Grain-oriented electrical steel sheet and method for refining magnetic domains therein
Laser-irradiated grooves with controlled orientation and sub-grain boundaries in grain-oriented electrical steel sheets enhance magnetic domain refinement, addressing shape and environmental issues of existing methods, thereby improving iron loss and magnetic flux density.
Patent Information
- Application Number
- JP2022537572
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-12-20
- Filing Date
- 2020-12-18
- Publication Date
- 2024-10-03
- Estimated Expiration
- 2040-12-18
AI Technical Summary
Existing methods for refining magnetic domains in grain-oriented electrical steel sheets, such as etching and roll processing, face challenges in controlling groove shape, environmental impact, and stability, leading to inconsistent iron loss characteristics and magnetic flux density deterioration.
A method involving laser irradiation to form grooves on the steel sheet with controlled orientation and sub-grain boundaries, followed by insulating coating, to minimize magnetic flux density deterioration during stress relaxation annealing.
The method effectively refines magnetic domains, improving iron loss and maintaining magnetic flux density by controlling crystal grain orientation and sub-grain boundaries within specific ranges.
Smart Images

Figure 0007561194000002 
Figure 0007561194000003 
Figure 0007561194000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a grain-oriented electrical steel sheet and a method for refining its magnetic domains, and more particularly to a grain-oriented electrical steel sheet and a method for refining its magnetic domains, in which a deterioration in magnetic flux density is minimized due to complete encroachment of a secondary recrystallized structure of a base part during stress relaxation or recrystallization at a lower part of a groove during annealing heat treatment at a temperature equal to or higher than the recrystallization temperature of the grain-oriented electrical steel sheet. [Background technology]
[0002] Grain-oriented electrical steel sheets are used as core materials for electromagnetic products such as transformers, and improve the energy conversion efficiency by reducing the power loss of electrical equipment. To achieve this, steel sheets with excellent core loss and high drop ratios at the time of lamination and winding are required. Grain-oriented electrical steel sheets are made by hot rolling, cold rolling and annealing processes, and the grains are recrystallized in the rolling direction in the {110} direction. <001> It is a functional steel sheet with a texture oriented in the direction (also known as "Goss Texture").
[0003] Magnetic domain refinement is known as a method for reducing the iron loss of grain-oriented electrical steel sheets. That is, the large magnetic domains that grain-oriented electrical steel sheets have are refined by scratching the magnetic domains or applying energetic shocks to them. In this case, the amount of energy consumed when the magnetic domains are magnetized and their direction changes can be reduced compared to when the magnetic domains were large. There are two methods for refining magnetic domains: permanent magnetic domain refinement, in which the improvement effect is maintained even after heat treatment, and temporary magnetic domain refinement, in which the improvement effect is not maintained. Permanent magnetic domain refinement methods that show iron loss improvement effects even after stress relief heat treatment above the heat treatment temperature at which recovery occurs can be classified into etching, rolling, and laser methods. With the etching method, grooves are formed on the steel sheet surface through selective electrochemical reactions in a solution, making it difficult to control the shape of the grooves and to ensure uniform iron loss characteristics in the width direction of the final product. In addition, it has the disadvantage of being unfriendly to the environment due to the acid solution used as a solvent.
[0004] The permanent magnetic domain refinement method using rolls is a magnetic domain refinement technology that produces an iron loss improvement effect by forming protrusions on a roll and pressing the material roll or plate to form grooves of a certain width and depth on the surface, and then annealing to partially cause recrystallization under the grooves. The roll method has the disadvantages of low reliability because it is difficult to ensure stability against machining and stable iron loss due to thickness, and the process is complicated, and iron loss and magnetic flux density characteristics deteriorate immediately after groove formation (before stress relief annealing). The permanent magnetic domain miniaturization method using a laser is a method in which a high-power laser is irradiated onto the surface of an electromagnetic steel sheet moving at high speed, and the laser irradiation melts the base portion to form a groove. Summary of the Invention [Problem to be solved by the invention]
[0005] An object of the present invention is to provide a grain-oriented electrical steel sheet and a method for refining its magnetic domains, which minimizes deterioration of magnetic flux density caused by the stress concentration areas and resolidified structures formed under grooves being encroached upon by the secondary recrystallized structure of the base during recoating or stress relief annealing at or above the recrystallization temperature. [Means for solving the problem]
[0006] The grain-oriented electrical steel sheet of the present invention is characterized in that it comprises grooves present on the surface of the electrical steel sheet and recrystallizations abutting the lower parts of the grooves, and the average orientation difference between the recrystallizations abutting the lower parts of the grooves and the other recrystallizations is 0.5 to 10°.
[0007] The recrystallization in contact with the lower part of the groove preferably includes a sub-boundary, and each groove preferably has a sub-boundary of 10 μm to 700 μm in length. The number of the subgrain boundaries may be 1 to 10 per groove.
[0008] The insulating film may further include an insulating coating abutting on the groove. The groove depth is preferably 3 to 15% of the steel sheet thickness, and the groove width is preferably 10 to 50 μm.
[0009] The method for refining magnetic domains of grain-oriented electrical steel sheet according to the present invention includes the steps of preparing a cold-rolled steel sheet, subjecting the cold-rolled steel sheet to primary recrystallization annealing, subjecting the cold-rolled steel sheet to secondary recrystallization annealing, irradiating a laser on the steel sheet on which secondary recrystallization annealing has been completed to form grooves, and forming an insulating coating on the steel sheet on which the grooves have been formed. During the laser irradiation, the laser energy density is 3.0 to 8.0 J / mm 2 It is characterized in that:
[0010] The laser output may be 500W or more, the laser scanning speed may be 5m / s or more, and the laser scanning distance may be 100mm or more. The wavelength of the laser is preferably 1.06 to 10.6 μm.
[0011] It is preferable that the length of the laser beam is 100 to 500 μm and the width of the laser beam is 10 to 27 μm. The step of forming the insulating coating may include a step of heat treating at a temperature of 750 to 950°C. Effect of the Invention
[0012] According to an embodiment of the present invention, the grooves are formed to improve core loss during annealing at or above the recrystallization temperature, while the grain orientation below the grooves is appropriately formed within 10° to minimize degradation of magnetic flux density. [Brief description of the drawings]
[0013] [Figure 1] FIG. 2 is a schematic diagram of a rolled surface (ND surface) of a grain-oriented electrical steel sheet according to one embodiment of the present invention. [Diagram 2] FIG. 1 is a schematic diagram of a cross section (TD surface) of a grain-oriented electrical steel sheet according to an embodiment of the present invention. [Diagram 3]FIG. 1 is a schematic diagram of a cross section (TD surface) of an existing grain-oriented electrical steel sheet. [Figure 4] FIG. 1 is a schematic diagram of a cross section (TD surface) of a grain-oriented electrical steel sheet according to an embodiment of the present invention. [Diagram 5] FIG. 2 is a schematic diagram showing a shape of a laser beam according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] Terms such as first, second, and third are used to describe various parts, components, regions, layers, and / or sections, but are not limited thereto. These terms are used only to distinguish one part, component, region, layer, or section from another part, component, region, layer, or section. Thus, a first part, component, region, layer, or section described below can be referred to as a second part, component, region, layer, or section without departing from the scope of the present invention. The terminology used herein is merely for the purpose of referring to particular embodiments and is not intended to limit the invention. As used herein, the singular form includes the plural form unless the phrase clearly indicates otherwise. As used in the specification, the meaning of "comprising" embodies the specified features, regions, integers, steps, operations, elements and / or components and does not exclude the presence or addition of other features, regions, integers, steps, operations, elements and / or components.
[0015] When an element is referred to as being "on" or "on" another element, it may be immediately on or above the other element, or there may be other elements between them. In contrast, when an element is referred to as being "directly on" another element, there are no other elements between them. Unless otherwise defined, all terms, including technical and scientific terms, used herein have the same meaning as commonly understood by a person having ordinary skill in the art to which the present invention belongs. Terms defined in commonly used dictionaries are additionally interpreted to have a meaning consistent with the relevant technical literature and the currently disclosed contents, and are not interpreted as ideal or very formal meanings unless defined. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention will now be described in detail with reference to exemplary embodiments thereof, so that those skilled in the art will be able to easily practice the present invention. However, the present invention may be embodied in many different forms and is not limited to the embodiments set forth herein.
[0016] FIG. 1 is a schematic diagram of the rolled surface (ND surface) of a grain-oriented electrical steel sheet according to one embodiment of the present invention. As shown in FIG. 1, a grain-oriented electrical steel sheet 10 according to an embodiment of the present invention has linear grooves 20 formed on one or both sides of the electrical steel sheet in a direction intersecting the rolling direction (RD direction). As shown in Fig. 1, the longitudinal direction of the groove 20 (RD direction in Fig. 1) and the rolling direction (RD direction) may form an angle of 75 to 88 degrees. When the groove 20 is formed at this angle, it can contribute to improving the iron loss of the grain-oriented electrical steel sheet. The grooves 20 can be formed continuously or intermittently along the direction perpendicular to the rolling direction (TD) of the steel sheet. When the grooves 20 are formed intermittently, it is preferable that 2 to 10 grooves are formed along the rolling direction perpendicular to the rolling direction (TD) of the steel sheet. FIG. 1 shows a case where 4 grooves 20 are formed intermittently.
[0017] FIG. 2 is a schematic diagram of a cross section (TD plane) of a grain-oriented electrical steel sheet according to an embodiment of the present invention. 2, the grain-oriented electrical steel sheet according to an embodiment of the present invention has grooves 20 on the surface and secondary recrystallization 31 in contact with the lower part of the grooves 20. In an embodiment of the present invention, the degree of orientation of the secondary recrystallization 31 can be controlled to minimize the deterioration of magnetic properties due to the formation of the grooves 20. The secondary recrystallizations 31 in contact with the lower part of the groove 20 are distinguished from other recrystallizations 32. The other secondary recrystallizations 32 are secondary recrystallizations 32 that do not contact the groove 20, and are secondary recrystallizations 32 formed near the surface where no groove 20 is formed or secondary recrystallizations 32 formed inside the steel sheet.
[0018] In one embodiment of the present invention, the secondary recrystallization 31 in contact with the lower part of the groove 20 has a grain size of several mm to several tens of mm, which is the size of grains that appear in ordinary grain-oriented electrical steel sheets, and therefore, in the thickness direction, the grains are mostly perforated. The grain size of the secondary recrystallization 31 is calculated as the diameter of a hypothetical circle having the same area as the recrystallization 31 with respect to a plane perpendicular to the rolling direction (TD plane). In one embodiment of the present invention, the orientation of the secondary recrystallization 31 in contact with the groove is controlled by various process conditions, but the most important process conditions are the shape of the laser beam formed on the steel sheet and the energy density conditions when irradiating the laser. That is, when grooves are formed in a secondary recrystallized sheet and the steel sheet is heat treated at a temperature equal to or higher than the recrystallization temperature, the average crystal grain orientation difference of the secondary recrystallization in contact with the groove 20 can be formed to be 0.5 to 10° if the energy density conditions are appropriate. More specifically, it can be formed to be 0.5 to 5°.
[0019] When a laser is irradiated onto a steel sheet where secondary recrystallization has been completed, shocks due to the heat of the laser occur below the grooves 20, some of which form as sub-boundaries 33. After the grooves 20 are formed, the sub-boundaries 33 grow during heat treatment in the insulating coating formation process. A sub-boundary 33 is defined as a defect occurrence area within a crystal grain that occurs when the density of lattice defects such as potential or twins is locally increased within the same crystal grain by locally applying thermal or mechanical stress, and differs from a general grain boundary because it appears only in a limited area of the crystal lattice.
[0020] Subgrain boundaries exist in the secondary recrystallization 31 that contacts the groove 20 with a continuous or discontinuous length of 10 μm to 700 μm per groove. The reference plane is a plane cutting the length of the groove 20, and when analyzing the secondary recrystallization 31 that contacts the groove 20 in a photograph measured by SEM or EBSD (Electron Backscatter Diffraction), the part where the crystal orientation differs by 0.5 to 10° near the bottom of the groove 20 located within the grain is determined to be a subgrain boundary 33, and these lengths can be measured and detected. If the length of the subgrain boundary 33 is excessively long or short, it adversely affects the orientation of the secondary recrystallization 31 in contact with the groove 20, ultimately resulting in inferior magnetic properties. More specifically, the length of the subgrain boundary 33 is preferably 300 to 700 μm.
[0021] A plurality of subgrain boundaries may be present intermittently. In this case, the total length of all the subgrain boundaries present in the vicinity of the groove in the secondary recrystallization 31 can satisfy the above-mentioned range. As described above, there can be 1 to 10 subgrain boundaries per groove. The length of the subgrain boundary 33 is affected by the energy density of the laser and the shape of the laser beam when the groove 20 is formed, and by the heat treatment conditions in the insulating film formation process after the groove 20 is formed.
[0022] Figure 3 is a schematic diagram of the cross section (TD surface) of an existing grain-oriented electrical steel sheet. After forming an insulating coating, a laser was irradiated to form grooves. As shown in FIG. 3, it can be seen that fewer subgrain boundaries 33 are formed in the secondary recrystallization 31 adjacent to the groove 20 compared to FIG. This is because the subgrain boundaries 33 were formed only by the thermal shock of the laser, and the subgrain boundaries 33 did not grow properly thereafter. In this case, unlike the embodiment of the present invention, the difference in the orientation between the secondary recrystallization 31 in contact with the groove 20 and the other secondary recrystallizations 32 exceeds 10°. In this case, as described above, there is a risk that the magnetic flux density will be significantly inferior.
[0023] FIG. 4 is a schematic diagram of a cross section (TD plane) of a grain-oriented electrical steel sheet according to an embodiment of the present invention. The formation of grooves 20 according to one embodiment of the present invention will now be described with reference to FIG. Groove 20 width W G If the width of the groove 20 is too narrow or too wide, there is a risk that a suitable effect of refining the magnetic domains cannot be obtained. Groove Depth H G The groove depth is preferably 3 to 15% of the steel sheet thickness. If the groove depth is too shallow, the iron loss improvement effect cannot be sufficiently obtained. If the groove depth is too deep, there is a risk that the structural characteristics of the steel sheet 10 will be significantly changed by strong laser irradiation or that a large amount of hill-up and spatter will be formed, deteriorating the magnetic properties. Therefore, it is preferable to control the depth of the groove 20 within the above range. More specifically, the depth of the groove 20 is preferably 5 to 10% of the steel sheet thickness.
[0024] As described above, in one embodiment of the present invention, a groove is formed by irradiating a laser on a steel sheet that has been subjected to secondary recrystallization annealing, and therefore, no metal oxide layer 40 exists on the top of the groove. The metal oxide layer 40 is a layer formed by a reaction between an annealing separator and an oxide layer on the surface of the steel sheet during the secondary recrystallization annealing process. As an example, when an MgO annealing separator is applied, a forsterite layer is formed. As shown in FIG. 4, a metal oxide layer 40 exists on the top of a steel sheet 10 where no groove 20 is formed, whereas no metal oxide layer 40 exists on the groove 20. Thereafter, as described above, the insulating coating is formed, so that the insulating coating 50 is in contact with the grooves. In other words, the metal oxide layer 40 is not present between the grooves 20 and the insulating coating 50. The insulating coating 50 may be any common insulating coating without limitation. For example, it may contain up to 10% by weight of a mineral, up to 60% by weight of silica, and up to 60% by weight of a metal phosphate. Additionally, it may further contain up to 4% by weight of boric acid.
[0025] A method for refining magnetic domains in a grain-oriented electrical steel sheet according to an embodiment of the present invention includes the steps of preparing a cold-rolled steel sheet, subjecting the cold-rolled steel sheet to primary recrystallization annealing, subjecting the cold-rolled steel sheet to secondary recrystallization annealing, irradiating a laser onto the steel sheet on which the secondary recrystallization annealing has been completed to form grooves, and forming an insulating coating on the steel sheet on which the grooves have been formed. First, a cold-rolled steel sheet is prepared. In one embodiment of the present invention, the features lie in the magnetic domain refinement method, the grooves 20 formed, and the recrystallization 31 present below the grooves 20, and the cold-rolled steel sheet to be subjected to magnetic domain refinement can be used without any restrictions. In particular, the effect of the present invention is achieved regardless of the alloy composition of the cold-rolled steel sheet. Therefore, a detailed description of the alloy composition of the cold-rolled steel sheet will be omitted. Next, the cold rolled sheet is subjected to primary recrystallization annealing.
[0026] The primary recrystallization annealing step is widely known in the field of grain-oriented electrical steel sheets, so a detailed description will be omitted. The primary recrystallization annealing process may include decarburization or decarburization and nitridation, and annealing may be performed in a humid atmosphere for decarburization or decarburization and nitridation. The crack temperature in the primary recrystallization annealing step is preferably 710 to 870°C. Also, the dew point temperature is preferably 40 to 70°C. Next, an annealing separator is applied to the steel sheet, followed by secondary recrystallization annealing. Annealing separators are widely known, so a detailed description is omitted. As an example, an annealing separator containing MgO as a main component can be used.
[0027] The purpose of secondary recrystallization annealing is to obtain {110} <001> The oxide layer formed during the texture formation and primary recrystallization annealing reacts with MgO to form a metal oxide (glassy) film 40, imparting insulation and removing impurities that impair magnetic properties. In the method of secondary recrystallization annealing, a mixture of nitrogen and hydrogen is maintained in the temperature rise section before secondary recrystallization occurs, protecting the nitrides that act as grain growth inhibitors, allowing secondary recrystallization to develop well, and after secondary recrystallization is complete, at the crack stage, the material is maintained in a 100% hydrogen atmosphere for a long time to remove impurities. The secondary recrystallization annealing step can be carried out at a cracking temperature of 900 to 1210°C. Next, a laser is irradiated onto the steel sheet after the secondary recrystallization annealing to form grooves. As described above, in one embodiment of the present invention, the order of the steps of forming the grooves, the shape of the beam formed on the sheet, and the energy density of the laser when forming the grooves are important.
[0028] The grooves 20 are formed by irradiating the laser in a direction intersecting the rolling direction (RD direction). Laser density is 3.0~8.0J / mm 2 If the laser density is too low, the thermal effect on the lower part of the groove 20 is small, and fine recrystallization is generated, and even if the heat treatment is performed in the subsequent insulating coating formation process, the recrystallization 31 in contact with the lower part of the groove 20 cannot grow sufficiently. On the other hand, if the laser density is too high, a large amount of hill-ups and spatters are formed due to the melting of the steel sheet, and due to these effects, the degree of orientation of the recrystallization 31 may be significantly inferior. Therefore, the laser density can be adjusted within the above range. More specifically, the laser density is 3.0 to 7.0 J / mm 2 It is good to be.
[0029] The laser output is preferably 500W or more, the laser scanning speed is 5m / s or more, and the laser scanning distance is 100mm or more. By using an appropriate output, scanning speed, and scanning distance, recrystallization can be appropriately formed at the bottom of the groove. More specifically, the laser output is preferably 500-10kW, the laser scanning speed is 10-80m / s, and the laser scanning distance is 100-500mm. There is no restriction on the laser oscillation mode. That is, continuous wave or pulsed mode can be used. In this way, the groove 20 shown in Figs. 1 and 2 is formed by irradiating the laser so that the surface beam absorptance is equal to or greater than the heat of fusion of the silver on the steel plate. In particular, a Gaussian mode (TEMoo M2 ≦ 1.10) laser can be used. Taking into consideration the energy absorption rate of the steel sheet 10 on which the metal oxide layer 40 is formed, a laser having a wavelength in the range of 1.06 to 10.6 μm can be used.
[0030] 5 is a schematic diagram showing the shape of a laser beam according to one embodiment of the present invention. In the step of forming grooves, the laser beam length L in the direction perpendicular to the rolling direction of the steel sheet (TD direction) is preferably 100 to 500 μm. If the beam length L in the direction perpendicular to the rolling direction (TD direction) is too short, the time for which the laser is irradiated becomes too short, making it impossible to form appropriate grooves, and therefore making it difficult to obtain an iron loss improvement effect. More specifically, the beam length L is preferably 150 to 450 μm. The laser beam width W in the rolling direction (RD direction) of the steel sheet is preferably 10 to 27 μm. If the beam width W is excessively short or long, the width of the groove 20 becomes narrow or wide, and there is a risk that an appropriate magnetic domain refining effect cannot be obtained. Although the beam shape is shown as an ellipse in FIG. 5, there is no restriction on the shape, such as a sphere or a rectangle.
[0031] After the step of forming the groove, the method may further include the step of controlling the height of the sputters to 3.5 μm or less by acid washing or brushing. Next, an insulating coating is formed on the grooved steel plate. The method for forming the insulating coating layer is not particularly limited, and as an example, the insulating coating layer can be formed by applying an insulating coating liquid containing phosphate. Such an insulating coating liquid can contain 10% by weight or less of inorganic compounds, 60% by weight or less of silica, and 60% by weight or less of metal phosphate. In this case, the metal phosphate may be Al phosphate, Mg phosphate, or a combination thereof, and the content of Al, Mg, or a combination thereof based on the weight of the insulating coating liquid may be 15% by weight or more. The coating liquid may further contain 4% by weight or less of boric acid.
[0032] After applying the insulating coating liquid, the insulating coating can be formed by heat treatment. At this time, the temperature is preferably 750 to 900° C. By controlling the temperature within an appropriate range, the grain size of the recrystallized particles 31 can be appropriately controlled. The present invention will be described in more detail with reference to the following examples, which are merely for illustrative purposes and are not intended to limit the scope of the present invention. EXAMPLES
[0033] Examples 1 to 5 A 0.27 mm grain-oriented electrical steel sheet that had undergone secondary recrystallization was prepared. A 1.0 kW Gaussian mode continuous wave laser was irradiated onto this electrical steel sheet to form grooves at an angle of 86° with the RD direction. The width W of the laser beam was 13 μm, and the length L of the laser beam was 200 μm. Grooves were formed intermittently in 8 sections in the TD direction. The laser energy density and groove depth were changed as shown in Table 1 below. After that, an insulating coating liquid was applied and the substrate was heat-treated at a temperature of 840° C. for 1.5 minutes.
[0034] Table 1 shows the iron loss improvement rate and magnetic flux density deterioration rate. The iron loss improvement rate was calculated by measuring the iron loss W1 of the electromagnetic steel sheet without grooves and the iron loss W2 of the electromagnetic steel sheet with grooves and calculating it as (W1-W2) / W1. The iron loss is the iron loss value W when the magnetic flux density is 1.7 Tesla and the frequency is 50 Hz. 17 / 50 was measured. The rate of magnetic flux density degradation was calculated by measuring the magnetic flux density B1 of an electrical steel sheet without grooves and the magnetic flux density B2 of an electrical steel sheet with grooves, and then calculating it as (B2-B1) / B1. The magnetic flux density was measured as the magnitude of the magnetic flux density (B8, Tesla) induced under a magnetic field of 800A / m. The grain size, orientation difference, and subgrain boundary length of the recrystallized grains 31 in contact with the bottom of the groove in the cross section perpendicular to the rolling direction (TD plane) and other recrystallized grains 32 were measured by EBSD and summarized in Table 1 below.
[0035] Comparative Example 1 The same procedure as in Example 1 was carried out, except that the cold-rolled sheet was irradiated with a laser, and then subjected to primary recrystallization and secondary recrystallization annealing. Comparative Examples 2 and 3 The same procedure as in Example 1 was carried out, but the laser beam shape, laser energy density, and groove depth were changed as shown in Table 1 below.
[0036] [Table 1]
[0037] As shown in Table 1, when the laser shape and the laser energy density are appropriately controlled during groove formation, the orientation difference of the recrystallization 31 in contact with the bottom of the groove is low, and it can be confirmed that the core loss and magnetic flux density are excellent. On the other hand, in Comparative Example 1, the cold rolled sheet was irradiated with a laser, and it can be seen that subgrain boundaries were hardly formed, the degree of orientation was low, and the magnetic flux density was inferior. In Comparative Example 2, it can be seen that the shape and energy density of the laser were not properly adjusted, so that subgrain boundaries were hardly formed, the degree of orientation was low, and the magnetic flux density was inferior. In Comparative Example 3, it can be seen that the shape of the laser is not properly adjusted, so that subgrain boundaries are hardly formed and the magnetic flux density is inferior.
[0038] The present invention is not limited to the embodiments, but can be manufactured in various different forms, and a person skilled in the art to which the present invention pertains can understand that the present invention can be embodied in other forms without changing the technical idea or essential features of the present invention. Therefore, it should be understood that the above-described embodiments are all illustrative and not limiting. [Explanation of symbols]
[0039] 10: Grain-oriented electrical steel sheet 20: Groove 31: Secondary recrystallization abutting the bottom of the groove 32: Other secondary recrystallizations 33: Subgrain boundary 40: Metal oxide layer 50: Insulating coating
Claims
1. Grooves on the surface of the electrical steel sheet, and The recrystallized grains include recrystallized grains in contact with the grooves and other recrystallized grains not in contact with the grooves, the difference in average orientation between the recrystallized grains in contact with the grooves and the other recrystallized grains is 0.5 to 10°; The grain-oriented electrical steel sheet is characterized in that the recrystallized grains in contact with the grooves include subgrain boundaries, and each recrystallized grain in contact with the groove has a subgrain boundary having a length of 10 μm to 700 μm.
2. The grain-oriented electrical steel sheet according to claim 1 , further comprising an insulating coating abutting on the groove.
3. 3. The grain-oriented electrical steel sheet according to claim 1, wherein the groove depth is 3 to 15% of the thickness of the steel sheet, and the groove width is 10 to 50 μm.
4. preparing a cold rolled steel sheet; subjecting the cold rolled steel sheet to primary recrystallization annealing; subjecting the cold rolled steel sheet to secondary recrystallization annealing; forming a groove by irradiating a laser on a metal oxide film formed by a reaction between an oxide layer formed during the primary recrystallization annealing and MgO during the secondary recrystallization annealing process; and forming an insulating coating on the steel plate having the grooves; During the laser irradiation, the laser energy density is 2.5 to 8.0 J / mm 2 and The length of the laser beam is 100 to 450 μm and the width of the laser beam is 10 to 27 μm; the difference in average orientation between the recrystallized grains in contact with the grooves and the other recrystallized grains not in contact with the grooves is 0.5 to 10°; The recrystallized grains in contact with the grooves include subgrain boundaries, and each recrystallized grain in contact with the grooves has a subgrain boundary having a length of 10 μm to 700 μm.
5. 5. The method for refining magnetic domains in a grain-oriented electrical steel sheet according to claim 4, wherein the laser output is 500 W or more, the laser scanning speed is 5 m / s or more, and the laser scanning distance is 100 mm or more.
6. 6. The method for refining magnetic domains in a grain-oriented electrical steel sheet according to claim 4, wherein the wavelength of the laser is 1.06 to 10.6 μm.
7. 7. The method of claim 4, wherein the step of forming the insulating film comprises a step of heat treating the insulating film at a temperature of 750 to 950.degree. C.
Citation Information
Patent Citations
Method for producing grain oriented silicon steel sheet having excellent magnetic property
JP2005262217A
Directional electromagnetic steel sheet and manufacturing method therefor
JP2012031519A
Grain-oriented electrical steel sheet and method for producing the same
JP2012036446A
Grain-oriented electromagnetic steel sheet, and method for manufacturing the same
JP2012077380A
Electrical steel sheet and method for manufacturing the same
JP2015510543A