Lithium-ion battery positive electrode active material and its manufacturing method
The lithium ion battery positive electrode active material with sulfate salts and cobalt hydroxide coating stabilizes the interface with the electrolyte, improving cycle life and efficiency by forming a protective film and enhancing structural stability.
Patent Information
- Application Number
- JP2023500307
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-07-07
- Filing Date
- 2021-06-29
- Publication Date
- 2024-10-02
- Estimated Expiration
- 2041-06-29
AI Technical Summary
Existing lithium ion battery positive electrode active materials face challenges in achieving high structural stability and cycle life due to side reactions with electrolytes, and existing modifications like metal oxides and fluorides do not meet performance requirements, while sulfate ion introduction complicates manufacturing and increases costs.
A lithium ion battery positive electrode active material comprising a matrix with a sulfur compound in the form of sulfate salts, which forms alkyl sulfonate structures to stabilize the interface with the electrolyte, and optionally coated with cobalt hydroxide to enhance structural stability and electrochemical performance.
The sulfate salts improve the stability and cycle life of the battery by forming a protective film, while the cobalt hydroxide coating enhances efficiency and capacity, with a balanced S content of 0.06-0.13% optimizing performance without inhibiting lithium ion transfer.
Smart Images

Figure 0007560644000002 
Figure 0007560644000003 
Figure 0007560644000004
Abstract
Description
[Technical field]
[0001] The present invention belongs to the field of lithium ion battery positive electrode materials, and in particular to a lithium ion battery positive electrode active material and a method for preparing the same. [Background technology]
[0002] Lithium metal compounds, especially nickel-based lithium metal layered oxides, are common positive electrode active materials in lithium-ion batteries. During the charge and discharge process of lithium batteries, the positive electrode active material will undergo various side reactions with the electrolyte, which will cause the structure of the positive electrode material to be destroyed quickly. In order to improve the structural stability of the positive electrode material and mitigate the side reactions between the material and the electrolyte, it is common to top or coat the positive electrode material with metal oxides, metal fluorides, or metal phosphates, which are mainly intended to enhance the structural stability of the layered material or prevent the active material from directly contacting the electrolyte, thereby avoiding the occurrence of side reactions.
[0003] Although the above technical means can improve the performance of the positive electrode material to a certain extent, they still cannot meet the higher performance requirements of lithium batteries. In addition to the above-mentioned types of materials, sulfates can be introduced into lithium metal compounds to achieve certain effects in improving the performance of positive electrode materials. Patent US7645542B2 discloses a positive electrode active material containing sulfate ions, which reacts with the remaining lithium (lithium carbonate and lithium hydroxide) to form lithium sulfate, and improves the capacity of the active material by consuming the remaining lithium, but this technology has a high requirement for the content of sulfate ions, i.e., more than 0.4%, otherwise the sulfate ions are not enough to consume the remaining lithium, and the initial capacity cannot be improved; at the same time, the added sulfate is not lithium sulfate, otherwise it will react with the remaining lithium and cannot achieve the purpose of improving performance. Patent CN109742347A discloses a high nickel positive electrode material with a composite coating layer, in which a lithium metal layer structure and lithium phosphate or lithium sulfate are composite coating layers. The lithium sulfate coating improves the multiplication performance as a fast ion conductor, but it requires precipitation of phosphate or sulfate in the liquid phase and washing with an organic solvent, which makes the process complicated and the manufacturing cost high. Summary of the Invention [Problem to be solved by the invention]
[0004] The technical problem to be solved by the present invention is to overcome the shortages and deficiencies mentioned in the background art above, and to provide a positive electrode active material for a lithium ion battery and a method for preparing the same.
[0005] In order to solve the above technical problems, the technical solutions proposed by the present invention are as follows:
[0006] A lithium ion battery positive electrode active material includes a positive electrode active material matrix and a sulfur compound, in which the mass of S element accounts for 0.06 to 0.40% of the total mass of the lithium ion battery positive electrode active material, and the sulfur compound exists in the form of a sulfate.
[0007] The S element exists in the form of sulfate in the positive electrode active material, and the electron affinity of sulfate ion is high, and it can combine with the transition metal of the active material to stabilize the surface and interface. During the charge and discharge process of the lithium battery, the sulfate in the positive electrode active material reacts with the electrolyte to form an alkylsulfonate structure, and this functional group structure enhances the stability of the interface between the positive electrode active material and the electrolyte, prevents the electrolyte from destroying the surface of the positive electrode material, and acts as a protective film for the positive electrode active material to extend the cycle life of the lithium battery. If the content of the S element is too low, it is difficult to form sufficient alkylsulfonate functional groups, and it cannot play a role in enhancing the interface stability of the active material and the electrolyte; if the content of the S element is too high, the protective film formed is too thick, which inhibits the transfer of lithium ions and reduces the battery capacity.
[0008] The applicant of the present invention, through exploratory research and repeated testing and verification, found that when the content of S element reaches 0.06%, sufficient alkylsulfonate functional groups can be formed, and the stability of the interface between the active material and the electrolyte can be significantly improved; at the same time, when the content of S does not exceed 0.13%, the thickness of the formed protective film has little inhibition of lithium ion transfer, and the decrease in battery capacity is not significant. However, after the content of S element exceeds 0.13%, the thickness of the formed alkylsulfonate protective layer increases with the increase in the content of S, but the improvement in cycle performance is not significant, and at the same time, the deintercalation of lithium ions is severely hindered, causing the capacity decrease to be rapid. Therefore, in order to achieve both good cycle performance and capacity, the mass ratio of S element in the sulfur compound to the total mass of the positive electrode active material of the lithium ion battery is preferably 0.06 to 0.13%.
[0009] For the above lithium ion battery positive electrode active material, preferably, the sulfur compound includes one or more of lithium sulfate, cobalt sulfate, manganese sulfate, aluminum sulfate, magnesium sulfate, titanium sulfate, zirconium sulfate, sodium sulfate, sodium metabisulfite, and ammonium sulfate. Different types of sulfates have different effects on the lithium metal compound, and the introduction of sulfate ions enhances the stability of the positive electrode active material in the electrolyte, but the separately introduced metals have different additional effects on the lithium metal compound. For example, the addition of cobalt sulfate, manganese sulfate, and the introduction of Co and Mn enhance the structural stability of the lithium metal compound, the addition of aluminum sulfate, and the introduction of Al enhance the structural and thermal stability of the positive electrode active material, but reduce the capacity, and the addition of sodium sulfate and sodium metabisulfite can replace the Li site, expand the lattice volume, and reduce the transfer resistance of lithium ions, but reduce the capacity. The addition of lithium sulfate can significantly improve the cycle performance, initial efficiency and discharge capacity. The presence of sulfate ions can improve the cycle performance, and the introduction of Li can replenish the missing Li in the lattice, playing the role of a lithium replenisher, so the initial efficiency and discharge capacity are also improved.
[0010] For the above lithium ion battery positive electrode active material, preferably, the sulfur compound is mainly coated on the surface of the positive electrode active material matrix.
[0011] In the above-mentioned lithium ion battery positive electrode active material, preferably, the surface of the positive electrode active material matrix is also coated with cobalt hydroxide, the amount of the cobalt hydroxide coating is calculated in terms of cobalt element, and the mass of the coated cobalt element accounts for 0.1-1.5% of the total mass of the lithium ion battery positive electrode active material. The coated cobalt hydroxide reacts with the remaining lithium to form a lithium cobalt oxide structure, which can enhance the surface structure stability and improve the efficiency and multiplication performance, and has a complementary effect with the sulfate material coated on the surface, co-enhancing the electrochemical performance of the active material.
[0012] For the above lithium ion battery positive electrode active material, preferably, the sulfur compound is mainly topped on the positive electrode active material matrix.
[0013] For the above lithium ion battery positive electrode active material, preferably, the chemical formula of the positive electrode active material matrix is Li x Ni y M (1-y) O 2 where M is one or more of Co, Mn, Al, Mg, Ti, and Zr, and 0.95≦x≦1.05 and 0.50≦y≦1.
[0014] As a general inventive idea, the present invention further provides a method for preparing the above-mentioned lithium ion battery positive electrode active material, comprising: mixing a positive electrode active material matrix and a sulfur compound in a stoichiometric ratio, and calcining the mixture to obtain a lithium ion positive electrode active material, wherein the calcination temperature is 300-750°C, and the calcination time is 3-15 hours.
[0015] The sulfate may be introduced in the form of coating, i.e., the sulfate and the positive electrode active material matrix are co-sintered, in which case the sulfate is uniformly distributed on the interface and surface of the active material, which can improve the chemical stability of the active material in the electrolyte, and can also improve the thermal stability as well as the cycling performance during the electrochemical reaction process.
[0016] For the above manufacturing method, preferably cobalt hydroxide is also added during the mixing process.
[0017] As a general inventive idea, the present invention further provides a method for preparing the above-mentioned lithium ion battery positive electrode active material, comprising: mixing a positive electrode active material precursor, a lithium source and a sulfur compound in a stoichiometric ratio, and calcining the mixture to obtain a lithium ion positive electrode active material, wherein the calcination temperature is 650-950°C, and the calcination time is 6-18 hours.
[0018] In the above method, the lithium source is preferably one or more of lithium hydroxide, lithium carbonate, and lithium sulfate. When the lithium source is lithium sulfate, the lithium source also provides sulfate ions.
[0019] Sulfuric acid may be introduced in the form of topping, that is, the positive electrode active material precursor, the lithium compound, and the sulfate are co-sintered to form a lithium metal compound containing sulfate, and the sulfate can fill the incomplete bond between the transition metal and oxygen and play a role in stabilizing the surface energy. The morphology and size of the primary particles of the active material topped with the sulfate are changed, and in addition to the cycle performance during the electrochemical reaction process, the capacity and efficiency can also be improved. At the same time, the positive electrode active material precursor itself may contain S and have the effect of topping.
[0020] Compared with the prior art, the advantages of the present invention are as follows:
[0021] (1) In the lithium ion battery positive electrode active material of the present invention, sulfate is distributed in the lithium metal compound matrix. During the charge and discharge process of the lithium battery, the sulfate in the positive electrode active material reacts with the electrolyte to form an alkylsulfonate structure. This functional group structure enhances the interface stability between the positive electrode active material and the electrolyte, prevents the electrolyte from damaging the surface of the positive electrode material, and serves as a protective film for the positive electrode active material, thereby improving the cycle performance of the positive electrode material and extending the cycle life of the lithium battery.
[0022] (2) For the lithium ion battery positive electrode active material of the present invention, different types of sulfur compounds can be introduced to meet different types of requirements, such as capacity, multiplication performance, safety, etc. The sulfate material provided by the present invention has universality for improving the cycle performance of different types of lithium metal compounds, and at the same time, different metal sulfates can be selected to meet various performance requirements.
[0023] (3) The present invention simultaneously coats cobalt hydroxide and sulfate on the surface of the positive electrode active material matrix, and the coated cobalt hydroxide reacts with the remaining lithium to form a lithium-cobalt oxygen structure, enhancing the surface structure stability, improving the efficiency and multiplication performance, and playing a complementary effect with the sulfate material to improve the cycle performance, thereby co-enhancing the electrochemical performance of the active material.
[0024] (4) The method steps for preparing the lithium battery positive electrode active material of the present invention are simple and easy to operate, the operation is convenient, there are many types of sulfates available, and the cost is low. [Brief description of the drawings]
[0025] [Figure 1] 1 is an SEM image of the positive electrode active material prepared in Example 3. [Diagram 2] 1 is a SEM image of the lithium metal compound employed in Comparative Example 1. [Diagram 3] 1 is an SEM image of a positive electrode active material prepared in Comparative Example 2. [Figure 4] FIG. 2 is a comparison diagram of the battery capacities made of the positive electrode active materials of each of the Examples and Comparative Examples. [Diagram 5] FIG. 2 is a comparison diagram of cycle capacity retention rates at 25° C. of batteries made of the positive electrode active materials of each of the Examples and Comparative Examples. [Figure 6] FIG. 2 is a comparison diagram of cycle capacity retention rates at 45° C. of batteries made of the positive electrode active materials of each of the Examples and Comparative Examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0026] In order to facilitate understanding of the present invention, the present invention will be described more fully and in detail below with reference to the drawings and preferred embodiments in the specification, but the scope of protection of the present invention is not limited to the following specific embodiments.
[0027] Unless otherwise defined, all technical terms used below have the same meaning as commonly understood by those skilled in the art. The technical terms used in this specification are only for the purpose of describing specific embodiments, and are not intended to limit the scope of protection of the present invention.
[0028] Unless otherwise stated, the various raw materials, reagents, instruments and devices, etc. used in the present invention can all be commercially purchased or manufactured by conventional methods.
[0029] Example 1: The lithium ion battery positive electrode active material of the present invention comprises a positive electrode active material matrix Li 1.01 Ni 0.88 Co 0.10 Al 0.02 O 2 and Li 2 SO 4 Including Li 2 SO 4 Of these, the S content accounts for 0.09% of the total mass of the positive electrode active material, and the Li 2 SO 4 is mainly coated on the surface of the positive electrode active material matrix.
[0030] The method for producing the lithium ion battery positive electrode active material of this embodiment is as follows: (1)Molecular formula Li 1.01 Ni 0.88 Co 0.10 Al 0.02 O 2 Weighing the lithium metal compound and lithium sulfate powder in a weighing ratio and uniformly mixing them with a high-speed mechanical stirrer so that the S content of the mixture is 0.09%; (2) calcining the mixture obtained in step (1) in an oxygen atmosphere for 6 hours, the calcination temperature is 650° C., and the calcined material is a positive electrode active material including a lithium metal compound and a sulfate.
[0031] The positive electrode active material obtained in this example was used to manufacture a button battery with a lithium sheet as the negative electrode, and the measurement results are shown in Figures 4 to 6. 0.2C charge / discharge was performed at 25°C and a voltage range of 3.0 to 4.3V, and the discharge specific capacity was 208.5mAh / g. After 50 cycles of 1C / 1C charge / discharge, the capacity retention was 95.3%. After 50 cycles of 0.5C / 0.5C charge / discharge at 45°C, the capacity retention was 92.9%.
[0032] Example 2: The lithium ion battery positive electrode active material of the present invention comprises a positive electrode active material matrix Li 1.03 Ni 0.88 Co 0.10 Al 0.02 O 2 and Al 2 (SO 4 ) 3 Contains Al 2 (SO 4 ) 3 Of these, the S content accounts for 0.12% of the total mass of the positive electrode active material, and the Al content accounts for 0.12% of the total mass of the positive electrode active material. 2 (SO 4 ) 3 is mainly topped on the positive electrode active material matrix.
[0033] The method for producing the lithium ion battery positive electrode active material of this embodiment is as follows: (1) uniformly mixing nickel cobalt aluminum hydroxide precursor, lithium hydroxide, and aluminum sulfate in a measured ratio, the amount of lithium hydroxide added is such that the molar ratio Li / Me (Me=Ni+Co+Al) in the active material is 1.03, and the amount of aluminum sulfate added is such that S accounts for 0.12% of the total mass of the lithium battery positive electrode active material; (2) calcining the mixture obtained in step (1) in an oxygen atmosphere at 750° C. for 15 hours, whereby the calcined product is a positive electrode active material comprising a lithium metal compound and a sulfate.
[0034] The obtained aluminum sulfate-topped positive electrode active material was used to manufacture a button battery with a lithium sheet as the negative electrode, and measurements were performed. That is, 0.2C charge / discharge was performed under conditions of 25°C and a voltage range of 3.0 to 4.3V. The discharge specific capacity was 207.7mAh / g, and the capacity retention after 50 cycles of 1C / 1C charge / discharge was 94.9%, and the capacity retention after 50 cycles of 0.5C / 0.5C charge / discharge at 45°C was 92.4%.
[0035] Example 3: The lithium ion battery positive electrode active material of the present invention comprises a positive electrode active material matrix Li 1.01 Ni 0.88 Co 0.10 Al 0.02 O 2 and CoSO 4 Including CoSO 4 Of these, the S content accounts for 0.13% of the total mass of the positive electrode active material, and CoSO 4 is mainly coated on the surface of the positive electrode active material matrix.
[0036] The method for producing the lithium ion battery positive electrode active material of this embodiment is as follows: (1)Molecular formula Li 1.01 Ni 0.88 Co 0.10 Al 0.02 O 2 and mixing the lithium metal compound and cobalt sulfate powder by a high-speed mechanical stirrer to homogeneously mix the mixture, the S content of the mixture being 0.13% and the added Co content being 0.24%; (2) calcining the mixture of step (1) in an oxygen atmosphere at a high temperature of 650° C. for 6 hours, whereby the calcined material is a positive electrode active material comprising a lithium metal compound and a sulfate.
[0037] Observation with a scanning electron microscope shows that the primary particles coated on the surface of the sintered cobalt sulfate positive electrode material are uneven and not flat, as shown in Figure 1, but it is clear that the cobalt sulfate powder reacts and melts after being sintered at high temperatures, and also penetrates into the lithium metal compound.
[0038] The positive electrode active material obtained in this example was used to manufacture a button battery with a lithium sheet as the negative electrode, and the measurement results are shown in Figures 4 to 6. 0.2C charge / discharge was performed at 25°C and a voltage range of 3.0 to 4.3V, and the discharge specific capacity was 207.5mAh / g. After 50 cycles of 1C / 1C charge / discharge, the capacity retention was 95.2%. After 50 cycles of 0.5C / 0.5C charge / discharge at 45°C, the capacity retention was 92.7%.
[0039] Example 4: The lithium ion battery positive electrode active material of the present invention comprises a positive electrode active material matrix Li 1.01 Ni 0.88 Co 0.10 Al 0.02 O 2 and Li 2 SO 4 , Co(OH) 2 Including Li 2 SO 4 Of these, the S content was 0.09% of the total mass of the positive electrode active material, the coated cobalt content was 0.24%, and the Li 2 SO 4 and Co(OH) 2 is co-coated on the surface of the positive electrode active material matrix.
[0040] The method for producing the lithium ion battery positive electrode active material of this embodiment is as follows: (1)Molecular formula Li 1.01 Ni 0.88 Co 0.10 Al 0.02 O 2 The lithium metal compound, lithium sulfate, and cobalt hydroxide powder are mixed in a predetermined mass ratio and mixed uniformly by a high-speed mechanical stirrer, where the S content of the lithium sulfate added accounts for 0.09% of the total mass of the positive electrode active material, and the Co content of the cobalt hydroxide added is the same as the Co content of the cobalt sulfate added in Example 3, both being 0.24%; (2) calcining the mixture of step (1) in an oxygen atmosphere at a high temperature of 650° C. for 6 hours, whereby the calcined material is a positive electrode active material comprising a lithium metal compound and a sulfate.
[0041] The obtained positive electrode material co-coated with lithium sulfate and cobalt hydroxide was used to manufacture a button battery with a lithium sheet as the negative electrode, and the measurement results are shown in Figures 4 to 6. 0.2C charge / discharge was performed at 25°C and in the voltage range of 3.0 to 4.3V, and the discharge specific capacity was 209.3mAh / g. After 50 cycles of 1C / 1C charge / discharge, the capacity retention was 96.1%, and after 50 cycles of 0.5C / 0.5C charge / discharge at 45°C, the capacity retention was 93.2%.
[0042] Example 5 The lithium ion battery positive electrode active material of the present invention comprises a positive electrode active material matrix Li 1.01 Ni 0.88 Co 0.10 Al 0.02 O 2 and CoSO 4 Including CoSO 4 Of these, the S content accounts for 0.06% of the total mass of the positive electrode active material, and CoSO 4 is mainly coated on the surface of the positive electrode active material matrix.
[0043] The method for producing the lithium ion battery positive electrode active material of this embodiment is as follows: (1)Molecular formula Li 1.01 Ni 0.88 Co 0.10 Al 0.02 O 2 and mixing the lithium metal compound and cobalt sulfate powder by a high-speed mechanical stirrer, the mixture having an S content of 0.06%; (2) calcining the mixture of step (1) in an oxygen atmosphere at a high temperature of 650° C. for 6 hours, whereby the calcined material is a positive electrode active material comprising a lithium metal compound and a sulfate.
[0044] The positive electrode active material obtained in this embodiment is used to manufacture a button battery with a lithium sheet as the negative electrode, and the battery is measured. The battery is charged and discharged at 0.2C at 25°C and in a voltage range of 3.0-4.3V. The discharge specific capacity is 207.8mAh / g, and the capacity retention rate after 50 cycles of 1C / 1C charge and discharge is 94.5%. The capacity retention rate after 50 cycles of 0.5C / 0.5C charge and discharge at 45°C is 92.1%.
[0045] Example 6 The lithium ion battery positive electrode active material of the present invention comprises a positive electrode active material matrix Li 1.01 Ni 0.88 Co 0.10 Al 0.02 O 2 and CoSO 4 Including CoSO 4 Of these, the S content accounts for 0.40% of the total mass of the positive electrode active material, and CoSO 4 is mainly coated on the surface of the positive electrode active material matrix.
[0046] The method for producing the lithium ion battery positive electrode active material of this embodiment is as follows: (1)Molecular formula Li 1.01 Ni 0.88 Co 0.10 Al 0.02 O 2 and cobalt sulfate powder, and uniformly mix them by a high-speed mechanical stirrer, the S content of the mixture being 0.40%; (2) calcining the mixture of step (1) in an oxygen atmosphere at a high temperature of 650° C. for 6 hours, whereby the calcined material is a positive electrode active material comprising a lithium metal compound and a sulfate.
[0047] The positive electrode active material obtained in this embodiment is used to prepare a button battery with a lithium sheet as the negative electrode, and the battery is measured. The battery is charged and discharged at 0.2C at 25°C and in a voltage range of 3.0-4.3V. The discharge specific capacity is 206.2mAh / g, and the capacity retention rate after 50 cycles of 1C / 1C charge and discharge is 95.2%. The capacity retention rate after 50 cycles of 0.5C / 0.5C charge and discharge at 45°C is 92.8%.
[0048] Comparative Example 1: In Example 1, the molecular formula Li 1.01 Ni 0.88 Co 0.10 Al 0.02 O 2 The lithium metal oxide of the lithium ion battery was measured and found to have an S content of about 0.02%, which was mainly due to sulfate impurities introduced into the precursor material used to synthesize the positive electrode material. Scanning electron microscopy revealed that the surface of the material was smooth, as shown in Figure 2.
[0049] This uncoated positive electrode matrix (molecular formula Li 1.01 Ni 0.88 Co 0.10 Al 0.02 O 2 The lithium metal oxide (Li metal oxide) was fabricated into a button battery with a lithium sheet as the negative electrode, and the measurement results are shown in Figures 4 to 6. 0.2C charge / discharge was performed at 25°C and in the voltage range of 3.0 to 4.3V, and the discharge specific capacity was 203.2mAh / g. After 50 cycles of 1C / 1C charge / discharge, the capacity retention was 92.1%, and after 50 cycles of 0.5C / 0.5C charge / discharge at 45°C, the capacity retention was 87.7%.
[0050] Comparing the lithium sulfate coating of Example 1 and the cobalt sulfate coating of the positive electrode material of Example 3, it is demonstrated that the introduction of sulfate significantly improves the cycling performance of the material.
[0051] Comparative Example 2: The same lithium metal oxide Li as in Example 1 1.01 Ni 0.88 Co 0.10 Al 0.02O 2 A cobalt hydroxide coating was employed on this material using the same cobalt content added as in Example 3.
[0052] The method for producing the positive electrode active material of this comparative example is as follows: (1)Molecular formula Li 1.01 Ni 0.88 Co 0.10 Al 0.02 O 2 and cobalt hydroxide powder in a predetermined mass ratio, and then mixed uniformly by a high-speed mechanical stirrer, in which the Co content of the cobalt hydroxide is 0.24%, which is the same as the Co content of the cobalt sulfate in Example 3; (2) sintering the mixture of step (1) at a high temperature of 650° C. for 6 hours in an oxygen atmosphere, whereby the sintered material is a positive electrode active material coated with cobalt hydroxide.
[0053] Observation with a scanning electron microscope revealed that the primary particles covering the surface of the sintered positive electrode material were uneven and not flat, as shown in Figure 3. Measurements also revealed that the S content was approximately 0.02%, which was mainly due to the introduction of sulfate impurities into the precursor raw material used to synthesize the positive electrode material.
[0054] The obtained positive electrode material coated with cobalt hydroxide was manufactured into a button battery using a lithium sheet as the negative electrode, and the measurement results are shown in Figures 4 to 6. 0.2C charge / discharge was performed under conditions of 25°C and a voltage range of 3.0 to 4.3V, and the discharge specific capacity was 203.8mAh / g. After 50 cycles of 1C / 1C charge / discharge, the capacity retention was 92.3%, and after 50 cycles of 0.5C / 0.5C charge / discharge at 45°C, the capacity retention was 89.7%.
[0055] Comparative Example 3: The lithium ion battery positive electrode active material of the present invention comprises a positive electrode active material matrix Li 1.01 Ni 0.88 Co 0.10 Al 0.02 O2 and CoSO 4 Including CoSO 4 Of these, the S content accounts for 0.50% of the total mass of the positive electrode active material, and CoSO 4 is mainly coated on the surface of the positive electrode active material matrix.
[0056] The method for producing the lithium battery positive electrode active material of this comparative example is as follows: (1)Molecular formula Li 1.01 Ni 0.88 Co 0.10 Al 0.02 O 2 and mixing the lithium metal compound and cobalt sulfate powder by a high-speed mechanical stirrer, the mixture having an S content of 0.50%; (2) calcining the mixture of step (1) in an oxygen atmosphere at a high temperature of 650° C. for 6 hours, whereby the calcined material is a positive electrode active material comprising a lithium metal compound and a sulfate.
[0057] The obtained positive electrode active material was fabricated into a button battery using a lithium sheet as the negative electrode, and the battery was measured. The battery was charged and discharged at 0.2C at 25°C and in a voltage range of 3.0 to 4.3V. The discharge specific capacity was 203.4mAh / g, and the capacity retention rate after 50 cycles of 1C / 1C charge and discharge was 95.0%. The capacity retention rate after 50 cycles of 0.5C / 0.5C charge and discharge at 45°C was 92.9%.
[0058] Table 1 shows the electrical performance results of the positive electrode active materials of each of the examples and comparative examples.
[0059] Table 1. Electrical performance results of the positive electrode active materials of each Example and Comparative Example JPEG0007560644000001.jpg140170
[0060] By comparing Example 3 and Comparative Example 2, it is shown that although Co is introduced into the coating in both cases, the addition of sulfate in the examples can significantly improve the cyclability compared to the coating of cobalt hydroxide. Comparative Example 1, Example 4, and Comparative Example 2 show that the co-coating of lithium sulfate and cobalt hydroxide can improve the material cyclability and also significantly improve the capacity.
Claims
1. The present invention comprises a lithium ion battery positive electrode active material matrix and a sulfur compound, wherein the mass of S element in the sulfur compound accounts for 0.06-0.40% of the total mass of the lithium ion battery positive electrode active material, and the sulfur compound is distributed in the lithium ion battery positive electrode active material in the form of sulfate; The sulfur compound is mainly coated on the surface of the positive electrode active material matrix, The surface of the positive electrode active material matrix is also coated with cobalt hydroxide, the coating amount of the cobalt hydroxide is calculated in terms of cobalt element, and the mass of the coated cobalt element accounts for 0.1-1.5% of the total mass of the lithium ion battery positive electrode active material; 1. A lithium ion battery positive electrode active material comprising:
2. Among the sulfur compounds, the mass of S element accounts for 0.06-0.13% of the total mass of the lithium-ion battery positive electrode active material; 2. The lithium ion battery positive electrode active material according to claim 1 .
3. The sulfur compounds include one or more of lithium sulfate, cobalt sulfate, manganese sulfate, aluminum sulfate, magnesium sulfate, titanium sulfate, zirconium sulfate, sodium sulfate, sodium metabisulfite, and ammonium sulfate; 2. The lithium ion battery positive electrode active material according to claim 1 .
4. The sulfur compound is mainly topped on the positive electrode active material matrix; The positive electrode active material for a lithium ion battery according to any one of claims 1 to 3.
5. Mixing the positive electrode active material matrix and the sulfur compound in a stoichiometric manner and calcining to obtain a lithium ion positive electrode active material, the calcination temperature is 300-750° C., and the calcination time is 3-15 hours; A method for producing the positive electrode active material for a lithium ion battery according to any one of claims 1 to 3.
6. Cobalt hydroxide is also added during the mixing process. The method according to claim 5 .
7. The method includes stoichiometrically mixing a positive electrode active material precursor, a lithium source, and a sulfur compound, and calcining the mixture to obtain a lithium ion positive electrode active material, the calcination temperature being 650-950° C., and the calcination time being 6-18 hours; A method for producing the positive electrode active material for a lithium ion battery according to any one of claims 1 to 4.
Citation Information
Patent Citations
Lithium cobalt composite oxide, method for preparing the same, positive pole active substance of lithium secondary cell, and lithium secondary cell
JP2003020229A
Positive electrode active material for nonaqueous electrolyte secondary battery and manufacturing method therefor, and nonaqueous electrolyte secondary battery
JP2010080394A
Positive electrode active material for nonaqueous electrolyte secondary battery and method for manufacturing the same
JP2018014208A
Cathod material for Lithium second battery of whichsurface is processed and manufacturing method thereof
KR1020050048453A
Method of preparing cobalt and lithium ion-coated nickel and manganese-based cathode material
US20100068376A1