Separators for power storage devices
The separator with a thermoplastic polymer-containing layer addresses the trade-off between adhesiveness and injectability by optimizing dot-like pattern dimensions and contact angle, enhancing both properties for improved power storage device performance.
Patent Information
- Application Number
- JP2023546973
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-09-07
- Filing Date
- 2022-09-07
- Publication Date
- 2024-10-02
- Estimated Expiration
- 2042-09-07
AI Technical Summary
Conventional separators for power storage devices face challenges in achieving both adhesiveness with electrodes and injectability of electrolyte, with a trade-off relationship between the two properties, making it difficult to improve both simultaneously.
A separator design featuring a thermoplastic polymer-containing layer with a specific dot-like pattern, where the dot diameter ranges from 20 μm to 1,000 μm, and the distance between dots ranges from 100 μm to 3,000 μm, with a contact angle of 0° to 20°, and a total coverage area ratio of 5% to 55%, enhancing adhesion and electrolyte injection performance.
The separator achieves both improved adhesiveness with electrodes and injectability of electrolyte, contributing to better productivity and performance of power storage devices.
Smart Images

Figure 0007560678000014 
Figure 0007560678000015 
Figure 0007560678000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a separator for an electricity storage device. [Background technology]
[0002] In recent years, the development of power storage devices, such as non-aqueous electrolyte batteries, has been actively carried out. In general, in non-aqueous electrolyte batteries, such as lithium ion batteries, a microporous membrane is provided as a separator between positive and negative electrodes. Such a separator has the function of preventing direct contact between the positive and negative electrodes and allowing ions to pass through the electrolyte held in the micropores.
[0003] In addition to the safety performance that has traditionally been required of separators, such as the characteristic of quickly stopping the battery reaction in the event of abnormal heating (fuse characteristic) and the ability to maintain its shape even at high temperatures and prevent the dangerous situation of direct reaction between the positive and negative electrode materials (short-circuit characteristic), separators are also required to have improved adhesion to the electrodes from the perspective of uniforming charge and discharge currents and suppressing lithium dendrites.
[0004] In order to impart various functions to the separator in addition to safety and adhesion to the electrodes, coating or lamination of a functional layer onto the microporous membrane has been investigated (Patent Documents 1 to 6).
[0005] For example, Patent Document 1 describes that, from the viewpoint of improving the handling property and adhesive property when winding a battery and the lithium ion permeability, a thermoplastic polymer-containing layer is formed in a dot pattern on at least one surface of a microporous membrane as a separator substrate, and the dot diameter and the distance between the dots are adjusted.
[0006] Patent Document 2 describes that in order to improve the separation between a separator having a porous coating layer and an electrode, and to improve the detachment phenomenon of inorganic particles in the porous coating layer, a separator substrate is coated with an inorganic particle-containing porous layer in a dot pattern, and the average dot diameter and the distance between the dots are adjusted.
[0007] Patent Document 3 focuses on a technology for improving the absorption of the electrolyte into the electrode by penetrating the electrolyte to the center of the positive or negative electrode when an adhesive separator is used in a battery, but with regard to the dot pattern coating of the adhesive layer onto the separator substrate, it merely lists the maximum dot diameter and the arrangement pitch of the dots.
[0008] In Patent Document 4, from the viewpoint of suppressing an increase in resistance acting inside a secondary battery when a separator including an adhesive layer is mounted in a secondary battery by coating the entire surface of the porous substrate, a dot pattern of the adhesive layer is illustrated and the distance between the dots is specified for a separator having an acrylate adhesive layer formed on at least one side of a porous substrate.
[0009] Patent Documents 5 and 6 describe the provision of an acrylate-based adhesive layer formed of a plurality of dots spaced apart from each other at a predetermined interval on the surface of a porous coating layer in order to suppress a decrease in the adhesive strength between a separator containing inorganic particles and an electrode, and also provide examples of the average diameter of the dots. [Prior art documents] [Patent documents]
[0010] [Patent Document 1] International Publication No. 2014 / 017651 [Patent Document 2] Special Publication No. 2011-512005 [Patent Document 3] International Publication No. 2020 / 067208 [Patent Document 4] Special Publication No. 2018-535534 [Patent Document 5] JP 2015-99777 A [Patent Document 6] JP 2015-99776 A Summary of the Invention [Problem to be solved by the invention]
[0011] When a separator including a microporous membrane as a separator substrate and an adhesive layer coated or laminated on at least one side of the microporous membrane is used in assembling cells of an electricity storage device, the injectability in the electrolyte injection step may deteriorate.
[0012] However, for conventional separators for electricity storage devices that include a microporous membrane as a substrate and an adhesive layer formed in a dot pattern on the substrate, there is a trade-off between improving the adhesive strength with the electrode and improving the injectability of the electrolyte, making it difficult to achieve both.
[0013] In view of the above circumstances, an object of the present invention is to provide a separator for an electricity storage device that can achieve both adhesiveness and liquid injectability, and an electricity storage device including the separator. [Means for solving the problem]
[0014] As a result of extensive research, the present inventors have found that the above-mentioned problems can be solved by elucidating the factors of the injectability of a thermoplastic polymer-containing layer in coating or lamination on a substrate and specifying the dot pattern of the thermoplastic polymer-containing layer. [1] A separator for an electric storage device comprising: a substrate; and a thermoplastic polymer-containing layer formed on at least one surface of the substrate, the thermoplastic polymer-containing layer including a thermoplastic polymer, the thermoplastic polymer-containing layer has a dot-like pattern, The diameter of the dots is 20 μm or more and 1,000 μm or less, The distance between dots is 100 μm or more and 3,000 μm or less, The diameter of the dots and the distance between the dots are expressed by the following formula: Distance between dots / diameter of dot = 0.5 to 4 and The separator for an electricity storage device, wherein the contact angle between the thermoplastic polymer-containing layer and an electrolyte solution is 0° or more and 20° or less. [2] 2. The separator for an electricity storage device according to item 1, wherein the average dot height is 0.2 μm or more and 10 μm or less. [3] 3. The separator for an electricity storage device according to item 1 or 2, wherein a total coverage area ratio of the thermoplastic polymer-containing layer to the surface of the substrate is 5% or more and 55% or less. [4] The thermoplastic polymer-containing layer has a basis weight of 0.03 g / m 2 More than 0.3g / m 2 4. The separator for an electricity storage device according to any one of items 1 to 3, which is as follows: [5] 5. The separator for an electricity storage device according to any one of items 1 to 4, wherein the thermoplastic polymer has an average particle size of 0.1 μm or more and 2.0 μm or less. [6] 6. The separator for an electricity storage device according to any one of items 1 to 5, wherein the thermoplastic polymer has at least two glass transition temperatures, at least one of the glass transition temperatures being in a range of less than 20° C., and at least one of the glass transition temperatures being in a range of 40° C. or higher and 110° C. or lower. [7] 7. The separator for an electricity storage device according to any one of items 1 to 6, which has an asymmetric multilayer structure with respect to the substrate. [8] 8. The separator for an electricity storage device according to any one of items 1 to 7, wherein the thermoplastic polymer-containing layers are provided on both sides of the substrate, and a porous layer containing an inorganic filler and a resin binder is formed between one side of the substrate and the thermoplastic polymer-containing layer. [9] 9. An electricity storage device comprising a positive electrode, a negative electrode, the electricity storage device separator according to item 8, and a nonaqueous electrolyte, wherein the electricity storage device separator is disposed such that a side having the porous layer faces the positive electrode with respect to the substrate.
[10] 9. An electricity storage device comprising: a positive electrode, a negative electrode, the separator for an electricity storage device according to any one of items 1 to 8, and a non-aqueous electrolyte. Effect of the Invention
[0015] According to the present invention, it is possible to provide a separator for an electricity storage device that is capable of achieving both adhesiveness and liquid injectability, and an electricity storage device including the separator. [Brief description of the drawings]
[0016] [Figure 1] FIG. 1 is a schematic plan view illustrating the dot diameter and inter-dot distance according to one embodiment of the present invention, in which FIG. 1(a) shows a pattern excluding areas with dimensions of 10 μm or less, and FIG. 1(b) shows an area where a thermoplastic polymer is continuously present and a particle-scattered area. [Diagram 2] FIG. 1 is a schematic plan view showing defined regions where thermoplastic polymer is continuously present in order to explain the dot diameter and inter-dot distance in one embodiment of the present invention; FIG. 2(a) shows a pattern excluding regions with dimensions of 10 μm or less; FIG. 2(b) shows regions where thermoplastic polymer is continuously present and particle-splattered regions; FIGS. 2(c)-(d) show regions where thermoplastic polymer is continuously present, regions where thermoplastic polymer is not present and particle-splattered regions; FIG. 2(e) shows a cloverleaf pattern; FIG. 2(f) shows teardrop-shaped tailing of dots; and FIG. 2(g) shows the distance between multiple dots. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] Hereinafter, a mode for carrying out the present invention (hereinafter, referred to as "the present embodiment") will be described in detail. Note that the present invention is not limited to the following embodiment, and can be carried out in various modifications within the scope of the gist of the present invention.
[0018] <Separators for power storage devices> The separator for an electricity storage device according to this embodiment (hereinafter also simply referred to as a "separator") comprises a substrate, a thermoplastic polymer-containing layer formed on at least one surface of the substrate and containing a thermoplastic polymer; The thermoplastic polymer-containing layer has a specific dot-like pattern.
[0019] The separator may have a thermoplastic polymer-containing layer on one or both surfaces of the substrate, and may optionally have a porous layer between the substrate surface and the thermoplastic polymer-containing layer, or on a substrate surface on which the thermoplastic polymer-containing layer is not formed.
[0020] (Dot pattern of thermoplastic polymer-containing layer) The thermoplastic polymer-containing layer according to the present embodiment has a dot pattern, the diameter of the dots is 20 μm or more and 1,000 μm or less, the distance between the dots is 100 μm or more and 3,000 μm or less, and the dot diameter and the distance between the dots satisfy the following formula: Distance between dots / diameter of dot = 0.5 to 4 The relationship expressed as:
[0021] The dot-like shape indicates that there are parts containing a thermoplastic polymer and parts not containing a thermoplastic polymer on the polyolefin microporous membrane, and the parts containing the thermoplastic polymer are present in islands. Note that, in the thermoplastic polymer-containing layer, the parts containing the thermoplastic polymer may be independent.
[0022] In the present embodiment, the dot pattern of the thermoplastic polymer-containing layer is as follows: 20μm≦dot diameter≦1,000μm 100μm≦distance between dots≦3,000μm 0.5≦distance between dots / diameter of dot≦4 By optimizing the separator to satisfy the above requirements and improving the adhesion efficiency with the electrodes, the company was able to realize a separator that has a higher level of adhesion (to the electrodes) than before while suppressing the inhibition of electrolyte permeability, and furthermore has improved wettability, achieving both adhesion and electrolyte injection properties. Furthermore, the compatibility of adhesion and electrolyte injection properties with the separator also contributes to improving the productivity of electricity storage devices that include the separator.
[0023] In this specification, the injectability refers to the ease with which an electrolyte permeates into electrodes and separators during an electrolyte injection process in assembling cells for an electricity storage device that uses a separator, and is expressed as the shortness of time required from the start of injection to the completion of permeation.
[0024] Although not wishing to be bound by theory, when a cell of an electricity storage device is assembled using a separator having a thermoplastic polymer-containing layer laminated or coated on the surface of a substrate, the pourability factor is calculated by the following Lucas-Washburn equation:
number
[0025] When the above Lucas-Washburn equation is applied to the separator according to the present embodiment, it is considered that γ (surface tension) and μ (viscosity) are largely dependent on the electrolyte, whereas r (capillary diameter) is characterized by the separator, and the contact angle (θ) is characterized by the wettability of the separator and / or the electrodes. More specifically, the following two points are factors that affect the injectability: · the distance between the dots in the thermoplastic polymer-containing layer and / or the distance between the separator and the electrodes; - Wettability of separator and electrodes It was found that when the viscosity of the electrolyte is in the range of 0.1 mPa s to 10 mP s, or when the surface tension of the electrolyte is in the range of 20 mN / m to 50 mN / m, the injectability becomes a particular issue, and when the separator according to the present embodiment is used for an electrolyte having these physical property ranges, the injectability of the entire cell is excellent.
[0026] In this embodiment, by optimizing the dot diameter, the distance between dots, and the distance between dots / diameter between dots for the dot pattern of the thermoplastic polymer-containing layer within the above numerical ranges, the distance between dots and / or the distance between the separator and the electrode can be increased to increase r (capillary diameter), the wettability of the separator can be increased to increase the contact angle (θ), and l (permeation distance), which corresponds to the penetration of the electrolyte between the separator and the electrode, can be increased in the above Lucas-Washburn equation, thereby improving the injection property of the entire cell of the electricity storage device.
[0027] From the viewpoint of achieving both adhesiveness and pourability, and increasing the permeation distance as described above, the diameter of the dots in the thermoplastic polymer-containing layer is preferably 20 μm or more and 1000 μm or less, more preferably 50 μm or more and 800 μm or less, even more preferably 100 μm or more and 700 μm or less, particularly preferably 145 μm or more and 600 μm or less, and most preferably 150 μm or more and 600 μm or less.
[0028] The distance between dots in the thermoplastic polymer-containing layer is preferably 100 μm or more and 3000 μm or less, more preferably 200 μm or more and 2500 μm or less, even more preferably 400 μm or more and 2000 μm or less, and particularly preferably 501 μm or more and 1500 μm or less, from the viewpoint of ensuring sufficient gaps between the multiple dots to ensure a permeation flow path for the electrolyte and to facilitate good air escape.
[0029] From the viewpoint of achieving an excellent balance between the adhesive strength to the electrode and the injectability of the electrolyte, the distance between dots / diameter of the dot in the thermoplastic polymer-containing layer is preferably 0.5 or more and 4 or less, more preferably 0.7 or more and 3.8 or less, even more preferably 1 or more and 3.5 or less, even more preferably within the range of 1.3 to 3.5, and particularly preferably 2 or more and 3.3 or less.
[0030] With regard to the dot pattern of the thermoplastic polymer-containing layer, from the viewpoints of the distance between the separator and the electrode and the wettability of the separator, the average dot height is preferably 0.2 μm or more and 10 μm or less, more preferably 0.5 μm or more and 10 μm or less, or 1.0 μm or more and 10 μm or less, even more preferably 0.5 μm or more and 4 μm or less, or 1.0 μm or more and 4 μm or less, even more preferably 0.5 μm or more and 3 μm or less, and particularly preferably 1 μm or more and 3 μm or less.
[0031] The arrangement angle of the dots in the thermoplastic polymer-containing layer is preferably less than 40° from the viewpoint of improving air escape, and the lower limit of the arrangement angle is not limited, but may be, for example, 0° or more.
[0032] For the dot pattern of the thermoplastic polymer-containing layer, the rate of change in the distance between dots before and after the electrolyte solution is absorbed into the separator is preferably 0% to 20%, more preferably 0% to 10%. If the rate of change in the distance between dots before and after the electrolyte solution is absorbed into the separator is within the above numerical range, the balance between adhesion and injectability tends to be excellent.
[0033] The dot pattern of the thermoplastic polymer-containing layer specified above can be achieved, for example, in the separator manufacturing process, by optimizing the thermoplastic polymer-containing coating liquid, adjusting the polymer concentration or coating amount of the coating liquid and the coating method or coating conditions, or by devising a printing plate.
[0034] The components of the separator according to this embodiment will be described below.
[0035] [Thermoplastic polymer-containing layer] The thermoplastic polymer-containing layer according to this embodiment contains a thermoplastic polymer.
[0036] [Contact angle between thermoplastic polymer-containing layer and electrolyte] From the viewpoints of excellent electrolyte injectability, less air pockets, and a short injection time, the thermoplastic polymer-containing layer preferably has a contact angle with the electrolyte of 0° to 20°, more preferably 2° to 18°, and even more preferably 4° to 16°. The contact angle of the thermoplastic polymer-containing layer with the electrolyte is preferably measured on a surface of the thermoplastic polymer-containing layer formed in a dot pattern.
[0037] The contact angle of the thermoplastic polymer-containing layer with the electrolyte can be adjusted within the above-described numerical range by, for example, controlling the total coverage area ratio of the thermoplastic polymer-containing layer to the substrate surface, the particle size of the thermoplastic polymer, the corona treatment intensity of the substrate surface, the drying speed, the viscosity of the coating material, the pH of the coating material, and the like in the process of forming the thermoplastic polymer-containing layer.
[0038] (Thermoplastic polymer) The thermoplastic polymer used in the present embodiment is not particularly limited, and examples thereof include polyolefin resins such as polyethylene, polypropylene, and α-polyolefin; fluorine-containing resins such as polyvinylidene fluoride and polytetrafluoroethylene and copolymers containing these; diene-based polymers containing conjugated dienes such as butadiene and isoprene as monomer units or copolymers containing these and hydrogenated products thereof; acrylic polymers containing acrylic acid esters, methacrylic acid esters, and the like as monomer units or copolymers containing these and hydrogenated products thereof; rubbers such as ethylene propylene rubber, polyvinyl alcohol, and polyvinyl acetate; cellulose derivatives such as ethyl cellulose, methyl cellulose, hydroxyethyl cellulose, and carboxymethyl cellulose; resins having a melting point and / or glass transition temperature of 180° C. or higher, such as polyphenylene ether, polysulfone, polyethersulfone, polyphenylene sulfide, polyetherimide, polyamideimide, polyamide, and polyester, and mixtures thereof. In addition, as a monomer used in synthesizing the thermoplastic polymer, a monomer having at least one group selected from the group consisting of a hydroxyl group, a sulfonic acid group, a carboxyl group, an amide group, and a cyano group can also be used.
[0039] Among these thermoplastic polymers, diene-based polymers, acrylic polymers and fluorine-based polymers are preferred because they have excellent binding properties with the electrode active material, and excellent strength or flexibility.
[0040] (Diene Polymer) The diene polymer is not particularly limited, but is a polymer containing a monomer unit obtained by polymerizing a conjugated diene having two conjugated double bonds, such as butadiene or isoprene. The conjugated diene monomer is not particularly limited, but examples thereof include 1,3-butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, 2-phenyl-1,3-butadiene, 1,3-pentadiene, 2-methyl-1,3-pentadiene, 1,3-hexadiene, 4,5-diethyl-1,3-octadiene, and 3-butyl-1,3-octadiene. These may be polymerized alone or copolymerized.
[0041] The proportion of monomer units obtained by polymerizing a conjugated diene in the diene polymer is not particularly limited, but is, for example, 40% by mass or more, preferably 50% by mass or more, and more preferably 60% by mass or more, of the total diene polymer.
[0042] The diene polymer is not particularly limited, but may be, for example, a homopolymer of a conjugated diene such as polybutadiene or polyisoprene, or a copolymer of a conjugated diene and a copolymerizable monomer. The copolymerizable monomer is not particularly limited, but may be, for example, a (meth)acrylate monomer described below or the following monomer (hereinafter also referred to as "other monomer").
[0043] The "other monomer" is not particularly limited, but examples thereof include α,β-unsaturated nitrile compounds such as acrylonitrile and methacrylonitrile; unsaturated carboxylic acids such as acrylic acid, methacrylic acid, itaconic acid, and fumaric acid; styrene-based monomers such as styrene, chlorostyrene, vinyltoluene, t-butylstyrene, vinylbenzoic acid, methyl vinylbenzoate, vinylnaphthalene, chloromethylstyrene, hydroxymethylstyrene, α-methylstyrene, and divinylbenzene; olefins such as ethylene and propylene; halogen atom-containing monomers such as vinyl chloride and vinylidene chloride; vinyl esters such as vinyl acetate, vinyl propionate, vinyl butyrate, and vinyl benzoate; methyl vinyl ether, and ethyl vinyl ether. vinyl ethers such as butyl vinyl ether; vinyl ketones such as methyl vinyl ketone, ethyl vinyl ketone, butyl vinyl ketone, hexyl vinyl ketone, isopropenyl vinyl ketone; heterocycle-containing vinyl compounds such as N-vinyl pyrrolidone, vinyl pyridine, vinyl imidazole; acrylic acid ester and / or methacrylic acid ester compounds such as methyl acrylate, methyl methacrylate; hydroxyalkyl group-containing compounds such as β-hydroxyethyl acrylate, β-hydroxyethyl methacrylate; amide monomers such as acrylamide, N-methylolacrylamide, acrylamido-2-methylpropanesulfonic acid, etc., and these may be used alone or in combination of two or more.
[0044] (Acrylic polymer) The acrylic polymer is not particularly limited, but is preferably a polymer containing a monomer unit obtained by polymerizing a (meth)acrylate monomer.
[0045] In this specification, "(meth)acrylic acid" refers to "acrylic acid or methacrylic acid", and "(meth)acrylate" refers to "acrylate or methacrylate".
[0046] The (meth)acrylate monomer is not particularly limited, but examples thereof include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, t-butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, and the like. Examples of the acrylate include alkyl (meth)acrylates such as acrylate, lauryl (meth)acrylate, n-tetradecyl (meth)acrylate, and stearyl (meth)acrylate; hydroxy group-containing (meth)acrylates such as hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, and hydroxybutyl (meth)acrylate; amino group-containing (meth)acrylates such as aminoethyl (meth)acrylate; and epoxy group-containing (meth)acrylates such as glycidyl (meth)acrylate.
[0047] The proportion of monomer units obtained by polymerizing (meth)acrylate monomers is not particularly limited, but is, for example, 40% by mass or more, preferably 50% by mass or more, and more preferably 60% by mass or more of the total acrylic polymer. Examples of the acrylic polymer include homopolymers of (meth)acrylate monomers and copolymers of the homopolymers and copolymerizable monomers. Examples of the copolymerizable monomers include the "other monomers" listed in the above diene polymer section, and these may be used alone or in combination of two or more.
[0048] (Fluorine-based polymer) The fluorine-based polymer is not particularly limited, but examples thereof include a homopolymer of vinylidene fluoride and a copolymer of the homopolymer and a monomer copolymerizable therewith. The fluorine-based polymer is preferable from the viewpoint of electrochemical stability.
[0049] The proportion of monomer units obtained by polymerizing vinylidene fluoride is not particularly limited, but is, for example, 40% by mass or more, preferably 50% by mass or more, more preferably 60% by mass or more. The monomer copolymerizable with vinylidene fluoride is not particularly limited, but examples thereof include fluorine-containing ethylenically unsaturated compounds such as vinyl fluoride, tetrafluoroethylene, trifluorochloroethylene, hexafluoropropylene, hexafluoroisobutylene, perfluoroacrylic acid, perfluoromethacrylic acid, fluoroalkyl esters of acrylic acid or methacrylic acid, fluorine-free ethylenically unsaturated compounds such as cyclohexyl vinyl ether and hydroxyethyl vinyl ether, and fluorine-free diene compounds such as butadiene, isoprene, and chloroprene.
[0050] Among the fluoropolymers, vinylidene fluoride homopolymers, vinylidene fluoride / tetrafluoroethylene copolymers, vinylidene fluoride / tetrafluoroethylene / hexafluoropropylene copolymers, etc. are preferred. A particularly preferred fluoropolymer is vinylidene fluoride / tetrafluoroethylene / hexafluoropropylene copolymer, the monomer composition of which is usually 30-90% by mass of vinylidene fluoride, 50-9% by mass of tetrafluoroethylene, and 20-1% by mass of hexafluoropropylene. These fluororesin particles may be used alone or in combination of two or more kinds.
[0051] Furthermore, as the monomer used in synthesizing the thermoplastic polymer, a monomer having a hydroxyl group, a carboxyl group, an amino group, a sulfonic acid group, an amide group, or a cyano group can also be used.
[0052] The monomer having a hydroxy group is not particularly limited, but examples thereof include vinyl monomers such as penteneol.
[0053] The monomer having a carboxyl group is not particularly limited, but examples thereof include unsaturated carboxylic acids having an ethylenic double bond such as (meth)acrylic acid and itaconic acid, and vinyl monomers such as pentenoic acid.
[0054] The monomer having an amino group is not particularly limited, but examples thereof include 2-aminoethyl methacrylate.
[0055] The monomer having a sulfonic acid group is not particularly limited, but examples thereof include vinyl sulfonic acid, methyl vinyl sulfonic acid, (meth)allylsulfonic acid, styrenesulfonic acid, (meth)acrylic acid-2-ethylsulfonate, 2-acrylamido-2-methylpropanesulfonic acid, and 3-allyloxy-2-hydroxypropanesulfonic acid.
[0056] The monomer having an amide group is not particularly limited, but examples thereof include acrylamide, methacrylamide, N-methylol acrylamide, and N-methylol methacrylamide.
[0057] The monomer having a cyano group is not particularly limited, but examples thereof include acrylonitrile, methacrylonitrile, α-chloroacrylonitrile, α-cyanoethyl acrylate, and the like.
[0058] The thermoplastic polymer used in the present embodiment may be a single polymer or a mixture of two or more types of polymers, but preferably contains two or more types of polymers. The thermoplastic polymer may be used together with a solvent, and the solvent may be one that can disperse the thermoplastic polymer uniformly and stably, such as N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, water, ethanol, toluene, hot xylene, methylene chloride, hexane, etc., and among them, aqueous solvents are preferred. The thermoplastic polymer may be used in the form of a latex.
[0059] (glass transition temperature of thermoplastic polymer) From the viewpoints of ensuring the distance between the electrodes and the separator in an electricity storage device while exerting adhesive strength with the separator electrodes and shortening the injection time of the electrolyte, it is preferable for the thermoplastic polymer to have thermal properties such that it has at least two glass transition temperatures, at least one of which is in a range below 20°C, and at least one of which is in a range of 40°C or higher and 110°C or lower.
[0060] The glass transition temperature is determined from a DSC curve obtained by differential scanning calorimetry (DSC). In this specification, the glass transition temperature may also be expressed as Tg.
[0061] Specifically, it is determined by the intersection of a straight line extending from the low-temperature side baseline to the high-temperature side in the DSC curve with a tangent to the inflection point of the step-like change in the glass transition. For more details, the method described in the Examples can be referred to.
[0062] Here, "glass transition" refers to a change in heat quantity that occurs on the endothermic side in DSC due to a change in the state of the polymer test piece. Such a change in heat quantity is observed as a step-like change or a combination of a step-like change and a peak in the DSC curve.
[0063] The term "step change" refers to the portion of a DSC curve where the curve leaves the previous baseline and transitions to a new baseline, and includes any combination of a peak and a step change.
[0064] The "inflection point" refers to the point at which the gradient of the step-like change in the DSC curve is maximum, or can be expressed as the point at which the step-like change changes from an upwardly convex curve to a downwardly convex curve.
[0065] The term "peak" refers to the portion of a DSC curve from when the curve leaves the baseline to when it returns to the baseline.
[0066] The term "baseline" refers to a DSC curve in the temperature range where no transition or reaction occurs in the test specimen.
[0067] In this embodiment, at least one of the glass transition temperatures of the thermoplastic polymers used is in the range of less than 20° C., which provides excellent adhesion to a substrate such as a microporous membrane, and as a result, provides excellent adhesion between the separator and the electrodes. At least one of the glass transition temperatures of the thermoplastic polymers used is more preferably in the range of 15° C. or less, and even more preferably in the range of −30° C. or more and 15° C. or less. It is particularly preferable that the glass transition temperature in the range of less than 20° C. is only in the range of −30° C. or more and 15° C. or less, in order to maintain good handleability while increasing the adhesion between the thermoplastic polymer and the microporous membrane.
[0068] In this embodiment, at least one of the glass transition temperatures of the thermoplastic polymers used is in the range of 40° C. to 110° C., so that the adhesiveness and handling between the separator and the electrode are excellent, and further, the distance between the electrode surface and the separator substrate surface in the electricity storage device can be maintained, and the injection time of the electrolyte can be shortened. At least one of the glass transition temperatures of the thermoplastic polymers used is more preferably in the range of 45° C. to 100° C., and even more preferably in the range of 50° C. to 95° C. In terms of handling, Tg70° C. or higher is preferable, as long as it does not impede the effects of the present invention.
[0069] The fact that a thermoplastic polymer has two glass transition temperatures can be achieved, for example, by blending two or more types of thermoplastic polymers, or by using a thermoplastic polymer having a core-shell structure, but is not limited to these methods. A core-shell structure is a polymer in the form of a double structure in which the polymer belonging to the central portion and the polymer belonging to the outer shell portion have different compositions.
[0070] In particular, the polymer blend or core-shell structure can control the glass transition temperature of the entire thermoplastic polymer by combining a polymer with a high glass transition temperature and a polymer with a low glass transition temperature. In addition, multiple functions can be imparted to the entire thermoplastic polymer. For example, in the case of a blend, a polymer having a glass transition temperature in the range of 20°C or higher and a polymer having a glass transition temperature in the range of less than 20°C can be blended to achieve both stickiness resistance and wettability to the polyolefin microporous membrane. The mixing ratio of the polymer having a glass transition temperature in the range of 20°C or higher and the polymer having a glass transition temperature in the range of less than 20°C is preferably in the range of 0.1:99.9 to 99.9:0.1, more preferably 5:95 to 95:5, even more preferably 50:50 to 95:5, and even more preferably 60:40 to 90:10. In the case of a core-shell structure, the adhesiveness or compatibility with other materials such as a polyolefin microporous membrane can be adjusted by changing the outer shell polymer, and the polymer in the central portion can be adjusted to have improved adhesiveness to an electrode after heat pressing, for example. Also, the viscoelasticity can be controlled by combining a polymer with high viscosity and a polymer with high elasticity.
[0071] The glass transition temperature of the shell of the thermoplastic polymer having a core-shell structure is not particularly limited, but is preferably less than 20° C., more preferably 15° C. or less, and even more preferably −30° C. or more and 15° C. or less. The glass transition temperature of the core of the thermoplastic polymer having a core-shell structure is not particularly limited, but is preferably 20° C. or more, more preferably 20° C. or more and 120° C. or less, and even more preferably 50° C. or more and 120° C. or less.
[0072] In the present embodiment, the glass transition temperature, i.e., Tg, of the thermoplastic polymer can be appropriately adjusted, for example, by changing the monomer components and the input ratio of each monomer used to produce the thermoplastic polymer. That is, it can be roughly estimated from the Tg of the homopolymer generally shown for each monomer used to produce the thermoplastic polymer (for example, as described in "Polymer Handbook" (A WILEY-INTERSCIENCE PUBLICATION)) and the blending ratio of the monomers. For example, a copolymer having a high Tg can be obtained by blending a high ratio of monomers such as styrene, methyl methacrylate, and acrylonitrile, which give a polymer with a Tg of about 100°C. On the other hand, a copolymer having a low Tg can be obtained by blending a high ratio of monomers such as butadiene, which gives a polymer with a Tg of about -80°C, or n-butyl acrylate and 2-ethylhexyl acrylate, which give a polymer with a Tg of about -50°C.
[0073] The Tg of the polymer can be roughly calculated by the FOX formula (the following formula (1)). The glass transition point of the thermoplastic polymer according to the present embodiment is measured by the above-mentioned method using DSC. 1 / Tg=W1 / Tg1+W2 / Tg2+···+W i / Tg i +···W n / Tg n (1) In formula (1), Tg(K) is the Tg of the copolymer, Tg i (K) is the Tg of the homopolymer of each monomer i, W i indicates the mass fraction of each monomer.}
[0074] (Structure of Thermoplastic Polymer-Containing Layer) In the thermoplastic polymer-containing layer, it is preferable that a thermoplastic resin having a glass transition temperature of 40°C to 110°C is present on the outermost surface side of the electricity storage device separator, and a thermoplastic resin having a glass transition temperature of less than 20°C is present on the interface side between the polyolefin microporous membrane and the thermoplastic polymer-containing layer. The "outermost surface" refers to the surface of the thermoplastic polymer-containing layer that contacts the electrode when the electricity storage device separator and the electrode are laminated. The "interface" refers to the surface of the thermoplastic polymer-containing layer that contacts the polyolefin microporous membrane.
[0075] In the thermoplastic polymer-containing layer, the thermoplastic polymer having a glass transition temperature of 40°C to 110°C is present on the outermost surface side of the separator for an electricity storage device, which tends to provide excellent adhesion to the microporous membrane, and as a result, excellent adhesion between the separator and the electrodes. In addition, the thermoplastic polymer having a glass transition temperature of less than 20°C is present on the interface side between the polyolefin microporous membrane and the thermoplastic polymer-containing layer, which tends to provide excellent adhesion and handling between the separator and the electrodes. By having such a thermoplastic polymer-containing layer, the separator tends to have improved adhesion and handling between the separator and the electrodes.
[0076] The above-mentioned structure can be achieved by (a) the thermoplastic polymer comprising a particulate thermoplastic polymer and a binder polymer that bonds the particulate thermoplastic polymer to the polyolefin microporous membrane with the particulate thermoplastic polymer exposed on the surface, the particulate thermoplastic polymer having a glass transition temperature in the range of 40°C to 110°C, and a thermoplastic polymer having a glass transition temperature of less than 20°C being present at the interface between the polyolefin microporous membrane and the thermoplastic polymer-containing layer, (b) the thermoplastic polymer having a laminated structure, the glass transition temperature of the thermoplastic polymer in the part that will be the outermost layer when used as a separator being in the range of 40°C to 110°C, and a thermoplastic polymer having a glass transition temperature of less than 20°C being present at the interface between the polyolefin microporous membrane and the thermoplastic polymer-containing layer, etc. The (b) thermoplastic polymer may have a laminated structure of polymers with different Tg.
[0077] (Average particle size of thermoplastic polymer) The structure of the thermoplastic polymer in the present embodiment is not particularly limited, but may be, for example, granular. Such a structure tends to improve the adhesiveness between the separator and the electrode and the handleability of the separator. Here, granular refers to a state in which each thermoplastic polymer has an outline when measured with a scanning electron microscope (SEM), and may be elongated, spherical, polygonal, or the like.
[0078] The average particle size of the granular thermoplastic polymer is preferably 0.1 μm or more and 2.0 μm or less, more preferably 0.16 μm or more and 1.5 μm or less, even more preferably 0.2 μm or more and 1.0 μm or less, and most preferably 0.3 μm or more and 0.6 μm or less, from the viewpoint of being able to maintain the distance between multiple electrodes via the separator while exerting adhesive strength with the separator electrodes, and shortening the time it takes to inject the electrolyte into the electricity storage device by reducing the contact angle of the separator surface with the electrolyte.
[0079] (Swelling degree of thermoplastic polymer in electrolyte) The thermoplastic polymer in the present embodiment preferably has swelling properties in the electrolyte from the viewpoint of battery characteristics such as cycle characteristics and the change rate of the distance between dots before and after immersion of the electrolyte in the separator as described above. The swelling degree of the thermoplastic polymer in the electrolyte is preferably 2 times or more and 15 times or less. The swelling degree of the thermoplastic polymer in the electrolyte can be measured by the method described later in the examples. The swelling degree of the thermoplastic polymer in the electrolyte in the present embodiment can be adjusted, for example, by changing the monomer components to be polymerized and the input ratio of each monomer.
[0080] (Weight per side of thermoplastic polymer-containing layer) In the separator according to the present embodiment, the basis weight per side of the thermoplastic polymer-containing layer is set to 0.03 g / m from the viewpoint of adhesive strength. 2 More than 0.3g / m 2 It is preferable that the content is 0.04 g / m or less. 2 More than 0.15g / m 2 More preferably, it is equal to or less than 0.06 g / m 2 More than 0.10g / m 2 The basis weight of the thermoplastic polymer-containing layer can be adjusted by changing the polymer concentration of the coating solution or the coating amount of the polymer solution. From the viewpoint of suppressing deformation of the cell shape due to expansion and contraction of the electrodes and improving the cycle characteristics of the battery, within a range that does not impair the effects of the present invention, it is set to 0.08 g / m 2 A range exceeding this is preferred.
[0081] (Coating of substrate surface with thermoplastic polymer-containing layer) In this embodiment, the total coverage area ratio of the thermoplastic polymer-containing layer to the substrate surface is preferably 5% to 55%, more preferably 6% to 40%, and even more preferably 7% to 30%, from the viewpoint of shortening the time for pouring the electrolyte into the power storage device including the separator while maintaining the adhesive strength between the separator and the electrodes. The total coverage area ratio S of the thermoplastic polymer-containing layer present on the substrate surface is calculated by the following formula. S(%)=total coverage area of thermoplastic polymer-containing layer÷surface area of substrate×100 The total coverage area ratio of the thermoplastic polymer-containing layer can be adjusted by changing the polymer concentration of the coating solution or the coating amount of the polymer solution, as well as the coating method and coating conditions.
[0082] In the present embodiment, from the viewpoint of shortening the time required to complete injection of an electrolyte into an electricity storage device including a separator while maintaining the adhesive strength of the separator with the electrodes, it is preferable that the above-mentioned inter-dot distance / dot diameter of the thermoplastic polymer-containing layer and the total coverage area ratio of the thermoplastic polymer-containing layer to the surface of the substrate satisfy the following relationship. Relationship 1: the distance between dots / the diameter of the dots is 1.4 or more and 4 or less, and the total coverage area ratio is 5% or more and 22% or less. In particular, from the viewpoint of achieving a better balance between the adhesive strength and the shortening of the time to complete the liquid injection, it is preferable to set the distance between dots / the diameter of the dots to 2.0 or more and 3.5 or less, and the total coverage area ratio to 6% or more and 15% or less, and to control at least one of the above-mentioned dot diameter, the basis weight per one side of the thermoplastic polymer-containing layer, and the thickness of the porous layer described below to within a predetermined range. Specifically, when controlling the dot diameter, it is preferable to set it to 200 μm or more and 800 μm or less, and when controlling the basis weight per one side of the thermoplastic polymer-containing layer, it is preferable to set it to 0.04 g / m 2 More than 0.12g / m 2 When the thickness of the porous layer is controlled, it is preferably 0.5 μm or more and 2.0 μm or less. Relationship 2: the distance between dots / diameter of dots is 0.8 to 1.3, and the total coverage area ratio is 23% to 46%. Furthermore, from the viewpoint of achieving a better balance between the adhesive strength and shortening the time to complete injection, the thickness of the polyolefin microporous film described below is preferably 9 μm or less, and more preferably 7 μm or less. Relationship 3: the inter-dot distance / dot diameter is 0.5 or more and 0.7 or less, and the total coverage area ratio is 47% or more and 55% or less. With respect to the relationship between the distance between dots / diameter of dots and the total coverage area ratio of the thermoplastic polymer-containing layer, from the viewpoint of achieving a better balance between the adhesive strength and shortening the time required to complete injection, it is preferable to adopt Relationship 1 or Relationship 2, and it is particularly preferable to adopt Relationship 2. In order to evaluate whether the balance between the adhesive strength (N / m) and the shortening of the injection completion time (min) is good, any of the following indices may be used. Index 1: Adhesive strength is 4.0 N / m or more, and the time to complete injection is 17 min or less; Index 2: Adhesive strength is 2.5N / m or more, and the time to complete injection is 15min or less; Index 3: Adhesion strength is 2.4 N / m or more, and the time to complete injection is 11 min or less; Index 4: Adhesion strength is 2.2N / m or more, and the time to complete injection is 9min or less; Index 5: Adhesive strength is 2.1 N / m or more, and the time required to complete injection is 8 minutes or less. The balance between the adhesive strength (N / m) and the shortening of the time to complete liquid injection (min) is evaluated as being better balanced when any one of the above indicators 1 to 4 is satisfied and the adhesive strength is higher and the time to complete liquid injection is shorter.
[0083] [Base material] Since the separator needs to have insulating properties and ion permeability, the separator substrate is generally formed from an insulating material having a porous structure, such as paper, a polyolefin nonwoven fabric, or a resin microporous membrane. In particular, as a separator substrate used in an electricity storage device such as a nonaqueous secondary battery having a positive electrode and a negative electrode capable of absorbing and releasing lithium and a nonaqueous electrolyte solution obtained by dissolving an electrolyte in a nonaqueous solvent, a polyolefin microporous membrane that has oxidation-reduction resistance and can form a dense and uniform porous structure is preferred.
[0084] (Polyolefin microporous membrane) The polyolefin microporous membrane in the present embodiment is not particularly limited, but may be, for example, a microporous membrane made of a polyolefin resin composition containing polyolefin, and is preferably a porous membrane mainly made of polyolefin resin. The polyolefin microporous membrane in the present embodiment is not particularly limited in the content of polyolefin resin, but from the viewpoint of shutdown performance when used as a separator for an electric storage device, it is preferable that the porous membrane is made of a polyolefin resin composition in which polyolefin resin accounts for 50% or more and 100% or less of the mass fraction of all components constituting the porous membrane. The proportion of polyolefin resin is more preferably 60% or more and 100% or less, and even more preferably 70% or more and 100% or less.
[0085] The polyolefin resin is not particularly limited, but refers to a polyolefin resin used in normal extrusion, injection, inflation, and blow molding, etc., and can be a homopolymer, copolymer, multistage polymer, etc. of ethylene, propylene, 1-butene, 4-methyl-1-pentene, 1-hexene, 1-octene, etc. Also, polyolefins selected from the group consisting of these homopolymers, copolymers, and multistage polymers can be used alone or in combination.
[0086] Representative examples of polyolefin resins include, but are not limited to, polyethylenes such as low-density polyethylene, linear low-density polyethylene, medium-density polyethylene, high-density polyethylene, and ultra-high molecular weight polyethylene, isotactic polypropylene, atactic polypropylene, ethylene-propylene random copolymer, polybutene, and ethylene-propylene rubber.
[0087] When the separator of the present embodiment is used as a battery separator, it is preferable to use polyethylene as the main component because of its low melting point and high strength, and it is particularly preferable to use a resin mainly composed of high density polyethylene. High density polyethylene is defined as polyethylene having a density of 0.942 g / cm3 as measured according to JIS K 7112. 3This refers to polyethylene having the above properties.
[0088] In addition, from the viewpoint of improving the heat resistance of the porous membrane, it is more preferable to use a porous membrane made of a resin composition containing polypropylene and a polyolefin resin other than polypropylene. Here, the three-dimensional structure of the polypropylene is not limited, and may be any of isotactic polypropylene, syndiotactic polypropylene, and atactic polypropylene.
[0089] The ratio of polypropylene to the total polyolefin in the polyolefin resin composition is not particularly limited, but from the viewpoint of achieving both heat resistance and good shutdown function, it is preferably 1 to 35 mass%, more preferably 3 to 20 mass%, and even more preferably 4 to 10 mass%. In this case, there is no limitation on the polyolefin resin other than polypropylene, and examples thereof include homopolymers or copolymers of olefin hydrocarbons such as ethylene, 1-butene, 4-methyl-1-pentene, 1-hexene, and 1-octene. Specific examples include polyethylene, polybutene, and ethylene-propylene random copolymers.
[0090] From the viewpoint of the shutdown property in which the pores are closed by thermal melting, it is preferable to use polyethylene such as low density polyethylene, linear low density polyethylene, medium density polyethylene, high density polyethylene, and ultra-high molecular weight polyethylene as the polyolefin resin other than polypropylene. Among these, from the viewpoint of strength, it is preferable to use polyethylene having a density of 0.93 g / cm as measured according to JIS K 7112. 3 More than 0.97g / cm 3 It is more preferable to use polyethylene that is:
[0091] The viscosity average molecular weight of the polyolefin resin constituting the polyolefin microporous membrane is not particularly limited, but is preferably 30,000 to 12 million, more preferably 50,000 to less than 2 million, even more preferably 100,000 to less than 1.2 million, and most preferably 500,000 to less than 1 million. When the viscosity average molecular weight is 30,000 or more, the melt tension during melt molding becomes large, improving moldability, and the strength tends to be high due to entanglement between polymers. On the other hand, when the viscosity average molecular weight is 12 million or less, it is preferable because it is easy to uniformly melt-knead, and the moldability of the sheet, especially the thickness stability, tends to be excellent. Furthermore, when the viscosity average molecular weight is less than 1 million, it is preferable because the pores are easily blocked when the temperature rises, and a good shutdown function tends to be obtained. For example, instead of using a polyolefin having a viscosity average molecular weight of less than 1 million alone, a mixture of a polyolefin having a viscosity average molecular weight of 2 million and a polyolefin having a viscosity average molecular weight of 270,000, the viscosity average molecular weight of which is less than 1 million, may be used.
[0092] The polyolefin microporous film in the present embodiment may contain any additive. Such additives are not particularly limited, and examples thereof include polymers other than polyolefins; inorganic particles; antioxidants such as phenols, phosphorus, and sulfur; metal soaps such as calcium stearate and zinc stearate; ultraviolet absorbers; light stabilizers; antistatic agents; antifogging agents; and coloring pigments. The total content of these additives is preferably 20 parts by mass or less, more preferably 10 parts by mass or less, and even more preferably 5 parts by mass or less, relative to 100 parts by mass of the polyolefin resin composition.
[0093] (Physical properties of microporous polyolefin membrane) Polyolefin microporous membrane weight (g / m 2 The puncture strength when converted to 50gf / (g / m 2 ) or more, or 60gf / (g / m 2 ) or more. 2 ) or more than 60gf / (g / m2 A polyolefin microporous membrane having a puncture strength converted into basis weight of 70 gf / (g / m) or more tends to be less likely to break in an impact test of an electricity storage device. From the viewpoint of improving the safety, for example, impact resistance, of an electricity storage device while maintaining the strength of the polyolefin microporous membrane, the puncture strength converted into basis weight is more preferably 70 gf / (g / m) or more. 2 ) or more, more preferably 80 gf / (g / m 2 ) or more. The puncture strength converted into basis weight is not limited, but is, for example, 200 gf / (g / m 2 ) or less, 150gf / (g / m 2 ) or less, or 140gf / (g / m 2 ) or less. Note that the CCS unit "gf" can be converted to the SI unit "N" according to the formula: 1N ≈ 102.0 gf.
[0094] The lower limit of the pin puncture strength of the polyolefin microporous film not converted into basis weight (hereinafter simply referred to as pin puncture strength) is preferably 100 gf or more, more preferably 200 gf or more, and even more preferably 300 or more. A pin puncture strength of 100 gf or more is preferable from the viewpoint of suppressing breakage of the polyolefin microporous film in an impact test. In addition, the upper limit of the pin puncture strength of the polyolefin microporous film is preferably 1000 gf or less, more preferably 800 gf or less, and even more preferably 700 gf or less from the viewpoint of stability during film formation. The lower limit can be used as long as it allows stable production of film formation and battery production. The upper limit is set in balance with other properties. The pin puncture strength can be increased by increasing the shear force applied to the molded product during extrusion or by increasing the orientation of the molecular chains due to stretching, but the thermal stability is deteriorated due to an increase in residual stress as the strength increases, so it is controlled according to the purpose.
[0095] The porosity of the polyolefin microporous film in the present embodiment is not particularly limited, but is preferably 20% or more, more preferably 35% or more, even more preferably 40% or more, and is preferably 80% or less, more preferably 60% or less, even more preferably 55% or less, and particularly preferably 50% or less. A porosity of 20% or more is preferable from the viewpoint of ensuring the permeability of the separator. On the other hand, a porosity of 80% or less is preferable from the viewpoint of ensuring the pin puncture strength. In addition, a porosity of 50% or less is preferable from the viewpoint of shortening the injection time since the amount of electrolyte to be filled can be reduced. The porosity can be adjusted by changing the stretching ratio, etc.
[0096] The thickness of the polyolefin microporous membrane in the present embodiment is not particularly limited, but is preferably 2 μm or more, more preferably 4 μm or more, and even more preferably 5 μm or more, and its upper limit is preferably 30 μm or less, more preferably 20 μm or less, even more preferably 16 μm or less, even more preferably 12 μm or less, particularly preferably 9 μm or less, and most preferably 7 μm or less. A membrane thickness of 2 μm or more is preferable from the viewpoint of improving mechanical strength. On the other hand, a membrane thickness of 30 μm or less is preferable because it tends to be advantageous in terms of increasing the capacity of the battery since the volume occupied by the separator is reduced. In addition, a membrane thickness of 12 μm or less, 9 μm or less, or 7 μm or less is preferable from the viewpoint of shortening the injection time since the electrolyte filling amount can be reduced.
[0097] The air permeability of the polyolefin microporous membrane in the present embodiment is not particularly limited, but is preferably 10 sec / 100 cm 3 More than 20sec / 100cm, more preferably 20sec / 100cm 3 More preferably, 30 sec / 100 cm 3 and most preferably 40 sec / 100 cm 3 and preferably 300 sec / 100 cm 3 Less than 200sec / 100cm, more preferably 3 More preferably, it is 180 sec / 100 cm or less. 3and more preferably 140 sec / 100 cm 3 The air permeability is 10sec / 100cm 3 It is preferable to set the air permeability to 500 sec / 100 cm or more from the viewpoint of suppressing self-discharge of the electricity storage device. 3 It is preferable from the viewpoint of obtaining good charge / discharge characteristics to set the air permeability as follows: The air permeability can be adjusted by changing the stretching temperature, the stretching ratio, and the like.
[0098] The average pore size of the polyolefin microporous membrane in this embodiment is preferably 0.15 μm or less, more preferably 0.1 μm or less, and the lower limit is preferably 0.01 μm or more. When used as a separator for an electricity storage device, an average pore size of 0.15 μm or less is suitable from the viewpoint of suppressing self-discharge of the electricity storage device and suppressing a decrease in capacity. The average pore size can be adjusted by changing the stretching ratio when producing the polyolefin microporous membrane.
[0099] The short circuit temperature, which is an index of heat resistance of the polyolefin microporous membrane in this embodiment, is preferably not less than 140° C., more preferably not less than 150° C., and even more preferably not less than 160° C. A short circuit temperature of not less than 140° C. is preferable when the membrane is used as a separator for an electricity storage device, from the viewpoint of safety of the electricity storage device.
[0100] The viscosity average molecular weight of the polyolefin microporous membrane in the present embodiment is not particularly limited, but is preferably from 100,000 to 5 million, more preferably from 300,000 to 1.5 million, and even more preferably from 500,000 to 1 million. A viscosity average molecular weight of from 100,000 to 5 million is preferred from the viewpoints of the pin puncture strength, permeability, heat shrinkage, and shutdown function of the polyolefin microporous membrane.
[0101] (Method of producing a microporous polyolefin membrane) The method for producing the polyolefin microporous film in the present embodiment is not particularly limited, and known production methods can be adopted.For example, the method of melt-kneading a polyolefin resin composition and a plasticizer to form a sheet, and then stretching it as necessary, and then extracting the plasticizer to make it porous; the method of melt-kneading a polyolefin resin composition and extruding it at a high draw ratio, and then peeling the polyolefin crystal interface by heat treatment and stretching to make it porous; the method of melt-kneading a polyolefin resin composition and an inorganic filler to form it on a sheet, and then peeling the interface between the polyolefin and the inorganic filler by stretching to make it porous; the method of dissolving a polyolefin resin composition, immersing it in a poor solvent for polyolefin, solidifying the polyolefin, and simultaneously removing the solvent to make it porous, etc. are mentioned below.As an example of the method for producing a porous film, the method of melt-kneading a polyolefin resin composition and a plasticizer to form it into a sheet, and then extracting the plasticizer is described.
[0102] First, the polyolefin resin composition and the plasticizer are melt-kneaded. As a melt-kneading method, for example, a method in which a polyolefin resin and other additives as necessary are put into a resin kneading device such as an extruder, a kneader, a lab plastomill, a kneading roll, a Banbury mixer, etc., and a plasticizer is introduced at an arbitrary ratio while heating and melting the resin components, and kneaded. In this case, it is preferable to pre-knead the polyolefin resin, other additives, and the plasticizer in a predetermined ratio using a Henschel mixer or the like before putting them into the resin kneading device. More preferably, only a part of the plasticizer is put in the pre-kneading, and the remaining plasticizer is kneaded while being side-fed into the resin kneading device. By doing so, the dispersibility of the plasticizer is improved, and when a sheet-shaped molded body of the melt-kneaded mixture of the resin composition and the plasticizer is stretched in a later process, it can be stretched at a high ratio without breaking the film.
[0103] As the plasticizer, a non-volatile solvent capable of forming a homogeneous solution at or above the melting point of the polyolefin can be used. Specific examples of such non-volatile solvents include, for example, hydrocarbons such as liquid paraffin and paraffin wax; esters such as dioctyl phthalate and dibutyl phthalate; and higher alcohols such as oleyl alcohol and stearyl alcohol. Among these, liquid paraffin is preferred because it has high compatibility with polyethylene and polypropylene, and even when the molten kneaded product is stretched, the interfacial peeling between the resin and the plasticizer is unlikely to occur, which tends to facilitate uniform stretching.
[0104] The ratio of the polyolefin resin composition and the plasticizer is not particularly limited as long as they can be uniformly melt-kneaded and molded into a sheet. For example, the mass fraction of the plasticizer in the composition consisting of the polyolefin resin composition and the plasticizer is preferably 30 to 80 mass%, more preferably 40 to 70 mass%. When the mass fraction of the plasticizer is 80 mass% or less, the melt tension during melt molding is unlikely to be insufficient, and moldability tends to be improved. On the other hand, when the mass fraction is 30 mass% or more, even if the mixture of the polyolefin resin composition and the plasticizer is stretched at a high ratio, the polyolefin chain does not break, a uniform and fine pore structure is formed, and the strength is likely to increase.
[0105] Next, the molten mixture is molded into a sheet. As a method for producing a sheet-shaped molded product, for example, the molten mixture is extruded into a sheet through a T-die or the like, and is brought into contact with a heat conductor to a temperature sufficiently lower than the crystallization temperature of the resin component to solidify it. As the heat conductor used for cooling and solidifying, metal, water, air, or the plasticizer itself can be used, but a metal roll is preferred because it has high heat conduction efficiency. In this case, when the sheet is brought into contact with the metal roll, it is more preferred to sandwich the sheet between the rolls, since the efficiency of heat conduction is further increased, the sheet is oriented, the film strength is increased, and the surface smoothness of the sheet is improved. When extruding the sheet into a sheet from a T-die, the die lip interval is preferably 400 μm or more and 3000 μm or less, and more preferably 500 μm or more and 2500 μm or less. When the die lip interval is 400 μm or more, the amount of scum is reduced, and the influence on the film quality such as streaks and defects is small, and film breakage and the like in the subsequent stretching process tends to be prevented. On the other hand, when the die lip distance is 3000 μm or less, the cooling rate is fast, which makes it possible to prevent uneven cooling and tends to maintain the thickness stability of the sheet.
[0106] It is preferable to stretch the sheet-like molded body thus obtained. As the stretching process, either uniaxial stretching or biaxial stretching can be suitably used, but biaxial stretching is preferable from the viewpoint of the strength of the obtained porous film. When the sheet-like molded body is stretched in the biaxial direction at a high magnification, the molecules are oriented in the plane direction, and the finally obtained porous film is less likely to tear and has high puncture strength. Examples of the stretching method include simultaneous biaxial stretching, sequential biaxial stretching, multi-stage stretching, and multiple stretching, and simultaneous biaxial stretching is preferable from the viewpoint of improving puncture strength, uniformity of stretching, and shutdown property.
[0107] Here, simultaneous biaxial stretching refers to a stretching method in which stretching in the MD direction (machine direction of the microporous membrane) and stretching in the TD direction (direction crossing the MD of the microporous membrane at an angle of 90°) are performed simultaneously, and the stretching ratios in each direction may be different. Sequential biaxial stretching refers to a stretching method in which stretching in the MD direction or the TD direction is performed independently, and while stretching is performed in the MD direction or the TD direction, the other direction is in an unconstrained state or fixed at a fixed length.
[0108] The stretching ratio is preferably in the range of 20 times or more and 100 times or less in area ratio, more preferably in the range of 25 times or more and 50 times or less. The stretching ratio in each axial direction is preferably in the range of 4 times or more and 10 times or less in MD direction, and 4 times or more and 10 times or less in TD direction, more preferably in the range of 5 times or more and 8 times or less in MD direction, and 5 times or more and 8 times or less in TD direction. If the total area ratio is 20 times or more, the obtained porous membrane tends to have sufficient strength, while if the total area ratio is 100 times or less, the membrane breakage in the stretching process is prevented and high productivity tends to be obtained.
[0109] The sheet-like molded body may also be rolled. Rolling can be performed, for example, by a pressing method using a double belt press or the like. Rolling can increase the orientation of the surface layer part in particular. The rolling area ratio is preferably greater than 1 and less than 3 times, and more preferably greater than 1 and less than 2 times. If the rolling ratio is greater than 1, the surface orientation increases and the membrane strength of the finally obtained porous membrane tends to increase. On the other hand, if the rolling ratio is 3 times or less, the orientation difference between the surface layer part and the central interior is small, and a uniform porous structure tends to be formed in the thickness direction of the membrane, which is preferable.
[0110] Next, the plasticizer is removed from the sheet-shaped molded body to obtain a porous membrane. For example, a method for removing the plasticizer includes a method of immersing the sheet-shaped molded body in an extraction solvent to extract the plasticizer and then drying the sheet-shaped molded body sufficiently. The method for extracting the plasticizer may be either a batch method or a continuous method. In order to suppress the shrinkage of the porous membrane, it is preferable to restrain the end of the sheet-shaped molded body during a series of steps of immersion and drying. In addition, it is preferable that the amount of plasticizer remaining in the porous membrane is less than 1% by mass.
[0111] As the extraction solvent, it is preferable to use one that is a poor solvent for polyolefin resin and a good solvent for plasticizer, and has a boiling point lower than the melting point of polyolefin resin. Examples of such extraction solvents include hydrocarbons such as n-hexane and cyclohexane; halogenated hydrocarbons such as methylene chloride and 1,1,1-trichloroethane; non-chlorine halogenated solvents such as hydrofluoroether and hydrofluorocarbon; alcohols such as ethanol and isopropanol; ethers such as diethyl ether and tetrahydrofuran; and ketones such as acetone and methyl ethyl ketone. These extraction solvents may be recovered and reused by operations such as distillation.
[0112] In order to suppress the shrinkage of the porous membrane, a heat treatment such as heat setting or heat relaxation may be performed after the stretching step or after the formation of the porous membrane. The porous membrane may also be subjected to post-treatment such as hydrophilization treatment with a surfactant or crosslinking treatment with ionizing radiation.
[0113] [Porous layer] The separator for an electric storage device according to the present embodiment may also include a porous layer containing an inorganic filler and a resin binder. The position of the porous layer may be at least a part of the surface of the polyolefin microporous membrane, at least a part of the surface of the thermoplastic polymer-containing layer, and / or between the polyolefin microporous membrane and the thermoplastic polymer-containing layer. The porous layer may be provided on one or both sides of the polyolefin microporous membrane. The porous layer contributes to improving thermal stability, etc. Hereinafter, a microporous membrane provided with a porous layer is referred to as a multilayer porous membrane.
[0114] (Inorganic filler) The inorganic filler used in the porous layer is not particularly limited, but is preferably one that has a melting point of 200° C. or higher, has high electrical insulation properties, and is electrochemically stable within the range of use of lithium ion secondary batteries.
[0115] Examples of inorganic filler materials include oxide ceramics such as alumina, silica, titania, zirconia, magnesia, ceria, yttria, zinc oxide, and iron oxide; nitride ceramics such as silicon nitride, titanium nitride, and boron nitride; ceramics such as silicon carbide, calcium carbonate, magnesium sulfate, aluminum sulfate, barium sulfate, aluminum hydroxide, aluminum oxide hydroxide, or boehmite, potassium titanate, talc, kaolinite, dickite, nacrite, halloysite, pyrophyllite, montmorillonite, sericite, mica, amesite, bentonite, asbestos, zeolite, calcium silicate, magnesium silicate, diatomaceous earth, and silica sand; and glass fibers. Among these, at least one selected from the group consisting of alumina, boehmite, and barium sulfate is preferred from the viewpoint of stability in a lithium ion secondary battery. In addition, as the boehmite, synthetic boehmite is preferred, which can reduce ionic impurities that adversely affect the characteristics of an electrochemical element.
[0116] Examples of the shape of the inorganic filler include plate-like, scaly, polyhedral, needle-like, columnar, granular, spherical, spindle-like, block-like, etc., and a combination of a plurality of inorganic fillers having the above shapes may be used. Among these, the block shape is preferred from the viewpoint of the balance between permeability and heat resistance.
[0117] The aspect ratio of the inorganic filler is preferably 1.0 to 5.0, more preferably 1.1 to 3.0. The aspect ratio of 5.0 or less is preferable from the viewpoint of suppressing the amount of moisture adsorption of the multilayer porous membrane and suppressing capacity deterioration during repeated cycles, and from the viewpoint of suppressing deformation at a temperature exceeding the melting point of the polyolefin microporous membrane.
[0118] The specific surface area of the inorganic filler is 3.0 m 2 / g or more 17m 2 / g or less, and more preferably 5.0m 2 / g or more 15m 2 / g or less, more preferably 6.5m 2 / g or more 13m 2 / g or less. The specific surface area is 17m 2 / g or less is preferable from the viewpoint of suppressing the amount of moisture adsorbed by the multilayer porous membrane and suppressing the capacity deterioration during repeated cycles. 2 / g or more is preferable from the viewpoint of suppressing deformation at a temperature exceeding the melting point of the polyolefin microporous membrane. The specific surface area of the inorganic filler is measured by the BET adsorption method.
[0119] In the particle size distribution of a slurry containing inorganic filler, the average particle size D of inorganic particles 50 is preferably 0.10 μm or more and 1.40 μm or less, more preferably 0.20 μm or more and 0.80 μm or less, and even more preferably 0.25 μm or more and 0.50 μm or less. 50 It is preferable that the multilayer porous film has a diameter of 0.10 μm or more in order to suppress the amount of moisture adsorbed by the multilayer porous film and to suppress the deterioration of the capacity when the multilayer porous film is cycled. 50 It is preferable for the microporous polyolefin membrane to have a thickness of 1.40 μm or less in terms of suppressing deformation at a temperature exceeding the melting point of the membrane.
[0120] In addition, in the particle size distribution of the slurry containing inorganic filler, the D 10 is preferably 0.08 μm or more and 0.80 μm or less, more preferably 0.09 μm or more and 0.50 μm or less, and even more preferably 0.10 μm or more and 0.35 μm or less. 10 It is preferable that the multilayer porous film has a diameter of 0.08 μm or more in order to suppress the amount of moisture adsorbed by the multilayer porous film and to suppress the deterioration of the capacity when the multilayer porous film is cycled. 10 It is preferable for the thickness to be 0.80 μm or less from the viewpoint of suppressing deformation at a temperature exceeding the melting point of the polyolefin microporous membrane.
[0121] Methods for adjusting the particle size distribution of the inorganic filler as described above include, for example, a method of pulverizing the inorganic filler using a ball mill, bead mill, jet mill, etc. to obtain the desired particle size distribution, and a method of preparing fillers with multiple particle size distributions and then blending them.
[0122] The proportion of the inorganic filler in the porous layer can be appropriately determined from the viewpoints of the adhesiveness of the inorganic filler, the permeability and heat resistance of the multilayer porous membrane, etc., but is preferably from 50% by mass to less than 100% by mass, more preferably from 70% by mass to 99.99% by mass, even more preferably from 80% by mass to 99.9% by mass, and particularly preferably from 90% by mass to 99% by mass.
[0123] (Resin binder) The type of resin binder is not particularly limited, but when the multilayer porous membrane in the present embodiment is used as a separator for a lithium ion secondary battery, it is preferable to use a resin binder that is insoluble in the electrolyte of the lithium ion secondary battery and is electrochemically stable within the range of use of the lithium ion secondary battery.
[0124] Specific examples of the resin binder include the following 1) to 7). 1) Polyolefins: for example, polyethylene, polypropylene, ethylene propylene rubber, and modified products thereof; 2) Conjugated diene polymers: for example, styrene-butadiene copolymers and their hydrogenated products, acrylonitrile-butadiene copolymers and their hydrogenated products, acrylonitrile-butadiene-styrene copolymers and their hydrogenated products; 3) Acrylic polymers: for example, methacrylate-acrylate copolymers, styrene-acrylate copolymers, acrylonitrile-acrylate copolymers; 4) Polyvinyl alcohol-based resins: for example, polyvinyl alcohol, polyvinyl acetate; 5) Fluorine-containing resins: for example, polyvinylidene fluoride, polytetrafluoroethylene, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene copolymer, ethylene-tetrafluoroethylene copolymer; 6) Cellulose derivatives: for example, ethyl cellulose, methyl cellulose, hydroxyethyl cellulose, carboxymethyl cellulose; 7) Resins having a melting point and / or glass transition temperature of 180°C or higher, or polymers having no melting point but a decomposition temperature of 200°C or higher: for example, polyphenylene ether, polysulfone, polyethersulfone, polyphenylene sulfide, polyetherimide, polyamideimide, polyamide, and polyester.
[0125] From the viewpoint of further improving safety in the event of a short circuit, 3) acrylic polymers, 5) fluorine-containing resins, and 7) polyamides as polymers are preferred. As polyamides, from the viewpoint of durability, wholly aromatic polyamides, particularly polymetaphenylene isophthalamide, are preferred.
[0126] From the viewpoint of compatibility between the resin binder and the electrodes, the above 2) conjugated diene polymer is preferred, and from the viewpoint of voltage resistance, the above 3) acrylic polymer and 5) fluorine-containing resin are preferred.
[0127] The above-mentioned 2) conjugated diene polymer is a polymer containing a conjugated diene compound as a monomer unit.
[0128] Examples of the conjugated diene compound include 1,3-butadiene, 2-methyl-1,3-butadiene, 2,3-dimethyl-1,3-butadiene, 2-chloro-1,3-butadiene, substituted linear conjugated pentadiene, substituted and side chain conjugated hexadienes, etc., which may be used alone or in combination of two or more. Among these, 1,3-butadiene is particularly preferred.
[0129] The acrylic polymer (3) is a polymer containing a (meth)acrylic compound as a monomer unit. The (meth)acrylic compound is at least one selected from the group consisting of (meth)acrylic acid and (meth)acrylic acid esters.
[0130] Examples of the (meth)acrylic acid ester used in the acrylic polymer 3) above include (meth)acrylic acid alkyl esters, such as methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, butyl acrylate, butyl methacrylate, 2-ethylhexyl acrylate, and 2-ethylhexyl methacrylate; and epoxy group-containing (meth)acrylic acid esters, such as glycidyl acrylate and glycidyl methacrylate; and these may be used alone or in combination of two or more. Among the above, 2-ethylhexyl acrylate (EHA) and butyl acrylate (BA) are particularly preferred.
[0131] From the viewpoint of safety in a crash test, the acrylic polymer is preferably a polymer containing EHA or BA as a main structural unit. The main structural unit refers to a polymer portion corresponding to a monomer that accounts for 40 mol % or more of the total raw materials for forming the polymer.
[0132] The above 2) conjugated diene polymer and 3) acrylic polymer may be obtained by copolymerizing other monomers copolymerizable therewith. Examples of the copolymerizable other monomers used include unsaturated carboxylic acid alkyl esters, aromatic vinyl monomers, cyanide vinyl monomers, unsaturated monomers containing hydroxyalkyl groups, unsaturated carboxylic acid amide monomers, crotonic acid, maleic acid, maleic anhydride, fumaric acid, itaconic acid, etc., which may be used alone or in combination of two or more. Among the above, unsaturated carboxylic acid alkyl ester monomers are particularly preferred. Examples of unsaturated carboxylic acid alkyl ester monomers include dimethyl fumarate, diethyl fumarate, dimethyl maleate, diethyl maleate, dimethyl itaconate, monomethyl fumarate, monoethyl fumarate, etc., which may be used alone or in combination of two or more.
[0133] The above-mentioned 2) conjugated diene polymer may be one obtained by copolymerizing the above-mentioned (meth)acrylic compound as another monomer.
[0134] The resin binder is preferably in the form of latex, and more preferably in the form of an acrylic polymer latex, from the viewpoint of providing strong binding force between multiple inorganic particles even at high temperatures exceeding room temperature and suppressing thermal shrinkage.
[0135] The average particle size of the resin binder is preferably 50 to 500 nm, more preferably 60 to 460 nm, and even more preferably 80 to 250 nm. When the average particle size of the resin binder is 50 nm or more, when a porous layer containing an inorganic filler and a binder is laminated on at least one side of a polyolefin porous membrane, ion permeability is unlikely to decrease, and high output characteristics are easily obtained. In addition, even when the temperature rises rapidly during abnormal heat generation, smooth shutdown characteristics are exhibited, and high safety is easily obtained. When the average particle size of the resin binder is 500 nm or less, good binding properties are exhibited, and when the porous membrane is formed into a multilayer porous membrane, heat shrinkage is good, and safety tends to be excellent.
[0136] The average particle size of the resin binder can be controlled by adjusting the polymerization time, polymerization temperature, raw material composition ratio, raw material charging order, pH, and the like.
[0137] A dispersant such as a surfactant may be added to the coating liquid to stabilize the dispersion or improve the coatability. The dispersant is adsorbed to the surface of inorganic particles in the slurry and stabilizes the inorganic particles by electrostatic repulsion, and is, for example, a polycarboxylate, a sulfonate, or a polyoxyether. The amount of the dispersant added is preferably 0.2 parts by weight or more and 5.0 parts by weight or less, and more preferably 0.3 parts by weight or more and 1.0 parts by weight or less, calculated as a solid content, relative to 100 parts by weight of the inorganic filler.
[0138] (Properties, composition and formation method of porous layer) The thickness of the porous layer is preferably 0.5 μm or more and 5.0 μm or less, more preferably 0.7 μm or more and 4.0 μm or less, even more preferably 0.8 μm or more and 3.9 μm or less, even more preferably 1.0 μm or more and 3.0 μm or less, and particularly preferably 1.5 μm or more and 2.0 μm or less. The thickness of the porous layer is preferably 0.5 μm or more from the viewpoint of suppressing deformation at a temperature exceeding the melting point of the porous membrane. The thickness of the porous layer is preferably 5.0 μm or less from the viewpoint of improving the battery capacity and suppressing the amount of water adsorption of the multilayer porous membrane. In addition, the thickness of the porous layer is preferably 3.9 μm or less, more preferably 2.0 μm or less from the viewpoint of shortening the injection time since the electrolyte filling amount can be reduced.
[0139] The layer density in the porous layer is 1.10 g / (m 2 ·μm) or more 3.00g / (m 2 .μm) or less, and more preferably 1.20 g / (m 2 ·μm) or more 2.90g / (m 2 ·μm), and more preferably 1.40 g / (m 2 ·μm) or more 2.70g / (m 2 ·μm), particularly preferably 1.50 g / (m 2 ·μm) or more 2.50g / (m 2The layer density in the porous layer is 1.10 g / (m 2 It is preferable that the layer density in the porous layer is 3.00 g / (m 2 ) or more in order to suppress deformation at a temperature exceeding the melting point of the polyolefin microporous membrane. 2 A thickness of 1.0 μm or less is preferable from the viewpoints of maintaining the ion permeability of the porous layer and suppressing deterioration of capacity when cycles are repeated.
[0140] An example of a method for forming the porous layer is a method in which a coating liquid containing an inorganic filler and a resin binder is applied to at least one surface of a porous film mainly composed of a polyolefin resin to form a porous layer.
[0141] The solvent for the coating liquid is preferably one in which the inorganic filler and the resin binder can be uniformly and stably dispersed, and examples thereof include N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, water, ethanol, toluene, hot xylene, methylene chloride, and hexane.
[0142] In order to stabilize the dispersion and improve the coatability, various additives such as dispersants such as surfactants, thickeners, wetting agents, antifoaming agents, and pH adjusters containing acids and alkalis may be added to the coating liquid. These additives are preferably ones that can be removed when the solvent is removed, but they may remain in the porous layer as long as they are electrochemically stable within the range of use of the lithium ion secondary battery, do not inhibit the battery reaction, and are stable up to about 200°C.
[0143] The method for dispersing the inorganic filler and the resin binder in the solvent of the coating liquid is not particularly limited as long as it can realize the dispersion characteristics of the coating liquid required for the coating step, for example, a ball mill, a bead mill, a planetary ball mill, a vibrating ball mill, a sand mill, a colloid mill, an attritor, a roll mill, high-speed impeller dispersion, a disperser, a homogenizer, a high-speed impact mill, ultrasonic dispersion, mechanical stirring with a stirring blade, etc. can be mentioned.
[0144] The method for applying the coating liquid to the microporous membrane is not particularly limited as long as it is a method that can realize the required layer thickness and coating area, and examples include a gravure coater method, a small diameter gravure coater method, a reverse roll coater method, a transfer roll coater method, a kiss coater method, a dip coater method, a knife coater method, an air doctor coater method, a blade coater method, a rod coater method, a squeeze coater method, a cast coater method, a die coater method, a screen printing method, a spray coating method, and the like.
[0145] Furthermore, it is preferable to subject the surface of the microporous membrane as the separator substrate to a surface treatment prior to application of the coating liquid, since this makes it easier to apply the coating liquid and improves the adhesion between the inorganic filler-containing porous layer and the microporous membrane surface after application. The method of surface treatment is not particularly limited as long as it does not significantly impair the porous structure of the microporous membrane, and examples of the method include a corona discharge treatment method, a mechanical roughening method, a solvent treatment method, an acid treatment method, and an ultraviolet oxidation method.
[0146] The method for removing the solvent from the coating film after coating is not particularly limited as long as it does not adversely affect the microporous film, and examples thereof include a method in which the porous film is dried at a temperature below its melting point while being fixed, a method in which the porous film is dried under reduced pressure at a low temperature, etc. From the viewpoint of controlling the shrinkage stress in the MD direction of the porous film and the multilayer porous film, it is preferable to appropriately adjust the drying temperature, winding tension, etc.
[0147] [Separator properties and composition] From the viewpoints of excellent electrolyte injectability, less air pockets, and a short injection time, the separator preferably has a contact angle of the electrolyte of 0° to 20°, more preferably 2° to 18°, and even more preferably 4° to 16°. The contact angle of the electrolyte is preferably measured on the surface of the separator on which the thermoplastic polymer-containing layer is formed, and more preferably on the surface of the separator on which the thermoplastic polymer-containing layer is formed in a dot pattern.
[0148] The lower limit of the thickness of the separator for an electricity storage device is preferably 2.5 μm or more, more preferably 4.5 μm or more, and even more preferably 5.5 μm or more from the viewpoint of ensuring the strength of the separator for an electricity storage device. On the other hand, the upper limit of the thickness of the separator for an electricity storage device is preferably 35 μm or less, more preferably 18 μm or less, from the viewpoint of obtaining good charge / discharge characteristics, and is even more preferably 14 μm or less, particularly preferably 12 μm or less, and most preferably 8 μm or less, from the viewpoint of achieving both good charge / discharge characteristics and pourability.
[0149] The lower limit of the air permeability of the separator for the electricity storage device is preferably 10 sec / 100 cm 3 More than 20sec / 100cm, more preferably 20sec / 100cm 3 More preferably, 30 sec / 100 cm 3 and most preferably 40 sec / 100 cm 3 The upper limit is preferably 500 sec / 100 cm 3 Less than 300sec / 100cm, more preferably 300sec / 100cm 3 Less than 200sec / 100cm, more preferably 3 The air permeability is 10sec / 100cm 3 When the separator is used for an electricity storage device, it is preferable from the viewpoint of further suppressing self-discharge of the electricity storage device. 3 The following is preferable from the viewpoint of obtaining good charge / discharge characteristics. The air permeability of the separator for an electricity storage device can be adjusted by changing the stretching temperature and stretching ratio when producing the polyolefin microporous membrane, the total covering area ratio of the thermoplastic polymer-containing layer, the existence form, etc.
[0150] The power storage device separator has a shutdown temperature, which is an indicator of the safety of the power storage device, of preferably 160°C or lower, more preferably 155°C or lower, even more preferably 150°C or lower, and most preferably 145°C or lower.
[0151] The separator for an electricity storage device has a short-circuit temperature, which is an index of heat resistance, of preferably 140° C. or higher, more preferably 150° C. or higher, and further preferably 160° C. or higher. When the separator is used for an electricity storage device, a short-circuit temperature of 160° C. or higher is preferable from the viewpoint of safety of the electricity storage device.
[0152] From the viewpoint of efficiently exerting the effects of the present invention, the separator preferably has an asymmetric multilayer structure based on the substrate, and more preferably has a multilayer structure in which a thermoplastic polymer-containing layer is provided on both sides of the substrate, and a porous layer containing an inorganic filler and a resin binder is formed between one side of the substrate and the thermoplastic polymer-containing layer. An asymmetric structure in which a porous layer containing an inorganic filler and a resin binder is formed only on one side of the substrate is preferred from the viewpoints of improving productivity by simplifying the coating process and improving adhesive strength.
[0153] [Separator manufacturing method] The method for forming a thermoplastic polymer-containing layer on a polyolefin microporous membrane is not particularly limited, and examples thereof include a method of coating a coating liquid containing a thermoplastic polymer onto a polyolefin microporous membrane.
[0154] The method of applying the coating solution containing a thermoplastic polymer to the polyolefin microporous membrane is not particularly limited as long as it can achieve the required layer thickness and coating area. For example, gravure coater method, small diameter gravure coater method, reverse roll coater method, transfer roll coater method, kiss coater method, dip coater method, knife coater method, air doctor coater method, blade coater method, rod coater method, squeeze coater method, cast coater method, die coater method, screen printing method, spray coating method, spray coater coating method, inkjet coating method, etc. can be mentioned. Among these, gravure coater method or spray coating method is preferred from the viewpoint of high degree of freedom of the coating shape of the thermoplastic polymer and easy to obtain a preferred area ratio. In addition, from the viewpoint of adjusting the dot pattern of the thermoplastic polymer-containing layer as described above, gravure coater method, inkjet coating, and coating method that is easy to adjust the printing plate are preferred.
[0155] When a thermoplastic polymer is coated onto a polyolefin microporous membrane, if the coating liquid penetrates into the interior of the microporous membrane, the adhesive resin fills the surfaces and interiors of the pores, reducing permeability. Therefore, a poor solvent for the thermoplastic polymer is preferred as a medium for the coating liquid.
[0156] When a poor solvent for the thermoplastic polymer is used as the medium for the coating liquid, the coating liquid does not penetrate into the microporous membrane, and the adhesive polymer is mainly present on the surface of the microporous membrane, which is preferable from the viewpoint of suppressing the decrease in permeability. As such a medium, water is preferable. In addition, the medium that can be used in combination with water is not particularly limited, but may include ethanol, methanol, etc.
[0157] From the viewpoint of adjusting the dot pattern of the thermoplastic polymer-containing layer as described above, it is preferable to optimize the thermoplastic polymer-containing coating liquid (also simply called paint) using the thermoplastic polymer, poor solvent, etc. described above.
[0158] For the thermoplastic polymer-containing coating solution, from the viewpoint of adjusting the contact angle of the thermoplastic polymer-containing layer or separator with the electrolyte within the numerical range described above, the paint viscosity is preferably within the range of 30 mPa·s to 100 mPa·s, and more preferably within the range of 50 mPa·s to 80 mPa·s. If the paint viscosity is within the range described above, the appropriate thickening suppresses leveling, and the dot surface is provided with an uneven structure of the thermoplastic polymer particles, tending to improve wettability.
[0159] For the thermoplastic polymer-containing coating solution, from the viewpoint of adjusting the contact angle of the thermoplastic polymer-containing layer or separator with the electrolyte within the above-described numerical range, the paint pH is preferably within the range of 5 to 7.9, more preferably within the range of 5.5 to 7.7. The paint pH within the above-described range can appropriately suppress electrostatic repulsion and reduce dispersion stability, thereby suppressing close-packing of the thermoplastic polymer particles in the drying process, thereby improving wettability due to the uneven structure of the thermoplastic polymer particles.
[0160] Furthermore, it is preferable to subject the microporous membrane as the separator substrate to a surface treatment prior to coating, since this makes it easier to apply the coating liquid and improves the adhesion between the microporous membrane or porous layer and the adhesive polymer. The method of surface treatment is not particularly limited as long as it does not significantly impair the porous structure of the microporous membrane, and examples of the method include corona discharge treatment, plasma treatment, mechanical roughening, solvent treatment, acid treatment, and ultraviolet oxidation.
[0161] In the case of the corona discharge treatment method, from the viewpoint of adjusting the contact angle of the thermoplastic polymer-containing layer or the separator with the electrolyte to within the above-described numerical range, the corona treatment intensity of the substrate surface is 1 W / (m 2 / min) or more 40W / (m 2 / min) or less, and 3W / (m 2 / min) or more 32W / (m 2 / min) or less, and more preferably 5W / (m 2 / min) or more 25W / (m2 / min) or less. By using a corona treatment intensity within the above range, the affinity with the electrolyte is improved by introducing a hydrophilic group onto the substrate surface, and the wettability tends to be improved. Furthermore, it is also preferable to perform a corona discharge treatment after the dot pattern of the thermoplastic polymer-containing layer is formed by coating.
[0162] The method for removing the solvent from the coating film after coating is not particularly limited as long as it does not adversely affect the porous film. For example, a method of drying the porous film at a temperature below its melting point while fixing it, a method of drying under reduced pressure at a low temperature, a method of immersing the porous film in a poor solvent for the adhesive polymer to coagulate the adhesive polymer and simultaneously extract the solvent, etc. can be mentioned.
[0163] In drying the coating film, the drying speed is set to 0.03 g / (m) from the viewpoint of adjusting the contact angle of the thermoplastic polymer-containing layer or separator with the electrolyte to within the above-described numerical range. 2 ·s) or more 4.0g / (m 2 s) or less, and 0.05g / (m 2 ·s) or more 3.5g / (m 2 s) or less, and more preferably 0.1 g / (m 2 ·s) or more 3.0g / (m 2 It is more preferable that the drying speed is within the range of 0.1 -s). When the drying speed is within the above range, the appropriate drying speed suppresses leveling, and an uneven structure of the thermoplastic polymer particles is formed on the dot surface, tending to improve wettability. From the same viewpoint, when drying the coating film, it is also preferable to increase the temperature by heating or heating to an extent that does not damage the particle shape of the thermoplastic polymer-containing layer.
[0164] [Laminate] The laminate according to the present embodiment is a laminate of a separator and an electrode. The separator according to the present embodiment can be used as a laminate by adhering it to an electrode. The laminate has excellent handling properties when wound and rate characteristics of an electricity storage device, and also has excellent adhesion and permeability between the thermoplastic polymer and the polyolefin microporous membrane. Therefore, the use of the laminate is not particularly limited, but it can be suitably used, for example, in batteries such as nonaqueous electrolyte secondary batteries or electricity storage devices such as condensers and capacitors.
[0165] As the electrodes used in the laminate of this embodiment, those described in the section on power storage devices described later can be used. The method for producing a laminate using the separator of this embodiment is not particularly limited, but for example, the laminate can be produced by stacking the separator of this embodiment and an electrode, and heating and / or pressing as necessary. Heating and / or pressing can be performed when stacking the electrode and the separator. In addition, the laminate can also be produced by stacking the electrode and the separator, and then winding them into a circular or flat spiral shape, and then heating and / or pressing the resulting wound body.
[0166] The laminate can also be produced by laminating the positive electrode-separator-negative electrode-separator or negative electrode-separator-positive electrode-separator in a flat plate shape, and heating and / or pressing as necessary. In terms of efficiently exerting the effects of the present invention, it is preferable that the separator is arranged so that the side of the separator having the porous layer described above faces the positive electrode, with the separator substrate as a reference.
[0167] More specifically, the separator of the present embodiment is prepared as a vertically elongated separator having a width of 10 to 500 mm (preferably 80 to 500 mm) and a length of 200 to 4000 m (preferably 1000 to 4000 m), and the separators are stacked in the order of positive electrode-separator-negative electrode-separator, or negative electrode-separator-positive electrode-separator, and heated and / or pressed as necessary to produce the separator.
[0168] The heating temperature is preferably 40 to 120°C. The heating time is preferably 5 seconds to 30 minutes. The pressure during pressing is preferably 1 to 30 MPa. The pressing time is preferably 5 seconds to 30 minutes. The order of heating and pressing may be heating followed by pressing, pressing followed by heating, or pressing and heating may be performed simultaneously. Of these, pressing and heating are preferably performed simultaneously.
[0169] <Electricity storage device> The separator according to the present embodiment can be used as a separator in a battery, a condenser, a capacitor, etc., or for separating substances. In particular, when used as a separator for an electricity storage device, it is possible to impart adhesion to an electrode and excellent battery performance. Hereinafter, a preferred embodiment in the case where the electricity storage device is a non-aqueous electrolyte secondary battery will be described.
[0170] When a nonaqueous electrolyte secondary battery is manufactured using the separator of the present embodiment, the positive electrode, negative electrode, and nonaqueous electrolyte are not limited, and any known electrolytes can be used.
[0171] The positive electrode material is not particularly limited, but examples thereof include lithium-containing composite oxides such as LiCoO2, LiNiO2, spinel-type LiMnO4, and olivine-type LiFePO4.
[0172] The negative electrode material is not particularly limited, but examples thereof include carbon materials such as graphite, non-graphitizable carbon, easily graphitizable carbon, and composite carbon bodies; silicon, tin, metallic lithium, and various alloy materials.
[0173] The non-aqueous electrolyte is not particularly limited, but an electrolyte solution in which an electrolyte is dissolved in an organic solvent can be used. Examples of the organic solvent include propylene carbonate, ethylene carbonate, dimethyl carbonate, diethyl carbonate, and ethyl methyl carbonate, and examples of the electrolyte include lithium salts such as LiClO4, LiBF4, and LiPF6.
[0174] The method for producing an electricity storage device using the separator of the present embodiment is not particularly limited. When the electricity storage device is a secondary battery, for example, the separator of the present embodiment is prepared as a vertically elongated separator having a width of 10 to 500 mm (preferably 80 to 500 mm) and a length of 200 to 4000 m (preferably 1000 to 4000 m), the separators are stacked in the order of positive electrode-separator-negative electrode-separator, or negative electrode-separator-positive electrode-separator, and wound into a circular or flat spiral to obtain a wound body, the wound body is placed in a battery can, and an electrolyte solution is further injected to produce the electricity storage device.
[0175] At this time, the above-mentioned laminate may be formed by heating and / or pressing the wound body. The wound body may also be manufactured by using the above-mentioned laminate wound into a circular or flat spiral shape. The power storage device may also be manufactured by laminating the positive electrode-separator-negative electrode-separator or the negative electrode-separator-positive electrode-separator in this order in a flat plate shape, or by laminating the above-mentioned laminate with a bag-shaped film, injecting an electrolyte solution, and, in some cases, performing a heating and / or pressing process. The above-mentioned heating and / or pressing process may be performed before and / or after the process of injecting an electrolyte solution.
[0176] In an electricity storage device including a positive electrode, a negative electrode, a separator, and a non-aqueous electrolyte, the separator is preferably arranged such that the side having the porous layer described above faces the positive electrode, based on the substrate, from the viewpoint of efficiently exerting the effects of the present invention.
[0177] The measured values of the various parameters described above are values measured according to the measurement methods in the examples described below, unless otherwise specified. EXAMPLES
[0178] The present invention will be described in detail below based on examples and comparative examples, but the present invention is not limited to these examples. The measurement and evaluation methods for various physical properties used in the following production examples, examples, and comparative examples are as follows. Unless otherwise specified, the various measurements and evaluations were performed at room temperature of 23°C, at 1 atmospheric pressure, and at a relative humidity of 50%.
[0179] [Measurement method] <Viscosity average molecular weight (hereinafter also referred to as "Mv")> Based on ASRM-D4020, the intrinsic viscosity [η] in decalin solvent at 135°C was determined, and the Mv of polyethylene was calculated using the following formula. [η]=0.00068×Mv 0.67 Moreover, the Mv of polypropylene was calculated from the following formula. [η]=1.10×10 -4 Mv 0.80
[0180] <Average particle size of thermoplastic polymer> The average particle size of the thermoplastic polymer was measured using a particle size measuring device (Microtrac MT3300EXII, manufactured by Nikkiso Co., Ltd.). An aqueous dispersion of thermoplastic polymer particles was prepared (solid content: 25-30%). The measurement conditions were a loading index of 0.15-0.3 and a measurement time of 300 seconds. The particle size value at which the cumulative frequency of the obtained data was 50% was taken as the average particle size (μm) and is shown in Tables 1-1 to 1-12 below. The average particle size of the thermoplastic polymer may be calculated by measuring the particle sizes of 100 different thermoplastic polymer particles when observed using a scanning electron microscope (SEM) (model: S-4800, manufactured by Hitachi) at a magnification at which the diameter of a single particle can be measured (for example, 10,000 times when the thermoplastic polymer is approximately 0.5 μm), and then calculating the average particle size.
[0181] <Basis weight of polyolefin microporous membrane and basis weight per side of thermoplastic polymer-containing layer> A 10 cm x 10 cm square sample (polyolefin porous substrate or polyolefin porous substrate + inorganic filler porous layer) was cut out and its weight was measured using an electronic balance AEL-200 manufactured by Shimadzu Corporation. The weight obtained was multiplied by 100 to obtain the mass of 1 m 2 Weight of the membrane per unit (g / m 2 ) was calculated. A 10 cm x 10 cm square sample was cut from the separator in which a thermoplastic polymer-containing layer was formed on the substrate, and the weight was measured using an electronic balance AEL-200. The weight obtained was multiplied by 100 to obtain the mass of 1 m 2 Separator weight per unit (g / m 2 ) was calculated. The basis weight per side of the thermoplastic polymer-containing layer was calculated from the difference in basis weight before and after the formation of the thermoplastic polymer-containing layer. Alternatively, the basis weight per side of the thermoplastic polymer-containing layer may be calculated by peeling off the thermoplastic polymer-containing layer from the surface of a 10 cm x 10 cm square sample and calculating the weight loss rate (of the peeled off sample) using a thermogravimetric differential thermal analyzer (NEXTA STA 200RV, manufactured by Hitachi High-Tech Science Corporation), or may be calculated from the change in weight before and after peeling.
[0182] <Porosity of polyolefin microporous membrane (%)> A 10 cm x 10 cm square sample was cut from the polyolefin microporous membrane and its volume (cm 3 ) and mass (g), and the film density was calculated to be 0.95 (g / cm 3 ) was calculated using the following formula: Porosity = (volume - mass / film density) / volume x 100
[0183] <Air permeability (sec / 100cm 3 )> The air permeability was determined as the air permeability resistance measured using a Gurley air permeability meter G-B2 (trademark) manufactured by Toyo Seiki Co., Ltd. in accordance with JIS P-8117.
[0184] <Puncture strength of microporous polyolefin membrane (g)> Using a handy compression tester KES-G5 (trademark) manufactured by Kato Tech, the polyolefin microporous membrane was fixed with a sample holder having an opening diameter of 11.3 mm. Next, a puncture test was performed on the center of the fixed polyolefin microporous membrane in an atmosphere of 25°C with a needle tip curvature radius of 0.5 mm and a puncture speed of 2 mm / sec to obtain the puncture strength (g) as the maximum puncture load. The puncture strength converted into basis weight can also be calculated from the puncture strength and basis weight.
[0185] <Glass transition temperature of thermoplastic polymer (℃)> An appropriate amount of the thermoplastic polymer coating solution (non-volatile content = 30%) was placed on an aluminum dish and dried for 30 minutes in a hot air dryer at 130 ° C. Approximately 17 mg of the dried film was packed into an aluminum container for measurement, and a DSC curve and a DDSC curve were obtained under a nitrogen atmosphere using a DSC measurement device (Shimadzu Corporation, DSC6220). The measurement conditions were as follows. (1st stage heating program) Start at 70℃, increase temperature at a rate of 15℃ per minute. After reaching 110℃, maintain temperature for 5 minutes. (2nd stage cooling program) Decrease temperature from 110℃ at a rate of 40℃ per minute. After reaching -50℃, maintain for 5 minutes. (Third stage heating program) The temperature was increased from -50°C to 130°C at a rate of 15°C per minute. DSC and DDSC data were obtained during this third temperature increase. The glass transition temperature (Tg) was determined as the intersection point between the baseline (a straight line extending the baseline of the obtained DSC curve toward the higher temperature side) and the tangent at the inflection point (the point where the upward convex curve changes to a downward convex curve).
[0186] <Dot diameter and distance between dots> The dot diameter of the coating pattern is defined as the region where the thermoplastic polymer is continuously present when observed using a scanning electron microscope (SEM) (model: S-4800, manufactured by Hitachi) at a magnification where one dot can be observed in one field of view (for example, 300 times when the dot diameter is about 200 μm). The region where the thermoplastic polymer is continuously present is a region having a width of more than 10 μm in a continuous manner. The region where the thermoplastic polymer is continuously present is formed, for example, by thermoplastic polymer particles being continuously densely contacted in the surface direction.
[0187] Fig. 1 is a schematic plan view of a separator for explaining the dot diameter and the distance between dots. For example, in SEM plan view of a separator, as shown in Fig. 1(a), a pattern of a region (X) where the thermoplastic polymer is continuously present is defined by excluding a region with a width of 10 μm or less from an SEM image, and as shown in Fig. 1(b), the region (X) where the thermoplastic polymer is continuously present is defined by visual inspection so as not to include a region where the thermoplastic polymer is discontinuously scattered (particle scattering portion sp).
[0188] FIG. 2 is a schematic plan view after a region (X) where thermoplastic polymer is continuously present as shown in FIG. 1 has been defined in order to explain the dot diameter and the distance between dots, and the region (X) is shown shaded in FIG. 2.
[0189] The dot diameter in the region (X) where the thermoplastic polymer is continuously present was measured using a microscope (model: VHX-7000, manufactured by Keyence Corporation). The sample separator was photographed with coaxial epi-illumination at a magnification that allows the measurement of the diameter of at least five dots (for example, 100x when the dot diameter is approximately 200 μm). From the command "Measurement / Scale", "Plane Measurement" and "Diameter" were selected.
[0190] As shown in Fig. 2(e), for example, in the case of dots formed in a cloverleaf shape on a porous layer containing inorganic particles and a resin binder, the diameter of the circle (CC) circumscribing the region (X) where the thermoplastic polymer is continuously present was used. The diameter of each circumscribing circle (CC) was measured for multiple dots (five dots), and the average of these was calculated as the dot diameter.
[0191] In addition, as shown in Fig. 2(f), when the dots have a teardrop-shaped tail (e.g., dots formed directly on a polyolefin substrate) or an elliptical shape, the diameter of the largest circle (MIC) inscribed in the region (X) where the thermoplastic polymer is continuously present was used. The diameter of each largest inscribed circle (MIC) was measured for multiple dots (5 dots), and the average of these was calculated as the dot diameter.
[0192] In addition, for example, as shown in Figures 2(c) to (d), in the case where there is a region (X) where the thermoplastic polymer is continuously present and a region (Y) where the thermoplastic polymer is not present, the circumference of the region (X) where the thermoplastic polymer is continuously present, the circumference of the circumscribing circle (CC) of the dots as shown in Figure 2(e), or the circumference of the maximum inscribing circle (MIC) of the dots as shown in Figure 2(f) is defined as the outer edge of the dot, and the distance from the outer edge of a certain dot to the outer edge of the nearest other dot is defined as the "distance between dots". The distances were measured in measurement mode at five observation points, and the average value was calculated as the distance between dots. Figure 2(g) shows the dot diameter a and the distance between dots b for multiple dots. If the contrast is unclear, a different light source (model: PD2-1024, manufactured by CCS Inc.) may be used.
[0193] As shown in, for example, Figure 1(a) and Figures 2(b) to (d), the presence of a particle scattering part (a region where thermoplastic polymer particles are discontinuously deposited without contacting each other) (sp) generated by spray coating, inkjet coating, gravure coating, etc. is preferable from the viewpoint of achieving a better balance between adhesive strength and pourability, but when measuring the dot diameter (a) and defining the outer edge of the dot, the circumscribing circle (CC) or maximum inscribing circle (MIC) is specified in the region excluding this particle scattering part (sp).
[0194] <Total coverage area ratio (%) of thermoplastic polymer-containing layer to substrate surface> The total coverage area ratio of the coating pattern of the thermoplastic polymer-containing layer to the substrate surface was measured using a microscope (model: VHX-7000, manufactured by Keyence Corporation). The sample separator was photographed by coaxial epi-illumination at a magnification at which 10 or more dots could be observed simultaneously (for example, 100 times when the dot diameter is about 200 μm). From the command "Measurement / Scale", select "Automatic area measurement (particle count)", "Extraction method brightness (standard)", and "Fill holes", select an appropriate brightness (preferably between -10 and 10) to binarize the coated and uncoated parts of the thermoplastic polymer-containing layer, and measure the total coverage area ratio of the thermoplastic polymer-containing layer. If the contrast is unclear, a different light source (model: PD2-1024, manufactured by CCS Inc.) may be used.
[0195] <Measurement of the average height of the thermoplastic polymer-containing layer> The separator sample is subjected to cross-section processing by BIB (broad ion beam). Cross-section processing is performed using Hitachi High-Tech IM4000 under the following processing conditions: beam type argon, acceleration voltage 3 kV, and beam current 25 to 35 μA. During processing, the multilayer porous membrane is cooled down to just before processing as necessary in order to suppress heat damage. Specifically, the multilayer porous membrane is left in a cooling device at -40°C for a day and night. This results in a smooth separator cross section. The height of the thermoplastic polymer-containing layer was measured using a scanning electron microscope (SEM) (model: S-4800, Hitachi). Osmium was vapor-deposited, and observation was performed under conditions of an acceleration voltage of 1.0 kV and 5000 times magnification, and the maximum thickness of the thermoplastic polymer-containing layer was measured at five observation points, and the average value of these was calculated as the average height. In the case of a dot pattern, the distance from the substrate surface to the apex of a dot along the thickness direction of the thermoplastic polymer-containing layer is defined as the maximum dot thickness, and the average dot height is calculated in the same manner as above.
[0196] <Adhesion to electrodes> The separator for the power storage device obtained in each Example and Comparative Example and the positive electrode (manufactured by Enertech, positive electrode material: LiCoO2, conductive additive: acetylene black, L / W: 36 mg / cm on both sides) as an adherend 2 , thickness of Al collector: 15 μm, thickness of positive electrode after pressing: 120 μm) or negative electrode (manufactured by Enertech, negative electrode material: graphite, conductive additive: acetylene black, L / W: 20 mg / cm on both sides 2 , Cu current collector thickness: 10 μm, negative electrode thickness after pressing: 140 μm) were cut into a rectangle with a width of 15 mm and a length of 60 mm. The separator was laminated so that the thermoplastic polymer-containing layer and the positive electrode or the negative electrode faced each other to obtain a laminate. For separators having a porous layer containing inorganic particles and a resin binder on only one side of the polyolefin microporous membrane, a positive electrode was used in the case of the porous layer containing inorganic particles and a resin binder side, and a negative electrode was used in the case of the polyolefin substrate side to prepare a laminate. Then, each laminate was pressed under the following conditions. Press pressure: 1MPa Temperature: 90℃ Press time: 5 seconds. For the laminate after pressing, a 90° peel test was performed at a peel speed of 50 mm / min using Imada Co., Ltd. force gauges ZP5N and MX2-500N (product name) by fixing the electrode and gripping and pulling the separator, and the peel strength was measured. At this time, the average value of the peel strength in the peel test for a length of 40 mm performed under the above conditions was adopted as the adhesive strength with the electrode. When a separator that achieves an adhesive strength of 2 N / m or more obtained by this method is used in an electricity storage device, the adhesive strength with the opposing positive and negative electrodes is good.
[0197] <Electrolyte injection> The separator for the power storage device obtained in each Example and Comparative Example and the positive electrode (manufactured by Enertech, positive electrode material: LiCoO2, conductive additive: acetylene black, L / W: 36 mg / cm on both sides) as an adherend 2 , thickness of Al collector: 15 μm, thickness of positive electrode after pressing: 120 μm) or negative electrode (manufactured by Enertech, negative electrode material: graphite, conductive additive: acetylene black, L / W: 20 mg / cm on both sides 2 , Cu current collector thickness: 10 μm, negative electrode thickness after pressing: 140 μm) were cut into a rectangle with a width of 15 mm and a length of 60 mm. The separator was laminated so that the thermoplastic polymer-containing layer and the positive or negative electrode faced each other to obtain a laminate. For separators having a porous layer containing inorganic particles and a resin binder on only one side of the polyolefin microporous membrane, a positive electrode was used in the case of the porous layer containing inorganic particles and a resin binder side, and a negative electrode was used in the case of the polyolefin substrate side to prepare a laminate. Then, each laminate was pressed under the following conditions. Press pressure: 1MPa Temperature: 90℃ Press time: 5 seconds The laminate after pressing was sandwiched between two glass plates (Matsunami Glass, S1214, size: 76 × 26 mm, thickness: 1.2 to 1.5 mm) and fixed at three points on both sides and the top with clips (KOKUYO, JB34c, double clip (medium), silver, mouth width 25 mm), and immersed in electrolyte (Kishida Chemical, LBG-00307, ethylene carbonate (EC): diethyl carbonate (DEC) = (2: 3 volume / volume %)). The parts where the electrolyte had permeated the separator and electrode surfaces were visually observed from the separator side, and the time required for the electrolyte to permeate the entire surface was used as the injection completion time. The injection completion time was measured for each of the laminate of the positive electrode and separator and the laminate of the negative electrode and separator.
[0198] In the case of in-vehicle cells, the injection takes time as the cell width increases, which can become a bottleneck in the cell manufacturing process. To solve this problem, it is desirable to make the injection process 60 hours or less. Assuming a typical in-vehicle battery size (e.g., 200 mm wide), an electricity storage device using a separator that achieves an injection completion time of 20 minutes or less obtained by this method in both a laminate of a positive electrode and a separator and a laminate of a negative electrode and a separator can reduce the injection time to 60 hours or less. An electricity storage device using a separator that achieves an injection completion time of 20 minutes or less obtained by this method has good electrolyte penetration at the interfaces with the opposing positive and negative electrodes, improving the injection properties of the entire cell.
[0199] <Contact angle measurement of electrolyte> A glass plate (Matsunami Glass Co., Ltd., S1214, size: 76 x 26 mm, thickness: 1.2 to 1.5 mm) is attached to the measurement surface and the opposite surface of the separator for the power storage device obtained in each Example and Comparative Example using double-sided tape (Nichiban Co., Ltd., Nicetack, NW-15) to prepare a measurement sample. Using a dynamic contact angle meter (Kyowa Interface Science Co., Ltd., model DCA-VM), a 2 μL droplet of electrolyte (Kishida Chemical Co., Ltd., LBG-00307, EC / DEC (2:3 v / v %)) is prepared at the tip of a syringe needle and then dropped onto the measurement sample, and the contact angle 6000 ms after the liquid separation was adopted. The contact angle was measured in a thermostatic room at a temperature of 23 ° C and a humidity of 42%.
[0200] <Change in distance between dots before and after immersion in electrolyte> The separators for the power storage device obtained in each of the Examples and Comparative Examples were immersed in propylene carbonate (LBG-64955, PC, manufactured by Kishida Chemical Co., Ltd.) as an electrolyte, and the electrolyte was thoroughly permeated. After standing for 24 hours, the separators were taken out and the surfaces were washed with ethanol. The dot gap d2 (μm) was measured in the same manner as in the above item <Dot diameter and distance between dots>, and the ratio of the dot gap d1 (μm) before immersion in the electrolyte was calculated as the change rate Δd (%) of the dot gap using the following calculation formula. △d=(d1-d2) / d1*100
[0201] <Thermoplastic polymer> The following thermoplastic polymers were prepared: Acrylic 1 A high Tg (Tg=62° C.) acrylic latex and a low Tg (Tg<20° C.) acrylic latex were blended to form a latex blend (acrylic 1, average particle size: 0.5 μm). Acrylic 2 A high Tg (Tg=56° C.) acrylic latex and a low Tg (Tg<20° C.) acrylic latex were blended to form a latex blend (acrylic 2, average particle size: 0.5 μm). Acrylic 3 A high Tg (Tg=95° C.) acrylic latex and a low Tg (Tg<20° C.) acrylic latex were blended to form a latex blend (acrylic 3, average particle size: 0.55 μm). Acrylic 4 Acrylate-based particles (Tg = 20°C) were dispersed in water to form a latex (acrylic 4, average particle size: 0.12 μm). ·SBR Styrene-butadiene copolymer particles were dispersed in water to form a latex (SBR, average particle size: 0.15 μm). PVDF Commercially available polyvinylidene fluoride (PVDF-HFP copolymer, Tm = 150°C, average particle size: 0.2μm) was prepared. For coating, a slurry was prepared by mixing an acrylic latex (Tg < 20°C) in an amount sufficient to ensure binding strength after coating (PVDF:acrylic = 4:1 or 10:1 by solids weight ratio) and used. Acrylic control 1 A coating fluid containing the thermoplastic polymer described in Example 12B of WO 2014 / 017651 was prepared and used as an acrylic control 1. Acrylic control 2 A coating liquid containing the thermoplastic polymer described in Example 1 of Japanese Patent No. 7103760 was prepared and used as an acrylic control 2. Acrylic control 3 A coating fluid containing the thermoplastic polymer described in Example 7A of Japanese Patent No. 6688006 was prepared and used as acrylic control 3.
[0202] <Example 1> (Production of polyolefin microporous membrane 1A) 47 parts by mass of homopolymer high density polyethylene having an Mv of 700,000, 46 parts by mass of homopolymer high density polyethylene having an Mv of 300,000, and 7 parts by mass of homopolymer polypropylene having an Mv of 700,000 were dry blended using a tumbler blender. 1 part by mass of tetrakis-[methylene-(3',5'-di-t-butyl-4'-hydroxyphenyl)propionate]methane was added as an antioxidant to 99 parts by mass of the obtained polyolefin mixture, and the mixture was dry blended again using the tumbler blender to obtain a mixture. The obtained mixture was fed to a twin-screw extruder by a feeder under a nitrogen atmosphere. Liquid paraffin (dynamic viscosity at 37.78°C 7.59 x 10 -5 m 2 / s) was injected into the extruder cylinder by a plunger pump. The operating conditions of the feeder and pump were adjusted so that the proportion of liquid paraffin in the entire mixture to be extruded was 68 parts by mass, that is, the polymer concentration was 32 parts by mass.
[0203] Next, they were melt-kneaded in a twin-screw extruder while being heated to 160°C, and the resulting melt-kneaded product was extruded through a T-die onto a cooling roll controlled at a surface temperature of 80°C, and the extrudate was cast by contacting the cooling roll and cooling to solidify, thereby obtaining a sheet-like molded product. This sheet was stretched under conditions of a magnification of 7x6.4 times and a temperature of 122°C using a simultaneous biaxial stretching machine, and then immersed in methylene chloride to extract and remove liquid paraffin, dried, and stretched 1.85 times in the transverse direction at a temperature of 132°C using a tenter stretching machine. Then, this stretched sheet was relaxed by about 10% in the width direction and heat-treated to obtain a polyolefin microporous membrane 1A.
[0204] For the obtained polyolefin microporous membrane 1A, the physical properties (membrane thickness, basis weight, porosity, air permeability, pin puncture strength, etc.) were measured by the above-mentioned methods, if necessary.
[0205] (Production of polyolefin microporous membranes 2A and 3A) Polyolefin microporous membranes 2A and 3A were obtained in the same manner as in 1A, except that the production conditions were appropriately changed to adjust the physical properties (membrane thickness, basis weight, porosity, air permeability, puncture strength, etc.).
[0206] (Dot coating of thermoplastic polymer-containing layer onto polyolefin microporous film) A porous layer containing inorganic particles and a resin binder was formed on one side of the polyolefin microporous membrane 1A (porous layer thickness 2 μm), and then, under the conditions of the dot pattern, coverage area ratio, and basis weight per side shown in Table 1, acrylic 1 was dot-coated as a coating liquid on both surfaces of the polyolefin microporous membrane 1A by gravure or inkjet printing, and the coating liquid was dried at 40° C. to remove water from the coating liquid, thereby obtaining a separator for a storage device having a thermoplastic polymer-containing layer in a dot pattern on both sides of the polyolefin microporous membrane. The obtained separator was evaluated by the above method. The obtained results are also shown in Table 1. Gravure coating is preferred from the viewpoint that the degree of unevenness of the dots is 70% or less of the dot height, more preferably 50% or less, and even more preferably 30% or less. The degree of unevenness of the dots can be measured with a laser microscope (Olympus Corporation, model OLS5000-SAF).
[0207] <Examples 2 to 35 and Comparative Examples 1 to 23> As shown in Table 1, a separator for an electricity storage device having a thermoplastic polymer-containing layer on both sides of a polyolefin microporous membrane was obtained in the same manner as in Example 1, except that the conditions such as the type of thermoplastic polymer, the dot pattern, the coverage area ratio, and the basis weight were changed. The obtained separator was evaluated by the above-mentioned method. The injection completion time, adhesive strength, and contact angle were measured for each side of the separator by the method described in the above item <Pourability of electrolyte solution>, and the values of the side with the longest injection completion time were adopted. The obtained results are shown in Table 1.
[0208] In Example 30, a porous layer containing inorganic particles and a resin binder was formed on one side of polyolefin microporous membrane 1A (porous layer thickness: 4 μm), and then a thermoplastic polymer-containing layer was applied in a dot pattern to both sides of polyolefin microporous membrane 1A under the conditions shown in Table 1 to obtain a separator having a symmetrical multilayer structure with respect to polyolefin microporous membrane 1A.
[0209] In Example 31, a porous layer containing inorganic particles and a resin binder was formed on one side of polyolefin microporous membrane 2A (porous layer thickness: 3 μm), and then a thermoplastic polymer-containing layer was applied in a dot pattern to both sides of polyolefin microporous membrane 1A under the conditions shown in Table 1 to obtain a separator having a symmetrical multilayer structure with respect to polyolefin microporous membrane 1A.
[0210] In Example 32, a porous layer containing inorganic particles and a resin binder was formed on both sides of polyolefin microporous membrane 2A (each side of the porous layer had a thickness of 1.5 μm), and then a thermoplastic polymer-containing layer was applied in a dot pattern to both sides of polyolefin microporous membrane 2A under the conditions shown in Table 1 to obtain a separator having a symmetrical multilayer structure with respect to polyolefin microporous membrane 2A. The injection completion time and adhesive strength were measured for the positive electrode and the negative electrode by the method described in the above items <Adhesion to electrode> and <Injection of electrolyte>, and the values for the combination with the electrode having the longest injection completion time were used.
[0211] In Example 33, a porous layer containing inorganic particles and a resin binder was formed on one side of polyolefin microporous membrane 1A, and then a thermoplastic polymer-containing layer was applied in a dot pattern to both sides of polyolefin microporous membrane 1A under the conditions shown below to obtain a separator having an asymmetric multilayer structure based on polyolefin microporous membrane 1A. -Porous layer containing inorganic particles and resin binder Dot diameter: 200μm, distance between dots: 125μ, distance between dots / dot diameter: 0.6, dot height: 1μm, total coverage area of thermoplastic polymer-containing layer: 50%, weight of thermoplastic polymer-containing layer on one side: 0.2g / m 2 Polyolefin substrate side Dot diameter: 200 μm, distance between dots: 420 μm, distance between dots / dot diameter: 2.1, dot height: 1 μm, total coverage area of thermoplastic polymer-containing layer: 12%, weight of thermoplastic polymer-containing layer on one side: 0.06 g / m 2 The time to complete injection, adhesive strength, and contact angle were measured for each side of the separator by the method described in the above item <Injection property of electrolyte>, and the values for the side with the longest time were used.
[0212] In Example 34, a porous layer containing inorganic particles and a resin binder was formed on one side of polyolefin microporous membrane 3A, and then a thermoplastic polymer-containing layer was applied in a dot pattern to both sides of polyolefin microporous membrane 3A under the conditions shown in Table 1 to obtain a separator having an asymmetric multilayer structure based on polyolefin microporous membrane 3A.
[0213] In Comparative Examples 10 and 11, the total coverage area ratio of the thermoplastic polymer-containing layer is shown as 90% in Table 1, but a porous layer containing inorganic particles and a resin binder was formed on the polyolefin microporous membrane 1A, and then acrylic 1 and PVDF were applied to the entire surface, respectively.
[0214] In Comparative Example 12, a separator was obtained by the method described in Example 12B of International Publication No. 2014 / 017651 (Patent Document 1), and was subjected to the above measurements and evaluations.
[0215] In Comparative Example 19, a separator was obtained by the method described in Example 1 of Japanese Patent No. 7103760, and was subjected to the above measurements and evaluations.
[0216] In Comparative Example 21, a separator was obtained by the method described in Example 7A of Japanese Patent No. 6688006, and was subjected to the above measurements and evaluations.
[0217] [Table 1-1]
[0218]
Table 1-2
[0219]
Table 1-3
[0220]
Table 1-4
[0221]
Table 1-5
[0222]
Table 1-6
[0223]
Table 1-7
[0224]
Table 1-8
[0225]
Table 1-9
[0226]
Table 1-10
[0227]
Table 1-11
[0228] [Table 1-12] [Explanation of symbols]
[0229] A: Dot diameter b: distance between dots sp: particle scattering part X: Region where thermoplastic polymer exists continuously Y: Thermoplastic polymer nonexistence region MIC: Maximum inscribed circle CC: circumscribed circle
Claims
1. A separator for an electric storage device comprising: a substrate; and a thermoplastic polymer-containing layer formed on at least one surface of the substrate, the thermoplastic polymer-containing layer including a thermoplastic polymer, the thermoplastic polymer-containing layer has a dot-like pattern, The diameter of the dot is 20 μm or more and 1,000 μm or less, The distance between dots is 100 μm or more and 3,000 μm or less, The diameter of the dots and the distance between the dots are expressed by the following formula: Distance between dots / diameter of dot = 0.5 to 4 and The separator for an electricity storage device, wherein a contact angle between the thermoplastic polymer-containing layer and an electrolyte (ethylene carbonate (EC) / diethyl carbonate (DEC) (2:3 v / v %)) is 0° or more and 20° or less.
2. 2. The separator for an electricity storage device according to claim 1, wherein the average dot height is 0.2 μm or more and 10 μm or less.
3. 3 . The separator for an electricity storage device according to claim 1 , wherein a total coverage area ratio of the thermoplastic polymer-containing layer to the surface of the substrate is 5% or more and 55% or less.
4. The thermoplastic polymer-containing layer has a basis weight of 0.03 g / m 2 0.3g / m or more 2 The separator for an electricity storage device according to claim 1 or 2, wherein:
5. 3. The electricity storage device separator according to claim 1, wherein the thermoplastic polymer has an average particle size of 0.1 μm or more and 2.0 μm or less.
6. 3. The separator for an electric storage device according to claim 1 or 2, wherein the thermoplastic polymer has at least two glass transition temperatures, at least one of the glass transition temperatures being in a range below 20°C, and at least one of the glass transition temperatures being in a range of 40°C or higher and 110°C or lower.
7. The separator for an electricity storage device according to claim 1 or 2, which has an asymmetric multilayer structure with respect to the substrate.
8. 3. The separator for an electricity storage device according to claim 1, wherein the thermoplastic polymer-containing layers are provided on both sides of the substrate, and a porous layer containing an inorganic filler and a resin binder is formed between one side of the substrate and the thermoplastic polymer-containing layer.
9. 9. An electricity storage device comprising a positive electrode, a negative electrode, the separator for an electricity storage device according to claim 8, and a non-aqueous electrolyte solution, wherein the separator for an electricity storage device is arranged such that a side having the porous layer faces the positive electrode with respect to the substrate.
10. 3. An electricity storage device comprising: a positive electrode, a negative electrode, the separator for an electricity storage device according to claim 1 or 2, and a non-aqueous electrolyte.
Citation Information
Patent Citations
Partially hydrophilized microporous polyolefin membrane
JP2000248095A
Separator with improved binding properties to electrodes and electrochemical element equipped therewith
JP2011512005A
Separator, lithium battery including the same, method of manufacturing separator, and method of manufacturing lithium battery
JP2015099776A
Separator for lithium battery, lithium battery including the same, and method of manufacturing lithium battery
JP2015099777A
Separation membrane and battery provided with the same
JP2018535534A