Method for manufacturing grain-oriented electrical steel sheet and intermediate steel sheet for grain-oriented electrical steel sheet

By controlling annealing and cooling processes to form a film-like oxide layer on grain-oriented electrical steel sheets, the method enhances insulating film adhesion and water resistance, addressing peeling issues and maintaining low core loss.

JP7560779B2Active Publication Date: 2024-10-03NIPPON STEEL CORPORATION
View PDF 16 Cites 0 Cited by

Patent Information

Application Number
JP2023094128
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-01-16
Filing Date
2023-06-07
Publication Date
2024-10-03
Estimated Expiration
2040-01-16

AI Technical Summary

Technical Problem

Existing grain-oriented electrical steel sheets with silicon oxide intermediate layers face issues with insulating film adhesion and water resistance, leading to peeling due to moisture exposure, which affects magnetic properties and core loss.

Method used

A method involving controlled annealing and cooling processes to form a film-like oxide layer on the steel sheet surface, minimizing internal oxides and enhancing the adhesion of the intermediate silicon oxide layer, thereby improving film adhesion and water resistance.

Benefits of technology

The method results in a grain-oriented electrical steel sheet with improved insulating film adhesion and water resistance, maintaining low core loss and magnetic properties even under bending and moisture exposure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007560779000001
    Figure 0007560779000001
Patent Text Reader

Abstract

To provide a grain-oriented electromagnetic steel sheet which has an intermediate layer mainly composed of silicon oxide, in which adhesion of an insulating film is improved, and in which water resistance, which has not been conventionally recognized as a problem, is improved, and to provide a production method of an intermediate steel sheet for the grain-oriented electromagnetic steel sheet.SOLUTION: A production method of a grain-oriented electromagnetic steel sheet comprises a hot rolling step, a hot rolling sheet annealing step, a cold rolling step, a decarburizing annealing step, an annealing separator coating step, a finishing annealing step, a cooling step in which the base steel sheet after the finishing annealing step is cooled under an atmosphere in which the oxidation degree PH2O / PH2 indicated by the ratio of the steam partial pressure to the hydrogen partial pressure is set to 0.30-100000 in a temperature range of 1100-500°C, an intermediate layer forming step, and an insulating film forming step.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a grain-oriented electrical steel sheet and an intermediate steel sheet for a grain-oriented electrical steel sheet. This application claims priority based on Japanese Patent Application No. 2019-5200, filed on January 16, 2019, the contents of which are incorporated herein by reference. [Background technology]

[0002] Grain-oriented electrical steel sheets are used as iron core materials for transformers, etc. Grain-oriented electrical steel sheets are required to have magnetic properties such as low core loss.

[0003] Usually, a coating is formed on the surface of grain-oriented electrical steel sheets in order to reduce iron loss. This coating reduces the iron loss of each steel sheet by applying tension to the grain-oriented electrical steel sheet. This coating also ensures electrical insulation between the steel sheets when the grain-oriented electrical steel sheets are stacked together to form an iron core, thereby reducing the iron loss of the iron core.

[0004] An example of a grain-oriented electrical steel sheet having a coating is one in which a finish-annealed pure coating mainly composed of forsterite (Mg2SiO4) is formed on the surface of a base steel sheet, and an insulating coating is further formed on the surface of the finish-annealed pure coating. In other words, in this case, the coating on the base steel sheet includes a finish annealed coating and an insulating coating. The finish-annealed pure coating and the insulating coating each have the functions of both insulation and applying tension to the base steel sheet.

[0005] The finish annealed pure coating, which is mainly composed of forsterite (Mg2SiO4), is formed during the finish annealing, which causes secondary recrystallization in the steel sheet, by a reaction between an annealing separator mainly composed of magnesia (MgO) and the base steel sheet during heat treatment at 600 to 1200°C for 30 hours or more.

[0006] The insulating coating is formed by applying a coating solution containing, for example, phosphoric acid or a phosphate, colloidal silica, and chromic anhydride or a chromate to the steel sheet after finish annealing, and baking and drying at 300 to 950°C for 10 seconds or more.

[0007] In order for an insulating coating to exert its functions of insulation and tensioning the base steel sheet, these coatings (finish annealing coating and insulating coating) are required to have high adhesion to the base steel sheet.

[0008] Conventionally, the adhesion has been ensured mainly by the anchor effect of the unevenness of the interface between the base steel sheet and the finish-hardened pure coating. However, the unevenness of the interface also hinders the magnetic domain wall movement when the grain-oriented electrical steel sheet is magnetized. Therefore, the unevenness of the interface is also a factor that prevents the reduction of iron loss in the grain-oriented electrical steel sheet.

[0009] When a finish annealing film such as a forsterite film is formed, unevenness occurs at the interface between the base steel sheet and the finish annealing film. Therefore, in order to reduce iron loss, it is effective to suppress the formation of the finish annealing film and smooth the surface of the base steel sheet.

[0010] For example, Patent Documents 1 and 2 propose techniques for smoothing the surface of a base steel sheet without the presence of a finish-annealed pure coating mainly composed of forsterite in order to promote low iron loss.

[0011] Specifically, Patent Document 1 discloses a method for producing grain-oriented electrical steel sheet in which a finish annealed pure film is removed by pickling or the like and the surface of the base steel sheet is smoothed by chemical polishing or electrolytic polishing. Patent Document 2 discloses a method for producing grain-oriented electrical steel sheet in which an annealing separator containing alumina (Al2O3) is used during finish annealing to suppress the formation of a finish annealed film itself and smooth the surface of the base steel sheet.

[0012] However, when an insulating coating is formed in contact with (directly on) a smooth base steel sheet surface on which no finish annealing coating is formed, as can be obtained by the techniques of Patent Documents 1 and 2, there is a problem in that the insulating coating is difficult to adhere to the base steel sheet surface (sufficient adhesion cannot be obtained).

[0013] To address these issues, for example, Patent Documents 3, 4, 5, and 6 propose a technique of forming an intermediate layer (base coating) between the base steel sheet and the insulating coating in order to improve the adhesion of the insulating coating to the smoothed surface of the base steel sheet.

[0014] Patent Document 3 discloses a method of forming an intermediate layer on the surface of a base steel sheet by applying an aqueous solution of phosphate or alkali metal silicate to the surface of the base steel sheet. Patent Documents 4 to 6 disclose methods of forming an externally oxidized silicon oxide film as an intermediate layer by subjecting the base steel sheet to a heat treatment for several tens of seconds to several minutes with appropriately controlled temperature and atmosphere.

[0015] The intermediate layers proposed in Patent Documents 3 to 6 are effective to some extent in improving the adhesion of the insulating coating to the base steel sheet and in suppressing the decrease in iron loss by smoothing out the irregularities at the interface between the base steel sheet and the coating. However, in recent years, there has been a demand for further improvement in the coating adhesion. In response to this demand, new technologies have been proposed, as shown in Patent Documents 7, 8, 9, 10, 11, and 12.

[0016] Patent Document 7 discloses a technique for forming a granular outer oxide on the surface of a base steel sheet in addition to an outer oxide film mainly made of silicon oxide. Patent Document 8 discloses a technique for controlling cavities in an outer oxide film mainly made of silicon oxide.

[0017] Patent Documents 9 to 11 disclose techniques for modifying an outer oxide film mainly composed of silicon oxide by incorporating metallic iron or metal-based oxides (e.g., Si-Mn-Cr oxide, Si-Mn-Ca-Ti oxide, Fe oxide, etc.).

[0018] Patent Document 12 discloses a grain-oriented electrical steel sheet having a multi-layer intermediate layer including an oxide film mainly made of silicon oxide produced by an oxidation reaction and a coating layer mainly made of silicon oxide formed by coating and baking.

[0019] As described above, a grain-oriented electrical steel sheet has been proposed that uses an outer oxide film mainly made of silicon oxide as an intermediate layer, thereby ensuring adhesion of the insulating coating to the base steel sheet even if the surface of the base steel sheet is smoothed, and also has excellent magnetic properties.

[0020] Incidentally, when grain-oriented electrical steel sheets are used as the iron cores of transformers, such as wound cores or EI cores, the grain-oriented electrical steel sheets are processed, such as by bending, into the desired shape. When grain-oriented electrical steel sheets having an intermediate layer processed into the desired shape are used in transformers, the insulating coating may peel off due to reactions with moisture in the air or moisture in the oil in which the iron core is immersed. For this reason, grain-oriented electrical steel sheets used as the iron cores of transformers, such as wound cores or EI cores, are required to have not only good adhesion of the insulating coating to the base steel sheet, but also water resistance. However, among the technologies described in the patent documents relating to the above-mentioned grain-oriented electrical steel sheet having an intermediate layer mainly made of silicon oxide, there is no document that mentions peeling of the insulating coating due to water. [Prior art documents] [Patent documents]

[0021] [Patent Document 1] Japanese Patent Publication No. 49-096920 [Patent Document 2] International Publication No. 2002 / 088403 [Patent Document 3] Japanese Patent Application Publication No. 05-279747 [Patent Document 4] Japanese Patent Publication No. 06-184762 [Patent Document 5] Japanese Patent Publication No. 09-078252 [Patent Document 6] Japanese Patent Publication No. 07-278833 [Patent Document 7] Japanese Patent Publication No. 2002-322566 [Patent Document 8] Japanese Patent Publication No. 2002-363763 [Patent Document 9] Japanese Patent Application Publication No. 2003-313644 [Patent Document 10] Japanese Patent Application Publication No. 2003-171773 [Patent Document 11] Japanese Patent Application Publication No. 2002-348643 [Patent Document 12] Japanese Patent Publication No. 2004-342679 Summary of the Invention [Problem to be solved by the invention]

[0022] The present invention has been made in view of the above problems. An object of the present invention is to provide a grain-oriented electrical steel sheet having an intermediate layer mainly made of silicon oxide, which achieves improved adhesion of an insulating coating and improved water resistance, which has not been recognized as a problem in the past, and a method for manufacturing an intermediate steel sheet for the grain-oriented electrical steel sheet. In addition, excellent water resistance means that the progress of peeling of the insulating coating caused by corrosion when water adheres to the surface of the grain-oriented electrical steel sheet can be suppressed. [Means for solving the problem]

[0023] The gist of the present invention is as follows. (1) A steel sheet comprising: a base steel sheet; an intermediate layer formed on the surface of the base steel sheet and mainly composed of silicon oxide; and an insulating coating formed on the surface of the intermediate layer, wherein the number density of oxides in a region 10 μm deep from the surface of the base steel sheet toward the inside of the base steel sheet is 0.020 particles / μm 2After a bending test using a mandrel in accordance with JIS K 5600-5-1 (1999), the area ratio of the intermediate layer remaining area where the intermediate layer remains without peeling in the area where the insulating coating has peeled off is 20% or more, and in an adhesion test conducted in accordance with the bending resistance test of JIS K 5600-5-1 (1999), when the diameter of the wound mandrel is 10 mm, the area where the insulating coating has peeled off is 7.5 mm 2 When the diameter of the mandrel around which the insulation film is wound is 16 mm, the peeled area of ​​the insulation film is 5.0 mm 2 a hot rolling process for producing a hot rolled steel sheet by heating a slab at 1280°C or less and then hot rolling the slab; a hot rolled sheet annealing process for producing an annealed steel sheet by hot rolled sheet annealing; a cold rolling process for producing a cold rolled steel sheet by cold rolling the annealed steel sheet; a decarburization annealing process for producing a mother steel sheet by decarburization annealing the cold rolled steel sheet; an annealing separator application process for applying an annealing separator having a composition containing 50 mass% or more of alumina (Al2O3) and 0 to 50 mass% of magnesia (MgO) as the balance to the mother steel sheet; a finish annealing process for performing finish annealing on the mother steel sheet after the annealing separator application process; H2O / P H2 a cooling step of cooling the base steel sheet in an atmosphere with a viscosity of 0.30 to 100,000; an intermediate layer forming step of heat treating the base steel sheet after the cooling step to form an intermediate layer mainly made of silicon oxide on a surface of the base steel sheet; and an insulating coating forming step of forming an insulating coating on the surface of the intermediate layer after the intermediate layer forming step.

[0024] (2) A method for producing an intermediate steel sheet for the grain-oriented electrical steel sheet described in (1) above, comprising the steps of: a hot rolling process in which a slab is heated to 1280°C or less and then hot-rolled to produce a hot-rolled steel sheet; a hot-rolled sheet annealing process in which the hot-rolled steel sheet is annealed to produce an annealed steel sheet; a cold rolling process in which the annealed steel sheet is cold-rolled to produce a cold-rolled steel sheet; and a decarburization annealing process in which the cold-rolled steel sheet is decarburized to produce a mother steel sheet. The present invention includes a decarburization annealing step of producing a steel sheet having a composition including 50 mass% or more of alumina (Al2O3) and the balance 0 to 50 mass% of magnesia (MgO), a finish annealing step of subjecting the base steel sheet after the annealing separator application step to finish annealing, and a degree of oxidation P, which is represented by the ratio of water vapor partial pressure to hydrogen partial pressure in a temperature range of 1100 to 500°C, of ​​the base steel sheet after the finish annealing step. H2O / P H2 and a cooling step of cooling the intermediate steel sheet for grain-oriented electrical steel sheet in an atmosphere having a viscosity of 0.30 to 100,000. The intermediate steel sheet for grain-oriented electrical steel sheet comprises a base steel sheet and a film-like oxide formed on the surface of the base steel sheet, the film-like oxide is present so as to cover the surface of the base steel sheet in a film-like form, and the number density of the oxide in a region from the outermost surface of the base steel sheet to a depth of 10 μm toward the inside of the base steel sheet is 0.020 particles / μm. 2 The method for producing an intermediate steel sheet for a grain-oriented electrical steel sheet is as follows. Effect of the Invention

[0025] Effects of the Invention The present invention can provide a grain-oriented electrical steel sheet having an intermediate layer mainly made of silicon oxide, which has excellent adhesion to an insulating coating and water resistance, and a method for manufacturing an intermediate steel sheet for this grain-oriented electrical steel sheet. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0026] The present inventors have investigated methods for solving the above-mentioned problems.

[0027] The inventors first observed areas where the insulating coating had peeled off due to moisture in the air or moisture in the oil in which the iron core was immersed (hereinafter referred to as "insulating coating peeled areas"), and as a result, the inventors noticed that the structure of the insulating coating peeled off due to water correlated with the structure of the insulating coating peeled off due to bending deformation.

[0028] Specifically, the following applies: The present inventors first carried out a bending test as specified in JIS K 5600-5-1 (1999) on grain-oriented electrical steel sheets having an intermediate layer and an insulating coating. After the bending test, the surface of the test piece (the surface on the inner side of the bend) was observed with a scanning electron microscope (SEM) to observe the area where the insulating coating had peeled off. As a result of the observation, the area where the insulating coating had peeled off (insulating coating peeled area) included an area where the insulating coating had peeled off but the intermediate layer remained (intermediate layer remaining area), and an area where the intermediate layer had peeled off together with the insulating coating, exposing the surface of the base steel sheet (base steel) (base steel exposed area).

[0029] Both of these regions where the intermediate layer remained and the region where the base steel sheet was exposed also appeared in grain-oriented electrical steel sheets when the insulating coating had been peeled off by water. When the insulating coating had been peeled off by water, the total area of ​​the regions where the base steel sheet was exposed was larger than the total area of ​​the regions where the intermediate layer remained, in the regions where the insulating coating had been peeled off.

[0030] Based on the above findings, the present inventors considered the following regarding the peeling property of the insulating film caused by water in grain-oriented electrical steel sheets having an intermediate layer mainly made of silicon oxide. When a part of the insulating film peels off due to bending or the like, the greater the ratio of the total area of ​​the base steel sheet exposed region in the insulating film peeling region, the greater the peeling progress rate of the insulating film caused by water. In other words, peeling of the insulating film caused by water is further accelerated. Although the reason for this is unclear, it is thought that the base steel sheet exposed region corrodes due to contact with water, and this corrosion accelerates peeling of the insulating film. On the other hand, the greater the ratio of the total area of ​​the intermediate layer remaining region in the insulating film peeling region, the smaller the peeling progress rate of the insulating film caused by water. The degree of peeling of the insulating film caused by water correlates with the ratio of the intermediate layer remaining region in the insulating film peeling region when a bending test specified in JIS K 5600-5-1 (1999) is performed.

[0031] Furthermore, the present inventors investigated a method for increasing the area ratio of the remaining intermediate layer in the insulating coating peeled region after the bending test, focusing on the change in adhesion between the base steel sheet and the intermediate layer caused by controlling the surface condition of the base steel sheet before the formation of the intermediate layer.

[0032] As a result, the inventors discovered that by selecting an appropriate annealing separator, and then controlling the atmosphere during the cooling process of final annealing to appropriately adjust the oxidation state of the base steel sheet surface at the end of final annealing, the adhesion of the intermediate layer formed subsequently can be improved.

[0033] Specifically, the magnesia (MgO) content of the annealing separator is set to 50 mass% or less, and the vicinity of the surface layer of the base steel sheet is made to be free of internally oxidized oxides at least at the time when the secondary recrystallization is completed. The time when the secondary recrystallization is completed means the time when the cooling of the finish annealing is started.

[0034] Here, internal oxidation type means a state in which, when observed on the cross section of the steel sheet, the oxide does not penetrate to the surface of the base steel sheet, but exists surrounded by the base steel sheet. Examples of internal oxidation type oxides (hereinafter also referred to as internal oxides) include forsterite (Mg2SiO4), silica (Si-O), and mullite (Al-Si-O). If internal oxidation type oxides are formed in the base steel sheet, the iron loss of the grain-oriented electrical steel sheet will deteriorate.

[0035] Furthermore, for the atmosphere in the temperature range of 1100 to 500 °C in the cooling process of the final annealing, the degree of oxidation (P H2O / P H2 ) is set in the range of 0.30 to 100,000, and an external oxidation type oxide is formed on the surface of the base steel sheet.

[0036] Here, the external oxidation type does not mean an oxide form that penetrates into the inside of the base steel sheet as in the internal oxidation type, but a state in which the oxide covers the surface of the base steel sheet almost uniformly, that is, in a film-like form. Therefore, hereinafter, the external oxidation type oxide may also be referred to as a film-like oxide. The external oxidation type oxide is a compound of the elements of the base steel sheet and oxygen. In this embodiment, for example, there is an oxide having a layered structure of iron oxide (FeO, Fe2O3) and fayalite (Fe-Si-O).

[0037] "Internal oxidation" and "external oxidation" are not technically classified according to the above-mentioned form, but according to the oxidation mechanism. However, such a classification in the present invention can be complicated, and it can be difficult to confirm the mechanism after oxidation. Therefore, in this embodiment, the classification according to the form of the oxide resulting from the oxidation is described.

[0038] The reason why control of oxides on the surface of the base steel sheet after final annealing increases the area ratio of the remaining intermediate layer in the insulating coating peeled region after the bending test is not clear, but the following factors are thought to be the cause. The intermediate layer formed in the intermediate layer formation process is generally considered to be formed during the oxidation of the Si-containing base steel sheet. However, if an oxide already exists on the surface of the base steel sheet after final annealing, it is necessary to consider the effect of the reduction of this oxide on the intermediate layer. In the wide temperature range of 1100 to 500 ° C after final annealing, the external oxidation type oxide that is formed relatively slowly with the temperature drop is considered to be film-like and has high continuity between the base steel sheet and the oxide, such as changes in element concentration and structure in the plate thickness direction. It is considered that the intermediate layer is formed while such oxide is reduced, and the atomic bonding structure between the base steel sheet surface and the intermediate layer becomes stronger, improving adhesion.

[0039] If the oxides have a form in which they have penetrated into the base steel sheet, they are not reduced when the intermediate layer is formed, and unevenness remains at the interface between the base steel sheet and the intermediate layer. This becomes an obstacle to the movement of the domain walls when the electrical steel sheet is magnetized. Therefore, it is considered necessary to avoid the formation of internally oxidized oxides as much as possible.

[0040] We will now describe the grain-oriented electrical steel sheet according to one embodiment of the present invention (grain-oriented electrical steel sheet according to this embodiment) completed based on the above findings, the intermediate steel sheet for the grain-oriented electrical steel sheet according to this embodiment, and the manufacturing methods thereof. The grain-oriented electrical steel sheet according to this embodiment comprises a base steel sheet, an intermediate layer formed on the surface of the base steel sheet and mainly made of silicon oxide, and an insulating coating formed on the surface of the intermediate layer. The number density of oxides in a region extending from the surface of the base steel sheet to a depth of 10 μm toward the inside of the base steel sheet (a region beginning at the surface of the base steel sheet and ending at a depth of 10 μm in the depth direction (thickness direction) from the surface) is 0.020 particles / μm. 2In addition, after a bending test using a mandrel in accordance with JIS K 5600-5-1 (1999), the area ratio of the area where the intermediate layer remains unpeeled in the area where the insulating coating has peeled off is 20% or more, and in an adhesion test conducted in accordance with the bending endurance test of JIS K 5600-5-1 (1999), the area where the insulating coating has peeled off is 7.5 mm2 or less when the diameter of the mandrel around which the cable is wrapped is 10 mm, and the area where the insulating coating has peeled off is 5.0 mm2 or less when the diameter of the mandrel around which the cable is wrapped is 16 mm.

[0041] [Grain-oriented electrical steel sheet] The grain-oriented electrical steel sheet according to this embodiment is obtained by forming an intermediate layer and an insulating coating on an intermediate steel sheet for grain-oriented electrical steel sheet. In other words, the grain-oriented electrical steel sheet according to this embodiment comprises a base steel sheet and a coating formed in contact with the surface of the base steel sheet. This coating comprises an intermediate layer formed in contact with the surface of the base steel sheet and an insulating coating formed in contact with the surface of the intermediate layer.

[0042] [Base steel plate] The grain-oriented electrical steel sheet according to this embodiment is characterized by the number density of oxides in the surface layer of the base steel sheet and the configuration of the coating (intermediate layer and insulating coating) formed on the surface of the base steel sheet. Specifically, the number density of oxides in the area 10 μm deep from the surface of the base steel sheet toward the inside of the base steel sheet is 0.020 particles / μm 2 In this embodiment, the number density of oxides is 0.020 particles / μm 2 The state where the number density of oxides in the region from the surface of the base steel sheet to a depth of 10 μm toward the inside of the base steel sheet is 0.020 particles / μm or less is expressed as "substantially no internal oxides are present". In other words, the surface layer portion of the base steel sheet provided in the grain-oriented electrical steel sheet according to this embodiment (a region from the surface of the base steel sheet to a depth of 10 μm toward the inside of the base steel sheet) is substantially free of internal oxides, which are oxides that have penetrated into the inside of the base steel sheet. 2 If it is over 100%, the iron loss of the grain-oriented electrical steel sheet is deteriorated.

[0043] The number density of oxides in the above region (internal oxides) can be determined by the following method: observing a steel sheet cross section perpendicular to the rolling direction with a scanning electron microscope (SEM) at a magnification of 5000x or more, and measuring the number density of oxides with a circle equivalent diameter of 0.1 μm or more in a region 100 μm in a direction parallel to the steel sheet surface and 10 μm deep from the surface (outermost surface) of the base steel sheet toward the inside of the base steel sheet.

[0044] Furthermore, in the grain-oriented electrical steel sheet according to the present embodiment, the area ratio of the intermediate layer remaining region, where the intermediate layer does not peel off and remains, to the region where the insulating coating has peeled off is 20% or more after a bending test using a mandrel in accordance with JIS K 5600-5-1 (1999). The diameter of the mandrel is, for example, 10 to 16 mm.

[0045] It is believed that if the base steel sheet is exposed, it will corrode upon contact with water, causing further peeling of the insulating coating. On the other hand, if the adhesion between the base steel sheet and the intermediate layer is high, the intermediate layer will remain without peeling even in areas where the insulating coating has peeled off. In other words, even if the insulating coating peels off, it is believed that as long as the intermediate layer remains, corrosion of the base steel sheet can be suppressed and further peeling of the insulating coating can be suppressed. For this reason, in the grain-oriented electrical steel sheet according to this embodiment, the adhesion between the base steel sheet and the intermediate layer is improved.

[0046] The base steel sheet of the grain-oriented electrical steel sheet according to this embodiment is controlled so that the area ratio of the intermediate layer remaining area where the intermediate layer does not peel off and remains in the area where the insulating film peels off after a bending test (hereinafter, may be referred to as the intermediate layer remaining rate) is 20% or more, and therefore has excellent water resistance. If the area ratio of the intermediate layer remaining area is less than 20%, the water resistance decreases. The intermediate layer remaining rate may be 100%.

[0047] The base steel sheet of the grain-oriented electrical steel sheet according to the present embodiment is not particularly limited in chemical composition and structure as long as it satisfies the number density of the internal oxides and the area ratio of the remaining intermediate layer region. For example, the base steel sheet of the present embodiment may be a base steel sheet of a general grain-oriented electrical steel sheet. An example of the base steel sheet of the grain-oriented electrical steel sheet according to the present embodiment will be described below.

[0048] [Chemical composition of base steel plate] The chemical composition of the base steel sheet of the grain-oriented electrical steel sheet according to this embodiment can be the same as that of a base steel sheet in a general grain-oriented electrical steel sheet. The chemical composition of the base steel sheet contains, for example, the following elements. Unless otherwise specified, "%" used for the content of each element in the chemical composition of the base steel sheet means mass %. Numerical ranges described with "~" include the lower limit and upper limit.

[0049] The base steel sheet of the grain-oriented electrical steel sheet according to this embodiment contains, for example, 0.50 to 7.00% Si, 0.005% or less C, and 0.0050% or less N, with the balance being Fe and impurities. Below, the reasons for limiting a representative example of the chemical composition of the base steel sheet of the grain-oriented electrical steel sheet according to this embodiment will be described.

[0050] Si: 0.50-7.00% Silicon (Si) increases the electrical resistance of grain-oriented electrical steel sheets and reduces iron loss. If the Si content is less than 0.50%, this effect is not sufficiently obtained. Therefore, the Si content is preferably 0.50% or more. The Si content is more preferably 1.50% or more, and further preferably 2.50% or more. On the other hand, if the Si content exceeds 7.00%, the saturation magnetic flux density of the mother steel sheet decreases, and the iron loss of the grain-oriented electrical steel sheet deteriorates. Therefore, the Si content is preferably 7.00% or less. The Si content is more preferably 5.50% or less, and further preferably 4.50% or less.

[0051] C: 0.005% or less Carbon (C) forms compounds in the base steel sheet and deteriorates the core loss of the grain-oriented electrical steel sheet. Therefore, the C content is preferably 0.005% or less. The C content is more preferably 0.004% or less, and further preferably 0.003% or less. On the other hand, since it is preferable that the C content is as low as possible, 0% is acceptable, but C may be contained as an impurity in steel in some cases, and therefore the C content may be more than 0%.

[0052] N: 0.0050% or less Nitrogen (N) forms compounds in the base steel sheet and deteriorates the core loss of the grain-oriented electrical steel sheet. Therefore, the N content is preferably 0.0050% or less. The N content is more preferably 0.0040% or less, and further preferably 0.0030% or less. On the other hand, since it is preferable that the N content is as low as possible, 0% is acceptable, but N may be contained as an impurity in steel in some cases, and therefore the N content may be more than 0%.

[0053] The balance of the chemical composition of the base steel sheet is composed of Fe and impurities. Note that the "impurities" referred to here refer to elements that are mixed in from components contained in raw materials or components mixed in during the manufacturing process when the base steel sheet is industrially manufactured, and that do not substantially affect the effects obtained by the grain-oriented electrical steel sheet according to the present embodiment.

[0054] [Optional element] The chemical composition of the base steel sheet basically contains the above elements with the remainder being Fe and impurities, but for the purpose of improving magnetic properties and solving manufacturing problems, one or more optional elements may be contained in place of a portion of Fe. Examples of optional elements contained in place of a portion of Fe include the following elements. These elements do not need to be contained, so the lower limit is 0%. On the other hand, if the content of these elements is too high, precipitates are generated and the iron loss of the grain-oriented electrical steel sheet deteriorates, or ferrite transformation is suppressed, so that the GOSS orientation cannot be sufficiently obtained, or the saturation magnetic flux density decreases, thereby deteriorating the iron loss of the grain-oriented electrical steel sheet. Therefore, even if they are contained, it is preferable to keep them within the following ranges. Acid-soluble Al: 0.0065% or less, Mn: 1.00% or less, S and Se: 0.001% or less in total Bi: 0.010% or less, B: 0.0080% or less, Ti: 0.015% or less, Nb: 0.020% or less, V: 0.015% or less, Sn: 0.50% or less, Sb: 0.50% or less, Cr: 0.30% or less, Cu: 0.40% or less, P: 0.50% or less, Ni: 1.00% or less, and Mo: 0.10% or less. Note that "S and Se: 0.001% or less in total" may mean that the base steel sheet contains only S or Se, and the content of either S or Se is 0.001% or less, or that the base steel sheet contains both S and Se, and the content of S and Se is 0.001% or less in total.

[0055] The chemical composition of the base steel sheet of the grain-oriented electrical steel sheet according to this embodiment described above is obtained by employing the manufacturing method of the grain-oriented electrical steel sheet according to this embodiment using a slab having the chemical composition described below.

[0056] The chemical composition of the base steel sheet of the grain-oriented electrical steel sheet according to this embodiment may be measured using spark optical emission spectrometry (Spark-OES). When the content is small, it may be measured using inductively coupled plasma-mass spectrometry (ICP-MS) as necessary. Acid-soluble Al may be measured by ICP-MS using the filtrate obtained by thermally decomposing a sample with acid. C and S may be measured using a combustion-infrared absorption method, and N may be measured using an inert gas fusion-thermal conductivity method.

[0057] [Surface roughness of base steel plate] The roughness of the surface of the base steel sheet is not particularly limited. However, if irregularities are formed on the surface of the base steel sheet, the effect of reducing iron loss may be hindered. In order to avoid such a hindrance to the effect of reducing iron loss, for example, the roughness of the surface of the base steel sheet is preferably 1.0 μm or less in terms of Ra (arithmetic mean roughness). A more preferred upper limit of the arithmetic mean roughness Ra of the surface of the base steel sheet is 0.8 μm, and an even more preferred upper limit is 0.6 μm. The lower limit of the arithmetic mean roughness Ra of the surface of the base steel sheet may be 0.001 μm.

[0058] The arithmetic mean roughness Ra of the surface of the base steel sheet is measured by the following method. A sample is taken with a cross section perpendicular to the rolling direction of the grain-oriented electrical steel sheet as the observation surface. The roughness of the base steel sheet surface on the obtained observation surface is measured. Specifically, when a coating such as a finish-baked pure coating or an intermediate layer is formed on the surface of the base steel sheet, the interface between the base steel sheet and the intermediate layer on the observation surface (cross section) is measured with an accuracy of 0.01 μm or better, and when no coating is formed and the surface of the base steel sheet is exposed, the position coordinates in the sheet thickness direction of the base steel sheet surface on the observation surface (cross section) are measured with an accuracy of 0.01 μm or better, and the arithmetic mean roughness Ra according to JIS B 0601 (2001) is calculated. The measurement is performed over a range of 2 mm (total of 20,000 points) continuous at 0.1 μm pitch in a direction parallel to the surface of the base steel sheet, and the arithmetic mean roughness Ra is calculated with a reference length of 2 mm. The arithmetic mean roughness Ra is calculated by the above method at at least five arbitrary points on the surface of the base steel sheet, and the average value of the Ra values ​​obtained at each point is defined as the arithmetic mean roughness Ra of the surface of the base steel sheet. This observation can be performed by SEM, and it is practical to apply image processing to measure the position coordinates.

[0059] [Middle layer] The intermediate layer is formed in contact with the surface of the base steel sheet, which is substantially free of internal oxides. The intermediate layer is an outer oxide film mainly composed of silicon oxide. Here, "mainly composed of silicon oxide" means that the composition of the intermediate layer satisfies the following: Fe content less than 30 atomic %, P content less than 5 atomic %, Si content less than 50 atomic % and 20 atomic % or more, O content less than 80 atomic % and 50 atomic % or more, and Mg content less than 10 atomic %.

[0060] The intermediate layer is a layer disposed between the base steel sheet and the insulating coating, and is effective for bonding the base steel sheet and the insulating coating. The intermediate layer is formed, for example, by reducing a film-like oxide formed by carrying out a specific cooling step in the final annealing step, as described in the manufacturing process below.

[0061] The silicon oxide that constitutes the main part of the intermediate layer is preferably SiOx (x = 1.0 to 2.0), and more preferably SiOx (x = 1.5 to 2.0). This is because silicon oxide is more stable. Silica (SiO2) can be formed by carrying out a sufficient heat treatment to form silicon oxide on the surface of the base steel sheet.

[0062] Silicon oxide exists in an amorphous state in the intermediate layer formed by subjecting the base steel sheet to heat treatment under conditions consisting of 20-50 volume % hydrogen, the balance being nitrogen and impurities, and held at a temperature range of 600-1150°C for 10-600 seconds in an atmosphere with a dew point of -20-2°C. The intermediate layer mainly composed of amorphous silicon oxide formed under these heat treatment conditions is a dense intermediate layer that has high strength to withstand thermal stress, has a relatively small elastic modulus, and is capable of easily relaxing thermal stress, making it preferable.

[0063] The base steel sheet of grain-oriented electrical steel sheet contains a high concentration of Si (for example, Si: 0.50 to 7.00 mass%). This creates a strong chemical affinity between the intermediate layer, which is mainly made of silicon oxide, and the base steel sheet, resulting in strong adhesion between the intermediate layer and the base steel sheet.

[0064] The thickness of the intermediate layer is not particularly limited. If the thickness is 2 nm or more, the adhesion of the insulating coating to the base steel sheet is more effectively increased, so the preferred thickness of the intermediate layer is 2 nm or more, and more preferably 5 nm or more. If the thickness of the intermediate layer is 400 nm or less, defects such as voids and cracks in the intermediate layer are effectively suppressed. Therefore, the preferred thickness of the intermediate layer is 400 nm or less, and more preferably 300 nm or less. The intermediate layer is preferably made thin within a range that ensures the coating adhesion, which can shorten the formation time and contribute to high productivity, and can also suppress the decrease in the space factor when used as an iron core. Therefore, the thickness of the intermediate layer is more preferably 100 nm or less, and even more preferably 50 nm or less.

[0065] The thickness of the intermediate layer is measured as follows. The cross section of the intermediate layer is observed and measured with a TEM (transmission electron microscope) with an electron beam diameter of 10 nm. Specifically, for example, for TEM observation, a sample is cut out so as to have an observation cross section parallel to the sheet thickness direction, and in the observation cross section of the sample, the width in the direction parallel to the surface of the base steel sheet is 10 μm or more, and from a measurement area including the intermediate layer, the above-mentioned base steel sheet, and the insulating coating described below, five or more measurement positions separated from each other by 2 μm or more in the width direction are selected, and the thickness of the intermediate layer is measured with the TEM. The average of the measured values ​​is taken as the thickness of the intermediate layer. When the thickness of the intermediate layer at each measurement position in the measurement area is measured with the TEM, the layer existing between the above-mentioned base steel sheet and the insulating coating is measured as the intermediate layer.

[0066] [Insulating film] The insulating film is formed on the surface of the intermediate layer. A known insulating film can be used. As an example, the insulating film is mainly composed of a compound containing P, O, and Si, and may contain Cr. The insulating film applies tension to the mother steel sheet to reduce the iron loss of the steel sheet. The insulating film further ensures electrical insulation between the grain-oriented electrical steel sheets when the grain-oriented electrical steel sheets are stacked for use.

[0067] If the insulating coating is thin, the tension applied to the base steel sheet decreases and the insulating properties also decrease, so the thickness of the insulating coating is preferably 0.1 μm or more, and more preferably 0.5 μm or more. On the other hand, if the thickness of the insulating coating exceeds 10 μm, there is a risk of cracks occurring in the insulating coating during the insulating coating formation stage, so the thickness of the insulating coating is preferably 10 μm or less, and more preferably 5 μm or less. The thickness of the insulating coating can be measured by observing the cross section of the insulating coating (or the grain-oriented electrical steel sheet) with a TEM (transmission electron microscope). The specific measurement method may be the same as the method for measuring the thickness of the intermediate layer.

[0068] If necessary, the insulating coating may be subjected to a magnetic domain refining process by laser, plasma, mechanical methods, etching, or other methods to form localized micro-distorted regions or grooves.

[0069] [Characteristics of the coating structure of grain-oriented electrical steel sheets] In the grain-oriented electrical steel sheet according to the present embodiment, after a bending test using a mandrel in accordance with JIS K 5600-5-1 (1999), the area ratio of the intermediate layer remaining area in which the intermediate layer does not peel off and remains in the area where the insulating film has peeled off is controlled to be 20% or more. Therefore, when a bending test in accordance with JIS K 5600-5-1 (1999) is performed, the area ratio of the intermediate layer remaining area in which the intermediate layer does not peel off and remains in the area where the insulating film has peeled off is 20% or more. The above-mentioned area ratio of the intermediate layer remaining area is preferably 30% or more, more preferably 40% or more. The intermediate layer remaining area may be 100%.

[0070] The area ratio of the remaining intermediate layer region is determined by the following method. A rectangular sample measuring 10 mm in the direction perpendicular to the rolling direction of the grain-oriented electrical steel sheet and 150 mm in the direction parallel to the rolling direction is taken. The observation surface of the 10 mm x 150 mm sample of the test piece is the surface that contains the coating. A bending test is carried out on the taken sample in accordance with JIS K 5600-5-1 (1999). Specifically, the taken sample is wrapped around a round bar (mandrel) with a diameter of 10 to 16 mm and bent 180°. The test piece is then bent back.

[0071] The observation surface (inner surface of the bend) after the bending test is observed using a SEM COMPO image, and the area of ​​the observation surface where the insulation coating has peeled off (insulation coating peeled area) is identified. Specifically, the COMPO image of the observation surface is converted into a monochrome image with 256 gradations, and the area with gradations of 50% or less from the white side is determined to be the area where the insulation coating has peeled off. The total area of ​​the identified insulation coating peeled areas is calculated.

[0072] The evaluation area of ​​insulation coating peeling in the bending test is defined by the following formula. If the area of ​​insulation coating peeling is less than 5% of the evaluation area, the bending diameter is reduced (a mandrel with a smaller diameter is used) and the test is reevaluated. If the reevaluation shows that the area of ​​insulation coating peeling is 5% or more of the evaluation area, the area ratio of the remaining intermediate layer is calculated. (Evaluation area for insulation film peeling) = (Mandrel diameter) × (Pi) ÷ 2

[0073] Furthermore, the insulating film peeled region of the observation surface is mapped using an energy dispersive X-ray spectrometer (SEM-EDS) to obtain the Si concentration distribution in atomic percent. In the obtained Si concentration distribution, the maximum and minimum values ​​of the Si concentration are identified. The region that satisfies the following formula is defined as the intermediate layer remaining region. (Si concentration in the region)>{(maximum Si concentration)+(minimum Si concentration)} / 2 However, when the maximum value of the Si concentration and the minimum value of the Si concentration satisfy the following formula, the area ratio of the remaining intermediate layer region is set to 0%. (Maximum Si concentration) - (Minimum Si concentration) < 5 atomic %

[0074] The ratio of the total area of ​​the remaining intermediate layer region on the observation surface to the total area of ​​the insulating coating peeled region (peeled coating portion) mapped by EDS is defined as the area ratio (%) of the remaining intermediate layer region. In other words, the area ratio of the remaining intermediate layer region is defined by the following formula. Area ratio of remaining intermediate layer area = (total area of ​​remaining intermediate layer area) / (total area of ​​EDS mapping) × 100 Here, the total EDS mapping area is 15 mm 2 The area ratio of the intermediate layer remaining region may be calculated as the average value of multiple test pieces when the area of ​​the peeled coating portion is insufficient for one test piece.

[0075] If the area ratio of the remaining intermediate layer area where the intermediate layer remains unpeeled in the area where the insulating coating has peeled off after a bending test using a mandrel in accordance with JIS K 5600-5-1 (1999) is 20% or more, the adhesion of the intermediate layer to the base steel sheet is sufficiently high. Therefore, in this case, even if part of the insulating coating has peeled off, the base steel sheet is covered with the intermediate layer, so that the progress of peeling of the insulating coating due to corrosion caused by the adhesion of water can be suppressed. In other words, the water resistance of the grain-oriented electrical steel sheet can be improved.

[0076] [Intermediate steel sheets for grain-oriented electrical steel sheets] The intermediate steel sheet for grain-oriented electrical steel sheet according to this embodiment comprises a base steel sheet and a film-like oxide formed on the surface of the base steel sheet. The film-like oxide is present so as to cover the surface of the base steel sheet in a film-like form. The base steel sheet has a number density of oxides (internal oxides) present in the base steel sheet in a region 10 μm deep from the surface of the base steel sheet toward the inside of the base steel sheet of 0.020 pieces / μm 2 The following is the result. This intermediate steel sheet is a steel sheet used in the manufacture of the grain-oriented electrical steel sheet according to this embodiment, and is a steel sheet after finish annealing (more specifically, after the cooling process described below and before the intermediate layer forming process). An intermediate layer mainly made of silicon oxide is formed on the surface of the mother steel sheet of this intermediate steel sheet, and an insulating coating is further formed on the surface of the intermediate layer, thereby obtaining the grain-oriented electrical steel sheet according to this embodiment.

[0077] In the intermediate steel sheet for the grain-oriented electrical steel sheet according to this embodiment, the surface of the base steel sheet is substantially free of internal oxides, which are oxides that have penetrated into the inside of the base steel sheet. If internal oxides are present after final annealing, the internal oxides are not reduced when the intermediate layer is formed, and the internal oxides remain on the surface of the base steel sheet. These internal oxides become an obstacle to the movement of domain walls when the grain-oriented electrical steel sheet is magnetized, and the iron loss of the grain-oriented electrical steel sheet deteriorates. On the other hand, a film-like oxide formed by external oxidation is present on the surface of the base steel sheet, covering the surface of the base steel sheet in a film-like form.

[0078] Specifically, the absence of internal oxides means that the number density of oxides in a region extending from the surface (outermost surface) of the base steel sheet to a depth of 10 μm in the sheet thickness direction toward the inside of the base steel sheet (the region beginning at the surface of the base steel sheet and ending at a depth of 10 μm in the depth direction (thickness direction) from the surface) is 0.020 particles / μm 2 The number density of oxides in this region can be determined by observing the cross section of the steel sheet with a scanning electron microscope (SEM) at a magnification of 5000x or more, and measuring the number density of oxides with a circular equivalent diameter of 0.1 μm or more in a region 100 μm in a direction parallel to the steel sheet surface and 10 μm deep from the surface of the base steel sheet toward the inside of the base steel sheet. The number density of this internal oxide does not change even if an intermediate layer or an insulating film is formed.

[0079] The oxides are formed into a film-like structure that covers the entire surface of the base steel sheet by adjusting the conditions of the cooling process after the final annealing. Specifically, in the cooling process after the final annealing, the base steel sheet is cooled to a temperature range of 1100 to 500°C, and the oxidation degree (P H2O / P H2 This can be achieved by cooling in an atmosphere with an oxidation degree of 0.30 to 100,000. If the oxidation degree is 0.30 to 100,000, the film-like oxide will have a hierarchical structure and will uniformly cover the surface of the base steel sheet. As a result, an intermediate layer that is strongly bonded to the base steel sheet will be formed in the next process, which is thought to improve the adhesion of the insulating coating.

[0080] The film-like oxides after the final annealing are mainly iron oxides (FeO, Fe2O3) and fayalite (Fe-Si-O). Therefore, it is considered that the Fe in the iron oxide is reduced in the atmosphere that mainly forms the intermediate layer in the next process, and the film-like oxides are replaced by an intermediate layer mainly composed of externally oxidized silicon oxide.

[0081] Next, a method for producing the grain-oriented electrical steel sheet according to the present embodiment and a method for producing an intermediate steel sheet for the grain-oriented electrical steel sheet according to the present embodiment will be described. The coatings (intermediate layer and insulating coating) having the above-mentioned characteristics can be produced, for example, by the production method described below.

[0082] The intermediate steel sheet for the grain-oriented electrical steel sheet according to this embodiment is obtained by a manufacturing method including the following steps (S0) to (S62). (S0) Preparation process (S1) Hot rolling process (S2) Hot rolled plate annealing process (S3) Cold rolling process (S4) Decarburization annealing process (S5) Annealing separator application process (S61) Finish annealing process (S62) Cooling process

[0083] The grain-oriented electrical steel sheet according to this embodiment is obtained by a manufacturing method that further includes steps (S7) and (S8) in addition to the above steps (S0) to (S62). (S7) Intermediate layer formation process (S8) Insulation film formation process

[0084] Each step will be described below.

[0085] [S0: Preparation process] In the preparation step, a slab is prepared. The method for producing the slab is not limited, but the following method is exemplified. Molten steel is produced (smelted). A slab is produced using the molten steel. The slab may be produced by a continuous casting method. An ingot may be produced using the molten steel, and the ingot may be bloomed to produce a slab. The slab may be produced by other methods. The thickness of the slab is not particularly limited. The thickness of the slab is, for example, 150 to 350 mm. The thickness of the slab is preferably 220 to 280 mm. As the slab, a so-called thin slab having a thickness of 10 to 70 mm may be used. When a thin slab is used, rough rolling before finish rolling can be omitted in the hot rolling process.

[0086] [Chemical composition of slabs] The chemical composition of the slab can be set to the following range, for example, taking into consideration the contents that change during the manufacturing process from the slab to the grain-oriented electrical steel sheet in order to obtain the chemical composition of the base steel sheet in a typical grain-oriented electrical steel sheet. Note that "%" used for the content of each element in the chemical composition of the slab means mass % unless otherwise specified. Numerical ranges described with "~" include the lower limit and upper limit. Si: 0.80-7.00%, C: 0.085% or less, Acid soluble Al: 0.010~0.065%, N: 0.0040~0.0120%, Mn: 0.05 to 1.00%, S and Se: 0.003 to 0.015% in total, and Remainder: Fe and impurities. Each element will be described below.

[0087] Si: 0.80-7.00% Silicon (Si) increases the electrical resistance of grain-oriented electrical steel sheets and reduces iron loss. If the Si content is less than 0.80%, gamma transformation occurs during final annealing, damaging the crystal orientation of the grain-oriented electrical steel sheets. On the other hand, if the Si content exceeds 7.00%, the cold workability decreases and cracks are likely to occur during cold rolling. Therefore, the Si content is preferably 0.80 to 7.00%. The Si content is more preferably 2.00% or more, and further preferably 2.50% or more. The Si content is more preferably 4.50% or less, and further preferably 4.00% or less.

[0088] C: 0.085% or less Carbon (C) is inevitably contained. Although C is an effective element for controlling the primary recrystallization structure, it has a negative effect on magnetic properties. Therefore, the C content is preferably 0.085% or less. The C content is preferably as low as possible. However, when considering the productivity in industrial production, the C content is preferably 0.020% or more, and more preferably 0.040% or more. C is purified in the decarburization annealing process and the finish annealing process described below, and the C content becomes 0.005% or less after the finish annealing process.

[0089] Acid soluble Al: 0.010~0.065% Acid-soluble aluminum (Al) combines with N to precipitate as (Al,Si)N, and functions as an inhibitor. When the content of acid-soluble Al is 0.010 to 0.065%, the secondary recrystallization is stable. Therefore, the content of acid-soluble Al is preferably 0.010 to 0.065%. The content of acid-soluble Al is more preferably 0.015% or more, and further preferably 0.020% or more. From the viewpoint of the stability of secondary recrystallization, the content of acid-soluble Al is more preferably 0.045% or less, and further preferably 0.035% or less. If acid-soluble Al remains after final annealing, it forms a compound and deteriorates the iron loss of the grain-oriented electrical steel sheet. Therefore, it is preferable to reduce the amount of acid-soluble Al contained in the steel sheet after final annealing as much as possible by purification during final annealing. Depending on the conditions of the final annealing, the steel sheet after final annealing may not contain acid-soluble Al.

[0090] N: 0.0040~0.0120% Nitrogen (N) combines with Al to function as an inhibitor. If the N content is less than 0.0040%, a sufficient amount of inhibitor is not generated. The N content is more preferably 0.0050% or more, and further preferably 0.0060% or more. On the other hand, if the N content exceeds 0.0120%, blisters, a type of defect, tend to occur in the steel sheet. Therefore, the N content is preferably 0.0040 to 0.0120%. The N content is more preferably 0.0110% or less, and further preferably 0.0100% or less. N is purified in the final annealing process, and the N content after the final annealing process is 0.0050% or less.

[0091] Mn: 0.05 to 1.00% Manganese (Mn) combines with S or Se to produce MnS or MnSe, and functions as an inhibitor. When the Mn content is within the range of 0.05 to 1.00%, secondary recrystallization is stable. Therefore, the preferred Mn content is 0.05 to 1.00%. The Mn content is preferably 0.06% or more, and more preferably 0.07% or more. Moreover, the Mn content is more preferably 0.50% or less, and further preferably 0.20% or less. Depending on the conditions of the final annealing, the steel sheet after the final annealing may not contain Mn.

[0092] S and Se: 0.003 to 0.015% in total Sulfur (S) and selenium (Se) combine with Mn to produce MnS or MnSe, and function as inhibitors. If the total content of S and Se is 0.003 to 0.015%, the secondary recrystallization is stable. Therefore, the total content of S and Se is preferably 0.003 to 0.015%. If S and Se remain after final annealing, they form compounds and deteriorate the iron loss of the grain-oriented electrical steel sheet. Therefore, it is preferable to reduce the amount of S and Se contained in the steel sheet after final annealing as much as possible by purification during final annealing. Depending on the conditions of the final annealing, the steel sheet after final annealing may not contain S and Se.

[0093] Here, "the total content of S and Se is 0.003 to 0.015%" may mean that the slab contains only one of S or Se and the content of either S or Se is 0.003 to 0.015%, or that the slab contains both S and Se and the total content of S and Se is 0.003 to 0.015%.

[0094] The balance of the chemical composition of the slab used in manufacturing the grain-oriented electrical steel sheet according to the present embodiment is composed of Fe and impurities. The "impurities" referred to here mean elements that are mixed in from components contained in raw materials or components mixed in during the manufacturing process when the base steel sheet of the grain-oriented electrical steel sheet according to the present embodiment is industrially manufactured, and that do not substantially adversely affect the effects obtained by the grain-oriented electrical steel sheet according to the present embodiment.

[0095] [Optional element] The chemical composition of the slab may contain one or more optional elements in place of a portion of Fe, taking into consideration the strengthening of the inhibitor function by compound formation and the effect on magnetic properties. Examples of optional elements contained in place of a portion of Fe include the following elements. These elements are optional elements and do not need to be contained, so the lower limit is 0%. Bi: 0.010% or less, B: 0.080% or less, Ti: 0.015% or less, Nb: 0.20% or less, V: 0.15% or less, Sn: 0.50% or less, Sb: 0.50% or less, Cr: 0.30% or less, Cu: 0.40% or less, P: 0.50% or less, Ni: 1.00% or less, and Mo: 0.10% or less.

[0096] [S1: Hot rolling process] In the hot rolling process, the prepared slab is hot rolled using a hot rolling mill to produce a steel plate (hot-rolled steel plate). Specifically, first, the slab is heated. For example, the slab is placed in a known heating furnace or a known soaking furnace and heated. The preferred heating temperature of the slab is 1280°C or lower. By setting the heating temperature of the slab to 1280°C or lower, it is possible to avoid various problems (such as the need for a dedicated heating furnace and a large amount of molten scale) that occur when the slab is heated at a temperature higher than 1280°C. The preferred upper limit of the heating temperature of the slab is 1250°C. The heating time of the slab may be 40 to 120 minutes.

[0097] The lower limit of the heating temperature of the slab is not particularly limited. However, if the heating temperature is too low, hot rolling becomes difficult and productivity may decrease. Therefore, the heating temperature may be set in consideration of productivity within a range of 1280°C or less. The preferred lower limit of the heating temperature of the slab is 1100°C.

[0098] It is also possible to omit the slab heating step itself and start hot rolling after casting before the slab temperature drops.

[0099] The heated slab is hot-rolled using a hot rolling mill to produce a hot-rolled steel sheet. The hot rolling mill includes, for example, a roughing mill and a finishing mill arranged downstream of the roughing mill. The roughing mill includes roughing stands arranged in a row. Each roughing stand includes a plurality of rolls arranged one above the other. The finishing mill also includes finishing stands arranged in a row. Each finishing stand includes a plurality of rolls arranged one above the other. After the heated steel material is rolled by the roughing mill, it is further rolled by the finishing mill to produce a hot-rolled steel sheet.

[0100] The thickness of the hot-rolled steel sheet produced by hot rolling is not particularly limited. The thickness of the hot-rolled steel sheet is, for example, 3.5 mm or less. The finishing temperature in the hot rolling process (the temperature of the steel sheet at the exit side of the finishing rolling stand that finally rolls down the steel sheet in the finishing mill) is, for example, 900 to 1000°C. Through the above hot rolling process, a hot-rolled steel sheet is manufactured.

[0101] [S2: Hot rolled plate annealing process] In the hot-rolled sheet annealing process, the hot-rolled steel sheet obtained in the hot rolling process is subjected to hot-rolled sheet annealing to obtain an annealed steel sheet.

[0102] Well-known conditions may be used for the hot-rolled sheet annealing conditions. For example, the annealing temperature in the hot-rolled sheet annealing (furnace temperature in the hot-rolled sheet annealing furnace) is 750 to 1200° C. The holding time at the annealing temperature is, for example, 30 to 600 seconds.

[0103] [S3: Cold rolling process] In the cold rolling process, cold rolling is performed on the annealed steel sheet after the hot-rolled sheet annealing.

[0104] In the cold rolling step, cold rolling may be performed only once or may be performed multiple times. When cold rolling is performed multiple times, intermediate annealing for the purpose of softening may be performed after cold rolling, and then cold rolling may be performed again. The intermediate annealing conditions may be any known method. Before cold rolling the annealed steel sheet, the annealed steel sheet may be subjected to pickling treatment.

[0105] When multiple cold rolling steps are performed without performing an intermediate annealing step, it may be difficult to obtain uniform properties in the manufactured grain-oriented electrical steel sheet. On the other hand, when multiple cold rolling steps are performed and an intermediate annealing step is performed between each cold rolling step, the manufactured grain-oriented electrical steel sheet may have a low magnetic flux density. Therefore, the number of cold rolling steps and the presence or absence of an intermediate annealing step are determined depending on the properties required for the grain-oriented electrical steel sheet to be finally manufactured and the manufacturing cost.

[0106] In one or more cold rollings, the cumulative cold rolling ratio (cumulative rolling reduction) is preferably 80% or more, and more preferably 90% or more. The preferred upper limit of the cumulative cold rolling ratio is 95%. Here, the cumulative cold rolling ratio (%) is defined as follows. Cumulative cold rolling rate (%) = (1 - thickness of cold rolled steel sheet after the last cold rolling / thickness of annealed steel sheet before the start of the first cold rolling) x 100

[0107] The cold-rolled steel sheet obtained by the cold rolling step is wound into a coil. The thickness of the cold-rolled steel sheet is not particularly limited, but in order to further reduce iron loss, it is preferably 0.35 mm or less, and more preferably 0.30 mm or less.

[0108] [S4: Decarburization annealing process] In the decarburization annealing process, decarburization annealing is performed on the cold-rolled steel sheet obtained in the cold rolling process. Decarburization annealing is carried out, for example, by the following method: A cold-rolled steel sheet is loaded into a heat treatment furnace. The temperature of the heat treatment furnace (decarburization annealing temperature) is, for example, kept at 800 to 950°C for 30 to 180 seconds, and the atmosphere of the heat treatment furnace is a moist atmosphere containing hydrogen and nitrogen. By carrying out decarburization annealing under the above-mentioned conditions, primary recrystallization occurs and carbon in the steel sheet is removed from the steel sheet.

[0109] [S5: Annealing separator application process] In the annealing separator application step, the annealing separator is applied to the surface of the base steel sheet after decarburization annealing. In a general method for manufacturing grain-oriented electrical steel sheet, an annealing separator containing 90% by mass or more of MgO is used. In this case, however, a glass film having an uneven shape is formed on the surface of the steel sheet. When a glass film having an uneven shape is formed, iron loss deteriorates. Therefore, in the method for manufacturing grain-oriented electrical steel sheet according to the present embodiment, an annealing separator having a composition containing 50% by mass or more of alumina (Al2O3) and the remainder of magnesia (MgO): 0 to 50% by mass is used as the annealing separator. If the MgO content is 50% by mass or less, it is possible to form a film-like oxide while suppressing the formation of an internal oxide that causes unevenness at the interface with the steel sheet. The upper limit of MgO in the annealing separator is preferably 45% by mass, and more preferably 40% by mass.

[0110] The lower limit of MgO is preferably 10 mass%, and more preferably 15 mass%. If the content of MgO is 10 mass% or more, the formation of mullite (Al-Si-O), which is a type of inner oxide, can be suppressed. This makes it possible to suppress the deterioration of iron loss due to the inner oxide. Al2O3 may be 100 mass %, or may be 90 mass % or less, or 85 mass % or less, or may be 55 mass % or more, or 60 mass % or more.

[0111] [S61: Finish annealing process] In the final annealing process, the mother steel sheet (coil) after the annealing separator application process is subjected to final annealing, which causes the annealing separator to be baked in and secondary recrystallization to occur in the mother steel sheet.

[0112] When the final annealing is performed, the surface of the base steel sheet is oxidized and a film-like oxide is formed on the surface of the base steel sheet. For example, when an annealing separator containing Al2O3 as a main component is applied, a film-like oxide is formed that is mainly composed of oxides of Fe and Si, which are the main components of the steel sheet.

[0113] The final annealing conditions are, for example, as follows: The atmosphere in the furnace during the final annealing is not particularly limited, and may be any well-known atmosphere.

[0114] Final annealing temperature: 1100~1300℃ Holding time at final annealing temperature: 20 to 24 hours If the final annealing temperature is 1100 to 1300° C., sufficient secondary recrystallization occurs, improving the magnetic properties of the grain-oriented electrical steel sheet, and the film-like oxide is formed on the surface of the base steel sheet. If the final annealing temperature is less than 1100°C, sufficient secondary recrystallization may not occur. If it is more than 1300°C, the coil strength may decrease at high temperatures, causing deformation of the coil. If the holding time is less than 20 hours, purification may be insufficient. On the other hand, if the holding time is more than 24 hours, the productivity decreases, which is not preferable.

[0115] [S62: Cooling process] After the final annealing process, a cooling process is carried out to cool the base steel sheet. At this time, in the temperature range where the base steel sheet is 1100 to 500°C, the oxidation degree (P H2O / P H2 Cooling is performed in a gas atmosphere with a thermal expansion coefficient of 0.30 to 100,000. The temperature range of 1,100 to 500°C is a temperature range in which oxidation of the base steel sheet can occur. Therefore, by controlling oxidation over this wide temperature range, a desirable oxide film can be formed.

[0116] If the oxidation degree in the temperature range of 1100 to 500°C is less than 0.30, the oxide itself is not formed. In this case, the adhesion of the intermediate layer formed in the next intermediate layer forming step to the base steel sheet is reduced. As a result, in the manufactured grain-oriented electrical steel sheet, after a bending test performed using a mandrel in accordance with JIS K 5600-5-1 (1999), the area ratio of the intermediate layer remaining area in which the intermediate layer does not peel off in the area where the insulating coating has peeled off is less than 20%. As a result, the peeling resistance (water resistance) of the insulating coating due to water is reduced. On the other hand, if the oxidation degree in the above temperature range exceeds 100,000, an internal oxide is formed. In this case, the internal oxide remains without being reduced even after the intermediate layer is formed, and the core loss of the grain-oriented electrical steel sheet is deteriorated. Therefore, the oxidation degree of the atmosphere in the temperature range of 1100 to 500°C of the base steel sheet is 0.30 to 100,000.

[0117] There are no particular limitations on the cooling method in the temperature range where the base steel sheet reaches 1100 to 500° C. For example, the cooling method may be a method in which the heater is turned off in batch annealing and cooling is continued as is.

[0118] Through the above steps, a base steel sheet that is substantially free of internal oxides and has a film-like oxide formed thereon, i.e., an intermediate steel sheet for the grain-oriented electrical steel sheet according to this embodiment, is manufactured. The intermediate steel sheet for the grain-oriented electrical steel sheet according to this embodiment does not substantially contain internal oxides. Therefore, the surface of the base steel sheet after the finish annealing step is smooth and unevenness is suppressed. For example, the arithmetic mean roughness Ra of the surface of the base steel sheet is 1.0 μm or less. Therefore, the grain-oriented electrical steel sheet obtained by using this intermediate steel sheet can achieve low iron loss.

[0119] The above-mentioned finish annealing also serves as purification annealing, which removes inhibitor elements such as Al, N, Mn, S and Se from the steel.

[0120] [S7: Intermediate layer formation process] In the intermediate layer forming step, a heat treatment is performed on the intermediate steel sheet for the grain-oriented electrical steel sheet according to this embodiment, thereby forming an intermediate layer that is in contact with the surface of the base steel sheet and is mainly made of silicon oxide.

[0121] The conditions of the heat treatment for forming the intermediate layer are not particularly limited. When the intermediate layer is formed to a thickness of 2 to 400 nm, it is preferable to hold the temperature in the range of 300 to 1150° C. for 5 to 120 seconds, and more preferably to hold the temperature in the range of 600 to 1150° C. for 10 to 60 seconds. Furthermore, from the viewpoint of preventing oxidation of the inside of the base steel sheet, it is preferable to use a reducing atmosphere during heating up to the temperature range to be maintained and during maintaining the temperature, and it is more preferable to use a nitrogen atmosphere mixed with hydrogen. An example of a nitrogen atmosphere mixed with hydrogen is an atmosphere consisting of 5 to 50 volume % hydrogen and the balance nitrogen and impurities, and having a dew point of -20 to 2°C. In particular, an atmosphere consisting of 10 to 35 volume % hydrogen, the balance nitrogen and impurities, and having a dew point of -10 to 0°C is preferred.

[0122] In the intermediate layer forming step, the film-like oxide is reduced to form an intermediate layer mainly composed of silicon oxide. This improves the adhesion of the intermediate layer to the base steel sheet. As a result, in the produced grain-oriented electrical steel sheet, the area ratio of the intermediate layer remaining area, where the intermediate layer remains without peeling, in the area where the insulating coating has peeled off is 20% or more after a bending test performed using a mandrel in accordance with JIS K 5600-5-1 (1999).

[0123] The heat treatment in the intermediate layer forming step may be a separate heat treatment for the purpose of forming the intermediate layer only. The heat treatment may also be performed simultaneously or consecutively with the heat treatment for the purpose of forming the insulating film. When a separate heat treatment for the purpose of forming the intermediate layer only is performed, a separate heat treatment for the purpose of forming the insulating film is performed thereafter.

[0124] [S8: Insulation film formation process] In the insulating film forming step, an insulating film made of a compound containing P, O and Si is formed on the surface of the intermediate layer. The insulating film may further contain Cr.

[0125] In the insulating film forming process, a coating solution containing phosphoric acid or a phosphate, colloidal silica, and, if necessary, chromic anhydride or a chromate is applied to the surface of the intermediate layer. After the coating solution is applied, baking is performed to form an insulating film in contact with the surface of the intermediate layer.

[0126] Examples of phosphates include phosphates of Ca, Al, Mg, Sr, etc. Colloidal silica is not particularly limited, and its particle size can be used appropriately. Furthermore, various elements and compounds may be further added to the coating solution to improve various properties.

[0127] The baking conditions are not particularly limited. For example, the baking conditions include an atmosphere of hydrogen, water vapor, and nitrogen, and the oxidation degree (P H2O / P H2 ): The conditions are to hold the material in an atmosphere of 0.0001 to 1.0 at a temperature range of 300 to 1150°C for 5 to 300 seconds.

[0128] In the insulating film forming process, the above coating solution is applied to the surface of the intermediate layer, and the oxidation degree of the atmosphere (P H2O / P H2 It is preferable to bake the material in an atmosphere with an oxidation degree of 0.001 to 0.1 at a temperature range of 300°C to 900°C for 10 seconds or more. If the oxidation degree of the atmosphere is 0.001 or more, the phosphate, which is the main constituent phase of the insulating film, is less likely to decompose, and water resistance is further improved. Also, if the oxidation degree of the atmosphere is 0.1 or less, iron loss can be further reduced.

[0129] In the insulating film forming process, it is preferable to cool the steel sheet in an atmosphere in which the oxidation degree of the above gas is kept low so that the insulating film and the intermediate layer are not changed after baking. The cooling conditions may be general conditions, but for example, an atmosphere consisting of hydrogen, nitrogen, water vapor and impurities and having an oxidation degree (P H2O / PH2 ): It is sufficient to make the atmosphere less than 0.01.

[0130] The method for producing a grain-oriented electrical steel sheet according to the present embodiment may further include a step generally performed in the method for producing a grain-oriented electrical steel sheet. For example, the method for producing a grain-oriented electrical steel sheet according to the present embodiment may further include a nitriding step of performing a nitriding treatment to increase the N content in the base steel sheet after the decarburization annealing step and before the annealing separator application step. This is because the magnetic flux density can be stably improved even if the temperature gradient applied to the steel sheet at the boundary between the primary recrystallization region and the secondary recrystallization region is low. The nitriding treatment may be any general treatment. For example, a treatment of annealing in an atmosphere containing a nitriding gas such as ammonia, a treatment of finish annealing a decarburization annealed steel sheet coated with an annealing separator containing a nitriding powder such as MnN, etc. may be mentioned.

[0131] The present invention is not limited to the above-described embodiment. The above-described embodiment is merely an example, and any embodiment that has substantially the same configuration as the technical idea described in the claims of the present invention and exhibits similar effects is included in the technical scope of the present invention. EXAMPLES

[0132] The present invention will be specifically described below by presenting examples. In the following, the conditions in the examples are one example of conditions adopted to confirm the feasibility and effects of the present invention. The present invention is not limited to this one example of conditions. Various conditions can be adopted in the present invention as long as they do not deviate from the gist of the present invention and achieve the object of the present invention.

[0133] A slab having a chemical composition containing 3.30% Si, 0.050% C, 0.030% acid-soluble Al, 0.0080% N, 0.10% Mn, 0.005% S and Se in total, with the remainder being Fe and impurities, was prepared. The slab was soaked at 1150°C for 60 minutes, and the heated slab was hot-rolled to produce a hot-rolled steel sheet having a thickness of 2.6 mm. The produced hot-rolled steel sheet was annealed to produce an annealed steel sheet. The hot-rolled steel sheet was annealed at an annealing temperature of 900°C for 120 seconds. The obtained annealed steel sheet was cold-rolled to produce a cold-rolled steel sheet having a final thickness of 0.23 mm.

[0134] The obtained cold-rolled steel sheet was subjected to decarburization annealing under the conditions of holding at 850° C. for 90 seconds in a wet atmosphere containing 75 volume % hydrogen and the remainder nitrogen and impurities.

[0135] The surface of the obtained steel sheet was coated with an annealing separator containing MgO in the ratio shown in Table 1. In the annealing separator, the remainder other than MgO was Al2O3.

[0136] The annealing separator was applied to the dried steel sheet, which was then subjected to finish annealing and cooled to obtain a base steel sheet. The finish annealing conditions were heating to 1200°C at a heating rate of 15°C / hour in a hydrogen-nitrogen mixed atmosphere, and then holding at 1200°C in a hydrogen atmosphere for 20 hours. The heater was turned off for the base steel sheet after the finish annealing in the batch annealing, and the sheet was cooled as is. The degree of oxidation (P H2O / P H2 ) are as shown in Table 1. In addition, the chemical composition of the base steel sheets after final annealing was as follows: Si: 3.30%, C: 0.002% or less, acid-soluble Al: 0.0030% or less, N: 0.0020% or less, Mn: 0.10%, S and Se: 0.0005% or less in total, with the remainder being Fe and impurities.

[0137] [Table 1]

[0138] For Test Nos. 1 to 12, the base steel sheets after the finish annealing were subjected to a heat treatment for simultaneously forming an intermediate layer and an insulating coating. The conditions for the intermediate layer and insulating film forming process were as follows. A coating solution was applied to the steel sheet surface. The composition of the coating solution for test numbers 1 to 10 was, by mass, 50% phosphate, 45% colloidal silica, and 5% chromic anhydride. The composition of the coating solution for test numbers 11 to 12 was, by mass, 55% phosphate, and 45% colloidal silica. The steel sheet to which the coating solution was applied was subjected to a test for measuring the oxidation degree (P H2O / P H2 ):0.1 atmosphere, heated to 850°C and held there for 30 seconds.

[0139] For test numbers 13 to 17, the intermediate layer forming step and the insulating film forming step were carried out separately. The base steel sheet after the final annealing was subjected to a heat treatment to form an intermediate layer. The conditions for the intermediate layer forming step were as follows. Degree of oxidation (P H2O / P H2 ):0.01 atmosphere, heated to 850°C and held for 30 seconds. An insulating film was then formed on the base steel sheet on which the intermediate layer had been formed. In the insulating film formation process, a coating solution was applied to the surface of the intermediate layer. The coating solution had a composition of 60% phosphate and 40% colloidal silica. The steel sheet on which the coating solution had been applied was heated to 850°C in an atmosphere of 75% by volume of hydrogen, the remainder being nitrogen and impurities, and held at this temperature for 30 seconds to form an insulating film, and then cooled to room temperature.

[0140] [Cross-section observation] Test pieces having a cross section perpendicular to the rolling direction were taken from each grain-oriented electrical steel sheet of test number, and the cross section was observed using a scanning electron microscope (SEM). The magnification was 10,000 times, and the observation was performed over a range of 100 μm in a direction parallel to the steel sheet surface in a region 10 μm deep from the steel sheet surface. In test numbers 1 to 8, test numbers 11 to 15, and test number 17, almost no internal oxide was formed. In other words, the number density of oxides with a circle equivalent diameter of 0.1 μm or more in a region 10 μm deep from the surface of the base steel sheet toward the inside of the base steel sheet was 0.020 pieces / μm. 2 The results were as follows. On the other hand, in test numbers 9 and 16, a large amount of internal oxides, mainly silicon oxides, which form irregularities on the surface of the base steel sheet were formed. In other words, the number density of oxides with a circle equivalent diameter of 0.1 μm or more in the region 10 μm deep from the surface of the base steel sheet toward the inside of the base steel sheet was 0.020 pieces / μm. 2 In test number 10, a large amount of internal oxides having a circle equivalent diameter of 0.1 μm or more, mainly composed of forsterite that forms irregularities on the surface of the base steel sheet, were formed.

[0141] For the grain-oriented electrical steel sheets of each test number, cross-sectional observation using a TEM (transmission electron microscope) confirmed that the composition of the intermediate layer was as follows, using electron beam diffraction patterns and EDX (energy dispersive X-ray analysis): Fe content less than 30 atomic %, P content less than 5 atomic %, Si content less than 50 atomic % and 20 atomic % or more, O content less than 80 atomic % and 50 atomic % or more, and Mg content less than 10 atomic %.

[0142] [Adhesion test] The adhesion test was carried out in accordance with the bending resistance test of JIS K 5600-5-1 (1999). Test pieces of 80 mm in the rolling direction and 40 mm in the direction perpendicular to the rolling direction were taken from the grain-oriented electrical steel sheets of test numbers 1 to 17. The taken test pieces were wrapped around a mandrel with a diameter of 10 mm or 16 mm. For the adhesion test, a 180° bending was performed using a type 1 test device described in the bending resistance test of JIS K 5600-5-1 (1999). The total area of ​​the area where the insulating film had peeled off was measured for the inner surface of the bent test piece after bending (insulating film peeling area). Thereafter, the area ratio of the remaining intermediate layer region was determined by the method described above. The results are shown in Table 1. Note that the bending diameter in Table 1 indicates the diameter of the mandrel. When the diameter of the mandrel is 10 mm, the area of ​​the insulation film peeled off is 7.5 mm 2 When the diameter of the mandrel around which the insulation film was wrapped was 16 mm, the peeled area of ​​the insulation film was 5.0 mm or less. 2 If the thickness was less than or equal to the thickness, it was determined that the adhesion was excellent.

[0143] The evaluation area of ​​the insulating coating peeled off in the bending test was defined by the following formula. If the area of ​​the insulating coating peeled off was less than 5% of the evaluation area, the bending diameter (diameter of the mandrel) was reduced and the test was reevaluated. If the reevaluation showed that the area of ​​the insulating coating peeled off was 5% or more of the evaluation area, the area ratio of the remaining intermediate layer was calculated. (Evaluation area) = (Bending diameter) × (Pi) ÷ 2

[0144] The area ratio of the remaining intermediate layer region was determined by mapping the identified insulating coating peeled region using an energy dispersive X-ray spectrometer (SEM-EDS) to obtain the Si concentration distribution, and in the obtained Si concentration distribution, the maximum and minimum Si concentrations were identified. The region that satisfied the following formula was defined as the remaining intermediate layer region. (Si concentration in the region)>{(maximum Si concentration)+(minimum Si concentration)} / 2 The ratio of the total area of ​​the defined remaining intermediate layer region to the total area of ​​the EDS mapping of the peeled-off film portion was defined as the area ratio (%) of the remaining intermediate layer region. When the area ratio of the remaining intermediate layer region was 20% or more, it was judged as passing, since it met the requirements stipulated in the present invention. On the other hand, when the area ratio of the remaining intermediate layer region was less than 20%, it was judged as failing, since it did not meet the requirements stipulated in the present invention. However, when the maximum value and the minimum value of the Si concentration satisfy the following formula, the area ratio of the remaining intermediate layer region is set to 0%. (Maximum Si concentration) - (Minimum Si concentration) < 5 atomic %

[0145] [Water resistance test] A bending test was carried out on the test pieces of test numbers 1 to 17 under the same conditions as the adhesion test. The bent portion (bending area) of the test piece was immersed in pure water for one minute while it was still bent. After one minute had passed, the test piece was pulled out. The test piece was then dried. The test piece was unbent, and the area of ​​the insulating film peeled off after immersion in water was calculated by image analysis. The area of ​​peeled off due to water was calculated by the following formula. The results are shown in Table 1. (Area peeled off by water) = (Area peeled off of insulation film after immersion in water) - (Area peeled off of insulation film) The peeling area caused by water is 5.0 mm 2 If the peeling area due to water was 5.0 mm or less, it was judged to be excellent in water resistance. 2 If it was over 100%, it was judged to have poor water resistance.

[0146] [Iron loss measurement] Based on JIS C 2550-1, the iron loss W17 / 50 (W / kg) was measured using the Epstein test at an excitation magnetic flux density of 1.7T and a frequency of 50Hz. When the iron loss W17 / 50 was less than 1.00, it was judged that the iron loss was good. On the other hand, when the iron loss W17 / 50 was 1.00 or more, it was judged that the iron loss was poor.

[0147] Referring to Table 1, Test No. 2, Test No. 4, Test No. 7, Test No. 8, Test No. 12, Test No. 14 and Test No. 15 had small areas of peeled insulating coating, and the area ratio of the remaining intermediate layer area was 20% or more, indicating excellent adhesion and water resistance. In particular, Test No. 2, Test No. 4, Test No. 7, Test No. 8, Test No. 14 and Test No. 15 had areas of peeled off by water that were smaller than the areas of peeled off insulating coating, indicating superior water resistance. Furthermore, in these inventive examples, the number density of internal oxides with a circle equivalent diameter of 0.1 μm or more was 0.020 pieces / μm 2 The iron loss was also good. Furthermore, in these inventive examples, the arithmetic mean roughness Ra of the surface of the base steel sheet was 1.0 μm or less, and the thickness of the intermediate layer was 2 to 400 nm. The arithmetic mean roughness Ra and the thickness of the intermediate layer were measured by the methods described above.

[0148] On the other hand, in the test numbers 1, 3, 5, 11, 13, and 17, the oxidation degree in the cooling process was less than 0.30. Therefore, the area ratio of the remaining intermediate layer region was less than 20%, and the adhesion was low. In the test numbers 1, 3, 5, 11, 13, and 17, the peeling area due to water was 5.0 mm 2 and the water resistance was poor.

[0149] In test numbers 9 and 16, the oxidation degree in the cooling process after the final annealing exceeded 100,000. As a result, an inner oxide mainly composed of silicon oxide was formed, and the number density of the inner oxide was 0.020 pieces / μm 2 As a result, the low core loss required for grain-oriented electrical steel sheets could not be achieved.

[0150] In test number 10, the MgO content in the annealing separator was high. As a result, inner oxides mainly composed of forsterite were formed, and the number density of inner oxides with a circle equivalent diameter of 0.1 μm or more was 0.020 pieces / μm 2 As a result, the low core loss required for grain-oriented electrical steel sheets could not be achieved. In Test No. 1, Test No. 3, Test No. 5, Test No. 9, Test No. 10, Test No. 11, Test No. 13, and Test No. 16, the peeled area of ​​the insulating film was also large.

[0151] The embodiments of the present invention have been described above. However, the above-described embodiments are merely examples for carrying out the present invention. Therefore, the present invention is not limited to the above-described embodiments, and the above-described embodiments can be appropriately modified and carried out without departing from the spirit of the present invention. [Industrial Applicability]

[0152] Effects of the Invention The present invention can provide a grain-oriented electrical steel sheet having an intermediate layer mainly made of silicon oxide, which has excellent adhesion to an insulating coating and water resistance, and a method for manufacturing an intermediate steel sheet for this grain-oriented electrical steel sheet.

Claims

1. A base steel plate; an intermediate layer formed on a surface of the base steel sheet and mainly composed of silicon oxide; an insulating coating formed on a surface of the intermediate layer, The number density of oxides in a region 10 μm deep from the surface of the base steel sheet toward the inside of the base steel sheet is 0.020 particles / μm 2 is as follows: after a bending test using a mandrel in accordance with JIS K 5600-5-1 (1999), in a region where the insulating coating has peeled off, the area ratio of an intermediate layer remaining region where the intermediate layer remains without peeling off is 20% or more, In an adhesion test conducted in accordance with the bending resistance test of JIS K 5600-5-1 (1999), when the diameter of the wound mandrel was 10 mm, the area of ​​the insulating film peeled off was 7.5 mm 2 When the diameter of the mandrel around which the insulation film is wound is 16 mm, the peeled area of ​​the insulation film is 5.0 mm or less. 2 A method for producing a grain-oriented electrical steel sheet, comprising: a hot rolling step of heating the slab at 1280°C or less and then hot rolling the slab to produce a hot-rolled steel sheet; A hot-rolled sheet annealing process for producing an annealed steel sheet by performing hot-rolled sheet annealing on the hot-rolled steel sheet; A cold rolling process in which cold rolling is performed on the annealed steel sheet to produce a cold-rolled steel sheet; a decarburization annealing step of producing a base steel sheet by performing decarburization annealing on the cold-rolled steel sheet; an annealing separator application step of applying an annealing separator having a composition containing 50% by mass or more of alumina and 0 to 50% by mass of magnesia as the balance to the base steel sheet; a finish annealing process in which finish annealing is performed on the base steel sheet after the annealing separator application process; The base steel sheet after the final annealing process is subjected to oxidation at a temperature range of 1100 to 500° C., where the oxidation degree P is the ratio of the water vapor partial pressure to the hydrogen partial pressure. H2O / P H2 A cooling step of cooling the mixture in an atmosphere having a molecular weight of 0.30 to 100,000; an intermediate layer forming step of heat treating the base steel sheet after the cooling step to form an intermediate layer mainly made of silicon oxide on the surface of the base steel sheet; and forming an insulating film on a surface of the intermediate layer after the intermediate layer forming step. Manufacturing method of grain-oriented electrical steel sheet.

2. A method for producing an intermediate steel sheet for the grain-oriented electrical steel sheet according to claim 1, comprising the steps of: a hot rolling step of heating the slab at 1280°C or less and then hot rolling the slab to produce a hot-rolled steel sheet; A hot-rolled sheet annealing process for producing an annealed steel sheet by performing hot-rolled sheet annealing on the hot-rolled steel sheet; A cold rolling process in which cold rolling is performed on the annealed steel sheet to produce a cold-rolled steel sheet; a decarburization annealing step of producing a base steel sheet by performing decarburization annealing on the cold-rolled steel sheet; an annealing separator application step of applying an annealing separator having a composition containing 50% by mass or more of alumina and 0 to 50% by mass of magnesia as the balance to the base steel sheet; a finish annealing step of performing finish annealing on the base steel sheet after the annealing separator application step; The base steel sheet after the final annealing process is subjected to oxidation at a temperature range of 1100 to 500° C., where the oxidation degree P is the ratio of the water vapor partial pressure to the hydrogen partial pressure. H2O / P H2 A cooling step of cooling the mixture in an atmosphere having a molecular weight of 0.30 to 100,000; Equipped with The intermediate steel sheet for the grain-oriented electrical steel sheet comprises a base steel sheet, A film-like oxide formed on the surface of the base steel sheet; Equipped with The film-like oxide is present so as to cover the surface of the base steel sheet in the form of a film, The number density of oxides in a region 10 μm deep from the surface of the base steel sheet toward the inside of the base steel sheet is 0.020 particles / μm 2 The method for producing an intermediate steel sheet for a grain-oriented electrical steel sheet is as follows.

Citation Information

Patent Citations

  • JP1974096920A

  • Production of grain-oriented silicon steel sheet having metallic luster and excellent in magnetic property

    JP1993263135A

  • Formation of insulating film on grain oriented electrical steel sheet

    JP1993279747A

  • Formation of insulated film on grain-oriented silicon steel sheet

    JP1994184762A

  • Method for forming insulating film on grain-oriented silicon steel sheet

    JP1995278833A