Positive Electrode and Electrochemical Device
By controlling the morphology and orientation of lithium-transition metal composite oxide particles on the current collector with a specific Dp/Dv ratio, the positive electrode's cycle performance is improved, addressing issues of pulverization and cracking.
Patent Information
- Application Number
- JP2023513778
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-12-24
- Publication Date
- 2024-10-04
- Estimated Expiration
- 2040-12-24
AI Technical Summary
Current positive electrodes in lithium-ion secondary batteries face challenges in improving cycle performance due to issues such as pulverization and cracking of lithium-transition metal composite oxide particles, which are exacerbated by uneven distribution and orientation on the current collector.
Control the morphology and orientation of lithium-transition metal composite oxide particles on the current collector by maintaining a specific ratio of average particle diameters (Dp/Dv) between 1.1 to 2.3, ensuring dominant and non-dominant crystal planes are appropriately distributed, and adjusting parameters like cold rolling pressure and direction to achieve uniform distribution.
This approach enhances the positive electrode's high-pressure cycling performance by preventing pulverization and cracking, maintaining stability and electrochemical performance.
Smart Images

Figure 0007561973000004 
Figure 0007561973000005 
Figure 0007561973000006
Abstract
Description
[Technical field]
[0001] This application relates to the field of battery technology, and in particular to positive electrodes and electrochemical devices. [Background technology]
[0002] With the development of new energy technology and the progress of research on energy storage materials, secondary batteries such as lithium ion batteries are widely used. The market requirements for the performance of secondary batteries are also becoming stricter. The positive electrode is an important factor that affects the performance of secondary batteries, and the shape of the lithium transition metal composite oxide has an important effect on the capacity and stability of the positive electrode.
[0003] Therefore, there is room for improvement in current positive electrodes and secondary batteries. Summary of the Invention
[0004] The present application aims to solve at least some of the technical problems in the related art, and to provide a positive electrode that can improve the lithium ion release ability of the lithium transition metal composite oxide on the side in contact with the electrolyte, improve the positive electrode stability, and reduce problems such as powdering due to phase transition of particles, by controlling the morphology of the lithium transition metal composite oxide and the orientation state of the lithium transition metal composite oxide on the surface of a current collector.
[0005] In one aspect of the present application, the present application provides a positive electrode including a positive electrode active material layer located on a current collector, the positive electrode active material layer including a lithium transition metal composite oxide, where Dp is an average particle size of the lithium transition metal composite oxide in a direction parallel to the plane on which the current collector is located, and Dv is an average particle size of the lithium transition metal composite oxide in a direction perpendicular to the plane on which the current collector is located, and the relationship 1.1≦Dp / Dv≦2.3 is satisfied. The present inventors have found that by controlling the shape of the lithium transition metal composite oxide particles and controlling the distribution orientation of the lithium transition metal composite oxide on the surface of the current collector, problems such as powdering of the positive electrode caused by phase transition or cracking of the lithium transition metal composite oxide during use (charge and discharge) can be alleviated, and the positive electrode has good high-pressure cycle performance.
[0006] According to some embodiments of the present application, the lithium transition metal composite oxide satisfies 5 μm≦Dp≦25 μm, so that the lithium transition metal composite oxide has good orientation on the current collector, and the dominant and non-dominant crystal planes of the particles are more rationally arranged, so that the positive electrode has good high-pressure cycle performance.
[0007] According to some embodiments of the present application, the lithium transition metal composite oxide has a temperature coefficient of 0.8≦(Dp+Dv) / 2D N50 ≦1.25, D N50 is the median diameter of the lithium transition metal composite oxide.
[0008] According to some embodiments of the present application, the lithium transition metal complex oxide has an R-3m space group structure.
[0009] According to some embodiments of the present application, the lithium transition metal composite oxide is Li x1 Ni y1 Co z1 Mn k Z q O b-a T acomprising, Z comprises at least one selected from the group consisting of B, Mg, Al, Si, P, S, Ti, Cr, Fe, Cu, Zn, Ga, Y, Zr, Mo, Ag, W, In, Sn, Pb, Sb and Ce, T is a halogen, and x1, y1, z1, k, q, a and b satisfy 0.2 < x1 ≤ 1.2, 0 ≤ y1 ≤ 1, 0 ≤ z1 ≤ 1, 0 ≤ k ≤ 1, 0 ≤ q ≤ 1, 1 ≤ b ≤ 2 and 0 ≤ a ≤ 1, respectively.
[0010] According to some embodiments of the present application, the lithium transition metal composite oxide has a P63mc space group structure.
[0011] According to some embodiments of the present application, the lithium transition metal composite oxide is Li x2 Na z2 Co 1-y2 M y2 O 2±n X n comprising, 0.6 < x2 < 0.95, 0 ≤ y2 < 0.15, 0 ≤ z2 < 0.03, 0 ≤ n ≤ 0.2, M comprises at least one selected from the group consisting of Al, Mg, Ti, Mn, Fe, Ni, Zn, Cu, Nb, Cr and Zr, and X is a halogen.
[0012] According to some embodiments of the present application, when the electrochemical device including the positive electrode is charged to a voltage of 4.6V, the positive electrode has at least a characteristic peak P1 and a characteristic peak P2 in the range of 17° to 20° in the X-ray diffraction spectrum, and satisfies that the peak intensity I1 of P1 is greater than the peak intensity I2 of P2.
[0013] According to some embodiments of the present application, when the electrochemical device including the positive electrode is discharged to a voltage of 3.0V, the positive electrode satisfies having a characteristic peak P3 in the range of 17° to 20° in the X-ray diffraction spectrum. The peak intensity I3 of P3 satisfies (I1 - I2) ≤ I3 ≤ (I1 + I2). Thereby, the positive electrode can have better cycle stability.
[0014] According to some embodiments of the present application, the ratio I1 / I3 of the peak intensity I1 of P1 to the peak intensity I3 of P3 is 0.8 or more, which allows the lithium transition metal composite oxide in the positive electrode to maintain good crystallinity during cycling.
[0015] According to some embodiments of the present application, the lithium transition metal composite oxide has a long axis average particle diameter D1 and a short axis average particle diameter D2, and the long axis average particle diameter D1 and the short axis average particle diameter D2 satisfy 1.4≦(D1 / D2)≦5.5. According to some embodiments of the present application, the lithium transition metal composite oxide has a long axis average particle diameter D1 and a short axis average particle diameter D2, and the long axis average particle diameter D1 and the short axis average particle diameter D2 satisfy 1.4≦(D1 / D2)≦3.8. As a result, the lithium transition metal composite oxide has a good particle morphology and an appropriate ratio of active crystal faces to inactive crystal faces.
[0016] According to some embodiments of the present application, 7 μm≦D1≦28 μm.
[0017] According to some embodiments of the present application, the positive electrode satisfies the following conditions: when an electrochemical device including the positive electrode is charged and discharged 8 times in a range of 3.0 V to 4.6 V, and discharged to a voltage of 3.0 V, the peak position shift of the highest peak in the X-ray diffraction spectrum of the positive electrode after the cycle is 0.1° or less compared to the positive electrode before the cycle, and the rate of change in the half-width of the highest peak is less than 5%. As a result, the positive electrode particles have good cycle performance.
[0018] In another aspect, the present application provides an electrochemical device comprising the positive electrode described above, a negative electrode, and a separator, such that the secondary battery has all the features and advantages of the positive electrode described above, which are not described here.
[0019] According to some embodiments of the present application, the negative electrode has stripes on its surface when discharged to a voltage of 3.0V.
[0020] In another aspect of the present application, the present application provides a method for preparing the above-mentioned positive electrode, the method comprising: providing a lithium transition metal composite oxide, mixing the lithium transition metal composite oxide with a conductive agent and a binder to form a positive electrode slurry, coating the positive electrode slurry on a surface of a current collector, and cold rolling the current collector with the positive electrode slurry, the cold rolling being performed under a pressure of 30-40 tons, a cold rolling speed being 3-4 meters / minute, and a pressed density of 4.05-4.25 g / cm. 3 This makes it possible to easily obtain the above-mentioned positive electrode and to provide the positive electrode with good cycle performance.
[0021] According to some examples of the present application, the weight ratio of the lithium transition metal composite oxide, the conductive agent, and the binder in the positive electrode slurry is (94-99):(0.5-3):(0.5-3). This makes it possible to obtain a positive electrode slurry having an appropriate blending ratio of the conductive agent, the lithium transition metal composite oxide, and the binder.
[0022] According to some embodiments of the present application, the method further includes drying the positive electrode slurry on the surface of the current collector after applying the positive electrode slurry to the surface of the current collector and before performing the cold rolling treatment, and further includes chopping the current collector after performing the cold rolling treatment.
[0023] In another aspect of the present application, the present application provides a method for modifying an anode, the method comprising spreading an additive on a surface of an anode active material layer and performing a roll press treatment, the additive comprising at least one selected from the group consisting of lithium powder, lithium ribbon, and a lithium-containing compound. [Brief description of the drawings]
[0024] [Figure 1] FIG. 1 is a schematic diagram showing the structure of a positive electrode in one embodiment of the present application. [Diagram 2] FIG. 2 is a structural schematic diagram of an electrochemical device according to one embodiment of the present application. [Diagram 3]FIG. 3 is a schematic flow diagram of a method for preparing a positive electrode in one embodiment of the present application. [Figure 4] FIG. 4 is a scanning electron microscope photograph of the positive electrode in Example 1 of the present application. [Diagram 5] FIG. 5 is an X-ray diffraction spectrum of the positive electrode in Example 1 of the present application. [Figure 6] FIG. 6 is an X-ray diffraction spectrum of the positive electrode in Comparative Example 1 of the present application. [Figure 7] FIG. 7 is an optical photograph of the negative electrode in Example 1 of the present application. [Figure 8] FIG. 8 is an optical photograph of the negative electrode in Comparative Example 1 of the present application. [Figure 9] FIG. 9 is a graph showing the measurement results of cycle performance in Example 1 and Comparative Example 1 of the present application. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0025] The following describes the examples of the present application in detail. The examples described below are illustrative and are used only to interpret the present application, but cannot be understood as limiting the present application. If no specific techniques or conditions are specified in the examples, they are performed according to the techniques or conditions described in the literature in the field or according to the product specifications. If no manufacturer is specified, the reagents or equipment used are all commercially available general products.
[0026] The present application has been completed based on the following findings and research by the inventors.
[0027] Current positive electrodes, for example, positive electrodes of lithium ion secondary batteries, can achieve control over the performance of the positive electrode by controlling the size and morphology of the particles of the active Li-containing material in the lithium transition metal composite oxide. However, current positive electrodes still have a problem in improving cycle performance. The present inventor has found that in addition to the morphological characteristics of the lithium transition metal composite oxide itself, the orientation of the lithium transition metal composite oxide in the current collector also affects the performance of the positive electrode. In particular, lithium transition metal composite oxides are not usually perfectly symmetrical spherical particles, and the shape of the positive electrode material is limited to the growth control of its crystal faces, with the dominant crystal faces in the particles growing faster and the other crystal faces growing slower. Therefore, lithium transition metal composite oxides are in most cases ellipsoidal rather than perfectly spherical. When control is exercised over the synthesis conditions, the proportion of crystal faces of the obtained lithium transition metal composite oxide also changes. For example, if there are too many dominant crystal faces in the lithium transition metal composite oxide, the long side of the ellipsoid sphere of the obtained lithium transition metal composite oxide is much larger than the short side. By controlling the reduction of the proportion of the dominant crystal plane and the increase of the other crystal planes, particles close to spherical shape can be obtained. For cobalt-based materials such as lithium cobalt oxide, the dominant crystal plane cannot release lithium but is very stable, and the crystal plane with the largest proportion in the non-dominant crystal plane, for example the 104 crystal plane, can release lithium but is not stable and prone to phase transition. For this reason, if there are too many dominant crystal planes, the lithium release of the material will be affected and the shape will be too flat and difficult to process. Conversely, if there are too many non-dominant crystal planes, the particle surface will be unstable and prone to phase transition, resulting in failure. When forming a positive electrode, generally, a lithium transition metal composite oxide is mixed with conductive particles and components such as a binder as a slurry, and then the slurry is applied to the surface of a positive electrode current collector, and after a series of processes such as drying and cold rolling, the lithium transition metal composite oxide is distributed on the current collector surface with a certain orientation.
[0028] Since the lithium transition metal composite oxide is not a symmetric particle, the performance of the lithium transition metal composite oxide cannot be fully exhibited unless the orientation of the lithium transition metal composite oxide distributed on the current collector is controlled. For example, if the dominant crystal face is exposed too much on the side of the current collector facing the electrolyte, the stability of the positive electrode is good, but the distance between the non-dominant crystal face and the electrolyte is large, so that the lithium release performance of the positive electrode is affected. On the other hand, if the non-dominant crystal face is exposed too much on the side of the current collector facing the electrolyte, the stability of the positive electrode is poor and the positive electrode material is easily powdered. In addition, the lithium transition metal composite oxide is damaged during processing, is unevenly distributed on the surface of the positive electrode current collector, or has a disturbed orientation, which is disadvantageous to the electrochemical performance of the lithium transition metal composite oxide.
[0029] In view of this, in one embodiment of the present application, the present application provides a positive electrode. Referring to FIG. 1, the positive electrode 100 includes a current collector 110 and an active material layer 120, the active material layer 120 being located on the current collector 110, and the active material layer 120 includes a lithium transition metal composite oxide 120A, a lithium transition metal composite oxide 120B, and a lithium transition metal composite oxide 120C. The ratio Dp / Dv of the average particle diameter Dp of the lithium transition metal composite oxides 120A, 120B, and 120C in a direction parallel to the plane on which the current collector 110 is located (the A-A' direction shown in the figure) to the average particle diameter Dv in a direction perpendicular to the plane on which the current collector 110 is located (the B-B' direction shown in the figure) satisfies 1.1≦Dp / Dv≦2.3. The inventors have found that the positive electrode has good high-pressure cycle performance, and that by controlling the shape of the lithium transition metal composite oxide particles and controlling the orientation of their distribution on the surface of the current collector, problems such as powdering of the positive electrode due to phase transition and cracking of the lithium transition metal composite oxide during use (charging and discharging) can be alleviated.
[0030] As described above, the lithium transition metal composite oxide is distributed on the current collector in a certain orientation, and the ratio of Dp and Dv of the lithium transition metal composite oxide can be controlled to more appropriately grasp the state in which the lithium transition metal composite oxide is distributed on the surface of the current collector. This allows the electrochemical performance of the lithium transition metal composite oxide to be fully reflected in the positive electrode. Specifically, for ellipsoidal or flat particles, when most of the lithium transition metal composite oxides are distributed so that the diameter of the long axis of the particles is parallel to the plane on which the current collector 110 is located (120B shown in FIG. 1), the inactive surface faces the battery negative electrode, and at this time, the lithium migration path increases, and the stability of the particles in this state is good and they are not easily powdered. When most of the lithium transition metal composite oxides are distributed so that the diameter of the long axis of the particles is perpendicular to the plane on which the current collector 110 is located, as shown in 120A in the figure, at this time, the active surface faces the battery negative electrode, and the particles are easily damaged during processing, which affects the performance of the positive electrode. By controlling the particle morphology of the lithium transition metal composite oxide itself and adjusting parameters during processing, including but not limited to the cold rolling pressure and pressure direction, it is possible to ensure that the ratio of Dp to Dv is within a certain range. In other words, the lithium transition metal composite oxide at this time has a sufficient non-dominant crystal face facing the battery negative electrode, so that the positive electrode has good electrochemical performance and there is no deterioration in cycle performance due to excessive exposure of the dominant crystal face to the electrolyte side.
[0031] According to some embodiments of the present application, when Dp / Dv is in the range of 1.1 to 2.3, the positive electrode material particles are uniformly distributed on the current collector 110. When Dp / Dv is in the range of 1.1 to 2.3, the active and inactive surfaces of the lithium transition metal composite oxide in the direction facing the battery negative electrode are in a reasonable range, and can be maintained even after processing. When Dp / Dv is smaller than 1.1, the inactive crystal surface of the positive electrode facing the battery negative electrode is too small, and the lithium transition metal composite oxide is easily damaged and powdered. When Dp / Dv is larger than 2.3, the lithium transition metal composite oxide on the positive electrode surface is too flat or overpressurized, which affects the electrochemical performance of the positive electrode.
[0032] In this application, unless otherwise specified, the average particle size is the average diameter of the particles. The average diameter can be measured as follows. A randomly selected portion of the positive electrode is processed with a microtome to obtain a cross section. The diameters of the particles in the cross section are measured and recorded in parallel and perpendicular directions. The diameter is the maximum length of the particle in the defined direction. In the statistical method, particles are selected in order from left to right and from top to bottom, and the statistical number of the average particle size is 100 particles. Dp of the inclined lithium transition metal composite oxide 120C shown in FIG. 1 is the maximum length of the particle along the A-A' direction in the cross section of the positive electrode (viewing angle shown in FIG. 1), and Dv of the lithium transition metal composite oxide 120C is the maximum length of the particle along the B-B' direction.
[0033] According to some embodiments of the present application, the lithium transition metal composite oxide has a long axis average particle diameter D1 and a short axis average particle diameter D2, and the long axis average particle diameter D1 and the short axis average particle diameter D2 satisfy 1.4≦(D1 / D2)≦5.5. According to some embodiments of the present application, the long axis average particle diameter D1 and the short axis average particle diameter D2 satisfy 1.4≦(D1 / D2)≦3.8. As a result, the lithium transition metal composite oxide has a good particle morphology and an appropriate ratio of active crystal faces to inactive crystal faces.
[0034] According to some embodiments of the present application, the long axis average particle diameter D1 satisfies 7 μm≦D1≦28 μm, so that the lithium transition metal composite oxide has a good particle morphology and an appropriate ratio of active crystal faces to inactive crystal faces.
[0035] According to some embodiments of the present application, the above-mentioned lithium transition metal composite oxide further satisfies 5 μm≦Dp≦25 μm, which allows the lithium transition metal composite oxide to have good orientation on the current collector and more rationally arrange the dominant and non-dominant crystal planes in the particles, thereby making the positive electrode have good high-pressure cycle performance.
[0036] According to some embodiments of the present application, the lithium transition metal composite oxide further has a ratio of 0.8≦(Dp+Dv) / 2D N50 ≦1.25, where D N50 is the median diameter of the lithium transition metal composite oxide. Those skilled in the art will understand that the particle size of a typical cobalt-based positive electrode material is not completely uniform, and the lithium transition metal composite oxide in the positive electrode may be large particles, small particles, or a mixture of large and small particles. However, the particle size may be within a certain range. N50 is the average particle size of the medium-sized particles. N50 From the relationship, it can be determined whether the lithium transition metal composite oxide retains the designed particle shape characteristics during processing. Specifically, the value of Dp + Dv is 2D N50 If the diameter is much larger or smaller than (Dp+Dv) / 2D, the particles may be damaged during processing, or the lithium transition metal composite oxide may be unevenly distributed on the surface of the current collector, or the orientation may be disturbed. All of these are detrimental to the electrochemical performance. N50 When the ratio is 0.8 to 1.25, it is ensured that the lithium transition metal composite oxide is not damaged during processing or is not damaged to such an extent that it seriously affects the performance of the obtained positive electrode, and the lithium transition metal composite oxide can be distributed relatively uniformly on the surface of the current collector with a certain orientation.
[0037] According to some embodiments of the present application, the specific chemical composition and structure of the lithium transition metal composite oxide are not particularly limited, and can be selected by those skilled in the art according to the actual battery performance needs. For example, according to some embodiments of the present application, the lithium transition metal composite oxide has an R-3m space group structure. According to some embodiments of the present application, the chemical composition of the lithium transition metal composite oxide is Li x1 Ni y1 Co z1 Mn k Z q O b-a T awherein Z contains at least one selected from the group consisting of B, Mg, Al, Si, P, S, Ti, Cr, Fe, Cu, Zn, Ga, Y, Zr, Mo, Ag, W, In, Sn, Pb, Sb and Ce; T is a halogen; and x1, y1, z1, k, q, a and b may respectively satisfy 0.2 < x1 ≦ 1.2, 0 ≦ y1 ≦ 1, 0 ≦ z1 ≦ 1, 0 ≦ k ≦ 1, 0 ≦ q ≦ 1, 1 ≦ b ≦ 2 and 0 ≦ a ≦ 1. According to some embodiments of the present application, the lithium transition metal composite oxide has a P63mc space group structure. According to some embodiments of the present application, the chemical composition of the lithium transition metal composite oxide is Li x2 Na z2 Co 1-y2 My2O 2±n X n where 0.6 < x2 < 0.95, 0 ≦ y2 < 0.15, 0 ≦ z2 < 0.03, 0 ≦ n ≦ 0.2; M contains at least one selected from the group consisting of Al, Mg, Ti, Mn, Fe, Ni, Zn, Cu, Nb, Cr and Zr; for example, the type of element of M may be one, two, or three or more. When multiple M elements are included, y is the sum of the atomic ratios of the multiple M elements. More specifically, Li x2 Na z2 Co 1-y2 M y2 O 2±n X n wherein x may satisfy 0.6 < x < 0.85.
[0038] According to some embodiments of the present application, when an electrochemical device including the positive electrode is discharged to a voltage of 3.0 V, the X-ray diffraction spectrum of the lithium transition metal composite oxide has a characteristic peak P3 in the range of 17° to 20°. In addition, when an electrochemical device including the positive electrode is charged to a voltage of 4.6 V, the lithium transition metal composite oxide exhibits two phases, the lithium content in the two phases is different, and the proportion of the part with a low lithium content is large. That is, when a cell including the positive electrode is charged to a voltage of 4.6 V, the X-ray diffraction spectrum has at least a characteristic peak P1 and a characteristic peak P2 in the range of 17° to 20°, and the peak intensity I1 of the P1 is greater than the peak intensity I2 of the P2. As described above, crystallinity determines the performance of a material, and the better the crystallinity, the less likely the material is to be powdered and the better the cycle stability. Specifically, the ratio I1 / I3 of the peak intensity I1 of P1 to the peak intensity I3 of P3 is 0.8 or more. That is, the crystallinity is reflected in the peak intensity I1 being in a range close to the initial peak intensity I3. For example, when the peak intensity I1 is smaller than 0.8 times the peak intensity I3, it indicates that the deterioration of the crystallinity of the material becomes more significant. When the lithium transition metal composite oxide is discharged to 3.0V, it returns to the initial state, and when cracks occur in the material due to distortion at this time, I3 is lower than I1-I2. However, when the peak intensity in the initial state exceeds I1+I2, it indicates that there is a risk of pulverization at high voltage. Specifically, pulverization is a process in which the crystallinity of the lithium transition metal composite oxide is reduced, such as cracking, decomposition, and phase transition. Therefore, by satisfying (I1-I2)≦I3≦(I1+I2), the peak intensity I3 of P3 can have good crystallinity and good cycle performance in the positive electrode.
[0039] According to some embodiments of the present application, after the electrochemical device is fully charged and discharged to 3.0V, the surface of the negative electrode has stripes parallel to the fold direction. The stripes are derived from traces left by additives added to the negative electrode after they are consumed. This allows the lithium transition metal composite oxide in the positive electrode, together with the structure of the negative electrode (e.g., additives), to make the positive electrode have a more stable cycle performance. Furthermore, the positive electrode can maintain the structural stability of the positive electrode active material in the charge and discharge states during its application. That is, there is little change in the crystal structure of the material, and I1, I2, and I3 are more stable. In addition, after it is fully discharged to the initial state, both the shift and broadening of the I3 peak are small. In general, the shift of the characteristic peak in XRD indicates the loss of active lithium, and the broadening indicates the pulverization of the material.
[0040] The positive electrode exemplified in the present application satisfies the following requirements: when an electrochemical device including the positive electrode is charged and discharged 10 times in a voltage range of 3.0 V to 4.6 V, the shift in the peak position of the highest peak in the X-ray diffraction spectrum is 0.1° or less, and the rate of change in the half-width of the highest peak is less than 5% when the device is discharged to a voltage of 3.0 V. This proves that the positive electrode provided by the present application has good stability, and the loss of active lithium in the material and the powdering of the positive electrode active material (lithium transition metal composite oxide) during use are both small.
[0041] In another aspect of the present application, the present application provides an electrochemical device. Referring to FIG. 2, the electrochemical device 1000 includes a positive electrode 100, a separator 200, and a negative electrode 300. The positive electrode 100 is as described above, and the separator 200 separates the positive electrode 100 and the negative electrode 300. As a result, the electrochemical device has all the features and advantages of the positive electrode described above, and the description thereof will be omitted here. In any case, the electrochemical device has good cycle performance and capacity.
[0042] It is understood by those skilled in the art that, in order to achieve the function of the electrochemical device, the electrochemical device can further include an electrolyte. The specific shape of the electrochemical device is not particularly limited, and can be selected and designed by those skilled in the art according to actual needs.
[0043] In another aspect of the present application, the present application provides a method for preparing the above-mentioned positive electrode. With reference to FIG. 3, the method may include the following steps:
[0044] S100: Providing a positive electrode material and forming a positive electrode slurry
[0045] According to some embodiments of the present application, the step may include providing a lithium transition metal composite oxide and forming a positive electrode slurry. Specifically, the above-mentioned lithium transition metal composite oxide, a conductive agent, and a binder may be mixed to form a positive electrode slurry.
[0046] According to some embodiments of the present application, the weight ratio of the lithium transition metal composite oxide, the conductive agent, and the binder in the positive electrode slurry may be (94-99):(0.5-3):(0.5-3). This allows a positive electrode slurry having an appropriate blend ratio of the conductive agent, the lithium transition metal composite oxide, and the binder to be obtained. For example, specifically, the weight ratio of the lithium transition metal composite oxide, the conductive agent, and the binder in the positive electrode slurry may be 97:1.4:1.6.
[0047] The composition and form of the lithium transition metal composite oxide have been described in detail above, so the description will be omitted here. Those skilled in the art can select an appropriate lithium transition metal composite oxide according to the specific performance demands of the positive electrode. The specific type of the conductive agent is not particularly limited, and may be, for example, conductive carbon black, graphene, etc. The binder may be, but is not limited to, polyvinylidene fluoride, etc.
[0048] S200: Applying the positive electrode slurry to a surface of a current collector.
[0049] According to some embodiments of the present application, in this step, the positive electrode slurry formed in advance may be applied to the surface of the current collector. The specific parameters and manner of applying the positive electrode slurry are not particularly limited as long as the positive electrode slurry can be uniformly applied to one side of the current collector.
[0050] S300: performing a cold rolling process on the current collector having the positive electrode slurry.
[0051] According to some embodiments of the present application, in this step, the current collector having the positive electrode slurry is subjected to a cold rolling treatment. Specifically, the cold rolling treatment is performed under a pressure of 30 to 40 tons, the cold rolling speed is 3 to 4 meters / min, and the pressed density is 4.05 to 4.25 g / cm. 3 The control may be performed in a similar manner.
[0052] This results in a positive electrode in which the average particle diameter Dp of the lithium transition metal composite oxide in the direction parallel to the plane on which the current collector is located and the average particle diameter Dv of the lithium transition metal composite oxide in the direction perpendicular to the plane on which the current collector is located satisfy the above-mentioned conditions. This positive electrode has all the characteristics and advantages of the positive electrode described above, and the description thereof will be omitted here. In any case, the positive electrode obtained by this method has good cycle performance.
[0053] The inventors have found that by adjusting the pressure value, cold rolling speed, and cold rolling compression density in the cold rolling process, it is possible to control the lithium transition metal composite oxide having an appropriate particle shape to be uniformly distributed on the surface of the current collector with a certain orientation. This ensures that the morphology of the lithium transition metal composite oxide is not damaged by the preparation process such as cold rolling, and also allows the arrangement of the dominant and non-dominant crystal planes of the lithium transition metal composite oxide on the surface of the current collector to be adjusted. As a result, a positive electrode with good cycle performance and electrical performance can be obtained.
[0054] According to some embodiments of the present application, after the positive electrode slurry is applied to the surface of the current collector, the method may further include drying the positive electrode slurry applied to the surface of the current collector before performing the cold rolling treatment. Specific parameters of the drying treatment are not particularly limited, and those skilled in the art may select parameters and methods of the drying treatment according to actual conditions in order to obtain a slurry layer with a uniform thickness.
[0055] After the cold rolling process, the current collector may be further cut to obtain a positive electrode having appropriate dimensions.
[0056] According to some embodiments of the present application, the negative electrode of the electrochemical device may further include an additive. This further includes an operation of covering the surface of the negative electrode active material layer with the additive. Specifically, the additive can be formed on the negative electrode active material layer by performing a roll press treatment. For example, the negative electrode having the additive can be roll pressed at a pressure of 5 to 30 tons and a speed of 0.5 to 2 meters per second. According to some embodiments of the present application, the additive may include at least one selected from the group consisting of lithium powder, lithium ribbon, and lithium-containing compound. This can further improve the quality of the electrochemical device obtained by the method.
[0057] [Example] Preparation of positive electrode pieces: The positive electrode material obtained in the following example, conductive carbon black as a conductive agent, and polyvinylidene fluoride as a binder were thoroughly stirred in an N-methylpyrrolidone (NMP) solvent system in a weight ratio of 97:1.5:1.5, and then mixed uniformly to form a positive electrode slurry. The positive electrode slurry was applied to an aluminum foil as a current collector at a coating weight of 17.2 mg / cm. 2 The mixture was applied onto a current collector so as to obtain a positive electrode piece after drying, cold rolling, and cutting.
[0058] Preparation of negative electrode pieces: Copper foil was used as a current collector, artificial graphite was used as a negative electrode active material, and styrene butadiene rubber and sodium carboxymethyl cellulose were used as binders. The artificial graphite, styrene butadiene rubber, and sodium carboxymethyl cellulose were mixed in a weight ratio of 96:2:2 and dispersed in deionized water to form a slurry, which was then uniformly stirred and applied to copper foil and dried to form a negative electrode active material layer, which was then cold-rolled to obtain negative electrode pieces. In some of the examples, the amount of 2.5 mg / cm was added to the surface of the negative electrode active material layer. 2 Then, the lithium ribbon was further added, and the negative electrode piece containing the additive was obtained through cold rolling.
[0059] Preparation of the separator: A porous polymer film made of polyethylene with a thickness of 8 μm was used.
[0060] Preparation of electrolyte: In an environment with a water content of less than 10 ppm, lithium hexafluorophosphate (1.15 mol / L) was mixed with a non-aqueous organic solvent (ethylene carbonate (EC): propylene carbonate (PC): diethyl carbonate (DEC) = 1:1:1, weight ratio) to obtain an electrolyte.
[0061] Preparation of lithium ion battery: A positive electrode, a separator, and a negative electrode were stacked in this order so that the separator was interposed between the positive electrode and the negative electrode to play a role of isolation, and then wound up to obtain an electrode assembly. The electrode assembly was placed in an aluminum packaging exterior, and after removing moisture at 80°C, the above-mentioned electrolyte was injected, sealed, and subjected to processes such as chemical formation, degassing, and shaping, a lithium ion battery was obtained.
[0062] Observation method for creases in the negative electrode: After fully charging the lithium-ion battery and discharging it to 3.0V, it was disassembled in a dry room or glove box, and the negative electrode was spread and flattened, and then photographed with a camera to obtain a clear image with appropriate multiples, and it was observed whether there were stripes on the surface of the negative electrode.
[0063] Measurement method of cycle performance: At 25°C, charge to 4.6V at a constant current of 0.7C, change to a constant voltage until the cutoff current is 0.025C, and discharge to 3.0V at 0.5C. The capacity retention rate of the lithium-ion battery after 200 cycles was recorded, taking the discharge capacity of the first cycle as 100%.
[0064] X-ray powder diffraction measurement method: The lithium-ion battery was adjusted to the corresponding voltage with a current density of 10 mA / s, left to stand for 5 min, and then disassembled in a glove box or dry room. The central part of the positive electrode was selected and cut to obtain a piece with a size of 3 × 3 cm. The diffraction peaks in the range of 10 to 80° were collected at a collection speed of 1° / min using a Bruker X-ray powder diffractometer and characterized.
[0065] Measurement method of Dp and Dv: A cross section perpendicular to the surface of the current collector was obtained by processing a piece of positive electrode with a microtome. The diameters of the particles on the cross section were measured and recorded in the direction parallel to the plane on which the current collector was located and in the direction perpendicular to the plane on which the current collector was located. The diameter was the maximum length of the particle in the defined direction. The statistical method was to select particles from left to right and top to bottom, and the statistical number of average particle diameters was 100 particles.
[0066] Example 1 Cobalt nitrate and aluminum nitrate were mixed in a molar ratio of Co:Al=99:1, and dissolved in deionized water of 5 times the total mass of cobalt nitrate and aluminum nitrate. Sodium carbonate and ammonia water were added to adjust the pH of the reaction system to 8.2, and the mixture was thoroughly stirred for 24 hours to obtain a precipitate. Ammonium oxalate, an additive, was added to the precipitate at 0.5% of the precipitate mass, mixed uniformly, and fired at 800°C for 24 hours to obtain a precursor. The precursor and sodium carbonate were uniformly mixed in a ratio of Co:Na=0.99:0.75 (stoichiometric ratio), and reacted at 800°C for 36 hours to obtain a powder material. The powder was thoroughly polished for 3 hours, and then uniformly mixed with lithium nitrate in a molar ratio of Na:Li=1:5 and reacted at 250°C for 8 hours. The reaction product was washed with deionized water at least five times, and then the powder was dried to obtain the positive electrode material Li. 0.73 Na 0.01 Co0.99 Al 0.01 O2 was obtained. 0.73 Na 0.01 Co 0.99 Al 0.01 The O2 positive electrode material powder, conductive carbon, and binder were mixed with NMP in a weight ratio of 97:1.5:1.5 to prepare a slurry, which was then applied to the surface of an Al current collector and dried in an oven at 120°C for 2 hours. After this, the slurry was rolled at a speed of 3.5 m / min and 4.15 g / cm 3 The resultant was cold-rolled at a pressure of 35 tons to obtain a compaction density of 1.0 kg / cm2 and a compaction density of 1.0 kg / cm2. The resultant was cut into pieces of a positive electrode.
[0067] The amount of the negative electrode active material layer added is 2.5 mg / cm 2 Then, the additive, a simple lithium ribbon, was added, and the mixture was roll-pressed to obtain a negative electrode piece having an additive.
[0068] Example 2 Cobalt nitrate and titanium nitrate were mixed in a ratio of Co:Ti=95:5, and dissolved in deionized water of 5 times the total mass of cobalt nitrate and titanium nitrate. Sodium carbonate and ammonia water were added to adjust the pH of the reaction system to 6.5, and the mixture was thoroughly stirred for 12 hours to obtain a precipitate. Sodium hydrogen carbonate, an additive, was added to the precipitate at 0.5% of the precipitate mass, mixed uniformly, and baked at 750°C for 24 hours to obtain a precursor. The precursor and sodium carbonate were uniformly mixed in a ratio of Co:Na=0.95:0.76 (stoichiometric ratio), and reacted at 800°C for 36 hours to obtain a powder material. The powder was thoroughly polished for 3 hours, and then uniformly mixed with lithium nitrate in a ratio of Na:Li=1:5 and reacted at 250°C for 8 hours. The reaction product was washed with deionized water at least 5 times, and then the powder was dried to obtain the positive electrode material Li. 0.74 Na 0.01 Co 0.95 Ti 0.05 Got O2.
[0069] The slurry, cold rolling parameters and additives were all the same as in Example 1.
[0070] Example 3: The pH of the reaction system was adjusted to 8.7, and the system was thoroughly stirred for 24 hours and then calcined at 900°C for 36 hours to obtain a precursor, which was then finally used as the positive electrode material Li 0.73 Na 0.01 Co 0.99 Al 0.01 The preparation method was the same as in Example 1, except that O2 was obtained.
[0071] Example 4: The preparation method was the same as in Example 2, except that sodium carbonate and aqueous ammonia were added to adjust the pH of the reaction system to 8.5, and the reaction system was thoroughly stirred for 24 hours and calcined at 950°C for 48 hours to obtain a precursor.
[0072] Example 5: The precursor and sodium carbonate were mixed uniformly, and then reacted at 850°C for 24 hours to obtain a powder material. After thoroughly grinding for 3 hours, the powder material was mixed uniformly with lithium nitrate in a molar ratio of Na:Li=1:5 and reacted at 450°C for 12 hours. The cold rolling process was performed at a cold rolling speed of 3 meters / min and a rolling speed of 4.16 g / cm. 3 The preparation method was the same as in Example 1, except that the compaction density was 1000 g / g and the pressure was 30 tons.
[0073] Example 6: The preparation method was the same as Example 1, except that the negative electrode pieces were not modified with an additive.
[0074] Example 7: The preparation method was the same as in Example 1, except that the precursor was obtained by reacting at 950° C. for 48 hours.
[0075] Example 8: Li in R-3m space group structure 0.7 CoO2 was used as the positive electrode material. The slurry and cold rolling parameters were the same as in Example 1. The negative electrode pieces were not modified with additives.
[0076] Example 9: Li in R-3m space group structure 0.75 Co 0.86 Mg 0.14 O2 was used as the positive electrode material. The slurry and cold rolling parameters were the same as in Example 1. The negative electrode pieces were not modified with additives.
[0077] Example 10: Li in R-3m space group structure 0.99 Co 0.99 Al 0.01 O2 was used as the positive electrode material. The slurry and cold rolling parameters were the same as in Example 1. The negative electrode pieces were not modified with additives.
[0078] Comparative Example 1 Cobalt nitrate and aluminum nitrate were mixed in a ratio of Co:Al=99:1, and dissolved in deionized water of 5 times the total mass of cobalt nitrate and aluminum nitrate. Sodium carbonate and ammonia water were added to adjust the pH of the reaction system to 9.8, and the mixture was thoroughly stirred for 36 hours to obtain a precipitate. Ammonium oxalate, an additive, was added to the precipitate at 0.5% of the precipitate mass, mixed uniformly, and baked at 600°C for 24 hours to obtain a precursor. The precursor and sodium carbonate were uniformly mixed in a ratio of Co:Na=0.99:0.77 (stoichiometric ratio), and reacted at 1000°C for 36 hours to obtain a powder material. The powder was thoroughly polished for 3 hours, and then uniformly mixed with lithium nitrate in a ratio of Na:Li=1:5 and reacted at 600°C for 8 hours. The reaction product was washed with deionized water at least 5 times, and then the powder was dried to obtain the positive electrode material Li. 0.76 Na 0.01 Co 0.99 Ai 0.01 Got O2.
[0079] The slurry and cold rolling parameters were the same as in Example 1. No additive modification was performed on the negative electrode pieces.
[0080] Comparative Example 2: The preparation method was the same as that of Comparative Example 1, except that sodium hydroxide was added to adjust the pH of the reaction system to 11.8.
[0081] Comparative Example 3: The preparation method was the same as that of Comparative Example 1, except that the precursor was obtained by calcining at 1000°C for 24 hours, and the powder material was obtained by reacting at 1050°C for 24 hours, and the negative electrode piece was not modified with an additive.
[0082] Comparative Example 4: R-3m space group structure Li0.88 The preparation method was the same as in Example 8, except that CoO2 was used as the positive electrode material.
[0083] Comparative Example 5: Cold rolling speed of 6 meters / minute, 4.29 g / cm 3 The preparation method was the same as in Example 1, except that the cold rolling was performed at a pressed density of 1000 g / cm2 and a pressure of 65 tons, and the negative electrode pieces were not modified with additives.
[0084] Comparative Example 6: Li of R-3m space group structure with D1 of 6.4 μm and D2 of 4.6 μm 0.99 Co 0.99 Al 0.01 O2 is used as the positive electrode material, and the cold-rolled compressed density is 3.94 g / cm 3 The preparation method was the same as in Example 10, except that
[0085] X-ray powder diffraction measurements were performed on Example 1 and Comparative Example 1. Referring to FIG. 5 and FIG. 6, it can be seen that the characteristic peak broadening and peak shift of Example 1 are smaller than those of Comparative Example 1 at the corresponding voltages (4.6 V and 3.0 V). Referring to FIG. 7 and FIG. 8, it can be seen that the twisted stripes seen in Example 1 did not occur on the surface of Comparative Example 1. Referring to FIG. 9, it can be seen that the cycle capacity retention rate of Comparative Example 1 was significantly reduced. The measurement results of each of the above-mentioned Examples and Comparative Examples are shown in Table 1 below. In Table 1, Y indicates the presence of stripes on the negative electrode, and N indicates the absence of stripes on the negative electrode.
[0086] [Table 1]
[0087] From Table 1, it can be seen that regardless of whether the positive electrode material has a P63mc or R-3m structure, all of the examples in which Dp / Dv is within the range limited by the present application have good cycle performance and are superior to the comparative examples. N50By setting the ratio of lithium to lithium ions in the range of 0.8 to 1.25, it is possible to obtain more excellent cycle stability. Comparison between Example 1 and Example 6 shows that the cycle stability can be further improved by supplying lithium to the positive electrode material having the P63mc structure using an additive.
[0088] Furthermore, from Comparative Example 1 and Comparative Example 5, it can be seen that if the ratio D1 / D2 of the long axis average particle diameter D1 to the short axis average particle diameter D2 of the positive electrode material is too small and / or the cold rolling conditions are not appropriate, it is difficult to achieve the Dp / Dv defined in the present application, and the cycle stability is correspondingly poor.
[0089] X-ray powder diffraction measurements were performed on some of the samples of the examples and comparative examples, and the measurement results are shown in Table 2 below.
[0090] [Table 2]
[0091] From Table 2 above, it can be seen that I1 / I3 in Comparative Example 1 is smaller than 0.8. This indicates that there is a risk of powdering at high voltage. Therefore, the cycle retention rate of Comparative Example 1 is also significantly lower than that of the Examples.
[0092] After eight cycles, the rate of change in I2 / I3 in X-ray powder diffraction, and the rate of change in peak shift and half-width were measured. The measurement results are shown in Table 3 below.
[0093] [Table 3]
[0094] From Table 3 above, it can be seen that Examples 1, 8 and 9 all have relatively small peak shifts, and the change rate of I2 / I3 and the change rate of half-width are also significantly lower than those of Comparative Example 4. This indicates that they have good stability. The above viewpoint is also verified by the retention rate after 200 cycles at 4.6V.
[0095] The above description is merely illustrative of the present application, and is not intended to be any limitation to the present application. The present application has been disclosed above in preferred embodiments, but these embodiments are not intended to limit the present application. Any changes or modifications made by those skilled in the art using the technical contents disclosed above within the scope of the technical solution of the present invention are equivalent to the embodiments of the present application, and are included in the scope of the technical solution of the present invention. [Explanation of symbols]
[0096] 100: positive electrode, 110: current collector, 120A to 120C: lithium transition metal composite oxide, 120: active material layer, 200: separator, 300: negative electrode, 1000: electrochemical device.
Claims
1. a positive electrode active material layer disposed on a current collector, the positive electrode active material layer contains a lithium transition metal composite oxide, where Dp is an average particle diameter of the lithium transition metal composite oxide in a direction parallel to the plane on which the current collector is located, and Dv is an average particle diameter of the lithium transition metal composite oxide in a direction perpendicular to the plane on which the current collector is located, the relationship 1.1≦Dp / Dv≦2.3 is satisfied, The lithium transition metal composite oxide has a long axis average particle diameter D 1 and a short axis average particle diameter D 2 , and satisfies 1.4≦(D 1 / D 2 )≦5.
5. Positive electrode.
2. The positive electrode according to claim 1 , wherein the lithium transition metal composite oxide satisfies 5 μm≦Dp≦25 μm.
3. The lithium transition metal composite oxide has a satisfying condition of 0.8≦(Dp+Dv) / 2D N50 ≦1.25, D N50 The positive electrode according to claim 1 , wherein R is a median diameter of the lithium transition metal composite oxide.
4. a) The lithium transition metal composite oxide has an R-3m space group structure, and the lithium transition metal composite oxide is Li x1 Ni y1 Co z1 Mn k Z q O b-a T a Z includes at least one selected from the group consisting of B, Mg, Al, Si, P, S, Ti, Cr, Fe, Cu, Zn, Ga, Y, Zr, Mo, Ag, W, In, Sn, Pb, Sb, and Ce, T is a halogen, and x1, y1, z1, k, q, a, and b each satisfy 0.2<x1≦1.2, 0≦y1≦1, 0≦z1≦1, 0≦k≦1, 0≦q≦1, 1≦b≦2, and 0≦a≦1, b) The lithium transition metal composite oxide has a P63mc space group structure, and the lithium transition metal composite oxide is Li x2 Na z2 Co 1-y2 M y2 O 2±n X n wherein 0.6<x2<0.95, 0≦y2<0.15, 0≦z2<0.03, and 0≦n≦0.2, M includes at least one selected from the group consisting of Al, Mg, Ti, Mn, Fe, Ni, Zn, Cu, Nb, Cr, and Zr, and X is a halogen; The positive electrode according to claim 1 , which satisfies at least one of the above.
5. The lithium transition metal composite oxide has a thickness of 7 μm≦D 1 The positive electrode according to claim 1 , wherein the thickness satisfies ≦28 μm.
6. When an electrochemical device including the positive electrode is charged to a voltage of 4.6 V, the positive electrode has at least a characteristic peak P 1 and the characteristic peak P 2 and 1 Peak intensity I 1 is the P 2 Peak intensity I 2 Satisfying greater than, and When the electrochemical device was discharged to a voltage of 3.0 V, the positive electrode had a characteristic peak P 3 and P 3 Peak intensity I 3 (I 1 -I 2 )≦I 3 ≦(I 1 +I 2 2. The positive electrode according to claim 1 ,
7. The P 3 Peak intensity I 3 The above P 1 Peak intensity I 1 Ratio I 1 / I 3 The positive electrode of claim 6 , wherein R is 0.8 or more.
8. 2. The positive electrode according to claim 1, wherein, when an electrochemical device including the positive electrode is subjected to eight charge-discharge cycles in a range of 3.0 V to 4.6 V and discharged to a voltage of 3.0 V, the positive electrode satisfies the following: a peak position shift of a highest peak in an X-ray diffraction spectrum of the positive electrode after the cycles is 0.1° or less compared to the positive electrode before the cycles, and a rate of change in half-width of the highest peak is less than 5%.
9. An electrochemical device comprising the positive electrode according to any one of claims 1 to 8, a negative electrode, and a separator.
10. 10. The electrochemical device of claim 9, wherein the negative electrode has stripes on its surface when discharged to a voltage of 3.0V.
11. An electronic device comprising an electrochemical device according to any one of claims 9 to 10.
Citation Information
Patent Citations
Nonaqueous electrolyte cell
JP1997199127A
Positive electrode active material for non-aqueous lithium secondary battery and the non-aqueous lithium secondary battery using the active material
JP2002279985A
Positive electrode active substance for lithium ion secondary battery and its manufacturing method
JP2003151546A
Positive active material for nonaqueous electrolyte secondary battery and nonaqueous electrolyte secondary battery using this
JP2007173210A
Method of forming crystal-oriented cathode active material plate
JP2014164836A