Extrudable halogen-free flame retardant composition
A halogen-free flame retardant composition with polyolefin copolymers and high inorganic filler content addresses inefficiencies in producing Euroclass A2 panels, enabling extrusion-based manufacturing that meets fire safety standards and improves mechanical strength.
Patent Information
- Application Number
- JP2021558625
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-04-03
- Filing Date
- 2020-03-26
- Publication Date
- 2024-10-04
- Estimated Expiration
- 2040-03-26
AI Technical Summary
Current methods for producing Euroclass A2 rated aluminum composite panels are inefficient and costly, as they require sintering processes that are slow and difficult to handle, and direct extrusion is challenging with polyolefin-based formulations containing over 83% inorganic filler.
A halogen-free flame retardant composition comprising polyolefin copolymers with a melt flow index of 350-1000 g/10 min and greater than 83% inorganic filler, enabling extrudable core materials for aluminum composite panels with improved mechanical strength and flexibility.
The composition allows for economical and efficient production of Euroclass A2 rated panels through extrusion, meeting fire safety standards while enhancing mechanical properties and processability.
Smart Images

Figure 0007561759000011 
Figure 0007561759000001 
Figure 0007561759000002
Abstract
Description
[Technical field]
[0001] (CROSS REFERENCE TO RELATED APPLICATIONS) This application claims priority to U.S. Provisional Patent Application No. 62 / 828,621, filed April 3, 2019, the entire disclosure of which is incorporated herein by reference.
[0002] FIELD OF THE DISCLOSURE
[0002] Embodiments described herein relate generally to halogen-free flame retardant materials, and in particular to halogen-free flame retardant materials for use in the core layer of aluminum composite panels. [Background technology]
[0003] Aluminum composite panels are rigid composite designs made from a polymer core and bonded to aluminum face sheets with adhesive tie layers.
[0004] Common applications for aluminum composite panels are infrastructure facade systems, visual displays, and transportation. For example, aluminum composite panels can be used in exposed facade systems on high rise buildings. Summary of the Invention [Problem to be solved by the invention]
[0005] Following recent fires in high-rise buildings, stricter fire regulations are being imposed on building facade systems.
[0006] Aluminum composite panels and their fire performance and fuel load can be important to the safety of the façade system. Test criteria are defined by the fire performance rating of the aluminum composite panel's core material. Such a rating may depend on the total heat of combustion (also called heat value or higher calorific value (PCS)), fire growth rate (FIGRA), flammability, and / or total heat release (THR) of the core material. In some incidents, the presence of a non-flame retardant polymer composite core may allow the fire to spread to the façade system during a fire incident.
[0007] Today, manufacturers of aluminum composite panels supply fire-retardant panels designed for facade systems to meet Euro Class B, which specifies the limited flammability of the core material, or the more stringent Euro Class A2 rating. As panels are manufactured and sold worldwide, Euro Class A2 is becoming a global requirement.
[0008] Currently, core materials that meet Euro Class A2 fire safety are processed by sintering on a double band press, which is often obtained from a slurry of inorganic non-combustible components in an aqueous binder system. However, the sintering process is relatively slow and expensive, and the sheets are relatively difficult to handle. In addition, sintered core materials with high loading levels usually have low mechanical strength. Furthermore, the sintering process may require specific manufacturing equipment. On the other hand, conventional non-Euro Class A2 rated composite panels may be produced using sheet extrusion lines. However, for polyolefin-based formulations with inorganic filler contents above 83 wt.%, extrusion or direct extrusion is difficult or impossible. Direct extrusion in this context involves combining the compounding process and final shaping into flat sheets in one processing step. [Means for solving the problem]
[0009] Thus, there is a need for compositions that can be extruded in the production of Euroclass A2 rated core materials for aluminum composite panels.Embodiments of the present disclosure meet these needs by providing compositions that include one or more polyolefin copolymers having a melt flow index between 350 grams per 10 minutes (g / 10 min) and 1000 g / 10 min, measured at 190° C. and 2.16 kg, and greater than 83 wt. % of an inorganic filler, based on the total weight of the halogen-free flame retardant composition.
[0010] It is believed that the inclusion of more than 83 wt% inorganic filler can meet Euro Class A2 ratings, meaning that the formulation has a PCS of less than 3 MJ / kg according to EN ISO 1716. At filler levels of 83 wt% or more, the polymer backbone of the disclosed compositions can enable extrudable compositions that can be utilized as core layers in economical and efficient manufacturing processes for aluminum composite panels. Additionally, embodiments of the present disclosure can enable improved mechanical strength and flexibility when compared to conventional sintered Euro Class A2 rated compositions.
[0011] According to at least one embodiment of the present disclosure, a halogen-free flame retardant composition is provided, comprising one or more polyolefin copolymers having a melt flow index of 350 grams / 10 minutes (g / 10 min) to 1000 g / 10 min measured at 190° C. and 2.16 kg, the one or more polyolefin copolymers comprising maleic anhydride grafted polyolefin, ethylene-vinyl acetate copolymer, and one or more of talc, CaCO3, magnesium hydroxide, aluminum trihydrate, silicon dioxide, siloxane, or mica in an amount of more than 83 wt % of inorganic fillers based on the total weight of the halogen-free flame retardant composition.
[0012] According to at least one embodiment of the present disclosure, a composite panel is provided. The composite panel embodiment may include a first metal layer, a second metal layer, a core layer disposed between the first metal layer and the second metal layer, a first tie layer disposed between the first metal layer and the core layer, and a second tie layer disposed between the second metal layer and the core layer, wherein the core layer comprises a halogen-free flame retardant composition described herein.
[0013] According to at least one embodiment of the present disclosure, a method of manufacturing a composite panel is provided. The method embodiment may include extruding a core layer, applying a first tie layer and a second tie layer to opposing surfaces of the core layer, and laminating a first metal layer and a second metal layer to the first tie layer and the second tie layer, respectively, after application to the core layer, to produce a composite panel, wherein the core layer comprises a halogen-free flame retardant composition as described herein.
[0014] These and other embodiments are described in more detail in the detailed description of the invention below.
[0015] The following detailed description of certain embodiments of the present disclosure can be best understood when read in conjunction with the following drawings, in which like structure is indicated with like reference numerals and in which: [Brief description of the drawings]
[0016] [Figure 1] FIG. 1 is a schematic diagram of an embodiment of a composite panel according to embodiments described herein. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] Certain embodiments of the present application will now be described. These embodiments are provided so that this disclosure will be thorough and complete, and will fully convey the scope of the subject matter to those skilled in the art.
[0018] The term "polymer" refers to a polymeric compound prepared by polymerizing monomers, whether of the same or different types. Thus, the general term polymer encompasses the term "homopolymer," which usually refers to a polymer prepared from only one type of monomer, and "copolymer" refers to a polymer prepared from two or more different monomers. As used herein, the term "interpolymer" refers to a polymer prepared by polymerization of at least two different types of monomers. Thus, the general term interpolymer includes copolymers or polymers prepared from more than two different types of monomers, such as terpolymers.
[0019] As used herein, "polyolefin" or "olefin-based polymer" can include ethylene-based polymers and propylene-based polymers.
[0020] "Polyethylene" or "ethylene-based polymer" shall mean a polymer containing greater than 50 mole percent units derived from ethylene monomer. This includes ethylene-based homopolymers or copolymers (meaning units derived from two or more comonomers). Common forms of ethylene-based polymers known in the art include, but are not limited to, low density polyethylene (LDPE), linear low density polyethylene (LLDPE), ultra low density polyethylene (ULDPE), very low density polyethylene (VLDPE), single-site catalyzed linear low density polyethylene including both linear and substantially linear low density resins (m-LLDPE), medium density polyethylene (MDPE), and high density polyethylene (HDPE).
[0021] "Polyethylene" or "propylene-based polymer" shall mean a polymer containing greater than 50 mole percent units derived from propylene monomers. This includes propylene-based homopolymers or copolymers (meaning units derived from two or more comonomers). Common forms of ethylene-based polymers known in the art include, but are not limited to, impact polypropylene copolymers icPP, random copolymers rcPP, polypropylene homopolymers hPP, ethylene-propylene copolymers (POE plastomers), and polypropylene reactor blends.
[0022] With particular reference to the embodiment of the halogen-free flame retardant composition as described herein, the embodiment of the halogen-free flame retardant composition comprises one or more polyolefin copolymers having a melt flow index of 350 grams / 10 minutes (g / 10 min) to 1000 g / 10 min measured at 190° C. and 2.16 kg, the one or more polyolefin copolymers comprising maleic anhydride grafted polyolefin, ethylene-vinyl acetate copolymer, or blends thereof, and more than 83 wt % of inorganic filler, based on the total weight of the halogen-free flame retardant composition, which may comprise one or more of talc, CaCO3, magnesium hydroxide, aluminum trihydrate, silicon dioxide, siloxane, or mica.
[0023] In embodiments, the halogen-free flame retardant composition described herein may include one or more polyolefin copolymers. In some embodiments, the halogen-free flame retardant composition may include less than 17 wt% of one or more copolymers based on the total weight of the halogen-free flame retardant composition. In other embodiments, the halogen-free flame retardant composition may include from about 10 wt% to about 17 wt%, from about 10 wt% to about 15 wt%, from about 10 wt% to about 13 wt%, from about 10 wt% to about 11 wt%, from about 11 wt% to about 17 wt%, from about 11 wt% to about 15 wt%, from about 11 wt% to about 13 wt%, from about 13 wt% to about 17 wt%, from about 13 wt% to about 15 wt%, or from about 15 wt% to about 17 wt% of one or more copolymers.
[0024] In embodiments, the one or more polyolefin copolymers may include ethylene-vinyl acetate copolymers, maleic anhydride grafted polymers, maleic anhydride copolymers, ethylene-acrylic or ethylene-methacrylic acid copolymers, or copolymers of ethylene (ethyl-, methyl-, butyl-) acrylate, or combinations thereof.
[0025] In embodiments, the halogen-free flame retardant compositions described herein may include one or more polyolefin copolymers. In some embodiments, the one or more polyolefin copolymers may include maleic anhydride grafted polyolefins.
[0026] In an embodiment, the maleic anhydride grafted polyolefin may be an ethylene-based polymer grafted with maleic anhydride grafting monomer. Suitable ethylene-based polymers in the maleic anhydride grafted polyolefin include, but are not limited to, polyethylene homopolymers and copolymers with α-olefins, copolymers of ethylene and vinyl acetate, and copolymers of ethylene and one or more alkyl (meth)acrylates. In a particular embodiment, the maleic anhydride grafted polyolefin may include one or more of maleic anhydride grafted linear low density polyethylene (LLDPE), maleic anhydride grafted polyethylene elastomer, or a combination thereof.
[0027] In embodiments, the maleic anhydride grafted polyolefin may be a propylene-based polymer grafted with maleic anhydride grafting monomer. Suitable propylene-based polymers in the maleic anhydride grafted polyolefin include, but are not limited to, propylene homopolymers and copolymers with α-olefins, copolymers of ethylene and vinyl acetate, and copolymers of ethylene and one or more alkyl (meth)acrylates. In certain embodiments, the maleic anhydride grafted polyolefin may include one or more of maleic anhydride grafted polypropylene, maleic anhydride grafted polypropylene-ethylene plastomer, or a combination thereof.
[0028] When the ethylene-based polymer is a polyethylene homopolymer or a copolymer of ethylene and one or more α-olefins, the ethylene-based polymer can be linear or substantially linear. Suitable α-olefin comonomers, which can be either aliphatic or aromatic, can include C3-C20 α-olefins, C3-C16 α-olefins, or C3-C10 α-olefins. In one or more embodiments, the α-olefin can be a C3-C10 aliphatic α-olefin selected from the group consisting of propylene, 1-butene, 1-hexene, and 1-octene. In an embodiment, the α-olefin is propylene.
[0029] Without being bound by theory, it is believed that the maleic anhydride grafted polyolefins may interact with inorganic fillers to reduce dripping, thus providing halogen-free flame retardant compositions with improved mechanical properties and improved fire performance.
[0030] In one or more embodiments, the maleic anhydride grafted polyolefin comprises about 0.1% to about 10%, about 0.1% to about 5%, 0.5% to about 1.8%, or about 0.1% to about 0.5% by weight of maleic anhydride grafted monomer based on the total weight of the maleic anhydride grafted polyolefin. The weight percentage of the ethylene-based polymer is complementary to the amount of maleic anhydride grafted monomer, so that the sum of the weight percentages of the ethylene-based polymer and the maleic anhydride grafted monomer is 100% by weight. Thus, the maleic anhydride grafted polyolefin comprises up to 90%, up to 95%, or 96-99% by weight of ethylene-based polymer based on the total weight of the maleic anhydride grafted polyolefin.
[0031] In one or more embodiments, the maleic anhydride grafted polyolefin may have a melt index (I2) of about 350 grams / 10 minutes (g / 10 min), or about 400 g / 10 minutes to about 800 g / 10 minutes, about 400 g / 10 minutes to about 600 g / 10 minutes, about 500 to about 1000 grams / 10 minutes (g / 10 min), or about 500 g / 10 minutes to about 800 g / 10 minutes, about 500 g / 10 minutes to about 600 g / 10 minutes, about 600 g / 10 minutes to about 1000 g / 10 minutes, about 600 g / 10 minutes to about 800 g / 10 minutes, or about 800 g / 10 minutes to about 1000 g / 10 minutes, as measured at 190° C. and 2.16 kg according to ASTM D1238.
[0032] In further embodiments, the maleic anhydride grafted polyolefin has a viscosity of less than about 0.910 grams per cubic centimeter (g / cc), from about 0.860 g / cc to about 0.910 g / cc, from about 0.860 g / cc to about 0.900 g / cc, from about 0.860 g / cc to about 0.890 g / cc, from about 0.860 g / cc to about 0.880 g / cc, from about 0.860 g / cc to about 0.870 g / cc, from about 0.870 g / cc to about 0.910 g / cc, from about 0.870 g / cc The maleic anhydride grafted polyolefin has a density of about 0.900 g / cc, about 0.870 g / cc to about 0.890 g / cc, about 0.870 g / cc to about 0.880 g / cc, about 0.880 g / cc to about 0.910 g / cc, about 0.880 g / cc to about 0.900 g / cc, about 0.880 g / cc to about 0.890 g / cc, about 0.890 g / cc to about 0.910 g / cc, about 0.890 g / cc to about 0.900 g / cc, or about 0.900 g / cc to about 0.910 g / cc. In an embodiment, the maleic anhydride grafted polyolefin can be a maleic anhydride grafted polyolefin elastomer having a Brookfield viscosity of greater than 8,000 cP or about 8,000 cP to about 20,000 cP when measured at 177°C.
[0033] Various commercial embodiments are contemplated as suitable. For example, suitable maleic anhydride grafted polyolefins are commercially available from Dow Chemical Company, for example, under the trade names AFFINITY™ GA 1000R and FUSABOND™ P353D.
[0034] Various amounts of maleic anhydride grafted polyolefin are believed to be suitable within the halogen-free flame retardant composition. In embodiments, the halogen-free flame retardant composition may include up to 17 wt.% of maleic anhydride grafted polyolefin, based on the total weight of the halogen-free flame retardant composition. In other embodiments, the halogen-free flame retardant composition may include about 5 wt.% to about 15 wt.%, about 5 wt.% to about 10 wt.%, about 10 wt.% to about 15 wt.%, or about 10 wt.% to about 17 wt.% of maleic anhydride grafted polyolefin, based on the total weight of the halogen-free flame retardant composition.
[0035] As previously mentioned, in embodiments, the halogen-free flame retardant compositions described herein may include one or more polyolefin copolymers. In embodiments, the halogen-free flame retardant compositions described herein may include ethylene-vinyl acetate copolymer (EVA). Ethylene-vinyl acetate copolymers are ethylene-based polymers such as ethylene and vinyl acetate. In embodiments, the ethylene-vinyl acetate copolymer may include about 20% to about 90% by weight ethylene and about 10% to about 80% by weight vinyl acetate, based on the total weight of the ethylene-vinyl acetate copolymer. In other embodiments, the ethylene-vinyl acetate copolymer may comprise one or more of about 20% to about 80% by weight, about 20% to about 60% by weight, about 20% to about 40% by weight, about 20% to about 30% by weight, about 20% to about 25% by weight, about 25% to about 90% by weight, about 25% to about 80% by weight, about 25% to about 60% by weight, about 25% to about 40% by weight, or about 25% to about 30% by weight of ethylene, based on the total weight of the ethylene-ethylene-vinyl acetate copolymer.
[0036] In other embodiments, the one or more polyolefin copolymers may be ethylene-based and may include acrylate or methacrylate groups. In embodiments, the one or more polyolefin copolymers may include ethylene-acrylic or ethylene-methacrylic acid copolymers, copolymers of ethylene (ethyl-, methyl-, butyl-), acrylates, or combinations thereof. These copolymers may, in embodiments, include from about 20% to about 90% by weight ethylene, and from about 10% to about 80% by weight copolymerized functional groups. In other embodiments, the copolymer may comprise from about 20% to about 80% by weight, from about 20% to about 60% by weight, from about 20% to about 40% by weight, from about 20% to about 30% by weight, from about 20% to about 25% by weight, from about 25% to about 90% by weight, from about 25% to about 80% by weight, from about 25% to about 60% by weight, from about 25% to about 40% by weight, or from about 25% to about 30% by weight ethylene, based on the total weight of the copolymer.
[0037] Due to the nature of their chemical composition, ethylene-vinyl acetate copolymers and other copolymers are believed to have a lower calorific value (PCS) compared to polyethylene homopolymers. Therefore, ethylene-vinyl acetate copolymers and other copolymers are believed to contribute less to the calorific value in the halogen-free flame retardant compositions described herein. This may allow embodiments of the halogen-free flame retardant compositions to include a higher fraction of one or more polyolefin copolymers, which provides improved processability.
[0038] In one or more embodiments, the melt index (I2) of the ethylene-vinyl acetate copolymer can be from about 350 to about 1000 grams per 10 minutes (g / 10 min), from about 400 to about 1000 g / 10 min, from about 500 g / 10 min to about 1000 g / 10 min, from about 500 g / 10 min to about 800 g / 10 min, from about 500 g / 10 min to about 600 g / 10 min, from about 600 g / 10 min to about 1000 g / 10 min, from about 600 g / 10 min to about 800 g / 10 min, or from about 800 g / 10 min to about 1000 g / 10 min, measured according to ASTM D1238 at 190° C. and 2.16 kg.
[0039] In further embodiments, the ethylene-vinyl acetate copolymer has a density of less than about 0.955 grams per cubic centimeter (g / cc), or from about 0.860 to about 0.955 g / cc, as measured according to ASTM Method No. D792-91. Other density ranges can be from about 0.870 to about 0.950 g / cc, or from 0.875 to about 0.950 g / cc.
[0040] Various commercial embodiments are contemplated as suitable. For example, a suitable ethylene-vinyl acetate copolymer may be commercially available from EI du Pont de Nemours and Company under the trade name ELVAX™. In a further embodiment, a suitable ethylene-vinyl acetate copolymer may be commercially available from EI du Pont de Nemours and Company under the trade name ELVAX™ 210W.
[0041] Various amounts of ethylene-vinyl acetate copolymer are believed to be suitable within the halogen-free flame retardant composition. In embodiments, the halogen-free flame retardant composition may include up to 17 wt.% of ethylene-vinyl acetate copolymer, based on the total weight of the halogen-free flame retardant composition. In other embodiments, the halogen-free flame retardant composition may include from about 5 wt.% to about 15 wt.%, from about 5 wt.% to about 10 wt.%, from about 10 wt.% to about 15 wt.%, from about 10 wt.% to about 17 wt.% of ethylene-vinyl acetate copolymer, based on the total weight of the halogen-free flame retardant composition.
[0042] In embodiments, the halogen-free flame retardant compositions described herein may include various filler materials, which may be collectively referred to herein as "fillers". The filler materials may include inorganic fillers. Inorganic fillers include CaCO3, BaSO4, CaSO4, silicates, talc, kaolin, clay, mica, silicon dioxide, inorganic flame retardants, and combinations thereof. Inorganic flame retardants include aluminum trihydrate, aluminum oxide, magnesium hydroxide, huntite, boehmite, and their auxiliaries. In embodiments, intumescent flame retardants may be utilized, including calcined clay, graphene, and polyphosphonates. The filler materials may include radical scavenger flame retardants, such as phosphonates, phosphites, melamines, or hindered amines. In further embodiments, the inorganic fillers may be anhydrous inorganic fillers or at least mostly anhydrous inorganic fillers (by weight).
[0043] In some embodiments, the filler can comprise about 51% to about 100% by weight, about 51% to about 80% by weight, about 51% to about 60% by weight, about 60% to about 100% by weight, about 60% to about 80% by weight, or about 80% to about 100% by weight of anhydrous inorganic filler, based on the total weight of the filler in the halogen-free flame retardant composition.
[0044] Without being bound by theory, it is believed that the fire retardant properties of a filler may depend on the amount of water released into the filler. In some embodiments, the filler content may include a majority of anhydrous inorganic fillers that release relatively little water. In general, when water is released, it contributes to fire safety because the steam produced reduces the temperature and retards combustion. In the case of aluminum composite panels, the release of water vapor can cause delamination of the composite panel, leading to structural problems and the risk of fire. The choice of filler and fire retardant package may depend on the design of the final product.
[0045] Filler selection can be influenced by the particle size and particle size distribution of the filler, which can affect the processing, physical properties, and fire performance of the halogen-free flame retardant composition. Reducing the particle size increases the melt viscosity and reduces processability, but improves tear resistance, tensile strength, and elongation at break. For water-releasing flame retardants, more uniform water release can improve the burning behavior. When droplet burning is an issue, finer particles can improve fire performance by reducing dripping behavior.
[0046] Filler selection may be influenced by surface coatings and surface morphology. Surface coatings, including but not limited to silanes, polyolefin waxes and calcium stearate, can improve the processing behavior of the filler by acting as internal or external lubricants, thereby reducing the viscosity. However, organic surface coatings may contribute to fuel loading and therefore reduce the fire performance of the filler. Functional filler coatings may interact with the functional groups of the polymer or the polymer itself to improve physical properties as well as fire performance in terms of dripping. Without being bound by theory, it is believed that spherical morphology does not increase the viscosity of the core filler composition compared to plates or flakes. Spherical structures may function as processing aids, such as certain silicon dioxides, while coarse and ground fillers may worsen processing behavior.
[0047] The halogen-free flame retardant compositions described herein may include greater than 83 wt% of filler, based on the total weight of the halogen-free flame retardant composition. In other embodiments, the halogen-free flame retardant composition may include greater than 83 wt% of filler, based on the total weight of the halogen-free flame retardant composition. In other embodiments, the halogen-free flame retardant composition may include greater than 83 wt% of filler, based on the total weight of the halogen-free flame retardant composition. %, about 85% to about 87% by weight, about 85% to about 86% by weight, about 86% to about 90% by weight, about 86% to about 89% by weight, about 86% to about 88% by weight, about 86% to about 87% by weight, about 87% to about 90% by weight, about 87% to about 89% by weight, about 87% to about 88% by weight, about 88% to about 90% by weight, about 88% to about 89% by weight, or about 89% to about 90% by weight of filler.
[0048] The halogen-free flame retardant composition described herein may include an internal inorganic lubricant. In some embodiments, the inorganic internal lubricant may include organosiloxane and amorphous silicon dioxide. Without being bound by theory, the internal inorganic lubricant may improve the dispersion of components in the halogen-free flame retardant composition, thereby allowing for better flow, higher extrusion speeds, and a smoother surface of the final product. Examples of inorganic internal lubricants include, but are not limited to, Sidistar T120U silicon dioxide supplied by Elkem Silicon Materials or Siloxane SFD-5 from Dow Chemical Company.
[0049] In one or more embodiments, the halogen-free flame retardant composition described herein may have properties that enable it to achieve a Euro Class A2 fire rating.
[0050] Additionally, the halogen-free flame retardant compositions described herein may have a fuel loading (which may also be referred to as a total calorific value (PCS)) of less than 3 MJ / kg, as measured according to EN ISO 1716, as described below in the Test Methods section of this disclosure. In other embodiments, the halogen-free flame retardant compositions described herein may have a fuel loading or total calorific value (PCS) of less than 2.5 MJ / kg, or less than 2.0, as measured according to EN ISO 1716.
[0051] Additionally, the halogen-free flame retardant compositions described herein may have a flammability rating that meets Euroclass A2 requirements when measured according to EN ISO 1182, as described below in the Test Methods section of this disclosure. The quantities used in the European classification are the temperature rise in the oven (ΔT), the mass loss of the sample (Δm), and the sustained burning time of the sample (t f To meet the requirements of Euroclass A2, the halogen-free flame retardant compositions described herein may have a ΔT (temperature) of about 50° C. or less, a Δm (mass) of about 50% or less, and a tf (burn time) of less than 20 seconds.
[0052] The halogen-free flame retardant compositions described herein may have a total heat release that meets Euro Class A2 requirements when measured according to EN ISO 13823, as described later in the Test Methods section of this disclosure. The EN ISO 13823 classification parameters are: Flame Growth Rate Index (FIGRA) (measured in W / s), Transverse Flame Spread (LFS); Total Heat Release (THR) for droplet and particle burning occurring during the first 600 seconds (s) of the test. 600s ), smoke growth rate index (SMOGRA) (m 2 / s 2 ), total smoke production (TSP 600s To meet the requirements of Euro Class A2, the halogen-free flame retardant compositions described herein have a FIGRA of about 120 W / s or less, an LFS below the edge of the test specimen, and a THS of about 7.5 MJ or less. 600s may have:
[0053] According to embodiments of the present disclosure, there is provided a composite panel comprising an embodiment of the halogen-free flame retardant composition described herein.
[0054] Referring now to the embodiment of FIG. 1, a composite panel (100) may include a first metal layer (110), a second metal layer (110), a core layer (130) disposed between the first metal layer (110) and the second metal layer (130), a first bonding layer (120) disposed between the first metal layer (110) and the core layer (110), and a second bonding layer (120) disposed between the second metal layer (110) and the core layer (130).
[0055] In embodiments, the first metal layer (100), the second metal layer (200), or both, may comprise aluminum, stainless steel, painted steel, titanium, copper, zinc, or combinations thereof. In embodiments, the first metal layer, the second metal layer, or both, may have a width of about 0.2 mm to about 0.5 mm. In other embodiments, the first metal layer, the second metal layer, or both, may have a width of about 0.2 mm to about 0.4 mm, about 0.2 mm to about 0.3 mm, about 0.3 mm to about 0.5 mm, about 0.3 mm to about 0.4 mm, or about 0.4 to about 0.5 mm.
[0056] In embodiments, the adhesive bonding layer may include one or more adhesive resins. In embodiments, the adhesive bonding layer may include MAH-grafted polyolefin homo- or interpolymers. Based on the manufacturing of the metal composite panel, the adhesive bonding layer may be co-extruded or applied by film lamination. Depending on the manufacturing process and the requirements of the final product, the adhesive bonding layer may be based on low crystalline polyolefin elastomers or have a relatively highly crystalline linear low density polyethylene structure. Depending on the requirements of fire performance, the adhesive bonding layer may be formulated with inorganic fillers or flame retardants. It is believed that various commercial embodiments are suitable for the adhesive bonding layer. For example, suitable adhesive resins that may be utilized as the first and second bonding layers may be commercially available under the trade name Bynel® from Dow Chemical Company EI du Pont de Nemours and Company, Lucalen A 2920 M from LyondellBasell, and Guangzhou Lushan New Materials Co., Ltd. in Lushan.
[0057] In one or more embodiments, the first adhesive bonding layer, the second adhesive bonding layer, or both, can have a thickness of about 20 μm to about 100 μm. In other embodiments, the first adhesive bonding layer, the second adhesive bonding layer, or both, can have a width of about 20 μm to about 90 μm, about 20 μm to about 80 μm, about 20 μm to about 60 μm, about 20 μm to about 40 μm, about 30 μm to about 100 μm, 30 μm to about 80 μm, about 30 μm to about 60 μm, about 30 μm to about 40 μm, about 40 μm to about 100 μm, about 40 μm to about 80 μm, about 40 μm to about 60 μm, about 60 μm to about 100 μm, about 60 μm to about 80 μm, or about 80 μm to about 100 μm.
[0058] In embodiments, the core layer (300) may include embodiments of the halogen-free flame retardant compositions described herein. In embodiments, the core layer may have a width of about 1 mm to about 5 mm. In other embodiments, the core layer may have a width of about 2 mm to about 4 mm, about 2 mm to about 3 mm, about 3 mm to about 5 mm, about 3 mm to about 4 mm, or about 4 mm to about 5 mm.
[0059] In embodiments, the composite panels described herein may achieve a Euroclass A2 fire resistance rating based on the properties of the core layer (130).
[0060] A method for producing an embodiment of a composite panel comprising the halogen-free flame retardant composition described herein may include extrusion of a core layer. It is believed that providing an extrudable core layer material comprising an embodiment of the halogen-free flame retardant composition described herein may enable an economical and simple process for the production of a composite panel that still meets Euroclass A2 fire rating.
[0061] In an embodiment, a composite panel may be produced by extruding an embodiment of the halogen-free flame retardant composition described herein through a flat slit die and forming the composition in a rolling press to form the core layer (130) and process the final dimensions. The core layer (130) may then be fed in-line to a lamination process or rolled for later processing. In a further embodiment, the method of producing a composite panel may include co-extruding a first bonding layer (120) and a second bonding layer (120) onto the core layer (130). In another embodiment, the method of producing a composite panel may include laminating a first bonding layer (120) and a second bonding layer (120) onto the core layer (130). In an embodiment, the method of producing a composite panel may include laminating a first metal layer (110) and a second metal layer (110) onto the first bonding layer (120) and the second bonding layer (120) in-line, thereby producing a composite panel (100).
[0062] In a further embodiment, the halogen-free flame retardant composition used in the core layer (130) may include one or more pre-compounding steps. Without being bound by theory, one or more pre-compounding steps may improve the processability and compatibility of the polyolefin system in the direct extrusion of the core layer (100). During direct extrusion, additional fillers can be fed by a side feeder into the molten pre-compound (or "pre-batch") of the halogen-free flame retardant composition, allowing more steps in the manufacture of the composite panel.
[0063] Test Method
[0064] The test methods used herein include the following:
[0065] Euroclass System Standard
[0066] The Euroclass system is a standards organization that publishes specifications, test protocols and guidelines for testing the fire resistance of building elements. In the Euroclass system, building products are classified into seven classes based on their reaction characteristics to combustion. The test methods and classification criteria for construction products (excluding flooring) are summarized in Table 1 below. [Table 1]
[0067] Non-flammability test - EN ISO 1182
[0068] The purpose of the non-combustibility test EN ISO 1182 is to identify products that cannot contribute to a fire. To carry out EN ISO 1182, a cylindrical test specimen is inserted into a vertical tube furnace with a temperature of about 750 ° C. The temperature change due to the possible combustion of the specimen is monitored by a thermocouple. The burning time of the specimen is observed visually. After the test, the mass loss of the specimen is measured.
[0069] The quantities used in the European classification are the temperature rise in the furnace (ΔT), the mass loss of the sample (Δm), and the sustained burning time of the sample (t f ).
[0070] Total Heat Release Test - EN ISO 1716
[0071] Total Calorific Value (PCS) test EN ISO 1716 is used to determine the maximum potential total heat release (MJ / kg or MJ / m2) of a product upon complete combustion. 2 In EN ISO 1716, a powdered test sample is ignited in a pressurized oxygen atmosphere in a sealed steel cylinder surrounded by a water jacket (the calorimeter bomb) and the temperature rise of the water during combustion is measured. The total calorific value can then be calculated based on the temperature rise, the mass of the sample, and a correction factor.
[0072] Single flammability test - EN 13823
[0073] The Single Burn Item (SBI) EN 13823 test can be used to simulate a single burn item. In EN 13823, the test specimen is mounted on a specimen holder with two vertical wings made of non-combustible board. The specimen holder wings, with dimensions of 1.0 m x 1.5 m and 0.5 m x 1.5 m, form a right-angled corner configuration. Depending on the final application and use of the specimen to be tested, the specimen can be tested on the board or as a stand-alone product. Heat exposure on the surface of the specimen is produced by a right-angled triangular propane gas burner placed in the bottom corner formed by the wings of the specimen. The heat output of the burner is 30 kW and the heat output is approximately 300 cm. 2 Approximately 40kW / m 2 A maximum heat exposure of 1000 psi is obtained. The burner simulates a single combustion item. Combustion gases generated during the test are collected by a hood and drawn into an exhaust duct equipped with sensors to measure temperature, light attenuation, mole fractions of O2 and CO2, as well as flow-induced pressure differences in the duct.
[0074] The performance of the specimens is evaluated over a 20-minute exposure period. During the test, the heat release rate (HRR) is measured using oxygen consumption calorimetry. The smoke production rate (SPR) is measured in the exhaust duct based on light attenuation. Falling of burning droplets or particles is visually observed during the first 600 seconds of thermal exposure to the specimen. In addition, lateral flame spread is observed to determine whether the flame front reaches the outer edge of the wing of the larger specimen at any height between 500 millimeters (mm) and 1000 mm during the test.
[0075] The classification parameters for the SBI test are flame growth rate index (FIGRA) (W / s), lateral flame spread (LFS), total heat release (THR 600s ) for smoke generation. Additional classification parameters are the Smoke Growth Rate Index (SMOGRA) (m 2 / s 2 ) and total smoke production (TSP 600s ) and is defined in terms of the burning of droplets and particles occurring during the first 600 seconds (s) of the test.
[0076] The FIGRA and SMOGRA items are calculated as follows:
number
[0077] THR 600s and TSP 600s The value of is calculated over the first 600 seconds of the test as follows:
number
[0078] Ignition Test - EN ISO 11925-2
[0079] The ignition test EN ISO 11925-2 can be used to test the direct impingement of a small flame on a specimen. In EN ISO 11925-2, a test specimen with dimensions of 250 mm x 90 mm is mounted vertically in a U-shaped specimen holder. A 20 mm high propane gas flame is applied to the specimen at a 45° angle. The point of application is either 40 mm above the bottom edge of the surface centre line (surface exposed) or in the centre of the width of the bottom edge (edge exposed). A filter paper is placed under the specimen holder and the fall of the burning piece is monitored.
[0080] Depending on the class of the product, two different flame application times and test durations are used. For Class E, the flame application time is 15 seconds and the test ends 20 seconds after the flame is removed. For Classes B, C, and D, the flame application time is 30 seconds and the maximum duration of the test is 60 seconds after the flame is removed. As previously shown in Table 1, EN ISO 11925-2 is not the test method specifically used to determine the Euroclass A2 rating, but EN ISO 11925-2 testing may be mandatory for building products that comply with the Euroclass fire rating system, including the metal composite panels disclosed herein.
[0081] The classification criteria are based on observing whether the flame spread (Fs) reaches 150 mm within 60 seconds of the application of the flame and whether the filter paper underneath the sample is ignited by the burning particles. In addition, the onset and duration of the flame and glow are observed.
[0082] Melt Index (I2)
[0083] To test the melt index (I2), the ethylene-based polymer sample is measured at 190° C. and 2.16 kg according to ASTM D1238. Values are reported in g / 10 min, which corresponds to grams dissolved per 10 minutes.
[0084] density
[0085] To test density, samples are prepared and measured according to ASTM D4703 and are expressed in grams per cubic centimeter (g / cc or g / cm 3 ) Measurements are made within one hour of pressing the sample using ASTM D792, Method B.
[0086] Working Example
[0087] The following examples are illustrative of the features of the present disclosure and are not intended to limit the scope of the present disclosure. The following experiments analyzed the performance of embodiments of the halogen-free flame retardant compositions described herein.
[0088] Materials used to prepare the examples described below included ELVAX™ 210W supplied by EI du Pont de Nemours and Company as a polymeric carrier, AFFINITY™ GA1000R supplied by The Dow Chemical Company, Midland, MI as a polymeric carrier, and FUSABOND™ P353 supplied by The Dow Chemical Company, Midland, MI as a polymeric carrier. Sidistar T120U supplied by Elkem as an amorphous silicon dioxide processing aid, Kenreact LICA38 supplied by Kenrich as a titanate based processing aid, Imerys 15 and MW-100 supplied by Imerys Carbonate are crude calcium carbonate fillers, Omyacarb10-AV supplied by Omya as a crude calcium carbonate filler, Omyamaxx supplied by Omya as a coated calcium carbonate filler, Hidromag Q3005 supplied by Chimica del Rey as a magnesium hydroxide flame retardant and filler, ADEKA FLAMESTAB FS2200S supplied by Adeka as a phosphate based flame retardant, Martinal ON313 supplied by Huber Martinswerke as an aluminum trihydrate filler, and Martinal ON107LEO supplied by Huber Martinswerke as an aluminum trihydrate with processing aid.
[0089] Example 1 - Preparation of Samples 1 to 12
[0090] Samples 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, and 12 were prepared as follows.
[0091] First, masterbatches of polymer carrier and filler were pre-compounded to produce compounds A, B, C, D, E, F, and G. Compounds A through G were prepared using the amounts of materials listed in Table 2. [Table 2]
[0092] The materials were combined in the amounts shown in Table 2 to produce pre-batch samples Compounds A-G using a Buss PR 46 co-kneader, with processing conditions shown in Table 3. [Table 3]
[0093] Pre-batch sample compounds A-G from step 1 were then directly extruded in a 25 mm, 42 L / D co-rotating twin screw extruder. Additional filler was side fed into the molten pre-batch sample compounds A-G from compounding step 1 to increase the filler content according to the amounts provided in Table 4 below. Table 5 shows the final formulations of Samples 1-14 used as the extrudable core layer. [Table 4] [Table 5]
[0094] As shown in Tables 2, 4 and 5, Sample 1 contains a blend of ethylene-vinyl acetate copolymer and maleic anhydride-grafted polyethylene with 86.6 wt% filler, Sample 2 contains a blend of ethylene-vinyl acetate copolymer and maleic anhydride-grafted polyethylene with 84.6 wt% filler, Sample 3 contains only ethylene-vinyl acetate copolymer with 87 wt% filler, Sample 4 contains only ethylene-vinyl acetate copolymer with 87 wt% filler, and Sample 5 contains only ethylene-vinyl acetate copolymer and maleic anhydride-grafted polyethylene with 85.2 wt% filler. Sample 1 contained a blend of ethylene-vinyl acetate copolymer and maleic anhydride grafted polyethylene and 87 weight percent filler, Sample 7 contained maleic anhydride grafted polyethylene and 87.5 weight percent filler, Sample 8 contained only maleic anhydride-grafted polyethylene and 87.7 weight percent filler, Sample 11 contained a blend of ethylene-vinyl acetate copolymer and maleic anhydride grafted polyethylene and greater than 84.6 weight percent filler, and Sample 12 contained a blend of ethylene-vinyl acetate copolymer, maleic anhydride-grafted polyethylene and maleic anhydride grafted polypropylene and 84.5 weight percent filler.
[0095] Comparative sample 6 contained only maleic anhydride grafted polyethylene and 77.5 wt.% filler, comparative sample 9 contained a blend of ethylene-vinyl acetate copolymer and maleic anhydride grafted polyethylene and 82.8 wt.% filler, and comparative sample 10 contained a blend of ethylene-vinyl acetate copolymer and maleic anhydride grafted polyethylene and 78.9 wt.% filler.
[0096] Final samples 1-12 were extruded through a 300 mm flat slit die in a 25 mm co-rotating twin screw extruder and fed into a three-roll calendering apparatus to form 1 mm thick core layer sample sheets. Table 6 lists the processing conditions for direct extrusion of the final formulations listed in Table 5. [Table 6]
[0097] Example 2 - TGA analysis to determine resulting filler concentration
[0098] Thermogravimetric analysis (TGA) of the samples was performed according to ASTM E1131 to verify the final inorganic filler content of sample sheets 1-3, 9, and 10. Based on the TGA results, the filler loading of sample sheets 1-3 was 83 wt% or greater, while the filler loading of sheets 9 and 10 was less than 83 wt%. These results are shown in Table 7 below. [Table 7]
[0099] Example 3: Total Heat Release Test - EN ISO 1716
[0100] Sample sheets 2, 3, 9, and 10 were evaluated according to EN ISO 1716. To evaluate the samples, three tests were performed for each sample and the average of the three tests is reported in Table 8. [Table 8]
[0101] As shown in Table 8, the results showed low total heat values of 2.81 for Sample 2 (83% filler loading) and 2.51 MJ / kg for Sample 3 (87% filler loading), both of which passed the Euroclass A2 fire rating requirement with a requirement of less than 3 MJ / kg. Comparative Sample Sheets 9 and 10, each with an inorganic filler loading of less than 83% by weight (81% and 80% by weight, respectively), had total heat values of less than 3 MJ / kg and did not pass the Euroclass A2 fire rating requirement.
[0102] It will be apparent that modifications and variations are possible without departing from the scope of the present disclosure, as defined in the appended claims. More specifically, certain aspects of the present disclosure are Although identified herein as preferred or particularly advantageous, it is not intended that the present disclosure be necessarily limited to those aspects. The present application also relates to the following aspects: (1) one or more polyolefin copolymers having a melt flow index, measured at 190° C. and 2.16 kg, of 350 grams per 10 minutes (g / 10 min) to 1000 g / 10 min, the one or more polyolefin copolymers comprising one or more of a maleic anhydride grafted polyolefin and an ethylene-vinyl acetate copolymer; and A halogen-free flame retardant composition comprising at least 83 wt. % of an inorganic filler, based on the total weight of the halogen-free flame retardant composition. (2) The halogen-free flame retardant composition according to (1) above, wherein the halogen-free flame retardant composition comprises less than 17% by weight of one or more polyolefin copolymers. (3) The halogen-free flame retardant composition according to (1), wherein the halogen-free flame retardant composition comprises at least 85% by weight of an inorganic filler based on the total weight of the halogen-free flame retardant composition. (4) The halogen-free flame-retardant composition according to any one of (1) to (3), wherein the one or more ethylene copolymers include an ethylene-vinyl acetate copolymer. (5) The halogen-free flame-retardant composition according to any one of (1) to (4), wherein the composition has a fuel load of less than 3 MJ / kg when measured according to ENISO 1716. (6) the composition has an oven temperature rise of about 50° C. or less, a sample mass loss of about 50% or less, and a sustained burn time of the sample of about 20 seconds, when measured according to EN ISO 1182; The halogen-free flame-retardant composition according to any one of (1) to (5) above. (7) The halogen-free flame-retardant composition according to any one of (1) to (6), wherein the total weight of the inorganic filler comprises a majority of anhydrous inorganic filler. (8) The halogen-free flame-retardant composition according to any one of (1) to (7) above, further comprising an internal inorganic lubricant. (9) The halogen-free flame-retardant composition according to any one of (1) to (8), wherein the maleic anhydride-grafted polyolefin is a maleic anhydride-grafted elastomer having a Brookfield viscosity of more than 8,000 cP when measured at 177°C. (10) a first metal layer; A second metal layer; a core layer disposed between the first metal layer and the second metal layer; a first tie layer disposed between the first metal layer and the core layer; and a second bonding layer disposed between the second metal layer and the core layer, The core layer is made of the halogen-free flame-retardant composition according to any one of (1) to (9). Includes composite panels. (11) The composite panel of (9) above, wherein the first metal layer, the second metal layer, or both, comprise aluminum. (12) The composite panel according to (9) or (10), wherein the core layer has a thickness of 1 mm to 5 mm. (13) The composite panel according to any one of (9) to (11), wherein the composite panel has a Euro Class A2 fire resistance rating. (14) A method for producing the composite panel according to any one of (9) to (12), extruding a core layer; applying first and second tie layers to opposing sides of the core layer; and applying to said bonding layer and then laminating first and second metal layers onto the first and second bonding layers, respectively, to produce said composite panel. (15) The method according to (13) above, wherein the first and second bonding layers are applied by coextrusion or lamination.
Claims
1. one or more polyolefin copolymers having a melt flow index of 350 grams per 10 minutes (g / 10 min) to 1000 g / 10 min, measured at 190° C. and 2.16 kg, said one or more polyolefin copolymers comprising a maleic anhydride grafted polyolefin; and A halogen-free flame retardant composition comprising at least 83 wt. % of an inorganic filler, based on a total weight of the halogen-free flame retardant composition, said inorganic filler comprising CaCO 3 .
2. 10. The halogen-free flame retardant composition of claim 1, wherein the halogen-free flame retardant composition comprises less than 17 wt% of one or more polyolefin copolymers.
3. 2. The halogen-free flame retardant composition of claim 1, wherein the halogen-free flame retardant composition comprises at least 85 wt. % of inorganic filler, based on the total weight of the halogen-free flame retardant composition.
4. The halogen-free flame retardant composition according to any one of claims 1 to 3, wherein the one or more polyolefin copolymers further comprise an ethylene-vinyl acetate copolymer.
5. The halogen-free flame retardant composition according to any one of claims 1 to 4, wherein the composition has a fuel loading of less than 3 MJ / kg, as measured according to EN ISO 1716.
6. The composition has an oven temperature rise of about 50° C. or less, a sample mass loss of about 50% or less, and a sample sustained burn time of about 20 seconds, when measured according to EN ISO 1182. The halogen-free flame retardant composition according to any one of claims 1 to 5.
7. The halogen-free flame-retardant composition of any one of claims 1 to 6, wherein the inorganic filler further comprises at least one compound selected from the group consisting of BaSO4, CaSO4, silicates, talc, kaolin, clay, mica, aluminum trihydrate, aluminum oxide, magnesium hydroxide, huntite, boehmite, and combinations thereof.
8. The halogen-free flame retardant composition of any one of claims 1 to 7, further comprising an internal inorganic lubricant.
9. The halogen-free flame retardant composition according to any one of claims 1 to 8, wherein the maleic anhydride grafted polyolefin is a maleic anhydride grafted elastomer having a Brookfield viscosity of more than 8,000 cP when measured at 177°C.
10. A first metal layer; A second metal layer; a core layer disposed between the first metal layer and the second metal layer; a first tie layer disposed between the first metal layer and the core layer; and a second bonding layer disposed between the second metal layer and the core layer, The core layer comprises the halogen-free flame-retardant composition according to any one of claims 1 to 9. Includes composite panels.
11. The composite panel of claim 10 , wherein the first metal layer, the second metal layer, or both, comprise aluminum.
12. A composite panel according to claim 10 or 11, wherein the core layer has a thickness of from 1 mm to 5 mm.
13. 13. The composite panel according to any one of claims 10 to 12, wherein the composite panel is Euroclass A2 fire rated.
14. A method for producing a composite panel according to any one of claims 10 to 12, comprising the steps of: extruding a core layer; applying first and second tie layers to opposing sides of the core layer; and subsequently laminating first and second metal layers onto the first and second bonding layers, respectively, to produce the composite panel.
15. The method of claim 14 , wherein the first and second tie layers are applied by coextrusion or lamination.
Citation Information
Patent Citations
Halogen-free flame-retardant polymer sandwich layer material for fireproofing plastic-aluminum plate and preparation thereof
CN101463160A
Filled polyethylene composition
JP2001513833A
Resin composition for forming external water-tight filling material of flame-retardant water-tight cable and manufacturing method of flame-retardant water-tight cable using the same
JP2019059846A
Flame retardant metal-resin composite material
WO2019159929A1