Iron oxide magnetic powder and its manufacturing method

The controlled production of ε-Fe2O3 magnetic powders with specific particle size and shape addresses coercive force variations, improving magnetic recording media performance by enhancing recording density and stability.

JP7561557B2Active Publication Date: 2024-10-04DOWA ELECTRONICS MATERIALS CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2020162736
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-09-30
Filing Date
2020-09-28
Publication Date
2024-10-04
Estimated Expiration
2040-09-28

AI Technical Summary

Technical Problem

Existing ε-Fe2O3 magnetic powders for high-density magnetic recording media suffer from variations in coercive force distribution, particle shape irregularities, and high content of fine and coarse particles, which hinder recording density and stability.

Method used

The production method involves controlling the particle size distribution by neutralizing a solution containing trivalent iron ions and metal elements, coating precursor particles with silicon oxide, and heat-treating them to achieve particles with an average diameter of 10-20 nm, circularity of 0.955 or more, and reduced fine and coarse particle content.

Benefits of technology

The method results in magnetic powders with narrow particle size distribution, improved magnetic properties, and enhanced recording density, stability, and reduced noise in electromagnetic conversion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007561557000005
    Figure 0007561557000005
  • Figure 0007561557000006
    Figure 0007561557000006
  • Figure 0007561557000007
    Figure 0007561557000007
Patent Text Reader

Abstract

To provide an iron-based oxide magnetic powder suitable for use in magnetic recording media in which the contents of fine particles and coarse particles are sufficiently reduced and the particle shape is close to a true sphere.SOLUTION: An iron-based oxide magnetic powder obtainable by a process that comprises a step in which (i) a raw material solution that contains a) trivalent iron ions or b) trivalent iron ions and metal element ions partially replacing Fe-sites, (ii) and an alkaline solution for neutralizing the raw material solution, are added to a reaction system to adjust the pH of the reaction system to 1.0-3.0; a step in which a hydroxycarboxylic acid is added to the obtained reaction solution and then the pH of the reaction system is neutralized to 7.0-10.0; and a step in which the resulting precipitate of iron oxyhydroxide containing substituted metal elements is coated with a silicon oxide and then heated, thereby obtaining an iron-based oxide magnetic powder which contains sufficiently reduced amount of fine particles and coarse particles, has a particle shape close to a true sphere, and is composed of ε iron oxide particles in which Fe sites are partially replaced with other metal elements.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an iron-based oxide magnetic powder suitable for high-density magnetic recording media, radio wave absorbers, etc., and in particular to a magnetic powder having an average particle size on the order of nanometers, and a method for producing the same. [Background technology]

[0002] ε-Fe2O3 is an extremely rare phase among iron oxides, but nanometer-sized particles have a thermal conductivity of 20 kOe (1.59 × 10 6 Since ε-Fe2O3 exhibits a huge coercive force (Hc) of about 10 ...

[0003] Meanwhile, in the field of magnetic recording, magnetic recording media with a high ratio of the reproduction signal level to particulate noise (C / N ratio: Carrier to Noise Ratio) are being developed, and in order to increase the recording density, there is a demand for finer magnetic particles that make up the magnetic recording layer. However, in general, finer magnetic particles tend to deteriorate their environmental resistance and thermal stability, and there is concern that the magnetic properties of the magnetic particles may decrease under the usage or storage environment. Therefore, by replacing part of the Fe site of ε-Fe2O3 with other metals with excellent heat resistance, it is possible to obtain a magnetic recording medium with the general formula ε-A x B y Fe 2-x-y O3 or ε-A x B y C z Fe 2-x-y-zVarious partial substitution products of ε-Fe2O3 (where A is a divalent metal element such as Co, Ni, Mn, or Zn, B is a tetravalent metal element such as Ti, and C is a trivalent metal element such as In, Ga, or Al) have been developed that have reduced particle size, variable coercive force, and excellent environmental resistance and thermal stability (Patent Document 3).

[0004] Since ε-Fe2O3 is obtained as a stable phase with a size on the order of nanometers, a special method is required for its production. The above-mentioned Patent Documents 1 to 3 disclose a method for producing ε-Fe2O3 by using fine crystals of iron oxyhydroxide produced by a liquid phase method as a precursor, coating the precursor with silicon oxide by a sol-gel method, and then heat-treating the precursor. As the liquid phase method, a reverse micelle method using an organic solvent as a reaction medium and a method using only an aqueous solution as a reaction medium are disclosed. However, since the magnetic properties of ε-Fe2O3 or partially substituted ε-Fe2O3 obtained by these methods vary, it has been proposed to improve their magnetic properties by removing the silicon oxide coating after heat treatment and performing a classification process.

[0005] The ε-Fe2O3 or ε-type iron oxide partially substituted with Fe produced by the conventional production methods disclosed in the above Patent Documents 1 to 3 has excellent magnetic properties, but depending on the production conditions, there are cases where variation in coercive force distribution is observed. In response to the problem of variation in coercive force distribution, Patent Document 4 discloses a method for producing an ε-type iron oxide magnetic particle powder containing a substitution metal element, which comprises adding an alkali to an aqueous solution containing trivalent iron ions and ions of metal M partially substituting Fe sites to neutralize the pH to pH 1.0 to 3.0, adding hydroxycarboxylic acid D in an amount of 0.125 to 1.0 in terms of a molar ratio D / Fe to the amount of trivalent iron ions or a molar ratio (D / (Fe+M)) to the total amount of trivalent iron ions and ions of the substitution metal M, further adding an alkali to neutralize the pH to pH 7.0 to 10.0, and covering the resulting iron oxyhydroxide containing the substitution metal element with silicon oxide and heating it. Hydroxycarboxylic acids, which are carboxylic acids that have an OH group in their molecule, form complexes with the trivalent iron ions dissolved in the reaction solution, delaying the reaction that forms iron hydroxide when further alkali is added in the next step, and are said to have the effect of narrowing the distribution of the average particle size of the precursor microparticles containing iron oxyhydroxide that are generated as a result. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2008-174405 A [Patent Document 2] International Publication No. 2008 / 029861 [Patent Document 3] International Publication No. 2008 / 149785 [Patent Document 4] JP 2017-024981 A Summary of the Invention [Problem to be solved by the invention]

[0007] The ε-type iron-based oxide magnetic powder containing substitutional metal elements produced by the manufacturing method disclosed in Patent Document 4 had a narrow particle size distribution and a low content of fine particles that do not contribute to magnetic recording characteristics, and as a result was excellent in that it had a narrow coercive force distribution. However, there was still room for improvement in order to increase the recording density of magnetic recording media. When applying ε-type iron oxide magnetic powder to a magnetic recording medium, it is desirable not only to control the average particle size but also to reduce the proportion of fine particles and coarse particles whose particle size is far from the average value as much as possible. The presence of fine particles, even if their volume ratio in the magnetic powder is small, causes an increase in noise in the electromagnetic conversion characteristic SNR of the magnetic recording medium. In addition, coarse particles have too high a coercive force and cannot be written by a magnetic head, and if their proportion is high, it causes a decrease in magnetic recording density. The ε-type iron oxide magnetic powder containing a substituted metal element manufactured by the manufacturing method disclosed in Patent Document 4 cannot be said to have a sufficiently reduced content of the fine particles and coarse particles, and there are still problems in increasing the recording density of magnetic recording media.

[0008] Furthermore, there is also a problem that the ε-type iron-based oxide magnetic powder containing a substitution metal element produced by the production method disclosed in Patent Document 4 has an irregular particle shape. If the particle shape is irregular, the uneven parts of the particles may interfere with each other and hinder the orientation of the particles when the particles are magnetically oriented during the production of a magnetic recording medium, so it is desirable for the particle shape to be as close to a perfect sphere as possible.

[0009] In view of the above problems, the present invention provides an iron-based oxide magnetic powder consisting of ε-iron oxide particles in which part of the Fe sites is substituted with other metal elements, the content of fine particles and coarse particles being sufficiently reduced and the particle shape being nearly spherical, suitable for use in magnetic recording media, and a method for producing the iron-based oxide magnetic powder. [Means for solving the problem]

[0010] In order to solve the above problems, the present invention provides (1) Provided is an iron-based oxide magnetic powder consisting of epsilon-iron oxide particles in which some of the Fe sites have been substituted with other metal elements, the powder having an average particle size measured by a transmission electron microscope of 10 nm or more and 20 nm or less, the percentage of particles having a particle size of 8 nm or less being 5% or less, the percentage of particles having a particle size of 20 nm or more being 25% or less, and the average circularity of the particles observed by a transmission electron microscope being 0.955 or more. (2) The coefficient of variation of particle size of the ε-iron oxide particles in which a portion of the Fe sites is substituted with another metal element, as measured by a transmission electron microscope, is preferably 20% or more and 30% or less. (3) The metal element substituting a portion of the Fe sites is preferably one or more of Ga, Co, and Ti. (4) The metal element substituting a portion of the Fe site may be one or more of Ga, Co, Ti, Ni, Mn, Cr, Nd, Dy and Gd.

[0011] In the present invention, (5) A method for producing an iron-based oxide magnetic powder comprising particles of ε-iron oxide or ε-iron oxide in which a part of the Fe site is substituted with another metal element, the particles having an average particle diameter of 10 nm or more and 20 nm or less as measured by a transmission electron microscope, A raw solution preparation step of preparing an aqueous solution containing trivalent iron ions or trivalent iron ions and ions of a metal element that substitutes a part of the Fe site (hereinafter referred to as a raw solution) and an alkaline aqueous solution for neutralizing the raw solution; a first neutralization step of continuously or intermittently adding and mixing the raw material solution and the aqueous alkaline solution to a reaction system to adjust the pH of the reaction system to 1.0 or more and 3.0 or less; adding a hydroxycarboxylic acid to the aqueous solution after the first neutralization step; a second neutralization step of adding an alkali to the aqueous solution containing the hydroxycarboxylic acid to neutralize the pH to 7.0 or more and 10.0 or less to obtain a slurry containing a precipitate of iron oxyhydroxide or iron oxyhydroxide containing a substituted metal element; a step of adding a silicon compound having a hydrolyzable group to a slurry containing the iron oxyhydroxide or the iron oxyhydroxide containing a substitution metal element, and coating the iron oxyhydroxide or the iron oxyhydroxide containing a substitution metal element with a hydrolysis product of the silicon compound; heating the iron oxyhydroxide or iron oxyhydroxide containing a substituted metal element coated with the hydrolysis product of a silicon compound to obtain epsilon iron oxide coated with silicon oxide or epsilon iron oxide in which a portion of the Fe site is substituted with another metal element; The present invention provides a method for producing an iron-based oxide magnetic powder, comprising the steps of: (6) The first neutralization step described in the above item (5) is preferably a step in which the raw material solution and the aqueous alkaline solution containing 0.4 equivalents or more and 0.9 equivalents or less of alkali relative to the sum of the amounts of acid radicals contained in the raw material solution are added continuously or intermittently to a reaction system not containing trivalent iron ions and ions of a metal element substituting a part of the Fe sites, and mixed to adjust the pH of the reaction system to 1.0 or more and 3.0 or less. (7) The first neutralization step described in (5) above may be a step in which, when the raw material solution and the aqueous alkali solution are each continuously or intermittently added to a reaction system already containing trivalent iron ions, or trivalent iron ions and ions of a metal element substituting a portion of the Fe sites, the amount of trivalent iron ions and ions of a metal element already contained in the reaction system is 50 mol % or less of the sum of the amount of the trivalent iron ions and ions of a metal element substituting a portion of the Fe sites and the amount of the trivalent iron ions and ions of a metal element substituting a portion of the Fe sites contained in the raw material solution added to the reaction system, the raw material solution and the aqueous alkali solution containing 0.4 equivalents to 1.8 equivalents of alkali with respect to the sum of the amounts of acid radicals contained in the raw material solution are each continuously or intermittently added to the reaction system and mixed, to adjust the pH of the reaction system to 1.0 to 3.0. (8) In the first neutralization step of the above item (6), it is preferable to adjust the addition rates of the raw material solution and the aqueous alkali solution so that the cumulative amount of the aqueous alkali solution added relative to the total cumulative amount of acid radicals contained in the raw material solution is maintained in the range of 0.4 equivalents or more and 0.9 equivalents or less throughout the step. (9) In the first neutralization step of the above item (5), it is preferable to add the raw material solution and the alkaline aqueous solution over a period of 10 minutes or more. (10) The slurry containing iron oxyhydroxide or iron oxyhydroxide containing a substituted metal element obtained in the second neutralization step in (5) above preferably has an average particle size of 300 nm or less as measured with a dynamic light scattering particle size distribution analyzer. (11) As a source of the trivalent iron ion contained in the raw material solution of the above item (5), it is preferable to use iron(III) chloride. (12) The cumulative amount of alkali added relative to the total cumulative amount of acid radicals added in the raw solution of (6) above is preferably 0.6 equivalents or more and 0.9 equivalents or less throughout the first neutralization step. (13) The cumulative amount of alkali added relative to the total cumulative amount of acid radicals added in the raw solution of (7) above is preferably 0.4 equivalents or more and 1.8 equivalents or less throughout the first neutralization step. Effect of the Invention

[0012] By using the manufacturing method of the present invention, it is possible to obtain an iron-based oxide magnetic powder in which the content of fine particles and coarse particles that do not contribute to improving magnetic recording characteristics is sufficiently reduced, and the particle shape is close to spherical, making it suitable for use in magnetic recording media. [Brief description of the drawings]

[0013] [Figure 1] 1 is a TEM photograph of the iron-based oxide magnetic powder obtained in Example 1. [Diagram 2] 1 is a TEM photograph of the iron oxyhydroxide crystals containing a substitution element obtained in Example 1. [Diagram 3]1 is a TEM photograph of the iron oxyhydroxide crystals containing a substitution element obtained in Comparative Example 1. [Figure 4] 3 is a TEM photograph of the iron-based oxide magnetic powder obtained in Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] [Iron-based oxide magnetic powder] The iron-based oxide magnetic powder obtained by the present invention is composed of ε-iron oxide particles, or ε-iron oxide particles in which part of the Fe site is substituted with other metal elements (hereinafter, may be referred to as substituted ε-iron oxide particles). The magnetic powder may contain a different phase (e.g., α-Fe2O3 in which part of the Fe site is substituted with other metal elements) that is unavoidable in the manufacturing process. It is possible to confirm that the magnetic powder is composed of ε-iron oxide particles in which part of the Fe site is substituted with other metal elements using X-ray diffraction (XRD), high-energy electron diffraction (HEED), etc.

[0015] Substituted ε-iron oxide particles that can be produced by the production method of the present invention include the following. General formula ε-C z Fe 2-z O3 (where C is one or more trivalent metallic elements selected from In, Ga, Al, Cr, Nd, Dy, and Gd). General formula ε-A x B y Fe 2-x-y O3 (wherein A is one or more divalent metallic elements selected from Co, Ni, Mn, and Zn, and B is one or more tetravalent metallic elements selected from Ti and Sn). General formula ε-A x C z Fe 2-x-z O3 (where A is one or more divalent metallic elements selected from Co, Ni, Mn, and Zn, and C is one or more trivalent metallic elements selected from In, Ga, Al, Cr, Nd, Dy, and Gd). General formula ε-B y C z Fe 2-y-zO3 (wherein B is one or more tetravalent metallic elements selected from Ti and Sn, and C is one or more trivalent metallic elements selected from In, Ga, Al, Cr, Nd, Dy, and Gd). General formula ε-A x B y C z Fe 2-x-y-z O3 (wherein A is one or more divalent metal elements selected from Co, Ni, Mn, and Zn, B is one or more tetravalent metal elements selected from Ti and Sn, and C is one or more trivalent metal elements selected from In, Ga, Al, Cr, Nd, Dy, and Gd). From the viewpoint of the balance between magnetic properties and thermal stability, the metal element substituting a part of the Fe site is preferably one or more of Ga, Co and Ti. In addition to Ga, Co and Ti, one or more of Ni, Mn, Cr, Nd, Dy and Gd can be used as the substituting element.

[0016] [Particle size] The ε iron oxide particles or substituted ε iron oxide particles constituting the iron-based oxide magnetic powder of the present invention preferably have an average particle diameter measured by a transmission electron microscope (hereinafter sometimes referred to as the TEM average particle diameter) of 10 nm or more and 20 nm or less. If the TEM average particle diameter is 20 nm or less, the electromagnetic conversion characteristics can be improved when the iron-based oxide magnetic powder is used in a magnetic recording medium. The TEM average particle diameter is preferably 17 nm or less. If the TEM average particle diameter of the ε iron oxide particles or substituted ε iron oxide particles becomes small, the proportion of fine particles that do not contribute to improving the magnetic characteristics increases, and the magnetic characteristics per unit mass of the magnetic powder deteriorate, so the TEM average particle diameter is preferably 10 nm or more.

[0017] The iron-based oxide magnetic powder of the present invention is characterized in that, for the ε-iron oxide particles or substituted ε-iron oxide particles, the proportion of particles having a particle diameter of 8 nm or less as measured by a transmission electron microscope (hereinafter sometimes referred to as TEM particle diameter) is 5% or less, and the proportion of particles having a TEM particle diameter of 20 nm or more is 25% or less. ε-iron oxide particles or substituted ε-iron oxide particles with a TEM particle diameter of 8 nm or less have a low coercive force and therefore do not contribute to magnetic recording even if present in a magnetic recording medium, and may instead lead to an increase in noise components in the electromagnetic conversion characteristics of the magnetic recording medium. Therefore, it is preferable that the number ratio of particles with a TEM particle diameter of 8 nm or less in the ε-iron oxide particles or substituted ε-iron oxide particles is as small as possible. Since the number ratio of particles with a TEM particle diameter of 8 nm or less in the iron-based oxide magnetic powder of the present invention is 5% or less, the amount of noise components in the electromagnetic conversion characteristics when the iron-based oxide magnetic powder is used in a magnetic recording medium can be reduced compared to when a conventional iron-based oxide magnetic powder is used. In addition, in the iron-based oxide magnetic powder consisting of ε-iron oxide particles or substituted ε-iron oxide particles having a TEM average particle size of 10 nm or more and 20 nm or less, ε-iron oxide particles or substituted ε-iron oxide particles having a TEM particle size of 20 nm or more have a larger coercive force than particles having an average particle size, so that even if they are present in a magnetic recording medium, magnetic recording cannot be written by a magnetic head, and they are particles that do not contribute to magnetic recording, so they may lead to a decrease in the magnetic recording density of the medium. Therefore, it is preferable that the number ratio of particles of 20 nm or more is small. Since the number ratio of particles having a TEM particle size of 20 nm or more in the iron-based oxide magnetic powder of the present invention is 25% or less, the magnetic recording density when the iron-based oxide magnetic powder is used in a magnetic recording medium can be improved compared to the case of using conventional iron-based oxide magnetic powder.

[0018] The iron-based oxide magnetic powder of the present invention preferably has a particle size coefficient of variation of 20% or more and 30% or less for the ε-iron oxide particles or substituted ε-iron oxide particles constituting the magnetic powder. Setting the particle size coefficient of variation to 20% or more and 30% or less is advantageous for improving the electromagnetic conversion characteristics when the iron-based oxide magnetic powder is used in a magnetic recording medium.

[0019] [Average circularity] In the present invention, the particle shape of the ε iron oxide particles or substituted ε iron oxide particles is evaluated by the average circularity of the particles observed under a transmission electron microscope, as defined below. Circularity is a concept for evaluating how close the shape of a certain particle is to a perfect sphere, and refers to a value obtained by dividing the product of the projected area of ​​the particle and 4π by the square of the perimeter of the projected image of the particle, and takes a value of 0 to 1. In the case of a perfect circle, the circularity is 1. The method for measuring circularity will be described later, but for the substituted ε iron oxide particles, the number of particles for which the circularity is measured is increased and the average value is calculated, so that the deviation of the ε iron oxide particles or substituted ε iron oxide particles from a perfect sphere can be evaluated. The ε-iron oxide particles or substituted ε-iron oxide particles constituting the iron-based oxide magnetic powder of the present invention preferably have an average particle circularity of 0.955 or more as observed by a transmission electron microscope. If the average particle circularity is 0.955 or more, when a magnetic recording medium is manufactured by orienting the ε-iron oxide particles or substituted ε-iron oxide particles by an external magnetic field, the substituted ε-iron oxide particles are more likely to be oriented, which results in an improvement in the magnetic recording density of the magnetic recording medium. It is more preferable that the average particle circularity observed by a transmission electron microscope is 0.96 or more.

[0020] [Method of manufacturing iron-based oxide magnetic powder] In the method for producing the iron-based oxide magnetic powder of the present invention, the precursor particles, which are precursors of the ε iron oxide particles or substituted ε iron oxide particles, are characterized by having a larger particle size and better dispersibility than precursor particles obtained by conventional known production methods. The present inventors presume that in the precursor particle production process disclosed in Patent Document 4, very fine precursor particles with a particle size of 1 nm or less are produced, and the precursor particles are coated with a silicon compound in a state of agglomeration to the order of several tens of nm and then subjected to a firing process, resulting in the formation of iron-based oxide particles with an average particle size of about 10 to 30 nm. In the production method disclosed in Patent Document 4, it is difficult to arbitrarily control the degree of agglomeration of the precursor particles, and it is considered that only iron-based oxide magnetic powders with a wide particle size distribution were obtained as a result. In the production method of the present invention, precursor particles with a large particle size and good dispersibility are obtained by improving the production method of the precursor particles, and it is believed that by using such a precursor, the ratio of particles finer than the average particle size or coarse iron-based oxide particles produced can be reduced, and ε iron oxide particles or substituted ε iron oxide particles with a particle shape closer to a true sphere can be obtained.

[0021] [Starting materials] In the method for producing the iron-based oxide magnetic powder of the present invention, an acidic aqueous solution (raw material solution) containing trivalent iron ions or trivalent iron ions and metal ions of a metal element that will eventually replace the Fe site of the ε-iron oxide particles is used as a starting material for the iron-based oxide magnetic particles. In this specification, acidic refers to a pH of 7 or less. As a supply source of these iron ions or metal ions of the replacement element, water-soluble inorganic acid salts such as nitrates, sulfates, and chlorides can be used in terms of ease of availability and cost. In order to finally obtain ε-iron oxide particles or substituted ε-iron oxide particles, it is preferable to go through β-FeOOH as a precursor, and since halogen ions are necessary to obtain β-FeOOH as the crystal structure of the precursor, it is preferable to use iron(III) chloride among the iron salts exemplified. When using nitrates or sulfates, the desired precursor can be obtained by adding halogen ions using hydrochloric acid, hydrofluoric acid, or the like. In the production method of the present invention, in the raw solution preparation step, the raw solution and an aqueous alkali solution to be used for neutralizing the raw solution in the first neutralization step described below are prepared in advance. The alkali for neutralizing the raw solution may be any of alkali metal or alkaline earth hydroxides, ammonia water, and ammonium salts such as ammonium hydrogen carbonate, but it is preferable to use ammonia water or ammonium hydrogen carbonate, which are unlikely to leave impurities when the raw solution is finally heat-treated to form ε-iron oxide particles or substituted ε-iron oxide particles.

[0022] [First neutralization step] The most important technical feature of the method for producing the iron-based oxide magnetic powder of the present invention is that in the first neutralization step, the raw material solution obtained in the previous step and an alkaline aqueous solution for neutralizing it are added to the reaction system, which will be described later. In the conventional method for producing iron-based oxide magnetic powders consisting of ε-iron oxide particles or substituted ε-iron oxide particles using an aqueous solution, an alkaline aqueous solution is normally added continuously to the entire amount of the raw material solution used in the reaction. In this case, a time lag occurs between the addition of the alkaline aqueous solution and the reaction system becoming homogeneously mixed, and metal ions and OH groups are generated in the reaction system. - It is presumed that local fluctuations in the composition ratio of ions locally caused local changes in the generation frequency and particle size of the aforementioned precursors generated by the neutralization reaction, making it difficult to control the degree of aggregation of the precursor particles. In contrast, in the first neutralization step in the production method of the present invention, the concentrations of the raw material solution and the alkaline aqueous solution to be added and the addition rates thereof to the reaction system can be changed arbitrarily, so that the metal ions and OH groups in the reaction system can be neutralized. - It becomes possible to more uniformly control the composition ratio of ions, and precursor particles having a large particle size and good dispersibility can be obtained, resulting in an iron-based oxide magnetic powder having a narrow particle size distribution.

[0023] In the first neutralization step of the production method of the present invention, the raw material solution and the alkaline aqueous solution obtained in the previous step are added to the reaction system continuously or intermittently and mixed, and the pH of the reaction system is adjusted to 1.0 to 3.0. Although the detailed crystal structure is unknown in the aqueous solution obtained by mixing the raw material solution and the alkaline aqueous solution, it is believed that extremely fine particles of oxyhydroxide of trivalent iron or a substituted metal element, hydroxide of trivalent iron or a substituted metal element, or a mixture thereof are generated to form a colloidal solution. In the production method of the present invention, the metal ions and OH in the reaction system are mixed. - Since the composition ratio of ions can be precisely controlled, it becomes possible to control the state in which the colloidal particles are generated to a desired state. In this specification, the reaction system refers to a reaction solution in which a raw material solution and an alkaline aqueous solution are mixed and a neutralization reaction occurs. In the first embodiment of the present invention, the first neutralization step is typically started by simultaneously adding the raw material solution and the alkaline aqueous solution to pure water, which is a reaction system that does not contain trivalent iron ions and ions of metal elements that substitute for a part of the Fe sites. In this case, the reaction system at the very beginning is pure water, and the reaction system after the start of the addition of the raw material solution and the alkaline aqueous solution becomes a reaction solution in which the pure water, the raw material solution, and the alkaline aqueous solution are mixed. In the first embodiment of this production method, the raw material solution and the alkaline aqueous solution may be added simultaneously directly to an empty reaction vessel for containing the reaction solution. In this case, the reaction system is a mixed solution of the raw material solution and the alkaline aqueous solution. In a second embodiment of the manufacturing method of the present invention, the initial reaction system is an acidic metal salt solution containing trivalent iron ions or trivalent iron ions and ions of a metal element that replaces a part of the Fe site, and the raw material solution and an alkali are added to this metal salt solution at the same time. Here, the type of metal salt contained in the metal salt solution may be the same as the form of the metal salt contained in the raw material solution described above. In this case, the amount of metal ions contained in the metal salt solution, which is the initial reaction system, is preferably 50 mol % or less of the total amount of metal ions contained in the metal salt solution and the amount of metal ions contained in the raw material solution added in the first neutralization step.

[0024] In the first neutralization step of the first embodiment of the production method of the present invention, an aqueous alkali solution containing 0.4 to 0.9 equivalents of alkali relative to the sum of the amounts of the raw solution and the acid radicals contained in the raw solution is added to adjust the pH of the reaction system to 1.0 to 3.0. In the case of chlorides, the acid radical is Cl. - , and NO3 in the case of nitrates. - , and SO4 in the case of sulfates. 2- Refers to... In this case, the equivalent [moles of alkali used for neutralization × alkali valence] / [(moles of acid radicals contained in raw solution × valence of acid radicals)] Here, the alkali valence is the number of OH atoms stoichiometrically generated from 1 mol of alkali. - The number of moles of an ion. For example, the alkali valences of NaOH, Ca(OH)2, and NH3 are 1, 2, and 1, respectively. The valence of an acid radical is the valence of an anion of the acid radical. For example, chloride Cl - , Nitrate NO3 - and sulfate SO4 2- The valences of the acid radicals are 1, 1, and 2, respectively. If the amount of alkali added is less than 0.4 equivalents, the amount of colloid generated by neutralization of the raw solution is reduced, and the effect of the present invention cannot be obtained, which is not preferable. If the amount of alkali added is more than 0.9 equivalents, the dispersibility of the resulting colloidal solution is deteriorated, and the effect of the present invention cannot be obtained, which is not preferable. If the pH after neutralization is less than 1.0, the amount of colloid generated by neutralization of the raw solution is reduced, and the effect of the present invention cannot be obtained, which is not preferable. If the pH after neutralization is more than 3.0, the dispersibility of the resulting colloidal solution is deteriorated, and the effect of the present invention cannot be obtained, which is also not preferable. The pH values ​​described in this specification were measured using a glass electrode based on JIS Z8802. The pH standard solution refers to a value measured using a pH meter calibrated with an appropriate buffer solution according to the pH range to be measured. The pH values ​​described in this specification are values ​​directly read from the pH meter compensated by a temperature compensation electrode under reaction temperature conditions.

[0025] The raw material solution and the alkaline aqueous solution may be added continuously or intermittently. The rate of addition of the raw material solution and the alkaline aqueous solution may be constant or may be changed during the process. The raw material solution and the alkaline aqueous solution are added at the same time, but the addition of either the raw material solution or the alkaline aqueous solution may be completed first, and there may be a time when only the other is added. In the first neutralization step of the production method of the present invention, the raw material solution and the aqueous alkali solution are added to the reaction system continuously or intermittently, so it is preferable to control the addition rate of each of them using the concept of "cumulative alkali addition equivalent", which is the number of equivalents of the cumulative addition amount of alkali to 1 equivalent of the total cumulative addition amount of acid radical. [The cumulative amount of alkali moles used for neutralization × alkali valence] / [(The cumulative amount of acid radicals in moles contained in the raw solution × the valence of acid radicals)] It can be expressed as: In the first neutralization step of the first embodiment of the production method of the present invention, it is preferable to adjust the addition rates of the raw material solution and the aqueous alkali solution so that the cumulative alkali addition equivalent is maintained in the range of 0.4 equivalents to 0.9 equivalents throughout the first neutralization step, and more preferably, the cumulative alkali addition equivalent is 0.6 equivalents to 0.9 equivalents throughout the first neutralization step. Strictly speaking, if the timings at which the addition of the raw material solution and the aqueous alkaline solution is started are not exactly the same, the cumulative equivalent of the added alkali may not be 0.4 or more and 0.9 or less equivalents at the very beginning of the reaction. In such a case, the timings at which the addition of the raw material solution and the aqueous alkaline solution is started are deemed to be exactly the same.

[0026] By adjusting the cumulative alkali addition equivalent in the first neutralization step to 0.4 equivalents or more throughout the first neutralization step, it is possible to prevent the free trivalent iron ion concentration in the reaction system from increasing, and therefore the number of precursor core particles formed when an alkali is added to the reaction system can be reduced. As a result, the particle size of the colloid contained in the colloidal solution obtained in the first neutralization step can be made larger than that in Patent Document 4, and the particle size of the precursor particles of the ε iron oxide particles or substituted ε iron oxide particles obtained in the subsequent second neutralization step can be made larger. If the cumulative alkali addition equivalent is not maintained at 0.4 equivalents or more and there is a period when it becomes less than 0.4 equivalents, the particle size of the colloid contained in the colloidal solution obtained in the first neutralization step becomes small, and as a result, the effect of the present invention cannot be obtained.

[0027] By adjusting the cumulative alkali addition equivalent in the first neutralization step to 0.9 equivalents or less throughout the first neutralization step, the pH of the reaction system can be prevented from exceeding 3.0, and the precursor particles can grow in a dispersed state in the reaction system. As a result, precursor particles with good dispersibility (i.e., little interparticle aggregation) and narrow particle size distribution can be obtained in the subsequent second neutralization step. If the cumulative alkali addition equivalent is not maintained at 0.9 equivalents or less and there is a period when it exceeds 0.9 equivalents, the dispersibility of the colloidal solution obtained in the first neutralization step becomes poor (i.e., there is a lot of interparticle aggregation), and as a result, the effect of the present invention cannot be obtained.

[0028] In the first neutralization step of the second embodiment of the production method of the present invention, the raw material solution and an aqueous alkali solution containing 0.4 to 1.8 equivalents of alkali relative to the sum of the amounts of acid radicals contained in the raw material solution are added to adjust the pH of the reaction system to 1.0 to 3.0. In the first neutralization step of the second embodiment of the production method of the present invention, it is preferable to adjust the addition rates of the raw material solution and the aqueous alkali solution so that the cumulative alkali addition equivalent is maintained in the range of 0.4 to 1.8 equivalents and the pH of the reaction system is maintained in the range of 3.0 or less (preferably 0.0 or more) throughout the neutralization step, and the pH is adjusted to 1.0 to 3.0 at the end of the first neutralization step.

[0029] The total metal ion concentration in the raw solution is not particularly specified in the present invention, but it is preferable to adjust the total concentration after the addition of alkali in the second neutralization step to 0.01 mol / kg or more and 0.5 mol / kg or less. If it is less than 0.01 mol / kg, the amount of iron-based oxide magnetic powder obtained in one reaction is small, which is not economically preferable. If the total metal ion concentration exceeds 0.5 mol / kg, the reaction solution is likely to gel due to rapid hydroxide precipitation, which is not preferable. The alkali concentration of the alkaline aqueous solution, in other words, the pH of the alkaline aqueous solution, is also appropriately adjusted based on the same idea. In the first neutralization step of the production method of the present invention, the raw material solution and the alkaline aqueous solution are added to the reaction system over a period of 10 minutes or more and mixed. If the addition time is less than 10 minutes, the core particles of the precursor are generated all at once immediately after the addition, and the ions that would have been used for the core growth are consumed, resulting in a small size of the precursor, which is undesirable in terms of obtaining the effects of the present invention. Although the particle size of the colloid obtained in the first neutralization step can be controlled by extending the addition time, extending the time too much is not preferable because it reduces productivity. Therefore, the addition time is preferably 10 min to 480 min, more preferably 60 min to 300 min. In the production method of the present invention, the treatment temperature during the first neutralization treatment is not particularly limited, but is preferably 20°C or higher and 60°C or lower.

[0030] [Hydroxycarboxylic acid addition process] In the manufacturing method of the present invention, a hydroxycarboxylic acid is added to the colloidal solution obtained in the first neutralization step described above. The hydroxycarboxylic acid is a carboxylic acid having an OH group in the molecule, and acts as a complexing agent for iron ions. Here, the hydroxycarboxylic acid forms a complex with the trivalent iron ions dissolved in the reaction solution, and is considered to have the effect of delaying the reaction of forming iron hydroxide when the second neutralization treatment is performed in the next step, thereby narrowing the distribution of the average particle size of the precursor fine particles containing iron oxyhydroxide that are generated as a result. It is considered that the hydroxycarboxylic acid also forms a partial complex with the metal ion of the substitution element. The type and amount of the hydroxycarboxylic acid to be added may follow the known technology of Patent Document 4. There are many types of hydroxycarboxylic acids, including glycolic acid, lactic acid, various hydroxybutyric acids, glyceric acid, malic acid, tartaric acid, citric acid, and mevalonic acid. From the viewpoint of complexing ability, polyvalent aliphatic hydroxycarboxylic acids are preferred, and from the viewpoints of cost and availability, tartaric acid, citric acid, and malic acid are more preferred. The amount of hydroxycarboxylic acid added is preferably such that the molar ratio (D / (Fe+M)) of the amount of hydroxycarboxylic acid to the combined amount of trivalent iron ions and ions of the substituting metal element M is 0.125 or more and 1.0 or less. The hydroxycarboxylic acid may be added under mechanical stirring without changing the reaction temperature in the first neutralization step, which is the preceding step. It may be added to the reaction solution in the form of a solid, but it is preferable to add it in the form of an aqueous solution in order to ensure the uniformity of the reaction.

[0031] [Second neutralization process] In the production method of the present invention, an alkali is further added to the reaction solution after the addition of the hydroxycarboxylic acid, and the reaction solution is neutralized until the pH is 7.0 or more and 10.0 or less. The alkali to be added can be the same aqueous alkali solution used in the first neutralization step, but a solution with a different alkali concentration can also be used. In this step, the nuclei of the iron oxyhydroxide, which is a precursor of the ε-iron oxide particles or substituted ε-iron oxide particles generated in the first neutralization step, grow to form the final precursor particles. In this step, by making the pH after neutralization 7.0 or more and 10.0 or less, when the trivalent iron and the replacing metal element are neutralized, it is possible to obtain an iron oxyhydroxide containing the replacing metal element as a solid without leaving the dissolved ions of the trivalent iron and the replacing metal element in the reaction solution. If the pH after neutralization is less than 7.0, the replacing metal element that was not completely neutralized in the first neutralization step, such as Co, remains as ions in the solution, causing a composition shift in the recovered solid, and the replacing metal element is wasted, which is not preferable from the viewpoint of production cost. In addition, if the pH after neutralization exceeds 10.0, the neutralization effect is saturated, and when an amphoteric metal such as Al is used as the replacing metal element, there are problems such as ions remaining in the solution, composition shift, and replacing metal element being wasted, as in the case of a pH of less than 7.0, which is not preferable. The iron oxyhydroxide particles or substituted metal element-containing iron oxyhydroxide particles (precursor particles) contained in the slurry obtained in this step preferably have an average diameter measured by a dynamic light scattering particle size distribution analyzer (hereinafter sometimes referred to as DLS average diameter) of 300 nm or less, more preferably 100 nm or less, and even more preferably 70 nm or less. Such a small DLS average diameter means that the precursor particles have good dispersibility and a low degree of aggregation, which is advantageous for reducing the proportion of coarse particles having a particle diameter of 20 nm or more for the ε iron oxide particles or substituted ε iron oxide particles that constitute the finally obtained iron-based oxide magnetic powder. There is no particular restriction on the lower limit of the DLS average diameter of the slurry containing the precursor particles, but the production method of the present invention can obtain particles of about 20 nm or more.

[0032] [Washing process] In the manufacturing method of the present invention, the precursor iron oxyhydroxide produced in the above steps has a small DLS average diameter and high dispersibility. However, the ionic strength in the solution increases as the hydroxycarboxylic acid addition step and neutralization step are carried out in the previous steps. If the ionic strength remains high, it will become an aggregated system in the subsequent silicon oxide coating step, which is not preferable. Therefore, it is preferable to wash the slurry obtained in the above step with water to reduce the ionic strength in the solution and make it in a dispersed state. There is no particular restriction on the method of washing, but in consideration of the maintenance of particle dispersibility in this step, washing uniformity, connection with previous and subsequent steps, and handleability, a method of washing with water while the slurry is in a state of being in a slurry state is preferable. Considering these points, washing with water using an ultrafiltration membrane or an ion exchange membrane is preferable. In the case of washing with an ultrafiltration membrane, a membrane with a molecular weight cutoff that does not allow particles to pass through to the filtrate side is used, and it is preferable to end the washing until the electrical conductivity of the filtrate is 200 mS / m or less, more preferably 100 mS / m or less, and even more preferably 30 mS / m or less. If there are a large number of residual ions, the melting point of the silicon oxide will be locally decreased in the subsequent heating step, which will lead to a problem that sintering will occur when obtaining ε-iron oxide, resulting in the formation of coarse particles.

[0033] [Silicon oxide coating process] In the manufacturing method of the present invention, since the precursor particles generated in the above steps are unlikely to undergo a phase change to substituted ε-iron oxide particles even if they are subjected to a heat treatment in their original state, the precursor particles are coated with a silicon oxide prior to the heat treatment. As a method for coating with silicon oxide, it is preferable to apply a sol-gel method. Note that the silicon oxide here includes not only those with a stoichiometric composition, but also those with a non-stoichiometric composition such as silanol derivatives described later.

[0034] In the case of the sol-gel method, a silicon compound having a hydrolyzable group, for example, tetraethoxysilane (TEOS), tetramethoxysilane (TMOS), or a silane compound such as various silane coupling agents, is added to the aqueous solution of dispersed iron oxyhydroxide crystals or iron oxyhydroxide crystals containing a substitution element after the precursor reaction, and a hydrolysis reaction is caused under stirring, and the surface of the iron oxyhydroxide crystals is coated with the generated silanol derivative. An acid catalyst or an alkali catalyst may also be added. Considering the processing time, it is preferable to add them. A typical example of an acid catalyst is hydrochloric acid, and an alkali catalyst is ammonia. When an acid catalyst is used, it is necessary to add only an amount that does not dissolve the iron oxyhydroxide particles or the iron oxyhydroxide particles containing a substitution element. The specific method for coating with silicon oxide can be the same as that of the sol-gel method in the known process. For example, the reaction temperature for coating with silicon oxide by the sol-gel method is 20°C to 60°C, and the reaction time is about 1 hour to 20 hours. After the coating process with silicon oxide, solid-liquid separation and drying are performed to obtain a sample before the heating process. After the coating process, water washing may be performed before solid-liquid separation. In addition, a flocculant may be added during solid-liquid separation.

[0035] [Heating process] In the manufacturing method of the present invention, the precursor particles coated with silicon oxide are heat-treated to obtain ε-iron oxide particles or substituted ε-iron oxide particles. Before the heat treatment, a washing and drying step may be performed. The heat treatment is performed in an oxidizing atmosphere, which may be an air atmosphere. The heat treatment temperature varies depending on the amount of silicon oxide coating, so it is not a general rule, but the heating can be performed in the range of about 700°C to 1300°C. If the heating temperature is too low, different phases or compounds with insufficient phase transformation are likely to be mixed. If the lower limit of the heating temperature is set to 700°C or higher, the substituted ε-iron oxide particles, which are the object of the present invention, can be selectively and stably obtained, and the generation of different phases or compounds with insufficient phase transformation can be suppressed. If the heating temperature is high, α-Fe2O3 and partial substitution products of α-Fe2O3, which are thermodynamically stable phases, are likely to be generated, so the heat treatment is preferably performed at 900°C to 1200°C, more preferably 950°C to 1150°C. The heat treatment time can be adjusted within a range of about 0.5 to 10 hours, but good results are likely to be obtained within a range of 2 to 5 hours. By the above steps, ε-iron oxide particles or substituted ε-iron oxide particles coated with silicon oxide can be obtained. If necessary, the silicon oxide coating may be dissolved and removed using an alkaline aqueous solution.

[0036] [Transmission electron microscope (TEM) observation] TEM observation of the iron-based oxide magnetic powder obtained by the manufacturing method of the present invention was carried out under the following conditions. A JEM-1011 manufactured by JEOL Ltd. was used for TEM observation. For particle observation, TEM photographs taken at magnifications of 10,000x and 100,000x were used (those after removing the silicon oxide coating). -Measurement of average particle size, particle size distribution, and circularity- Digitizing was used to evaluate the TEM average particle size, particle size distribution, and circularity. Mac-View Ver. 4.0 was used as the image processing software. When using this image processing software, the particle size of a particle is calculated as the length of the long side of the rectangle that circumscribes the particle and has the smallest area. The circularity of a particle is calculated as the product of the particle's area and 4π divided by the square of the particle's perimeter. More than 200 particles were measured. Among the particles shown on the transmission electron microscope photograph, the selection criteria for particles to be measured were as follows: [1] Particles with any part lying outside the field of view of the photograph will not be measured. [2] Particles that are clearly defined and isolated are measured. [3] Particles that are independent and can be measured as single particles will be measured, even if they deviate from the average particle shape. [4] When particles overlap but have a clear boundary between them and the overall shape of the particle can be determined, each particle is measured as a single particle. [5] Particles that overlap, have unclear boundaries, and whose overall shape cannot be determined are not measured as their shape cannot be determined. The number average value of the particle diameters of the particles selected based on the above criteria was calculated, and this was taken as the average particle diameter of the iron oxide magnetic powder as observed by TEM. In addition, the "standard deviation of the particle diameters of the selected particles" was divided by the "number average value of the particle diameters of the selected particles (=average particle diameter)" to calculate the coefficient of variation of the particle diameters as observed by TEM. In addition, the number average value of the circularity of the selected particles was calculated, and this was taken as the average circularity of the iron oxide magnetic powder as observed by TEM.

[0037] [DLS average diameter of precursor] The DLS particle size of the slurry containing iron oxyhydroxide or iron oxyhydroxide containing a substituted metal element obtained by the production method of the present invention was measured by a dynamic light scattering particle size distribution measurement method under the following conditions. The dynamic light scattering particle size distribution analyzer used was manufactured by Otsuka Electronics Co., Ltd. (FPAR-1000K high sensitivity model), and the fiber probe used was a dilute system probe. The measurement conditions were: measurement time (seconds) 180 seconds, repetition count 1 time, and solvent setting Water. The analysis mode was the cumulant method.

[0038] [Composition analysis by inductively coupled plasma emission spectrometry (ICP)] The composition of the obtained ε-type iron oxide magnetic powder was analyzed. The composition analysis was performed using an Agilent Technologies ICP-720ES, with the measurement wavelengths (nm) being Fe; 259.940 nm, Ga; 294.363 nm, Co; 230.786 nm, Ti; 336.122 nm, Mn; 257.610 nm, Ni; 231.604 nm, Cr; 267.716 nm, Nd; 406.108 nm, Dy; 353.171 nm, and Gd; 342.246 nm. The measurement wavelength for each metal element was selected according to the composition of the iron oxide magnetic powder to be analyzed, so that there was no interference from the spectra of other elements and the linearity of the calibration curve could be obtained.

[0039] [Magnetic hysteresis curve (BH curve) measurement] The magnetic properties of the obtained ε-type iron-based oxide magnetic powder were measured under the following conditions. In the case of iron oxide magnetic powder consisting of ε-iron oxide particles or ε-iron oxide particles in which some of the Fe sites have been replaced with other metal elements, a vibrating sample magnetometer (VSM) (VSM-5 manufactured by Toei Kogyo Co., Ltd.) was used as the magnetic property measurement device, and the applied magnetic field was 1035 kA / m (13 kOe) and the M measurement range was 0.005 A m 2 The magnetic properties were measured at a magnetic field change rate of 15 (kA / m s), a time constant of 0.03 seconds, and a wait time of 0.1 seconds. The BH curve was used to evaluate the coercive force Hc, saturation magnetization σs, and SFD, and the differential BH curve was used to evaluate the low Hc components that do not contribute to magnetic recording. In this case, the vertical intercept of the differential BH curve at a magnetic field of 0 was taken as I L , the peak height on the high Hc side is I HThe SFD is the value obtained by dividing the half-width of the peak on the high Hc side by the coercive force Hc. The attached software (Ver. 2.1) made by Toei Kogyo Co., Ltd. was used for this measurement and evaluation. The value at the maximum magnetic field of the differential BH curve is I Hmax Then, I Hmax / I H If is less than 0.2, the above measurement results are used. Hmax / I H If the error was greater than 0.2, the measurement was repeated using the following procedure. The measurement was performed with an applied magnetic field of 1035 kA / m (13 kOe). Hmax / I H When the value exceeds 0.2, a high-temperature superconducting VSM (VSM-5HSC manufactured by Toei Kogyo Co., Ltd.) is used, and the applied magnetic field Hmax is 2387 kA / m (30 kOe) and the M measurement range is 0.005 A m 2 The magnetic properties were measured at a magnetic field change rate of 30 kA / (m s), a time constant of 0.03 seconds, and a wait time of 0.1 seconds. Hmax / I H If is 0.2 or less, use the above measurement results and Hmax / I H If the value exceeded 0.2, the measurement was repeated again using the following procedure. Measurements were performed at applied magnetic fields of 1035 kA / m (13 kOe) and 2387 kA / m (30 kOe). Hmax / I H When the value exceeds 0.2, a high-temperature superconducting VSM (VSM-5HSC manufactured by Toei Kogyo Co., Ltd.) is used, and the applied magnetic field Hmax is 3979 kA / m (50 kOe) and the M measurement range is 0.005 A m 2 The magnetic properties were measured at a magnetic field change rate of 30 kA / (m s), a time constant of 0.03 seconds, and a wait time of 0.1 seconds. Hmax / I H was confirmed to be 0.2 or less, and this measurement result was used. EXAMPLES

[0040] [Example 1] A raw material solution was prepared by mixing 313.9 g of ferric chloride (III) hexahydrate with a purity of 99% by mass as an iron raw material containing chloride ions, 195.1 g of gallium (III) nitrate solution with a Ga concentration of 9.4% by mass and a nitric acid concentration of 24% as raw materials of substitution elements, 15.8 g of cobalt (II) nitrate hexahydrate with a purity of 97% by mass, 10.9 g of titanium (IV) chloride solution with a Ti concentration of 16.5% by mass and a chloride ion concentration of 31% by mass, and 398.0 g of pure water. The molar ratio of metal ions in this raw material solution is Fe:Ga:Co:Ti=1.530:0.350:0.070:0.050. Next, 1500 g of pure water was added to a 5L reaction tank, and the liquid temperature was adjusted to 40°C while mechanically stirring with a stirring blade. Next, while continuing stirring and keeping the liquid temperature at 40°C, the raw material solution and 6.4 mass% aqueous ammonia solution as an aqueous alkali solution were added simultaneously to the pure water, and then the liquid temperature was kept at 40°C and stirred for 60 minutes to obtain a colloidal solution (step 1, first neutralization step). Here, the raw material solution was added continuously at an addition rate of 3.9 g / min over 240 minutes, and the aqueous ammonia solution was added continuously at an addition rate of 3.9 g / min over 240 minutes. During the addition of the raw material solution and the aqueous ammonia solution, the cumulative amount of alkali added relative to the total cumulative amount of acid radicals added contained in the raw material solution was 0.80 equivalents. The pH of the obtained colloidal solution was 1.8. Next, 288.75 g of citric acid solution with a citric acid concentration of 20% by mass was added continuously to the colloidal solution obtained in step 1 as a hydroxycarboxylic acid over a period of 60 minutes at 40° C. (hydroxycarboxylic acid addition step), and then 152.86 g of 22.4% by mass ammonia aqueous solution was added all at once, and the mixture was kept stirred for 10 minutes at a temperature of 40° C. to obtain a slurry of precursor particles, which is an intermediate product (step 2, second neutralization step). The pH after the addition of 152.86 g of the ammonia solution was 8.6. The DLS average diameter was 39 nm. A TEM photograph of the iron oxyhydroxide crystals containing the substitution element obtained up to step 2 is shown in FIG. 2.

[0041] The precursor slurry obtained in step 2 was collected and washed with an ultrafiltration membrane, a membrane with a UF molecular weight cutoff of 50,000, until the electrical conductivity of the filtrate became 30 mS / m or less (step 3). The washed slurry obtained in step 3 was sprayed 10 times from a φ0.1 mm nozzle at a pressure of 245 MPa using a wet atomization device (Starburst Mini, model number HJP-25001, manufactured by Sugino Machine Co., Ltd.) (step 4). After that, 506.1 g of the washed slurry obtained in step 4 was taken, the temperature was adjusted to 40°C while stirring, 138.8 g of 22.1 mass% ammonia aqueous solution and 1171.3 g of 2-propanol were added and stirred for 5 minutes, and 552.8 g of tetraethoxysilane (TEOS) was added as a silicon compound having a hydrolyzable group over 35 minutes. After that, the liquid temperature was kept at 40°C and stirring was continued for 7 hours, and the silicon compound hydrolysis product was coated. The obtained solution was then washed and separated into solid and liquid, and collected as a cake (step 5).

[0042] After drying the cake obtained in step 5 (precursor coated with gel-like hydrolysis product), the dried powder was heat-treated in an air furnace at 1130°C for 4 hours to obtain ε-iron oxide powder in which some of the Fe sites coated with silicon oxide were replaced with other metal elements. Note that the hydrolysis product of the silicon compound is converted to an oxide when heat-treated in an air atmosphere (step 6). The powder of ε-iron oxide in which the silicon oxide-coated Fe sites had been partially substituted with other metal elements obtained in step 6 was stirred in a 20 mass% NaOH aqueous solution at approximately 60°C for 24 hours to remove the silicon oxide from the particle surfaces, thereby obtaining a slurry containing ε-iron oxide particles in which the Fe sites had been partially substituted with other metal elements (step 7).

[0043] The slurry obtained in step 7 was washed with pure water until the electrical conductivity was ≦15 mS / m, thereby obtaining a washed slurry according to Example 1. A 1% by mass aqueous sulfuric acid solution was added to the washed slurry to adjust the pH to 6.5, and the slurry was then filtered through a membrane. The cake was recovered and then dried, thereby obtaining an iron-based oxide magnetic powder according to Example 1. The coercive force of this iron-based oxide magnetic powder was 177 kA / m, and the saturation magnetization was 17.9 Am. 2 / kg, SFD is 1.00, I L / IH The value was 0.41. The obtained iron-based oxide magnetic powder according to Example 1 was dispersed in pure water using an ultrasonic disperser to prepare a slurry, and the prepared slurry was dropped and attached to a collodion film on a grid, naturally dried, and then carbon deposition was performed and subjected to TEM observation. Measurements of 200 particles by TEM observation showed that the TEM average particle size was 16.6 nm, the number ratio of particles with a particle size of 8 nm or less was 0.0%, the number ratio of particles with a particle size of 20 nm or more was 14.9%, the coefficient of variation (CV value) was 20%, and the average circularity of the particles was 0.972. Figure 1 shows a TEM photograph of the iron-based oxide magnetic powder obtained in this example. The length indicated by the white horizontal line displayed in the lower right of the TEM photograph is 100 nm. In addition, a composition analysis was performed to calculate the molar composition ratio of each metal element when the total amount of iron and the substituted metal element was 2 moles. The above manufacturing conditions are shown in Tables 1 and 2, and the measurement results of the obtained iron-based oxide magnetic powder are shown in Tables 3 and 4 (the same applies to the following Examples and Comparative Examples).

[0044] [Example 2] The molar ratio of metal ions in the raw solution was Fe:Ga:Co:Ti=1.505:0.375:0.070:0.050, and the total molar amount of Fe, Ga, Co and Ti in the raw solution was the same as in Example 1. The amounts of ferric chloride (III) hexahydrate, Ga(III) nitrate solution, cobalt(II) nitrate hexahydrate and titanium(IV) chloride solution were changed, and the treatment with the wet microparticulation device was not performed. The iron-based oxide magnetic powder of Example 2 was obtained by the same procedure as in Example 1. The pH of the obtained colloidal solution was 1.8, and the pH after the ammonia solution was added all at once in the second neutralization step was 8.6. The DLS average diameter of the precursor particles contained in the slurry after washing was 54 nm. The magnetic properties of this iron oxide magnetic powder were measured and found to be coercive force of 191 kA / m and saturation magnetization of 17.8 Am. 2 / kg, SFD was 1.08, I L / I H The value was 0.48. In addition, this iron-based oxide magnetic powder was subjected to TEM observation in the same manner as in Example 1, and the results showed that the TEM average particle diameter was 16.3 nm, the number fraction of particles with a particle diameter of 8 nm or less was 0.9%, the number fraction of particles with a particle diameter of 20 nm or more was 14.9%, the coefficient of variation (CV value) was 25%, and the average circularity of the particles was 0.970.

[0045] [Example 3] The iron-based oxide magnetic powder of Example 3 was obtained by the same procedure as in Example 1, except that the amount of citric acid solution added was 216.6 g and the treatment with the wet microparticulation device was not performed. The pH of the obtained colloidal solution was 1.8, and the pH after the ammonia solution was added all at once in the second neutralization step was 8.5. The DLS average diameter of the precursor particles contained in the slurry after washing was 44 nm. The magnetic properties of this iron oxide magnetic powder were measured and found to be coercive force of 154 kA / m and saturation magnetization of 18.3 Am. 2 / kg, SFD is 1.25, I L / I H The value was 0.51. In addition, this iron-based oxide magnetic powder was subjected to TEM observation using the same procedure as in Example 1, and the results showed that the TEM average particle diameter was 15.2 nm, the number proportion of particles with a particle diameter of 8 nm or less was 2.3%, the number proportion of particles with a particle diameter of 20 nm or more was 7.7%, the coefficient of variation (CV value) was 24%, and the average circularity of the particles was 0.968.

[0046] [Example 4] The iron-based oxide magnetic powder of Example 4 was obtained by the same procedure as in Example 1, except that the amount of citric acid solution added was 433.2 g and the treatment with the wet microparticulation device was not performed. The pH of the obtained colloidal solution was 1.8, and the pH after the ammonia solution was added all at once in the second neutralization step was 8.1. The DLS average diameter of the precursor particles contained in the slurry after washing was 31 nm. The magnetic properties of this iron oxide magnetic powder were measured and found to be coercive force of 185 kA / m and saturation magnetization of 18.0 Am. 2 / kg, SFD was 1.07, I L / I H The value was 0.44. In addition, this iron-based oxide magnetic powder was subjected to TEM observation in the same manner as in Example 1, and the results showed that the TEM average particle diameter was 16.1 nm, the number fraction of particles with a particle diameter of 8 nm or less was 0.0%, the number fraction of particles with a particle diameter of 20 nm or more was 17.0%, the coefficient of variation (CV value) was 24%, and the average circularity of the particles was 0.967.

[0047] [Example 5] The iron-based oxide magnetic powder of Example 4 was obtained by the same procedure as in Example 1, except that the concentration of the aqueous ammonia solution added in the first neutralization step was 6.9 mass % and no treatment was performed using a wet microparticulation device. During the addition of the raw material solution and the aqueous ammonia solution, the ratio of the cumulative amount of alkali added to the total cumulative amount of acid radicals contained in the raw material solution was 0.85 equivalents, the pH of the resulting colloidal solution was 2.2, and the pH after the ammonia solution was added all at once in the second neutralization step was 9.0. The DLS average diameter of the precursor particles contained in the slurry after washing was 221 nm. The magnetic properties of this iron oxide magnetic powder were measured and found to be coercive force of 182 kA / m and saturation magnetization of 18.1 Am. 2 / kg, SFD is 1.10, I L / I H The value was 0.44. In addition, this iron-based oxide magnetic powder was subjected to TEM observation using the same procedure as in Example 1, and the results showed that the TEM average particle diameter was 17.6 nm, the number proportion of particles with a particle diameter of 8 nm or less was 0.4%, the number proportion of particles with a particle diameter of 20 nm or more was 23.6%, the coefficient of variation (CV value) was 30%, and the average circularity of the particles was 0.965.

[0048] [Comparative Example 1] This example is an example in which an experiment was carried out in the same procedure as in Example 1 of Patent Document 4. In a 5L reaction tank, 291.32g of ferric nitrate (III) nonahydrate with a purity of 99.4%, 80.18g of Ga(III) nitrate solution with a Ga concentration of 10.1%, 6.58g of cobalt(II) nitrate hexahydrate with a purity of 97%, and 7.14g of titanium(IV) sulfate n-hydrate with a Ti concentration of 14.7% were dissolved in 3214.78g of pure water while mechanically stirring with a stirring blade under the conditions of 40°C in an air atmosphere. The molar ratio of metal ions in this charged solution was Fe:Ga:Co:Ti=1.635:0.265:0.050:0.050. In an air atmosphere at 40°C, 166.29 g of 21.2% ammonia solution was added all at once while mechanically stirring with a stirring blade, and stirring was continued for 2 hours. At the beginning of the addition, the liquid was brown and cloudy, but after 2 hours, it became a transparent brown reaction liquid with a pH of 2.0 (first neutralization step). Next, 252.66 g of citric acid solution with a citric acid concentration of 10% by mass was added continuously over 1 hour under the condition of 40°C, and then 200 g of 10 mass% ammonia solution was added all at once to adjust the pH to 8.5, and the mixture was kept at 40°C for 1 hour with stirring to generate crystals of iron oxyhydroxide containing the substitution element of the precursor, which is an intermediate product (step 11, second neutralization step). The results of TEM observation of the iron oxyhydroxide crystals containing the substitution element obtained in this comparative example are shown in Figure 3. The length indicated by the white horizontal line shown in the lower right of the TEM photograph is 100 nm. When the slurry obtained in step 11 was subjected to measurement of the DLS average diameter of the precursor particles, the result was outside the allowable measurement range (up to 500 nm), and the DLS average diameter could not be measured.

[0049] Then, 488.13 g of tetraethoxysilane was added to the precursor slurry obtained in step 11 over 35 minutes while stirring at 30°C in an air atmosphere. The temperature was maintained at 30°C and stirring was continued for about one day. After that, a solution of 194.7 g of ammonium sulfate dissolved in 300 g of pure water was added, and the resulting solution was washed and separated into solid and liquid, and collected as a cake (step 12). After drying the precipitate obtained in step 12, the dried powder was subjected to a heat treatment at 1,070°C for 4 hours in a furnace in an air atmosphere, to obtain a powder of ε-iron oxide in which some of the Fe sites covered with silicon oxide were replaced with other metal elements (step 13).

[0050] The heat-treated powder obtained in step 13 was stirred in a 20 mass% NaOH aqueous solution at about 70°C for 24 hours to remove silicon oxide from the particle surface. Next, the powder was washed until the electrical conductivity of the washing slurry was ≦15 mS / m, and then the solid content was collected and dried to obtain an iron-based oxide magnetic powder according to Comparative Example 1. The obtained magnetic powder was subjected to chemical analysis of the composition, TEM observation, and measurement of the magnetic properties. The magnetic properties of this iron oxide magnetic powder were measured and found to be coercive force of 313 kA / m and saturation magnetization of 15.8 Am. 2 / kg, SFD was 0.89, I L / I H The value of was 0.50. Furthermore, when this iron-based oxide magnetic powder was subjected to TEM observation in the same manner as in Example 1, the results showed that the TEM average particle size was 16.6 nm, the number ratio of particles with a particle size of 8 nm or less was 5.8%, the number ratio of particles with a particle size of 20 nm or more was 26.0%, the coefficient of variation (CV value) was 40%, and the average circularity of the particles was 0.919. Figure 4 shows a TEM photograph of the iron-based oxide magnetic powder obtained in this comparative example. The length indicated by the white horizontal line shown on the left of the TEM photograph is 50 nm.

[0051] [Comparative Example 2] This example is an example in which an experiment was carried out in the same procedure as in Example 6 of Patent Document 4. The iron-based oxide magnetic powder according to Comparative Example 2 was obtained by the same procedure as Comparative Example 1, except that the reaction temperature from the first neutralization step to the second neutralization step was 20°C, the amount of citric acid solution added was 505.32g, and the heat treatment temperature of the dried powder was 1055°C. The pH of the obtained colloidal solution was 2.0, and the pH after the ammonia solution was added all at once in the second neutralization step was 8.5. In addition, the DLS average diameter of the precursor particles contained in the slurry obtained in the second neutralization step was outside the allowable measurement range (up to 500nm), and the DLS average diameter could not be measured. The obtained magnetic powder was subjected to chemical analysis of the composition, TEM observation, and measurement of the magnetic properties. The magnetic properties of this iron oxide magnetic powder were measured and found to be coercive force of 390 kA / m and saturation magnetization of 16.9 Am. 2 / kg, SFD was 0.83, I L / I H The value of was 0.46. Furthermore, when this iron-based oxide magnetic powder was subjected to TEM observation in the same manner as in Example 1, the TEM average particle size was 16.3 nm, the number ratio of particles with a particle size of 8 nm or less was 4.0%, the number ratio of particles with a particle size of 20 nm or more was 25.4%, the coefficient of variation (CV value) was 37%, and the average circularity of the particles was 0.910.

[0052] From the results of Comparative Examples 1 and 2, it can be seen that in the production method according to the conventional technology of Patent Document 4, since the raw material solution and alkali are not added continuously or intermittently to the reaction system in the first neutralization step, but an alkali is added to the raw material solution, the particle size of the obtained precursor becomes small and the DLS average diameter becomes large, that is, the dispersibility becomes poor, as shown in Figure 3. Furthermore, it can be seen that as a result, the particle size distribution of the obtained iron-based oxide particles becomes wide, and the particle shape of the obtained iron-based oxide particles becomes distorted.

[0053] [Comparative Example 3] In a 5L reaction tank, 345.3g of ferric chloride (III) hexahydrate with a purity of 99% by mass, 214.6g of Ga(III) nitrate solution with a Ga concentration of 9.4% by mass, 17.4g of cobalt(II) nitrate hexahydrate with a purity of 97% by mass, and 12.0g of titanium(IV) chloride solution with a Ti concentration of 16.5% by mass were dissolved in 3214.8g of pure water while mechanically stirring with a stirring blade under the conditions of 50°C in an air atmosphere. The molar ratio of metal ions in this raw solution was Fe:Ga:Co:Ti=1.530:0.350:0.070:0.050. In an air atmosphere at 50°C, 166.3 g of 21.2% ammonia solution was added all at once while mechanically stirring with a stirring blade, and stirring was continued for 2 hours. At the beginning of the addition, the liquid was brown and cloudy, but after 2 hours it became a transparent brown reaction liquid with a pH of 1.9. Next, 288.8 g of a citric acid solution with a citric acid concentration of 10% by mass was added continuously over 1 hour at 50° C., and then 200 g of a 10% by mass ammonia solution was added all at once to adjust the pH to 8.6, and the mixture was kept at 50° C. with stirring for 1 hour to produce crystals of iron oxyhydroxide containing the substitution element of the precursor, which is the intermediate product. (Step 21, second neutralization step) The DLS average diameter of the precursor particles contained in the slurry obtained in step 21 was measured, and the DLS average diameter was 160 nm.

[0054] Then, 488.13 g of tetraethoxysilane was added to the precursor slurry obtained in step 21 over 35 minutes while stirring at 30°C in an air atmosphere. The temperature was maintained at 30°C and stirring was continued for about one day. Then, a solution of 194.7 g of ammonium sulfate dissolved in 300 g of pure water was added, and the resulting solution was washed and subjected to solid-liquid separation, and collected as a cake (step 22). After drying the precipitate obtained in step 22, the dried powder was subjected to heat treatment at 1070°C for 4 hours in a furnace in an air atmosphere to obtain iron-based oxide magnetic particle powder coated with silicon oxide (step 23).

[0055] The heat-treated powder obtained in step 23 was stirred in a 20 mass% NaOH aqueous solution at about 70°C for 24 hours to remove silicon oxide from the particle surface. Next, the powder was washed until the electrical conductivity of the washing slurry was ≦15 mS / m, and then the solid content was collected and dried to obtain an iron-based oxide magnetic powder according to Comparative Example 3. The obtained magnetic powder was subjected to chemical analysis of the composition, TEM observation, and measurement of the magnetic properties. The magnetic properties of this iron oxide magnetic powder were measured and found to be coercive force of 242 kA / m and saturation magnetization of 15.7 Am. 2 / kg, SFD was 2.14, I L / I H The value of was 0.72. Furthermore, when this iron-based oxide magnetic powder was subjected to TEM observation in the same manner as in Example 1, the TEM average particle size was 14.5 nm, the number ratio of particles with a particle size of 8 nm or less was 7.1%, the number ratio of particles with a particle size of 20 nm or more was 14.2%, the coefficient of variation (CV value) was 35%, and the average circularity of the particles was 0.923.

[0056] From the results of Comparative Example 3, it is clear that when iron chloride was used as the iron raw material in the manufacturing method of Patent Document 4, which is the conventional technology, the DLS average diameter of the obtained precursor slurry was smaller than when iron nitrate was used as the iron raw material as in Comparative Examples 1 and 2, and the proportion of particles having a particle diameter of 20 nm or more in the obtained iron-based oxide magnetic powder was lower, but the proportion of particles having a particle diameter of 8 nm or more was higher than in the Examples, indicating a problem in terms of particle size distribution.

[0057] [Comparative Example 4] A precursor slurry was obtained by carrying out the same procedure as in Example 1 up to the second neutralization step, except that the aqueous ammonia solution was continuously added at an addition rate of 7.8 g / min. The colloidal solution obtained in the first neutralization step had a pH of 3.6, and the pH after the aqueous ammonia solution was added all at once in the second neutralization step was 9.3. When the obtained precursor slurry was subjected to DLS average diameter measurement, the result was outside the allowable measurement range (up to 500 nm), and the DLS average diameter could not be measured. The DLS average diameter of the precursor slurry was very large, and it was predicted that even if subsequent steps were carried out, an iron-based oxide magnetic powder with a wide particle size distribution, in which the proportion of particles 20 nm or larger was more than 25%, would be obtained. Therefore, no operations beyond the second neutralization step were carried out.

[0058] [Example 6] As the raw material solution, 1013 g of an aqueous solution with a Fe(III) concentration of 1.113 mol / kg and a chloride ion concentration of 3.338 mol / kg was prepared. Next, 1603 g of an aqueous solution with a Fe(III) concentration of 0.234 mol / kg and a chloride ion concentration of 0.703 mol / kg was placed in a 5 L reaction tank, and the liquid temperature was adjusted to 40 ° C. while mechanically stirring with a stirring blade. Next, while continuing the stirring and keeping the liquid temperature at 40 ° C., the raw material solution and a 3.337 mol / kg aqueous ammonia solution were added simultaneously to this aqueous solution, and then the liquid temperature was kept at 40 ° C. and stirred for 60 minutes to obtain a colloidal solution (Step 1, first neutralization step). Here, the raw material solution was added continuously at an addition rate of 5.6 g / min over 180 minutes, and the aqueous ammonia solution was added continuously at an addition rate of 5.6 g / min over 180 minutes. During the addition of the raw material solution and the aqueous ammonia solution, the ratio of the cumulative amount of alkali added to the total cumulative amount of acid radicals contained in the raw material solution was 1.0 equivalent. The pH of the resulting colloidal solution was 1.8. Next, 289g of citric acid solution with a citric acid concentration of 1.041 mol / kg was added continuously to the colloidal solution obtained in step 1 as a hydroxycarboxylic acid over a period of 60 minutes at 40°C (hydroxycarboxylic acid addition step), and then 189g of ammonia solution with a concentration of 12.864 mol / kg was added all at once, and the mixture was kept at 40°C for 10 minutes while stirring to obtain a precursor slurry, which is an intermediate product (step 2, second neutralization step). After adding 189g of ammonia solution all at once, the pH was 8.5.

[0059] The precursor slurry obtained in step 2 was collected and washed with an ultrafiltration membrane, a membrane with a UF molecular weight cutoff of 50,000, until the electrical conductivity of the filtrate became 30 mS / m or less (step 3). After that, 868 g of the washed slurry obtained in step 3 was taken, and pure water was added to make the total volume 950 g. The temperature was adjusted to 40°C while stirring, and 260 g of 21.92 mass% ammonia aqueous solution and 1171 g of ethanol were added and stirred for 5 minutes, and 1028 g of tetraethoxysilane (TEOS) was added as a silicon compound having a hydrolyzable group over 35 minutes. After that, the liquid temperature was kept at 40°C and stirring was continued for 1 hour, and the silicon compound hydrolysis product was coated. The obtained solution was then washed and separated into solid and liquid, and collected as a cake (step 4).

[0060] The cake obtained in step 4 (precursor coated with gel-like hydrolysis product) was dried, and then the dried powder was heat-treated in a furnace in an air atmosphere at 1060°C for 4 hours to obtain ε-iron oxide powder coated with silicon oxide. Note that the hydrolysis product of the silicon compound is converted to an oxide when heat-treated in an air atmosphere (step 5). The silicon oxide-coated ε-iron oxide powder obtained in step 5 was stirred in a 20 mass % NaOH aqueous solution at approximately 60°C for 24 hours to remove the silicon oxide from the particle surfaces, thereby obtaining a slurry containing ε-iron oxide particles (step 6).

[0061] The slurry obtained in step 6 was washed with pure water until the electrical conductivity became ≦15 mS / m, thereby obtaining a washed slurry according to Example 6. A 1% by mass aqueous sulfuric acid solution was added to the washed slurry to adjust the pH to 6.5, and then the slurry was subjected to membrane filtration. The cake was recovered and then dried, thereby obtaining an iron-based oxide magnetic powder according to Example 6. The magnetic properties of this iron oxide magnetic powder were measured and found to be coercive force of 1236 kA / m and saturation magnetization of 15.0 Am. 2 / kg, SFD was 0.89, I L / I H The value was 0.31. In addition, this iron-based oxide magnetic powder was subjected to TEM observation in the same manner as in Example 1, and the results showed that the TEM average particle diameter was 13.9 nm, the number proportion of particles with a particle diameter of 8 nm or less was 2.1%, the number proportion of particles with a particle diameter of 20 nm or more was 4.2%, the coefficient of variation (CV value) was 25%, and the average circularity of the particles was 0.958.

[0062] [Example 7] As the raw material solution, 1019 g of an aqueous solution with a Fe(III) concentration of 1.056 mol / kg, a Co(II) concentration of 0.066 mol / kg, a chloride ion concentration of 3.167 mol / kg, and a nitrate ion concentration of 0.133 mol / kg was prepared. Next, 1598 g of an aqueous solution with a Fe(III) concentration of 0.225 mol / kg and a chloride ion concentration of 0.674 mol / kg was placed in a 5 L reaction tank, and the liquid temperature was adjusted to 40 ° C. while mechanically stirring with a stirring blade. Next, while continuing the stirring and keeping the liquid temperature at 40 ° C., the raw material solution and a 3.267 mol / kg aqueous ammonia solution were added simultaneously to this aqueous solution, and then the liquid temperature was kept at 40 ° C. and stirred for 60 minutes to obtain a colloidal solution (Step 1, first neutralization step). Here, the raw material solution was added continuously at an addition rate of 4.2 g / min over 240 minutes, and the aqueous ammonia solution was added continuously at an addition rate of 4.2 g / min over 240 minutes. During the addition of the raw material solution and the aqueous ammonia solution, the ratio of the cumulative amount of alkali added to the total cumulative amount of acid radicals contained in the raw material solution was 0.99 equivalents. The pH of the resulting colloidal solution was 2.1. Next, 289 g of citric acid solution with a citric acid concentration of 1.041 mol / kg was added continuously over 60 minutes at 40° C. to the colloidal solution obtained in step 1 (hydroxycarboxylic acid addition step), and then 194 g of ammonia solution with a concentration of 12.347 mol / kg was added all at once, and the mixture was kept at 40° C. for 10 minutes while stirring to obtain a precursor slurry, which is an intermediate product (step 2, second neutralization step). The pH after the addition of 194 g of ammonia solution all at once was 9.2.

[0063] The precursor slurry obtained in step 2 was collected and washed with an ultrafiltration membrane, a membrane with a UF molecular weight cutoff of 50,000, until the electrical conductivity of the filtrate became 30 mS / m or less (step 3). After that, 894 g of the washed slurry obtained in step 3 was taken, and pure water was added to make the total volume 950 g. The temperature was adjusted to 40°C while stirring, and 271 g of 21.04 mass% ammonia aqueous solution and 1171 g of ethanol were added and stirred for 5 minutes, and 1028 g of tetraethoxysilane (TEOS) was added as a silicon compound having a hydrolyzable group over 35 minutes. After that, the liquid temperature was kept at 40°C and stirring was continued for 1 hour, and the silicon compound hydrolysis product was coated. The obtained solution was then washed and separated into solid and liquid, and collected as a cake (step 4).

[0064] After drying the cake obtained in step 4 (precursor coated with gel-like hydrolysis product), the dried powder was heat-treated in a furnace in an air atmosphere at 1080°C for 4 hours to obtain ε-iron oxide powder in which some of the Fe sites coated with silicon oxide were replaced with other metal elements. Note that the hydrolysis product of the silicon compound is converted to an oxide when heat-treated in an air atmosphere (step 5). The powder of ε-iron oxide in which the silicon oxide-coated Fe sites had been partially substituted with other metal elements obtained in step 5 was stirred in a 20 mass% NaOH aqueous solution at approximately 60°C for 24 hours to remove the silicon oxide from the particle surfaces, thereby obtaining a slurry containing ε-iron oxide particles in which the Fe sites had been partially substituted with other metal elements (step 6).

[0065] The slurry obtained in step 6 was washed with pure water until the electrical conductivity became ≦15 mS / m, thereby obtaining a washed slurry according to Example 7. A 1% by mass aqueous sulfuric acid solution was added to the washed slurry to adjust the pH to 6.5, and the slurry was then subjected to membrane filtration. The cake was recovered and then dried, thereby obtaining an iron-based oxide magnetic powder according to Example 7. The magnetic properties of this iron oxide magnetic powder were measured and found to be coercive force of 706 kA / m and saturation magnetization of 20.4 Am. 2 / kg, SFD is 2.65, I L / I H The value was 0.79. In addition, this iron-based oxide magnetic powder was subjected to TEM observation using the same procedure as in Example 1, and the results showed that the TEM average particle diameter was 14.8 nm, the number proportion of particles with a particle diameter of 8 nm or less was 2.3%, the number proportion of particles with a particle diameter of 20 nm or more was 10.6%, the coefficient of variation (CV value) was 34%, and the average circularity of the particles was 0.967.

[0066] [Example 8] As the raw material solution, 1021 g of an aqueous solution with a Fe(III) concentration of 1.055 mol / kg, a Ti(IV) concentration of 0.066 mol / kg, and a chloride ion concentration of 3.332 mol / kg was prepared. Next, 1598 g of an aqueous solution with a Fe(III) concentration of 0.225 mol / kg and a chloride ion concentration of 0.674 mol / kg was placed in a 5 L reaction tank, and the liquid temperature was adjusted to 40 ° C. while mechanically stirring with a stirring blade. Next, while continuing the stirring and keeping the liquid temperature at 40 ° C., the raw material solution and a 3.290 mol / kg aqueous ammonia solution were added simultaneously to this aqueous solution, and then the liquid temperature was kept at 40 ° C. and stirred for 60 minutes to obtain a colloidal solution (Step 1, first neutralization step). Here, the raw material solution was added continuously at an addition rate of 4.3 g / min over 240 minutes, and the aqueous ammonia solution was added continuously at an addition rate of 4.3 g / min over 240 minutes. During the addition of the raw material solution and the aqueous ammonia solution, the ratio of the cumulative amount of alkali added to the total cumulative amount of acid radicals contained in the raw material solution was 0.99 equivalents. The pH of the resulting colloidal solution was 1.8. Next, 289 g of citric acid solution with a citric acid concentration of 1.041 mol / kg was added continuously over 60 minutes at 40° C. to the colloidal solution obtained in step 1 (hydroxycarboxylic acid addition step), and then 196 g of ammonia solution with a concentration of 12.347 mol / kg was added all at once, and the mixture was kept at 40° C. for 10 minutes while stirring to obtain a precursor slurry, which is an intermediate product (step 2, second neutralization step). After adding 194 g of ammonia solution all at once, the pH was 9.1.

[0067] The precursor slurry obtained in step 2 was collected and washed with an ultrafiltration membrane, a membrane with a UF molecular weight cutoff of 50,000, until the electrical conductivity of the filtrate became 30 mS / m or less (step 3). After that, 882 g of the washed slurry obtained in step 3 was taken, and pure water was added to make the total volume 950 g. The temperature was adjusted to 40°C while stirring, and 271 g of 21.04 mass% ammonia aqueous solution and 1171 g of ethanol were added and stirred for 5 minutes, and 1028 g of tetraethoxysilane (TEOS) was added as a silicon compound having a hydrolyzable group over 35 minutes. After that, the liquid temperature was kept at 40°C and stirring was continued for 1 hour, and the silicon compound hydrolysis product was coated. The obtained solution was then washed and separated into solid and liquid, and collected as a cake (step 4).

[0068] After drying the cake obtained in step 4 (precursor coated with gel-like hydrolysis product), the dried powder was heat-treated in an air furnace at 1130°C for 4 hours to obtain ε-iron oxide powder in which some of the Fe sites coated with silicon oxide were replaced with other metal elements. Note that the hydrolysis product of the silicon compound is converted to an oxide when heat-treated in an air atmosphere (step 5). The powder of ε-iron oxide in which the silicon oxide-coated Fe sites had been partially substituted with other metal elements obtained in step 5 was stirred in a 20 mass% NaOH aqueous solution at approximately 60°C for 15 hours to remove the silicon oxide from the particle surfaces, thereby obtaining a slurry containing ε-iron oxide particles in which the Fe sites had been partially substituted with other metal elements (step 6).

[0069] The slurry obtained in step 6 was washed with pure water until the electrical conductivity became ≦15 mS / m, thereby obtaining a washed slurry according to Example 8. A 1% by mass aqueous sulfuric acid solution was added to the washed slurry to adjust the pH to 6.5, and then the slurry was subjected to membrane filtration. The cake was recovered and then dried, thereby obtaining an iron-based oxide magnetic powder according to Example 8. The magnetic properties of this iron oxide magnetic powder were measured and found to be coercive force of 1318 kA / m and saturation magnetization of 15.8 Am. 2 / kg, SFD was 0.69, I L / I HThe value was 0.19. In addition, this iron-based oxide magnetic powder was subjected to TEM observation in the same manner as in Example 1, and the results showed that the TEM average particle diameter was 15.6 nm, the number proportion of particles with a particle diameter of 8 nm or less was 1.5%, the number proportion of particles with a particle diameter of 20 nm or more was 12.9%, the coefficient of variation (CV value) was 30%, and the average circularity of the particles was 0.973.

[0070] [Example 9] As the raw material solution, 822 g of an aqueous solution with a Fe(III) concentration of 1.132 mol / kg, a Ga(III) concentration of 0.320 mol / kg, a chloride ion concentration of 3.549 mol / kg, and a nitrate ion concentration of 0.955 mol / kg was prepared. Next, 1584 g of an aqueous solution with a Fe(III) concentration of 0.196 mol / kg and a chloride ion concentration of 0.614 mol / kg was placed in a 5 L reaction tank, and the liquid temperature was adjusted to 40 ° C. while mechanically stirring with a stirring blade. Next, while continuing the stirring and keeping the liquid temperature at 40 ° C., the raw material solution and a 2.275 mol / kg aqueous ammonia solution were added simultaneously to this aqueous solution, and then the liquid temperature was kept at 40 ° C. while stirring for 60 minutes to obtain a colloidal solution (step 1, first neutralization step). Here, the raw material solution was added continuously at an addition rate of 3.4 g / min over 240 minutes, and the aqueous ammonia solution was added continuously at an addition rate of 3.4 g / min over 240 minutes. During the addition of the raw material solution and the aqueous ammonia solution, the ratio of the cumulative amount of alkali added to the total cumulative amount of acid radicals contained in the raw material solution was 0.51 equivalents. The pH of the resulting colloidal solution was 1.6. Next, 289 g of citric acid solution with a citric acid concentration of 1.041 mol / kg was added continuously over 60 minutes at 40° C. to the colloidal solution obtained in step 1 (hydroxycarboxylic acid addition step), and then 283 g of ammonia solution with a concentration of 14.707 mol / kg was added all at once, and the mixture was kept at 40° C. for 10 minutes while stirring to obtain a precursor slurry, which is an intermediate product (step 2, second neutralization step). The pH after the addition of 283 g of ammonia solution all at once was 8.9.

[0071] The precursor slurry obtained in step 2 was collected and washed with an ultrafiltration membrane, a membrane with a UF molecular weight cutoff of 50,000, until the electrical conductivity of the filtrate became 150 mS / m or less (step 3). After that, 1119 g of the washed slurry obtained in step 3 was taken, and pure water was added to make the total volume 1150 g. The temperature was adjusted to 40°C while stirring, and 142 g of 25.06 mass% ammonia aqueous solution and 1406 g of 2-propanol were added and stirred for 5 minutes, and 640 g of tetraethoxysilane (TEOS) was added as a silicon compound having a hydrolyzable group over 35 minutes. After that, the liquid temperature was kept at 40°C and stirring was continued for 1 hour, and the silicon compound hydrolysis product was coated. The obtained solution was then washed and separated into solid and liquid, and collected as a cake (step 4).

[0072] After drying the cake obtained in step 4 (precursor coated with gel-like hydrolysis product), the dried powder was heat-treated in a furnace in an air atmosphere at 1100°C for 4 hours to obtain ε-iron oxide powder in which some of the Fe sites coated with silicon oxide were replaced with other metal elements. Note that the hydrolysis product of the silicon compound is converted to an oxide when heat-treated in an air atmosphere (step 5). The powder of ε-iron oxide in which the silicon oxide-coated Fe sites had been partially substituted with other metal elements obtained in step 5 was stirred in a 20 mass% NaOH aqueous solution at approximately 60°C for 14 hours to remove the silicon oxide from the particle surfaces, thereby obtaining a slurry containing ε-iron oxide particles in which the Fe sites had been partially substituted with other metal elements (step 6).

[0073] The slurry obtained in step 6 was washed with pure water until the electrical conductivity became ≦15 mS / m, thereby obtaining a washed slurry according to Example 9. A 1% by mass aqueous sulfuric acid solution was added to the washed slurry to adjust the pH to 6.5, and then the slurry was subjected to membrane filtration. The cake was recovered and then dried, thereby obtaining an iron-based oxide magnetic powder according to Example 9. The magnetic properties of this iron oxide magnetic powder were measured and found to be coercive force of 655 kA / m and saturation magnetization of 20.4 Am. 2 / kg, SFD was 0.71, I L / I HThe value was 0.21. In addition, this iron-based oxide magnetic powder was subjected to TEM observation using the same procedure as in Example 1, and the results showed that the TEM average particle diameter was 17.0 nm, the number proportion of particles with a particle diameter of 8 nm or less was 0.3%, the number proportion of particles with a particle diameter of 20 nm or more was 24.2%, the coefficient of variation (CV value) was 30%, and the average circularity of the particles was 0.958.

[0074] [Example 10] As the raw material solution, 1013 g of an aqueous solution with Fe(III) concentration of 1.063 mol / kg, Co(II) concentration of 0.033 mol / kg, Ti(IV) concentration of 0.033 mol / kg, chloride ion concentration of 3.274 mol / kg, and nitrate ion concentration of 0.067 mol / kg was prepared. Next, 1598 g of an aqueous solution with Fe(III) concentration of 0.225 mol / kg and chloride ion concentration of 0.674 mol / kg was placed in a 5 L reaction tank, and the liquid temperature was adjusted to 40 ° C. while mechanically stirring with a stirring blade. Next, while continuing the stirring and keeping the liquid temperature at 40 ° C., the raw material solution and 3.302 mol / kg of ammonia aqueous solution were added simultaneously to this aqueous solution, and then the liquid temperature was kept at 40 ° C. and stirred for 60 minutes to obtain a colloidal solution (step 1, first neutralization step). Here, the raw material solution was added continuously at a rate of 4.2 g / min over 240 minutes, and the aqueous ammonia solution was added continuously at a rate of 4.2 g / min over 240 minutes. During the addition of the raw material solution and the aqueous ammonia solution, the ratio of the cumulative amount of alkali added to the total cumulative amount of acid radicals contained in the raw material solution was 0.99 equivalents. The pH of the resulting colloidal solution was 2.0. Next, 289 g of citric acid solution with a citric acid concentration of 1.041 mol / kg was added continuously to the colloidal solution obtained in step 1 as a hydroxycarboxylic acid over a period of 60 minutes at 40° C. (hydroxycarboxylic acid addition step), and then 185 g of ammonia solution with a concentration of 12.993 mol / kg was added all at once. The mixture was then kept at 40° C. for 10 minutes while stirring to obtain a precursor slurry, which is an intermediate product (step 2, second neutralization step). The pH after the addition of 185 g of ammonia solution all at once was 8.9.

[0075] The precursor slurry obtained in step 2 was collected and washed with an ultrafiltration membrane, a membrane with a UF molecular weight cutoff of 50,000, until the electrical conductivity of the filtrate became 30 mS / m or less (step 3). After that, 865 g of the washed slurry obtained in step 3 was taken, and pure water was added to make the total volume 950 g. The temperature was adjusted to 40°C while stirring, and 258 g of 22.14 mass% ammonia aqueous solution and 1171 g of ethanol were added and stirred for 5 minutes, and 1028 g of tetraethoxysilane (TEOS) was added as a silicon compound having a hydrolyzable group over 35 minutes. After that, the liquid temperature was kept at 40°C and stirring was continued for 1 hour, and the silicon compound hydrolysis product was coated on the mixture. The obtained solution was then washed and separated into solid and liquid, and collected as a cake (step 4).

[0076] After drying the cake obtained in step 4 (precursor coated with gel-like hydrolysis product), the dried powder was heat-treated in an air furnace at 1130°C for 4 hours to obtain ε-iron oxide powder in which some of the Fe sites coated with silicon oxide were replaced with other metal elements. Note that the hydrolysis product of the silicon compound is converted to an oxide when heat-treated in an air atmosphere (step 5). The powder of ε-iron oxide in which the silicon oxide-coated Fe sites had been partially substituted with other metal elements obtained in step 5 was stirred in a 20 mass% NaOH aqueous solution at approximately 60°C for 24 hours to remove the silicon oxide from the particle surfaces, thereby obtaining a slurry containing ε-iron oxide particles in which the Fe sites had been partially substituted with other metal elements (step 6).

[0077] The slurry obtained in step 6 was washed with pure water until the electrical conductivity became ≦15 mS / m, thereby obtaining a washed slurry according to Example 10. A 1% by mass aqueous sulfuric acid solution was added to the washed slurry to adjust the pH to 6.5, and then the slurry was subjected to membrane filtration. The cake was recovered and then dried, thereby obtaining an iron-based oxide magnetic powder according to Example 10. The magnetic properties of this iron oxide magnetic powder were measured and found to be coercive force of 779 kA / m and saturation magnetization of 15.8 Am. 2 / kg, SFD is 0.70, I L / I HThe value was 0.20. In addition, this iron-based oxide magnetic powder was subjected to TEM observation in the same manner as in Example 1, and the results showed that the TEM average particle diameter was 16.2 nm, the number fraction of particles with a particle diameter of 8 nm or less was 0.8%, the number fraction of particles with a particle diameter of 20 nm or more was 14.2%, the coefficient of variation (CV value) was 24%, and the average circularity of the particles was 0.975.

[0078] [Example 11] As the raw material solution, 936 g of an aqueous solution with Fe(III) concentration of 0.921 mol / kg, Ga(III) concentration of 0.321 mol / kg, Co(II) concentration of 0.056 mol / kg, chloride ion concentration of 0.551 mol / kg, and nitrate ion concentration of 3.396 mol / kg was prepared. Next, 1578 g of an aqueous solution with Fe(III) concentration of 0.182 mol / kg and chloride ion concentration of 0.547 mol / kg was placed in a 5 L reaction tank, and the liquid temperature was adjusted to 40 ° C. while mechanically stirring with a stirring blade. Next, while continuing the stirring and keeping the liquid temperature at 40 ° C., the raw material solution and 3.651 mol / kg ammonia aqueous solution were added simultaneously to this aqueous solution, and then the liquid temperature was kept at 40 ° C. and stirred for 60 minutes to obtain a colloidal solution (step 1, first neutralization step). Here, the raw material solution was added continuously at a rate of 3.9 g / min over 240 minutes, and the aqueous ammonia solution was added continuously at a rate of 3.9 g / min over 240 minutes. During the addition of the raw material solution and the aqueous ammonia solution, the ratio of the cumulative amount of alkali added to the total cumulative amount of acid radicals contained in the raw material solution was 0.93 equivalents. The pH of the resulting colloidal solution was 2.0. Next, 289 g of citric acid solution with a citric acid concentration of 1.041 mol / kg was added continuously to the colloidal solution obtained in step 1 as a hydroxycarboxylic acid over a period of 60 minutes at 40° C. (hydroxycarboxylic acid addition step), and then 196 g of ammonia solution with a concentration of 12.553 mol / kg was added all at once. The mixture was then kept at 40° C. for 10 minutes while stirring to obtain a precursor slurry, which is an intermediate product (step 2, second neutralization step). The pH after the addition of 196 g of ammonia solution all at once was 8.6.

[0079] The precursor slurry obtained in step 2 was collected and washed with an ultrafiltration membrane, a membrane with a UF molecular weight cutoff of 50,000, until the electrical conductivity of the filtrate became 150 mS / m or less (step 3). After that, 1121 g of the washed slurry obtained in step 3 was taken, and pure water was added to make the total volume 1150 g. The temperature was adjusted to 40°C while stirring, and 345 g of 21.39 mass% ammonia aqueous solution and 1406 g of 2-propanol were added and stirred for 5 minutes, and 1327 g of tetraethoxysilane (TEOS) was added as a silicon compound having a hydrolyzable group over 35 minutes. After that, the liquid temperature was kept at 40°C and stirring was continued for 1 hour, and the silicon compound hydrolysis product was coated. The obtained solution was then washed and separated into solid and liquid, and collected as a cake (step 4).

[0080] After drying the cake obtained in step 4 (precursor coated with gel-like hydrolysis product), the dried powder was heat-treated in an air furnace at 1060°C for 4 hours to obtain ε-iron oxide powder in which some of the Fe sites coated with silicon oxide were replaced with other metal elements. Note that the hydrolysis product of the silicon compound is converted to an oxide when heat-treated in an air atmosphere (step 5). The powder of ε-iron oxide in which the silicon oxide-coated Fe sites had been partially substituted with other metal elements obtained in step 5 was stirred in a 20 mass% NaOH aqueous solution at approximately 60°C for 14 hours to remove the silicon oxide from the particle surfaces, thereby obtaining a slurry containing ε-iron oxide particles in which the Fe sites had been partially substituted with other metal elements (step 6).

[0081] The slurry obtained in step 6 was washed with pure water until the electrical conductivity became ≦15 mS / m, thereby obtaining a washed slurry according to Example 11. A 1% by mass aqueous sulfuric acid solution was added to the washed slurry to adjust the pH to 6.5, and then the slurry was subjected to membrane filtration. The cake was recovered and then dried, thereby obtaining an iron-based oxide magnetic powder according to Example 11. The magnetic properties of this iron oxide magnetic powder were measured and found to be coercive force of 339 kA / m and saturation magnetization of 16.4 Am. 2 / kg, SFD is 1.05, I L / IH The value was 0.49. In addition, this iron-based oxide magnetic powder was subjected to TEM observation in the same manner as in Example 1, and the results showed that the TEM average particle diameter was 15.0 nm, the number fraction of particles with a particle diameter of 8 nm or less was 2.0%, the number fraction of particles with a particle diameter of 20 nm or more was 8.5%, the coefficient of variation (CV value) was 22%, and the average circularity of the particles was 0.968.

[0082] [Example 12] As the raw material solution, 894 g of an aqueous solution with Fe(III) concentration of 1.009 mol / kg, Ga(III) concentration of 0.294 mol / kg, Ti(IV) concentration of 0.042 mol / kg, chloride ion concentration of 3.270 mol / kg, and nitrate ion concentration of 0.878 mol / kg was prepared. Next, 1581 g of an aqueous solution with Fe(III) concentration of 0.190 mol / kg and chloride ion concentration of 0.596 mol / kg was placed in a 5 L reaction tank, and the liquid temperature was adjusted to 30 ° C. while mechanically stirring with a stirring blade. Next, while continuing the stirring and keeping the liquid temperature at 30 ° C., the raw material solution and 4.423 mol / kg of ammonia aqueous solution were added simultaneously to this aqueous solution, and then the liquid temperature was kept at 30 ° C. and stirred for 60 minutes to obtain a colloidal solution (step 1, first neutralization step). Here, the raw material solution was added continuously at a rate of 3.7 g / min over 240 minutes, and the aqueous ammonia solution was added continuously at a rate of 3.7 g / min over 240 minutes. During the addition of the raw material solution and the aqueous ammonia solution, the ratio of the cumulative amount of alkali added to the total cumulative amount of acid radicals contained in the raw material solution was 1.07 equivalents. The pH of the resulting colloidal solution was 2.3. Next, 289 g of citric acid solution with a citric acid concentration of 1.041 mol / kg was added continuously to the colloidal solution obtained in step 1 as a hydroxycarboxylic acid over a period of 60 minutes at 30° C. (hydroxycarboxylic acid addition step), and then 139 g of ammonia solution with a concentration of 14.707 mol / kg was added all at once. The mixture was then kept at 30° C. for 10 minutes while stirring to obtain a precursor slurry, which is an intermediate product (step 2, second neutralization step). The pH after the addition of 139 g of ammonia solution all at once was 8.9.

[0083] The precursor slurry obtained in step 2 was collected and washed with an ultrafiltration membrane, a membrane with a UF molecular weight cutoff of 50,000, until the electrical conductivity of the filtrate became 150 mS / m or less (step 3). After that, 1114 g of the washed slurry obtained in step 3 was taken, and pure water was added to make the total volume 1150 g. The temperature was adjusted to 30°C while stirring, and 142 g of 25.06 mass% ammonia aqueous solution and 1406 g of 2-propanol were added and stirred for 5 minutes, and 640 g of tetraethoxysilane (TEOS) was added as a silicon compound having a hydrolyzable group over 35 minutes. After that, the liquid temperature was kept at 30°C and stirring was continued for 1 hour, and the silicon compound hydrolysis product was coated. The obtained solution was then washed and separated into solid and liquid, and collected as a cake (step 4).

[0084] After drying the cake obtained in step 4 (precursor coated with gel-like hydrolysis product), the dried powder was heat-treated in a furnace in an air atmosphere at 1100°C for 4 hours to obtain ε-iron oxide powder in which some of the Fe sites coated with silicon oxide were replaced with other metal elements. Note that the hydrolysis product of the silicon compound is converted to an oxide when heat-treated in an air atmosphere (step 5). The powder of ε-iron oxide in which the silicon oxide-coated Fe sites had been partially substituted with other metal elements obtained in step 5 was stirred in a 20 mass% NaOH aqueous solution at approximately 60°C for 14 hours to remove the silicon oxide from the particle surfaces, thereby obtaining a slurry containing ε-iron oxide particles in which the Fe sites had been partially substituted with other metal elements (step 6).

[0085] The slurry obtained in step 6 was washed with pure water until the electrical conductivity became ≦15 mS / m, thereby obtaining a washed slurry according to Example 12. A 1% by mass aqueous sulfuric acid solution was added to the washed slurry to adjust the pH to 6.5, and then the slurry was subjected to membrane filtration. The cake was recovered and then dried, thereby obtaining an iron-based oxide magnetic powder according to Example 12. The magnetic properties of this iron oxide magnetic powder were measured and found to be coercive force of 485 kA / m and saturation magnetization of 20.5 Am. 2 / kg, SFD is 1.31, I L / IH The value was 0.44. In addition, this iron-based oxide magnetic powder was subjected to TEM observation in the same manner as in Example 1, and the results showed that the TEM average particle diameter was 15.2 nm, the number proportion of particles with a particle diameter of 8 nm or less was 2.2%, the number proportion of particles with a particle diameter of 20 nm or more was 14.0%, the coefficient of variation (CV value) was 39%, and the average circularity of the particles was 0.955.

[0086] [Example 13] As the raw material solution, 893 g of raw material solution with Fe(III) concentration of 0.928 mol / kg, Ga(III) concentration of 0.202 mol / kg, Co(II) concentration of 0.038 mol / kg, Ti(IV) concentration of 0.038 mol / kg, Mn(II) concentration of 0.168 mol / kg, chloride ion concentration of 2.880 mol / kg, and nitrate ion concentration of 1.051 mol / kg was prepared. Next, 1575 g of an aqueous solution with Fe(III) concentration of 0.175 mol / kg and chloride ion concentration of 0.526 mol / kg was placed in a 5 L reaction tank, and the liquid temperature was adjusted to 40 ° C. while mechanically stirring with a stirring blade. Next, while continuing the stirring and keeping the liquid temperature at 40 ° C., the raw material solution and 3.644 mol / kg aqueous ammonia solution were added simultaneously to this aqueous solution, and then the liquid temperature was kept at 40 ° C. and stirred for 60 minutes to obtain a colloidal solution (step 1, first neutralization step). Here, the raw material solution was added continuously at a rate of 3.7 g / min over 240 minutes, and the aqueous ammonia solution was added continuously at a rate of 3.7 g / min over 240 minutes. During the addition of the raw material solution and the aqueous ammonia solution, the ratio of the cumulative amount of alkali added to the total cumulative amount of acid radicals contained in the raw material solution was 0.93 equivalents. The pH of the resulting colloidal solution was 2.1. Next, 260g of citric acid solution with a citric acid concentration of 1.041 mol / kg was added continuously to the colloidal solution obtained in step 1 as a hydroxycarboxylic acid over a period of 60 minutes at 40°C (hydroxycarboxylic acid addition step), and then 188g of ammonia solution with a concentration of 12.465 mol / kg was added all at once, and the mixture was kept at 40°C for 10 minutes while stirring to obtain a precursor slurry, which is an intermediate product (step 2, second neutralization step). After adding 188g of ammonia solution all at once, the pH was 8.7.

[0087] The precursor slurry obtained in step 2 was collected and washed with an ultrafiltration membrane, a membrane with a UF molecular weight cutoff of 50,000, until the electrical conductivity of the filtrate became 30 mS / m or less (step 3). After that, 1107g of the washed slurry obtained in step 3 was taken, and pure water was added to make the total volume 1150g. The temperature was adjusted to 40°C while stirring, and 153g of 23.24 mass% ammonia aqueous solution and 1406g of 2-propanol were added and stirred for 5 minutes, and 640g of tetraethoxysilane (TEOS) was added as a silicon compound having a hydrolyzable group over 35 minutes. After that, the liquid temperature was kept at 40°C and stirring was continued for 1 hour, and the silicon compound hydrolysis product was coated on the slurry. The obtained solution was then washed and separated into solid and liquid, and collected as a cake (step 4).

[0088] After drying the cake obtained in step 4 (precursor coated with gel-like hydrolysis product), the dried powder was heat-treated in an air furnace at 1130°C for 4 hours to obtain ε-iron oxide powder in which some of the Fe sites coated with silicon oxide were replaced with other metal elements. Note that the hydrolysis product of the silicon compound is converted to an oxide when heat-treated in an air atmosphere (step 5). The powder of ε-iron oxide in which the silicon oxide-coated Fe sites had been partially substituted with other metal elements obtained in step 5 was stirred in a 20 mass% NaOH aqueous solution at approximately 60°C for 14 hours to remove the silicon oxide from the particle surfaces, thereby obtaining a slurry containing ε-iron oxide particles in which the Fe sites had been partially substituted with other metal elements (step 6).

[0089] The slurry obtained in step 6 was washed with pure water until the electrical conductivity became ≦15 mS / m, thereby obtaining a washed slurry according to Example 13. A 1% by mass aqueous sulfuric acid solution was added to the washed slurry to adjust the pH to 6.5, and then the slurry was subjected to membrane filtration. The cake was recovered and then dried, thereby obtaining an iron-based oxide magnetic powder according to Example 13. The magnetic properties of this iron oxide magnetic powder were measured and found to be coercive force of 569 kA / m and saturation magnetization of 18.3 Am. 2 / kg, SFD is 0.75, I L / I H The value was 0.21. In addition, this iron-based oxide magnetic powder was subjected to TEM observation in the same manner as in Example 1, and the results showed that the TEM average particle diameter was 16.8 nm, the number fraction of particles with a particle diameter of 8 nm or less was 0.4%, the number fraction of particles with a particle diameter of 20 nm or more was 17.8%, the coefficient of variation (CV value) was 24%, and the average circularity of the particles was 0.972.

[0090] [Example 14] As the raw material solution, 893 g of an aqueous solution with Fe(III) concentration of 0.993 mol / kg, Ga(III) concentration of 0.235 mol / kg, Co(II) concentration of 0.038 mol / kg, Ni(II) concentration of 0.084 mol / kg, chloride ion concentration of 2.980 mol / kg, and nitrate ion concentration of 1.005 mol / kg was prepared. Next, 1581 g of an aqueous solution with Fe(III) concentration of 0.187 mol / kg and chloride ion concentration of 0.561 mol / kg was placed in a 5 L reaction tank, and the liquid temperature was adjusted to 40 ° C. while mechanically stirring with a stirring blade. Next, while continuing the stirring and maintaining the liquid temperature at 40 ° C., the raw material solution and 3.734 mol / kg aqueous ammonia solution were added simultaneously to this aqueous solution, and then the liquid temperature was kept at 40 ° C. and stirred for 60 minutes to obtain a colloidal solution (step 1, first neutralization step). Here, the raw material solution was added continuously at a rate of 3.7 g / min over 240 minutes, and the aqueous ammonia solution was added continuously at a rate of 3.7 g / min over 240 minutes. During the addition of the raw material solution and the aqueous ammonia solution, the ratio of the cumulative amount of alkali added to the total cumulative amount of acid radicals contained in the raw material solution was 0.94 equivalents. The pH of the resulting colloidal solution was 2.1. Next, 274 g of citric acid solution with a citric acid concentration of 1.041 mol / kg was added continuously to the colloidal solution obtained in step 1 as a hydroxycarboxylic acid over a period of 60 minutes at 40° C. (hydroxycarboxylic acid addition step), and then 193 g of ammonia solution with a concentration of 12.465 mol / kg was added all at once. The mixture was then kept at 40° C. for 10 minutes while stirring to obtain a precursor slurry, which is an intermediate product (step 2, second neutralization step). After adding 188 g of ammonia solution all at once, the pH was 8.8.

[0091] The precursor slurry obtained in step 2 was collected and washed with an ultrafiltration membrane, a membrane with a UF molecular weight cutoff of 50,000, until the electrical conductivity of the filtrate became 30 mS / m or less (step 3). After that, 1057g of the washed slurry obtained in step 3 was taken, and pure water was added to make the total volume 1150g. The temperature was adjusted to 40°C while stirring, and 347g of 21.24 mass% ammonia aqueous solution and 1406g of ethanol were added and stirred for 5 minutes, and 1327g of tetraethoxysilane (TEOS) was added as a silicon compound having a hydrolyzable group over 35 minutes. After that, the liquid temperature was kept at 40°C and stirring was continued for 1 hour, and the silicon compound hydrolysis product was coated. The obtained solution was then washed and separated into solid and liquid, and collected as a cake (step 4).

[0092] After drying the cake obtained in step 4 (precursor coated with gel-like hydrolysis product), the dried powder was heat-treated in an air furnace at 1130°C for 4 hours to obtain ε-iron oxide powder in which some of the Fe sites coated with silicon oxide were replaced with other metal elements. Note that the hydrolysis product of the silicon compound is converted to an oxide when heat-treated in an air atmosphere (step 5). The powder of ε-iron oxide in which the silicon oxide-coated Fe sites had been partially substituted with other metal elements obtained in step 5 was stirred in a 20 mass% NaOH aqueous solution at approximately 60°C for 14 hours to remove the silicon oxide from the particle surfaces, thereby obtaining a slurry containing ε-iron oxide particles in which the Fe sites had been partially substituted with other metal elements (step 6).

[0093] The slurry obtained in step 6 was washed with pure water until the electrical conductivity became ≦15 mS / m, thereby obtaining a washed slurry according to Example 14. A 1% by mass aqueous sulfuric acid solution was added to the washed slurry to adjust the pH to 6.5, and then the slurry was subjected to membrane filtration. The cake was recovered and then dried, thereby obtaining an iron-based oxide magnetic powder according to Example 14. The magnetic properties of this iron oxide magnetic powder were measured and found to be coercive force of 394 kA / m and saturation magnetization of 23.4 Am. 2 / kg, SFD is 1.53, I L / I H The value was 1.31. In addition, this iron-based oxide magnetic powder was subjected to TEM observation using the same procedure as in Example 1, and the results showed that the TEM average particle diameter was 14.6 nm, the number fraction of particles with a particle diameter of 8 nm or less was 1.9%, the number fraction of particles with a particle diameter of 20 nm or more was 7.0%, the coefficient of variation (CV value) was 25%, and the average circularity of the particles was 0.967.

[0094] [Example 15] As the raw material solution, 895 g of an aqueous solution with Fe(III) concentration of 0.991 mol / kg, Ga(III) concentration of 0.235 mol / kg, Co(II) concentration of 0.038 mol / kg, Cr(III) concentration of 0.084 mol / kg, chloride ion concentration of 2.974 mol / kg, and nitrate ion concentration of 1.087 mol / kg was prepared. Next, 1581 g of an aqueous solution with Fe(III) concentration of 0.187 mol / kg and chloride ion concentration of 0.561 mol / kg was placed in a 5 L reaction tank, and the liquid temperature was adjusted to 40 ° C. while mechanically stirring with a stirring blade. Next, while continuing the stirring and keeping the liquid temperature at 40 ° C., the raw material solution and 3.808 mol / kg of ammonia aqueous solution were added simultaneously to this aqueous solution, and then the liquid temperature was kept at 40 ° C. and stirred for 60 minutes to obtain a colloidal solution (step 1, first neutralization step). Here, the raw material solution was added continuously at a rate of 3.7 g / min over 240 minutes, and the aqueous ammonia solution was added continuously at a rate of 3.7 g / min over 240 minutes. During the addition of the raw material solution and the aqueous ammonia solution, the ratio of the cumulative amount of alkali added to the total cumulative amount of acid radicals contained in the raw material solution was 0.94 equivalents. The pH of the resulting colloidal solution was 2.0. Next, 289 g of citric acid solution with a citric acid concentration of 1.041 mol / kg was added continuously over 60 minutes at 40° C. to the colloidal solution obtained in step 1 (hydroxycarboxylic acid addition step), and then 196 g of ammonia solution with a concentration of 12.553 mol / kg was added all at once, and the mixture was kept at 40° C. for 10 minutes while stirring to obtain a precursor slurry, which is an intermediate product (step 2, second neutralization step). The pH after the addition of 196 g of ammonia solution all at once was 8.5.

[0095] The precursor slurry obtained in step 2 was collected and washed with an ultrafiltration membrane, a membrane with a UF molecular weight cutoff of 50,000, until the electrical conductivity of the filtrate became 30 mS / m or less (step 3). After that, 1084 g of the washed slurry obtained in step 3 was taken, and pure water was added to make the total volume 1150 g. The temperature was adjusted to 40°C while stirring, and 345 g of 21.39 mass% ammonia aqueous solution and 1406 g of ethanol were added and stirred for 5 minutes, and 1327 g of tetraethoxysilane (TEOS) was added as a silicon compound having a hydrolyzable group over 35 minutes. After that, the liquid temperature was kept at 40°C and stirring was continued for 1 hour, and the silicon compound hydrolysis product was coated. The obtained solution was then washed and separated into solid and liquid, and collected as a cake (step 4).

[0096] After drying the cake obtained in step 4 (precursor coated with gel-like hydrolysis product), the dried powder was heat-treated in an air furnace at 1130°C for 4 hours to obtain ε-iron oxide powder in which some of the Fe sites coated with silicon oxide were replaced with other metal elements. Note that the hydrolysis product of the silicon compound is converted to an oxide when heat-treated in an air atmosphere (step 5). The powder of ε-iron oxide in which the silicon oxide-coated Fe sites had been partially substituted with other metal elements obtained in step 5 was stirred in a 20 mass% NaOH aqueous solution at approximately 60°C for 14 hours to remove the silicon oxide from the particle surfaces, thereby obtaining a slurry containing ε-iron oxide particles in which the Fe sites had been partially substituted with other metal elements (step 6).

[0097] The slurry obtained in step 6 was washed with pure water until the electrical conductivity became ≦15 mS / m, thereby obtaining a washed slurry according to Example 15. A 1% by mass aqueous sulfuric acid solution was added to the washed slurry to adjust the pH to 6.5, and then the slurry was filtered through a membrane. The cake was recovered and then dried, thereby obtaining an iron-based oxide magnetic powder according to Example 15. The magnetic properties of this iron oxide magnetic powder were measured and found to be coercive force of 400 kA / m and saturation magnetization of 15.3 Am. 2 / kg, SFD is 2.28, I L / I HThe value was 0.76. In addition, this iron-based oxide magnetic powder was subjected to TEM observation in the same manner as in Example 1, and the results showed that the TEM average particle diameter was 14.9 nm, the number fraction of particles with a particle diameter of 8 nm or less was 0.5%, the number fraction of particles with a particle diameter of 20 nm or more was 9.9%, the coefficient of variation (CV value) was 28%, and the average circularity of the particles was 0.968.

[0098] [Example 16] As the raw material solution, 894 g of an aqueous solution with Fe(III) concentration of 1.024 mol / kg, Ga(III) concentration of 0.235 mol / kg, Co(II) concentration of 0.038 mol / kg, Nd(III) concentration of 0.042 mol / kg, chloride ion concentration of 3.072 mol / kg, and nitrate ion concentration of 0.962 mol / kg was prepared. Next, 1583 g of an aqueous solution with Fe(III) concentration of 0.193 mol / kg and chloride ion concentration of 0.578 mol / kg was placed in a 5 L reaction tank, and the liquid temperature was adjusted to 40 ° C. while mechanically stirring with a stirring blade. Next, while continuing the stirring and keeping the liquid temperature at 40 ° C., the raw material solution and 3.793 mol / kg ammonia aqueous solution were added simultaneously to this aqueous solution, and then the liquid temperature was kept at 40 ° C. and stirred for 60 minutes to obtain a colloidal solution (step 1, first neutralization step). Here, the raw material solution was added continuously at a rate of 3.7 g / min over 240 minutes, and the aqueous ammonia solution was added continuously at a rate of 3.7 g / min over 240 minutes. During the addition of the raw material solution and the aqueous ammonia solution, the ratio of the cumulative amount of alkali added to the total cumulative amount of acid radicals contained in the raw material solution was 0.94 equivalents. The pH of the resulting colloidal solution was 2.0. Next, 282 g of citric acid solution with a citric acid concentration of 1.041 mol / kg was added continuously to the colloidal solution obtained in step 1 as a hydroxycarboxylic acid over a period of 60 minutes at 40° C. (hydroxycarboxylic acid addition step), and then 196 g of ammonia solution with a concentration of 12.465 mol / kg was added all at once. The mixture was then kept at 40° C. for 10 minutes while stirring to obtain a precursor slurry, which is an intermediate product (step 2, second neutralization step). The pH after the addition of 196 g of ammonia solution all at once was 8.8.

[0099] The precursor slurry obtained in step 2 was collected and washed with an ultrafiltration membrane, a membrane with a UF molecular weight cutoff of 50,000, until the electrical conductivity of the filtrate became 30 mS / m or less (step 3). After that, 1120 g of the washed slurry obtained in step 3 was taken, and pure water was added to make the total volume 1150 g. The temperature was adjusted to 40°C while stirring, and 347 g of 21.24 mass% ammonia aqueous solution and 1406 g of ethanol were added and stirred for 5 minutes, and 1327 g of tetraethoxysilane (TEOS) was added as a silicon compound having a hydrolyzable group over 35 minutes. After that, the liquid temperature was kept at 40°C and stirring was continued for 1 hour, and the silicon compound hydrolysis product was coated. The obtained solution was then washed and separated into solid and liquid, and collected as a cake (step 4).

[0100] After drying the cake obtained in step 4 (precursor coated with gel-like hydrolysis product), the dried powder was heat-treated in an air furnace at 1090°C for 4 hours to obtain ε-iron oxide powder in which some of the Fe sites coated with silicon oxide were replaced with other metal elements. Note that the hydrolysis product of the silicon compound is converted to an oxide when heat-treated in an air atmosphere (step 5). The powder of ε-iron oxide in which the silicon oxide-coated Fe sites had been partially substituted with other metal elements obtained in step 5 was stirred in a 20 mass% NaOH aqueous solution at approximately 60°C for 24 hours to remove the silicon oxide from the particle surfaces, thereby obtaining a slurry containing ε-iron oxide particles in which the Fe sites had been partially substituted with other metal elements (step 6).

[0101] The slurry obtained in step 6 was washed with pure water until the electrical conductivity became ≦15 mS / m, thereby obtaining a washed slurry according to Example 16. A 1% by mass aqueous sulfuric acid solution was added to the washed slurry to adjust the pH to 6.5, and then the slurry was subjected to membrane filtration. The cake was recovered and then dried, thereby obtaining an iron-based oxide magnetic powder according to Example 16. The magnetic properties of this iron oxide magnetic powder were measured and found to be coercive force of 415 kA / m and saturation magnetization of 18.9 Am. 2 / kg, SFD is 2.03, I L / IH The value was 0.58. In addition, this iron-based oxide magnetic powder was subjected to TEM observation using the same procedure as in Example 1, and the results showed that the TEM average particle diameter was 13.8 nm, the number fraction of particles with a particle diameter of 8 nm or less was 1.9%, the number fraction of particles with a particle diameter of 20 nm or more was 6.7%, the coefficient of variation (CV value) was 25%, and the average circularity of the particles was 0.966.

[0102] [Example 17] As the raw material solution, 894 g of an aqueous solution with Fe(III) concentration of 1.024 mol / kg, Ga(III) concentration of 0.235 mol / kg, Co(II) concentration of 0.038 mol / kg, Dy(III) concentration of 0.042 mol / kg, chloride ion concentration of 3.072 mol / kg, and nitrate ion concentration of 0.962 mol / kg was prepared. Next, 1583 g of an aqueous solution with Fe(III) concentration of 0.193 mol / kg and chloride ion concentration of 0.578 mol / kg was placed in a 5 L reaction tank, and the liquid temperature was adjusted to 40 ° C. while mechanically stirring with a stirring blade. Next, while continuing the stirring and keeping the liquid temperature at 40 ° C., the raw material solution and 3.793 mol / kg ammonia aqueous solution were added simultaneously to this aqueous solution, and then the liquid temperature was kept at 40 ° C. and stirred for 60 minutes to obtain a colloidal solution (step 1, first neutralization step). Here, the raw material solution was added continuously at a rate of 3.7 g / min over 240 minutes, and the aqueous ammonia solution was added continuously at a rate of 3.7 g / min over 240 minutes. During the addition of the raw material solution and the aqueous ammonia solution, the ratio of the cumulative amount of alkali added to the total cumulative amount of acid radicals contained in the raw material solution was 0.94 equivalents. The pH of the resulting colloidal solution was 2.1. Next, 282 g of citric acid solution with a citric acid concentration of 1.041 mol / kg was added continuously to the colloidal solution obtained in step 1 as a hydroxycarboxylic acid over a period of 60 minutes at 40° C. (hydroxycarboxylic acid addition step), and then 196 g of ammonia solution with a concentration of 12.465 mol / kg was added all at once. The mixture was then kept at 40° C. for 10 minutes while stirring to obtain a precursor slurry, which is an intermediate product (step 2, second neutralization step). The pH after the addition of 196 g of ammonia solution all at once was 8.8.

[0103] The precursor slurry obtained in step 2 was collected and washed with an ultrafiltration membrane, a membrane with a UF molecular weight cutoff of 50,000, until the electrical conductivity of the filtrate became 30 mS / m or less (step 3). After that, 1097 g of the washed slurry obtained in step 3 was taken, and pure water was added to make the total volume 1150 g. The temperature was adjusted to 40°C while stirring, and 347 g of 21.24 mass% ammonia aqueous solution and 1406 g of ethanol were added and stirred for 5 minutes, and 1327 g of tetraethoxysilane (TEOS) was added as a silicon compound having a hydrolyzable group over 35 minutes. After that, the liquid temperature was kept at 40°C and stirring was continued for 1 hour, and the silicon compound hydrolysis product was coated. The obtained solution was then washed and separated into solid and liquid, and collected as a cake (step 4).

[0104] After drying the cake obtained in step 4 (precursor coated with gel-like hydrolysis product), the dried powder was heat-treated in an air furnace at 1090°C for 4 hours to obtain ε-iron oxide powder in which some of the Fe sites coated with silicon oxide were replaced with other metal elements. Note that the hydrolysis product of the silicon compound is converted to an oxide when heat-treated in an air atmosphere (step 5). The powder of ε-iron oxide in which the silicon oxide-coated Fe sites had been partially substituted with other metal elements obtained in step 5 was stirred in a 20 mass% NaOH aqueous solution at approximately 60°C for 24 hours to remove the silicon oxide from the particle surfaces, thereby obtaining a slurry containing ε-iron oxide particles in which the Fe sites had been partially substituted with other metal elements (step 6).

[0105] The slurry obtained in step 6 was washed with pure water until the electrical conductivity became ≦15 mS / m, thereby obtaining a washed slurry according to Example 17. A 1% by mass aqueous sulfuric acid solution was added to the washed slurry to adjust the pH to 6.5, and then the slurry was subjected to membrane filtration. The cake was recovered and then dried, thereby obtaining an iron-based oxide magnetic powder according to Example 17. The magnetic properties of this iron oxide magnetic powder were measured and found to be coercive force of 441 kA / m and saturation magnetization of 19.0 Am. 2 / kg, SFD was 1.97, IL / I H The value was 0.55. In addition, this iron-based oxide magnetic powder was subjected to TEM observation in the same manner as in Example 1, and the results showed that the TEM average particle diameter was 13.9 nm, the number proportion of particles with a particle diameter of 8 nm or less was 3.0%, the number proportion of particles with a particle diameter of 20 nm or more was 5.6%, the coefficient of variation (CV value) was 25%, and the average circularity of the particles was 0.966.

[0106] [Example 18] As the raw material solution, 894 g of an aqueous solution with Fe(III) concentration of 1.024 mol / kg, Ga(III) concentration of 0.235 mol / kg, Co(II) concentration of 0.038 mol / kg, Gd(III) concentration of 0.042 mol / kg, chloride ion concentration of 3.072 mol / kg, and nitrate ion concentration of 0.962 mol / kg was prepared. Next, 1583 g of an aqueous solution with Fe(III) concentration of 0.193 mol / kg and chloride ion concentration of 0.578 mol / kg was placed in a 5 L reaction tank, and the liquid temperature was adjusted to 40 ° C. while mechanically stirring with a stirring blade. Next, while continuing the stirring and keeping the liquid temperature at 40 ° C., the raw material solution and 3.793 mol / kg ammonia aqueous solution were added simultaneously to this aqueous solution, and then the liquid temperature was kept at 40 ° C. and stirred for 60 minutes to obtain a colloidal solution (step 1, first neutralization step). Here, the raw material solution was added continuously at a rate of 3.7 g / min over 240 minutes, and the aqueous ammonia solution was added continuously at a rate of 3.7 g / min over 240 minutes. During the addition of the raw material solution and the aqueous ammonia solution, the ratio of the cumulative amount of alkali added to the total cumulative amount of acid radicals contained in the raw material solution was 0.94 equivalents. The pH of the resulting colloidal solution was 2.1. Next, 282 g of citric acid solution with a citric acid concentration of 1.041 mol / kg was added continuously to the colloidal solution obtained in step 1 as a hydroxycarboxylic acid over a period of 60 minutes at 40° C. (hydroxycarboxylic acid addition step), and then 196 g of ammonia solution with a concentration of 12.465 mol / kg was added all at once. The mixture was then kept at 40° C. for 10 minutes while stirring to obtain a precursor slurry, which is an intermediate product (step 2, second neutralization step). The pH after the addition of 196 g of ammonia solution all at once was 8.8.

[0107] The precursor slurry obtained in step 2 was collected and washed with an ultrafiltration membrane, a membrane with a UF molecular weight cutoff of 50,000, until the electrical conductivity of the filtrate became 30 mS / m or less (step 3). After that, 1132 g of the washed slurry obtained in step 3 was taken, and pure water was added to make the total volume 1150 g. The temperature was adjusted to 40°C while stirring, and 347 g of 21.24 mass% ammonia aqueous solution and 1406 g of ethanol were added and stirred for 5 minutes, and 1327 g of tetraethoxysilane (TEOS) was added as a silicon compound having a hydrolyzable group over 35 minutes. After that, the liquid temperature was kept at 40°C and stirring was continued for 1 hour, and the silicon compound hydrolysis product was coated. The obtained solution was then washed and separated into solid and liquid, and collected as a cake (step 4).

[0108] After drying the cake obtained in step 4 (precursor coated with gel-like hydrolysis product), the dried powder was heat-treated in an air furnace at 1090°C for 4 hours to obtain ε-iron oxide powder in which some of the Fe sites coated with silicon oxide were replaced with other metal elements. Note that the hydrolysis product of the silicon compound is converted to an oxide when heat-treated in an air atmosphere (step 5). The powder of ε-iron oxide in which the silicon oxide-coated Fe sites had been partially substituted with other metal elements obtained in step 5 was stirred in a 20 mass% NaOH aqueous solution at approximately 60°C for 24 hours to remove the silicon oxide from the particle surfaces, thereby obtaining a slurry containing ε-iron oxide particles in which the Fe sites had been partially substituted with other metal elements (step 6).

[0109] The slurry obtained in step 6 was washed with pure water until the electrical conductivity became ≦15 mS / m, thereby obtaining a washed slurry according to Example 18. A 1% by mass aqueous sulfuric acid solution was added to the washed slurry to adjust the pH to 6.5, and then the slurry was filtered through a membrane. The cake was recovered and then dried, thereby obtaining an iron-based oxide magnetic powder according to Example 18. The magnetic properties of this iron oxide magnetic powder were measured and found to be coercive force of 426 kA / m and saturation magnetization of 18.8 Am. 2 / kg, SFD is 1.46, I L / I H The value was 0.58. In addition, this iron-based oxide magnetic powder was subjected to TEM observation in the same manner as in Example 1, and the results showed that the TEM average particle diameter was 13.7 nm, the number fraction of particles with a particle diameter of 8 nm or less was 0.9%, the number fraction of particles with a particle diameter of 20 nm or more was 2.7%, the coefficient of variation (CV value) was 25%, and the average circularity of the particles was 0.966.

[0110] [Example 19] As the raw material solution, 941 g of an aqueous solution with Fe(III) concentration of 1.366 mol / kg, Ga(III) concentration of 0.160 mol / kg, Co(II) concentration of 0.036 mol / kg, Ti(IV) concentration of 0.036 mol / kg, chloride ion concentration of 4.190 mol / kg, and nitrate ion concentration of 0.606 mol / kg was prepared. Next, 1500 g of pure water was placed in a 5 L reaction tank, and the liquid temperature was adjusted to 40 ° C. while mechanically stirring with a stirring blade. Next, while continuing the stirring and keeping the liquid temperature at 40 ° C., the raw material solution and 3.836 mol / kg aqueous ammonia solution were added simultaneously to the pure water, and then the liquid temperature was kept at 40 ° C. and stirred for 60 minutes to obtain a colloidal solution (step 1, first neutralization step). Here, the raw material solution was added continuously at an addition rate of 3.9 g / min over 240 minutes, and the aqueous ammonia solution was added continuously at an addition rate of 3.9 g / min over 240 minutes. During the addition of the raw material solution and the aqueous ammonia solution, the ratio of the cumulative amount of alkali added to the total cumulative amount of acid radicals contained in the raw material solution was 0.80 equivalents. The pH of the resulting colloidal solution was 1.9. Next, 289 g of citric acid solution with a citric acid concentration of 1.041 mol / kg was added continuously to the colloidal solution obtained in step 1 as a hydroxycarboxylic acid over a period of 60 minutes at 40° C. (hydroxycarboxylic acid addition step), and then 190 g of ammonia solution with a concentration of 12.835 mol / kg was added all at once. The mixture was then kept at 40° C. for 10 minutes while stirring to obtain a precursor slurry, which is an intermediate product (step 2, second neutralization step). After adding 196 g of ammonia solution all at once, the pH was 8.6.

[0111] The precursor slurry obtained in step 2 was collected and washed with an ultrafiltration membrane, a membrane with a UF molecular weight cutoff of 50,000, until the electrical conductivity of the filtrate became 30 mS / m or less (step 3). After that, 705 g of the washed slurry obtained in step 3 was taken, and pure water was added to make the total weight 757 g. The temperature was adjusted to 40°C while stirring, and 207 g of 22.25 mass% ammonia aqueous solution and 945 g of 2-propanol were added and stirred for 5 minutes, and 829 g of tetraethoxysilane (TEOS) was added as a silicon compound having a hydrolyzable group over 35 minutes. After that, the liquid temperature was kept at 40°C and stirring was continued for 1 hour, and the silicon compound hydrolysis product was coated on the mixture. The obtained solution was then washed and separated into solid and liquid, and collected as a cake (step 4).

[0112] After drying the cake obtained in step 4 (precursor coated with gel-like hydrolysis product), the dried powder was heat-treated in an air furnace at 1050°C for 4 hours to obtain ε-iron oxide powder in which some of the Fe sites coated with silicon oxide were replaced with other metal elements. Note that the hydrolysis product of the silicon compound is converted to an oxide when heat-treated in an air atmosphere (step 5). The powder of ε-iron oxide in which the silicon oxide-coated Fe sites had been partially substituted with other metal elements obtained in step 5 was stirred in a 20 mass% NaOH aqueous solution at approximately 60°C for 24 hours to remove the silicon oxide from the particle surfaces, thereby obtaining a slurry containing ε-iron oxide particles in which the Fe sites had been partially substituted with other metal elements (step 6).

[0113] The slurry obtained in step 6 was washed with pure water until the electrical conductivity became ≦15 mS / m, thereby obtaining a washed slurry according to Example 18. A 1% by mass aqueous sulfuric acid solution was added to the washed slurry to adjust the pH to 6.5, and then the slurry was filtered through a membrane. The cake was recovered and then dried, thereby obtaining an iron-based oxide magnetic powder according to Example 18. The magnetic properties of this iron oxide magnetic powder were measured and found to be coercive force of 313 kA / m and saturation magnetization of 14.2 Am. 2 / kg, SFD was 2.39, I L / IH The value was 0.93. In addition, this iron-based oxide magnetic powder was subjected to TEM observation in the same manner as in Example 1, and the results showed that the TEM average particle diameter was 13.5 nm, the number proportion of particles with a particle diameter of 8 nm or less was 0.5%, the number proportion of particles with a particle diameter of 20 nm or more was 15.1%, the coefficient of variation (CV value) was 30%, and the average circularity of the particles was 0.959.

[0114] [Table 1]

[0115] [Table 2]

[0116] [Table 3]

[0117] [Table 4]

Claims

1. An iron-based oxide magnetic powder consisting of particles of ε-iron oxide or ε-iron oxide in which part of the Fe sites has been substituted with other metal elements, the particles having an average particle diameter of 10 nm or more and 20 nm or less as measured by a transmission electron microscope, the number ratio of particles having a particle diameter of 8 nm or less being 5% or less, the number ratio of particles having a particle diameter of 20 nm or more being 25% or less, and the average circularity of the particles observed by a transmission electron microscope being 0.955 or more.

2. 2. The iron-based oxide magnetic powder according to claim 1, wherein the coefficient of variation of particle size of the ε-iron oxide or the ε-iron oxide having a part of the Fe sites substituted with another metal element as measured by a transmission electron microscope is 20% or more and 30% or less.

3. 3. The iron-based oxide magnetic powder according to claim 1, wherein the metal element substituting a portion of the Fe sites is one or more of Ga, Co and Ti.

4. 2. The iron-based oxide magnetic powder according to claim 1, wherein the metal element substituting a portion of the Fe sites is one or more of Ga, Co, Ti, Ni, Mn, Cr, Nd, Dy and Gd.

5. A method for producing an iron-based oxide magnetic powder comprising particles of ε-iron oxide or ε-iron oxide in which a part of the Fe site is substituted with another metal element, the method comprising the steps of: a raw solution preparation step of preparing an aqueous solution containing trivalent iron ions or trivalent iron ions and ions of a metal element that substitutes a part of the Fe site (hereinafter referred to as a raw solution) and an alkaline aqueous solution for neutralizing the raw solution; a first neutralization step of continuously or intermittently adding and mixing the raw material solution and the aqueous alkaline solution to a reaction system to adjust the pH of the reaction system to 1.0 or more and 3.0 or less; adding a hydroxycarboxylic acid to the aqueous solution after the first neutralization step; a second neutralization step of adding an alkali to the aqueous solution containing the hydroxycarboxylic acid to neutralize the pH to 7.0 or more and 10.0 or less to obtain a slurry containing a precipitate of iron oxyhydroxide or iron oxyhydroxide containing a substituted metal element; a step of adding a silicon compound having a hydrolyzable group to a slurry containing the iron oxyhydroxide or the iron oxyhydroxide containing a substitution metal element, and coating the iron oxyhydroxide or the iron oxyhydroxide containing a substitution metal element with a hydrolysis product of the silicon compound; a step of heating the iron oxyhydroxide or the iron oxyhydroxide containing a substituted metal element coated with the hydrolysis product of the silicon compound to obtain an ε-iron oxide coated with silicon oxide or an ε-iron oxide in which a part of the Fe sites is substituted with another metal element; The method for producing the iron-based oxide magnetic powder according to claim 1, comprising:

6. 6. The method for producing an iron-based oxide magnetic powder according to claim 5, wherein the first neutralization step comprises continuously or intermittently adding and mixing the raw material solution and the aqueous alkaline solution containing 0.4 equivalents or more and 0.9 equivalents or less of alkali relative to the sum of the amounts of acid radicals contained in the raw material solution to a reaction system not containing trivalent iron ions and ions of metal elements substituting a portion of the Fe sites, to adjust the pH of the reaction system to 1.0 or more and 3.0 or less.

7. In the first neutralization step, when the raw material solution and the aqueous alkaline solution are added continuously or intermittently to a reaction system that already contains trivalent iron ions, or trivalent iron ions and ions of a metal element that replaces a part of the Fe sites, the amount of the trivalent iron ions and ions of a metal element that replaces a part of the Fe sites already contained in the reaction system is adjusted to a value that is equal to or larger than the amount of the trivalent iron ions and ions of a metal element that replaces a part of the Fe sites added to the reaction system.

5. The method for producing an iron-based oxide magnetic powder according to claim 4, wherein the raw material solution and the aqueous alkaline solution containing 0.4 to 1.8 equivalents of alkali relative to the sum of the amounts of trivalent iron ions and metal element ions substituting a portion of the Fe sites contained in the raw material solution to be added are each added continuously or intermittently to a reaction system and mixed to adjust the pH of the reaction system to 1.0 to 3.

0.

8. 7. The method for producing an iron-based oxide magnetic powder according to claim 6, wherein in the first neutralization step, the addition rates of the raw material solution and the aqueous alkaline solution are adjusted to maintain the cumulative addition amount of the alkali relative to the total cumulative addition amount of the acid radicals contained in the raw material solution in the range of 0.4 equivalents or more and 0.9 equivalents or less throughout the step.

9. 6. The method for producing an iron-based oxide magnetic powder according to claim 5, wherein in the first neutralization step, the raw material solution and the alkaline aqueous solution are added over a period of 10 minutes or more.

10. 6. The method for producing an iron-based oxide magnetic powder according to claim 5, wherein the slurry containing the iron oxyhydroxide or the iron oxyhydroxide containing a substituted metal element obtained in the second neutralization step has an average particle size of 300 nm or less as measured by a dynamic light scattering particle size distribution analyzer.

11. 6. The method for producing an iron-based oxide magnetic powder according to claim 5, wherein iron (III) chloride is used as a source of the trivalent iron ions contained in the raw material solution.

12. 7. The method for producing an iron-based oxide magnetic powder according to claim 6, wherein the cumulative amount of alkali added relative to the total cumulative amount of acid radicals added contained in the raw material solution is 0.6 equivalents or more and 0.9 equivalents or less through the first neutralization step.

13. 8. The method for producing an iron-based oxide magnetic powder according to claim 7, wherein the cumulative amount of alkali added relative to the total cumulative amount of acid radicals added contained in the raw material solution is 0.4 equivalents or more and 1.8 equivalents or less through the first neutralization step.

Citation Information

Patent Citations

  • epsi-IRON OXIDE POWDER HAVING IMPROVED MAGNETIC PROPERTY

    JP2008063201A

  • METHOD FOR PRODUCING epsilon-Fe2O3 CRYSTAL

    JP2008174405A

  • Ferrous oxide magnetic particle powder, method for manufacturing the same, coating material, and magnetic recording medium

    JP2016130208A

  • Manufacturing method of iron-based oxide magnetic particle powder

    JP2017024981A

  • Core shell particle, baked product of core shell particle, method of producing core shell particle, epsilon type iron oxide compound particle, method of producing epsilon type iron oxide compound particle, magnetic recording medium, and method of producing magnetic recording medium