Electrode mixture for secondary battery, electrode mixture sheet for secondary battery and method for producing same, and secondary battery
By employing powdered PTFE with a fine fiber structure in electrode mixtures, the challenges of flexibility and cost in conventional PTFE-based electrode mixtures are addressed, resulting in high-capacity, low-resistance secondary batteries with reduced gas generation.
Patent Information
- Application Number
- JP2022546325
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-09-01
- Filing Date
- 2021-08-31
- Publication Date
- 2024-10-03
- Estimated Expiration
- 2041-08-31
AI Technical Summary
Conventional electrode mixtures for secondary batteries, particularly those using polytetrafluoroethylene (PTFE) as a binder, face challenges in achieving optimal performance due to insufficient fibrillation, leading to issues such as high costs from using expensive solvents and subpar flexibility and conductivity.
The use of powdered PTFE with a fine fiber structure having a fibril diameter of 70 nm or less, combined with a specific water content and particle size, to enhance the binding properties and flexibility of electrode mixtures, eliminating the need for solvents and reducing production costs.
This approach results in electrodes with improved flexibility, lower resistance, and reduced gas generation, leading to secondary batteries with higher initial capacity and better performance.
Smart Images

Figure 0007560764000004 
Figure 0007560764000001 
Figure 0007560764000002
Abstract
Description
[Technical field]
[0001] The present disclosure relates to an electrode mixture for a secondary battery, an electrode mixture sheet for a secondary battery and a method for producing the same, and a secondary battery. [Background technology]
[0002] In lithium ion secondary batteries, a common practice is to prepare an electrode mixture by coating a slurry obtained by mixing an electrode active material and a conductive assistant with a binder and a solvent, and then drying the resulting slurry.
[0003] On the other hand, polytetrafluoroethylene resin is a polymer that easily becomes fibrillated, and it is sometimes used as a binder after being fibrillated.
[0004] Patent Document 1 discloses a method for producing an electrode in which a mixture containing an active material and a polytetrafluoroethylene mixed binder material is subjected to high shear treatment using a jet mill to fibrillate the polytetrafluoroethylene. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Special Publication No. 2017-517862 Summary of the Invention [Problem to be solved by the invention]
[0006] An object of the present disclosure is to provide an electrode mixture for a secondary battery having good properties, an electrode mixture sheet for a secondary battery containing the electrode mixture, and a secondary battery using the electrode mixture sheet. Another object of the present disclosure is to provide a method for producing an electrode mixture sheet containing a polytetrafluoroethylene resin having a fine fiber structure. [Means for solving the problem]
[0007] The present disclosure provides an electrode mixture for a secondary battery containing an electrode active material and a binder, The electrode mixture for a secondary battery is obtained by using a powdered raw material composition containing an electrode active material and a binder, The raw material composition is Binder Powdered It is a polytetrafluoroethylene resin, In the combination drug Polytetrafluoroethylene resin is an electrode material for secondary batteries characterized by having a fibrous structure with a fibril diameter (median value) of 70 nm or less.
[0008] The electrode mixture for secondary batteries is preferably for lithium ion batteries. 。
[0009] The powdered polytetrafluoroethylene resin preferably has a moisture content of 500 ppm or less. The powdered polytetrafluoroethylene resin preferably has a standard specific gravity of 2.11 to 2.20.
[0010] The powdered polytetrafluoroethylene resin preferably contains 50% by mass or more of polytetrafluoroethylene resin having a secondary particle diameter of 500 μm or more. The powdered polytetrafluoroethylene resin preferably contains 80% by mass or more of polytetrafluoroethylene resin having a secondary particle diameter of 500 μm or more.
[0011] The present disclosure also relates to an electrode mixture sheet for secondary batteries, which includes the above-mentioned electrode mixture for secondary batteries. The electrode mixture sheet for a secondary battery is for a negative electrode, and the electrode active material preferably contains silicon as a constituent element. The secondary battery electrode mixture sheet is for a positive electrode and preferably has a density of 3.00 g / cc or more. The secondary battery electrode mixture sheet is for a negative electrode and preferably has a density of 1.3 g / cc or more.
[0012] The present disclosure includes an electrode active material and a binder. Powder-like(1) applying shear force to the raw material composition while mixing the raw material composition; A step (2) of forming the electrode mixture obtained in the step (1) into a bulk form; and A step (3) of rolling the bulk electrode mixture obtained in the step (2) into a sheet. A method for producing an electrode mixture sheet for a secondary battery, comprising: the above This is also a method for producing an electrode mixture sheet for a secondary battery, characterized in that the binder is a powdered polytetrafluoroethylene resin.
[0013] The present disclosure also relates to a secondary battery having the above-mentioned electrode mixture sheet for secondary batteries. Effect of the Invention
[0014] In the present disclosure, an electrode mixture for obtaining an electrode having excellent flexibility and performance can be obtained. Therefore, a battery having high initial capacity, low resistance, and little gas generation can be obtained. Furthermore, in the manufacturing method of the present disclosure, an electrode mixture sheet for making an electrode having excellent flexibility and a battery having excellent performance can be manufactured. [Brief description of the drawings]
[0015] [Figure 1] 1 is a scanning electron microscope photograph showing the cross-sectional state of the negative electrode mixture sheet used in Example 5. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] The present disclosure will be described in detail below. The present disclosure provides an electrode mixture for use in a secondary battery, and in particular, an electrode mixture that can be suitably used in a type of secondary battery that uses an electrolyte solution. In the electrode mixture of the present disclosure, polytetrafluoroethylene resin (PTFE) is used as a binder. In the conventional electrode mixture for secondary batteries, a resin that dissolves in a solvent, such as polyvinylidene fluoride, is used as a binder, and the electrode mixture is generally prepared by coating and drying a slurry containing the binder.
[0017] It is known that powdered PTFE easily fibrillates when shear stress is applied. PTFE can be used as a binder by utilizing this fibrillating property. In other words, fibrillated PTFE binds other powder components by entangling them, and thus PTFE can act as a binder when molding the powder components.
[0018] However, even when fibrillated PTFE is used as a binder, if the fibrillation is insufficient, it cannot exhibit good performance when used as an electrode mixture. In the present disclosure, this point has been examined, and by carrying out fine fibrillation processing so that PTFE has a fibrous structure with a fibril diameter (median value) of 70 nm or less, the fibrillated PTFE can exhibit good performance as a binder for electrode mixtures.
[0019] That is, the present disclosure has discovered that when PTFE is used as a binder, by making it have a fine fibrous structure, an electrode mixture having good properties can be obtained, and thus the present disclosure has been completed.
[0020] The electrode mixture of the present disclosure is obtained by using a raw material composition containing an electrode active material and a binder, and the binder is preferably powdered PTFE. By using PTFE powder as the raw material instead of PTFE aqueous dispersion, the electrode mixture contains less moisture derived from the raw material, and there is no problem caused by the presence of moisture, which has the advantage of improving battery performance.
[0021] Furthermore, it is preferable that the raw material composition does not substantially contain a liquid medium. Thus, the electrode mixture of the present disclosure has the advantage of not using a solvent in the production. That is, in the conventional electrode mixture forming method, a solvent in which a binder is dissolved is used to prepare a slurry in which powders, which are the electrode mixture components, are dispersed, and the electrode mixture is prepared by applying and drying the slurry. In this case, a solvent that dissolves the binder is used. However, the solvent that can dissolve polyvinylidene fluoride, which is a binder resin that has been commonly used in the past, is limited to a specific solvent such as N-methylpyrrolidone. For this reason, it is necessary to use an expensive solvent, which causes an increase in costs.
[0022] The electrode mixture of the present disclosure has, as a component, PTFE having a fibrous structure with a fibril diameter (median) of 70 nm or less. In the present disclosure, it is important that the fibril diameter (median) is 70 nm or less. In this way, PTFE with a small fibril diameter is present in the electrode mixture, and this has the effect of binding the powders of the components constituting the electrode mixture together and provides flexibility, thereby achieving the object of the present invention.
[0023] The fibril diameter (median value) is a value measured by the following method. (1) Using a scanning electron microscope (S-4800, manufactured by Hitachi, Ltd.), a magnified photograph (7000x) of the electrode mixture sheet is taken to obtain an image. (2) Draw two equally spaced horizontal lines on this image to divide it into thirds. (3) For all PTFE fibers on the upper straight line, measure the diameter at three points per PTFE fiber, and take the average value as the diameter of the PTFE fiber. The three measurement points are the intersection of the PTFE fiber with the straight line, and points shifted 0.5 μm above and below the intersection (excluding unfiberized PTFE primary particles). (4) Repeat step (3) above for all the PTFE fibers in the lower straight line. (5) The screen is moved 1 mm to the right from the first image, and another image is taken, and the diameter of the PTFE fiber is measured using the above (3) and (4). This process is repeated until the number of fibers measured exceeds 80. (6) The median value of the diameters of all the PTFE fibers measured above was taken as the fibril diameter.
[0024] The fibril diameter (median) is preferably 65 nm or less. If the fibrillation proceeds too much, flexibility tends to be lost. The lower limit is not particularly limited, but from the viewpoint of strength, it is preferably, for example, 15 nm or more, and more preferably 20 nm or more.
[0025] The method for obtaining PTFE having the above fibril diameter (median value) is not particularly limited, but for example, A step (1) of applying a shear force to a raw material composition containing an electrode active material and a binder while mixing the raw material composition. A step (2) of forming the electrode mixture obtained in the step (1) into a bulk form; and The electrode mixture in bulk obtained in the step (2) is rolled into a sheet in a step (3).
[0026] In such a method, for example, in step (1), by setting the mixing condition of the raw material composition to 1000 rpm or less, it is possible to promote fibrillation of PTFE while maintaining flexibility, and by controlling the applied shear stress, it is possible to set the PTFE fibril diameter (median) to 70 nm or less.
[0027] It is also preferable to have a step (4) after the step (3) in which the obtained rolled sheet is rolled under a larger load into a thinner sheet. It is also preferable to repeat the step (4). The fibril diameter can also be adjusted by crushing the obtained rolled sheet after step (3) or step (4), forming it into a bulk shape again, and rolling it into a sheet shape in step (5). Step (5) is preferably repeated, for example, from 1 to 12 times.
[0028] That is, by applying a shearing force, the PTFE powder is fibrillated, and the fibrillated particles are entangled with the powder components such as the electrode active material, thereby producing an electrode mixture. The production method will be described later.
[0029] In the present disclosure, the PTFE is not particularly limited and may be a homopolymer or a copolymer that can be fibrillated, with a homopolymer being more preferred. In the case of copolymers, examples of the fluorine atom-containing comonomer include chlorotrifluoroethylene, hexafluoropropylene, fluoroalkylethylene, perfluoroalkylethylene, and fluoroalkyl fluorovinyl ether.
[0030] The above-mentioned "PTFE powder" does not mean a dispersed state mixed with a liquid medium, but a solid state as a powder. By using such a state and producing an electrode mixture using PTFE in the absence of a liquid medium, the object of the present disclosure can be suitably achieved.
[0031] The powdered PTFE used as a raw material for preparing the electrode mixture of the present disclosure preferably has a moisture content of 500 ppm or less. A moisture content of 500 ppm or less is preferable in that a secondary battery having initial characteristics of little gas generation can be fabricated. The water content is more preferably 300 ppm or less.
[0032] The powdered PTFE used as a raw material for preparing the electrode mixture of the present disclosure preferably has a standard specific gravity of 2.11 to 2.20. The standard specific gravity being within this range is advantageous in that an electrode mixture sheet with high strength can be produced. The lower limit of the standard specific gravity is more preferably 2.12 or more. The upper limit of the standard specific gravity is more preferably 2.19 or less, and even more preferably 2.18 or less.
[0033] Standard specific gravity (SSG) is measured by preparing a sample in accordance with ASTM D-4895-89 and measuring the specific gravity of the obtained sample by the water displacement method.
[0034] The powdered PTFE preferably contains 50% by mass or more, more preferably 80% by mass or more, of PTFE having a secondary particle diameter of 500 μm or more. By containing PTFE having a secondary particle diameter of 500 μm or more within this range, there is an advantage that an electrode mixture sheet with high strength can be produced. By using PTFE with a secondary particle size of 500 μm or more, it is possible to obtain an electrode mixture sheet with lower resistance and excellent toughness.
[0035] The lower limit of the secondary particle diameter of the powdered PTFE is more preferably 300 μm, and even more preferably 350 μm. The upper limit of the secondary particle diameter is more preferably 700 μm or less, and even more preferably 600 μm or less. The secondary particle diameter can be determined, for example, by a sieving method.
[0036] The powdered PTFE has an average primary particle size of preferably 150 nm or more, more preferably 180 nm or more, even more preferably 210 nm or more, and particularly preferably 220 nm or more, since this allows the electrode mixture sheet to have higher strength and excellent homogeneity. The larger the average primary particle diameter of PTFE, the more suppressed the increase in extrusion pressure when extrusion molding is performed using the powder, and the better the moldability. The upper limit is not particularly limited, but may be 500 nm. From the viewpoint of productivity in the polymerization process, it is preferably 350 nm.
[0037] The above average primary particle diameter can be determined by preparing a calibration curve of the transmittance of 550 nm projected light per unit length of an aqueous dispersion of PTFE obtained by polymerization, the polymer concentration of which is adjusted to 0.22% by mass, and the average primary particle diameter determined by measuring the unidirectional diameter in a transmission electron microscope photograph, and measuring the above transmittance for the aqueous dispersion to be measured, and then based on the calibration curve.
[0038] The PTFE used in the present disclosure may have a core-shell structure.The PTFE having a core-shell structure may be, for example, polytetrafluoroethylene that contains a core of high molecular weight polytetrafluoroethylene and a shell of lower molecular weight polytetrafluoroethylene or modified polytetrafluoroethylene in the particle.The polytetrafluoroethylene described in JP-A-2005-527652 may be, for example, the polytetrafluoroethylene.
[0039] Powdered PTFE that satisfies the above-mentioned parameters can be obtained by a conventional manufacturing method, for example, by following the manufacturing methods described in International Publication No. 2015-080291 and International Publication No. 2012-086710.
[0040] The electrode mixture for secondary batteries of the present disclosure contains an electrode active material, a binder, etc. The content of the binder in the electrode mixture for secondary batteries is preferably 0.2 to 10 mass %, more preferably 0.3 to 6.0 mass %. If the binder is within the above range, it is possible to form a self-supporting sheet with excellent handleability while suppressing an increase in electrode resistance.
[0041] Furthermore, the electrode mixture for a secondary battery according to the present disclosure may contain a conductive assistant, if necessary. The electrode active material, the conductive assistant, etc. will be described below.
[0042] (electrode active material) First, the positive electrode active material is not particularly limited as long as it can electrochemically absorb and release alkali metal ions, but for example, a material containing an alkali metal and at least one transition metal is preferable. Specific examples include an alkali metal-containing transition metal composite oxide, an alkali metal-containing transition metal phosphate compound, a conductive polymer, etc. Among them, the positive electrode active material is preferably an alkali metal-containing transition metal composite oxide that produces high voltage. The alkali metal ion may be a lithium ion, a sodium ion, a potassium ion, or the like. In a preferred embodiment, the alkali metal ion may be a lithium ion. That is, in this embodiment, the alkali metal ion secondary battery is a lithium ion secondary battery.
[0043] Examples of the alkali metal-containing transition metal composite oxide include: Formula:M a Mn 2-b M 1 b O4 (Wherein, M is at least one metal selected from the group consisting of Li, Na, and K; 0.9≦a; 0≦b≦1.5; M 1 is at least one metal selected from the group consisting of Fe, Co, Ni, Cu, Zn, Al, Sn, Cr, V, Ti, Mg, Ca, Sr, B, Ga, In, Si and Ge), Formula:MNi 1-c M 2 CO2 (Wherein, M is at least one metal selected from the group consisting of Li, Na, and K; 0≦c≦0.5; M 2 is at least one metal selected from the group consisting of Fe, Co, Mn, Cu, Zn, Al, Sn, Cr, V, Ti, Mg, Ca, Sr, B, Ga, In, Si and Ge), or Formula:MCo 1-d M 3 d O2 (Wherein, M is at least one metal selected from the group consisting of Li, Na, and K; 0≦d≦0.5; M 3 and alkali metal-cobalt composite oxides represented by the formula (I) are at least one metal selected from the group consisting of Fe, Ni, Mn, Cu, Zn, Al, Sn, Cr, V, Ti, Mg, Ca, Sr, B, Ga, In, Si, and Ge. In the above, M is preferably one metal selected from the group consisting of Li, Na and K, more preferably Li or Na, and further preferably Li.
[0044] Among these, MCoO2, MMnO2, MNiO2, MMn2O4, and MNi are the most popular because they can provide high energy density and high output secondary batteries. 0.8 Co 0.15 Al 0.05 O2, or MNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 and the like are preferred, and a compound represented by the following general formula (3) is preferred. MNi h Co i Mn j M 5 k O2(3) (In the formula, M is at least one metal selected from the group consisting of Li, Na, and K, and M 5 represents at least one selected from the group consisting of Fe, Cu, Zn, Al, Sn, Cr, V, Ti, Mg, Ca, Sr, B, Ga, In, Si, and Ge, and (h+i+j+k)=1.0, 0≦h≦1.0, 0≦i≦1.0, 0≦j≦1.5, and 0≦k≦0.2.
[0045] The alkali metal-containing transition metal phosphate compound is, for example, a compound represented by the following formula (4): M e M 4 f (PO4) g (4) (In the formula, M is at least one metal selected from the group consisting of Li, Na, and K, and M 4represents at least one selected from the group consisting of V, Ti, Cr, Mn, Fe, Co, Ni, and Cu, and examples thereof include compounds represented by the formula 0.5≦e≦3, 1≦f≦2, 1≦g≦3). In the above, M is preferably one metal selected from the group consisting of Li, Na and K, more preferably Li or Na, and further preferably Li.
[0046] The transition metal of the lithium-containing transition metal phosphate compound is preferably V, Ti, Cr, Mn, Fe, Co, Ni, Cu, etc., and specific examples include iron phosphates such as LiFePO4, Li3Fe2(PO4)3, LiFeP2O7, cobalt phosphates such as LiCoPO4, and lithium transition metal phosphate compounds in which a part of the transition metal atoms that constitute the main part of these compounds has been substituted with other elements such as Al, Ti, V, Cr, Mn, Fe, Co, Li, Ni, Cu, Zn, Mg, Ga, Zr, Nb, Si, etc. The lithium-containing transition metal phosphate compound preferably has an olivine structure.
[0047] Other positive electrode active materials include MFePO4 and MNi 0.8 Co 0.2 O2, M 1.2 Fe 0.4 Mn 0.4 O2, MNi 0.5 Mn 1.5 O2, MV3O6, M2MnO3 (wherein M is at least one metal selected from the group consisting of Li, Na, and K), etc. In particular, M2MnO3, MNi 0.5 Mn 1.5 A positive electrode active material such as O2 is preferable in that the crystal structure does not collapse when the secondary battery is operated at a voltage exceeding 4.4 V or at a voltage of 4.6 V or more. Therefore, an electrochemical device such as a secondary battery using a positive electrode material containing the above-mentioned positive electrode active material is preferable because the remaining capacity is unlikely to decrease and the resistance increase rate is unlikely to change even when stored at high temperatures, and the battery performance is not deteriorated even when operated at high voltages.
[0048] As other positive electrode active materials, M2MnO3 and MM 6 O2 (wherein M is at least one metal selected from the group consisting of Li, Na, and K, and M 6 is a transition metal such as Co, Ni, Mn, Fe, etc.) and solid solution materials thereof can also be mentioned.
[0049] Examples of the solid solution material include, for example, an alkali metal manganese oxide represented by the general formula Mx[Mn (1-y) M 7 y O z Here, M in the formula is at least one metal selected from the group consisting of Li, Na, and K, and M 7 consists of at least one metal element other than M and Mn, and includes, for example, one or more elements selected from the group consisting of Co, Ni, Fe, Ti, Mo, W, Cr, Zr, and Sn. Also, the values of x, y, and z in the formula are in the range of 1 < x < 2, 0 ≦ y < 1, and 1.5 < z < 3. Among them, a manganese-containing solid solution material in which LiNiO2 or LiCoO2 is solid-solved based on Li2MnO3 such as Li 1.2 Mn 0.5 Co 0.14 Ni 0.14 O2 is preferable because it can provide an alkali metal ion secondary battery having a high energy density.
[0050] In addition, it is preferable to include lithium phosphate in the positive electrode active material because the continuous charging characteristics are improved. There is no limitation on the use of lithium phosphate, but it is preferable to mix and use the above positive electrode active material and lithium phosphate. The amount of lithium phosphate used is preferably at least 0.1% by mass, more preferably at least 0.3% by mass, still more preferably at least 0.5% by mass, and preferably at most 10% by mass, more preferably at most 8% by mass, still more preferably at most 5% by mass, based on the total of the above positive electrode active material and lithium phosphate.
[0051] The conductive polymer may be a p-doped conductive polymer or an n-doped conductive polymer, and may be a polyacetylene-based polymer, a polyphenylene-based polymer, a heterocyclic polymer, an ionic polymer, a ladder polymer, a network polymer, or the like.
[0052] In addition, a substance having a different composition may be attached to the surface of the positive electrode active material. Examples of the surface-attaching substance include oxides such as aluminum oxide, silicon oxide, titanium oxide, zirconium oxide, magnesium oxide, calcium oxide, boron oxide, antimony oxide, and bismuth oxide, sulfates such as lithium sulfate, sodium sulfate, potassium sulfate, magnesium sulfate, calcium sulfate, and aluminum sulfate, carbonates such as lithium carbonate, calcium carbonate, and magnesium carbonate, and carbon.
[0053] These surface-attaching substances can be attached to the surface of the positive electrode active material by, for example, a method of dissolving or suspending in a solvent, impregnating or adding to the positive electrode active material, and then drying, a method of dissolving or suspending a surface-attaching substance precursor in a solvent, impregnating and adding to the positive electrode active material, and then reacting by heating, a method of adding to a positive electrode active material precursor and simultaneously baking, etc. When carbon is attached, a method of mechanically attaching carbonaceous material in the form of, for example, activated carbon, etc., afterwards can also be used.
[0054] The amount of the surface-attached substance is preferably 0.1 ppm or more, more preferably 1 ppm or more, and even more preferably 10 ppm or more, and preferably 20% or less, more preferably 10% or less, and even more preferably 5% or less, by mass relative to the positive electrode active material. The surface-attached substance can suppress the oxidation reaction of the electrolyte on the surface of the positive electrode active material, and can improve the battery life. If the amount of attachment is too small, the effect is not fully expressed, and if it is too large, the resistance may increase due to the obstruction of the ingress and egress of lithium ions.
[0055] The shape of the particles of the positive electrode active material may be any of the conventional shapes such as block, polyhedron, sphere, oval sphere, plate, needle, column, etc. Primary particles may be aggregated to form secondary particles.
[0056] The tap density of the positive electrode active material is preferably 0.5 g / cm 3 More preferably, 0.8 g / cm 3 More preferably, 1.0 g / cm 3 That is all. If the tap density of the positive electrode active material is below the lower limit, the amount of dispersion medium required during the formation of the positive electrode active material layer increases, and the amount of conductive material and binder required also increases, restricting the filling rate of the positive electrode active material in the positive electrode active material layer and possibly restricting the battery capacity. By using a composite oxide powder with a high tap density, a high density positive electrode active material layer can be formed. Generally, the higher the tap density, the more preferable it is, and there is no particular upper limit, but if it is too high, the diffusion of lithium ions in the positive electrode active material layer using the electrolyte as a medium becomes rate-limiting, and the load characteristics may be easily deteriorated, so that the upper limit is preferably 4.0 g / cm. 3 Less than or equal to 3.7 g / cm 3 More preferably, 3.5 g / cm 3 The following is the result. In the present disclosure, the tap density is the powder packing density (tap density) g / cm when 5 to 10 g of the positive electrode active material powder is placed in a 10 ml glass measuring cylinder and tapped 200 times with a stroke of about 20 mm. 3 is required.
[0057] The median diameter d50 of the particles of the positive electrode active material (secondary particle diameter when primary particles are aggregated to form secondary particles) is preferably 0.3 μm or more, more preferably 0.5 μm or more, even more preferably 0.8 μm or more, and most preferably 1.0 μm or more, and is preferably 30 μm or less, more preferably 27 μm or less, even more preferably 25 μm or less, and most preferably 22 μm or less. If it is below the lower limit, a high tap density product may not be obtained, and if it exceeds the upper limit, it may take time for lithium to diffuse within the particles, resulting in a decrease in battery performance, or problems such as streaking may occur when preparing the positive electrode of a battery, that is, when the active material, conductive material, binder, etc. are slurried with a solvent and applied in a thin film. Here, by mixing two or more types of the above positive electrode active materials having different median diameters d50, the filling property during the preparation of the positive electrode can be further improved.
[0058] In the present disclosure, the median diameter d50 is measured by a known laser diffraction / scattering type particle size distribution analyzer. When using HORIBA's LA-920 as the particle size distribution analyzer, a 0.1% by mass sodium hexametaphosphate aqueous solution is used as the dispersion medium for the measurement, and the measurement is performed after ultrasonic dispersion for 5 minutes with a measurement refractive index set to 1.24.
[0059] In the case where the primary particles are aggregated to form secondary particles, the average primary particle diameter of the positive electrode active material is preferably 0.05 μm or more, more preferably 0.1 μm or more, and even more preferably 0.2 μm or more, and the upper limit is preferably 5 μm or less, more preferably 4 μm or less, even more preferably 3 μm or less, and most preferably 2 μm or less. If the upper limit is exceeded, it is difficult to form spherical secondary particles, which may adversely affect the powder packing property or greatly reduce the specific surface area, and therefore the battery performance such as output characteristics may be likely to decrease. On the other hand, if the lower limit is exceeded, problems such as poor reversibility of charge and discharge may occur due to underdeveloped crystals.
[0060] In the present disclosure, the average primary particle diameter of the positive electrode active material is measured by observation using a scanning electron microscope (SEM). Specifically, in a photograph at a magnification of 10,000 times, the longest intercept value of a horizontal line at the left and right boundaries of the primary particles is obtained for any 50 primary particles, and the average value is calculated.
[0061] The BET specific surface area of the positive electrode active material is preferably 0.1 m 2 / g or more, more preferably 0.2m 2 / g or more, more preferably 0.3m 2 / g or more, and the upper limit is preferably 50m 2 / g or less, more preferably 40m 2 / g or less, more preferably 30m 2 If the BET specific surface area is smaller than this range, the battery performance is likely to decrease, whereas if it is larger, it is difficult to increase the tap density, and problems may easily occur in the application property when forming the positive electrode active material layer.
[0062] In the present disclosure, the BET specific surface area is defined as a value measured by a surface area meter (e.g., a fully automatic surface area measuring device manufactured by Okura Riken Co., Ltd.) using a nitrogen adsorption BET single-point method based on a gas flow method, after pre-drying a sample at 150°C for 30 minutes under a nitrogen flow and using a nitrogen-helium mixed gas precisely adjusted so that the relative pressure of nitrogen to atmospheric pressure is 0.3.
[0063] When the secondary battery of the present disclosure is used as a large-scale lithium-ion secondary battery for hybrid automobiles or distributed power sources, high output is required, so that the particles of the positive electrode active material are preferably mainly secondary particles. The positive electrode active material particles preferably contain 0.5 to 7.0 volume % of fine particles having an average secondary particle size of 40 μm or less and an average primary particle size of 1 μm or less. By containing fine particles having an average primary particle size of 1 μm or less, the contact area with the electrolyte increases, and the diffusion of lithium ions between the electrode mixture and the electrolyte can be made faster, resulting in improved output performance of the battery.
[0064] The manufacturing method of the positive electrode active material is a general method for manufacturing inorganic compounds.In particular, various methods can be considered for making spherical or elliptical active materials, for example, the raw material of transition metal is dissolved or crushed and dispersed in a solvent such as water, and the pH is adjusted while stirring to make and recover spherical precursors, which are dried as necessary, and then LiOH, Li2CO3, LiNO3, or other Li sources are added and calcined at high temperature to obtain active materials.
[0065] For the production of the positive electrode, the positive electrode active material may be used alone, or two or more of different compositions may be used in any combination or ratio. In this case, a preferred combination is LiCoO2 and LiNi 0.33 Co 0.33 Mn 0.33 Examples of such a combination include a combination with a ternary system such as O2, a combination of LiCoO2 and LiMn2O4 or a combination in which a portion of the Mn is replaced with another transition metal, or a combination of LiFePO4 and LiCoO2 or a combination in which a portion of the Co is replaced with another transition metal.
[0066] The content of the positive electrode active material in the positive electrode mixture is preferably 50 to 99.5% by mass, and more preferably 80 to 99% by mass, in view of high battery capacity. The content of the positive electrode active material is preferably 80% by mass or more, more preferably 82% by mass or more, and particularly preferably 84% by mass or more. The upper limit is preferably 99% by mass or less, more preferably 98% by mass or less. If the content of the positive electrode active material in the positive electrode mixture is low, the electric capacity may be insufficient. Conversely, if the content is too high, the strength of the positive electrode may be insufficient.
[0067] The negative electrode active material is not particularly limited, and examples thereof include carbonaceous materials such as lithium metal, artificial graphite, graphite carbon fiber, resin-sintered carbon, pyrolytic vapor-grown carbon, coke, mesocarbon microbeads (MCMB), furfuryl alcohol resin-sintered carbon, polyacene, pitch-based carbon fiber, vapor-grown carbon fiber, natural graphite, and non-graphitizable carbon; silicon-containing compounds such as silicon and silicon alloys; and Li4Ti5O 12 Among them, those containing at least a carbonaceous material and silicon-containing compounds are particularly suitable.
[0068] The negative electrode active material used in the present disclosure preferably contains silicon as a constituent element. By using the negative electrode active material containing silicon as a constituent element, a high-capacity battery can be produced.
[0069] The silicon-containing particles are preferably silicon particles, particles having a structure in which silicon particles are dispersed in a silicon-based compound, silicon oxide particles represented by the general formula SiOx (0.5≦x≦1.6), or a mixture thereof. By using these, a negative electrode mixture for a lithium ion secondary battery having a higher initial charge / discharge efficiency, a high capacity, and excellent cycle characteristics can be obtained.
[0070] Silicon oxide in the present disclosure is a general term for amorphous silicon oxide, and silicon oxide before disproportionation is represented by the general formula SiOx (0.5≦x≦1.6). x is preferably 0.8≦x<1.6, and more preferably 0.8≦x<1.3. This silicon oxide can be obtained, for example, by heating a mixture of silicon dioxide and metallic silicon to produce silicon monoxide gas, which is then cooled and precipitated.
[0071] Particles having a structure in which silicon particles are dispersed in a silicon-based compound can be obtained, for example, by a method of baking a mixture of silicon particles and a silicon-based compound, or by heat treating silicon oxide particles before disproportionation represented by the general formula SiOx in an inert non-oxidizing atmosphere such as argon at a temperature of 400°C or higher, preferably 800 to 1,100°C, to perform a disproportionation reaction. In particular, the material obtained by the latter method is preferable because the silicon microcrystals are uniformly dispersed. The size of the silicon nanoparticles can be made 1 to 100 nm by the above-mentioned disproportionation reaction. Note that the silicon oxide in the particles having a structure in which silicon nanoparticles are dispersed in silicon oxide is preferably silicon dioxide. Note that it is possible to confirm that silicon nanoparticles (crystals) are dispersed in amorphous silicon oxide by a transmission electron microscope.
[0072] The physical properties of the silicon-containing particles can be appropriately selected depending on the composite particles to be produced. For example, the average particle size is preferably 0.1 to 50 μm, and the lower limit is more preferably 0.2 μm or more, and even more preferably 0.5 μm or more. The upper limit is more preferably 30 μm or less, and even more preferably 20 μm or less. The average particle size in the present invention is represented by the weight average particle size measured by a particle size distribution measurement using a laser diffraction method.
[0073] The BET specific surface area of silicon-containing particles is 0.5 to 100 m 2 / g is preferable, and 1 to 20m 2 / g is more preferable. 2 / g or more, there is no risk of the adhesiveness decreasing when applied to an electrode, resulting in a decrease in battery characteristics. 2 / g or less, the proportion of silicon dioxide on the particle surface becomes large, and there is no risk of a decrease in battery capacity when used as a negative electrode material for a lithium ion secondary battery.
[0074] The silicon-containing particles are coated with carbon to impart electrical conductivity, which leads to improved battery characteristics. Methods for imparting electrical conductivity include mixing with conductive particles such as graphite, coating the surfaces of the silicon-containing particles with a carbon coating, and combining both methods. The carbon coating method is preferred, and chemical vapor deposition (CVD) is more preferred as the coating method.
[0075] In order to increase the capacity of the resulting electrode mixture, the content of the negative electrode active material is preferably 40% by mass or more, more preferably 50% by mass or more, and particularly preferably 60% by mass or more in the electrode mixture, and the upper limit is preferably 99% by mass or less, more preferably 98% by mass or less.
[0076] (Conductive assistant) Any known conductive material can be used as the conductive assistant. Specific examples include metal materials such as copper and nickel, graphite such as natural graphite and artificial graphite, carbon black such as acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black, and carbon materials such as needle coke, carbon nanotubes, fullerene, and amorphous carbon such as VGCF. These may be used alone or in any combination and ratio of two or more.
[0077] The conductive assistant is used in an electrode mixture so that it is contained in an amount of usually 0.01% by mass or more, preferably 0.1% by mass or more, more preferably 1% by mass or more, and usually 50% by mass or less, preferably 30% by mass or less, more preferably 15% by mass or less. If the content is lower than this range, the conductivity may be insufficient. Conversely, if the content is higher than this range, the battery capacity may decrease.
[0078] (Other Ingredients) The electrode mixture may further contain a thermoplastic resin. Examples of the thermoplastic resin include vinylidene fluoride, polypropylene, polyethylene, polystyrene, polyethylene terephthalate, and polyethylene oxide. One type may be used alone, or two or more types may be used in any combination and ratio.
[0079] The ratio of the thermoplastic resin to the electrode active material is usually 0.01% by mass or more, preferably 0.05% by mass or more, more preferably 0.10% by mass or more, and usually 3.0% by mass or less, preferably 2.5% by mass or less, more preferably 2.0% by mass or less. The addition of the thermoplastic resin can improve the mechanical strength of the electrode. If the ratio exceeds this range, the ratio of the electrode active material in the electrode mixture decreases, which may cause problems such as a decrease in the battery capacity or an increase in the resistance between the active materials.
[0080] In the electrode mixture of the present disclosure, the content of the binder is usually 0.1% by mass or more, preferably 0.5% by mass or more, more preferably 1.0% by mass or more, and usually 50% by mass or less, preferably 40% by mass or less, more preferably 30% by mass or less, and most preferably 10% by mass or less, as the ratio of the binder in the electrode mixture. If the ratio of the binder is too low, the electrode mixture active material cannot be sufficiently held, resulting in insufficient mechanical strength of the electrode mixture sheet, which may deteriorate the battery performance such as cycle characteristics. On the other hand, if the ratio is too high, it may lead to a decrease in battery capacity and conductivity.
[0081] The electrode mixture of the present disclosure can be used as an electrode mixture for secondary batteries. In particular, the electrode mixture of the present disclosure is suitable for lithium ion secondary batteries. When used in a secondary battery, the electrode mixture of the present disclosure is usually used in the form of a sheet.
[0082] An example of a specific method for producing an electrode mixture sheet containing an electrode mixture will be described below. The electrode mixture sheet of the present disclosure is A step (1) of applying a shear force to a raw material composition containing an electrode active material, a binder, and, if necessary, a conductive assistant, while mixing the raw material composition. A step (2) of forming the electrode mixture obtained in the step (1) into a bulk form; and A step (3) of rolling the bulk electrode mixture obtained in the step (2) into a sheet. The electrode mixture sheet for a secondary battery having the above structure can be obtained by the method for producing the electrode mixture sheet for a secondary battery having the above structure.
[0083] In the above step (1), at the stage where the raw material composition is mixed and shear force is applied, the resulting electrode mixture is present in a state without a fixed shape, with the electrode active material, binder, etc. simply being mixed together. Specific mixing methods include mixing methods using a W-type mixer, V-type mixer, drum-type mixer, ribbon mixer, conical screw-type mixer, single-shape kneader, twin-shape kneader, mix muller, stirring mixer, planetary mixer, etc.
[0084] In the above step (1), the mixing conditions may be appropriately set by the number of revolutions and the mixing time. For example, the number of revolutions is preferably 1000 rpm or less. It is preferably 10 rpm or more, more preferably 15 rpm or more, and even more preferably 20 rpm or more, and is preferably 900 rpm or less, more preferably 800 rpm or less, and even more preferably 700 rpm. If it is below the above range, it will take a long time to mix, which will affect productivity. If it is above the above range, fibrillation will proceed excessively, and the electrode mixture sheet may have poor strength and flexibility.
[0085] In the above step (2), forming into a bulk form means forming the electrode mixture into a single mass. Specific methods for forming the material into a bulk form include extrusion molding, press molding, and the like. In addition, the term "bulk" does not specify a particular shape, and may refer to a state in which the material is in the form of a single mass, including rods, sheets, spheres, cubes, etc. The size of the mass is preferably such that the diameter or the smallest side of the cross section is 10,000 μm or more, more preferably 20,000 μm or more.
[0086] Specific examples of the rolling method in the above step (3) include rolling methods using a roll press, a plate press, a calendar roll machine, or the like.
[0087] It is also preferable to have a step (4) after step (3) in which a larger load is applied to the obtained rolled sheet to roll it into a thinner sheet. It is also preferable to repeat step (4). In this way, the rolled sheet is not thinned all at once, but is rolled little by little in stages, thereby improving flexibility. The number of times of step (4) is preferably from 2 to 10, and more preferably from 3 to 9. A specific rolling method includes, for example, a method in which a rolled sheet is passed between two or more rotating rolls to process it into a thinner sheet.
[0088] From the viewpoint of adjusting the fibril diameter, it is also preferable to have a step (5) after step (3) or step (4) in which the rolled sheet is roughly crushed, then formed into a bulk shape again, and rolled into a sheet. It is also preferable to repeat step (5). The number of times of step (5) is preferably 1 to 12 times, more preferably 2 to 11 times.
[0089] In step (5), specific methods for roughly crushing the rolled sheet and forming it into a bulk shape include folding the rolled sheet, forming it into a rod or thin sheet shape, chipping, etc. In this disclosure, "rough crushing" means changing the shape of the rolled sheet obtained in step (3) or step (4) into a different shape in order to roll it into a sheet shape in the next step, and also includes the case where the rolled sheet is simply folded.
[0090] Furthermore, step (4) may be carried out after step (5), or may be carried out repeatedly. Moreover, uniaxial or biaxial stretching may be carried out in steps (2), (3), (4) and (5). The fibril diameter (median) can also be adjusted by the degree of crushing in step (5).
[0091] In the above steps (3), (4) or (5), the rolling ratio is preferably 10% or more, more preferably 20% or more, and is preferably 80% or less, more preferably 65% or less, and even more preferably 50% or less. If the rolling ratio is below the above range, the number of rolling times increases and it takes time, which affects productivity. If the rolling ratio is above the above range, fibrillation may proceed excessively, resulting in an electrode mixture sheet with poor strength and flexibility. The rolling ratio here refers to the reduction rate of the thickness of the sample after rolling to the thickness before rolling. The sample before rolling may be a bulk raw material composition or a sheet-like raw material composition. The thickness of the sample refers to the thickness in the direction in which a load is applied during rolling.
[0092] As described above, the PTFE powder is fibrillated by applying a shear force. In order to obtain a fibrous structure with a fibril diameter (median) of 70 nm or less, excessive shear stress may promote fibrillation too much, resulting in loss of flexibility. In addition, weak shear stress may not be sufficient in terms of strength. For this reason, by performing the steps of applying an appropriate shear stress to the PTFE during mixing or rolling to promote fibrillation, and rolling the resin to stretch it into a sheet shape within the above range, it is possible to obtain a fibrous structure with a fibril diameter (median) of 70 nm or less.
[0093] The electrode mixture sheet of the present disclosure can be used as an electrode mixture sheet for a secondary battery. It can be either a negative electrode or a positive electrode. In particular, the electrode mixture sheet of the present disclosure is suitable for a lithium ion secondary battery.
[0094] (positive electrode) In the present disclosure, the positive electrode is preferably composed of a current collector and an electrode mixture sheet containing the above-mentioned positive electrode active material. Examples of the material for the positive electrode current collector include metals such as aluminum, titanium, tantalum, stainless steel, and nickel, or metal materials such as alloys thereof, and carbon materials such as carbon cloth and carbon paper. Among these, metal materials, particularly aluminum or its alloys, are preferred.
[0095] The shape of the current collector may be metal foil, metal cylinder, metal coil, metal plate, expanded metal, punched metal, foamed metal, etc. in the case of a metal material, or carbon plate, carbon thin film, carbon cylinder, etc. Among these, metal foil is preferred. The metal foil may be appropriately formed into a mesh shape. The thickness of the metal foil is arbitrary, but is usually 1 μm or more, preferably 3 μm or more, more preferably 5 μm or more, and is usually 1 mm or less, preferably 100 μm or less, more preferably 50 μm or less. If the metal foil is thinner than this range, the strength required as a current collector may be insufficient. Conversely, if the metal foil is thicker than this range, the handling properties may be impaired.
[0096] In addition, it is also preferable that the surface of the current collector is coated with a conductive assistant from the viewpoint of reducing the electrical contact resistance between the current collector and the positive electrode mixture sheet. Examples of the conductive assistant include carbon and precious metals such as gold, platinum, and silver.
[0097] The thickness ratio of the current collector to the positive electrode mixture sheet is not particularly limited, but the value of (thickness of one side of the positive electrode mixture sheet immediately before injecting the electrolyte) / (thickness of the current collector) is preferably 20 or less, more preferably 15 or less, most preferably 10 or less, and is preferably 0.5 or more, more preferably 0.8 or more, most preferably 1 or more. If it exceeds this range, the current collector may generate heat due to Joule heat during charging and discharging at high current density. If it is below this range, the volume ratio of the current collector to the positive electrode active material increases, and the capacity of the battery may decrease.
[0098] The positive electrode may be manufactured by a conventional method, for example, a method in which the above-mentioned electrode mixture sheet and a current collector are laminated with an adhesive therebetween, and then vacuum dried.
[0099] The density of the positive electrode mixture sheet is preferably 3.00 g / cm 3 More preferably, 3.10 g / cm 3 More preferably, 3.20 g / cm 3 or more, and preferably 3.80 g / cm 3 Less than or equal to 3.75 g / cm 3 More preferably, 3.70 g / cm 3 The range is as follows. If the range is exceeded, the permeability of the electrolyte to the vicinity of the interface between the current collector and the active material decreases, and the charge / discharge characteristics, particularly at high current density, may decrease, making it impossible to obtain high output. If the range is exceeded, the conductivity between the active materials may decrease, the battery resistance may increase, and high output may not be obtained.
[0100] The area of the positive electrode mixture sheet is preferably made larger than the outer surface area of the battery exterior case from the viewpoint of increasing the stability at high output and high temperature. Specifically, the total electrode mixture area of the positive electrode relative to the surface area of the exterior of the secondary battery is preferably 15 times or more in area ratio, and more preferably 40 times or more. In the case of a bottomed rectangular shape, the outer surface area of the battery exterior case refers to the total area calculated from the vertical, horizontal and thickness dimensions of the case part filled with the power generating element excluding the protruding part of the terminal. In the case of a bottomed cylindrical shape, it is the geometric surface area of the case part filled with the power generating element excluding the protruding part of the terminal as a cylinder. The total electrode mixture area of the positive electrode refers to the geometric surface area of the positive electrode mixture layer facing the mixture layer containing the negative electrode active material, and in a structure in which a positive electrode mixture layer is formed on both sides via a current collector, it refers to the sum of the areas calculated separately for each side.
[0101] The thickness of the positive electrode is not particularly limited, but from the viewpoint of high capacity and high output, the thickness of the mixture sheet minus the thickness of the current collector is preferably 10 μm or more, more preferably 20 μm or more, as a lower limit for one side of the current collector, and is also preferably 500 μm or less, more preferably 450 μm or less.
[0102] The positive electrode may have a surface to which a substance of a different composition is attached, such as oxides, such as aluminum oxide, silicon oxide, titanium oxide, zirconium oxide, magnesium oxide, calcium oxide, boron oxide, antimony oxide, and bismuth oxide, sulfates, such as lithium sulfate, sodium sulfate, potassium sulfate, magnesium sulfate, calcium sulfate, and aluminum sulfate, carbonates, such as lithium carbonate, calcium carbonate, and magnesium carbonate, and carbon.
[0103] (Negative electrode) In the present disclosure, the negative electrode is preferably composed of a current collector and an electrode mixture sheet containing the above-mentioned negative electrode active material. Examples of the material for the negative electrode current collector include metals such as copper, nickel, titanium, tantalum, and stainless steel, and metal materials such as alloys thereof; and carbon materials such as carbon cloth and carbon paper. Among these, metal materials, particularly copper, nickel, and alloys thereof are preferred.
[0104] The shape of the current collector may be metal foil, metal cylinder, metal coil, metal plate, expanded metal, punched metal, foamed metal, etc. in the case of a metal material, or carbon plate, carbon thin film, carbon cylinder, etc. Among these, metal foil is preferred. The metal foil may be appropriately formed into a mesh shape. The thickness of the metal foil is arbitrary, but is usually 1 μm or more, preferably 3 μm or more, more preferably 5 μm or more, and is usually 1 mm or less, preferably 100 μm or less, more preferably 50 μm or less. If the metal foil is thinner than this range, the strength required as a current collector may be insufficient. Conversely, if the metal foil is thicker than this range, the handling properties may be impaired.
[0105] The negative electrode may be produced by a conventional method, for example, a method in which the above-mentioned electrode mixture sheet and a current collector are laminated with an adhesive therebetween, and then vacuum dried.
[0106] The density of the negative electrode mixture sheet is preferably 1.3 g / cm 3 More preferably, 1.4 g / cm 3 More preferably, 1.5 g / cm 3 More preferably, it is 2.0 g / cm 3 Less than or equal to 1.9 g / cm 3 More preferably, 1.8 g / cm 3 The range is as follows. If the range is exceeded, the permeability of the electrolyte to the vicinity of the interface between the current collector and the active material decreases, and the charge / discharge characteristics, particularly at high current density, may decrease, making it impossible to obtain high output. If the range is exceeded, the conductivity between the active materials may decrease, the battery resistance may increase, and high output may not be obtained.
[0107] The thickness of the negative electrode is not particularly limited, but from the viewpoint of high capacity and high output, the thickness of the mixture sheet minus the thickness of the current collector is preferably 10 μm or more, more preferably 20 μm or more, as a lower limit for one side of the current collector, and is also preferably 500 μm or less, more preferably 450 μm or less.
[0108] (Secondary battery) The present disclosure also relates to a secondary battery using the electrode mixture sheet. The secondary battery of the present disclosure can use an electrolyte, a separator, and the like used in known secondary batteries. These will be described in detail below.
[0109] (electrolyte) As the non-aqueous electrolyte, a solution in which a known electrolyte salt is dissolved in a known organic solvent for dissolving electrolyte salts can be used.
[0110] The organic solvent for dissolving the electrolyte salt is not particularly limited, and one or more of known hydrocarbon solvents such as propylene carbonate, ethylene carbonate, butylene carbonate, γ-butyrolactone, 1,2-dimethoxyethane, 1,2-diethoxyethane, dimethyl carbonate, diethyl carbonate, and ethyl methyl carbonate; and fluorine-based solvents such as fluoroethylene carbonate, fluoroether, and fluorinated carbonate can be used.
[0111] Examples of the electrolyte salt include LiClO4, LiAsF6, LiBF4, LiPF6, LiN(SO2CF3)2, and LiN(SO2C2F5)2. From the viewpoint of good cycle characteristics, LiPF6, LiBF4, LiN(SO2CF3)2, LiN(SO2C2F5)2, or combinations thereof are particularly preferred.
[0112] The concentration of the electrolyte salt must be 0.8 mol / L or more, and preferably 1.0 mol / L or more. The upper limit depends on the organic solvent used to dissolve the electrolyte salt, but is usually 1.5 mol / L.
[0113] (Separator) The secondary battery of the present disclosure preferably further includes a separator. The material and shape of the separator are not particularly limited as long as they are stable to the electrolyte and have excellent liquid retention, and known materials can be used. Among them, it is preferable to use a material such as a resin, glass fiber, or inorganic material that is stable to the electrolyte of the present disclosure or the electrolyte used in the alkali metal secondary battery of the present disclosure, and to use a porous sheet or nonwoven fabric that has excellent liquid retention.
[0114] Examples of materials that can be used for the resin and glass fiber separator include polyolefins such as polyethylene and polypropylene, aromatic polyamides, polytetrafluoroethylene, polyethersulfone, glass filters, etc. These materials, such as polypropylene / polyethylene two-layer film and polypropylene / polyethylene / polypropylene three-layer film, may be used alone or in any combination and ratio of two or more. Among these, the separator is preferably a porous sheet or nonwoven fabric made of a polyolefin such as polyethylene or polypropylene, because of its excellent electrolyte permeability and shutdown effect.
[0115] The thickness of the separator is arbitrary, but is usually 1 μm or more, preferably 5 μm or more, more preferably 8 μm or more, and is usually 50 μm or less, preferably 40 μm or less, more preferably 30 μm or less. If the separator is thinner than the above range, the insulating properties and mechanical strength may be reduced. If the separator is thicker than the above range, not only may the battery performance such as rate characteristics be reduced, but also the energy density of the entire electrolyte battery may be reduced.
[0116] Furthermore, when a porous material such as a porous sheet or nonwoven fabric is used as the separator, the porosity of the separator is optional, but is usually 20% or more, preferably 35% or more, more preferably 45% or more, and is usually 90% or less, preferably 85% or less, more preferably 75% or less. If the porosity is too small, the membrane resistance tends to increase and the rate characteristics tend to deteriorate. If the porosity is too large, the mechanical strength of the separator tends to decrease and the insulating properties tend to decrease.
[0117] The average pore size of the separator is also optional, but is usually 0.5 μm or less, preferably 0.2 μm or less, and usually 0.05 μm or more. If the average pore size exceeds the above range, short circuits are likely to occur. If the average pore size is below the above range, the membrane resistance increases and the rate characteristics may deteriorate.
[0118] On the other hand, examples of inorganic materials that can be used include oxides such as alumina and silicon dioxide, nitrides such as aluminum nitride and silicon nitride, and sulfates such as barium sulfate and calcium sulfate, and these are in particulate or fibrous form.
[0119] As for the form, a thin film such as a nonwoven fabric, a woven fabric, or a microporous film is used. In the thin film form, a film with a pore size of 0.01 to 1 μm and a thickness of 5 to 50 μm is preferably used. In addition to the above independent thin film form, a separator can be used in which a composite porous layer containing the above inorganic particles is formed on the surface layer of the positive electrode and / or negative electrode using a resin binder. For example, a porous layer may be formed on both sides of the positive electrode using alumina particles with 90% particle size of less than 1 μm and a fluororesin as a binder.
[0120] (Battery design) The electrode mixture group may be either a laminated structure of the positive electrode and the negative electrode with the separator interposed therebetween, or a structure of the positive electrode and the negative electrode spirally wound with the separator interposed therebetween. The ratio of the volume of the electrode mixture group to the internal volume of the battery (hereinafter referred to as the electrode mixture group occupancy rate) is usually 40% or more, preferably 50% or more, and usually 90% or less, preferably 80% or less.
[0121] If the electrode mixture group occupancy rate is below the above range, the battery capacity may become small, whereas if it exceeds the above range, the void space is small, and the battery becomes hot, causing the components to expand, or the vapor pressure of the electrolyte liquid component to increase, causing the internal pressure to increase, deteriorating various characteristics of the battery, such as the charge / discharge cycle performance and high-temperature storage, and further causing the gas release valve for releasing the internal pressure to operate.
[0122] The current collecting structure is not particularly limited, but in order to more effectively improve the charge / discharge characteristics at high current density by the electrolyte, it is preferable to use a structure that reduces the resistance of the wiring and joints. When the internal resistance is reduced in this way, the effect of using the electrolyte is particularly good.
[0123] In the case where the electrode mixture group has the above-mentioned laminated structure, a structure formed by bundling the metal core parts of each electrode mixture layer and welding them to a terminal is preferably used. When the area of one electrode mixture is large, the internal resistance increases, so it is also preferably used to reduce the resistance by providing multiple terminals in the electrode mixture. In the case where the electrode mixture group has the above-mentioned wound structure, the internal resistance can be reduced by providing multiple lead structures on each of the positive electrode and the negative electrode and bundling them to a terminal.
[0124] The material of the exterior case is not particularly limited as long as it is a material stable against the electrolyte used. Specifically, metals such as nickel-plated steel plate, stainless steel, aluminum or aluminum alloy, magnesium alloy, or a laminate film of resin and aluminum foil (laminate film) are used. From the viewpoint of weight reduction, metals such as aluminum or aluminum alloy, and laminate film are preferably used.
[0125] In the case of an exterior case using metals, there are cases in which the metals are welded together by laser welding, resistance welding, or ultrasonic welding to form a sealed structure, or cases in which the metals are used via a resin gasket to form a crimped structure. In the case of an exterior case using the laminate film, there are cases in which the resin layers are heat-sealed together to form a sealed structure. In order to improve the sealing property, a resin different from the resin used in the laminate film may be interposed between the resin layers. In particular, when the resin layer is heat-sealed via a current collecting terminal to form a sealed structure, the joining between the metal and the resin is performed, so that a resin having a polar group or a modified resin into which a polar group has been introduced is preferably used as the interposed resin.
[0126] The shape of the secondary battery of the present disclosure is arbitrary, and examples of the shape include a cylindrical shape, a square shape, a laminated shape, a coin shape, a large shape, etc. The shapes and configurations of the positive electrode, the negative electrode, and the separator can be changed according to the shape of each battery. EXAMPLES
[0127] The present disclosure will now be described in detail with reference to examples. In the following examples, unless otherwise specified, "parts" and "%" represent "parts by mass" and "% by mass", respectively.
[0128] [Preparation Example 1] Powdered PTFE-A was prepared by referring to Preparation Example 2 of International Publication No. 2015-080291.
[0129] [Preparation Example 2] Powdered PTFE-B was prepared by referring to Example 3 of International Publication No. 2015-080291.
[0130] [Preparation Example 3] Powdered PTFE-C was prepared with reference to Preparation Example 1 of WO 2012 / 086710.
[0131] [Preparation Example 4] Powdered PTFE-D was prepared by referring to Preparation Example 1 of International Patent No. 2012-063622. The physical properties of the prepared PTFE are shown in Table 1.
[0132] [Table 1]
[0133] Example 1 <Preparation of positive electrode mixture sheet> Li(Ni 0.6 Mn 0.2 Co 0.2 )O2 (NMC622) and carbon black as a conductive additive were weighed out and stirred in a mortar at 200 rpm for 1 hour to obtain a mixture. The powdered PTFE-C was used after drying in a vacuum dryer at 50° C. for 1 hour. The powdered PTFE was sieved in advance using a stainless steel sieve with 500 μm openings, and the PTFE remaining on the sieve was used. Thereafter, powdered PTFE was added as a binder to the container containing the mixture, and the mixture was stirred at 40 rpm for 2 hours to obtain a mixture in which the mass ratio of the positive electrode active material:binder:conductive assistant was 95:2:3. The resulting mixture was formed into a bulk form and rolled into a sheet. After that, the previously obtained rolled sheet was roughly crushed by folding it in two, and then formed into a bulk shape again, and then rolled into a sheet shape using a metal roll on a flat plate, and the process of promoting fibrillation was repeated four times. After that, by further rolling, a positive electrode mixture sheet with a thickness of about 500 μm was obtained. Furthermore, the positive electrode mixture sheet was cut into 5 cm x 5 cm, put into a roll press machine and rolled. In order to further promote fibrillation, a load of 2 kN was repeatedly applied to adjust the thickness. The gap was adjusted so that the final thickness of the positive electrode mixture layer was 101 μm. The initial rolling rate was the largest, at 27%.
[0134] <Preparation of positive electrode> The sheet was attached to a 20 μm aluminum foil. The adhesive was a slurry of polyvinylidene fluoride (PVDF) dissolved in N-methylpyrrolidone (NMP) and carbon nanotubes (CNT) dispersed in it. The above-mentioned adhesive was applied to the aluminum foil, and the sheet-shaped positive electrode mixture was placed on top of it while being careful not to trap air bubbles. It was then vacuum-dried at 100°C for 30 minutes to produce a positive electrode sheet integrated with the current collector.
[0135] <Preparation of negative electrode> The negative electrode active material was artificial graphite powder, the thickener was an aqueous dispersion of sodium carboxylmethylcellulose (concentration of sodium carboxymethylcellulose: 1.5% by mass), the binder was an aqueous dispersion of styrene-butadiene rubber (SBR) (concentration of styrene-butadiene rubber: 50% by mass), and water was added as a solvent, and the solid content was mixed in a mixer in an aqueous solvent at 97.6:1.2:1.2 (mass%) to prepare a negative electrode mixture slurry. The mixture was uniformly applied to a copper foil having a thickness of 20 μm, dried (110 ° C, 30 minutes), and then compressed and formed with a load of 10 kN by a press machine to prepare a negative electrode sheet integrated with a current collector. The thickness of the negative electrode mixture layer was 99 μm.
[0136] <Preparation of electrolyte> As an organic solvent, a mixed solvent of ethylene carbonate (EC) and ethyl methyl carbonate (EMC) (EC:EMC = 30:70 (volume ratio)) was weighed into a sample bottle, and fluoroethylene carbonate (FEC) and vinylene carbonate (VC) were dissolved in it at 1 mass% each to prepare an electrolyte. The concentration of LiPF6 salt in the electrolyte was adjusted to 1.0 mol / L, and the electrolyte was obtained by mixing at 23°C.
[0137] <Battery Construction> The negative electrode sheet, positive electrode sheet and polyethylene separator prepared above were laminated in this order: negative electrode, separator and positive electrode, to prepare a battery element. This battery element was inserted into a bag made of a laminate film of aluminum (40 μm thick) coated on both sides with a resin layer, with the positive and negative terminals protruding, and then electrolyte was injected into each bag and vacuum sealed to produce a sheet-shaped lithium-ion secondary battery.
[0138] (Examples 2 to 4) Lithium ion secondary batteries were produced in the same manner as in Example 1 except that the PTFE shown in Table 2 was used.
[0139] Comparative Example 1 <Preparation of positive electrode mixture sheet> NMC622 as a positive electrode active material and carbon black as a conductive assistant were weighed out and stirred in a mortar at 200 rpm for 1 hour to obtain a mixture. Thereafter, the powdered PTFE shown in Table 2 was added as a binder to the container containing the mixture, and the mixture was stirred at 40 rpm for 2 hours, and then kneaded in a mixer at 1400 rpm for a total of 5 minutes to obtain a mixture. The solid content was adjusted to a mass ratio of positive electrode active material: binder: conductive assistant = 95:2:3. The resulting mixture was formed into a bulk form and rolled into a sheet. After that, the previously obtained rolled sheet was folded in two to be crushed roughly, and then formed into a bulk shape again, and then rolled into a sheet shape using a metal roll on a flat plate, and the process of promoting fibrillation was repeated four times. After that, by further rolling, a positive electrode mixture sheet with a thickness of 500 μm was obtained. Furthermore, the positive electrode mixture sheet was cut into 5 cm x 5 cm, and rolled by putting it into a roll press machine. Furthermore, in order to promote fibrillation, a load of 10 kN was repeatedly applied to adjust the thickness. The gap was adjusted so that the final thickness of the positive electrode mixture layer was 101 μm. The initial rolling rate was the largest, at 52%.
[0140] <Battery Construction> A lithium ion secondary battery was produced in the same manner as in Example 1 except for using the positive electrode mixture sheet produced above.
[0141] Comparative Example 2 Using the PTFE shown in Table 2, and otherwise following the same procedures as in Comparative Example 1, lithium ion secondary batteries were produced.
[0142] Example 5 <Preparation of negative electrode mixture sheet> As the negative electrode active material, 25.65 g of artificial graphite powder and 2.85 g of SiO were weighed and stirred in a mortar at 200 rpm for 1 hour to obtain a mixture. The powdered PTFE was dried in a vacuum dryer at 50°C for 1 hour before use. The powdered PTFE-C was sieved in advance using a stainless steel sieve with a mesh size of 500 μm, and the powder remaining on the sieve was used. Then, 2.0 g of powdered PTFE was added as a binder to the container containing the mixture, and the mixture was stirred at 40 rpm for 2 hours to obtain a mixture. The obtained mixture was formed into a bulk shape and rolled into a sheet shape. After that, the previously obtained rolled sheet was folded in two to be crushed roughly, and then formed into a bulk shape again, and then rolled into a sheet shape using a metal roll on a flat plate, and the process of promoting fibrillation was repeated four times. After that, by further rolling, a negative electrode mixture sheet with a thickness of 500 μm was obtained. Furthermore, the negative electrode mixture sheet was cut into 5 cm x 5 cm, put into a roll press machine and rolled. In order to further promote fibrillation, a load of 2 kN was repeatedly applied to adjust the thickness. The gap was adjusted to make the final thickness of the negative electrode mixture layer 101 μm. The initial rolling rate was the largest, at 38%.
[0143] <Preparation of negative electrode> The copper foil was attached to a thickness of 20 μm. The adhesive was a slurry of PVDF dissolved in NMP and CNT dispersed therein. The adhesive was applied to the copper foil, and the negative electrode mixture sheet was placed on the copper foil while being careful not to trap air bubbles. The sheet was then vacuum dried at 100°C for 30 minutes to produce a negative electrode sheet integrated with the current collector.
[0144] <Preparation of positive electrode> Li(Ni) as a positive electrode active material 1 / 3 Mn 1 / 3 Co 1 / 3 95% by mass of 02 (NMC111), 3% by mass of acetylene black as a conductive assistant, and 2% by mass of PVdF as a binder were mixed in NMP solvent to form a slurry. The obtained slurry was uniformly applied to an aluminum foil having a thickness of 20 μm, dried (110°C, 30 minutes), and then compressed with a load of 10 kN using a press machine to form a positive electrode sheet integrated with a current collector. The thickness of the electrode mixture layer was approximately 100 μm.
[0145] <Battery Construction> A lithium ion secondary battery was produced in the same manner as in Example 1 except for using the negative electrode and positive electrode produced above.
[0146] (Examples 6 to 8) Using the PTFE shown in Table 3 respectively, and otherwise in the same manner as in Example 5, a lithium ion secondary battery was fabricated.
[0147] (Comparative Example 3) ><Fabrication of Anode Composite Sheet> Weighed 25.65 g of artificial graphite powder and 2.85 g of SiO as anode active materials, and stirred them in a mortar at 200 rpm for 1 hour to obtain a mixture. Thereafter, 2.0 g of the powdery PTFE shown in Table 3 was added as a binder to the container containing the mixture, and kneaded at 1400 rpm for a total of 5 minutes to obtain a mixture. The obtained mixture was formed into a bulk shape and rolled into a sheet shape. Thereafter, the rolled sheet obtained above was crushed by folding it in half twice, formed into a bulk shape again, and then rolled into a sheet shape using a metal roll on a flat plate to promote fibrillation. This process was repeated four times. Thereafter, by further rolling, an anode composite sheet with a thickness of 500 μm was obtained. Furthermore, the anode composite sheet was cut into 5 cm × 5 cm, put into a roll press, and rolled. The thickness was adjusted by repeatedly applying a load of 10 kN. The gap was adjusted so that the thickness of the final anode composite layer was 101 μm. The rolling rate of the first time was the largest at 78%.
[0148] ><Fabrication of Battery> Using the anode composite sheet fabricated above, and otherwise in the same manner as in Example 5, a lithium ion secondary battery was fabricated.
[0149] (Comparative Example 4) Using the PTFE shown in Table 2, and otherwise in the same manner as in Comparative Example 3, a lithium ion secondary battery was obtained.
[0150] (Reference Example 1) ><Fabrication Method of SiO Anode - Slurry> 25.65g of artificial graphite powder as the negative electrode active material, 2.85g of SiO, 2.0g of polyacrylic acid as a binder, and 20g of N-methylpyrrolidone (NMP) as a solvent were mixed in a mixer to prepare SiO negative electrode mixture slurry. The mixture was uniformly applied to a copper foil with a thickness of 20 μm, dried (110 ° C, 30 minutes), and then compressed and molded with a press to prepare a negative electrode sheet integrated with a current collector. The thickness of the electrode mixture layer was 95 μm.
[0151] <Battery Construction> A lithium ion secondary battery was produced in the same manner as in Example 5 except for using the negative electrode sheet produced above.
[0152] Each test was carried out in the following manner. [Measurement of moisture content] The powdered PTFE was dried in a vacuum dryer at 50°C for 1 hour before use. The moisture content of the PTFE after vacuum drying was measured using a Karl Fischer moisture meter (ADP-511 / MKC-510N, manufactured by Kyoto Electronics Manufacturing Co., Ltd.) with a boat-type moisture vaporizer, and the moisture vaporized by heating to 210°C in the moisture vaporizer was measured. Nitrogen gas was flowed as the carrier gas at a flow rate of 200 mL / min, and the measurement time was 30 minutes. Chem-Aqua was used as the Karl Fischer reagent. The sample amount was 1.5 g.
[0153] [PTFE fibril diameter (median) (nm)] (1) Using a scanning electron microscope (S-4800, manufactured by Hitachi, Ltd.), a magnified photograph (7000x) of the electrode mixture sheet is taken to obtain an image. (2) Draw two equally spaced horizontal lines on this image to divide it into thirds. (3) For all PTFE fibers on the straight line above, measure the diameter at three points per PTFE fiber, and take the average value as the diameter of the PTFE fiber. The three measurement points are the intersection of the PTFE fiber with the straight line, and points shifted 0.5 μm above and below the intersection (excluding unfiberized PTFE primary particles). (4) Repeat step (3) above for all the PTFE fibers in the lower straight line. (5) The screen is moved 1 mm to the right from the first image, and another image is taken, and the diameter of the PTFE fiber is measured using the above (3) and (4). This process is repeated until the number of fibers measured exceeds 80. (6) The median value of the diameters of all the PTFE fibers measured above was taken as the fibril diameter.
[0154] For reference, a scanning electron microscope photograph showing the cross-sectional state of the electrode mixture sheet used in Example 5 is shown in FIG.
[0155] [Strength measurement] Using a tensile tester (Shimadzu Corporation, Autograph AGS-X Series AGS-100NX), measurements were performed on 4 mm wide rectangular electrode mixture test pieces at 100 mm / min. The chuck distance was 30 mm. Displacement was applied until breakage, and the maximum stress of the measurement results was taken as the strength of each sample. In Table 2, Comparative Example 1 was standardized as 100%, and in Table 3, Comparative Example 3 was standardized as 100%.
[0156] [Flexibility] The electrode mixture sheet was cut out to prepare a 2 cm x 10 cm test piece. The electrode mixture sheet was wrapped around a round bar with a diameter of 4 mm, and the electrode mixture sheet was visually inspected and evaluated according to the following criteria. A: No cracks were observed. Δ: Cracks were observed, but no breakage was observed. ×: Broken.
[0157] <Battery testing> [Initial discharge capacity test] The lithium ion secondary battery produced above was sandwiched between plates and pressurized, and then at 25°C, it was charged at a constant current-constant voltage (hereinafter referred to as CC / CV charging) (0.1C cut) to 4.2V at a current equivalent to 1C, and then discharged to 3V at a constant current of 1C, which constitutes one cycle, and the initial discharge capacity was calculated from the discharge capacity at the third cycle. In Table 2, Comparative Example 1 is standardized as 100%, and in Table 3, Comparative Example 3 is standardized as 100%.
[0158] [60℃ 2W storage test and gas generation measurement] The lithium ion secondary battery manufactured above is sandwiched between plates and pressurized, and then CC / CV charged (0.1C cut) to 4.2V with a current equivalent to 1C, and the volume of the battery is measured by Archimedes' method, and this is the volume before storage. Next, the batteries for which the charging has been completed are placed in a thermostatic chamber set at 60°C and kept there for two weeks. After that, the batteries are removed from the thermostatic chamber and left at room temperature for two hours, and then the volume is measured by Archimedes' method, and this is the volume after storage. The difference between the volume after storage and the volume before storage is calculated, and this is the amount of gas generated (ml), and in Table 2, Comparative Example 1 is set to 100%, and in Table 3, Comparative Example 3 is set to 100%. (Volume after storage) - (Volume before storage) = Amount of gas generated (ml)
[0159] [Resistance rating] The battery for which the evaluation of the discharge capacity after 10 cycles at 25° C. was completed was charged at 25° C. with a constant current of 1 C to half the initial discharge capacity. The impedance of the battery was measured by applying an AC voltage amplitude of 10 mV at 25° C., and the real axis resistance at 0.1 Hz was calculated. In Table 2, Comparative Example 1 was standardized as 100%, and in Table 3, Comparative Example 3 was standardized as 100%.
[0160] The test results are shown in Tables 2 and 3.
[0161] [Table 2]
[0162] [Table 3]
[0163] From the results in Tables 2 and 3, the electrode mixture sheets of the examples were excellent in flexibility, and the physical properties of the secondary battery were also good. [Industrial Applicability]
[0164] The electrode mixture for secondary batteries according to the present disclosure can be used in the production of lithium ion secondary batteries.
Claims
1. An electrode mixture for a secondary battery containing an electrode active material and a binder, The electrode mixture for a secondary battery is obtained by using a powdered raw material composition containing an electrode active material and a binder, The raw material composition has a binder that is a powdered polytetrafluoroethylene resin, 1. An electrode mixture for a secondary battery, wherein the polytetrafluoroethylene resin in the mixture has a fibrous structure with a fibril diameter (median value) of 70 nm or less.
2. 2. The electrode mixture for a secondary battery according to claim 1, which is for a lithium ion secondary battery.
3. 3. The electrode mixture for a secondary battery according to claim 1, wherein the powdered polytetrafluoroethylene resin has a moisture content of 500 ppm or less.
4. 4. The electrode mixture for a secondary battery according to claim 1, 2 or 3, wherein the powdered polytetrafluoroethylene resin has a standard specific gravity of 2.11 to 2.
20.
5. 5. The electrode mixture for a secondary battery according to claim 1, 2, 3 or 4, wherein the powdered polytetrafluoroethylene resin contains 50 mass % or more of polytetrafluoroethylene resin having a secondary particle diameter of 500 μm or more.
6. 5. The electrode mixture for a secondary battery according to claim 1, 2, 3 or 4, wherein the powdered polytetrafluoroethylene resin contains 80 mass % or more of polytetrafluoroethylene resin having a secondary particle diameter of 500 μm or more.
7. An electrode mixture sheet for secondary batteries comprising the electrode mixture for secondary batteries according to any one of claims 1 to 6.
8. 8. The electrode mixture sheet for a secondary battery according to claim 7, which is for a negative electrode, and the electrode active material contains silicon as a constituent element.
9. 8. The electrode mixture sheet for a secondary battery according to claim 7, which is for a positive electrode and has a density of 3.0 g / cc or more.
10. 9. The electrode mixture sheet for a secondary battery according to claim 7 or 8, which is for a negative electrode and has a density of 1.3 g / cc or more.
11. A step (1) of applying a shear force to a powdery raw material composition containing an electrode active material and a binder while mixing the powdery raw material composition. A step (2) of forming the electrode mixture obtained by the step (1) into a bulk form; and A step (3) of rolling the bulk electrode mixture obtained in the step (2) into a sheet.
13. A method for producing an electrode mixture sheet for a secondary battery, comprising:
12. A secondary battery comprising the electrode mixture sheet for secondary batteries according to any one of claims 7 to 10.
Citation Information
Patent Citations
Manufacture of lithium secondary battery
JP1998302780A
Binder composition for electrode of lithium secondary battery
JP2011150931A
Manufacturing method of electrode for electricity-storage devices, electrode for electricity-storage device, and electricity-storage device
JP2012094331A
Binder composition for electrode
JP2012119297A
Electrode material, magnesium fuel battery, and method for manufacturing electrode material
JP2015015153A