Transparent laminate
Stabilizing the pH of a conductive layer with a poly(3,4-disubstituted thiophene) and polyanion complex in a transparent laminate enhances adhesiveness and conductivity, addressing stability issues in existing laminates.
Patent Information
- Application Number
- JP2020103911
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-06-16
- Publication Date
- 2024-10-02
- Estimated Expiration
- 2039-07-09
AI Technical Summary
Existing transparent laminates with conductive layers and adhesive layers on transparent resin films face issues with adhesiveness and conductivity stability, particularly when using conductive polymers like poly(3,4-disubstituted thiophene) complexes, which suffer from pH changes over time, affecting adhesion and durability.
A conductive layer composed of a poly(3,4-disubstituted thiophene) and polyanion complex is stabilized by blending it with an aqueous resin and an alkali compound, aged to maintain a pH of 4 to 9, and applied on a transparent resin film, ensuring high adhesiveness and conductivity.
The laminate maintains high adhesiveness and conductivity, with the conductive layer exhibiting a surface resistivity of 4×10^2 to 1×10^10 Ω/sq, and demonstrates stable adhesion even under high temperature and humidity conditions.
Smart Images

Figure 0007560275000001 
Figure 0007560275000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a transparent laminate, and more particularly to a transparent laminate having a conductive layer and an adhesive layer laminated on a transparent resin film, in which the conductive layer has high adhesion to the adhesive layer and has high electrical conductivity. [Background technology]
[0002] Various optical films and optical filters used in liquid crystal display devices and the like may be required to have properties such as adhesion of lamination and antistatic properties in addition to excellent optical properties. For example, in a liquid crystal display device, polarizing plates are arranged on both sides of a liquid crystal cell, and only light polarized in a specific direction among light irradiated from a light source and transmitted through a liquid crystal layer is emitted as display light. Here, in a liquid crystal display device, it is necessary to stabilize the liquid crystal orientation to prevent image disturbance, so that the polarizing plate is required to have antistatic properties in order to prevent disturbance of the electric field in the liquid crystal cell.
[0003] In Patent Document 1, an optical film is provided with antistatic properties by forming a layer structure in which a conductive layer is disposed between a transparent resin film and an adhesive layer. In this optical film, a specific adhesive layer made of a nitrogen-containing acrylic adhesive is used to strengthen the adhesion between the adhesive layer and the conductive layer. However, in the manufacturing method disclosed in Patent Document 1, the conductive polymer contained in the conductive layer cannot be stabilized, and the adhesion between the adhesive layer and the conductive layer cannot be strengthened unless a specific adhesive layer is used.
[0004] Patent Document 2 also discloses an optical film in which a conductive layer is disposed between a transparent resin film and an adhesive layer. The conductive layer contains a conductive polymer that is soluble in an organic solvent, and as a result, the adhesive layer and the conductive layer maintain their adhesion even after storage under high temperature and high humidity conditions. However, the polyaniline-based conductive polymer used in Patent Document 2 tends to show coloration, and its durability is not sufficient. There is no mention of stabilization of other conductive polymers. In particular, no method is suggested for strengthening the adhesion between the adhesive layer and the conductive layer that contains a complex of poly(3,4-disubstituted thiophene) and a polyanion. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2006-116809 A [Patent Document 2] JP 2006-212783 A Summary of the Invention [Problem to be solved by the invention]
[0006] The present invention aims to improve the adhesion between a conductive layer and an adhesive layer while maintaining electrical conductivity in a transparent laminate comprising a conductive layer and an adhesive layer laminated in this order on a transparent resin film. [Means for solving the problem]
[0007] The present inventors have found that when a conductive layer is formed by a conventional method, the pH of the conductive polymer contained in the conductive layer changes over time, which changes the properties of the conductive layer and impairs the adhesiveness to the adhesive layer. They have also found that the adhesiveness to the adhesive layer can be improved by blending a pH-stabilized conductive polymer into the conductive layer, and have completed the present invention.
[0008] That is, the present invention provides a transparent laminate comprising a transparent resin film (A), a conductive layer (B), and an adhesive layer (C) laminated in this order on the transparent resin film (A), the transparent resin film (A) being made of one or more resins selected from the group consisting of acrylic resins, cycloolefin resins, and cellulose resins, the conductive layer (B) being made of a conductive layer-forming composition containing a conductive polymer (b1) which is a complex of poly(3,4-disubstituted thiophene) and a polyanion, and an aqueous resin (b2), and the surface resistivity on the conductive layer (B) is 4×10 2 ~1×10 10 Ω / sq.
[0009] The aqueous resin (b2) is preferably a mixture of three or more resins selected from the group consisting of acrylic resins, polyether resins, polyester resins, polyurethane resins, polyolefin resins, siloxane resins, and oxazoline resins.
[0010] The conductive layer (B) is preferably formed by drying the coated conductive layer-forming composition at 80° C. or less for 5 minutes or less.
[0011] The present invention also relates to a conductive composition for producing a composition for forming a conductive layer in the transparent laminate, the conductive composition comprising a conductive polymer (b1) which is a complex of poly(3,4-disubstituted thiophene) and a polyanion, an alkaline compound, and water, and having a pH of 4 to 9.
[0012] The conductive composition is preferably aged for 100 hours or more.
[0013] The conductive composition preferably has a pH value reduced by 0.2 or more from that immediately after preparation.
[0014] The conductive composition preferably has a pH drop of 0.15 or less per week.
[0015] The present invention also relates to a pre-aging composition for producing the conductive composition, which comprises a conductive polymer (b1) that is a complex of poly(3,4-disubstituted thiophene) and a polyanion, an alkaline compound, and water, and has a pH of 5 to 10.
[0016] The alkaline compound is preferably a nitrogen-based compound.
[0017] The pre-ripening composition preferably further contains an aqueous resin (b2).
[0018] Preferably, the pre-ripening composition further comprises a preservative.
[0019] The pre-aged composition preferably further contains an organic solvent.
[0020] The present invention also relates to a method for producing a conductive composition, which comprises a step of aging the pre-aged composition at 1 to 42° C. for 100 to 10,000 hours.
[0021] The present invention also relates to a composition for forming a conductive layer, comprising the conductive composition, and 100 parts by weight or more of an aqueous diluent relative to 100 parts by weight of the conductive composition, and / or 1 to 1,000 parts by weight of an aqueous resin (b2) relative to 100 parts by weight of the solid content of the conductive composition.
[0022] The present invention also relates to a conductive composition obtained by aging the pre-aged composition, and a conductive layer-forming composition comprising 100 parts by weight or more of an aqueous diluent relative to 100 parts by weight of the pre-aged composition, and / or 1 to 1,000 parts by weight of an aqueous resin (b2) relative to 100 parts by weight of the solid content of the pre-aged composition.
[0023] The present invention also relates to a method for producing a method for producing a polymerizable compound comprising the steps of: (i) a step of mixing a conductive polymer (b1), which is a complex of poly(3,4-disubstituted thiophene) and a polyanion, an alkaline compound, and water to produce a pre-ripening composition having a pH of 5 to 10; (ii) aging the pre-aged composition; and (iii) adding an aqueous diluent and / or an aqueous resin (b2) to the aged composition in that order, The present invention relates to a method for producing the conductive layer-forming composition.
[0024] The maturation in the step (ii) (ii-1) Aging the pre-aging composition for 100 hours or more; (ii-2) decreasing the pH of the pre-ripening composition by 0.2 or more; or (ii-3) Aging the composition until the pH decrease per week of the composition before aging is 0.15 or less; It is preferable that the above-mentioned method be used.
[0025] The present invention also relates to a method for producing the transparent laminate, comprising the steps of applying the conductive layer-forming composition to a transparent resin film (A) and drying the applied conductive layer-forming composition at 100° C. or lower for 5 minutes or less. Effect of the Invention
[0026] The transparent laminate of the present invention has high adhesion between the conductive layer and the adhesive layer while maintaining electrical conductivity of the entire transparent laminate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0027] <<Transparent laminate>> The transparent laminate of the present invention is a transparent laminate comprising a conductive layer (B) and an adhesive layer (C) laminated in this order on a transparent resin film (A), the transparent resin film (A) being made of one or more resins selected from the group consisting of acrylic resins, cycloolefin resins, and cellulose resins, the conductive layer (B) being made of a conductive layer-forming composition containing a conductive polymer (b1) which is a complex of poly(3,4-disubstituted thiophene) and a polyanion, and an aqueous resin (b2), and the surface resistivity on the conductive layer (B) is 4×10 2 ~1×10 10 Ω / sq.
[0028] <Transparent resin film (A)> The transparent resin film is made of a resin selected from the group consisting of acrylic resins, cycloolefin resins, and cellulose resins. These resins are excellent in flexibility, transparency, easy moldability, etc. Examples of acrylic resins include polymethyl methacrylate resin (PMMA). Examples of cycloolefin resins include cycloolefin polymer resin (COP). Examples of cellulose resins include triacetyl cellulose (TAC) resin. These transparent resin films may be used alone or in combination of two or more.
[0029] The thickness of the transparent resin film is not particularly limited, but is preferably 10 to 1000 μm, and more preferably 25 to 500 μm, and the total light transmittance of the transparent resin film is preferably 60% or more, more preferably 70% or more, and even more preferably 80% or more.
[0030] Before applying the conductive layer-forming composition described below, the surface of the transparent resin film (A) may be subjected to a surface treatment in advance, if necessary. Examples of the surface treatment include corona treatment, excimer treatment, plasma treatment, glow treatment, ozone treatment, itro treatment, flame treatment, and primer treatment. The corona treatment can be performed, for example, by discharging in normal air pressure using a corona treatment machine manufactured by Kasuga Electric Co., Ltd. The excimer treatment can be performed by irradiating an excimer lamp. The excimer lamp is a UV lamp containing Xe and having a wavelength of 180 nm or less. The plasma treatment can be performed, for example, by discharging in normal air pressure or in an inert gas atmosphere such as nitrogen or argon using a plasma discharge machine manufactured by Sekisui Chemical Co., Ltd. The glow treatment and ozone treatment can also be performed according to the usual method. These treatments may be performed in combination with each other on the transparent resin film (A).
[0031] <Conductive layer (B)> The conductive layer (B) is made of a conductive layer-forming composition containing a conductive polymer (b1), which is a complex of poly(3,4-disubstituted thiophene) and a polyanion, and an aqueous resin (b2), and can be formed by applying the conductive layer-forming composition onto the surface of the transparent resin film (A). The conductive layer (B) may be formed by directly applying the conductive layer-forming composition onto the transparent resin film (A), or may be formed by applying the conductive layer-forming composition onto a layer such as a primer layer that has been previously provided on the transparent resin film (A).
[0032] The conductive layer (B) can be obtained by applying the conductive layer-forming composition to at least one surface of the transparent resin film (A) and then drying it. The method for applying the conductive layer-forming composition is not particularly limited and any known method can be used, such as roll coating, bar coating, dip coating, spin coating, etc.
[0033] The drying of the conductive layer-forming composition after application is not particularly limited as long as it can remove the solvent contained in the conductive layer-forming composition, and may be performed by a known method, for example, using a fan oven, an infrared oven, a vacuum oven, etc.
[0034] The drying temperature of the conductive layer-forming composition is preferably 100° C. or less, more preferably 40 to 80° C. The drying time is preferably 5 minutes or less, more preferably 0.3 to 3 minutes.
[0035] The thickness of the conductive layer (B) is preferably from 1 to 300 nm, more preferably from 5 to 250 nm, and further preferably from 10 to 200 nm. The thickness of the conductive layer (B) refers to a value obtained by measurement according to the method described in the examples.
[0036] In the transparent laminate of the present invention, the surface resistivity on the conductive layer (B) is 4×10 2 ~1×10 10 Ω / sq, 5×10 2 ~1×10 9 The surface resistivity of the conductive layer (B) is preferably Ω / sq. The surface resistivity of the conductive layer (B) refers to a value obtained by forming the conductive layer (B) on the transparent resin film (A) and then measuring the surface resistivity by the method described in the Examples.
[0037] <Composition for forming conductive layer> The conductive layer-forming composition contains a conductive polymer (b1), which is a complex of poly(3,4-disubstituted thiophene) and a polyanion, and an aqueous resin (b2).
[0038] <Conductive polymer (b1)> The conductive polymer (b1) is a complex of poly(3,4-disubstituted thiophene) and a polyanion, where the polyanion is a dopant for the poly(3,4-disubstituted thiophene).
[0039] The poly(3,4-disubstituted thiophene) is preferably a poly(3,4-dialkoxythiophene) or a poly(3,4-alkylenedioxythiophene). The poly(3,4-dialkoxythiophene) or the poly(3,4-alkylenedioxythiophene) is preferably a poly(3,4-dialkoxythiophene) represented by the following formula (I):
[0040] [ka]
[0041] Preferred are polythiophenes in cationic form consisting of repeating structural units of the formula: Here, R 1 and R 2 are each independently a hydrogen atom or C 1-4 or they are bonded together to form an alkyl group of C 1-4 C represents an alkylene group. 1-4 The alkyl group is not particularly limited, but examples thereof include a methyl group, an ethyl group, a propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, and a t-butyl group. Also, R 1 and R 2 If C is bonded 1-4 The alkylene group in is not particularly limited, but examples thereof include a methylene group, a 1,2-ethylene group, a 1,3-propylene group, a 1,4-butylene group, a 1-methyl-1,2-ethylene group, a 1-ethyl-1,2-ethylene group, a 1-methyl-1,3-propylene group, and a 2-methyl-1,3-propylene group. Among these, a methylene group, a 1,2-ethylene group, and a 1,3-propylene group are preferred, and a 1,2-ethylene group is more preferred. 1-4 and C 1-4 The alkylene group may have some of its hydrogen atoms substituted. 1-4As the polythiophene having an alkylene group, poly(3,4-ethylenedioxythiophene) is particularly preferred.
[0042] The weight-average molecular weight of the conductive polymer (b1) is preferably 500 to 100,000, more preferably 1,000 to 10,000, and even more preferably 1,200 to 5,000. If the weight-average molecular weight is less than 500, the required viscosity may not be ensured when the conductive polymer is used as a conductive composition, and the conductivity may decrease when the conductive polymer is used as a conductive layer (B).
[0043] The polyanion forms a complex by forming an ion pair with the polythiophene (derivative), and the polythiophene (derivative) can be stably dispersed in water. The polyanion is not particularly limited, but examples thereof include carboxylic acid polymers (e.g., polyacrylic acid, polymaleic acid, polymethacrylic acid, etc.), sulfonic acid polymers (e.g., polystyrene sulfonic acid, polyvinyl sulfonic acid, polyisoprene sulfonic acid, etc.), etc. These carboxylic acid polymers and sulfonic acid polymers may also be copolymers of vinyl carboxylic acids and vinyl sulfonic acids with other polymerizable monomers, for example, acrylates, aromatic vinyl compounds such as styrene and vinyl naphthalene. Among these, polystyrene sulfonic acid is preferred, polystyrene sulfonate is more preferred, and amine salt or ammonium salt of polystyrene sulfonic acid is even more preferred.
[0044] Regarding the amine salt of polystyrene sulfonic acid, the amine is not particularly limited, but examples thereof include trimethylamine (TMA), triethylamine (TEA), tri-n-propylamine (TPA), tri-n-butylamine (TBA), ethyldimethylamine, N,N-dimethylethanolamine, morpholine, etc. These may be used alone or in combination of two or more.
[0045] The weight-average molecular weight of the polystyrene sulfonic acid is preferably 10,000 to 1,000,000, and more preferably 30,000 to 500,000. If a polystyrene sulfonic acid having a molecular weight outside this range is used, the dispersion stability of the polythiophene-based conductive polymer in water may decrease. The weight-average molecular weight is a value measured by gel permeation chromatography (GPC).
[0046] From the viewpoint of particularly excellent conductivity, the conductive polymer (b1) is preferably a complex of poly(3,4-ethylenedioxythiophene) and polystyrenesulfonic acid. Also, from the viewpoint of storage stability of the conductive layer-forming composition and adhesion between the conductive layer (B) and the adhesive layer (C), it is preferably a complex of polythiophene having a repeating structural unit represented by general formula (I) and an amine salt or ammonium salt of polystyrenesulfonic acid.
[0047] The conductivity of the conductive polymer (b1) is not particularly limited, but from the viewpoint of imparting sufficient conductivity to the conductive layer (B), it is preferably 0.01 S / cm or more, and more preferably 1 S / cm or more.
[0048] The content of the conductive polymer (b1) in the conductive layer-forming composition is 0.01 to 100.0 mg / m when the conductive layer (B) is formed on the transparent resin film (A). 2 The amount is preferably 1 to 50.0 mg / m 2 More preferably, the amount is 0.01 mg / m 2 If it is less than 100.0 mg / m, the electrical conductivity of the conductive layer (B) may not be sufficiently ensured. 2 If it exceeds this range, it may cause adverse effects on the strength and film-forming properties of the coating film.
[0049] <Aqueous resin (b2)> The aqueous resin (b2) is blended to impart film-forming properties, strength, and the like to the conductive layer. The timing of blending the aqueous resin (b2) is not particularly limited as long as it is blended in the conductive layer-forming composition, and it may be blended in the pre-ripening composition or may be added to the ripened conductive composition. In addition, when blending multiple types of aqueous resins (b2), it is preferable to add at least one type after ripening the pre-ripening composition from the viewpoint of the adhesive strength between the conductive layer (B) and the transparent resin film (A) and the adhesive layer (C). Examples of the aqueous resin (b2) include acrylic resins, polyether resins, polyester resins, polyurethane resins, polyolefin resins, siloxanes, and oxazoline resins. The aqueous resin (b2) is preferably soluble or dispersible in water to facilitate blending with the conductive polymer (b1). The resin may be solubilized or dispersed as a result of imparting a hydrophilic functional group to the resin, or may be forcibly solubilized or dispersed by an emulsifier.
[0050] In addition, the aqueous resin (b2) contained in the conductive layer-forming composition is preferably a mixture of three or more selected from the group consisting of acrylic resin, polyether resin, polyester resin, polyurethane resin, polyolefin resin, siloxane, and oxazoline resin. Furthermore, among the mixture of three or more, it is more preferable to include at least one selected from the group consisting of acrylic resin, polyurethane resin, and polyolefin resin. By using such a mixture of three or more, the effect of stably expressing the adhesive strength between the conductive layer (B) and the transparent resin film and the adhesive layer is achieved.
[0051] Examples of the acrylic resin include (meth)acrylic resins and vinyl ester resins. These acrylic resins may be polymers containing, as constituent monomers, polymerizable monomers having an acid group such as a carboxyl group, an acid anhydride group, a sulfonic acid group, or a phosphoric acid group, and a fluoro group such as a perfluoroalkyl group or a perfluoroalkenyl group. For example, a homopolymer or copolymer of a polymerizable monomer having an acid group, a copolymer of a polymerizable monomer having an acid group and a copolymerizable monomer, and the like may be mentioned.
[0052] The (meth)acrylic resin may be polymerized with a copolymerizable monomer as long as it contains a (meth)acrylic monomer as a main constituent monomer (e.g., 50 mol % or more). At least one of the (meth)acrylic monomer and the copolymerizable monomer preferably has an acid group.
[0053] Examples of the (meth)acrylic resin include a (meth)acrylic monomer having an acid group [(meth)acrylic acid, sulfoalkyl (meth)acrylate, sulfonic acid group-containing (meth)acrylamide, etc.] or a copolymer thereof, a copolymer of a (meth)acrylic monomer which may have an acid group and another polymerizable monomer having an acid group [another polymerizable carboxylic acid, a polymerizable polycarboxylic acid or anhydride, vinyl aromatic sulfonic acid, etc.] and / or a copolymerizable monomer [for example, (meth)acrylic acid alkyl ester, glycidyl (meth)acrylate, (meth)acrylonitrile, aromatic vinyl monomer, etc.] ... having an acid group and another polymerizable monomer having an acid group [another polymerizable carboxylic acid, a polymerizable polycarboxylic acid or anhydride, vinyl aromatic sulfonic acid, etc.] and / or a copolymerizable monomer [for example, (meth)acrylic acid alkyl ester, glycidyl (meth)acrylate, (meth)acrylonitrile, aromatic vinyl monomer, etc.], a copolymer of a (meth)acrylic monomer having an acid group and another polymerizable monomer having an acid group [another polymerizable carboxylic acid, a polymerizable polycarboxylic acid or anhydride, vinyl aromatic sulfonic acid, etc.], a copolymer of a (meth)acrylic monomer having an acid group and another polymerizable monomer having an acid group [another polymerizable carboxylic acid, a polymerizable polycarboxylic acid or anhydride, vinyl aromatic sulfonic acid, etc.], and a copolymer of a (meth)acrylic monomer having an acid group and another polymerizable monomer having an acid group [another polymerizable carboxylic acid, a polymerizable polycarboxylic acid or anhydride, vinyl aromatic sulfonic acid, etc.] and / or a and (meth)acrylic copolymerizable monomers [for example, (meth)acrylic acid alkyl esters, hydroxyalkyl (meth)acrylates, glycidyl (meth)acrylates, (meth)acrylonitrile, etc.], (meth)acrylic monomers not having an acid group [alkyl (meth)acrylates, aryl (meth)acrylates, fluorene-based (meth)acrylates, etc.] or copolymers thereof, rosin-modified urethane acrylates, specially modified acrylic resins, urethane acrylates, epoxy acrylates, urethane acrylate emulsions, etc. can be mentioned.
[0054] Among these (meth)acrylic resins, (meth)acrylic acid-(meth)acrylic acid ester polymers (acrylic acid-methyl methacrylate copolymers, etc.), (meth)acrylic acid-(meth)acrylic acid ester-styrene copolymers (acrylic acid-methyl methacrylate-styrene copolymers, etc.), and the like are preferred.
[0055] Examples of the polyether resin include polyalkylene glycol, polyvinyl alcohol, polyether polyol, polyglycerin, pullulan, and derivatives thereof. These polyether resins may have an acid group such as a carboxyl group, an acid anhydride group, a sulfonic acid group, or a phosphoric acid group, a fluoro group such as a perfluoroalkyl group or a perfluoroalkenyl group, and an alkyl group or an alkenyl group.
[0056] The polyester resin is not particularly limited as long as it is a polymer compound obtained by a method of polycondensing a compound having two or more carboxyl groups in a molecule with a compound having two or more hydroxyl groups, a method of directly dehydrating polycondensing a hydroxycarboxylic acid, or a method of ring-opening polymerization of a cyclic ester of a hydroxycarboxylic acid. For example, a compound having two or more hydroxyl groups (diol component) includes an aliphatic diol, an alicyclic diol, an aromatic diol, a (poly)carbonate diol, a polyether diol, a polyester diol, etc., a compound having two or more carboxyl groups in a molecule (dicarboxylic acid component) includes an aliphatic dicarboxylic acid, an aromatic dicarboxylic acid, an alicyclic dicarboxylic acid, etc., and a cyclic ester of a hydroxycarboxylic acid includes lactide, glycolide, ε-caprolactone, etc. General names of the obtained polymer compounds include polyethylene terephthalate, polytrimethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polybutylene naphthalate, etc. These polyester resins may have an acid group such as a carboxyl group, an acid anhydride group, a sulfonic acid group or a phosphoric acid group, a fluoro group such as a perfluoroalkyl group or a perfluoroalkenyl group, an alkyl group or an alkenyl group.
[0057] The polyurethane resin is not particularly limited as long as it is a polymeric compound obtained by copolymerizing a compound having an isocyanate group and a compound having a hydroxyl group, and examples thereof include ester-ether polyurethane resin, ether polyurethane resin, polyester polyurethane resin, carbonate polyurethane resin, and acrylic polyurethane resin. These polyurethane resins may have nonionic, anionic, or cationic hydrophilic polar groups introduced. Examples of sources for introducing hydrophilic polar groups include linear nonionic hydrophilic polar groups such as poly(oxyethylene) polyol, anionic hydrophilic polar groups such as -COOM and -SO3M (M represents an alkali metal, an ammonium group, or an organic amine), and cationic hydrophilic polar groups such as quaternary ammonium salts.
[0058] Examples of polyolefin resins include polyethylene, polypropylene, poly-4-methyl-1-pentene, poly-1-butene, chlorinated polypropylene, maleic anhydride-modified polypropylene, maleic anhydride-modified chlorinated polypropylene, etc. These polyolefin resins may be copolymers with α-olefin comonomers such as butene-1, pentene-1, hexene-1, heptene-1, octene-1, cyclopentene, cyclohexene, and norbornene, and comonomers such as vinyl acetate, acrylic acid esters, and methacrylic acid esters, and may have hydrophilic polar groups introduced therein, such as carboxylic acid groups (-COOH), sulfo groups (-SO3H), sulfino groups (-SO2H), phosphono groups (-PO2H), vinyl alcohol chains, vinylpyrrolidone chains, and ether chains.
[0059] The siloxane is a high molecular weight alkoxysilane formed by condensing alkoxysilane monomers represented by the following formula (II) and has one or more siloxane bonds (Si-O-Si) in one molecule. SiR4(II) (In the formula, R is hydrogen, a hydroxyl group, an alkoxy group having 1 to 4 carbon atoms, an alkyl group which may have a substituent, or a phenyl group which may have a substituent, provided that at least one of the four R's is an alkoxy group having 1 to 4 carbon atoms or a hydroxyl group.)
[0060] The structure of the siloxane is not particularly limited, and may be linear or branched. The siloxane may be a compound represented by formula (II) used alone or in combination of two or more kinds. These siloxanes may be modified with a polyether group, a polyalkyl group, a polyester group, or a polyol group. The modified form may be linear or branched.
[0061] Examples of the oxazoline resin include addition-polymerizable oxazoline compounds such as 2-isopropenyl-2-oxazoline, 2-vinyl-2-oxazoline, and 2-vinyl-4-methyl-2-oxazoline. Commercially available products include EPOCROS WS-300, WS-500, and WS-700 (manufactured by Nippon Shokubai Co., Ltd.). By incorporating an oxazoline resin, crosslinking occurs between the conductive polymers (b1) themselves or between the conductive polymers (b1) and the aqueous resin (b2), thereby improving the coating strength of the conductive layer (B).
[0062] The content of the aqueous resin (b2) in the conductive layer-forming composition is not particularly limited, but is preferably 10 to 5000 parts by weight, more preferably 30 to 3000 parts by weight, and even more preferably 50 to 2000 parts by weight, per 100 parts by weight of the conductive polymer (b1). When the content of the aqueous resin (b2) is within the above range, sufficient conductivity can be ensured in the conductive layer.
[0063] The conductive layer-forming composition is obtained by diluting a conductive composition containing a conductive polymer (b1), an alkaline compound, and water and having a pH of 4 to 9 with an aqueous diluent and / or an aqueous resin (b2). The conductive composition will be described later. When the aqueous resin (b2) is added to the conductive composition whose pH has been stabilized through aging, deterioration such as aggregation and component separation of the aqueous resin (b2) can be suppressed under conditions in which moisture and organic solvents evaporate in the conductive layer forming process, and this is effective in improving the adhesive strength between the conductive layer (B) and the transparent resin film (A) and the adhesive layer (C). In addition, by adding an aqueous diluent after aging, the pH can be stabilized by aging in a short period of time.
[0064] Examples of the aqueous diluent include water and alcohol. As the alcohol, ethanol, methanol, 2-propanol, 1-propanol, etc. are preferable. A mixture of these may be used, for example, a mixture of water and ethanol may be used as the aqueous diluent. When a mixture is used, the concentration of the alcohol is preferably 0 to 50% by weight, more preferably 0 to 40% by weight, and further preferably 0 to 30% by weight.
[0065] When diluting with an aqueous diluent, the amount of diluent added is preferably 100 parts by weight or more, more preferably 350 parts by weight or more, relative to 100 parts by weight of the conductive composition. The upper limit of the amount added is not particularly limited, but is, for example, 3000 parts by weight. Since the weight change of the pre-ripening composition before and after aging is usually 5% or less, the amount of aqueous diluent added is preferably 100 parts by weight or more, more preferably 350 parts by weight or more, relative to 100 parts by weight of the pre-ripening composition, and the upper limit is, for example, 3000 parts by weight.
[0066] When diluting with aqueous resin (b2), the amount of aqueous resin (b2) added is preferably 1 to 1000 parts by weight, more preferably 50 to 500 parts by weight, per 100 parts by weight of the solid content of the conductive composition. Here, when the aqueous resin (b2) is dispersed, the amount added is the weight part of the solid content. Since the weight change of the composition before aging before and after aging is usually 5% or less, the amount of aqueous resin (b2) added is preferably 1 to 1000 parts by weight, more preferably 50 to 500 parts by weight, per 100 parts by weight of the solid content of the composition before aging.
[0067] The conductive layer-forming composition has a solids concentration of preferably 0.05 to 6%, more preferably 0.1 to 5%, and even more preferably 0.1 to 4.5%, and a pH of preferably 4.0 to 9.0, and more preferably 5.0 to 8.5.
[0068] As described above, the conductive layer-forming composition preferably contains a mixture of three or more aqueous resins (b2). When diluting the conductive composition with the aqueous resin (b2), a conductive composition that does not contain the aqueous resin (b2) may be diluted with three or more aqueous resins (b2), or a conductive composition that contains one or two types of aqueous resins (b2) may be diluted with one or more aqueous resins (b2).
[0069] <Conductive composition and pre-aged composition> The conductive composition contains a conductive polymer (b1) which is a complex of poly(3,4-disubstituted thiophene) and a polyanion, an alkaline compound, and water, and has a pH of 4 to 9. The conductive composition is used for producing the conductive layer-forming composition.
[0070] The composition before aging contains a conductive polymer (b1) which is a complex of poly(3,4-disubstituted thiophene) and a polyanion, an alkaline compound, and water, and has a pH of 5 to 10. The conductive composition is obtained by aging the composition before aging.
[0071] The complex of poly(3,4-disubstituted thiophene) and polyanion is often strongly acidic with pH 1.0 to 3.5 as an aqueous dispersion with 1% solid content, and when an aqueous resin is added to it, some of the aqueous resin may aggregate, depending on the type of the aqueous resin, and the aggregation becomes particularly noticeable in the high concentration state during the drying process after coating. Therefore, it is preferable to neutralize it by adding an alkaline compound.
[0072] The alkaline compound is not particularly limited as long as it can increase the pH when added to an aqueous solution, and examples of the alkaline compound include bases containing alkali metals or alkaline earth metals, NH3, nitrogen-based aliphatic compounds, and nitrogen-based aromatic compounds. Examples of bases containing alkali metals or alkaline earth metals include sodium hydroxide, potassium hydroxide, magnesium hydroxide, calcium hydroxide, sodium hydrogen carbonate, and potassium hydrogen carbonate. Examples of nitrogen-based aliphatic compounds include triethanolamine, ethanolamine, diethanolamine, dimethylamine, diethylamine, dipropylamine, trimethylamine, triethylamine, and tripropylamine. Examples of nitrogen-based aromatic compounds include imidazole, 2-methylimidazole, 2-propylimidazole, 1-(2-hydroxyethyl)imidazole, 2-ethyl-4-methylimidazole, 1,2-dimethylimidazole, 1-cyanoethyl-2-methylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 2-aminobenzimidazole, pyridine, aniline, and toluidine. The above-mentioned alkaline compounds may be used alone or in combination of two or more kinds, and among these, NH3, nitrogen-based aliphatic compounds, and nitrogen-based aromatic compounds are preferred, NH3 and nitrogen-based aliphatic compounds are more preferred, and triethanolamine and NH3 are even more preferred. The amount of the alkaline compound to be added is not particularly limited as long as it is an amount that realizes a predetermined pH for the conductive composition and the pre-aged composition.
[0073] The composition before aging is a composition immediately after mixing the conductive polymer (b1), which is a complex of poly(3,4-disubstituted thiophene) and polyanion, the alkaline compound, and water. The conductive polymer (b1) exists in a complex folded dispersion state, and the alkaline compound does not easily penetrate into the inside. Also, since the polyanion forms a salt with the poly(3,4-disubstituted thiophene), it is considered that the configuration gradually changes to a stable configuration after neutralization with the alkaline compound. Therefore, it is considered that the alkaline compound and the polyanion do not form an optimal salt immediately after the addition of the alkaline compound. The pH of the composition before aging is 5 to 10, but pH 6 to 10 is preferable, and pH 7 to 9 is more preferable.
[0074] A conductive composition is obtained by aging the pre-aging composition for 100 hours or more. Aging refers to gradually converging the neutralization reaction between the complex of poly(3,4-disubstituted thiophene) and polyanion and the alkali compound. The aging time is 100 hours or more, preferably 100 to 10,000 hours, and more preferably 200 to 5,000 hours. The aging temperature is preferably 1 to 42°C, and more preferably 4 to 30°C. If the aging time is less than 100 hours or the aging temperature is less than 1°C, the aging becomes insufficient, and the conductive layer (B) formed using the composition tends to be unable to stably exhibit the adhesive strength with the transparent resin film and the adhesive layer. If the aging time exceeds 10,000 hours or the aging temperature exceeds 42°C, the composition may be denatured. Even within the above aging temperature range, aging at a high temperature can shorten the aging time, but there is a concern that the conductive polymer or aqueous resin may aggregate, or foreign matter such as algae or mold may occur. Aging at low temperatures reduces these concerns, but requires a long aging time. It is preferable to carry out the aging in a sealed state to prevent evaporation of the solvent.
[0075] The pH of the conductive composition is lowered by aging compared to the composition before aging, and is pH 4 to 9, preferably pH 5 to 9, and more preferably pH 6.9 to 8.8. The pH of the conductive composition is preferably lower by 0.2 or more, more preferably 0.4 or more, and even more preferably 0.5 or more than the pH of the composition before aging.
[0076] In addition, since the conductive composition has been aged, the change in pH over time is suppressed, and when stored stationary at 15°C for one week, the decrease in pH is preferably 0.15 or less, and more preferably 0.1 or less.
[0077] The pre-ripening composition may further contain an aqueous resin (b2). The aqueous resin (b2) has been described above. When the pre-ripening composition contains the aqueous resin (b2), the amount of the aqueous resin added is preferably 1 to 90% by weight, more preferably 10 to 80% by weight, based on the solid content of the pre-ripening composition.
[0078] The pre-ripened composition may further contain a preservative. Examples of the preservative include quaternary ammonium salts such as benzalkonium chloride, dodecyl dimethyl benzyl aminium chloride, and didecyl dimethyl ammonium chloride, parabens such as methyl paraben and ethyl paraben, isothiazolinone such as methylisothiazolinone and chloromethylisothiazolinone, salicylates, sorbates, benzoates, dehydroacetates, bronopol, and phenoxyethanol. When a preservative is contained, its concentration is preferably 0.0001 to 0.1% by weight based on 100 parts by weight of the solid content in the pre-ripened composition. The closer the pH is to neutral, the more likely algae and mold are to grow, and the smaller the amount of organic solvent added, the more likely algae and mold are to grow. Therefore, it is preferable to adjust the preservative according to the composition of the pre-ripened composition.
[0079] The pre-ripening composition may further contain an organic solvent as a solvent other than water. The organic solvent may be alcohols such as methanol, ethanol, 2-propanol, and 1-propanol; ethylene glycols such as ethylene glycol, diethylene glycol, trimethylene glycol, triethylene glycol, and tetraethylene glycol; glycol ethers such as ethylene glycol monomethyl ether, diethylene glycol monomethyl ether, ethylene glycol diethyl ether, and diethylene glycol dimethyl ether; glycol ether acetates such as ethylene glycol monoethyl ether acetate, diethylene glycol monoethyl ether acetate, and diethylene glycol monobutyl ether acetate; propylene glycols such as propylene glycol, dipropylene glycol, and tripropylene glycol; propylene glycol ethers such as propylene glycol monoethyl ether, dipropylene glycol monomethyl ether, propylene glycol dimethyl ether, and propylene glycol diethyl ether; propylene glycols such as propylene glycol monomethyl ether acetate. Ether acetates; ethers such as diethyl ether, diisopropyl ether, methyl t-butyl ether, and tetrahydrofuran; ketones such as acetone, methyl ethyl ketone, and methyl isobutyl ketone; hydrocarbons such as toluene, xylene (o-, m-, or p-xylene), hexane, and heptane; esters such as butyl acetate; halogens, amide compounds such as acetonitrile, N-methylformamide, N,N-dimethylformamide, γ-butyrolactone, and N-methylpyrrolidone; 1,4-butanediol, 1,5 Examples of the isocyanate include hydroxyl group-containing compounds such as 1,2-pentanediol, 1,6-hexanediol, neopentyl glycol, catechol, cyclohexanediol, cyclohexanedimethanol, glycerin, diethylene glycol monoethyl ether, and propylene glycol monomethyl ether; carbonyl group-containing compounds such as isophorone, propylene carbonate, cyclohexanone, acetylacetone, ethyl acetate, ethyl acetoacetate, methyl orthoacetate, and ethyl orthoformate; and compounds having a sulfo group such as dimethyl sulfoxide.
[0080] Among these, ethylene glycols, which are high boiling point and high polarity solvents, and solvents having an amide group or a sulfo group are preferred because they have the effect of improving the conductivity of the conductive polymer (b1). Furthermore, alcohols such as methanol, ethanol, and 2-propanol, which are low boiling point solvents, are preferred because they have the effect of improving the wettability of the conductive composition and accelerating the drying speed. Both high polarity solvents and low boiling point solvents have the effect of suppressing the generation of foreign matter due to algae and mold during aging. When an organic solvent having a boiling point of 100 degrees or more is contained, it is preferably 1 to 20% by weight in the composition before aging, and when an organic solvent having a boiling point of 100 degrees or less is contained, it is preferably 1 to 70% by weight in the composition before aging. When the content of the organic solvent is high, the conductive polymer tends to easily aggregate, so aging at a low temperature is preferred. By adding water or a mixed solvent of water and an organic solvent, the solid content of the composition before aging is preferably 0.1 to 8.0%, more preferably 1.0 to 6.0%, and even more preferably 1.5 to 4.0%.
[0081] <Adhesive layer (C)> The adhesive layer (C) is laminated on the surface of the conductive layer (B) that is not in contact with the transparent resin film (A). The adhesive layer is formed using an adhesive composition containing an adhesive. The adhesive is not particularly limited and may be any known adhesive. Specifically, examples of the adhesive include (meth)acrylic resins obtained by homopolymerizing or copolymerizing various (meth)acrylic acid ester monomers, ethylene / vinyl acetate copolymer resins, silicone resins such as silicone rubber having a dimethylsiloxane skeleton, polyurethane resins obtained by polyaddition of polyol and polyisocyanate, natural rubber, rubber resins such as styrene-isoprene-styrene block copolymers (SIS block copolymers), styrene-butadiene-styrene block copolymers (SBS block copolymers), styrene-ethylene-butylene-styrene block copolymers (SEBS block copolymers), styrene-butadiene rubber, polybutadiene, polyisoprene, polyisobutylene, butyl rubber, and chloroprene rubber. Among these, (meth)acrylic resins, silicone resins, and polyurethane resins are preferred because they have excellent chemical stability, a high degree of freedom in designing chemical structures, and are easy to adjust adhesive strength. Furthermore, (meth)acrylic resins and polyurethane resins are also preferred because they have excellent transparency.
[0082] In addition to the adhesive, a crosslinking agent, an antistatic agent, a silane coupling agent, a surfactant, a solvent, and the like may be added to the adhesive composition.
[0083] As the crosslinking agent, a polyfunctional metal chelate or an organic crosslinking agent can be used. As the polyfunctional metal chelate, a polyvalent metal is covalently or coordinately bonded to an organic compound, and examples of the polyvalent metal atom include Al, Cr, Zr, Co, Cu, Fe, Ni, V, Zn, In, Ca, Mg, Mn, Y, Ce, Sr, Ba, Mo, La, Sn, and Ti. Examples of the atom in the organic compound that is covalently or coordinately bonded include oxygen atoms, and examples of the organic compound include alkyl esters, alcohol compounds, carboxylic acid compounds, ether compounds, and ketone compounds. Examples of the organic crosslinking agent include isocyanate-based, peroxide-based, epoxy-based, and imine-based organic crosslinking agents. The content of the crosslinking agent in the adhesive composition is not particularly limited, but is preferably 10 parts by weight or less, more preferably 0.01 to 5 parts by weight, and even more preferably 0.02 to 3 parts by weight, relative to 100 parts by weight of the adhesive.
[0084] As the antistatic agent, from the viewpoints of compatibility with the adhesive and transparency, an ionic compound is preferred, and an ionic liquid is particularly preferred. By adding an antistatic agent to the adhesive composition, the conductivity of the entire laminate can be improved. The content of the antistatic agent is preferably 0.01 to 30 parts by weight, more preferably 0.05 to 20 parts by weight, based on 100 parts by weight of the adhesive (e.g., (meth)acrylic resin).
[0085] As a method for laminating the adhesive layer (C) on the conductive layer (B), a conventionally known method can be used, for example, a transfer method in which an adhesive layer formed on a release film is transferred to the conductive layer (B), a coating method in which an adhesive composition containing an adhesive is applied to the conductive layer (B) and crosslinked or heated and dried, etc. Among these, the transfer method is preferred because it can be applied to a transparent resin film (A) with low solvent resistance and the properties of the surface of the conductive layer (B) are easily maintained.
[0086] When the adhesive layer (C) is laminated on the conductive layer (B) by the transfer method, first, the adhesive composition is applied onto a release film, and then dried, irradiated with ultraviolet light, and / or heated to form an adhesive layer on the release film. The adhesive composition can be applied onto the release film by a conventionally known method, and specifically, the method described above for applying the conductive layer-forming composition onto the transparent resin film (A) can be mentioned. The formed adhesive layer is brought into contact with the conductive layer (B), whereby the adhesive layer (C) can be transferred onto the conductive layer (B). The thickness of the adhesive layer (C) is not particularly limited, but is preferably 5 to 100 μm.
[0087] <<Method of manufacturing transparent laminate>> The method for producing the conductive laminate of the present invention includes the steps of applying the conductive layer-forming composition to a transparent resin film (A) and drying the applied conductive layer-forming composition at 100° C. or lower for 5 minutes or less.
[0088] The transparent resin film (A) and the conductive layer-forming composition are as described above. The drying temperature and time are also as described above in relation to the conductive layer-forming composition.
[0089] <<Optical components>> The transparent laminate of the present invention can be suitably used as an optical member. The optical member is not particularly limited as long as it is required to have high adhesion between the conductive layer and the adhesive layer while maintaining electrical conductivity, and examples of the optical member include a polarizing plate, a surface protective film, a transparent conductive film, and an antistatic film.
[0090] The present invention will be described with reference to examples, but the present invention is not limited to the following examples. In the following, "parts" and "%" mean "parts by weight" and "% by weight", respectively, unless otherwise specified.
[0091] 1. Main materials used 1-1. Transparent resin film (A) Acrylic resin (made in Manufacturing Example 1: acrylic) Triacetyl cellulose resin (Fujifilm, Fujitac TJ25UL:TAC) Cycloolefin resin (ZEON Corporation, ZEONOR ZF-14:COP)
[0092] 1-2. Pre-ripening composition and conductive layer-forming composition 1-2-1. Conductive polymer (b1) PEDOT / PSS water dispersion (prepared in Example 2) PEDOT / PSS water dispersion (Heraeus, PH1000) 1-2-2. Water-based resin (b2) Acrylic resin (Nippon Carbide, (product number) Nikasol RX-3020) Polyurethane resin (ADEKA, product number: ADEKA BONTITOR HUX-895) Alkyl-containing polyether resin (Clariant, product number LCN-407) Fluorine-containing polyether resin (manufactured by Neos, product number: Futergent 212M) Polyether modified siloxane resin (BYK-333, manufactured by BYK) Oxazoline resin (manufactured by Nippon Shokubai, product number: Epocross WS700) Polyolefin resin (TOYOBO, product number: HARDLEN EW-5303) 1-2-3.Solvent Ethylene glycol (Tokyo Chemical Industry Co., Ltd.) Diethylene glycol (Tokyo Chemical Industry Co., Ltd.) Dimethyl sulfoxide (DMSO) (Tokyo Chemical Industry Co., Ltd.) N-Methylpyrrolidone (Tokyo Chemical Industry Co., Ltd.) Ethanol (Tokyo Chemical Industry Co., Ltd.)
[0093] 1-3. Adhesive composition (materials of Production Example 3) Acrylic resin (SK Dyne 2094, manufactured by Soken Chemical Industries, Ltd., solid content: 25%) Isocyanate-based crosslinking agent (Takenate D160N, manufactured by Mitsui Chemicals, Inc.) Peroxide-based crosslinking agent (Niper BMT, manufactured by Nippon Oil & Fats Co., Ltd.) · Silane coupling agent (Shin-Etsu Chemical Co., Ltd.: KBM-403)
[0094] 1-4. Pretreatment of transparent resin film (A) 1-4-1. Excimer treatment An excimer light irradiation unit SUS05 manufactured by Ushio Inc. was used.
[0095] 1-4-2. Corona treatment Using a corona treatment device CT-0212 manufactured by Kasuga Electric Co., Ltd., one side of the transparent resin film (A) was subjected to corona discharge treatment (corona discharge electron irradiation dose: 77 W / m 2 / min) was performed.
[0096] 1-4-3. Primer treatment 5.0 g of polyester urethane (manufactured by Daiichi Kogyo Seiyaku, product name: Superflex 210, solid content: 33%), 65.0 g of pure water, and 0.5 g of 1 wt% ammonia water were mixed and stirred. Then, 1.2 g of a crosslinking agent (oxazoline-containing polymer, manufactured by Nippon Shokubai, product name: Epocross WS-700, solid content: 25%) and 0.8 g of colloidal silica (manufactured by Fuso Chemical Industry, Quartron PL-3, solid content: 20 wt%) were added and stirred to obtain a primer composition. The primer composition was applied to the transparent resin film (A) with a wire bar so that the thickness after drying would be 100 nm.
[0097] 2. Evaluation Method 2-1. Adhesive strength between conductive layer (B) and adhesive layer (C) A total of 25 test pieces were used: 5 pieces of non-alkali glass, 5 pieces of non-alkali glass treated with hydrofluoric acid, 5 pieces of non-alkali glass with ITO vapor deposition, 5 pieces of non-alkali glass treated with hydrofluoric acid with ITO vapor deposition, and 5 pieces of PET film with ITO vapor deposition. The adhesive layer of the transparent laminate was attached to each test piece, and after 30 minutes, the test pieces were peeled off. The presence or absence of adhesive residue on the adhesive layer was observed with a CCD to evaluate the initial adhesive strength. The adhesion rate was calculated using the following formula. Adhesion rate (%) = (25-(number of test pieces with adhesive residue)) / 25 x 100 In addition, an adhesive layer was attached to a transparent laminate on each test piece, and after maintaining the test piece at 60°C and 93% Rh for 500 hours, the test piece was peeled off and the adhesive strength after the heat resistance test was evaluated based on whether or not any adhesive residue remained on the adhesive layer.
[0098] 2-2.pH decrease rate The composition obtained by aging the unaged composition, i.e., the conductive composition, was stored at 15° C., and the period until the pH value decreased by 0.2 was measured, and the rate of decrease in pH value per week was calculated.
[0099] 2-3. Stability of pre-ripening composition after long-term storage at 30°C The pre-aged composition was allowed to stand for 1000 hours in a warehouse set at 30° C., after which the liquid state was visually observed to confirm the presence or absence of foreign matter.
[0100] 2-4. Surface resistivity of conductive layer (B) After forming a conductive layer (B) on a transparent resin film (A), measurements were performed using a Mitsubishi Chemical Corporation Hiresta UP (MCP-HT-450, product name) probe UA and an applied voltage of 10V to 500V in accordance with JIS K7194.
[0101] (Production Example 1) Preparation of (meth)acrylic resin substrate Pellets of a mixture (Tg 127°C) of 90 parts by weight of a (meth)acrylic resin having a lactone ring structure (copolymerization monomer weight ratio = methyl methacrylate / methyl 2-(hydroxymethyl)acrylate = 8 / 2, lactone cyclization rate approximately 100%, lactone ring structure content 19.4%, weight average molecular weight 133,000, melt flow rate 6.5 g / 10 min (240°C, 10 kgf), Tg 131°C) and 10 parts by weight of an acrylonitrile-styrene (AS) resin (Toyo AS AS20, manufactured by Toyo Styrene Co., Ltd.) were fed to a twin-screw extruder and melt-extruded into a sheet at approximately 280°C to obtain a (meth)acrylic resin sheet having a lactone ring structure having a thickness of 110 μm. This unstretched sheet was stretched 2.0 times vertically and 2.4 times horizontally at a temperature of 160° C. to obtain a (meth)acrylic resin substrate (thickness: 40 μm, in-plane retardation Δnd: 0.8 nm, thickness direction retardation Rth: 1.5 nm).
[0102] (Production Example 2) Preparation of PEDOT / PSS Water Dispersion Using a 2000ml three-neck glass flask equipped with a cooling tube, 92.3 parts of polystyrene sulfonic acid aqueous solution (Akzo Nobel, VERSA-TL72) and 7.1 parts of 3,4-ethylenedioxythiophene (EDOT) were added to 1000 parts of ion-exchanged water to obtain a mixed solution. While stirring this mixed solution, a solution in which 4.0 parts of ferric sulfate and 14.8 parts of ammonium peroxodisulfate were dissolved in 100 parts of ion-exchanged water was added, and the mixture was stirred at 20°C for 24 hours to perform oxidative polymerization. Next, 15% by weight of a cation exchange resin (Organo Corporation, Amberlite IR120B) and an anion exchange resin (Organo Corporation, Amberlite IRA67) were added, and the mixture was further stirred for 18 hours. The resulting reaction mixture was filtered with a glass filter, and then homogenized 10 times at 100 MPa with a high-pressure homogenizer to obtain a PEDOT / PSS aqueous dispersion with a solid content of 1.3%.
[0103] (Production Example 3) Preparation of adhesive composition The adhesive composition was prepared by mixing 0.1 part by weight of an isocyanate crosslinking agent, 0.3 part by weight of a peroxide crosslinking agent, and 0.2 part by weight of a silane coupling agent with respect to 100 parts by weight of the solid content of the acrylic resin.
[0104] (Examples 1 to 12, Comparative Examples 1 and 2) Preparation and Evaluation of Transparent Laminates A pre-aged composition was prepared by blending the components shown in Table 1. A conductive composition was prepared by aging the obtained pre-aged composition in a blow-molded high-density polyethylene container (manufactured by Sekisui Seiki Kogyo Co., Ltd.) under the temperature and time conditions shown in Table 1. The obtained conductive layer-forming composition was diluted with an aqueous diluent and / or aqueous resin (b2) to prepare a conductive layer-forming composition.
[0105] The conductive layer-forming composition was applied onto a transparent resin film (A) using a wire bar, and heated under the conditions shown in Table 1 to form a conductive layer (B) having a theoretical film thickness shown in Table 1 on the transparent resin film (A). The theoretical film thickness was calculated using the following formula. Theoretical film thickness (nm) = Wire bar No. x Solid content of conductive layer-forming composition x 1000
[0106] The adhesive composition of Production Example 3 was applied to one side of a PET film (Mitsubishi Chemical Corporation, MRF38) treated with a silicone-based release agent, and then dried so that the thickness of the adhesive layer after drying was 20 μm, to form an adhesive layer on the surface of the PET film. This adhesive layer was transferred to a conductive layer (B) formed on a transparent resin film (A) to produce a transparent laminate.
[0107] For each Example and Comparative Example, the pH change of the composition before aging due to aging, the pH change when diluted with the aqueous diluent and / or aqueous resin (b2), the surface resistivity on the conductive layer (B), the adhesive strength, and the stability of the composition before aging after long-term storage at 30° C. were evaluated. The results are shown in Table 1.
[0108] [Table 1]
[0109] In Comparative Example 1, the conductive layer forming composition was produced without adding an alkaline compound to the pre-ripening composition, and as a result, the adhesion rate and conductivity were poor. This is thought to be because the pH was too low, particularly in the drying process during film formation, causing aggregation of the aqueous resin. Furthermore, in Comparative Example 2, the conductive layer forming composition was not added with an aqueous resin, and therefore the adhesion rate was poor. In Comparative Example 2, the preservative was not added, and therefore the generation of foreign matter was observed after long-term storage of the pre-ripening composition. In Examples 1 to 12, the conductive layer (B) had excellent conductivity because an alkaline compound was added to the pre-ripening composition and then ripened. Furthermore, excellent adhesive strength was stably expressed, and high adhesive strength was maintained even after the heat resistance test.
Claims
1. A step of obtaining a mixture containing a conductive polymer (b1), which is a complex of poly(3,4-disubstituted thiophene) and a polyanion, an alkali compound, and water and having a pH of 5 to 10; and A step of aging the mixture at 1 to 42° C. for 100 to 10,000 hours to obtain a conductive composition. A method for producing a conductive composition, comprising the steps of: When the conductive composition is stored at 15° C. for one week, the decrease in pH is 0.15 or less; A manufacturing method in which, when the pH of a conductive composition immediately after production is A and the pH when the conductive composition is left standing at 15°C for one week from immediately after production is B, A and B satisfy the following relationships (i) and (ii): (i) 4≦A≦9 (ii) 4≦B≦9
2. The method for producing a conductive composition according to claim 1 , wherein the alkaline compound is a nitrogen-based compound.
3. Obtaining a conductive composition by the method according to claim 1 or 2; and A step of obtaining a conductive layer-forming composition by adding 100 to 3000 parts by weight of an aqueous diluent relative to 100 parts by weight of the conductive composition, and / or 1 to 1000 parts by weight of an aqueous resin (b2) relative to 100 parts by weight of the solid content of the conductive composition. Including, A method for producing a conductive layer-forming composition.
4. The aqueous resin (b2) is a mixture of three or more resins selected from the group consisting of an acrylic resin, a polyether resin, a polyester resin, a polyurethane resin, a polyolefin resin, a siloxane resin, and an oxazoline resin; The method for producing the conductive layer-forming composition according to claim 3 .
5. A step of obtaining a conductive layer-forming composition by the production method according to claim 3 or 4; A step of applying the conductive layer-forming composition to a transparent resin film (A) made of one or more resins selected from the group consisting of acrylic resins, cycloolefin resins, and cellulose resins; A step of drying the applied conductive layer-forming composition at 40 to 100° C. for 0.3 to 5 minutes to form a conductive layer (B); and A step of forming an adhesive layer (C) on the conductive layer (B). Including, A method for producing a transparent laminate comprising laminating a conductive layer (B) and an adhesive layer (C) in this order on a transparent resin film (A), the method comprising the steps of: The surface resistivity of the conductive layer (B) is 4×10 2 ~1×10 10 Ω / sq. Manufacturing method.
Citation Information
Patent Citations
Antistatic adhesion type optical film and image display
JP2006116809A
Antistatic optical film, antistatic pressure-sensitive adhesive type optical film and image display device
JP2006212783A
Antistatic adhesive optical film and image display device
JP2009009125A
Surface protective film
JP2009107329A
Composition for electroconductive coating, electroconductive thin film, and electroconductive film
JP2012172024A