Antifouling paint composition
The optimized low-VOC antifouling paint composition with a specific monomer blend and rosin derivative addresses viscosity and stress issues, ensuring effective and durable antifouling performance even in low-temperature conditions.
Patent Information
- Application Number
- JP2020174825
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-10-16
- Publication Date
- 2024-10-04
- Estimated Expiration
- 2040-10-16
AI Technical Summary
Conventional low-VOC hydrolyzable antifouling paints face issues with high viscosity, leading to poor painting workability and film appearance, increased internal stress due to hydrolysis, and reduced water resistance, resulting in peeling and cracking, especially in low-temperature environments and over time, which compromises long-term antifouling performance.
A low-VOC antifouling paint composition optimized with a specific monomer composition of silyl ester copolymer and rosin derivative, within a defined molecular weight range, to maintain low viscosity and suppress internal stress, ensuring crack resistance and effective antifouling properties even in low-temperature conditions.
The composition achieves both long-term antifouling properties and crack resistance, with improved coating workability in low-temperature environments, maintaining film integrity and effectiveness over time.
Smart Images

Figure 0007561567000005 
Figure 0007561567000001 
Figure 0007561567000002
Abstract
Description
[Technical field]
[0001] The present invention relates to an antifouling coating composition, an antifouling coating film, a substrate with an antifouling coating film, and a method for producing a substrate with an antifouling coating film. [Background technology]
[0002] A wide variety of aquatic organisms, including animals such as oysters, mussels, and barnacles, plants such as seaweed, and bacteria, are likely to adhere to the surfaces of substrates (ships, underwater structures, fishing nets, water supply and drainage pipes for factories, etc.) that are exposed to water (oceans, rivers, lakes, marshes, etc.) for long periods of time in the natural environment. When such aquatic organisms adhere to the substrate surface, they can damage the appearance and cause various problems. For example, if the substrate is a ship, the increased resistance caused by the water flow can lead to a slower ship speed and increased fuel consumption. If the substrate is an underwater structure, the anticorrosive coating applied to the substrate surface can be damaged, resulting in damage such as a decrease in strength and functionality and a significant shortening of the substrate lifespan. If the substrate is a fishing net such as an aquaculture net or fixed net, the mesh can be clogged by aquatic organisms, causing serious problems such as the death of cultured organisms and fished organisms due to lack of oxygen. In addition, if the substrate is a seawater supply and drainage pipe in a factory or a thermal or nuclear power plant, the attachment and proliferation of aquatic organisms can cause the blockage of the water supply and drainage pipe and a decrease in the flow rate.
[0003] In order to prevent the adhesion of aquatic organisms that cause such problems, an antifouling coating film is usually formed by applying an antifouling coating material to the surface of a substrate. Among these antifouling coating materials, hydrolysis-type antifouling coating materials are widely used because of their advantages such as excellent antifouling performance, and as one of them, antifouling coating materials containing silyl ester copolymers have been developed.
[0004] In recent years, there has been a strong demand for hydrolyzable antifouling paint compositions that have a low content of volatile organic compounds (hereinafter, referred to as volatile organic compounds: VOCs) mainly resulting from organic solvents (described below) and that can reduce the environmental load and adverse effects on the health of painters (hereinafter, referred to as low-VOC hydrolyzable antifouling paints). The following Patent Documents 1 and 2 relate to low-VOC hydrolyzable antifouling paints. Patent Document 1 discloses a silyl ester copolymer solution containing a silyl ester copolymer having a weight-average molecular weight of 1,500 to 20,000, having a solids content of at least 55 mass% and a viscosity of less than 20 poise at 25°C, and an antifouling coating composition containing the silyl ester copolymer, having a VOC content of less than 400 g / L and a viscosity of less than 20 poise at 25°C.
[0005] Patent Document 2 discloses an antifouling coating composition which contains a polymer (A) having a number average molecular weight of 1,000 to 20,000, which is obtained by polymerizing a polymerizable unsaturated carboxylate triorganosilyl, and at least one zinc salt (B) selected from a rosin zinc salt and a zinc salt of a rosin derivative in a specific weight ratio to the polymer (A), and which is substantially free of rosin or rosin derivatives having a free carboxy group. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Special Publication No. 2009-513736 [Patent Document 2] International Publication No. 2009 / 066632 Summary of the Invention [Problem to be solved by the invention]
[0007] An antifouling coating film formed from a hydrolyzable antifouling paint composition that imparts a function of preventing adhesion of aquatic organisms to substrates such as ships (hereinafter referred to as antifouling properties) exhibits antifouling properties, for example, as a hydrolysis reaction progresses from the coating film surface when the ship is sailing, causing the coating film to dissolve. Conventional hydrolysis-type antifouling paint compositions use resins with relatively high molecular weights to ensure long-term durability, and therefore many of them have high viscosity. In order to ensure good coating workability and coating appearance, it is necessary to blend a large amount of organic solvents, which places a heavy burden on the environment. Due to recent environmental issues and regulations, there is a high demand for low VOCs with low organic solvent content in antifouling paints. One method for achieving low VOCs is to reduce the molecular weight of the resin, but this tends to reduce the water resistance of the antifouling coating film formed, and due to the low molecular weight, the flexibility of the antifouling coating film formed tends to be insufficient, and internal stress tends to increase due to deterioration over time (progression of hydrolysis reaction). Such antifouling coating films with high internal stress are correlated with a high risk of peeling and cracking, and naturally, the antifouling properties of antifouling coating films that have peeled or cracked are reduced, so it is desirable to have low internal stress. The antifouling coating film formed by the low-VOC hydrolysis-type antifouling paints disclosed in Patent Documents 1 and 2 does not sufficiently suppress the increase in internal stress after deterioration over time, and has problems such as a loss of physical properties and antifouling properties over the long term.It has been found that, particularly in large ships which have a long period between repair painting and a long expected service life, cracks, peeling, and fouling due to the increase in internal stress in the coating film occur while the ship is in service. In particular, in the case of an antifouling coating film containing a silyl ester copolymer, as the hydrolysis reaction progresses inside the coating film, the coating film hardness increases, which increases the internal stress of the coating film, making the coating film more susceptible to the above problems. In addition, because low-VOC hydrolysis-type antifouling paints contain a small amount of organic solvent, the resin viscosity is highly temperature-dependent, and the viscosity is high in low-temperature environments (e.g., 10°C), which can cause problems during painting work.
[0008] The above-mentioned Patent Documents 1 and 2 disclose antifouling coating compositions using triorganosilyl ester hydrolyzed resins, but the compositions differ in the monomer composition, molecular weight, and blended components of the silyl ester polymers in the present application, and there is a problem of peeling and cracking due to increased internal stress caused by aging. None of the compositions in the present application examine the excellent long-term physical properties and antifouling properties achieved by reducing the viscosity and suppressing the internal stress, as in the present invention, and the focus of the present invention is different. The present invention aims to provide a low-VOC antifouling coating composition which is capable of achieving both long-term antifouling properties and crack resistance and also has excellent coating workability even in a low-temperature environment (10°C); an antifouling coating film formed from the antifouling coating composition; and a substrate with an antifouling coating film having the antifouling coating film and a method for producing the same. [Means for solving the problem]
[0009] The present inventors have conducted extensive research to solve the above problems, and have found that the above problems can be solved by optimizing the monomer composition and molecular weight of the silyl ester copolymer, and by selecting an elution aid. That is, the present invention relates to the following [1] to
[10] . [1] An antifouling coating composition comprising a silyl ester copolymer (A) and rosin and / or a derivative thereof (B), having a VOC (volatile organic compound) content of 400 g / L or less, the silyl ester copolymer (A) comprising, relative to 100 parts by mass of all structural units, 55 to 65 parts by mass of structural units derived from triisopropylsilyl methacrylate (a1), 15 to 35 parts by mass of structural units derived from 2-methoxyethyl methacrylate (a2), and structural units derived from an ethylenically unsaturated monomer (a3) having no carboxy group other than triisopropylsilyl methacrylate (a1) and 2-methoxyethyl methacrylate (a2), and having a weight average molecular weight (Mw) of 18,000 to 28,000. [2] The antifouling coating composition according to [1], wherein the mass ratio (WA / WB) of the content (WA) of the silyl ester copolymer (A) to the content (WB) of the rosin and / or its derivative (B) in the antifouling coating composition is 0.5 or more and 10 or less. [3] The antifouling coating composition according to [1] or [2], wherein the viscosity (KU value) of the antifouling coating composition measured using a Stormer viscometer at a temperature of 10°C is 120 or less. [4] The antifouling coating composition according to any one of [1] to [3], wherein the phosphor bronze plate has a maximum warpage height h of 15 mm or less, as measured by the following procedures (1) to (3). (1) An antifouling paint composition is applied to the entire surface of one side of a phosphor bronze plate measuring 120 mm in length, 20 mm in width, and 0.1 mm in thickness, so that the dry film thickness is 100 μm, and the plate is dried at 23°C and 50% humidity for 7 days to prepare a test specimen. (2) The test specimen prepared in (1) above is immersed in seawater at 50°C for three months. (3) The test specimen (2) above is removed from the seawater and dried at 23°C and 50% humidity for 1 hour. The test specimen is then placed on a horizontal surface with the antifouling coating composition coated surface facing up, and the maximum warpage height h (mm) is measured. [5] The antifouling coating composition according to any one of [1] to [4], wherein the content of the imidazole compound in the solid content of the antifouling coating composition is 0.01 mass % or less. [6] The antifouling coating composition according to any one of [1] to [5], wherein the ethylenically unsaturated monomer (a3) having no carboxy group other than the triisopropylsilyl methacrylate (a1) and the 2-methoxyethyl methacrylate (a2) is a (meth)acrylic acid ester. [7] An antifouling coating film formed from the antifouling coating composition according to any one of [1] to [6]. [8] A substrate having an antifouling coating film, comprising a substrate and the antifouling coating film according to [7] provided on a surface of the substrate. [9] The substrate with an antifouling coating film according to [8], wherein the substrate is at least one selected from ships, underwater structures, fishing equipment, and water supply and drainage pipes.
[10] A method for producing a substrate with an antifouling coating film, comprising a step of applying the antifouling coating composition according to any one of [1] to [6] to a substrate, or impregnating the substrate with the antifouling coating composition according to any one of [1] to [6]. Effect of the Invention
[0010] According to the present invention, it is possible to provide a low-VOC antifouling coating composition which is capable of achieving both long-term antifouling properties and crack resistance and also has excellent coating workability even in a low-temperature environment (10°C), an antifouling coating film formed from the antifouling coating composition, and a substrate with an antifouling coating film having the antifouling coating film and a method for producing the same. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 is a schematic diagram showing a method for measuring internal stress (maximum warpage height of a phosphor bronze plate) in an example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Hereinafter, an embodiment of the present invention will be described in detail. Each of the components described in this specification may be used alone or in combination of two or more. "(Meth)acrylate" is a general term for acrylate and methacrylate. The same applies to the use of (meth)acrylic acid, etc. "Structural unit derived from XX" means XX is A 1 A 2 C=CA 3 A 4 (C=C is a polymerizable carbon-carbon double bond, A 1 ~A 4 are atoms or groups bonded to carbon atoms), then, for example, the structural unit is represented by the following formula:
[0013] [ka]
[0014] [Anti-fouling paint composition] The antifouling coating composition of the present invention (hereinafter also referred to as "the composition") contains a silyl ester copolymer (A) and rosin and / or a derivative thereof (B), has a VOC (volatile organic compound) content of 400 g / L or less, and the silyl ester copolymer (A) is composed of structural units derived from triisopropylsilyl methacrylate (a1) in an amount of 55 to 65 parts by mass, structural units derived from 2-methoxyethyl methacrylate (a2) in an amount of 15 to 35 parts by mass, and structural units derived from an ethylenically unsaturated monomer (a3) having no carboxy group other than triisopropylsilyl methacrylate (a1) and 2-methoxyethyl methacrylate (a2), relative to 100 parts by mass of all structural units, and has a weight average molecular weight (Mw) of 18,000 to 28,000. According to the present invention, there is provided a low-VOC antifouling coating composition which is capable of achieving both long-term antifouling properties and crack resistance, and which also has excellent coating workability even in a low-temperature environment (10°C).
[0015] Although the detailed reasons why the antifouling coating composition of the present invention provides the above-mentioned effects are unclear, part of the reasons is thought to be as follows. Conventionally, in antifouling coating compositions using silyl ester hydrolyzable resins, resins with relatively high molecular weights have been used to ensure long-term durability. In contrast, in the present invention, by adopting a silyl ester copolymer (A) containing a specific amount of structural units derived from a specific monomer and rosin and / or its derivative (B) as an elution aid, it has been revealed that high antifouling properties can be maintained in a specific weight-average molecular weight range that is lower than conventional ones. In addition, since the silyl ester copolymer (A) has a low molecular weight, it can be used as a hydrolyzable antifouling coating material with low viscosity and low VOC, and further, an antifouling coating composition with excellent paintability even in a low temperature environment was obtained. In addition, the antifouling coating film formed from the antifouling coating composition of the present invention has a lower molecular weight than conventional ones, but by adopting a silyl ester copolymer (A) containing a specific amount of structural units derived from a specific monomer, the internal stress is low, and even if the formed antifouling coating film deteriorates over time, the occurrence of cracks is suppressed, and antifouling properties are maintained for a long period of time. The present invention will be described in detail below.
[0016] <Silyl ester copolymer (A)> In the present invention, the silyl ester copolymer (A) comprises, relative to 100 parts by mass of all structural units, 55 to 65 parts by mass of structural units derived from triisopropylsilyl methacrylate (a1), 15 to 35 parts by mass of structural units derived from 2-methoxyethyl methacrylate (a2), and structural units derived from an ethylenically unsaturated monomer (a3) having no carboxy group other than triisopropylsilyl methacrylate (a1) and 2-methoxyethyl methacrylate (a2), and has a weight average molecular weight (Mw) of 18,000 to 28,000. That is, the above silyl ester copolymer (A) preferably satisfies the following conditions 1 to 4. Condition 1: From the viewpoint of improving the hydrolysis (dissipation) and static antifouling properties of the formed antifouling coating film, the content of the structural unit derived from triisopropylsilyl methacrylate (a1) is 55 parts by mass or more and 65 parts by mass or less, preferably 58 parts by mass or more and 62 parts by mass or less, based on 100 parts by mass of all structural units. If the content of the structural unit derived from (a1) is less than 55 parts by mass, the hydrolysis property tends to decrease and the antifouling property tends to decrease. On the other hand, if it exceeds 65 parts by mass, the hardness of the coating film tends to increase due to the progress of the hydrolysis reaction inside the coating film, and peeling or cracking due to the increase in internal stress tends to occur. Condition 2: From the viewpoint of improving the hydrolysis property (consumability) and static antifouling property of the antifouling coating film formed, the content of the structural unit derived from 2-methoxyethyl methacrylate (a2) is 15 parts by mass or more and 35 parts by mass or less, and preferably 20 parts by mass or more and 30 parts by mass or less, relative to 100 parts by mass of all structural units. If the content of the structural unit derived from (a2) is less than 15 parts by mass, the hydrophilicity of the antifouling coating film formed tends to be insufficient and the antifouling property tends to decrease, whereas if it exceeds 35 parts by mass, the hydrophilicity of the antifouling coating film formed becomes too high and the water resistance becomes insufficient, and the internal stress increases as the hydrolysis reaction proceeds, tending to cause peeling and cracking. Condition 3: The weight average molecular weight (Mw) of the silyl ester copolymer (A) is 18,000 or more and 28,000 or less, preferably 18,000 or more and 26,000 or less, from the viewpoint of achieving both long-term antifouling and crack resistance, because it is advantageous to lower the viscosity of the composition, and the antifouling coating film formed has excellent static antifouling properties while suppressing the increase in internal stress. If the Mw of the copolymer (A) is less than 18,000, the water resistance of the antifouling coating film formed becomes insufficient, and the increase in internal stress due to the progress of hydrolysis reaction becomes significant, increasing the risk of peeling and cracking. On the other hand, if the Mw exceeds 28,000, the viscosity of the obtained antifouling coating composition becomes high, making it difficult to ensure good coating workability and smoothness of the coating film, and the antifouling properties tend to be inferior due to the influence of unevenness generated on the coating film surface. The Mw can be determined by gel permeation chromatography (GPC) measurement under the conditions employed in the examples described below or an equivalent method. Condition 4: From the viewpoint of lowering the viscosity of the composition and suppressing an increase in internal stress, it is preferable that the silyl ester copolymer (A) has no carboxy group and has substantially no acid value.
[0017] When the silyl ester copolymer (A) has an acid value and is used as a low-VOC hydrolysis-type antifouling coating composition, the viscosity of the coating material is likely to increase due to the influence of the copolymer (A), and the coating workability and the leveling property of the antifouling coating film formed are reduced, which makes it easier for aquatic organisms to adhere, that is, the antifouling property tends to decrease. In addition, when the silyl ester copolymer (A) has an acid value and the antifouling coating composition contains a metal oxide such as cuprous oxide or zinc oxide described below, the viscosity of the coating material is likely to increase due to the crosslinking between the copolymer (A) and the metal oxide, and the internal stress of the antifouling coating film formed tends to increase due to the progress of the hydrolysis reaction. Incidentally, "substantially no acid value" specifically means that the acid value is less than 0.1 mgKOH / g. As described above, when the silyl ester copolymer (A) satisfies the above conditions 1 to 4, a low-VOC antifouling coating composition capable of achieving both long-term antifouling properties and crack resistance can be obtained.
[0018] The content of the silyl ester copolymer (A) in the coating composition is preferably 5% by mass or more, more preferably 10% by mass or more, from the viewpoint of improving various antifouling coating performances such as coating workability, long-term storage stability, water resistance of the coating film formed, suppression of an increase in internal stress, hydrolysis (consumability), static antifouling property, and appearance, and is preferably 50% by mass or less, more preferably 30% by mass or less, and even more preferably 20% by mass or less. The content of the silyl ester copolymer (A) in the solids (heating residue, non-volatile content) of the antifouling coating composition is, for the same reasons as above, preferably 5% by mass or more, more preferably 10% by mass or more, and preferably 50% by mass or less, more preferably 30% by mass or less, and even more preferably 20% by mass or less. In this specification, the solid content (heating residue, non-volatile content) of the composition is the heating residue obtained by the following method or an equivalent method. 1.5 g of the composition was weighed out into a metal test dish of known mass, spread on the bottom, placed in a thermostatic chamber maintained at 105 to 110°C and heated for 3 hours, removed and cooled to room temperature (e.g., 23°C), and then weighed again to determine the amount remaining in the metal test dish. The same applies to the solid content of each component.
[0019] 2-Methoxyethyl methacrylate (a2) has good compatibility with triisopropylsilyl methacrylate (a1) and has the same degree of reactivity as triisopropylsilyl methacrylate (a1), so that structural units derived from each monomer are evenly (randomly) incorporated into the resulting copolymer, imparting appropriate flexibility and hydrophilicity.
[0020] The silyl ester copolymer (A) has a structural unit derived from an ethylenically unsaturated monomer (a3) (hereinafter simply referred to as "ethylenically unsaturated monomer (a3)") that does not have a carboxy group other than triisopropylsilyl methacrylate (a1) and 2-methoxyethyl methacrylate (a2). The ethylenically unsaturated monomer (a3) can be any ethylenically unsaturated monomer that is not the above-mentioned triisopropylsilyl methacrylate (a1) and 2-methoxyethyl methacrylate (a2) and does not have a carboxy group, and can be used without limitation. Examples of the ethylenically unsaturated monomer (a3) include (meth)acrylates, polyfunctional (meth)acrylates, vinyl monomers, silyl acrylates, metal ester group-containing (meth)acrylates, and (poly)organosiloxane structure-containing (meth)acrylates.
[0021] Specific examples of the ethylenically unsaturated monomer (a3) include, for example, (Meth)acrylates, specifically, methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, octyl (meth)acrylate, isooctyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, 3,5,5-trimethylhexyl (meth)acrylate, lauryl (meth)acrylate, )acrylate, tridecyl (meth)acrylate, cetyl (meth)acrylate, stearyl (meth)acrylate, and other alkyl (meth)acrylates; cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, and other alicyclic (meth)acrylates; phenyl (meth)acrylate, benzyl (meth)acrylate, and other aromatic (meth)acrylates; hydroxymethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, hydroxyalkyl (meth)acrylates such as methoxymethyl (meth)acrylate, 2-methoxyethyl acrylate, ethoxymethyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, 4-methoxybutyl (meth)acrylate, methoxypropyl (meth)acrylate, ethoxypropyl (meth)acrylate, propoxyethyl (meth)acrylate, 2-butoxyethyl (meth)acrylate, isobutoxyethyl (meth)acrylate, phenoxyethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, Alkoxyalkyl (meth)acrylates or aryloxyalkyl (meth)acrylates such as methoxy-3-phenoxypropyl (meth)acrylate; glycol-based (meth)acrylates such as ethoxy-diethylene glycol (meth)acrylate, methoxy-triethylene glycol (meth)acrylate, methoxy-dipropylene glycol (meth)acrylate; cyclic ether-containing (meth)acrylates such as glycidyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate; (meth)acrylic acid esters; Polyfunctional (meth)acrylates, specifically, tetraethylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, 1,3-butanediol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, ethylene glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, trimethylolpropane tri(meth)acrylate, di(trimethylolpropane) tetra(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate; Vinyl esters, specifically, vinyl acetate, isobutyl vinyl ether, vinyl toluene, (meth)acrylonitrile, vinyl propionate, vinyl benzoate; Vinyl monomers, specifically, vinyl acetate, vinyl propionate, vinyl benzoate, isobutyl vinyl ether, styrene, α-methylstyrene, vinyl toluene, (meth)acrylonitrile; Silyl acrylates, in particular triisopropylsilyl acrylate; Metal ester group-containing (meth)acrylates, specifically, zinc (meth)acrylate, zinc di(meth)acrylate, zinc di(3-acryloyloxypropionate), zinc acrylate (methacrylate), zinc (meth)acrylate (naphthenate), copper (meth)acrylate, copper di(meth)acrylate, copper acrylate (methacrylate), copper di(3-acryloyloxypropionate), copper (meth)acrylate (naphthenate); Examples include:
[0022] Among these, as the ethylenically unsaturated monomer (a3), (meth)acrylates are preferred, and alkyl (meth)acrylates are more preferred. The alkyl group preferably has 1 or more and 12 or less carbon atoms, more preferably 1 or more and 8 or less carbon atoms, and further preferably 1 or more and 6 or less carbon atoms. The ethylenically unsaturated monomer (a3) having no carboxy group is more preferably at least one selected from the group consisting of methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, and butyl (meth)acrylate, and it is particularly preferable to use methyl (meth)acrylate and butyl (meth)acrylate in combination.
[0023] In the present invention, the silyl ester copolymer (A) is composed of structural units derived from the above monomers (a1) to (a3). Therefore, it does not have structural units derived from monomers other than the above (a1) to (a3), such as structural units derived from ethylenically unsaturated monomers having a carboxy group. However, this does not exclude that, for example, a structural unit derived from triisopropylsilyl methacrylate (a1) may have a carboxy group by hydrolysis after preparation of the silyl ester copolymer (A) or the present composition. As a result, at least in the state where no hydrolysis occurs in the silyl ester copolymer (A), the acid value is 0 mgKOH / g.
[0024] The silyl ester copolymer (A) is prepared by copolymerizing at least the above triisopropylsilyl methacrylate (a1), the above 2-methoxyethyl methacrylate (a2) and the above ethylenically unsaturated monomer (a3) by a known polymerization method. The polymerization method is not particularly limited, but may include solution polymerization, bulk polymerization, semi-batch polymerization, suspension polymerization, pressure polymerization, coordination polymerization, living polymerization, or radical or ionic polymerization in emulsion polymerization. Among these, it is preferable to use a general-purpose organic solvent and carry out solution polymerization of the above (a1) to (a3) in order to improve the productivity and manufacturing workability of the silyl ester copolymer (A) and to prepare a silyl ester copolymer (A) having a relatively low viscosity. Examples of general-purpose organic solvents include aromatic hydrocarbon solvents such as toluene, xylene, ethylbenzene, mesitylene, and coal tar naphtha; aliphatic hydrocarbon solvents such as pentane, hexane, heptane, and octane; alicyclic hydrocarbon organic solvents such as cyclohexane, methylcyclohexane, and ethylcyclohexane; alcohol solvents such as ethanol, propanol, isopropyl alcohol, butanol, and isobutanol; ether solvents such as propylene glycol monomethyl ether and dipropylene glycol monomethyl ether; ketone solvents such as methyl ethyl ketone, methyl isobutyl ketone, methyl amyl ketone, cyclohexanone, acetylacetone, and acetone; and ester solvents such as ethyl acetate, butyl acetate, and propylene glycol monomethyl ether acetate. The solution polymerization can be produced by the following procedure. A solvent is charged into a reaction vessel equipped with a stirrer, a condenser, a thermometer, a dropping device, a nitrogen inlet tube, and a heating / cooling jacket, and the mixture is heated and stirred under a nitrogen stream at a temperature of about 60 to 200° C. While maintaining the same temperature, a mixture of the above-mentioned monomers, a polymerization initiator, and, if necessary, a solvent and a chain transfer agent are dropped from the dropping device, preferably so as to obtain the ratio of the structural units described above, to carry out a polymerization reaction, thereby obtaining a silyl ester copolymer (A).
[0025] The polymerization initiator is not particularly limited, and various radical polymerization catalysts can be used. Specific examples include azo compounds such as 2,2'-azobis(2-methylbutyronitrile) (AMBN), 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis(isobutyronitrile), and 4,4'-azobis-4-cyanovaleric acid, and peroxides such as benzoyl peroxide, hydrogen peroxide, cumene hydroperoxide, tert-butyl peroxy-2-ethylhexanoate, tert-butyl peroxybenzoate, tert-butyl peroxyoctoate, potassium persulfate, and sodium persulfate. These radical polymerization initiators may be added to the reaction system only at the start of the reaction, or may be added to the reaction system both at the start of the reaction and during the reaction. The amount of the polymerization initiator used in producing the silyl ester copolymer (A) is preferably 0.1 to 20 parts by mass, more preferably 0.5 to 5 parts by mass, per 100 parts by mass of the total of the above monomers (reactive raw materials). The chain transfer agent is not particularly limited, and examples thereof include α-methylstyrene dimer, thioglycolic acid, diterpene, terpinolene, γ-terpinene; mercaptans such as tert-dodecyl mercaptan and n-dodecyl mercaptan; halides such as carbon tetrachloride, methylene chloride, bromoform and bromotrichloroethane; and secondary alcohols such as isopropanol and glycerin. When a chain transfer agent is used in the production of the silyl ester polymer (A), the amount used is preferably 0.1 to 5 parts by mass per 100 parts by mass of the total of the above monomers (reaction raw materials).
[0026] The ratio of the amounts (mass) of the monomers (a1) to (a3) fed to the polymerization reaction tends to coincide with the ratio of the contents (mass) of the structural units (a1) to (a3) contained in the copolymer to be prepared. Therefore, the ratio can be adjusted to a desired value based on the amounts (mass) of the (a1) and (a2) fed to the polymerization reaction so as to meet the above conditions 1 and 2.
[0027] <Rosin and / or its derivatives (B)> The present composition contains rosin and / or its derivative (B) from the viewpoint of accelerating wear of the antifouling coating film formed and particularly improving the static antifouling properties. The present composition has improved static antifouling properties in particular by combining the silyl ester copolymer (A) with the rosin and / or its derivative (B).
[0028] In the present invention, rosin and / or its derivatives are used as the elution aid. Other elution aids include, for example, monocarboxylic acids such as naphthenic acid, cycloalkenyl carboxylic acid, bicycloalkenyl carboxylic acid, versatic acid, and trimethylisobutenylcyclohexene carboxylic acid. By using rosin and / or its derivatives as the elution aid in the present composition, it is possible to obtain a low-viscosity antifouling coating composition while reducing the amount of solvent used. In addition to the rosin and / or its derivative (B), other elution aids may be used, but the content of the other elution aids in the antifouling coating composition is preferably 50 parts by mass or less, more preferably 30 parts by mass or less, still more preferably 10 parts by mass or less, and particularly preferably 0 part by mass, per 100 parts by mass of the rosin and / or its derivative (B). In other words, it is preferable that the composition does not contain other elution aids.
[0029] Here, among the rosin and / or derivatives thereof (B), examples of the rosin include gum rosin, wood rosin, tall oil rosin, etc. Examples of the rosin derivative include hydrogenated rosin, disproportionated rosin, rosin ester, rosin metal salt, etc. As the rosin and / or derivatives thereof (B), from the viewpoint of the antifouling properties of the antifouling coating film to be formed, rosin is preferred, and gum rosin is more preferred.
[0030] In addition, in the present composition, the mass ratio (WA / WB) of the content (WA) of the silyl ester copolymer (A) to the content (WB) of the rosin and / or its derivative (B) is preferably 0.5 or more and 10 or less, more preferably 0.65 or more and 8 or less, and even more preferably 1 or more and 7 or less.
[0031] <Optional ingredients> The present composition may further contain one or more components selected from the group consisting of copper or a copper compound (C), an organic antifouling agent (D), other binder components (E), a coloring pigment (F), an extender pigment (G), a pigment dispersant (H), a plasticizer (I), an anti-sagging agent (J), an anti-settling agent (K), a dehydrating agent (L), and a solvent (M). Regarding each of the components explained below, one or more kinds can be used.
[0032] [Copper or copper compounds (C)] The composition may contain copper or a copper compound (C) (excluding copper pyrithione) in order to further improve the antifouling properties of the antifouling coating film formed. The copper compound may be either an organic or inorganic copper compound, and examples thereof include powdered copper (copper powder), cuprous oxide, copper thiocyanate (copper rhodanide), cupronickel, and the like. Of the copper or copper compounds (C), it is preferred to contain cuprous oxide from the viewpoint of improving the antifouling properties, particularly against aquatic organisms such as animals, and the water resistance of the antifouling coating film to be formed.
[0033] The average particle size of the cuprous oxide is preferably 1 μm or more and 30 μm or less, more preferably 2 μm or more and 10 μm or less, from the viewpoint of improving the antifouling property and water resistance of the antifouling coating film to be formed.
[0034] The cuprous oxide is preferably surface-treated with glycerin, stearic acid, lauric acid, sucrose, lecithin, mineral oil, or the like, in that it can improve antifouling properties and long-term storage stability. As such cuprous oxide, commercially available products can be used, and examples thereof include "NC-301" (average particle size: 2 to 4 μm) manufactured by NC Tech Co., Ltd., "NC-803" (average particle size: 6 to 10 μm) manufactured by NC Tech Co., Ltd., "NORDOX" manufactured by Nordox Industrier AS, "Red Copp97N Premium" manufactured by AMERICAN CHEMET Co., "Purple Copp" manufactured by AMERICAN CHEMET Co., and "LoLoTint97" manufactured by AMERICAN CHEMET Co.
[0035] When the present composition contains copper or a copper compound (C), the content thereof is preferably 20 mass % or more, more preferably 40 mass % or more, even more preferably 55 mass % or more, and preferably 80 mass % or less, more preferably 75 mass % or less, even more preferably 70 mass % or less, of the solid content of the antifouling coating composition, in order to improve the antifouling properties and water resistance of the antifouling coating film formed from the antifouling coating composition.
[0036] [Organic antifouling agent (D)] The present composition may contain an organic antifouling agent (D) other than the copper or copper compound (C) in order to further improve the antifouling properties of the antifouling coating film to be formed. Examples of the organic antifouling agent (D) include copper pyrithione, zinc pyrithione, 4,5-dichloro-2-n-octyl-4-isothiazolin-3-one (also known as DCOIT), 4-bromo-2-(4-chlorophenyl)-5-(trifluoromethyl)-1H-pyrrole-3-carbonitrile (also known as tralopyril), 4,5-dimethyl-1H-imidazole, (+ / -)-4-[1-(2,3-dimethylphenyl)ethyl]-1H-imidazole (also known as medetomidine), borane-nitrogen base adducts (pyridinetriphenylborane, 4-isopropylpyridinediphenylmethylborane, etc.), N,N-dimethyl-N'-(3,4-dichlorophenyl)urea, N-(2,4,6-trichlorophenyl)urea, N,N-dimethyl-N'-phenyl-(N-fluorodichloromethylthio)sulfamide, tetraalkylthiuram disulfide, zinc dimethyl dithiocarbamate, zinc ethylene bisdithiocarbamate, 2,3-dichloro-N-(2',6'-diethylphenyl)maleimide, and 2,3-dichloro-N-(2'-ethyl-6'-methylphenyl)maleimide.
[0037] Among these organic antifouling agents (D), copper pyrithione and 4,5-dichloro-2-n-octyl-4-isothiazolin-3-one are preferred, and copper pyrithione is more preferred.
[0038] The antifouling coating composition of the present invention may contain an imidazole compound as the organic antifouling agent (D). However, since imidazole compounds are highly basic and tend to promote the hydrolysis reaction of the silyl ester copolymer (A) and increase the internal stress of the antifouling coating film, it is preferable that the content of the imidazole compound is small. The content of the imidazole compound in the solid content of the antifouling coating composition is preferably 0.1 mass % or less, more preferably 0.01 mass % or less, and even more preferably 0.001 mass % or less, with no particular lower limit and particularly preferably 0 mass %. Examples of the imidazole compound include 2-methylimidazole, 4-methylimidazole, 4,5-dimethyl-1H-imidazole, and (+ / -)-4-[1-(2,3-dimethylphenyl)ethyl]-1H-imidazole (also known as medetomidine).
[0039] When the present composition contains an organic antifouling agent (D), the content thereof is, from the viewpoints of coating workability and the antifouling properties and water resistance of the antifouling coating film to be formed, preferably 0.5 mass % or more, more preferably 0.8 mass % or more, even more preferably 1 mass % or more, and preferably 10 mass % or less, more preferably 8 mass % or less, even more preferably 5 mass % or less, of the solid content of the antifouling coating composition.
[0040] [Other binder components (E)] The present composition may contain a binder component (E) other than the silyl ester copolymer (A) for the purpose of imparting static antifouling property, water resistance, crack resistance and strength to the antifouling coating film. Other examples of the binder component (E) include acrylic copolymers (acrylic resins), vinyl polymers, n-paraffins, and terpene phenols.
[0041] The acrylic copolymer may be one obtained by polymerizing the ethylenically unsaturated monomer (a3). From the viewpoint of static soiling resistance, it is preferable that the acrylic copolymer contains a structural unit derived from at least one selected from the group consisting of (meth)acrylates, vinyl monomers, silyl acrylates, and metal ester group-containing (meth)acrylates exemplified as the ethylenically unsaturated monomer (a3).
[0042] When the antifouling coating composition of the present invention contains another binder component (E), the content thereof is preferably from 1 to 20% by mass based on the solid content of the antifouling coating composition. On the other hand, when the antifouling coating composition of the present invention contains another binder component (E) having a carboxy group and substantially having an acid value, the effect of the present invention may not be obtained or the effect may be weakened. Therefore, the content of the other binder component (E) in the antifouling coating composition of the present invention is preferably 50 parts by mass or less, more preferably 30 parts by mass or less, and even more preferably 10 parts by mass or less, relative to 100 parts by mass of the silyl ester copolymer (A), and it is particularly preferable that the antifouling coating composition does not contain the other binder component (E).
[0043] [Color pigment (F)] The present composition may contain a color pigment (F) in order to adjust the color tone of the antifouling coating film to be formed or to impart any desired color tone. Examples of the color pigment (F) include various known organic or inorganic color pigments. Examples of organic color pigments include naphthol red and phthalocyanine blue. Examples of inorganic color pigments include carbon black, titanium oxide, red iron oxide (red iron oxide), black iron oxide, and yellow iron oxide.
[0044] The composition may contain a colorant other than the color pigment (F), such as a dye, together with the color pigment (F) or in place of the color pigment (F). When the present composition contains a color pigment (F), the content thereof is determined in a preferable amount depending on the hiding power required for the antifouling coating film to be formed and the desired viscosity according to the application form of the antifouling paint composition, and is preferably from 0.5 to 10 mass %, more preferably from 1 to 5 mass %, of the solid content of the antifouling paint composition.
[0045] [Extender pigment (G)] The present composition may contain an extender pigment (G) for the purpose of improving the physical properties of the formed antifouling coating film, such as crack resistance. Examples of the extender pigment (G) include talc, zinc oxide, silica (diatomaceous earth, acid clay, etc.), mica, clay, potassium feldspar, calcium carbonate, kaolin, alumina white, white carbon, aluminum hydroxide, magnesium carbonate, barium carbonate, barium sulfate, zinc sulfide, etc. Among these, talc, zinc oxide, silica, mica, clay, calcium carbonate, kaolin, barium sulfate, and potassium feldspar are preferred. When the present composition contains an extender pigment (G), taking into consideration that the antifouling coating film to be formed has better coating film properties such as crack resistance, and that the viscosity can be adjusted to a desired level depending on the application form of the antifouling paint composition, the content of the extender pigment (G) is preferably at least 1 mass %, more preferably at least 3 mass %, even more preferably at least 5 mass %, and is preferably at most 50 mass %, more preferably at most 30 mass %, even more preferably at most 15 mass %, of the solids content of the antifouling paint composition.
[0046] [Pigment dispersant (H)] When the present composition contains a color pigment (F) and / or a body pigment (G), the composition may contain a pigment dispersant (H) from the viewpoint of improving the dispersibility of the color pigment (F) and / or the body pigment (G). Examples of the pigment dispersant (H) include various known organic or inorganic pigment dispersants. Examples of the pigment dispersant include aliphatic amines or organic acids, "Disperbyk-101" (manufactured by BYK Japan Co., Ltd.), "ANTI-TERRA-U 100" (manufactured by BYK Japan Co., Ltd., salt of unsaturated polyaminoamide and low molecular weight polyester acid), and "BYK P-104" (manufactured by BYK Japan Co., Ltd., unsaturated polycarboxylic acid polymer). When the antifouling coating composition of the present invention contains a pigment dispersant (H), the content of the pigment dispersant (H) in the solid content of the antifouling coating composition is preferably 0.01 mass % or more, more preferably 0.05 mass % or more, and preferably 5.0 mass % or less, more preferably 2.0 mass % or less.
[0047] [Plasticizer (I)] The present composition may contain a plasticizer (I) in order to improve the crack resistance of the resulting antifouling coating film. Examples of the plasticizer (I) include tricresyl phosphate (TCP), chlorinated paraffin (chlorinated paraffin), petroleum resins, ketone resins, polyvinyl ethyl ether, dialkyl phthalate, etc. Among these, as the plasticizer (I), chlorinated paraffin (chlorinated paraffin), petroleum resins, and ketone resins are preferred, since they can improve the water resistance of the antifouling coating film formed and adjust the hydrolysis property (consumption property) of the coating film. Specific examples of chlorinated paraffins include "TOYOPARAX A-40 / A-50 / A-70 / A-145 / A-150" manufactured by Tosoh Corporation. In addition, examples of petroleum resins include C5-based, C9-based, styrene-based, dichloropentadiene-based, and hydrogenated versions of these. Specific examples of petroleum resins include "Quinton 1500 / 1700" manufactured by Zeon Corporation. When the present composition contains a plasticizer (I), its content is preferably 0.1 mass % or more, more preferably 0.5 mass % or more, and preferably 10 mass % or less, more preferably 5 mass % or less, based on the solid content of the antifouling coating composition. When the content of the plasticizer (I) is within the above range, the plasticity of the antifouling coating film can be well maintained.
[0048] [Anti-sagging agent (J)] The present composition may contain an anti-sagging agent (J) (also called a flow-stopping agent) so as to reduce the occurrence of sagging due to the coating composition when applied to a substrate. Examples of the anti-sagging agent (J) include amide wax (fatty acid amide, etc.), hydrogenated castor oil wax, mixtures thereof, and synthetic fine silica (Aerosil (registered trademark), etc.), and among these, amide wax or synthetic fine silica is preferred. The use of amide wax or synthetic fine silica as the anti-sagging agent (J) is preferred in that the storage stability of the antifouling coating composition can be improved. Commercially available anti-sagging agents (J) include "Disparlon A630-20X" manufactured by Kusumoto Chemical Industries, Ltd. and "ASA T-250F" manufactured by Ito Oil Mills, Ltd. The anti-sagging agents (J) may be used alone or in combination of two or more kinds. When the present composition contains an anti-sagging agent (J), the content thereof is preferably 0.01 mass % or more, more preferably 0.03 mass % or more, even more preferably 0.1 mass % or more, and preferably 10 mass % or less, more preferably 3 mass % or less, even more preferably 1 mass % or less, based on the solid content of the antifouling coating composition.
[0049] [Anti-settling agent (K)] The present composition may contain an anti-settling agent (K) from the viewpoints of preventing the occurrence of precipitation during storage and improving stirrability. Examples of the anti-settling agent (K) include stearates of Al, Ca, or Zn, polyethylene wax, and oxidized polyethylene wax, and among these, oxidized polyethylene wax is preferred. An example of a commercially available oxidized polyethylene wax is "Disparlon 4200-20X" manufactured by Kusumoto Chemicals Co., Ltd. When the composition contains an anti-settling agent (K), the content thereof is preferably 0.01 mass % or more, more preferably 0.03 mass % or more, even more preferably 0.05 mass % or more, and preferably 10 mass % or less, more preferably 3 mass % or less, even more preferably 1 mass % or less, based on the solid content of the antifouling coating composition.
[0050] [Dehydrating agent (L)] The composition has long-term storage stability because it contains the silyl ester copolymer (A) which has excellent storage stability, but it is possible to obtain even better long-term storage stability by adding a dehydrating agent (L) as necessary. Examples of the dehydrating agent (L) include inorganic dehydrating agents and organic dehydrating agents. As inorganic dehydrating agents, synthetic zeolite, anhydrous gypsum and hemihydrate gypsum are preferred. As organic dehydrating agents, alkoxysilanes such as tetramethoxysilane, tetraethoxysilane, tetrapropoxysilane, tetrabutoxysilane, tetraphenoxysilane, methyltriethoxysilane, dimethyldiethoxysilane and trimethylethoxysilane, polyalkoxysilanes which are partial hydrolysis condensates thereof, and orthoformic acid alkyl esters such as methyl orthoformate and ethyl orthoformate are preferred. Tetraethoxysilane (also known as ethyl silicate) of alkoxysilanes is particularly preferred. When the composition contains a dehydrating agent (L), the content thereof is preferably 0.1 mass% or more, more preferably 0.2 mass% or more, even more preferably 0.5 mass% or more, and preferably 10 mass% or less, more preferably 2 mass% or less, even more preferably 1 mass% or less, based on the solid content of the antifouling coating composition. When the content of the dehydrating agent (L) is within the above range, the storage stability of the antifouling coating composition can be maintained better.
[0051] [Solvent (M)] The present composition may contain a solvent (M) as necessary for the purpose of improving the dispersibility of the silyl ester copolymer (A), etc., maintaining the viscosity of the coating composition low, and improving the spray atomization property. The solvent (M) may be the solvent used when preparing the silyl ester copolymer (A), or may be a solvent added separately when mixing the silyl ester copolymer (A) with other components as necessary.
[0052] As the solvent (M), aromatic hydrocarbon-based, aliphatic hydrocarbon-based, alicyclic hydrocarbon-based, alcohol-based, ether-based, ketone-based, and ester-based organic solvents can be used, with aromatic hydrocarbon-based organic solvents being preferred. Examples of aromatic hydrocarbon organic solvents include toluene, xylene, mesitylene, and coal tar naphtha. Examples of the aliphatic hydrocarbon organic solvent include pentane, hexane, heptane, and octane. Examples of the alicyclic hydrocarbon organic solvent include cyclohexane, methylcyclohexane, and ethylcyclohexane. Examples of the alcohol-based organic solvent include ethanol, propanol, isopropyl alcohol, butanol, and isobutanol. Examples of the ether-based organic solvent include propylene glycol monomethyl ether and dipropylene glycol monomethyl ether. Examples of the ketone organic solvent include methyl ethyl ketone, methyl isobutyl ketone, methyl amyl ketone, cyclohexanone, acetylacetone, and acetone. Examples of the ester-based organic solvent include ethyl acetate, butyl acetate, and propylene glycol monomethyl ether acetate.
[0053] When the composition contains a solvent (M), its content is determined by the desired viscosity depending on the application form of the coating composition, etc.; in the present invention, from the viewpoint of keeping the VOC content at 400 g / L or less, it is preferable to use a small amount of solvent (M), and the content of solvent (M) in the coating composition is preferably 40 mass % or less, more preferably 30 mass % or less, and even more preferably 20 mass % or less; and from the viewpoint of keeping the viscosity of the coating composition low, it is preferably 5 mass % or more, more preferably 10 mass % or more, and even more preferably 15 mass % or more.
[0054] [Other components other than those mentioned above] In addition to the components described above, the composition may contain, for example, a surface conditioner, a leveling agent, an antifoaming agent, etc. Specific examples include "BYK-350" (manufactured by BYK Japan K.K., surface conditioner, acrylic copolymer), "BYK-354" (manufactured by BYK Japan K.K., antifoaming agent, acrylic polymer), etc.
[0055] The composition preferably contains a small amount of sulfonic acid group-containing compound. By containing a sulfonic acid group-containing compound, the internal stress of the antifouling coating film formed increases, and cracks tend to occur. The content of the sulfonic acid group-containing compound is preferably 0.5 mass% or less, more preferably 0.1 mass% or less, even more preferably 0.01 mass% or less, and particularly preferably 0 mass% based on the solid content of the antifouling coating composition. Examples of the sulfonic acid group-containing compound include sulfonic acid compounds and sulfonic acid polymers. The sulfonic acid compound is a compound having one or more sulfonic acid groups in the molecule, and means a sulfonic acid-containing compound other than a sulfonic acid polymer, specifically a compound having no repeating unit in the molecule, that is, a low molecular weight compound. Examples of the sulfonic acid compound include aliphatic sulfonic acid compounds such as methanesulfonic acid, trifluoromethanesulfonic acid, ethanesulfonic acid, vinylsulfonic acid, and 1-propanesulfonic acid, and aromatic sulfonic acid compounds such as benzenesulfonic acid, alkylbenzenesulfonic acid, diphenylsulfonic acid, and naphthalenesulfonic acid. The sulfonic acid polymer is a polymer having one or more sulfonic acid groups in the molecule, and includes, as a structural unit of the sulfonic acid polymer, a structural unit derived from a monomer having at least one sulfonic acid group in one molecule. Examples of the monomer having a sulfonic acid group include styrene sulfonic acid, isoprene sulfonic acid, vinyl sulfonic acid, allyl sulfonic acid, isoamylene sulfonic acid, 2-(meth)acrylamide-2-methylpropane sulfonic acid, and methallyl sulfonic acid, and is preferably polystyrene sulfonic acid.
[0056] <Characteristics of antifouling paint composition> [Viscosity at 10°C] In order to ensure coating workability in low-temperature environments, the composition preferably has a low viscosity even in low-temperature environments, and the viscosity (KU value) measured using a Stormer viscometer at a temperature of 10° C. of the antifouling coating composition is preferably 120 or less, more preferably 115 or less, and even more preferably 110 or less. In addition, from the viewpoint of suppressing sagging during coating, the viscosity is preferably 50 or more, more preferably 60 or more, and even more preferably 70 or more. The viscosity (KU value) is measured by the method described in the Examples below.
[0057] [Internal stress] It is preferable that the antifouling coating film obtained from the present composition shows little increase in internal stress due to the progress of the hydrolysis reaction, and this increase in internal stress can be measured by the method described below. That is, the composition has a maximum warpage height h of preferably 15 mm or less, more preferably 14 mm or less, and even more preferably 13 mm or less, as measured by the following procedures (1) to (3). There is no particular lower limit, and the maximum warpage height h is 0 mm or more. (1) A test specimen is prepared by coating one entire surface of a phosphor bronze plate measuring 120 mm in length, 20 mm in width, and 0.1 mm in thickness with an antifouling paint composition so that the dry film thickness is 100 μm, and then drying the plate at 23°C and 50% humidity for 7 days. (2) The test specimen prepared in (1) above is immersed in seawater at 50°C for three months. (3) The test specimen (2) above is removed from the seawater and dried at 23°C and 50% humidity for 1 hour. The test specimen is then placed on a horizontal surface with the antifouling coating composition coated surface facing up, and the maximum warpage height h (mm) is measured. In addition, when drying in the above (1) and (3), do not ventilate. In the antifouling coating film formed by the conventional antifouling paint composition, as the hydrolysis reaction progresses, for example, the formation of a crosslinked structure between a metal atom in the coating film and an acid group, particularly a carboxy group of the resin component, progresses, and the coating film shrinks, which results in an increase in internal stress and tends to cause cracks in the coating film, etc. It is believed that the increase in internal stress is suppressed in the present composition because the silyl ester copolymer (A) is substantially free of carboxy groups.
[0058] [Anti-fouling coating film] The antifouling coating film of the present invention (hereinafter also referred to as "the present coating film") is an antifouling coating film formed from the present composition described above. The present coating film can be formed by applying or impregnating the present composition onto a substrate and then drying it. The present coating film is preferably an antifouling coating film used for the purpose of preventing substrates from being fouled by aquatic organisms in water.
[0059] [Substrate with antifouling coating film and method for producing same] The substrate with an antifouling coating film of the present invention comprises a substrate and the coating film provided on the surface of the substrate. The method for producing a substrate having an antifouling coating film preferably comprises a step of applying the composition to a substrate (application step), or a step of impregnating a substrate with the composition, and a step of drying the antifouling coating composition.
[0060] <Coating process> Examples of methods for applying the present composition include known methods such as brush coating, roller coating, spraying, roll coater coating, flow coater coating, slit coater coating, gravure coater coating, spin coater coating, curtain roll coater coating, electrostatic coating, dip coating, silk printing, and spin coating. The thickness of the coating film formed from the antifouling coating composition is set so that the antifouling coating film finally formed has a thickness described below. The coating film may be formed by one coating, or by two or more coatings (two or more coatings). The thickness of the present coating film is not particularly limited, but is preferably 5 μm or more, more preferably 10 μm or more, and even more preferably 50 μm or more, and is preferably 1,000 μm or less, more preferably 500 μm or less, and even more preferably 300 μm or less. When the present coating film has such an embodiment, the antifouling coating film has excellent long-term antifouling properties.
[0061] <Drying process> The antifouling coating composition applied by the above-mentioned method can be dried, for example, by leaving it under conditions of 23°C, preferably for 0.5 to 14 days, more preferably for 1 to 10 days, to obtain an antifouling coating film. The antifouling coating composition may be dried under heating and / or with air blowing.
[0062] Here, the substrate is not particularly limited, but is preferably a substrate that comes into contact with seawater or fresh water, more preferably at least one selected from ships, underwater structures, fishing equipment, and water supply and drainage pipes, more preferably ships and underwater structures, and particularly preferably ships.Specific examples include ships (e.g., large steel ships such as container ships and tankers, fishing boats, FRP ships, wooden ships, yachts, and other ship hull shells, particularly the waterline to bottom parts, including any of these shipbuilding or repair ships), underwater structures (e.g., oil pipelines, water conveyance piping, circulating water pipes, water supply and drainage outlets of factories and thermal and nuclear power plants, undersea cables, seawater utilization equipment (seawater pumps, etc.), megafloats, coastal roads, undersea tunnels, port facilities, various underwater civil engineering structures in canals, waterways, etc.), fishing equipment (e.g., ropes, fishing nets, fishing gear, floats or buoys, etc.), water supply and drainage pipes for seawater in factories and thermal and nuclear power plants, etc.
[0063] The material of the substrate is not particularly limited, but examples thereof, particularly for ships, include steel, aluminum, wood, and FRP. Furthermore, the above-mentioned substrate may be one that has been treated with other treatment agents such as a rust inhibitor, may have a coating film such as a primer formed on its surface in advance, may have the present composition already applied thereto, or may be an old antifouling coating film that has deteriorated over time after the present coating film or another antifouling coating film has been formed thereon, and is not particularly limited. EXAMPLES
[0064] (Preparation of Silyl Ester Copolymer Solution (A1)) [Production Example 1] A reaction vessel equipped with a stirrer, a condenser, a thermometer, a nitrogen inlet tube and a dropping device was charged with 43 parts of xylene and 10 parts of triisopropylsilyl methacrylate, and heated and stirred under a nitrogen atmosphere until the liquid temperature reached 80°C. While maintaining the same conditions, a mixture of monomers (55 parts of triisopropylsilyl methacrylate, 25 parts of 2-methoxyethyl methacrylate, 5 parts of methyl methacrylate, 5 parts of butyl acrylate) and a polymerization initiator (1.35 parts of 2,2'-azobis(isobutyronitrile)) was dropped into the reaction vessel over 2 hours from the dropping device. After continuing to heat and stir at the same temperature for 1 hour and at a liquid temperature of 88°C for 1 hour, the liquid temperature was raised to 95°C. While maintaining the same temperature, 0.1 parts of 2,2'-azobis(isobutyronitrile) was added a total of 4 times at 30 minute intervals, and the liquid temperature was raised to 105°C. After continuing to heat and stir at the same temperature for 30 minutes, 23.7 parts of xylene was added to the reaction vessel to obtain a solution of silyl ester copolymer (A1) (copolymer solution (A1)). The weight average molecular weight of the silyl ester copolymer (A1) was 24,848. The solid content (heating residue) of the above solution was 60% by mass. Table 1 shows the raw materials used and the properties of the silyl ester copolymer solution (A1).
[0065] (1) Content of solids (heating residue) in the silyl ester copolymer solution 1.5 g of the copolymer solution (X1(g)) was weighed out into a metal test dish of known mass, spread on the bottom, placed in a thermostatic chamber maintained at 105-110°C under 1 atmosphere and heated for 3 hours, removed and cooled, and then weighed again to determine the remaining amount (X2(g)) in the metal test dish. The content (mass%) of solids (heating residue) was calculated using the following formula. Solid content (heated residue) content (mass%)=X2 / X1×100
[0066] (2) Average molecular weight of silyl ester copolymer The weight average molecular weight (Mw) of the silyl ester copolymer was measured by gel permeation chromatography (GPC) under the following conditions. (GPC conditions) Equipment: "HLC-8320GPC" (Tosoh Corporation) Column: 1 "TSKgel guardcolumn SuperMPHZ-M" + 2 "TSKgel SuperMultiporeHZ-M" (both manufactured by Tosoh Corporation) Eluent: tetrahydrofuran (THF) Flow rate: 0.35mL / min Detector: RI Column thermostat temperature: 40℃ Standard material: polystyrene Sample preparation method: An eluent was added to the silyl ester copolymer solution obtained in each production example, and the solution was filtered through a membrane filter to obtain a filtrate, which was used as a GPC measurement sample.
[0067] (3) Viscosity of copolymer solution The viscosity (unit: mPa·s) of the silyl ester copolymer solution at a liquid temperature of 25°C was measured using an E-type viscometer (Tokyo Keiki Co., Ltd.).
[0068] (Preparation of Silyl Ester-Containing Copolymer Solutions (A2) to (A5) and (B1) to (B10)) [Manufacturing Examples 2 to 15] The monomers used in Production Example 1 were replaced with the types and amounts shown in Table 1, and the reaction temperature and time were appropriately adjusted, but the same procedure as in Production Example 1 was repeated to prepare silyl ester copolymer solutions (A2) to (A5) and (B1) to (B10), and the various properties were measured. The results are shown in Table 1.
[0069] [Table 1]
[0070] <Production of antifouling coating composition> Table 2 shows a list of raw materials used in the preparation of the antifouling coating composition.
[0071] [Table 2]
[0072] [Example 1] 8.0 parts by mass of xylene, 21.0 parts by mass of silyl ester copolymer solution (A1), 4.0 parts by mass of WW rosin, and 0.5 parts by mass of ethyl silicate 28 were added to a plastic container, and mixed using a paint shaker until each component was uniformly dispersed or dissolved. Then, 5.0 parts by mass of two types of zinc oxide, 4.0 parts by mass of TTK talc, 3.0 parts by mass of red iron oxide No. 404, 1.0 part by mass of Copper Omadine Powder, 52.0 parts by mass of cuprous oxide NC-301, 0.5 parts by mass of Disparlon 4200-20X, and 150 parts by mass of glass beads were further added to the plastic container, and these components were dispersed by stirring for 1 hour using a paint shaker. After dispersion, 1.0 part by mass of Disparlon A630-20X was further added and the mixture was stirred for 20 minutes using a paint shaker, after which the glass beads were removed from the mixture using a filter net (opening: 80 mesh) to prepare an antifouling coating composition.
[0073] [Examples 2 to 7, Comparative Examples 1 to 11] The antifouling coating compositions of Examples 2 to 7 and Comparative Examples 1 to 11 were prepared in the same manner as in Example 1, except that the composition of each component was changed as shown in Table 3. The components were mixed and stirred in the proportions (parts by mass) shown in Table 3 to obtain antifouling coating compositions. The amount of each component listed in Table 3 indicates the amount in its original form.
[0074] (1)VOC mass measurement The calculation was performed using the specific gravity and solids (heating residue) content (mass%) of the coating composition shown below according to the following formula. VOC(g / L)=Paint specific gravity×1000×(100-solid content) / 100 (2) Specific gravity At 23° C., the mass of the antifouling coating composition filled in a specific gravity cup having an internal volume of 100 mL was measured to measure the specific gravity (paint specific gravity). (3) Solid content (heated residue) (mass%) 1.5 g (X1(g)) of each antifouling coating composition was weighed out into a metal test dish of known mass, spread on the bottom, placed in a thermostatic chamber maintained at 105-110°C under 1 atmosphere and heated for 3 hours, removed and cooled, and then weighed again to determine the remaining amount (X2(g)) in the metal test dish. The content (mass%) of solids (heating residue) was calculated by the following formula. Solid content (heated residue) content (mass%)=X2 / X1×100
[0075] <Paint viscosity measurement> The viscosity (KU value) of each of the antifouling coating compositions obtained in the Examples and Comparative Examples was measured under the following conditions based on the provisions of JIS K-5600-2-2:1999, without adjusting the viscosity by diluting with a solvent, at two levels of antifouling coating composition temperature, 23°C and 10°C, by putting 250 mL of each composition into a cylindrical container with a diameter of 73 mm and a height of 80 mm. Stormer Viscometer: Coating Tester Industrial Stormer Viscometer Set temperature: 23℃±0.5℃, 10℃±0.5℃ Sample volume: 250mL Weight: 75g~1000g
[0076] <Low temperature spray workability> Each of the antifouling coating compositions prepared in the Examples and Comparative Examples was kept at 10°C and sprayed with an air spray without adjusting the viscosity by diluting with a solvent, etc., and the spread of the spray pattern was visually confirmed. Evaluation was performed according to the following criteria. (Evaluation Criteria) A: When the antifouling coating composition is applied to a substrate using an air spray, the antifouling coating composition is sprayed in the form of a mist of fine particles, the spray pattern is uniform, and there is no unevenness in the amount of the antifouling coating composition applied to the substrate. B: When the antifouling coating composition is applied to a substrate using an air spray, the antifouling coating composition is sprayed as large particles and the spray pattern is broad, streaky, non-uniform, and there is an uneven amount of antifouling coating composition applied to the substrate.
[0077] <Measurement of internal stress (maximum warpage height of phosphorus bronze plate)> The antifouling paint was applied to the entire surface of one side of a phosphor bronze plate (manufactured by Nippon Test Panel Co., Ltd.) with a length of 120 mm, width of 20 mm, and thickness of 0.1 mm using a film applicator so that the dry film thickness was 100 μm, and then dried without ventilation for 7 days at 23°C and humidity of 50%. After that, the plate was immersed in seawater at 50°C for 3 months, and then removed from the seawater and dried without ventilation for 1 hour at 23°C and humidity of 50%. After that, the plate was placed horizontally with the antifouling paint-coated surface of the test specimen facing up as shown in Figure 1, and the maximum warpage height h (mm) was measured. When the specimen was placed horizontally and the warpage heights on both sides were different, the warpage heights on both sides were measured, and the larger warpage height was taken as the maximum warpage height h (mm).
[0078] <Evaluation of crack resistance> In the above-mentioned internal stress measurement, the antifouling paint-coated surface of the test specimen after measuring the maximum warpage height was visually observed and evaluated as follows. A: No cracks were observed. B: Cracks are observed.
[0079] <Waterside static antifouling evaluation test for antifouling coating film> [Static soiling resistance test] On a sandblasted steel plate (length 300 mm × width 100 mm × thickness 3.2 mm), an epoxy-based anticorrosive paint (trade name "Banno 500", manufactured by Chugoku Toryo Co., Ltd.) was applied to a dry film thickness of about 150 μm, and dried at 23 ° C for one day. Next, an epoxy-based binder paint (trade name "Banno 500N", manufactured by Chugoku Toryo Co., Ltd.) was applied to the cured coating film using an air spray to a dry film thickness of about 100 μm, and dried at 23 ° C for one day. Furthermore, each of the antifouling paint compositions of the above examples and comparative examples was applied thereon without adjusting the viscosity by diluting with a solvent to a dry film thickness of about 100 μm, and dried at 23 ° C for 7 days to prepare a test plate with an antifouling coating film. The prepared test plate was placed in the Seto Inland Sea off the coast of Hatsukaichi City, Hiroshima Prefecture, in Hiroshima Bay, so that half of the test plate (the lower half) was immersed in seawater. After that, the adhesion area (%) of aquatic organisms on the antifouling coating film surface at the water's edge (a 10 cm wide area under dry and wet conditions) was measured one month later and every three months. The static antifouling properties of the antifouling coating film were evaluated according to the following evaluation criteria.
[0080] (Evaluation Criteria) 0: No aquatic organisms attached 0.5: The area of aquatic organisms attached is greater than 0% and less than 10%. 1: The area of aquatic organisms attached is more than 10% and less than 20% 2: The area of aquatic organisms attached is more than 20% and less than 30% 3: The area of aquatic organisms attached is more than 30% but less than 40% 4: The area of aquatic organisms attached is more than 40% and less than 50% 5: The area of aquatic organisms attached exceeds 50%.
[0081] [Table 3]
[0082] In Examples 1 to 7, the antifouling coating compositions had a VOC of 400 g / L or less, and had low viscosity even at a low temperature (10° C.), and were excellent in low-temperature spray workability. Furthermore, the antifouling coating films formed from the antifouling coating compositions had suppressed increases in internal stress, suppressed the occurrence of cracks, and were also excellent in long-term static antifouling properties. On the other hand, in Comparative Example 1 in which the silyl ester copolymer solution B1 containing triisopropylsilyl acrylate instead of triisopropylsilyl methacrylate was used, the increase in internal stress was significant and the occurrence of cracks was observed. In Comparative Example 2, in which the content of the structural unit derived from triisopropylsilyl methacrylate is less than 55 parts by mass relative to 100 parts by mass of all structural units, was used, the long-term antifouling property was poor. In addition, compared with Examples 1 to 7, the maximum warpage height was high and the increase in internal stress was also large. In Comparative Example 3, in which silyl ester copolymer solution B3 was used in which the content of structural units derived from 2-methoxyethyl methacrylate exceeded 35 parts by mass per 100 parts by mass of all structural units, there was a significant increase in internal stress and the occurrence of cracks was observed. In Comparative Example 4, in which the silyl ester copolymer solution B4 having Mw of less than 18,000 was used, the increase in internal stress was significant, and the occurrence of cracks was observed. In Comparative Example 5, which used the silyl ester copolymer solution B5 having a Mw of more than 28,000, the viscosity was high and the low-temperature spray workability was poor. In addition, the long-term static soiling resistance was poor. In Comparative Example 6, in which the content of the structural unit derived from triisopropylsilyl methacrylate was more than 65 parts by mass relative to 100 parts by mass of all structural units, the internal stress increased significantly, and when an antifouling coating film was formed on a phosphor bronze plate, the coating film peeled off. Also, cracks occurred in the static antifouling test. In Comparative Example 7, which used the silyl ester copolymer solution B7 having a structural unit derived from methacrylic acid, an ethylenically unsaturated compound having a carboxyl group, the viscosity at low temperature was high and the low-temperature spray workability was poor.In addition, compared with Examples 1 to 7, the maximum warpage height was high, the increase in internal stress was large, and the long-term antifouling property was also poor. In comparison example 8, in which silyl ester copolymer solution B8 was used, in which the content of structural units derived from 2-methoxyethyl methacrylate was less than 15 parts by mass per 100 parts by mass of all structural units, a significant increase in internal stress was observed and peeling of the coating film was observed. In Comparative Example 9, in which the silyl ester copolymer solution B9 containing 2-methoxyethyl acrylate was used instead of 2-methoxyethyl methacrylate, the increase in internal stress was large, and cracks occurred. In Comparative Example 10, in which the silyl ester copolymer solution B10 containing glycerin monomethacrylate was used instead of 2-methoxyethyl methacrylate, the internal stress increased significantly and cracks occurred. Comparative Example 11, which did not contain rosin and / or its derivative (B), experienced a large increase in internal stress, resulting in the occurrence of cracks.
Claims
1. An antifouling coating composition comprising a silyl ester copolymer (A) and a rosin and / or a derivative thereof (B), The VOC (volatile organic compound) content is 400 g / L or less, The content of the imidazole compound in the solid content of the antifouling coating composition is 0.1 mass% or less, the silyl ester copolymer (A) comprises, relative to 100 parts by mass of all structural units, 55 parts by mass or more and 65 parts by mass or less of structural units derived from triisopropylsilyl methacrylate (a1), 15 parts by mass or more and 35 parts by mass or less of structural units derived from 2-methoxyethyl methacrylate (a2), and structural units derived from an ethylenically unsaturated monomer (a3) having no carboxy group other than triisopropylsilyl methacrylate (a1) and 2-methoxyethyl methacrylate (a2), and has a weight average molecular weight (Mw) of 18,000 or more and 28,000 or less; Antifouling coating composition.
2. 2. The antifouling coating composition according to claim 1, wherein a mass ratio (WA / WB) of a content (WA) of the silyl ester-based copolymer (A) to a content (WB) of the rosin and / or derivative thereof (B) in the antifouling coating composition is 0.5 or more and 10 or less.
3. 3. The antifouling coating composition according to claim 1, wherein the viscosity (KU value) of the antifouling coating composition measured at a temperature of 10° C. using a Stormer viscometer is 120 or less.
4. The antifouling coating composition according to any one of claims 1 to 3, wherein the phosphor bronze plate has a maximum warpage height h of 15 mm or less, as measured by the following procedures (1) to (3). (1) A test specimen is prepared by coating one entire surface of a phosphor bronze plate having a length of 120 mm, a width of 20 mm and a thickness of 0.1 mm with an antifouling coating composition so that the dry film thickness is 100 μm, and then drying the plate at 23° C. and a humidity of 50% for 7 days. (2) The test specimen prepared in (1) above is immersed in seawater at 50° C. for three months. (3) The test specimen from (2) above is removed from the seawater and dried at 23°C and 50% humidity for 1 hour. The test specimen is then placed on a horizontal surface with the antifouling coating composition coated surface facing up, and the maximum warpage height h (mm) is measured.
5. The antifouling coating composition according to any one of claims 1 to 4, wherein the content of the imidazole compound in the solid content of the antifouling coating composition is 0.01 mass % or less.
6. The antifouling coating composition according to any one of claims 1 to 5, wherein the ethylenically unsaturated monomer (a3) having no carboxy group other than triisopropylsilyl methacrylate (a1) and 2-methoxyethyl methacrylate (a2) is a (meth)acrylic acid ester.
7. The antifouling coating composition according to any one of claims 1 to 6, wherein the weight average molecular weight of the silyl ester copolymer (A) is 18,000 or more and 26,000 or less.
8. An antifouling coating film formed from the antifouling coating composition according to any one of claims 1 to 7.
9. A substrate with an antifouling coating film, comprising: a substrate; and the antifouling coating film according to claim 8 provided on a surface of the substrate.
10. The substrate with an antifouling coating film according to claim 9, wherein the substrate is at least one selected from ships, underwater structures, fishing materials, and water supply and drainage pipes.
11. A method for producing a substrate with an antifouling coating film, comprising a step of applying the antifouling coating composition according to any one of claims 1 to 7 to a substrate or impregnating a substrate with the antifouling coating composition according to any one of claims 1 to 7.
Citation Information
Patent Citations
Antifouling composition
EP3078715A1
Proportional divider
JP1985067199A
Silyl ester copolymer composition
JP2009513736A
Contamination-proof coating composition, manufacturing method for the composition, contamination-proof coating film formed using the composition, coated article having the coating film on surface, and contamination-proofing treatment method for forming the coating film
JP2011026357A
Heat-proof coating method