Positive electrode active material precursor for secondary battery, positive electrode active material, and lithium secondary battery including the same

The development of a lithium transition metal oxide with aligned crystal planes and radial primary particle structure addresses the structural instability of high-nickel NCM-based materials, improving the life and resistance of lithium secondary batteries.

JP7562207B2Active Publication Date: 2024-10-07LG CHEM LTD
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2022546106
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-01-29
Filing Date
2021-01-29
Publication Date
2024-10-07
Estimated Expiration
2041-01-29

AI Technical Summary

Technical Problem

Existing lithium cobalt oxide-based positive electrode active materials face challenges with high cost, supply instability, and structural instability in high-nickel NCM-based materials, leading to reduced lifetime and resistance characteristics in lithium secondary batteries.

Method used

A positive electrode active material precursor is developed with a specific hydroxide composition (Ni x1 Co y1 Mn z1 Al s1 (OH) 2, where primary particles are aligned radially and crystal grains have parallel (001) planes, formed through controlled coprecipitation of transition metal and aluminum solutions, followed by firing with a lithium source to create a lithium transition metal oxide (Li a [Ni b Co c Mn d Al e ] 1-f M 1 f O 2) with aligned (003) planes.

Benefits of technology

The solution enhances the life characteristics and resistance of lithium secondary batteries by ensuring uniform aluminum distribution, improved lithium mobility, and structural stability, resulting in superior capacity retention and reduced resistance increase.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007562207000002
    Figure 0007562207000002
  • Figure 0007562207000003
    Figure 0007562207000003
  • Figure 0007562207000004
    Figure 0007562207000004
Patent Text Reader

Abstract

The present invention relates to a cathode active material precursor, a method for producing the same, and a cathode active material produced using the cathode active material precursor. The cathode active material precursor of the present invention is a cathode active material precursor made of a hydroxide represented by Chemical Formula 1, and the cathode active material precursor is a secondary particle formed by aggregating a plurality of primary particles, the major axes of the primary particles are aligned in a direction from the center toward the surface of the secondary particle, and the primary particles include crystal grains whose (001) planes are aligned parallel to the major axes of the primary particles.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This application claims the benefit of priority based on Korean Patent Application No. 10-2020-0010699, filed on January 29, 2020, the entire contents of which are incorporated herein by reference.

[0002] The present invention relates to a positive electrode active material precursor for a secondary battery, a positive electrode active material, a method for producing the same, and a lithium secondary battery including the same. [Background technology]

[0003] Recently, with the rapid spread of electronic devices using batteries, such as mobile phones, notebook computers, and electric vehicles, the demand for secondary batteries that are small, lightweight, and have a relatively high capacity is rapidly increasing. In particular, lithium secondary batteries are lightweight and have high energy density, and are in the spotlight as a driving power source for portable devices. Therefore, active research and development efforts are being made to improve the performance of lithium secondary batteries.

[0004] In a lithium secondary battery, an organic electrolyte or polymer electrolyte is charged between a positive electrode and a negative electrode, which are made of active materials that allow the intercalation and deintercalation of lithium ions, and electrical energy is generated through oxidation and reduction reactions that occur when lithium ions are inserted and deintercalated at the positive and negative electrodes.

[0005] Lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), lithium manganese oxide (LiMnO2 or LiMn2O4, etc.), lithium iron phosphate compound (LiFePO4), etc. have been used as positive electrode active materials for lithium secondary batteries. Among them, lithium cobalt oxide (LiCoO2) is widely used due to its advantages of high operating voltage and excellent capacity characteristics, and is applied as a positive electrode active material for high voltage. However, due to the rising price of cobalt (Co) and unstable supply, there are limitations to its mass use as a power source in fields such as electric vehicles, and there is an increasing need to develop alternative positive electrode active materials.

[0006] Therefore, nickel-cobalt-manganese-based lithium composite transition metal oxides (hereinafter simply referred to as "NCM-based lithium composite transition metal oxides") have been developed in which part of the cobalt (Co) is replaced with nickel (Ni) and manganese (Mn). Recently, with the increasing demand for high-capacity batteries, technology is being researched to increase the capacity by increasing the nickel content in NCM-based positive electrode active materials. In the case of high-nickel NCM-based positive electrode active materials containing a high concentration of nickel, although the capacity characteristics are excellent, there is a problem that the structural stability is low and the life characteristics are deteriorated. Therefore, a method of doping high-nickel NCM-based positive electrode active materials with Al to improve the structural stability has been proposed. Conventionally, methods of doping Al into NCM-based positive electrode active materials have been used, such as a dry doping method in which an aluminum-containing raw material is mixed together with a positive electrode active material precursor and a lithium raw material when the positive electrode active material precursor is mixed, and then calcined, or a wet doping method in which a coprecipitation reaction is performed using a metal solution containing nickel, manganese, cobalt, and aluminum during the production of the positive electrode active material precursor to dope the precursor with Al.

[0007] However, in the case of dry doping, aluminum (Al) is difficult to distribute uniformly in the NCM-based positive electrode active material, and there is a problem that it is difficult to control the doping into the lithium layer. In addition, in the case of aluminum (Al) wet doping in which aluminum (Al) is doped during coprecipitation of the NCM-based positive electrode active material precursor, if aluminum cations are dissolved in a transition metal solution containing nickel, cobalt, manganese cations as in the past, an undesired side reaction with the anions occurs, hindering the growth of the precursor or making it difficult to control the crystal orientation.

[0008] Therefore, there is a need to develop a positive electrode active material precursor and a positive electrode active material that can exhibit excellent life characteristics and resistance characteristics when applied to a lithium secondary battery. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] Korean Patent Publication No. 2017-0063418 Summary of the Invention [Problem to be solved by the invention]

[0010] An object of the present invention is to provide a positive electrode active material precursor that can significantly improve the life characteristics and resistance increase when applied to a lithium secondary battery, and a method for producing the same.

[0011] Another object of the present invention is to provide a positive electrode active material produced using the positive electrode active material precursor, and a positive electrode for a secondary battery and a lithium secondary battery including the same. [Means for solving the problem]

[0012] The present invention provides a positive electrode active material precursor for a secondary battery, which is made of a hydroxide represented by the following chemical formula 1, wherein the positive electrode active material precursor is a secondary particle formed by agglomeration of a plurality of primary particles, the major axes of the primary particles are aligned in a direction from the center toward the surface of the secondary particle, and the primary particles include crystal grains whose (001) planes are aligned parallel to the major axes of the primary particles. [Chemical formula 1] Ni x1 Co y1 Mn z1 Al s1 (OH)2 In the above formula 1, 0.7≦x1≦0.99, 0 <y1<0.3、0<z1<0.3、0.01≦s1≦0.1である。

[0013] The present invention also provides a method for producing a positive electrode active material precursor for a secondary battery, the method comprising the steps of: preparing a transition metal-containing solution containing nickel (Ni), cobalt (Co) and manganese (Mn) cations and an aluminum-containing solution containing aluminum (Al) cations; and introducing the transition metal-containing solution and the aluminum-containing solution into a reactor, respectively, and introducing a basic aqueous solution and an ammonium solution to carry out a co-precipitation reaction to form a positive electrode active material precursor.

[0014] In addition, the present invention provides a method for preparing a positive electrode active material for a secondary battery, comprising mixing the positive electrode active material precursor prepared as above with a lithium source and calcining the mixture to form a lithium transition metal oxide.

[0015] The present invention also provides a positive electrode active material for a secondary battery, comprising a lithium transition metal oxide represented by the following chemical formula 2, the lithium transition metal oxide being a secondary particle formed by agglomeration of a plurality of primary particles, the major axes of the primary particles being aligned in a direction from the center to the surface of the secondary particle, and the primary particles including crystal grains having (003) planes aligned parallel to the major axes of the primary particles: [Chemical formula 2] Li a [Ni b Co c Mn d Al e ]1-f M 1 f O2 In the above Chemical Formula 2, M 1 is one or more selected from the group consisting of Zr, B, W, Mg, Ce, Hf, Ta, La, Ti, Sr, Ba, F, P and S, and 0.8≦a≦1.2, 0.7≦b≦0.99, 0 <c<0.3、0<d<0.3、0.01≦e≦0.1、0≦f≦0.1である。

[0016] The present invention also provides a positive electrode and a lithium secondary battery each containing the positive electrode active material. Effect of the Invention

[0017] According to the present invention, it is possible to provide a positive electrode active material precursor capable of significantly improving life characteristics and resistance increase, and a positive electrode active material produced using the same.

[0018] Furthermore, the life characteristics and resistance characteristics of a lithium secondary battery using the positive electrode active material can be significantly improved. [Brief description of the drawings]

[0019] [Figure 1] 1 is a TEM image of a cross section of a positive electrode active material precursor prepared in Example 1. [Diagram 2] 3 is a TEM image of a cross section of the positive electrode active material produced in Example 2. [Diagram 3] 1 is a SEM image of a positive electrode active material precursor prepared in Comparative Example 1. [Figure 4] 1 is a TEM image of a cross section of a positive electrode active material prepared in Comparative Example 2. [Diagram 5] 1 is a graph showing cycle characteristics of lithium secondary batteries using the positive electrode active materials produced in Example 2 and Comparative Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] In the following, the present invention will be described in more detail in order to facilitate understanding of the present invention. The terms and words used in the present specification and claims should not be interpreted as being limited to their ordinary or dictionary meanings, but should be interpreted as meanings and concepts that are consistent with the technical idea of ​​the present invention, based on the principle that the inventors can appropriately define the concepts of terms in order to best describe their invention.

[0021] In the present invention, the term "crystalline" refers to a single crystal particle unit having a regular atomic arrangement. In the present invention, the arrangement of crystal planes of a crystalline may be confirmed by analyzing a cross section of a cathode active material precursor or a cathode active material particle to be measured using a transmission electron microscope (TEM), and the TEM analysis may be performed using a selected area diffraction pattern (SADP) and / or a fast Fourier transform (FFT).

[0022] In the present invention, the term "primary particle" refers to the smallest particle unit that can be distinguished as a single mass when a cross section of a positive electrode active material particle or a positive electrode active material precursor particle is observed through a transmission electron microscopy (TEM), and may consist of one crystal grain or multiple crystal grains.

[0023] In the present invention, the aspect ratio of the primary particles may be calculated by measuring the length of a minor axis and the length of a major axis of each primary particle in a TEM image of a cross section of a positive electrode active material precursor or a positive electrode active material particle, and then calculating the ratio of the length of the major axis to the length of the minor axis. The average value may be measured by determining an arithmetic average value of the aspect ratios of each measured primary particle.

[0024] In the present invention, the term "secondary particles" refers to a secondary structure formed by the aggregation of a plurality of primary particles. The average particle size of the secondary particles can be measured using a particle size analyzer, and in the present invention, a Microtrac S3500 was used as the particle size analyzer.

[0025] In the present invention, the "particle size Dn" of the positive electrode active material means the particle size at the n% point of the volume cumulative distribution of particle size. 50 is the particle size at the 50% point of the cumulative volume distribution by particle size, and D 90 is the particle size at the 90% point of the volume cumulative distribution by particle size, D 10 is the particle size at the 10% point of the cumulative volume distribution by particle size. The above Dn can be measured using the laser diffraction method. Specifically, the powder to be measured is dispersed in a dispersion medium (distilled water), and then introduced into a commercially available laser diffraction particle size measuring device (e.g., Microtrac S3500). When the particles pass through a laser beam, the difference in the diffraction pattern due to the particle size is measured to calculate the particle size distribution. By calculating the particle sizes at the 10%, 50%, and 90% points of the cumulative volume distribution by particle size in the measuring device, D 10 , D 50 and D. 90 can be measured.

[0026] <Positive electrode active material precursor> First, a method for producing a positive electrode active material precursor according to the present invention will be described.

[0027] The method for producing a positive electrode active material precursor of the present invention includes the steps of preparing a transition metal-containing solution containing nickel (Ni), cobalt (Co), and manganese (Mn) cations and an aluminum-containing solution containing aluminum (Al) cations, and adding the transition metal-containing solution and the aluminum-containing solution to a reactor, and then adding a basic aqueous solution and an ammonium solution to cause a co-precipitation reaction to form a positive electrode active material precursor.

[0028] The method for producing the positive electrode active material precursor will now be described in detail step by step.

[0029] First, a transition metal-containing solution containing cations of nickel (Ni), cobalt (Co) and manganese (Mn) and an aluminum-containing solution containing cations of aluminum (Al) are prepared.

[0030] The transition metal-containing solution can include, for example, a nickel (Ni)-containing source material, a cobalt (Co)-containing source material, and a manganese (Mn)-containing source material.

[0031] The nickel (Ni)-containing raw material may be, for example, a nickel-containing acetate, nitrate, sulfate, halide, sulfide, hydroxide, oxide, or oxyhydroxide, and specifically may be, but is not limited to, Ni(OH)2, NiO, NiOOH, NiCO3·2Ni(OH)2·4H2O, NiC2O2·2H2O, Ni(NO3)2·6H2O, NiSO4, NiSO4·6H2O, fatty acid nickel salt, nickel halide, or a combination thereof.

[0032] The cobalt (Co)-containing raw material may be a cobalt-containing acetate, nitrate, sulfate, halide, sulfide, hydroxide, oxide, or oxyhydroxide, and specifically may be Co(OH)2, CoOOH, Co(OCOCH3)2·4H2O, Co(NO3)2·6H2O, CoSO4, Co(SO4)2·7H2O, or a combination thereof, but is not limited thereto.

[0033] The manganese (Mn)-containing raw material may be, for example, a manganese-containing acetate, nitrate, sulfate, halide, sulfide, hydroxide, oxide, oxyhydroxide, or a combination thereof, and specifically may be manganese oxides such as Mn2O3, MnO2, and Mn3O4; manganese salts such as MnCO3, Mn(NO3)2, MnSO4, manganese acetate, manganese dicarboxylate, manganese citrate, and manganese fatty acid salt; manganese oxyhydroxide, manganese chloride, or a combination thereof, but is not limited thereto.

[0034] The transition metal-containing solution may be prepared by adding a nickel (Ni)-containing raw material, a cobalt (Co)-containing raw material, and a manganese (Mn)-containing raw material to a solvent, specifically, water or a mixed solvent of an organic solvent (e.g., alcohol, etc.) that is uniformly miscible with water, or by mixing an aqueous solution of a nickel (Ni)-containing raw material, an aqueous solution of a cobalt (Co)-containing raw material, and a manganese (Mn)-containing raw material. Meanwhile, the transition metal-containing solution may contain 70 atm% to 99 atm%, 80 atm% to 98 atm%, 85 atm% to 98 atm%, or 88 atm% to 95 atm% of nickel among the total transition metals.

[0035] In addition, the transition metal-containing solution may contain cobalt in a concentration of more than 0 atm% and less than 0.3 atm%, 0.01 atm% or more and less than 0.2 atm%, 0.01 atm% or more and less than 0.15 atm%, or 0.01 atm% or more and less than 0.12 atm% of all transition metals.

[0036] Furthermore, the transition metal-containing solution may contain manganese among all transition metals at more than 0 atm% and less than 0.3 atm%, at least 0.01 atm% and less than 0.2 atm%, at least 0.01 atm% and less than 0.15 atm%, or at least 0.01 atm% and less than 0.12 atm%.

[0037] The aluminum (Al)-containing solution includes an aluminum (Al)-containing source material, and the aluminum (Al)-containing source material may be, for example, aluminum chloride, aluminum acetate, aluminum nitrate, aluminum hydroxide, or a combination thereof, but is not limited thereto.

[0038] The aluminum (Al)-containing solution may be prepared by adding an aluminum (Al)-containing raw material to a solvent, specifically, water or a mixed solvent of an organic solvent (e.g., alcohol, etc.) that is uniformly miscible with water.

[0039] Next, the transition metal-containing solution and the aluminum-containing solution are respectively charged into a reactor, and then a basic aqueous solution and an ammonium solution are charged to cause a coprecipitation reaction to form a positive electrode active material precursor.

[0040] In the manufacturing method according to an embodiment of the present invention, the transition metal-containing solution and the aluminum-containing solution are respectively introduced into a reactor. In the past, when manufacturing an aluminum-doped cathode active material precursor, it was common to mix nickel-containing raw material, cobalt-containing raw material, manganese-containing raw material, and aluminum-containing raw material to prepare a metal aqueous solution, and then co-precipitate the metal aqueous solution to form precursor particles. However, according to this conventional method, aluminum cations contained in the metal aqueous solution react with anions present in the metal aqueous solution to form aluminum sulfate, which can be an obstacle to particle growth. In particular, when the nickel content of the metal aqueous solution is 70 atm% or more and the aluminum content is 1 atm% or more, this problem becomes particularly prominent, making it difficult to manufacture a precursor of the desired size.

[0041] However, according to one embodiment of the present invention, when a transition metal-containing solution containing nickel, cobalt, and manganese and an aluminum-containing solution are separately prepared and then introduced into a reactor, the growth of the precursor particles is not inhibited and the precursor particles can be grown to a desired size even when the nickel content is 70 atm% or more and the aluminum content is 1 mol% or more.

[0042] In addition, when a coprecipitation reaction is performed using a transition metal-containing solution and an aluminum-containing solution that are separately prepared as in the present invention, the orientation of the primary particles and the arrangement of the crystal planes can be specified and controlled. Specifically, when a positive electrode active material precursor is produced by the method of the present invention, a positive electrode active material precursor can be produced that includes crystal grains in which the major axes of the primary particles are aligned in a direction from the center to the surface of the secondary particles and the (001) plane is arranged parallel to the major axes of the primary particles.

[0043] On the other hand, the arrangement of the primary particles and the crystal grain structure of the positive electrode active material are influenced by the arrangement of the primary particles and the crystal grain structure of the positive electrode active material precursor. When a positive electrode active material is manufactured using a positive electrode active material precursor having a structure in which the major axis of the primary particles is arranged in a direction from the center to the surface of the secondary particles, i.e., a radial arrangement structure, the primary particles of the positive electrode active material are also arranged in a direction from the center to the surface of the secondary particles. On the other hand, since lithium ions move along the interface between the primary particles in the positive electrode active material particles, when the primary particles are arranged radially, the migration path of the lithium ions inside the particles is shortened, and the effect of improving lithium mobility can be obtained.

[0044] Meanwhile, the (001) plane of the positive electrode active material precursor is converted to a (003) plane after firing. Therefore, a positive electrode active material manufactured using a positive electrode active material precursor containing crystal grains whose (001) planes are arranged parallel to the long axis of the primary particles contains crystal grains whose (003) planes are arranged parallel to the long axis of the primary particles. In lithium transition metal oxides, the (003) plane is a stable crystal plane that does not allow lithium to be inserted / extracted. When the (003) plane is arranged parallel to the long axis of the primary particles, the stable (003) plane is widely formed on the surface of the primary particles, which can minimize structural deterioration due to insertion / extraction of lithium ions and improve life characteristics.

[0045] Meanwhile, the transition metal-containing solution and the aluminum-containing solution may be added in amounts such that the molar ratio of the total transition metals (i.e., Ni+Co+Mn) contained in the transition metal-containing solution to the aluminum contained in the aluminum-containing solution is 0.99:0.01-0.90:0.10, preferably 0.99:0.01-0.92:0.08, and more preferably 0.99:0.01-0.95-0.05. When the amounts of the transition metal-containing solution and the aluminum-containing solution added satisfy the above ranges, a cathode active material precursor having a desired composition can be prepared.

[0046] Meanwhile, the ammonium solution may contain, as a complexing agent, for example, but not limited to, NH4OH, (NH4)2SO4, NH4NO3, NH4Cl, CH3COONH4, (NH4)2CO3, or a combination thereof. Meanwhile, the ammonium solution may be used in the form of an aqueous solution, and in this case, the solvent may be water or a mixture of water and an organic solvent (e.g., alcohol, etc.) that is uniformly miscible with water.

[0047] The basic solution may contain an alkali compound such as a hydroxide of an alkali metal or an alkaline earth metal, a hydrate thereof, or a combination thereof, such as NaOH, KOH, or Ca(OH)2, as a precipitant. The basic solution may also be used in the form of an aqueous solution, and in this case, the solvent may be water or a mixture of water and an organic solvent (e.g., alcohol, etc.) that is uniformly miscible with water.

[0048] The basic compound is added to adjust the pH of the reaction solution, and the amount of the basic compound can be adjusted so that the pH of the reaction solution during the coprecipitation reaction is maintained at 10.5 to 12.2, more preferably at 11.0 to 11.5, and even more preferably at 11.3 to 11.45.

[0049] On the other hand, the coprecipitation reaction can be carried out under an inert atmosphere such as nitrogen or argon, and the temperature inside the reactor during the coprecipitation reaction can be 45 to 65°C, more preferably 50 to 60°C, and even more preferably 53 to 58°C.

[0050] When the pH of the reaction solution, the temperature of the reactor, and the atmosphere satisfy the above conditions, the crystallinity of the precursor particles increases, and the ratio of the (001) plane increases, which can improve the life characteristics.

[0051] Next, the positive electrode active material precursor according to the present invention will be described.

[0052] The cathode active material precursor according to the present invention is produced by the method of the present invention, and is made of a hydroxide represented by the following chemical formula 1, and is a secondary particle formed by agglomeration of a plurality of primary particles, the major axes of the primary particles are aligned in a direction from the center to the surface of the secondary particle, and the primary particles include crystal grains whose (001) planes are aligned parallel to the major axes of the primary particles:

[0053] [Chemical formula 1] Ni x1 Co y1 Mn z1 Al s1 (OH)2

[0054] The x1 represents a molar ratio of nickel to all metal elements in the transition metal hydroxide, and may be 0.7≦x1≦0.99, 0.8≦x1≦0.98, 0.85≦x1≦0.98, or 0.88≦x1≦0.95. When the nickel content in the transition metal hydroxide satisfies the above range, a positive electrode active material having high capacity characteristics can be produced.

[0055] The y1 represents a molar ratio of cobalt to the total metal elements in the transition metal hydroxide, and is 0 <y1<0.3、0.01≦y1<0.2、0.01≦y1<0.14、または0.01≦y1<0.12であることができる。

[0056] The z1 represents a molar ratio of manganese to all metal elements in the transition metal hydroxide, and is 0 <z1<0.3、0.01≦z1<0.2、0.01≦z1<0.14、または0.01≦z1<0.12であることができる。

[0057] The s1 represents a molar ratio of aluminum to all metal elements in the transition metal hydroxide, and may be 0.01≦s1≦0.1, 0.01≦s1≦0.08, or 0.01≦s1≦0.05. When the aluminum (Al) content in the transition metal hydroxide satisfies this range, cation disordering and the formation of oxygen vacancies can be suppressed during the preparation of a positive electrode active material, thereby improving the life characteristics and resistance increase rate characteristics.

[0058] Meanwhile, the positive electrode active material precursor preferably has aluminum (Al) uniformly distributed throughout the particle. That is, aluminum may be contained without a concentration gradient within the secondary particles of the positive electrode active material precursor. By uniformly distributing aluminum (Al) within the secondary particles without a concentration gradient, the entanglement of aluminum (Al) is suppressed, minimizing capacity loss, and improving life characteristics and resistance increase rate characteristics with a small amount of aluminum (Al).

[0059] Preferably, the positive electrode active material precursor of the present invention can be one in which nickel, manganese, cobalt and aluminum are distributed in uniform concentrations throughout the secondary particles without concentration gradients.

[0060] Meanwhile, the cathode active material precursor according to the present invention may be a secondary particle formed by agglomeration of a plurality of primary particles, and the major axis of the primary particle may be arranged in a direction from the center to the surface of the secondary particle. As described above, the primary particle orientation of the cathode active material shows the same tendency as the primary particle orientation of the cathode active material precursor, and since lithium ions move along the interface between the primary particles in the cathode active material particles, when the cathode active material has a structure in which the major axis of the primary particle is arranged in a direction from the center to the surface of the secondary particle, i.e., a radial structure, the migration path of the lithium ions inside the cathode active material particles is shortened, and the effect of improving lithium mobility can be obtained.

[0061] In addition, the primary particles of the cathode active material precursor according to the present invention include crystal grains whose (001) planes are arranged parallel to the long axis of the primary particles. The (001) plane of the cathode active material precursor is converted to a (003) plane after sintering, and thus the primary particles of the cathode active material prepared using the cathode active material precursor containing such crystal grains include crystal grains whose (003) planes are arranged parallel to the long axis of the primary particles. When the (003) planes are arranged parallel to the long axis of the primary particles, the area of ​​the (003) planes exposed at the interface between the primary particles becomes large. Since the (003) plane is a stable crystal plane into which lithium ions cannot be inserted / extracted, when the external exposed area of ​​the (003) plane is large, the structural deterioration of the active material due to the insertion / extraction of lithium ions is suppressed, and thus the effect of improving the life characteristics can be obtained.

[0062] Meanwhile, the primary particles of the positive electrode active material precursor may be columnar, and in this case, the aspect ratio of the primary particles may be 3 or more. More preferably, the aspect ratio of the primary particles of the positive electrode active material precursor may be 3 to 15, and further preferably 5 to 8. When the aspect ratio of the primary particles of the positive electrode active material precursor satisfies the above range, there is an effect that the lithium migration path between the inside and outside of the primary particles can be shortened.

[0063] The average particle size D of the secondary particles of the positive electrode active material precursor of the present invention 50When the average particle size of the secondary particles of the positive electrode active material precursor falls within the above range, advantageous effects can be obtained in terms of energy density, life, and gas generation.

[0064] <Cathode active material> Next, the positive electrode active material and the method for producing the same according to the present invention will be described.

[0065] The positive electrode active material according to the present invention can be prepared by mixing the positive electrode active material precursor of the present invention and a lithium source, and calcining the mixture to form a lithium transition metal oxide.

[0066] The positive electrode active material precursor is as described above.

[0067] The lithium source may be a lithium-containing sulfate, nitrate, acetate, carbonate, oxalate, citrate, halide, hydroxide, or oxyhydroxide, and is not particularly limited as long as it can be dissolved in water. Specifically, the lithium source may be Li2CO3, LiNO3, LiNO2, LiOH, LiOH·H2O, LiH, LiF, LiCl, LiBr, LiI, CH3COOLi, Li2O, Li2SO4, CH3COOLi, or Li3C6H5O7, and any one or a mixture of two or more of these may be used.

[0068] After mixing the positive electrode active material precursor and the lithium source, the mixture is fired at 730 to 830° C. to form a lithium transition metal oxide. The mixture is more preferably fired at 750 to 810° C., and even more preferably fired at 780 to 800° C., for 5 to 20 hours, and more preferably fired for 8 to 15 hours.

[0069] On the other hand, if necessary, a doping element M 1 The raw material containing M may be further mixed. 1can be, for example, one or more selected from the group consisting of Zr, B, W, Mg, Ce, Hf, Ta, La, Ti, Sr, Ba, F, P and S, and the doping element M 1 The raw material containing M 1 It may contain acetates, nitrates, sulfates, halides, sulfides, hydroxides, oxides, oxyhydroxides or combinations thereof. Upon calcination, M 1 When further mixing, M 1 The element diffuses into the lithium transition metal oxide to be doped, and the effect of improving the structural stability of the positive electrode active material can be obtained.

[0070] The positive electrode active material of the present invention thus prepared comprises a lithium transition metal oxide represented by the following chemical formula 2, wherein the lithium transition metal oxide is a secondary particle formed by agglomeration of a plurality of primary particles, the major axes of the primary particles are aligned in a direction from the center to the surface of the secondary particle, and the primary particles comprise crystal grains whose (003) planes are aligned parallel to the major axes of the primary particles.

[0071] [Chemical formula 2] Li a [Ni b Co c Mn d Al e ] 1-f M 1 f O2

[0072] In the above Chemical Formula 2, M 1 is a doping element doped into the lithium transition metal oxide, and can be, for example, one or more selected from the group consisting of Zr, B, W, Mg, Ce, Hf, Ta, La, Ti, Sr, Ba, F, P and S.

[0073] The a represents a molar ratio of lithium in the lithium transition metal oxide, and may be 0.8≦a≦1.2, 0.85≦a≦1.15, or 0.9≦a≦1.1.

[0074] The b represents a molar ratio of nickel to the total moles of transition metals in the lithium transition metal oxide, and may be 0.7≦b≦0.99, 0.8≦b≦0.98, 0.85≦b≦0.98, or 0.85≦b≦0.95.

[0075] The c represents a molar ratio of cobalt to the total mole number of transition metals in the lithium transition metal oxide, and is 0 <c<0.3、0.01≦c<0.2、0.01≦c<0.14または0.01≦c<0.12であることができる。

[0076] The d represents a molar ratio of manganese to the total mole number of transition metals in the lithium transition metal oxide, and is 0 <d<0.3、0.01≦d<0.2、0.01≦d<0.14または0.01≦d<0.12であることができる。

[0077] The e represents a molar ratio of aluminum to the total number of moles of transition metals in the lithium transition metal oxide, and may be 0.01≦e≦0.1, 0.01≦e≦0.08, or 0.01≦e≦0.05.

[0078] The f is a doping element M doped into the transition metal layer in the lithium transition metal oxide. 1 and may be 0≦f≦0.1, 0≦f≦0.05, or 0≦f≦0.03.

[0079] Meanwhile, the positive electrode active material preferably has aluminum (Al) uniformly distributed throughout the entire secondary particles. That is, aluminum may be contained in the secondary particles of the positive electrode active material without a concentration gradient. By uniformly distributing aluminum (Al) within the secondary particles without a concentration gradient, the entanglement of aluminum (Al) is suppressed, minimizing capacity loss, and improving life characteristics and resistance increase rate characteristics with a small amount of aluminum (Al).

[0080] Preferably, the positive electrode active material of the present invention may be one in which nickel, manganese, cobalt and aluminum are distributed in uniform concentrations throughout the secondary particles without concentration gradients.

[0081] Meanwhile, the cathode active material according to the present invention may be a secondary particle formed by agglomeration of a plurality of primary particles, and the major axis of the primary particle may be arranged in a direction from the center to the surface of the secondary particle. Since lithium ions move along the interface between the primary particles in the cathode active material particle, when the cathode active material has a structure in which the major axis of the primary particle is arranged in a direction from the center to the surface of the secondary particle, i.e., a radial structure, the migration path of the lithium ions inside the cathode active material particle is shortened, and an effect of improving lithium mobility can be obtained.

[0082] In addition, the primary particles of the positive electrode active material according to the present invention include crystal grains in which the (003) plane is arranged parallel to the long axis of the primary particle. When the (003) plane is arranged parallel to the long axis of the primary particle, the area of ​​the (003) plane exposed at the interface between the primary particles becomes large. Since the (003) plane is a stable crystal plane into which lithium ions cannot be inserted / extracted, when the external exposed area of ​​the (003) plane is large, structural deterioration of the active material due to insertion / extraction of lithium ions is suppressed, thereby improving the life characteristics.

[0083] Meanwhile, the primary particles of the positive electrode active material may be columnar, and in this case, the aspect ratio of the primary particles may be 1.5 or more, preferably 1.5 to 10, more preferably 2.5 to 8, and further preferably 2.5 to 5. When the aspect ratio of the primary particles of the positive electrode active material satisfies the above range, there is an effect that the lithium migration path between the inside and outside of the primary particles can be shortened.

[0084] The average particle size D of the secondary particles of the positive electrode active material of the present invention 50 When the average particle size of the secondary particles of the positive electrode active material is within the above range, more advantageous effects can be obtained in terms of energy density, life, and gas generation.

[0085] <Positive electrodes and lithium secondary batteries> According to another embodiment of the present invention, there is provided a positive electrode for a secondary battery and a lithium secondary battery, each of which includes the positive electrode active material prepared as above.

[0086] Specifically, the positive electrode includes a positive electrode current collector and a positive electrode active material layer formed on the positive electrode current collector and including the positive electrode active material.

[0087] In the positive electrode, the positive electrode current collector is not particularly limited as long as it does not cause a chemical change in the battery and has conductivity, and for example, stainless steel, aluminum, nickel, titanium, baked carbon, or aluminum or stainless steel surface treated with carbon, nickel, titanium, silver, etc. can be used. In addition, the positive electrode current collector can usually have a thickness of 3 to 500 μm, and fine irregularities can be formed on the surface of the positive electrode current collector to increase the adhesive force of the positive electrode active material. For example, it can be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.

[0088] The positive electrode active material layer may contain a conductive material and a binder in addition to the positive electrode active material.

[0089] In this case, the conductive material is used to give conductivity to the electrode, and can be used without any particular limitation as long as it does not cause a chemical change in the battery that is constructed and has electronic conductivity. Specific examples include graphite such as natural graphite and artificial graphite; carbon-based materials such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, thermal black, and carbon fibers; metal powders or metal fibers such as copper, nickel, aluminum, and silver; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive polymers such as polyphenylene derivatives, and among these, one type alone or a mixture of two or more types can be used. The conductive material can usually be contained in an amount of 1 to 30% by weight based on the total weight of the positive electrode active material layer.

[0090] In addition, the binder plays a role in improving the adhesion between the positive electrode active material particles and the adhesive strength between the positive electrode active material and the positive electrode current collector. Specific examples include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer rubber (EPDM rubber), sulfonated-EPDM, styrene butadiene rubber (SBR), fluororubber, or various copolymers thereof, and among these, one type alone or a mixture of two or more types may be used. The binder may be included in an amount of 1 to 30% by weight based on the total weight of the positive electrode active material layer.

[0091] The positive electrode may be manufactured by a typical method for manufacturing a positive electrode, except for using the positive electrode active material. Specifically, the positive electrode may be manufactured by applying a composition for forming a positive electrode active material layer containing the positive electrode active material and, optionally, a binder and a conductive material, onto the entire positive electrode assembly, followed by drying and rolling. In this case, the types and contents of the positive electrode active material, binder, and conductive material are as described above.

[0092] The solvent may be a solvent commonly used in the art, and may include dimethyl sulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), acetone, water, etc., and one or more of these may be used alone or in combination. The amount of the solvent used is sufficient to dissolve or disperse the positive electrode active material, conductive material, and binder, and to provide a viscosity that allows excellent thickness uniformity during subsequent coating for the production of a positive electrode, taking into consideration the coating thickness of the slurry and the manufacturing yield.

[0093] As another method, the positive electrode can also be produced by casting the composition for forming a positive electrode active material layer on another support, peeling the composition from the support, and laminating the resulting film on a positive electrode current collector.

[0094] According to yet another embodiment of the present invention, there is provided an electrochemical device including the positive electrode. The electrochemical device may be, for example, a battery or a capacitor, and more specifically, a lithium secondary battery.

[0095] The lithium secondary battery specifically includes a positive electrode, a negative electrode facing the positive electrode, a separator interposed between the positive electrode and the negative electrode, and an electrolyte, and the positive electrode is as described above. The lithium secondary battery may further include a battery container that houses an electrode assembly of the positive electrode, the negative electrode, and the separator, and a sealing member that seals the battery container.

[0096] In the lithium secondary battery, the negative electrode includes a negative electrode current collector and a negative electrode active material layer located on the negative electrode current collector.

[0097] The negative electrode current collector is not particularly limited as long as it does not cause a chemical change in the battery and has high conductivity, and may be, for example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface treated with carbon, nickel, titanium, silver, or aluminum-cadmium alloy. The negative electrode current collector may have a thickness of usually 3 to 500 μm, and like the positive electrode current collector, the surface of the current collector may be formed with fine irregularities to strengthen the binding force of the negative electrode active material. For example, it may be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.

[0098] The negative electrode active material layer includes a negative electrode active material and, optionally, a binder and a conductive material. For example, the negative electrode active material layer can be manufactured by applying a negative electrode forming composition including a negative electrode active material and, optionally, a binder and a conductive material onto a negative electrode current collector and drying the composition, or by casting the composition onto another support and then peeling the composition from the support to obtain a film, which is then laminated onto the negative electrode current collector.

[0099] The negative electrode active material may be a compound capable of reversible intercalation and deintercalation of lithium. Specific examples of the negative electrode active material include carbonaceous materials such as artificial graphite, natural graphite, graphitized carbon fiber, and amorphous carbon; metallic compounds capable of alloying with lithium such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Cd, Si alloys, Sn alloys, and Al alloys; SiO β (0<β<2), metal oxides capable of doping and dedoping lithium, such as SnO2, vanadium oxide, and lithium vanadium oxide; or composites containing the metallic compounds and carbonaceous materials, such as Si-C composites and Sn-C composites, and any one or a mixture of two or more of these may be used. In addition, a metallic lithium thin film may be used as the negative electrode active material. In addition, both low crystalline carbon and high crystalline carbon may be used as the carbon material. Representative examples of low crystalline carbon include soft carbon and hard carbon, and representative examples of high crystalline carbon include amorphous, plate-like, flake-like, spherical or fibrous natural graphite or artificial graphite, Kish graphite, pyrolytic carbon, mesophase pitch based carbon fiber, meso-carbon microbeads, mesophase pitches, and high-temperature fired carbon such as petroleum or coal tar pitch derived cokes.

[0100] The binder and conductive material may be as described above for the positive electrode.

[0101] Meanwhile, in the lithium secondary battery, the separator separates the negative electrode and the positive electrode and provides a path for lithium ions to move. Any separator that is generally used as a separator in a lithium secondary battery can be used without any particular limitation. In particular, a separator that has low resistance to ion movement of the electrolyte and has excellent electrolyte humidification ability is preferable. Specifically, a porous polymer film, for example, a porous polymer film made of a polyolefin-based polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer, or a laminate structure of two or more layers thereof can be used. In addition, a conventional porous nonwoven fabric, for example, a nonwoven fabric made of a high-melting point glass fiber, a polyethylene terephthalate fiber, etc. can be used. In addition, a coated separator containing a ceramic component or a polymeric material can be used to ensure heat resistance or mechanical strength, and can be selectively used in a single layer or multilayer structure.

[0102] In addition, examples of the electrolyte used in the present invention include organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel polymer electrolytes, solid inorganic electrolytes, and molten inorganic electrolytes that can be used in the production of lithium secondary batteries, but are not limited to these.

[0103] Specifically, the electrolyte may include an organic solvent and a lithium salt.

[0104] The organic solvent can be used without any particular limitation as long as it serves as a medium through which ions involved in the electrochemical reaction of the battery can move. Specifically, the organic solvent can be an ester solvent such as methyl acetate, ethyl acetate, γ-butyrolactone, or ε-caprolactone; an ether solvent such as dibutyl ether or tetrahydrofuran; a ketone solvent such as cyclohexanone; an aromatic hydrocarbon solvent such as benzene or fluorobenzene; dimethylcarbonate (DMC), diethylcarbonate (DEC), ethylmethylcarbonate (EMC), ethylene carbonate (EC), or propylene carbonate (propylene carbonate). Examples of the solvents that can be used include carbonate-based solvents such as ethylene carbonate (PC), alcohol-based solvents such as ethyl alcohol and isopropyl alcohol, nitriles such as R-CN (R is a C2-C20 straight-chain, branched or cyclic hydrocarbon group that can contain a double bond aromatic ring or an ether bond), amides such as dimethylformamide, dioxolanes such as 1,3-dioxolane, and sulfolanes. Among these, carbonate-based solvents are preferred, and a mixture of a cyclic carbonate (e.g., ethylene carbonate or propylene carbonate) having high ionic conductivity and high dielectric constant that can enhance the charge / discharge performance of a battery and a low-viscosity linear carbonate compound (e.g., ethyl methyl carbonate, dimethyl carbonate or diethyl carbonate) is more preferred. In this case, when the cyclic carbonate and the linear carbonate are mixed in a volume ratio of about 1:1 to about 1:9, the electrolyte can exhibit excellent performance.

[0105] The lithium salt can be used without any particular limitation as long as it is a compound capable of providing lithium ions used in a lithium secondary battery. Specifically, the lithium salt can be LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO2, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiCl, LiI, or LiB(C2O4)2. The lithium salt is preferably used in a concentration range of 0.1 to 2.0M. When the concentration of the lithium salt is within the above range, the electrolyte has appropriate conductivity and viscosity, so that it can exhibit excellent electrolyte performance and lithium ions can move effectively.

[0106] In addition to the electrolyte components, the electrolyte may further contain one or more additives such as haloalkylene carbonate compounds such as difluoroethylene carbonate, pyridine, triethyl phosphite, triethanolamine, cyclic ethers, ethylenediamine, n-glyme, hexamethylphosphoric triamide, nitrobenzene derivatives, sulfur, quinoneimine dyes, N-substituted oxazolidinones, N,N-substituted imidazolidines, ethylene glycol dialkyl ethers, ammonium salts, pyrrole, 2-methoxyethanol, or aluminum trichloride, in order to improve the life characteristics of the battery, suppress the decrease in the capacity of the battery, and improve the discharge capacity of the battery. In this case, the additives may be contained in an amount of 0.1 to 5 wt % based on the total weight of the electrolyte.

[0107] As described above, the lithium secondary battery including the positive electrode active material according to the present invention stably exhibits excellent discharge capacity, output characteristics and capacity retention rate, and is therefore useful in portable devices such as mobile phones, notebook computers and digital cameras, and electric vehicles such as hybrid electric vehicles (HEVs).

[0108] Therefore, according to another embodiment of the present invention, there is provided a battery module including the lithium secondary battery as a unit cell, and a battery pack including the same.

[0109] The battery module or battery pack may be used as a power source for one or more medium- to large-sized devices, such as a power tool; an electric vehicle (EV), a hybrid electric vehicle, and a plug-in hybrid electric vehicle (PHEV); or a power storage system.

[0110] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention may be embodied in various different forms and should not be construed as limited to the embodiments set forth herein.

[0111] Example 1 After putting 4 liters of distilled water into a reactor (volume 20L), the temperature was maintained at 58℃, and a 2.29 mol / L transition metal aqueous solution, which was a mixture of NiSO4, CoSO4, and MnSO4 with a nickel:cobalt:manganese molar ratio of 88:5:7, was fed into the reactor at 500ml / hr, and a 1.145 mol / L Al(NO3)3 aqueous solution was fed into the reactor at 20ml / hr. A 9 wt% ammonia aqueous solution was continuously fed into the reactor at 510ml / hr. A 15 wt% sodium hydroxide aqueous solution was then fed at 306ml / hr, and the feeding of the sodium hydroxide aqueous solution was adjusted to maintain the pH at 11.4.

[0112] The mixture was stirred at 600 rpm for the first 30 minutes to generate nuclei, and then stirred at 250-600 rpm to grow particles. After 20 hours of coprecipitation reaction, when the inside of the batch reactor was filled, stirring was stopped to allow the precursor particles to settle, and the supernatant liquid was removed leaving 4 L of the reaction product, after which the reaction was carried out again. The reaction was continued for a total of 40 hours to form precursor particles. The precursor particles were separated and washed with water, then dried in a hot air dryer at 130°C for more than 12 hours, crushed and sieved to obtain Ni 0.86 Co 0.05 Mn 0.07 Al 0.02 A positive electrode active material precursor having the composition (OH)2 was prepared.

[0113] Example 2 The positive electrode active material precursor prepared in Example 1, LiOH, and ZrO2 were mixed so that the molar ratio of (Ni+Co+Mn+Al):Li:Zr was 1:1.07:0.0015, and the mixture was fired at 790°C for 10 hours in an oxygen atmosphere to produce a positive electrode active material doped with 1,500 ppm of Zr and having a molar ratio of Ni:Co:Mn:Al of 86:5:7:2.

[0114] Comparative Example 1 After adding 4 liters of distilled water to a reactor (volume 20 L), the temperature was maintained at 58°C, and a 2.29 mol / L transition metal aqueous solution, which was a mixture of NiSO4, CoSO4, MnSO4, and AlSO4 with a nickel:cobalt:manganese:aluminum molar ratio of 86:5:7:2, was added to the reactor at 500 ml / hr, and a 9 wt% ammonia aqueous solution was continuously added to the reactor at 510 ml / hr. Then, a 15 wt% sodium hydroxide aqueous solution was added at 306 ml / hr, and the sodium hydroxide aqueous solution was added at a rate adjusted so that the pH was maintained at 11.4.

[0115] The mixture was stirred at 600 rpm for the first 30 minutes to generate nuclei, and then stirred at 250-600 rpm to grow particles. After 20 hours of coprecipitation reaction, when the inside of the batch reactor was filled, stirring was stopped to allow the precursor particles to precipitate, and the supernatant liquid was removed leaving 4 L of the reaction product, and the reaction was carried out again. The reaction was continued for a total of 40 hours to form precursor particles. The precursor particles were separated and washed with water, then dried in a hot air dryer at 130°C for more than 12 hours, crushed and sieved to obtain Ni 0.86 Co 0.05 Mn 0.07 Al 0.02 A positive electrode active material precursor having the composition (OH)2 was prepared.

[0116] Comparative Example 2 After adding 4 liters of distilled water to a reactor (volume 20 L), the temperature was maintained at 58°C, and a 2.29 mol / L transition metal aqueous solution, which was a mixture of NiSO4, CoSO4, and MnSO4 so that the molar ratio of nickel:cobalt:manganese was 88:5:7, was added to the reactor at 510 ml / hr, and a 9 wt% ammonia aqueous solution was continuously added to the reactor at 510 ml / hr. Then, a 15 wt% sodium hydroxide aqueous solution was added at 306 ml / hr, and the sodium hydroxide aqueous solution was added at a rate adjusted so that the pH was maintained at 11.4.

[0117] The mixture was stirred at 600 rpm for the first 30 minutes to generate nuclei, and then stirred at 250-600 rpm to grow particles. After 20 hours of coprecipitation reaction, the inside of the batch reactor was filled, and stirring was stopped to allow the precursor particles to settle. After removing the supernatant liquid, leaving 4 L of reactant, the reaction was started again. After a total of 40 hours of reaction, Ni 0.88 Co 0.05 Mn 0.07 Precursor particles were formed having a composition of (OH)2.

[0118] The positive electrode active material precursor prepared above, LiOH, Al2O3, and ZrO2 were mixed so that the molar ratio of (Ni+Co+Mn):Li:Al:Zr was 1:1.07:0.02:0.0015, and calcined at 770°C for 10 hours in an oxygen atmosphere to prepare a positive electrode active material doped with 1,500 ppm of Zr and having a molar ratio of Ni:Co:Mn:Al of 86:5:7:2.

[0119] [Experimental Example 1: Confirmation of Positive Electrode Active Material Precursor and Positive Electrode Active Material] Transmission electron microscope (TEM) analysis was performed to measure the crystal structure and the aspect ratio of the primary particles of the positive electrode active material precursor and the positive electrode active material of Examples 1 and 2 and Comparative Examples 1 and 2. The TEM analysis was performed using selected area diffraction pattern (SADP) and FAST Fourier transform (FFT).

[0120] The results are shown in Figures 1 to 4.

[0121] Figure 1 is a TEM image of a cross section of the positive electrode active material precursor prepared in Example 1. As shown in Figure 1, the positive electrode active material precursor of Example 1 had Al uniformly distributed throughout the particle, and the major axes of the primary particles were aligned in a direction from the center to the surface of the secondary particles.

[0122] In addition, the length of the short axis and the length of the long axis of the primary particles were measured by TEM image analysis to calculate the aspect ratio of the primary particles, and the aspect ratio of the measured primary particles was 6.7 on average.

[0123] In addition, the crystal grain structure was confirmed by SADP, and it was confirmed that the (001) plane was arranged parallel to the long axis of the primary particles. The direction of the (001) plane is indicated by the arrow.

[0124] Figure 2 is a TEM image of a cross section of the positive electrode active material prepared in Example 2. As shown in Figure 2, in the positive electrode active material of Example 2, Al was uniformly distributed throughout the secondary particles, and the major axes of the primary particles were aligned in the direction from the center to the surface of the secondary particles.

[0125] In addition, the length of the short axis and the length of the long axis of the primary particles were measured by TEM image analysis to calculate the aspect ratio of the primary particles, and the aspect ratio of the measured primary particles was 3.2 on average.

[0126] In addition, the crystal grain structure was confirmed by SADP, and the (003) plane was found to be aligned parallel to the long axis of the primary particles. The direction of the (003) plane is indicated by the arrow.

[0127] FIG. 3 is a SEM image of the positive electrode active material precursor prepared in Comparative Example 1. As shown in FIG. 3, the positive electrode active material precursor of Comparative Example 1 shows the presence of small NCM seed-shaped particles and a compound of Al and sulfur. In addition, even after 40 hours of reaction, there was no secondary particle D 50 It is evident that the grain size was 5 μm or less, and almost no grain growth occurred.

[0128] Figure 4 is a TEM image of a cross section of the positive electrode active material prepared in Comparative Example 2. As shown in Figure 4, in the positive electrode active material of Comparative Example 2, Al was uniformly distributed throughout the secondary particles, and the major axes of the primary particles were aligned in a direction from the center to the surface of the secondary particles.

[0129] In addition, the length of the short axis and the length of the long axis of the primary particles were measured by TEM image analysis to calculate the aspect ratio of the primary particles, and the aspect ratio of the measured primary particles was 2.4 on average.

[0130] In addition, the crystal grain structure was confirmed by SADP, and it was found that the (003) plane was distributed in various directions. The directions of the (003) planes are indicated by arrows.

[0131] [Experimental example 2: Life characteristics, resistance increase rate characteristics] The positive electrode active materials prepared in Example 2 and Comparative Example 2, the carbon black conductive material, and the PVdF binder were mixed in a weight ratio of 96:2:2 in N-methylpyrrolidone solvent to prepare a positive electrode mixture, which was then coated on one side of an aluminum current collector, dried at 100° C., and rolled to prepare a positive electrode.

[0132] The negative electrode used was lithium metal.

[0133] A porous polyethylene separator was interposed between the positive and negative electrodes to prepare an electrode assembly, and the electrode assembly was placed inside a case, and an electrolyte was injected into the case to prepare a lithium secondary battery. The electrolyte was prepared by dissolving lithium hexafluorophosphate (LiPF6) at a concentration of 1.0 M in an organic solvent consisting of ethylene carbonate / ethyl methyl carbonate / diethyl carbonate / (EC / EMC / DEC mixed volume ratio = 3 / 4 / 3).

[0134] Each lithium secondary battery cell thus manufactured was charged at 45° C. with a constant current of 1C to 4.25V with a 3C cut off. Thereafter, it was discharged at a constant current of 0.33C to 3.0V. The above charge and discharge behavior was regarded as one cycle, and this cycle was repeated 100 times, after which the capacity retention rate and the resistance increase rate according to the cycle were measured. In the case of the capacity retention rate, the capacity at the 100th cycle was divided by the initial capacity and multiplied by 100 to calculate the value, and in the case of the resistance increase rate, the resistance at the 100th cycle was divided by the initial resistance and multiplied by 100 to calculate the value. The results are shown in Table 1 and FIG. 5 below.

[0135] [Table 1]

[0136] Referring to Table 1 and FIG. 5, the positive electrode active material of Example 2 was remarkably excellent in the characteristics of capacity retention rate and resistance increase rate, while the positive electrode active material of Comparative Example 2 prepared by Al dry doping was inferior in the characteristics of capacity retention rate and resistance increase rate.

Claims

1. providing a transition metal-containing solution containing cations of nickel (Ni), cobalt (Co) and manganese (Mn) and an aluminum-containing solution containing cations of aluminum (Al); and feeding the transition metal-containing solution and the aluminum-containing solution into a reactor, and feeding a basic aqueous solution and an ammonium solution into the reactor to cause a co-precipitation reaction to form a positive electrode active material precursor, The positive electrode active material precursor is composed of a hydroxide represented by the following chemical formula 1: The positive electrode active material precursor is a secondary particle formed by agglomeration of a plurality of cylindrical primary particles, the major axes of the primary particles are arranged in a direction from the center to the surface of the secondary particle, and the primary particles include crystal grains whose (001) planes are arranged parallel to the major axes of the primary particles: [Chemical formula 1] Ni x1 Co y1 Mn z1 Al s1 (OH) 2 In the above Chemical Formula 1, 0.7≦x1≦0.99, 0<y1<0.3, 0<z1<0.3, and 0.01≦s1≦0.

1.

2. 2. The method for producing a positive electrode active material precursor for a secondary battery according to claim 1, wherein the pH of the reaction solution during the coprecipitation reaction is 10.5 to 12.

2.

3. 3. The method for producing a positive electrode active material precursor for a secondary battery according to claim 1, wherein the temperature in the reactor during the coprecipitation reaction is 45° C. to 65° C.

4. 4. The method for producing a positive electrode active material precursor for a secondary battery according to claim 1, wherein the aluminum-containing solution contains aluminum chloride, aluminum acetate, aluminum nitrate, aluminum hydroxide, or a combination thereof.

5. A method for producing a positive electrode active material for a secondary battery, comprising mixing the positive electrode active material precursor produced by the method according to claim 1 with a lithium source and calcining the mixture to form a lithium transition metal oxide.

Citation Information

Patent Citations

  • Electrode active material, and method of manufacturing the same

    JP2013065397A

  • Nickel compound hydroxide and method for producing the same, positive pole active substance for nonaqueous electrolyte secondary cell and method for producing the same, and nonaqueous electrolyte secondary cell

    JP2013147416A

  • Nickel-based active material for lithium secondary battery, method of preparing the same, and lithium secondary battery including positive electrode including the same

    JP2018014325A

  • Method for evaluating thermal stability of nickel-containing positive electrode active material particle powder for nonaqueous electrolyte secondary battery

    JP2018037393A

  • Nickel-based active material for lithium secondary battery, manufacturing method thereof, and lithium secondary battery including positive electrode including the same

    JP2018092931A