Non-oriented electrical steel sheet, iron core and motor core, and manufacturing method of iron core and motor core
The non-oriented electrical steel sheet with controlled chemical compositions and insulating coatings forms carbides with free carbon, addressing the issue of carbide precipitation and achieving low core loss.
Patent Information
- Application Number
- JP2023554591
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-10-13
- Filing Date
- 2022-10-12
- Publication Date
- 2024-10-03
- Estimated Expiration
- 2042-10-12
AI Technical Summary
Existing methods to improve magnetic properties in non-oriented electrical steel sheets by increasing Si content, reducing sulfides, and strain relief annealing result in lower than expected iron loss improvement due to carbide precipitation at grain boundaries.
A non-oriented electrical steel sheet with specific chemical compositions and insulating coatings containing elements like Mn, Ti, Zr, Hf, Ta, Nb, V, Mo, and Zn to form carbides with free carbon, preventing its intrusion into the steel sheet and reducing hysteresis loss.
Stabilizes the magnetic properties by suppressing carbide precipitation, resulting in a non-oriented electrical steel sheet with low core loss.
Smart Images

Figure 0007560795000003 
Figure 0007560795000001 
Figure 0007560795000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a non-oriented electrical steel sheet, an iron core, a motor core, and a method for manufacturing the iron core and the motor core. [Background technology]
[0002] In recent years, global environmental issues have been attracting attention, and the demand for energy conservation efforts is increasing. In particular, there is a strong demand for high efficiency in electrical equipment. For this reason, there is an increasing demand for improved magnetic properties in non-oriented electrical steel sheets, which are widely used as iron core materials for motors, generators, etc.
[0003] This trend is particularly evident in drive motors for electric vehicles and hybrid vehicles, and motors for air conditioner compressors. For this reason, there is a demand for further improvement in the magnetic properties, particularly reduction in iron loss, of non-oriented electrical steel sheets for the motor cores of these various motors.
[0004] Conventionally, in order to reduce iron loss, the Si content has been increased and sulfides have been reduced (see, for example, Patent Document 1, etc.). Increasing the Si content has the effect of increasing resistivity and reducing eddy current loss. Also, reducing sulfides can reduce precipitates that inhibit grain boundary movement, promoting grain coarsening and reducing hysteresis loss. In addition, attempts have been made to improve magnetic properties by stress relief annealing to remove punching strain. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2000-54085 A Summary of the Invention [Problem to be solved by the invention]
[0006] However, when the inventors simultaneously implemented three measures to improve the magnetic properties, namely, increasing the silicon content, reducing sulfides, and performing stress relief annealing, the improvement in iron loss was less than expected.
[0007] The present invention has been made to solve such problems, and has an object to stably obtain non-oriented electrical steel sheets with low core loss. [Means for solving the problem]
[0008] The present invention relates to the following non-oriented electrical steel sheet, iron core, motor core, and methods for manufacturing the iron core and motor core.
[0009] (1) A steel plate having a base material and an insulating coating formed on a surface of the base material, The chemical composition of the base steel sheet is, in mass%, C: 0.0030% or less, Si: 3.2-6.5%, Mn: 0.05-3.5%, P: 0.005-0.10%, S: 0.0030% or less, Al: 1.0% or less, Ti: 0.0030% or less, B: 0.0010% or less, Mo: 0.030% or less, V: 0.0010% or less, Ca: 0 to 0.0050%, Mg: 0 to 0.0050%, REM: 0~0.0050%, The balance is Fe and impurities. The following formula (i) is satisfied: The chemical composition of the insulating coating satisfies the following formula (ii): Non-oriented electrical steel sheet. S-5 / 3×Mg-4 / 5×Ca-1 / 4×REM<0.0005 ···(i) [M]-[C]+1 / 2×[O]>0 (ii) Here, the element symbols in the above formula (i) represent the content (mass%) of each element in the base steel plate, and [M] in the above formula (ii) represents the total atomic concentration (at%) of one or more elements selected from Mn, Ti, Zr, Hf, Ta, Nb, V, Mo, and Zn contained in the insulating coating, and [C] and [O] represent the atomic concentrations (at%) of C and O contained in the insulating coating, respectively.
[0010] (2) The chemical composition of the base steel sheet is, in mass%, replacing a part of Fe, Sn: 0.10% or less, Sb: 0.10% or less, Ni: 0.10% or less, Cr: 0.10% or less, and Cu: 0.10% or less, The non-oriented electrical steel sheet according to (1) above.
[0011] (3) The thickness of the base steel plate is less than 0.30 mm, and the thickness of the insulating coating is 1.0 μm or less. The non-oriented electrical steel sheet according to (1) or (2) above.
[0012] (4) Used for applications in which the material is punched into a specified shape, laminated, and then stress relief annealed at a temperature range of 750 to 900 ° C. The non-oriented electrical steel sheet according to any one of (1) to (3) above.
[0013] (5) Five of the non-oriented electrical steel sheets are stacked, and then annealed at 800°C for two hours in an atmosphere of 100% N2 with a dew point of -30°C. When the C concentration in the base steel sheet of one of the five stacked non-oriented electrical steel sheets at the center in the stacking direction is measured, the increase in C concentration from the C concentration in the base steel sheet of the non-oriented electrical steel sheet before annealing is 1 ppm or less. The non-oriented electrical steel sheet according to any one of (1) to (4) above.
[0014] (6) Five of the non-oriented electrical steel sheets are stacked, and then annealed at 800°C for two hours in an atmosphere of 100% N2 and a dew point of -30°C. The iron loss W is measured using one of the five stacked non-oriented electrical steel sheets at the center in the stacking direction. 10 / 400 is less than 11.5W / kg, The non-oriented electrical steel sheet according to any one of (1) to (5) above.
[0015] (7) Five of the non-oriented electrical steel sheets are stacked together, and then annealed at 800°C for two hours in an atmosphere of 100% N2 and a dew point of -30°C. After that, the amount of carbides contained in the insulating coating of one non-oriented electrical steel sheet at the center in the stacking direction among the five stacked non-oriented electrical steel sheets is 10 mg / m2 or more in terms of carbon content. 2 That's all. The non-oriented electrical steel sheet according to any one of (1) to (6) above.
[0016] (8) The non-oriented electrical steel sheet according to any one of (1) to (7) above is included. Iron core.
[0017] (9) A method of manufacturing a laminated non-oriented electrical steel sheet according to any one of (1) to (7) above, Manufacturing method of iron core.
[0018] (10) A motor core including a rotor core and a stator core, in which a plurality of non-oriented electromagnetic steel sheets are laminated, The non-oriented electrical steel sheet comprises a base steel sheet and an insulating coating formed on a surface of the base steel sheet, The chemical composition of the base steel sheet is, in mass%, C: 0.0030% or less, Si: 3.2-6.5%, Mn: 0.05-3.5%, P: 0.005-0.10%, S: 0.0030% or less, Al: 1.0% or less, Ti: 0.0030% or less, B: 0.0010% or less, Mo: 0.030% or less, V: 0.0010% or less, Ca: 0 to 0.0050%, Mg: 0 to 0.0050%, REM: 0~0.0050%, The balance is Fe and impurities. The following formula (i) is satisfied: a chemical composition of the insulating coating in the non-oriented electrical steel sheet constituting the rotor core satisfies the following formula (ii), The amount of carbides contained in the insulating coating of the non-oriented electrical steel sheet constituting the stator core is 10 mg / m, calculated as the carbon content. 2 That's all. Motor core. S-5 / 3×Mg-4 / 5×Ca-1 / 4×REM<0.0005 ···(i) [M]-[C]+1 / 2×[O]>0 (ii) Here, the element symbols in the above formula (i) represent the content (mass%) of each element in the base steel plate, and [M] in the above formula (ii) represents the total atomic concentration (at%) of one or more elements selected from Mn, Ti, Zr, Hf, Ta, Nb, V, Mo, and Zn contained in the insulating coating, and [C] and [O] represent the atomic concentrations (at%) of C and O contained in the insulating coating, respectively.
[0019] (11) The non-oriented electrical steel sheet according to any one of (1) to (7) above is punched into a predetermined shape, laminated, and then subjected to stress relief annealing in a temperature range of 750 to 900 ° C. A manufacturing method for a motor core. Effect of the Invention
[0020] According to the present invention, it is possible to stably obtain non-oriented electrical steel sheets with low core loss. [Brief description of the drawings]
[0021] [Figure 1]FIG. 1 is a diagram showing the relationship between the amount of increase in C concentration and iron loss (hysteresis loss). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] As a result of investigations conducted by the present inventors to solve the above problems, the present inventors have come to the following findings.
[0023] First, an investigation was conducted into the reason why iron loss did not improve as much as expected when the three magnetic property improvement measures of increasing silicon content, reducing sulfides, and performing stress relief annealing were implemented simultaneously.
[0024] As a result, it was found that when multiple non-oriented electrical steel sheets are laminated and then stress relief annealed at high temperatures, the organic resin in the insulating coating is thermally decomposed, and while some of it is released as gas, the remaining carbon remains free. It was also discovered that this remaining carbon penetrates the steel sheet and reacts with Si, Mn, Cr, etc. in the steel, and precipitates as carbides such as SiC, MnC, and CrC (chemical bond ratios are omitted as there are many types) at the grain boundaries. This type of reaction is more likely to occur when multiple electrical steel sheets are heated in a laminated state. These carbides hinder domain wall motion, increasing hysteresis loss and causing deterioration of iron loss.
[0025] The precipitation of carbides such as SiC does not occur when the Si content in the steel is low. In addition, when the amount of so-called free S that remains without being consumed as precipitates is large, the penetration of carbon in the insulating coating into the steel sheet is suppressed. Furthermore, when the stress relief annealing temperature is low, the decomposition of the organic resin and the penetration of carbon into the steel sheet are also suppressed. In other words, when the three conditions of high Si content, reduced sulfides, and high-temperature stress relief annealing are met, the deterioration of iron loss due to carbide precipitation becomes apparent.
[0026] Therefore, the inventors of the present invention conducted further investigations into methods for suppressing the deterioration of iron loss due to the precipitation of carbides and discovered that by adding one or more elements selected from Mn, Ti, Zr, Hf, Ta, Nb, V, Mo, and Zn to the insulating coating, free or remaining carbon in the insulating coating reacts with these elements to form carbides, which are rendered harmless.
[0027] The present invention has been made based on the above findings. Each of the features of the present invention will be described in detail below.
[0028] 1. Overall structure The non-oriented electrical steel sheet according to one embodiment of the present invention includes a base steel sheet and an insulating coating formed on the surface of the base steel sheet. The chemical compositions of the base steel sheet and the insulating coating will be described below.
[0029] 2. Chemical composition of base steel plate The reasons for limiting the content of each element are as follows. In the following description, "%" for the content means "mass %."
[0030] C: 0.0030% or less C contributes to increasing the strength of steel sheets, but is an element that causes iron loss degradation. If the C content exceeds 0.0030%, iron loss degradation occurs in the non-oriented electrical steel sheet, and good magnetic properties cannot be obtained. Therefore, the C content is set to 0.0030% or less. The C content is preferably set to 0.0027% or less, and more preferably set to 0.0025% or less. Note that an excessive reduction in the C content leads to an increase in manufacturing costs, so it is preferably set to 0.0001% or more, and more preferably set to 0.0005% or more.
[0031] Silicon: 3.2 to 6.5% Silicon is an element that increases the electrical resistance of steel and improves iron loss. In addition, silicon has a large solid solution strengthening ability, so it is also an effective element for increasing the strength of steel sheets. On the other hand, if the silicon content is excessive, the workability may be significantly deteriorated, and it may become difficult to perform cold rolling. Therefore, the silicon content is set to 3.2 to 6.5%. The silicon content is preferably 3.3% or more, and is preferably 6.0% or less, 5.5% or less, 5.0% or less, or 4.5% or less.
[0032] Mn: 0.05 to 3.5% Mn is an element that increases the electrical resistance of steel and improves iron loss. If the Mn content is too low, the effect of increasing electrical resistance is small, and fine sulfides (MnS) are precipitated, which may deteriorate grain growth during final annealing. On the other hand, if the Mn content is excessive, the magnetic flux density may decrease. Therefore, the Mn content is set to 0.05 to 3.5%. The Mn content is preferably 0.10% or more, or 0.20% or more, and is preferably 3.0% or less, less than 3.0%, 2.8% or less, or 2.5% or less.
[0033] P: 0.005-0.10% P is contained in steel as an impurity, and if its content is excessive, the ductility of the steel sheet may be significantly reduced. On the other hand, P is an element with high solid solution strengthening ability, so it is an effective element for increasing the strength of the steel sheet. In addition, P also has the effect of suppressing the formation of carbides after stress relief annealing by competing with C to segregate at grain boundaries. Therefore, the P content is set to 0.005 to 0.10%. The P content is preferably 0.050% or less.
[0034] S: 0.0030% or less S is an element that increases iron loss by forming fine precipitates of MnS, thereby degrading the magnetic properties of steel sheets. Therefore, the S content is set to 0.0030% or less. The S content is preferably set to 0.0015% or less. There is no need to set a lower limit for the S content, but excessive reduction of S leads to a significant increase in steelmaking costs. Therefore, the S content is preferably set to 0.0005% or more.
[0035] Al: 1.0% or less Al is an element that increases the electrical resistance of steel and improves iron loss. However, if the Al content is excessive, the magnetic flux density may decrease. Therefore, the Al content is set to 1.0% or less. The Al content is preferably 0.80% or less. To obtain the above effects, the Al content is preferably 0.0005% or more, and more preferably more than 0.0010%, more than 0.010%, or 0.10% or more. In this specification, the Al content means the content of sol.Al (acid-soluble Al).
[0036] Ti: 0.0030% or less B: 0.0010% or less Mo: 0.030% or less V:0.0010% or less Ti, B, Mo, and V are elements that are inevitably mixed in, and can combine with carbon or nitrogen to form precipitates (carbides, nitrides). When carbides or nitrides are formed, these precipitates themselves may deteriorate the magnetic properties. Furthermore, they may inhibit the growth of crystal grains during finish annealing, deteriorating the magnetic properties. Therefore, the Ti content is set to 0.0030% or less, the B content to 0.0010% or less, the Mo content to 0.030% or less, and the V content to 0.0010% or less.
[0037] The Ti content is preferably 0.0020% or less, the B content is preferably 0.0008% or less, the Mo content is preferably 0.020% or less, and the V content is preferably 0.0008% or less. There is no need to set a lower limit for the contents of these elements, and they may be 0%, but extreme reduction may lead to an increase in manufacturing costs. Therefore, the Ti content is preferably 0.0005% or more, the B content is preferably 0.0001% or more, the Mo content is preferably 0.005% or more, and the V content is preferably 0.0001% or more.
[0038] Ca: 0 to 0.0050% Magnesium: 0 to 0.0050% REM: 0 to 0.0050% Since Ca, Mg and REM are elements that form sulfides to fix S and contribute to reducing iron loss, one or more selected from these are contained so as to satisfy the following formula (i). However, since excessive inclusion may result in poor economic efficiency, the Ca: 0.0050% or less, Mg: 0.0050% or less, and REM: 0.0050% or less are set. S-5 / 3×Mg-4 / 5×Ca-1 / 4×REM<0.0005 ···(i) In the above formula (i), the element symbols represent the content (mass %) of each element in the base steel sheet.
[0039] Sn: 0.10% or less Sb: 0.10% or less Ni: 0.10% or less Cr:0.10% or less Cu:0.10% or less Sn, Sb, Ni, Cr, and Cu are elements that are inevitably mixed in. However, since these elements also improve the magnetic properties, they may be intentionally included.
[0040] However, since excessive inclusion may lead to poor economic efficiency, when intentionally included, the content of each element is set to 0.10% or less, and preferably 0.05% or less. When it is desired to obtain an effect of improving magnetic properties, it is preferable to include one or more selected from Sn: 0.01% or more, Sb: 0.01% or more, Ni: 0.01% or more, Cr: 0.01% or more, and Cu: 0.01% or more.
[0041] In the chemical composition of the base steel sheet of the present invention, the balance is Fe and impurities. Here, the term "impurities" refers to components that are mixed in due to various factors in raw materials such as ores and scraps and manufacturing processes during industrial production of steel, and are permissible within a range that does not adversely affect the present invention.
[0042] 3. Chemical composition of the insulating coating In the non-oriented electrical steel sheet of the present invention, the type of insulating coating is not particularly limited, but it is preferably a composite coating of an inorganic compound such as a phosphate-based, silica-based, or Zr-based compound and an organic resin. Conventionally, chromate-based insulating coatings using dichromate as the main raw material have been mainly used, but since hexavalent chromium is highly toxic, it is preferable that the insulating coating does not contain chromium from the viewpoint of protecting the working environment during production.
[0043] Furthermore, there is no limitation on the type of organic resin, and for example, one or more types selected from acrylic resin, styrene resin, acrylic-styrene resin, epoxy resin, polyester resin, phenol resin, and urethane resin can be used.
[0044] As described above, in order to fix the free or remaining carbon in the insulating coating as carbide and render it harmless, the present invention includes in the insulating coating one or more elements selected from Mn, Ti, Zr, Hf, Ta, Nb, V, Mo, and Zn. More specifically, the chemical composition of the insulating coating needs to satisfy the following formula (ii): [M]-[C]+1 / 2×[O]>0 (ii) In the above formula (ii), [M] means the total atomic concentration (at%) of one or more elements selected from Mn, Ti, Zr, Hf, Ta, Nb, V, Mo, and Zn, and [C] and [O] mean the atomic concentrations (at%) of C and O contained in the insulating coating, respectively.
[0045] Among the above elements, Zn has a relatively low carbide-forming ability. Mn also has a higher carbide-forming ability than Zn, but its carbide-forming ability is lower than other elements. Therefore, the insulating coating preferably contains one or more elements selected from Mn, Ti, Zr, Hf, Ta, Nb, V, and Mo, excluding Zn, in a range that satisfies the above formula (ii), and more preferably contains one or more elements selected from Ti, Zr, Hf, Ta, Nb, V, and Mo, excluding Zn and Mn, in a range that satisfies the above formula (ii).
[0046] In the present invention, [M], [C] and [O] in the insulating coating are measured by the following procedure. First, a case where the insulating coating contains an inorganic compound such as a phosphoric acid or silica compound and can be dissolved by alkali treatment will be described. First, the weight measurement and chemical composition analysis are performed on the entire non-oriented electrical steel sheet including the insulating coating. In this embodiment, the chemical composition is analyzed by ICP-MS for [M]. [C] is analyzed by burning the sample and measuring infrared absorbance in accordance with JIS G 1211-3:2018 (hereinafter, also referred to as "combustion-infrared absorption method"). [O] is quantified by melting the sample in a graphite crucible in a He atmosphere and analyzing the carbon dioxide gas generated by the melting with an infrared detector. Next, the weight measurement and chemical composition analysis are performed on the base material from which the insulating coating has been removed by alkali treatment in the same manner. Then, [M], [C] and [O] in the insulating coating are calculated from the difference before and after the removal of the insulating coating.
[0047] Next, we will explain the case where the insulating coating contains inorganic compounds such as Zr and cannot be dissolved by alkaline treatment. First, only the surface layer is peeled off by mechanical polishing so that the entire insulating coating is included. In this case, alumina is used as the polishing agent. After that, only the base material adhering to the insulating coating is completely removed using hydrochloric acid. Then, the separated insulating coating is subjected to chemical composition analysis using the above-mentioned method to determine [M], [C], and [O] in the insulating coating.
[0048] 4.Thickness In the non-oriented electrical steel sheet of this embodiment, there is no need to impose any particular restrictions on the thickness of the base steel sheet or the thickness of the insulating coating. However, if the thickness of the base steel sheet is 0.30 mm or more, or the thickness of the insulating coating exceeds 1.0 μm, carbon produced by the thermal decomposition of the organic resin is likely to be released as carbon dioxide gas from between the laminated steel sheets, making it difficult for free or remaining carbon to occur.
[0049] That is, the effects of the present invention are more pronounced when the base steel sheet and the insulating coating are thin, so the thickness of the base steel sheet is preferably less than 0.30 mm, and the thickness of the insulating coating is preferably 1.0 μm or less.
[0050] 5. Iron cores and motor cores An iron core according to one embodiment of the present invention includes the non-oriented electromagnetic steel sheet described above. The iron core is obtained by stacking a plurality of non-oriented electromagnetic steel sheets. It is sufficient that some or all of the plurality of stacked non-oriented electromagnetic steel sheets are the non-oriented electromagnetic steel sheets described above.
[0051] Moreover, a motor core according to an embodiment of the present invention includes a rotor core and a stator core. Here, strength is required for the rotor core. For that reason, the rotor core is obtained by punching the above-mentioned non-oriented electrical steel sheet into a predetermined shape and laminating a plurality of sheets. That is, the rotor core in this embodiment is not subjected to stress relief annealing. Therefore, the chemical composition of the insulating coating in the non-oriented electrical steel sheet constituting the rotor core satisfies the above-mentioned formula (ii).
[0052] On the other hand, the stator core is required to have better magnetic properties. Therefore, the stator core is obtained by punching the above-mentioned non-oriented electrical steel sheet into a predetermined shape, stacking a plurality of sheets, and then performing stress relief annealing. As described above, when a plurality of non-oriented electrical steel sheets are stacked and then subjected to stress relief annealing, the organic resin in the insulating coating is thermally decomposed, and some carbon is liberated and remains. In the present invention, the insulating coating contains one or more elements selected from Mn, Ti, Zr, Hf, Ta, Nb, V, Mo, and Zn, so that the liberated and remaining carbon in the insulating coating is fixed as carbide.
[0053] Therefore, in the motor core of this embodiment, the insulating coating after stress relief annealing, i.e., the insulating coating of the non-oriented electrical steel sheet that constitutes the stator core, has a carbon content of 10 mg / m 2 In other words, the amount of carbide in the insulation coating is 10 mg / m2 or more in terms of carbon content. 2This means that the carbon liberated by the thermal decomposition of the organic resin in the insulating coating was prevented from forming carbides with one or more elements selected from Mn, Ti, Zr, Hf, Ta, Nb, V, Mo, and Zn as constituent elements of the insulating coating, and from penetrating into the base steel sheet. The amount of carbides in the insulating coating was 13 mg / m 2 Above 15mg / m 2 The above carbide may be a carbide containing one or more elements selected from the group consisting of Mn, Ti, Zr, Hf, Ta, Nb, V, Mo, and Zn.
[0054] The amount of carbide in terms of the carbon content in the insulating coating means the amount of carbon in the carbide contained in the insulating coating formed on the surface of the base steel sheet per unit area. In this embodiment, the amount of carbide in the insulating coating is measured by the following procedure. First, a case will be described in which the insulating coating contains an inorganic compound such as a phosphoric acid or silica compound and can be dissolved by an alkaline treatment. First, only the insulating coating is dissolved by the alkaline treatment. At this time, the carbide does not dissolve and remains in the alkaline solution as a residue. Therefore, the residue is filtered and dried, and the carbon amount is measured by a combustion-infrared absorption method. Then, the weight is divided by the surface area of the dissolved base steel sheet on which the insulating coating was formed to obtain the amount of carbide in terms of the carbon content in the insulating coating.
[0055] Next, a case where the insulating coating contains inorganic compounds such as Zr and cannot be dissolved by alkali treatment will be described. First, only the surface layer is peeled off by mechanical polishing so that the entire insulating coating is included. In this case, alumina is used as the abrasive. Then, the base material attached to the insulating coating is completely removed using hydrochloric acid. The residue after removing the base material is filtered and dried, and the carbon amount is measured by the combustion-infrared absorption method. The amount of carbon is then divided by the surface area of the dissolved base steel sheet on which the insulating coating was formed to determine the amount of carbon in the insulating coating. Note that since it is considered that no carbon remains as a resin in the insulating coating after stress relief annealing, the measured carbon amount is all due to carbides.
[0056] 6. Relationship between carbon concentration increase and iron loss As described above, when the organic resin in the insulating coating is thermally decomposed by high-temperature stress relief annealing, and the free and remaining carbon penetrates the base steel sheet and precipitates as SiC, MnC, CrC, etc., this leads to deterioration in iron loss. In other words, the greater the increase in C concentration in the base steel sheet after stress relief annealing, the greater the deterioration in iron loss. Therefore, in the present invention, the increase in C concentration is used as an index of the degree of improvement in iron loss.
[0057] The C concentration increase can be determined, for example, by the following method. First, five 100 mm x 100 mm non-oriented electrical steel sheets are stacked, and then annealed in an atmosphere of 100% N2 (dew point less than 30°C) at 800°C for two hours. Then, one of the five stacked non-oriented electrical steel sheets is taken out from the center in the stacking direction, and the C concentration in the base steel sheet is measured. The increase from the C concentration in the base steel sheet before annealing is taken as the C concentration increase.
[0058] Here, to measure the carbon concentration in the base steel sheet, the insulating coating is removed by mechanical polishing on both sides of the non-oriented electrical steel sheet. In order to completely remove the insulating coating, the insulating coating is removed, and once the base material is visible, another 10 μm is removed in the thickness direction. After that, the carbon concentration of the remaining base steel sheet is measured using the combustion-infrared absorption method.
[0059] The relationship between the increase in C concentration in the base steel sheet after stress relief annealing and the iron loss has been confirmed by preliminary experiments conducted by the present inventors, the results of which are shown below.
[0060] The chemical composition of the insulating coating was adjusted to prepare non-oriented electrical steel sheets having various values of [M]-[C]+1 / 2×[O] in the non-oriented electrical steel sheet of Test No. 1 shown in Table 1 described later. The increase in C concentration of the obtained non-oriented electrical steel sheets was measured by the method described above.
[0061] Furthermore, the Epstein test specified in JIS C 2550-1:2011 was carried out on the same non-oriented electrical steel sheet, i.e., one non-oriented electrical steel sheet in the center of the lamination direction taken out after lamination and annealing. The iron loss obtained by DC measurement between ±1.0 T was compared with the hysteresis loss at 1 Hz, Wh 10 / 1 The hysteresis loss at 400Hz is Wh 10 / 400 was calculated as 400 times that amount.
[0062] Fig. 1 is a diagram showing the relationship between the increase in C concentration and iron loss (hysteresis loss). As shown in Fig. 1, a good correlation is observed between the increase in C concentration and iron loss, and the lower the increase in C concentration, the better the iron loss. This shows that the increase in C concentration is useful as an index of the degree of improvement in iron loss.
[0063] 7. Manufacturing method of non-oriented electrical steel sheet There is no particular limitation on the method for manufacturing the non-oriented electrical steel sheet of this embodiment. For example, after heating a slab having the above-mentioned chemical composition, hot rolling is performed, and if necessary, hot-rolled sheet annealing is performed, pickling is performed, cold rolling is performed, and then finish annealing is performed to obtain a base steel sheet. Note that, if necessary, skin pass rolling may be performed after the finish annealing.
[0064] There are no particular limitations on the conditions for hot-rolled sheet annealing, cold rolling, and finish annealing, but hot-rolled sheet annealing is preferably performed in a temperature range of 900 to 1100° C. Regarding cold rolling, from the viewpoint of rolling properties, the sheet may be heated to 80 to 300° C. before rolling. Regarding finish annealing, it is preferable to perform it in a temperature range of 700 to 1050° C., and more preferably in a temperature range of 900° C. or less.
[0065] The reduction ratio in the skin pass rolling is preferably 1 to 10%. By setting the reduction ratio to 1% or more, the strain necessary for strain-induced grain growth can be sufficiently obtained. On the other hand, by setting the reduction ratio to 10% or less, the non-uniformity of the amount of strain for each crystal orientation can be maintained.
[0066] Next, an insulating coating is formed on the surface of the obtained base steel sheet. The process for forming the insulating coating is not particularly limited, and the insulating coating treatment liquid having the above-mentioned chemical composition may be applied and dried. However, from the viewpoint of suppressing the penetration of carbon into the base steel sheet, it is important to control the heating rate of the treatment liquid during drying and baking.
[0067] Specifically, the heating rate for drying and baking the treatment solution is preferably 40°C / s or more, and more preferably 50°C / s or more. If the heating rate is slow, the coating surface becomes flat, which inhibits the escape of carbon dioxide gas during stress relief annealing, and increases the amount of carbon penetrating into the steel. Conversely, if the heating rate is fast, fine irregularities are created, making it easier to avoid the adverse effects of carbon.
[0068] Furthermore, the baking temperature is preferably in the range of 270°C to 350°C. If the baking temperature is less than 270°C, the coating surface becomes flat, which inhibits the escape of carbon dioxide gas during stress relief annealing, increasing the amount of carbon penetrating into the steel, and conversely, if the baking temperature is high, fine irregularities are formed, making it easier to avoid the adverse effects of carbon. On the other hand, if the baking temperature is too high, the resin in the coating starts to burn at this stage, and punchability deteriorates. It is more preferable that the baking temperature be 300°C to 350°C.
[0069] In addition, the surface of the base steel sheet on which the insulating coating is formed may be subjected to any pretreatment, such as a degreasing treatment with an alkali or the like, or an acid pickling treatment with hydrochloric acid, sulfuric acid, phosphoric acid or the like, before the treatment liquid is applied, or may be left as it is after finish annealing without being subjected to these pretreatments.
[0070] 8. Manufacturing method of iron core and motor core The manufacturing method of an iron core according to one embodiment of the present invention includes a step of stacking the non-oriented electromagnetic steel sheets. At this time, a plurality of non-oriented electromagnetic steel sheets are stacked. Some or all of the plurality of stacked non-oriented electromagnetic steel sheets may be the non-oriented electromagnetic steel sheets described above.
[0071] The non-oriented electrical steel sheets are punched into a predetermined shape, laminated, and then subjected to stress relief annealing to obtain a motor core. As described above, it is preferable not to perform stress relief annealing on the rotor core, so the motor core referred to here is preferably a stator core.
[0072] There are no particular limitations on the conditions for stress relief annealing, but from the viewpoint of improving magnetic properties, it is preferable to perform stress relief annealing at a high temperature, and specifically, the annealing temperature is preferably in the range of 750 to 900° C. There are also no limitations on the annealing time, and it is preferable to set it, for example, to 0.5 to 5.0 hours. Note that the annealing time is the time during which the motor core is at 750° C. or higher, and the heating time and cooling time at temperatures below 750° C. may be set appropriately.
[0073] As described above, when stress relief annealing is performed at high temperatures, deterioration of iron loss due to carbide precipitation tends to become evident, but in the present invention, this can be suppressed by optimizing the chemical composition of the insulating coating. In other words, the non-oriented electrical steel sheet according to this embodiment can be suitably used in applications in which stress relief annealing is performed at a temperature range of 750 to 900°C after punching into a predetermined shape and laminating.
[0074] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. EXAMPLES
[0075] A slab having a predetermined chemical composition was heated to 1150°C, and then hot-rolled at a finishing temperature of 800°C and a finishing thickness of 2.2 mm, and coiled at 700°C to obtain a hot-rolled steel sheet. The obtained hot-rolled steel sheet was subjected to hot-rolled sheet annealing at 950°C for 40 s, and the surface scale was removed by pickling. The above steel sheet was further cold-rolled to obtain a cold-rolled steel sheet having a thickness of 0.25 mm.
[0076] Thereafter, the steel sheets were subjected to finish annealing under the conditions of 900°C x 20 seconds to obtain base steel sheets. The chemical compositions of the obtained base steel sheets are shown in Table 1. The thickness of each base steel sheet was 0.25 mm.
[0077] [Table 1]
[0078] Next, an insulating coating solution consisting of the components shown in Table 2 was applied to the surface of the base steel sheet, and then the insulating coating was formed by baking in air at the temperature shown in Table 2, thereby producing a non-oriented electrical steel sheet. The chemical composition and thickness of the insulating coating are also shown in Table 2.
[0079] [Table 2]
[0080] The non-oriented electrical steel sheets were then punched out into a predetermined shape, and five sheets were stacked together, after which stress relief annealing was performed by holding the sheet at 800°C for two hours in an atmosphere of 100% N2 (dew point -30°C). One sheet in the center of the stacked five non-oriented electrical steel sheets was taken out, and the core loss W of the non-oriented electrical steel sheet was measured by the Epstein test specified in JIS C 2550-1:2011. 10 / 400 (W / kg) was measured. 10 / 400 means the total iron loss occurring under the conditions of a maximum magnetic flux density of 1.0 T and a frequency of 400 Hz. In this embodiment, the iron loss W 10 / 400 It was determined that the iron loss was low when the iron loss was less than 11.5 W / kg.
[0081] Next, the C concentration in the base steel sheet of one of the non-oriented electrical steel sheets at the center of the lamination direction was measured and compared with the C concentration in the base steel sheet before annealing to determine the increase in C concentration. The results are also shown in Table 2.
[0082] As shown in Table 2, in the test Nos. 1 to 3, 5 to 7, 9, 10, 12, 16 to 18, 20, 21, and 23 of the present invention examples which satisfy the formula (ii), the increase in the C concentration was 1 ppm or less, and the iron loss was also excellent. On the other hand, in the test Nos. 4, 8, 13 to 15, and 19 of the comparative examples, since the formula (ii) was not satisfied, the increase in the C concentration was large, and the iron loss was deteriorated. In addition, in the test No. 11, although the formula (ii) was not satisfied, the thickness of the insulating coating exceeded 1.0 μm, so the increase in the C concentration was not large. In the test No. 22, since the formula (i) was not satisfied, although the formula (ii) was satisfied and the increase in the C concentration was 1 ppm or less, the iron loss was deteriorated.
[0083] Furthermore, in test No. 24, the baking conditions were inappropriate, which resulted in a large increase in C concentration and a deterioration in iron loss. And in test No. 25, the baking conditions were inappropriate and formula (ii) was not satisfied, which resulted in a large increase in C concentration and a deterioration in iron loss. [Industrial Applicability]
[0084] As described above, according to the present invention, it is possible to stably obtain non-oriented electrical steel sheets with low core loss.
Claims
1. A base steel plate and an insulating coating formed on a surface of the base steel plate, The insulating coating is a composite coating of an inorganic compound and an organic resin, The chemical composition of the base steel sheet is, in mass%, C: 0.0030% or less, Si: 3.2 to 6.5%, Mn: 0.05-3.5%, P: 0.005-0.10%, S: 0.0030% or less, Al: 1.0% or less, Ti: 0.0030% or less, B: 0.0010% or less, Mo: 0.030% or less, V: 0.0010% or less, Ca: 0-0.0050%, Mg: 0 to 0.0050%, REM: 0 to 0.0050%, The balance is Fe and impurities. The following formula (i) is satisfied: The chemical composition of the insulating coating satisfies the following formula (ii): It is used in applications where the sheet is punched into a specified shape, laminated, and then stress relief annealed at a temperature range of 750 to 900°C. Non-oriented electrical steel sheet. S-5 / 3×Mg-4 / 5×Ca-1 / 4×REM<0.0005...(i) [M]-[C]+1 / 2×[O]>0...(ii) Here, the element symbols in the above formula (i) represent the content (mass %) of each element in the base steel sheet, the insulating coating contains one or more elements selected from Mn, Ti, Zr, Hf, Ta, Nb, V, and Mo, [M] in the above formula (ii) represents the total atomic concentration (at %) of Mn, Ti, Zr, Hf, Ta, Nb, V, and Mo, and [C] and [O] represent the atomic concentrations (at %) of C and O contained in the insulating coating, respectively.
2. The chemical composition of the base steel sheet is, in mass%, replacing a part of Fe, Sn: 0.10% or less, Sb: 0.10% or less, Ni: 0.10% or less, Cr: 0.10% or less, and Cu: 0.10% or less, The non-oriented electrical steel sheet according to claim 1.
3. The thickness of the base steel plate is less than 0.30 mm, and the thickness of the insulating coating is 1.0 μm or less. The non-oriented electrical steel sheet according to claim 1.
4. The thickness of the base steel plate is less than 0.30 mm, and the thickness of the insulating coating is 1.0 μm or less. The non-oriented electrical steel sheet according to claim 2.
5. Five of the non-oriented electrical steel sheets are stacked together, and then 2 : After annealing at 800°C for 2 hours in an atmosphere with a 100% carbon content and a dew point of -30°C, when the C concentration in the base steel sheet of one non-oriented electrical steel sheet at the center in the stacking direction among the five stacked non-oriented electrical steel sheets is measured, the C concentration increase from the C concentration in the base steel sheet of the non-oriented electrical steel sheet before annealing is 1 ppm or less, The non-oriented electrical steel sheet according to any one of claims 1 to 4.
6. Five of the non-oriented electrical steel sheets are stacked together, and then 2 : Iron loss W measured using one non-oriented electrical steel sheet at the center of the lamination direction among the five laminated non-oriented electrical steel sheets after annealing at 800 ° C. for 2 hours in an atmosphere with a 100% weight and a dew point of -30 ° C. 10/400 is less than 11.5 W / kg; The non-oriented electrical steel sheet according to any one of claims 1 to 4.
7. Five of the non-oriented electrical steel sheets are stacked together, and then 2 : After annealing at 800°C for 2 hours in an atmosphere with a 100% carbon content and a dew point of -30°C, the amount of carbides contained in the insulating coating of one non-oriented electrical steel sheet at the center in the lamination direction among the five laminated non-oriented electrical steel sheets is 10 mg / m2 or more in terms of carbon content. 2 That's all. The non-oriented electrical steel sheet according to any one of claims 1 to 4.
8. The non-oriented electrical steel sheet according to any one of claims 1 to 4, Iron core.
9. A process for laminating the non-oriented electrical steel sheets according to any one of claims 1 to 4, Manufacturing method of iron core.
10. A motor core including a rotor core and a stator core, in which a plurality of non-oriented electromagnetic steel sheets are laminated, The non-oriented electrical steel sheet comprises a base steel sheet and an insulating coating formed on a surface of the base steel sheet, The insulating coating is a composite coating of an inorganic compound and an organic resin, The chemical composition of the base steel sheet is, in mass%, C: 0.0030% or less, Si: 3.2 to 6.5%, Mn: 0.05-3.5%, P: 0.005-0.10%, S: 0.0030% or less, Al: 1.0% or less, Ti: 0.0030% or less, B: 0.0010% or less, Mo: 0.030% or less, V: 0.0010% or less, Ca: 0-0.0050%, Mg: 0 to 0.0050%, REM: 0 to 0.0050%, The balance is Fe and impurities. The following formula (i) is satisfied: A chemical composition of the insulating coating of the non-oriented electrical steel sheet constituting the rotor core satisfies the following formula (ii), and The five non-oriented electromagnetic steel sheets constituting the rotor core are laminated, and then N 2 : After annealing at 800°C for 2 hours in an atmosphere with a 100% carbon content and a dew point of -30°C, the amount of carbides contained in the insulating coating of one non-oriented electrical steel sheet at the center in the lamination direction among the five laminated non-oriented electrical steel sheets is 10 mg / m2 or more in terms of carbon content. 2 That's all. The amount of carbides contained in the insulating coating of the non-oriented electrical steel sheet constituting the stator core is 10 mg / m, calculated as the carbon content. 2 That's all. Motor core. S-5 / 3×Mg-4 / 5×Ca-1 / 4×REM<0.0005...(i) [M]-[C]+1 / 2×[O]>0...(ii) It means the atomic concentration (at %) of each element. Here, the element symbols in the above formula (i) represent the content (mass %) of each element in the base steel sheet, the insulating coating contains one or more elements selected from Mn, Ti, Zr, Hf, Ta, Nb, V, and Mo, [M] in the above formula (ii) represents the total atomic concentration (at %) of Mn, Ti, Zr, Hf, Ta, Nb, V, and Mo, and [C] and [O] represent the atomic concentrations (at %) of C and O contained in the insulating coating, respectively.
11. The non-oriented electrical steel sheet according to any one of claims 1 to 4 is punched into a predetermined shape, laminated, and then subjected to stress relief annealing in a temperature range of 750 to 900 ° C. A manufacturing method for a motor core.
Citation Information
Patent Citations
Nonoriented silicon steel sheet with low iron loss and excellent punchability
JP2000054085A
Nonoriented silicon steel sheet excellent in high frequency magnetic property and weldability
JP2001295001A
Non-oriented electrical steel sheet
JP2009068055A
Non-oriented electrical steel sheet and method for manufacturing the same
JP2021031714A
Electromagnetic steel sheet
WO2016125783A1
Cited By
Rotating electric machine and method for manufacturing the same
JP2026163835A