Light emitting device and method for manufacturing same
A light-emitting device with a light-attenuating layer composed of transparent thermoplastic elastomers and titanium black effectively suppresses external light reflection, addressing the cost issue of circularly polarizing plates and maintaining device brightness.
Patent Information
- Application Number
- JP2019224626
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2019-12-12
- Publication Date
- 2024-10-04
- Estimated Expiration
- 2039-12-12
AI Technical Summary
The use of circularly polarizing plates in light-emitting devices to suppress external light reflection is costly, necessitating the development of a more cost-effective solution to achieve the same effect.
A light-emitting device configuration incorporating a light-attenuating layer with a total light transmittance of 45% to 75% composed of a transparent material A1 and a material B1 that absorbs or reflects visible light, where material A1 includes thermoplastic elastomers and material B1 includes titanium black, is employed to reduce external light reflection.
The proposed configuration effectively suppresses external light reflection while maintaining device brightness, offering a cost-effective alternative to circularly polarizing plates by using a thinner and more versatile light-attenuating layer.
Smart Images

Figure 0007561495000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a light emitting device and a method for manufacturing the same. [Background technology]
[0002] Light-emitting elements such as organic electroluminescence elements (organic EL elements) may include a reflective element such as a reflective electrode in order to improve light extraction efficiency. When external light is incident on a light-emitting element having a reflecting element, the external light is reflected by the reflecting element, and the reflected external light may make the light-emitting element difficult to see. Therefore, light-emitting devices including a light-emitting element having a reflecting element often include a member or mechanism for suppressing reflection of external light. An example of a member for suppressing reflection of external light is a circular polarizing plate (see Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Japanese Patent Application Publication No. 8-321381 Summary of the Invention [Problem to be solved by the invention]
[0004] Since a circularly polarizing plate is composed of a plurality of optical layers, the manufacturing cost is high. Therefore, from the viewpoint of reducing the manufacturing cost of a light-emitting device, a new member capable of suppressing the reflection of external light is required. In addition, a light-emitting device having a novel configuration capable of suppressing the reflection of external light and a method for manufacturing such a light-emitting device are required. [Means for solving the problem]
[0005] Means for Solving the Problems The present inventors conducted extensive research to find a solution to the above problems, and discovered that reflection of external light can be suppressed by combining a specific light-reducing layer with a light-emitting element, thereby completing the present invention. That is, the present invention provides the following.
[0006] [1] A light-emitting element including a reflective element, and a dimming layer arranged on the viewing side of the reflective element and having a total light transmittance of 45% or more and 75% or less; A light emitting device, wherein the light reducing layer comprises a transparent material A1 and a material B1 that absorbs or reflects visible light. [2] The light-emitting device according to [1], wherein the thickness of the dimming layer is 1 μm or more and less than 100 μm. [3] The light-emitting device according to [1] or [2], wherein the linear transmittance of the dimming layer at a wavelength of 500 nm is greater than the linear transmittance at a wavelength of 600 nm. [4] The light-emitting device according to any one of [1] to [3], wherein the transparent material A1 contains a thermoplastic elastomer. [5] The light-emitting device according to [4], wherein the thermoplastic elastomer comprises at least one selected from the group consisting of hydrogenated aromatic vinyl compound-conjugated diene block copolymers and modified products thereof. [6] The light-emitting device according to any one of [1] to [3], wherein the transparent material A1 includes at least one selected from the group consisting of a cured product of a photocurable resin and an adhesive. [7] The light-emitting device according to any one of [1] to [6], wherein the material B1 contains at least titanium black. [8] The light-emitting device according to any one of [1] to [7], wherein the light-reducing layer further contains hygroscopic particles, and the content of the hygroscopic particles in the light-reducing layer is 5% by weight or more and 50% by weight or less. [9] The light-emitting device according to any one of [1] to [8], wherein the light-emitting element is an organic electroluminescence element.
[10] A method for producing the light-emitting device according to any one of [1] to [9], comprising the steps of: A step (1) of preparing a coating liquid including the transparent material A1 or a material for forming the transparent material A1, the material B1 that absorbs or reflects visible light, and a solvent; and (2) forming the light-reducing layer from the coating liquid, The step (2) A step (2a) of applying the coating liquid onto a substrate to form a coating film; and (2b) removing the solvent from the coating film. Effect of the Invention
[0007] According to the present invention, it is possible to provide a light-emitting device capable of suppressing reflection of external light and a method for manufacturing such a light-emitting device. [Brief description of the drawings]
[0008] [Figure 1] FIG. 1 is a cross-sectional view that illustrates a light-emitting device according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] The present invention will be described in detail below with reference to embodiments and examples. However, the present invention is not limited to the embodiments and examples shown below, and may be modified and implemented as desired without departing from the scope of the claims of the present invention and their equivalents.
[0010] In the following description, the term "(meth)acrylic acid" includes "acrylic acid", "methacrylic acid", and combinations thereof. The term "(meth)acryloyl" encompasses "acryloyl," "methacryloyl," and combinations thereof. The term "(meth)acrylonitrile" includes "acrylonitrile", "methacrylonitrile", and combinations thereof. The term "(meth)acrylate" encompasses "acrylate," "methacrylate," and combinations thereof. The term "(meth)acrylamide" encompasses "acrylamide," "methacrylamide," and combinations thereof.
[0011] In the following description, visible light refers to light with a wavelength of 400 nm or more and 700 nm or less.
[0012] [1. Overview of light-emitting devices] A light-emitting device according to one embodiment of the present invention includes a light-emitting element including a reflective element, and a light-reducing layer that is disposed on the viewing side of the reflective element and has a total light transmittance of 45% or more and 75% or less. The light-reducing layer includes a transparent material A1 and a material B1 that absorbs or reflects visible light.
[0013] [1.1. Light-emitting element] The light-emitting element is any light-emitting element that includes a reflective element. The reflective element is an element that can reflect external light incident on the light-emitting element. Examples of such light-emitting elements include light-emitting diode elements (e.g., inorganic light-emitting diode elements, organic light-emitting diode elements (organic electroluminescence elements)) equipped with a reflective electrode. The light-emitting diode element may be a bottom-emission type that extracts light from the substrate side, or a top-emission type that extracts light from the side opposite the substrate side. The reflective electrode is usually disposed on the side opposite the light-emitting layer from which the light is extracted. Thus, in the top-emission type, the reflective electrode is usually disposed between the light-emitting layer and the substrate, and in the bottom-emission type, the reflective electrode is usually disposed on the side opposite the substrate from which the light-emitting layer is extracted (between the light-emitting layer and the sealing layer if the light-emitting diode element has a sealing layer). Preferably, the light-emitting element is an organic electroluminescence element having a reflective electrode.
[0014] [1.2. Light-reducing layer] [1.2.1. Placement of the light-reducing layer] The light-reducing layer is disposed on the viewing side of the reflective element included in the light-emitting element. 1 is a cross-sectional view showing a light-emitting device according to an embodiment of the present invention. As shown in FIG. 1, the light-emitting device 100 includes a light-emitting element 60 and a light-attenuating layer 50. The light-emitting element 60 includes a substrate 10, a first electrode 20 formed on the substrate 10, and a second electrode 40. The first electrode 20 functions as a reflective electrode, and the light-emitting device 100 is a top-emission type device in which light is extracted from a surface 50U opposite to the substrate 10. Therefore, the surface 50U side of the light-emitting device 100 is the viewing side. The light-emitting layer 30 is disposed between the first electrode 20 and the second electrode 40. In addition to the light-emitting layer 30, a functional layer such as an electron injection layer, an electron transport layer, a hole transport layer, or a hole injection layer may be disposed between the first electrode 20 and the second electrode 40. The light-attenuating layer 50 is disposed on the second electrode 40. The light-attenuating layer 50 is disposed on the viewing side of the first electrode 20, which serves as a reflective electrode. The light-attenuating layer 50 is disposed at a position farther from the substrate 10 than the first electrode 20. Since the light-reducing layer 50 is disposed on the viewing side of the first electrode 20 serving as a reflective electrode (reflective element), it is possible to attenuate external light reflected from the reflective electrode.
[0015] [1.2.2. Materials for the light-reducing layer] The light-reducing layer includes a transparent material A1 and a material B1 that absorbs or reflects visible light.
[0016] [Transparent material A1] A transparent material is usually a material whose haze value is 5% or less when made into a test piece with a thickness of 0.02 mm. The haze value is usually 0% or more. The haze value can be measured in accordance with JIS K7136.
[0017] The content of the transparent material A1 in the light-reducing layer may be any content ratio that allows the total light transmittance of the light-reducing layer to fall within a specified range described below, but is preferably 50% by weight or more, more preferably 60% by weight or more, and even more preferably 70% by weight or more, and is usually less than 100% by weight, preferably 99.8% by weight or less, and more preferably 99.5% by weight or less.
[0018] The transparent material A1 usually contains a polymer. Examples of polymers that can be contained in the transparent material A1 include polyester; polyurethane; silicone; acrylic polymer; copolymer of acrylic monomer and aromatic vinyl compound; polyolefin (e.g., polybutadiene, polyisoprene, polyisobutylene, polyethylene propylene, polypropylene butene, polyethylene propylene butene); copolymer of olefin and aromatic vinyl compound (e.g., styrene-butadiene-styrene block copolymer, styrene-ethylenebutylene-styrene block copolymer, styrene-ethylenebutylene random copolymer), hydrogenated products thereof, and modified products of the hydrogenated products thereof (e.g., hydrogenated block copolymer and modified products thereof disclosed in International Publication WO 2016 / 163409); polyvinyl ether; and the like. The transparent material A1 may contain one type of polymer alone or a combination of two or more types.
[0019] The transparent material A1 may include a material classified as a thermoplastic elastomer, a cured product of a photocurable resin, and / or an adhesive. Thus, in one embodiment, the transparent material A1 preferably includes a thermoplastic elastomer. In another embodiment, the transparent material A1 preferably includes one or more selected from the group consisting of a cured product of a photocurable resin and an adhesive.
[0020] (Thermoplastic elastomer) Thermoplastic elastomers are materials that exhibit rubber characteristics at room temperature, but become plasticized at high temperatures to enable molding. Such thermoplastic elastomers are characterized by being resistant to elongation and breakage under the load of a small force. Specifically, thermoplastic elastomers exhibit Young's modulus of 0.001 to 1 GPa and tensile elongation (breaking elongation) of 100 to 1000% at 23°C. Thermoplastic elastomers also exhibit a sharp drop in storage modulus and a peak in loss tangent tanδ (loss modulus / storage modulus) or a value exceeding 1, softening in the high temperature range of 40°C to 200°C. Young's modulus and tensile elongation can be measured according to JIS K7113. Loss tangent tanδ can be measured using a commercially available dynamic viscoelasticity measuring device.
[0021] Thermoplastic elastomers generally do not contain residual solvents, or if they do, the amount is small, so outgassing is low. Therefore, by using a material containing a thermoplastic elastomer as the transparent material A1, it is possible to suppress changes in the characteristics of the light-emitting element due to outgassing. In addition, by using a material containing a thermoplastic elastomer as the transparent material A1, the material of the dimming layer can be prevented from moving when the dimming layer is folded, and as a result, unevenness in the thickness of the dimming layer caused by folding the light-emitting device can be prevented.
[0022] When the transparent material A1 contains a thermoplastic elastomer, the weight proportion of the thermoplastic elastomer in the transparent material A1 is preferably 50% by weight or more, more preferably 60% by weight or more, and even more preferably 70% by weight or more, and is usually 100% by weight or less, and may be 100% by weight.
[0023] The thermoplastic elastomer that can be contained in the transparent material A1 preferably includes at least one selected from the group consisting of hydrogenated aromatic vinyl compound-conjugated diene block copolymers and modified products thereof. Hereinafter, the hydrogenated aromatic vinyl compound-conjugated diene block copolymers are also referred to as copolymer (a1).
[0024] The total weight proportion of the copolymer (a1) and the modified copolymer (a1) in the thermoplastic elastomer is preferably 90% by weight or more, more preferably 95% by weight or more, and even more preferably 98% by weight or more, and is usually 100% by weight or less, and may be 99.9% by weight or less.
[0025] The thermoplastic elastomer may contain any polymer in addition to the copolymer (a1) and the modified copolymer (a1). The total weight proportion of any polymer in the thermoplastic elastomer is preferably 10% by weight or less, more preferably 5% by weight or less, and even more preferably 2% by weight or less, and is usually 0% by weight or more, and may be 0% by weight.
[0026] (Copolymer (a1) (hydrogenated aromatic vinyl compound-conjugated diene block copolymer)) The hydrogenated aromatic vinyl compound-conjugated diene block copolymer is a hydrogenated product of an aromatic vinyl compound-conjugated diene block copolymer. That is, the hydrogenated aromatic vinyl compound-conjugated diene block copolymer has a structure obtained by hydrogenating a part or all of the carbon-carbon unsaturated bonds (including the carbon-carbon unsaturated bonds derived from the conjugated diene) in the main chain and the side chain of the aromatic vinyl compound-conjugated diene block copolymer, the carbon-carbon unsaturated bonds in the aromatic ring, or both of them. However, in the present application, the hydrogenated product is not limited by its production method.
[0027] As the aromatic vinyl compound, styrene and its derivatives; vinylnaphthalene and its derivatives are preferred, styrene and its derivatives are more preferred, and from the viewpoint of industrial availability, it is particularly preferred to use styrene. As the conjugated diene, a chain conjugated diene (straight-chain conjugated diene, branched-chain conjugated diene) is preferred, and specific examples thereof include 1,3-butadiene, isoprene (2-methyl-1,3-butadiene), 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, etc. Among these, 1,3-butadiene and isoprene are particularly preferred because of their industrial availability.
[0028] The aromatic vinyl compound-conjugated diene block copolymer is preferably selected from styrene-butadiene block copolymers, styrene-butadiene-styrene block copolymers, styrene-isoprene block copolymers, styrene-isoprene-styrene block copolymers, and mixtures thereof. More specific examples of these include those described in prior art documents such as JP-A-2-133406, JP-A-2-305814, JP-A-3-72512, JP-A-3-74409, and WO 2015 / 099079.
[0029] The hydrogenation rate of the hydrogenated aromatic vinyl compound-conjugated diene block copolymer is preferably 90% or more, more preferably 97% or more, particularly preferably 99% or more, and is usually 100% or less. The higher the hydrogenation rate, the better the heat resistance and light resistance of the light-reducing layer. Here, the hydrogenation rate of the hydrogenated product is 1 It can be determined by H-NMR measurement.
[0030] The hydrogenation rate of the carbon-carbon unsaturated bonds in the main chain and side chain of the hydrogenated aromatic vinyl compound-conjugated diene block copolymer is preferably 95% or more, more preferably 99% or more, and usually 100% or less. By increasing the hydrogenation rate of the carbon-carbon unsaturated bonds in the main chain and side chain of the hydrogenated aromatic vinyl compound-conjugated diene block copolymer, the light resistance and oxidation resistance of the light-reducing layer can be further improved.
[0031] In addition, the hydrogenation rate of the carbon-carbon unsaturated bond of the aromatic ring of the hydrogenated aromatic vinyl compound-conjugated diene block copolymer is preferably 90% or more, more preferably 93% or more, particularly preferably 95% or more, and is usually 100% or less. By increasing the hydrogenation rate of the carbon-carbon unsaturated bond of the aromatic ring, the glass transition temperature of the hydrogenated product increases, so that the heat resistance of the light-reducing layer can be effectively improved. Furthermore, the photoelastic coefficient of the light-reducing layer can be reduced, thereby reducing the occurrence of retardation.
[0032] The hydrogenated aromatic vinyl compound-conjugated diene block copolymer is preferably one having a structure in which both the unsaturated bonds and aromatic rings derived from the conjugated diene are hydrogenated.
[0033] Particularly preferred block forms of the hydrogenated aromatic vinyl compound-conjugated diene block copolymer are a triblock copolymer in which a block [A] of a hydrogenated aromatic vinyl polymer is bonded to both ends of a block [B] of a hydrogenated conjugated diene polymer, and a pentablock copolymer in which a polymer block [B] is bonded to both ends of a polymer block [A] and a polymer block [A] is bonded to the other ends of each of the polymer blocks [B]. In particular, a triblock copolymer of [A]-[B]-[A] is particularly preferred because it is easy to produce and the physical properties as a thermoplastic elastomer can be set within the desired range.
[0034] When the mass fraction of all aromatic vinyl monomer units in the entire aromatic vinyl compound-conjugated diene block copolymer is wA, and the mass fraction of all conjugated diene monomer units in the block copolymer in the entire block copolymer is wB, the ratio of wA to wB (wA:wB) is preferably 20 / 80 or more, more preferably 30 / 70 or more, and preferably 60 / 40 or less, more preferably 55 / 45 or less. By making the ratio wA / wB equal to or greater than the lower limit of the range, the heat resistance of the light-reducing layer can be improved. Also, by making it equal to or less than the upper limit, the flexibility of the light-reducing layer can be increased.
[0035] (Modified product of copolymer (a1)) An example of the modified copolymer (a1) is a modified copolymer (a1) having a silicon atom-containing polar group. An example of the modified copolymer (a1) having a silicon atom-containing polar group is a polymer having a structure obtained by graft polymerization of copolymer (a1) and a compound having a functional group such as a silicon atom-containing polar group. The modified product is not limited by its manufacturing method. The modified copolymer (a1) is preferably a modified copolymer (a1) having a silicon atom-containing polar group, and the silicon atom-containing polar group is preferably an alkoxysilyl group.
[0036] Examples of compounds having a silicon atom-containing polar group that can be used as a monomer for graft polymerization include ethylenically unsaturated silane compounds having an alkoxysilyl group (e.g., vinyltrimethoxysilane, vinyltriethoxysilane, allyltrimethoxysilane, allyltriethoxysilane, dimethoxymethylvinylsilane, diethoxymethylvinylsilane, p-styryltrimethoxysilane, p-styryltriethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropyltriethoxysilane, 3-methacryloxypropylmethyldiethoxysilane, 3-acryloxypropyltrimethoxysilane, 3-acryloxypropyltriethoxysilane, and 2-norbornene-5-yltrimethoxysilane).
[0037] By reacting the copolymer (a1) with a compound having a silicon atom-containing polar group, a silicon atom-containing polar group can be introduced into the copolymer (a1) to obtain a modified product having a silicon atom-containing polar group. When an alkoxysilyl group is introduced as a silicon atom-containing polar group, the amount of the alkoxysilyl group introduced is preferably 0.1 parts by weight or more, more preferably 0.2 parts by weight or more, and even more preferably 0.3 parts by weight or more, and preferably 10 parts by weight or less, more preferably 5 parts by weight or less, and even more preferably 3 parts by weight or less, per 100 parts by weight of the copolymer (a1). When the amount of the alkoxysilyl group introduced is within the above range, it is possible to prevent the degree of crosslinking between alkoxysilyl groups decomposed by moisture or the like from becoming excessively high, so that the adhesiveness can be maintained at a high level. Examples of substances having an alkoxysilyl group used for introducing the alkoxysilyl group and modification methods include those described in prior art documents such as International Publication No. WO 2015 / 099079.
[0038] The amount of polar group introduced is 1 It can be measured by H-NMR spectrum. In addition, when the amount of polar group introduced is small, the number of integrations can be increased.
[0039] Introducing an alkoxysilyl group as a polar group into the copolymer (a1) is called silane modification. In the silane modification, the alkoxysilyl group may be directly bonded to the copolymer (a1) or may be bonded via a divalent organic group such as an alkylene group. Hereinafter, the polymer obtained by silane modification of the copolymer (a1) is also referred to as a "silane modified product."
[0040] The modified copolymer (a1) is preferably a silane-modified hydrogenated aromatic vinyl compound-conjugated diene block copolymer, and more preferably one or more silane-modified copolymers selected from a silane-modified hydrogenated styrene-butadiene block copolymer, a silane-modified hydrogenated styrene-butadiene-styrene block copolymer, a silane-modified hydrogenated styrene-isoprene block copolymer, and a silane-modified hydrogenated styrene-isoprene-styrene block copolymer.
[0041] (Weight average molecular weight and molecular weight distribution) The weight average molecular weight (Mw) of the thermoplastic elastomer is not particularly limited, but is preferably 20,000 or more, more preferably 30,000 or more, even more preferably 35,000 or more, and is preferably 200,000 or less, more preferably 100,000 or less, and even more preferably 70,000 or less. The weight average molecular weight (Mw) of the thermoplastic elastomer can be measured in terms of polystyrene by gel permeation chromatography using tetrahydrofuran as a solvent. The molecular weight distribution (Mw / Mn) of the thermoplastic elastomer is preferably 4 or less, more preferably 3 or less, even more preferably 2 or less, and preferably 1 or more. By setting the weight average molecular weight Mw and molecular weight distribution Mw / Mn of the elastomer within the above ranges, the mechanical strength and heat resistance of the light-reducing layer can be improved.
[0042] (glass transition temperature) The glass transition temperature of the thermoplastic elastomer is not particularly limited, but is preferably 40° C. or higher, more preferably 70° C. or higher, and is preferably 200° C. or lower, more preferably 180° C. or lower, and even more preferably 160° C. or lower. When a thermoplastic elastomer containing a block copolymer is used, the weight ratio of each polymer block is changed to adjust the glass transition temperature, thereby making it possible to achieve a balance between suppression of stickiness and flexibility of the light-reducing layer.
[0043] (Cured product of photocurable resin) A photocurable resin is a resin that can be cured by irradiation with light. Here, light includes electron beams, ultraviolet light, and visible light. Among them, ultraviolet-curable resins that can be cured by ultraviolet light are preferred because the time of curing can be easily controlled. The photocurable resin usually contains a polymerizable compound. The photocurable resin may contain only one type of polymerizable compound or may contain two or more types of polymerizable compounds in combination. The polymerizable compound usually has a polymerizable group. The polymerizable compound may be a compound having only one polymerizable group per molecule, or may be a compound having two or more polymerizable groups per molecule. The polymerizable compound may be any one of a monomer, an oligomer, and a polymer. The photocurable resin may be a resin containing only a monomer, a resin containing only an oligomer, a resin containing only a polymer, or a resin containing two or more kinds selected from the group consisting of a monomer, an oligomer, and a polymer, as the polymerizable compound.
[0044] The polymerizable group of the polymerizable compound (which may be a monomer, oligomer, or polymer) that the photocurable resin may contain is not particularly limited, and specific examples include (meth)acryloyl group, vinyl ether group, N-vinylamide group, vinyl ester group, aromatic vinyl group such as styryl group, oxetanyl group, oxiranyl group, glycidyl group, and cyclohexene oxide group. As the photocurable resin in this embodiment, for example, a resin containing a compound having these polymerizable groups may be used.
[0045] A polymerizable compound having a (meth)acryloyl group (which may be a monomer, oligomer, or polymer).Examples of the acrylates include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, sec-butyl (meth)acrylate, hexyl (meth)acrylate, octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, decyl (meth)acrylate, isobornyl (meth)acrylate, cyclohexyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, and 2-hydroxyethyl (meth)acrylate. Aliphatic mono(meth)acrylates such as dimethyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, and 2-hydroxybutyl (meth)acrylate; aromatic mono(meth)acrylates such as phenyl (meth)acrylate, benzyl (meth)acrylate, and 2-hydroxyphenylethyl (meth)acrylate; (meth)acrylamides such as N,N-dimethyl (meth)acrylamide, N,N-diethyl (meth)acrylamide, and N-acryloylmorpholine; ethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylamide, and aliphatic polyfunctional (meth)acrylates such as acrylate, 1,4-butanediol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, trimethylolpropane di(meth)acrylate, trimethylolpropane tri(meth)acrylate, and pentaerythritol penta(meth)acrylate; aromatic polyfunctional acrylates such as ethylene oxide modified bisphenol A (meth)acrylate and propylene oxide modified bisphenol A (meth)acrylate; 2-trifluoroethylene glycol di(meth)acrylate; Examples of fluorine-containing (meth)acrylates include fluorine-containing (meth)acrylates such as 2-trifluoromethylpropenoic acid trifluoroethyl ester, 2-trifluoromethylpropenoic acid t-butyl ester, 2,2,2-trifluoroethyl (meth)acrylate, 2,2,3,3-tetrafluoropropyl (meth)acrylate, 1H,1H,5H-octafluoropentyl (meth)acrylate, and perfluorooctylethyl (meth)acrylate; so-called epoxy (meth)acrylates obtained by adding (meth)acrylic acid to an epoxy resin; and various urethane (meth)acrylates.Examples of epoxy resins that can be used as a material for the epoxy (meth)acrylate include bisphenol A type epoxy resins, hydrogenated bisphenol A type epoxy resins, brominated bisphenol A type epoxy resins, bisphenol F type epoxy resins, novolac type epoxy resins, phenol novolac type epoxy resins, cresol novolac type epoxy resins, alicyclic epoxy resins, N-glycidyl type epoxy resins, bisphenol A novolac type epoxy resins, chelate type epoxy resins, glyoxal type epoxy resins, amino group-containing epoxy resins, rubber-modified epoxy resins, dicyclopentadiene phenolic type epoxy resins, silicone-modified epoxy resins, and ε-caprolactone-modified epoxy resins.
[0046] Examples of polymerizable compounds having a vinyl ether group and serving as monomers include aliphatic monovinyl ethers such as 2-ethylhexyl vinyl ether, octadecyl vinyl ether, 4-hydroxybutyl vinyl ether, diethylene glycol monovinyl ether, triethylene glycol monovinyl ether, 9-hydroxynonyl vinyl ether, methoxyethyl vinyl ether, and ethoxyethyl vinyl ether; alicyclic monovinyl ethers such as cyclohexyl vinyl ether, 4-hydroxycyclohexyl vinyl ether, cyclohexane dimethanol monovinyl ether, and tricyclodecanyl vinyl ether; aliphatic divinyl ethers such as 1,4-butanediol divinyl ether, nonanediol divinyl ether, and triethylene glycol divinyl ether; alicyclic divinyl ethers such as cyclohexanediol divinyl ether, cyclohexane dimethanol divinyl ether, tricyclodecane dimethanol divinyl ether, and pentacyclopentadecane dimethanol divinyl ether; and polyfunctional vinyl ethers such as trimethylolpropane trivinyl ether and pentaerythritol tetravinyl ether. Examples of polymerizable compounds having an N-vinylamide group and which are monomers include N-vinylformamide and N-vinylpyrrolidone.
[0047] Examples of polymerizable compounds having a vinyl ester group and being an oligomer or polymer include those available under the trade name "Lipoxy Series" manufactured by Showa Polymer Co., Ltd., those available under the trade name "Dick-Lite Series" manufactured by DIC Corporation, and those available under the trade name "Neopol Series" manufactured by Japan U-PICA Corporation.
[0048] Examples of polymerizable compounds having a styryl group and being monomers include styrene; styrene derivatives such as 2,4-dimethyl-α-methylstyrene, o-methylstyrene, m-methylstyrene, and p-methylstyrene; divinylbenzene; and divinylbiphenyl.
[0049] Examples of polymerizable compounds having a glycidyl group and being monomers include glycidol, allyl glycidyl ether, glycidyl (meth)acrylate, 2-ethylhexyl glycidyl ether, phenyl glycidyl ether, ethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, 1,6-hexanediol diglycidyl ether, diethylene glycol diglycidyl ether, hydrogenated bisphenol A diglycidyl ether, diglycidyl terephthalate, diglycidyl orthophthalate, N-glycidyl phthalimide, glycerol polyglycidyl ether, and trimethylolpropane polyglycidyl ether. Examples of polymerizable compounds having a glycidyl group and being oligomers or polymers include polymers of allyl glycidyl ether, polymers of glycidyl (meth)acrylate, bisphenol A type epoxy resins, hydrogenated bisphenol A type epoxy resins, bisphenol F type epoxy resins, novolac type epoxy resins, and N-glycidyl type epoxy resins.
[0050] Examples of polymerizable compounds having a cyclohexene oxide group and being monomers include cyclohexene oxide, 1,2-epoxy-4-vinylcyclohexane, 3,4-epoxycyclohexane carboxylate allyl, 3,4-epoxycyclohexylmethyl (meth)acrylate, 1,2:8,9 diepoxy limonene, and the trade name "Celloxide 2021P" manufactured by Daicel Chemical Industries, Ltd. Examples of compounds having a cyclohexene oxide group and being oligomers or polymers include polymers of 3,4-epoxycyclohexane carboxylate allyl, polymers of 3,4-epoxycyclohexylmethyl (meth)acrylate, trade names "Epolead GT401" manufactured by Daicel Chemical Industries, Ltd., trade names "EHPE3150" manufactured by Daicel Chemical Industries, Ltd., and trade names "EHPE3150CE" manufactured by Daicel Chemical Industries, Ltd.
[0051] Examples of polymerizable compounds having an oxetanyl group (which may be a monomer, oligomer, or polymer) include those sold under the trade name "ARON OXETANE series" by Toagosei Co., Ltd., and those sold under the trade name "ETERNACOLL OXETAN series" by Ube Industries, Ltd.
[0052] In addition, a commercially available product may be used as the photocurable resin. Examples of the commercially available product include commercially available ultraviolet curable resins for nanoimprinting, such as "PAK-01" (manufactured by Toyo Gosei Co., Ltd.) and "NIF-A-1" (manufactured by Asahi Glass Co., Ltd.).
[0053] The photocurable resin may contain a photopolymerization initiator. The photopolymerization initiator is a substance that generates active species such as radicals and cations by irradiation with light, and initiates a polymerization reaction of a polymerizable compound. The type of photopolymerization initiator may be appropriately selected depending on the polymerizable compound that may be contained in the photocurable resin.
[0054] The light-reducing layer, which includes a transparent material A1 containing a cured product of a photocurable resin, can be formed by forming a composition containing a photocurable resin and a material B1 that absorbs or reflects visible light, which will be described later, into a film and then curing the composition by irradiating it with light.
[0055] (Adhesive) Examples of the adhesive include rubber-based adhesives, acrylic-based adhesives, polyester-based adhesives, polyurethane-based adhesives, and silicone-based adhesives. Among them, rubber-based adhesives and acrylic-based adhesives are preferred because they can be directly attached onto the layer (e.g., passivation layer) on the viewing side of the light-emitting element. The adhesive may be photocurable, non-photocurable, thermally crosslinkable, non-crosslinkable, or a combination of these.
[0056] (Rubber adhesive) Examples of rubber-based adhesives include compositions containing rubber. Examples of rubbers that can be contained in rubber-based adhesives include olefin-based rubbers such as polybutadiene, polyisoprene, polybutene, and isobutylene-isoprene rubber; and styrene-based rubbers such as copolymers of styrene and olefin.
[0057] (Acrylic adhesive) Examples of acrylic pressure-sensitive adhesives include compositions containing acrylic polymers, which refer to polymers containing acrylic monomer units such as (meth)acrylic acid, (meth)acrylic acid esters, (meth)acrylamide, and (meth)acrylonitrile. Examples of such acrylic polymers include copolymers containing aromatic ring-containing monomer units, hydroxyl group-containing monomer units, and (meth)acrylic acid ester-based monomer units.
[0058] Examples of aromatic ring-containing monomers include benzyl (meth)acrylate, benzyloxyethyl (meth)acrylate, phenoxyethyl (meth)acrylate, phenoxydiethylene glycol (meth)acrylate, ethylene oxide-modified cresol (meth)acrylate, ethylene oxide-modified nonylphenol (meth)acrylate, and biphenyloxyethyl (meth)acrylate.
[0059] Examples of hydroxyl group-containing monomers include acrylic acid hydroxyalkyl esters such as 2-hydroxyethyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 5-hydroxypentyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, and 8-hydroxyoctyl (meth)acrylate; caprolactone-modified monomers such as caprolactone-modified 2-hydroxyethyl (meth)acrylate; oxyalkylene-modified monomers such as diethylene glycol (meth)acrylate and polyethylene glycol (meth)acrylate; primary hydroxyl group-containing monomers such as 2-acryloyloxyethyl 2-hydroxyethyl phthalate, N-methylol (meth)acrylamide, and hydroxyethyl acrylamide; secondary hydroxyl group-containing monomers such as 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, and 3-chloro-2-hydroxypropyl (meth)acrylate; and tertiary hydroxyl group-containing monomers such as 2,2-dimethyl-2-hydroxyethyl (meth)acrylate.
[0060] Examples of (meth)acrylic acid ester monomers include methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, iso-butyl (meth)acrylate, tert-butyl (meth)acrylate, n-propyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, isodecyl (meth)acrylate, lauryl (meth)acrylate, cetyl (meth)acrylate, stearyl (meth)acrylate, cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, hydroxypropyl acrylate, methoxyethyl (meth)acrylate, butoxyethyl (meth)acrylate, and dimethylaminoethyl (meth)acrylate. The acrylic polymer may further contain other optional monomer units, examples of which include styrene units, styrene derivative units, and vinyl ester units (e.g., vinyl acetate).
[0061] (Polyester adhesive) Examples of polyester-based pressure-sensitive adhesives include compositions containing polyesters made from polycarboxylic acids such as dicarboxylic acids and polyols such as diols. Examples of polycarboxylic acids that can be used as raw materials for polyesters that can be contained in the adhesive include aromatic dicarboxylic acids (e.g., terephthalic acid, isophthalic acid, naphthalenedicarboxylic acid), aliphatic dicarboxylic acids (e.g., succinic acid, adipic acid, sebacic acid, azelaic acid, fumaric acid, maleic acid, itaconic acid), alicyclic dicarboxylic acids (e.g., tetrahydrophthalic acid, hexahydrophthalic acid, cyclohexanedicarboxylic acid), trimellitic acid, and the like. Examples of polyols that can be used as raw materials for polyesters that can be contained in the adhesive include fatty acid esters derived from castor oil, dimer diols derived from oleic acid, glycerol monostearate, and the like; and aliphatic glycols such as ethylene glycol, 1,2-propylene glycol, 1,3-propanediol, 2-methyl-1,3-propanediol, 1,2-butanediol, 1,3-butanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 3-methyl-1,5-pentanediol, neopentyl glycol, diethylene glycol, dipropylene glycol, 2,2,4-trimethyl-1,5-pentanediol, 2-ethyl-2-butylpropanediol, 1,9-nonanediol, 2-methyloctanediol, 1,10-decanediol, 1,4-cyclohexanedimethanol, and 1,2-cyclohexanedimethanol.
[0062] (Polyurethane adhesive) An example of a polyurethane-based pressure-sensitive adhesive is a composition containing polyurethane made from polyol and polyisocyanate. Examples of polyols that can be used as a raw material for polyurethane contained in the PSA include polyester polyols and polyether polyols. Examples of polyisocyanates that can be used as raw materials for polyurethanes that can be contained in adhesives include aromatic polyisocyanates (e.g., 1,3-phenylene diisocyanate, 1,4-phenylene diisocyanate, 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, 1,3,5-triisocyanatobenzene, 2,4,6-triisocyanatotoluene, 4,4'-diphenylmethane diisocyanate, 2,4'-diphenylmethane diisocyanate, 4,4'-diphenylether ... socyanates, dianisidine diisocyanate, naphthalene-1,5-diisocyanate, 4,4',4''-triphenylmethane triisocyanate), aliphatic polyisocyanates (e.g. trimethylene diisocyanate, tetramethylene diisocyanate, pentamethylene diisocyanate, hexamethylene diisocyanate, dodecamethylene diisocyanate, 1,2-propylene diisocyanate, 2,3-butylene diisocyanate, 1,3-butylene diisocyanate, 2,4, 4-Trimethylhexamethylene diisocyanate, 2,2,4-Trimethylhexamethylene diisocyanate), aromatic aliphatic polyisocyanates (e.g., 1,3-xylylene diisocyanate, 1,4-xylylene diisocyanate, 2,4,5,6-tetramethyl-1,3-xylylene diisocyanate, 2,3,5,6-tetramethyl-1,4-xylylene diisocyanate), and alicyclic polyisocyanates (e.g., isophorone diisocyanate, 1,3-cyclohexane diisocyanate, methyl-2,4-cyclohexane diisocyanate, methyl-2,6-cyclohexane diisocyanate, 1,3,5-cyclohexane triisocyanate, 2-methyl-1,3,5-cyclohexane triisocyanate, 4,4'-dicyclohexylmethane diisocyanate, 2,4'-dicyclohexylmethane diisocyanate, 4,4'-dicyclohexyl ether diisocyanate, and norbornene diisocyanate.
[0063] (Silicone adhesive) Examples of silicone-based pressure-sensitive adhesives include pressure-sensitive adhesives containing a compound whose main skeleton has a siloxane consisting of Si-O bonds with high bond energy. Specific examples include silicone pressure-sensitive adhesives containing organopolysiloxane, and silicone pressure-sensitive adhesives containing a mixture of diorganopolysiloxane having alkenyl groups and diorganopolysiloxane not having alkenyl groups.
[0064] [Materials that absorb or reflect visible light B1] The material that absorbs or reflects visible light refers to a material that can impart the function of attenuating visible light to the light-reducing layer by absorbing or reflecting visible light. Material B1 may be a material that absorbs or reflects light in the entire visible light range, or may be a material that absorbs or reflects light in a part of the visible light range. Material B1 may be a material that not only absorbs or reflects visible light, but also absorbs or reflects light other than visible light.
[0065] Examples of material B1 include inorganic pigments, organic pigments, and combinations thereof. Examples of inorganic pigments include metal oxide particles, metal nitride particles, metal oxynitride particles, and carbon black. Examples of metal elements constituting the metal oxide particles, metal nitride particles, and metal oxynitride particles include niobium, vanadium, cobalt, chromium, copper, manganese, ruthenium, iron, nickel, tin, titanium, zirconium, and silver. The metal oxide particles, metal nitride particles, and metal oxynitride particles may contain two or more metal elements. Examples of organic pigments include cyanine-based pigments, phthalocyanine-based pigments, squarium-based pigments, nitro-based pigments, azo-based pigments, dioxazine-based pigments, quinacridone-based pigments, and quinophthalone-based pigments.
[0066] The average particle diameter of the pigment that can be contained in material B1 is preferably 200 nm or less, more preferably 100 nm or less, from the viewpoint of dispersing the pigment well in the light-reducing layer and reducing the haze value of the light-reducing layer, and is usually greater than 0 nm, for example, 3 nm or more. Here, the average particle size is the number average particle size of primary particles.
[0067] The number average particle size of the primary particles can be measured using a laser diffraction granulometer. When the number average particle size of the primary particles measured using a laser diffraction particle sizer is less than 40 nm, the number average particle size of the primary particles can be suitably measured using a particle size measuring device using a dynamic light scattering method. The measurement by the dynamic light scattering method may be performed in the state of a dispersion liquid in which the particles are dispersed in a solvent.
[0068] In addition, when the number average particle size of the primary particles measured using a laser diffraction particle sizer is less than 40 nm, or when the measurement cannot be performed using the laser diffraction method and the dynamic light scattering method, the number average particle size can be suitably obtained by observation using an electron microscope. Specifically, the number average particle size can be obtained by the following method. Using an electron microscope, the sum of the short axis and the long axis of the primary particles for each of 50 particles is obtained, and the arithmetic mean value obtained by dividing the obtained sum by 2 can be used as the number average particle size. The number average particle size may be observed for particles in the cross section of the light-reducing layer, or may be observed for particles in the material for forming the light-reducing layer.
[0069] As the material B1, one type of material may be used, or two or more types of materials may be used in combination in any ratio.
[0070] It is preferred that material B1 contains an inorganic pigment since it is less likely to bleed out of the light-reducing layer. Material B1 preferably contains a black pigment, as this allows the light-reducing layer to be achromatic. Material B1 more preferably comprises a black inorganic pigment. Material B1 further preferably contains titanium black. Examples of black inorganic pigments include graphite powder, magnetite powder (Fe3O4) graphite powder, carbon black, iron oxide, low-order titanium oxide, titanium black (titanium oxynitride), titanium nitride, high-resistance black powder containing titanium black and insulating powder containing at least one selected from the group consisting of Y2O3, ZrO2, Al2O3, SiO2, TiO2, and V2O5, and high-resistance black powder containing titanium black and insulating powder containing at least one selected from the group consisting of Y2O3, ZrO2, Al2O3, SiO2, TiO2, and V2O5. Among these, titanium black and high-resistance black powder have high insulating properties and can be used in combination with the transparent material A1 to obtain a 10% or less insulating property. 13 This is preferable because it is easy to realize an insulating light-reducing layer having a surface resistance of Ω / □ or more.
[0071] The weight proportion of the black inorganic pigment in material B1 is preferably 10% by weight or more, more preferably 15% by weight or more, and is usually 100% by weight or less, and may be 100% by weight.
[0072] The weight ratio of the material B1 in the light-reducing layer can be adjusted so that the light-reducing layer has a desired total light transmittance. The weight ratio of the material B1 in the light-reducing layer is not particularly limited, but is preferably 0.2% by weight or more, more preferably 0.5% by weight or more, and is preferably 10% by weight or less, more preferably 5% by weight or less.
[0073] [Optional components] In addition to the transparent material A1 and the material B1, the light-reducing layer may contain any other component as long as the effect of the present invention is not significantly impaired. The optional components include dispersants, hygroscopic particles, antioxidants, plasticizers, ultraviolet absorbers, lubricants, and inorganic fillers that do not fall under the category of material B1. The optional components may be used alone or in combination of two or more in any ratio.
[0074] (Dispersant) The light-reducing layer may contain a dispersant. The dispersant allows the material B1 to be well dispersed in the light-reducing layer. Examples of the dispersant include surfactants such as cationic surfactants, anionic surfactants, and nonionic surfactants; wetting dispersants (e.g., wetting dispersants containing an acidic or basic adsorption group and a compatible group such as an alkyl chain skeleton); and polymer dispersants. The amount of dispersant may be, for example, 0.1 parts by weight or more, for example 0.2 parts by weight or more, for example 10 parts by weight or less, for example 5 parts by weight or less, based on 10 parts by weight of material B1.
[0075] (hygroscopic particles) The light-reducing layer may contain hygroscopic particles. Examples of materials constituting hygroscopic particles include compounds (oxides, hydroxides, salts, etc.) that contain alkali metals, alkaline earth metals, and aluminum and do not contain silicon (e.g., barium oxide, magnesium oxide, calcium oxide, strontium oxide, aluminum hydroxide, hydrotalcite, etc.), organometallic compounds described in JP-A-2005-298598, and basic hygroscopic agents such as clay containing metal oxides; and acidic hygroscopic agents such as inorganic compounds containing silicon (e.g., silica gel, nanoporous silica, zeolite).
[0076] The material of the hygroscopic particles is preferably one or more substances selected from the group consisting of zeolite and hydrotalcite. Zeolite is more preferable because it has a particularly high hygroscopic ability. In addition, zeolite releases water when dried, so it can be reused. As the material for the hygroscopic particles, one type may be used alone, or two or more types may be used in combination at any ratio. By including hygroscopic particles in the light-reducing layer, the light-reducing layer can function as a sealing layer that protects the light-emitting element from moisture in the air.
[0077] When the light-reducing layer contains hygroscopic particles, the content of the hygroscopic particles in the light-reducing layer is preferably 5% by weight or more, more preferably 10% by weight or more, even more preferably 15% by weight or more, and is preferably 50% by weight or less, more preferably 40% by weight or less.
[0078] (Antioxidants) The light-reducing layer may contain an antioxidant. Examples of the antioxidant include phosphorus-based antioxidants, phenol-based antioxidants, and sulfur-based antioxidants, and phosphorus-based antioxidants are preferred because they are less colored.
[0079] Examples of phosphorus-based antioxidants include monophosphite compounds such as triphenyl phosphite, diphenyl isodecyl phosphite, phenyl diisodecyl phosphite, tris(nonylphenyl) phosphite, tris(dinonylphenyl) phosphite, tris(2,4-di-t-butylphenyl) phosphite, and 10-(3,5-di-t-butyl-4-hydroxybenzyl)-9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide; 4,4'-butylidene-bis(3-methyl-6-t-butylphenyl-di-tridecyl phosphite; diphosphite compounds such as 4,4'-isopropylidene-bis(phenyl-di-alkyl(C12-C15)phosphite); 6-[3-(3-t-butyl-4-hydroxy-5-methylphenyl)propoxy]-2,4,8,10-tetrakis-t-butyldibenzo[d,f][1.3.2]dioxaphosphepine, 6-[3-(3,5-di-t-butyl-4-hydroxyphenyl)propoxy]-2,4,8,10-tetrakis-t-butyldibenzo[d,f][1.3.2]dioxaphosphepine, and the like.
[0080] The amount of the antioxidant is preferably 0.01 parts by weight or more, more preferably 0.05 parts by weight or more, even more preferably 0.1 parts by weight or more, and preferably 1 part by weight or less, more preferably 0.5 parts by weight or less, even more preferably 0.3 parts by weight or less, based on 100 parts by weight of the polymer that can be contained in the transparent material A1. By using the antioxidant in an amount equal to or more than the lower limit of the above range, the durability of the dimming layer can be improved. By using the antioxidant in an amount equal to or less than the upper limit of the above range, the durability can be efficiently improved.
[0081] [1.2.3. Characteristics of the light-reducing layer] (Total light transmittance) The light-reducing layer has a total light transmittance of usually 45% or more, preferably 50% or more, and usually 75% or less, preferably 70% or less. When the total light transmittance of the light-reducing layer falls within the above range, reflection of external light can be effectively suppressed. The total light transmittance is a value measured in accordance with JIS K7361-1 using a D65 light source. The total light transmittance can be measured with a haze meter (for example, "NDH4000" manufactured by Nippon Denshoku Industries Co., Ltd.).
[0082] (Linear transmittance) The light-reducing layer has a linear transmittance in the wavelength range of 400 nm to 700 nm of preferably 35% or more, more preferably 40% or more, and preferably 75% or less, more preferably 70% or less. The linear transmittance of the light-reducing layer can be measured by a spectrophotometer. The light-reducing layer has a linear transmittance at a wavelength of 400 nm of preferably 40% or more, more preferably 45% or more, and preferably 75% or less, more preferably 70% or less. The light-reducing layer has a linear transmittance at a wavelength of 500 nm of preferably 40% or more, more preferably 45% or more, and preferably 75% or less, more preferably 70% or less. The light-reducing layer has a linear transmittance at a wavelength of 600 nm of preferably 40% or more, more preferably 45% or more, and preferably 70% or less, more preferably 65% or less. The light-reducing layer has a linear transmittance at a wavelength of 700 nm of preferably 35% or more, more preferably 40% or more, and preferably 65% or less, more preferably 60% or less. In addition, it is preferable that the linear transmittance of the light-reducing layer at a wavelength of 500 nm is greater than the linear transmittance of the light-reducing layer at a wavelength of 600 nm, from the viewpoint of making the reflected light when the light-reducing layer is attached to a display bluish in color. Furthermore, the light-reducing layer preferably has a polarization degree of 50% or less, more preferably 20% or less, and even more preferably 5% or less. With a small polarization degree, the light reflected by the reflective element is further reduced, and the black display state of the display can be darkened.
[0083] (Hayes) The haze value of the light-reducing layer is preferably 30% or less, more preferably 25% or less, and even more preferably 20% or less. The smaller the haze value, the better. However, the haze value is usually 0% or more, and may be 0.5% or more. By making the haze value of the light-reducing layer equal to or less than the upper limit, the image displayed by the light-emitting device can be made clearer.
[0084] (Thickness of the light-reducing layer) The light-reducing layer may have any thickness depending on the weight ratio of the material B1 contained in the light-reducing layer, the desired total light transmittance, the desired mechanical strength, and the like. The upper limit of the thickness of the light-reducing layer is preferably less than 100 μm, more preferably 50 μm or less, from the viewpoint of making the light-emitting device thinner. The lower limit of the thickness of the light-reducing layer is preferably 1 μm or more, more preferably 5 μm or more, from the viewpoint of reducing the ratio of material B1 to transparent material A1 to prevent aggregation, distributing material B1 more uniformly in the light-reducing layer, and obtaining a predetermined total light transmittance.
[0085] [1.3. Function of light-emitting devices] In the light emitting device of the present embodiment, the light-reducing layer attenuates the light reflected from the reflective element, thereby suppressing reflection of external light. In addition, a film having a high phase difference (e.g., a polyethylene terephthalate (PET) film) has a depolarizing effect, so that it is usually limited to be combined with a light-emitting device having a circular polarizer. On the other hand, the dimming layer included in the light-emitting device of the present embodiment can be combined with a film having a high phase difference, such as a PET film, so that the options for the members constituting the light-emitting device can be expanded.
[0086] [2. Manufacturing method of light-emitting device] The light emitting device can be manufactured by any method. For example, the light-reducing layer of the light emitting device can be manufactured by any method such as a melt extrusion method, a solution casting method, or a coating method. For example, a light emitting device can be produced by a method including the following steps (1) and (2). Step (1): A step of preparing a coating liquid containing the transparent material A1 or a material for forming the transparent material A1, the material B1 that absorbs or reflects visible light, and a solvent. Step (2): forming the light-reducing layer from the coating liquid. A method for manufacturing a light emitting device according to one embodiment of the present invention will now be described.
[0087] [2.1. Process (1)] In step (1), a coating liquid is prepared. The coating liquid includes the transparent material A1 or a material for forming the transparent material A1, the material B1, and a solvent. The material for forming the transparent material A1 is a material that changes into the transparent material A1 by a treatment such as heating or light irradiation. When the transparent material A1 includes a thermoplastic elastomer, the coating liquid usually includes a thermoplastic elastomer. When the transparent material A1 includes a cured product of a photocurable resin, the coating liquid usually includes a photocurable resin. When the transparent material A1 includes an adhesive, the coating liquid may include a material that changes into an adhesive by a treatment such as heating or light irradiation.
[0088] Here, the solvent may be a normal solvent capable of dissolving the components of the coating liquid, or a dispersion medium capable of dispersing the components of the coating liquid. Examples of the solvent include aliphatic hydrocarbon solvents (e.g., hexane, heptane, octane, nonane, decane, undecane, dodecane, tridecane); alicyclic hydrocarbon solvents (e.g., cyclohexane, cyclopentane, cyclooctane, methylcyclohexane, ethylcyclohexane); aromatic hydrocarbon solvents (e.g., toluene, xylene, decalin, tetralin); ether solvents (e.g., tetrahydrofuran); amide solvents (e.g., N,N-dimethylformamide); and any combination thereof.
[0089] The coating liquid may be prepared by any method. For example, the coating liquid can be prepared by a method of preparing a solution or dispersion (liquid B1) containing material B1 and a solvent, separately preparing a solution or dispersion (liquid A1) containing transparent material A1 or a material for forming it and a solvent, and mixing liquid B1 and liquid A1; a method of adding transparent material A1 or a material for forming it to liquid B1 and mixing them; or a method of adding material B1 to liquid A1 and mixing them. As the coating liquid, a commercially available product may be used.
[0090] [2.2. Process (2)] In step (2), a light-reducing layer is formed from the coating liquid. Step (2) usually includes steps (2a) and (2b).
[0091] (Step (2a)) In step (2a), the coating liquid is applied onto a substrate to form a coating film. Any substrate can be used as the substrate to which the coating liquid is applied. The substrate may be a rigid member or a flexible member. Examples of the substrate include a glass plate and a resin film. Examples of the material of the resin film include polycarbonate, polyethylene terephthalate, acrylic resin, and cycloolefin resin, and among them, cycloolefin resin is preferred from the viewpoints of transparency, low moisture absorption, dimensional stability, and processability.
[0092] A conventionally known method can be used as the coating method. Examples of the coating method include a bar coating method, a dip coating method, a spray coating method, a spin coating method, a roll coating method, and a die coating method, and the bar coating method or the die coating method is preferable. A commercially available applicator can be used to carry out the bar coating method.
[0093] (Step (2b)) In step (2b), the solvent is removed from the coating film obtained in step (2a). Any method can be used to remove the solvent from the coating film, and examples of the method include heating with hot air or infrared radiation, and reducing pressure. Heating and reducing pressure may be used in combination.
[0094] [2.3. Optional process] The method for producing the light-emitting device according to the present embodiment may include any other steps in addition to the above steps. Examples of the optional steps include a step of curing the coating film, a step of peeling off the substrate from a laminate including the substrate and the light-reducing layer, and a step of providing the light-reducing layer on the viewing side of the reflective element of the light-emitting element. For example, when the coating liquid contains a curable resin such as a photocurable resin, the method for producing a light-emitting device preferably includes a step (2c) of performing a curing treatment of the coating film simultaneously with the step (2b) or after the step (2b). The curing treatment may be any treatment depending on the type of curable resin. For example, in the case of a thermosetting resin, a heat treatment may be performed. In the case of a photocurable resin, a light irradiation treatment may be performed. A plurality of treatments may be performed as the curing treatment. For example, both a heat treatment and a light irradiation treatment may be performed as the curing treatment. EXAMPLES
[0095] The present invention will be described in detail below with reference to examples. However, the present invention is not limited to the examples shown below, and can be modified and carried out as desired without departing from the scope of the claims of the present invention and the scope of equivalents thereto.
[0096] In the following description, the units "%" and "parts" are by weight unless otherwise specified. Furthermore, the operations described below were carried out at room temperature and pressure unless otherwise specified.
[0097] [Evaluation method] (Film thickness) The thickness of the light-reducing layer formed on the glass plate was measured using a contact surface roughness meter ("ET4000" manufactured by Kosaka Laboratory). Specifically, a part of the light-reducing layer was scraped off until the glass was exposed on the surface, and the step between the substrate and the light-reducing layer was measured using the contact surface roughness meter.
[0098] (Young's modulus, tensile elongation and tan δ of resin) The Young's modulus and tensile elongation of the resin at 23°C were measured in accordance with JIS K7113. The loss tangent tan δ (loss modulus / storage modulus) of the resin at temperatures between 40°C and 200°C was measured by cutting the resin into a film and using a 10 mm wide x 20 mm long test piece as the film and using a Hitachi High-Tech Science Corporation DMS6100 dynamic viscoelasticity measuring device.
[0099] (Linear transmittance of light-reducing layer) Using a spectrophotometer ("V-570" manufactured by JASCO Corporation), the linear transmittance of the light-reducing layer formed on the glass plate was measured in the wavelength range of 400 nm to 700 nm. Specifically, the linear transmittance of the entire glass plate and the light-reducing layer was measured, and the linear light transmittance of the glass plate was approximated to 100%, and the linear transmittance obtained was regarded as the linear transmittance of the light-reducing layer.
[0100] (Total light transmittance of light-reducing layer) The total light transmittance of the light-reducing layer formed on the glass plate was measured in accordance with JIS K7361-1 using a D65 light source. The measuring device used was "NDH4000" manufactured by Nippon Denshoku Industries Co., Ltd. The total light transmittance of the entire glass plate and the light-reducing layer was measured, and the total light transmittance of the glass plate was approximated to 100%, and the obtained total light transmittance was regarded as the total light transmittance of the light-reducing layer.
[0101] (Haze value) The haze value of the light-reducing layer formed on the glass plate was measured using a haze meter ("NDH4000" manufactured by Nippon Denshoku Industries Co., Ltd.).
[0102] [Production Example 1] (P1-1. Production of hydrogenated block copolymers) A hydrogenated block copolymer was produced by the following procedure using styrene as the aromatic vinyl compound and isoprene as the linear conjugated diene compound. The hydrogenated block copolymer produced has a triblock structure in which polymer block [A] is bonded to both ends of polymer block [B].
[0103] 256 parts of dehydrated cyclohexane, 25.0 parts of dehydrated styrene, and 0.615 parts of n-dibutyl ether were placed in a reactor equipped with a stirrer and the inside of the reactor was fully replaced with nitrogen, and 1.35 parts of n-butyllithium (15% cyclohexane solution) was added with stirring at 60° C. to initiate polymerization, and the reaction was continued for 60 minutes at 60° C. with stirring. The polymerization conversion rate at this point was 99.5% (the polymerization conversion rate was measured by gas chromatography. The same applies below).
[0104] Next, 50.0 parts of dehydrated isoprene was added, and stirring was continued at the same temperature for 30 minutes. At this point, the polymerization conversion rate was 99%. Thereafter, 25.0 parts of dehydrated styrene was further added and stirred at the same temperature for 60 minutes. At this point, the polymerization conversion rate was nearly 100%. Next, 0.5 parts of isopropyl alcohol was added to the reaction solution to terminate the reaction, thereby obtaining a solution (i) containing a block copolymer. The weight average molecular weight (Mw) of the block copolymer in the obtained solution (i) was 44,900, and the molecular weight distribution (Mw / Mn) was 1.03 (measured in polystyrene equivalent values by gel permeation chromatography using tetrahydrofuran as a solvent. The same applies below).
[0105] Next, the solution (i) was transferred to a pressure-resistant reactor equipped with a stirrer, and 4.0 parts of a silica-alumina supported nickel catalyst (E22U, nickel loading 60%; manufactured by JGC Chemical Industries, Ltd.) as a hydrogenation catalyst and 350 parts of dehydrated cyclohexane were added and mixed to the solution (i). The inside of the reactor was replaced with hydrogen gas, and hydrogen was further supplied while stirring the solution, and the hydrogenation reaction was carried out at a temperature of 170°C and a pressure of 4.5 MPa for 6 hours to hydrogenate the block copolymer, thereby obtaining a solution (iii) containing a hydrogenated product (ii) of the block copolymer. The weight average molecular weight (Mw) of the hydrogenated product (ii) in the solution (iii) was 45,100, and the molecular weight distribution (Mw / Mn) was 1.04.
[0106] After the hydrogenation reaction was completed, the solution (iii) was filtered to remove the hydrogenation catalyst. Then, 1.0 part of a xylene solution containing 0.1 part of a phosphorus-based antioxidant, 6-[3-(3-t-butyl-4-hydroxy-5-methylphenyl)propoxy]-2,4,8,10-tetrakis-t-butyldibenzo[d,f][1.3.2]dioxaphosphepine (Sumitomo Chemical Co., Ltd., "Sumilizer (registered trademark) GP"; hereinafter, referred to as "antioxidant A") was added to the filtered solution (iii) and dissolved therein to obtain a solution (iv).
[0107] Next, the solution (iv) was filtered through a Zeta Plus (registered trademark) filter 30H (manufactured by Cuno, pore size 0.5 μm to 1 μm), and then successively filtered through another metal fiber filter (pore size 0.4 μm, manufactured by Nichidai) to remove minute solids. From the filtered solution (iv), the solvent cyclohexane, xylene, and other volatile components were removed at a temperature of 260° C. and a pressure of 0.001 MPa or less using a cylindrical concentrating dryer (product name "CONTROL", manufactured by Hitachi, Ltd.). Then, the solids were extruded in a molten state into a strand shape from a die directly connected to the concentrating dryer, cooled, and cut with a pelletizer to obtain 85 parts of pellets (v) containing a hydrogenated block copolymer and antioxidant A. The weight average molecular weight (Mw) of the hydrogenated block copolymer (hydrogenated block copolymer) in the obtained pellets (v) was 45,000, and the molecular weight distribution (Mw / Mn) was 1.08. In addition, 1The hydrogenation rate measured by H-NMR was 99.9%. A film-like test piece was prepared from the pellet (v), and the glass transition temperature Tg was evaluated by the tan δ peak of a dynamic viscoelasticity measuring device, which was 130°C. The peak value of tan δ of the pellet (v) at 40°C or higher and 200°C or lower was 1.4. The Young's modulus of the pellet (vi) at 23°C was 0.6 GPa, and the tensile elongation was 550%. Therefore, the obtained hydrogenated block copolymer was a thermoplastic elastomer.
[0108] [Production Example 2] Using the pellets (v) of the hydrogenated block copolymer (hydrogenated block copolymer) obtained in Production Example 1, a silane-modified hydrogenated block copolymer (an alkoxysilyl-modified hydrogenated block copolymer) was obtained by the following method.
[0109] (P2-1. Preparation of silane-modified hydrogenated block copolymer) To 100 parts of the pellets (v) obtained in (P1-1) of Production Example 1, 2.0 parts of vinyltrimethoxysilane and 0.2 parts of di-t-butyl peroxide were added to obtain a mixture. This mixture was kneaded using a twin-screw extruder at a barrel temperature of 210°C and a residence time of 80 to 90 seconds. The kneaded mixture was extruded and cut with a pelletizer to obtain pellets (vi) of the silane-modified hydrogenated block copolymer. A film-shaped test piece was made from this pellet (vi), and the glass transition temperature Tg was evaluated by the tan δ peak of a dynamic viscoelasticity measuring device, and was found to be 124°C. The peak value of tan δ of this pellet (vi) at 40°C to 200°C was 1.3. The Young's modulus of this pellet (vi) at 23°C was 0.5 GPa, and the tensile elongation was 550%. Therefore, the obtained silane-modified hydrogenated block copolymer was a thermoplastic elastomer. The refractive index (n1) of the pellet (vi) measured with an Abbe refractometer was 1.50.
[0110] [Example 1] (Preparing the coating solution) To 10 parts of "Titanium Black" (average primary particle diameter 70 nm, measured by a laser diffraction particle sizer) as material B1, 1 part of a dispersant whose main component is 12-hydroxystearic acid oligomer and 189 parts of cyclohexane were added and dispersed using a paint shaker to prepare a titanium black dispersion. Next, a resin solution was prepared as the transparent material A1 by adding 70 parts of cyclohexane to 30 parts of the pellets (vi) of the silane-modified hydrogenated block copolymer obtained in Production Example 2. 8.4 parts of the titanium black dispersion were added to this solution to prepare a titanium oxide-dispersed resin solution containing 1.4% titanium oxide particles based on the solid content.
[0111] (Light-reducing layer forming process) The resulting titanium black dispersed resin solution was applied to a glass plate using an applicator and dried in an oven at 110°C for 3 minutes to produce a light-reducing layer. The thickness of the light-reducing layer after drying was 20μm.
[0112] The linear transmittance of the light-reducing layer formed on the glass plate was measured in the wavelength range of 400 to 700 nm by the above-mentioned method. As a result, the linear transmittance was 51% at a wavelength of 400 nm, 57% at a wavelength of 500 nm, 52% at a wavelength of 600 nm, and 49% at a wavelength of 700 nm, and it was found that the light-reducing layer had light-shielding properties. In addition, the total light transmittance of the light-reducing layer formed on this glass plate was 61.9%, and the haze value was 17%.
[0113] (Evaluation of light-emitting devices) The diffusion film provided on the viewing side surface of an organic electroluminescent lighting device (organic EL lighting device) (Konica Corporation's "Symfos OLED-010K") was removed. The reflectance of the organic EL lighting device from the viewing side of the device after the diffusion film was removed was measured using a spectrophotometer (JASCO Corporation's "V-570"), and was found to be 28% at a wavelength of 400 nm, 76.5% at a wavelength of 500 nm, 79.5% at a wavelength of 600 nm, and 74% at a wavelength of 700 nm. In addition, when the device was turned on with the diffusion film removed, the brightness was measured at 6.7 lm using an Imaging Sphere device manufactured by Radiant Imaging with an aperture of 3 cmΦ.
[0114] Next, the light-reducing layer was placed on the viewing side surface of the device, and the reflectance was measured; it was 13% at a wavelength of 400 nm, 30% at a wavelength of 500 nm, 28% at a wavelength of 600 nm, and 23% at a wavelength of 700 nm. Furthermore, when the device having the dimming layer disposed thereon was visually observed under an environment of 50 lx, no reflection from the electrodes was observed. Furthermore, when the device with the dimming layer was turned on and the brightness was measured at an aperture of 3 cmΦ, it was 3.6 lm.
[0115] [Example 2] To 10 parts of "Titanium Black" (average primary particle diameter 20 nm, measured by electron microscope) as material B1, 2 parts of a dispersant mainly composed of 12-hydroxystearic acid oligomer and 188 parts of cyclohexane were added and dispersed with a paint shaker to prepare Titanium Black Dispersion Liquid 2. The average particle size of the primary particles of the titanium black used was measured by the following method. The sum of the short axis and long axis of the primary particle of each of the 50 particles was determined by observation using an electron microscope, and the resulting sum was divided by 2 to obtain the arithmetic mean value, which was used as the average particle size. Next, a resin solution was prepared as transparent material A1 by adding 70 parts of cyclohexane to 30 parts of the pellets (vi) of the silane-modified hydrogenated block copolymer obtained in Production Example 2. 17 parts of titanium black dispersion was added to this solution to prepare titanium oxide-dispersed resin solution 2 containing 2.8% titanium oxide particles based on the solid content.
[0116] (Light-reducing layer forming process) The resulting titanium black dispersed resin solution was applied onto a glass plate using an applicator and dried in an oven at 110° C. for 3 minutes to prepare a light-reducing layer 2. The thickness of the light-reducing layer 2 after drying was 7.5 μm.
[0117] The linear transmittance of the light-reducing layer 2 formed on the glass plate was measured in the wavelength range of 400 to 700 nm by the above-mentioned method. As a result, the linear transmittance was 50% at a wavelength of 400 nm, 56% at a wavelength of 500 nm, 50% at a wavelength of 600 nm, and 46% at a wavelength of 700 nm, and it was found that the light-reducing layer had light-shielding properties. In addition, the total light transmittance of the light-reducing layer formed on this glass plate was 60.4%, and the haze value was 13%.
[0118] (Evaluation of light-emitting devices) An organic EL lighting device similar to that in Example 1 was prepared, except that the diffusion film was removed. Next, in the same manner as in Example 1, the dimming layer 2 was placed on the viewing side surface of the device and the reflectance was measured, which was 13% at a wavelength of 400 nm, 28% at a wavelength of 500 nm, 25% at a wavelength of 600 nm, and 20% at a wavelength of 700 nm. Furthermore, when the device having the dimming layer disposed thereon was visually observed under an environment of 50 lx, no reflection from the electrodes was observed. Furthermore, when the device with the dimming layer was turned on and the brightness was measured at an aperture of 3 cmΦ, it was 3.6 lm.
[0119] [Comparative Example 1] (Preparation of coating solution and formation of light-reducing layer) A light-reducing layer was prepared in the same manner as in (preparation of coating solution) and (step of forming light-reducing layer) of Example 1, except for the following changes. The formulation of the titanium black dispersion has been changed to 4.5 parts of "titanium black", 0.5 parts of dispersant, and 195 parts of cyclohexane.
[0120] The linear transmittance of the light-reducing layer formed on the glass plate was measured in the wavelength range of 400 to 700 nm by the above-mentioned method. As a result, the linear transmittance was 66% at a wavelength of 400 nm, 73% at a wavelength of 500 nm, 67% at a wavelength of 600 nm, and 63% at a wavelength of 700 nm, and it was found that the light-reducing layer had light-shielding properties. In addition, the total light transmittance of the light-reducing layer formed on the glass plate was 80.2%, and the haze value was 8%.
[0121] (Evaluation of light-emitting devices) An organic EL lighting device similar to that in Example 1 was prepared, except that the diffusion film was removed. Next, similarly to Example 1, the dimming layer was placed on the viewing side surface of the device and the reflectance was measured, which was 22% at a wavelength of 400 nm, 52% at a wavelength of 500 nm, 50% at a wavelength of 600 nm, and 40% at a wavelength of 700 nm. Furthermore, when the device having the dimming layer disposed thereon was visually observed under an environment of 50 lx, reflection from the electrodes was observed.
[0122] [Reference example 1] In the same manner as in Example 1, 70 parts of cyclohexane was added to 30 parts of the pellets (vi) of the silane-modified hydrogenated block copolymer obtained in Production Example 2 to prepare a resin solution. No titanium black dispersion was added to the resin solution. The resin solution was applied to a glass plate using an applicator and dried to prepare a resin layer. The thickness of the resin layer after drying was 20 μm.
[0123] The linear transmittance of the resin layer formed on the glass plate was measured in the wavelength range of 400 to 700 nm by the above-mentioned method, and the results showed linear transmittance of 92% at wavelength of 400 nm, 92% at wavelength of 500 nm, 92% at wavelength of 600 nm, and 92% at wavelength of 700 nm.
[0124] The linear transmittance of the light-reducing layer obtained in Example 1 is smaller than the linear transmittance of the resin layer obtained in Reference Example 2, which does not contain "Titanium Black," in the visible light range, that is, wavelengths of 400 nm, 500 nm, 600 nm, and 700 nm. Therefore, it is found that "Titanium Black" is a material that can impart the function of attenuating visible light to the light-reducing layer, and is a material that absorbs or reflects visible light.
[0125] [Reference example 2] An organic EL lighting device was prepared from which the diffusion film had been removed, similar to that of Example 1. A circular polarizing plate (transmittance 43.3%, a linear polarizing plate combined with a ¼ wavelength plate (Zeon Corporation's "ZD12")) was placed on the viewing side surface of the device, and the reflectance was measured using a spectrophotometer in the same manner as in Example 1, and was found to be 5.1% at a wavelength of 400 nm, 5.2% at a wavelength of 500 nm, 4.5% at a wavelength of 600 nm, and 7.4% at a wavelength of 700 nm. When the device with the circular polarizing plate disposed thereon was turned on and the brightness was measured with an aperture of 3 cmΦ in the same manner as in Example 1, it was 2.67 lm.
[0126] From the above results, the following points can be seen. In the light-emitting devices of Examples 1 and 2, which include a dimming layer having a total light transmittance of 45% or more and 75% or less, no reflection from the electrodes was observed. On the other hand, in the light emitting device of Comparative Example 1 including a dimming layer with a total light transmittance of more than 75%, reflection from the electrodes was observed. The light emitting device of Example 1 had a brightness of 3.6 lm, and the light emitting device of Example 2 had a brightness of 3.6 lm. On the other hand, the light emitting device of Reference Example 2 including a circular polarizing plate had a brightness of 2.67 lm, which was darker than that of the light emitting device of Example 1. These results show that the light-emitting device of the present invention, which includes a predetermined light-reducing layer, can suppress reflection of external light. [Explanation of symbols]
[0127] 10 Substrate 20 First electrode 30 Light-emitting layer 40 Second electrode 50 Darkening Layer 50U side 60 Light emitting element 100 Light Emitting Devices
Claims
1. A light-emitting element including a reflective element, and a dimming layer arranged on the viewing side of the reflective element and having a total light transmittance of 45% or more and 75% or less, The light-reducing layer includes a transparent material A1, a material B1 that absorbs or reflects visible light, and hygroscopic particles; The content of the hygroscopic particles in the light-reducing layer is 5% by weight or more and 50% by weight or less, the transparent material A1 includes a thermoplastic elastomer, The light emitting device, wherein the thermoplastic elastomer comprises a silane modified hydrogenated aromatic vinyl compound-conjugated diene block copolymer.
2. The light-emitting device of claim 1 , wherein the light-reducing layer has a thickness of 1 μm or more and less than 100 μm.
3. 3. The light-emitting device according to claim 1, wherein the linear transmittance of the light-reducing layer at a wavelength of 500 nm is greater than the linear transmittance at a wavelength of 600 nm.
4. The light-emitting device according to any one of claims 1 to 3, wherein said material B1 comprises at least titanium black.
5. The light-emitting device according to any one of claims 1 to 4, wherein the light-emitting element is an organic electroluminescence element.
6. A method for producing the light-emitting device according to any one of claims 1 to 5, comprising the steps of: A step (1) of preparing a coating liquid including the transparent material A1 or a material for forming the transparent material A1, the material B1 that absorbs or reflects visible light, and a solvent; and (2) forming the light-reducing layer from the coating liquid, The step (2) A step (2a) of applying the coating liquid onto a substrate to form a coating film; and (2b) removing the solvent from the coating film.
Citation Information
Patent Citations
Organic electroluminescent element
JP1996321381A
Organic electroluminescence display device color filter and organic electroluminescence display device
JP2015031863A
Material for electronic device and organic electroluminescence device
JP2019133852A
Optical laminate
WO2018230453A1