BARRIER LAMINATE FILM, METHOD FOR PRODUCING BARRIER LAMINATE FILM, AND PACKAGING MATERIAL COMPRISING BARRIER LAMINATE FILM
The barrier laminate film, with a polyester base and aluminum oxide vapor-deposited layer, addresses the challenges of gas permeation and puncture resistance, offering improved structural integrity and cost-effectiveness for packaging applications.
Patent Information
- Application Number
- JP2023092613
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-03-07
- Filing Date
- 2023-06-05
- Publication Date
- 2024-10-04
- Estimated Expiration
- 2039-03-28
AI Technical Summary
Conventional packaging materials face challenges in balancing gas barrier properties with puncture resistance and moisture resistance, particularly with nylon films that absorb moisture and have poor heat resistance, leading to increased costs due to the use of multiple plastic films.
A barrier laminate film comprising a polyester-based base material with a vapor-deposited layer of metal or inorganic compounds, featuring a loop stiffness of 0.0017N or more, a tensile strength-to-elongation ratio of 2.0 MPa/% or more, and a thickness of 16 μm to 25 μm, along with a transparent vapor-deposited layer containing aluminum oxide and a controlled transition region for improved adhesion.
The solution provides a laminate film with enhanced gas barrier properties and puncture resistance, suitable for high-temperature sterilization processes, while maintaining structural integrity and reducing material costs.
Smart Images

Figure 0007561331000001 
Figure 0007561331000002 
Figure 0007561331000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a barrier laminate film having a substrate and a vapor deposition layer provided on the substrate, and a method for producing the barrier laminate film. The present invention also relates to a packaging material including the barrier laminate film and a thermoplastic resin layer laminated on the barrier laminate film. [Background technology]
[0002] Conventionally, various packaging materials have been developed and proposed for filling and packaging various items such as food and beverages, medicines, chemicals, cosmetics, etc. Such packaging materials are required to have various physical properties depending on the purpose of packaging, the contents to be filled, the storage and distribution of the packaged product, etc. For example, one of those physical properties is gas barrier properties that prevent the transmission of oxygen, water vapor, etc.
[0003] Conventionally, various gas barrier materials that prevent the permeation of oxygen, water vapor, etc. have been developed and proposed. For example, gas barrier materials such as aluminum foil, nylon film or polyethylene terephthalate film having a coating film of polyvinylidene chloride resin, polyvinyl alcohol film, saponified film of ethylene-vinyl acetate copolymer, polyacrylonitrile resin film, etc. have been developed and proposed.
[0004] Furthermore, in recent years, transparent barrier films have been proposed that have a configuration in which a vapor-deposited layer of an inorganic oxide such as silicon oxide or aluminum oxide is provided on a plastic substrate, or a barrier film that has a vapor-deposited layer of a metal such as aluminum, etc. For example, Patent Document 1 proposes producing a barrier film by forming a vapor-deposited layer of an inorganic oxide on a nylon film. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2007-303000 A Summary of the Invention [Problem to be solved by the invention]
[0006] Packaging materials are required to have a property that prevents a packaging bag from being torn even when a sharp-edged member comes into contact with the packaging bag, that is, a so-called puncture resistance. The nylon film described in Patent Document 1 is known as a film having high puncture resistance. On the other hand, nylon is prone to absorbing moisture and has poor heat resistance. Therefore, it is difficult to use a nylon film as a film that constitutes the outer surface of a packaging material. For example, in Patent Document 1, a base film containing a polyester resin or the like is laminated on the outer surface side of the nylon film via an adhesive layer. In this way, the packaging material contains two plastic films, a nylon film and a base film, which increases the cost of the packaging material.
[0007] An object of the present invention is to provide a barrier laminate film that can effectively solve these problems. [Means for solving the problem]
[0008] The present invention provides a barrier laminate film comprising a substrate and a vapor deposition layer containing a metal or an inorganic compound and provided on the substrate, the substrate having a loop stiffness of 0.0017 N or more in a machine direction and a direction perpendicular to the machine direction and containing polyester as a main component, a value obtained by dividing the tensile strength of the substrate by the tensile elongation in at least one direction is 2.0 [MPa / %] or more, and the substrate has a thickness of 16 μm or more and 25 μm or less.
[0009] In the barrier laminate film according to the present invention, the substrate may have a puncture strength of 9.5 N or more.
[0010] The barrier laminate film according to the present invention may further comprise a gas barrier coating film provided on the vapor deposition layer.
[0011] In the barrier laminate film according to the present invention, the vapor-deposited layer may be a transparent vapor-deposited layer containing an inorganic compound.
[0012] In the barrier laminate film according to the present invention, the deposition layer is a transparent deposition layer containing aluminum oxide, and the transparent deposition layer includes a transition region, and the transition region is a region containing elementally bonded Al that is detected by etching the deposition film from the transparent deposition layer side using time-of-flight secondary ion mass spectrometry (TOF-SIMS). 2 O 4 The transition region may be between the position of the peak of H and the interface between the transparent vapor deposition layer and the first plastic film, and the ratio of the thickness of the transition region to the thickness of the transparent vapor deposition layer may be 5% or more and 60% or less.
[0013] The present invention provides a method for producing a barrier laminate film, comprising: a step of preparing a substrate; and a deposition step of depositing a metal or an inorganic compound on the substrate to form a deposition layer on the substrate, wherein the substrate has a loop stiffness of 0.0017 N or more in a machine direction and a direction perpendicular to the machine direction and contains polyester as a main component, a value obtained by dividing the tensile strength of the substrate by its tensile elongation is 2.0 [MPa / %] or more in at least one direction, and the substrate has a thickness of 16 μm or more and 25 μm or less.
[0014] The method for producing a barrier laminate film according to the present invention may further include a plasma pretreatment step of subjecting the substrate to a plasma treatment to form a plasma-treated surface on the substrate, and the deposition step may include forming the deposition layer on the plasma-treated surface of the substrate.
[0015] In the method for producing a barrier laminate film according to the present invention, the vapor deposition step may form the vapor deposition layer on the plasma-treated surface of the substrate by physical vapor deposition.
[0016] In the method for producing a barrier laminate film according to the present invention, the plasma pretreatment step includes a step of supplying a mixed gas of oxygen gas and an inert gas as a plasma raw material gas, and a mixing ratio of the oxygen gas to the inert gas (oxygen gas / inert gas) may be within a range of 6 / 1 to 1 / 1.
[0017] In the method for producing a barrier laminate film according to the present invention, the vapor deposition layer may be a transparent vapor deposition layer containing an inorganic compound, and the film production method may further include a step of applying a coating agent for a gas barrier coating film onto the vapor deposition layer and drying the applied coating agent by heating to form a gas barrier coating film.
[0018] In the method for producing a barrier laminate film according to the present invention, the gas barrier coating film may be a layer formed by coating a mixed solution of a metal alkoxide and a water-soluble polymer, and drying the coated layer by heating.
[0019] In the method for producing a barrier laminate film according to the present invention, the gas barrier coating film may be a layer formed by coating a mixed solution of a metal alkoxide, a silane coupling agent and a water-soluble polymer, and drying the coated layer by heating.
[0020] The present invention provides a packaging material comprising: a substrate; a barrier laminate film having a vapor deposition layer containing a metal or an inorganic compound provided on the substrate; and a thermoplastic resin layer laminated on the barrier laminate film, wherein the substrate has a loop stiffness of 0.0017 N or more in the machine direction and in the perpendicular direction and contains polyester as a main component, the tensile strength of the substrate divided by the tensile elongation is 2.0 [MPa / %] or more in at least one direction, and the substrate has a thickness of 16 μm or more and 25 μm or less.
[0021] The packaging material according to the present invention may be used for packaging bags for boiling or for retort sterilization. Effect of the Invention
[0022] According to the present invention, it is possible to provide a barrier laminate film having gas barrier properties and strength. [Brief description of the drawings]
[0023] [Figure 1] 1 is a cross-sectional view showing an example of a barrier laminate film according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a cross-sectional view showing another example of a barrier laminate film. [Diagram 3] FIG. 2 is a plan view showing an example of a loop stiffness measuring device. [Figure 4] FIG. 4 is a cross-sectional view of the loop stiffness measuring device of FIG. 3 taken along line VV. [Diagram 5] FIG. 1 is a diagram for explaining a process of attaching a test piece to a loop stiffness measuring device. [Figure 6] FIG. 13 is a diagram for explaining a step of forming a loop portion in a test piece. [Figure 7] FIG. 13 is a diagram for explaining a process of applying a load to a loop portion of a test piece. [Figure 8] FIG. 13 is a diagram for explaining a process of applying a load to a loop portion of a test piece. [Figure 9] FIG. 1 is a cross-sectional view showing an example of a substrate containing PBT. [Figure 10] FIG. 2 is a diagram showing an example of the results of analyzing a vapor-deposited layer of a barrier laminate film using a time-of-flight secondary ion mass spectrometer. [Figure 11] FIG. 1 is a diagram showing an example of a film forming apparatus for forming a deposition layer on a substrate. [Figure 12] FIG. 1 is a cross-sectional view showing an example of a packaging material including a barrier laminate film. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0024] Hereinafter, a barrier laminate film and a deposition apparatus for depositing a vapor-deposited layer of the barrier laminate film according to an embodiment of the present invention will be described in detail with reference to the drawings. Note that the examples are merely illustrative and do not limit the present invention in any way.
[0025] <Barrier laminate film> 1 is a cross-sectional view showing an example of a barrier laminate film 5 according to an embodiment of the present invention. The barrier laminate film 5 includes a substrate 1 and a deposition layer 2 provided on the substrate 1.
[0026] 2 is a cross-sectional view showing another example of a barrier laminate film 5 according to an embodiment of the present invention. The barrier laminate film 5 includes a substrate 1, a deposition layer 2 provided on the substrate 1, and a gas barrier coating film 3 provided on the deposition layer 2.
[0027] Although not shown, the barrier laminate film 5 may further include a printed layer provided on the substrate 1, on the deposition layer 2, or on the gas barrier coating film 3. The printed layer is a layer for indicating product information or imparting aesthetics to a packaging bag made of a packaging material 8 (described later) including the barrier laminate film 5. The printed layer expresses letters, numbers, symbols, figures, patterns, etc. As a material for forming the printed layer, ink for gravure printing or ink for flexographic printing can be used. A specific example of an ink for gravure printing is Finart manufactured by DIC Graphics Corporation.
[0028] Each of the components of the barrier laminate film 5 will now be described.
[0029] [Base material] The substrate 1 used in the barrier laminate film 5 is a polyester film containing polyester as a main component. The substrate 1 contains, for example, 51% by mass or more of polyester. The polyester is preferably a polyester mainly composed of an aromatic polyester consisting of at least one aromatic dicarboxylic acid selected from terephthalic acid, isophthalic acid, and 2,6-naphthalenedicarboxylic acid, and at least one aliphatic alcohol selected from ethylene glycol, 1,3-propanediol, and 1,4-butanediol. For example, the polyester is polyethylene terephthalate (hereinafter also referred to as PET), polybutylene terephthalate (hereinafter also referred to as PBT), etc. For example, the substrate 1 may contain 51% by mass or more of PET as a main component, or 51% by mass or more of PBT as a main component.
[0030] In order to prevent a packaging bag made of a packaging material including the barrier laminate film 5 from being torn when a sharp member having a pointed tip comes into contact with the bag, it is preferable that the substrate 1 of the barrier laminate film 5 has resistance such as puncture resistance. Therefore, in this embodiment, it is proposed to use either a high-stiffness PET film or a PBT film as the substrate 1. This can increase the puncture strength of the substrate 1, for example. For example, the puncture strength of the substrate 1 can be 9.5 N or more, more preferably 10 N or more. In addition, the ratio of the tensile strength to the tensile elongation of the substrate 1 can be increased. For example, the value obtained by dividing the tensile strength of the substrate by the tensile elongation in at least one direction is 2.0 [MPa / %] or more. This can provide the packaging material including the barrier laminate film 5 with the rigidity required to prevent the bag from being torn even when a sharp member having a pointed tip comes into contact with the packaging material.
[0031] The high stiffness PET film and the PBT film will be described in detail below. First, the high stiffness PET film will be described.
[0032] The high stiffness PET film is a stretched plastic film having a loop stiffness of 0.0017 N or more in the machine direction (MD) and the transverse direction (TD) and containing 51 mass % or more of PET. The thickness of the high stiffness PET film is preferably 5 μm or more, more preferably 7 μm or more. The thickness of the high stiffness PET film is preferably 25 μm or less, more preferably 20 μm or less.
[0033] The loop stiffness is a parameter that indicates the stiffness of a film. A method for measuring the loop stiffness will be described below with reference to Figs.
[0034] The measurement method described below can be used not only for single-layer films such as stretched plastic films, but also for films with multiple layers such as vapor-deposited films and laminated films. A vapor-deposited film is a film that includes a single-layer film and a vapor-deposited layer formed on the single-layer film, such as the above-mentioned barrier laminated film 5. A laminated film is a film that includes multiple laminated films, such as the packaging material 8 described below.
[0035] FIG. 3 is a plan view showing the test piece 40 and the loop stiffness measuring instrument 45, and FIG. 4 is a cross-sectional view of the test piece 40 and the loop stiffness measuring instrument 45 of FIG. 3 taken along line IV-IV. The test piece 40 is a rectangular film having a long side and a short side. In the present application, the length L1 of the long side of the test piece 40 is set to 150 mm, and the length L2 of the short side is set to 15 mm. As the loop stiffness measuring instrument 45, for example, No. 581 Loop Stiffness Tester (registered trademark) LOOP STIFFNESS TESTER DA type manufactured by Toyo Seiki Seisakusho Co., Ltd. can be used. The length L1 of the long side of the test piece 40 can be adjusted as long as the test piece 40 can be held by a pair of chuck parts 46 described later.
[0036] The loop stiffness measuring device 45 has a pair of chuck portions 46 for gripping a pair of ends in the long side direction of the test piece 40, and a support member 47 for supporting the chuck portions 46. The chuck portions 46 include a first chuck 461 and a second chuck 462. In the state shown in FIG. 3 and FIG. 4, the test piece 40 is placed on the pair of first chucks 461, and the second chuck 462 does not yet grip the test piece 40 between the first chuck 461 and the second chuck 462. As will be described later, during measurement, the test piece 40 is gripped between the first chuck 461 and the second chuck 462 of the chuck portions 46. The second chuck 462 may be connected to the first chuck 461 via a hinge mechanism.
[0037] When a film to be measured, such as a stretched plastic film, a vapor-deposited film, or a laminated film, is available in a state before the film is processed into a packaged product, the test piece 40 may be prepared by cutting the film to be measured. Also, the test piece 40 may be prepared by cutting a packaged product made of a packaging material, such as a bag, and taking out the film to be measured.
[0038] A method for measuring the loop stiffness of the test piece 40 using the loop stiffness measuring device 45 will be described. First, as shown in FIG. 3 and FIG. 4, the test piece 40 is placed on the first chuck 461 of a pair of chuck parts 46 arranged with a gap L3 therebetween. In the present application, the gap L3 is set so that the length of the loop part 41 (hereinafter also referred to as the loop length) described later is 60 mm. The test piece 40 includes an inner surface 40x located on the first chuck 461 side and an outer surface 40y located on the opposite side of the inner surface 40x. When the test piece 40 is made of a packaging material, the inner surface 40x and the outer surface 40y of the test piece 40 coincide with the inner surface and the outer surface of the packaging material. Next, as shown in FIG. 5, the second chuck 462 is placed on the test piece 40 so as to grip the end of the long side direction of the test piece 40 between the first chuck 461 and the second chuck 462.
[0039] Next, as shown in FIG. 6, at least one of the pair of chucks 46 is slid on the support member 47 in a direction in which the distance between the pair of chucks 46 is reduced. This allows the loop portion 41 to be formed in the test piece 40. The test piece 40 shown in FIG. 6 has the loop portion 41, a pair of intermediate portions 42, and a pair of fixing portions 43. The pair of fixing portions 43 are portions of the test piece 40 that are gripped by the pair of chucks 46. The pair of intermediate portions 42 are portions of the test piece 40 that are located between the loop portion 41 and the pair of intermediate portions 42. As shown in FIG. 6, the chuck portion 46 is slid on the support member 47 until the inner surfaces 40x of the pair of intermediate portions 42 come into contact with each other. This allows the loop portion 41 having a loop length of 60 mm to be formed. The loop length of the loop portion 41 is the length of the test piece 40 between position P1 where the surface of one second chuck 462 on the loop portion 41 side intersects with the test piece 40, and position P2 where the surface of the other second chuck 462 on the loop portion 41 side intersects with the test piece 40. When the thickness of the test piece 40 is ignored, the above-mentioned interval L3 is a value obtained by adding 2×t to the length of the loop portion 41, where t is the thickness of the second chuck 462 of the chuck portion 46.
[0040] Then, as shown in FIG. 7, the posture of the chuck portion 46 is adjusted so that the protruding direction Y of the loop portion 41 relative to the chuck portion 46 is horizontal. For example, the posture of the chuck portion 46 supported by the support member 47 is adjusted by moving the support member 47 so that the normal direction of the support member 47 is horizontal. In the example shown in FIG. 7, the protruding direction Y of the loop portion 41 coincides with the thickness direction of the chuck portion. Also, the load cell 48 is prepared at a position separated by a distance Z1 from the second chuck 462 in the protruding direction Y of the loop portion 41. In this application, the distance Z1 is set to 50 mm. Next, the load cell 48 is moved at a speed V by a distance Z2 shown in FIG. 7 toward the loop portion 41 of the test piece 40. The distance Z2 is set so that the load cell 48 contacts the loop portion 41 and then pushes the loop portion 41 toward the chuck portion 46 side, as shown in FIG. 7 and FIG. 8. In this application, the distance Z2 is set to 40 mm. In this case, the distance Z3 between the load cell 48 and the second chuck 462 of the chuck portion 46 when the load cell 48 is pressing the loop portion 41 towards the chuck portion 46 is 10 mm. The speed V at which the load cell 48 is moved was set to 3.3 mm / sec.
[0041] 8, the load cell 48 is moved by a distance Z2 toward the chuck portion 46, and in a state in which the load cell 48 is pressing into the loop portion 41 of the test piece 40, the value of the load applied to the load cell 48 from the loop portion 41 becomes stable, and then the value of the load is recorded. The value of the load thus obtained is used as the loop stiffness of the film constituting the test piece 40. In this application, unless otherwise specified, the environment during the measurement of the loop stiffness is a temperature of 23°C and a relative humidity of 50%.
[0042] The preferred mechanical properties of the high stiffness PET film will now be further described. The puncture strength of the high stiffness PET film is preferably 9.5 N or more, and more preferably 10.0 N or more.
[0043] The tensile strength of the high stiffness PET film in the machine direction is preferably 250 MPa or more, more preferably 280 MPa or more.The tensile strength of the high stiffness PET film in the perpendicular direction is preferably 250 MPa or more, more preferably 280 MPa or more. The tensile elongation of the high stiffness PET film in the machine direction is preferably 130% or less, more preferably 120% or less, and the tensile elongation of the high stiffness PET film in the perpendicular direction is preferably 120% or less, more preferably 110% or less. As described above, the tensile strength of the high stiffness PET film divided by the tensile elongation in at least one direction is preferably 2.0 [MPa / %] or more. For example, the tensile strength of the high stiffness film divided by the tensile elongation in the transverse direction (TD) is preferably 2.0 [MPa / %] or more, more preferably 2.2 [MPa / %] or more. The tensile strength of the high stiffness film divided by the tensile elongation in the machine direction (MD) is preferably 1.8 [MPa / %] or more, more preferably 2.0 [MPa / %] or more. The tensile strength and tensile elongation can be measured in accordance with JIS K7127. As a measuring instrument, a tensile tester STA-1150 manufactured by Orientec Co., Ltd. can be used. As a test piece, a rectangular film cut from a high stiffness PET film having a width of 15 mm and a length of 150 mm can be used. The distance between a pair of chucks holding the test piece at the start of the measurement is 100 mm, and the tensile speed is 300 mm / min. The environmental temperature during the test is 25°C, and the relative humidity is 50%. The tensile strength and tensile elongation of the barrier laminate film 5 having a high stiffness PET film, the tensile strength and tensile elongation of the PBT film, and the tensile strength and tensile elongation of the barrier laminate film 5 having a PBT film are also measured in the same manner as in the case of the high stiffness PET film.
[0044] The heat shrinkage of the high stiffness PET film in the machine direction is preferably 0.7% or less, more preferably 0.5% or less. The heat shrinkage of the high stiffness PET film in the perpendicular direction is preferably 0.7% or less, more preferably 0.5% or less. The heating temperature for measuring the heat shrinkage is 100°C, and the heating time is 40 minutes. The Young's modulus of the high stiffness PET film in the machine direction is preferably 4.0 GPa or more, more preferably 4.5 MPa or more, and the Young's modulus of the high stiffness PET film in the perpendicular direction is preferably 4.0 GPa or more, more preferably 4.5 GPa or more.
[0045] In the manufacturing process of the high stiffness PET film, for example, first, a PET film obtained by melting and molding polyethylene terephthalate is stretched 3 to 4.5 times in the machine direction and the perpendicular direction at 90°C to 145°C in a first stretching step. Then, a plastic film is stretched 1.1 to 3.0 times in the machine direction and the perpendicular direction at 100°C to 145°C in a second stretching step. Then, heat setting is performed at a temperature of 190°C to 220°C. Then, relaxation treatment (treatment to reduce the film width) of about 0.2% to 2.5% is performed at a temperature of 100°C to 190°C in the machine direction and the perpendicular direction. In these steps, a high stiffness PET film having the above-mentioned mechanical properties can be obtained by adjusting the stretch ratio, stretching temperature, heat setting temperature, and relaxation treatment rate.
[0046] Next, preferred mechanical properties of the barrier laminate film 5 having the above-mentioned high stiffness PET film as the substrate 1 will be further described. The loop stiffness of the barrier laminate film 5 in both the machine direction (MD) and the transverse direction (TD) is preferably 0.0017 N or more. The puncture strength of the barrier laminate film 5 is preferably 9.5 N or more, and more preferably 10.0 N or more. The tensile strength of the barrier laminate film 5 in the machine direction is preferably 250 MPa or more, more preferably 280 MPa or more. The tensile strength of the barrier laminate film 5 in the perpendicular direction is preferably 250 MPa or more, more preferably 280 MPa or more. The tensile elongation of the barrier laminate film 5 in the machine direction is preferably 130% or less, more preferably 120% or less. The tensile elongation of the barrier laminate film 5 in the perpendicular direction is preferably 120% or less, more preferably 110% or less. Preferably, in at least one direction, the value of the tensile strength of the barrier laminate film 5 divided by the tensile elongation is 2.0 [MPa / %] or more. For example, the value of the tensile strength of the barrier laminate film 5 divided by the tensile elongation in the transverse direction (TD) is preferably 2.0 [MPa / %] or more, more preferably 2.2 [MPa / %] or more. The value of the tensile strength of the barrier laminate film 5 divided by the tensile elongation in the machine direction (MD) is preferably 1.8 [MPa / %] or more, more preferably 2.0 [MPa / %] or more. The thermal shrinkage of the barrier laminate film 5 in the machine direction is preferably 0.7% or less, more preferably 0.5% or less. The thermal shrinkage of the barrier laminate film 5 in the perpendicular direction is preferably 0.7% or less, more preferably 0.5% or less. The heating temperature for measuring the thermal shrinkage is 100°C, and the heating time is 40 minutes. The Young's modulus of the barrier laminate film 5 in the machine direction is preferably 4.0 GPa or more, more preferably 4.5 MPa or more. The Young's modulus of the barrier laminate film 5 in the perpendicular direction is preferably 4.0 GPa or more, more preferably 4.5 GPa or more.
[0047] The PET constituting the high stiffness PET film may contain biomass-derived PET. In this case, the high stiffness PET film may be composed only of biomass-derived PET. Alternatively, the high stiffness PET film may be composed of biomass-derived PET and fossil fuel-derived PET. By containing biomass-derived PET in the high stiffness PET film, the amount of fossil fuel-derived PET can be reduced compared to the conventional method, so that carbon dioxide emissions can be reduced and environmental load can be reduced. Note that the biomass-derived PET has ethylene glycol derived from biomass as a diol unit and terephthalic acid derived from fossil fuel as a dicarboxylic acid unit. The fossil fuel-derived PET has ethylene glycol derived from fossil fuel as a diol unit and terephthalic acid derived from fossil fuel as a dicarboxylic acid unit.
[0048] Carbon dioxide in the atmosphere contains a certain proportion of C14 (105.5 pMC), so it is known that the C14 content in plants that grow by absorbing carbon dioxide from the atmosphere, such as corn, is also about 105.5 pMC. It is also known that fossil fuels contain almost no C14. Therefore, the proportion of carbon derived from biomass can be calculated by measuring the proportion of C14 in the total carbon atoms in PET. In the present invention, the "biomass degree" indicates the weight ratio of biomass-derived components. Taking PET as an example, PET is a polymer of ethylene glycol containing 2 carbon atoms and terephthalic acid containing 8 carbon atoms in a molar ratio of 1:1. When only biomass-derived ethylene glycol is used as the PET ethylene glycol, the weight ratio of biomass-derived components in PET is 31.25%, so the theoretical value of the biomass degree of PET is 31.25%. Specifically, the mass of PET is 192, of which the mass derived from biomass-derived ethylene glycol is 60, so 60÷192×100=31.25. In addition, the weight ratio of biomass-derived components in PET derived from fossil fuels is 0%, and the biomass degree of PET derived from fossil fuels is 0%. In the present invention, the biomass degree of the high stiffness PET film is preferably 5.0% or more, and more preferably 10.0% or more. In addition, the biomass degree of the high stiffness PET film is preferably 30.0% or less.
[0049] Biomass-derived ethylene glycol is made from ethanol (biomass ethanol) produced from biomass as a raw material. For example, biomass-derived ethylene glycol can be obtained by a method of producing ethylene glycol from biomass ethanol via ethylene oxide using a conventionally known method. Examples of raw materials for biomass ethanol include corn, sugarcane, beet, and manioc. Commercially available biomass ethylene glycol may also be used, and for example, biomass ethylene glycol commercially available from India Glycoal Limited can be suitably used. The biomass ethylene glycol from India Glycoal Limited is made from sugarcane molasses as a raw material.
[0050] Next, the PBT film will be described. The PBT film is a stretched plastic film containing 51% by mass or more of PBT. The advantages of the base material 1 containing PBT will be described below.
[0051] PBT has excellent heat resistance. Therefore, when a packaging bag for containing contents such as food is subjected to a boiling treatment or a retort treatment, the substrate 1 can be prevented from being deformed or the strength of the substrate 1 can be prevented from being reduced. The retort treatment is a treatment in which the contents are filled into the packaging bag, the packaging bag is sealed, and then the packaging bag is heated under pressure using steam or heated hot water. The temperature of the retort treatment is, for example, 120°C or higher. The boiling treatment is a treatment in which the contents are filled into the bag 10, the bag 10 is sealed, and then the bag 10 is heated in a water bath under atmospheric pressure. The temperature of the boiling treatment is, for example, 90°C or higher and 100°C or lower.
[0052] In addition, PBT has high strength. Therefore, the packaging bag can have puncture resistance, similarly to the case where the packaging material 8 constituting the packaging bag contains nylon. The puncture strength of the PBT film is preferably 9.5 N or more, and more preferably 10.0 N or more.
[0053] The tensile strength of the PBT film in the machine direction is preferably 150 MPa or more, more preferably 180 MPa or more, and the tensile strength of the PBT film in the perpendicular direction is preferably 250 MPa or more, more preferably 280 MPa or more. The tensile elongation of the PBT film in the machine direction is preferably 220% or less, more preferably 200% or less, and the tensile elongation of the PBT film in the perpendicular direction is preferably 120% or less, more preferably 110% or less. Preferably, the value of the tensile strength of the PBT film divided by the tensile elongation in at least one direction is 2.0 [MPa / %] or more. For example, the value of the tensile strength of the PBT film divided by the tensile elongation in the perpendicular direction (TD) is preferably 2.0 [MPa / %] or more, more preferably 2.2 [MPa / %] or more, and even more preferably 2.5 [MPa / %] or more.
[0054] In addition, PBT has the property of being less resistant to moisture absorption than nylon. Therefore, even if the base material 1 containing PBT is disposed on the outer surface of the packaging material 8, it is possible to prevent the base material 1 from absorbing moisture, which would result in a decrease in the laminate strength of the packaging material 8.
[0055] Next, preferred mechanical properties of the barrier laminate film 5 having the above-mentioned PBT film as the substrate 1 will be further described. The puncture strength of the barrier laminate film 5 is preferably 9.5 N or more, and more preferably 10.0 N or more. The tensile strength of the barrier laminate film 5 in the machine direction is preferably 150 MPa or more, more preferably 180 MPa or more.The tensile strength of the barrier laminate film 5 in the perpendicular direction is preferably 250 MPa or more, more preferably 280 MPa or more. The tensile elongation of the barrier laminate film 5 in the machine direction is preferably 220% or less, more preferably 200% or less. The tensile elongation of the barrier laminate film 5 in the perpendicular direction is preferably 120% or less, more preferably 110% or less. Preferably, in at least one direction, the value obtained by dividing the tensile strength of the barrier laminate film 5 by the tensile elongation is 2.0 [MPa / %] or more. For example, the value obtained by dividing the tensile strength of the barrier laminate film 5 by the tensile elongation in the perpendicular direction (TD) is preferably 2.0 [MPa / %] or more, more preferably 2.2 [MPa / %] or more, and further preferably 2.5 [MPa / %] or more.
[0056] The structure of the PBT-containing substrate 1 will be described in detail below. In the present embodiment, the PBT-containing substrate 1 may have either the first structure or the second structure described below.
[0057] [First configuration of the substrate containing PBT] The content of PBT in the base material 1 according to the first configuration is preferably 51% by mass or more, more preferably 60% by mass or more, even more preferably 70% by mass or more, particularly preferably 75% by mass or more, and most preferably 80% by mass or more. By making the content of PBT 51% by mass or more, the base material 1 can have excellent impact strength and pinhole resistance.
[0058] The PBT used as the main constituent preferably contains 90 mol % or more, more preferably 95 mol % or more, even more preferably 98 mol % or more, and most preferably 100 mol % of terephthalic acid as a dicarboxylic acid component, and preferably contains 90 mol % or more, more preferably 95 mol % or more, even more preferably 97 mol % or more of 1,4-butanediol as a glycol component, and most preferably contains no by-products other than those generated by ether bonds of 1,4-butanediol during polymerization.
[0059] The substrate 1 may contain a polyester resin other than PBT. This makes it possible to adjust the film formability and the mechanical properties of the substrate 1 when the film-like substrate 1 is biaxially stretched, for example. Examples of polyester resins other than PBT include polyester resins such as PET, polyethylene naphthalate (PEN), polybutylene naphthalate (PBN), and polypropylene terephthalate (PPT), as well as PBT resins copolymerized with dicarboxylic acids such as isophthalic acid, orthophthalic acid, naphthalenedicarboxylic acid, biphenyl dicarboxylic acid, cyclohexane dicarboxylic acid, adipic acid, azelaic acid, and sebacic acid, and PBT resins copolymerized with diol components such as ethylene glycol, 1,3-propylene glycol, 1,2-propylene glycol, neopentyl glycol, 1,5-pentanediol, 1,6-hexanediol, diethylene glycol, cyclohexanediol, polyethylene glycol, polytetramethylene glycol, and polycarbonate diol.
[0060] The amount of the polyester resin other than PBT added is preferably 49% by mass or less, more preferably 40% by mass or less. If the amount of the polyester resin other than PBT added exceeds 49% by mass, the mechanical properties of PBT may be impaired, and impact strength, pinhole resistance, and draw formability may become insufficient.
[0061] The substrate 1 may contain, as an additive, a polyester-based or polyamide-based elastomer obtained by copolymerizing at least one of a soft polyether component, a polycarbonate component, and a polyester component. This can improve pinhole resistance when bent. The amount of additive added is, for example, 20% by mass. If the amount of additive added exceeds 20% by mass, the effect of the additive may become saturated, or the transparency of the substrate 1 may decrease.
[0062] An example of a method for producing the film-like substrate 1 according to the first configuration will be described. Here, a method for producing the film-like substrate 1 by a casting method will be described. More specifically, a method in which resins of the same composition are cast in multiple layers during casting will be described.
[0063] Since PBT has a high crystallization rate, crystallization also progresses during casting. If PBT is cast in a single layer without being multi-layered, there is no barrier to suppress the growth of the crystals, so the crystals grow to a large size, and the yield stress of the resulting unstretched raw material increases. This makes the unstretched raw material more likely to break when biaxially stretched. In addition, the yield stress of the resulting biaxially stretched film increases, which may result in insufficient formability of the biaxially stretched film. In contrast, if the same resin is multi-layered during casting, the stretching stress of the unstretched sheet can be reduced, allowing stable biaxial stretching and lowering the yield stress of the resulting biaxially stretched film, resulting in a flexible film with high breaking strength.
[0064] FIG. 9 is a cross-sectional view showing an example of the layer structure of the substrate 1. When the substrate 1 is produced by casting a resin in a multi-layered form, as shown in FIG. 9, the substrate 1 is made of a multi-layer structure including a plurality of layers 1a. Each of the plurality of layers 1a contains PBT as a main component. For example, each of the plurality of layers 1a contains preferably 51% by mass or more of PBT, more preferably 60% by mass or more of PBT. In addition, in the plurality of layers 1a, the n+1th layer 1a is directly laminated on the nth layer 1a. In other words, no adhesive layer or adhesive layer is interposed between the plurality of layers 1a.
[0065] The reason why multi-layering improves the properties of PBT film is presumed to be as follows. When resins are layered, even if the resin composition is the same, there is an interface between the layers, and this interface accelerates crystallization. On the other hand, the growth of large crystals that exceed the thickness of the layers is suppressed. This is thought to result in a smaller size of the crystals (spherulites).
[0066] As a specific method for reducing the size of spherulites by multi-layering, a general multi-layering device (such as a multi-layer feed block, a static mixer, or a multi-layer multi-manifold) can be used. For example, a method can be used in which thermoplastic resins sent out from different flow paths using two or more extruders are laminated in multiple layers using a feed block, a static mixer, a multi-manifold die, or the like. When resins of the same composition are multi-layered, it is also possible to use only one extruder and introduce the above-mentioned multi-layering device into the melt line from the extruder to the die.
[0067] The substrate 1 is made of a multilayer structure including at least 10 layers 1a, preferably 60 layers or more, more preferably 250 layers or more, and even more preferably 1000 layers or more. By increasing the number of layers, the size of the spherulites in the PBT in the unstretched raw roll can be reduced, and the subsequent biaxial stretching can be stably performed. In addition, the yield stress of the PBT in the biaxially stretched film state can be reduced. Preferably, the diameter of the spherulites in the PBT in the unstretched raw roll is 500 nm or less.
[0068] When an unstretched raw PBT is biaxially stretched to produce a biaxially stretched film, the stretching temperature in the longitudinal stretching direction (hereinafter, MD) (hereinafter, also referred to as MD stretching temperature) is preferably 40° C. or higher, more preferably 45° C. or higher. By setting the MD stretching temperature at 40° C. or higher, it is possible to prevent the film from breaking. In addition, the MD stretching temperature is preferably 100° C. or lower, more preferably 95° C. or lower. By setting the MD stretching temperature at 100° C. or lower, it is possible to prevent the phenomenon in which the biaxially stretched film does not become oriented.
[0069] The stretching ratio in MD (hereinafter also referred to as MD stretching ratio) is preferably 2.5 times or more. This allows the biaxially stretched film to be oriented, and good mechanical properties and uniform thickness can be achieved. The MD stretching ratio is, for example, 5 times or less.
[0070] The stretching temperature in the transverse stretching direction (hereinafter also referred to as TD) (hereinafter also referred to as TD stretching temperature) is preferably 40° C. or higher. By setting the TD stretching temperature at 40° C. or higher, it is possible to prevent the film from breaking. In addition, the TD stretching temperature is preferably 100° C. or lower. By setting the TD stretching temperature at 100° C. or lower, it is possible to prevent the phenomenon in which the biaxially stretched film does not become oriented.
[0071] The stretching ratio in TD (hereinafter also referred to as TD stretching ratio) is preferably 2.5 times or more. This allows the biaxially stretched film to be oriented, and good mechanical properties and uniform thickness can be achieved. The stretching ratio in MD is, for example, 5 times or less.
[0072] The TD relaxation ratio is preferably 0.5% or more. This can prevent the biaxially stretched PBT film from breaking during heat setting. The TD relaxation ratio is preferably 10% or less. This can prevent the biaxially stretched PBT film from becoming slack and causing thickness unevenness.
[0073] The thickness of the layer 1a of the substrate 1 shown in Fig. 9 is preferably 3 nm or more, more preferably 10 nm or more, and is preferably 200 nm or less, more preferably 100 nm or less. The thickness of the substrate 1 is preferably 9 μm or more, more preferably 12 μm or more. The thickness of the substrate 1 is preferably 25 μm or less, more preferably 20 μm or less. By making the thickness of the substrate 1 9 μm or more, the substrate 1 has sufficient strength. By making the thickness of the substrate 1 25 μm or less, the substrate 1 exhibits excellent formability. Therefore, the process of manufacturing a packaging bag by processing the packaging material 8 including the substrate 1 can be efficiently carried out.
[0074] [Second configuration of the substrate containing PBT] The substrate 1 according to the second configuration is made of a monolayer film containing a polyester having butylene terephthalate as the main repeating unit. For example, the substrate 1 contains a homo- or copolymer-type polyester obtained by condensing 1,4-butanediol or its ester-forming derivative as a glycol component and terephthalic acid or its ester-forming derivative as a dibasic acid component. The content of PBT in the substrate 1 according to the second configuration is preferably 51% by mass or more, more preferably 60% by mass or more, even more preferably 70% by mass or more, even more preferably 80% by mass or more, and most preferably 90% by mass or more. In addition, the substrate 1 according to the second configuration is preferably composed of only polybutylene terephthalate and additives.
[0075] In order to impart mechanical strength to the substrate 1, it is preferable for the PBT to have a melting point of 200° C. or more and 250° C. or less and an IV value (intrinsic viscosity) of 1.10 dl / g or more and 1.35 dl / g or less. It is particularly preferable for the PBT to have a melting point of 215° C. or more and 225° C. or less and an IV value of 1.15 dl / g or more and 1.30 dl / g or less. These IV values may be satisfied by the entire material constituting the substrate 1. The IV value can be calculated based on JIS K 7367-5:2000.
[0076] The substrate 1 according to the second configuration may contain a polyester resin other than PBT, such as PET, in the range of 30% by mass or less. By containing PET in addition to PBT, the crystallization of PBT can be suppressed, and the stretchability of the PBT film can be improved. As the PET to be blended with the PBT of the substrate 1, a polyester having ethylene terephthalate as the main repeating unit can be used. For example, a homotype having ethylene glycol as the glycol component and terephthalic acid as the dibasic acid component as the main components can be preferably used. In order to impart good mechanical strength properties, PET having a melting point of 240°C or more and 265°C or less and an IV value of 0.55 dl / g or more and 0.90 dl / g or less is preferable. Furthermore, PET having a melting point of 245°C or more and 260°C or less and an IV value of 0.60 dl / g or more and 0.80 dl / g or less is particularly preferable. By making the blending amount of PET 30% by mass or less, it is possible to prevent the rigidity of the unstretched raw material and the stretched film from becoming too high. This makes it possible to prevent the stretched film from becoming brittle, which leads to a decrease in the pressure resistance, impact strength, puncture strength, etc. of the stretched film. It is also possible to prevent the occurrence of poor stretching when stretching the unstretched raw material.
[0077] The substrate 1 may contain additives such as lubricants, antiblocking agents, inorganic fillers, antioxidants, UV absorbers, antistatic agents, flame retardants, plasticizers, colorants, crystallization inhibitors, and crystallization accelerators, as necessary. In order to prevent a decrease in viscosity due to hydrolysis during heat melting, the polyester resin pellets used as the raw material for the substrate 1 are preferably used after being sufficiently pre-dried so that the moisture content is 0.05% by weight or less, preferably 0.01% by weight or less, before heat melting.
[0078] An example of a method for producing the film-like substrate 1 according to the second configuration will be described.
[0079] In order to stably produce the film of the substrate 1 having the above-mentioned configuration, it is important to suppress the growth of crystals in the unstretched raw roll. Specifically, when the extruded PBT melt is cooled to form a film, the crystallization temperature range of the polymer is cooled at a certain rate or higher, that is, the raw roll cooling rate is an important factor. The raw roll cooling rate is, for example, 200 ° C / sec or higher, preferably 250 ° C / sec or higher, and particularly preferably 350 ° C / sec or higher. The unstretched raw roll formed into a film at a high cooling rate maintains a low crystallinity state, so the stability of the bubble during stretching is improved. Furthermore, high-speed film formation is also possible, so the productivity of the film is also improved. If the cooling rate is less than 200 ° C / sec, the crystallinity of the obtained unstretched raw roll is considered to be high and the stretchability is considered to be reduced. In addition, in extreme cases, the stretching bubble may burst and the stretching may not continue.
[0080] The unstretched raw material containing PBT as a main component is preferably transported to the space where the biaxial stretching is performed while maintaining the atmospheric temperature at 25° C. or less, preferably at 20° C. or less. This makes it possible to maintain the crystallinity of the unstretched raw material immediately after film formation even if the residence time is long.
[0081] The biaxial stretching method for stretching the unstretched raw sheet to obtain a stretched film is not particularly limited. For example, the film may be stretched in the longitudinal direction and the transverse direction simultaneously by the tubular method or the tenter method, or may be stretched in the longitudinal direction and the transverse direction successively. Among these, the tubular method is particularly preferably used since it can obtain a stretched film having a good balance of physical properties in the circumferential direction.
[0082] In the tubular method, the unstretched raw film introduced into the stretching space is passed between a pair of low-speed nip rolls, and then heated by a stretching heater while air is forced into the nip rolls. After the stretching is completed, air is blown onto the stretched film by a cooling shoulder air ring. In consideration of the stretching stability and the strength properties, transparency, and thickness uniformity of the stretched film, the stretching ratio is preferably 2.7 times or more and 4.5 times or less in MD and TD. By setting the stretching ratio to 2.7 times or more, the tensile modulus and impact strength of the stretched film can be sufficiently secured. In addition, by setting the stretching ratio to 4.5 times or less, excessive strain of the molecular chain due to stretching can be suppressed, and the occurrence of breakage or puncture during stretching can be suppressed, so that the stretched film can be stably produced.
[0083] The stretching temperature is preferably 40°C or higher and 80°C or lower, and particularly preferably 45°C or higher and 65°C or lower. Since the unstretched raw film produced at the above-mentioned high cooling rate has low crystallinity, the unstretched raw film can be stably stretched even when the stretching temperature is relatively low. In addition, by setting the stretching temperature to 80°C or lower, the vibration of the stretching bubble can be suppressed, and a stretched film with good thickness accuracy can be obtained. In addition, by setting the stretching temperature to 40°C or higher, excessive stretch-oriented crystallization due to low-temperature stretching can be suppressed, and whitening of the film can be prevented.
[0084] The substrate 1 produced as described above is composed of a single layer containing polyester having butylene terephthalate as a main repeating unit, for example. According to the above-mentioned production method, the unstretched raw fabric is formed at a high cooling rate, so that even if the unstretched raw fabric is composed of a single layer, it can maintain a low crystallinity, and therefore the unstretched raw fabric can be stably stretched.
[0085] The base material 1 contains PBT, which can increase the heat resistance of the barrier laminate film 5 and the packaging material 8 containing the barrier laminate film 5. For example, the tensile modulus of the barrier laminate film 5 and the packaging material 8 can be sufficiently increased. In particular, the tensile modulus of the barrier laminate film 5 and the packaging material 8 in a high-temperature atmosphere, for example, an atmosphere of 100°C (hereinafter also referred to as hot tensile modulus) can be sufficiently increased.
[0086] [Vapour-deposited layer] Next, the deposition layer 2 will be described.
[0087] The deposition layer 2 is a thin film having a gas barrier property that prevents or blocks the transmission of oxygen gas, water vapor, and the like. The deposition layer 2 may be a metal layer containing a metal having a light-shielding property such as aluminum, or may be a transparent deposition layer formed of a transparent inorganic compound. For example, the deposition layer 2 is a transparent deposition layer formed of a transparent inorganic oxide.
[0088] Hereinafter, the case where the deposition layer 2 is a transparent deposition layer will be described. The inorganic oxide forming the deposition layer 2 contains, as a main component, an aluminum compound, such as at least aluminum oxide or aluminum nitride, carbide, or hydroxide, either alone or in combination. For example, the inorganic oxide contains aluminum oxide as a main component. The deposition layer 2 may be a layer containing a silicon compound as a main component. For example, the inorganic oxide layer contains silicon oxide (silicon oxide) as a main component. Furthermore, the deposition layer 2 may be a layer containing an aluminum compound such as the above-mentioned aluminum oxide as a main component, and further containing a metal oxide such as silicon oxide, silicon nitride, silicon oxynitride, silicon carbide, magnesium oxide, titanium oxide, tin oxide, indium oxide, zinc oxide, zirconium oxide, or the like, or a nitride or carbide of these metals, or a mixture thereof.
[0089] The thickness of the deposition layer 2 is preferably 3 nm or more and 50 nm or less, and more preferably 9 nm or more and 30 nm or less.
[0090] (Gas barrier coating film) The gas barrier coating film 3 serves to mechanically and chemically protect the vapor-deposited layer 2 when the vapor-deposited layer 2 is a transparent vapor-deposited layer, and to improve the barrier properties of the barrier laminate film 5, and is laminated so as to be in contact with the vapor-deposited layer 2. The gas barrier coating film 3 is a cured film formed from a coating agent for gas barrier coating films, which is made of a resin composition containing a metal alkoxide, a hydroxyl-containing water-soluble resin, and a silane coupling agent added as necessary.
[0091] The mass ratio of the hydroxyl-containing water-soluble resin to the metal alkoxide in the resin composition is preferably 5 / 95 or more and 20 / 80 or less, and more preferably 8 / 92 or more and 15 / 85 or less. If it is smaller than the above range, the barrier effect of the barrier coating layer tends to be insufficient, and if it is larger than the above range, the rigidity and brittleness of the barrier coating layer tends to be large.
[0092] The thickness of the gas barrier coating film 3 is preferably 100 nm or more and 800 nm or less. If it is thinner than the above range, the barrier effect of the gas barrier coating film 3 tends to be insufficient, and if it is thicker than the above range, the rigidity and brittleness tend to be high.
[0093] Metal alkoxides are represented by the general formula R 1 nM(OR 2 )m (wherein, R 1 , R 2 represents a hydrogen atom or an organic group having 1 to 8 carbon atoms, M represents a metal atom, n represents an integer of 0 or more, m represents an integer of 1 or more, and n+m represents the atomic valence of M. 1 , R 2 may be the same or different. ) · · · (I).
[0094] Specific examples of metal atoms represented by M in the metal alkoxide include silicon, zirconium, titanium, aluminum, tin, lead, borane, and the like. For example, it is preferable to use an alkoxysilane in which M is Si (silicon).
[0095] In the above general formula (I), OR 2 Specific examples of the alkyl group include alkoxy groups such as a hydroxyl group, a methoxy group, an ethoxy group, an n-propoxy group, an n-butoxy group, an i-propoxy group, a butoxy group, a 3-methacryloxy group, a 3-acryloxy group, and a phenoxy group, and the like.
[0096] In the above, R 1 Specific examples of the alkyl group include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, a phenyl group, a p-styryl group, a 3-chloropropyl group, a trifluoromethyl group, a vinyl group, a γ-glycidoxypropyl group, a methacryl group, and a γ-aminopropyl group.
[0097] Specific examples of alkoxysilanes include tetramethoxysilane, tetraethoxysilane, tetrapropoxysilane, tetraisopropoxysilane, tetrabutoxysilane, tetraphenoxysilane, methyltrimethoxysilane, methyltriethoxysilane, methyltripropoxysilane, methyltributoxysilane, methyltriphenoxysilane, phenylphenoxysilane, ethyltrimethoxysilane, ethyltriethoxysilane, dimethyldimethoxysilane, dimethyldiethoxysilane, n-propyltrimethoxysilane, n-propyltriethoxysilane, isopropyltrimethoxysilane, isopropyltriethoxysilane, dimethyldiethoxysilane, and diphenyldimethoxysilane. Examples of the alkoxysilane include various alkoxysilanes and phenoxysilanes such as silane, diphenyldiethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, phenyltrimethoxysilane, phenyltriethoxysilane, p-styryltrimethoxysilane, 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropylmethyldiethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropyltriethoxysilane, 3-acryloxypropyltrimethoxysilane, 3-acryloxypropyltriethoxysilane, 3-chloropropyltriethoxysilane, trifluoromethyltrimethoxysilane, and 1,6-bis(trimethoxysilyl)hexane. In the present embodiment, condensation polymers of these alkoxysilanes can also be used, and specifically, for example, polytetramethoxysilane, polytetraethoxysilane, etc. can be used.
[0098] The silane coupling agent is used to adjust the crosslink density of the cured film made of the metal alkoxide and the hydroxyl group-containing water-soluble resin, thereby providing the film with barrier properties and resistance to hot water treatment.
[0099] The silane coupling agent has the general formula: 3 nSi(OR 4 )4-n ···(II) (In the formula, R 3 and R 4each independently represents an organic functional group, and n is 1 to 3. It is expressed as:
[0100] In the above general formula (II), R 3 Examples of R include a hydrocarbon group such as an alkyl group or an alkylene group, an epoxy group, a (meth)acryloxy group, a ureido group, a vinyl group, an amino group, an isocyanurate group, or a functional group having an isocyanate group. 3 At least one of R is preferably a functional group having an epoxy group, and more preferably a 3-glycidoxypropyl group and a 2-(3,4-epoxycyclohexyl) group. 3 may be the same or different.
[0101] In the above general formula (II), R 4 is, for example, an organic functional group having 1 to 8 carbon atoms, preferably an alkyl group having 1 to 8 carbon atoms, which may have a branch, or an alkoxyalkyl group having 3 to 7 carbon atoms. For example, examples of the alkyl group having 1 to 8 carbon atoms include a methyl group, an ethyl group, an n-propyl group, an i-propyl group, an n-butyl group, and a sec-butyl group. Examples of the alkoxyalkyl group having 3 to 7 carbon atoms include a group in which one hydrogen atom has been removed from a straight-chain or branched-chain ether, such as methyl ethyl ether, diethyl ether, methyl propyl ether, methyl isopropyl ether, ethyl propyl ether, ethyl isopropyl ether, methyl butyl ether, ethyl butyl ether, methyl sec-butyl ether, ethyl sec-butyl ether, methyl tert-butyl ether, and ethyl tert-butyl ether. Note that (OR 4 ) may be the same or different.
[0102] Examples of the silane coupling agent represented by the above general formula (II) include 3-glycidoxypropyltrimethoxysilane and 3-glycidoxypropyltriethoxysilane when n = 1. Examples of the silane coupling agent include 3-glycidoxypropylmethyldimethoxysilane and 3-glycidoxypropylmethyldiethoxysilane when n = 2, and 3-glycidoxypropyldimethylmethoxysilane, 3-glycidoxypropyldimethylethoxysilane, 2-(3,4-epoxycyclohexyl)dimethylmethoxysilane, and 2-(3,4-epoxycyclohexyl)dimethylethoxysilane when n = 3.
[0103] In particular, the crosslink density of the cured film of the barrier coating layer using 3-glycidoxypropylmethyldimethoxysilane and 3-glycidoxypropylmethyldiethoxysilane is lower than that of the system using trialkoxysilane. Therefore, the cured film has excellent gas barrier properties and hot water treatment resistance, while also being flexible and has excellent bending resistance, so that the gas barrier properties of the packaging material using the barrier film are unlikely to deteriorate even after the Gelbo flex test.
[0104] The silane coupling agent may be a mixture of those where n=1, 2, or 3, and the ratio of the amounts and the amount of the silane coupling agent used are determined depending on the design of the cured film of the barrier coating layer.
[0105] The hydroxyl-containing water-soluble resin is capable of dehydration co-condensation with the metal alkoxide, and the saponification degree is preferably 90% or more and 100% or less, more preferably 95% or more and 100% or less, and even more preferably 99% or more and 100% or less. If the saponification degree is smaller than the above range, the hardness of the barrier coating layer is likely to decrease.
[0106] Specific examples of the hydroxyl group-containing water-soluble resin include polyvinyl alcohol resins, ethylene-vinyl alcohol copolymers, and polymers of bifunctional phenolic compounds and bifunctional epoxy compounds, each of which may be used alone, or may be used in combination of two or more, or may be used as copolymers. Among these, polyvinyl alcohol is particularly preferred because of its excellent flexibility and affinity, and polyvinyl alcohol resins are suitable.
[0107] Specifically, for example, a polyvinyl alcohol resin obtained by saponifying polyvinyl acetate, or an ethylene-vinyl alcohol copolymer obtained by saponifying a copolymer of ethylene and vinyl acetate can be used. Examples of such polyvinyl alcohol-based resins include PVA-124 (saponification degree = 99%, polymerization degree = 2,400) manufactured by Kuraray Co., Ltd. and GOHSENOL NM-14 (saponification degree = 99%, polymerization degree = 1,400) manufactured by Nippon Synthetic Chemical Industry Co., Ltd.
[0108] (Preferable Structure of Barrier Laminate Film) Next, a preferred configuration of the barrier laminate film 5 in the thickness direction when the vapor-deposited layer 2 is a transparent vapor-deposited layer containing aluminum oxide will be described with reference to Fig. 10. Fig. 10 shows the results of measuring ions derived from the vapor-deposited layer 2 containing aluminum oxide and ions derived from the substrate 1 using time-of-flight secondary ion mass spectrometry (TOF-SIMS) while repeatedly soft-etching the surface of the barrier laminate film 5 on the side of the gas barrier coating film 3 at a constant speed with a Cs (cesium) ion gun. The vapor-deposited layer 2 of the barrier laminate film 5 includes a transition region identified by the graph analysis diagram shown in Fig. 10.
[0109] The transition region is an elemental bond Al that is transformed into aluminum hydroxide, which is detected by etching the barrier laminate film 5 from the gas barrier coating film 3 side using TOF-SIMS. 2 O 4 Position of the peak of H T 2 and the interface T between the deposition layer 2 and the substrate 11 The interface T between the deposition layer 2 and the substrate 1 is the region between the deposition layer 2 and the substrate 1. 1 is element C 6 The intensity of the graph is the intensity of element C in substrate 1. 6 In FIG. 10, the symbol W 1 represents the thickness of the transition region.
[0110] Thickness W of the transition region relative to the thickness of deposition layer 2 1 The ratio (hereinafter also referred to as the transformation rate of the transition region) is preferably 5% or more and 60% or less. By setting the transformation rate to 5% or more and 60% or less, it is possible to suppress the degradation of the barrier property of the barrier laminate film 5 against water vapor when a sterilization treatment such as boiling treatment or retort treatment is performed on a packaging material including the barrier laminate film 5. The retort treatment is a treatment in which a packaging bag made of a packaging material including the barrier laminate film 5 is filled with contents, the packaging bag is sealed, and then the packaging bag is heated under pressure. The temperature of the retort treatment is, for example, 120°C or more. The boiling treatment is a treatment in which a packaging bag is filled with contents, the packaging bag is sealed, and then the packaging bag is heated in a water bath under atmospheric pressure. The temperature of the boiling treatment is, for example, 90°C or more and 100°C or less. In addition, a packaging material including a barrier laminate film 5 having a transformation rate in the transition region of 5% or more and 60% or less can effectively function in maintaining its barrier properties against gases such as oxygen and water vapor even when used in packaging bags for applications in which sterilization treatments such as boiling treatment or retort treatment are not performed.
[0111] The interface between the substrate 1 and the vapor-deposited layer 2 is subjected to mechanical and chemical stress due to heat. Therefore, in order to prevent a decrease in adhesion and barrier properties, it is important to firmly coat the substrate 1 with the vapor-deposited layer 2 at the interface between the substrate 1 and the vapor-deposited layer 2.
[0112] Aluminum hydroxide has good adhesion to plastic films such as polyester film due to its chemical structure, and because it forms a dense network of its own, it has high water vapor barrier properties. However, the bond structure based on hydrogen bonds between the aluminum hydroxide and the plastic film is easily broken down microscopically by heat stress. In addition, water molecules easily penetrate into the aluminum hydroxide network due to the affinity between the grain boundaries of the aluminum hydroxide.
[0113] In this embodiment, in order to narrow as much as possible the transition region at the interface between the substrate 1 and the aluminum hydroxide in the deposition layer 2 containing aluminum oxide, the element bond Al 2 O 4 By focusing on H and controlling its abundance, the element-bonded Al 2 O 4 The aim is to suppress the generation of aluminum hydroxide from H and increase the ratio of the aluminum oxide layer, which contains relatively little aluminum hydroxide, thereby suppressing microscopic destruction of the deposition layer 2 caused by water molecules due to thermal stress and destruction of the interface with the plastic film. This makes it possible to provide a barrier laminate film 5 with unprecedented adhesion and barrier properties.
[0114] The deposition layer 2 containing aluminum oxide can be formed by forming the deposition layer 2 on the surface of the substrate 1 that has been pretreated with oxygen plasma. As the deposition method for forming the deposition layer 2, various deposition methods can be applied from among physical deposition and chemical deposition. As the physical deposition method, a method can be selected from the group consisting of deposition, sputtering, ion plating, ion beam assisted deposition, and cluster ion beam deposition, and as the chemical deposition method, a method can be selected from the group consisting of plasma CVD, plasma polymerization, thermal CVD, and catalytic reaction CVD. In this embodiment, the deposition method of physical deposition is preferable.
[0115] A specific example of a method for obtaining the graph in Fig. 10 will be described. First, etching is performed from the outermost surface of the gas barrier coating film 3 using Cs, and analysis is performed on element bonds at the interfaces between the gas barrier coating film 3, the deposition layer 2, and a film such as the substrate 1, and on element bonds in the deposition layer 2. This allows the graph shown in Fig. 10 to be obtained.
[0116] Next, a specific example of a method for analyzing the graph in Fig. 10 will be described. Here, a case where the gas barrier coating film 3 contains silicon oxide will be described.
[0117] First, in the graph, SiO, which is a constituent element of the gas barrier coating film 3, 2 The position where the strength of the gas barrier coating film 3 (mass number 59.96) is half that of the gas barrier coating film 3 is specified as the interface between the gas barrier coating film 3 and the deposition layer 2. 6 The position where the intensity of (mass number 72.00) is half that of the substrate 1 is identified as the interface between the substrate 1 and the deposited layer 2. The distance in the thickness direction between the two interfaces is used as the thickness of the deposited layer 2.
[0118] Next, the measured elemental bond Al 2 O 4 The peak of H (mass number 118.93) is obtained, and the region from the peak to the interface is defined as the transition region. 2 O 4 If it is composed of a material with the same mass number as H (mass number 118.93), it is necessary to separate the waveform of 118.93.
[0119] At the interface between the gas barrier coating film 3 and the deposition layer 2, a reactant AlSiO 4 and Al hydroxide 2 O 4 When H and H are generated, they and Al present at the interface between the substrate 1 and the deposition layer 2 are 2 O 4 In this manner, the separation of the waveforms can be appropriately handled depending on the material of the gas barrier coating film 3.
[0120] In waveform separation, for example, a profile of mass number 118.93 obtained by TOF-SIMS is subjected to nonlinear curve fitting using a Gaussian function, and overlapping peaks are separated using the least squares Levenberg-Marquardt algorithm.
[0121] The above analysis is based on the assumption that the barrier laminate film 5 includes the substrate 1, the deposition layer 2, and the gas barrier coating film 3, but the same analysis can be applied to the case where the barrier laminate film 5 includes the substrate 1 and the deposition layer 2 but does not include the gas barrier coating film 3. Even when the barrier laminate film 5 does not include the gas barrier coating film 3, by setting the conversion rate of the transition region of the deposition layer 2 within a predetermined range, it is possible to suppress a decrease in the barrier properties of the barrier laminate film 5 against water vapor when a packaging material including the barrier laminate film 5 is subjected to a sterilization treatment such as boiling or retort treatment. When the barrier laminate film 5 includes the substrate 1 and the deposition layer 2 and etching is performed from the deposition layer 2 side using time-of-flight secondary ion mass spectrometry (TOF-SIMS), it is preferable that the conversion rate of the transition region of the deposition layer 2 is 45% or less.
[0122] <Method of manufacturing the barrier laminate film> Next, an example of a method for producing the barrier laminate film 5 will be described.
[0123] First, a substrate 1 is prepared. Then, a deposition layer 2 containing aluminum oxide is formed on the surface of the substrate 1. Fig. 11 is a diagram showing an example of a film forming apparatus 60. The film forming apparatus 60 and a film forming method using the film forming apparatus 60 will be described below.
[0124] 11, in the film formation apparatus 60, partition walls 85a to 85c are formed in the decompression chamber 62. The partition walls 85a to 85c form the substrate transfer chamber 62A, the plasma pretreatment chamber 62B, and the film formation chamber 62C, and in particular, the plasma pretreatment chamber 62B and the film formation chamber 62C are formed as spaces surrounded by the partition walls and the partition walls 85a to 85c, and each chamber further has an exhaust chamber formed therein as necessary.
[0125] The plasma pretreatment chamber 62B and the plasma pretreatment process in the plasma pretreatment chamber 62B will be described. In the plasma pretreatment chamber 62B, a plasma pretreatment roller 70 that transports the substrate 1 to be pretreated and enables plasma treatment is provided so as to be partially exposed to the substrate transport chamber 62A. The substrate 1 is transported to the plasma pretreatment chamber 62B while being wound up.
[0126] The plasma pretreatment chamber 62B and the film formation chamber 62C are provided adjacent to the substrate transport chamber 62A, and the substrate 1 can be moved without being exposed to the atmosphere. The pretreatment chamber 62B and the substrate transport chamber 62A are connected by a rectangular hole, through which a part of the plasma pretreatment roller 70 protrudes to the substrate transport chamber 62A side, and a gap is opened between the wall of the transport chamber and the pretreatment roller 70, and the substrate 1 can be moved from the substrate transport chamber 62A to the film formation chamber 62C through the gap. The same structure is also formed between the substrate transport chamber 62A and the film formation chamber 62C, and the substrate 1 can be moved without being exposed to the atmosphere.
[0127] The substrate transport chamber 62A is provided with a winding roller as a winding means for winding up the substrate 1 having the deposition layer 2 formed on one side, which has been moved again to the substrate transport chamber 12A by the deposition roller 75, into a roll, so that the substrate 1 having the deposition layer 2 formed thereon can be wound up.
[0128] When producing a barrier laminate film 5 having a vapor-deposited layer 2 containing aluminum oxide, the plasma pretreatment chamber 62B is configured to separate the space where plasma is generated from other regions and to efficiently evacuate the opposing space, which facilitates control of plasma gas concentration and improves productivity. The pretreatment pressure formed by reducing the pressure can be set and maintained at about 0.1 Pa to 100 Pa, and in particular, the treatment pressure of the oxygen plasma pretreatment is preferably 1 to 20 Pa to achieve a preferred conversion rate in the transition region of the vapor-deposited layer 2 containing aluminum oxide.
[0129] The transport speed of the substrate 1 is not particularly limited, but from the viewpoint of production efficiency, it can be at least 200 to 1000 m / min. In particular, the transport speed for oxygen plasma pretreatment is preferably 300 to 800 m / min in order to obtain a conversion rate in the transition region of the deposition layer 2 containing aluminum oxide.
[0130] The plasma pretreatment roller 70 constituting the plasma pretreatment device is intended to prevent the substrate 1 from shrinking or being damaged by heat during plasma treatment by the plasma pretreatment means, and to apply oxygen plasma P uniformly and widely to the substrate 1. It is preferable that the pretreatment roller 70 can be adjusted to a constant temperature between -20°C and 100°C by adjusting the temperature of a temperature control medium circulating inside the pretreatment roller.
[0131] The plasma pretreatment means includes a plasma supply means and a magnetic forming means, and cooperates with the plasma pretreatment roller 70 to confine the oxygen plasma P near the surface of the substrate 1.
[0132] The plasma pretreatment means is provided so as to cover a part of the pretreatment roller 70. Specifically, the plasma supply means 72 and the magnetic field forming means 73 constituting the plasma pretreatment means are arranged along the surface near the outer periphery of the pretreatment roller 70. The plasma supply means 72 includes a plasma supply nozzle that supplies plasma raw material gas. The magnetic field forming means 73 has a magnet or the like to promote the generation of plasma P. The plasma pretreatment means also has an electrode 71 to which a voltage is applied between the pretreatment roller 70. Note that, in FIG. 11, an example is shown in which the electrode 71 and the plasma supply means 72 are separate members, but this is not limiting. Although not shown, the electrode 71 and the plasma supply means 72 may be configured by an integrated member.
[0133] By generating plasma P in the space between the pretreatment roller 70 and the magnetic forming means 73 and forming an area of high plasma density near the pretreatment roller 70 and the surface of the substrate 1, oxygen plasma pretreatment can be performed on the inner surface of the substrate 1 to form a plasma-treated surface.
[0134] The plasma supply means 72 of the plasma pretreatment means includes a raw material gas volatilization supply device 68 connected to a plasma supply nozzle provided outside the decompression chamber 62, and a raw material gas supply line for supplying raw material gas from the device. The plasma raw material gas to be supplied is oxygen alone or a mixed gas of oxygen gas and an inert gas, which is supplied from a gas reservoir through a flow rate controller while the flow rate of the gas is measured. The inert gas may be one or a mixed gas of two or more kinds selected from the group consisting of argon, helium, and nitrogen.
[0135] These gases are mixed at a predetermined ratio as necessary to form a plasma raw material gas alone or a mixed gas for plasma formation, which is then supplied to the plasma supply means. The single gas or mixed gas is supplied to the plasma supply nozzle of the plasma supply means, and supplied to the vicinity of the outer periphery of the pretreatment roller 70 where the supply port of the plasma supply nozzle opens. The nozzle opening is directed toward the substrate 1 on the pretreatment roller 70, and is arranged and configured so that oxygen plasma P can be diffused and supplied uniformly to the entire surface of the substrate 1. This allows uniform plasma pretreatment to be performed on a large area of the substrate 1.
[0136] In order to set the conversion rate of the transition region of the deposition layer 2 containing aluminum oxide to 5% or more and 60% or less as described above, the mixture ratio of oxygen gas and the inert gas (oxygen gas / inert gas) in the oxygen plasma pretreatment is preferably 6 / 1 to 1 / 1, more preferably 5 / 2 to 3 / 2. By setting the mixture ratio to 6 / 1 to 1 / 1, the film formation energy of the deposition layer 2 on the substrate 1 increases, and by setting it to 5 / 2 to 3 / 2, aluminum hydroxide is formed near the interface of the substrate 1, i.e., the conversion rate of the transition region decreases.
[0137] The electrode 71 functions as a counter electrode for the pretreatment roller 70. The plasma raw material gas supplied is excited by a potential difference due to a high-frequency voltage, a low-frequency voltage, or the like supplied between the electrode 71 and the pretreatment roller 70, and plasma P is generated and supplied.
[0138] Specifically, the electrode 71 is provided with a plasma pretreatment roller as a plasma power source, and an AC voltage with a frequency of 10 Hz to 2.5 GHz is applied between the opposing electrode, and input power control or impedance control or the like is performed to make it possible to apply any voltage between the electrode 71 and the plasma pretreatment roller 70. The film forming apparatus 60 is provided with a power source 82 capable of applying a bias voltage that makes the oxygen plasma P, which can physically or chemically modify the surface properties of the substrate 1, a positive potential.
[0139] The plasma intensity per unit area is preferably 50 to 8000 W·sec / m2 50W·sec / m 2 Below this, no effect of plasma pretreatment was observed, and below 8000W·sec / m 2 Above this level, the substrate 1 is prone to degradation due to the plasma, such as wear, damage, discoloration, and sintering. In particular, the plasma intensity per unit area is 100 to 1000 W·sec / m 2 By applying a bias voltage perpendicular to the substrate 1 and applying the above-mentioned plasma intensity, it is possible to stably improve the adhesion to the deposition layer 2 containing aluminum oxide.
[0140] The magnetic forming means 73 may be one in which an insulating spacer and a base plate are provided inside a magnet case, and a magnet is provided on the base plate. An insulating shield plate may be provided on the magnet case, and an electrode may be attached to the insulating shield plate. The magnet case and the electrode are electrically insulated, and even if the magnet case is installed and fixed inside the reduced pressure chamber 62, the electrode can be at an electrically floating level. By providing a magnet, reactivity in the vicinity of the surface of the substrate 1 is increased, making it possible to form a good plasma pre-treated surface at high speed.
[0141] Preferably, the magnet is configured so that the magnetic flux density at the surface of the substrate 1 is 10 Gauss to 10,000 Gauss. If the magnetic flux density at the surface of the substrate 1 is 10 Gauss or more, it becomes possible to sufficiently increase the reactivity in the vicinity of the surface of the substrate 1, and a good pre-treated surface can be formed at high speed.
[0142] Next, the film formation chamber 62C and the film formation process in the film formation chamber 62C will be described. The film formation apparatus 60 has a film formation roller 75 arranged in the reduced pressure film formation chamber 62C and a target of a vapor deposition film formation means 74 arranged opposite to the film formation roller 75. The film formation roller 75 wraps around the substrate 1 and transports it with the treated surface of the substrate 1, which has been pretreated in the plasma pretreatment device, facing outward. In the film formation process, the target of the vapor deposition film formation means 74 is evaporated to form an aluminum oxide film on the surface of the substrate 1.
[0143] The vapor deposition film forming means 74 is, for example, a resistance heating type, and uses an aluminum metal wire as an aluminum evaporation source, and supplies oxygen to oxidize the aluminum vapor while forming a vapor deposition layer 2 containing aluminum oxide on the surface of the substrate 1.
[0144] The thickness of the deposited layer 2 containing aluminum oxide formed as described above is preferably 3 to 50 nm, and more preferably 9 to 30 nm. Within this range, the barrier properties can be maintained. However, if the deposited layer 2 containing aluminum oxide is very thin, it becomes difficult to calculate the transformation rate of the transition region by TOF-SIMS measurement.
[0145] Next, a method for forming the gas barrier coating film 3 on the vapor deposition layer 2 will be described. First, the above-mentioned metal alkoxide, a silane coupling agent, a hydroxyl group-containing water-soluble resin, a reaction accelerator (a sol-gel catalyst, an acid, etc.), and an organic solvent such as water as a solvent, or an alcohol such as methyl alcohol, ethyl alcohol, or isopropanol, are mixed together to prepare a coating agent for a gas barrier coating film made of a resin composition.
[0146] When the gas barrier coating film 3 contains a silane coupling agent, the coating agent for the gas barrier coating film may be prepared as follows. First, a metal alkoxide such as an alkoxysilane is mixed with a silane coupling agent. The metal alkoxide and the silane coupling agent are preferably mixed at 10°C or less. This makes it easier for the film structure of the gas barrier coating film 3 to be formed to be dense. Next, the mixture of the metal alkoxide and the silane coupling agent is mixed with a hydroxyl group-containing water-soluble resin such as a polyvinyl alcohol resin.
[0147] After preparing the coating agent for gas barrier coating film, the coating agent for gas barrier coating film is applied on the deposition layer 2 by a conventional method and dried. This drying step further advances the condensation or co-condensation reaction to form a coating film. The above coating operation may be further repeated on the first coating film to form multiple coating films consisting of two or more layers.
[0148] Further, the substrate is heat-treated for 3 seconds to 10 minutes at a temperature in the range of 20 to 200° C., preferably 50 to 180° C., and at a temperature not higher than the softening point of the resin constituting the substrate 1. This makes it possible to form a gas barrier coating film 3 made of the coating agent for gas barrier coating film on the deposition layer 2. In this manner, a barrier laminate film 5 having the substrate 1, the deposition layer 2, and the gas barrier coating film 3 can be produced.
[0149] <Packaging materials> Next, the packaging material 8 for forming a packaging bag will be described. The packaging material 8 includes the above-mentioned barrier laminate film 5 and a thermoplastic resin layer 7 laminated on the barrier laminate film 5. In the example shown in Fig. 12, the thermoplastic resin layer 7 is laminated on the surface of the barrier laminate film 5 facing the deposition layer 2 via an adhesive layer 6. The thermoplastic resin layer 7 forms the inner surface of the packaging material 8 (the inner surface of the packaging bag formed by the packaging material 8). Although not shown, a printed layer may be provided between the barrier laminate film 5 and the adhesive layer 6.
[0150] (thermoplastic resin layer) The thermoplastic resin layer 7 may be any resin layer or film that can melt and be fused to each other by heat. For example, it is preferable to use a resin or film made of one or more of low-density polyethylene, medium-density polyethylene, high-density polyethylene, linear low-density polyethylene, polypropylene, polymethylpentene, polystyrene, ethylene-vinyl acetate copolymer, α-olefin copolymer, ionomer resin, ethylene-acrylic acid copolymer, ethylene-ethyl acrylate copolymer, ethylene-methyl methacrylate copolymer, ethylene-propylene copolymer, elastomer, etc., and among these, since it is the layer that comes into contact with the contents such as food, it is more preferable to use a resin or film made of one or more olefin-based resins such as polyethylene and polypropylene, which have excellent hygiene, heat resistance, chemical resistance and aroma retention. The thickness is preferably 3 μm or more and 100 μm or less, and more preferably 15 μm or more and 70 μm or less. The thermoplastic resin layer 7 is preferably made of an unstretched film. The term "unstretched" is a concept that includes not only a film that is not stretched at all, but also a film that is slightly stretched due to tension applied during film formation.
[0151] A packaging bag made of the packaging material 8 may be subjected to a sterilization treatment such as boiling or retort treatment at high temperatures. The thermoplastic resin layer 7 is preferably made of a material having heat resistance sufficient to withstand such high temperature treatments.
[0152] (Other Aspects) Another aspect of the present invention is a barrier laminate film comprising a substrate and a vapor deposition layer containing a metal or an inorganic compound provided on the substrate, the substrate containing polyester as a main component, and a value obtained by dividing the tensile strength of the substrate by its tensile elongation in at least one direction is 2.0 [MPa / %] or more.
[0153] In the barrier laminate film according to another aspect of the present invention, the substrate may have a puncture strength of 9.5 N or more.
[0154] In the barrier laminate film according to another embodiment of the present invention, the substrate may have a loop stiffness of 0.0017 N or more in the machine direction and in the perpendicular direction, and may contain polyester as a main component.
[0155] In the barrier laminate film according to another aspect of the present invention, the substrate may contain polybutylene terephthalate as a main component.
[0156] The barrier laminate film according to another embodiment of the present invention may further comprise a gas barrier coating film provided on the vapor deposition layer.
[0157] In the barrier laminate film according to another aspect of the present invention, the vapor deposition layer may be a transparent vapor deposition layer containing an inorganic compound.
[0158] In another embodiment of the barrier laminate film of the present invention, the deposition layer is a transparent deposition layer containing aluminum oxide, and the transparent deposition layer includes a transition region, and the transition region is an elemental bond Al that is detected by etching the deposition film from the transparent deposition layer side using time-of-flight secondary ion mass spectrometry (TOF-SIMS). 2 O 4 The transition region may be between the position of the peak of H and the interface between the transparent vapor deposition layer and the first plastic film, and the ratio of the thickness of the transition region to the thickness of the transparent vapor deposition layer may be 5% or more and 60% or less.
[0159] Another aspect of the present invention is a method for producing a barrier laminate film, comprising: a step of preparing a substrate; and a deposition step of depositing a metal or an inorganic compound onto the substrate to form a deposition layer on the substrate, wherein the substrate contains polyester as a main component, and a value obtained by dividing the tensile strength of the substrate by its tensile elongation in at least one direction is 2.0 [MPa / %] or more.
[0160] The method for producing a barrier laminate film according to another aspect of the present invention may further include a plasma pretreatment step of subjecting the substrate to a plasma treatment to form a plasma-treated surface on the substrate, and the deposition step may form the deposition layer on the plasma-treated surface of the substrate.
[0161] In the method for producing a barrier laminate film according to another aspect of the present invention, the vapor deposition step may form the vapor deposition layer on the plasma-treated surface of the substrate by physical vapor deposition.
[0162] In the method for producing a barrier laminate film according to another aspect of the present invention, the plasma pretreatment step includes a step of supplying a mixed gas of oxygen gas and an inert gas as a plasma raw material gas, and a mixing ratio of the oxygen gas to the inert gas (oxygen gas / inert gas) may be within a range of 6 / 1 to 1 / 1.
[0163] In the method for producing a barrier laminate film according to another aspect of the present invention, the deposition layer is a transparent deposition layer containing an inorganic compound, and the film production method may further include a step of applying a coating agent for a gas barrier coating film onto the deposition layer and drying the applied coating agent by heating to form a gas barrier coating film.
[0164] In the method for producing a barrier laminate film according to another embodiment of the present invention, the gas barrier coating film may be a layer formed by coating a mixed solution of a metal alkoxide and a water-soluble polymer, and drying the mixture by heating.
[0165] In the method for producing a barrier laminate film according to another embodiment of the present invention, the gas barrier coating film may be a layer formed by coating a mixed solution of a metal alkoxide, a silane coupling agent and a water-soluble polymer, and drying the mixture by heating.
[0166] Another aspect of the present invention is a packaging material comprising: a substrate; a barrier laminate film having a vapor deposition layer containing a metal or an inorganic compound provided on the substrate; and a thermoplastic resin layer laminated on the barrier laminate film, wherein the substrate contains polyester as a main component, and the value of the tensile strength of the substrate divided by the tensile elongation in at least one direction is 2.0 [MPa / %] or more.
[0167] In the packaging material according to another embodiment of the present invention, the packaging material may be used for a packaging bag for boiling or a packaging bag for retort sterilization. EXAMPLES
[0168] Next, the present invention will be described more specifically with reference to examples. However, the present invention is not limited to the description of the following examples as long as it does not depart from the gist of the present invention.
[0169] [Example A1] As the substrate 1, a high-stiffness PET film having a loop stiffness of 0.0017 N or more and made of petroleum-derived PET was prepared. Specifically, XP-55 manufactured by Toray Industries, Inc. was used as the high-stiffness PET film. The thickness of the high-stiffness PET film was 16 μm. The measured value of the loop stiffness of the high-stiffness PET film was 0.0021 N in both the machine direction and the perpendicular direction. The Young's modulus of the high-stiffness PET film in the machine direction was 4.8 GPa, and the Young's modulus of the high-stiffness polyester film in the perpendicular direction was 4.7 GPa. The tensile strength of the high stiffness PET film in the machine direction was 292 MPa, and the tensile strength of the high stiffness polyester film in the perpendicular direction was 257 MPa. The tensile elongation of the high stiffness PET film in the machine direction was 107%, and the tensile elongation of the high stiffness polyester film in the perpendicular direction was 102%. In this case, the tensile strength of the high stiffness PET film in the machine direction divided by the tensile elongation was 2.73 [MPa / %], and the tensile strength of the high stiffness PET film in the perpendicular direction divided by the tensile elongation was 2.52 [MPa / %]. The heat shrinkage of the high stiffness PET film in both the machine direction and the perpendicular direction was 0.4%.
[0170] Next, the puncture strength of the high stiffness PET film was measured in accordance with JIS Z1707 7.4. A & D Tensilon universal material testing machine RTC-1310 was used as the measuring device. Specifically, a semicircular needle with a diameter of 1.0 mm and a tip radius of 0.5 mm was pierced from the outer surface 30y side of the test piece of the high stiffness PET film in a fixed state at a speed of 50 mm / min (50 mm per minute), and the maximum value of the stress until the needle penetrated the high stiffness PET film was measured. The maximum value of the stress was measured for five or more test pieces, and the average value was taken as the puncture strength of the high stiffness PET film. The environment during the measurement was a temperature of 23 ° C and a relative humidity of 50%. As a result, the puncture strength was 10.2 N.
[0171] [Example A2] As the substrate 1, a PBT film including multiple layers and produced by a casting method, as described in the first configuration above, was prepared. The PBT content in each layer was 80%, the number of layers was 1024, and the thickness of the PBT film was 15 μm. The tensile strength of the PBT film in the machine direction was 191 MPa, and the tensile strength of the PBT film in the perpendicular direction was 289 MPa. The tensile elongation of the PBT film in the machine direction was 195%, and the tensile elongation of the PBT film in the perpendicular direction was 100%. In this case, the value obtained by dividing the tensile strength of the PBT film in the machine direction by the tensile elongation was 0.98 [MPa / %], and the value obtained by dividing the tensile strength of the PBT film in the perpendicular direction by the tensile elongation was 2.89 [MPa / %]. The thermal shrinkage of the PBT film in both the machine direction and the perpendicular direction was 0.4%.
[0172] [Example B1] An example in which a vapor-deposited layer 2 is formed on a substrate 1, and a gas-barrier coating film 3 is formed on the vapor-deposited layer 2 to produce a barrier laminate film 5 will be described.
[0173] First, a roll of the high stiffness PET film having a thickness of 16 μm used in the above-mentioned Example A1 was prepared as the substrate 1. Next, the substrate 1 was subjected to an oxygen plasma treatment using the above-mentioned film-forming apparatus 60 shown in FIG. 11, and then a deposition layer 2 containing aluminum oxide and having a thickness of 12 nm was formed on the oxygen plasma-treated surface. The oxygen plasma treatment and film-forming treatment will be described in detail below.
[0174] In the oxygen plasma treatment, plasma was introduced from the plasma supply nozzle 72 under the following conditions in the plasma pretreatment chamber 62B onto the surface of the substrate 1 on which the deposition layer 2 was to be formed, and the substrate 1 transported at a transport speed of 400 m / min was subjected to plasma pretreatment. As a result, an oxygen plasma-treated surface was formed on the surface of the substrate 1 on which the deposition layer 2 was to be formed. [Oxygen plasma pretreatment conditions] Plasma intensity: 200W·sec / m 2 Plasma formation gas ratio: oxygen / argon=2 / 1 Voltage applied between pretreatment drum and plasma supply nozzle: 340V Vacuum level in pre-treatment area: 3.8Pa
[0175] In the film formation process, in the film formation chamber 62C into which the substrate 1 continuously transported from the plasma pretreatment chamber 62B is carried in, a deposition layer 2 containing aluminum oxide having a thickness of 12 nm is formed on the substrate 1 by vacuum deposition using aluminum as a target on the oxygen plasma treated surface of the substrate 1. A reactive resistance heating method is adopted as the heating means for the vacuum deposition method. The film formation conditions are as follows. [Aluminum oxide film formation conditions] ·Vacuum degree: 8.1×10 -2 Pa -Conveying speed: 400m / min Oxygen gas supply: 20,000sccm
[0176] Subsequently, a gas barrier coating film 3 was formed on the deposition layer 2. Specifically, first, 385 g of water, 67 g of isopropyl alcohol, and 9.1 g of 0.5N hydrochloric acid were mixed and the solution was adjusted to pH 2.2, and 175 g of tetraethoxysilane as a metal alkoxide and 9.2 g of glycidoxypropyltrimethoxysilane as a silane coupling agent were mixed into the solution while cooling to 10° C. to prepare solution A. Solution B was prepared by mixing 14.7 g of polyvinyl alcohol having a polymerization degree of 2400 and a saponification degree of 99% or more as a water-soluble polymer, 324 g of water, and 17 g of isopropyl alcohol. Subsequently, the liquid A and the liquid B were mixed in a weight ratio of 6.5:3.5. The solution thus obtained was used as a coating agent for a gas barrier coating film.
[0177] The gas barrier coating film coating agent prepared above was coated by spin coating onto the deposition layer 2. Then, the coating was heated in an oven at 180° C. for 60 seconds to form a gas barrier coating film 3 having a thickness of about 400 nm on the deposition layer 2. In this manner, a barrier laminate film 5 having the substrate 1, the deposition layer 2, and the gas barrier coating film 3 was obtained.
[0178] For the barrier laminate film 5 of Example B1, the conversion rate, oxygen permeability, water vapor permeability and loop stiffness were measured.
[0179] (Metamorphic rate) In a vacuum environment, the surface of the gas barrier coating film 3 of the barrier laminate film 5 was repeatedly soft-etched at a constant rate with a Cs (cesium) ion gun, while ions derived from the gas barrier coating film 3, ions derived from the deposition layer 2, and ions derived from the substrate 1 were measured using time-of-flight secondary ion mass spectrometry (TOF-SIMS). 6 (mass number 72.00), Al derived from the aluminum oxide deposition film of deposition layer 2 2 O 4 Mass analysis of H (mass number 118.93) ions was performed.
[0180] The time-of-flight secondary ion mass spectrometer used in the TOF-SIMS was a TOF.SIMS5 manufactured by ION TOF, Inc., and measurements were performed under the following measurement conditions, resulting in the graph shown in FIG. (TOFSIMS measurement conditions) Primary ion type: Bi 3 ++(0.2pA,100μs) ·Measurement area: 150×150μm 2 Etching gun type: Cs (1keV, 60nA) Etching area: 600×600μm 2 Etching rate: 3sec / cycle Vacuum time: 1×10 -6>15 hours at <mbar Measurements using a time-of-flight secondary ion mass spectrometer were carried out within 30 hours after starting evacuation.
[0181] In the graph, SiO, which is a constituent element of the gas barrier coating film 3, 2 The position where the strength of the gas barrier coating film 3 (mass number 59.96) is half that of the gas barrier coating film 3 was specified as the interface between the gas barrier coating film 3 and the deposition layer 2. 6 The position where the intensity of the ion beam (mass number 72.00) was half that of the substrate 1 was identified as the interface between the substrate 1 and the deposited layer 2. The distance in the thickness direction between the two interfaces was used as the thickness of the deposited layer 2.
[0182] Next, the measured elemental bond Al 2 O 4 A peak representing H (mass number 118.93) was obtained, and the region from the peak to the interface was defined as the transition region. 2 O 4 If it is composed of a material with the same mass number as H (mass number 118.93), it is necessary to separate the waveform of 118.93.
[0183] At the interface between the gas barrier coating film 3 and the deposition layer 2, a reactant AlSiO 4 and Al hydroxide 2 O 4 When H and H are generated, they and Al present at the interface between the substrate 1 and the deposition layer 2 are 2 O 4 In this manner, the separation of the waveforms can be appropriately handled depending on the material of the gas barrier coating film 3.
[0184] In waveform separation, for example, a profile of mass number 118.93 obtained by TOF-SIMS may be subjected to nonlinear curve fitting using a Gaussian function, and overlapping peaks may be separated using the least squares Levenberg-Marquardt algorithm.
[0185] Two samples were prepared from the barrier laminate film 5 of Example B1, and the transformation rate of the deposition layer 2 of each of the two samples was calculated as follows (thickness W of the transition region). 1 The conversion rate was calculated as follows: (a) the conversion rate of the first sample was 36.2%, and (b) the conversion rate of the second sample was 28.8%.
[0186] (Loop Stiffness) The above-mentioned rectangular test piece 40 was prepared from the barrier laminate film 5 of Example B1, and the loop stiffness in the machine direction and the perpendicular direction was measured. The measuring device used was a Loop Stiffness Tester (registered trademark) No. 581 LOOP STIFFNESS TESTER DA type manufactured by Toyo Seiki Seisakusho. The environment during the measurement was a temperature of 23°C and a relative humidity of 50%. As a result, the loop stiffness in the machine direction of the barrier laminate film 5 was 0.0021 N, and the loop stiffness in the perpendicular direction was 0.0.0021 N.
[0187] (Oxygen permeability) The barrier laminate film 5 prepared as described above and a 60 μm-thick unstretched polypropylene film (CPP film) were bonded together by a dry lamination method using a two-component curing polyurethane adhesive to prepare a packaging material 8. As the CPP film, an unstretched polypropylene film ZK207 manufactured by Toray Advanced Film Co., Ltd. was used.
[0188] Next, the packaging material 8 was subjected to aging treatment for 48 hours, and then a sample for evaluating the oxygen transmission rate before retort treatment was prepared from the packaging material 8.
[0189] Also, a B5 size four-sided sealed pouch was produced using packaging material 8. Then, 100 mL of water was poured into the four-sided sealed pouch from the top opening, and then a seal was formed at the top to seal the four-sided sealed pouch. Then, the four-sided sealed pouch was subjected to a retort treatment at 121°C for 40 minutes. Next, the packaging material 8 constituting one side of the four-side sealed pouch after the retort treatment was cut out to prepare a sample for evaluating the oxygen transmission rate after the retort treatment.
[0190] Next, the sample before retort treatment and the sample after retort treatment were set so that the substrate 1 was on the oxygen supply side, and the oxygen permeability was measured in accordance with JIS K 7126 B method under measurement conditions of 23°C and 100% RH atmosphere. The measurement device used was an oxygen permeability measuring device (manufactured by Modern Control (MOCON) [model name: OX-TRAN 2 / 21]). As a result, the oxygen permeability of the sample before retort treatment was 0.24 cc / m 2 / 24hr / atm. The oxygen permeability of the sample after retort treatment was 0.20cc / m 2 / 24hr / atm. Thus, both before and after retort treatment, the oxygen permeability was 0.50cc / m 2 We were able to keep it below / 24hr / atm.
[0191] (Water vapor permeability) The water vapor permeability was measured using the same samples as those used for measuring the oxygen permeability. Specifically, each sample was set so that the substrate 1 was on the sensor side, and the water vapor permeability was measured in accordance with JIS K 7126 B method under measurement conditions of 37.8°C and 100% RH atmosphere. The measurement device used was a water vapor permeability measuring device (a measuring device manufactured by MOCON [model name: PERMATRAN 3 / 33]). As a result, the water vapor permeability of the sample before retort treatment was 0.61 g / m 2 / 24hr. The water vapor transmission rate of the sample after retort treatment was 1.05g / m 2 / 24hr. Thus, both before and after retort treatment, the water vapor transmission rate was 1.5 g / m 2 We were able to keep it below 24hr.
[0192] [Example B2] A barrier laminate film 5 including a substrate 1 and a deposition layer 2 provided on the substrate 1 was produced in the same manner as in Example B1, except that the gas barrier coating film 3 was not formed on the deposition layer 2. Then, in the same manner as in Example B1, two samples were prepared from the barrier laminate film 5 of Example B2, and the transformation rate of the deposition layer 2 for each of the two samples was measured (the thickness W of the transition region). 1 The conversion rate was calculated as follows: (a) the conversion rate of the first sample was 37.8% / the thickness of the vapor-deposited layer 2)×100(%). As a result, the conversion rate of the second sample was 37.8%, and the conversion rate of the third sample was 42.2%.
[0193] The above-mentioned rectangular test piece 40 was prepared from the barrier laminate film 5 of Example B2, and the loop stiffness in the machine direction and the perpendicular direction was measured in the same manner as in Example B1. As a result, the loop stiffness in the machine direction of the barrier laminate film 5 was 0.0021 N, and the loop stiffness in the perpendicular direction was 0.0021 N.
[0194] [Comparative Example B1] A barrier laminate film 5 including a substrate 1, a deposition layer 2 provided on the substrate 1, and a gas barrier coating film 3 provided on the deposition layer 2 was produced in the same manner as in Example B1, except that a biaxially stretched PET film having a loop stiffness of less than 0.0017 N in both the machine direction and the perpendicular direction and made of petroleum-derived PET was used as the substrate 1. Then, in the same manner as in Example B1, the above-mentioned rectangular test piece 40 was produced from the barrier laminate film 5 of Comparative Example B1, and the loop stiffness in the machine direction and perpendicular direction was measured. As a result, the loop stiffness in the machine direction of the barrier laminate film 5 was 0.0014 N, and the loop stiffness in the perpendicular direction was 0.0016 N. [Explanation of symbols]
[0195] 1 Base material 2 Deposited layer 3. Gas barrier coating film 5. Barrier laminate film 6 Adhesive layer 7 Thermoplastic resin layer 8 Packaging materials 60 Film deposition equipment 62 Decompression Chamber 62A Substrate transport chamber 62B Plasma pretreatment chamber 62C Film forming chamber 63 Unwinding roller 64 Guide roller 65 Winding roller 68 Raw gas volatilization supply device 69 Raw material gas supply nozzle 70 Plasma pretreatment roller 71 Electrode 72 Plasma supply nozzle 75 Coating roller 76 Film forming means 80 Vacuum Pump 81 Power supply wiring 82 Power supply 85a~85c Bulkhead
Claims
1. A substrate; A deposition layer provided on the substrate and containing a metal or an inorganic compound; The substrate has a loop stiffness of 0.0017 N or more in the machine direction and the perpendicular direction, and contains polyester as a main component; In at least one direction, the tensile strength of the substrate divided by the tensile elongation is 2.0 [MPa / %] or more; The thickness of the substrate is 16 μm or more and 25 μm or less.
2. 2. The barrier laminate film according to claim 1, wherein the substrate has a puncture strength of 9.5 N or more.
3. The barrier laminate film according to claim 1 or 2, further comprising a gas barrier coating film provided on the vapor deposition layer.
4. The barrier laminate film according to claim 1 , wherein the vapor deposition layer is a transparent vapor deposition layer containing an inorganic compound.
5. the deposition layer is a transparent deposition layer containing aluminum oxide, the transparent deposition layer includes a transition region; The transition region is an elemental bond Al detected by etching the barrier laminate film from the transparent deposition layer side using a time-of-flight secondary ion mass spectrometry (TOF-SIMS). 2 O 4 a region between the position of the H peak and the interface between the transparent deposition layer and the substrate, 4. The barrier laminate film according to claim 1, wherein a ratio of a thickness of the transition region to a thickness of the transparent vapor deposition layer is 5% or more and 60% or less.
6. Providing a substrate; A deposition step of depositing a metal or an inorganic compound on the substrate to form a deposition layer on the substrate, The substrate has a loop stiffness of 0.0017 N or more in the machine direction and the perpendicular direction, and contains polyester as a main component; In at least one direction, the tensile strength of the substrate divided by the tensile elongation is 2.0 [MPa / %] or more; The method for producing a barrier laminate film, wherein the substrate has a thickness of 16 μm or more and 25 μm or less.
7. The method further includes a plasma pretreatment step of subjecting the substrate to a plasma treatment to form a plasma-treated surface on the substrate, The method for producing a barrier laminate film according to claim 6 , wherein the vapor deposition step forms the vapor deposition layer on the plasma-treated surface of the substrate.
8. The method for producing a barrier laminate film according to claim 7 , wherein the vapor deposition step forms the vapor deposition layer on the plasma-treated surface of the substrate by physical vapor deposition.
9. The plasma pretreatment step includes a step of supplying a mixed gas of oxygen gas and an inert gas as a plasma raw material gas, The method for producing a barrier laminate film according to claim 7 or 8, wherein a mixing ratio of the oxygen gas to the inert gas (oxygen gas / inert gas) is within a range of 6 / 1 to 1 / 1.
10. the vapor deposition layer is a transparent vapor deposition layer containing an inorganic compound, 10. The method for producing a barrier laminate film according to claim 6, further comprising the step of applying a coating agent for a gas barrier coating film onto the deposition layer, and drying the applied coating agent by heating to form a gas barrier coating film.
11. The method for producing a barrier laminate film according to claim 10, wherein the gas barrier coating film is a layer formed by coating a mixed solution of a metal alkoxide and a water-soluble polymer, and drying the mixture by heating.
12. The method for producing a barrier laminate film according to claim 10, wherein the gas barrier coating film is a layer formed by coating a mixed solution of a metal alkoxide, a silane coupling agent, and a water-soluble polymer, and drying the mixture by heating.
13. A barrier laminate film having a substrate and a vapor-deposited layer containing a metal or an inorganic compound provided on the substrate; a thermoplastic resin layer laminated on the barrier laminate film, The substrate has a loop stiffness of 0.0017 N or more in the machine direction and the perpendicular direction, and contains polyester as a main component; In at least one direction, the tensile strength of the substrate divided by the tensile elongation is 2.0 [MPa / %] or more; The packaging material, wherein the thickness of the substrate is 16 μm or more and 25 μm or less.
14. The packaging material according to claim 13, which is used for a packaging bag for boiling or a packaging bag for retort sterilization.
Citation Information
Patent Citations
Laminated body having barrier property and manufacture thereof
JP1997123334A
Method for producing transparent barrier nylon film
JP2007303000A
Method for producing laminate, laminate, and packaging container using the laminate
JP2011083906A
Retort packaging material including biaxially stretched polybutylene terephthalate film
JP2012214248A
Laminate sheet
JP2016101721A