Thermal recording materials

The heat-sensitive recording material with a specific molar extinction coefficient ratio and non-photosensitive organic silver salt layer addresses the challenge of achieving high-contrast images using infrared laser light, enhancing fine detail reproduction.

JP7561048B2Active Publication Date: 2024-10-03MITSUBISHI PAPER MILLS LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2021009947
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-01-26
Publication Date
2024-10-03
Estimated Expiration
2041-01-26

AI Technical Summary

Technical Problem

Existing dry image forming methods using infrared laser light struggle to achieve high-contrast images due to insufficient or excessive irradiation, leading to issues with fine details like thin lines and minute dots.

Method used

A heat-sensitive recording material with a light-transmitting support, an infrared absorbing dye having a specific molar extinction coefficient ratio, and a non-photosensitive organic silver salt layer, free of silver halide, to enhance contrast through infrared laser irradiation.

Benefits of technology

The material achieves high-contrast images with improved fine detail reproduction by optimizing the molar extinction coefficient ratio and eliminating silver halide, resulting in efficient image formation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007561048000001
    Figure 0007561048000001
  • Figure 0007561048000002
    Figure 0007561048000002
  • Figure 0007561048000003
    Figure 0007561048000003
Patent Text Reader

Abstract

To provide a heat-sensitive recording material that can give a high-contrast image by irradiation with infrared laser light.SOLUTION: A heat-sensitive recording material has, on a light-transmitting support, at least an infrared absorption layer, a heat-sensitive recording layer, and a protective layer in the stated order. The infrared absorption layer contains an infrared absorption dye with a ratio ε(830) / ε(365) of 4.0 or more between a molar extinction coefficient ε(830) at 830 nm and a molar extinction coefficient ε(365) at 365 nm. The heat-sensitive recording layer contains non-photosensitive organic silver salts and is substantially free of photosensitive silver halides.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a heat-sensitive recording material on which an image is formed by irradiation with infrared laser light, and more particularly to a heat-sensitive recording material suitable for producing a copy manuscript. [Background technology]

[0002] As a high-quality image recording method for producing a copy-copy manuscript, a wet-processing image forming method using a silver halide photosensitive material has been generally used for a long time. However, the wet-processing image forming method requires waste liquid treatment such as a developer and a fixing solution, which places a large burden on the environment, and therefore various dry-processing image forming methods that do not require wet processing have been studied. Currently, image forming systems such as inkjet printers, electrophotography, and dye thermal transfer systems are in practical use. However, these dry-processing image forming methods have difficulty in obtaining a copy-copy manuscript having excellent light-shielding properties in the image area and excellent light transmission properties in the non-image area, that is, a so-called high-contrast copy-copy manuscript.

[0003] As a dry image forming method capable of obtaining a high contrast equivalent to that of a wet processing image forming method using a silver halide photosensitive material, there is a method of forming an image on a thermal recording material having a thermal recording layer on a support using a thermal head or infrared laser light. Among them, from the viewpoint of high density recording and high quality recording, a thermal recording method using infrared laser light is advantageous. As a thermal recording material that can be drawn by infrared laser light, for example, JP-A-6-194781 (Patent Document 1) discloses a thermal recording material that can record high density images and contains a thermally reducible silver source, a reducing agent for silver ions, a dye that absorbs laser light in the wavelength range of about 500 to 1100 nm, and a polymerizable binder, and JP-A-10-29377 (Patent Document 2) discloses a thermal recording material for infrared laser light that can record high quality images and contains an organic silver salt, a developer for the organic silver salt, an infrared absorbing dye, and a water-soluble binder. Furthermore, JP-A No. 2001-10229 (Patent Document 3) discloses a thermal color image forming material that contains a non-photosensitive organic silver salt, a reducing agent for silver ions, a binder, a color tone adjusting agent, and an absorbent that absorbs radiation in the wavelength range of 750 to 1100 nm, and that has a low ultraviolet concentration and little residual color.

[0004] However, in recent years, there has been a demand for higher density and higher resolution images, and even when the thermal recording materials disclosed in the above-mentioned patent documents are used as a plate manuscript, the contrast is insufficient, and fine image details such as thin lines and tiny dots may be lost due to insufficient or excessive exposure to light on the photosensitive material being made into a plate. Therefore, there has been a demand for further improvement in the contrast of thermal recording materials that form images by exposure to infrared laser light. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Application Publication No. 6-194781 [Patent Document 2] Japanese Patent Application Publication No. 10-29377 [Patent Document 3] JP 2001-10229 A Summary of the Invention [Problem to be solved by the invention]

[0006] An object of the present invention is to provide a heat-sensitive recording material which can provide a high-contrast image by irradiation with an infrared laser beam. [Means for solving the problem]

[0007] The above-mentioned problems are solved by the following invention. A heat-sensitive recording material comprising, on a light-transmitting support, at least an infrared absorbing layer containing an infrared absorbing dye having a ratio ε(830) / ε(365) of the molar absorption coefficient ε(830) at 830 nm to the molar absorption coefficient ε(365) at 365 nm of 4.0 or more, a heat-sensitive recording layer containing a non-photosensitive organic silver salt and substantially free of photosensitive silver halide, and a protective layer, in this order. Effect of the Invention

[0008] According to the present invention, it is possible to provide a heat-sensitive recording material which can provide a high-contrast image by irradiation with an infrared laser beam. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The present invention will be described in detail below.

[0010] The heat-sensitive recording material of the present invention has a light-transmitting support. Examples of such light-transmitting supports include resin films such as polyethylene terephthalate, polyethylene naphthalate, cellulose nitrate, and polycarbonate, and inorganic materials such as glass. In the present invention, the light-transmitting support means a support having a total light transmittance of 60% or more, and more preferably 70% or more. The haze value of the light-transmitting support is preferably 10% or less. The light-transmitting support may have known layers such as an easy-adhesion layer, a hard coat layer, and an antistatic layer. The thickness of the light-transmitting support in the present invention is not particularly specified, but is preferably 50 to 300 μm from the viewpoint of handling.

[0011] The heat-sensitive recording material of the present invention has an infrared absorbing layer on the light-transmitting support described above, which contains an infrared absorbing dye having a ratio ε(830) / ε(365) of the molar absorption coefficient ε(830) at 830 nm to the molar absorption coefficient ε(365) at 365 nm of 4.0 or more. The infrared absorbing dye in the present invention refers to a dye having absorption in the wavelength region of 600 to 1500 nm, preferably having an absorption maximum in the wavelength region of 650 to 1100 nm, and more preferably having an absorption maximum in the wavelength region of 750 to 1100 nm. The infrared absorbing dye in the present invention has low absorption in the wavelength region of 350 to 450 nm, where the emission peak in the ultraviolet region of high-pressure mercury lamps and chemical lamps exists, that is, the above-mentioned ε(830) / ε(365) is 4.0 or more, so that a heat-sensitive recording material that can obtain a high-contrast image by irradiation with infrared laser light can be obtained, and the upper limit is not particularly limited. Examples of such dyes include compounds having a polymethine skeleton, such as squarylium, cyanine, merocyanine, and bis(aminoaryl)polymethine. Specific examples of such dyes include compounds represented by the following general formulas (1) to (3), but the present invention is not limited to these.

[0012] [ka]

[0013] R in general formulas (1) to (3) 1 ~R 10 is a substituent, and examples thereof include a hydrogen atom, an alkyl group, an aryl group, an alkoxy group, an acyl group, an ester group, an amide group, a halogen atom, a hydroxyl group, a thiol group, a thioether group, and a sulfonyl group. These may be the same or different substituents, and may be bonded to other substituents to form a ring structure. X - represents an atom or atomic group having a negative charge, and examples thereof include halogen ions, oxoacids such as perchlorate ions, tetrafluoroborate, hexafluorophosphate, alkyl and aryl sulfonates, etc. Specific examples thereof include, but are not limited to, compounds such as exemplified compounds (1) to (3).

[0014] The content of the infrared absorbing dye is preferably 0.1 to 20% by mass based on the total solid content of the infrared absorbing layer.

[0015] In the present invention, the infrared absorbing layer preferably contains a binder component together with the infrared absorbing dye. Such a binder component is preferably a thermoplastic resin, and examples thereof include cellulose derivatives such as hydroxyethyl cellulose and hydroxypropyl cellulose, acrylic resins, polyester resins, polyurethane resins, vinyl chloride resins, vinyl acetate resins, polyolefin resins, polyvinyl acetal resins such as polyvinyl butyral resins, and polyvinyl alcohol resins. These binder components may be used by dissolving them in water or an organic solvent, or may be used as latexes in which hydrophobic polymer solids are dispersed in the form of fine particles, or as polymer molecules dispersed in the form of micelles. In the present invention, the above-mentioned binder components are preferably those which form a transparent coating after drying. Furthermore, these binder components may be used in combination of two or more resins which are compatible with each other as necessary.

[0016] The infrared absorbing layer of the heat-sensitive recording material of the present invention is preferably formed by preparing an infrared absorbing layer coating solution containing the above-mentioned infrared absorbing dye and binder component, coating the infrared absorbing layer coating solution on the above-mentioned light-transmitting support, and drying the same. The thickness of the infrared absorbing layer is preferably 0.01 to 5.0 μm.

[0017] For the purpose of improving the coating property, the infrared absorbing layer coating liquid may contain various surfactants. As the surfactant, any of nonionic, anionic and cationic surfactants may be used, and is not particularly limited.

[0018] It is preferable that the infrared absorbing layer of the heat-sensitive recording material of the present invention is substantially free of non-photosensitive organic silver salts, reducing agents, color toners, and stabilizers, which will be described later, from the viewpoints of improving the efficiency of image formation by infrared laser light, suppressing an increase in haze, etc. The term "substantially free" as used herein means that the total amount of each of the above-mentioned components is less than 5% by mass of the solid content of the infrared absorbing layer.

[0019] The heat-sensitive recording layer of the heat-sensitive recording material of the present invention contains an organic silver salt. The organic silver salt is a non-photosensitive organic silver salt, and is reduced by heating together with a reducing agent described later to form a silver image. Specifically, the organic silver salt may be a silver salt of an organic acid such as gallic acid, oxalic acid, behenic acid, stearic acid, palmitic acid, or lauric acid, as described in Research Disclosure No. 17029(II) or No. 29963(XVI) relating to heat-developable photosensitive materials; a silver salt of a carboxyalkylthiourea such as 1-(3-carboxypropyl)thiourea or 1-(3-carboxypropyl)-3,3-dimethylthiourea; a silver salt of an aldehyde such as formaldehyde, acetaldehyde, or butylaldehyde, or an aromatic thiourea such as salicylic acid, benzoic acid, 3,5-dihydroxybenzoic acid, or 5,5-thiodisalicylic acid; Examples of the silver salt include a complex of a polymer reaction product with a carboxylic acid and silver; a silver salt or complex of thiones such as 3-(2-carboxyethyl)-4-hydroxymethyl-4-thiazoline-2-thione and 3-carboxymethyl-4-methyl-4-thiazoline-2-thione; a silver salt or complex of a nitrogen-containing heterocycle selected from imidazole, pyrazole, urazole, 1,2,4-triazole, 1H-tetrazole, 3-amino-5-benzylthio-1,2,4-triazole and benzotriazole; a silver salt of saccharin, 5-chlorosalicylaldoxime, etc.; and a silver salt of a mercaptide. Among these, a silver salt of a fatty acid having 10 or more carbon atoms is preferred, and silver stearate and silver behenate are particularly preferred.

[0020] In the present invention, the content of the organic silver salt contained in the heat-sensitive recording layer can be appropriately adjusted depending on the maximum concentration required for use as a copy manuscript, and is preferably 0.5 to 2.0 g per square meter in terms of silver.

[0021] The heat-sensitive recording layer in the present invention does not substantially contain silver halide. Here, "substantially does not contain" means that the amount of silver halide contained in the heat-sensitive recording layer is less than 1% by mass based on the total solid content of the heat-sensitive recording layer, which suppresses an increase in transmission density in non-image areas during storage and normal use of the heat-sensitive recording material of the present invention, and provides a heat-sensitive recording material capable of making high-contrast images into plates.

[0022] In the present invention, the heat-sensitive recording layer preferably contains a reducing agent, such as pyrogallol, 4-stearoylpyrogallol, isopropyl gallate, ethyl 3,4-dihydroxybenzoate, 2,5-dihydroxybenzoic acid, etc., as described in U.S. Pat. No. 3,074,809, polyhydroxyindanes as described in U.S. Pat. No. 3,440,049 or JP-A No. 06-317870, or dihydroxybenzoic acid derivatives as described in JP-A No. 2001-328357.

[0023] The content of the reducing agent may vary widely depending on the type of reducing agent and the type of organic silver salt, but is preferably 0.1 to 3.0 mol, more preferably 0.5 to 2.0 mol, per mol of organic silver salt. For various purposes, two or more of the reducing agents may be used in combination.

[0024] The thermosensitive recording layer of the thermosensitive recording material of the present invention preferably contains a so-called color toning agent known in the field of thermography or photothermography. Examples of color toning agents are known in the above-mentioned Research Disclosure on Photothermographic Materials, items 17029(V) and 29963(XXII), and specifically include imides such as phthalimide, mercapto compounds such as 3-mercapto-1,2,4-triazole, phthalazine, phthalazone, 4-methylphthalic acid, tetrachlorophthalic acid and their anhydrides, and benzoxazine derivatives such as 1,3-benzoxazine-2,4-dione. For various purposes, two or more of the above-mentioned color toning agents may be used in combination.

[0025] The heat-sensitive recording layer of the heat-sensitive recording material of the present invention may contain various accelerators, stabilizers and their precursors for the purpose of suppressing or promoting the formation of image silver, improving the storage stability of the heat-sensitive recording material before and after image formation, etc. Specifically, they may be selected from benzotriazole, 5-methylbenzotriazole, 5-chlorobenzotriazole, 2-mercaptobenzotriazole, 2-mercaptobenzimidazole, 2-mercaptobenzothiazole, 2-mercaptobenzoxazole, 4-hydroxy-6-methyl-1,3,3a,7-tetrazaindene, 1-phenyl-5-mercaptotetrazole, 2-amino-5-mercapto-1,3,4-thiadiazole, 3-mercapto-5-phenyl-1,2,4-triazole, 4-benzamido-3-mercapto-5-phenyl-1,2,4-triazole, etc., which are known as photographic stabilizers and inhibitors. In addition, two or more of the above accelerators and stabilizers may be used in combination for various purposes.

[0026] The thermosensitive recording layer of the thermosensitive recording material of the present invention preferably contains a binder component. Such a binder component is preferably a thermoplastic resin, and for example, the same thermoplastic resin as the binder component of the infrared absorbing layer described above can be preferably used. Furthermore, the binder component may be a combination of two or more mutually compatible resins as necessary.

[0027] The content of the binder component contained in the thermosensitive recording layer is preferably 10 to 70% by mass based on the total solid content of the thermosensitive recording layer.

[0028] The binder component described above preferably does not contain free halide ions such as chloride ions and bromide ions. Halide ions react with the silver ions of the organic silver salt to form photosensitive silver halide, which causes a decrease in the light resistance of the heat-sensitive recording material of the present invention. Specifically, it is preferable that the amount of the free halide ions is 100 ppm or less relative to the amount of the binder component.

[0029] In the present invention, the thermosensitive recording layer is preferably adjacent to the infrared absorbing layer without any other layer, which makes it possible to efficiently form an image by irradiation with infrared laser light, and to obtain an image with a particularly high contrast.The method of forming the thermosensitive recording layer is preferably to prepare a thermosensitive recording layer coating solution containing the organic silver salt, reducing agent, color toner, and binder component, and to coat the thermosensitive recording layer coating solution on the infrared absorbing layer and dry it to form the thermosensitive recording layer.The thickness of the thermosensitive recording layer is preferably 0.5 to 20 μm.

[0030] For the purpose of improving the coating property, the coating solution for the heat-sensitive recording layer may contain various surfactants. The surfactants may be nonionic, anionic or cationic, and are not particularly limited.

[0031] The heat-sensitive recording material in the present invention has a protective layer on the heat-sensitive recording layer for the purpose of protecting the heat-sensitive recording layer from contact with the photosensitive material or impact during handling. The protective layer preferably contains a resin component, and specific examples of the resin component include gelatin, acrylic resin, polyester resin, polyurethane resin, vinyl chloride resin, vinyl acetate resin, polyolefin resin, polyvinyl alcohol resin, polyvinyl acetal resin, etc. These resins and aqueous dispersions of resins are commercially available and easily available. In addition, the protective layer may contain a crosslinking agent to improve the scratch resistance.

[0032] In the present invention, the protective layer may contain various matting agents for the purpose of improving the vacuum property and scratch resistance. When forming the protective layer, it is preferable to use the matting agent by dispersing it in the above-mentioned protective layer. A high-speed stirrer such as a homodisper is suitable for dispersing the matting agent.

[0033] The matting agent may be either an organic or inorganic matting agent. Examples of organic matting agents include silicone, polytetrafluoroethylene, polymethyl methacrylate, polyacrylate, etc., and examples of inorganic matting agents include silica, alumina, talc, mica, etc. Examples of commercially available products include Tospearl (registered trademark) 120, 130, 145, and 2000B, which are sold by Momentive Performance Materials Japan LLC as silicone resin matting agents, and Sunsphere (registered trademark) H-31, H-51, and NP-30, which are sold by AGC Si-Tech Co., Ltd. as silica matting agents. These are single fine particles, but the form of the matting agent may be either a single fine particle or a fine particle aggregate particle in which fine particles are aggregated.

[0034] The amount of the matting agent contained in the protective layer is preferably 0.5 to 40% by mass, and more preferably 1 to 30% by mass, based on the amount of the resin component.

[0035] In the present invention, the method for forming the protective layer is preferably to prepare a protective layer coating liquid containing the above-mentioned resin component, matting agent, etc., and coat the protective layer coating liquid on the above-mentioned thermosensitive recording layer, and dry it to form the protective layer. In addition, in order to improve the coating property, the thermosensitive recording layer coating liquid may contain various surfactants. As the surfactant, any of nonionic, anionic, and cationic surfactants may be used, and there is no particular limitation.

[0036] The thickness of the protective layer of the heat-sensitive recording material of the present invention can be varied widely depending on the type of resin component used and the desired heat sensitivity, but is selected from the range of 0.1 to 10 μm.

[0037] In the present invention, the coating method for the infrared absorbing layer, the thermosensitive recording layer, and the protective layer is not particularly limited, and can be selected from various coating methods such as those described in ED Cohen and EB Gutoff, "Modern Coating and Drying Technology", Wiley-VCH, Inc. New York, 1992. Furthermore, it is particularly preferable in terms of improving productivity to simultaneously coat a plurality of layers by a slide coating method using a slit-type die coater or a tandem coating method in which coating and drying are repeated by combining the same or different types of coater devices.

[0038] In addition to the infrared absorbing layer, the thermosensitive recording layer, and the protective layer, the thermosensitive recording material of the present invention may further have, if necessary, an easy-adhesion layer, a heat-insulating layer, etc. between the light-transmitting support and the infrared absorbing layer, an intermediate layer, etc. between the infrared absorbing layer, the thermosensitive recording layer, and the protective layer, an easy-peel layer, etc. on the protective layer, and an antistatic layer, etc. on the side of the light-transmitting support opposite the thermosensitive recording layer and the protective layer, but as described above, it is preferable that the infrared absorbing layer and the thermosensitive recording layer are adjacent to each other.

[0039] Using the above-mentioned heat-sensitive recording material, an image can be obtained by irradiating infrared laser light imagewise from the protective layer side of the heat-sensitive recording material. Examples of light sources for the infrared laser light include semiconductor lasers, He-Ne lasers, Ar lasers, carbon dioxide gas lasers, YAG lasers, fiber lasers, etc. The heat-sensitive recording material of the present invention can change the density of the image area by changing the energy and exposure time of the infrared laser light irradiated. EXAMPLES

[0040] The present invention will be described below using examples, but the present invention is not limited to these examples. In the description, "%" is based on mass.

[0041] <Example 1>

[0042] <Preparation and Coating of Infrared Absorbing Layer Coating Solution> 81 g of 2-butanone and 24 g of methanol were mixed with 9.0 g of polyvinyl butyral resin (Butvar (registered trademark) B-79, Eastman Chemical Japan Co., Ltd.) and 0.45 g of exemplary compound (3) (IRT, ε (830) / ε (365) = 6.2) as an infrared absorbing dye to prepare an infrared absorbing layer coating solution. This infrared absorbing layer coating solution was applied to a PET base (total light transmittance 92%, haze value 4%) with a thickness of 100 μm so that the film thickness after drying would be 1.2 μm, and dried at 50 ° C. Note that ε (830) and ε (365) were calculated by measuring the absorption spectrum of a 2-butanone solution of the infrared absorbing dye using a UV-2600 ultraviolet-visible spectrophotometer (Shimadzu Corporation, using a quartz cell with an optical path length of 1 cm).

[0043] <Preparation of Silver Behenate Dispersion> 20 g of silver behenate crystals and 22 g of polyvinyl butyral resin (Butvar B-79) were added to 175 g of 2-butanone, and a silver behenate dispersion (average particle size: 0.6 μm) was obtained using a bead mill (DYNO-MILL KD20B, manufactured by Willy & Bachofen) filled with zirconia beads having a diameter of 0.65 mm.

[0044] <Preparation and Coating of Thermal Recording Layer Coating Solution> To 45 g of 2-butanone, 2.4 g of polyvinyl butyral resin (Butvar B-79), 30 g of the above-mentioned silver behenate dispersion, 1.5 g of ethyl 3,4-dihydroxybenzoate as a reducing agent, 0.6 g of tetrachlorophthalic anhydride, and 1.2 g of phthalazone were added to prepare a heat-sensitive recording layer coating solution. This heat-sensitive recording layer coating solution was applied to the infrared absorbing layer already obtained as described above at a concentration of 1.1 g / m2 in terms of silver. 2 A heat-sensitive recording layer was formed by drying at 80° C. The silver halide content in the obtained heat-sensitive recording layer was less than 0.1% based on the total solid content of the heat-sensitive recording layer.

[0045] <Preparation and Application of Protective Layer Coating Solution> To 15.0 g of 2-butanone, 15.0 g of Beamset (registered trademark) 3702 (Arakawa Chemical Industries, Ltd.; mixture containing epoxy acrylate polymer, multifunctional acrylate compound, and photopolymerization initiator, solid content rate 59%) was added as a photocurable resin to obtain 30 g (of which, the solid content mass of the binder component was 8.4 g). This protective layer coating liquid was applied onto the above-mentioned thermosensitive recording layer so that the film thickness after drying would be 3.0 μm, and after drying at 60° C., the protective layer was cured by irradiating it with a high-pressure mercury lamp at an irradiation distance of 10 cm and a conveying speed of 5 m / min, and the thermosensitive recording material of Example 1 was obtained.

[0046] <Example 2> A heat-sensitive recording material of Example 2 was obtained in the same manner as in Example 1, except that in the preparation and application of the infrared absorbing layer coating liquid in Example 1, the infrared absorbing layer coating liquid was applied so that the film thickness after curing of the infrared absorbing layer would be 1.5 μm.

[0047] <Example 3> A heat-sensitive recording material of Example 3 was obtained in the same manner as in Example 1, except that in the preparation and application of the infrared absorbing layer coating liquid in Example 1, the infrared absorbing layer coating liquid was coated so that the film thickness after curing of the infrared absorbing layer would be 1.9 μm.

[0048] <Example 4> A thermal recording material of Example 4 was obtained in the same manner as in Example 1, except that in the preparation and application of the protective layer coating solution of Example 1, 9 g of polyvinyl butyral resin (Butvar B-79) was added to 81 g of 2-butanone and 24 g of methanol to prepare a protective layer coating solution, and the solution was coated so that the film thickness after drying would be 1.6 μm.

[0049] <Example 5> A heat-sensitive recording material of Example 5 was obtained in the same manner as in Example 1, except that in the preparation and coating of the infrared absorbing layer coating liquid of Example 1, 0.45 g of exemplary compound (1) (ε(830) / ε(365)=18.5) was added instead of IRT as the infrared absorbing dye, and the infrared absorbing layer coating liquid was coated so that the film thickness after drying would be 1.5 μm.

[0050] [ka]

[0051] <Example 6> A heat-sensitive recording material of Example 6 was obtained in the same manner as in Example 1, except that in the preparation and coating of the infrared absorbing layer coating solution of Example 1, 0.45 g of the exemplary compound (1) was added instead of IRT as the infrared absorbing dye, and the infrared absorbing layer coating solution was coated so that the film thickness after drying would be 2.3 μm.

[0052] <Comparative Example 1> A thermal recording material of Comparative Example 1 was obtained in the same manner as in Example 1, except that in Example 1, no infrared absorbing layer was applied, and instead the thermal recording layer was applied onto a 100 μm-thick PET base (total light transmittance 92%, haze value 4%).

[0053] <Comparative Example 2> A thermosensitive recording material of Comparative Example 2 was obtained in the same manner as in Example 1, except that in Example 1, no infrared absorbing layer was applied, and 0.045 g of exemplary compound (3) was added as an infrared absorbing dye in the preparation and application of a thermosensitive recording layer coating solution, and the solution was applied onto a 100 μm-thick PET base (total light transmittance 92%, haze value 4%).

[0054] <Comparative Example 3> In Example 1, the infrared absorbing layer was not coated, and the thermosensitive recording layer coating liquid was coated on a 100 μm-thick PET base (total light transmittance 92%, haze value 4%). In preparing and coating the protective layer coating liquid, 9 g of polyvinyl butyral resin (Butvar B-79) and 0.45 g of exemplary compound (3) as an infrared absorbing dye were added to 81 g of 2-butanone and 24 g of methanol to prepare the protective layer coating liquid, and the protective layer coating liquid was coated so that the film thickness after drying would be 1.6 μm. A thermosensitive recording material of Comparative Example 3 was obtained in the same manner as in Example 1, except that the infrared absorbing layer coating liquid was coated so that the film thickness after drying would be 1.6 μm.

[0055] <Comparative Example 4> A heat-sensitive recording material of Comparative Example 4 was obtained in the same manner as in Example 1, except that in the preparation and coating of the infrared absorbing layer coating solution of Example 1, 0.07 g of IX-2-IR-14 (manufactured by Nippon Shokubai Co., Ltd., phthalocyanine dye, ε(830) / ε(365)=2.6) was added instead of IRT as the infrared absorbing dye.

[0056] The thermal recording materials of Examples 1 to 6 and Comparative Examples 1 to 4 thus obtained were used in a thermal CTP setter (AURA600E, manufactured by Guangzhou Amsky Technology Co Ltd) to form an image (20 mm (width) x 200 mm (length)) having 50 microdots with a diameter of 20 μm (negative image) and a solid area, while changing the drum rotation speed to 300 rpm and the exposure output to 200 mW to 800 mW.

[0057] <Transmission density measurement> After the above image formation, the transmission densities of the solid images and non-image areas of the thermal recording materials of Examples 1 to 6 and Comparative Examples 1 to 4 were measured using an X-Rite (registered trademark) 361T (UV mode) manufactured by X-Rite, Inc. The exposure output value, the transmission density of the solid images (Dmax), and the transmission density of the non-image areas (Dmin) when the maximum transmission density of each thermal recording material was obtained are shown in Table 1.

[0058] <Return performance evaluation> The thermal recording material after the image formation was used as a mask film to make a negative resin plate (TORELIEF (registered trademark) MF95DIIJ, thickness 0.95 mm, manufactured by Toray Industries, Inc.) using a platemaking machine (Takano Processor DX-A4, manufactured by Takano Machinery Works, Ltd.), and the return characteristics of the thermal recording material were evaluated. The evaluation results are shown in Table 1, with 49 or more of the 50 microdots with a diameter of 20 μm remaining on the resin plate after platemaking being marked as ◯, 30 to 48 remaining being △, and 0 to 29 remaining being ×.

[0059] [Table 1]

[0060] As is clear from the results in Table 1, it is understood that the present invention provides a heat-sensitive recording material capable of producing a high-contrast image.

Claims

1. A heat-sensitive recording material having, on a transparent support, at least in this order: an infrared absorbing layer containing an infrared absorbing dye having a ratio ε(830) / ε(365) of the molar absorption coefficient ε(830) at 830 nm to the molar absorption coefficient ε(365) at 365 nm of 4.0 or more; a heat-sensitive recording layer containing a non-photosensitive organic silver salt and substantially free of photosensitive silver halide; and a protective layer, wherein the infrared absorbing dye is a compound represented by any one of the following general formulas (1) to (3): 【Chemistry 1】 [In the general formulas (1) to (3), R 1 to R 10 may be the same or different. R 1 to R 10 are a hydrogen atom, an alkyl group, an aryl group, an alkoxy group, an acyl group, an ester group, an amide group, a halogen atom, a hydroxy group, a thiol group, a thioether group, or a sulfonyl group, or are bonded to other substituents to form a ring structure. X - is a halogen ion, an oxoacid ion, tetrafluoroborate, hexafluorophosphate, an alkylsulfonate, or an arylsulfonate.]

2. A heat-sensitive recording material having, on a transparent support, at least in this order: an infrared absorbing layer containing an infrared absorbing dye having a ratio ε(830) / ε(365) of the molar absorption coefficient ε(830) at 830 nm to the molar absorption coefficient ε(365) at 365 nm of 4.0 or more; a heat-sensitive recording layer containing a non-photosensitive organic silver salt and substantially free of photosensitive silver halide; and a protective layer, wherein the infrared absorbing dye is any one of the following exemplary compounds (1) to (3). 【Chemistry 2】

Citation Information

Patent Citations

  • Laser-scanning thermorecording material

    JP1994194781A

  • Heat-sensitive material suitably used for direct thermal recording

    JP1995323667A

  • Methods and materials for forming heat mode images

    JP1997504239A

  • Thermosensitive recording material and thermal recording

    JP1998029377A

  • Method for forming image and image recording medium

    JP1999198532A