A
Method for producing cellulose nanofibers
JP2008308802A