Resin sheet having hair-like bodies and molded product thereof

The integration of urethane elastomer with specific molecular weight and composition ratios in a thermoplastic resin sheet with hair-like bodies ensures the maintenance of tactility during secondary molding processes, achieving a smooth and soft texture.

JP7562008B2Active Publication Date: 2024-10-04DENKA CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023545525
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-08-30
Filing Date
2022-08-26
Publication Date
2024-10-04
Estimated Expiration
2042-08-26

AI Technical Summary

Technical Problem

Resin sheets with hair-like bodies lose their tactility during secondary molding processes, making it difficult to maintain good texture after being attached to surfaces.

Method used

A thermoplastic resin sheet with hair-like bodies integrated into a continuous phase base layer, using a urethane elastomer with specific molecular weight and composition ratios, ensuring no structural boundaries between the base layer and hair-like bodies.

Benefits of technology

The resin sheet maintains good tactility even after secondary molding, providing a smooth, soft, and fluffy feel.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007562008000002
    Figure 0007562008000002
  • Figure 0007562008000003
    Figure 0007562008000003
  • Figure 0007562008000004
    Figure 0007562008000004
Patent Text Reader

Abstract

The purpose of the present invention is to provide a resin sheet which, even after having undergone secondary forming, can retain a satisfactory touch and a formed article of the resin sheet. The resin sheet is a thermoplastic resin sheet which has flocky projections regularly arranged on at least one surface of a substrate layer, and the substrate layer and the flocky projections have no structural boundary therebetween and have formed a continuous phase, wherein the substrate layer and the flocky projections are constituted from a thermoplastic resin composition including a urethane-based elastomer and the urethane-based elastomer comprises a component (A) derived from a polyol having a number-average molecular weight of 450-900 and a component (B) derived from an aliphatic diol having 2 to 10 carbon atoms, the (A) / (B) molar ratio being 60:40 to 88:12. 
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin sheet having hair-like bodies and a molded article thereof. [Background technology]

[0002] Conventionally, sheets of paper and polymer materials have been used as interior materials for automobiles, housings for accessories, housings for electronic devices and home appliances, building materials such as wallpaper, housings for toys and game consoles, and components for daily necessities. As a method for imparting a good tactile sensation to the surface of a sheet, for example, Patent Document 1 proposes a resin sheet having hair-like bodies regularly arranged on the surface. On the other hand, when such a resin sheet is used as an interior part such as a dashboard or a seat of an automobile, it is necessary to perform secondary molding and attach it to the surface of the object.

[0003] [Patent Document 1] International Publication No. 2018 / 016562 Summary of the Invention

[0004] However, it has been found that such a resin sheet loses its hair-like bodies during the process of secondary molding and attaching it to the surface of an object, and there is a risk that the good tactile feel cannot be maintained. An object of the present invention is to provide a resin sheet that can maintain a good tactile feel even after secondary molding, and a molded article made from the resin sheet.

[0005] That is, the present inventors have investigated various means and have found that in a thermoplastic resin sheet having regularly arranged hair-like bodies on at least one surface of a base layer, with no structural boundary between the base layer and the hair-like bodies forming a continuous phase, the thermoplastic resin composition constituting the base layer and the hair-like bodies contains a urethane-based elastomer, and the urethane-based elastomer contains component (A) derived from a polyol having a number average molecular weight of 450 to 900 and component (B) derived from an aliphatic diol having 2 to 10 carbon atoms, and by adjusting the molar ratio of (A) to (B) to be 60:40 to 88:12, good tactile feel can be maintained even after secondary molding, thereby completing the present invention.

[0006] The present invention, which solves the above problems, comprises the following: (1) A thermoplastic resin sheet having regularly arranged hair-like bodies on at least one surface of a base layer, with no structural boundary between the base layer and the hair-like bodies forming a continuous phase, wherein the thermoplastic resin composition constituting the base layer and the hair-like bodies contains a urethane-based elastomer, the urethane-based elastomer containing a component (A) derived from a polyol having a number average molecular weight of 450 to 900 and a component (B) derived from an aliphatic diol having 2 to 10 carbon atoms, and the molar ratio of (A) to (B) is 60:40 to 88:12. (2) The resin sheet according to (1), wherein the average height of the hairs is 30 μm or more and 500 μm or less, the average diameter of the hairs is 1 μm or more and 50 μm or less, and the average spacing of the hairs is 20 μm or more and 200 μm or less. (3) The resin sheet according to (1) or (2), wherein the polyol is a polycarbonate-based diol. (4) A resin sheet according to any one of (1) to (3), having a base layer on the side of the undercoat layer opposite to the hair-like bodies. (5) A molded product of the resin sheet according to any one of (1) to (4). (6) The molded product according to (5), which is an insert molded product or a vacuum molded product. (7) The molded article according to (5) or (6), which is provided on the surface of an automobile interior material, an electronic device exterior material, or a cosmetic container.

[0007] According to the present invention, it is possible to provide a resin sheet capable of maintaining a good tactile feel even after secondary molding, and a molded article made from the resin sheet. [Brief description of the drawings]

[0008] [Figure 1] 1 is a schematic vertical cross-sectional side view showing a resin sheet according to a first embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic plan view of the resin sheet of FIG. [Diagram 3] FIG. 4 is a schematic vertical cross-sectional side view showing a laminated structure of a resin sheet according to a second embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Various embodiments of the resin sheet will be described below, followed by a description of a method for manufacturing the resin sheet. However, in cases where a particular description given for one embodiment also applies to other embodiments, that description will be omitted in the other embodiments.

[0010] [First embodiment] The resin sheet according to the first embodiment of the present invention is a thermoplastic resin sheet having regularly arranged hair-like bodies on at least one surface of a base layer, with no structural boundary between the base layer and the hair-like bodies forming a continuous phase, wherein the thermoplastic resin constituting the base layer and the hair-like bodies contains a urethane-based elastomer, and the urethane-based elastomer contains a component (A) derived from a polyol having a number average molecular weight of 450 to 900 and a component (B) derived from an aliphatic diol having 2 to 10 carbon atoms, and the molar ratio of (A) to (B) is 60:40 to 88:12.

[0011] <Underlayer> The underlayer (1a) is a layer that underlies the hairy bodies, and refers to the portion of the reference numeral 1 other than the hairy bodies 1b on the surface. The thickness of the underlayer refers to the thickness from the root of the hairy bodies to the surface on the opposite side of the underlayer. The average thickness of the underlayer is preferably 15 μm to 500 μm, more preferably 30 μm to 300 μm, and more preferably 50 μm to 150 μm. By making the thickness 15 μm or more, the height of the hairy bodies can be fully expressed. Furthermore, by making the thickness 500 μm or less, the hairy bodies can be efficiently formed. There may be no structural boundary between the underlayer and the hairy bodies, and a continuous phase may be formed. "There is no structural boundary" means that the underlayer and the hairy bodies are formed integrally, and there is no structurally clear boundary between them. Furthermore, "the continuous phase is formed" means that there is no seam between the underlayer and the hairy bodies, and they are not discontinuous (continuous phase). In this respect, it is different from a structure in which hairy bodies are planted on the underlayer. The undercoat layer and the hair may have the same composition, and the bond between the undercoat layer and the hair may include a covalent bond. A covalent bond is a chemical bond formed by sharing an electron pair between two atoms. In a thermoplastic resin, which is a chain molecule of monomers, the individual polymers are bonded by covalent bonds, which are stronger than the van der Waals bonds or hydrogen bonds that act between polymer molecules. The undercoat layer and the capillaries may be derived from the same solid thermoplastic resin sheet, which is not separate. Derived from the same solid thermoplastic resin sheet means, for example, that the capillaries and the undercoat layer are directly or indirectly obtained based on the same resin sheet. The base layer and the hair-like bodies may be formed from the same solid thermoplastic resin sheet. Formed from the same solid thermoplastic resin sheet means that the hair-like bodies and the base layer are directly formed by processing a single resin sheet. Since there is no structural boundary between the base layer and the hair-like bodies, and a continuous phase is formed, separation of the hair-like bodies from the base layer due to external stimuli is suppressed, resulting in a sheet with a good tactile feel. In addition, the sheet can be manufactured in fewer steps than when the hair-like bodies are implanted.

[0012] The undercoat layer and the hair-like bodies are made of the same thermoplastic resin composition containing a thermoplastic resin as a main component. Here, "containing a thermoplastic resin as a main component" means that the composition contains 50% by mass or more. Preferably, the composition contains 60% by mass or more, 70% by mass or more, 80% by mass or more, or 90% by mass or more. As the thermoplastic resin in this embodiment, a urethane-based elastomer (TPU) can be used. In one embodiment of the present invention, the composition may further contain at least one thermoplastic resin selected from the group consisting of a styrene-based resin, a polyolefin-based resin, a polyvinyl chloride resin, a thermoplastic elastomer, and a fluorine-based resin.

[0013] Urethane elastomers are resins made from diisocyanates and polyols as reaction raw materials. The combination of diisocyanates is as follows: diphenylmethane diisocyanate (MDI)-based, H 12 Any combination of MDI, hexamethylene diisocyanate (HDI) and polyol of polyether, polyester or polycarbonate may be selected, or a combination of a plurality of them may be used. In one embodiment of the present invention, a combination of MDI or HDI diisocyanate and carbonate polyol is preferably used.

[0014] In this embodiment, the urethane elastomer contains a component (A) derived from a polyol having a number average molecular weight of 450 to 900, and a component (B) derived from an aliphatic diol having 2 to 10 carbon atoms. In other words, the urethane elastomer of this embodiment is a resin containing at least two kinds of reaction raw materials, a polyol having a number average molecular weight of 450 to 900 and an aliphatic diol having 2 to 10 carbon atoms.

[0015] Here, "component derived from X" means X or a reaction residue of X in a synthetic product using X as a reaction raw material. For example, component (A) derived from a polyol having a number average molecular weight of 450 to 900 means a polyol residue in a urethane component synthesized using a polyol having a number average molecular weight of 450 to 900 as a raw material, and component (B) derived from an aliphatic diol having 2 to 10 carbon atoms means a diol residue in a urethane component synthesized using an aliphatic diol having 2 to 10 carbon atoms as a raw material.

[0016] "Polyol having a number average molecular weight of 450 to 900" means a compound having two or more hydroxyl groups (-OH) with a number average molecular weight of 450 to 900. The number of hydroxyl groups of the polyol is not particularly limited as long as it is 2 or more, including 2. The number average molecular weight of the polyol is preferably 475 to 875, more preferably 500 to 850. By having a number average molecular weight of 450 or more, the heat resistance temperature of the TPU synthesized using component (A) increases, and the hair-like body formed by the TPU can maintain a good touch even after secondary molding, and by having a number average molecular weight of 900 or less, the hardness of the TPU synthesized using component (A) is prevented from becoming higher than necessary, and the hair-like body formed by the TPU has a good touch. As the polyol of this embodiment, polycarbonate-based diols, polyether-based diols, polyester-based diols, etc. can be suitably used, and among them, polycarbonate-based diols are preferable. Polycarbonate-based diols can be produced by polycondensing an aliphatic linear diol with a carbonate compound such as dialkyl carbonate or diphenyl carbonate through an ester exchange reaction, and the number average molecular weight of the polyol can be adjusted by adjusting the amount of the compounds. Examples of aliphatic linear diols include 1,4-butanediol, 1,5-pentanediol, and 1,6-hexanediol, and among these, polycarbonate-based diols using 1,6-hexanediol are preferred. Examples of polyether diols include polyethylene glycol, polytrimethylene ether glycol, polytetramethylene ether glycol, polyhexamethylene ether glycol, etc., which are obtained by ring-opening polymerization of cyclic ether compounds. Among these, polytetramethylene ether glycol is preferred from the viewpoints of mechanical properties, moldability, and cold resistance in the TPU to be synthesized. Examples of polyester diols include polyester diols obtained from aliphatic dicarboxylic acids and aliphatic diols, polyester diols obtained from aromatic dicarboxylic acids and aliphatic diols, polycaprolactone diols obtained by ring-opening polymerization of ε-caprolactone, etc. Among these, polyester diols obtained from aliphatic dicarboxylic acids and aliphatic diols are preferred from the viewpoints of availability and viscosity control of the resulting TPU. The number average molecular weight can be calculated based on the following formula. Number average molecular weight = (56100 x number of hydroxyl groups) / hydroxyl value (The hydroxyl value of the polyol can be determined by titration in accordance with JIS K 1557. The unit of the hydroxyl value is mgKOH / g. The acid value of the polyol can be determined by titration in accordance with JIS K 1557. The unit of the acid value is mgKOH / g.

[0017] The number average molecular weight can also be determined based on GPC under the following conditions. [Gel Permeation Chromatography (GPC)] A tetrahydrofuran (THF) solution with a polymer concentration of 1 mg / 1 mL is prepared, and in a GPC measurement device, a column is stabilized in a heat chamber at 40°C. THF is passed through the column at this temperature as a solvent at a flow rate of 1 mL per minute, and approximately 100 μL of the THF sample solution is injected to measure the molecular weight distribution of the polymer.

[0018] When measuring the molecular weight distribution of a polymer using GPC, the logarithm of the molecular weight of the polymer in the eluent passing through the detector decreases monotonically as the elution volume (elution rate x elution time) increases. In other words, the higher the molecular weight, the faster it is eluted from the column. Furthermore, the signal strength is proportional to the amount of polymer present in the eluent passing through the detector. By creating a calibration curve showing the relationship between elution time and molecular weight using standard polystyrene, the elution curve detected by the differential refractometer can be converted into a curve with signal strength on the vertical axis and the logarithm of the molecular weight converted into polystyrene on the horizontal axis (hereinafter referred to as the molecular weight curve). Standard polystyrene samples for creating the calibration curve are polystyrene with a molecular weight of 10 2 ~10 7 For example, the time at which the value is 0.2 or more from the baseline value can be defined as the start point of the peak, and the time at which the value is 0.2 or more from the baseline value after the peak showing the minimum molecular weight can be defined as the end point of the peak.

[0019] "Aliphatic diol having 2 to 10 carbon atoms" means a hydrocarbon compound having two hydroxyl groups and having 2 to 10 carbon atoms. The carbon number is preferably 2 to 8, and more preferably 2 to 6. Among them, 1,4-butanediol having 4 carbon atoms is preferable. By making the carbon number 10 or less, the number average molecular weight of the aliphatic diol can be suppressed to a low value, for example, less than 400 or less than 200. Specific examples of the aliphatic diol include ethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,8-octanediol, 1,9-nonanediol, neopentyl glycol, diethylene glycol, triethylene glycol, and the like.

[0020] In the urethane-based elastomer of the present embodiment, the molar ratio of the component (A) derived from a polyol having a number average molecular weight of 450 to 900 and the component (B) derived from an aliphatic diol having 2 to 10 carbon atoms is 60:40 to 88:12. 63:37 to 87:13 is more preferable. In addition, by making it 78:22 to 88:12, a moist touch can be obtained, and by making it 60:40 to 77:23, a dry touch can be obtained. By making the component (A) derived from a polyol having a number average molecular weight of 450 to 900 60 mol % or more, a good touch can be obtained, and by making it 88 mol % or less, large deformation or disappearance of the hair-like body due to secondary formation can be suppressed. The molar ratio of the component (A) derived from a polyol having a number average molecular weight of 450 to 900 and the component (B) derived from an aliphatic diol having 2 to 10 carbon atoms can be measured using 13C-NMR or the like in addition to being calculated from the raw materials used.

[0021] As the diisocyanate, aromatic diisocyanate, aliphatic diisocyanate, and alicyclic diisocyanate can be used. Specific examples of aromatic diisocyanate include 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, 4,4'-diphenylmethane diisocyanate, 2,4'-diphenylmethane diisocyanate, and 2,2'-diphenylmethane diisocyanate. Specific examples of aliphatic diisocyanate include hexamethylene diisocyanate, tetramethylene diisocyanate, 2-methyl-pentane-1,5-diisocyanate, and 3-methyl-pentane-1,5-diisocyanate. Specific examples of alicyclic diisocyanate include hydrogenated tolylene diisocyanate, hydrogenated xylene diisocyanate, hydrogenated diphenylmethane diisocyanate, and isophorone diisocyanate.

[0022] In one embodiment of the present invention, the molar ratio of diisocyanate, which is a reaction raw material for a urethane-based elastomer, to the sum of component (A) derived from a polyol and component (B) derived from an aliphatic diol is preferably 70:30 to 30:70, more preferably 60:40 to 40:60, and even more preferably 50:50.

[0023] As the styrene-based resin, homopolymers or copolymers of styrene-based monomers such as styrene, α-methylstyrene, p-methylstyrene, dimethylstyrene, pt-butylstyrene, chlorostyrene, etc., copolymers of these styrene-based monomers with other monomers, such as styrene-acrylonitrile copolymers (AS resins), or graft polymers obtained by graft polymerization of the above-mentioned styrene-based monomers with other polymers, such as polybutadiene, styrene-butadiene copolymers, polyisoprene, polychloroprene, etc., in the presence of diene rubber polymers, such as polystyrene, high impact polystyrene (HIPS resin), styrene-acrylonitrile graft polymers (ABS resins), etc., can be used. Styrene-based thermoplastic elastomers can also be used.

[0024] The polyolefin resin means a resin made of a polymer containing α-olefin as a monomer, and includes polyethylene resin and polypropylene resin. As the polyethylene resin, high density polyethylene, low density polyethylene, linear low density polyethylene, linear medium density polyethylene, etc. can be used, and not only a single substance but also a copolymer, grafted product, or blend having the structure can be used. As the latter resin, for example, a copolymer or blend of a resin having a polar group in the polyethylene chain, such as an ethylene-vinyl acetate copolymer, an ethylene-acrylic acid copolymer, an ethylene-acrylic acid ester copolymer, an ethylene-methacrylic acid ester copolymer, an ethylene-vinyl acetate-vinyl chloride copolymer, or a ternary copolymer with an acid anhydride, can be mentioned.

[0025] As the polypropylene resin, homopolypropylene, random polypropylene, block polypropylene, etc. can be used. When homopolypropylene is used, the structure of the homopolypropylene may be any of isotactic, atactic, and syndiotactic. When random polypropylene is used, the α-olefin to be copolymerized with propylene preferably has 2 to 20 carbon atoms, more preferably has 4 to 12 carbon atoms, such as ethylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-nonene, and 1-decene. When block polypropylene is used, a block copolymer (block polypropylene), a block copolymer containing a rubber component, or a graft copolymer can be used. In addition to using these olefin resins alone, other olefin resins can also be used in combination.

[0026] As the polyvinyl chloride resin, a vinyl chloride homopolymer or a copolymer of vinyl chloride and other comonomers can be used. When polyvinyl chloride is a copolymer, it may be a random copolymer or a graft copolymer. An example of a graft copolymer is one in which vinyl chloride is graft-polymerized onto an ethylene-vinyl acetate copolymer or a thermoplastic urethane polymer as a backbone polymer. The polyvinyl chloride of this embodiment is a soft polyvinyl chloride that can be extruded, and is a composition containing additives such as a polymer plasticizer. As the polymer plasticizer, a known polymer plasticizer can be used, and preferred examples include ethylene copolymer polymer plasticizers such as ethylene-vinyl acetate-carbon monoxide copolymer, ethylene-(meth)acrylic acid ester-carbon monoxide copolymer, and ethylene-vinyl acetate copolymer with a high vinyl acetate content.

[0027] Thermoplastic elastomers include those having a structure in which a soft polymeric substance and a hard polymeric substance are combined. Specific examples include styrene-based elastomers, olefin-based elastomers, vinyl chloride-based elastomers, polyester-based elastomers, and polyamide-based elastomers. These elastomers can be selected from those generally available on the market.

[0028] As the fluorine-based resin, a homopolymer of vinylidene fluoride and a vinylidene fluoride copolymer mainly composed of vinylidene fluoride can be used. Polyvinylidene fluoride (PVDF) resin is a crystalline resin that exhibits various crystal structures such as α type, β type, γ type, and αp type, and examples of the vinylidene fluoride copolymer include vinylidene fluoride-hexafluoropropylene copolymer, vinylidene fluoride-tetrafluoroethylene copolymer, vinylidene fluoride-chlorotrifluoroethylene copolymer, vinylidene fluoride-trifluoroethylene copolymer, vinylidene fluoride-tetrafluoroethylene-hexafluoropropylene ternary copolymer, vinylidene fluoride-chlorotrifluoroethylene-hexafluoropropylene ternary copolymer, and a mixture of two or more of these.

[0029] The melt mass flow rate of the thermoplastic resin composition at 190°C to 300°C is preferably 4g / 10min or more. By making it 4g / 10min or more, the transferability of the shape of the capillaries can be improved. The melt mass flow rate is a value measured under the conditions of a test temperature range of 190°C to 300°C and a load (2.16kg to 10.0kg) according to JIS K 7210.

[0030] The thermoplastic resin composition may be an alloy of the above thermoplastic resins in any ratio within the range not impairing the effects of the present invention. Furthermore, other additives may be contained. As other additives, within the range not impairing the effects of the present invention, additives such as water-repellent, oil-repellent, colorants such as pigments and dyes, lubricants and release agents such as silicone oil and alkyl esters, fibrous reinforcing agents such as glass fibers, fillers such as granular fine particles such as talc, clay, and silica, and scaly fine particles such as mica, low molecular weight antistatic agents such as salt compounds of sulfonic acid and alkali metals, polymeric antistatic agents such as polyether ester amides, flame retardants, antibacterial agents, antiviral agents, and heat stabilizers can be added. In addition, scrap resin generated in the resin sheet manufacturing process can be mixed and used.

[0031] Examples of water- and oil-repellents include silicone-based water- and oil-repellents, carnauba wax, and fluorine-based water- and oil-repellents. Examples of silicone include organopolysiloxane, dimethylpolysiloxane, methylphenylpolysiloxane, and methylhydrogenpolysiloxane, among which dimethylpolysiloxane is preferably used. Examples of commercially available products include "Clinbell CB50-PP", "Clinbell CB-30PE", "Clinbell CB-1", and "Clinbell CB-50AB" (manufactured by Fuji Chemical Co., Ltd.), which are alloys of silicone with resin. Examples of commercially available carnauba wax include "Carnauba No. 1" (manufactured by Nikko Rica Co., Ltd.), and examples of commercially available fluorine-based water- and oil-repellents include surfactants having perfluoroalkyl groups, and examples of commercially available products include "Surflon KT-PA" (manufactured by AGC Seimi Chemical Co., Ltd.). The amount of water- and oil-repellents added is preferably 0.5% by mass to 25% by mass. If the content is less than 0.5% by mass, there is a risk that sufficient water- and oil-repellent effects will not be obtained, whereas if the content exceeds 25% by mass, there is a risk that moldability will deteriorate.

[0032] Examples of the antistatic agent include polyether ester amide-based polymer-type antistatic agents and ionomer-based polymer-type antistatic agents. Commercially available polyether ester amide-based polymer-type antistatic agents include "Pellestat 230", "Pellestat 6500", "Pelectron AS", and "Pelectron HS" (manufactured by Sanyo Chemical Industries, Ltd.). Commercially available ionomer-based polymer-type antistatic agents include "Entira SD100" and "Entira MK400" (manufactured by Mitsui DuPont Polychemicals, Ltd.). The amount of the antistatic agent added is preferably 5% to 30% by mass. If the amount is less than 5% by mass, sufficient antistatic properties may not be obtained, and if the amount is more than 30% by mass, the production cost increases.

[0033] Either inorganic or organic antibacterial agents may be added. In consideration of dispersibility, inorganic agents are preferred. Specific examples include inorganic antibacterial agents of metal ions (Ag, Zn, Cu) and calcined shell calcium antibacterial agents. Commercially available inorganic antibacterial agents of metal ions include "Bactekiller BM102VT" (manufactured by Fuji Chemical Co., Ltd.), "Novaron VZF200", "Novaron (AG300)" (manufactured by Toa Gosei Co., Ltd.), "KM-10D-G", and "IM-10D-L" (manufactured by Sinanen Zeomic Co., Ltd.). Calcined shell calcium antibacterial agents include "Scallow" (manufactured by FID Co., Ltd.). The amount of antibacterial agent added is preferably 0.5% to 5% by mass. If the amount is less than 0.5% by mass, sufficient antibacterial properties may not be obtained, and if the amount is more than 5% by mass, production costs will increase.

[0034] As the lubricant / release agent, alkyl lubricants / release agents such as aliphatic hydrocarbon compounds, higher fatty acid compounds, higher aliphatic alcohol compounds, and fatty acid amide compounds, silicon lubricants / release agents, and fluorine lubricants / release agents can be used. When using a lubricant / release agent, the amount of the lubricant / release agent added is preferably 0.01 to 5 parts by mass, more preferably 0.05 to 3 parts by mass, and even more preferably 0.1 to 2 parts by mass, out of a total of 100 parts by mass including the resin composition. By making the amount of the lubricant / release agent 0.01 parts by mass or more, the risk of the release effect being reduced is reduced, and by making the amount 5 parts by mass or less, the risk of bleeding out onto the sheet surface is reduced.

[0035] Also, a masterbatch in which a lubricant and a release agent are pre-alloyed with a thermoplastic resin can be used. For example, a commercially available masterbatch based on a urethane-based thermoplastic elastomer is "Wax Master V" (manufactured by BASF), and in consideration of production efficiency, it is preferable to use a masterbatch. The amount of the masterbatch added is preferably 1 to 8 parts by mass, more preferably 2 to 7 parts by mass, and even more preferably 3 to 6 parts by mass, out of a total of 100 parts by mass including the resin composition.

[0036] <hairy body> The hair-like bodies (1b) refer to the parts that extend in a hair-like manner from the surface of the base layer (1a) as shown in FIG. 1. The hair-like bodies are regularly arranged on the surface of the base layer. Here, regularly arranged means that the hair-like bodies are arranged in a non-random arrangement, that is, in a state where the hair-like bodies are arranged in an orderly manner (for example, at regular intervals) in one or two directions. The arrangement state of the hair-like bodies is used to judge whether the arrangement of the hair-like bodies is regular or not. In one embodiment, the hair-like bodies are located on the base layer at a predetermined interval, and the positions of the bottom surfaces of the hair-like bodies are regularly arranged in the longitudinal and lateral directions of the base layer. The arrangement form of the hair-like bodies is not particularly limited, and a checkerboard arrangement or a staggered arrangement in which the hair-like bodies are arranged vertically and horizontally can be selected. The hair-like bodies are regularly arranged on the surface of the base layer, so that they are uniform and free of unevenness, and a good tactile sensation is easily expressed. When a load is applied to the hair-like bodies, for example by tracing them with a finger, the hairs fall down, and a finger mark that appears to have a different luster and color tone from the surrounding parts can be formed. The hair-like material can also provide a suede-like, brushed sheet-like feel.

[0037] The average height (h) of the hairs is preferably 30 μm to 500 μm, more preferably 60 μm to 250 μm, even more preferably 80 μm to 200 μm, and even more preferably 90 μm to 180 μm. By making the average height 30 μm or more, a good tactile sensation can be sufficiently ensured, and by making the average height 500 μm or less, good tactile sensations such as a moist feeling, a soft feeling, and a fluffy feeling can be obtained. When the hair is almost vertical to the base layer, the length from the base to the tip of the hair represents the height of the hair. On the other hand, when the hair is inclined to the base layer or has a rolled part, the height of the hair is the distance from the surface of the base layer to the point where the hair is farthest from the surface of the base layer. The total value of the intervals divided by multi-point measurement from the tip to the center of the base of the hair is the length of the hair. The average height and length of the hairs can be determined by measuring the height and length of the hairs at any number of points on the resin sheet using an electron microscope and image processing software, and then calculating the arithmetic mean value of the measured values.

[0038] The average diameter (d) of the hairs is preferably 1 μm to 50 μm, more preferably 5 μm to 50 μm, and even more preferably 5 μm to 40 μm. By making the average diameter of the hairs 1 μm or more, a good tactile sensation can be ensured, and by making the average diameter of the hairs 50 μm or less, good tactile sensations such as a moist feeling, a soft feeling, and a fluffy feeling can be obtained. The average diameter of the hairs is determined by measuring the diameter of the mid-height (h / 2) of the hairs from several points on the resin sheet using an electron microscope and image processing software, and taking the arithmetic average value of the measured values. The aspect ratio of the hair-like bodies can be expressed as (average height of hair-like bodies / average diameter of hair-like bodies). The aspect ratio of the hair-like bodies is preferably 2 to 20, more preferably 2 to 10, and even more preferably 2 to 5. By setting the aspect ratio to 2 or more, good tactile sensation can be ensured, and by setting the aspect ratio to 20 or less, not only good tactile sensation such as moist, soft, and fluffy sensation can be obtained, but also the risk of the ratio of the height to the length of the hair-like bodies becoming equal to or less than a certain level can be reduced. On the other hand, the aspect ratio can also be based on the average bottom diameter of the hair-like bodies. The average bottom diameter of the hair-like bodies is preferably 10 μm to 150 μm, more preferably 20 μm to 120 μm, and even more preferably 30 μm to 100 μm. The average bottom diameter of the hair-like bodies is determined by measuring the intervals between adjacent hair-like bodies at several points on the resin sheet and using the arithmetic average value of the measured values. The aspect ratio based on the bottom diameter of the hair-like bodies is preferably 1.0 to 10, more preferably 1.0 to 5, and even more preferably 1.0 to 2.5. By setting the aspect ratio to 1.0 or more, good tactile sensation can be ensured, and by setting the aspect ratio to 10 or less, not only good tactile sensation such as moist feeling, soft feeling, and fluffy feeling can be obtained, but also the risk of the ratio of the height to the length of the hair-like bodies becoming equal to or less than a certain level can be reduced.

[0039] The average spacing (t) of the hairs is preferably 20 μm to 200 μm, more preferably 40 μm to 150 μm, and even more preferably 40 μm to 100 μm. The spacing of the hairs means the distance between the center of the root of a hair and the center of the root of an adjacent hair, as shown in FIG. 2, for example. By setting the average spacing to 20 μm or more, good tactile sensation is ensured, and by setting the average spacing to 200 μm or less, good tactile sensation such as moist, soft, and fluffy sensation is obtained. The average spacing of the hairs is determined by measuring the spacing between adjacent hairs at several points on the resin sheet, and calculating the arithmetic average value of the measured values.

[0040] The shape of the hair-like body is not particularly limited, but may be a shape in which the hair-like body extends in a direction away from the base layer and gradually becomes thinner as it approaches the tip, or a bulge may be formed at the tip. In other words, the shape may be such that the cross-sectional area gradually decreases as it moves away from the base layer, then increases once and terminates. The shape of the tip of the hair-like body may be bud-shaped or mushroom-shaped. The hair-like body may have a portion located at the base end extending in a direction away from the base layer, a portion extending from the portion located at the base end and bending with a constant curvature or gradually changing curvature, or even a portion wound in a spiral or spiral shape. In this case, the tip of the hair-like body may be folded inward. Such a shape produces a good tactile sensation. Furthermore, the bud-shaped or mushroom-shaped portion is hollow, which produces a better tactile sensation. When a bud or mushroom shape is formed at the tip of the hair, the ratio of the average diameter of the bud or mushroom shape to the average diameter of the hair is preferably 1.1 or more. The height of the bud or mushroom shape is preferably 7 μm or more. The average diameter of the hair, the average diameter of the width of the bud or mushroom shape, and the height are measured using an electron scanning microscope photograph, and the arithmetic average value is used. The hair is made of a thermoplastic resin. As the thermoplastic resin, the same resin as that usable in the above-mentioned undercoat layer can be used.

[0041] The thermoplastic resin contained in the underlayer and the hair may at least partially form a three-dimensional crosslinked structure (e.g., a three-dimensional network structure). For example, in one embodiment, at least a part of the hair may be crosslinked, in another embodiment, the entire surface of the hair may be crosslinked, and in yet another embodiment, the entire hair (from the boundary with the underlayer to the tip) may be crosslinked. Methods for forming a crosslinked body include, for example, a method of irradiating an electron beam onto a surface having hair after molding a resin sheet, and a method of adding an organic peroxide and forming the resin sheet by heating and humidifying during or after molding. Commercially available resins to which an organic peroxide has been added include "Linkron" manufactured by Mitsubishi Chemical Corporation. In this embodiment, it is preferable to form a crosslinked body (electron beam crosslinked body) by irradiating an electron beam.

[0042] <Resin sheet> In this embodiment, "tactile sensation" refers to the texture and feel of the surface of the resin sheet. It is determined whether the surface of the resin sheet feels comfortable to the touch, and if so, a good tactile sensation is one that feels moist, soft, fluffy, or other specific pleasant feel to the touch.

[0043] In one embodiment of the present invention, the thickness of the resin sheet refers to the sheet thickness that is the sum of the average height of the hair-like bodies and the average thickness of the base layer. The sheet thickness is preferably 65 μm to 1600 μm, more preferably 115 μm to 1050 μm, and even more preferably 165 μm to 550 μm. By making the thickness 65 μm or more, a good tactile sensation can be sufficiently ensured, and by making the thickness 1600 μm or less, the manufacturing cost can be reduced.

[0044] [Second embodiment] An example of the resin sheet according to the second embodiment of the present invention is a resin sheet in which a base layer is formed on the surface of the foundation layer opposite to the hair-like bodies, as shown in Fig. 3. That is, the layer structure of the resin sheet according to the second embodiment is, from top to bottom, the hair-like bodies, the foundation layer (1), and the base layer (2). Here, the hair-like body is the same as that described in the first embodiment, so the description will be omitted. However, the thickness of the hair-like body and the base layer, which is expressed by the sum of the average height of the hair-like body and the average thickness of the base layer, is preferably 150 μm to 1500 μm, more preferably 150 μm to 1050 μm, and even more preferably 150 μm to 500 μm. By making it 150 μm or more, good tactile sensation can be ensured, and by making it 1500 μm or less, production costs can be reduced. The average thickness of the base layer is preferably 50 μm to 1500 μm, more preferably 100 μm to 1000 μm, and further preferably 150 μm to 500 μm. By making it 50 μm or more, the film formation process becomes easy, and by making it 1500 μm or less, the production cost can be reduced. For the base layer in the resin sheet according to the second embodiment, a thermoplastic resin having excellent adhesiveness to the underlayer is preferably used, and polycarbonate-based resin, polyester-based resin, or polymer alloy resin thereof can be suitably used. The mass ratio of the polycarbonate-based resin to the polyester-based resin is preferably 50:50 to 90:10, more preferably 60:40 to 80:20, and even more preferably 65:35 to 75:25. Here, the polymer alloy resin refers to a polymer multi-component system, and may be a polymer blend having a certain degree of compatibility due to mixing or the like, a block copolymer or a graft copolymer obtained by copolymerization, or a mixture of resins that are not compatible with each other.

[0045] Examples of polycarbonate resins include those derived from aliphatic dihydroxy compounds and those derived from aromatic dihydroxy compounds. For example, those derived from aromatic dihydroxy compounds can be suitably used, and in particular, those derived from aromatic dihydroxy compounds (bisphenols) in which two aromatic dihydroxy compounds are bonded via a certain type of bonding group are preferred. These can be produced by a known method of polycondensation of a dihydroxy compound with phosgene or a carbonate ester, and are not limited to this method, and commercially available resins can also be used.

[0046] Examples of polyester-based resins that can be used include polyethylene terephthalate, polybutylene terephthalate, polyethylene-2,6-naphthalate, polymethylene terephthalate, and polyester resins copolymerized with, as a copolymerization component, a diol component such as diethylene glycol, neopentyl glycol, or polyalkylene glycol, or a dicarboxylic acid component such as adipic acid, sebacic acid, phthalic acid, isophthalic acid, or 2,6-naphthalenedicarboxylic acid.

[0047] The base layer may contain other additives as necessary. As other additives, within the range that does not impair the effects of the present invention, additives such as water repellents, oil repellents, pigments, dyes, and other colorants, lubricants and release agents such as silicone oil and alkyl esters, fibrous reinforcing agents such as glass fibers, fillers such as granular fine particles such as talc, clay, and silica, and scaly fine particles such as mica, low molecular weight antistatic agents such as salt compounds of sulfonic acid and alkali metals, high molecular weight antistatic agents such as polyether ester amides, flame retardants, antibacterial agents, antiviral agents, and heat stabilizers can be added. In addition, scrap resin generated in the resin sheet manufacturing process can be mixed and used. In addition, within the range that does not impair the effects of the present invention, the base layer may have a partially crosslinked structure.

[0048] [Manufacturing of resin sheets] The method for producing a resin sheet according to the present invention is not limited and may be any method, but typically includes a step of melt-extruding a raw resin and imparting regularly arranged hair-like bodies to at least one surface of the obtained extruded resin sheet.

[0049] Any resin sheet molding method can be used to prepare the multi-layer resin sheet. For example, a feed block or a multi-manifold die can be used. The layer structure of each embodiment of the resin sheet of the present invention is basically as described above. In addition, for example, scrap raw materials generated in the manufacturing process of the resin sheet or molded container of the present invention may be added to the base layer or laminated as an additional layer as long as there is no deterioration in physical properties, etc.

[0050] The method of providing the hair-like bodies is not particularly limited, and any method known to those skilled in the art can be used. For example, a method of manufacturing using an extrusion molding method, a method of manufacturing using a roll-to-roll method, a method of manufacturing using a photolithography method, a method of manufacturing using a heat press method, a method of manufacturing using a pattern roll and a UV-curable resin, a method of manufacturing using a 3D printer, a method of embedding the hair-like bodies in a resin layer and then covalently bonding them by a polymerization reaction, etc.

[0051] For example, when using an extrusion molding method, a resin sheet according to the present invention can be produced by extruding a resin sheet using a T-die method, and casting the resin sheet with a transfer roll having an uneven surface and a touch roll so as to impart a hair-like shape to the surface of the resin sheet. As the transfer roll having the unevenness processing, a roll surface having fine unevenness of several μm to several hundred μm in size can be used, which is formed regularly by laser engraving, electroforming, etching, mill engraving, or the like. Here, "regular" means that the unevenness is arranged in a non-random manner, that is, in a state where it is arranged orderly in one or two directions. In some embodiments, the unevenness can be arranged in a checkerboard arrangement arranged vertically and horizontally or a staggered arrangement. As the shape of the uneven portion, for example, in the case of the shape of the recess, a pyramid shape (a circular cone, a square pyramid, a triangular pyramid, a hexagonal pyramid, etc.), a semicircle, a rectangle (a square prism), etc. can be mentioned. As for the size, the opening diameter of the recess, the depth of the recess, and the interval between the recess shapes are several μm to several hundred μm. As the material of the transfer roll, for example, metal, ceramic, etc. can be used. The interval between the hair-like bodies can be adjusted by adjusting the interval between the recesses of the transfer roll, and the height of the hair-like bodies can be adjusted by adjusting the depth of the recesses of the transfer roll, and the touch can also be adjusted. It is also preferred to process the transfer roll surface into unevenness with a high aspect ratio. For example, when processing the recessed shape on the transfer roll surface, the aspect ratio (recess depth / recess opening diameter) is preferably 1.0 to 9.0 or 1.0 to 2.0. To process the transfer roll surface into unevenness with a high aspect ratio, a laser engraving method or an electroforming method is particularly preferably used since it is suitable for precise processing in the depth direction compared to an etching method, a blasting method, a mill engraving method, and the like. The transfer roll may be made of a material such as metal or ceramic. The touch roll may be made of various materials, such as silicone rubber, NBR rubber, EPT rubber, butyl rubber, chloroprene rubber, or fluororubber. In one embodiment, a touch roll having a rubber hardness (JIS K 6253) of 40 to 100 may be used. A Teflon (registered trademark) layer may be formed on the surface of the touch roll. The touch roll may be made of various materials, for example, silicone rubber, NBR rubber, EPT rubber, butyl rubber, chloroprene rubber, or fluororubber. In one embodiment, a touch roll having a rubber hardness (JIS K 6253) of 40 to 100 may be used. A Teflon (registered trademark) layer may be formed on the surface of the touch roll. By using the above-mentioned roll set of the transfer roll and the touch roll, the resin sheet of the present embodiment can be manufactured. In one embodiment, the temperature of the transfer roll is adjusted to a temperature near the crystalline melting temperature, glass transition point, or melting point of the thermoplastic resin (for example, 100 to 150°C when random polypropylene is used), and the pinch pressure between the transfer roll and the touch roll is adjusted to 30 to 120 kg / cm. 2 The resin sheet of this embodiment can be manufactured by casting the resin sheet as described above. The cast resin sheet is taken up at a line speed of 0.5 to 30 m / min using a pinch roll or the like. Although the above embodiments have been specifically described, the present invention is not limited to these.

[0052] [Molded products] The molded product of the present invention is a molded product using the resin sheet of the present invention. The resin sheet of the present invention can be applied to general molding, and the molding method includes insert molding, in-mold molding, general vacuum molding, pressure molding, and applications of these methods include a method of heating and softening a resin sheet in a vacuum state and releasing it under atmospheric pressure to overlay (mold) it onto the surface of an existing molded product, but is not limited thereto. In addition, as a method of heating and softening a sheet before molding, a known sheet heating method such as radiant heating using an infrared heater or the like, which is non-contact heating, can be applied. In a certain embodiment of vacuum pressure molding, for example, the resin sheet is heated at a surface temperature of 60°C to 220°C for 20 seconds to 480 seconds, and then molded onto the surface of an existing molded product, and can be stretched 1.05 to 2.50 times depending on the shape of the surface.

[0053] [Goods] The resin sheet having the hair-like bodies on its surface according to the present invention can be used in applications requiring the above-mentioned good tactile sensation. For example, the resin sheet of the present invention can be used as an automobile interior material, an electronic device exterior material, or a surface material for cosmetic containers.

[0054] Examples of automobile interior materials include steering wheels, dashboards, levers, switches, and the like, which are parts that are touched by the hands inside the automobile. For example, an interior material in which the above-mentioned resin sheet is molded and laminated on the surface of a known instrument panel or pillar (for example, JP 2009-184421 A) can be mentioned. By laminating the resin sheet, an interior material with good tactile sensation can be obtained. As the material of the resin sheet to be laminated, olefin resin, PVC resin, or urethane elastomer is preferable, taking into consideration light resistance and chemical resistance. The method of laminating the resin sheet and the interior material is not particularly limited.

[0055] Examples of the exterior material for electronic devices include transmitter housings for keyless entry systems, smartphone housings, smartphone cases, music player cases, game machine housings, digital camera housings, electronic notebook housings, calculator housings, tablet housings, mobile personal computer housings, keyboards, and mice. For example, a portable transmitter in which the resin sheet of the present invention is molded and bonded to the surface of a portable transmitter housing for a known keyless entry system (for example, JP-A-2005-228911) can be mentioned. By bonding the resin sheet, a portable transmitter with good tactile sensation can be obtained. As the material of the resin sheet to be bonded, an olefin resin or a urethane elastomer is preferable. The method for bonding the resin sheet to the housing is not particularly limited.

[0056] Examples of the cosmetic container include containers for face cream, pack cream, foundation, and eye shadow, and examples thereof include a cosmetic container in which the resin sheet of the present invention is molded and bonded to the surface of a cover member of a known foundation container (JP Patent Publication 2017-29608 A). By bonding the resin sheet, a cosmetic container with good tactile sensation can be obtained. As the material of the resin sheet to be bonded, an olefin-based resin or a urethane-based elastomer is preferable. The method of bonding the resin sheet is not particularly limited.

[0057] Furthermore, a hairy sheet can be produced by printing characters or patterns on the surface of the hairy body by a general printing method (offset printing, gravure printing, flexographic printing, screen printing, foil stamping, etc.) and applied to the above-mentioned applications. The material of the resin sheet to be printed is not particularly limited, but it is preferable to take into consideration the printability with the ink used for printing.

[0058] In addition, the resin sheet of the present invention can be laminated (dry laminate, extrusion laminate) with printed matter (paper, metal thin film, etc.) on which characters, patterns, etc. are printed, nonwoven fabric, etc. to produce a laminate, which can be laminated, for example, on the printed surface of a business card to produce a business card with a tactile feel. The material of the resin sheet to be laminated is not particularly limited. EXAMPLES

[0059] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to the contents of the examples. In the examples, "parts" are by weight.

[0060] The various raw materials used in the examples and the methods for producing them are as follows. (Polyol A-1) In a reactor equipped with an agitator, a thermometer, a heater, and a distillation column, 926 g of 1,6-hexanediol (hereinafter, 1,6HD) and 671 g of diethyl carbonate (hereinafter, DEC) were charged so that the molar ratio of 1,6-hexanediol (hereinafter, 1,6HD) to diethyl carbonate (hereinafter, DEC) was 1.38:1, and 0.05 g of tetrabutyl titanate (hereinafter, TBT) was further charged as a reaction catalyst, and the temperature was gradually increased to 190 ° C. under a nitrogen stream. When the distillation of ethanol slowed down and the top temperature of the distillation column became 50 ° C. or less, the reaction temperature was kept at 190 ° C. and the pressure was gradually reduced to 1.3 kPa, and the reaction was continued for another 7 hours at a pressure of 1.3 kPa or less. The reaction was further continued at a reaction temperature of 190 ° C. under a reduced pressure of 1.3 kPa or less until the hydroxyl value of the reaction product became 222 to 226 (mgKOH / g), and polyol A-1 was obtained. The hydroxyl value of Polyol A-1 was 224.4 (mgKOH / g), and the number average molecular weight was calculated to be 500. (Polyol A-2) Polyol A-2 was obtained by synthesizing in the same manner as for the production of Polyol B-1, except that 913 g of 1,6-HD and 686 g of DEC were charged so that the molar ratio of 1,6-HD and DEC was 1.33: 1. The hydroxyl value of Polyol A-2 was 172.6 (mgKOH / g), and the number average molecular weight was calculated to be 650. (Polyol A-3) Polyol A-3 was obtained by synthesizing in the same manner as for the production of Polyol B-1, except that 898 g of 1,6-HD and 700 g of DEC were charged so that the molar ratio of 1,6-HD and DEC was 1.28: 1. The hydroxyl value of Polyol A-3 was 149.6 (mgKOH / g), and the number average molecular weight was calculated to be 750. (Polyol A-4) Polyol A-4 was obtained by synthesizing in the same manner as for the production of Polyol B-1, except that 878 g of 1,6-HD and 720 g of DEC were charged so that the molar ratio of 1,6-HD and DEC was 1.22: 1. The hydroxyl value of Polyol A-4 was 132.0 (mgKOH / g), and the number average molecular weight was calculated to be 850. (Polyol A-5) Polyol A-5 was obtained by synthesizing in the same manner as for the production of Polyol B-1, except that 938 g of 1,6-HD and 660 g of DEC were charged so that the molar ratio of 1,6-HD and DEC was 1.42: 1. The hydroxyl value of Polyol A-5 was 280.5 (mgKOH / g), and the number average molecular weight was calculated to be 400. (Polyol A-6) Polyol A-6 was obtained by synthesizing in the same manner as in the production of Polyol B-1, except that 872 g of 1,6-HD and 726 g of DEC were charged so that the molar ratio of 1,6-HD and DEC was 1.20: 1. The hydroxyl value of Polyol A-6 was 118.1 (mgKOH / g), and the number average molecular weight was calculated to be 950. The number average molecular weight was calculated based on the following formula. Number average molecular weight = (56100 x 2) / hydroxyl value (The hydroxyl value of the polycarbonate diol was determined by titration in accordance with JIS K 1557. The unit of the hydroxyl value is mgKOH / g. The acid value of the polycarbonate diol was determined by titration in accordance with JIS K 1557. The unit of the acid value is mgKOH / g. (B) Aliphatic diol: 1,4-butanediol (C-1) Diisocyanate: Hexamethylene diisocyanate (HDI) (C-2) Diisocyanate: 4,4'-diphenylmethane diisocyanate (MDI) (D) Release agent masterbatch "Wax Master V" (manufactured by BASF) (E) PC / polyester resin "PCX-6694" (manufactured by Sumika Polycarbonate Co., Ltd.)

[0061] (Production of TPU for capillaries and base layer) Polyol (A) and aliphatic diol (B) were added to a reaction vessel equipped with a stirrer and thermometer and mixed uniformly to obtain the composition shown in Table 1. The resulting mixture was heated to 100°C, after which diisocyanate (C) was added and forcibly stirred with a hand mixer. When the reaction temperature reached 130°C, the mixture was poured onto release paper and solidified. The resulting solid was aged in an electric furnace at 120°C for 1 hour and cooled to room temperature, after which the solid was pulverized to obtain flake-shaped TPU. The obtained flake-like TPU was compounded with (D) a release agent master batch in a weight ratio of 95:5 in a twin-screw extruder, and the obtained strands were granulated to obtain TPU pellets (G) that would be used as the raw material for the capillary body and undercoat layer.

[0062] (Production of resin sheet having hair-like bodies) [Examples 1 to 6, Comparative Examples 1 to 3] The above TPU (G) which becomes the capillary body and the undercoat layer is poured from one 40 mm single screw extruder, and the (E) PC / polyester resin which becomes the base layer is poured from one 65 mm single screw extruder, and the resin sheet extruded by the T-die method is unevenly processed by chromium oxide spraying and laser engraving, and is cast using a transfer roll which is unevenly processed and adjusted to 60 ° C to 150 ° C, and a touch roll made of silicon-based rubber with a rubber hardness of 70 adjusted to 10 ° C to 90 ° C, and is taken up at a line speed of 1 m / min to 15 m / min using a pinch roll. As a result, a resin sheet having the composition, thickness and surface shape shown in Table 1 was obtained.

[0063] The methods for evaluating various properties of the resin sheets produced in the examples and comparative examples and the molded products obtained by vacuum and pressure molding of the resin sheets are as follows.

[0064] (1) Average height of hairs, average length of hairs, average diameter of hairs, average spacing of hairs, average thickness of base layer The height (h) of the hairs of the resin sheet, the diameter (d) of the hairs, the interval (t) of the hairs, the thickness of the base layer, and the thickness of the base layer were measured using a laser microscope (VK-X100, manufactured by Keyence Corporation). The measured samples were cut out from three arbitrary locations of the resin sheet using a microtome. The average height of the hairs was measured by measuring the height of 10 hairs for each sample, and the arithmetic average value of the 30 measured values ​​was used. For the average diameter of the hairs, the diameter of 10 hairs at the mid-height (h / 2) for each sample was measured, and the arithmetic average value of the 30 measured values ​​was used. For the average interval of the hairs, the distance between the center of the root of the hairs and the center of the root of the adjacent hairs was measured at 10 locations for each sample, and the arithmetic average value of the 30 measured values ​​was used. For the average thickness of the base layer, the thickness from the root of the hairs to the interface of the other layer was measured at 10 locations for each sample, and the arithmetic average value of the 30 measured values ​​was used. The average thickness of the base layer was measured at 10 points for each sample from the boundary with the undercoat layer to the interface opposite the side having the hairs, and the arithmetic mean value of the 30 measured values ​​was used.

[0065] (2) Evaluation of texture after secondary molding The obtained resin sheet was subjected to insert molding. A mold for an injection insert molding machine capable of obtaining a resin plate having a width of 250 mm, a length of 140 mm, and a thickness of 3 mm was prepared, and the resin sheet was trimmed so that the resin sheet fit snugly on the surface formed by the width of 250 mm and the length of 140 mm. The trimmed resin sheet was arranged so that the surface having the hair-like bodies contacted the mold surface and the base material layer faced the wood species flow side of the cavity. The mold had a single gate on the surface formed by the width of 250 mm and the thickness of 3 mm, and the injected resin flowed in parallel with the resin sheet. A PC resin heated to 280 ° C and molten was injected into the mold in which such a resin sheet was arranged, using an injection molding machine, to obtain an insert molded product of a resin sheet having hair-like bodies. For the good tactile sensation, a sensory evaluation was conducted by having a total of 10 external panelists, 5 men and 5 women, touch the resin sheet. The specific tactile sensation (smooth, silky, moist, dry, rough, etc.) when touching the surface of the resin sheet was evaluated on a scale of 10 points, and the tactile sensation with the highest score was regarded as the tactile sensation of the surface of the resin sheet. In Table 1, "◯" indicates that the score for smooth, silky, or moist was high, and that a good tactile sensation like a suede-like raised sheet was obtained even after secondary molding. "X" indicates that the score for dry or rough was high, and that a good tactile sensation was not obtained after secondary molding.

[0066] Using the resin sheets obtained in each of the Examples and Comparative Examples, evaluation tests were carried out for various properties, and the results are shown in Table 1.

[0067] [Table 1]

[0068] The results shown in Table 1 reveal the following: All of the resin sheets of Examples 1 to 6 maintained a good tactile feel even after secondary molding. On the other hand, the resin sheet of Comparative Example 1 was a resin sheet in which component (A) was derived from a polyol having a number average molecular weight of 950 and the molar ratio of component (A) to component (B) was 90:10, but the hair-like bodies were significantly deformed by secondary molding, and the feel was dry and not good. The resin sheet of Comparative Example 2 was a resin sheet having a molar ratio of component (A) to component (B) of 92:8, but the hair-like bodies were significantly deformed by secondary molding, and the feel was dry and not good. The resin sheet of Comparative Example 3 was a resin sheet in which component (A) was derived from a polyol having a number average molecular weight of 400 and the molar ratio of component (A) to component (B) was 58:42. Although the hair-like bodies were maintained even after secondary molding, the thermoplastic resin composition constituting the base layer and the hair-like bodies was hard and rough to the touch, and did not have a good touch either before or after secondary molding.

[0069] Although the present invention has been described above using various embodiments, it goes without saying that the technical scope of the present invention is not limited to the scope described in the above embodiments. It is clear to those skilled in the art that various modifications and improvements can be made to the above embodiments. In addition, it is clear from the description of the claims that forms with such modifications or improvements can also be included in the technical scope of the present invention. [Industrial Applicability]

[0070] The resin sheet of the present embodiment can maintain a good tactile feel even after secondary molding, and therefore has industrial applicability as a resin sheet capable of secondary molding and a molded product thereof. [Explanation of symbols]

[0071] 1. Hairy body and base layer 1a Base layer 1b Ciliary body d Hair diameter h Height of the hair t Hair spacing 2 Base material layer

Claims

1. A thermoplastic resin sheet having regularly arranged hair-like bodies on at least one surface of a base layer, with no structural boundary between the base layer and the hair-like bodies forming a continuous phase, wherein a thermoplastic resin composition constituting the base layer and the hair-like bodies contains a urethane-based elastomer, the urethane-based elastomer containing a component (A) derived from a polyol having a number average molecular weight of 450 to 900 and a component (B) derived from an aliphatic diol having 2 to 10 carbon atoms, and the molar ratio of (A) to (B) is 60:40 to 88:

12.

2. 2. The resin sheet according to claim 1, wherein the average height of the hairs is 30 μm or more and 500 μm or less, the average diameter of the hairs is 1 μm or more and 50 μm or less, and the average spacing between the hairs is 20 μm or more and 200 μm or less.

3. The resin sheet according to claim 1 or 2, wherein the polyol is a polycarbonate-based diol.

4. The resin sheet according to claim 1 or 2, further comprising a base layer on a surface of the undercoat layer opposite to the hair-like bodies.

5. A molded product made from the resin sheet according to claim 1 or 2.

6. The molded article according to claim 5, which is an insert molded article or a vacuum molded article.

7. The molded article according to claim 5 , which is provided on the surface of an automobile interior material, an electronic device exterior material, or a cosmetic container.

Citation Information

Patent Citations

  • Laminate and its manufacture

    JP1997248891A

  • Resin sheet with hair-like body and molded product thereof

    JP2020189420A

  • JPP7446284B

  • Double-cast slush molding compositions

    US20100310843A1