Modified high nickel positive electrode material and its manufacturing method

The modified high-nickel cathode material with a sulfate topping modification addresses low capacity and safety issues by enhancing structural stability and lithium ion migration, resulting in improved performance in lithium-ion batteries.

JP7560643B2Active Publication Date: 2024-10-02HUNAN SHANSHAN ENERGY TECH CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023500303
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-07-30
Filing Date
2021-06-29
Publication Date
2024-10-02
Estimated Expiration
2041-06-29

AI Technical Summary

Technical Problem

Current high-nickel positive electrode materials exhibit low capacity and poor safety performance, limiting their applications in lithium-ion batteries.

Method used

A modified high-nickel cathode material with a sulfate (SO42-) topping modification, featuring an outward-sloping gradient distribution in secondary particles, enhances structural stability and lithium ion migration, achieved through a manufacturing process involving mixing, sintering, and washing to control SO42- content and distribution.

Benefits of technology

The modified material improves initial capacity and safety performance by stabilizing the structure, increasing lithium ion migration rates, and reducing side reactions, resulting in higher reversible capacity and improved safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007560643000002
    Figure 0007560643000002
  • Figure 0007560643000003
    Figure 0007560643000003
  • Figure 0007560643000004
    Figure 0007560643000004
Patent Text Reader

Abstract

A modified high-nickel positive electrode material is provided. [Solution] The modified high nickel cathode material of the present invention is 2- It is a topping-modified high-nickel cathode material, and SO4 2- The secondary particles of the modified high-nickel positive electrode material exhibit a gradient distribution with an outward rise. The manufacturing method involves mixing the high-nickel positive electrode material, a lithium source, and a sulfate, sintering the mixture to obtain a matrix material, and then washing and drying the matrix material to obtain the modified high-nickel positive electrode material. 2- The secondary particles exhibit an outward-rising gradient distribution, and many OSO bonds and cations attract each other on the inside, which increases the lithium ion migration speed inside the material, greatly improving the initial capacity of the material, and the low SO4 2- has a low content of corresponding inactive lithium material, which reduces the barrier for lithium ion migration between primary particles, improves the lithium ion migration rate between primary particles of the material, and reduces the side reaction between Li2SO4 and the electrolyte, thereby improving the safety performance of the material.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention belongs to the field of lithium ion battery positive electrode materials, and in particular to a modified high nickel positive electrode material and a method for preparing the same. [Background technology]

[0002] Lithium-ion batteries are environmentally friendly storage batteries that can be used in 3C products, power tools, new energy vehicles and other fields. As the main active material, the positive electrode material plays a very important role in lithium-ion batteries. Positive electrode materials can be divided into lithium manganese oxide, lithium nickel oxide, lithium cobalt oxide, high-nickel ternary materials, lithium iron phosphate, etc. As the requirements for energy density of lithium-ion batteries continue to increase, high-nickel ternary positive electrode materials have become one of the research hotspots.

[0003] High nickel ternary positive electrode materials are composed of three elements, Ni, Co and M (M is Al or Mn), and are typical R-3m layer structure materials, in which Ni provides high energy density, Co inhibits cation mixing, and Al / Mn improves material safety and structural stability. In lithium-ion batteries, Li + When the battery is charged, it leaves the positive electrode structure, enters the electrolyte, and enters the negative electrode through the diaphragm. When the battery is discharged, it leaves the negative electrode material, a reverse reaction occurs, and it embeds itself in the active sites of the Li layer in the positive electrode active material.

[0004] However, the current high nickel positive electrode materials generally have the problem of low capacity and poor safety performance, and their applications are limited. Therefore, it is necessary to improve the high nickel positive electrode materials. The patent document with publication number CN109616658A discloses a high nickel positive electrode material co-doped with selenium and sulfate, and its manufacturing method and use, which improves the capacity and multiplication performance of the lithium ion positive electrode material through the synergistic effect of doping selenium and sulfate anions, but this method still has certain limitations, and the electrochemical performance of the positive electrode material still has room for further improvement. Summary of the Invention [Problem to be solved by the invention]

[0005] The technical problem to be solved by the present invention is to overcome the deficiencies and shortcomings mentioned in the background art and provide a modified high-nickel positive electrode material with high capacity and good safety performance, and a method for preparing the same.

[0006] In order to solve the above technical problems, the technical solutions proposed by the present invention are as follows: A modified high-nickel positive electrode material, the modified high-nickel positive electrode material comprising SO4 2- It is a high nickel positive electrode material with topping modification, and SO4 2- exhibits an outwardly rising gradient distribution in the secondary particles of the modified high-nickel positive electrode material.

[0007] Regarding the modified high-nickel positive electrode material, preferably, the secondary particles of the modified high-nickel positive electrode material are spherical, and in a spherical region having a distance L<0.6R from the center of the spherical secondary particle as the starting point to the center, SO4 2- The content of SO4 in the total secondary particles 2- The content of SO4 is 60-80% in the annular region with a distance of 0.6R≦L≦R to the center of the ball. 2- The content of SO4 in the total secondary particles 2- The content of is 20 to 40%, and R is the radius of the secondary particle.

[0008] Regarding the above modified high nickel positive electrode material, preferably, the chemical formula of the modified high nickel positive electrode material is Li x Ni y Co (1-y-z) M z S γ O2, 0.98≦x≦1.1, 0.8≦y≦1, 0≦z≦0.2, 0.003≦γ≦0.015, and M is Al or Mn.

[0009] Regarding the above modified high nickel positive electrode material, preferably, the cell size of the modified high nickel positive electrode material is 150-200 nm.

[0010] As a general inventive concept, the present invention further provides a method for producing the modified high nickel positive electrode material, (1) mixing a high-nickel positive electrode material precursor, a lithium source, and a sulfate salt, and sintering the resulting mixture to obtain a matrix material; (2) washing and drying the matrix material to obtain a modified high-nickel cathode material.

[0011] In the above-mentioned manufacturing method, preferably, in step (1), the amount of sulfate added is SO4 2- When calculated, SO4 2- The amount of added is 0.5-2.7% of the total mass of the mixture.

[0012] In the above-mentioned production method, preferably, in step (1), the sulfate is one or more of nickel sulfate, cobalt sulfate, aluminum sulfate, lithium sulfate, sodium sulfate, and ammonium sulfate.

[0013] In the above-mentioned manufacturing method, preferably, in step (1), the sintering temperature is 600 to 900° C. and the sintering time is 3 to 20 hours.

[0014] In the above-mentioned manufacturing method, preferably, in the step (2), the mass ratio of the matrix material to deionized water during the washing operation is (1:0.5) to (1:5), and the washing time is 20 to 40 minutes.

[0015] Compared with the prior art, the advantages of the present invention are as follows:

[0016] (1) SO4 of the present invention 2- For topping-modified high nickel positive electrode materials, SO4 2- The secondary particles have an outward-rising gradient distribution, and many OSO bonds and cations on the inside attract each other, which plays a role in stabilizing the structure. This improves the lithium ion migration speed inside the material, greatly improves the initial capacity of the material, and has a low SO4 2-The corresponding inactive lithium material has a low content, which reduces the barrier for lithium ion migration between the primary particles, improves the lithium ion migration rate between the primary particles of the material, and further improves the initial capacity, while reducing the side reaction between Li2SO4 and the electrolyte, thereby improving the safety performance of the material.

[0017] (2) In the manufacturing method of the present invention, SO4 2- The material topped with SO4 is washed and the surface of the secondary particles is cleaned. 2- By reducing the content of SO4 in secondary particles, 2- The distribution of Li forms an outward-facing structure, and the internal OSO bonds and cations attract each other, stabilizing the structure. + and SO4 2- The lithium ions combine with each other to form the fast ion conductor lithium sulfate, which is distributed throughout the material, increasing the lithium ion migration speed within the material and significantly improving the initial capacity.

[0018] (3) In the manufacturing method of the present invention, after the material is washed, the lithium sulfate on the surface of the secondary particles is washed away, the specific surface area is increased, the contact sites between the material and the electrolyte are increased, the migration of lithium ions is accelerated, the initial capacity is further improved, and after washing, the surface SO4 2- The content is significantly reduced, and SO4 2- It forms a structure with an outward rise in content, and combines good capacity and safety performance.

[0019] (4) The modified high-nickel positive electrode material of the present invention has a large amount of SO4 2- The topping reduces the cell size and reduces the site occupancy of lithium ions, increasing the number of lithium vacancies, lowering the barrier for lithium ion migration and making it easier for lithium ions to be inserted / extracted from the structure, thereby increasing the reversible capacity of the material. [Brief description of the drawings]

[0020] [Figure 1]FIG. 2 is an XRD diagram of the intermediate product obtained after primary sintering of the modified high-nickel cathode material in Example 3 and Comparative Example 1. [Diagram 2] 1 is a SEM image of a cross section of an intermediate product obtained after primary sintering of the modified high-nickel cathode material in Example 3. [Diagram 3] 1 is a SEM image of the middle cross section of an intermediate product secondary particle obtained after primary sintering of the modified high-nickel cathode material in Example 3. [Figure 4] FIG. 1 is an EDS point scan of the middle of a cross section of an intermediate product secondary particle obtained after primary sintering of the modified high-nickel positive electrode material in Example 3. [Diagram 5] 1 is a SEM image of a cross-sectional edge of an intermediate product secondary particle obtained after primary sintering of the modified high-nickel cathode material in Example 3. [Figure 6] FIG. 1 is an EDS point scan of a cross-sectional edge of an intermediate product secondary particle obtained after primary sintering of the modified high-nickel positive electrode material in Example 3. [Figure 7] FIG. 11 is an EDS line scan diagram of a cross section of a product secondary particle obtained by washing and drying the modified high-nickel positive electrode material in Example 3. [Figure 8] 1 is a SEM image of a cross section of an intermediate product obtained after primary sintering of the modified high-nickel cathode material in Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] In order to facilitate understanding of the present invention, the present invention will be described more fully and in detail below with reference to the drawings and preferred embodiments in the specification, but the scope of protection of the present invention is not limited to the following specific embodiments. Unless otherwise defined, all technical terms used below have the same meaning as commonly understood by those skilled in the art. The technical terms used in this specification are only for the purpose of describing specific embodiments, and are not intended to limit the scope of protection of the present invention.

[0022] Unless otherwise stated, the various raw materials, reagents, instruments and devices, etc. used in the present invention can all be commercially purchased or manufactured by conventional methods.

[0023] Example 1: The modified high nickel positive electrode material of the present invention is 2- The secondary particles of the modified high-nickel positive electrode material are spherical, and the SO4 2- The secondary particles show an outward-rising gradient distribution, and in the spherical region with a distance L<0.6R from the center of the spherical secondary particle, SO4 2- The content of SO4 in the total secondary particles 2- The content of SO4 in the modified high nickel positive electrode material is 65-70%. 2- The content of Li is 0.1%, and the chemical composition of the modified high nickel positive electrode material is Li 1.03 Ni 0.88 Co 0.1 Al 0.02 S 0.003 It's O2.

[0024] The method for producing the modified high nickel cathode material of this embodiment is as follows: (1) Nickel-cobalt-aluminum hydroxide, lithium hydroxide, and lithium sulfate were mixed (the molar ratio of nickel, cobalt, and aluminum to lithium in the mixture was 1:1.04, and the mixture was treated with SO4 2- the content of is 0.5%), and placing the mixture in an oxygen atmosphere furnace and sintering it at 760° C. for 15 hours; (2) disaggregating and sieving the sintered material to obtain a high nickel lithium cobalt aluminate matrix material; (3) Washing the obtained matrix material with deionized water, the matrix material and deionized water are washed in a mass ratio of 1:1.5 for 30 minutes, filtered, and the filter cake is dried in a vacuum oven for 12 hours. The dried product is sieved to obtain the final product, wherein the SO4 2- and wherein the content of is 0.1%.

[0025] The obtained positive electrode material was manufactured into a button battery with a lithium sheet as the negative electrode, and evaluation measurements were performed. The battery was charged and discharged at 0.1C at room temperature in a voltage range of 3.0 to 4.3V. Table 1 shows the characteristics of the cell size, S content before and after cleaning, residual lithium, and initial capacity of the material.

[0026] Example 2: The modified high nickel positive electrode material of the present invention is 2- The topping-modified high-nickel positive electrode material is composed of secondary particles, which are spherical in shape and can be used for SO4 2- The secondary particles show an outward-rising gradient distribution, and in the spherical region with a distance L<0.6R from the center of the spherical secondary particle, SO4 2- The content of SO4 in the total secondary particles 2- The content of SO4 in the modified high nickel positive electrode material accounts for 70-75%. 2- The content of Li is 0.15%, and the chemical composition of the modified high nickel positive electrode material is Li 1.03 Ni 0.88 Co 0.1 Al 0.02 S 0.0045 It's O2.

[0027] The method for producing the modified high nickel cathode material of this embodiment is as follows: (1) Nickel-cobalt-aluminum hydroxide, lithium hydroxide, and lithium sulfate were mixed (the molar ratio of nickel, cobalt, and aluminum to lithium in the mixture was 1:1.04, and the mixture was treated with SO4 2- the content of is 1.1%), and placing the mixture in an oxygen atmosphere furnace and sintering it at 760° C. for 15 hours; (2) disaggregating and sieving the sintered material to obtain a high nickel lithium cobalt aluminate matrix material; (3) washing the obtained matrix material with deionized water, and washing the matrix material with the aqueous solution in a mass ratio of 1:1.5 for 30 minutes, filtering, and drying the filter cake in a vacuum oven for 12 hours, and sieving the dried product to obtain the final product, the modified high-nickel positive electrode material, wherein the SO4 2- The content of is 0.15%.

[0028] The obtained positive electrode material was manufactured into a button battery with a lithium sheet as the negative electrode, and evaluation measurements were performed. The battery was charged and discharged at 0.1C at room temperature in a voltage range of 3.0 to 4.3V. Table 1 shows the characteristics of the cell size, S content before and after cleaning, residual lithium, and initial capacity of the material.

[0029] Example 3: The modified high nickel positive electrode material of the present invention is 2- The topping-modified high-nickel positive electrode material is composed of secondary particles, which are spherical in shape and can be used for SO4 2- The secondary particles show an outward-rising gradient distribution, and in the spherical region with a distance L<0.6R from the center of the spherical secondary particle, SO4 2- The content of SO4 in the total secondary particles 2- The content of SO4 in the modified high nickel positive electrode material accounts for 75-80%. 2- The content of Li is 0.4%, and the chemical composition of the modified high nickel positive electrode material is Li 1.03 Ni 0.88 Co 0.1 Al 0.02 S 0.012 It's O2.

[0030] The method for producing the modified high nickel cathode material of this embodiment is as follows: (1) Nickel-cobalt-aluminum hydroxide, lithium hydroxide, and lithium sulfate were mixed (the molar ratio of nickel, cobalt, and aluminum to lithium in the mixture was 1:1.04, and SO4 2-the content is 2.7%), placing the mixture in an oxygen atmosphere furnace and sintering it at 760° C. for 15 hours; (2) The sintered material is disaggregated and sieved to obtain a high-nickel lithium-nickel-cobalt-aluminum oxide matrix material. The high-nickel matrix material is measured by a D8 ADVANCE X-ray diffractometer to obtain curve 2 in Figure 1, and Li2SO4 diffraction peaks are found at the left and right of the diffraction angle of 22.15 degrees. The high-nickel matrix material is photographed and characterized by EDS using a SEM to obtain Figures 2, 3, 4, 5, and 6, and SO4 is shown in Figure 2. 2- After topping, the primary particles are small and have many pores. Figures 3, 4, 5, and 6 show that the secondary particles all contain a certain amount of SO4 2- to exist; (3) Washing the obtained matrix material with deionized water, the matrix material and deionized water are washed in a mass ratio of 1:1.5 for 30 minutes, filtered, the filter cake is dried in a vacuum oven for 12 hours, and the dried product is sieved to obtain the final product, the modified high-nickel positive electrode material, wherein the SO4 2- and wherein the content of is 0.4%.

[0031] The obtained modified high-nickel cathode material was characterized by EDS and Fig. 7 shows the material after cleaning and drying. The secondary particles of SO4 2- The distribution of SO4 on the surface is outwardly upward, but most of the SO4 on the surface is removed by cleaning. 2- It is stated that SO4 is washed away in a spherical area with a distance L<0.6R to the center of the secondary particle. 2- The content of SO4 in the total secondary particles 2- It accounts for approximately 60-80% of the content.

[0032] The obtained modified positive electrode material was manufactured into a button battery with a lithium sheet as the negative electrode, and evaluation measurements were performed. The battery was charged and discharged at 0.1C at room temperature and in a voltage range of 3.0 to 4.3V. Table 1 shows the cell size, S content before and after cleaning, residual lithium, and initial capacity of the material.

[0033] Example 4: The modified high nickel positive electrode material of the present invention is 2- The topping-modified high-nickel positive electrode material is composed of secondary particles, which are spherical in shape and can be used for SO4 2- The secondary particles show an outward-rising gradient distribution, and in the spherical region with a distance L<0.6R from the center of the spherical secondary particle, SO4 2- The content of SO4 in the total secondary particles 2- The content of SO4 in the modified high nickel positive electrode material accounts for 70-75%. 2- The content of Li is 0.15%, and the chemical composition of the modified high nickel positive electrode material is Li 1.03 Ni 0.88 Co 0.1 Al 0.02 S 0.0045 It's O2.

[0034] The method for producing the modified high nickel cathode material of this embodiment is as follows: (1) Nickel-cobalt-aluminum hydroxide, lithium hydroxide, and lithium sulfate were mixed (the molar ratio of nickel, cobalt, and aluminum to lithium was 1:1.04, and SO4 2- the content of is 1.1%), and placing the mixture in an oxygen atmosphere furnace and sintering it at 760° C. for 15 hours; (2) disaggregating and sieving the sintered material to obtain a high nickel lithium cobalt aluminate matrix material; (3) Washing the obtained matrix material with deionized water, the matrix material and the aqueous solution are washed in a mass ratio of 1:1.5, washed for 30 minutes, filtered, the filter cake is dried in a vacuum oven for 12 hours, and the dried product is sieved to obtain the final product, wherein the SO42- The content of is 0.15%.

[0035] The obtained positive electrode material was manufactured into a button battery with a lithium sheet as the negative electrode, and evaluation measurements were performed. The battery was charged and discharged at 0.1C at room temperature in a voltage range of 3.0 to 4.3V. Table 1 shows the characteristics of the cell size, S content before and after cleaning, residual lithium, and initial capacity of the material.

[0036] Comparative Example 1: The method for producing the high nickel positive electrode material of this comparative example is as follows: (1) mixing nickel-cobalt-aluminum hydroxide and lithium hydroxide (the molar ratio of the total number of moles of nickel, cobalt and aluminum to lithium is 1:1.04), placing the mixture in an oxygen atmosphere furnace, and sintering it at 760°C for 15 hours; (2) The sintered material is disaggregated and sieved to obtain high-nickel lithium-cobalt aluminum oxide matrix material Li 1.03 Ni 0.88 Co 0.1 Al 0.02 O2, the matrix material is measured using a D8 ADVANCE X-ray diffractometer to obtain curve 1 in FIG. 1, and no other peaks appear in addition to the characteristic peaks of NCA; (3) washing the obtained matrix material with deionized water, and washing the matrix material with the aqueous solution in a mass ratio of 1:1.5 for 30 minutes, filtering, and drying the filter cake in a vacuum oven for 12 hours, and sieving the dried product to obtain the final product of high nickel positive electrode material, wherein the SO4 2- The content of SO4 is 0.06% (due to limitations in the precursor manufacturing process, the product contains a small amount of SO4 2- and

[0037] The resulting high nickel positive electrode material was characterized using a scanning electron microscope to obtain FIG. 8, which shows that the primary particles are larger than those in FIG. 2 and that there is less pore distribution.

[0038] The obtained positive electrode material was manufactured into a button battery with a lithium sheet as the negative electrode, and evaluation measurements were performed. The battery was charged and discharged at 0.1C at room temperature in a voltage range of 3.0 to 4.3V. Table 1 shows the characteristics of the cell size, S content before and after cleaning, residual lithium, and initial capacity of the material.

[0039] Comparative Example 2: The method for producing the modified high nickel positive electrode material of this comparative example is as follows: (1) Nickel-cobalt-aluminum hydroxide, lithium hydroxide, and lithium sulfate were mixed (the molar ratio of nickel, cobalt, and aluminum to lithium was 1:1.04, and SO4 2- the content of is 4.2%), and placing the mixture in an oxygen atmosphere furnace and sintering it at 760° C. for 15 hours; (2) The sintered material is disaggregated and sieved to obtain the high-nickel lithium-cobalt-aluminate matrix material Li 1.03 Ni 0.88 Co 0.1 Al 0.02 obtaining O2; (3) Washing the obtained matrix material with deionized water, the matrix material and the aqueous solution are washed in a mass ratio of 1:1.5, washed for 30 minutes, filtered, the filter cake is dried in a vacuum oven for 12 hours, and the dried product is sieved to obtain the final product, wherein the SO4 2- The content of is 0.5%.

[0040] The obtained positive electrode material was manufactured into a button battery with a lithium sheet as the negative electrode, and evaluation measurements were performed. The battery was charged and discharged at 0.1C at room temperature in a voltage range of 3.0 to 4.3V. Table 1 shows the characteristics of the cell size, S content before and after cleaning, residual lithium, and initial capacity of the material.

[0041] Comparative Example 3: The method for producing the modified high nickel positive electrode material of this comparative example is as follows: (1) mixing nickel-cobalt-aluminum hydroxide and lithium hydroxide (the mole ratio of nickel, cobalt and aluminum to lithium is 1:1.04), placing the mixture in an oxygen atmosphere furnace, and sintering at 710°C for 15 hours; (2) The sintered material is disaggregated and sieved to obtain the high-nickel lithium-cobalt-aluminate matrix material Li 1.03 Ni 0.88 Co 0.1 Al 0.02 obtaining O2; (3) washing the obtained matrix material with deionized water, the matrix material and deionized water are washed in a mass ratio of 1:1.5, washed for 30 minutes, filtered, the filter cake is dried in a vacuum oven for 12 hours, and the dried product is sieved to obtain the final product, wherein the SO4 2- and wherein the content of is 0.06%.

[0042] The obtained positive electrode material was manufactured into a button battery with a lithium sheet as the negative electrode, and evaluation measurements were performed. The battery was charged and discharged at 0.1C at room temperature in a voltage range of 3.0 to 4.3V. Table 1 shows the characteristics of the cell size, S content before and after cleaning, residual lithium, and initial capacity of the material.

[0043] Comparative Example 4: The method for producing the modified high nickel positive electrode material of this comparative example is as follows: (1) Nickel-cobalt-aluminum hydroxide, lithium hydroxide, and lithium sulfate were mixed (the molar ratio of nickel, cobalt, and aluminum to lithium in the mixture was 1:1.04, and the mixture was treated with SO4 2- the content is 0.15%), and placing the mixture in an oxygen atmosphere furnace and sintering it at 740° C. for 15 hours; (2) disintegrating and sieving the sintered material to obtain a final product of high nickel lithium cobalt aluminum oxide material, and removing SO4 2-The final product produced has not been treated with a cleaning step and therefore contains, in the range of secondary particles, SO4 2- appears to be uniformly distributed.

[0044] The obtained modified high-nickel positive electrode material was manufactured into a button battery with a lithium sheet as the negative electrode, and evaluation measurements were performed. The battery was charged and discharged at 0.1C at room temperature and in a voltage range of 3.0 to 4.3V. The cell size, S content before and after cleaning, residual lithium, and initial capacity of the material were shown in Table 1.

[0045] Table 1. Performance of modified high-nickel positive electrode materials manufactured in each Example and Comparative Example JPEG0007560643000001.jpg175170

[0046] As can be seen from Table 1, before sintering, SO4 2- The amount of SO4 added is controlled within the range of 0.5 to 2.7%. After washing and drying, 2- The content is in the range of 0.1-0.4%, the cell size of the modified high nickel positive electrode material is 150-200nm, and the initial capacity of the modified high nickel positive electrode material is more than 215mAh / g, which is high capacity.

[0047] As can be seen from Example 1 and Comparative Examples 1 and 2, the primary sintering SO4 2- If the amount of added is too low, the improvement of the capacity before and after cleaning is not significant, and the initial capacity of the final product is lower than the 5 mAh / g or more of the technical solution of the present invention. 2- If the amount of added is too high, the cell size will be too small, which will affect the normal capacity.

[0048] As can be seen from Comparative Example 3 and Example 1, when the particle sizes of the obtained positive electrode material are relatively close, the SO4 2- The topping material is SO4 2- The capacity after washing is improved and the initial capacity of the final product is higher than that of untopped materials.

[0049] As can be seen from Comparative Example 4 and Example 3, the particle sizes are relatively close, and the final product SO4 2- If the content is consistent, SO4 2- The electrochemical performance of the positive electrode material with the outward distribution of SO4 2- This has a distinct advantage over positive electrode materials in which the isotopes are uniformly distributed, as manifested primarily in a higher initial capacity.

Claims

1. SO 4 2- A high nickel positive electrode material with topping modification, SO 4 2- However, the secondary particles of the modified high nickel positive electrode material have an outwardly rising gradient distribution; the secondary particles of the modified high-nickel positive electrode material are spherical, and in a spherical region having a distance L<0.6R from the center of the spherical secondary particle as the starting point to the center, the content of SO 4 2- accounts for 60 to 80% of the content of SO 4 2- in the entire secondary particle, and in an annular region having a distance of 0.6R≦L≦R from the center to the center, the content of SO 4 2- accounts for 20 to 40% of the content of SO 4 2- in the entire secondary particle; 1. A modified high nickel positive electrode material comprising:

2. The chemical formula of the modified high nickel positive electrode material is Li x Ni y Co (1-y-z) M z S γ O 2 0.98≦x≦1.1, 0.8≦y≦1, 0≦z≦0.2, 0.003≦γ≦0.015, and M is Al or Mn; 2. The modified high nickel positive electrode material of claim 1.

3. The cell size of the modified high nickel cathode material is 150-200 nm; 3. The modified high nickel positive electrode material of claim 1 or 2.

4. (1) mixing and sintering a high nickel positive electrode material precursor, a lithium source, and a sulfate to obtain a matrix material; (2) washing and drying the matrix material to obtain a modified high-nickel cathode material; A method for producing the modified high nickel positive electrode material according to any one of claims 1 to 3.

5. In step (1), the amount of sulfate added is SO 4 2- When calculated, SO 4 2- The amount of addition accounts for 0.5% to 2.7% of the total mass of the mixture; The method according to claim 4 .

6. In step (1), the sulfate is one or more of nickel sulfate, cobalt sulfate, aluminum sulfate, lithium sulfate, sodium sulfate, and ammonium sulfate; The method according to claim 4 .

7. In step (1), the sintering temperature is 600 to 900° C. and the time is 3 to 20 hours; The method according to any one of claims 4 to 6.

8. In step (2), during the washing operation, the mass ratio of the matrix material to deionized water is (1:0.5) to (1:5), and the washing time is 20 to 40 minutes; The method according to any one of claims 4 to 6.

Citation Information

Patent Citations

  • Lithium secondary battery

    JP2007165301A

  • Positive electrode active material for nonaqueous electrolyte secondary batteries, manufacturing method thereof, and nonaqueous electrolyte secondary battery

    JP2015026455A

  • Positive electrode active material for lithium ion battery, positive electrode for lithium ion battery, and lithium ion battery

    JP2016184472A

  • Positive electrode active material for nonaqueous electrolyte secondary battery, manufacturing method thereof, and nonaqueous electrolyte secondary battery

    JP2017084628A