Silicon-carbon negative electrode material and preparation method of silicon-carbon negative electrode material

By adopting porous silicon carbon matrix structure and spherical design, the problem of volume expansion and irregular morphology of silicon negative electrode materials is solved, the mechanical strength and cyclic electrochemical performance of silicon carbon negative electrode materials are improved, and the stability and efficiency are achieved .

CN118983419APending Publication Date: 2024-11-19GUANGDONG KAIJIN NEW ENERGY TECH CORP LTD
View PDF 0 Cites 6 Cited by

Patent Information

Application Number
CN202411076046.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The volume expansion of silicon negative electrode material during the cycle process is severe, causing the SEI film on the surface to rupture, consume lithium ions, and reduce electrochemical performance. The silicon carbon negative electrode material produced by carbon coating is irregular in shape and uneven stress distribution, which affects it. Stability and conductivity.

Method used

The porous silicon-carbon matrix structure is adopted, including nanosilicon, silicate layer, carbon-covered inner layer and carbon filler, to form a spherical silicon-carbon negative electrode material, and the nanosilicon slurry state is adjusted through spherical additives, and heat treatment is carried out after spray drying. Carbon outer layer improves the mechanical strength and cycle stability of the material.

Benefits of technology

The uniform expansion stress distribution of silicon-carbon anode material is achieved, the mechanical strength and cyclic electrochemical properties are improved, the SEI growth is reduced, and the material stability and first-time Coulomb efficiency are enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118983419A_ABST
    Figure CN118983419A_ABST
Patent Text Reader

Abstract

The invention provides a silicon-carbon negative electrode material and a preparation method thereof. The silicon-carbon negative electrode material comprises an inner core and a shell layer. The inner core comprises a porous silicon-carbon substrate, and the shell layer comprises a carbon-coated outer layer. The porous silicon-carbon substrate comprises nano silicon, a silicate layer, a carbon-coated inner layer and a carbon filling body from inside to outside. The carbon filling body has a pore structure, and the circularity of the silicon-carbon negative electrode material is greater than or equal to 0.9. The silicon-carbon negative electrode material is spherical, not only can effectively inhibit expansion of silicon, but also is uniform in stress distribution and not easy to crack when the silicon is expanded, and has relatively good electrochemical properties such as circulation and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of battery material preparation, and in particular to a silicon-carbon negative electrode material and a method for preparing the silicon-carbon negative electrode material. Background Art

[0002] Lithium-ion batteries have been successfully applied in portable electronic devices, new energy vehicles, energy storage and other fields. With the development of society, the market demand for high energy density and power density lithium-ion batteries is getting higher and higher, while the capacity of graphite is close to the theoretical capacity (372mAh / g). Its theoretical capacity is low and it is difficult to meet the market demand for high energy density lithium-ion batteries. Silicon has received extensive attention due to its high theoretical specific capacity (4200mAh / g), relatively low lithium insertion platform (0.4V), wide resources and environmental friendliness.

[0003] Silicon negative electrode materials have a high theoretical capacity (4200mAh / g) and are abundant in resources. They are ideal negative electrode materials and are currently receiving widespread attention and research in the industry. However, compared with graphite negative electrode materials, silicon negative electrode materials have obvious disadvantages, and the volume expansion during the cycle process is extremely high. During the cycle process, severe volume expansion will cause the SEI film on the surface of silicon particles to rupture, consume lithium ions, and regenerate new SEI films, which will eventually cause the SEI film on the surface of silicon particles to become thicker and thicker, blocking the deintercalation of lithium ions, so the electrochemical performance of the material is seriously attenuated.

[0004] Although the industry also uses carbon coating to make silicon-carbon composite materials to improve the structural stability and electrical conductivity of the material, the resulting silicon-carbon negative electrode material usually has an irregular morphology. Due to the uneven stress distribution when the irregular silicon-carbon negative electrode material expands when embedded with lithium, it is easy to break, resulting in capacity attenuation, which affects its promotion and application in the market. Summary of the invention

[0005] In view of the above problems, the purpose of the present invention is to provide a silicon-carbon negative electrode material and a preparation method. The silicon-carbon negative electrode material is spherical, which can not only effectively inhibit the expansion of silicon, but also has uniform stress distribution when silicon expands, is not easy to break, and has better electrochemical performance such as cycle.

[0006] To achieve the above-mentioned object, the first aspect of the present invention provides a silicon-carbon negative electrode material. The silicon-carbon negative electrode material comprises a core and a shell layer, wherein the core comprises a porous silicon-carbon matrix, the shell layer comprises a carbon-coated outer layer, the porous silicon-carbon matrix comprises nano-silicon, a silicate layer, a carbon-coated inner layer and a carbon filler from the inside to the outside, the carbon filler has a pore structure, and the circularity of the silicon-carbon negative electrode material is ≥0.9.

[0007] The silicon-carbon negative electrode material of the present invention has at least the following technical effects.

[0008] (1) The circularity of the silicon-carbon negative electrode material is ≥0.9. It has a spherical structure, which can evenly distribute stress when silicon expands. The material is difficult to break, has high mechanical strength, and has better electrochemical performance such as cycling.

[0009] (2) The triple coating layers of carbon coating outer layer, carbon coating inner layer and carbon filling body can improve the stability of silicon-carbon negative electrode materials. Even if the material is broken, it can prevent side reactions from occurring, thereby improving cycle stability and avoiding cycle diving and other phenomena.

[0010] (3) The silicate layer encapsulating nano-silicon can buffer the volume expansion of silicon and form a protective layer on the surface of nano-silicon, further preventing the nano-silicon from directly contacting the electrolyte and causing side reactions, while also improving the initial coulombic efficiency of the material.

[0011] (4) The pore structure in the silicon-carbon negative electrode material can buffer the volume expansion, reduce the expansion rate, and reduce the growth of SEI, thereby improving the cycle stability of the material.

[0012] In some embodiments, the total pore volume of the silicon-carbon negative electrode material is 0.025 cm 3 / g to 0.200cm 3 / g.

[0013] In some embodiments, the repose angle of the silicon-carbon negative electrode material is <30°.

[0014] In some embodiments, the relative true density of the silicon-carbon negative electrode material is K, 0.70≤K≤0.95.

[0015] In some embodiments, the compaction density corresponding to the rebound rate inflection point of the silicon-carbon negative electrode material is ≥1.60 g / cm 3 .

[0016] In some embodiments, the average pore size of nitrogen adsorption of the silicon-carbon negative electrode material is d, d≤Dv50.

[0017] In some embodiments, the specific surface area of ​​the silicon-carbon negative electrode material is 0.5 m 2 / g to 5.0m 2 / g.

[0018] In some embodiments, the silicon grain size of the silicon-carbon negative electrode material is 1 nm to 15 nm.

[0019] In some embodiments, the tap density of the silicon-carbon negative electrode material is ≥ 0.95 g / cm 3 .

[0020] In some embodiments, the true density of the silicon-carbon negative electrode material is 1.50 g / cm 3 Up to 2.00g / cm3 .

[0021] In some embodiments, the carbon content of the silicon-carbon negative electrode material is 25 wt.% to 50 wt.%.

[0022] In some embodiments, the silicon content of the silicon-carbon negative electrode material is 48 wt.% to 67 wt.%.

[0023] In some embodiments, the oxygen content of the silicon-carbon negative electrode material is 1 wt.% to 10 wt.%.

[0024] In some embodiments, the metal content of the silicon-carbon negative electrode material is 0.1 wt.% to 2.0 wt.%.

[0025] In some embodiments, the first reversible specific capacity of the silicon-carbon negative electrode material is ≥1800 mAh / g.

[0026] In some embodiments, the first coulombic efficiency of the silicon-carbon negative electrode material is ≥88%.

[0027] In some embodiments, the expansion rate of the silicon-carbon negative electrode material after 100 cycles is ≤40%.

[0028] In some embodiments, the capacity retention rate of the silicon-carbon negative electrode material after 100 cycles is ≥95%.

[0029] In some embodiments, the particle size of the silicon-carbon negative electrode material satisfies 1 μm≤Dv50≤10 μm, Dv100≤30 μm, (Dv90-Dv10) / Dv50≤2.0, and Dv60 / Dv10≤3.

[0030] In some embodiments, the porosity difference of the silicon-carbon negative electrode material on the same cross section is σ1, σ1≤5%, and the porosity difference of the silicon-carbon negative electrode material on different cross sections is σ2, σ2≤10%.

[0031] In some embodiments, the silicate layer comprises M x SiO y layer, wherein M is selected from at least one of Ni, Co, Mn, Fe, Ca and Zn, 0<x<0.1, 1≤y≤2.

[0032] In some embodiments, the carbon filler accounts for 20 wt.% to 45 wt.% of the silicon-carbon negative electrode material.

[0033] In some embodiments, the carbon coating outer layer accounts for 3 wt.% to 10 wt.% of the silicon-carbon negative electrode material.

[0034] In some embodiments, the pore structure includes micropores, mesopores, and macropores.

[0035] In some embodiments, the pore volume of micropores with a pore size of 0.4 nm to 2.0 nm is ≤ 0.001 cm 3 / g, the mesopore volume of the pore size is 2nm to 50nm ≤0.01cm 3 / g, the pore volume of macropores with pore diameters ranging from 50nm to 500nm is 0.025cm 3 / g to 0.200cm 3 / g.

[0036] In some embodiments, the micropore volume with a pore size of 0.4nm to 2.0nm accounts for 0% to 1% of the total pore volume, the mesopore volume with a pore size of 2nm to 50nm accounts for 0% to 10% of the total pore volume, and the macropore volume with a pore size of 50nm to 500nm accounts for 90% to 99% of the total pore volume.

[0037] In some embodiments, the pore volume of macropores with pore diameters of 50 nm to 150 nm accounts for more than 50% of the total pore volume.

[0038] A second aspect of the present invention provides a method for preparing a silicon-carbon negative electrode material, comprising the following steps.

[0039] (I) grinding silicon powder, a carbon source, a dispersant and an organic solvent to prepare a nano-silicon slurry;

[0040] (II) adding a spheroidizing additive to the nano-silicon slurry and dispersing the mixture to obtain a mixed slurry, and spray-drying the mixed slurry to obtain a spherical precursor, wherein the spheroidizing additive is an inorganic ionic compound soluble in the organic solvent, and the boiling point of the spheroidizing additive is greater than 500° C. and the solubility in the organic solvent is greater than 20 g / L, and the mass ratio of the silicon powder to the spheroidizing additive is 1:0.1 to 1.0;

[0041] (III) heat treating the spherical precursor at 500° C. to 700° C. and then coating the spherical precursor with a carbon filler to obtain an intermediate;

[0042] (IV) After removing the spheroidizing additive in the intermediate, the intermediate is coated with a carbon outer layer.

[0043] In the preparation method of the silicon-carbon negative electrode material of the present invention, silicon powder, carbon source, dispersant and organic solvent are sand-milled to obtain nano-silicon with an oxide layer on the surface, and the nano-silicon, carbon source and dispersant are uniformly dispersed in the organic solvent. Under the action of the dispersant, the spheroidizing additive is added and uniformly dispersed in the mixed slurry. A certain amount of specific spheroidizing additive can change the state of the nano-silicon slurry, so that the nano-silicon silica particles are micro-agglomerated to avoid the formation of a dense shell layer on the surface during subsequent spray drying, resulting in loose and easy collapse inside, so a spherical precursor can be obtained. The dispersant can be removed by heat treatment and the carbon source can be carbonized to form a carbon coating inner layer coated on the surface of the nano-silicon. At the same time, due to the easy water absorption of the spheroidizing additive, part of the spheroidizing additive forms a hydrated compound, which is decomposed by heat treatment to form oxides and hydrogen chloride. The oxide reacts with SiO2 in the oxide layer on the surface of the nano-silicon at high temperature. y Combined to form MxSiO y When coating the carbon filler, the spheroidizing additive is distributed in the carbon filler, and then after removal, a pore structure is formed at the corresponding position of the carbon filler. Since the spheroidizing additive is evenly distributed during the spray drying process, the formed pore structure is also evenly distributed. Finally, coating the carbon outer layer can reduce the specific surface area of ​​the material, increase the electronic conductivity, hinder side reactions, and inhibit the volume expansion of silicon.

[0044] In some embodiments, the Dv50 of the silicon powder satisfies 1 μm≤Dv50≤10 μm.

[0045] In some embodiments, the silicon content of the silicon powder is ≥ 95 wt.%.

[0046] In some embodiments, the carbon source includes at least one of phenolic resin, citric acid, asphalt, sucrose, glucose, fructose, lignin, tannic acid, and dopamine.

[0047] In some embodiments, the dispersant includes at least one of n-dodecylamine, triethanolamine, isoamyl alcohol, oleic acid, and cycloalkylsulfonic acid.

[0048] In some embodiments, the organic solvent includes at least one of methanol, ethanol, propanol, isopropanol, acetone, toluene, and xylene.

[0049] In some embodiments, the mass ratio of silicon powder, carbon source, dispersant and solvent is 1:0.02-0.15:0.05-0.10:2-10.

[0050] In some embodiments, the sanding speed is 500 rpm to 1500 rpm.

[0051] In some embodiments, the nano-silicon slurry contains nano-silicon, the particle size of the nano-silicon satisfies 50nm≤Dv50≤150nm, Dv100≤400nm, and the oxygen content in the nano-silicon is ≤15wt.%.

[0052] In some embodiments, the spheroidizing additive includes at least one of NiCl2, CoCl2, MnCl2, FeCl2, CaCl2, and ZnCl2.

[0053] In some embodiments, the viscosity of the mixed slurry is 1 mPas to 500 mPas.

[0054] In some embodiments, the mixed slurry has a solid content of 20% to 50%.

[0055] In some embodiments, the linear velocity of the atomizer used in the spray drying is 150 m / s to 250 m / s.

[0056] In some embodiments, the inlet air temperature of the spray drying is 110°C to 200°C.

[0057] In some embodiments, the outlet air temperature of the spray drying is 70°C to 120°C.

[0058] In some embodiments, the spray drying has a spray yield of ≥ 90%.

[0059] In some embodiments, the heat treatment is performed under an inert atmosphere comprising at least one of helium, neon, argon, krypton, and xenon.

[0060] In some embodiments, the heating rate of the heat treatment is 1° C. / min to 5° C. / min.

[0061] In some embodiments, the carbon filler may be filled multiple times, and the treatment temperature during filling is 500° C. to 1000° C.

[0062] In some embodiments, the carbon sources of the carbon filler and the carbon outer layer are each independently a liquid carbon source, a solid carbon source, and a gaseous carbon source.

[0063] In some embodiments, vacuum roasting, water washing or alcohol washing is used to remove the spheroidizing additive.

[0064] In some embodiments, the vacuum calcination is performed in a vacuum furnace, the temperature of the vacuum calcination is 500° C. to 900° C., the vacuum degree in the vacuum furnace is ≤100 Pa, and the time of the vacuum calcination is 2 h to 24 h.

[0065] In some embodiments, the water washing or alcohol washing may be performed multiple times until the Cl element content in the silicon-carbon negative electrode material is less than 0.01 wt.%.

[0066] In some embodiments, the solvent used in the alcohol washing is methanol, ethanol, propanol or isopropanol.

[0067] In some embodiments, the sanding includes coarse grinding and fine grinding.

[0068] In some embodiments, the coarse grinding uses coarse grinding balls, the diameter of the coarse grinding balls is 0.1 mm to 1.0 mm, and the coarse grinding time is 1 h to 8 h.

[0069] In some embodiments, the fine grinding uses fine grinding balls, the diameter of the fine grinding balls is 0.03 mm to 0.20 mm, and the sanding time of the fine grinding is 2 h to 24 h. BRIEF DESCRIPTION OF THE DRAWINGS

[0070] Figure 1 It is a schematic structural diagram of the silicon-carbon negative electrode material of the present invention.

[0071] Figure 2 This is the SEM image of the silicon-carbon negative electrode material of Example 1.

[0072] Figure 3 This is a CP cross-sectional morphology image of the silicon-carbon negative electrode material of Example 1.

[0073] Figure 4 This is the SEM image of the silicon-carbon negative electrode material of Comparative Example 1.

[0074] Figure 5 This is the CP cross-sectional morphology of the silicon-carbon negative electrode material of Comparative Example 1. DETAILED DESCRIPTION

[0075] The silicon-carbon negative electrode material of the present invention can be used alone or mixed with other negative electrode active materials (such as natural graphite, artificial graphite, soft carbon and / or hard carbon, etc.). The silicon-carbon negative electrode material can be applied to secondary batteries, which include positive electrode materials and negative electrode materials. The positive electrode material includes at least one of a lithium cobalt oxide positive electrode material, a lithium iron phosphate positive electrode material, a nickel cobalt manganese oxide positive electrode material, and a nickel cobalt aluminum oxide positive electrode material.

[0076] The structure of the silicon-carbon negative electrode material of the present invention can be Figure 1 An example is given below. Figure 1 As shown, the silicon-carbon negative electrode material 100 includes a core 10 and a shell 30. The core 10 includes a porous silicon-carbon matrix, and the shell 30 includes a carbon-coated outer layer. The porous silicon-carbon matrix includes nano-silicon 11, a silicate layer 13, a carbon-coated inner layer 15 and a carbon filler 17 from the inside to the outside, and the carbon filler 17 has a pore structure 50.

[0077] The first reversible specific capacity of the silicon-carbon negative electrode material of the present invention is ≥1800mAh / g. As a technical solution, the capacity of the silicon-carbon negative electrode material is 2000mAh / g to 2500mAh / g. As an example, the capacity of the silicon-carbon negative electrode material may be, but is not limited to, ≥1800mAh / g, ≥1900mAh / g, ≥2000mAh / g, ≥2100mAh / g, ≥2200mAh / g, ≥2300mAh / g, ≥2400mAh / g. The first coulombic efficiency of the silicon-carbon negative electrode material is ≥88%. As a technical solution, the first coulombic efficiency of the silicon-carbon negative electrode material is ≥90%. As an example, the first coulombic efficiency of the silicon-carbon negative electrode material may be, but is not limited to, ≥88%, ≥89%, ≥90%, ≥91%, ≥92%, ≥93%. The expansion rate of the silicon-carbon negative electrode material after 100 cycles is ≤40%. As an example, it can be, but not limited to, ≤40%, ≤38%, ≤36%, ≤34%, ≤32%, ≤30%, ≤28%, ≤25%. The capacity retention rate of the silicon-carbon negative electrode material after 100 cycles is ≥95%. As an example, it can be, but not limited to, ≥95%, ≥96%, ≥97%, ≥98%.

[0078] The circularity of the silicon-carbon negative electrode material is ≥0.9. As an example, the circularity can be, but not limited to, 0.90, 0.91, 0.92, 0.93, 0.94, 0.95, 0.96, 0.97, 0.98. The repose angle of the silicon-carbon negative electrode material is <30°. As an example, the repose angle can be, but not limited to, 29°, 28°, 27°, 26°, 25°, 24°, 23°, 22, 21°. The compaction density corresponding to the inflection point of the rebound rate of the silicon-carbon negative electrode material is ≥1.60g / cm 3 , can be but not limited to 1.60g / cm 3 , 1.61g / cm 3 , 1.62g / cm 3 、1.63g / cm 3 , 1.64g / cm 3 , 1.65g / cm 3 、1.66g / cm 3 , 1.67g / cm 3 、1.68g / cm 3 , 1.69g / cm 3 , 1.70g / cm 3 The rebound rate inflection point is the critical point of particle crushing. Its compaction density is high, indicating that the material structure is stable and not prone to rupture. The average pore size of nitrogen adsorption of silicon-carbon negative electrode material is d, d≤Dv50, Dv50 is the particle size of nano-silicon, and d can be calculated based on BET (4V / A). The specific surface area of ​​silicon-carbon negative electrode material is 0.5m 2 / g to 5.0m 2 / g, as an example, it can be but not limited to 0.5m 2 / g, 1.0m 2 / g, 1.5m 2 / g, 2.0m 2 / g, 2.5m 2 / g, 3.0m 2 / g, 3.5m 2 / g, 4.0m 2 / g, 4.5m 2 / g, 5.0m 2 / g. The silicon grain size of the silicon-carbon negative electrode material is 1nm to 15nm. As a technical solution, the silicon grain size may be 1nm to 10nm, or 1nm to 6nm. As an example, the silicon grain size may be, but is not limited to, 1nm, 2nm, 3nm, 4nm, 5nm, 6nm, 7nm, 8nm, 9nm, 10nm, 11nm, 12nm, 13nm, 14nm, 15nm. The particle size of the silicon-carbon negative electrode material satisfies 1μm≤Dv50≤10μm, Dv100≤30μm, (Dv90-Dv10) / Dv50≤2.0, Dv60 / Dv10≤3. The tap density of the silicon-carbon negative electrode material is ≥0.95g / cm 3 As a technical solution, the tap density is ≥1.00g / cm 3 As an example, the tap density of the silicon-carbon negative electrode material may be, but is not limited to, 0.95 g / cm 3 , 1.00g / cm 3 , 1.05g / cm 3 , 1.10g / cm 3 , 1.15g / cm 3 , 1.20g / cm 3 The true density of silicon-carbon negative electrode material is 1.50g / cm 3 Up to 2.00g / cm 3 As an example, the true density of the silicon-carbon negative electrode material may be, but is not limited to, 1.50 g / cm 3 , 1.55g / cm 3 , 1.60g / cm 3 , 1.65g / cm 3 , 1.70g / cm 3 , 1.75g / cm 3 , 1.80g / cm 3 , 1.85g / cm 3 , 1.90g / cm 3 , 1.95g / cm 3 , 2.00g / cm 3The relative true density of the silicon-carbon negative electrode material is K, 0.70≤K≤0.95. As an example, K may be, but is not limited to, 0.70, 0.75, 0.80, 0.85, 0.90, 0.95, where the calculation formula of K is as follows.

[0079] K = true density / (1.82*carbon content + 2.30*(1-carbon content))

[0080] The carbon content of the silicon-carbon negative electrode material is 25wt.% to 50wt.%, and as an example, it can be, but not limited to, 25wt.%, 27wt.%, 30wt.%, 33wt.%, 35wt.%, 37wt.%, 40wt.%, 43wt.%, 45wt.%, 47wt.%, 50wt.%. The silicon content of the silicon-carbon negative electrode material is 48wt.% to 67wt.%, and as an example, it can be, but not limited to, 48wt.%, 50wt.%, 52wt.%, 54wt.%, 56wt.%, 58wt.%, 60wt.%, 63wt.%, 65wt.%, 67wt.%. The oxygen content of the silicon-carbon negative electrode material is 1wt.% to 10wt.%, as an example, it can be but not limited to 1wt.%, 2wt.%, 3wt.%, 4wt.%, 5wt.%, 6wt.%, 7wt.%, 8wt.%, 9wt.%, 10wt.%. The metal content of the silicon-carbon negative electrode material is 0.1wt.% to 2.0wt.%, as an example, it can be but not limited to 0.1wt.%, 0.3wt.%, 0.5wt.%, 0.7wt.%, 0.9wt.%, 1.0wt.%, 1.3wt.%, 1.5wt.%, 1.7wt.%, 1.9wt.%, 2.0wt.%.

[0081] The total pore volume of the silicon-carbon anode material is 0.025 cm 3 / g to 0.200cm 3 / g, as an example, the total pore volume can be, but is not limited to, 0.025cm 3 / g, 0.050cm 3 / g, 0.075cm 3 / g, 0.100cm 3 / g, 0.125cm 3 / g, 0.150cm 3 / g, 0.175cm 3 / g, 0.200cm 3 / g. The pore structure includes micropores, mesopores and macropores. The pore volume of micropores with a pore size of 0.4nm to 2.0nm is ≤0.001cm 3 / g, the mesopore volume of the pore size is 2nm to 50nm ≤0.01cm 3 / g, the pore volume of macropores with pore diameters ranging from 50nm to 500nm is 0.025cm 3 / g to 0.200cm 3 / g. The pore volume of micropores with a pore size of 0.4nm to 2.0nm accounts for 0% to 1% of the total pore volume, the pore volume of mesopores with a pore size of 2nm to 50nm accounts for 0% to 10% of the total pore volume, and the pore volume of macropores with a pore size of 50nm to 500nm accounts for 90% to 99% of the total pore volume. The pore volume of macropores with a pore size of 50nm to 150nm accounts for more than 50% of the total pore volume, so the pore structure in the silicon-carbon negative electrode material of the present invention is mainly macropores, which can effectively alleviate the expansion of silicon. The porosity difference of the silicon-carbon negative electrode material on the same section is σ1, σ1≤5%, and the porosity difference of the silicon-carbon negative electrode material on different sections is σ2, σ2≤10%. As an example, σ1 can be but not less than 5%, 4%, 3%, 2%, 1%. σ2 can be but not less than 10%, 9%, 8%, 7%, 6%, 5%, 4%, 3%. Small values ​​of σ1 and σ2 indicate uniform pore distribution, which helps to relieve the stress of silicon expansion and avoid particle rupture caused by uneven stress. The calculation of σ1 and σ2 can be as follows: select any two 2.0μm*2.0μm areas on the same cross section of silicon-carbon negative electrode material, and their porosity is P1 and P2, σ1 = (P1-P2) / P2; select any two 2μm*2μm areas on the cross section of different silicon-carbon negative electrode materials, and their porosity is P3 and P4, σ2 = (P3-P4) / P4.

[0082] In addition, the silicate layer of the silicon-carbon negative electrode material contains M x SiO y layer, wherein M is selected from at least one of Ni, Co, Mn, Fe, Ca and Zn, 0<x<0.1, 1≤y≤2, which comes from the metal in the spheroidizing additive and the SiO in the surface oxide layer of the nano-silicon y The carbon filler accounts for 20wt.% to 45wt.% of the silicon-carbon negative electrode material, and as an example, it can be, but not limited to, 20wt.%, 25wt.%, 30wt.%, 35wt.%, 40wt.%, 45wt.%. The carbon coating outer layer accounts for 3wt.% to 10wt.% of the silicon-carbon negative electrode material, and as an example, it can be, but not limited to, 3wt.%, 4wt.%, 5wt.%, 6wt.%, 7wt.%, 8wt.%, 9wt.%, 10wt.%.

[0083] The method for preparing the silicon-carbon negative electrode material of the present invention may include the following steps.

[0084] (I) Silicon powder, a carbon source, a dispersant and an organic solvent are sand-ground to prepare nano-silicon slurry.

[0085] (II) adding a spheroidizing additive to the nano-silicon slurry and dispersing the mixture to obtain a mixed slurry, and spray drying the mixed slurry to obtain a spherical precursor.

[0086] (III) The spherical precursor is heat treated and then coated with a carbon filler to obtain an intermediate.

[0087] (IV) After removing the spheroidizing additive in the intermediate, the carbon outer layer is coated.

[0088] Wherein, the Dv50 of silicon powder in step (I) satisfies 1μm≤Dv50≤10μm, as an example, the Dv50 of silicon powder can be but not limited to 1μm, 2μm, 3μm, 4μm, 5μm, 6μm, 7μm, 8μm, 9μm, 10μm. The silicon content of silicon powder is ≥95wt.%, as an example, the silicon content of silicon powder can be but not limited to 95wt.%, 96wt.%, 97wt.%, 98wt.%, 99wt.%. The carbon source includes at least one of phenolic resin, citric acid, asphalt, sucrose, glucose, fructose, lignin, tannic acid and dopamine. The dispersant includes at least one of n-dodecylamine, triethanolamine, isoamyl alcohol, oleic acid and cycloalkylsulfonic acid. The organic solvent includes at least one of methanol, ethanol, propanol, isopropanol, acetone, toluene and xylene. The mass ratio of silicon powder, carbon source, dispersant and solvent is 1:0.02-0.15:0.05-0.10:2-10. As an example, the mass ratio of the four can be, but is not limited to, 1:0.02:0.05:2, 1:0.02:0.08:2, 1:0.02:0.10:2, 1:0.02:0.05:5, 1:0.02:0.08:8, 1:0.02:0.10:10, 1:0.08:0.05:2, 1:0.08:0.08:2, 1:0.08:0.10:2, 1:0.08:0.05: 5. 1:0.08:0.08:8, 1:0.08:0.10:10, 1:0.10:0.05:2, 1:0.10:0.08:2, 1:0.10:0.10:2, 1:0.10:0.05:5, 1:0.10:0.08:8, 1:0.10:0.10:10, 1:0.15:0.05:2, 1:0.15:0.08:2, 1:0.15:0.10:2, 1:0.15:0.05:5, 1:0.15:0.08:8, 1:0.15:0.10:10.

[0089] The speed of sanding is 500rpm to 1500rpm, and as an example, it can be but not limited to 500rpm, 600rpm, 700rpm, 800rpm, 900rpm, 1000rpm, 1100rpm, 1200rpm, 1300rpm, 1400rpm, 1500rpm. Sanding includes coarse grinding and fine grinding, and coarse grinding and fine grinding can be carried out simultaneously. Coarse grinding uses coarse grinding balls, and the diameter of the coarse grinding balls is 0.1mm to 1.0mm, and as an example, it can be but not limited to 0.1mm, 0.2mm, 0.3mm, 0.4mm, 0.5mm, 0.6mm, 0.7mm, 0.8mm, 0.9mm, 1.0mm. The sanding time of coarse grinding is 1h to 8h, and as an example, it can be but not limited to 1h, 2h, 3h, 4h, 5h, 6h, 7h, 8h. Fine grinding uses fine grinding balls, and the diameter of the fine grinding balls is 0.03mm to 0.20mm. As an example, it can be but not limited to 0.03mm, 0.05mm, 0.10mm, 0.15mm, 0.20mm. The sanding time of fine grinding is 2h to 24h. As an example, it can be but not limited to 2h, 4h, 6h, 8h, 10h, 12h, 14h, 16h, 18h, 20h, 22h, 24h.

[0090] The nano-silicon slurry contains nano-silicon, and the particle size of the nano-silicon satisfies 50nm≤Dv50≤150nm, Dv100≤400nm, and the oxygen content in the nano-silicon is ≤15wt.%. As an example, Dv50 can be, but is not limited to, 50nm, 60nm, 70nm, 80nm, 90nm, 100nm, 110nm, 120nm, 130nm, 140nm, 150nm. Dv100 can be, but is not limited to, 100nm, 120nm, 140nm, 160nm, 180nm, 200nm, 220nm, 240nm, 260nm, 280nm, 300nm, 320nm, 340nm, 360nm, 380nm, 400nm. The oxygen content in the nano silicon can be, but is not limited to, 1wt.%, 2wt.%, 3wt.%, 4wt.%, 5wt.%, 6wt.%, 7wt.%, 8wt.%, 9wt.%, 10wt.%, 11wt.%, 12wt.%, 13wt.%, 14wt.%, 15wt.%. In step (II), the spheroidizing additive is an inorganic ionic compound soluble in an organic solvent. The boiling point of the spheroidizing additive is greater than 700° C., and the solubility of the spheroidizing additive in the organic solvent is greater than 20g / L, i.e., the solubility of such additive in the organic solvent is better and can be removed by washing. The spheroidizing additive includes at least one of NiCl2 (boiling point of 987°C), CoCl2 (boiling point of 1049°C), MnCl2 (boiling point of 1190°C), FeCl2 (boiling point of 1023°C), CaCl2 (boiling point of 1600°C) and ZnCl2 (boiling point of 732°C). Nano silicon slurry is a uniformly dispersed colloidal solution. The colloid has both attractive and repulsive forces. Such additives are strong electrolytes soluble in alcohol. The addition of electrolytes will reduce the charge of the colloid particles, reduce the repulsive force of the colloid particles, and make the particles micro-agglomerate, and form a dense spherical precursor through spray drying. Therefore, such spheroidizing additives can not only adjust the state of nano silicon slurry and micro-agglomerate nano silica gel particles, but also have a boiling point higher than 500°C, do not react when heated at low temperature, and can be removed by high temperature, water washing or alcohol washing. The mass ratio of silicon powder to spheroidizing additive is 1:0.1-1.0. As an example, the mass ratio can be but not limited to 1:0.1, 1:0.2, 1:0.3, 1:0.4, 1:0.5, 1:0.6, 1:0.7, 1:0.8, 1:0.9, 0.1:1.0. The amount of spheroidizing additive cannot be too low, otherwise the ionic strength is insufficient, and the morphology of the slurry after spraying can only be slightly improved, and a completely spherical morphology cannot be obtained.

[0091] The viscosity of the mixed slurry is 1mPas to 500mPas. As an example, the viscosity can be but not limited to 1mPas, 50mPas, 100mPas, 150mPas, 200mPas, 250mPas, 300mPas, 350mPas, 400mPas, 450mPas, 500mPas. The viscosity should not be too large, otherwise it will affect the self-assembly of the material, easily form a hollow or internal concave structure, and easily cause the spray pipe to be blocked, and spray drying cannot be performed normally. The solid content of the mixed slurry is 20% to 50%. As an example, the solid content can be but not limited to 20%, 25%, 30%, 35%, 40%, 45%, 50%. The solid content should not be too high, otherwise the viscosity is too high and the pipeline is easily blocked, and it is impossible to spray normally. If the solid content is too small, it is easy to form a shell layer on the surface of the particles during spray drying, resulting in internal looseness. The linear speed of the atomizer used in spray drying is 150m / s to 250m / s. As an example, the linear speed can be, but not limited to, 150m / s, 160m / s, 170m / s, 180m / s, 190m / s, 200m / s, 210m / s, 220m / s, 230m / s, 240m / s, 250m / s. The inlet air temperature of spray drying is 110°C to 200°C. As an example, the inlet air temperature can be, but not limited to, 110°C, 120°C, 130°C, 140°C, 150°C, 160°C, 170°C, 180°C, 190°C, 200°C. The outlet air temperature of spray drying is 70°C to 120°C. As an example, the outlet air temperature can be, but not limited to, 70°C, 80°C, 90°C, 100°C, 110°C, 120°C. The spray yield of spray drying is ≥90%. As an example, the spray yield can be, but is not limited to, 90%, 91%, 92%, 93%, 94%, or 95%.

[0092] The heat treatment temperature of step (III) is 500°C to 700°C. As an example, the heat treatment temperature may be, but is not limited to, 500°C, 520°C, 540°C, 560°C, 580°C, 600°C, 620°C, 640°C, 660°C, 680°C, and 700°C. The heating rate of the heat treatment is 1°C / min to 5°C / min. As an example, the heating rate may be, but is not limited to, 1°C / min, 2°C / min, 3°C / min, 4°C / min, and 5°C / min. The heat treatment is carried out under an inert atmosphere, and the inert atmosphere includes at least one of helium, neon, argon, krypton, and xenon. The spheroidizing additive of the inorganic ionic compound is easy to absorb water, and is partially converted into oxides during the heat treatment process. The oxides combine with the silicon oxide on the surface of the nano-silicon to form M x SiO y The carbon source and the carbonizable dispersant form a carbon coating inner layer during the heat treatment process. Since the carbon source content is low, the formed carbon coating inner layer is thinner.

[0093] The carbon source of the carbon filler is a liquid carbon source, a solid carbon source and a gaseous carbon source. In other words, the carbon filler can be formed by liquid coating, solid coating and gas coating, and the liquid coating, solid coating and gas coating can be carried out in a conventional manner. The liquid coating and solid coating can be carried out in a vacuum furnace to increase the density of the material. The liquid carbon source includes resins and / or polyvinyl pyrrolidone. The solid carbon source includes at least one of asphalt, sucrose, glucose, polyaniline, polyvinyl alcohol and polypyrrole. The gaseous carbon source includes at least one of methane, ethane, acetylene, propane and ethylene. The carbon filler can be filled multiple times, and the treatment temperature during filling is 500°C to 1000°C. As an example, the treatment temperature can be, but is not limited to, 500°C, 550°C, 600°C, 650°C, 700°C, 750°C, 800°C, 850°C, 900°C, 950°C, 1000°C. The formed carbon filler accounts for 20wt.% to 45wt.% of the silicon-carbon negative electrode material. As an example, it can be but not limited to 20wt.%, 25wt.%, 30wt.%, 35wt.%, 40wt.%, 45wt.%. The content of the carbon filler is relatively high, so when coating the carbon filler, the spheroidizing additive can be dispersed in the carbon source of the carbon filler. The carbon filler formed by liquid phase coating, solid phase coating and gas phase coating usually has a certain pore structure, so during subsequent water washing or alcohol washing, the solution can enter the material through the pore structure and dissolve and remove the spheroidizing additive.

[0094] Step (IV) Removal of spheroidizing additives Vacuum roasting, water washing or alcohol washing can be used to remove spheroidizing additives. Vacuum roasting is carried out in a vacuum furnace, and the temperature of vacuum roasting is 500°C to 900°C. As an example, it can be but not limited to 500°C, 600°C, 700°C, 800°C, 900°C. The vacuum degree in the vacuum furnace is ≤100Pa, and the time of vacuum roasting is 2h to 24h. As an example, the roasting time can be but not limited to 2h, 4h, 6h, 8h, 10h, 12h, 14h, 16h, 18h, 20h, 22h, 24h. Water washing or alcohol washing can be washed multiple times until the Cl element content in the silicon-carbon negative electrode material is less than 0.01wt.%. The solvent used for alcohol washing is methanol, ethanol, propanol or isopropanol.

[0095] The carbon source of the carbon outer layer is a liquid carbon source, a solid carbon source and a gaseous carbon source. In other words, the carbon outer layer can be formed by liquid coating, solid coating and gas coating, and the liquid coating, solid coating and gas coating can be carried out in a conventional manner. The liquid carbon source includes resins and / or polyvinyl pyrrolidone. The solid carbon source includes at least one of asphalt, sucrose, glucose, polyaniline, polyvinyl alcohol and polypyrrole. The gaseous carbon source includes at least one of methane, ethane, acetylene, propane and ethylene. The formed carbon outer layer accounts for 3wt.% to 10wt.% of the silicon-carbon negative electrode material. As an example, it can be but not limited to 3wt.%, 4wt.%, 5wt.%, 6wt.%, 7wt.%, 8wt.%, 9wt.%, 10wt.%.

[0096] In order to better illustrate the purpose, technical scheme and beneficial effects of the present invention, the present invention will be further described below in conjunction with specific embodiments. It should be noted that the following implementation method is a further explanation of the present invention and should not be used as a limitation of the present invention. The embodiments of the present invention include a description of the technical scheme of the silicon-carbon negative electrode material and a description of the technical scheme of the preparation method of the silicon-carbon negative electrode material.

[0097] Example 1

[0098] This embodiment is a method for preparing a silicon-carbon negative electrode material, which includes the following steps.

[0099] (I) 10 kg of silicon powder (Dv50 is 5.5 μm, silicon content is 97 wt.%), 1 kg of asphalt, 0.7 kg of triethanolamine and 40 kg of ethanol were sand-milled together, firstly coarsely ground with a zirconia ball of 0.4 mm in diameter for 4 h, the speed of the sand mill was 1000 rpm, and then finely ground with a zirconia ball of 0.1 mm in diameter for 10 h, the speed of the sand mill was 1500 rpm, to obtain nano silicon slurry. The Dv10 of nano silicon in the nano silicon slurry was measured by Malvern particle size analyzer, and it was found that the Dv50 was 127 nm, the Dv90 was 196 nm, the Dv100 was 247 nm, (Dv90-Dv10) / Dv50 was 1.09, and the oxygen content in the nano silicon was 9 wt.%.

[0100] (II) Add 2kg of anhydrous zinc chloride (boiling point 732°C, solubility in ethanol>20g / L) to the nano-silicon slurry and disperse at 1000rpm for 1h to obtain a mixed slurry, the viscosity of the mixed slurry is 24.5mPas, and the solid content is 24%. The mixed slurry is spray-dried, the inlet air temperature is 160°C, the outlet air temperature is 80°C, the linear speed of the atomizer is 180m / s, the feed amount is 10kg / h, the spray yield is 91%, and a spherical precursor is obtained after cooling.

[0101] (III) The spherical precursor was placed in a rotary kiln, and the temperature was first raised to 150°C at a heating rate of 5°C / min for 2 h, and then raised to 550°C for 4 h. The reactants were mixed with asphalt in a ratio of 2:1 (the carbon coating increment was about 26 wt%), and then placed in an atmosphere furnace, with nitrogen protection, and the temperature was raised to 650°C at a heating rate of 1°C / min for 5 h to obtain an intermediate.

[0102] (IV) Washing with water at a mass ratio of 1:5 between the intermediate and water at a temperature of 50°C in a vacuum device at a vacuum degree of 100 Pa, stirring for 10 hours, and then filtering by pressure, and then rinsing with deionized water 100 times the mass of the material until the Cl element content in the material is less than 0.01wt.%, and drying with air at 60°C. Then loading into a rotary kiln, heating to 800°C at a heating rate of 5°C / min, and coating with acetylene gas, the carbon coating amount accounting for 4wt.% of the silicon-carbon negative electrode material.

[0103] The silicon-carbon negative electrode material prepared in Example 1 was subjected to SEM examination, and the results are as follows: Figure 2 As shown. Figure 2 It can be seen that the morphology of the prepared silicon-carbon negative electrode material is spherical and has a high degree of circularity. The silicon-carbon negative electrode material prepared in Example 1 was subjected to CP section testing, and the results are as follows: Figure 3 As shown. Figure 3 It can be seen that the pore size distribution of the prepared silicon-carbon negative electrode material is uniform.

[0104] Example 2

[0105] This embodiment is a method for preparing a silicon-carbon negative electrode material, which includes the following steps.

[0106] (I) Same as step (I) of Example 1.

[0107] (II) Add 2 kg of anhydrous ferrous chloride (boiling point 1023°C, solubility in ethanol> 20 g / L) to the nano-silicon slurry and disperse at 1000 rpm for 1 hour to obtain a mixed slurry with a viscosity of 24.5 mPas and a solid content of 24%. The mixed slurry was spray dried with an inlet air temperature of 160°C, an outlet air temperature of 80°C, an atomizer linear speed of 180 m / s, a feed rate of 10 kg / h, a spray yield of 91%, and a spherical precursor after cooling.

[0108] (III) Same as step (III) in Example 1.

[0109] (IV) Same as step (IV) of Example 1.

[0110] Example 3

[0111] This embodiment is a method for preparing a silicon-carbon negative electrode material, which includes the following steps.

[0112] (I) Same as step (I) of Example 1.

[0113] (II) Add 2kg of anhydrous nickel chloride (boiling point 987°C, solubility in ethanol>20g / L) to the nano-silicon slurry and disperse at 1000rpm for 1h to obtain a mixed slurry, the viscosity of the mixed slurry is 24.5mPas, and the solid content is 24%. The mixed slurry is spray-dried, the inlet air temperature is 160°C, the outlet air temperature is 80°C, the linear speed of the atomizer is 180m / s, the feed amount is 10kg / h, the spray yield is 91%, and a spherical precursor is obtained after cooling.

[0114] (III) Same as step (III) in Example 1.

[0115] (IV) Same as step (IV) of Example 1.

[0116] Example 4

[0117] This embodiment is a method for preparing a silicon-carbon negative electrode material, which includes the following steps.

[0118] (I) Same as step (I) of Example 1.

[0119] (II) Add 2kg of anhydrous cobalt chloride (boiling point 1049°C, solubility in ethanol>20g / L) to the nano-silicon slurry and disperse at 1000rpm for 1h to obtain a mixed slurry with a viscosity of 24.5mPas and a solid content of 24%. The mixed slurry was spray dried with an inlet air temperature of 160°C, an outlet air temperature of 80°C, an atomizer linear speed of 180m / s, a feed rate of 10kg / h, a spray yield of 91%, and a spherical precursor after cooling.

[0120] (III) Same as step (III) in Example 1.

[0121] (IV) Same as step (IV) of Example 1.

[0122] Example 5

[0123] This embodiment is a method for preparing a silicon-carbon negative electrode material, which includes the following steps.

[0124] (I) Same as step (I) of Example 1.

[0125] (II) Add 2kg of anhydrous manganese chloride (boiling point 1190°C, solubility in ethanol>20g / L) to the nano-silicon slurry and disperse at 1000rpm for 1h to obtain a mixed slurry with a viscosity of 24.5mPas and a solid content of 24%. The mixed slurry was spray dried with an inlet air temperature of 160°C, an outlet air temperature of 80°C, an atomizer linear speed of 180m / s, a feed rate of 10kg / h, a spray yield of 91%, and a spherical precursor after cooling.

[0126] (III) Same as step (III) in Example 1.

[0127] (IV) Same as step (IV) of Example 1.

[0128] Example 6

[0129] This embodiment is a method for preparing a silicon-carbon negative electrode material, which includes the following steps.

[0130] (I) Same as step (I) of Example 1.

[0131] (II) 1 kg of anhydrous zinc chloride (boiling point of 732°C, solubility in ethanol>20 g / L) and 1 kg of anhydrous manganese chloride (boiling point of 1190°C, solubility in ethanol>20 g / L) were added to the nano-silicon slurry and dispersed at 1000 rpm for 1 hour to obtain a mixed slurry with a viscosity of 24.5 mPas and a solid content of 23%. The mixed slurry was spray dried with an inlet air temperature of 160°C, an outlet air temperature of 80°C, an atomizer linear speed of 180 m / s, a feed rate of 10 kg / h, a spray yield of 91%, and a spherical precursor after cooling.

[0132] (III) Same as step (III) in Example 1.

[0133] (IV) Same as step (IV) of Example 1.

[0134] Example 7

[0135] This embodiment is a method for preparing a silicon-carbon negative electrode material, which includes the following steps.

[0136] (I) Same as step (I) of Example 1.

[0137] (II) 4 kg of anhydrous zinc chloride (boiling point 732°C, solubility in ethanol>20 g / L) was added to the nano-silicon slurry and dispersed at 1000 rpm for 1 hour to obtain a mixed slurry with a viscosity of 24.5 mPas and a solid content of 27%. The mixed slurry was spray dried with an inlet air temperature of 160°C, an outlet air temperature of 80°C, an atomizer linear speed of 180 m / s, a feed rate of 10 kg / h, a spray yield of 91%, and a spherical precursor after cooling.

[0138] (III) Same as step (III) in Example 1.

[0139] (IV) Same as step (IV) of Example 1.

[0140] Example 8

[0141] This embodiment is a method for preparing a silicon-carbon negative electrode material, which includes the following steps.

[0142] (I) Same as step (I) of Example 1.

[0143] (II) Same as step I in Example 1.

[0144] (III) The spherical precursor was placed in a rotary kiln, and the temperature was first raised to 150°C for 2 h at a heating rate of 5°C / min under a nitrogen atmosphere, and then raised to 550°C for 4 h. The reactant was mixed with a phenolic resin solution in a ratio of 2:1 (the carbon coating increment was about 26 wt%), and then placed in a box furnace for calcination, with a vacuum degree of ≤10 Pa, and the temperature was raised to 600°C for 5 h at a heating rate of 1°C / min to obtain an intermediate.

[0145] (IV) Same as step (IV) of Example 1.

[0146] Example 9

[0147] This embodiment is a method for preparing a silicon-carbon negative electrode material, which includes the following steps.

[0148] (I) Same as step (I) of Example 1.

[0149] (II) Same as step (II) of Example 1.

[0150] (III) The spherical precursor was placed in a rotary kiln, and the temperature was first raised to 150°C for 2 h at a heating rate of 5°C / min under a nitrogen atmosphere, and then raised to 550°C for 4 h. The reactants were mixed with asphalt in a ratio of 1:0.4 (the carbon coating increment was about 21.9 wt%), and then placed in a vacuum furnace for calcination with a vacuum degree of ≤10 Pa, and the temperature was raised to 650°C for 5 h at a heating rate of 1°C / min to obtain an intermediate.

[0151] (IV) Same as step (IV) of Example 1.

[0152] Example 10

[0153] This embodiment is a method for preparing a silicon-carbon negative electrode material, which includes the following steps.

[0154] (I) Same as step (I) of Example 1.

[0155] (II) Same as step (II) of Example 1.

[0156] (III) The spherical precursor was placed in a rotary kiln, and the temperature was first raised to 150°C for 2 h at a heating rate of 5°C / min under a nitrogen atmosphere, and then raised to 550°C for 4 h. The reactants were mixed with asphalt in a ratio of 2:1.2 (the carbon coating increment was about 29.6 wt%), and then placed in a vacuum furnace for calcination, with a vacuum degree of ≤10 Pa, and the temperature was raised to 650°C for 5 h at a heating rate of 1°C / min to obtain an intermediate.

[0157] (IV) Same as step (IV) of Example 1.

[0158] Embodiment 11

[0159] This embodiment is a method for preparing a silicon-carbon negative electrode material, which includes the following steps.

[0160] (I) 10kg silicon powder (Dv50 is 8.5μm, silicon content is 98wt.%), 1.5kg phenolic resin, 1.0kg n-dodecylamine and 50kg acetone are sand-milled together, firstly coarsely ground for 4h using a zirconia ball with a diameter of 0.4mm, the speed of the sand mill is 1000rpm, and then finely ground for 10h using a zirconia ball with a diameter of 0.1mm, the speed of the sand mill is 1500rpm, to obtain nano silicon slurry. The Dv10 of nano silicon in the nano silicon slurry is measured by Malvern particle size analyzer, and it is 57nm, Dv50 is 127nm, Dv90 is 196nm, Dv100 is 247nm, (Dv90-Dv10) / Dv50 is 1.09, and the oxygen content in the nano silicon is 9wt.%.

[0161] (II) Add 2kg of anhydrous zinc chloride (boiling point 732°C, solubility in acetone>20g / L) to the nano-silicon slurry and disperse at 1000rpm for 1h to obtain a mixed slurry with a viscosity of 24.5mPas and a solid content of 21%. The mixed slurry was spray dried with an inlet air temperature of 160°C, an outlet air temperature of 80°C, an atomizer linear speed of 180m / s, a feed rate of 10kg / h, a spray yield of 91%, and a spherical precursor after cooling.

[0162] (III) The spherical precursor was placed in a rotary kiln, heated to 200°C for 1 h at a heating rate of 10°C / min under a nitrogen atmosphere, and then heated to 650°C for 3 h. The reactants were mixed with asphalt in a ratio of 2:1 (the carbon coating increment was about 26 wt%), and then placed in a vacuum furnace for calcination with a vacuum degree of ≤10 Pa, and heated to 650°C for 5 h at a heating rate of 1°C / min to obtain an intermediate.

[0163] (IV) Same as step (IV) of Example 1.

[0164] Example 12

[0165] This embodiment is a method for preparing a silicon-carbon negative electrode material, which includes the following steps.

[0166] (I) 10 kg of silicon powder (Dv50 is 5.5 μm, silicon content is 97 wt.%), 1 kg of asphalt, 0.7 kg of triethanolamine and 20 kg of ethanol were sand-milled together, firstly coarsely ground for 3 h using a zirconia ball with a diameter of 0.6 mm, the speed of the sand mill being 1200 rpm, and then finely ground for 16 h using a zirconia ball with a diameter of 0.05 mm, the speed of the sand mill being 1400 rpm, to obtain a nano-silicon slurry. The Dv10 of the nano-silicon in the nano-silicon slurry was measured by a Malvern particle size analyzer to be 60 nm, Dv50 to be 128 nm, Dv90 to be 190 nm, Dv100 to be 220 nm, (Dv90-Dv10) / Dv50 to be 1.02, and the oxygen content in the nano-silicon was 7 wt.%.

[0167] (II) Add 2kg of anhydrous calcium chloride (boiling point of 1600°C, solubility in ethanol>20g / L) to the nano-silicon slurry and disperse at 1500rpm for 1h to obtain a mixed slurry, the viscosity of the mixed slurry is 43.5mPas, and the solid content is 39%. The mixed slurry is spray-dried, the air inlet temperature is 190°C, the air outlet temperature is 100°C, the linear speed of the atomizer is 200m / s, the feed amount is 12kg / h, the spray yield is 92%, and a spherical precursor is obtained after cooling.

[0168] (III) The spherical precursor was placed in a rotary kiln, and the temperature was first raised to 150°C for 2 h at a heating rate of 3°C / min under an argon atmosphere, and then raised to 550°C for 4 h. The reactants were mixed with asphalt in a ratio of 2:1 (the carbon coating increment was about 26 wt%), and then placed in a vacuum furnace for calcination with a vacuum degree of ≤10 Pa, and the temperature was raised to 680°C for 4 h at a heating rate of 3°C / min to obtain an intermediate.

[0169] (IV) Same as step (IV) of Example 1.

[0170] Embodiment 13

[0171] This embodiment is a method for preparing a silicon-carbon negative electrode material, which includes the following steps.

[0172] (I) Same as step (I) of Example 1.

[0173] (II) Same as step (II) of Example 1.

[0174] (III) Same as step (III) in Example 1.

[0175] (IV) Alcohol washing is performed at a mass ratio of 1:7 between the intermediate and ethanol, the alcohol washing temperature is 40°C, the alcohol washing is performed in a vacuum device, the vacuum degree is 100Pa, stirring is continued for 12h, and then filter pressing is performed, and then rinsing is performed with ethanol 100 times the mass of the material until the Cl element content in the material is less than 0.01wt.%, and then air drying is performed at 50°C. Then it is loaded into a rotary kiln, mixed with asphalt at a ratio of 2:0.3 (the carbon coating increment is about 9.5wt%), and then placed in a vacuum furnace for roasting, the vacuum degree is ≤10Pa, and the temperature is raised to 650°C at a heating rate of 1°C / min and kept for 2h.

[0176] Comparative Example 1

[0177] This comparative example is a method for preparing a silicon-carbon negative electrode material, which includes the following steps.

[0178] (I) Same as step (I) of Example 1.

[0179] (II) The nano-silicon slurry was spray dried, with an inlet air temperature of 160° C., an outlet air temperature of 80° C., an atomizer linear velocity of 180 m / s, a feed rate of 10 kg / h, a spray yield of 91%, and a spherical precursor obtained after cooling.

[0180] (III) Same as step (III) in Example 1.

[0181] (IV) Same as step (IV) of Example 1.

[0182] The silicon-carbon negative electrode material prepared in Comparative Example 1 was subjected to SEM detection, and the results are as follows: Figure 4 As shown in the figure, the morphology of the prepared silicon-carbon negative electrode material is irregular and has a low circularity. The silicon-carbon negative electrode material prepared in Comparative Example 1 was tested on the CP section, and the results are as follows: Figure 5 As shown in the figure, it can be seen that the pores of the prepared silicon-carbon negative electrode material are very few and unevenly distributed.

[0183] Comparative Example 2

[0184] This comparative example is a method for preparing a silicon-carbon negative electrode material, which includes the following steps.

[0185] (I) Same as step (I) of Example 1.

[0186] (II) Add 2kg of anhydrous sodium chloride (boiling point 1465°C, solubility in ethanol <20g / L) to the nano-silicon slurry and disperse at 1000rpm for 1h to obtain a mixed slurry, the viscosity of the mixed slurry is 24.5mPas, and the solid content is 24%. The mixed slurry is spray-dried, the air inlet temperature is 160°C, the air outlet temperature is 80°C, the linear speed of the atomizer is 180m / s, the feed amount is 10kg / h, the spray yield is 91%, and a spherical precursor is obtained after cooling.

[0187] (III) Same as step (III) in Example 1.

[0188] (IV) Same as step (IV) of Example 1.

[0189] Comparative Example 3

[0190] This comparative example is a method for preparing a silicon-carbon negative electrode material, which includes the following steps.

[0191] (I) Same as step (I) of Example 1.

[0192] (II) 0.5 kg of anhydrous zinc chloride (boiling point 731° C.) was added to the nano-silicon slurry and dispersed at 1000 rpm for 1 hour to obtain a mixed slurry, the viscosity of the mixed slurry was 24.5 mPas, and the solid content was 22%. The mixed slurry was spray-dried, the air inlet temperature was 160° C., the air outlet temperature was 80° C., the linear speed of the atomizer was 180 m / s, the feed amount was 10 kg / h, the spray yield was 91%, and a spherical precursor was obtained after cooling.

[0193] (III) Same as step (III) in Example 1.

[0194] (IV) Same as step (IV) of Example 1.

[0195] Comparative Example 4

[0196] This comparative example is a method for preparing a silicon-carbon negative electrode material, which includes the following steps.

[0197] (I) 10 kg of silicon powder (Dv50 is 5.5 μm, silicon content is 97 wt.%), 1 kg of asphalt, 0.7 kg of triethanolamine, 2 kg of anhydrous zinc chloride (boiling point is 732°C, solubility in ethanol> 20 g / L) and 40 kg of ethanol were sand-milled together, firstly coarsely ground for 4 h using a zirconia ball with a diameter of 0.4 mm, the speed of the sand mill being 1000 rpm, and then finely ground for 10 h using a zirconia ball with a diameter of 0.10 mm, the speed of the sand mill being 1500 rpm, to obtain nano-silicon slurry. The Dv10 of nano-silicon in the nano-silicon slurry was measured by a Malvern particle size analyzer to be 97 nm, Dv50 to be 259 nm, Dv90 to be 396 nm, Dv100 to be 847 nm, (Dv90-Dv10) / Dv50 to be 1.15, and the oxygen content in the nano-silicon was 11.5 wt.%.

[0198] (II) The nano-silicon slurry was spray dried, with an inlet air temperature of 160° C., an outlet air temperature of 80° C., an atomizer linear velocity of 180 m / s, a feed rate of 10 kg / h, a spray yield of 91%, and a spherical precursor obtained after cooling.

[0199] (III) Same as step (III) in Example 1.

[0200] (IV) Same as step (IV) of Example 1.

[0201] The silicon-carbon negative electrode materials obtained in Examples 1 to 13 and Comparative Examples 1 to 4 were subjected to various performance tests. The test conditions are as follows. The test results are shown in Tables 1 and 2.

[0202] (1) Angle of repose test

[0203] A funnel with a neck length of 4 cm and an inner diameter of 0.6 cm was used to hold the spherical silicon-carbon negative electrode material. The funnel was fixed on an iron frame. The diameter of the test chassis was 10 cm, and the edge was slightly raised. The distance between the bottom of the funnel and the test chassis was 10 cm. The silicon-carbon negative electrode material was dripped onto the test chassis through the funnel to form a conical structure. The cone height was measured with a ruler. The angle of repose was calculated using the formula: tan(a) = cone height / chassis radius

[0204] (2) Circularity test

[0205] ImageJ was used to calculate circularity. First, File>Open to open the FESEM image to be analyzed, (Image>type>8bit) convert the image to 8bit, Adjust>Threshold, adjust the color range, identify the particle morphology, click Apply, Process>Binary>Fill Holes to fill the spheres (there are blanks in the middle of some spheres), Process>Binary>watershed to split the overlapping spheres, then Analyze>Set Measurements, check Shape descriptors, Redirect to select the image name to be processed, click OK, and finally Analyze>Analyze Particles, Size range 100-Infinity, circularity range 0-1.0, show select Masks, check Display results, Exclude on edges, Summarize and Overlay, and click OK. Circ. in the Summary file corresponds to the average circularity (Count≥100 is required).

[0206] (3) Rebound rate inflection point test

[0207] The prepared silicon-carbon negative electrode material was used as the active material, mixed with the aqueous dispersion of acrylonitrile multipolymer (LA132, solid content 15%) and the conductive agent (Super P) in a mass ratio of 92:6:2, and an appropriate amount of water was added as a solvent to adjust the solid content of the slurry to 55%, which was coated on copper foil and vacuum dried to obtain a silicon negative electrode sheet. The density of the silicon-carbon negative electrode material was calculated according to the compaction density of 13.0 g / cm 3 Up to 1.80g / cm 3 Roll compaction (each tap density increases by 0.5 g / cm 3 ), test the roller thickness, calculate the rebound rate, make a compaction density-rebound rate curve, and obtain the rebound rate inflection point (i.e. the critical point of particle crushing).

[0208] (4) Porosity calculation

[0209] ImageJ was used to calculate the porosity of the selected particle area. First, File>Open to open the FESEM image to be analyzed, and use a rectangular frame to select the cross-section of the spherical particle with a rectangular size of 2.0μm*2.0μm; Image->Duplicate to extract the framed area, (Image>type>8bit) to convert the image to 8bit, Adjust>Threshold, adjust the color range, identify the pore morphology, click Apply, and obtain the porosity based on the pore area and the area of ​​the framed area.

[0210] (5) Aperture test

[0211] The pore size analysis was performed using an ASAP2460 multi-station fully automatic specific surface area and pore size analyzer. The test mode was Micropore Analysis, the degassing temperature was 300°C, the degassing time was 6h, the pressure value was 69 points, and the low-pressure air intake was 10CC.

[0212] (6) Density test

[0213] The true density was measured using a 1200e true density tester, with a gas pressure of 0.14Mpa to 0.15Mpa, a weighing volume of 80% of the sample cell, and 5 test data with RSD ≤ 0.02%.

[0214] The tap density was measured using a BT-312 tap density tester, with the sample height in the measuring cylinder ranging from 21 mL to 25 mL, a vibration frequency of 250 times / min, and 5000 vibrations.

[0215] The compaction density refers to the standard GB / T24533-2019, using the UTM7305 battery powder compaction density meter, sample mass 1g, pressure 10KN, displacement 10mm / min.

[0216] (7) Use a specific surface area analyzer to measure the specific surface area.

[0217] (8) Use a carbon-sulfur analyzer to test the carbon content of the silicon-carbon negative electrode material.

[0218] (9) An oxygen-nitrogen analyzer was used to test the oxygen content of the silicon-carbon negative electrode material, and XRF was used to test the silicon and metal element contents.

[0219] (10) Electrochemical test

[0220] The prepared silicon-carbon negative electrode material was used as the active material, mixed with the aqueous dispersion of the binder acrylonitrile multipolymer (LA132, solid content 15%) and the conductive agent (Super P) in a mass ratio of 92:6:2, and an appropriate amount of water was added as a solvent to adjust the solid content of the slurry to 55%, which was coated on a copper foil, and vacuum dried and rolled to prepare a negative electrode sheet. A metal lithium sheet was used as the counter electrode, 1 mol / L LiPF6 and a three-component mixed solvent of EC:DMC:EMC=1:1:1 (v / v / v) were used to form an electrolyte, and a polypropylene microporous membrane was used as a diaphragm to assemble a CR2032 button cell in a glove box filled with inert gas. The charge and discharge test of the button cell was carried out on a LANHE battery test system.

[0221] The first charge and discharge performance test: At room temperature, discharge at a constant current of 0.1C to a voltage of 0.01V, then discharge at a constant current of 0.02C to a voltage of 0.005V, and charge at a constant current of 0.1C to a voltage of 1.5V to obtain the first reversible specific capacity and the first coulombic efficiency.

[0222] Cycle performance test: Under room temperature conditions, 1C constant current charge and discharge to 0.01V, then 0.05C constant current discharge to 0.005V, and finally 1C constant current charge to 1.5V to obtain the lithium desorption specific capacity. This cycle is repeated 100 times, and the capacity retention rate and expansion rate after 100 cycles are calculated.

[0223] Table 1 Performance tests of silicon-carbon negative electrode materials of Examples 1 to 13 and Comparative Examples 1 to 4 (I)

[0224]

[0225]

[0226] Table 2 Performance tests of silicon-carbon negative electrode materials of Examples 1 to 13 and Comparative Examples 1 to 4 (II)

[0227]

[0228] Table 3 Performance tests of silicon-carbon negative electrode materials of Examples 1 to 13 and Comparative Examples 1 to 4 (III)

[0229]

[0230] From the results in Tables 1 to 3, it can be seen that the silicon-carbon negative electrode materials prepared in Examples 1 to 13 have a higher roundness, and the compaction density corresponding to the inflection point of the rebound rate is higher. The structure of the material is stable and not easy to break, and its corresponding electrochemical performance is also better.

[0231] In Comparative Example 1, no spheroidizing additive was added, and the repulsive force of the nano-silicon slurry was strong. During the spraying process, a dense shell layer was easily formed on the outer layer first, and the inside was loose, and it collapsed after drying to form an irregular structure, so a spherical silicon-carbon precursor could not be obtained, so the performance of the obtained silicon-carbon negative electrode material was poor. In Comparative Example 2, sodium chloride was added. Sodium chloride is difficult to dissolve in organic solvents, and the solubility does not meet the solubility of >20g / L. It is difficult to change the state of the nano-silicon slurry, and it is difficult to spray to obtain a spherical precursor. In Comparative Example 3, the content of the spheroidizing additive added is too little, and the ionic strength is insufficient. It can only slightly improve the spray morphology, and it is difficult to obtain a spherical silicon-carbon negative electrode material. The spheroidizing additive added in Comparative Example 4 is directly added to the preparation process of the nano-silicon slurry, which affects the ball milling efficiency, leads to an increase in the particle size of the nano-silicon, destroys the protective effect of the dispersant on the nano-silicon, increases the nano-silicon oxygen content, and has poor dispersion uniformity of the spray slurry. The surface of the particles after spraying is rough and the specific surface area is large.

[0232] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention is described in detail with reference to the preferred embodiments, it is not limited to those listed in the embodiments. Those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. Silicon-carbon negative electrode material, characterized in that: It includes an inner core and a shell layer, wherein the inner core includes a porous silicon-carbon matrix, the shell layer includes a carbon-coated outer layer, the porous silicon-carbon matrix includes nano-silicon, a silicate layer, a carbon-coated inner layer and a carbon filler from the inside to the outside, the carbon filler has a pore structure, and the circularity of the silicon-carbon negative electrode material is ≥0.

9.

2. The silicon-carbon negative electrode material according to claim 1, characterized in that: The invention comprises at least one of the following features (1) to (22): (1) The total pore volume of the silicon-carbon negative electrode material is 0.025 cm 3 / g to 0.200cm 3 / g; (2) The repose angle of the silicon-carbon negative electrode material is less than 30°; (3) The relative true density of the silicon-carbon negative electrode material is K, 0.70≤K≤0.95; (4) The compaction density corresponding to the rebound rate inflection point of the silicon-carbon negative electrode material is ≥1.60g / cm 3 ; (5) The average nitrogen adsorption pore size of the silicon-carbon negative electrode material is d, d≤Dv50; (6) The specific surface area of ​​the silicon-carbon negative electrode material is 0.5 m 2 / g to 5.0m 2 / g; (7) The silicon grain size of the silicon-carbon negative electrode material is 1 nm to 15 nm; (8) The tap density of the silicon-carbon negative electrode material is ≥ 0.95 g / cm 3 ; (9) The true density of the silicon-carbon negative electrode material is 1.50 g / cm 3 Up to 2.00g / cm 3 ; (10) The carbon content of the silicon-carbon negative electrode material is 25wt.% to 50wt.%; (11) The silicon content of the silicon-carbon negative electrode material is 48wt.% to 67wt.%; (12) The oxygen content of the silicon-carbon negative electrode material is 1 wt.% to 10 wt.%; (13) The metal content of the silicon-carbon negative electrode material is 0.1wt.% to 2.0wt.%; (14) The first reversible specific capacity of the silicon-carbon negative electrode material is ≥ 1800 mAh / g; (15) The first coulombic efficiency of the silicon-carbon negative electrode material is ≥88%; (16) The expansion rate of the silicon-carbon negative electrode material after 100 cycles is ≤40%; (17) The capacity retention rate of the silicon-carbon negative electrode material after 100 cycles is ≥ 95%; (18) The particle size of the silicon-carbon negative electrode material satisfies 1 μm ≤ Dv50 ≤ 10 μm, Dv100 ≤ 30 μm, (Dv90-Dv10) / Dv50 ≤ 2.0, Dv60 / Dv10 ≤ 3; (19) The porosity difference of the silicon-carbon negative electrode material on the same cross section is σ1, σ1≤5%, and the porosity difference of the silicon-carbon negative electrode material on different cross sections is σ2, σ2≤10%; (20) The silicate layer comprises M x SiO y layer, wherein M is selected from at least one of Ni, Co, Mn, Fe, Ca and Zn, 0<x<0.1, 1≤y≤2; (21) The carbon filler accounts for 20wt.% to 45wt.% of the silicon-carbon negative electrode material; (22) The carbon coating outer layer accounts for 3wt.% to 10wt.% of the silicon-carbon negative electrode material.

3. The silicon-carbon negative electrode material according to claim 1, characterized in that: The pore structure includes micropores, mesopores and macropores.

4. The silicon-carbon negative electrode material according to claim 3, characterized in that: Includes at least one of the following features ① to ③: ① Micropores with pore diameters of 0.4nm to 2.0nm, pore volume ≤ 0.001cm 3 / g, the mesopore volume of the pore size is 2nm to 50nm ≤0.01cm 3 / g, the pore volume of macropores with pore diameters ranging from 50nm to 500nm is 0.025cm 3 / g to 0.200cm 3 / g; ② The micropore volume with a pore size of 0.4nm to 2.0nm accounts for 0% to 1% of the total pore volume, the mesopore volume with a pore size of 2nm to 50nm accounts for 0% to 10% of the total pore volume, and the macropore volume with a pore size of 50nm to 500nm accounts for 90% to 99% of the total pore volume; ③ The pore volume of macropores with pore diameters ranging from 50nm to 150nm accounts for more than 50% of the total pore volume.

5. A method for preparing a silicon-carbon negative electrode material, characterized in that: Includes steps: (I) preparing nano-silicon slurry by sand grinding silicon powder, a carbon source, a dispersant and an organic solvent; (II) adding a spheroidizing additive to the nano-silicon slurry and dispersing the mixture to obtain a mixed slurry, and spray-drying the mixed slurry to obtain a spherical precursor, wherein the spheroidizing additive is an inorganic ionic compound soluble in an organic solvent, and the boiling point of the spheroidizing additive is greater than 500° C. and the solubility in the organic solvent is greater than 20 g / L, and the mass ratio of the silicon powder to the spheroidizing additive is 1:0.1 to 1.0; (III) heat treating the spherical precursor at 500° C. to 700° C. and then coating the spherical precursor with a carbon filler to obtain an intermediate; (IV) After removing the spheroidizing additive in the intermediate, the intermediate is coated with a carbon outer layer.

6. The method for preparing the silicon-carbon negative electrode material according to claim 5, characterized in that: Includes at least one of the following features (i) to (nineteen): (1) The Dv50 of the silicon powder satisfies 1 μm ≤ Dv50 ≤ 10 μm; (ii) the silicon content of the silicon powder is ≥ 95wt.%; (iii) the carbon source comprises at least one of phenolic resin, citric acid, asphalt, sucrose, glucose, fructose, lignin, tannic acid and dopamine; (iv) the dispersant comprises at least one of n-dodecylamine, triethanolamine, isoamyl alcohol, oleic acid and cycloalkylsulfonic acid; (v) the organic solvent comprises at least one of methanol, ethanol, propanol, isopropanol, acetone, toluene and xylene; (vi) The mass ratio of silicon powder, carbon source, dispersant and solvent is 1:0.02-0.15:0.05-0.10:2-10; (VII) The sanding speed is 500 rpm to 1500 rpm; (VIII) The nano-silicon slurry contains nano-silicon, the particle size of the nano-silicon satisfies 50nm≤Dv50≤150nm, Dv100≤400nm, and the oxygen content of the nano-silicon is ≤15wt.%; (ix) the spheroidizing additive includes at least one of NiCl2, CoCl2, MnCl2, FeCl2, CaCl2 and ZnCl2; (10) The viscosity of the mixed slurry is 1 mPas to 500 mPas; (XI) The solid content of the mixed slurry is 20% to 50%; (XII) The linear speed of the atomizer used in the spray drying is 150m / s to 250m / s; (XIII) The air inlet temperature of the spray drying is 110°C to 200°C; (14) The outlet air temperature of the spray drying is 70°C to 120°C; (XV) The spray drying spray yield is ≥90%; (16) the heat treatment is carried out under an inert atmosphere, wherein the inert atmosphere comprises at least one of helium, neon, argon, krypton and xenon; (XVII) The heating rate of the heat treatment is 1°C / min to 5°C / min; (XVIII) The carbon filling body may be filled multiple times, and the treatment temperature during filling is 500°C to 1000°C; (19) The carbon sources of the carbon filler and the carbon outer layer are independently a liquid carbon source, a solid carbon source and a gaseous carbon source.

7. The method for preparing the silicon-carbon negative electrode material according to claim 5, characterized in that: The spheroidizing additive is removed by vacuum roasting, water washing or alcohol washing.

8. The method for preparing the silicon-carbon negative electrode material according to claim 7, characterized in that: The method comprises at least one of the following features (i) to (iii): (i) the vacuum calcination is carried out in a vacuum furnace, the temperature of the vacuum calcination is 500° C. to 900° C., the vacuum degree in the vacuum furnace is ≤100 Pa, and the vacuum calcination time is 2 h to 24 h; (ii) the water washing or alcohol washing may be performed multiple times until the Cl element content in the silicon-carbon negative electrode material is less than 0.01 wt.%; (iii) The solvent used in the alcohol washing is methanol, ethanol, propanol or isopropanol.

9. The method for preparing the silicon-carbon negative electrode material according to claim 5, characterized in that: The sand grinding includes coarse grinding and fine grinding.

10. The method for preparing the silicon-carbon negative electrode material according to claim 9, characterized in that: Includes at least one of the following features (a) to (b): (A) The coarse grinding is performed using coarse grinding balls, the diameter of the coarse grinding balls is 0.1 mm to 1.0 mm, and the coarse grinding time is 1 h to 8 h; (B) The fine grinding adopts fine grinding balls, the diameter of the fine grinding balls is 0.03mm to 0.20mm, and the sand grinding time of the fine grinding is 2h to 24h.

Citation Information

Cited By

  • Silicon carbon-graphite negative electrode active material, negative electrode material and application of silicon carbon-graphite negative electrode active material

    CN119786577A

  • Silicon-carbon composite negative electrode material and preparation method and application thereof

    CN120933326A

  • Preparation method of two-stage composite silicon-carbon negative electrode material

    CN121260783A

  • Preparation method of two-stage composite silicon-carbon negative electrode material

    CN121260783B

  • Negative plate, manufacturing method thereof and battery

    CN121583869A